Laminate production method

The method enhances photomask fidelity and resolution in laminate manufacturing by using a photosensitive transfer material with controlled exposure and an ND filter, addressing distortions and protrusions in resin patterns for semiconductor and metal mask applications.

JP2024146491APending Publication Date: 2024-10-15FUJIFILM CORP

Patent Information

Application Number
JP2023059426
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional methods for manufacturing laminates using photosensitive transfer materials result in distortions and unnatural protrusions in resin patterns, leading to poor photomask fidelity and high resolution issues, particularly in the formation of fine patterns for semiconductor package substrates and metal masks with minute through-holes.

Method used

A method for manufacturing a laminate involving a photosensitive transfer material with a temporary support and a transfer layer containing an alkali-soluble resin, photopolymerization initiator, and a polymerizable compound, where exposure is performed at a predetermined low exposure amount using a Stouffer 21-step tablet as a mask, with an ND filter to maintain stable exposure dose, and a contact exposure method to achieve high photomask fidelity.

Benefits of technology

The method produces resin patterns with excellent photomask fidelity and line width uniformity, addressing the issues of distortions and protrusions, enabling high-resolution patterns for semiconductor package substrates and metal masks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146491000009
    Figure 2024146491000009
  • Figure 2024146491000010
    Figure 2024146491000010
  • Figure 2024146491000011
    Figure 2024146491000011
Patent Text Reader

Abstract

To provide a laminate production method capable of acquiring a resin pattern which is excellent in photo mask fidelity.SOLUTION: There is provided a laminate production method comprising: an adhering step for adhering a photosensitive transfer material and a substrate, so that, a transfer layer of the photosensitive transfer material contacts the substrate, the photosensitive transfer material including a temporary support, an alkali soluble resin, a photoinitiator, and a transfer layer including a photosensitive resin layer including, a polymerizable compound with an ethylenic double bond; a step for pattern exposure for pattern exposing, the transfer layer through a photomask; and a development step for development of the transfer layer subjected to pattern exposing, for forming a resin pattern. An exposure amount S1 of the pattern exposure is 80% or less of an exposure amount S0 when, after adhering the substrate and the photosensitive transfer material, then, a Stauffer 21st step tablet is exposure as a mask and is subjected to development, a maximum residual film step number is 6.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing a laminate. [Background technology]

[0002] Photosensitive transfer materials, also known as dry film resists, are widely used because they can be easily used to form resist patterns on various substrates by thermal lamination, for example, to form wiring patterns in the manufacturing process of semiconductor package substrates and metal masks used in the manufacture of OLEDs (Organic Light Emitting Diodes).

[0003] For example, Patent Document 1 describes a photosensitive element capable of forming a resist pattern, which is described as "a photosensitive element comprising a support film and a photosensitive layer derived from a photosensitive resin composition formed on the support film, the haze of the support film being 0.01 to 1.5%, and the total number of particles with a diameter of 5 μm or more and aggregates with a diameter of 5 μm or more contained in the support film being 5 pieces / mm 2 The photosensitive layer contains a binder polymer, a photopolymerizable compound having an ethylenically unsaturated bond, and a photopolymerization initiator, and the thickness T of the photosensitive layer and the absorbance A of the photosensitive layer at 365 nm satisfy the relationship represented by the formula (I): 0.001≦A / T≦0.020 (I). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2012 / 081680 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of one embodiment of the present disclosure is to provide a method for producing a laminate which provides a resin pattern with excellent photomask fidelity. [Means for solving the problem]

[0006] The present disclosure includes the following aspects. <1> a lamination step of laminating a photosensitive transfer material including a temporary support and a transfer layer having a photosensitive resin layer containing an alkali-soluble resin, a photopolymerization initiator, and a polymerizable compound having an ethylenic double bond, to a substrate such that the transfer layer side of the photosensitive transfer material is in contact with the substrate; the above Transfer layer an exposure step of exposing the resultant to a pattern through a photomask; and The above pattern exposed Transfer layer a developing step of developing the resin pattern, The exposure dose S1 of the pattern exposure is 80% or less of the exposure dose S0 at which the maximum number of remaining film steps is 6 when the photosensitive transfer material and the substrate are laminated together, and then the photosensitive transfer material is exposed using a Stouffer 21-step tablet as a mask and developed. A method for manufacturing a laminate.

[0007] <2> The transmittance of the photosensitive transfer material at the maximum sensitivity wavelength is 70% or more. <1> A method for producing the laminate described in claim 1. <3> The exposure step is a step of performing pattern exposure by further interposing an ND filter between the photosensitive resin layer and an exposure light source. <1> or <2> A method for producing the laminate described in claim 1. <4> The reflectance of the ND filter is 30% or less. <3> A method for producing the laminate described in claim 1. <5> The transmittance of the ND filter is 25% to 75%. <3> or <4> A method for producing the laminate described in claim 1. <6> The exposure method used in the exposure step is a contact exposure method. <1> ~ <5> 13. A method for producing the laminate according to claim 12. <7> The thickness of the photosensitive resin layer is 5 μm or less. <1> ~ <6> 13. A method for producing the laminate according to claim 12. <8> The photopolymerization initiator is a hexaarylbisimidazole-based photopolymerization initiator. <1> ~ <7> 13. A method for producing the laminate according to claim 12. <9> The photosensitive resin layer further contains a sensitizer. <1> ~ <8> 13. A method for producing the laminate according to claim 12. <10> a value obtained by dividing the content of the photopolymerization initiator in the photosensitive resin layer by the content of the sensitizer in the photosensitive resin layer is, on a mass basis, 20 or more and 300 or less; <9> A method for producing the laminate described in claim 1. <11> The sensitizer is a benzophenone-based sensitizer. <9> or <10> A method for producing the laminate described in claim 1. <12> When the thickness of the photosensitive resin layer is X μm and the content of the sensitizer in the photosensitive resin layer is Y mass %, the value obtained by multiplying the value of X by the value of Y and then multiplying the result by 10 is 0.5 or more and 5.0 or less. <9> ~ <11> 13. A method for producing the laminate according to claim 12. <13> The exposure dose S0 is 60 mJ / cm 2 Below is the <1> ~ <12> 13. A method for producing the laminate according to claim 12. <14> An intermediate layer is provided between the temporary support and the photosensitive resin layer. <1> ~ <13> 13. A method for producing the laminate according to claim 12. <15> The intermediate layer has a water-soluble resin layer. <14> A method for producing the laminate described in claim 1. <16> The intermediate layer has a thermoplastic resin layer and a water-soluble resin layer. <14> or <15> A method for producing the laminate described in claim 1. <17> A step of removing the temporary support is provided between the lamination step and the exposure step. <1> ~ <16> 13. A method for producing the laminate according to claim 12. <18> an opening width Wr of the resin pattern is wider than a light-shielding width Wm of a light-shielding pattern of the photomask; <1> ~ <17> 13. A method for producing the laminate according to claim 12. <19> The opening width Wr of the resin pattern is 20 μm or less. <18> A method for producing the laminate described in claim 1.

[0008] <20> the substrate has a metal layer on the surface in contact with the photosensitive transfer material, and the method comprises the steps of: after the developing step, etching the metal layer in the region where the resin pattern is not formed, and then removing the resin pattern to form a metal pattern layer; or, after plating the metal layer in the region where the resin pattern is not formed, removing the resin pattern, and then etching the metal layer exposed by removing the resin pattern to form a metal pattern layer. <1> ~ <19> 13. A method for producing the laminate according to claim 12.

[0009] <21> the substrate is a metal substrate having a first surface and a second surface opposite to the first surface, and after the developing step, the metal substrate in an area where the resin pattern is not formed is etched to form a through hole penetrating the metal substrate, and then the resin pattern is removed to form a metal pattern layer. <1> ~ <19> 13. A method for producing the laminate according to claim 12.

[0010] <22> The metal substrate contains an iron-nickel alloy. <21> A method for producing the laminate described in claim 1. <23> The metal pattern layer has a rectangular through hole. <21> or <22> A method for producing the laminate described in claim 1. <24> The laminate is a metal mask. <21> ~ <23> 13. A method for producing the laminate according to claim 12. <25> The laminate is a semiconductor package. <20> A method for producing the laminate described in claim 1. Effect of the Invention

[0011] According to one embodiment of the present disclosure, there is provided a method for producing a laminate which provides a resin pattern with excellent photomask fidelity. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic diagram showing an example of the configuration of a photosensitive transfer material. [Figure 2A] FIG. 2A is a model diagram of an opening pattern in which no protrusions are observed on either side of the diagonal line. [Figure 2B] FIG. 2B is a model diagram of an opening pattern in which protrusions are observed on both sides of a diagonal line. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, embodiments of the present disclosure will be described in detail. The present disclosure is not limited to the following embodiments. The following embodiments may be modified as appropriate within the scope of the present disclosure.

[0014] In the present disclosure, a numerical range indicated using "~" indicates a range including the numerical value described before "~" as the lower limit and the numerical value described before "~" as the upper limit. In the numerical ranges described in stages in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with the upper limit or lower limit of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples.

[0015] In this disclosure, "(meth)acrylic" refers to acrylic, methacrylic, or both acrylic and methacrylic.

[0016] In this disclosure, "(meth)acrylate" refers to acrylate, methacrylate, or both acrylate and methacrylate.

[0017] In the present disclosure, "(meth)acryloyl" refers to acryloyl, methacryloyl, or both acryloyl and methacryloyl.

[0018] In the present disclosure, when a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the corresponding substances present in the composition, unless otherwise specified.

[0019] In the present disclosure, the term "step" encompasses not only independent steps, but also steps that cannot be clearly distinguished from other steps as long as a desired purpose is achieved.

[0020] In the present disclosure, a group (atomic group) that is not specified as substituted or unsubstituted includes a group (atomic group) that has no substituent and a group (atomic group) that has a substituent. For example, an "alkyl group" includes not only an alkyl group that has no substituent (i.e., an unsubstituted alkyl group) but also an alkyl group that has a substituent (i.e., a substituted alkyl group).

[0021] In the present disclosure, examples of light used for "exposure" generally include the bright line spectrum of a mercury lamp, far ultraviolet light represented by an excimer laser, extreme ultraviolet light (EUV light), X-rays, electron beams, and other actinic rays (active energy rays).

[0022] Chemical structural formulae in the present disclosure may be described as simplified structural formulae in which hydrogen atoms are omitted.

[0023] In the present disclosure, "mass %" and "weight %" are synonymous, and "parts by mass" and "parts by weight" are synonymous.

[0024] In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments.

[0025] In this disclosure, ordinal numbers (e.g., "first" and "second") are terms used to distinguish components, and do not limit the number of components or the priority of the components.

[0026] In the present disclosure, "transparent" means that the average transmittance of visible light with a wavelength of 400 nm to 700 nm is 80% or more, and preferably 90% or more.

[0027] In the present disclosure, unless otherwise specified, the weight average molecular weight (Mw) and number average molecular weight (Mn) are molecular weights determined by detecting with a differential refractometer using a gel permeation chromatography (GPC) analyzer with columns of TSKgel GMHxL, TSKgel G4000HxL, or TSKgel G2000HxL (all product names manufactured by Tosoh Corporation) in a solvent of THF (tetrahydrofuran), and converting the molecular weight using polystyrene as a standard substance.

[0028] In the present disclosure, "alkali-soluble" means that the solubility in 100 g of a 1% by mass aqueous solution of sodium carbonate at a liquid temperature of 22°C is 0.1 g or more.

[0029] In the present disclosure, "water-soluble" means that the solubility in 100 g of water having a liquid temperature of 22°C and a pH of 7.0 is 0.1 g or more.

[0030] In this disclosure, "solids" means all components excluding solvent.

[0031] <Method of manufacturing laminate> The method for producing a laminate according to the present disclosure includes a lamination step (hereinafter also simply referred to as a "lamination step") of laminating a photosensitive transfer material having a temporary support and a transfer layer including a photosensitive resin layer containing an alkali-soluble resin, a photopolymerization initiator, and a polymerizable compound having an ethylenic double bond, to a substrate such that the transfer layer side of the photosensitive transfer material is in contact with the substrate; an exposure step of exposing the transfer layer to a pattern through a photomask (hereinafter also simply referred to as an "exposure step"); and A development step (hereinafter, also simply referred to as "development step") of developing the pattern-exposed transfer layer to form a resin pattern, The exposure dose S1 of the pattern exposure is 80% or less of the exposure dose S0 at which the maximum number of remaining film steps is 6 when the photosensitive transfer material and the substrate are laminated together, exposed using a Stouffer 21-step tablet as a mask, and then developed.

[0032] The method for producing a laminate according to the present disclosure may include other steps in addition to the laminating step, the exposing step, and the developing step. The method for producing a laminate according to the present disclosure preferably includes, after the development step, a step of forming a metal pattern layer (hereinafter also referred to as a "metal pattern layer forming step"). The method for producing a laminate according to the present disclosure preferably includes a step of removing the temporary support (hereinafter also referred to as a "temporary support removing step") between the laminating step and the exposure step. Furthermore, the method for producing a laminate according to the present disclosure preferably includes a step of removing a protective film (hereinafter also referred to as a "protective film removing step") before the laminating step, as necessary.

[0033] Patterning using photosensitive transfer materials, also known as dry film resists, requires high resolution. For example, in the manufacturing process of semiconductor package substrates, attempts are being made to form copper wiring patterns of 3 μm or less by using fine patterns formed with dry film resists in a semi-additive process. In addition, metal masks with minute through-holes used in the manufacture of OLEDs require finer hole widths of 15 μm or less in line with the trend toward higher definition OLEDs.

[0034] However, conventional methods can result in distortion of the shape of the resin pattern (resist pattern) (specifically, unnatural protrusions or constrictions), making it difficult to obtain photomask fidelity for the resin pattern, and are not necessarily suitable for achieving high resolution.

[0035] As an example, in the manufacture of metal masks with minute through-holes, when forming a rectangular minute pattern, unnatural protrusions or constrictions may occur at the corners of the rectangular holes in the resin pattern for forming the through-holes. It is presumed that the unnatural protrusions and constrictions that occur in the resin pattern are formed when the light is amplified (or attenuated) at the corners due to the overlapping of diffracted light generated during exposure. Such issues significantly reduce the quality of the metal mask, and ultimately the quality when a fluorescent material is evaporated in a pattern using the metal mask.

[0036] Therefore, the present inventors have intensively studied to solve such problems, and have found that a resin pattern with excellent photomask fidelity can be obtained by the method for producing a laminate according to the present disclosure. In the method for producing a laminate according to the present disclosure, a predetermined low exposure dose is performed in the step of pattern exposure, that is, the exposure dose S1 of the pattern exposure is 80% or less of the exposure dose S0 at which the maximum number of remaining film steps is 6 steps when the photosensitive transfer material and the substrate are laminated together, exposed using a Stouffer 21-step tablet as a mask, and then developed, so that the photomask fidelity of the obtained resin pattern is excellent. In addition, in one embodiment of the method for producing a laminate according to the present disclosure, a resin pattern with excellent photomask fidelity and line width uniformity can be obtained.

[0037] On the other hand, Patent Document 1 does not focus on the predetermined low dose exposure applied to the method for producing a laminate according to the present disclosure.

[0038] Hereinafter, each step of the method for producing a laminate according to the present disclosure will be described in detail. In addition, preferred embodiments of the photosensitive transfer material and the substrate used in the method for producing a laminate according to the present disclosure will be described below after describing each step of the production method.

[0039] <Protection film removal process> The method for producing a laminate according to the present disclosure preferably includes a step of removing a protective film from a photosensitive transfer material (protective film removing step). The method for removing the protective film is not limited, and a known method can be applied.

[0040] <Lamination process> The method for producing a laminate according to the present disclosure includes a lamination step of laminating a photosensitive transfer material having a temporary support and a transfer layer including a photosensitive resin layer containing an alkali-soluble resin, a photopolymerization initiator, and a polymerizable compound having an ethylenic double bond, to a substrate such that the transfer layer side of the photosensitive transfer material is in contact with the substrate.

[0041] In the lamination step, when the photosensitive transfer material further comprises a layer other than the protective film (e.g., a high refractive index layer and / or a low refractive index layer) on the surface of the photosensitive resin layer that does not face the temporary support, the surface of the photosensitive resin layer that does not face the temporary support is laminated to the substrate via that layer.

[0042] The photosensitive transfer material and the substrate may be laminated by a known method. In the lamination step, it is preferable to press the photosensitive transfer material and the substrate. For example, it is preferable to laminate the transfer layer side of the photosensitive transfer material and the substrate, and apply pressure and heat using a roll or other means to press the photosensitive transfer material and the substrate.

[0043] A known lamination method can be suitably used as a method for pressing the substrate and the photosensitive transfer material. In the lamination step, a known laminator such as a laminator, a vacuum laminator, or an autocut laminator that can increase productivity can be used. The lamination temperature is not particularly limited, but is preferably, for example, 70°C to 130°C.

[0044] When the photosensitive transfer material includes a protective film, the lamination step is carried out after the protective film is removed in the protective film removing step.

[0045] <Pressing process> After laminating the photosensitive transfer material and the substrate, a step of pressing the laminate of the photosensitive transfer material and the substrate (hereinafter also referred to as a "pressurizing step") may be performed. The laminate to be pressed is preferably a laminate including a substrate, a transfer layer, and a temporary support in this order. The laminate to be pressed may be a laminate including a substrate and a transfer layer in this order. For example, after the laminating step, when the temporary support is removed by a temporary support removing step described later, a laminate including a substrate and a transfer layer in this order is formed. In the pressurizing step, the laminate obtained by laminating the photosensitive transfer material and the substrate may be pressurized in an autoclave. For example, the pressurizing step can be performed at 50°C, 0.5 MPa, and 60 minutes. By pressurizing the laminate, the adhesion between the transfer layer and the substrate can be improved, and the followability of the transfer layer to the unevenness of the surface of the substrate is improved. The pressurizing step is preferably performed before the exposure step.

[0046] <Temporary support removal process> The method for producing a laminate according to the present disclosure preferably includes a step of removing a temporary support (a temporary support removing step) between the lamination step and the exposure step. By removing the temporary support prior to the exposure step, the generation of pinholes originating from the temporary support is suppressed, blurring of the optical image is reduced, and the photomask fidelity and line width uniformity of the obtained resin pattern can be further improved.

[0047] The method for removing the temporary support in the temporary support removing step is not particularly limited, and a mechanism similar to the cover film peeling mechanism described in paragraphs 0161 to 0162 of JP-A No. 2010-072589 can be used.

[0048] <Exposure process> The method for producing a laminate according to the present disclosure includes an exposure step (exposure step) of exposing the transfer layer to light through a photomask in a pattern. "Patternwise exposing the transfer layer" means forming exposed and non-exposed parts in the photosensitive resin layer by irradiating the transfer layer having a photosensitive resin layer with light through a photomask. The positional relationship between the exposed and non-exposed regions in the patternwise exposure is not particularly limited. The positional relationship between the exposed and non-exposed parts can be determined, for example, according to the shape of the desired resin pattern.

[0049] The light used for the pattern exposure is preferably applied to the transfer layer in a direction from the transfer layer to the substrate. The light for pattern exposure of the transfer layer preferably contains at least one wavelength selected from the group consisting of 365 nm and 405 nm.

[0050] Examples of light sources include discharge lamps such as extra-high pressure mercury lamps, high pressure mercury lamps, and metal halide lamps; and semiconductor light sources such as LEDs (Light Emitting Diodes) and LDs (Laser Diodes).

[0051] The exposure amount S1 of the pattern exposure (i.e., the actual exposure amount) is 80% or less of the exposure amount S0 at which the maximum number of remaining film steps is 6 when the photosensitive transfer material and the substrate are laminated together, exposed using a Stouffer 21-step step tablet as a mask, and then developed. That is, in this exposure process, the exposure amount S1 is set so that the exposure amount S1 / exposure amount S0×100 is 80% or less. The exposure amount S1 / exposure amount S0×100 is preferably 50% or less, and more preferably 25% or less. The lower limit of the exposure amount S1 / exposure amount S0×100 is, for example, 10% or more.

[0052] The exposure dose S0 is set to 200 mJ / cm from the viewpoint of shortening the production time (takt time) and improving productivity. 2 Less than 60 mJ / cm is preferable. 2 The lower limit of the exposure dose S0 is, for example, 5 mJ / cm 2 That's all.

[0053] The "Stofer 21-step Step Tablet" is an exposure mask for evaluating the sensitivity of photosensitive materials, which has a 21-step pattern with gradually changing transmittance, and is designed so that the transmittance drops by 1 / √2 at step 1 and by 1 / 2 at step 2. The "Stofer 21-step Step Tablet" is available from Stoufer Industries, Inc.

