Alumina-based composite oxide and method for producing alumina-based composite oxide
The alumina-based composite oxide with controlled element distribution addresses the issue of catalyst agglomeration by ensuring high affinity support and diffusion barriers, maintaining catalyst activity and stability at high temperatures.
Patent Information
- Application Number
- JP2023059185
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing alumina-containing composite oxides used as catalyst supports face challenges in suppressing agglomeration of catalytic metal elements at high temperatures due to uniform element distribution, leading to inactivity and potential agglomeration of metal catalysts over time.
The development of an alumina-based composite oxide with controlled element distribution, characterized by specific variations in alumina and other oxide content within tertiary particles, ensuring high affinity support for metal catalysts and acting as diffusion barriers to prevent agglomeration and maintain catalyst activity.
The controlled element distribution in the alumina-based composite oxide effectively suppresses agglomeration of metal catalysts at high temperatures, maintaining their active state and preventing deterioration, thereby enhancing catalytic activity and stability.
Smart Images

Figure 2024146344000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an alumina-based composite oxide and a method for producing an alumina-based composite oxide. [Background technology]
[0002] As has been incorporated into recent exhaust gas regulation modes, the exhaust gas temperature rises significantly when driving at high speeds and ultra-high speeds. As a result, the operating temperature of exhaust gas purification catalysts has also risen significantly compared to conventional methods, making it difficult to suppress the aggregation of catalytic metal elements due to sintering.
[0003] Patent Document 1 discloses a composite metal oxide porous body useful as a catalyst support, which is a mixture of first ultrafine particles containing alumina and second ultrafine particles containing zirconia, in which the first ultrafine particles and the second ultrafine particles are uniformly dispersed so as to satisfy the condition that, for all metal elements contained in the porous body at 0.1 mass % or more, the content (mass %) of the metal elements is measured at 100 measurement points in a microanalysis area of 20 nm square by energy dispersive X-ray spectroscopy using a scanning transmission electron microscope with a spherical aberration correction function, and the standard deviation of the content of each metal element obtained is 10 or less (see claim 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2011 / 030875 Summary of the Invention [Problem to be solved by the invention]
[0005] Conventionally, in alumina-containing composite oxides for supporting catalytic metal elements, materials having a uniform element distribution have been used in order to suppress aggregation of the catalytic metal elements when exposed to high temperature regions for long periods of time, as exemplified in Patent Document 1.
[0006] However, the inventors have found that if the element distribution in the alumina-containing composite oxide is extremely uniform, there is a possibility that the metal catalyst element will aggregate on elements of the alumina-containing composite oxide that tend to become inactive when exposed to high temperatures for a long period of time.
[0007] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide an alumina-containing composite oxide capable of suppressing aggregation of catalytic metal elements when exposed to a high temperature range for a long period of time, and a method for producing the alumina-based composite oxide capable of obtaining the alumina-based composite oxide. [Means for solving the problem]
[0008] In order to solve the above-mentioned problems, the present inventors have conducted extensive research into alumina-containing composite oxides, and have found that it is possible to more effectively suppress the aggregation of catalytic metal elements when exposed to high temperatures for a long period of time by appropriately controlling the element distribution of the alumina-containing composite oxide with high precision, thereby completing the present invention.
[0009] That is, the present invention provides the following. [1] Alumina, Ceria and / or zirconia Contains An alumina-based composite oxide characterized by satisfying all of the following (1) to (4) in point analysis of a total of 50 points by energy dispersive X-ray spectroscopy according to the following procedures a to c: (1) There is at least one measurement point out of 50 points where the alumina content is 50% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 50% by mass or less, (2) There is at least one measurement point out of 50 where the alumina content is 1% by mass or more and less than 50% by mass, and the content of oxides of elements other than alumina is more than 50% by mass and less than 99% by mass, (3) The difference between the maximum and minimum alumina content of 50 measurement points is 20 or more and 95 or less, (4) The difference between the maximum and minimum contents of oxides of elements other than alumina at 50 measurement points is 20 or more and 95 or less. <Procedure> a: From the particle images observed with a scanning electron microscope, one particle image having a cross section of 4 μm or more in length and 4 μm or more in width is selected. b: Composition analysis is performed at 25 measurement points spaced 1 μm apart within an area of 4 μm vertically and 4 μm horizontally of the selected particle image. c: Select another particle image different from the one selected in step a and perform the same composition analysis as in step b.
[0010] According to the above-mentioned configuration, in the particle having a cross section of 4 μm or more in length and 4 μm or more in width, there is a variation in the element distribution that satisfies the above (1) to (4). That is, in the tertiary particles constituting the alumina-based composite oxide, there is a certain degree of variation in the element distribution. Therefore, when the metal catalyst element is supported on the alumina-based composite oxide, the metal catalyst element is supported preferentially on the element with high affinity. When the affinity with the support is high, even when exposed to a high temperature range for a long time, the aggregation of the metal catalyst elements is suppressed due to the anchor effect, etc., and the metal catalyst is maintained in a more active state. In addition, there are many cases where an element with high affinity with the metal catalyst element acts as a promoter. Therefore, by preferentially supporting the metal catalyst element near the promoter, it is expected that the catalytic activity will be improved. In addition, since the alumina and the added metal element are present in the same tertiary particle, when exposed to a high temperature range for a long time, the alumina and the added metal element act as diffusion barriers to each other, and the deterioration of the catalyst is suppressed.
[0011] Furthermore, the present invention provides the following: [2] The alumina-based composite oxide according to [1], which further satisfies all of the following (5) to (6) in the point analysis of the 50 points: (5) There is at least one measurement point out of 50 where the alumina content is 55% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 45% by mass or less, (6) There is at least one measurement point out of 50 where the alumina content is between 1% by mass and 45% by mass, and the content of oxides of elements other than alumina is between 55% by mass and 99% by mass.
[0012] If there is variation within the tertiary particles constituting the alumina-based composite oxide that satisfies not only the above (1) to (4) but also the above (5) to (6), aggregation of the metal catalyst element is further suppressed.
[0013] Furthermore, the present invention provides the following: [3] The alumina-based composite oxide according to [1], which further satisfies all of the following (7) to (8) in the point analysis of the 50 points: (7) There are 10 or more measurement points out of 50 points in which the alumina content is 50% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 50% by mass or less, (8) There are 10 or more measurement points out of 50 where the alumina content is 1 mass% or more and less than 50 mass%, and the content of oxides of elements other than alumina is more than 50 mass% and 99 mass% or less.
[0014] According to the invention [3] above, aggregation of the metal catalyst elements is further suppressed.
[0015] Furthermore, the present invention provides the following: [4] The alumina-based composite oxide according to [2], which further satisfies all of the following (9) to (10) in the point analysis of the 50 points: (9) There are 5 or more measurement points out of 50 where the alumina content is 55% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 45% by mass or less, (10) There are 5 or more measurement points out of 50 where the alumina content is 1% by mass or more and 45% by mass or less, and the content of oxides of elements other than alumina is 55% by mass or more and 99% by mass or less.
[0016] When the tertiary particles constituting the alumina-based composite oxide have a variation that satisfies not only the above (1) to (4) but also the above (9) to (10), aggregation of the metal catalyst element is further suppressed.
[0017] Furthermore, the present invention provides the following: [5] The alumina-based composite oxide according to any one of [1] to [4], wherein the alumina content is 15% by mass or more and 80% by mass or less in a composition analysis performed by a fluorescent X-ray method.
[0018] When the alumina content is 15 mass % or more and 80 mass % or less in a composition analysis obtained by a fluorescent X-ray method, aggregation of a metal catalyst element is further suppressed when the metal catalyst element is supported on the alumina-based composite oxide.
[0019] In addition, the composition analysis obtained by X-ray fluorescence spectroscopy gives the content of each oxide contained in the entire alumina-based composite oxide. On the other hand, the point analysis using energy dispersive X-ray spectroscopy (above [1] and above [2]) gives the content of each oxide at the measurement point on the surface to be analyzed, not the entire alumina-based composite oxide.
[0020] Furthermore, the present invention provides the following: [6] The alumina-based composite oxide according to any one of [1] to [5], wherein the content of ceria and / or zirconia is 0.1 mass % or more and 85 mass % or less in a composition analysis obtained by a fluorescent X-ray method.
[0021] Since ceria and / or zirconia function as promoters, a ceria and / or zirconia content of 0.1% by mass or more is suitable as a catalyst support, and a ceria and / or zirconia content of 85% by mass or less can suppress thermal degradation.
[0022] Furthermore, the present invention provides the following: [7] The alumina-based composite oxide according to any one of [1] to [6] above, which contains at least one oxide of a rare earth element (excluding cerium and promethium) as an oxide other than alumina, ceria, and zirconia.
[0023] When the catalyst contains one or more oxides of rare earth elements (excluding cerium and promethium), the crystal phases of alumina, ceria, and zirconia are stabilized, and deterioration of the catalyst is further suppressed.
