Electrophotographic photoreceptor
A protective layer for electrophotographic photoreceptors using a polymer of a compound with polymerizable functional groups and urethane bonds addresses solubility issues, resulting in improved electrical and mechanical properties.
Patent Information
- Application Number
- JP2023059156
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing electrophotographic photoreceptors face challenges in achieving a balance between excellent electrical properties such as potential retention and mechanical properties like hardness and elastic deformation rate, particularly due to the low solubility of electron-transporting compounds in organic solvents used for forming protective layers.
The development of a protective layer containing a polymer of a compound with at least one polymerizable functional group and a urethane bond, which enhances solubility in organic solvents and improves mechanical and electrical properties, including charge mobility.
This approach results in an electrophotographic photoreceptor with improved potential retention and mechanical strength, ensuring efficient manufacturing and enhanced performance.
Smart Images

Figure 2024146328000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrophotographic photoreceptor for use in copiers, printers, etc., which has at least a photosensitive layer and a protective layer sequentially provided on a conductive support, and which has improved electrical properties such as residual potential characteristics, and improved mechanical properties such as hardness and elastic deformation rate. [Background technology]
[0002] In printers and copiers, when a charged organic photoconductor (OPC) drum is irradiated with light, the part is discharged, an electrostatic latent image is generated, and an image is obtained by attaching toner to the electrostatic latent image. In such devices that use electrophotography, the photoconductor is the core material.
[0003] This type of organic photoreceptor has a wide range of material options and is easy to control the characteristics of the photoreceptor, so that "functionally separated photoreceptors" in which the functions of charge generation and transport are shared by different compounds are becoming mainstream. For example, a single-layer electrophotographic photoreceptor (hereinafter referred to as a "single-layer photoreceptor") having a charge generation material (CGM) and a charge transport material (CTM) in the same layer, and a laminated electrophotographic photoreceptor (hereinafter referred to as a "laminated photoreceptor") formed by laminating a charge generation layer containing a charge generation material (CGM) and a charge transport layer containing a charge transport material (CTM) are known. In addition, the charging method of the photoreceptor can be a negative charging method in which the photoreceptor surface is negatively charged, or a positive charging method in which the photoreceptor surface is positively charged. Combinations of layer structures and charging methods of photoreceptors currently in practical use include "negatively charged multi-layer photoreceptors" and "positively charged single-layer photoreceptors."
[0004] A "negatively charged laminated photoreceptor" generally has a structure in which an undercoat layer (UCL) made of a resin or the like is provided on a conductive substrate such as an aluminum tube, on which a charge generation layer (CGL) made of a charge generation material (CGM) and a resin or the like is provided, on which a charge transport layer (CTL) made of a hole transport material (HTM) and a resin or the like is provided.
[0005] On the other hand, a "positively charged single-layer photoreceptor" generally has a configuration in which an undercoat layer (UCL) made of a resin or the like is provided on a conductive substrate such as an aluminum tube, and a single-layer photosensitive layer made of a charge generating material (CGM), a hole transporting material (HTM), an electron transporting material (ETM), and a resin or the like is provided on top of the undercoat layer (UCL) (see, for example, Patent Document 1).
[0006] In either photoconductor, the surface of the photoconductor is first charged using corona discharge or contact, then the photoconductor is exposed to light to neutralize the surface charge, forming an electrostatic latent image due to the potential difference with the surrounding surface. Toner is then brought into contact with the photoconductor surface to form a toner image that corresponds to the electrostatic latent image, which is then transferred to paper or the like and heated to melt and fix it, completing the print.
[0007] As described above, the basic structure of an electrophotographic photoreceptor is a photosensitive layer formed on a conductive support. In order to improve abrasion resistance, etc., a protective layer may be provided on the photosensitive layer.
[0008] As a technique for improving the mechanical strength or abrasion resistance of the photoreceptor surface, a photoreceptor has been disclosed in which a layer containing a compound having a chain-polymerizable functional group as a binder resin is formed in the outermost layer of the photoreceptor, and this is polymerized by applying energy such as heat, light, or radiation to form a hardened resin layer (see, for example, Patent Documents 1 and 2). Such a protective layer is generally formed by dissolving a curable composition containing a compound having a chain polymerizable functional group in an organic solvent to prepare a coating liquid for forming a protective layer, and then coating the coating liquid for forming a protective layer on the surface of the photoreceptor. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] U.S. Pat. No. 9,417,538 [Patent Document 2] International Publication No. 2010 / 035683 Summary of the Invention [Problem to be solved by the invention]
[0010] As described above, it is known to provide a protective layer to improve the abrasion resistance of a photoreceptor. Among them, a protective layer using a curable compound (a compound having a chain polymerizable functional group) is particularly excellent in mechanical strength and can provide a good protective effect. On the other hand, from the viewpoint of improving the electrical properties of the photoreceptor, the protective layer is required to have good electron transport properties as well as mechanical strength. In order to improve the electron transport properties of the photoreceptor, it is effective to include a compound having an electron transport structure in the protective layer. However, it has been found that some compounds having an electron transport structure have insufficient solubility in the organic solvent used to prepare the coating solution for forming the protective layer, and the potential retention rate and mechanical properties of the photoreceptor obtained by forming a protective layer using this compound are insufficient.
[0011] An object of the present invention is to provide an electrophotographic photoreceptor having at least a photosensitive layer and a protective layer in this order on a conductive support, which is excellent in electrical properties such as potential retention rate, and mechanical properties such as hardness and elastic deformation rate, and further, the solubility of an electron transport compound used in forming the protective layer in an organic solvent. [Means for solving the problem]
[0012] The present inventors have discovered that by forming a protective layer containing a polymer of a compound having at least one polymerizable functional group and further having at least one urethane bond (also referred to as an "electron transporting compound"), a photoreceptor having excellent electrical properties such as potential holding ratio, and mechanical properties such as hardness and elastic deformation rate can be manufactured, and further that the electron transporting compound has excellent solubility in organic solvents. The present invention has been achieved based on these findings, and has the following gist.
[0013] [1] An electrophotographic photoreceptor having at least a photosensitive layer and a protective layer in this order on a conductive support, The protective layer of the electrophotographic photoreceptor contains a polymer of a compound represented by the following formula (1) and having at least one group represented by the following formula (1A) and at least one polymerizable functional group in one molecule.
[0014] TIFF2024146328000002.tif3282
[0015] In formula (1), X represents an electron transporting skeleton having a valence of n. A is a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, a group represented by the following formula (2), or a group represented by the following formula (1B). n represents an integer of 1 or more. When n is 1, A is a group represented by the following formula (2) or a group represented by the following formula (1B). When A is a group represented by the following formula (2), at least one of R1 and R2 is a group represented by the following formula (1B), or at least one of L1 and L2 is a group represented by the following formula (1A). At least one of Z is a polymerizable functional group. When A is a group represented by the following formula (1B), R3 is a polymerizable functional group. When n is 2 or more, the multiple A's may be the same or different from each other, and at least one of the multiple A's is a group represented by the following formula (2) or a group represented by the following formula (1B). When the A is a group represented by the following formula (2), at least one of R1 and R2 is a group represented by the following formula (1B), or at least one of L1 and L2 is a group represented by the following formula (1A). In addition, the A or at least one other A contains at least one polymerizable functional group in the structure.
[0016] TIFF2024146328000003.tif38150
[0017] In formula (2), * represents a bond to X. R1 and R2 each independently represent a hydrogen atom, an alkyl group which may have a substituent, an alkoxy group which may have a substituent, an aryloxy group which may have a substituent, a heteroaryloxy group which may have a substituent, an alkoxycarbonyl group which may have a substituent, a dialkylamino group which may have a substituent, a diarylamino group which may have a substituent, an arylalkylamino group which may have a substituent, an acyl group which may have a substituent, a haloalkyl group which may have a substituent, an alkylthio group which may have a substituent, an arylthio group which may have a substituent, a silyl group which may have a substituent, a siloxy group which may have a substituent, an aromatic hydrocarbon group which may have a substituent, or an aromatic heterocyclic group which may have a substituent, or a group represented by the following formula (1B). L1 and L2 each independently represent a direct bond, a divalent group, or a group represented by the following formula (1A). Z represents a hydrogen atom, an alkoxy group, an amide group, or a polymerizable functional group, provided that x1+y1=3, where x1 is an integer of 0 to 2, y1 is an integer of 1 to 3, x2+y2=3, where x2 is an integer of 0 to 2, y2 is an integer of 1 to 3, and when x1 is an integer of 2 or more, R1 may be the same or different from each other, and when y1 is an integer of 2 or more, R 2、 x2, y2, L 1、Each of L2 and Z may be the same or different from each other, when x2 is an integer of 2 or more, each of R2 may be the same or different from each other, and when y2 is an integer of 2 or more, each of L2 and Z may be the same or different from each other.
[0018] TIFF2024146328000004.tif33117
[0019] In formula (1B), * represents a bond to any atom in formula (1) or (2), and B1 and B2 each independently represent a direct bond or a divalent group. R3 represents a hydrogen atom, an alkyl group which may have a substituent, an alkoxy group which may have a substituent, an aryloxy group which may have a substituent, a heteroaryloxy group which may have a substituent, an alkoxycarbonyl group which may have a substituent, a dialkylamino group which may have a substituent, a diarylamino group which may have a substituent, an arylalkylamino group which may have a substituent, an acyl group which may have a substituent, a haloalkyl group which may have a substituent, an alkylthio group which may have a substituent, an arylthio group which may have a substituent, a silyl group which may have a substituent, a siloxy group which may have a substituent, an aromatic hydrocarbon group which may have a substituent, an aromatic heterocyclic group which may have a substituent, or a polymerizable functional group.
[0020] TIFF2024146328000005.tif33117
[0021] In formula (1A), B1 and B2 each independently represent a direct bond or a divalent group, and * represents a bond to any atom in formula (1).
[0022] [2] The electrophotographic photoreceptor according to [1] above, wherein in formula (1), X is represented by formula (3) or (4).
[0023] TIFF2024146328000006.tif106170
[0024] In formulas (3) and (4), G1~G12 each independently represents a hydrogen atom, a deuterium atom, a halogen atom, an alkyl group which may have a substituent, or an alkoxy group which may have a substituent, and * represents a bond to A.
[0025] [3] The electrophotographic photoreceptor according to the above [1] or [2], wherein in the above formula (1), at least one A is a group represented by the above formula (2).
[0026] [4] The electrophotographic photoreceptor according to any one of the above [1] to [3], wherein in the above formula (2), at least one of L1 and L2 is a group represented by the above formula (1A).
[0027] [5] The electrophotographic photoreceptor according to any one of [1] to [4] above, wherein the compound represented by formula (1) has at least two polymerizable functional groups in one molecule.
[0028] [6] The electrophotographic photoreceptor according to any one of [1] to [5] above, wherein the polymerizable functional group is selected from the following formulae (M1) to (M7):
[0029] TIFF2024146328000007.tif46150
[0030] In the above formulas (M1) to (M7), R 110 represents a hydrogen atom or an alkyl group which may have a substituent, and * represents the bonding position.
[0031] [7] The electrophotographic photoreceptor according to any one of the above [1] to [6], wherein in the formula (2), R1 is an alkyl group which may have a substituent.
[0032] [8] The electrophotographic photoreceptor according to any one of [1] to [7] above, wherein the protective layer further contains a polymer of a polymerizable compound having no electron transport skeleton. [9] The electrophotographic photoreceptor according to any one of [1] to [8] above, wherein the protective layer further contains an electron-donating compound.
[0033]
[10] An electrophotographic photoreceptor cartridge comprising the electrophotographic photoreceptor according to any one of [1] to [9].