[0054] That is, in the manufacturing method of the laminate according to the present disclosure, the exposure amount S0 at which the maximum number of remaining film steps is 6 is determined using the "Stouffer 21 step tablet", and the exposure amount S1 of the pattern exposure applied to the exposure step is set to an exposure amount that is 80% or less of the obtained exposure amount S0. Note that other exposure masks having the same configuration as the "Stouffer 21 step tablet" available from Stouffer Industries, Inc. can be regarded as the same as the "Stouffer 21 step tablet" in the present disclosure.

[0055] The development conditions when determining the exposure amount S0 are the same as the development conditions in the development process after performing pattern exposure with the exposure amount S1 in the exposure process. Specifically, the development conditions when determining the exposure amount S0 and the development conditions in the development process are set to use a developer having the same composition, the same developer temperature, and a development time that is twice the minimum development time. The "minimum development time" refers to the shortest time required for the unexposed portions of the photosensitive resin layer to be completely dissolved by development processing.

[0056] In the exposure step, from the viewpoint of performing stable exposure at a low exposure dose, it is preferable to perform pattern exposure by further interposing an ND filter (Neutral Density Filter) between the photosensitive resin layer and the exposure light source. The ND filter is an optical filter that has the function of reflecting or absorbing light of a photosensitive wavelength to attenuate the amount of light.

[0057] By using an ND filter, it is possible to maintain the exposure amount at a stable shutter speed of the exposure machine and to perform exposure at a low exposure amount, thereby obtaining a resin pattern with good line width uniformity.

[0058] The reflectance of the ND filter is preferably 30% or less in order to prevent deterioration of image quality due to stray light. The transmittance of the ND filter is preferably 25% to 75%, and more preferably 50% to 75%. The transmittance of the ND filter may be, for example, 25%, 50%, or 75%.

[0059] The reflectance of an ND filter is a value measured using a UV-Vis spectrophotometer with light of the maximum absorption wavelength. The transmittance of an ND filter is a value measured using a UV-visible spectrophotometer with light of the maximum absorption wavelength.

[0060] As the ultraviolet-visible spectrophotometer, for example, an ultraviolet-visible near-infrared spectrophotometer "V-670" manufactured by JASCO Corporation can be used.

[0061] The ND filter may be selected from known ND filters, taking into consideration the type of light source used and the exposure amount S1 to be set. Commercially available ND filters may be used. Examples of commercially available ND filters include HN0025, HN0050, and HN0070 (manufactured by Asahi Spectroscopy Co., Ltd.).

[0062] The ND filter may be disposed at any position between the photosensitive resin layer and the exposure light source, but is preferably disposed closer to the light source than the photomask.

[0063] The exposure step may be performed before or after the removal of the temporary support. When the exposure step is performed before the removal of the temporary support, the transfer layer may be exposed through the temporary support. In the exposure step, the transfer layer may be pattern-exposed with the photomask in contact with the transfer layer, or the transfer layer may be pattern-exposed with the photomask close to the transfer layer without contacting the transfer layer. In order to prevent contamination of the photomask due to contact between the photomask and the transfer layer and to avoid the influence of foreign matter attached to the photomask on the exposure, it is preferable to pattern-expose the transfer layer without removing the temporary support. When the transfer layer is pattern-exposed through the temporary support, it is preferable to remove the temporary support after the exposure step and before the development step. In addition, the exposure may be performed not only under atmospheric pressure but also under reduced pressure or vacuum, and may be performed by interposing a liquid such as water between the light source and the transfer layer.

[0064] From the viewpoint of the resolution of the resin pattern, it is preferable to use a contact exposure method, which is a method in which a photomask is brought into contact with the surface of an object to be exposed (such as a temporary support or a photosensitive resin layer) and exposed to light.

[0065] The photomask used in the exposure step may be, for example, a chrome mask, an emulsion mask, or a film mask.

[0066] The photomask is preferably such that the light shielding width Wm of the light shielding pattern is narrower than the opening width Wr of the resin pattern to be obtained. By making the light shielding width Wm of the photomask narrower than the opening width Wr of the resin pattern, the opening width Wr of the resin pattern is prevented from becoming wider than the preset target opening width during exposure with a low exposure dose. Therefore, the photomask fidelity is high, and a resin pattern can be obtained that is exactly the target opening width.

[0067] The light shielding width Wm of the photomask is a value measured by an optical microscope. A specific measuring method will be shown in the examples described later.

[0068] <Developing process> The method for producing a laminate according to the present disclosure includes a development step of developing the pattern-exposed transfer layer to form a resin pattern.

[0069] In the development step, the transfer layer is subjected to a development treatment to form a resin pattern. The resolution of the resin pattern formed through the development process determines the resolution of the metal pattern layer (e.g., wiring or through-hole) formed through the metal pattern layer forming process described below. In addition, for example, when the metal pattern layer is used for manufacturing an OLED, it is presumed that the resolution of the through-hole of the metal pattern layer determines the resolution of the pattern formed using a deposition mask.

[0070] The resin pattern is formed by removing the exposed or unexposed parts of the transfer layer. The photosensitive resin layer contained in the transfer layer is a negative photosensitive resin layer, and the unexposed parts of the transfer layer are removed by development treatment, and the exposed parts of the transfer layer form the resin pattern.

[0071] The opening width Wr of the resin pattern obtained through the development step is preferably wider than the light-shielding width Wm of the light-shielding pattern of the photomask.

[0072] The opening width Wr of the resin pattern is a value measured by an optical microscope. A specific measuring method will be shown in the examples described later. The details of the light blocking width Wm are the same as those explained in the exposure process, and therefore will not be explained here.

[0073] The opening width Wr of the resin pattern is preferably 20 μm or less, more preferably 5 μm to 20 μm, and further preferably 5 μm to 15 μm.

[0074] The development process is carried out, for example, using a developer. Examples of the developer include known developers (for example, the developer described in JP-A-5-72724). The developer is preferably an alkaline aqueous developer containing a compound with pKa=7 to 13 at a concentration of 0.05 mol / L to 5 mol / L. Examples of the alkaline compound contained in the alkaline aqueous developer include sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, and choline (2-hydroxyethyltrimethylammonium hydroxide).

[0075] The developer may contain a water-soluble organic solvent and a surfactant.

[0076] Preferred examples of the developer include the developer described in paragraph 0194 of WO 2015 / 093271.

[0077] The temperature of the developer is preferably 20°C to 40°C.

[0078] Examples of the development method include paddle development, shower development, shower and spin development, and dip development. Shower development is a development method in which a developing solution is sprayed onto an object by showering. Examples of the preferred development method include the development method described in paragraph 0195 of International Publication No. 2015 / 093271.

[0079] The developer and residue remaining after the development step are preferably removed by a known method. Examples of methods for removing the developer and residue include shower treatment and AirKnife treatment. In the shower treatment, liquids such as water and a cleaning agent are sprayed onto the object by showering. Residue may be removed by using a brush.

[0080] <Metal pattern layer formation process> The method for producing a laminate according to the present disclosure may include, after the development step, a step of forming a metal pattern layer (metal pattern layer formation step).

[0081] When the method for producing a laminate according to the present disclosure includes a metal pattern layer forming step after the development step, the metal pattern layer forming step is preferably the first or second aspect shown below.

[0082] In the metal pattern layer forming step of the first embodiment, The substrate has a metal layer on the surface that contacts the photosensitive transfer material, After etching the metal layer in the area where the resin pattern is not formed, the resin pattern is removed to form a metal pattern layer (also referred to as "mode (1)-1"); or After plating the metal layer in the area where the resin pattern is not formed, the resin pattern is removed, and the metal layer exposed by removing the resin pattern is etched to form a metal pattern layer (also referred to as "mode (1)-2").

[0083] In the metal pattern layer forming step of the second embodiment, the substrate is a metal substrate having a first surface and a second surface opposite the first surface; The metal substrate in the area where the resin pattern is not formed is etched to form through-holes penetrating the metal substrate, and then the resin pattern is removed to form a metal pattern layer.

[0084] The substrates used in the first and second embodiments will be described later.

[0085] (Etching process) In the first and second aspects of the metal pattern layer forming step, the resin pattern formed from the photosensitive resin layer is used as an etching resist to carry out an etching treatment.

[0086] The etching treatment may be a known method. Examples of the etching treatment include wet etching and dry etching (e.g., plasma etching). Examples of the etching treatment include the method described in paragraphs 0209 to 0210 of JP 2017-120435 A and the method described in paragraphs 0048 to 0054 of JP 2010-152155 A.

[0087] The etching process is preferably wet etching. In wet etching, an etching solution is usually used. The type of etching solution may be selected from acidic or alkaline etching solutions according to the target of etching. Examples of acidic etching solutions include aqueous solutions containing at least one acidic component selected from the group consisting of hydrochloric acid, sulfuric acid, nitric acid, acetic acid, hydrofluoric acid, oxalic acid, and phosphoric acid. Examples of acidic etching solutions include mixed aqueous solutions of the above-mentioned acidic component and at least one salt selected from the group consisting of ferric chloride, ammonium fluoride, and potassium permanganate. The acidic component may be a component that combines multiple acidic components. Examples of alkaline etching solutions include aqueous solutions containing at least one alkaline component selected from the group consisting of sodium hydroxide, potassium hydroxide, ammonia, organic amines, and salts of organic amines (such as tetramethylammonium hydroxide). Examples of alkaline etching solutions include mixed aqueous solutions of the above-mentioned alkaline component and a salt (such as potassium permanganate). The alkaline component may be a component that combines multiple alkaline components.

[0088] = Matters regarding through holes = In the metal pattern forming step of the second embodiment, an etching process is performed on the metal substrate in the area where the resin pattern is not formed, to form through-holes penetrating the metal substrate.

[0089] A plurality of through holes may be formed. The depth of the through hole corresponds to the thickness of the metal substrate. The through hole is usually defined by the inner surface of the metal substrate. The through hole may be defined by one or more faces. The faces defining the through hole observed in cross-sectional view may be straight or curved. The number, shape and arrangement of the through holes are determined, for example, according to the target pattern. The through hole extending from the first face to the second face forms an opening on the first face and forms an opening on the second face. The diameter of the opening formed on the first face corresponds to the diameter of the through hole on the first face described later, and the diameter of the opening formed on the second face corresponds to the diameter of the through hole on the second face described later. Examples of the shape of the through hole (specifically, the opening) observed in plan view include a circular shape, an elliptical shape and a rectangular shape. The shape of the through hole observed in plan view is preferably a rectangular shape, and more preferably a square or a rectangular shape. When the shape of the through hole observed in a plan view is a polygon (for example, a rectangle), some or all of the corners of the polygon may be rounded.

[0090] The average diameter of the through holes formed on the first surface of the metal substrate (hereinafter sometimes referred to as "average diameter D1 of the through holes") is preferably 15 μm to 100 μm, more preferably 20 μm to 50 μm, and even more preferably 20 μm to 30 μm. The average diameter of the through holes formed on the second surface of the metal substrate (hereinafter sometimes referred to as "average diameter D2 of the through holes") is preferably 25 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less. There is no lower limit for the average diameter D2 of the through holes.

[0091] In the present disclosure, the average diameter of the through holes is calculated by the arithmetic mean of the diameters of 10 through holes measured based on an image obtained using a scanning electron microscope (SEM).

[0092] (Resin pattern removal process) In the metal pattern layer forming step, it is preferable to carry out a treatment for removing the resin pattern. In the first embodiment (1)-1 and the second embodiment, the removal of the resin pattern is performed after the etching treatment. In the first embodiment (1)-2, the etching treatment is performed after the removal of the resin pattern.

[0093] The method for removing the resin pattern is not particularly limited, but includes a method for removing the resin pattern by chemical treatment, and a method for removing the resin pattern using a removal liquid is preferred.

[0094] The removal liquid may, for example, include a removal liquid containing an inorganic or organic alkaline component and water, dimethyl sulfoxide, N-methylpyrrolidone, or a mixed solvent thereof. The inorganic alkaline component may, for example, be sodium hydroxide or potassium hydroxide. The organic alkaline component may, for example, be a primary amine compound, a secondary amine compound, a tertiary amine compound, or a quaternary ammonium salt compound.

[0095] The resin pattern may be removed by immersing the laminate including the resin pattern in a removal liquid. The temperature of the removal liquid is preferably 30° C. to 80° C., and more preferably 50° C. to 80° C. The immersion time is preferably 1 minute to 30 minutes. In the immersion method, the removal liquid may be stirred.

[0096] The resin pattern may be removed, for example, by a spray, shower or puddle method using a removal liquid.

[0097] (Plating) As the plating treatment used in the metal pattern layer forming step of embodiment (1)-2, a known plating method can be applied, and for example, electrolytic plating (electrical plating) is preferable, and electrolytic copper plating is more preferable.

[0098] The components of the plating solution used in electrolytic plating include, for example, water-soluble copper salts. As the water-soluble copper salt, water-soluble copper salts that are usually used as components of plating solutions can be used. As the water-soluble copper salt, it is preferable that at least one kind selected from the group consisting of inorganic copper salts, copper salts of alkanesulfonic acids, copper salts of alkanolsulfonic acids, and copper salts of organic acids is used. As the inorganic copper salts, for example, copper sulfate, copper oxide, copper chloride, and copper carbonate are used. As the copper salts of alkanesulfonic acids, for example, copper methanesulfonate and copper propanesulfonate are used. As the copper salts of alkanolsulfonic acids, for example, copper isethionate and copper propanolsulfonate are used. As the copper salts of organic acids, for example, copper acetate, copper citrate, and copper tartrate are used. Furthermore, as a component of the plating solution used in the electrolytic plating, salts of other corresponding metals may be used in place of the copper mentioned above.

[0099] The plating solution may contain sulfuric acid, which allows the pH and sulfate ion concentration of the plating solution to be adjusted.

[0100] The method and conditions of electrolytic plating are not limited. For example, a metal pattern can be formed on the metal layer in the area where the resin pattern is not arranged by supplying the laminate after the development process to a plating tank containing a plating solution. In electrolytic plating, the metal pattern can be formed by controlling, for example, the current density and the transport speed of the substrate.

[0101] The temperature of the plating solution used in the electrolytic plating is preferably 70°C or less, and more preferably 10°C to 40°C. The current density in the electrolytic plating is preferably 0.1 A / dm2 to 100 A / dm2, and more preferably 0.5 A / dm2 to 20 A / dm2. By increasing the current density, the productivity of the conductor pattern can be improved. By decreasing the current density, the uniformity of the thickness of the metal pattern can be improved.

[0102] <Other processes> The method for producing a laminate according to the present disclosure may include any step (other step) other than the steps described above. Examples of the other steps include, but are not limited to, an electroless plating step, a sputtering step, a seed layer application step, and a seed layer etching step.

[0103] <Application> The laminate produced by the method for producing a laminate according to the present disclosure can be used for various purposes. In one embodiment, the method for producing a laminate according to the present disclosure can be applied to the production of various devices, such as input devices such as touch panels, and display devices such as organic electroluminescence display devices and liquid crystal display devices. In an embodiment, the method for producing a laminate according to the present disclosure can be applied to the production of a metal mask. Examples of the metal mask include deposition masks used in the production of OLEDs and the like. Examples of deposition masks include the deposition masks described in paragraphs 0245 to 0257 of JP 2022-168819 A. Furthermore, in one embodiment, the method for producing a laminate according to the present disclosure can be applied to the production of semiconductor packages.

[0104] <Substrate> As the substrate, a known substrate may be used. In one embodiment, the substrate may be a substrate having a metal layer, and more preferably has a metal layer on the surface of the substrate. The substrate may have any layer other than the metal layer, if necessary. Examples of the substrate include a resin substrate, a glass substrate, and a semiconductor substrate. Preferred embodiments of the substrate are described, for example, in paragraph 0140 of International Publication No. 2018 / 155193, the contents of which are incorporated herein by reference.

[0105] Examples of the base material constituting the substrate include glass, silicon, and films. The base material constituting the substrate is preferably transparent. In this specification, the term "transparent" means that the transmittance of light with a wavelength of 400 nm to 700 nm is 80% or more. The refractive index of the substrate constituting the substrate is preferably 1.50 to 1.52.

[0106] The transparent glass substrate may be a tempered glass such as Gorilla Glass manufactured by Corning Inc. In addition, the transparent glass substrate may be made of the materials described in JP-A-2010-86684, JP-A-2010-152809, and JP-A-2010-257492.

[0107] When a film substrate is used as the substrate, it is preferable to use a film substrate having small optical distortion and / or high transparency. Examples of such a film substrate include polyethylene terephthalate (PET), polyethylene naphthalate, polycarbonate, triacetyl cellulose, and cycloolefin polymer.

[0108] When the substrate is manufactured by a roll-to-roll method, a film substrate is preferable.

[0109] The metal layer of the substrate may be a conductive layer used in general circuit wiring or touch panel wiring. From the viewpoints of electrical conductivity and fine line formability, the conductive layer is preferably at least one layer selected from the group consisting of a metal layer, a conductive metal oxide layer, a graphene layer, a carbon nanotube layer, and a conductive polymer layer, more preferably a metal layer, and further preferably a copper layer or a silver layer.

[0110] The substrate may have one metal layer or two or more metal layers. When the substrate has two or more metal layers, the metal layers are preferably made of different materials.

[0111] Materials for the metal layer include metals and conductive metal oxides. Metals include Al, Zn, Cu, Fe, Ni, Cr, Mo, Ag, and Au. Conductive metal oxides include ITO (Indium Tin Oxide), IZO (Indium Zinc Oxide), and SiO2.

[0112] In an embodiment, the substrate may be a metal substrate having a first side and a second side opposite the first side.

[0113] The metal substrate may have a single-layer structure or a multi-layer structure. Metal elements contained in the metal substrate include, for example, Cu, Ni, Fe, Cr, Mn, and Co. The metal substrate preferably contains at least one metal element selected from the group consisting of Cu, Ni, Fe, Cr, Mn and Co, more preferably contains at least one metal element selected from the group consisting of Cu, Fe and Ni, and further preferably contains Cu. The metal substrate may contain elements other than the metal elements. Examples of elements other than the metal elements include B, C, N, O, P, S and Cl. An example of a preferred metal substrate is a copper substrate. A part or the whole of the metal substrate may be an alloy. Examples of the alloy include nickel-cobalt (Ni-Co) alloy and iron-nickel (Fe-Ni) alloy. In one embodiment, the metal substrate preferably contains an iron-nickel (Fe-Ni) alloy.

[0114] The first surface of the metal substrate may have a roughness Rmax of 0.5 μm to 5.0 μm.The second surface of the metal layer may have a roughness Rmax of 0.5 μm to 5.0 μm.

[0115] The average thickness of the metal substrate is preferably 30 μm to 500 μm, more preferably 40 μm to 400 μm, and further preferably 50 μm to 300 μm. The average thickness of the metal layer is calculated as the arithmetic average of thicknesses measured at five points by cross-sectional observation using a scanning electron microscope (SEM).

[0116] <Photosensitive transfer material> The photosensitive transfer material used in the method for producing a laminate according to the present disclosure includes a temporary support and a transfer layer having a photosensitive resin layer containing an alkali-soluble resin, a photopolymerization initiator, and a polymerizable compound having an ethylenic double bond, and may include layers other than the temporary support and the photosensitive resin layer. Examples of the other layers include a protective film, an intermediate layer (for example, a thermoplastic resin layer, and a water-soluble resin layer), and the like.

[0117] Fig. 1 is a schematic diagram showing an example of the configuration of a photosensitive transfer material. The photosensitive transfer material 10 shown in Fig. 1 has, in this order, a temporary support 11, a transfer layer 12 including a thermoplastic resin layer 13, a water-soluble resin layer 15, and a photosensitive resin layer 17, and a protective film 19. Although the photosensitive transfer material 10 shown in Fig. 1 has a form in which the thermoplastic resin layer 13 and the water-soluble resin layer 15 are arranged, the thermoplastic resin layer 13 and the water-soluble resin layer 15 may not be arranged.

[0118] The photosensitive transfer material used in the method for producing a laminate according to the present disclosure has a temporary support and a transfer layer including a photosensitive resin layer, and preferably has a temporary support, a transfer layer including a photosensitive resin layer, and a protective film in this order.

[0119] The photosensitive transfer material preferably has a transmittance at the maximum sensitivity wavelength of 70% or more, more preferably 80% or more, and even more preferably 85% or more. There is no particular upper limit, but it may be 100%.

[0120] If the transmittance at the maximum sensitivity wavelength is 70% or more, the photomask fidelity is more excellent.

[0121] The "maximum sensitivity wavelength" refers to the wavelength at which the minimum exposure amount at which the photosensitive resin layer reacts is determined as the spectral sensitivity for each wavelength of light. The maximum sensitivity wavelength can be determined, for example, as follows.