[0024] Furthermore, the present invention provides the following: [8] A method for producing an alumina-based composite oxide according to any one of the above [1] to [7], A step 1 of adding an acid to sodium aluminate to obtain a hydrated alumina suspension A; A step 2 of preparing an aqueous solution B-1 of a raw salt containing cerium and / or zirconium, and / or a suspension B-2 of a raw salt containing cerium and / or zirconium; Step 3 of obtaining a precipitate of an aluminum-based composite precursor by mixing the suspension A with the aqueous solution B-1 and / or the suspension B-2; and Step 4: obtaining an alumina-based composite oxide by heat-treating the precipitate A method for producing an alumina-based composite oxide comprising the steps of:
[0025] Although the general coprecipitation method is effective for producing composite oxides with uniform element distribution, it is difficult to control the element distribution by anything other than the solubility difference of the precipitate. On the other hand, in the mixing method in which crystallized alumina is mixed with crystallized ceria and zirconia, the constituent elements of each tertiary particle are the same as before mixing, resulting in an element distribution that makes it difficult to express the properties of the composite of alumina, ceria, and zirconia. In response to the above problems, according to the invention of [8], precursors of ceria and zirconia can be arranged on the surface and / or inside of hydrated alumina by mixing hydrated alumina suspension A with aqueous solution B-1 and / or suspension B-2 of raw salt containing cerium and / or zirconium. This makes it possible to make alumina secondary particles containing ceria and zirconia and secondary particles of ceria and zirconia containing alumina coexist within the tertiary particles of alumina-based composite oxide. In addition, it is possible to control the distribution of elements within the composite oxide tertiary particles by controlling the aggregation of hydrated alumina and precursors of ceria and zirconia. By using such a production method, it is possible to obtain an alumina-based composite oxide having the above-mentioned characteristics (1) to (4) of [1] above. Effect of the Invention
[0026] The present invention provides an alumina-containing composite oxide capable of suppressing aggregation of catalytic metal elements when exposed to a high temperature range for a long period of time, and a method for producing the alumina-based composite oxide capable of obtaining the alumina-based composite oxide. [Brief description of the drawings]
[0027] [Figure 1] FIG. 2 is a model diagram of tertiary particles of the alumina-based composite oxides of Examples 1 to 34. [Diagram 2] FIG. 2 is a model diagram of tertiary particles of alumina-based composite oxides according to Comparative Examples 1, 3 to 5, 7, 9, 12, and 13. [Diagram 3] FIG. 2 is a model diagram of tertiary particles of alumina-based composite oxides of Comparative Examples 2, 6, 8, 10, and 14. [Figure 4] FIG. 11 is a model diagram of a tertiary particle of an alumina-based composite oxide of Comparative Example 11. [Diagram 5] 1 is an X-ray diffraction spectrum of the alumina-based composite oxide of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Hereinafter, the embodiments of the present invention will be described. However, the present invention is not limited to these embodiments. In this specification, the alumina-based composite oxide is a general one that contains 10 mass % or less of impurity metal compounds including hafnium. In addition, in this specification, the expressions "contain" and "include" include the concepts of "contain", "include", "substantially consists of" and "consist only of".
[0029] The maximum and minimum values of the content of each component shown below are independently the preferred minimum and maximum values of the present invention, regardless of the contents of other components. Furthermore, the maximum and minimum values of various parameters (measured values, etc.) shown below are independently preferred minimum and maximum values of the present invention, regardless of the content (composition) of each component.
[0030] [Alumina-based composite oxide] The alumina-based composite oxide according to this embodiment is Alumina and Ceria and / or zirconia Contains An alumina-based composite oxide characterized by satisfying all of the following (1) to (4) in point analysis of a total of 50 points by energy dispersive X-ray spectroscopy according to the following procedures a to c: (1) There is at least one measurement point out of 50 points where the alumina content is 50% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 50% by mass or less, (2) There is at least one measurement point out of 50 where the alumina content is 1% by mass or more and less than 50% by mass, and the content of oxides of elements other than alumina is more than 50% by mass and less than 99% by mass, (3) The difference between the maximum and minimum alumina content of 50 measurement points is 20 or more and 95 or less, (4) The difference between the maximum and minimum contents of oxides of elements other than alumina at 50 measurement points is 20 or more and 95 or less. <Procedure> a: From the particle images observed with a scanning electron microscope, one particle image having a cross section of 4 μm or more in length and 4 μm or more in width is selected. b: Composition analysis is performed at 25 measurement points spaced 1 μm apart within an area of 4 μm vertically and 4 μm horizontally of the selected particle image. c: Select another particle image different from the one selected in step a and perform the same composition analysis as in step b.
[0031] According to the alumina-based composite oxide, within a particle having a cross section of 4 μm or more in length and 4 μm or more in width, the element distribution has a variation that satisfies the above (1) to (4). That is, within the tertiary particles that constitute the alumina-based composite oxide, the element distribution has a certain degree of variation. Therefore, when a metal catalyst element is supported on the alumina-based composite oxide, the metal catalyst element is supported preferentially on an element with a high affinity. When the affinity with the support is high, even when exposed to a high temperature range for a long time, the aggregation of the metal catalyst elements is suppressed due to the anchor effect, etc., and the metal catalyst is maintained in a more active state. In addition, elements with a high affinity with the metal catalyst element often act as a promoter. Therefore, the metal catalyst element is supported preferentially in the vicinity of the promoter, and the catalytic activity is expected to be improved. In addition, since the alumina and the added metal element are present in the same tertiary particle, when exposed to a high temperature range for a long time, each acts as a diffusion barrier, and the deterioration of the catalyst is suppressed.
[0032] In this specification, tertiary particles refer to particles formed by agglomeration of secondary particles, and secondary particles refer to particles formed by agglomeration of crystallites (primary particles).
[0033] From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there are two or more measurement points that satisfy the above (1), more preferably four or more measurement points, even more preferably seven or more measurement points, and particularly preferably ten or more measurement points. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there are 48 or less measurement points that satisfy the above (1), more preferably 46 or less, even more preferably 43 or less, and particularly preferably 40 or less. From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points that satisfy the above (1) is preferably 2 to 48, more preferably 4 to 46, even more preferably 7 to 43, and particularly preferably 10 to 40.
[0034] From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there are two or more measurement points that satisfy the above (2), more preferably four or more measurement points, even more preferably seven or more measurement points, and particularly preferably ten or more measurement points. From the viewpoint of suppressing aggregation of the metal catalyst element, it is preferable that there are 48 or less measurement points that satisfy the above (2), more preferably 46 or less, even more preferably 43 or less, and particularly preferably 40 or less. From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points that satisfy the above (2) is preferably 2 to 48, more preferably 4 to 46, even more preferably 7 to 43, and particularly preferably 10 to 40. The total number of measurement points that satisfy the above condition (1) and the above condition (2) is preferably 50. In other words, it is preferable that all of the 50 measurement points satisfy either the above condition (1) or the above condition (2).
[0035] In particular, it is preferable that the alumina-based composite oxide further satisfies all of the following (7) to (8). (7) There are 10 or more measurement points out of 50 points in which the alumina content is 50% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 50% by mass or less, (8) There are 10 or more measurement points out of 50 where the alumina content is 1 mass% or more and less than 50 mass%, and the content of oxides of elements other than alumina is more than 50 mass% and 99 mass% or less.
[0036] The difference between the maximum and minimum alumina contents of the 50 measurement points specified in (3) above is preferably 21 or more, more preferably 23 or more, and even more preferably 25 or more, from the viewpoint of suppressing aggregation of the metal catalyst element. The difference between the maximum and minimum alumina contents of the 50 measurement points specified in (3) above is preferably 94 or less, more preferably 92 or less, and even more preferably 90 or less, from the viewpoint of suppressing deterioration of the catalyst support (or suppressing aggregation of the metal catalyst element). The difference between the maximum and minimum alumina contents of the 50 measurement points specified in (3) above is preferably 21 or more and 94 or less, more preferably 23 or more and 92 or less, and even more preferably 25 or more and 90 or less, from the viewpoint of suppressing aggregation of the metal catalyst element.
[0037] The difference between the maximum and minimum values of the content of oxides of elements other than alumina at the 50 measurement points specified in (4) above is preferably 21 or more, more preferably 23 or more, and even more preferably 25 or more, from the viewpoint of suppressing aggregation of the metal catalyst element. The difference between the maximum and minimum values of the content of oxides of elements other than alumina at the 50 measurement points specified in (4) above is preferably 94 or less, more preferably 92 or less, and even more preferably 90 or less, from the viewpoint of suppressing deterioration of the catalyst support (or suppressing aggregation of the metal catalyst element). The difference between the maximum and minimum values of the content of oxides of elements other than alumina at the 50 measurement points specified in (4) above is preferably 21 or more and 94 or less, more preferably 23 or more and 92 or less, and even more preferably 25 or more and 90 or less, from the viewpoint of suppressing aggregation of the metal catalyst element.
[0038] The alumina-based composite oxide preferably further satisfies all of the following (5) and (6). (5) There is at least one measurement point out of 50 where the alumina content is 55% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 45% by mass or less, (6) There is at least one measurement point out of 50 where the alumina content is between 1% by mass and 45% by mass, and the content of oxides of elements other than alumina is between 55% by mass and 99% by mass.
[0039] If there is variation within the tertiary particles constituting the alumina-based composite oxide that satisfies not only the above (1) to (4) but also the above (5) to (6), aggregation of the metal catalyst element is further suppressed.