[11] An image forming apparatus having the electrophotographic photoreceptor according to any one of [1] to [9]. Effect of the Invention
[0034] According to the present invention, it is possible to provide an electrophotographic photoreceptor having at least a photosensitive layer and a protective layer in this order on a conductive support, which is excellent in electrical properties such as potential retention rate and mechanical properties such as hardness and elastic deformation rate. Moreover, in the present invention, since the electron transport compound used in forming the protective layer has excellent solubility in organic solvents such as alcohol-based solvents, when forming the protective layer, an electrophotographic photoreceptor having excellent electrical and mechanical properties can be efficiently manufactured with good workability due to its good solvent solubility. [Brief description of the drawings]
[0035] [Figure 1] 1 is a diagram illustrating an example of the configuration of an image forming apparatus that can be configured using an electrophotographic photoreceptor according to an example of the present invention. [Diagram 2] 1 is a graph showing a general relationship between the indentation depth of an indenter and a load curve when measuring the Martens hardness and elastic deformation rate of a photoreceptor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0036] The following describes in detail the mode for carrying out the present invention (hereinafter, the embodiment of the invention). Note that the present invention is not limited to the following embodiment, and can be carried out in various modifications within the scope of the gist of the present invention.
[0037] <<Photoreceptor of the present invention>> An electrophotographic photoreceptor according to one embodiment of the present invention (hereinafter also referred to as "the photoreceptor of the present invention") is an electrophotographic photoreceptor having at least a photosensitive layer and a protective layer, successively provided on a conductive support, and the protective layer contains a polymer of the compound of the present invention described below.
[0038] The photoreceptor of the present invention may optionally have layers other than the photosensitive layer and the protective layer. The charging method of the photoconductor of the present invention may be either a negative charging method in which the surface of the photoconductor is negatively charged or a positive charging method in which the surface of the photoconductor is positively charged. Among them, from the viewpoint of requiring the protective layer to have electron transport properties, the positive charging method is preferred because it is considered that the effect of the present invention can be further obtained with the positive charging method.
[0039] In the photoreceptor of the present invention, the side opposite the conductive support is the upper side or front side, and the conductive support side is the lower side or back side.
[0040] <Main protective layer> The protective layer of the compound of the present invention (sometimes referred to as "the protective layer") has at least one group represented by the following formula (1A) and at least one polymerizable functional group in one molecule, and contains a polymer of an electron transport compound represented by the following formula (1) (sometimes referred to as "the compound of the present invention").
[0041] In the present invention, the term "electron transporting compound" refers to a compound having an electron transporting property, in other words, a compound having an electron transporting skeleton.
[0042] TIFF2024146328000008.tif3282
[0043] In formula (1), X represents an n-valent electron transport skeleton, n represents an integer of 1 or more, and when n is 2 or more, a plurality of As may be the same or different. A has at least one group represented by formula (1A) having a urethane bond and at least one polymerizable functional group.
[0044] The mechanism by which the photoreceptor of the present invention exhibits the effect of having excellent electrical characteristics is believed to be as follows. Since the compound of the present invention has a urethane bond (particularly the NH portion), it has high affinity with the organic solvent used in the coating solution for forming the protective layer and has good solubility, so that the coating solution has good applicability and a uniform protective layer can be formed without unevenness. This is thought to improve the electron transport property in the protective layer and improve the potential retention rate of the photoconductor. In addition, since the compound of the present invention has a polymerizable functional group, the compound of the present invention is polymerized in the step of forming the protective layer described below to form a polymer, which can form a protective layer having excellent mechanical strength. In this case, the polymer may be a polymer formed by polymerizing the compounds of the present invention together, or, when the protective layer contains a polymerizable compound not having an electron transport skeleton, may be a copolymer formed by polymerizing the compound of the present invention with the polymerizable compound. Furthermore, since the compound of the present invention has an electron transport structure, by using the compound of the present invention in the formation of the protective layer, charge injection from the photosensitive layer to the protective layer and charge mobility to the outermost surface are enhanced through the electron transport skeleton, and an electrophotographic photoreceptor having excellent electrical properties such as potential retention can be obtained. In this case, if the electron transport structure of the compound of the present invention is a naphthalene diimide skeleton or a perylene diimide skeleton, the electron transport property is even more excellent and the potential retention rate is also even better. In particular, when the side chain having a urethane bond is branched, the solubility is even better.
[0045] From the viewpoint of more effectively obtaining the effect of the compound of the present invention, the present protective layer is preferably the outermost layer, that is, the outermost layer located on the opposite side to the conductive support. However, the present protective layer does not necessarily have to be the outermost layer, and the effect of the present invention can be obtained. For example, when some kind of segregation layer exists on the outermost layer of the photoreceptor, the present protective layer can be used to obtain the effect even if it is not the outermost layer.
[0046] In the following, we will first explain the compound of the present invention used in forming the protective layer of the present invention, and then we will explain the composition containing the compound of the present invention (hereinafter also referred to as the ``composition of the present invention'' or ``this composition'') and the electrophotographic photoreceptor of the present invention.
[0047] <<Compound of the present invention>> The compound of the present invention is preferably a compound represented by the following formula (1) and having at least one group represented by the following formula (1A) and at least one polymerizable functional group in one molecule. In particular, the compound of the present invention preferably has at least two polymerizable functional groups in one molecule. By having two or more polymerizable functional groups, crosslinking property is further increased, and the hardness of the present protective layer is increased, so that the mechanical strength can be further increased.
[0048] TIFF2024146328000009.tif3282
[0049] <Group represented by formula (1A)> The group represented by the following formula (1A) is a group characterized by having a urethane bond, particularly an NH moiety.
[0050] TIFF2024146328000010.tif33117
[0051] In formula (1A), B1 and B2 each independently represent a direct bond or a divalent group. Examples of the divalent group include an alkylene group, a divalent group having a ketone group, a divalent group having an ether bond, a divalent group having an ester bond, or a group formed by linking these groups. * represents a bond to any atom in formula (1).
[0052] <Polymerizable Functional Group> The compound of the present invention has one or more polymerizable functional groups in one molecule. If the polymerizable functional group is not present, the mechanical strength of the protective layer becomes insufficient. The compound of the present invention may have one or more polymerizable functional groups, but from the viewpoints of solubility in an organic solvent and curability, the number of polymerizable functional groups is preferably two or more, and more preferably four or more. On the other hand, from the viewpoint of the stability of the compound, the number of polymerizable functional groups possessed by the compound of the present invention is preferably 12 or less, more preferably 10 or less, and more preferably 8 or less.
[0053] The polymerizable functional group is not particularly limited as long as it is a functional group having polymerizability, and examples thereof include polymerizable functional groups represented by the following formulae (M1) to (M7).
[0054] TIFF2024146328000011.tif46150
[0055] In the above formulas (M1) to (M7), R 110 represents a hydrogen atom or an alkyl group which may have a substituent, and * represents the bonding position.
[0056] R in the above formulas (M1) to (M7) 110 As the group, a hydrogen atom or an alkyl group having no substituent is preferable, a hydrogen atom or an alkyl group having 1 to 10 carbon atoms is preferable, and a hydrogen atom or a methyl group is particularly preferable. When the compound of the present invention has two or more polymerizable functional groups, they do not all need to be the same and may be different, but from the viewpoint of curability, it is preferable that they are the same.
[0057] <x> In the above formula (1), X represents an electron transporting skeleton having a valence of n. X is preferably a skeleton represented by the following formula (3) or (4). When the electron transporting skeleton is a skeleton represented by formula (3), i.e., a naphthalene diimide skeleton, or a skeleton represented by formula (4), i.e., a perylene diimide skeleton, the electron transporting property is excellent and the electrical characteristics (VL) are further improved, which is more preferable.
[0058] TIFF2024146328000012.tif106170
[0059] In formulas (3) and (4), G1~G 12 Each independently represents a hydrogen atom, a deuterium atom, a halogen atom, an alkyl group which may have a substituent, or an alkoxy group which may have a substituent, and * represents a bond to A. From the viewpoint of electron transport properties, G1 to G 12 are preferably each independently a hydrogen atom or a halogen atom. From the viewpoint of solubility in organic solvents, G1 to G 12 It is also preferable that at least one, preferably at least two, and more preferably at least four of G1 to G2 be a halogen atom. 12 may all be halogen atoms, but usually, the number of halogen atoms is preferably 6 or less. G1~G 12 The halogen atom in may be one or more of a chlorine atom, a bromine atom and an iodine atom. From the viewpoint of the stability of the compound, a chlorine atom or a bromine atom is preferred, and a chlorine atom is particularly preferred. G1~G 12 By containing a halogen atom in the compound, the electron affinity is increased, and the electrical properties as an electron transporting compound are improved, so that a photoreceptor having excellent electrical properties can be obtained.
[0060] <n> In the above formula (1), n represents an integer of 1 or more, and when n is 2 or more, a plurality of As may be the same or different.
[0061] A in the above formula (1) is a hydrogen atom, an alkyl group which may have a substituent, an alkoxy group which may have a substituent, an aryloxy group which may have a substituent, a heteroaryloxy group which may have a substituent, an alkoxycarbonyl group which may have a substituent, a dialkylamino group which may have a substituent, a diarylamino group which may have a substituent, an arylalkylamino group which may have a substituent, an acyl group which may have a haloalkyl group, an alkylthio group which may have a substituent, an arylthio group which may have a substituent, a silyl group which may have a substituent, a siloxy group which may have a substituent, an aromatic hydrocarbon group which may have a substituent, an aromatic heterocyclic group which may have a substituent, a group represented by the following formula (2), or a group represented by the following formula (1B).
[0062] In the present invention, the phrase "optionally has a substituent" means that the group can have a substituent, and includes both the case where the group has a substituent and the case where the group does not have a substituent.
[0063] Since A in formula (1) has a group represented by formula (1A) and a polymerizable functional group, when n is 1, A is a group represented by the following formula (2) or a group represented by the following formula (1B). When A is a group represented by formula (2), at least one of R1 and R2 is a group represented by the following formula (1B), or at least one of L1 and L2 is a group represented by the above formula (1A). At least one of Z is a polymerizable functional group. When A is a group represented by formula (1B), R3 is a polymerizable functional group. When n is 2 or more, the multiple A's may be the same or different from each other, and at least one of the multiple A's is a group represented by the following formula (2) or a group represented by the following formula (1B). When the A is a group represented by the following formula (2), at least one of R1 and R2 is a group represented by the following formula (1B), or at least one of L1 and L2 is a group represented by the above formula (1A). The A or at least one other A contains at least one polymerizable functional group in the structure.
[0064] Among these, from the viewpoint of further improving the solubility in organic solvents, it is preferable that at least one of A is a group represented by formula (2).
[0065] (Group represented by formula (2)) The group represented by formula (2) is a group having a group represented by formula (1A) and a polymerizable functional group. Among them, from the viewpoint of further improving solubility in an organic solvent, it is more preferable that the group has two branches and a polymerizable functional group in a side chain.
[0066] TIFF2024146328000013.tif38150
[0067] In formula (2), * represents a bond to X. R1 and R2 each independently represent a hydrogen atom, an alkyl group which may have a substituent, an alkoxy group which may have a substituent, an aryloxy group which may have a substituent, a heteroaryloxy group which may have a substituent, an alkoxycarbonyl group which may have a substituent, a dialkylamino group which may have a substituent, a diarylamino group which may have a substituent, an arylalkylamino group which may have a substituent, an acyl group which may have a substituent, a haloalkyl group which may have a substituent, an alkylthio group which may have a substituent, an arylthio group which may have a substituent, a silyl group which may have a substituent, a siloxy group which may have a substituent, an aromatic hydrocarbon group which may have a substituent, or an aromatic heterocyclic group which may have a substituent, or a group represented by the following formula (1B). Among these, when R1 is an alkyl group which may have a substituent, the formula (2) is branched at the alkyl group, and the solubility in organic solvents is further improved, which is preferable.
[0068] In formula (2), L1 and L2 each independently represent a direct bond, a divalent group, or a group represented by the above formula (1A). Among these, at least one of L1 and L2 is preferably a group represented by the above formula (1A) since the solubility in organic solvents is further improved if the side chain having a urethane bond is branched.