[0122] When the photosensitive resin layer is irradiated with light of a specific wavelength through a Stouffer 4105 step wedge tablet (Stouffer Industries), the minimum exposure dose at which the photosensitive resin layer reacts is defined as Emin. The minimum exposure dose at which the photosensitive resin layer reacts is the exposure dose at which the photosensitive resin layer is exposed to a certain wavelength (e.g., 365 nm) through a step wedge tablet, and after development, the exposed photosensitive resin layer has the largest number of remaining film steps, i.e., the maximum number of remaining film steps. By changing the wavelength of irradiation, a spectral sensitivity curve can be obtained. Emin varies for each wavelength, and the wavelength at which Emin is at its minimum is the wavelength of maximum sensitivity.

[0123] In a negative photosensitive resin layer, the minimum exposure at which the exposed area remains can be taken as Emin. When the light source has a discrete light quantity distribution (such as g-line, h-line, or i-line) like a high-pressure mercury lamp, or when the wavelength of the irradiated light is controlled using a filter or the like, the wavelength with the highest sensitivity among the light that actually hits the photosensitive material is taken as the maximum sensitivity wavelength. For example, suppose that the minimum value of the spectral sensitivity curve of a certain photosensitive material is at 290 nm and the second is at 365 nm (i-line). Since high-pressure mercury lamps practically emit almost no light at 290 nm, when exposing this photosensitive material with a high-pressure mercury lamp, the maximum sensitivity wavelength is 365 nm.

[0124] The total thickness of the photosensitive transfer material is preferably 5 μm to 55 μm, more preferably 10 μm to 50 μm, and particularly preferably 20 μm to 40 μm. The total thickness of the photosensitive transfer material is measured by a method similar to the method for measuring the thickness of each layer described above.

[0125] In order to better exert the effects of the present disclosure, the layer thickness of each layer in the photosensitive transfer material, excluding the temporary support and the protective film, is preferably 20 μm or less, more preferably 10 μm or less, and particularly preferably 1 μm or more and 10 μm or less.

[0126] In addition, from the viewpoint of better exerting the effects of the present disclosure, the total thickness of the photosensitive resin layer, the water-soluble resin layer, and the thermoplastic resin layer in the photosensitive transfer material is preferably 20 μm or less, more preferably 10 μm or less, even more preferably 5 μm or less, and particularly preferably 1 μm or more and 5 μm or less.

[0127] Hereinafter, each of the components contained in the photosensitive transfer material will be described.

[0128] (Temporary Support) The photosensitive transfer material includes a temporary support. The temporary support is a support that supports the transfer layer and is removable from the transfer layer. The structure of the temporary support may be a single-layer structure or a multi-layer structure.

[0129] Examples of materials constituting the temporary support include glass substrates, resin films, and paper. From the viewpoints of strength, flexibility, and light transmittance, the temporary support is preferably a film, and more preferably a resin film. The temporary support is preferably a film that is flexible and does not significantly deform, shrink, or stretch under pressure, or under pressure and heat. Examples of films include polyethylene terephthalate films (e.g., biaxially stretched polyethylene terephthalate films), polymethyl methacrylate films, cellulose triacetate films, polystyrene films, polyimide films, and polycarbonate films. The temporary support is preferably a polyethylene terephthalate film. The film used as the temporary support is preferably free of deformations such as wrinkles and scratches.

[0130] From the viewpoint of enabling pattern exposure through the temporary support, it is preferable that the temporary support has high transparency, and the transmittance at 365 nm is preferably 60% or more, and more preferably 70% or more.

[0131] From the viewpoint of pattern formability during pattern exposure through the temporary support and transparency of the temporary support, the haze value of the temporary support is preferably small. The haze value of the temporary support is preferably 5% or less, more preferably 2% or less, even more preferably 0.5% or less, and particularly preferably 0.1% or less. The lower limit of the haze value of the temporary support is not limited. The lower limit of the haze value of the temporary support may be 0.01% or 0.001%. The haze value is measured using a haze meter (for example, haze meter NDH400 manufactured by Nippon Denshoku Industries Co., Ltd.).

[0132] From the viewpoint of pattern formability during pattern exposure through the temporary support and the transparency of the temporary support, it is preferable that the number of coarse particles, foreign matter, and defects contained in the temporary support is small. The number of particles, foreign matter, and defects with a diameter of 1 μm or more in the temporary support is 50 / 10 mm. 2 It is preferable that the number of pieces is less than 10 pieces / 10 mm. 2 More preferably, 3 pieces / 10 mm or less. 2 More preferably, 0 pieces / 10 mm or less. 2 It is particularly preferred that:

[0133] From the viewpoint of resolution in pattern exposure through the temporary support, the average thickness of the temporary support is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less. The average thickness of the temporary support is preferably 5 μm or more, and more preferably 10 μm or more. The average thickness of the temporary support is calculated by the arithmetic average of the thicknesses at five points measured by cross-sectional observation using a scanning electron microscope (SEM).

[0134] Preferred temporary supports include, for example, a biaxially oriented polyethylene terephthalate film having a thickness of 16 μm, a biaxially oriented polyethylene terephthalate film having a thickness of 12 μm, and a biaxially oriented polyethylene terephthalate film having a thickness of 9 μm.

[0135] Preferred embodiments of the temporary support are described, for example, in paragraphs 0017 to 0018 of JP 2014-85643 A, paragraphs 0019 to 0026 of JP 2016-27363 A, paragraphs 0041 to 0057 of WO 2012 / 081680 A, paragraphs 0029 to 0040 of WO 2018 / 179370 A, and paragraphs 0012 to 0032 of JP 2019-101405 A. The above publications are incorporated herein by reference.

[0136] From the viewpoint of handling, the temporary support may include a layer containing fine particles (hereinafter also referred to as "lubricant layer" in this paragraph). The lubricant layer is preferably disposed as the outermost layer on one or both sides of the temporary support. The diameter of the particles contained in the lubricant layer is preferably 0.05 μm to 0.8 μm. The average thickness of the lubricant layer is preferably 0.05 μm to 1.0 μm.

[0137] (Transfer layer) The photosensitive transfer material includes a transfer layer having a photosensitive resin layer. The photosensitive resin layer is a layer containing an alkali-soluble resin, a photopolymerization initiator, and a polymerizable compound having an ethylenic double bond. The structure of the transfer layer may be a single layer structure or a multi-layer structure.

[0138] (Component of transfer layer: photosensitive resin layer) The transfer layer includes a photosensitive resin layer. When the transfer layer has a single-layer structure, the transfer layer is a photosensitive resin layer. The photosensitive resin layer is a negative type photosensitive resin layer.

[0139] <<Alkali-soluble resin>> The photosensitive resin layer contains an alkali-soluble resin. A preferred alkali-soluble resin is, for example, a known alkali-soluble resin used in an etching resist. The alkali-soluble resin is preferably a binder polymer. The alkali-soluble resin is preferably an alkali-soluble resin having an acid group. A preferred alkali-soluble resin is the polymer A described below.

[0140] In order to suppress the swelling of the photosensitive resin layer by the developer, the acid value of the polymer A is preferably 220 mgKOH / g or less, more preferably less than 200 mgKOH / g, and even more preferably less than 190 mgKOH / g, in order to obtain a more excellent resolution. In order to obtain a more excellent developability, the acid value of the polymer A is preferably 60 mgKOH / g or more, more preferably 120 mgKOH / g or more, even more preferably 150 mgKOH / g or more, and particularly preferably 170 mgKOH / g or more. The acid value is the mass [mg] of potassium hydroxide required to neutralize 1 g of the sample. The acid value is calculated, for example, from the average content of acid groups in the compound. The acid value of the polymer A is adjusted, for example, by the type of structural unit constituting the polymer A and the content of the structural unit containing an acid group.

[0141] The weight average molecular weight of the polymer A is preferably 5,000 to 500,000. The weight average molecular weight of 500,000 or less is preferable from the viewpoint of improving resolution and developability. The weight average molecular weight of the polymer A is more preferably 100,000 or less, further preferably 60,000 or less, and particularly preferably 50,000 or less. On the other hand, the weight average molecular weight of 5,000 or more is preferable from the viewpoint of controlling the properties of the development aggregates and the properties of the unexposed film such as edge fuse property and cut chip property in the photosensitive resin layer. The weight average molecular weight of the polymer A is more preferably 10,000 or more, further preferably 20,000 or more, and particularly preferably 30,000 or more. The edge fuse property refers to the degree of the tendency of the photosensitive resin layer to protrude from the end face of the roll when the transfer film is wound into a roll. The cut chip property refers to the degree of the tendency of the chip to fly when the unexposed film is cut with a cutter. If these chips adhere to the upper surface of the photosensitive resin layer, they will be transferred to a mask in a subsequent exposure step, causing defective products. The polydispersity of the polymer A is preferably 1.0 to 6.0, more preferably 1.0 to 5.0, even more preferably 1.0 to 4.0, and particularly preferably 1.0 to 3.0. In the present disclosure, the weight average molecular weight (Mw) and number average molecular weight (Mn) are values ​​measured using gel permeation chromatography. The polydispersity is the ratio of the weight average molecular weight to the number average molecular weight (weight average molecular weight / number average molecular weight).

[0142] From the viewpoint of suppressing line width thickening and deterioration of resolution when the focal position is shifted during exposure, the polymer A preferably has an aromatic hydrocarbon group, and more preferably has a structural unit having an aromatic hydrocarbon group. Examples of aromatic hydrocarbon groups include substituted or unsubstituted phenyl groups and substituted or unsubstituted aralkyl groups. The content ratio of structural units having aromatic hydrocarbon groups in the polymer A is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, particularly preferably 45% by mass or more, and most preferably 50% by mass or more, based on the total mass of the polymer A. The upper limit is not particularly limited, but is preferably 95% by mass or less, more preferably 85% by mass or less. In addition, when multiple types of polymer A are contained, the content ratio of structural units having aromatic hydrocarbon groups is calculated as a weight average value.

[0143] Examples of monomers forming a structural unit having an aromatic hydrocarbon group include monomers having an aralkyl group, styrene, and polymerizable styrene derivatives (e.g., methylstyrene, vinyltoluene, tert-butoxystyrene, acetoxystyrene, 4-vinylbenzoic acid, styrene dimer, styrene trimer, etc.). Among them, monomers having an aralkyl group or styrene are preferred. In one embodiment, when the monomer forming the structural unit having an aromatic hydrocarbon group in polymer A is styrene, the content of the structural unit derived from styrene is preferably 20% by mass to 50% by mass, more preferably 25% by mass to 45% by mass, further preferably 30% by mass to 40% by mass, and particularly preferably 30% by mass to 35% by mass, based on the total mass of polymer A.

[0144] The aralkyl group includes a substituted or unsubstituted phenylalkyl group, and a substituted or unsubstituted benzyl group is preferable.

[0145] Examples of the monomer having a substituted or unsubstituted phenylalkyl group other than a benzyl group include phenylethyl (meth)acrylate.

[0146] Examples of the monomer having a substituted or unsubstituted benzyl group include (meth)acrylates having a substituted or unsubstituted benzyl group (e.g., benzyl (meth)acrylate, chlorobenzyl (meth)acrylate, etc.); and vinyl monomers having a benzyl group (e.g., vinylbenzyl chloride, vinylbenzyl alcohol, etc.). Among these, benzyl (meth)acrylate is preferred. In one embodiment, when the monomer forming the structural unit having an aromatic hydrocarbon group in the polymer A is benzyl (meth)acrylate, the content of the structural unit derived from benzyl (meth)acrylate is preferably 50% by mass to 95% by mass, more preferably 60% by mass to 90% by mass, further preferably 70% by mass to 90% by mass, and particularly preferably 75% by mass to 90% by mass, based on the total mass of the polymer A.

[0147] The polymer A having a structural unit having an aromatic hydrocarbon group is preferably obtained by polymerizing a monomer having an aromatic hydrocarbon group with at least one type of a first monomer described later and / or at least one type of a second monomer described later.

[0148] The polymer A having no structural unit having an aromatic hydrocarbon group is preferably obtained by polymerizing at least one type of first monomer described later, and more preferably obtained by copolymerizing at least one type of first monomer with at least one type of second monomer described later.

[0149] The first monomer is a monomer having a carboxy group in the molecule. Examples of the first monomer include (meth)acrylic acid, fumaric acid, cinnamic acid, crotonic acid, itaconic acid, 4-vinylbenzoic acid, maleic anhydride, and maleic acid half ester. Among these, (meth)acrylic acid is preferred.

[0150] The content of the structural units derived from the first monomer in polymer A is preferably 5% by mass to 50% by mass, more preferably 10% by mass to 40% by mass, and even more preferably 15% by mass to 30% by mass, based on the total mass of polymer A.

[0151] The content of the constitutional unit derived from the first monomer is preferably 10% by mass to 50% by mass based on the total mass of polymer A. A content of 10% by mass or more is preferable from the viewpoints of achieving good developability and controlling edge fusing properties, and is more preferably 15% by mass or more, and even more preferably 20% by mass or more. A content of 50% by mass or less is preferable from the viewpoints of high resolution and foot shape of the resist pattern, and furthermore, is preferable from the viewpoints of low resist density. This is preferable from the viewpoint of the chemical resistance of the pattern, and from these viewpoints, it is more preferably 35 mass % or less, further preferably 30 mass % or less, and particularly preferably 27 mass % or less.

[0152] The second monomer is a monomer that is non-acidic and has at least one ethylenically unsaturated group in the molecule. Examples of the second monomer include (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, cyclohexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; esters of vinyl alcohol such as vinyl acetate; and (meth)acrylonitrile. Among them, methyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and n-butyl (meth)acrylate are preferred, and methyl (meth)acrylate is particularly preferred.

[0153] The content of the structural units derived from the second monomer in polymer A is preferably 5% by mass to 60% by mass, more preferably 15% by mass to 50% by mass, and even more preferably 20% by mass to 45% by mass, based on the total mass of polymer A.

[0154] In addition, it is preferable that the polymer A contains at least one type of structural unit selected from the group consisting of structural units having an aralkyl group and structural units derived from styrene, from the viewpoint of suppressing line width thickening and deterioration of resolution when the focal position is shifted during exposure. As the polymer A, for example, a copolymer containing methacrylic acid, benzyl methacrylate, and styrene, a copolymer containing methacrylic acid, methyl methacrylate, benzyl methacrylate, and styrene, etc. are preferable.

[0155] In one embodiment, polymer A is preferably a polymer containing 25% to 40% by mass of structural units having an aromatic hydrocarbon group, 20% to 35% by mass of structural units derived from a first monomer, and 30% to 45% by mass of structural units derived from a second monomer. In another embodiment, polymer A is preferably a polymer containing 70% to 90% by mass of structural units having an aromatic hydrocarbon group, and 10% to 25% by mass of structural units derived from a first monomer.

[0156] The polymer A may have a branched structure and / or an alicyclic structure in the side chain. By using a monomer containing a group having a branched structure in the side chain or a monomer containing a group having an alicyclic structure in the side chain, the branched structure or alicyclic structure can be introduced into the side chain of the polymer A. The alicyclic structure may be a monocyclic structure or a polycyclic structure.

[0157] Specific examples of monomers containing a group having a branched structure in the side chain include i-propyl (meth)acrylate, i-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, i-amyl (meth)acrylate, t-amyl (meth)acrylate, isoamyl (meth)acrylate, 2-octyl (meth)acrylate, 3-octyl (meth)acrylate, and t-octyl (meth)acrylate, etc. Among these, i-propyl (meth)acrylate, i-butyl (meth)acrylate, or t-butyl methacrylate is preferred, and i-propyl methacrylate or t-butyl methacrylate is more preferred.

[0158] Specific examples of monomers containing a group having an alicyclic structure in the side chain include monomers having a monocyclic aliphatic hydrocarbon group and monomers having a polycyclic aliphatic hydrocarbon group. In addition, (meth)acrylates having an alicyclic hydrocarbon group having 5 to 20 carbon atoms (number of carbon atoms) are also included. More specific examples include (bicyclo[2.2.1]heptyl-2)(meth)acrylate, 1-adamantyl (meth)acrylate, and 2-(meth)acrylate. Damantyl, 3-methyl-1-adamantyl (meth)acrylate, 3,5-dimethyl-1-adamantyl (meth)acrylate, 3-ethyladamantyl (meth)acrylate, 3-methyl-5-ethyl-1-adamantyl (meth)acrylate, 3,5,8-triethyl-1-adamantyl (meth)acrylate, 3,5-dimethyl-8-ethyl-1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, 2-ethyl-2-adamantyl (meth)acrylate, 3-hydroxy-1-adamantyl (meth)acrylate, octahydro-4,7-menthanoyl (meth)acrylate Inden-5-yl, octahydro-4,7-menthanoinden-1-ylmethyl (meth)acrylate, 1-menthyl (meth)acrylate, tricyclodecane (meth)acrylate, 3-hydroxy-2,6,6-trimethyl-bicyclo[3.1.1]heptyl (meth)acrylate, 3,7,7-trimethyl-4-hydroxy-bicyclo[4.1.0]heptyl (meth)acrylate, (nor)bornyl (meth)acrylate, isobornyl (meth)acrylate, fenchyl (meth)acrylate, 2,2,5-trimethylcyclohexyl (meth)acrylate, and cyclohexyl (meth)acrylate.

[0159] Among these (meth)acrylic acid esters, cyclohexyl (meth)acrylate, (nor)bornyl (meth)acrylate, isobornyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-adamantyl (meth)acrylate, fenchyl (meth)acrylate, 1-menthyl (meth)acrylate, or tricyclodecane (meth)acrylate is preferred, and cyclohexyl (meth)acrylate, (nor)bornyl (meth)acrylate, isobornyl (meth)acrylate, 2-adamantyl (meth)acrylate, or tricyclodecane (meth)acrylate is more preferred.

[0160] The photosensitive resin layer may contain one type of polymer A alone or two or more types. When the photosensitive resin layer contains two or more types of polymer A, it is preferable to use a mixture of two types of polymer A having an aromatic hydrocarbon group, or to use a mixture of a polymer A having an aromatic hydrocarbon group and a polymer A not having an aromatic hydrocarbon group. In the latter case, the content of the polymer A having an aromatic hydrocarbon group is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more, based on the total mass of the polymer A.

[0161] The synthesis of polymer A is preferably carried out by adding an appropriate amount of a radical polymerization initiator such as benzoyl peroxide or azoisobutyronitrile to a solution obtained by diluting one or more of the monomers described above with a solvent such as acetone, methyl ethyl ketone, or isopropanol, and heating and stirring the solution. In some cases, the synthesis is carried out while dropping a part of the mixture into the reaction solution. In some cases, the desired concentration is adjusted by adding more solvent after the reaction is completed. As a synthesis method, bulk polymerization, suspension polymerization, or emulsion polymerization may be used in addition to solution polymerization.

[0162] The glass transition temperature Tg of the polymer A is preferably 30° C. or more and 135° C. or less. By using the polymer A having a Tg of 135° C. or less in the photosensitive resin layer, it is possible to suppress line width thickening or deterioration of resolution when the focal position is shifted during exposure. From this viewpoint, the Tg of the polymer A is more preferably 130° C. or less, further preferably 120° C. or less, and particularly preferably 110° C. or less. In addition, it is preferable to use the polymer A having a Tg of 30° C. or more from the viewpoint of improving edge fuse resistance. From this viewpoint, the Tg of the polymer A is more preferably 40° C. or more, further preferably 50° C. or more, particularly preferably 60° C. or more, and most preferably 70° C. or more.

[0163] As the alkali-soluble resin, an alkali-soluble resin to be described later in the description of the thermoplastic resin layer may be used.

[0164] The alkali-soluble resins may be used alone or in combination of two or more.

[0165] The proportion of the alkali-soluble resin to the total mass of the photosensitive resin layer is preferably 10% by mass to 90% by mass, more preferably 30% by mass to 70% by mass, and even more preferably 40% by mass to 60% by mass. It is preferable to set the proportion of the alkali-soluble resin to the photosensitive resin layer to 90% by mass or less from the viewpoint of controlling the development time. On the other hand, it is preferable to set the proportion of the alkali-soluble resin to the photosensitive resin layer to 10% by mass or more from the viewpoint of improving edge fuse resistance.

[0166] The photosensitive resin layer may contain a resin other than an alkali-soluble resin. The resin other than an alkali-soluble resin may be a resin having a solubility of less than 0.1 g in 100 g of a 1% by mass aqueous solution of sodium carbonate at a liquid temperature of 22° C., and examples of the resin include acrylic resin, styrene-acrylic copolymer (with a styrene content of 40% by mass or less), polyurethane resin, polyvinyl alcohol, polyvinyl formal, polyamide resin, polyester resin, epoxy resin, polyacetal resin, polyhydroxystyrene resin, polyimide resin, polybenzoxazole resin, polysiloxane resin, polyethyleneimine, polyallylamine, and polyalkylene glycol.