[0040] From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points that satisfy the above condition (5) is preferably two or more, more preferably three or more, and even more preferably five or more. From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points satisfying the above condition (5) is preferably 48 or less, more preferably 47 or less, and even more preferably 45 or less. From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points that satisfy the above condition (5) is preferably 2 to 48, more preferably 3 to 47, and even more preferably 5 to 45.
[0041] From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points that satisfy the above condition (6) is preferably two or more, more preferably three or more, and even more preferably five or more. From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points satisfying the above condition (6) is preferably 48 or less, more preferably 47 or less, and even more preferably 45 or less. From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points that satisfy the above condition (6) is preferably 2 to 48, more preferably 3 to 47, and even more preferably 5 to 45.
[0042] In particular, it is preferable that the alumina-based composite oxide further satisfies all of the following (9) and (10). (9) There are 5 or more measurement points out of 50 where the alumina content is 55% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 45% by mass or less, (10) There are 5 or more measurement points out of 50 where the alumina content is 1% by mass or more and 45% by mass or less, and the content of oxides of elements other than alumina is 55% by mass or more and 99% by mass or less.
[0043] It is preferable that the alumina-based composite oxide further satisfies all of the following (a) and (b). (a) There is at least one measurement point out of 50 where the alumina content is 60% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 40% by mass or less, (b) There is at least one measurement point out of 50 where the alumina content is between 1% by mass and 40% by mass, and the content of oxides of elements other than alumina is between 60% by mass and 99% by mass.
[0044] When the tertiary particles constituting the alumina-based composite oxide have a variation that satisfies not only the above (1) to (6) but also the above (a) to (b), aggregation of the metal catalyst element is further suppressed.
[0045] From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points that satisfy the above condition (a) is preferably two or more, more preferably three or more, and even more preferably four or more. From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points satisfying the above condition (a) is preferably 48 or less, more preferably 47 or less, and even more preferably 46 or less. From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points that satisfy (a) is preferably 2 to 48, more preferably 3 to 47, and even more preferably 4 to 46.
[0046] From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points that satisfy the above condition (b) is preferably two or more, more preferably three or more, and even more preferably four or more. From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points satisfying the above condition (b) is preferably 48 or less, more preferably 47 or less, and even more preferably 46 or less. From the viewpoint of suppressing aggregation of the metal catalyst element, the number of measurement points that satisfy (b) is preferably 2 to 48, more preferably 3 to 47, and even more preferably 4 to 46.
[0047] The above (1) to (10) and the above (a) to (b) can be controlled by the manufacturing method, specifically, by the manufacturing method described below. A step 1 of adding an acid to sodium aluminate to obtain a hydrated alumina suspension A; A step 2 of preparing an aqueous solution B-1 of a raw salt containing cerium and / or zirconium, and / or a suspension B-2 of a raw salt containing cerium and / or zirconium; Step 3 of obtaining a precipitate of an aluminum-based composite precursor by mixing the suspension A with the aqueous solution B-1 and / or the suspension B-2; and Step 4: obtaining an alumina-based composite oxide by heat-treating the precipitate A method for producing an alumina-based composite oxide comprising the steps of:
[0048] <Particle size D 50 > The particle diameter D of the alumina-based composite oxide 50 The particle diameter D is preferably 3.0 μm or more and 200 μm or less. 50 When the particle diameter D is 200 μm or less, no coarse particles remain when the powder is pulverized to a desired particle diameter. 50 When the diameter is 3.0 μm or more, it is possible to provide variation in element distribution within the same tertiary particle.
[0049] The particle diameter D50 The particle diameter D is more preferably 3.5 μm or more, and further preferably 4.0 μm or more. 50 is more preferably 150 μm or less, and further preferably 120 μm or less. 50 refers to a value obtained by the method described in the Examples.
[0050] <Particle size D 90 > The particle diameter D of the alumina-based composite oxide 90 The particle diameter D is preferably 4.0 μm or more and 300 μm or less. 90 When the particle diameter D is 300 μm or less, no coarse particles remain when the powder is pulverized to a desired particle diameter. 90 When the diameter is 4.0 μm or more, it is possible to provide variation in element distribution within the same tertiary particle.
[0051] The particle diameter D 90 The particle diameter D is more preferably 6.0 μm or more, and further preferably 8.0 μm or more. 90 is more preferably 250 μm or less, and further preferably 220 μm or less. 90 refers to a value obtained by the method described in the Examples.
[0052] In addition, the particle diameter D 50 When measuring, not only tertiary particles but also non-aggregated secondary particles may be included, but the amount of non-aggregated secondary particles that may be included in the alumina-based composite oxide is very small. 50 is the particle diameter of the tertiary particles D 50 It can be considered to represent.
[0053] The alumina-based composite oxide preferably has a pore volume of 0.10 mL / g or more and 1.0 mL / g or less over the entire range of pore diameter distribution (pore diameter of 3 nm or more and less than 200 nm) determined by nitrogen adsorption / desorption method. When the pore volume is 0.10 mL / g or more, the metal catalyst element is supported also in the pores, so that segregation of the metal catalyst element that is not supported is unlikely to occur. When the pore volume is 1.0 mL / g or less, the secondary particles present within the same tertiary particle are densely aggregated, and tertiary particles having variation in element distribution can be formed. The pore volume is more preferably 0.15 mL / g or more, and further preferably 0.20 mL / g or more. The pore volume is more preferably 0.90 mL / g or less, and further preferably 0.80 mL / g or less. The pore volume is more preferably 0.15 mL / g or more and 0.90 mL / g or less, and further preferably 0.20 mL / g or more and 0.80 mL / g or less.
[0054] [Rh particle size after Rh is supported and heat-treated] When the alumina content of the alumina-based composite oxide is 50% by mass or more and 80% by mass or less, it is preferable that the Rh particle size after supporting Rh under the following supporting conditions and performing a heat treatment under the following heat treatment conditions is 90 μm or less. When the alumina content of the alumina-based composite oxide is 30% by mass or more and less than 50% by mass, it is preferable that the Rh particle size after supporting Rh under the following supporting conditions and performing a heat treatment under the following heat treatment conditions is 95 μm or less. When the alumina content of the alumina-based composite oxide is 15% by mass or more and less than 30% by mass, it is preferable that the Rh particle size after supporting Rh under the following supporting conditions and performing a heat treatment under the following heat treatment conditions is 110 μm or less. When the Rh particle size after heat treatment is equal to or smaller than the above particle size, it can be said that aggregation of catalytic metal elements when exposed to high temperatures for a long period of time is further suppressed. <Supporting conditions> An 8% Rh nitrate solution is impregnated at 2% by mass (calculated as Rh) relative to 100% by mass of the alumina-based composite oxide, dried at 100°C, and then fired at 500°C for 5 hours to obtain Rh-supported powder. <Heat treatment conditions> The obtained Rh-supported powder is heat-treated in air at 1200° C. for 12 hours to obtain a post-heat-treatment sample.
[0055] When the alumina content is 50% by mass or more and 80% by mass or less, the Rh particle size is more preferably 85 μm or less, and further preferably 80 μm or less. When the alumina content is 30% by mass or more and less than 50% by mass, the Rh particle size is more preferably 90 μm or less, and further preferably 85 μm or less. When the alumina content is 15% by mass or more and less than 30% by mass, the Rh particle size is more preferably 105 μm or less, and further preferably 100 μm or less. The smaller the Rh particle size, the more preferable, and it is, for example, 20 μm or more, 30 μm or more, regardless of the alumina content.
[0056] The Rh particle size refers to a value obtained by the method described in the Examples.
[0057] The alumina-based composite oxide contains alumina. Since the alumina-based composite oxide contains alumina, it can be suitably used as a catalyst support.
[0058] The content of the alumina is preferably 15% by mass or more and 80% by mass or less in composition analysis obtained by fluorescent X-ray spectrometry. When the content of alumina is 15% by mass or more and 80% by mass or less, thermal deterioration of the catalyst is suppressed, and therefore, when a metal catalyst element is supported on the alumina-based composite oxide, aggregation of the metal catalyst element is further suppressed.
[0059] The alumina content is more preferably 20% by mass or more, and further preferably 25% by mass or more.The alumina content is more preferably 75% by mass or less, and further preferably 70% by mass or less.
[0060] The alumina-based composite oxide contains ceria and / or zirconia, and since the alumina-based composite oxide contains ceria and / or zirconia, it can be suitably used as a catalyst support.
[0061] The content of the ceria and / or zirconia is preferably 0.1% by mass or more and 85% by mass or less in composition analysis obtained by fluorescent X-ray method. Since ceria and / or zirconia function as a promoter, a ceria and / or zirconia content of 0.1% by mass or more is suitable as a catalyst support. Furthermore, a ceria and / or zirconia content of 85% by mass or less can suppress thermal degradation.
[0062] When the alumina-based composite oxide contains ceria, the content of the ceria is preferably 1% by mass or more and 80% by mass or less, as determined by composition analysis using a fluorescent X-ray method. The content of ceria is more preferably 3% by mass or more, and further preferably 6% by mass or more.The content of ceria is more preferably 75% by mass or less, and further preferably 70% by mass or less.