[0069] Z represents a hydrogen atom, an alkoxy group, an amide group, or a polymerizable functional group, provided that x1+y1=3, where x1 is an integer of 0 to 2, y1 is an integer of 1 to 3, x2+y2=3, where x2 is an integer of 0 to 2, y2 is an integer of 1 to 3, and when x1 is an integer of 2 or more, R1 may be the same or different from each other, and when y1 is an integer of 2 or more, R 2、 x2, y2, L 1、 Each of L2 and Z may be the same or different from each other, when x2 is an integer of 2 or more, each of R2 may be the same or different from each other, and when y2 is an integer of 2 or more, each of L2 and Z may be the same or different from each other.
[0070] (Group represented by formula (1B)) The group represented by formula (1B) is a monovalent group having a group represented by formula (1A).
[0071] TIFF2024146328000014.tif33117
[0072] In formula (1B), * represents a bond to any atom in formula (1) or (2). B1 and B2 each independently represent a direct bond or a divalent group. R3 represents a hydrogen atom, an alkyl group which may have a substituent, an alkoxy group which may have a substituent, an aryloxy group which may have a substituent, a heteroaryloxy group which may have a substituent, an alkoxycarbonyl group which may have a substituent, a dialkylamino group which may have a substituent, a diarylamino group which may have a substituent, an arylalkylamino group which may have a substituent, an acyl group which may have a substituent, a haloalkyl group which may have a substituent, an alkylthio group which may have a substituent, an arylthio group which may have a substituent, a silyl group which may have a substituent, a siloxy group which may have a substituent, an aromatic hydrocarbon group which may have a substituent, an aromatic heterocyclic group which may have a substituent, or a polymerizable functional group.
[0073] <Example> Specific examples of the compound of the present invention include those exemplified below, but the compound is not limited to these compounds.
[0074] TIFF2024146328000015.tif44170
[0075] TIFF2024146328000016.tif43170
[0076] TIFF2024146328000017.tif52170
[0077] TIFF2024146328000018.tif50170
[0078] TIFF2024146328000019.tif53170
[0079] TIFF2024146328000020.tif59170
[0080] TIFF2024146328000021.tif51170
[0081] TIFF2024146328000022.tif55170
[0082] TIFF2024146328000023.tif53170
[0083] TIFF2024146328000024.tif57170
[0084] TIFF2024146328000025.tif51170
[0085] TIFF2024146328000026.tif58170
[0086] TIFF2024146328000027.tif52170
[0087] TIFF2024146328000028.tif58170
[0088] TIFF2024146328000029.tif51170
[0089] TIFF2024146328000030.tif58170
[0090] TIFF2024146328000031.tif52170
[0091] TIFF2024146328000032.tif58170
[0092] TIFF2024146328000033.tif52170
[0093] TIFF2024146328000034.tif58170
[0094] <Method of producing the compound of the present invention> The compound of the present invention can be produced, for example, according to the method described in the Examples below.
[0095] <Solubility of the Compound of the Present Invention> The compound of the present invention has excellent solubility in organic solvents, particularly alcoholic solvents and mixed solvents containing alcoholic solvents, and is preferably soluble in a mixed solvent of toluene and 2-propanol (toluene 30% by mass, 2-propanol 70% by mass) at 3% by mass or more, particularly preferably 6% by mass or more.
[0096] <<The composition>> The composition of the present invention (hereinafter also referred to as "the composition") contains the above-mentioned compound of the present invention, and is used as a curable composition for preparing a coating liquid for forming a protective layer of the electrophotographic photoreceptor of the present invention, as described below.
[0097] The present composition contains an electron transporting compound containing at least the compound of the present invention, and optionally contains a polymerizable compound not having an electron transporting skeleton, an electron donating compound, a polymerization initiator, inorganic particles, and other materials. In the present invention, the term "composition" refers to a composition that is made up of only solid components that do not contain a solvent. Therefore, the content of each component such as the compound of the present invention in 100 parts by mass of the present composition described below corresponds to the content of each component in 100 parts by mass of the total mass of the protective layer formed using the present composition. The total mass of the protective layer means the total mass of the protective layer after curing, that is, the total mass of the solid content in the coating liquid for forming the protective layer, which will be described later.
[0098] <Electron transport compound> The electron transporting compound contained in the present composition includes at least the compound of the present invention, and may contain an electron transporting compound other than the compound of the present invention as necessary. The composition may contain only one type of the compound of the present invention, or may contain two or more types.
[0099] Examples of the electron transporting compound other than the compound of the present invention include the compounds shown below.
[0100] TIFF2024146328000035.tif173123
[0101] TIFF2024146328000036.tif85123
[0102] As for the electron transporting compounds other than the compound of the present invention, only one type may be contained in the composition, or two or more types may be contained.
[0103] From the viewpoint of electron transportability, the content of the electron transport compound in the composition is preferably 40 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 60 parts by mass or more, relative to 100 parts by mass of the total mass of the composition, while from the viewpoint of the hardness and elastic deformation rate of the protective layer, the content is preferably 90 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 70 parts by mass or less. When the composition contains an electron transporting compound other than the compound of the present invention, from the viewpoint of effectively obtaining the excellent solvent solubility, electrical properties, and mechanical properties due to the compound of the present invention, the content of the compound of the present invention is preferably 40 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 60 parts by mass or more, and may be 100 parts by mass, relative to 100 parts by mass of the total mass of the electron transporting compounds in the composition.
[0104] <Polymerizable Compound Not Having Electron Transporting Skeleton> The present composition may contain a polymerizable compound that does not have an electron transport skeleton. When the present composition contains a polymerizable compound that does not have an electron transport skeleton, the present protective layer described below contains a polymer of a polymerizable compound that does not have an electron transport skeleton. The compound of the present invention has one or more polymerizable functional groups, and therefore can also function as a curable compound. Therefore, even if the composition does not contain a polymerizable compound that does not have an electron transport skeleton, the protective layer can be formed with good curability by the method described below, but by using a polymerizable compound that does not have an electron transport skeleton in addition to the compound of the present invention, the mechanical strength of the protective layer formed can be further sufficient.
[0105] The polymerizable compound without an electron transport backbone may be a compound having a chain polymerizable functional group. Among them, a monomer, oligomer or polymer having a radical polymerizable functional group is preferable. Among them, a curable compound having crosslinking properties, particularly a photocurable compound, is preferable. For example, a curable compound having two or more radical polymerizable functional groups can be mentioned. A compound having one radical polymerizable functional group can also be used in combination.
[0106] The radically polymerizable functional group can include either an acryloyl group (including an acryloyloxy group) or a methacryloyl group (including a methacryloyloxy group), or both of these groups.
[0107] Preferred examples of the curable compound having a radically polymerizable functional group are given below. Examples of monomers having an acryloyl group or a methacryloyl group include trimethylolpropane triacrylate (TMPTA), trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, glycerol triacrylate, tris(acryloxyethyl)isocyanurate, dipentaerythritol hexaacrylate, dimethylolpropane tetraacrylate, pentaerythritol ethoxy tetraacrylate, EO-modified phosphate triacrylate, 2,2,5,5-tetrahydroxymethylcyclopentanone tetraacrylate, 2-hydroxy-3-acryloyloxypropyl methacrylate, polyethylene glycol diacrylate, and the like. acrylate, polypropylene glycol diacrylate, polytetramethylene glycol diacrylate, EO-modified bisphenol A diacrylate, PO-modified bisphenol A diacrylate, 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene, tricyclodecane dimethanol diacrylate, decanediol diacrylate, hexanediol diacrylate, ethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, EO-modified bisphenol A dimethacrylate, PO-modified bisphenol A dimethacrylate, tricyclodecane dimethanol dimethacrylate, decanediol dimethacrylate, hexanediol dimethacrylate, and the like.
[0108] Examples of oligomers and polymers having an acryloyl group or a methacryloyl group include urethane acrylate, ester acrylate, acrylic acrylate, epoxy acrylate, etc. Among these, urethane acrylate and ester acrylate are preferred, and among these, ester acrylate is more preferred.
[0109] The above compounds can be used alone or in combination of two or more kinds.
[0110] A preferred example of a polymerizable compound that does not have an electron transport skeleton is a polyfunctional acrylate compound that does not have an aromatic ring such as a benzene ring, as shown in the following structure. By including such a polyfunctional acrylate compound, the crosslinking property is increased, the hardness of the protective layer is increased, and the mechanical strength is increased, and in addition, the compound of the present invention can be dispersed and crystallization can be suppressed. Crystallization causes leakage current, which is not preferable for a photoreceptor.
[0111] TIFF2024146328000037.tif69170
[0112] When the present composition contains such a polymerizable compound having no electron transport skeleton, the content ratio (mass ratio) of the polymerizable compound to the electron transport compound in the present composition is preferably 1.5 or less, more preferably 1.0 or less, and even more preferably 0.75 or less from the viewpoint of electron transportability, while the content ratio (mass ratio) is preferably 0.2 or more, more preferably 0.3 or more, and even more preferably 0.4 or more from the viewpoint of hardness and elastic deformation rate of the protective layer. The content of the polymerizable compound not having an electron transport skeleton in the present composition corresponds to the content of the polymer in the present protective layer described below.
[0113] <Electron donor compound> The present composition may further contain an electron donating compound. When the present composition contains an electron donating compound, the present protective layer described below contains the electron donating compound.
[0114] In the present invention, the term "electron donating compound" refers to a compound that can donate electrons to the protective layer. In other words, the term "electron donating compound" refers to a compound that can reduce the energy barrier during electron transfer in the target compound (electron transporting compound) in the protective layer by any mechanism, and can inject electrons into the target compound. The mechanism may be, for example, a mechanism in which the electron donating compound directly transfers electrons to the target compound, a mechanism in which the electron donating compound and the target compound form a hydrogen bond to transfer electrons, or a mechanism in which the electron donating compound and the target compound form a hydrogen bond to reduce the energy barrier during electron transfer, and an electron transferred from the photosensitive layer is injected into the target compound present in the protective layer.
[0115] Examples of currently known electron donating compounds include compounds having structures such as triphenylmethane, acridine, amine, amidine, aniline, pyridine, xanthene, benzimidazole, guanidine, and phosphazene. Compounds that will be recognized to have such effects in the future are also included.
[0116] As described above, examples of the electron donating compound include compounds having structures such as triphenylmethane, acridine, amine, amidine, aniline, pyridine, xanthene, benzimidazole, guanidine, and phosphazene. Among them, compounds having a benzimidazole structure or a guanidine structure are preferred from the viewpoint of stability. As the guanidine structure, both a chain guanidine structure and a cyclic guanidine structure can be used, but from the viewpoint of stability, a cyclic guanidine structure is preferred.
[0117] The electron donor compound is preferably a compound having one or more heteroatoms in the molecule, and more preferably a compound having one or more nitrogen atoms (N atoms) in the molecule. From the viewpoint of stability, the number of heteroatoms in one molecule of the electron donor compound is preferably one or more, more preferably two or more, and even more preferably three or more. In addition, from the viewpoint of electron donating ability, the number of nitrogen atoms (N atoms) in one molecule of the electron donor compound is preferably one or more, more preferably two or more, and even more preferably three or more. From the viewpoint of stability, the electron donating compound is preferably a compound having one or more cyclic structures.
[0118] The electron donor compound is preferably an electron donor compound represented by the following formula (4) or (5). These electron donor compounds are activated, for example, when heated to room temperature or higher, and can donate electrons to the protective layer. Specifically, the electron donor compound represented by the following formula (4) is activated when heated to about 80° C. or higher, and can donate electrons to the protective layer. The electron donor compound represented by the following formula (5) is activated when heated to room temperature or higher, and can donate electrons to the protective layer. Thus, for example, when forming a protective layer, these compounds are activated by the temperature rise caused by ultraviolet irradiation, and can donate electrons to the protective layer.