[0167] <<Polymerizable compounds having ethylenic double bonds>> The photosensitive resin layer contains a polymerizable compound having an ethylenic double bond (hereinafter, also simply referred to as a "polymerizable compound"). The "polymerizable compound" refers to a compound that is polymerized by the action of a polymerization initiator and is different from the above-mentioned polymer.

[0168] The polymerizable compound is a compound having a polymerizable group having an ethylenic double bond. Examples of the polymerizable group having an ethylenic double bond include groups having an ethylenic unsaturated group such as vinyl group, acryloyl group, methacryloyl group, styryl group, and maleimide group. As the group having an ethylenic unsaturated group, acryloyl group or methacryloyl group is more preferred.

[0169] As the polymerizable compound, a compound having one or more ethylenically unsaturated groups (ethylenically unsaturated compound) is preferred, and a compound having two or more ethylenically unsaturated groups in one molecule (polyfunctional ethylenically unsaturated compound) is more preferred, in terms of superior resolution and peelability. In addition, the number of ethylenically unsaturated groups that the ethylenically unsaturated compound has in one molecule is preferably 6 or less, more preferably 3 or less, and even more preferably 2 or less, in terms of superior resolution and peelability.

[0170] In terms of a better balance between the photosensitivity, resolution, and peelability of the photosensitive resin layer, the photosensitive resin layer preferably contains a bifunctional or trifunctional ethylenically unsaturated compound having two or three ethylenically unsaturated groups in one molecule, and more preferably contains a bifunctional ethylenically unsaturated compound having two ethylenically unsaturated groups in one molecule. The content of the bifunctional ethylenically unsaturated compound relative to the total mass of the polymerizable compound is preferably 20% by mass or more, more preferably more than 40% by mass, and even more preferably 55% by mass or more, from the viewpoint of excellent peelability. The upper limit is not particularly limited, and may be 100% by mass. That is, all of the polymerizable compounds may be bifunctional ethylenically unsaturated compounds. In addition, the ethylenically unsaturated compound is preferably a (meth)acrylate compound having a (meth)acryloyl group as a polymerizable group.

[0171] The photosensitive resin layer preferably contains an ethylenically unsaturated compound B1 having an aromatic ring and two ethylenically unsaturated groups. The ethylenically unsaturated compound B1 is a bifunctional ethylenically unsaturated compound having one or more aromatic rings in one molecule among the above-mentioned ethylenically unsaturated compounds.

[0172] In the photosensitive resin layer, the mass ratio of the content of the ethylenically unsaturated compound B1 to the content of the ethylenically unsaturated compound is preferably 40% by mass or more, more preferably 50% by mass or more, even more preferably 55% by mass or more, and particularly preferably 60% by mass or more, from the viewpoint of better resolution. The upper limit is not particularly limited, but from the viewpoint of peelability, it is preferably 99% by mass or less, more preferably 95% by mass or less, even more preferably 90% by mass or less, and particularly preferably 85% by mass or less.

[0173] The aromatic ring of the ethylenically unsaturated compound B1 may be, for example, aromatic hydrocarbon rings such as benzene ring, naphthalene ring, anthracene ring, etc., aromatic heterocycles such as thiophene ring, furan ring, pyrrole ring, imidazole ring, triazole ring, pyridine ring, etc., and condensed rings thereof. Aromatic hydrocarbon rings are preferred, and benzene rings are more preferred. The aromatic ring may have a substituent. The ethylenically unsaturated compound B1 may have only one aromatic ring, or may have two or more aromatic rings.

[0174] The ethylenically unsaturated compound B1 preferably has a bisphenol structure, since it suppresses the swelling of the photosensitive resin layer caused by the developer, thereby improving the resolution. Examples of the bisphenol structure include the bisphenol A structure derived from bisphenol A (2,2-bis(4-hydroxyphenyl)propane), the bisphenol F structure derived from bisphenol F (2,2-bis(4-hydroxyphenyl)methane), and the bisphenol B structure derived from bisphenol B (2,2-bis(4-hydroxyphenyl)butane), and the bisphenol A structure is preferred.

[0175] Examples of the ethylenically unsaturated compound B1 having a bisphenol structure include a compound having a bisphenol structure and two polymerizable groups (preferably (meth)acryloyl groups) bonded to both ends of the bisphenol structure. The two polymerizable groups may be bonded directly to both ends of the bisphenol structure, or may be bonded via one or more alkyleneoxy groups. The alkyleneoxy groups added to both ends of the bisphenol structure are preferably ethyleneoxy groups or propyleneoxy groups, and more preferably ethyleneoxy groups. The number of alkyleneoxy groups added to the bisphenol structure is not particularly limited, but is preferably 4 to 16, more preferably 6 to 14 per molecule. The ethylenically unsaturated compound B1 having a bisphenol structure is described in paragraphs 0072 to 0080 of JP 2016-224162 A, and the contents of this publication are incorporated herein by reference.

[0176] As the ethylenically unsaturated compound B1, a bifunctional ethylenically unsaturated compound having a bisphenol A structure is preferable, and 2,2-bis(4-((meth)acryloxypolyalkoxy)phenyl)propane is more preferable. Examples of 2,2-bis(4-((meth)acryloxypolyalkoxy)phenyl)propane include 2,2-bis(4-(methacryloxydiethoxy)phenyl)propane (FA-324M, manufactured by Hitachi Chemical Co., Ltd.), 2,2-bis(4-(methacryloxyethoxypropoxy)phenyl)propane, 2,2-bis(4-(methacryloxypentaethoxy)phenyl)propane (BPE-500, manufactured by Shin-Nakamura Chemical Co., Ltd.), 2,2-bis(4-(methacryloxydodecaethoxy)phenyl)propane (BPE-500, manufactured by Shin-Nakamura Chemical Co., Ltd.), and 2,2-bis(4-(methacryloxydodecaethoxy)phenyl)propane (BPE-500, manufactured by Shin-Nakamura Chemical Co., Ltd.). Examples of such ethoxylated bisphenol A diacrylate include 2,2-bis(4-(methacryloxypentadecaethoxy)phenyl)propane (FA-3200MY, manufactured by Hitachi Chemical Co., Ltd.), 2,2-bis(4-(methacryloxypentadecaethoxy)phenyl)propane (BPE-1300, manufactured by Shin-Nakamura Chemical Co., Ltd.), 2,2-bis(4-(methacryloxydiethoxy)phenyl)propane (BPE-200, manufactured by Shin-Nakamura Chemical Co., Ltd.), and ethoxylated (10) bisphenol A diacrylate (NK Ester A-BPE-10, manufactured by Shin-Nakamura Chemical Co., Ltd.).

[0177] As the ethylenically unsaturated compound B1, from the viewpoints of the delay time line width change, the development temperature line width change, and the sensitivity, it is preferable to include a compound represented by the following formula (Bis).

[0178] [ka]

[0179] In formula (Bis), R1 and R2 each independently represent a hydrogen atom or a methyl group, A is C2H4, B is C3H6, n1 and n3 each independently represent an integer of 1 to 39, and n1+n3 is an integer of 2 to 40, n2 and n4 each independently represent an integer of 0 to 29, and n2+n4 is an integer of 0 to 30, and the arrangement of the repeating units of -(AO)- and -(BO)- may be random or block. In the case of block, either -(AO)- or -(BO)- may be on the bisphenol structure side. In one embodiment, n1+n2+n3+n4 is preferably an integer of 2 to 20, more preferably an integer of 2 to 16, and even more preferably an integer of 4 to 12. In addition, n2+n4 is preferably an integer of 0 to 10, more preferably an integer of 0 to 4, even more preferably an integer of 0 to 2, and particularly preferably 0.

[0180] The ethylenically unsaturated compound B1 may be used alone or in combination of two or more. The content of the ethylenically unsaturated compound B1 in the photosensitive resin layer is preferably 10% by mass or more, more preferably 20% by mass or more, based on the total mass of the photosensitive resin layer, from the viewpoint of better resolution. The upper limit is not particularly limited, but is preferably 70% by mass or less, more preferably 60% by mass or less, from the viewpoint of transferability and edge fusion (phenomenon in which components in the photosensitive resin layer bleed out from the edge of the transfer film).

[0181] The photosensitive resin layer may contain an ethylenically unsaturated compound other than the above-mentioned ethylenically unsaturated compound B1. The ethylenically unsaturated compound other than the ethylenically unsaturated compound B1 is not particularly limited and can be appropriately selected from known compounds. For example, a compound having one ethylenically unsaturated group in one molecule (monofunctional ethylenically unsaturated compound), a bifunctional ethylenically unsaturated compound without an aromatic ring, and a trifunctional or higher ethylenically unsaturated compound can be mentioned.

[0182] Examples of monofunctional ethylenically unsaturated compounds include ethyl (meth)acrylate, ethylhexyl (meth)acrylate, 2-(meth)acryloyloxyethyl succinate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and phenoxyethyl (meth)acrylate.

[0183] Examples of difunctional ethylenically unsaturated compounds having no aromatic ring include alkylene glycol di(meth)acrylate, polyalkylene glycol di(meth)acrylate, urethane di(meth)acrylate, and trimethylolpropane diacrylate.

[0184] Examples of alkylene glycol di(meth)acrylates include tricyclodecane dimethanol diacrylate (A-DCP, manufactured by Shin-Nakamura Chemical Co., Ltd.), tricyclodecane dimethanol dimethacrylate (DCP, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,9-nonanediol diacrylate (A-NOD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,6-hexanediol diacrylate (A-HD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), ethylene glycol dimethacrylate, 1,10-decanediol diacrylate, and neopentyl glycol di(meth)acrylate.

[0185] Examples of polyalkylene glycol di(meth)acrylates include polyethylene glycol di(meth)acrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, and polypropylene glycol di(meth)acrylate.

[0186] Examples of urethane di(meth)acrylate include propylene oxide modified urethane di(meth)acrylate, and ethylene oxide and propylene oxide modified urethane di(meth)acrylate. Examples of commercially available urethane di(meth)acrylate include 8UX-015A (manufactured by Taisei Fine Chemical Co., Ltd.), UA-32P (manufactured by Shin-Nakamura Chemical Co., Ltd.), and UA-1100H (manufactured by Shin-Nakamura Chemical Co., Ltd.).

[0187] Examples of trifunctional or higher ethylenically unsaturated compounds include dipentaerythritol (tri / tetra / penta / hexa)(meth)acrylate, pentaerythritol (tri / tetra)(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, trimethylolethane tri(meth)acrylate, isocyanuric acid tri(meth)acrylate, glycerin tri(meth)acrylate, and alkylene oxide modified products thereof. "(Tri / tetra / penta / hexa)(meth)acrylate" is a concept that includes tri(meth)acrylate, tetra(meth)acrylate, penta(meth)acrylate, and hexa(meth)acrylate, and "(tri / tetra)(meth)acrylate" is a concept that includes tri(meth)acrylate and tetra(meth)acrylate. In one embodiment, a photosensitive The layer preferably contains the above-mentioned ethylenically unsaturated compound B1 and a trifunctional or higher ethylenically unsaturated compound, and more preferably contains the above-mentioned ethylenically unsaturated compound B1 and two or more trifunctional or higher ethylenically unsaturated compounds. In this case, the mass ratio of the ethylenically unsaturated compound B1 to the trifunctional or higher ethylenically unsaturated compound is preferably (total mass of the ethylenically unsaturated compound B1):(total mass of the trifunctional or higher ethylenically unsaturated compound)=1:1 to 5:1, more preferably 1.2:1 to 4:1, and even more preferably 1.5:1 to 3:1. In one embodiment, the photosensitive resin layer preferably contains the above-mentioned ethylenically unsaturated compound B1 and two or more trifunctional ethylenically unsaturated compounds.

[0188] Examples of alkylene oxide modified trifunctional or higher ethylenically unsaturated compounds include caprolactone modified (meth)acrylate compounds (KAYARAD (registered trademark) DPCA-20 manufactured by Nippon Kayaku Co., Ltd., A-9300-1CL manufactured by Shin-Nakamura Chemical Co., Ltd., etc.), alkylene oxide modified (meth)acrylate compounds (KAYARAD RP-1040 manufactured by Nippon Kayaku Co., Ltd., ATM-35E and A-9300 manufactured by Shin-Nakamura Chemical Co., Ltd., EBECRYL (registered trademark) 135 manufactured by Daicel-Allnex Corporation, etc.), ethoxylated glycerin triacrylate (A-GLY-9E manufactured by Shin-Nakamura Chemical Co., Ltd., etc.), ARONIX (registered trademark) TO-2349 (manufactured by Toagosei Co., Ltd.), ARONIX M-520 (manufactured by Toagosei Co., Ltd.), and ARONIX M-510 (manufactured by Toagosei Co., Ltd.).

[0189] As the ethylenically unsaturated compound other than the ethylenically unsaturated compound B1, an ethylenically unsaturated compound having an acid group described in paragraphs 0025 to 0030 of JP-A No. 2004-239942 may be used.

[0190] From the viewpoints of resolution and linearity, the ratio of the content of the alkali-soluble resin to the content of the ethylenically unsaturated compound in the photosensitive resin layer is preferably 1.0 or less, more preferably 0.9 or less, and even more preferably 0.5 or more and 0.9 or less.

[0191] From the viewpoints of curability and resolution, the ethylenically unsaturated compound in the photosensitive resin layer preferably contains a (meth)acrylic compound, and more preferably contains a (meth)acrylate compound. From the viewpoints of curability, resolution and linearity, the ethylenically unsaturated compound in the photosensitive resin layer more preferably contains a (meth)acrylic compound, and the content of the acrylic compound relative to the total mass of the (meth)acrylic compound contained in the photosensitive resin layer is 60 mass% or less.

[0192] The molecular weight (weight average molecular weight (Mw) when the molecular weight has a distribution) of the ethylenically unsaturated compound including the ethylenically unsaturated compound B1 is preferably from 200 to 3,000, more preferably from 280 to 2,200, and even more preferably from 300 to 2,200.

[0193] The polymerizable compound may be used alone or in combination of two or more. The content of the polymerizable compound in the photosensitive resin layer is preferably 10% by mass to 70% by mass, more preferably 20% by mass to 60% by mass, and further preferably 20% by mass to 50% by mass, based on the total mass of the photosensitive resin layer.

[0194] <<Photopolymerization initiator>> The photosensitive resin layer contains a photopolymerization initiator. Examples of the photopolymerization initiator include a photoradical polymerization initiator and a photocationic polymerization initiator.

[0195] The photopolymerization initiator is a compound that initiates polymerization of a polymerizable compound when exposed to active light such as ultraviolet light, visible light, and X-rays. The photopolymerization initiator is not particularly limited, and any known photopolymerization initiator can be used. As the photopolymerization initiator, a photoradical polymerization initiator is preferred.

[0196] Examples of the photoradical polymerization initiator include a photopolymerization initiator having an oxime ester structure, a photopolymerization initiator having a biimidazole structure, a photopolymerization initiator having an α-aminoalkylphenone structure, a photopolymerization initiator having an α-hydroxyalkylphenone structure, a photopolymerization initiator having an acylphosphine oxide structure, and a photopolymerization initiator having an N-phenylglycine structure.

[0197] From the viewpoints of photosensitivity, visibility and resolution of exposed and non-exposed parts, the photosensitive resin layer preferably contains a photopolymerization initiator having a biimidazole structure as a photoradical polymerization initiator, and more preferably contains a hexaarylbisimidazole-based photopolymerization initiator. Specifically, the photoradical polymerization initiator preferably contains at least one selected from the group consisting of 2,4,5-triarylimidazole dimers and derivatives thereof. Note that the two 2,4,5-triarylimidazole structures in the 2,4,5-triarylimidazole dimers and derivatives thereof may be the same or different. Examples of derivatives of 2,4,5-triarylimidazole dimers include 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, and 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer.

[0198] As the photoradical polymerization initiator, for example, the polymerization initiators described in paragraphs 0031 to 0042 of JP-A No. 2011-95716 and paragraphs 0064 to 0081 of JP-A No. 2015-14783 may be used.

[0199] Examples of the photoradical polymerization initiator include ethyl dimethylaminobenzoate (DBE, CAS No. 10287-53-3), benzoin methyl ether, anisyl (p,p'-dimethoxybenzyl), TAZ-110 (trade name: manufactured by Midori Chemical Industry Co., Ltd.), benzophenone, TAZ-111 (trade name: manufactured by Midori Chemical Industry Co., Ltd.), Irgacure OXE01, OXE02, OXE03, OXE04 (manufactured by BASF), Omnirad 651 and 369 (trade names: manufactured by IGM Resins BV), and 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0200] Commercially available photoradical polymerization initiators include, for example, 1-[4-(phenylthio)phenyl]-1,2-octanedione-2-(O-benzoyloxime) (trade name: IRGACURE (registered trademark) OXE-01, manufactured by BASF), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone-1-(O-acetyloxime) (trade name: IRGACURE OXE-02, manufactured by BASF), and IRGACURE OXE-03 (manufactured by BASF), 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone (trade name: Omnirad 379EG, manufactured by IGM Resins BV), 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one (trade name: Omnirad 907, manufactured by IGM Resins BV), 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropan-1-one (trade name: Omnirad 127, manufactured by IGM Resins BV), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1 (trade name: Omnirad 369, manufactured by IGM Resins BV) BV), 2-hydroxy-2-methyl-1-phenylpropan-1-one (trade name: Omnirad 1 173, manufactured by IGM Resins BV), 1-hydroxycyclohexyl phenyl ketone (trade name: Omnirad 184, manufactured by IGM Resins BV), 2,2-dimethoxy-1,2-diphenylethan-1-one (trade name: Omnirad 651, manufactured by IGM Resins BV), 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (trade name: Omnirad TPO H, manufactured by IGM Resins BV), bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (trade name: Omnirad 819, manufactured by IGM Resins BV), oxime ester photoinitiator (trade name: Lunar 6, manufactured by DKSH Japan Co., Ltd.), 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbisimidazole (2-(2-chlorophenyl)-4,5-diphenylimidazole dimer) (trade name: B-CIM, manufactured by Hampford Chemical Industry Co., Ltd.), and 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer (trade name: BCTB, manufactured by Tokyo Chemical Industry Co., Ltd.), 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer (trade name: BCTB, manufactured by Tokyo Chemical Industry Co., Ltd.), 1-[4-(phenylthio)phenyl]-3-cyclopentylpropane-1,2-dione-2-(O -benzoyloxime) (trade name: TR-PBG-305, manufactured by Changzhou Strong Electronic New Materials Co., Ltd.), 1,2-propanedione, 3-cyclohexyl-1-[9-ethyl-6-(2-furanylcarbonyl)-9H-carbazol-3-yl]-, 2-(O-acetyloxime) (trade name: TR-PBG-326, manufactured by Changzhou Strong Electronic New Materials Co., Ltd.), and 3-cyclohexyl-1-(6-(2-(benzoyloxyimino)hexanoyl)-9-ethyl-9H-carbazol-3-yl)-propane-1,2-dione-2-(O-benzoyloxime) (trade name: TR-PBG-391, manufactured by Changzhou Strong Electronic New Materials Co., Ltd.).

[0201] A photocationic polymerization initiator (photoacid generator) is a compound that generates an acid when exposed to actinic rays. As the photocationic polymerization initiator, a compound that responds to actinic rays having a wavelength of 300 nm or more, preferably 300 to 450 nm, and generates an acid is preferred, but the chemical structure is not limited. In addition, even if a photocationic polymerization initiator is not directly sensitive to actinic rays having a wavelength of 300 nm or more, it can be preferably used in combination with a sensitizer as long as it responds to actinic rays having a wavelength of 300 nm or more and generates an acid when used in combination with a sensitizer.

[0202] As the photocationic polymerization initiator, a photocationic polymerization initiator that generates an acid having a pKa of 4 or less is preferable, a photocationic polymerization initiator that generates an acid having a pKa of 3 or less is more preferable, and a photocationic polymerization initiator that generates an acid having a pKa of 2 or less is particularly preferable. The lower limit of the pKa is not particularly set, but is preferably, for example, -10.0 or more.

[0203] Examples of the photocationic polymerization initiator include ionic photocationic polymerization initiators and nonionic photocationic polymerization initiators. Examples of the ionic photocationic polymerization initiator include onium salt compounds such as diaryliodonium salts and triarylsulfonium salts, and quaternary ammonium salts. Examples of the ionic photocationic polymerization initiator include the ionic photocationic polymerization initiators described in paragraphs 0114 to 0133 of JP-A-2014-85643. Examples of the nonionic photocationic polymerization initiator include trichloromethyl-s-triazines, diazomethane compounds, imide sulfonate compounds, and oxime sulfonate compounds. Examples of the trichloromethyl-s-triazines, diazomethane compounds, and imide sulfonate compounds include the compounds described in paragraphs 0083 to 0088 of JP-A-2011-221494. In addition, as the oxime sulfonate compound, the compounds described in paragraphs 0084 to 0088 of WO 2018 / 179640 may be used.