[0063] When the alumina-based composite oxide contains zirconia, the content of the zirconia is preferably 1% by mass or more and 75% by mass or less, as determined by composition analysis using a fluorescent X-ray method. The content of the zirconia is more preferably 5% by mass or more, and further preferably 10% by mass or more.The content of the zirconia is more preferably 70% by mass or less, and further preferably 65% by mass or less.
[0064] When the alumina-based composite oxide contains both ceria and zirconia, the total content of alumina, ceria, and zirconia is preferably 70% by mass or more and 98% by mass or less when the entire alumina-based composite oxide is taken as 100% by mass in a composition analysis obtained by a fluorescent X-ray method. By setting the total content of alumina, ceria, and zirconia to 70% by mass or more and 98% by mass or less, the alumina-based composite oxide can be more suitably used as a catalyst support.
[0065] When both ceria and zirconia are contained, the total content of alumina, ceria and zirconia is more preferably 75% by mass or more, and even more preferably 80% by mass or more, when the entire alumina-based composite oxide is taken as 100% by mass, in a composition analysis obtained by a fluorescent X-ray method.When both ceria and zirconia are contained, the total content of alumina, ceria and zirconia is more preferably 97% by mass or less, and even more preferably 96% by mass or less, when the entire alumina-based composite oxide is taken as 100% by mass.
[0066] In the alumina-based composite oxide containing ceria but not containing zirconia, the total content of alumina and ceria is preferably 70% by mass or more and 96% by mass or less when the total content of the alumina-based composite oxide is taken as 100% by mass in a composition analysis performed by a fluorescent X-ray method. By setting the total content of alumina and ceria to 70% by mass or more and 96% by mass or less, the alumina-based composite oxide can be more suitably used as a catalyst support.
[0067] In the case where ceria is contained but zirconia is not contained, the total content of alumina and ceria is more preferably 75% by mass or more when the entire alumina-based composite oxide is taken as 100% by mass, In the case where ceria is contained but zirconia is not contained, the total content of alumina and ceria is, when the entire alumina-based composite oxide is taken as 100 mass%, It is more preferably 95% by mass or less, and even more preferably 94% by mass or less.
[0068] In the alumina-based composite oxide containing zirconia but not containing ceria, the total content of alumina and zirconia is preferably 70% by mass or more and 96% by mass or less when the total content of the alumina-based composite oxide is taken as 100% by mass in a composition analysis performed by a fluorescent X-ray method. By setting the total content of alumina and zirconia to 70% by mass or more and 96% by mass or less, the alumina-based composite oxide can be more suitably used as a catalyst support.
[0069] When zirconia is contained but ceria is not contained, the total content of alumina and zirconia is more preferably 75 mass% or more, and even more preferably 80 mass% or more, when the total alumina-based composite oxide is 100 mass%.When zirconia is contained but ceria is not contained, the total content of alumina and zirconia is more preferably 95 mass% or less, and even more preferably 94 mass% or less, when the total alumina-based composite oxide is 100 mass%.
[0070] The alumina-based composite oxide preferably contains at least one oxide of a rare earth element (excluding cerium and promethium) as an oxide other than alumina, ceria, and zirconia. When the alumina-based composite oxide contains an oxide of a rare earth element other than cerium and promethium, aggregation of the metal catalyst element is further suppressed.
[0071] The alumina-based composite oxide preferably contains, among oxides of rare earth elements other than cerium and promethium, oxides of La, Nd, Pr, and Y. When the alumina-based composite oxide contains oxides of La, Nd, Pr, and Y, aggregation of the metal catalyst element is further suppressed.
[0072] When oxides of rare earth elements other than cerium and promethium are contained, the content of the oxides of rare earth elements other than cerium and promethium is preferably 2% by mass or more and 20% by mass or less when the entire alumina-based composite oxide is taken as 100% by mass in a composition analysis obtained by a fluorescent X-ray method. When the content of the oxides of rare earth elements other than cerium and promethium is 2% by mass or more and 20% by mass or less, aggregation of the metal catalyst element is further suppressed.
[0073] The content of the oxides of rare earth elements other than cerium and promethium is more preferably 3% by mass or more, and even more preferably 4% by mass or more, when the entire alumina-based composite oxide is taken as 100% by mass, in a composition analysis obtained by a fluorescent X-ray method. The content of the oxides of rare earth elements other than cerium and promethium is more preferably 18% by mass or less, and even more preferably 16% by mass or less, when the entire alumina-based composite oxide is taken as 100% by mass, in a composition analysis obtained by a fluorescent X-ray method.
[0074] The alumina-based composite oxide may contain one or more selected from (A) an oxide of at least one element selected from the group consisting of In, Si, Sn, Bi, P, and Zn, (B) a transition metal oxide (excluding oxides of rare earth elements), and (C) an alkaline earth metal oxide. These components (A) to (C) are hereinafter also referred to as "other oxides".
[0075] Examples of the transition metal oxide include one or more oxides selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Nb, Mo, Ta, and W. Examples of the alkaline earth metal oxide include one or more oxides selected from the group consisting of Mg, Ca, Sr, and Ba.
[0076] When the alumina-based composite oxide contains the other oxides, the content of the other oxides is preferably 0.1% by mass or more and 30% by mass or less when the entire alumina-based composite oxide is taken as 100% by mass. The content of the other oxides is more preferably 0.3% by mass or more and even more preferably 0.5% by mass or more when the entire alumina-based composite oxide is taken as 100% by mass. The content of the other oxides is more preferably 25% by mass or less and even more preferably 20% by mass or less when the entire alumina-based composite oxide is taken as 100% by mass.
[0077] Preferable composition ratios of the alumina-based composite oxide include the following combinations not exceeding 100% by mass in total (combinations that total 100% by mass). (1) Alumina: 40% to 80% Zirconia: 1% to 30% Ceria: 1% to 30% Oxides of rare earth elements (excluding cerium and promethium); 1% to 15% Other oxides: 0% to 10% (2) Alumina: 20% to 60% Zirconia: 20% to 70% Ceria: 1% to 40% Oxides of rare earth elements (excluding cerium and promethium); 1% to 15% Other oxides: 0% to 10% (3) Alumina: 20% to 60% Zirconia: 20% to 75% Celia: 0% to 30% Oxides of rare earth elements (excluding cerium and promethium); 1% to 15% Other oxides: 0% to 10% (4) Alumina: 20% to 60% Zirconia: 0% to 20% Celia: 20% to 70% Oxides of rare earth elements (excluding cerium and promethium); 5% to 20% Other oxides: 0% to 20% (5) Alumina: 20% to 60% Zirconia: 10% to 60% Celia: 0% to 40% Oxides of rare earth elements (excluding cerium and promethium); 1% to 15% Other oxides: 1% to 20%
[0078] The use of the alumina-based composite oxide is not particularly limited, but it is suitable for use as a catalyst carrier, and in particular, it is suitable for use as a catalyst carrier for an exhaust gas purification catalyst (exhaust gas purification catalyst carrier).
[0079] The metal catalyst element supported on the alumina-based composite oxide is not particularly limited, but for example, Rh, Pt, Pd, Au, Ru, Ag, Ni, Co, Mn, Cu, and Fe are preferable. The metal catalytic element supported on the alumina-based composite oxide may overlap with an element contained in the alumina-based composite oxide. For example, when the alumina-based composite oxide contains Fe, Fe may be used as the metal catalytic element supported on the alumina-based composite oxide.
[0080] [Method of manufacturing alumina-based composite oxide] An example of a method for producing an alumina-based composite oxide will be described below, however, the method for producing an alumina-based composite oxide of the present invention is not limited to the following example.
[0081] The method for producing an alumina-based composite oxide according to this embodiment includes the steps of: A step 1 of adding an acid to sodium aluminate to obtain a hydrated alumina suspension A; A step 2 of preparing an aqueous solution B-1 of a raw salt containing cerium and / or zirconium, and / or a suspension B-2 of a raw salt containing cerium and / or zirconium; Step 3 of obtaining a precipitate of an aluminum-based composite precursor by mixing the suspension A with the aqueous solution B-1 and / or the suspension B-2; and Step 4: obtaining an alumina-based composite oxide by heat-treating the precipitate The present invention relates to a method for producing an alumina-based composite oxide comprising the steps of:
[0082] Hereinafter, each step of the method for producing an alumina-based composite oxide according to this embodiment will be described.
[0083] (1) Process 1 In step 1, an acid is added to sodium aluminate (NaAl(OH)4) to obtain hydrated alumina suspension A.
[0084] The sodium aluminate may be in the form of a liquid or a powder, but when a gas is used as the acid, it is preferable to use the liquid form.
[0085] When a liquid sodium aluminate is used, the concentration of the sodium aluminate is preferably 1% by mass or more and 20% by mass or less in terms of aluminum oxide.
[0086] The temperature of the sodium aluminate is preferably 20° C. or higher and 90° C. or lower, more preferably 25° C. or higher, and further preferably 30° C. or higher. The temperature of the sodium aluminate is more preferably 85° C. or lower, and further preferably 80° C. or lower. By setting the temperature of the sodium aluminate within the above range, it becomes easier to obtain an alumina-based composite oxide having an element distribution that satisfies the above conditions (1) to (8). Specifically, the higher the temperature of the sodium aluminate, the greater the variation in element distribution that satisfies the above conditions (1) to (6).