[0119] TIFF2024146328000038.tif65127
[0120] In formula (4), E 1 ~E 4 are each independently preferably a hydrogen atom, a halogen atom, an optionally substituted alkyl group, an optionally substituted thioalkyl group, an optionally substituted thioaryl group, an optionally substituted arylsulfonyl group, an optionally substituted amino group, an optionally substituted alkylamino group, an optionally substituted arylamino group, an optionally substituted hydroxy group, an optionally substituted alkoxy group, an optionally substituted acylamino group, an optionally substituted acyloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted carboxy group, an optionally substituted carboxamido group, an optionally substituted carboalkoxy group, an optionally substituted acyl group, an optionally substituted sulfonyl group, an optionally substituted cyano group, an optionally substituted nitro group, or a derivative of any of these groups. Also, E 1 ~E 4 may be bonded to each other to form a ring.
[0121] In the above formula (4), h is an integer of 0 or more, and from the viewpoint of stability, it is preferably 2 or less, more preferably 1 or less, and even more preferably 0.
[0122] In the above formula (5), g1 is an integer of 1 or more, and from the viewpoint of electrical properties, it is preferably 4 or less, more preferably 3 or less, and even more preferably 2 or less.
[0123] In the above formula (5), Ar is preferably represented by the following formula (6).
[0124] TIFF2024146328000039.tif47120
[0125] In formula (6), * represents G in formula (5). 21 Represents a bond with. G 22 is preferably an alkyl group which may have a substituent, an alkoxy group which may have a substituent, or a halogen atom.
[0126] In formula (6), g2 is an integer of 0 or more, and from the viewpoint of stability, preferably 2 or less, more preferably 1 or less, and most preferably 0.
[0127] G in Equation (5) 21 is preferably a hydrocarbon group which may have a substituent. The number of carbon atoms in the hydrocarbon group is preferably 1 or more, more preferably 3 or more, and is preferably 12 or less, more preferably 10 or less. When g1 is 1, the hydrocarbon group is preferably an alkyl group, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a hexyl group, an octyl group, or a decyl group. When g1 is 2, the hydrocarbon group is preferably an alkylene group, such as a methylene group or an ethylene group.
[0128] From the viewpoint of electrical properties, the content of the electron donor compound in the composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1.0 parts by mass or more, relative to 100 parts by mass of the total composition. On the other hand, from the viewpoint of electrical properties, the content is preferably 25 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 5.0 parts by mass or less, relative to 100 parts by mass of the total composition.
[0129] Specific examples of the electron donating compound are shown below, but the compounds are not limited thereto.
[0130] TIFF2024146328000040.tif150110
[0131] The composition may contain one or more of these electron donor compounds.
[0132] <Polymerization initiator> Examples of the polymerization initiator include a thermal polymerization initiator and a photopolymerization initiator. Examples of the thermal polymerization initiator include peroxide compounds such as 2,5-dimethylhexane-2,5-dihydroperoxide, and azo compounds such as 2,2'-azobis(isobutyronitrile).
[0133] Photopolymerization initiators can be classified into direct cleavage type and hydrogen abstraction type depending on the radical generation mechanism. Direct cleavage photopolymerization initiators generate radicals by cleaving some of the covalent bonds in the molecule when they absorb light energy, whereas hydrogen abstraction photopolymerization initiators generate radicals when the molecule becomes excited by absorbing light energy and abstracts hydrogen from the hydrogen donor.
[0134] Examples of the direct cleavage type photopolymerization initiator include acetophenone or ketal compounds such as acetophenone, 2-benzoyl-2-propanol, 1-benzoylcyclohexanol, 2,2-diethoxyacetophenone, benzyl dimethyl ketal, and 2-methyl-4'-(methylthio)-2-morpholinopropiophenone; benzoin ether compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isobutyl ether, benzoin isopropyl ether, and O-tosylbenzoin; and acylphosphine oxide compounds such as diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and lithium phenyl(2,4,6-trimethylbenzoyl)phosphonate.
[0135] Examples of the hydrogen abstraction type photopolymerization initiator include benzophenone-based compounds such as benzophenone, 4-benzoylbenzoic acid, 2-benzoylbenzoic acid, methyl 2-benzoylbenzoate, methyl benzoylformate, benzyl, p-anisil, 2-benzoylnaphthalene, 4,4'-bis(dimethylamino)benzophenone, 4,4'-dichlorobenzophenone, and 1,4-dibenzoylbenzene; and anthraquinone- or thioxanthone-based compounds such as 2-ethylanthraquinone, 2-isopropylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and 2,4-dichlorothioxanthone. Other examples of the photopolymerization initiator include camphorquinone, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, acridine compounds, triazine compounds, and imidazole compounds.
[0136] In order to efficiently absorb light energy and generate radicals, the photopolymerization initiator preferably has an absorption wavelength in the wavelength region of the light source used for light irradiation. Among them, it is preferable to contain an acylphosphine oxide compound having an absorption wavelength on the relatively long wavelength side. In addition, from the viewpoint of supplementing the curability, it is more preferable to use an acylphosphine oxide compound and a hydrogen abstraction initiator in combination. In this case, the content ratio of the hydrogen abstraction initiator relative to the acylphosphine oxide compound is not particularly limited. From the viewpoint of supplementing the surface curability, it is preferably 0.1 parts by mass or more relative to 1 part by mass of the acylphosphine oxide compound, and from the viewpoint of maintaining the internal curability, it is preferably 5 parts by mass or less.
[0137] In addition, a photopolymerization promoter may be used alone or in combination with the photopolymerization initiator. Examples of photopolymerization promoters include triethanolamine, methyldiethanolamine, ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, (2-dimethylamino)ethyl benzoate, and 4,4'-dimethylaminobenzophenone.
[0138] The polymerization initiator may be used alone or in combination of two or more. The content of the polymerization initiator is 0.5 to 40 parts by mass, preferably 1 to 20 parts by mass, based on 100 parts by mass of the total content having radical polymerizability. The total content having radical polymerizability includes the compound of the present invention and the polymerizable compound not having an electron transport skeleton.
[0139] <Inorganic particles> The composition may contain inorganic particles from the viewpoint of improving the strong exposure characteristics and mechanical strength of the protective layer to be formed, or from the viewpoint of imparting charge transporting ability, although the inorganic particles are not an essential component of the composition of the present invention. In the present invention, by using the compound of the present invention, it is possible to form a protective layer having excellent mechanical strength without the need for containing inorganic particles.
[0140] Examples of the inorganic particles include metal powder, metal oxide, metal fluoride, potassium titanate, and boron nitride. Generally, any inorganic particles that can be used for an electrophotographic photoreceptor can be used. The inorganic particles may be of one type only, or a mixture of a plurality of types of particles.
[0141] <Other ingredients> The composition may contain other materials other than those described above, if necessary. Examples of other materials include stabilizers (heat stabilizers, ultraviolet absorbers, light stabilizers, antioxidants, etc.), dispersants, antistatic agents, colorants, lubricants, etc. These may be used alone or in any ratio and combination of two or more.
[0142] <Method of forming the protective layer> The protective layer is preferably formed from the composition described above. The method for forming the protective layer using the composition will be described below.
[0143] (Coating solution for forming protective layer) The present protective layer can be formed by applying the above-mentioned present composition, i.e., a curable composition containing an electron transporting compound including the compound of the present invention, and optionally containing a polymerizable compound not having an electron transporting skeleton, an electron donating compound, a polymerization initiator, inorganic particles, and other materials, to the present photosensitive layer as a coating liquid in which the composition is dissolved in a solvent or dispersed in a dispersion medium (hereinafter also referred to as "the present protective layer-forming coating liquid"), and curing the coating liquid.
[0144] The content of the electron transport compound including the compound of the present invention in the coating liquid for forming the protective layer is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, per 100 parts by mass of the solvent, from the viewpoints of film uniformity and solubility of the protective layer. The total content of the curable compound in the coating liquid for forming a protective layer, i.e., the compound of the present invention and the polymerizable compound having no electron transport skeleton, is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass, relative to 100 parts by mass of the solvent, from the viewpoint of residual potential, while it is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 1.5 parts by mass or more, from the viewpoint of hardness and elastic deformation rate of the protective layer.
[0145] The contents of other components in the present protective layer-forming coating liquid, i.e., components other than the electron transporting compound and the curable compound contained in the present composition, are similar to the contents of each component in the present composition described above.
[0146] As the solvent used in the present protective layer-forming coating liquid, for example, an organic solvent can be used. Examples of the organic solvent include alcohols such as methanol, ethanol, propanol, and 2-methoxyethanol; ethers such as tetrahydrofuran, 1,4-dioxane, and dimethoxyethane; esters such as methyl formate and ethyl acetate; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; aromatic hydrocarbons such as benzene, toluene, xylene, and anisole; chlorinated hydrocarbons such as dichloromethane, chloroform, 1,2-dichloroethane, 1,1,2-trichloroethane, 1,1,1-trichloroethane, tetrachloroethane, 1,2-dichloropropane, and trichloroethylene; nitrogen-containing compounds such as n-butylamine, isopropanolamine, diethylamine, triethanolamine, ethylenediamine, and triethylenediamine; and aprotic polar solvents such as acetonitrile, N-methylpyrrolidone, N,N-dimethylformamide, and dimethylsulfoxide. Mixed solvents of any combination and ratio among these can also be used. Among these, from the viewpoints of solubility and coatability, alcohols, ethers, aromatic hydrocarbons, and aprotic polar solvents are preferred, alcohols, ethers, and aromatic hydrocarbons are more preferred, alcohols and ethers are even more preferred, and alcohols are most preferred.
[0147] In addition, even if the organic solvent does not dissolve the electron transporting compound used in the protective layer of the photoreceptor of the present invention by itself, it can be used if it can dissolve the compound by mixing it with the above-mentioned organic solvent. In general, the use of a mixed solvent can reduce coating unevenness. When using a dip coating method as the coating method described below, it is preferable to select a solvent that does not dissolve the lower layer. From this viewpoint, it is particularly preferable to include an alcohol.
[0148] The ratio of the solvent to the solid content used in the coating solution for forming a protective layer varies depending on the coating method of the coating solution for forming a protective layer, and may be appropriately changed so as to form a uniform coating film in the coating method to be used.
[0149] (Method of applying the coating solution for forming the protective layer) The method for applying the coating solution for forming the protective layer is not particularly limited, and examples thereof include spray coating, spiral coating, ring coating, and dip coating.
[0150] After forming the coating film by the above coating method, the coating film is dried. In this case, the temperature and time of drying are not important as long as necessary and sufficient drying is obtained. However, if the protective layer is coated only by air drying after the photosensitive layer coating, it is preferable to perform sufficient drying by the method described later in the photosensitive layer forming method.
[0151] (Method of curing the protective layer) The protective layer can be formed by applying the coating solution for forming the protective layer and then curing the coating solution by applying external energy thereto. The external energy used in this case can include heat, light, and radiation.
[0152] Examples of methods for applying heat energy include heating methods using air, gases such as nitrogen, steam, various heat media, infrared rays, and electromagnetic waves. The heating can be performed from the coated surface side or the support side. The heating temperature is preferably 100°C or higher and 170°C or lower.
[0153] As for light energy, UV irradiation light sources that mainly emit light in the ultraviolet (UV) range, such as high-pressure mercury lamps, metal halide lamps, electrodeless lamp bulbs, light-emitting diodes, etc. It is also possible to select a visible light source according to the absorption wavelength of the polymerizable compound or photopolymerization initiator.
[0154] The light irradiation dose was set to 10 J / cm from the viewpoint of curing. 2 More than 15 J / cm is preferable. 2 More preferably, 20 J / cm or more. 2 More preferably, the electric field strength is 400 J / cm or more. 2 Less than 200 J / cm is preferable. 2 Less than 150 J / cm is more preferable. 2 The following is even more preferred: On the other hand, examples of radiation energy include those using electron beams (EB).
[0155] Among these energies, light energy is preferred from the viewpoints of ease of reaction rate control, simplicity of the device, and long pod life.
[0156] After the protective layer is cured, a heating step may be added from the viewpoints of relieving residual stress, relieving residual radicals, and improving electrical properties. The heating temperature is preferably 60° C. or higher, more preferably 100° C. or higher, and is preferably 200° C. or lower, more preferably 150° C. or lower.