[0204] The photosensitive resin layer is lightThe polymerization initiator may be contained alone or in combination of two or more. light The content of the polymerization initiator is not particularly limited, but is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1.0% by mass or more, based on the total mass of the photosensitive resin layer. The upper limit is not particularly limited, but is preferably 10% by mass or less, and more preferably 5% by mass or less, based on the total mass of the photosensitive resin layer.

[0205] <<Sensitizer>> The photosensitive resin layer preferably further contains a sensitizer. The sensitizer is not particularly limited, and known sensitizers, dyes, and pigments can be used. Examples of the sensitizer include benzophenone-based sensitizers such as dialkylaminobenzophenone compounds, pyrazoline compounds, anthracene compounds, coumarin compounds, xanthone compounds, thioxanthone compounds, acridone compounds, oxazole compounds, benzoxazole compounds, thiazole compounds, benzothiazole compounds, triazole compounds (e.g., 1,2,4-triazole), stilbene compounds, triazine compounds, thiophene compounds, naphthalimide compounds, triarylamine compounds, and aminoacridine compounds.

[0206] As the sensitizer, from the viewpoint of sensitizing effect and transparency at the maximum sensitivity wavelength, a benzophenone-based sensitizer is preferred. Benzophenone-based sensitizers have a high sensitizing effect and can provide high sensitivity with a small amount added, so that the transparency at the maximum sensitivity wavelength is high, and photomask fidelity and line width stability are improved, which is preferable. The benzophenone sensitizer is a sensitizer made of a compound having a benzophenone skeleton.

[0207] The sensitizer may be used alone or in combination of two or more kinds. When the photosensitive resin layer contains a sensitizer, the content of the sensitizer can be appropriately selected depending on the purpose, but from the viewpoints of improving the sensitivity to the light source and improving the curing speed by the balance between the polymerization speed and the chain transfer, the content is preferably 0.01% by mass to 5% by mass, more preferably 0.05% by mass to 1% by mass, based on the total mass of the photosensitive resin layer.

[0208] The value obtained by dividing the content of the photopolymerization initiator in the photosensitive resin layer by the content of the sensitizer in the photosensitive resin layer is, from the viewpoints of the sensitizing effect and the transparency at the maximum sensitivity wavelength, preferably from 20 to 300, more preferably from 30 to 300, and even more preferably from 100 to 200, by mass.

[0209] When the film thickness of the photosensitive resin layer is X μm and the content of the sensitizer in the photosensitive resin layer is Y mass %, the value obtained by multiplying the value of X and the value of Y and then multiplying the result by 10 is preferably 0.5 to 5.0, more preferably 0.5 to 3.0, and even more preferably 0.5 to 2.0.

[0210] <<Dye>> From the viewpoints of visibility of exposed and unexposed parts, pattern visibility after development, and resolution, the photosensitive resin layer preferably contains a dye, and more preferably contains a dye (also simply referred to as "dye N") whose maximum absorption wavelength in the wavelength range of 400 nm to 780 nm during color development is 450 nm or more and whose maximum absorption wavelength changes with an acid, a base, or a radical. When dye N is contained, the adhesion with adjacent layers (for example, a temporary support and an intermediate layer) is improved, and the resolution is more excellent, although the detailed mechanism is unknown.

[0211] In the present disclosure, the maximum absorption wavelength of a dye "changes with an acid, base, or radical" may mean any of the following: a dye in a colored state is decolorized by an acid, base, or radical, a dye in a decolorized state is colored by an acid, base, or radical, and a dye in a colored state is changed to a colored state of another hue. Specifically, the dye N may be a compound that changes from a decolorized state to a colored state by exposure, or a compound that changes from a colored state to a decolorized state by exposure. In this case, the dye may be a dye whose colored or decolored state changes when an acid, base, or radical is generated and acts in the photosensitive resin layer by exposure, or a dye whose colored or decolored state changes when the state (e.g., pH) in the photosensitive resin layer changes by an acid, base, or radical. The dye may also be a dye whose colored or decolored state changes when it is directly stimulated by an acid, base, or radical without exposure.

[0212] Among these, from the viewpoints of the visibility and resolution of exposed and unexposed areas, dye N is preferably a dye whose maximum absorption wavelength changes in response to an acid or a radical, and more preferably a dye whose maximum absorption wavelength changes in response to a radical.

[0213] From the viewpoints of visibility of exposed and unexposed areas and resolution, the photosensitive resin layer preferably contains both a dye N whose maximum absorption wavelength changes due to radicals, and a photoradical polymerization initiator.

[0214] From the viewpoint of visibility of exposed and unexposed areas, dye N is preferably a dye that develops color in response to an acid, a base, or a radical.

[0215] An example of the color-developing mechanism of dye N in the present disclosure is an embodiment in which a photoradical polymerization initiator, a cationic photopolymerization initiator (photoacid generator), or a photobase generator is added to a photosensitive resin layer, and after exposure, a radical-reactive dye, an acid-reactive dye, or a base-reactive dye (e.g., a leuco dye) develops color due to a radical, acid, or base generated from the photoradical polymerization initiator, the photocationic photopolymerization initiator, or the photobase generator.

[0216] From the viewpoint of visibility of exposed and non-exposed parts, the dye N preferably has a maximum absorption wavelength of 550 nm or more in the wavelength range of 400 nm to 780 nm when colored, more preferably 550 nm to 700 nm, and even more preferably 550 nm to 650 nm. Furthermore, the dye N may have only one maximum absorption wavelength in the wavelength range of 400 nm to 780 nm when colored, or may have two or more maximum absorption wavelengths. When the dye N has two or more maximum absorption wavelengths in the wavelength range of 400 nm to 780 nm when colored, it is sufficient that the maximum absorption wavelength with the highest absorbance among the two or more maximum absorption wavelengths is 450 nm or more.

[0217] The maximum absorption wavelength of dye N is determined by measuring the transmission spectrum of a solution containing dye N (liquid temperature 25°C) in the range of 400 nm to 780 nm using a spectrophotometer UV3100 (manufactured by Shimadzu Corporation) in an air atmosphere, and detecting the wavelength at which the light intensity is minimal (maximum absorption wavelength). This is obtained by:

[0218] Examples of the dye that develops or loses color upon exposure include leuco compounds. Examples of the dye that loses color upon exposure include leuco compounds, diarylmethane dyes, oxazine dyes, xanthene dyes, iminonaphthoquinone dyes, azomethine dyes, and anthraquinone dyes. As the dye N, a leuco compound is preferred from the viewpoint of visibility of exposed and non-exposed areas.

[0219] Examples of the leuco compound include a leuco compound having a triarylmethane skeleton (triarylmethane dye), a leuco compound having a spiropyran skeleton (spiropyran dye), a leuco compound having a fluoran skeleton (fluoran dye), a leuco compound having a diarylmethane skeleton (diarylmethane dye), a leuco compound having a rhodamine lactam skeleton (rhodamine lactam dye), a leuco compound having an indolylphthalide skeleton (indolylphthalide dye), and a leuco compound having a leucoauramine skeleton (leucoauramine dye). Among them, triarylmethane dye or fluoran dye is preferable, and a leuco compound having a triphenylmethane skeleton (triphenylmethane dye) or fluoran dye is more preferable.

[0220] From the viewpoint of visibility of the exposed and non-exposed parts, the leuco compound preferably has a lactone ring, a sultine ring, or a sultone ring. This allows the lactone ring, the sultine ring, or the sultone ring of the leuco compound to react with a radical generated from a photoradical polymerization initiator or an acid generated from a photocationic polymerization initiator, thereby changing the leuco compound to a ring-closed state to cause discoloration, or changing the leuco compound to a ring-open state to cause color development. The leuco compound is preferably a compound having a lactone ring, a sultine ring, or a sultone ring, which is opened by a radical or an acid to develop color, and more preferably a compound having a lactone ring, which is opened by a radical or an acid to develop color.

[0221] Examples of the pigment N include dyes. Examples of the dyes include brilliant green, ethyl violet, methyl green, crystal violet, basic fuchsin, methyl violet 2B, quinaldine red, rose bengal, metanil yellow, thymolsulfophthalein, xylenol blue, methyl orange, paramethyl red, Congo red, benzopurpurin 4B, α-naphthyl red, Nile blue 2B, Nile blue A, methyl violet, malachite green, parafuchsin, Victoria Pure Blue-naphthalenesulfonate, Victoria Pure Blue BOH (manufactured by Hodogaya Chemical Industry Co., Ltd.), Oil Blue #603 (manufactured by Orient Chemical Industry Co., Ltd.), Oil Pink #312 (manufactured by Orient Chemical Industry Co., Ltd.), Oil Red 5B (manufactured by Orient Chemical Industry Co., Ltd.), Oil Scarlet #308 (manufactured by Orient Chemical Industry Co., Ltd.), and the like. Examples of the oil-soluble pigments include 4-p-diethylaminophenylimino naphthoquinone, 2-carboxyanilino-4-p-diethylaminophenylimino naphthoquinone, 2-carboxystearylamino-4-pN,N-bis(hydroxyethyl)amino-phenylimino naphthoquinone, 1-phenyl-3-methyl-4-p-diethylaminophenylimino-5-pyrazolone, and 1-β-naphthyl-4-p-diethylaminophenylimino-5-pyrazolone.

[0222] Examples of the dye N include leuco compounds. Examples of the leuco compounds include p,p',p"-hexamethyltriaminotriphenylmethane (leuco crystal violet), Pergascript Blue SRB (manufactured by BASF), crystal violet lactone, malachite green lactone, benzoyl leuco methylene blue, 2-(N-phenyl-N-methylamino)-6-(Np-tolyl-N-ethyl)aminofluoran, 2-anilino-3-methyl-6-(N-ethyl-p-toluidino)fluoran, 3,6-dimethoxyfluoran, 3-(N,N-diethylamino)-5-methyl-7-(N,N-dibenzylamino)fluoran, 3-(N-cyclohexyl-N-methylamino)-6- Methyl-7-anilinofluoran, 3-(N,N-diethylamino)-6-methyl-7-anilinofluoran, 3-(N,N-diethylamino)-6-methyl-7-xylidinofluoran, 3-(N,N-diethylamino)-6-methyl-7-chlorofluoran, 3-(N,N-diethylamino)-6-methoxy-7-aminofluoran, 3-(N,N-diethylamino)-7-(4-chloroanilino)fluoran, 3-(N,N-diethylamino)-7-chlorofluoran, 3-(N,N-diethylamino)- 3-(N,N-diethylamino)-7-benzylaminofluoran, 3-(N,N-diethylamino)-7,8-benzofluoran, 3-(N,N-dibutylamino)-6-methyl-7-anilinofluoran, 3-(N,N-dibutylamino)-6-methyl-7-xylidinofluoran, 3-piperidino-6-methyl-7-anilinofluoran, 3-pyrrolidino-6-methyl-7-anilinofluoran, 3,3-bis(1-ethyl-2-methylindol-3-yl)phthalide, 3,3-bis(1-n-butyl-2-methylindol-3-yl)phthalide, Indol-3-yl)phthalide, 3,3-bis(p-dimethylaminophenyl)-6-dimethylaminophthalide, 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(4-diethylaminophenyl)-3-(1-ethyl-2-methylindol-3-yl)phthalide, and 3',6'-bis(diphenylamino)spiroisobenzofuran-1(3H),9'-[9H]xanthen-3-one.

[0223] From the viewpoints of visibility of exposed and unexposed areas, pattern visibility after development, and resolution, dye N is preferably a dye whose maximum absorption wavelength changes in response to radicals, and more preferably a dye that develops color in response to radicals.

[0224] As dye N, leuco crystal violet, crystal violet lactone, brilliant green, or Victoria Pure Blue-naphthalenesulfonate is preferred.

[0225] The dye may be used alone or in combination of two or more. The content of the dye is preferably 0.1% by mass or more, more preferably 0.1% by mass to 10% by mass, even more preferably 0.1% by mass to 5% by mass, and particularly preferably 0.1% by mass to 1% by mass, based on the total mass of the photosensitive resin layer, from the viewpoints of visibility of the exposed and non-exposed parts, pattern visibility after development, and resolution. The content of the dye N is preferably 0.1% by mass or more, more preferably 0.1% by mass to 10% by mass, even more preferably 0.1% by mass to 5% by mass, and particularly preferably 0.1% by mass to 1% by mass, based on the total mass of the photosensitive resin layer, from the viewpoints of visibility of the exposed and non-exposed parts, pattern visibility after development, and resolution.

[0226] The content of dye N means the content of dye when all of the dye N contained in the photosensitive resin layer is in a colored state. The following describes a method for quantifying the content of dye N, taking a dye that is colored by radicals as an example. Two types of solutions are prepared by dissolving 0.001 g or 0.01 g of dye in 100 mL of methyl ethyl ketone. A photoradical polymerization initiator Irgacure OXE01 (product name, manufactured by BASF) is added to each of the obtained solutions, and radicals are generated by irradiating light of 365 nm to cause all of the dyes to be in a colored state. Thereafter, the absorbance of each solution at a liquid temperature of 25°C is measured using a spectrophotometer (UV3100, manufactured by Shimadzu Corporation) in an air atmosphere, and a calibration curve is created. Next, the absorbance of the solution in which all of the dyes have been colored is measured in the same manner as above, except that 3 g of the photosensitive resin layer is dissolved in methyl ethyl ketone instead of the dye. The content of the dye contained in the photosensitive resin layer is calculated from the absorbance of the obtained solution containing the photosensitive resin layer based on a calibration curve.

[0227] <<Thermal crosslinkable compounds>> The photosensitive resin layer preferably contains a thermally crosslinkable compound from the viewpoints of the strength of the resulting cured film and the adhesion of the resulting uncured film. Note that a thermally crosslinkable compound having an ethylenically unsaturated group, which will be described later, is not treated as an ethylenically unsaturated compound but as a thermally crosslinkable compound.

[0228] Examples of the thermal crosslinking compound include methylol compounds and blocked isocyanate compounds. Among them, blocked isocyanate compounds are preferred from the viewpoint of the strength of the obtained cured film and the adhesion of the obtained uncured film. Since blocked isocyanate compounds react with hydroxyl groups and carboxyl groups, for example, when an alkali-soluble resin and / or an ethylenically unsaturated compound has at least one of a hydroxyl group and a carboxyl group, the hydrophilicity of the formed film decreases, and the function of the film obtained by curing the photosensitive resin layer when used as a protective film tends to be enhanced. The blocked isocyanate compound refers to a compound having a structure in which the isocyanate group of an isocyanate is protected (so-called masked) with a blocking agent.

[0229] The dissociation temperature of the blocked isocyanate compound is not particularly limited, but is preferably 100°C to 160°C, and more preferably 130°C to 150°C. The dissociation temperature of the blocked isocyanate means "the temperature of the endothermic peak accompanying the deprotection reaction of the blocked isocyanate when measured by DSC (Differential Scanning Calorimetry) analysis using a differential scanning calorimeter." As the differential scanning calorimeter, for example, a differential scanning calorimeter (model: DSC6200) manufactured by Seiko Instruments Inc. can be suitably used. However, the differential scanning calorimeter is not limited thereto.

[0230] Examples of blocking agents having a dissociation temperature of 100° C. to 160° C. include active methylene compounds [malonic acid diesters (dimethyl malonate, diethyl malonate, di-n-butyl malonate, di-2-ethylhexyl malonate, etc.)] and oxime compounds (formaldoxime, acetaldoxime, acetoxime, methyl ethyl ketoxime, cyclohexanone oxime, and other compounds having a structure represented by -C(=N-OH)- in the molecule). Among these, blocking agents having a dissociation temperature of 100° C. to 160° C. preferably contain oxime compounds, for example, from the viewpoint of storage stability.

[0231] The blocked isocyanate compound preferably has an isocyanurate structure, for example, from the viewpoint of improving the brittleness of the film and improving the adhesion to the transfer target. The blocked isocyanurate compound having an isocyanurate structure can be obtained, for example, by protecting hexamethylene diisocyanate by isocyanuration. Among the blocked isocyanate compounds having an isocyanurate structure, a compound having an oxime structure using an oxime compound as a blocking agent is preferred from the viewpoints that it is easier to set the dissociation temperature in a preferred range and to reduce development residues than a compound not having an oxime structure.

[0232] The blocked isocyanate compound may have a polymerizable group. The polymerizable group is not particularly limited, and a known polymerizable group can be used, and a radical polymerizable group is preferable. The polymerizable group includes an ethylenically unsaturated group such as a (meth)acryloxy group, a (meth)acrylamide group, or a styryl group, and a group having an epoxy group such as a glycidyl group. Among them, the polymerizable group is preferably an ethylenically unsaturated group, more preferably a (meth)acryloxy group, and even more preferably an acryloxy group.

[0233] As the blocked isocyanate compound, commercially available products can be used. Examples of commercially available blocked isocyanate compounds include Karenz (registered trademark) AOI-BM, Karenz (registered trademark) MOI-BM, Karenz (registered trademark) MOI-BP, etc. (all manufactured by Showa Denko K.K.), and blocked Duranate series (e.g., Duranate (registered trademark) TPA-B80E, Duranate (registered trademark) WT32-B75P, etc., manufactured by Asahi Kasei Chemicals Corporation). In addition, compounds having the following structure can also be used as the blocked isocyanate compound.

[0234] [ka]

[0235] The thermal crosslinking compound may be used alone or in combination of two or more. When the photosensitive resin layer contains a thermal crosslinking compound, the content of the thermal crosslinking compound is preferably 1% by mass to 50% by mass, more preferably 5% by mass to 30% by mass, based on the total mass of the photosensitive resin layer.

[0236] <<Other ingredients>> The photosensitive resin layer may contain other components. Examples of the other components include radical polymerization inhibitors, surfactants, various additives, etc. The other components may be used alone or in combination of two or more.

[0237] - Radical polymerization inhibitor - The photosensitive resin layer may contain a radical polymerization inhibitor. Examples of the radical polymerization inhibitor include the thermal polymerization inhibitors described in paragraph 0018 of Japanese Patent No. 4502784. Among them, phenothiazine, phenoxazine, or 4-methoxyphenol is preferable. Other radical polymerization inhibitors include naphthylamine, cuprous chloride, nitrosophenylhydroxyamine aluminum salt, and diphenylnitrosamine. In order not to impair the sensitivity of the photosensitive resin layer, it is preferable to use nitrosophenylhydroxyamine aluminum salt as the radical polymerization inhibitor.

[0238] The radical polymerization inhibitor may be used alone or in combination of two or more. When the photosensitive resin layer contains a radical polymerization inhibitor, the content of the radical polymerization inhibitor is preferably 0.001% by mass to 5.0% by mass, more preferably 0.01% by mass to 3.0% by mass, and even more preferably 0.02% by mass to 2.0% by mass, based on the total mass of the photosensitive resin layer. The content of the radical polymerization inhibitor is preferably 0.005% by mass to 5.0% by mass, more preferably 0.01% by mass to 3.0% by mass, and even more preferably 0.01% by mass to 1.0% by mass, based on the total mass of the polymerizable compound.

[0239] -Surfactants- The photosensitive resin layer may contain a surfactant. Examples of the surfactant include those described in paragraph 0017 of Japanese Patent No. 4502784 and paragraphs 0060 to 0071 of JP-A-2009-237362. The surfactant is preferably a nonionic surfactant, a fluorine-based surfactant, or a silicone-based surfactant.

[0240] Examples of nonionic surfactants include glycerol, trimethylolpropane, trimethylolethane, and their ethoxylates and propoxylates (e.g., glycerol propoxylate, glycerol ethoxylate, etc.), polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, polyethylene glycol dilaurate, polyethylene glycol distearate, sorbitan fatty acid esters, Pluronic (trade name) L10, L 31, L61, L62, 10R5, 17R2, 25R2 (all manufactured by BASF), Tetronic (trade name) 304, 701, 704, 901, 904, 150R1 (all manufactured by BASF), Solsperse (trade name) 20000 (all manufactured by Lubrizol Japan Co., Ltd.), NCW-101, NCW-1001, NCW-1002 (all manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd.), Paionin (trade name) D-6112, D-6112-W, D-6315 (all manufactured by Takemoto Oil Co., Ltd.), Olfin E1010, Surfynol 104, 400, 440 (all manufactured by Nissin Chemical Industry Co., Ltd.).