[0087] The acid to be added to the sodium aluminate may be in the form of gas or liquid. Specific examples of the acid include carbon dioxide, hydrochloric acid, nitric acid, sulfuric acid, and carboxylic acid. Among them, carbon dioxide gas is preferred from the viewpoint of low impurity content.
[0088] When carbon dioxide gas is blown into the sodium aluminate, the flow rate of the carbon dioxide gas is 1.7×10 -7 m 3 / s or more 1.7×10 -5 m 3 / s or less is preferable, and 5.0×10 -7 m 3 / s or more 5.0×10 -6 m 3 / s or less is more preferable. When carbon dioxide gas is blown into the sodium aluminate, the time for blowing the carbon dioxide gas is preferably from 6 hours to 48 hours, more preferably from 12 hours to 36 hours. By blowing carbon dioxide gas into the sodium aluminate under the above conditions, a suitable suspension A can be obtained.
[0089] (2) Process 2 In step 2, an aqueous solution B-1 of raw salt containing cerium and / or zirconium and / or a suspension B-2 of raw salt containing cerium and / or zirconium are prepared. In step 2, only the aqueous solution B-1 of raw salt containing cerium and / or zirconium may be prepared, only the suspension B-2 of raw salt containing cerium and / or zirconium may be prepared, or both the aqueous solution B-1 of raw salt containing cerium and / or zirconium and the suspension B-2 of raw salt containing cerium and / or zirconium may be prepared.
[0090] The aqueous solution B-1 can be obtained by mixing various raw material salts described below.
[0091] The suspension B-2 is obtained by subjecting the aqueous solution B-1 to a heat treatment. The temperature of the heat treatment is preferably from 140° C. to 250° C., more preferably from 160° C. to 200° C. The time of the heat treatment is preferably from 1 hour to 10 hours, more preferably from 2 hours to 5 hours. When the suspension B-2 is used, the variation in element distribution tends to be greater within the range satisfying the above (1) to (6) compared to the aqueous solution B-1.
[0092] When both the aqueous solution B-1 and the suspension B-2 are used, both the aqueous solution B-1 and the suspension B-2 may be prepared and mixed together for use.
[0093] Examples of the raw material salt containing cerium include at least one of cerium nitrate, cerium chloride, cerium acetate, etc. Among these, cerium nitrate, which is a nitrate salt, is preferred.
[0094] The raw material salt containing zirconium may be any salt capable of supplying zirconium ions, and may be, for example, at least one of zirconium oxynitrate, zirconium oxychloride, zirconium nitrate, etc. Among these, nitrate-based zirconium oxynitrate is preferred.
[0095] The aqueous solution B-1 and the suspension B-2 may contain a raw material salt including a rare earth element (excluding cerium and promethium).
[0096] Examples of rare earth elements (excluding cerium and promethium) include at least one of Sc, Y, La, Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, and Lu. Among these, Y, La, Nd, and Pr are preferred.
[0097] In addition to the above, the aqueous solution B-1 and the suspension B-2 may contain one or more elements selected from (A) at least one element selected from the group consisting of In, Si, Sn, Bi, P, and Zn, (B) transition metal elements (excluding rare earth elements and precious metal elements), and (C) alkaline earth metal elements.
[0098] The raw materials of rare earth elements, transition metal elements (excluding rare earth elements and noble metal elements), alkaline earth metals, In, Si, Sn, Bi and P are not particularly limited as long as they are water-soluble. Examples include nitrates, sulfates, acetates, chlorides, bromides, etc., but nitrates are preferred as raw material salts because they can suppress the remaining impurities. The purity of these raw materials is preferably 95% or more, and more preferably 98% or more.
[0099] The solvent for preparing the aqueous solution B-1 may be appropriately selected depending on the type of raw material salt, etc., but it is usually preferable to use water (pure water, ion-exchanged water, etc.: the same applies below).
[0100] The metal salt concentration in the aqueous solution B-1 is preferably 1% or more and 15% or less in terms of oxide. By making it 1% or more, the concentration can be made high to some extent, and the treatment time can be made suitable. Also, by making it 15% or less, the increase in viscosity during neutralization can be suppressed, and the compounding can be performed suitably.
[0101] (3) Process 3 In step 3, the suspension A is mixed with the aqueous solution B-1 and / or the suspension B-2 to obtain a precipitate of an aluminum-based composite precursor.
[0102] Specifically, in step 3, first, the suspension A obtained in step 1 is mixed with the aqueous solution B-1 and / or suspension B-2 obtained in step 2, and an alkali is added to obtain a precursor precipitate of an alumina-based composite oxide. Although there are no particular limitations on the mixing, it is preferable to add the aqueous solution B-1 and / or suspension B-2 prepared in step 2 to the suspension A prepared in step 1 from the viewpoint of productivity such as filterability in the next step.
[0103] The alkali is not limited, and examples of the alkali that can be used include ammonium hydroxide, ammonium bicarbonate, sodium hydroxide, potassium hydroxide, etc. Among these, sodium hydroxide is preferred from the viewpoint of industrial cost.
[0104] The amount of alkali to be added is not particularly limited as long as it can produce a precursor precipitate of an alumina-based composite oxide as a salt precipitate. Usually, the alkali is added so that the pH of the solution becomes 8.0 to 11.0, preferably 9.0 to 10.0.
[0105] Next, the resulting precipitate of the aluminum-based composite precursor is collected by solid-liquid separation, which may be any known method such as filtration, centrifugation, or decantation.
[0106] After recovery, it is preferable to wash the obtained alumina composite hydroxide with water as necessary to remove adhering impurities.
[0107] The obtained alumina composite hydroxide may be further dried as necessary. The drying method may be any known method, such as natural drying, heat drying, etc. Furthermore, if necessary, a crushing treatment, a classification treatment, etc. may be carried out after the drying treatment.
[0108] (4) Process 4 In step 4, the precipitate (recovered material) is heat-treated to obtain an alumina-based composite oxide.
[0109] The heat treatment temperature is not particularly limited, but is usually performed within the range of 500° C. to 1200° C. and 2 hours to 10 hours. The heat treatment atmosphere is not particularly limited, but may be in air or an oxidizing atmosphere.
[0110] The alumina-based composite oxide obtained by the heat treatment can be pulverized as necessary. The pulverization method is not particularly limited, but can be a general pulverizer such as a planetary mill, a ball mill, a hammer mill, or a jet mill.
[0111] In the above-mentioned method for producing an alumina-based composite oxide, the precursors of ceria and zirconia can be arranged on the surface and / or inside of the hydrated alumina by mixing the hydrated alumina suspension A with the aqueous solution B-1 and / or suspension B-2 of raw material salts containing cerium and / or zirconium. This makes it possible to make the secondary particles of alumina containing ceria and zirconia and the secondary particles of ceria and zirconia containing alumina coexist in the tertiary particles of the alumina-based composite oxide. In addition, it is possible to control the element distribution in the composite oxide tertiary particles by controlling the aggregation of the hydrated alumina and the precursors of ceria and zirconia. By using such a production method, it is possible to obtain an alumina-based composite oxide having the above characteristics (1) to (8). EXAMPLES
[0112] The present invention will be described in detail below using examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the invention. Note that the alumina-based composite oxides obtained in the examples and comparative examples contain 1 to 3 mass % of hafnium as an inevitable impurity relative to zirconium (calculated by the following formula (X)). <Expression(X)> ([Mass of hafnium] / ([Mass of zirconium]+[Mass of hafnium]))×100(%)
[0113] The maximum and minimum values of the content of each component shown in the following examples should be considered as the preferred minimum and maximum values of the present invention, regardless of the contents of other components. Furthermore, the maximum and minimum values of the measured values shown in the following examples should be considered as the preferred minimum and maximum values of the present invention, regardless of the content (composition) of each component.
[0114] [Preparation of alumina-based composite oxide] Example 1 Sodium aluminate (Asada Chemical Industry, #2019, 78 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 8 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 8 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 1.
[0115] Example 2 Sodium aluminate (Asada Chemical Industry, #2019, 78 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 70°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 8 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 8 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 2.
[0116] Example 3 Sodium aluminate (Asada Chemical Industry, #2019, 78 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 8 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 8 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. This aqueous solution B-1 was kept in an autoclave at 180° C. for 2 hours to prepare a composite metal salt suspension (suspension B-2). Suspension A and suspension B-2 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered by solid-liquid separation, washed, and the solid matter was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 3.
[0117] Example 4 Sodium aluminate (Asada Chemical Industry, #2019, 69 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 70°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 15 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 10 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), praseodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of praseodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 4.
[0118] Example 5 Sodium aluminate (Asada Chemical Industry, #2019, 54 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 35°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 20 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 10 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 4 g in terms of neodymium oxide), praseodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 4 g in terms of praseodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 5.
[0119] Example 6 Sodium aluminate (Asada Chemical Industry, #2019, 54 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 20 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 10 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 4 g in terms of neodymium oxide), praseodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 4 g in terms of praseodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 6.
[0120] Example 7 Sodium aluminate (Asada Chemical Industry, #2019, 54 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 70°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 20 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 10 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 4 g in terms of neodymium oxide), praseodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 4 g in terms of praseodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 7.