[0157] (layer thickness) From the viewpoint of abrasion resistance, the thickness of the protective layer is preferably 0.5 μm or more, more preferably 1 μm or more, and from the viewpoint of electrical properties, the thickness is preferably 5 μm or less, more preferably 4 μm or less. From the same viewpoint, the thickness of the protective layer is preferably 1 / 50 or more of the thickness of the photosensitive layer, more preferably 1 / 40 or more, and even more preferably 1 / 30 or more, while it is preferably 1 / 5 or less, more preferably 1 / 10 or less, and even more preferably 1 / 20 or less.
[0158] <Main photosensitive layer> The photosensitive layer in the photoreceptor of the present invention (hereinafter also referred to as "the present photosensitive layer") may be a layer containing at least a charge generating material (CGM) and a charge transport material.
[0159] The photosensitive layer may be a single-layer type photosensitive layer containing both a charge generating material and a charge transporting material in the same layer, or may be a laminated type photosensitive layer separated into a charge generating layer and a charge transporting layer.
[0160] <Single-layer type photosensitive layer> When the photosensitive layer is a single-layer type photosensitive layer, it is preferable that the layer contains at least a charge generating material (CGM), a hole transporting material (HTM), an electron transporting material (ETM), and a binder resin.
[0161] (Charge generating material) As the charge generating material (CGM) used in the present photosensitive layer, for example, various photoconductive materials such as inorganic photoconductive materials and organic pigments can be used. Among them, organic pigments are particularly preferred, and phthalocyanine pigments and azo pigments are more preferred.
[0162] In particular, when a phthalocyanine pigment is used as the charge generating material, specifically, metal-free phthalocyanine, phthalocyanines coordinated with metals such as copper, indium, gallium, tin, titanium, zinc, vanadium, silicon, germanium, etc., or oxides, halides, etc. thereof are used. Among them, particularly highly sensitive X-type and τ-type metal-free phthalocyanine, A-type, B-type, D-type titanyl phthalocyanine, vanadyl phthalocyanine, chloroindium phthalocyanine, chlorogallium phthalocyanine, hydroxygallium phthalocyanine, etc. are preferred.
[0163] When an azo pigment is used, various known bisazo pigments and trisazo pigments are preferably used.
[0164] The charge generating substance may be used alone or in any combination and ratio of two or more. When two or more charge generating substances are used in combination, the charge generating substances may be mixed after the charge generating substances are mixed, or may be mixed during the production or processing steps of the charge generating substances, such as synthesis, pigmentation, or crystallization.
[0165] From the viewpoint of electrical properties, it is desirable that the particle diameter of the charge generating material is small. Specifically, the particle diameter of the charge generating material is preferably 1 μm or less, more preferably 0.5 μm or less, and the lower limit is 0.01 μm or more. Here, the particle diameter of the charge generating material means the particle diameter in the state in which it is contained in the photosensitive layer.
[0166] The amount of the charge generating material in the single-layer photosensitive layer is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, from the viewpoint of sensitivity, and is preferably 50% by mass or less, more preferably 20% by mass or less, from the viewpoint of sensitivity and chargeability.
[0167] (charge transport material) Charge transport materials are classified into hole transport materials having mainly hole transporting ability and electron transport materials having mainly electron transporting ability. However, when the present photosensitive layer is a single-layer type photosensitive layer, it is preferable that at least a hole transport material and an electron transport material are contained in the same layer.
[0168] (Hole transport material) The hole transport material (HTM) can be selected from known materials and can be used, for example, electron donating materials such as heterocyclic compounds such as carbazole derivatives, indole derivatives, imidazole derivatives, oxazole derivatives, pyrazole derivatives, thiadiazole derivatives, and benzofuran derivatives, aniline derivatives, hydrazone derivatives, arylamine derivatives, stilbene derivatives, butadiene derivatives, and enamine derivatives, as well as compounds in which a plurality of these compounds are bonded, and polymers having groups made of these compounds in the main chain or side chain.
[0169] Among these, carbazole derivatives, arylamine derivatives, stilbene derivatives, butadiene derivatives and enamine derivatives, as well as combinations of a plurality of these compounds, are preferred, with arylamine derivatives and enamine derivatives being more preferred.
[0170] The hole transport material may be used alone or in any combination of two or more kinds in any ratio.
[0171] The amount of the hole transport substance in the single-layer photosensitive layer is preferably 20% by mass or more, more preferably 30% by mass or more, based on 100% by mass of the entire photosensitive layer, from the viewpoint of hole transportability, and is preferably 55% by mass or less, more preferably 45% by mass or less, from the viewpoint of solubility.
[0172] (electron transport material) The electron transport material (ETM) can be selected from known materials. For example, there can be mentioned electron-withdrawing substances such as aromatic nitro compounds such as 2,4,7-trinitrofluorenone, cyano compounds such as tetracyanoquinodimethane, quinone compounds such as diphenoquinone, known cyclic ketone compounds, and perylene pigments (perylene derivatives). Among these, from the viewpoint of electrical properties, quinone compounds and perylene pigments (perylene derivatives) are preferred, and quinone compounds are more preferred. Among the quinone compounds, diphenoquinone or dinaphthylquinone is preferable from the viewpoint of electrical properties, and among them, dinaphthylquinone is more preferable.
[0173] The electron transport material may be used alone or in any combination of two or more kinds in any ratio.
[0174] Preferred examples of the structure of the electron transport material are shown below.
[0175] TIFF2024146328000041.tif49166
[0176] Among the above electron transport materials, ET-2 and ET-5 are preferred from the viewpoint of electrical properties, with ET-2 being more preferred.
[0177] The amount of the electron transport material in the single-layer photosensitive layer is preferably 15% by mass or more, more preferably 25% by mass or more, based on 100% by mass of the entire photosensitive layer, from the viewpoint of electron transportability, and is preferably 40% by mass or less, more preferably 30% by mass or less, from the viewpoint of solubility.
[0178] (binder resin) Examples of the binder resin used in the photosensitive layer include vinyl polymers or copolymers thereof such as polymethyl methacrylate, polystyrene, and polyvinyl chloride; vinyl alcohol resins; polyvinyl butyral resins; polyvinyl formal resins; partially modified polyvinyl acetal resins; polyarylate resins; polyamide resins; polyurethane resins; polycarbonate resins; polyester resins; polyester carbonate resins; polyimide resins; phenoxy resins; epoxy resins; silicone resins; and partially crosslinked cured products thereof. The above resins may be modified with silicon reagents or the like. These may be used alone or in any ratio and combination of two or more.
[0179] The binder resin used in the present photosensitive layer preferably contains one or more types of polymers obtained by interfacial polymerization.
[0180] The binder resin obtained by the above interfacial polymerization is preferably a polycarbonate resin or a polyester resin, more preferably a polycarbonate resin or a polyarylate resin, and more preferably a polymer made from an aromatic diol.
[0181] (Other substances) In addition to the above materials, the photosensitive layer may contain additives such as well-known antioxidants, plasticizers, ultraviolet absorbers, electron-withdrawing compounds, leveling agents, and visible light shielding agents in order to improve film-forming properties, flexibility, coating properties, contamination resistance, gas resistance, and light resistance. The photosensitive layer may also contain various additives such as sensitizers, dyes, pigments (excluding the charge generating materials, hole transport materials, and electron transport materials described above), and surfactants, as necessary. Examples of surfactants include silicone oils and fluorine-based compounds. In the present invention, these may be used alone or in any ratio and combination of two or more of them.
[0182] For the purpose of reducing frictional resistance on the surface of the photosensitive layer, the photosensitive layer may contain a fluorine-based resin, a silicone resin, or the like, and may contain particles made of these resins or particles of an inorganic compound such as aluminum oxide.
[0183] (layer thickness) When the photosensitive layer is a single-layer type photosensitive layer, the thickness of the photosensitive layer is preferably 20 μm or more, more preferably 25 μm or more, from the viewpoint of dielectric breakdown resistance, and is preferably 50 μm or less, more preferably 40 μm or less, from the viewpoint of electrical properties.
[0184] <Laminated photosensitive layer> When the photoreceptor of the present invention is a laminated type photosensitive layer, for example, a structure in which a charge transport layer (CTL) containing a charge transport material is laminated on a charge generation layer (CGL) containing a charge generation material (CGM) can be mentioned. In this case, it is possible to provide layers other than the charge generation layer (CGL) and the charge transport layer (CTL).
[0185] (Charge Generation Layer (CGL)) The charge generating layer (CGL) usually contains a charge generating material (CGM) and a binder resin. The charge generating material (CGM) and the binder resin are the same as those described in the single-layer type photosensitive layer above.
[0186] In addition to the charge generating material and the binder resin, the charge generating layer may contain other components as necessary. For example, known additives such as antioxidants, plasticizers, ultraviolet absorbers, electron-withdrawing compounds, leveling agents, visible light shielding agents, and fillers may be contained in order to improve film-forming properties, flexibility, coating properties, stain resistance, gas resistance, light resistance, etc.
[0187] In the charge generation layer, if the ratio of the charge generation material is too high, the stability of the coating liquid may decrease due to aggregation of the charge generation material, while if the ratio of the charge generation material is too low, the sensitivity of the photoreceptor may decrease, so the compounding ratio (mass) of the charge generation material is preferably 10 parts by mass or more, more preferably 30 parts by mass or more, relative to 100 parts by mass of the binder resin. On the other hand, the compounding ratio (mass) of the charge generation material is preferably 1000 parts by mass or less, more preferably 500 parts by mass or less, relative to 100 parts by mass of the binder resin, and from the viewpoint of film strength, the ratio is more preferably 300 parts by mass or less, and particularly preferably 200 parts by mass or less.
[0188] The thickness of the charge generating layer is preferably 0.1 μm or more, more preferably 0.15 μm or more, and is preferably 10 μm or less, more preferably 0.6 μm or less.
[0189] (Charge transport layer (CTL)) The charge transport layer (CTL) usually contains a charge transport material and a binder resin. The charge transport material and the binder resin are the same as those explained in the single-layer type photosensitive layer.
[0190] In the charge transport layer (CTL), the mixing ratio of the hole transport material (HTM) to the binder resin is preferably 20 parts by mass or more per 100 parts by mass of the binder resin, more preferably 30 parts by mass or more from the viewpoint of reducing the residual potential, and even more preferably 40 parts by mass or more from the viewpoint of stability and charge mobility during repeated use. On the other hand, from the viewpoint of the thermal stability of the photosensitive layer, it is preferable to mix 200 parts by mass or less of the hole transport material (HTM) to 100 parts by mass of the binder resin, more preferably 150 parts by mass or less from the viewpoint of compatibility between the hole transport material (HTM) and the binder resin, and particularly preferably 120 parts by mass or less from the viewpoint of the glass transition temperature.
[0191] In the charge transport layer (CTL), the blending ratio of the electron transport material (ETM) to the binder resin is preferably 20 parts by mass or more per 100 parts by mass of the binder resin, more preferably 30 parts by mass or more from the viewpoint of reducing the residual potential, and even more preferably 40 parts by mass or more from the viewpoint of stability and charge mobility during repeated use. On the other hand, from the viewpoint of the thermal stability of the photosensitive layer, the blending ratio of the electron transport material (ETM) to 100 parts by mass of the binder resin is preferably 200 parts by mass or less, and from the viewpoint of compatibility between the electron transport material (ETM) and the binder resin, more preferably 150 parts by mass or less, and particularly preferably 120 parts by mass or less from the viewpoint of the glass transition temperature.
[0192] The charge transport layer may contain other components as necessary in addition to the electron transport material (ETM), hole transport material (HTM) and binder resin. For example, known additives such as antioxidants, plasticizers, ultraviolet absorbers, electron-withdrawing compounds, leveling agents, visible light shielding agents and fillers may be contained for the purpose of improving film-forming properties, flexibility, coatability, stain resistance, gas resistance, light resistance, etc.