[0241] Commercially available fluorine-based surfactants include, for example, Megafac (product name) F-171, F-172, F-173, F-176, F-177, F-141, F-142, F-143, F-144, F-437, F-444, F-475, F-477, F-479, F-482, F-551-A, F-552, F-554, F -555-A, F-556, F-557, F-558, F-559, F-560, F-561, F-565, F-563, F-568, F-575, F-780 , EXP, MFS-330, R-41, R-41-LM, R-01, R-40, R-40-LM, RS-43, TF-1956, RS-90, R-94, RS-7 Examples of such products include 2-K and DS-21 (manufactured by DIC Corporation), Fluorad (trade name) FC430, FC431, and FC171 (manufactured by Sumitomo 3M Limited), Surflon (trade name) S-382, SC-101, SC-103, SC-104, SC-105, SC-1068, SC-381, SC-383, S-393, and KH-40 (manufactured by AGC Inc.), PolyFox (trade name) PF636, PF656, PF6320, PF6520, and PF7002 (manufactured by OMNOVA), and Futergent (trade name) 710FM, 610FM, 601AD, 601ADH2, 602A, 215M, and 245F (manufactured by NEOS Corporation).

[0242] In addition, the fluorosurfactant may be an acrylic compound that has a molecular structure with a functional group containing a fluorine atom, and when heat is applied, the functional group containing the fluorine atom is cut and the fluorine atom is volatilized. Examples of such fluorosurfactants include the Megafac (product name) DS series manufactured by DIC Corporation (The Chemical Daily (February 22, 2016), Nikkei Business Daily (February 23, 2016)), for example, Megafac (product name) DS-21.

[0243] As the fluorine-based surfactant, it is also preferable to use a polymer of a fluorine atom-containing vinyl ether compound having a fluorinated alkyl group or a fluorinated alkylene ether group and a hydrophilic vinyl ether compound.

[0244] As the fluorine-based surfactant, a block polymer can also be used. As the fluorine-based surfactant, a fluorine-containing polymer compound containing a constitutional unit derived from a (meth)acrylate compound having a fluorine atom and a constitutional unit derived from a (meth)acrylate compound having two or more (preferably five or more) alkyleneoxy groups (preferably ethyleneoxy groups, propyleneoxy groups) can also be preferably used.

[0245] As the fluorine-based surfactant, a fluorine-containing polymer having an ethylenically unsaturated group in the side chain can be used, such as Megafac (product name) RS-101, RS-102, RS-718K, and RS-72-K (all manufactured by DIC Corporation).

[0246] As the fluorosurfactant, for example, a compound having a linear perfluoroalkyl group having 7 or more carbon atoms may be used. However, from the viewpoint of improving environmental compatibility, it is preferable to use an alternative material to perfluorooctanoic acid (PFOA) or perfluorooctanesulfonic acid (PFOS) as the fluorosurfactant.

[0247] Examples of silicone surfactants include linear polymers consisting of siloxane bonds, and modified siloxane polymers having organic groups introduced into the side chains or ends. Specific examples of silicone surfactants include DOWSIL (trade name) 8032 ADDITIVE, Toray Silicone DC3PA, Toray Silicone SH7PA, Toray Silicone DC11PA, Toray Silicone SH21PA, Toray Silicone SH28PA, Toray Silicone SH29PA, Toray Silicone SH30PA, and Toray Silicone SH8400 (all manufactured by Toray Dow Corning Co., Ltd.), as well as X-22-4952, X-22-4272, X-22-6266, KF-351A, K354L, KF-355A, KF -945, KF-640, KF-642, KF-643, X-22-6191, X-22-4515, KF-6004, KP-341, KF-6001, KF-6002 (all manufactured by Shin-Etsu Chemical Co., Ltd.), F-4440, TSF-4300, TSF-4445, TSF-4460, TSF-4452 (all manufactured by Momentive Performance Materials), BYK307, BYK323, BYK330 (all manufactured by BYK-Chemie).

[0248] The photosensitive resin layer may contain one type of surfactant alone or two or more types of surfactants. The content of the surfactant is preferably 0.001% by mass to 10% by mass, and more preferably 0.01% by mass to 3% by mass, based on the total mass of the photosensitive resin layer.

[0249] -Additives- The photosensitive resin layer may contain known additives as necessary. Examples of additives include plasticizers, heterocyclic compounds, benzotriazoles, carboxybenzotriazoles, pyridines (isonicotinamide, etc.), purine bases (adenine, etc.), and solvents. The photosensitive resin layer may contain one type of each additive alone, or two or more types.

[0250] Examples of benzotriazoles include 1,2,3-benzotriazole, 1-chloro-1,2,3-benzotriazole, bis(N-2-ethylhexyl)aminomethylene-1,2,3-benzotriazole, bis(N-2-ethylhexyl)aminomethylene-1,2,3-tolyltriazole, and bis(N-2-hydroxyethyl)aminomethylene-1,2,3-benzotriazole.

[0251] Examples of carboxybenzotriazoles include 4-carboxy-1,2,3-benzotriazole, 5-carboxy-1,2,3-benzotriazole, N-(N,N-di-2-ethylhexyl)aminomethylenecarboxybenzotriazole, N-(N,N-di-2-hydroxyethyl)aminomethylenecarboxybenzotriazole, N-(N,N-di-2-ethylhexyl)aminoethylenecarboxybenzotriazole, etc. Examples of carboxybenzotriazoles that can be used include commercially available products such as CBT-1 (Johoku Chemical Industry Co., Ltd., trade name).

[0252] The total content of benzotriazoles and carboxybenzotriazoles is preferably 0.01% by mass to 3% by mass, and more preferably 0.05% by mass to 1% by mass, based on the total mass of the photosensitive resin layer. A content of 0.01% by mass or more is preferable from the viewpoint of imparting storage stability to the photosensitive resin layer. On the other hand, a content of 3% by mass or less is preferable from the viewpoint of maintaining sensitivity and suppressing discoloration of the dye.

[0253] The photosensitive resin layer may contain at least one selected from the group consisting of plasticizers and heterocyclic compounds. Examples of the plasticizers and heterocyclic compounds include the compounds described in paragraphs 0097 to 0103 and paragraphs 0111 to 0118 of WO 2018 / 179640.

[0254] The photosensitive resin layer may contain a solvent. When the photosensitive resin layer is formed from a photosensitive composition containing a solvent, the solvent may remain in the photosensitive resin layer.

[0255] In addition, the photosensitive resin layer may further contain known additives such as metal oxide particles, antioxidants, dispersants, acid multipliers, development accelerators, conductive fibers, thermal acid generators, ultraviolet absorbers, thickeners, crosslinking agents, and organic or inorganic suspending agents.

[0256] Additives contained in the photosensitive resin layer are described in paragraphs 0165 to 0184 of JP2014-85643A, the contents of which are incorporated herein by reference.

[0257] The photosensitive resin layer may contain a predetermined amount of impurities. Specific examples of impurities include sodium, potassium, magnesium, calcium, iron, manganese, copper, aluminum, titanium, chromium, cobalt, nickel, zinc, tin, halogens, and ions thereof. Among them, halide ions, sodium ions, and potassium ions are easily mixed in as impurities, so the following contents are preferable.

[0258] <<Impurities etc.>> The content of impurities in the photosensitive resin layer is preferably 80 ppm or less, more preferably 10 ppm or less, and even more preferably 2 ppm or less, by mass. The content of impurities can be 1 ppb or more, and may be 0.1 ppm or more, by mass.

[0259] Methods for keeping the amount of impurities within the above range include selecting raw materials for the composition that contain a small amount of impurities, preventing impurities from being mixed in during the preparation of the photosensitive resin layer, and removing the impurities by washing. By such methods, the amount of impurities can be kept within the above range.

[0260] Impurities can be quantified by known methods such as ICP (Inductively Coupled Plasma) emission spectrometry, atomic absorption spectrometry, and ion chromatography.

[0261] The content of compounds such as benzene, formaldehyde, trichloroethylene, 1,3-butadiene, carbon tetrachloride, chloroform, N,N-dimethylformamide, N,N-dimethylacetamide, and hexane in the photosensitive resin layer is preferably low. The content of these compounds relative to the total mass of the photosensitive resin layer is preferably 100 ppm or less, more preferably 20 ppm or less, and even more preferably 4 ppm or less, based on mass. The lower limit can be 10 ppb or more, and can be 100 ppb or more, based on mass, relative to the total mass of the photosensitive resin layer. The content of these compounds can be suppressed in the same manner as the above-mentioned metal impurities. They can also be quantified by known measurement methods.

[0262] From the viewpoint of improving reliability and lamination properties, the water content in the photosensitive resin layer is preferably 0.01% by mass to 1.0% by mass, and more preferably 0.05% by mass to 0.5% by mass.

[0263] <<Residual monomer>> The photosensitive resin layer may contain residual monomers corresponding to each of the constituent units of the above-mentioned alkali-soluble resin. The content of the residual monomer is preferably 5,000 ppm by mass or less, more preferably 2,000 ppm by mass or less, and even more preferably 500 ppm by mass or less, based on the total mass of the alkali-soluble resin, from the viewpoints of patterning property and reliability. The lower limit is not particularly limited, but is preferably 1 ppm by mass or more, and more preferably 10 ppm by mass or more. The content of the residual monomer of each constituent unit of the alkali-soluble resin is preferably 3,000 ppm by mass or less, more preferably 600 ppm by mass or less, and even more preferably 100 ppm by mass or less, based on the total mass of the photosensitive resin layer, from the viewpoints of patterning property and reliability. The lower limit is not particularly limited, but is preferably 0.1 ppm by mass or more, and more preferably 1 ppm by mass or more.

[0264] The amount of residual monomers in the synthesis of an alkali-soluble resin by a polymer reaction is also preferably within the above range. For example, when the alkali-soluble resin is synthesized by reacting glycidyl acrylate with a carboxylic acid side chain, the content of glycidyl acrylate is preferably within the above range.

[0265] The amount of the residual monomer can be measured by a known method such as liquid chromatography or gas chromatography.

[0266] <<Pigments>> The photosensitive resin layer may be a colored layer containing a pigment. The pigment may be appropriately selected according to the desired hue, and may be selected from black pigments, white pigments, and pigments of chromatic colors other than black and white. Among them, when a black pattern is to be formed, a black pigment is preferably selected as the pigment.

[0267] As the black pigment, known black pigments (organic pigments, inorganic pigments, etc.) can be appropriately selected as long as the effects of the present disclosure are not impaired. Among them, from the viewpoint of optical density, suitable examples of black pigments include carbon black, titanium oxide, titanium carbide, iron oxide, titanium oxide, and graphite, and carbon black is particularly preferred. As carbon black, from the viewpoint of surface resistance, carbon black at least a part of the surface of which is coated with a resin is preferred. From the viewpoint of dispersion stability, the particle size of the black pigment is preferably 0.001 μm to 0.1 μm, and more preferably 0.01 μm to 0.08 μm in number average particle size. The particle size refers to the diameter of a circle having the same area as the area of ​​a pigment particle, which is calculated from a photograph of the pigment particle taken with an electron microscope, and the number average particle size refers to the average value obtained by calculating the above particle size for any 100 particles and averaging the particle sizes of the 100 particles thus calculated.

[0268] As a pigment other than the black pigment, the white pigment described in paragraphs 0015 and 0114 of JP-A-2005-007765 can be used. Specifically, among the white pigments, the inorganic pigment is preferably titanium oxide, zinc oxide, lithopone, precipitated calcium carbonate, white carbon, aluminum oxide, aluminum hydroxide, or barium sulfate, more preferably titanium oxide or zinc oxide, and even more preferably titanium oxide. As the inorganic pigment, rutile or anatase titanium oxide is more preferable, and rutile titanium oxide is particularly preferable.

[0269] The surface of titanium oxide may be subjected to silica treatment, alumina treatment, titania treatment, zirconia treatment, or organic treatment, or may be subjected to two or more treatments. This suppresses the catalytic activity of titanium oxide, and improves heat resistance, fading resistance, etc. From the viewpoint of reducing the thickness of the photosensitive resin layer after heating, the surface treatment of titanium oxide is preferably at least one of alumina treatment and zirconia treatment, and particularly preferably both alumina treatment and zirconia treatment.

[0270] When the photosensitive resin layer is a colored layer, it is also preferable that the photosensitive resin layer further contains a chromatic pigment other than a black pigment and a white pigment from the viewpoint of transferability. When a chromatic pigment is contained, the particle size of the chromatic pigment is preferably 0.1 μm or less, and more preferably 0.08 μm or less, in terms of superior dispersibility. As the chromatic pigment, for example, Victoria Pure Blue BO (Color Index (CI) 42595), Auramine (CI 41000), Fat Black HB (CI 26150), Monolight Yellow GT (CI Pigment Yellow 12), Permanent Yellow GR (CI Pigment Yellow 17), Permanent Yellow HR (CI Pigment Yellow 83), Permanent Carmine FBB (CI Pigment Red 146), Hoster Balm Red ESB (CI Pigment Violet 19), Permanent Ruby FBH (CI Pigment Red 11), Fastel Pink B Supra (CI Pigment Red 81), Monastral Fast Blue (CI Pigment Red 146 ... Permanent Ruby FBH (CI Pigment Red 11), Permanent Pink B Supra (CI Pigment Red 81), Monastral Fast Blue (CI Pigment Red 146), Permanent Yellow GR (CI Pigment Yellow 17), Permanent Yellow HR (CI Pigment Yellow 83), Permanent Carmine FBB (CI Pigment Red 146), Permanent Ruby FBH (CI Pigment Red 11), Permanent Pink B Supra (CI Pigment Red 81), Monastral Fast Blue (CI Pigment Red 146), Permanent Yellow GR (CI Pigment Yellow 17 Examples of pigments that can be used include CI Pigment Blue 15), Monolight Fast Black B (CI Pigment Black 1) and Carbon, CI Pigment Red 97, CI Pigment Red 122, CI Pigment Red 149, CI Pigment Red 168, CI Pigment Red 177, CI Pigment Red 180, CI Pigment Red 192, CI Pigment Red 215, CI Pigment Green 7, CI Pigment Blue 15:1, CI Pigment Blue 15:4, CI Pigment Blue 22, CI Pigment Blue 60, CI Pigment Blue 64, and CI Pigment Violet 23. Of these, CI Pigment Red 177 is preferred.

[0271] When the photosensitive resin layer contains a pigment, the pigment content is preferably more than 3 mass% and not more than 40 mass%, more preferably more than 3 mass% and not more than 35 mass%, even more preferably more than 5 mass% and not more than 35 mass%, and particularly preferably 10 mass% or more and not more than 35 mass%, relative to the total mass of the photosensitive resin layer.

[0272] When the photosensitive resin layer contains a pigment other than the black pigment (a white pigment and a chromatic pigment), the content of the pigment other than the black pigment is preferably 30% by mass or less, more preferably 1% by mass to 20% by mass, and further preferably 3% by mass to 15% by mass, based on the black pigment. It is nice.

[0273] In the method for producing a photosensitive resin layer containing a black pigment, the black pigment (preferably carbon black) is preferably introduced into the photosensitive composition described below in the form of a pigment dispersion. The dispersion may be prepared by adding a mixture obtained by previously mixing the black pigment and the pigment dispersant to an organic solvent (or vehicle) and dispersing the mixture with a dispersing machine. The pigment dispersant may be selected according to the pigment and the solvent, and for example, a commercially available dispersing agent may be used. The vehicle refers to the part of the medium in which the pigment is dispersed when the pigment dispersion is prepared, and is liquid and includes a binder component that holds the black pigment in a dispersed state and a solvent component (organic solvent) that dissolves and dilutes the binder component. The dispersing machine is not particularly limited, and examples thereof include known dispersing machines such as a kneader, a roll mill, an attritor, a super mill, a dissolver, a homomixer, and a sand mill. Furthermore, the fine pulverization may be performed by utilizing frictional force by mechanical grinding. For information on dispersers and fine grinding, see "Encyclopedia of Pigments" (by Kunizo Asakura, 1st Edition, Asakura Publishing, 2000, pp. 438 and 310).

[0274] <<Physical properties etc.>> From the viewpoints of developability and resolution, the film thickness (average thickness) of the photosensitive resin layer is preferably 20 μm or less, more preferably 10 μm or less, even more preferably 8 μm or less, and particularly preferably 5 μm or less. The average thickness of the photosensitive resin layer is preferably 0.5 μm or more, and more preferably 1 μm or more. When the transfer layer includes an intermediate layer (preferably a thermoplastic resin layer and / or a water-soluble resin layer) and a photosensitive resin layer, the average thickness of the photosensitive resin layer is preferably 4.8 μm or less, and more preferably 3 μm or less. The average thickness of the photosensitive resin layer is calculated by the arithmetic mean of thicknesses measured at five points by cross-sectional observation using a scanning electron microscope (SEM).

[0275] <<Formation method>> As long as the desired photosensitive resin layer can be obtained, the method for producing the photosensitive resin layer is not limited. For example, the method for forming the photosensitive resin layer includes preparing a photosensitive composition containing an alkali-soluble resin, an ethylenically unsaturated compound, a photopolymerization initiator and a solvent, applying the photosensitive composition to an object such as a temporary support, and drying the coating of the photosensitive composition to form the layer. The photosensitive resin layer may also be formed by applying the photosensitive composition to a protective film described later and drying it.

[0276] Examples of the photosensitive composition used for forming the photosensitive resin layer include compositions containing an alkali-soluble resin, an ethylenically unsaturated compound, a photopolymerization initiator, the above-mentioned optional components, and a solvent. The photosensitive composition preferably contains a solvent to adjust the viscosity of the photosensitive composition and facilitate the formation of the photosensitive resin layer.

[0277] -solvent- Examples of the solvent contained in the photosensitive composition include alkylene glycol ether solvents, alkylene glycol ether acetate solvents, alcohol solvents (methanol, ethanol, etc.), ketone solvents (acetone, methyl ethyl ketone, etc.), aromatic hydrocarbon solvents (toluene, etc.), aprotic polar solvents (N,N-dimethylformamide, etc.), cyclic ether solvents (tetrahydrofuran, etc.), ester solvents, amide solvents, lactone solvents, and mixed solvents containing two or more of these.

[0278] The photosensitive composition preferably contains at least one selected from the group consisting of alkylene glycol ether solvents and alkylene glycol ether acetate solvents.Among them, a mixed solvent containing at least one selected from the group consisting of alkylene glycol ether solvents and alkylene glycol ether acetate solvents and at least one selected from the group consisting of ketone solvents and cyclic ether solvents is more preferred, and a mixed solvent containing at least three of at least one selected from the group consisting of alkylene glycol ether solvents and alkylene glycol ether acetate solvents, a ketone solvent, and a cyclic ether solvent is even more preferred.

[0279] Examples of alkylene glycol ether solvents include ethylene glycol monoalkyl ethers, ethylene glycol dialkyl ethers, propylene glycol monoalkyl ethers, propylene glycol dialkyl ethers, diethylene glycol dialkyl ethers, dipropylene glycol monoalkyl ethers, and dipropylene glycol dialkyl ethers.

[0280] Examples of alkylene glycol ether acetate solvents include ethylene glycol monoalkyl ether acetate, propylene glycol monoalkyl ether acetate, diethylene glycol monoalkyl ether acetate, and dipropylene glycol monoalkyl ether acetate.

[0281] As the solvent, the solvents described in paragraphs 0092 to 0094 of International Publication No. 2018 / 179640 and the solvents described in paragraph 0014 of JP-A-2018-177889 may be used, the contents of which are incorporated herein by reference.

[0282] The photosensitive composition may contain one solvent alone or two or more solvents. The content of the solvent when applying the photosensitive composition is preferably 50 parts by mass to 1,900 parts by mass, more preferably 100 parts by mass to 900 parts by mass, based on 100 parts by mass of the total solid content in the photosensitive composition.

[0283] The method for preparing the photosensitive composition is not particularly limited, and for example, a method for preparing the photosensitive composition by dissolving each component in the above-mentioned solvent in advance and mixing the obtained solutions in a predetermined ratio is exemplified. The photosensitive composition is preferably filtered using a filter having a pore size of 0.2 μm to 30 μm before forming the photosensitive resin layer.

[0284] The method for applying the photosensitive composition is not particularly limited, and may be any known method, such as slit coating, spin coating, curtain coating, and inkjet coating.

[0285] As a method for drying the coating film of the photosensitive composition, heat drying and reduced pressure drying are preferred. In this specification, "drying" means removing at least a part of the solvent contained in the composition. Examples of the drying method include natural drying, heat drying, and reduced pressure drying. The above methods can be applied alone or in combination. The drying temperature is preferably 80°C or higher, more preferably 90°C or higher. The upper limit is preferably 130°C or lower, more preferably 120°C or lower. Drying can also be performed by continuously changing the temperature. The drying time is preferably 20 seconds or more, more preferably 40 seconds or more, and even more preferably 60 seconds or more. The upper limit is not particularly limited, but is preferably 600 seconds or less, more preferably 300 seconds or less.