[0121] Example 8 Sodium aluminate (Asada Chemical Industry, #2019, 42 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 50 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 8.
[0122] Example 9 Sodium aluminate (Asada Chemical Industry, #2019, 42 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 70°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 50 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 9.
[0123] Example 10 Sodium aluminate (Asada Chemical Industry, #2019, 42 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 50 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. This aqueous solution B-1 was kept in an autoclave at 180° C. for 2 hours to prepare a composite metal salt suspension (suspension B-2). Suspension A and suspension B-2 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 10.
[0124] Example 11 Sodium aluminate (Asada Chemical Industry, #2019, 42 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 50 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 11.
[0125] Example 12 Sodium aluminate (Asada Chemical Industry, #2019, 42 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 70°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 50 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 12.
[0126] Example 13 Sodium aluminate (Asada Chemical Industry, #2019, 42 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving diammonium cerium (IV) nitrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 50 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. This aqueous solution B-1 was kept in an autoclave at 180° C. for 2 hours to prepare a composite metal salt suspension (suspension B-2). Suspension A and suspension B-2 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 13.
[0127] Example 14 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 70°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 44 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 14.
[0128] Example 15 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 44 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. This aqueous solution B-1 was kept in an autoclave at 180° C. for 2 hours to prepare a composite metal salt suspension (suspension B-2). Suspension A and suspension B-2 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 15.
[0129] (Example 16) Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. Zirconium oxychloride octahydrate (Mitsuwa Chemical, special grade reagent, 44 g in terms of zirconium oxide) was dissolved in ion-exchanged water, and then 35% hydrochloric acid and ion-exchanged water were used to adjust the acid concentration to 0.67 N and the ZrO2 concentration to 4 wt / vol%. The aqueous solution was heated in an autoclave reactor at a temperature of 120°C and a pressure of 2×10 5After adjusting the pressure to Pa, 650 g of a 5% aqueous sodium sulfate solution was added and the mixture was maintained for an additional 15 minutes. Thereafter, the mixture was allowed to cool to room temperature to obtain a basic zirconium sulfate-containing slurry. Next, cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) were added to the basic zirconium sulfate-containing slurry, and a 25% aqueous sodium hydroxide solution was added until the pH reached 9, to prepare a composite metal salt suspension (suspension B). Suspension A and suspension B were mixed to obtain a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 16.
[0130] (Example 17) Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 60 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 10 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 17.
[0131] (Example 18) Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 70°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 60 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 10 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid matter was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 18.
[0132] (Example 19) Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 70 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 19.
[0133] (Example 20) Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 70°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 70 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 20.
[0134] Example 21 Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 70 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. This aqueous solution B-1 was kept in an autoclave at 180° C. for 2 hours to prepare a composite metal salt suspension (suspension B-2). Suspension A and suspension B-2 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 21.
[0135] Example 22 Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 70 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 22.
[0136] Example 23 Sodium aluminate (Asada Chemical Industry, #2019, 20 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 70°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 70 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide of Example 23.
[0137] (Example 24) Sodium aluminate (Asada Chemical Industry, #2019, 15 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 59 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 24.
[0138] (Example 25) Sodium aluminate (Asada Chemical Industry, #2019, 15 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 70°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 59 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 25.
[0139] (Example 26) Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 40 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of yttrium oxide), and titanium (IV) tetrachloride (Wako Pure Chemical, 4.0 g in terms of titanium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Example 26.
[0140] Example 27 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 40 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide), and monoammonium phosphate (Wako Reagents, special reagent grade, 4.0 g in terms of phosphate) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 27.
[0141] (Example 28) Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 40 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of yttrium oxide), and fumed silica AEROSIL (Nippon Aerosil, 4.0 g in terms of silicon oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide of Example 28.
[0142] (Example 29) Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 40 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of yttrium oxide), and ammonium metatungstate hydrate (Wako Reagent, 4.0 g in terms of tungsten oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide of Example 29.
[0143] (Example 30) Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 40 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of yttrium oxide), and magnesium nitrate hexahydrate (Wako Reagent, special reagent grade, 4.0 g in terms of magnesium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide of Example 30.
[0144] (Example 31) Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 40 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of yttrium oxide), and calcium nitrate hexahydrate (Wako Reagent, special reagent grade, 4.0 g in terms of calcium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide of Example 31.
[0145] Example 32 Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 40 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of yttrium oxide), and strontium nitrate hexahydrate (Wako Reagent, special reagent grade, 4.0 g in terms of strontium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide of Example 32.
[0146] (Example 33) Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate aqueous solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 40 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of yttrium oxide), and barium nitrate hexahydrate (Wako Reagent, special reagent grade, 4.0 g in terms of barium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide according to Example 33.
[0147] (Example 34) Sodium aluminate (Asada Chemical Industry, #2019, 30 g in terms of aluminum oxide) was diluted with ion-exchanged water to a concentration of 5% in terms of oxide, heated to 50°C, and carbon dioxide gas was injected at 100 sccm (1.7 × 10 -6 m 3 A hydrated alumina suspension (suspension A) was prepared by blowing in the mixture at a flow rate of 1000 g / s for 24 hours while maintaining the temperature at 100° C. A nitrate solution (aqueous solution B-1) was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special reagent grade, 43 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of neodymium oxide), yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special reagent grade, 2 g in terms of yttrium oxide), and iron (III) nitrate nonahydrate (Wako Reagent, special reagent grade, 1.0 g in terms of iron oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. The suspension A and the aqueous solution B-1 were mixed, and a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of an alumina-based composite oxide. Next, the precursor precipitate was recovered and washed by solid-liquid separation, and the solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized with a hammer mill to obtain the alumina-based composite oxide of Example 34.
[0148] Comparative Example 1 A nitrate aqueous solution was prepared by dissolving aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 78 g in terms of aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industries, Ltd., special reagent grade, 8 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 8 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 3% in terms of oxide. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% aqueous solution of ammonium bicarbonate. The aqueous solution of nitrate was then added to the aqueous solution of ammonium bicarbonate to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Comparative Example 1.
[0149] Comparative Example 2 A nitrate solution was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special grade, 8 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special grade, 8 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special grade, 2 g in terms of yttrium oxide) in ion-exchanged water to 5% in terms of oxide. This solution was kept in an autoclave at 180°C for 2 hours, and then a 25% by mass aqueous solution of sodium hydroxide was added until the pH reached 9, thereby obtaining a precursor precipitate of a ceria-zirconia composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain a ceria-zirconia composite oxide. The ceria and zirconia composite oxide were mixed with alumina (Sumitomo Chemical, AKP-G07, 78 g in terms of aluminum oxide) and pulverized with a hammer mill to obtain the alumina composite oxide according to Comparative Example 2.
[0150] Comparative Example 3 A nitrate aqueous solution was prepared by dissolving aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 69 g in terms of aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industries, Ltd., special reagent grade, 15 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 10 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of lanthanum oxide), praseodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of praseodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 3% in terms of oxide. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% aqueous solution of ammonium bicarbonate. The aqueous solution of nitrate was then added to the aqueous solution of ammonium bicarbonate to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Comparative Example 3.
[0151] Comparative Example 4 A nitrate aqueous solution was prepared by dissolving aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 54 g in terms of aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industries, Ltd., special reagent grade, 20 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 10 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of neodymium oxide), praseodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of praseodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 3% in terms of oxide. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% aqueous solution of ammonium bicarbonate. The aqueous solution of nitrate was then added to the aqueous solution of ammonium bicarbonate to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Comparative Example 4.
[0152] Comparative Example 5 A nitrate aqueous solution was prepared by dissolving aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 42 g in terms of aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industries, Ltd., special reagent grade, 50 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 3% in terms of oxide. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% aqueous solution of ammonium bicarbonate. The aqueous solution of nitrate was then added to the aqueous solution of ammonium bicarbonate to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Comparative Example 5.
[0153] Comparative Example 6 A nitrate solution was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special grade reagent, 50 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special grade reagent, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special grade reagent, 4 g in terms of yttrium oxide) in ion-exchanged water to 5% in terms of oxide. This solution was kept in an autoclave at 180°C for 2 hours, and then a 25% by mass aqueous sodium hydroxide solution was added until the pH reached 9, thereby obtaining a precursor precipitate of a ceria-zirconia composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain a ceria-zirconia composite oxide. The ceria and zirconia composite oxide were mixed with alumina (Sumitomo Chemical, AKP-G07, 42 g in terms of aluminum oxide) and pulverized with a hammer mill to obtain the alumina composite oxide according to Comparative Example 6.
[0154] Comparative Example 7 A nitrate aqueous solution was prepared by dissolving aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 42 g in terms of aluminum oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 50 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 3% in terms of oxide. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% aqueous solution of ammonium bicarbonate. The aqueous solution of nitrate was then added to the aqueous solution of ammonium bicarbonate to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Comparative Example 7.
[0155] Comparative Example 8 A nitrate aqueous solution was prepared by dissolving diammonium cerium (IV) nitrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 50 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 5% in terms of oxide. This aqueous solution was kept in an autoclave at 180°C for 2 hours, and then a 25% by mass aqueous solution of sodium hydroxide was added until the pH reached 9, thereby obtaining a precursor precipitate of a ceria-zirconia composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain a ceria-zirconia composite oxide. The ceria and zirconia composite oxide were mixed with alumina (Sumitomo Chemical, AKP-G07, 42 g in terms of aluminum oxide) and pulverized with a hammer mill to obtain the alumina composite oxide according to Comparative Example 8.