[0193] The thickness of the charge transport layer is not particularly limited, but from the viewpoints of electrical characteristics, image stability, and high resolution, it is preferably from 5 μm to 50 μm, more preferably from 10 μm to 40 μm, and even more preferably from 15 μm to 35 μm.
[0194] <Method of forming the present photosensitive layer> In either the laminated type or the single layer type, the above layers can be formed as follows. The substance to be contained is dissolved or dispersed in a solvent to obtain a coating solution, which is then applied to a conductive support by a known method such as dip coating, spray coating, nozzle coating, bar coating, roll coating, or blade coating, and the layers are then coated and dried in sequence to form a layer. However, the method is not limited to this.
[0195] The solvent or dispersion medium used to prepare the coating liquid is not particularly limited. Specific examples include alcohols, ethers, aromatic hydrocarbons, chlorinated hydrocarbons, etc. In addition, these may be used alone or in any combination of two or more kinds.
[0196] The amount of the solvent or dispersion medium used is not particularly limited. Taking into consideration the purpose of each layer and the properties of the selected solvent or dispersion medium, it is preferable to appropriately adjust the solid content concentration, viscosity, and other physical properties of the coating liquid so that they fall within the desired range. The coating film is preferably dried to the touch at room temperature, and then heated and dried for 1 minute to 2 hours at a temperature in the range of 30° C. to 200° C., either stationary or with a fan. The heating temperature may be constant, or the temperature may be changed during drying.
[0197] <Conductive support> The conductive support of the photoreceptor of the present invention (hereinafter also referred to as "the conductive support") is not particularly limited as long as it supports a layer formed thereon and exhibits electrical conductivity. Examples of the conductive support that can be used include metal materials such as aluminum, aluminum alloys, stainless steel, copper, and nickel; resin materials that have been made conductive by the coexistence of conductive powders such as metal, carbon, and tin oxide; and resins, glass, and paper with conductive materials such as aluminum, nickel, and ITO (indium oxide tin oxide) vapor-deposited or applied to their surfaces. The conductive support may be in the form of a drum, cylinder, sheet, belt, or the like. The conductive support may be a conductive support made of a metal material on which a conductive material having an appropriate resistance value is applied in order to control the conductivity and surface properties or to cover defects.
[0198] When a metal material such as an aluminum alloy is used as the conductive support, the metal material may be provided with an anodized coating before use. The average thickness of the anodic oxide coating is preferably 20 μm or less, and more preferably 7 μm or less. When forming an anodized coating on a metal material, it is preferable to carry out a sealing treatment. The sealing treatment can be carried out by a known method.
[0199] The surface of the conductive support may be smooth, or may be roughened by using a special cutting method, by polishing, or by mixing particles of an appropriate particle size into the material constituting the support.
[0200] <Main undercoat layer> The photoreceptor of the present invention may have an undercoat layer (also referred to as "subsequent undercoat layer") between the present conductive substrate and the present photosensitive layer in order to improve adhesion, blocking properties, and the like.
[0201] The undercoat layer may be made of, for example, a resin, a resin in which organic pigments or particles of metal oxides are dispersed, etc. The undercoat layer may also contain a known antioxidant, etc.
[0202] Examples of organic pigments used in the undercoat layer include phthalocyanine pigments, azo pigments, perylene pigments, etc. Among them, phthalocyanine pigments and azo pigments, specifically, the phthalocyanine pigments and azo pigments used as the charge generating material described above can be mentioned.
[0203] Examples of metal oxide particles used in the present undercoat layer include metal oxide particles containing one type of metal element, such as titanium oxide, aluminum oxide, silicon oxide, zirconium oxide, zinc oxide, iron oxide, etc., and metal oxide particles containing multiple metal elements, such as calcium titanate, strontium titanate, barium titanate, etc. In the undercoat layer, only one type of particle as above may be used, or multiple types of particles may be mixed in any ratio and combination.
[0204] Among the above metal oxide particles, titanium oxide and aluminum oxide are preferred, with titanium oxide being particularly preferred.
[0205] The particle size of the metal oxide particles used in the present undercoat layer is not particularly limited. From the viewpoint of the characteristics of the undercoat layer and the stability of the dispersion liquid for forming the undercoat layer, the average primary particle size is preferably 10 nm or more, and is preferably 100 nm or less, more preferably 50 nm or less.
[0206] The binder resin used in the present undercoat layer may be selected from, for example, polyvinyl acetal resins such as polyvinyl butyral resins; insulating resins such as polyarylate resins, polycarbonate resins, polyester resins, phenoxy resins, acrylic resins, methacrylic resins, polyamide resins, polyurethane resins, epoxy resins, silicone resins, polyvinyl alcohol resins, and styrene-alkyd resins. However, the binder resin is not limited to these polymers. These binder resins may be used alone or in a mixture of two or more kinds, or may be used in a cured form together with a curing agent. Among these, polyvinyl acetal resins, alcohol-soluble copolymerized polyamides, modified polyamides, etc. are preferred because they exhibit good dispersibility and coatability, and among these, alcohol-soluble copolymerized polyamides are particularly preferred.
[0207] The mixing ratio of the particles to the binder resin can be selected arbitrarily, but it is preferable to use it in the range of 10% by mass to 500% by mass from the viewpoint of the stability and coatability of the dispersion.
[0208] The thickness of the undercoat layer can be freely selected, but is preferably 0.1 μm or more and more preferably 20 μm or less in view of the characteristics of the electrophotographic photoreceptor and the coatability of the dispersion.
[0209] <Other layers> The photoreceptor of the present invention may have other layers, if necessary, in addition to the conductive substrate, photosensitive layer, protective layer and undercoat layer described above.
[0210] <Physical Properties of the Photoreceptor of the Present Invention> The photoreceptor of the present invention may have the following physical properties.
[0211] (Martens hardness) In the photoreceptor of the present invention, in order to provide sufficient wear resistance for practical use, the Martens hardness is set to 175 N / mm 2 More preferably, it is 200N / mm 2 Above all, 220N / mm 2 More preferably, it is equal to or greater than this. In the present invention, the Martens hardness of the photoreceptor means the Martens hardness measured from the surface side of the photoreceptor. The Martens hardness can be measured by the method described in the Examples below.
[0212] (Elastic deformation rate) In order to provide the photoreceptor of the present invention with sufficient wear resistance for practical use, its elastic deformation rate, although varying depending on the component composition of the protective layer, is preferably 25% or more, more preferably 30% or more, and even more preferably 40% or more. In the present invention, the elastic deformation rate of the photoreceptor means the elastic deformation rate measured from the surface side of the photoreceptor. The elastic deformation rate can be measured by the method described in the Examples below.
[0213] (residual potential) In the photoreceptor of the present invention, from the viewpoint of providing a residual potential sufficient for practical use, the residual potential, although varying depending on the component composition of the protective layer, is preferably 250 V or less, more preferably 200 V or less, even more preferably 150 V or less, and even more preferably 100 V or less. In the present invention, the residual potential of the photoconductor means the potential of the photoconductor after it has been charged and irradiated with exposure light.
[0214] <<Image forming apparatus of the present invention>> An image forming apparatus (hereinafter, also referred to as "image forming apparatus of the present invention") can be constructed using the photoreceptor of the present invention. However, the image forming apparatus of the present invention described below is one example of an image forming apparatus that can be constructed using the present electrophotographic photoreceptor.
[0215] As shown in FIG. 1, the image forming apparatus of the present invention is configured to include a photoreceptor 1 of the present invention, a charging device 2, an exposure device 3, and a developing device 4, and may further include a transfer device 5, a cleaning device 6, and a fixing device 7 as necessary.
[0216] The photoreceptor 1 of the present invention is not particularly limited as long as it is the photoreceptor of the present invention described above. As an example, Fig. 1 shows a drum-shaped photoreceptor in which the above-mentioned photosensitive layer is formed on the surface of a cylindrical conductive support. A charging device 2, an exposure device 3, a developing device 4, a transfer device 5, and a cleaning device 6 are arranged along the outer circumferential surface of the photoreceptor 1 of the present invention.
[0217] Examples of the charging device 2 include a non-contact corona charging device such as a corotron or scorotron, or a contact-type charging device (direct-type charging device) that charges the photoconductor surface by contacting a charging member to which a voltage is applied. Examples of contact charging devices include a charging roller and a charging brush. Note that FIG. 1 shows a roller-type charging device (charging roller) as an example of the charging device 2.
[0218] The type of exposure device 3 is not particularly limited as long as it can expose the photoreceptor 1 of the present invention to light and form an electrostatic latent image on the photosensitive surface of the photoreceptor 1 of the present invention. Moreover, the exposure may be performed by an internal exposure method of the photoconductor.
[0219] The type of toner T is arbitrary, and in addition to powder toner, polymerized toner produced by a suspension polymerization method, an emulsion polymerization method, or the like can be used.
[0220] The developing device 4 may have any configuration. The developing device 4 shown in Fig. 1 has a configuration in which the toner T is made into a thin layer by a regulating member (developing blade) 45, is triboelectrically charged to a predetermined polarity, and is carried by a developing roller 44 while being transported to contact the surface of the photoconductor 1. However, the configuration is not limited to this. The type of the transfer device 5 is not particularly limited, and any device using any method, such as electrostatic transfer methods such as corona transfer, roller transfer, and belt transfer, pressure transfer, and adhesive transfer, can be used.
[0221] There is no particular limitation on the cleaning device 6. For example, any cleaning device can be used, such as a brush cleaner, a magnetic roller cleaner, a blade cleaner, etc. If there is little or almost no toner remaining on the photoreceptor surface, the cleaning device 6 may not be necessary. The fixing device 7 may also have any configuration. In addition to the above-mentioned configuration, the image forming apparatus may be configured to perform, for example, a charge removal process.
[0222] Furthermore, the image forming apparatus may be further modified, for example, to be configured to perform processes such as a pre-exposure process and an auxiliary charging process, to be configured to perform offset printing, or even to be configured as a full-color tandem system using multiple types of toner.
[0223] <<Cartridge of the present invention>> The photoreceptor 1 of the present invention can be combined with one or more of a charging device 2, an exposure device 3, a developing device 4, a transfer device 5, a cleaning device 6, and a fixing device 7 to form an integrated cartridge (referred to as the "cartridge of the present invention"). However, the cartridge of the present invention described below is one example of an electrophotographic cartridge that can be constructed using the present electrophotographic photoreceptor.
[0224] The cartridge of the present invention can be configured to be detachable from the main body of an electrophotographic device such as a copying machine, a laser beam printer, etc. In that case, for example, when the photoreceptor 1 of the present invention or other members deteriorate, the electrophotographic photoreceptor cartridge can be removed from the main body of the image forming device and a new electrophotographic photoreceptor cartridge can be mounted in the main body of the image forming device, thereby facilitating the maintenance and management of the image forming device.
[0225] <<Explanation of terms>> In the present invention, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In addition, when it is expressed as "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the intention that "greater than X is preferable" or "less than Y is preferable." EXAMPLES
[0226] Hereinafter, the embodiment of the present invention will be described in more detail with reference to examples. However, the following examples are provided to explain the present invention in detail, and the present invention is not limited to the examples shown below, and can be modified as desired without departing from the gist of the present invention. In the following examples and comparative examples, the term "parts" refers to "parts by mass" unless otherwise specified.
[0227] As used herein, DMF means N,N-dimethylformamide and MEHQ means 4-methoxyphenol.
[0228] [Synthesis of compounds] The synthesis methods of compounds 1 and 2 of the present invention and comparative compounds 1 to 4 will be described below.
[0229] <Synthesis of Compound 1> The synthesis scheme of compound 1 is shown below.
[0230] TIFF2024146328000042.tif106170
[0231] The synthesis procedure for compound 1 is shown below.