[0286] (Components of transfer layer: intermediate layer) The transfer layer preferably includes an intermediate layer and a photosensitive resin layer. The intermediate layer can suppress the inclusion of air bubbles between the transfer layer and the object when the photosensitive transfer material and the object are bonded together, and can improve the adhesion between the transfer layer and the object. The intermediate layer can also improve the conformability of the transfer layer to an object having a rough surface. The intermediate layer is preferably disposed between the temporary support and the photosensitive resin layer. That is, the photosensitive transfer material preferably includes a temporary support, an intermediate layer, and a photosensitive resin layer in this order. The structure of the intermediate layer may be a single-layer structure or a multi-layer structure.

[0287] Examples of the intermediate layer include a thermoplastic resin layer and a water-soluble resin layer. The intermediate layer may be an embodiment including a water-soluble resin layer, or an embodiment including a thermoplastic resin layer and a water-soluble resin layer.

[0288] When the intermediate layer includes both a thermoplastic resin layer and a water-soluble resin layer, the photosensitive transfer material preferably includes a temporary support, a thermoplastic resin layer, a water-soluble resin layer, and a photosensitive resin layer in this order.In addition, the intermediate layer may also be an oxygen barrier layer having an oxygen barrier function, which is described as a "separation layer" in JP-A-5-72724.When the intermediate layer is an oxygen barrier layer, the sensitivity during exposure is improved, the time load of the exposure machine is reduced, and productivity is improved.

[0289] [Thermoplastic resin layer] The thermoplastic resin layer preferably contains an alkali-soluble resin as a thermoplastic resin, such as an acrylic resin, a polystyrene resin, a styrene-acrylic copolymer, a polyurethane resin, a polyvinyl alcohol, a polyvinyl formal, a polyamide resin, a polyester resin, an epoxy resin, a polyacetal resin, a polyhydroxystyrene resin, a polyimide resin, a polybenzoxazole resin, a polysiloxane resin, a polyethyleneimine, a polyallylamine, and a polyalkylene glycol.

[0290] The alkali-soluble resin is preferably an acrylic resin from the viewpoint of developability and adhesion to adjacent layers. The acrylic resin means a resin having at least one type of structural unit selected from the group consisting of structural units derived from (meth)acrylic acid, structural units derived from (meth)acrylic acid esters, and structural units derived from (meth)acrylic acid amides. The acrylic resin preferably has a total content of structural units derived from (meth)acrylic acid, structural units derived from (meth)acrylic acid esters, and structural units derived from (meth)acrylic acid amides of 50% by mass or more based on the total mass of the acrylic resin. In particular, the total content of the structural units derived from (meth)acrylic acid and the structural units derived from (meth)acrylic acid esters is preferably 30% by mass to 100% by mass, and more preferably 50% by mass to 100% by mass, relative to the total mass of the acrylic resin.

[0291] The alkali-soluble resin is preferably a polymer having an acid group, such as a carboxy group, a sulfo group, a phosphoric acid group, or a phosphonic acid group, with the carboxy group being preferred.

[0292] From the viewpoint of developability, the alkali-soluble resin is preferably an alkali-soluble resin having an acid value of 60 mgKOH / g or more, more preferably a carboxyl group-containing acrylic resin having an acid value of 60 mgKOH / g or more. The upper limit of the acid value of the alkali-soluble resin is not particularly limited, but is preferably 200 mgKOH / g or less, more preferably 150 mgKOH / g or less.

[0293] The carboxyl group-containing acrylic resin having an acid value of 60 mgKOH / g or more is not particularly limited, and may be appropriately selected from known resins. For example, an alkali-soluble resin that is a carboxyl group-containing acrylic resin having an acid value of 60 mgKOH / g or more among the polymers described in paragraph 0025 of JP-A-2011-95716, a carboxyl group-containing acrylic resin having an acid value of 60 mgKOH / g or more among the polymers described in paragraphs 0033 to 0052 of JP-A-2010-237589, and an alkali-soluble resin having an acid value of 60 mgKOH / g or more among the alkali-soluble resins described in paragraphs 0053 to 0068 of JP-A-2016-224162 may be used. Examples of the resin include carboxy group-containing acrylic resins.

[0294] The copolymerization ratio of the structural unit having a carboxy group in the carboxy group-containing acrylic resin is preferably 5% by mass to 50% by mass, more preferably 10% by mass to 40% by mass, and even more preferably 12% by mass to 30% by mass, relative to the total mass of the acrylic resin.

[0295] As the alkali-soluble resin, from the viewpoints of developability and adhesion to adjacent layers, an acrylic resin having a structural unit derived from (meth)acrylic acid is particularly preferred.

[0296] The alkali-soluble resin may have a reactive group. The reactive group may be a polymerizable group, for example, a group capable of addition polymerization, polycondensation, or polyaddition, and examples of the reactive group include ethylenically unsaturated groups, polycondensation groups such as hydroxyl groups and carboxyl groups, and polyaddition reactive groups such as epoxy groups and (blocked) isocyanate groups.

[0297] The weight average molecular weight (Mw) of the alkali-soluble resin is preferably 1,000 or more, more preferably from 10,000 to 100,000, and even more preferably from 20,000 to 50,000.

[0298] The thermoplastic resin layer may contain one type of alkali-soluble resin alone or two or more types. From the viewpoints of developability and adhesion to adjacent layers, the content of the alkali-soluble resin is preferably 10% by mass to 99% by mass, more preferably 20% by mass to 90% by mass, even more preferably 40% by mass to 80% by mass, and particularly preferably 50% by mass to 70% by mass, based on the total mass of the thermoplastic resin layer.

[0299] The thermoplastic resin layer preferably contains a dye (also simply referred to as "dye B") whose maximum absorption wavelength in the wavelength range of 400 nm to 780 nm during color development is 450 nm or more and whose maximum absorption wavelength changes depending on an acid, a base, or a radical. A preferred embodiment of dye B is the same as that of dye N, except for the points described below.

[0300] From the viewpoints of visibility and resolution of exposed and non-exposed areas, the dye B is preferably a dye whose maximum absorption wavelength changes with an acid or a radical, and more preferably a dye whose maximum absorption wavelength changes with an acid. From the viewpoints of visibility and resolution of exposed and non-exposed areas, the thermoplastic resin layer preferably contains both a dye whose maximum absorption wavelength changes with an acid as dye B, and a compound that generates an acid when exposed to light, which will be described later.

[0301] The dye B may be used alone or in combination of two or more kinds. The content of the dye B is preferably 0.2% by mass or more, more preferably 0.2% by mass to 6% by mass, even more preferably 0.2% by mass to 5% by mass, and particularly preferably 0.25% by mass to 3.0% by mass, based on the total mass of the thermoplastic resin layer, from the viewpoint of visibility of the exposed and non-exposed parts. The content of the dye B means the content of the dye when all of the dye B contained in the thermoplastic resin layer is in a colored state. The following describes a method for quantifying the content of the dye B, taking a dye that develops color by radicals as an example. Two types of solutions are prepared by dissolving 0.001 g or 0.01 g of the dye in 100 mL of methyl ethyl ketone. A photoradical polymerization initiator Irgacure OXE01 (trade name, manufactured by BASF) is added to each of the obtained solutions, and radicals are generated by irradiating light at 365 nm, causing all of the dyes to develop color. Then, in an air atmosphere, the absorbance of each solution at a liquid temperature of 25°C is measured using a spectrophotometer (UV3100, manufactured by Shimadzu Corporation) to create a calibration curve. Next, the absorbance of the solution in which all the dyes have been colored is measured in the same manner as above, except that 0.1 g of the thermoplastic resin layer is dissolved in methyl ethyl ketone instead of the dye. From the absorbance of the obtained solution containing the thermoplastic resin layer, the amount of the dye contained in the thermoplastic resin layer is calculated based on the calibration curve.

[0302] The thermoplastic resin layer may contain a compound (also simply referred to as "compound C") that generates an acid, a base, or a radical when exposed to light. Compound C is preferably a compound that generates an acid, a base, or a radical when exposed to actinic light such as ultraviolet light and visible light. Compound C may be a known photoacid generator, photobase generator, or photoradical polymerization initiator (photoradical generator). Of these, a photoacid generator is preferred.

[0303] From the viewpoint of resolution, the thermoplastic resin layer preferably contains a photoacid generator. Examples of the photoacid generator include the photocationic polymerization initiators that may be contained in the photosensitive resin layer described above, and the preferred aspects are the same as those described below.

[0304] From the viewpoints of sensitivity and resolution, the photoacid generator preferably contains at least one compound selected from the group consisting of an onium salt compound and an oxime sulfonate compound, and from the viewpoints of sensitivity, resolution and adhesion, it is more preferable to contain an oxime sulfonate compound. Also, as the photoacid generator, a photoacid generator having the following structure is also preferable.

[0305] [ka]

[0306] The thermoplastic resin layer may contain a photoradical polymerization initiator. Examples of the photoradical polymerization initiator include the photoradical polymerization initiators that may be contained in the photosensitive resin layer described above, and the preferred embodiments are also the same.

[0307] The thermoplastic resin layer may contain a photobase generator. The photobase generator is not particularly limited as long as it is a known photobase generator, and examples thereof include 2-nitrobenzylcyclohexylcarbamate, triphenylmethanol, O-carbamoylhydroxylamide, O-carbamoyloxime, {[(2,6-dinitrobenzyl)oxy]carbonyl}cyclohexylamine, bis{[(2-nitrobenzyl)oxy]carbonyl}hexane-1,6-diamine, 4-(methylthiobenzoyl)-1-methyl-1-morpholinoethane, (4-morpholinobenzoyl) -1-benzyl-1-dimethylaminopropane, N-(2-nitrobenzyloxycarbonyl)pyrrolidine, hexaamminecobalt(III) tris(triphenylmethylborate), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2,6-dimethyl-3,5-diacetyl-4-(2-nitrophenyl)-1,4-dihydropyridine, and 2,6-dimethyl-3,5-diacetyl-4-(2,4-dinitrophenyl)-1,4-dihydropyridine.

[0308] The thermoplastic resin layer may contain one type alone or two or more types of compound C. From the viewpoints of visibility and resolution of exposed and non-exposed areas, the content of compound C is preferably 0.1% by mass to 10% by mass, and more preferably 0.5% by mass to 5% by mass, based on the total mass of the thermoplastic resin layer.

[0309] The thermoplastic resin layer preferably contains a plasticizer from the viewpoints of resolution, adhesion to adjacent layers, and developability.

[0310] The plasticizer preferably has a smaller molecular weight (weight average molecular weight (Mw) in the case of an oligomer or polymer) than the alkali-soluble resin. The molecular weight (weight average molecular weight (Mw)) of the plasticizer is preferably 200 to 2,000.

[0311] The plasticizer is not particularly limited as long as it is a compound that is compatible with the alkali-soluble resin and exhibits plasticity, but from the viewpoint of imparting plasticity, the plasticizer preferably has an alkyleneoxy group in the molecule, more preferably a polyalkylene glycol compound. The alkyleneoxy group contained in the plasticizer more preferably has a polyethyleneoxy structure or a polypropyleneoxy structure.

[0312] In addition, from the viewpoints of resolution and storage stability, the plasticizer preferably contains a (meth)acrylate compound. From the viewpoints of compatibility, resolution, and adhesion to adjacent layers, it is more preferable that the alkali-soluble resin is an acrylic resin and the plasticizer contains a (meth)acrylate compound. Examples of the (meth)acrylate compound used as the plasticizer include the (meth)acrylate compounds described above as the ethylenically unsaturated compound contained in the photosensitive resin layer.

[0313] In the transfer film, when the thermoplastic resin layer and the photosensitive resin layer are laminated in direct contact with each other, it is preferable that both the thermoplastic resin layer and the photosensitive resin layer contain the same (meth)acrylate compound, because the thermoplastic resin layer and the photosensitive resin layer each contain the same (meth)acrylate compound, which suppresses component diffusion between the layers and improves storage stability.

[0314] When the thermoplastic resin layer contains a (meth)acrylate compound as a plasticizer, it is preferable that the (meth)acrylate compound does not polymerize even in the exposed area after exposure, from the viewpoint of adhesion to adjacent layers.

[0315] In addition, the (meth)acrylate compound used as a plasticizer is preferably a polyfunctional (meth)acrylate compound having two or more (meth)acryloyl groups in one molecule, from the viewpoints of resolution, adhesion to adjacent layers, and developability.

[0316] Furthermore, as the (meth)acrylate compound used as the plasticizer, a (meth)acrylate compound having an acid group or a urethane (meth)acrylate compound is also preferred.

[0317] The thermoplastic resin layer may contain one type of plasticizer alone or two or more types. From the viewpoints of resolution, adhesion to adjacent layers, and developability, the content of the plasticizer is preferably 1% by mass to 70% by mass, more preferably 10% by mass to 60% by mass, and even more preferably 20% by mass to 50% by mass, based on the total mass of the thermoplastic resin layer.

[0318] From the viewpoint of thickness uniformity, the thermoplastic resin layer preferably contains a surfactant. Examples of the surfactant include the surfactants that may be contained in the photosensitive resin layer described above, and the preferred embodiments are the same. The thermoplastic resin layer may contain one type of surfactant alone, or may contain two or more types. The content of the surfactant is preferably 0.001% by mass to 10% by mass, and more preferably 0.01% by mass to 3% by mass, based on the total mass of the thermoplastic resin layer.

[0319] The thermoplastic resin layer may contain a sensitizer. The sensitizer is not particularly limited, and may be any of the sensitizers that may be contained in the photosensitive resin layer described above. The thermoplastic resin layer may contain one type of sensitizer alone, or may contain two or more types of sensitizers. The content of the sensitizer can be appropriately selected depending on the purpose, but from the viewpoints of improving the sensitivity to the light source and the visibility of the exposed and non-exposed areas, it is preferable to use a sensitizer that is more favorable than the sensitizer that is less favorable than the sensitizer that is more ... Therefore, the content is preferably in the range of 0.01% by mass to 5% by mass, and more preferably in the range of 0.05% by mass to 1% by mass, based on the total mass of the thermoplastic resin layer.

[0320] The thermoplastic resin layer may contain known additives as necessary in addition to the above components. The thermoplastic resin layer is described in paragraphs

[0189] to

[0193] of JP2014-85643A, the contents of which are incorporated herein by reference.

[0321] The average thickness of the thermoplastic resin layer is preferably 1 μm or more, more preferably 2 μm or more, from the viewpoint of adhesion with adjacent layers. The upper limit is not particularly limited, but is preferably 20 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less, from the viewpoint of developability and resolution. The average thickness of the thermoplastic resin layer is calculated by the arithmetic average of the thicknesses at five points measured by cross-sectional observation using a scanning electron microscope (SEM).

[0322] As long as the desired thermoplastic resin layer can be obtained, the method for producing the thermoplastic resin layer is not limited. For example, the method for producing the thermoplastic resin layer includes preparing a thermoplastic resin composition containing the above-mentioned components and a solvent, applying the thermoplastic resin composition to an object such as a temporary support, and drying the coating film of the thermoplastic resin composition to form the layer. The thermoplastic resin composition preferably contains a solvent to adjust the viscosity of the thermoplastic resin composition and facilitate the formation of the thermoplastic resin layer.

[0323] The solvent contained in the thermoplastic resin composition is not particularly limited as long as it can dissolve or disperse the above-mentioned components contained in the thermoplastic resin layer. Examples of the solvent contained in the thermoplastic resin composition include the solvents that may be contained in the above-mentioned photosensitive composition, and the preferred embodiments are the same. The solvent contained in the thermoplastic resin composition may be one type alone or two or more types. The content of the solvent when applying the thermoplastic resin composition is preferably 50 parts by mass to 1,900 parts by mass, more preferably 100 parts by mass to 900 parts by mass, relative to 100 parts by mass of the total solid content in the thermoplastic resin composition.

[0324] The preparation of the thermoplastic resin composition and the formation of the thermoplastic resin layer may be carried out in accordance with the above-mentioned method for preparing the photosensitive composition and the method for forming the photosensitive resin layer. For example, a solution in which each component contained in the thermoplastic resin layer is dissolved in the above-mentioned solvent is prepared in advance, and the obtained solution is mixed in a predetermined ratio to prepare a thermoplastic resin composition, and then the obtained thermoplastic resin composition is applied to the surface of a temporary support, and the coating film of the thermoplastic resin composition is dried to form a thermoplastic resin layer. In addition, a photosensitive resin layer and a water-soluble resin layer may be formed on a protective film described later, and then a thermoplastic resin layer may be formed on the water-soluble resin layer.

[0325] [Water-soluble resin layer] The water-soluble resin layer preferably contains a water-soluble resin. Examples of the water-soluble resin include polyvinyl alcohol resins, polyvinylpyrrolidone resins, cellulose resins, acrylamide resins, polyethylene oxide resins, gelatin, vinyl ether resins, polyamide resins, and copolymers thereof. In order to suppress the mixing of components between multiple layers, the water-soluble resin contained in the water-soluble resin layer is preferably a resin different from both the polymer A contained in the photosensitive resin layer and the thermoplastic resin (e.g., an alkali-soluble resin) contained in the thermoplastic resin layer.

[0326] From the viewpoints of oxygen barrier properties and suppressing mixing of components when multiple layers are applied and during storage after application, the water-soluble resin layer preferably contains polyvinyl alcohol, and more preferably contains both polyvinyl alcohol and polyvinylpyrrolidone. The water-soluble resin layer also preferably contains polyvinyl alcohol, polyvinylpyrrolidone, and hydroxypropylmethylcellulose.

[0327] The water-soluble resin layer may contain one kind of water-soluble resin alone, or may contain two or more kinds of water-soluble resins.

[0328] The content of the water-soluble resin in the water-soluble resin layer is not particularly limited, but from the viewpoints of oxygen barrier properties and suppressing mixing of components when multiple layers are applied and during storage after application, the content is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, even more preferably 80% by mass to 100% by mass, and particularly preferably 90% by mass to 100% by mass, relative to the total mass of the water-soluble resin layer.

[0329] The water-soluble resin layer may contain additives such as a surfactant, if necessary.

[0330] The average thickness of the water-soluble resin layer is preferably 0.1 μm to 5 μm, and more preferably 0.5 μm to 3 μm. When the thickness of the water-soluble resin layer is within the above range, the oxygen barrier property is not reduced, mixing of components can be suppressed when multiple layers are applied and during storage after application, and an increase in the time required to remove the water-soluble resin layer during development can be suppressed. The average thickness of the water-soluble resin layer is calculated as the arithmetic mean of the thicknesses at five points measured by cross-sectional observation using a scanning electron microscope (SEM).

[0331] As long as the desired water-soluble resin layer can be obtained, the method for producing the water-soluble resin layer is not limited. The water-soluble resin layer is formed, for example, by preparing a water-soluble resin layer-forming composition containing a water-soluble resin and any additive, applying the composition to a thermoplastic resin layer or a photosensitive resin layer, and drying the coating of the water-soluble resin layer-forming composition. The water-soluble resin layer-forming composition preferably contains a solvent to adjust the viscosity of the water-soluble resin layer-forming composition and facilitate the formation of the water-soluble resin layer.

[0332] The solvent contained in the composition for forming a water-soluble resin layer is preferably at least one selected from the group consisting of water and water-miscible organic solvents, more preferably water or a mixed solvent of water and a water-miscible organic solvent. Examples of the water-miscible organic solvent include alcohols having 1 to 3 carbon atoms, acetone, ethylene glycol, and glycerin, preferably alcohols having 1 to 3 carbon atoms, and more preferably methanol or ethanol.

[0333] The transfer layer may further include other layers. Examples of the other layers include a refractive index adjustment layer (contrast enhancement layer). The contrast enhancement layer is described in paragraph 0134 of International Publication No. 2018 / 179640. The other layers are described in paragraphs 0194 to 0196 of JP-A-2014-85643. The contents of these publications are incorporated herein by reference.

[0334] (Protective film) The transfer film preferably includes a protective film. For example, the photosensitive transfer material preferably includes a temporary support, a transfer layer, and a protective film in this order.

[0335] Materials constituting the protective film include resin films and paper, and resin films are preferred from the viewpoints of strength and flexibility. Examples of resin films include polyethylene films, polypropylene films, polyethylene terephthalate films, cellulose triacetate films, polystyrene films, and polycarbonate films. Among these, polyethylene films, polypropylene films, and polyethylene terephthalate films are preferred.

[0336] The average thickness of the protective film is preferably 1 μm to 100 μm, more preferably 5 μm to 50 μm, further preferably 5 μm to 40 μm, and particularly preferably 15 μm to 30 μm. The average thickness of the protective film is calculated as the arithmetic average of the thicknesses measured at five points by cross-sectional observation using a scanning electron microscope (SEM).