[0156] Comparative Example 9 A nitrate aqueous solution was prepared by dissolving aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 30 g in terms of aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industries, Ltd., special reagent grade, 44 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 3% in terms of oxide. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% aqueous solution of ammonium bicarbonate. The aqueous solution of nitrate was then added to the aqueous solution of ammonium bicarbonate to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Comparative Example 9.
[0157] Comparative Example 10 Zirconium oxychloride octahydrate (Mitsuwa Chemical, special grade reagent, 44 g in terms of zirconium oxide) was dissolved in ion-exchanged water, and then 35% hydrochloric acid and ion-exchanged water were used to adjust the acid concentration to 0.67 N and the ZrO2 concentration to 4 wt / vol%. The aqueous solution was heated in an autoclave reactor at a temperature of 120°C and a pressure of 2×10 5 After adjusting the pressure to Pa, 650 g of a 5% aqueous sodium sulfate solution was added and the mixture was maintained for an additional 15 minutes. Thereafter, the mixture was allowed to cool to room temperature to obtain a basic zirconium sulfate-containing slurry. Next, cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 20 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, special reagent grade, 2 g in terms of yttrium oxide) were added to the basic zirconium sulfate-containing slurry, and a 25% aqueous sodium hydroxide solution was added until the pH reached 13, to obtain a precipitate. The precipitate was recovered by solid-liquid separation and washed. The solid content was calcined in an electric furnace in the air at 900°C for 5 hours to obtain a ceria-zirconia composite oxide. The ceria and zirconia composite oxides were mixed with alumina (Sumitomo Chemical, AKP-G07, 30 g in terms of aluminum oxide) and pulverized with a hammer mill to obtain an alumina composite oxide according to Comparative Example 10.
[0158] Comparative Example 11 Zirconium oxynitrate (Mitsuwa Chemical, special grade, 44g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical, special grade, 20g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special grade, 2g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special grade, 2g in terms of neodymium oxide) and yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special grade, 2g in terms of neodymium oxide) were dissolved in ion-exchanged water, and 1.2 molar amounts of hydrogen peroxide were added to the amount of cerium in the cerium nitrate and stirred to obtain a raw material solution. This aqueous solution was added to 1.2 molar amounts of ammonia water equivalent to the neutralization amount for the metal cations while stirring to obtain a precursor precipitate of ceria-zirconia composite oxide. The precipitate was then centrifuged and thoroughly washed, then dried in air at a temperature of 150° C. for 7 hours, and pre-fired at 330° C. for 5 hours to obtain a molded body. The molded body was pulverized in a pulverizer and then fired in air at 800° C. for 5 hours to obtain a ceria-zirconia composite oxide. Aluminum nitrate nonahydrate (Wako Pure Chemical Industries, special grade reagent, 30 g in terms of aluminum oxide) was dissolved in ion-exchanged water. The ceria and zirconia-based composite oxide was suspended in the aluminum nitrate aqueous solution and stirred for 3 hours. The mixture was heated with stirring to evaporate water. The remaining solid was kept in air at 110°C for 40 hours and then calcined at 800°C for 5 hours to obtain the alumina-based composite oxide according to Comparative Example 11.
[0159] Comparative Example 12 A nitrate aqueous solution was prepared by dissolving aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g in terms of aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industries, Ltd., special reagent grade, 60 g in terms of zirconium oxide), cerium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 10 g in terms of cerium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 3% in terms of oxide. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% aqueous solution of ammonium bicarbonate. The aqueous solution of nitrate was then added to the aqueous solution of ammonium bicarbonate to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Comparative Example 12.
[0160] Comparative Example 13 A nitrate aqueous solution was prepared by dissolving aluminum nitrate nonahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 20 g in terms of aluminum oxide), zirconium oxynitrate (Mitsuwa Chemical Industries, Ltd., special reagent grade, 70 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical Industries, Ltd., special reagent grade, 4 g in terms of yttrium oxide) in ion-exchanged water to a concentration of 3% in terms of oxide. Next, 400 g of ammonium bicarbonate was dissolved in 7600 g of ion-exchanged water to prepare a 5% aqueous solution of ammonium bicarbonate. The aqueous solution of nitrate was then added to the aqueous solution of ammonium bicarbonate to obtain a precursor precipitate of an alumina-based composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was calcined in an electric furnace in air at 900°C for 5 hours to obtain an alumina-based composite oxide. The alumina-based composite oxide was pulverized in a hammer mill to obtain the alumina-based composite oxide according to Comparative Example 13.
[0161] (Comparative Example 14) A nitrate solution was prepared by dissolving zirconium oxynitrate (Mitsuwa Chemical, special grade reagent, 70 g in terms of zirconium oxide), lanthanum nitrate hexahydrate (Wako Pure Chemical, special grade reagent, 4 g in terms of lanthanum oxide), neodymium (III) nitrate hexahydrate (Wako Pure Chemical, special grade reagent, 2 g in terms of neodymium oxide), and yttrium (III) nitrate hexahydrate (Wako Pure Chemical, special grade reagent, 4 g in terms of yttrium oxide) in ion-exchanged water to 5% in terms of oxide. This solution was kept in an autoclave at 180°C for 2 hours, and then a 25% by mass aqueous solution of sodium hydroxide was added until the pH reached 9, thereby obtaining a precursor precipitate of a ceria-zirconia composite oxide. The precipitate was then recovered by solid-liquid separation and washed. The solid content was fired in an electric furnace in air at 900°C for 5 hours to obtain a ceria-zirconia composite oxide. The ceria and zirconia composite oxide were mixed with alumina (Sumitomo Chemical, AKP-G07, 20 g in terms of aluminum oxide) and pulverized with a hammer mill to obtain the alumina composite oxide according to Comparative Example 14.
[0162] [Composition measurement] The compositions (in terms of oxide) of the alumina-based composite oxides of the examples and comparative examples were analyzed using a wavelength dispersive X-ray fluorescence spectrometer ("ZSX PrimusII" manufactured by Rigaku Corporation). The results are shown in Tables 1 to 6.
[0163] [Point analysis using energy dispersive X-ray spectroscopy] The alumina-based composite oxides of the examples and comparative examples were subjected to point analysis using energy dispersive X-ray spectroscopy. Specifically, the samples were first embedded in resin and the surfaces were polished. Then, point analysis was performed at a total of 50 points by the following steps a to c. <Procedure> a: One particle image having a cross section of 4 μm or more in length and 4 μm or more in width was selected from particle images observed with a scanning electron microscope (JEOL JSM-6700F). b: Composition analysis was performed at 25 measurement points at 1 μm intervals within an area of 4 μm vertically and 4 μm horizontally of the selected particle image. c: Another particle image different from that selected in step a was selected and subjected to the same composition analysis as in step b.
[0164] The 50 measured points were classified as follows, and the scores were compiled in a table. The results are shown in Tables 1 to 6. In some of the comparative examples, the particles had a core-shell structure. In these cases, the area 1 μm or more from the edge of the particle toward the center of the particle in the particle image was regarded as the core part (particle part) and point analysis was performed. <Classification> - Points with an alumina content of less than 1% by mass The number of measurement points where the alumina content is 1% by mass or more and less than 50% by mass, and the content of oxides of elements other than alumina is more than 50% by mass and less than 99% by mass. The number of measurement points where the alumina content is 50% to 99% by mass and the content of oxides of elements other than alumina is 1% to 50% by mass. -Alumina content is over 99% by mass The number of measurement points where the alumina content is between 1% and 45% by mass and the content of oxides of elements other than alumina is between 55% and 99% by mass. The number of measurement points where the alumina content is 55% to 99% by mass and the content of oxides of elements other than alumina is 1% to 45% by mass. The number of measurement points where the alumina content is between 1% and 40% by mass, and the content of oxides of elements other than alumina is between 60% and 99% by mass. The number of measurement points where the alumina content is between 60% and 99% by mass and the content of oxides of elements other than alumina is between 1% and 40% by mass.
[0165] The maximum and minimum values of the alumina content at the 50 measurement points, as well as the difference between the maximum and minimum values, are also shown in Tables 1 to 6. Additionally, the maximum values, minimum values, and differences between the maximum and minimum values of the contents of oxides of elements other than alumina at the 50 measurement points are also shown in Tables 1 to 6.