[0232] (Synthesis of Intermediate 1-1) Under a nitrogen atmosphere, 5,6,12,13-Tetrachloroperylo[3,4-cd:9,10-c'd']dipyran-1,3,8,10-tetrone (13.0 g, 24.5 mmol) and L-(+)-leucinol (7.2 g, 61.3 mmol) were added to 200 mL of toluene and stirred at 110 ° C for 9 hours. After cooling to room temperature, this solution was poured into 200 mL of ice water, and 1N hydrochloric acid was added to make the reaction solution acidic. Extraction was performed with toluene and tetrahydrofuran, and the organic layer was washed with water and then dried over magnesium sulfate. The obtained solid was filtered, the solvent of the filtrate was distilled off under reduced pressure, and the residue was dried to obtain intermediate 1-1 (yield 11.8 g, yield 66% by mass).
[0233] (Synthesis of Compound 1) Under a nitrogen atmosphere, 70 mL of dehydrated dichloromethane was added to intermediate 1-1 (5.1 g, 6.93 mmol), and 2-(acryloyloxy)ethyl isocyanate (2.5 g, 17.3 mmol) was added dropwise. 0.1 mL of dibutyltin dilaurate was added and stirred at room temperature for 12 hours. The reaction solution was poured into 200 mL of water, extracted with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The obtained solid was filtered, the solvent of the filtrate was distilled off under reduced pressure, and the residue was subjected to silica gel column chromatography to obtain compound 1 (yield 2.3 g, yield 33% by mass).
[0234] <Synthesis of compound 2> The synthesis scheme of compound 2 is shown below.
[0235] TIFF2024146328000043.tif80170
[0236] The synthesis procedure for compound 2 is shown below.
[0237] (Synthesis of intermediate 2-1) Under a nitrogen atmosphere, 150 mL of N,N-dimethylformamide was added to naphthalene-1,4,5,8-tetracarboxylic dianhydride (4.5 g, 16.9 mmol) and L-(+)-leucinol (4.4 mL, 33.7 mmol), and the mixture was stirred at 150° C. for 6 hours. After cooling to room temperature, the solution was poured into 200 mL of ice water, and 1N hydrochloric acid was added to make the solution acidic. Extraction was performed with ethyl acetate, and the organic layer was washed with water, dried over magnesium sulfate, and the obtained solid was filtered. The solvent of the filtrate was distilled off under reduced pressure, and the residue was dried to obtain intermediate 2-1 (yield 7.8 g, yield 99% by mass).
[0238] (Synthesis of compound 2) Under a nitrogen atmosphere, 100 mL of dehydrated dichloromethane was added to intermediate 2-1 (5.3 g, 11.4 mmol), and 2-(acryloyloxy)ethyl isocyanate (4.8 g, 34.1 mmol) was added dropwise. 0.1 mL of dibutyltin dilaurate was added and stirred at room temperature for 12 hours. The reaction solution was poured into 200 mL of water, extracted with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The obtained solid was filtered, the solvent of the filtrate was distilled off under reduced pressure, and the residue was subjected to silica gel column chromatography to obtain compound 2 (yield 3.9 g, yield 46% by mass).
[0239] <Synthesis of Comparative Compound 1> The synthesis scheme of comparative compound 1 is shown below.
[0240] TIFF2024146328000044.tif109170
[0241] The synthesis procedure for comparative compound 1 is shown below.
[0242] (Synthesis of intermediate C1-1) Under a nitrogen atmosphere, 200 mL of dehydrated dichloromethane was added to mono(2-acryloyloxyethyl) succinate (21.7 g, 100.4 mmol) and cooled on ice. Oxalyl chloride (11.2 mL, 130.5 mmol) was added dropwise, and the mixture was stirred for 1 hour under ice cooling and then stirred at room temperature for 12 hours. The solvent in the reaction solution was distilled off under reduced pressure, and the residue was dried to obtain intermediate C1-1 (yield 23 g, 97% by mass).
[0243] (Synthesis of intermediate C1-2) Under a nitrogen atmosphere, 3,4,9,10-perylenetetracarboxylic dianhydride (11.4 g, 29.0 mmol), zinc acetate (5.32 g, 29.0 mmol), 50 g of imidazole, and L-(+)-leucinol (8.5 g, 72.5 mmol) were mixed and stirred at 160 ° C for 7 hours. After cooling to room temperature, the mixture was dissolved in dichloromethane, and the solution was poured into 200 mL of ice water, and 1N hydrochloric acid was added to make the reaction solution acidic. Extraction was performed with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The obtained solid was filtered, the solvent of the filtrate was distilled off under reduced pressure, and the residue was subjected to silica gel column chromatography to obtain intermediate C1-2 (yield 12.0 g, yield 70 mass%).
[0244] (Synthesis of Comparative Compound 1) Under a nitrogen atmosphere, 100 mL of dehydrated dichloromethane and triethylamine (1.5 mL, 10.8 mmol) were added to intermediate C1-2 (1.6 g, 2.71 mmol) and cooled on ice. Intermediate C1-1 (1.4 g, 5.96 mmol) dissolved in 10 mL of dehydrated dichloromethane was added dropwise, stirred for 1 hour under ice cooling, and stirred for 1 hour at room temperature. The reaction solution was poured into 100 mL of water, extracted with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The obtained solid was filtered, the solvent of the filtrate was distilled off under reduced pressure, and the residue was subjected to silica gel column chromatography to obtain comparative compound 1 (yield 2.3 g, yield 85% by mass).
[0245] <Synthesis of Comparative Compound 2> The synthesis scheme of comparative compound 2 is shown below.
[0246] TIFF2024146328000045.tif46170
[0247] The synthesis procedure for comparative compound 2 is shown below.
[0248] (Synthesis of Comparative Compound 2) Under a nitrogen atmosphere, 3,4,9,10-perylenetetracarboxylic dianhydride (2.62 g, 6.69 mmol), zinc acetate (0.92 g, 5.02 mmol), imidazole 10 g, and tridecane-7-amine (4.00 g, 20.1 mmol) were mixed and stirred at 160 ° C for 5 hours. After cooling to room temperature, the mixture was dissolved in dichloromethane, and the solution was poured into 200 mL of ice water, and 1N hydrochloric acid was added to make the reaction solution acidic. Extraction was performed with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The obtained solid was filtered, the solvent of the filtrate was distilled off under reduced pressure, and the residue was subjected to silica gel column chromatography to obtain comparative compound 2 (yield 4.2 g, yield 83 mass%).
[0249] <Synthesis of Comparative Compound 3> The synthesis scheme of comparative compound 3 is shown below.
[0250] TIFF2024146328000046.tif55170
[0251] The synthesis procedure for comparative compound 3 is shown below.
[0252] (Synthesis of Comparative Compound 3) Under a nitrogen atmosphere, 50 mL of dehydrated dichloromethane and triethylamine (5.1 mL, 36.8 mmol) were added to intermediate 2-1 (4.3 g, 9.21 mmol) and cooled on ice. Intermediate C1-1 (4.8 g, 20.3 mmol) dissolved in 50 mL of dehydrated dichloromethane was added dropwise, and the mixture was stirred for 1 hour under ice cooling and at room temperature for 1 hour. The reaction solution was poured into 100 mL of water, extracted with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The obtained solid was filtered, the solvent of the filtrate was distilled off under reduced pressure, and the residue was subjected to silica gel column chromatography to obtain comparative compound 3 (yield 3.5 g, yield 45% by mass).
[0253] <Synthesis of Comparative Compound 4> The synthesis scheme of comparative compound 4 is shown below.
[0254] TIFF2024146328000047.tif68170
[0255] The synthesis procedure for comparative compound 4 is shown below.
[0256] (Synthesis of intermediate C4-1) Under a nitrogen atmosphere, 100 mL of dehydrated dichloromethane was added to [2-(2-methoxyethoxy)ethoxy]acetic acid (6.3 g, 35.3 mmol) and cooled on ice. 0.5 mL of N,N-dimethylformamide was added to this solution, and then oxalyl chloride (6.1 mL, 70.7 mmol) was added dropwise, and the mixture was stirred for 1 hour under ice cooling and then stirred at room temperature for 12 hours. After the solvent was distilled off under reduced pressure, the residue was dried to obtain intermediate C4-1 (yield 6.9 g, 99% by mass).
[0257] (Synthesis of Comparative Compound 4) Under a nitrogen atmosphere, 200 mL of dehydrated dichloromethane and triethylamine (25.0 mL, 180.6 mmol) were added to intermediate 1-1 (21.9 g, 30.1 mmol) and cooled on ice. Intermediate C4-1 (17.8 g, 90.4 mmol) dissolved in 50 mL of dehydrated dichloromethane was added dropwise, and the mixture was stirred for 1 hour under ice cooling and for 12 hours at room temperature. The reaction solution was poured into 100 mL of water, extracted with dichloromethane, and the organic layer was washed with water and then dried over magnesium sulfate. The obtained solid was filtered, the solvent of the filtrate was distilled off under reduced pressure, and the residue was subjected to silica gel column chromatography to obtain comparative compound 4 (yield 11.8 g, yield 37% by mass).
[0258] [Evaluation of solubility in organic solvents] Compounds 1 to 2 or comparative compounds 1 to 4 were added to a mixed solvent of toluene / 2-propanol = 3 / 7 (mass ratio) at room temperature (25 ° C.) so as to have a concentration of 6 mass %, and the mixture was stirred for 10 minutes with a rotor without heating or cooling. Thereafter, the state of dissolution was visually observed, and the solubility was evaluated according to the following criteria. If any insoluble residue was observed, the sample was heated in a water bath at a constant temperature (40°C) for 10 minutes, and the state of dissolution was visually observed again to evaluate the solubility. "◎" or "○" was determined to indicate excellent solubility in organic solvents. The evaluation results are shown in Table 1.
[0259] A: Completely dissolved at room temperature. ◯: A small amount of undissolved material was observed at room temperature, but it was completely dissolved when heated at 40°C for less than 10 minutes. △: Some of the material remained undissolved at room temperature, but was completely dissolved when heated at 40°C for 10 minutes or more. ×: Even after heating at 40°C for 10 minutes or more, some of the material remained undissolved.
[0260] Next, an electrophotographic photoreceptor was prepared by the following method, and the residual potential, hardness and elastic deformation rate were evaluated by the following methods. The evaluation results are shown in Table 1.
[0261] [Preparation of electrophotographic photoreceptor] <Preparation of Coating Solution P1 for Forming Undercoat Layer> 20 parts of D-type titanyl phthalocyanine, which shows a clear peak at a diffraction angle 2θ=27.3°±0.2° in powder X-ray diffraction using CuKα radiation, was mixed with 280 parts of 1,2-dimethoxyethane, and ground for 2 hours in a sand grinding mill to perform a fine dispersion treatment. 400 parts of a 1,2-dimethoxyethane solution containing 2.5% by mass of polyvinyl butyral (manufactured by Denki Kagaku Kogyo Co., Ltd., product name "Denka Butyral" #6000C) and 170 parts of 1,2-dimethoxyethane were further added and mixed to prepare a coating solution P1 for forming an undercoat layer with a solid content concentration of 3.4% by mass.
[0262] <Preparation of Coating Solution Q1 for Forming Single-Layer Photosensitive Layer> In powder X-ray diffraction using CuKα radiation, 2.6 parts of D-type titanyl phthalocyanine exhibiting a clear peak at a diffraction angle 2θ=27.3°±0.2°, 11.3 parts of a perylene pigment having the following structure, 0.5 parts of a polyvinyl butyral resin, 90 parts of the following hole transport material (HTM48, molecular weight 748), 70 parts of the following electron transport material (ET-2, molecular weight 424.2), 100 parts of a polycarbonate resin having a biphenyl structure, 0.05 parts of a silicone oil (manufactured by Shin-Etsu Silicones: product name KF-96) as a leveling agent, and 793.35 parts of a mixed solvent of tetrahydrofuran (hereinafter appropriately abbreviated as THF) and toluene (hereinafter appropriately abbreviated as TL) (THF 90% by mass, TL 10% by mass) were mixed to prepare a single-layer type photosensitive layer forming coating solution Q1 with a solid content concentration of 25% by mass.
[0263] TIFF2024146328000048.tif116170
[0264] <Preparation of Coating Solutions S1 to S8 for Forming Protective Layer> The curable compound (polymerizable compound not having an electron transport skeleton) shown in Table 1, the electron donor compound shown in Table 1, and the electron transport compound shown in Table 1 were used in the amounts shown in Table 1 to obtain protective layer-forming coating solutions S1 to S8 (solid concentration approximately 8.0% by mass), each of which had a solvent composition of toluene / 2-propanol = 3 / 7 (mass ratio). The symbols of the curable compounds and electron donor compounds in Table 1 represent the following. Curable compound: A-DPH (dipentaerythritol polyacrylate, product name "NK Ester A-DPH", manufactured by Shin-Nakamura Chemical Co., Ltd.) Curable compound: M9050 (Toagosei Co., Ltd. polyester acrylate product name "Aronix M-9050")
[0265] Electron donor compound: N-DMBI (N,N-dimethylbenzylamine, manufactured by Tokyo Chemical Industry Co., Ltd.)
[0266] [Examples 1 to 4, Comparative Examples 1 to 4] In Examples 1 to 4 and Comparative Examples 1 to 4, photoreceptors A1 to A8 were produced using the above-mentioned Compounds 1 and 2 and Comparative Compounds 1 to 4, and evaluated.
[0267] <Preparation of Single-Layer Photoreceptors A1 to A8> A single-layer photoreceptor was prepared according to the following procedure. An aluminum cylinder with a diameter of 30 mm and a length of 244 mm, the surface of which had been machined, was dip-coated with coating solution P1 for forming an undercoat layer, so that an undercoat layer was formed with a film thickness of 0.3 μm after drying. Onto the undercoat layer, coating solution Q1 for forming a single-layer type photosensitive layer was dip-coated, and dried at 100° C. for 24 minutes, so that a single-layer type photosensitive layer was formed with a film thickness of 32 μm after drying. Each of coating solutions S1 to S8 for forming a protective layer was ring-coated on the single-layer type photosensitive layer, and immediately after coating, 0.9 W / cm 365 nm LED light was applied while rotating the photoreceptor at 60 rpm under a nitrogen atmosphere. 2 By irradiating the photosensitive layer with an intensity of 1.0 μm for 1 minute, a protective layer was formed so that the thickness after curing would be 3.0 μm, thereby preparing photoreceptors A1 to A8, respectively.
[0268] [Measurement of Martens hardness and elastic deformation rate] The obtained photoreceptors A1 to A8 were measured from the surface side of the photoreceptor using a microhardness tester (Fischer: FISCHERSCOPE HM2000) under an environment of a temperature of 25° C. and a relative humidity of 50% under the following measurement conditions.
[0269] <Martens hardness and elastic deformation rate measurement conditions> Indenter: Vickers square pyramid diamond indenter with facing angle of 136° Maximum pressing load: 0.2mN Load time: 10 seconds Unloading time: 10 seconds
[0270] The Martens hardness is calculated according to the following formula. Martens hardness (N / mm 2 ) = Maximum indentation load / Indentation area at maximum indentation load
[0271] The elastic deformation rate is a value defined by the following formula, and is the ratio of the work performed by the membrane due to its elasticity when removing the load to the total work required for pressing. Elastic deformation rate (%) = (We / Wt) x 100 In the above formula, the total work load Wt (nJ) indicates the area enclosed by ABDA in Figure 2, and the elastic deformation work load We (nJ) indicates the area enclosed by CBDC. The larger the elastic deformation rate, the less likely deformation will remain due to the load, and an elastic deformation rate of 100 means that no deformation will remain.
[0272] In the present invention, the Martens hardness (shown as "hardness" in Table 1) is 220 N / mm 2 Anything above this was rated as "pass," and an elastic deformation rate of 40% or more was rated as "pass."
[0273] [Measurement of potential holding rate] The photoreceptors A1 to A8 obtained in the examples and comparative examples were attached to an electrophotographic property evaluation device manufactured in accordance with the measurement standard of the Society of Electrophotography (described in "Continued Fundamentals and Applications of Electrophotographic Technology," edited by the Society of Electrophotography, Corona Publishing, pp. 404-405), and the potential retention rate after a cycle of charging, exposure, potential measurement, and static elimination was measured as follows. To evaluate the electrical characteristics, the potential retention rate (%) was measured after charging to +700 V and leaving for 5 seconds. The measurement was performed in an environment of a temperature of 25°C and a relative humidity of 50% (N / N environment). The potential retention rate is shown in Table 1. The potential retention rate indicates the surface potential retention rate (%) when the photoconductor with a charged surface is left for a certain period of time. A higher surface potential retention rate (%) is better because the potential is maintained even over time and the charging properties are good, so it can be said to be a good result. In the present invention, a potential retention rate of 75% or more was deemed "pass."
[0274] [Table 1]
[0275] From Table 1, it was confirmed that Compounds 1 and 2 have excellent solubility in organic solvents. It is presumed that all of the compounds of the examples have high affinity with organic solvents and good solubility due to the presence of a urethane bond (particularly the NH moiety). It was also confirmed that the solubility is further improved when the side chain having the urethane bond is branched.
[0276] It was confirmed from Table 1 that the electrophotographic photoreceptors of Examples 1 to 4 using Compounds 1 and 2 as protective layer-forming materials had a high potential retention rate and excellent mechanical strength such as hardness and elastic deformation rate. Since each of the compounds 1 and 2 has a urethane bond (particularly the NH portion), it has high affinity with the organic solvent used in the coating solution for forming the protective layer and has good solubility, so that the coating solution has good applicability and a uniform protective layer can be formed without unevenness. This is believed to improve the electron transport property in the protective layer and improve the potential retention rate of the photoconductor. Furthermore, all of the compounds 1 and 2 have a polymerizable functional group and can be crosslinked with the curable compound in the protective layer, so that the mechanical strength (hardness, elastic deformation rate) of the protective layer becomes good. Each of Compounds 1 and 2 enhances charge injection from the photosensitive layer to the protective layer and charge mobility to the outermost surface through the electron transport skeleton, and can provide an electrophotographic photoreceptor excellent in electrical properties such as potential retention. In addition, since all of compounds 1 and 2 have one or more polymerizable functional groups, they can be polymerized with the curable compound in the protective layer, and it is believed that the mechanical strength (hardness, elastic deformation rate) of the protective layer was also sufficient. Therefore, as described above, when the protective layer of the photoreceptor contains a polymer of a compound represented by the above formula (1) and having at least one group represented by the following formula (1A) and at least one polymerizable functional group in one molecule, the protective layer can have excellent electrical properties such as potential holding ratio, mechanical properties such as hardness and elastic deformation rate, and further, the electron transport compound used in forming the protective layer has excellent solubility in organic solvents. [Explanation of symbols]
[0277] 1. Photoconductor (electrophotographic photoconductor) 2 Charging device (charging roller; charging section) 3 Exposure equipment (exposure section) 4. Developing device (developing section) 5. Transcription device 6 Cleaning device 7 Fixing device 41 Developer tank 42 Agitator 43 Supply roller 44 Developing roller 45 Regulatory Materials 71 Upper fixing member (pressure roller) 72 Lower fixing member (fixing roller) 73 Heating device T Toner P Recording paper (paper, medium) < / n> < / x>
Claims
1. An electrophotographic photoreceptor having at least a photosensitive layer and a protective layer in this order on a conductive support, The protective layer of the electrophotographic photoreceptor contains a polymer of a compound represented by the following formula (1) and having at least one group represented by the following formula (1A) and at least one polymerizable functional group in one molecule. In formula (1), X represents an n-valent electron transport skeleton. A is a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, a group represented by the following formula (2), or a group represented by the following formula (1B). n represents an integer of 1 or more. When n is 1, A is a group represented by the following formula (2) or a group represented by the following formula (1B). When A is a group represented by the following formula (2), R 1 and R 2 At least one of the groups represented by the following formula (1B) is a group represented by the following formula (1B): 1 and L 2 At least one of A is a group represented by the following formula (1A). At least one of Z is a polymerizable functional group. When A is a group represented by the following formula (1B), R 3 is a polymerizable functional group. When n is 2 or more, the multiple A's may be the same or different from each other, and at least one of the multiple A's is a group represented by the following formula (2) or a group represented by the following formula (1B). When A is a group represented by the following formula (2), R 1 and R 2 At least one of the groups represented by the following formula (1B) is a group represented by the following formula (1B): 1 and L 2 At least one of the A's is a group represented by the following formula (1A). In addition, the A's or at least one other A's contains at least one polymerizable functional group in the structure. In formula (2), * represents a bond to X. R 1 and R 2 each independently represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, or a group represented by the following formula (1B): L 1 and L 2 each independently represents a direct bond, a divalent group, or a group represented by the following formula (1A): Z represents a hydrogen atom, an alkoxy group, an amide group, or a polymerizable functional group, provided that x1+y1=3, where x1 is an integer of 0 to 2, y1 is an integer of 1 to 3, x2+y2=3, where x2 is an integer of 0 to 2, y2 is an integer of 1 to 3, and x1 is an integer of 2 or more; 1 may be the same or different from each other, and when y1 is an integer of 2 or more, R 2、 x2, y2, L 1、 L 2 and Z may be the same or different from each other, and when x2 is an integer of 2 or more, R 2 may be the same or different, and when y2 is an integer of 2 or more, L 2 and Z may be the same or different from each other. (In formula (1B), * represents a bond to any atom in formula (1) or (2), and B 1 and B 2 R each independently represents a direct bond or a divalent group. 3 represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted heteroaryloxy group, an optionally substituted alkoxycarbonyl group, an optionally substituted dialkylamino group, an optionally substituted diarylamino group, an optionally substituted arylalkylamino group, an optionally substituted acyl group, an optionally substituted haloalkyl group, an optionally substituted alkylthio group, an optionally substituted arylthio group, an optionally substituted silyl group, an optionally substituted siloxy group, an optionally substituted aromatic hydrocarbon group, an optionally substituted aromatic heterocyclic group, or a polymerizable functional group. (In formula (1A), B 1 and B 2 each independently represents a direct bond or a divalent group, and * represents a bond to any atom in formula (1).
2. 2. The electrophotographic photoreceptor according to claim 1, wherein in formula (1), X is represented by formula (3) or (4). (In formulas (3) and (4), G 1 ~G 12 each independently represents a hydrogen atom, a deuterium atom, a halogen atom, an alkyl group which may have a substituent, or an alkoxy group which may have a substituent, and * represents a bond to A.
3. 3. The electrophotographic photoreceptor according to claim 1, wherein at least one A in the formula (1) is a group represented by the formula (2).
4. In the formula (2), L 1 and L 2 The electrophotographic photoreceptor according to claim 3 , wherein at least one of the above is a group represented by formula (1A).
5. 3. The electrophotographic photoreceptor according to claim 1, wherein the compound represented by formula (1) has at least two polymerizable functional groups in one molecule.
6. 3. The electrophotographic photoreceptor according to claim 1, wherein the polymerizable functional group is selected from the following formulae (M1) to (M7): (In formulas (M1) to (M7), R 110 represents a hydrogen atom or an alkyl group which may have a substituent, and * represents the bonding position.
7. In the formula (2), R 1 3. The electrophotographic photoreceptor according to claim 1, wherein is an alkyl group which may have a substituent.
8. 3. The electrophotographic photoreceptor according to claim 1, wherein the protective layer further contains a polymer of a polymerizable compound having no electron transport skeleton.
9. 3. The electrophotographic photoreceptor according to claim 1, wherein the protective layer further contains an electron donating compound.
10. 3. An electrophotographic photoreceptor cartridge comprising the electrophotographic photoreceptor according to claim 1.
11. 3. An image forming apparatus comprising the electrophotographic photoreceptor according to claim 1.
Citation Information
Patent Citations
Photo conductor overcoat comprising radical polymerizable charge transport molecules and hexa-functional urethane acrylates
US9417538B2
Electrophotographic photoreceptor, image forming apparatus, and method for image formation
WO2010035683A1