[0166] [Measurement of pore volume] For the alumina-based composite oxides of the examples and comparative examples, a pore size distribution measuring device ("BELSOAP Mini II" manufactured by Microtrack Bell) was used to obtain nitrogen adsorption / desorption isotherms, and the pore size distribution was then calculated from the desorption process using the BJH method. The measurement conditions were as follows. Then, the pore volume was calculated over the entire range of the pore diameter distribution (pore diameters of 3 nm or more and less than 200 nm). The results are shown in the table. <Measurement conditions> Measurement equipment: Pore size distribution measurement equipment (Microtrack Bell BELSOAP Mini II) Measurement range: Pe / P0=0~1 Adsorption temperature: 77K Number of measurement points: 10 points on the adsorption side, 25 points on the desorption side
[0167] [Measurement of Rh particle size (catalyst particle diameter)] The alumina composite oxides of the examples and comparative examples were impregnated with 8% Rh nitrate solution (Tanaka Kikinzoku Kogyo Co., Ltd.) at 2% by weight in terms of Rh, dried at 100°C, and then calcined at 500°C for 5 hours to obtain Rh-supported powder. Next, the samples were heat-treated in air at 1200°C for 12 hours to obtain post-heat-treatment samples. 0.2 g of the samples were weighed into a cell, and the Rh particle size was measured by the CO pulse method using a Microtrack-Bel BELCAT B. The results are shown in Tables 1 to 6. As can be seen from Tables 1 to 6, when the alumina-based composite oxides of the examples were used, aggregation of Rh (catalytic metal element) was suppressed.
[0168] Here, for ease of understanding, model diagrams of tertiary particles of the alumina-based composite oxide of the example and the alumina-based composite oxide of the comparative example are shown in Figs. 1 to 4. As shown in FIG. 1, the alumina-based composite oxide 1 of Examples 1 to 34 is in the form of tertiary particles, and is composed of two types of secondary particles having different element distributions, i.e., Secondary particles 2 having an alumina content of 50% by mass or more and 99% by mass or less (secondary particles 2 having an element oxide content other than alumina of 1% by mass or more and 50% by mass or less); and secondary particles 3 having an element oxide content of more than 50 mass % and not more than 99 mass % other than alumina (secondary particles 3 having an alumina content of 1 mass % or more and less than 50 mass %). Therefore, even if exposed to high temperatures for a long period of time, aggregation of the catalytic metal elements is suppressed.
[0169] 2, the alumina-based composite oxides 4 of Comparative Example 1, Comparative Example 3 to Comparative Example 5, Comparative Example 7, Comparative Example 9, Comparative Example 12, and Comparative Example 13 are in the form of tertiary particles, but are composed only of secondary particles 5 with little bias in element distribution. In other words, the alumina-based composite oxides 4 of Comparative Example 1, Comparative Example 3 to Comparative Example 5, Comparative Example 7, Comparative Example 9, Comparative Example 12, and Comparative Example 13 have a small difference between the maximum and minimum alumina contents among the secondary particles. Therefore, when exposed to a high temperature range for a long period of time, the catalytic metal elements aggregate.
[0170] As shown in Fig. 3, the alumina-based composite oxides 6 of Comparative Examples 2, 6, 8, 10, and 14 are in the form of tertiary particles, but are composed of secondary particles 7 and 8, which have a significantly large element distribution. The alumina-based composite oxides 4 of Comparative Examples 2, 6, 8, 10, and 14 have a significantly large difference between the maximum and minimum alumina contents among the secondary particles. In other words, the alumina-based composite oxides 6 of Comparative Examples 2, 6, 8, 10, and 14 are tertiary particles as a mixture of alumina particles and oxides of elements other than alumina, and have an element distribution that makes it difficult to express the characteristics due to the composite of alumina and oxides of elements other than alumina. Therefore, when exposed to a high temperature range for a long time, the catalytic metal elements aggregate.
[0171] As shown in FIG. 4, the alumina-based composite oxide 9 of Comparative Example 11 is in the form of tertiary particles, and is composed of secondary particles 10 constituting a shell portion and secondary particles 11 constituting a core portion. Secondary particles 10 and 11 are composed of secondary particles 7 and 8, which have a significantly large bias in element distribution. In other words, alumina-based composite oxide 9 of Comparative Example 11 is a tertiary particle as a mixture of alumina particles and oxides of elements other than alumina, and has an element distribution that makes it difficult to realize the characteristics of composites of alumina and oxides of elements other than alumina. Therefore, when exposed to a high temperature range for a long time, the catalytic metal elements aggregate.
[0172] [Particle size D 50 , particle diameter D 90 Measurement of 0.15 g of the alumina composite oxide of each of the examples and comparative examples and 40 ml of 0.2% aqueous sodium hexametaphosphate solution were placed in a 50 ml beaker and dispersed for 2 minutes using an ultrasonic homogenizer "Sonifier S-450D" (Emerson Japan Co., Ltd.), and then placed in a device (laser diffraction particle size distribution measuring device ("LA-950" manufactured by Horiba, Ltd.)) for measurement. The results are shown in Table 1.
[0173] [X-ray diffraction spectrum] An X-ray diffraction spectrum was obtained for the alumina-based composite oxide of Example 1 using an X-ray diffractometer ("Ultima IV" manufactured by Rigaku). The measurement conditions were as follows. The results are shown in FIG. <Measurement conditions> Measurement equipment: X-ray diffraction equipment (Rigaku, Ultima IV) Source: CuKα source Tube voltage: 50kV Tube current: 30mA Scanning speed: 2θ=20~65°: 4° / min
[0174] [Table 1]
[0175] [Table 2]
[0176]
Table 3
[0177]
Table 4
[0178]
Table 5
[0179]
Table 6
Claims
1. Alumina and Ceria and / or zirconia Contains An alumina-based composite oxide characterized by satisfying all of the following (1) to (4) in point analysis of a total of 50 points by the following procedures a to c using energy dispersive X-ray spectroscopy: (1) There is at least one measurement point out of 50 points in which the alumina content is 50% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 50% by mass or less, (2) There is one or more measurement points out of 50 points in which the alumina content is 1 mass% or more and less than 50 mass%, and the content of element oxides other than alumina is more than 50 mass% and 99 mass% or less, (3) The difference between the maximum and minimum alumina contents of 50 measurement points is 20 or more and 95 or less; (4) The difference between the maximum and minimum contents of oxides of elements other than alumina at 50 measurement points is 20 or more and 95 or less. <Procedure> a: From particle images observed under a scanning electron microscope, one particle image having a cross section of 4 μm or more in length and 4 μm or more in width is selected. b: Composition analysis is performed at 25 measurement points spaced 1 μm apart within an area of 4 μm vertical by 4 μm horizontal on the selected particle image. c: Another particle image different from the one selected in step a is selected, and the composition analysis is performed in the same manner as in step b.
2. The alumina-based composite oxide according to claim 1, further comprising, in the point analysis of the 50 points, satisfying all of the following (5) to (6): (5) There is at least one measurement point out of 50 points in which the alumina content is 55% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 45% by mass or less, (6) There is one or more measurement points out of 50 where the alumina content is 1 mass % or more and 45 mass % or less, and the content of oxides of elements other than alumina is 55 mass % or more and 99 mass % or less.
3. The alumina-based composite oxide according to claim 1, further comprising, in the point analysis of the 50 points, satisfying all of the following (7) to (8): (7) There are 10 or more measurement points out of 50 points in which the alumina content is 50% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 50% by mass or less, (8) Of the 50 measurement points, there are 10 or more measurement points having an alumina content of 1 mass% or more and less than 50 mass%, and a content of oxides of elements other than alumina of more than 50 mass% and 99 mass% or less.
4. The alumina-based composite oxide according to claim 2, further comprising, in the point analysis of the 50 points, satisfying all of the following (9) to (10): (9) There are 5 or more measurement points out of 50 points in which the alumina content is 55% by mass or more and 99% by mass or less, and the content of oxides of elements other than alumina is 1% by mass or more and 45% by mass or less, (10) There are 5 or more measurement points out of 50 where the alumina content is 1% by mass or more and 45% by mass or less, and the content of oxides of elements other than alumina is 55% by mass or more and 99% by mass or less.
5. 5. The alumina-based composite oxide according to claim 1, wherein the alumina content is 15% by mass or more and 80% by mass or less in a composition analysis performed by a fluorescent X-ray method.
6. 5. The alumina-based composite oxide according to claim 1, wherein the content of ceria and / or zirconia is 0.1% by mass or more and 85% by mass or less in a composition analysis performed by a fluorescent X-ray method.
7. 5. The alumina-based composite oxide according to any one of claims 1 to 4, characterized in that it contains at least one oxide of a rare earth element (excluding cerium and promethium) as an oxide other than alumina, ceria, and zirconia.
8. A method for producing an alumina-based composite oxide according to any one of claims 1 to 4, comprising the steps of: Step 1: adding an acid to sodium aluminate to obtain a hydrated alumina suspension A; A step 2 of preparing an aqueous solution B-1 of a raw salt containing cerium and / or zirconium and / or a suspension B-2 of a raw salt containing cerium and / or zirconium; Step 3 of obtaining a precipitate of an aluminum-based composite precursor by mixing the suspension A with the aqueous solution B-1 and / or the suspension B-2; and Step 4: obtaining an alumina-based composite oxide by heat-treating the precipitate 2. A method for producing an alumina-based composite oxide comprising the steps of:
Citation Information
Patent Citations
Continuous manufacture of alumina gel product of preliminaryselected type and device therefor
JP1985215521A
Inorganic oxide, exhaust gas purification catalyst support and exhaust gas purification catalyst
JP2006036556A
Catalyst for use in purification of exhaust gas
JP2006298759A
Inorganic mixed oxide and exhaust gas purification catalyst using the same
JP2009107901A
Coating composites of Al2O3-CeO2 / ZrO2 and methods for producing them
JP2018508437A