[0337] The arithmetic mean roughness Ra of the surface of the protective film facing the transfer layer (hereinafter also simply referred to as the "surface of the protective film") is preferably 0.3 μm or less, more preferably 0.1 μm or less, and even more preferably 0.05 μm or less, from the viewpoint of superior resolution. When the Ra value of the surface of the protective film is within the above range, the uniformity of the thickness of the transfer layer and the resist pattern formed is improved. The lower limit of the Ra value of the surface of the protective film is not particularly limited, but it is preferably 0.001 μm or more.

[0338] The Ra value of the protective film surface is measured by the following method. Using a 3D optical profiler (New View7300, manufactured by Zygo), the surface of the protective film is measured under the following conditions to obtain a surface profile of the protective film. MetroPro ver8.3.2 Microscope Application is used as the measurement and analysis software. Next, the Surface Map screen is displayed in the above analysis software, and histogram data is obtained in the Surface Map screen. From the obtained histogram data, the arithmetic average roughness is calculated to obtain the Ra value of the protective film surface.

[0339] The protective film is introduced into the photosensitive transfer material by, for example, laminating the protective film and the transfer layer. The lamination of the protective film and the transfer layer is carried out, for example, by using a known laminator. Examples of the laminator include a vacuum laminator and an autocut laminator. The laminator is preferably a device equipped with any heatable roller such as a rubber roller and capable of applying pressure and heat.

[0340] [Method of producing photosensitive transfer material] The method for producing the photosensitive transfer material used in the present disclosure is not particularly limited, and a known method for producing the photosensitive transfer material, for example, a known method for forming each layer, can be used. Hereinafter, the method for producing the photosensitive transfer material used in the present disclosure will be described with reference to FIG. 1. However, the photosensitive transfer material used in the present disclosure is not limited to the one having the configuration shown in FIG.

[0341] Fig. 1 is a schematic cross-sectional view showing an example of a layer structure in one embodiment of a photosensitive transfer material used in the present disclosure. The photosensitive transfer material 10 shown in Fig. 1 has a structure in which a temporary support 11, a transfer layer 12 including a thermoplastic resin layer 13, a water-soluble resin layer 15, and a photosensitive resin layer 17, and a protective film 19 are laminated in this order.

[0342] Examples of methods for producing the photosensitive transfer material 10 include a method including the steps of applying a thermoplastic resin composition to the surface of a temporary support 11 and then drying the coating of the thermoplastic resin composition to form a thermoplastic resin layer 12, applying a water-soluble resin layer composition to the surface of a thermoplastic resin layer 13 and then drying the coating of the water-soluble resin layer composition to form a water-soluble resin layer 15, and applying a photosensitive resin composition containing an ethylenically unsaturated compound to the surface of the water-soluble resin layer 15 and then drying the coating of the photosensitive resin composition to form a photosensitive resin layer 17.

[0343] The photosensitive transfer material 10 is produced by pressing a protective film 19 onto the photosensitive resin layer 17 of the laminate produced by the above-mentioned production method. The production method of the photosensitive transfer material used in the present disclosure preferably includes a step of providing a protective film 19 so as to be in contact with the second surface of the photosensitive resin layer 17, thereby producing a photosensitive transfer material 10 including a temporary support 11, a thermoplastic resin layer 13, a water-soluble resin layer 15, a photosensitive resin layer 17, and a protective film 19. After producing the photosensitive transfer material 10 by the above-mentioned production method, the photosensitive transfer material 10 may be wound up to produce and store a roll-shaped photosensitive transfer material. EXAMPLES

[0344] The present disclosure will be described in detail below with reference to examples. However, the present disclosure is not limited to the following examples. In the following description, unless otherwise specified, "%" means "% by mass" and "parts" means "parts by mass".

[0345] <Example 1> (Production of Photosensitive Transfer Material 1) A photosensitive transfer material 1 including a temporary support (16KS40, Toray Industries, Inc., biaxially stretched PET film having a thickness of 16 μm), a thermoplastic resin layer, a water-soluble resin layer, a photosensitive resin layer, and a protective film in this order was manufactured by the following procedure. The photosensitive resin layer is a negative photosensitive resin layer containing an alkali-soluble resin, a photopolymerization initiator, and a polymerizable compound having an ethylenic double bond. In this example, the intermediate layer consisting of the thermoplastic resin layer and the water-soluble resin layer and the photosensitive resin layer constitute the transfer layer.

[0346] Composition A containing the components shown in the "thermoplastic resin layer" column in Table 1 was prepared. Composition A was applied onto a temporary support using a slit nozzle, and then the composition was heated at 80°C for 2 minutes. The composition A was dried to form a thermoplastic resin layer. The thickness of the thermoplastic resin layer is shown in Table 1. It is written.

[0347] Composition B was prepared, containing the components shown in the "Water-soluble resin layer" column of Table 1. Composition B was applied onto the thermoplastic resin layer using a slit nozzle, and then dried at 90°C for 2 minutes to form an intermediate layer. The thickness of the intermediate layer is shown in Table 1.

[0348] Composition C was prepared, containing the components shown in the "Photosensitive resin layer" column of Table 1. Composition C was applied onto the intermediate layer using a slit nozzle, and then the composition was heated at 80°C for 2 minutes. A photosensitive resin layer was formed by drying C. The thickness of the photosensitive resin layer is shown in Table 1.

[0349] Finally, a protective film (16KS40, manufactured by Toray Industries, Inc., thickness: 16 μm) was provided on the photosensitive resin layer.

[0350] In this manner, a photosensitive transfer material 1 was obtained.

[0351] <Production of Laminate> Next, a laminate was produced using the obtained photosensitive transfer material 1 by the following procedure. An Invar substrate was prepared as a metal substrate having a first surface and a second surface opposite to the first surface. The first surface and the second surface face in opposite directions. The roughness Rmax of the first surface of the Invar substrate is 0.80 μm. The roughness Rmax of the second surface of the Invar substrate is 0.90 μm. The average thickness of the Invar substrate is 50 μm.

[0352] The protective film was peeled off from the photosensitive transfer material 1. Using a roll laminator, the photosensitive transfer material 1 and an Invar substrate were laminated together under conditions of a temperature of 100°C, a linear pressure of 0.5 MPa, and a linear speed (lamination speed) of 4 m / min, and a transfer layer (i.e., a photosensitive resin layer, a water-soluble resin layer, and a thermoplastic resin layer) and a temporary support were disposed in this order on the first surface of the Invar substrate. The first surface of the Invar substrate was in contact with the photosensitive resin layer.

[0353] Next, without peeling off the temporary support, an exposure mask was attached to the temporary support. The exposure mask had a plurality of square light-shielding parts. The dimensions of each light-shielding part varied in 0.1 μm increments within a range of 10 μm length×10 μm width to 20 μm length×20 μm width. Exposure was performed by irradiating the transfer layer with light using a high-pressure mercury lamp exposure machine (MAP-1200L, manufactured by Dainihon Kaken Co., Ltd., dominant wavelength: 365 nm).

[0354] The exposure amount S1 was set to 25% of the exposure amount S0 at which the maximum number of remaining film steps was 6 when the photosensitive transfer material 1 was laminated onto an Invar substrate, exposed using a Stouffer 21-step tablet as a mask, and then developed. Specifically, the exposure dose at which the maximum number of remaining film stages is 6 is 55 mJ / cm 2 Therefore, the actual exposure dose S1 was 14 mJ / cm 2 No ND filter was used to reduce the amount of light exposure.

[0355] The actual exposure amount (exposure amount S1) was measured by the following procedure. A light meter was set in the center of the exposure sample installation location of the exposure machine, and the exposure amount set on the exposure machine was changed stepwise to create a calibration curve from the relationship with the exposure amount (actual exposure amount) detected by the light meter. The exposure amount set on the exposure machine that was the target actual exposure amount was read from this calibration curve, and the light was irradiated again on the light meter at that set exposure amount, the exposure amount was measured, and it was confirmed that it was the target actual exposure amount. If there was a deviation from the target actual exposure amount, this operation was repeated until the target actual exposure amount and the exposure amount matched.

[0356] The actual exposure was measured by placing a glass mask without a light-shielding pattern on the light receiving part, which allows the measurement of the actual exposure taking into account the reduction in illuminance due to reflection from the mask.

[0357] When an ND filter was used, it was placed closer to the light source than the exposure mask. The actual exposure was measured with the ND filter in place.

[0358] The illuminance meter used has a receiver that matches the maximum sensitivity wavelength of the exposed sample (i.e., a receiver with a measurement center wavelength close to the maximum sensitivity wavelength). The illuminance meter used is a USHIO ultraviolet actinometer (UIT-250). For example, if the maximum sensitivity wavelength is i-line, the receiver used is UVD-S365. If the maximum sensitivity wavelength is g-line or h-line, the exposure device used is UVD-S405.

[0359] The maximum sensitivity wavelength refers to the wavelength at which the minimum exposure amount is smallest when the minimum exposure amount at which the photosensitive resin layer reacts is calculated as the spectral sensitivity for each wavelength of light.

[0360] The maximum sensitivity wavelength was previously determined as follows. When a photosensitive resin layer on a substrate is irradiated with light of a specific wavelength through a Stouffer 4105 step wedge tablet, the minimum exposure at which the photosensitive material reacts is defined as Emin. By changing the wavelength of irradiation, a spectral sensitivity curve can be obtained. Since Emin differs for each wavelength, the wavelength at which it has the minimum value is the wavelength of maximum sensitivity.

[0361] In the negative photosensitive resin layer, the minimum exposure amount at which the exposed area remains is defined as Emin. When the light source has a discrete light quantity distribution (such as g-line, h-line, i-line) like a high-pressure mercury lamp, and when the wavelength of the irradiated light is controlled using a bandpass filter or the like, the wavelength with the highest sensitivity among the light that actually hits the photosensitive material is regarded as the maximum sensitivity wavelength. For example, suppose that the minimum value of the spectral sensitivity curve of a certain photosensitive material is at 290 nm, and the second is at 365 nm (i-line). Since high-pressure mercury lamps practically emit almost no light at 290 nm, when exposing this photosensitive material with a high-pressure mercury lamp, the maximum sensitivity wavelength is 365 nm.

[0362] The maximum sensitivity wavelength of the photosensitive transfer material 1 was i-line, 356 nm.

[0363] The development was carried out using a 1.0% by weight aqueous solution of sodium carbonate at 28°C as the developer, and the development time was set to twice the minimum development time. The minimum development time refers to the shortest time required for the unexposed portion of the photosensitive resin layer to completely dissolve by development processing. Development was carried out by shower development.

[0364] Specifically, first, the shortest time required for the unexposed photosensitive resin layer to completely dissolve by shower development was determined. Next, shower development was performed on the pattern-exposed photosensitive resin layer for twice the minimum development time. After that, the layer was treated with an Air Knife to remove the developer, and then showered with pure water at 25°C for 30 seconds, and then treated with an Air Knife again.

[0365] The development conditions for determining the maximum sensitivity wavelength, the development conditions for determining the maximum remaining film step number, and the development conditions for developing the samples were all the same as those described above.

[0366] <Photomask light shielding width Wm> The light-shielding width Wm of the photomask was determined by exposure and development using an exposure mask in which the dimensions of each light-shielding portion varied in 0.1 μm increments within a range of 10 μm length × 10 μm width to 20 μm length × 20 μm width, and the light-shielding width that gave the opening width of the resin pattern (resist opening width) in the obtained sample closest to 15.0 μm was selected.

[0367] <Transmittance at the wavelength of maximum sensitivity> Photosensitive transfer material 1 was applied to a 0.7 mm thick soda glass and the photosensitive transfer material 1 was laminated to the soda glass using a roll laminator under conditions of a temperature of 100°C, a linear pressure of 0.5 MPa, and a linear speed (lamination speed) of 4 m / min. A transfer layer (i.e., a photosensitive resin layer, a water-soluble resin layer, and a thermoplastic resin layer) and a temporary support were then arranged in this order on the soda glass.

[0368] The transmittance of the above sample at the maximum sensitivity wavelength (365 nm) was measured using a soda glass having a thickness of 0.7 mm as a reference.

[0369] <Examples 2 to 21, Comparative Examples 1 to 2> Photosensitive transfer materials 1 to 16 were obtained in the same manner as the photosensitive transfer material 1 produced in Example 1, except that the compositions shown in Tables 1 and 2 were used. The laminates of Examples 2 to 21 and Comparative Examples 1 and 2 were produced using any of the photosensitive transfer materials 1 to 16 described in Tables 1 and 2, and following the same procedure as in Example 1, except that the exposure method was changed as described in Tables 3 to 5.

[0370] <Evaluation> The laminates produced in the Examples and Comparative Examples were used to evaluate the following items.

[0371] (Resin pattern opening width Wr / Photomask light shielding width Wm) The ratio of the opening width Wr of the resin pattern to the light shielding width Wm of the corresponding photomask was defined as Wr / Wm. The opening width Wr of the resin pattern was determined by manufacturing four laminates of each of the examples and the comparative examples under the same conditions, measuring the opening widths (parts dissolved in the developer) at 16 points on the surface of each laminate, totaling 64 points, and using the average value.

[0372] (Photomask fidelity) The length (Wd) of the diagonal line of the opening pattern in which the opening width Wr (average value) of the obtained resin pattern is 15.0 μm and the length (Wd) of the diagonal line on both sides of the diagonal line Length between protrusions (Wp1 and Wp2) were measured, respectively. FIG. 2A shows a model diagram of an opening pattern in which no protrusions are observed on either side of the diagonal, and FIG. 2B shows a model diagram of an opening pattern in which protrusions are observed on either side of the diagonal. The value obtained by the following formula was rounded off to the first decimal place to obtain the protrusion ratio. Protrusion rate (%)=((Wp1+Wp2) / 2 / Wd)-1)×100 As shown in FIG. 2A, when no protrusions were observed on either side of the diagonal line (i.e., when Wp1 and Wp2 were not present), the protrusion rate was determined to be 0%. Based on the obtained protrusion ratio, the photomask fidelity was evaluated according to the following evaluation criteria.

[0373] -Evaluation criteria- 5: Protrusion rate 0% 4:Protrusion rate over 0% but below 5% 3: Protrusion rate more than 5% and less than 10%. 2:Protrusion ratio over 10% and below 20% 1: Protrusion rate over 20%

[0374] (Line width uniformity) Four laminates each of the examples and comparative examples were produced under the same conditions, and for each laminate, the opening widths (parts dissolved in the developer) were measured at 16 points on the surface, totaling 64 points, to determine the standard deviation σ. Based on the obtained standard deviation σ, the line width uniformity was evaluated according to the following evaluation criteria.

[0375] -Evaluation criteria- 5: σ≦0.2μm 4: 0.2μm<σ≦0.5μm 3: 0.5μm<σ≦1.0μm 2:1.0μm<σ≦1.5μm 1:1.5μm<σ

[0376] (Takt time) The exposure amount set by the exposure machine was regarded as the takt time, and evaluation was performed according to the following criteria. 5: Exposure setting of exposure machine: 30 mJ / cm 2 below 4: Exposure setting of exposure machine: 30 mJ / cm 2 Super 40mJ / cm 2 below 3: Exposure setting of exposure machine: 40 mJ / cm 2 Super 50mJ / cm 2 below 2: Exposure setting of exposure machine: 50 mJ / cm 2 Super 60mJ / cm 2 below 1: Exposure setting of exposure machine: 60 mJ / cm 2 Super

[0377] (Pinhole) Area of ​​the laminated resin pattern (resist) other than the openings: 1 mm 2The resin pattern was observed using an optical microscope (MX-63 manufactured by Olympus), and the number of defects (pinholes) occurring on the resin pattern was counted and evaluated according to the following evaluation criteria. 5: 2 or less pinholes 4: More than 2 pinholes and up to 5 pinholes 3: More than 5 pinholes and up to 10 pinholes 2: More than 10 pinholes and up to 50 1: More than 50 pinholes

[0378] The above evaluation results are shown in Tables 3 to 5.

[0379] [Table 1]

[0380] [Table 2]

[0381] A blank space in the composition columns shown in Tables 1 and 2 indicates that the corresponding component is not contained.

[0382] The following abbreviations shown in Tables 1 and 2 have the following meanings, respectively. "M / B": Ratio of the total mass of polymerizable compounds to the total mass of polymer "Polymer B1": benzyl methacrylate (BzMA) / methacrylic acid (MAA) / acrylic acid (AA) = 78 / 14.5 / 7.5 (mass ratio), Mw: 12,500, acid value: 187 mg KOH / g, glass transition temperature: 75°C, solid content: 30 mass% "Polymer B2": styrene (St) / methyl methacrylate (MMA) / methacrylic acid (MAA) / methacrylic acid-glycidyl methacrylate (GMA-MAA) = 47.7 / 1.3 / 19 / 32, Mw: 20,000, acid value: 124 mg KOH / g, glass transition temperature: 76°C, solid content: 30% by mass Incidentally, "methacrylic acid-glycidyl methacrylate" refers to a structural unit obtained by reacting a carboxy group of a structural unit derived from methacrylic acid with an epoxy group of glycidyl methacrylate. "Polymer B3": styrene (St) / methyl methacrylate (MMA) / methacrylic acid (MAA)=52 / 19 / 29, Mw: 50,000, acid value: 189 mg KOH / g, glass transition temperature: 131° C., solid content: 30% by mass "A-DCP": NK Ester A-DCP, tricyclodecane dimethanol diacrylate manufactured by Shin-Nakamura Chemical Co., Ltd. "8UX-015A": 8UX-015A, UV-curable urethane acrylate manufactured by Taisei Fine Chemical Co., Ltd. "TO-2349": Aronix TO-2349 manufactured by Toagosei Co., Ltd. "CBT-1": CBT-1 manufactured by Johoku Chemical Industry Co., Ltd., Carboxybenzotriazole "F-552": Megafac F-552 manufactured by DIC Corporation, fluorosurfactant, solid content = 30% by mass (methyl ethyl ketone solution) "PVA": PVA205, polyvinyl alcohol, manufactured by Kuraray Co., Ltd. "PVP": K-30, polyvinylpyrrolidone, manufactured by Nippon Shokubai Co., Ltd. "HPMC": Metolose 60SH-03, hydroxypropyl methylcellulose, manufactured by Shin-Etsu Chemical Co., Ltd. "F-444": Megafac F-444, a fluorosurfactant manufactured by DIC Corporation "MeOH": Methanol "BPE-500": NK Ester BPE-500, (2,2-bis(4-(methacryloxypentaethoxy)phenyl)propane) manufactured by Shin-Nakamura Chemical Co., Ltd. "BPE-100": A mixture of NK Ester BPE-100 manufactured by Shin-Nakamura Chemical Co., Ltd., (2,2-bis(4-(methacryloxymonoethoxy)phenyl)propane, and (2,2-bis(4-(methacryloxydiethoxy)phenyl)propane). "Aronix M-270": Aronix M-270 manufactured by Toagosei Co., Ltd., polypropylene glycol diacrylate "B-IMD": B-CIM (2-(2-chlorophenyl)-4,5-diphenylimidazole dimer) manufactured by Kurogane Kasei Co., Ltd. "EAB-F": 4,4′-bis(diethylamino)benzophenone obtained from Sanyo Trading Co., Ltd. "Phenidone 1% MEK solution": Methyl ethyl ketone solution containing 1% by mass of phenidone "Compound A": N-phenylcarbamoylmethyl-N-carboxymethylaniline manufactured by Fujifilm Wako Pure Chemical Corporation "LCV": Leuco Crystal Violet manufactured by Tokyo Chemical Industry Co., Ltd., a dye that changes color when exposed to radicals "MMPGAc": 1-methoxy-2-propyl acetate "MEK": Methyl ethyl ketone "MFG": 1-methoxy-2-propanol

[0383] [Table 3]

[0384] [Table 4]

[0385] [Table 5]

[0386] As shown in Tables 3 to 5, it is evident that according to the manufacturing methods of the laminates of the Examples, resin patterns with excellent photomask fidelity can be obtained. [Explanation of symbols]

[0387] 10: photosensitive transfer material, 11: temporary support, 12: transfer layer, 13: thermoplastic resin layer, 15: water-soluble resin layer, 17: photosensitive resin layer, 19: protective film, Wd: diagonal length of opening pattern, Wr: opening width of resin pattern, Wp1: length between protrusions, Wp2: length between protrusions

Claims

1. a lamination step of laminating a photosensitive transfer material including a temporary support and a transfer layer having a photosensitive resin layer containing an alkali-soluble resin, a photopolymerization initiator, and a polymerizable compound having an ethylenic double bond, to a substrate such that the transfer layer side of the photosensitive transfer material is in contact with the substrate; an exposure step of pattern-exposing the transfer layer through a photomask; and a developing step of developing the pattern-exposed transfer layer to form a resin pattern, The exposure dose S of the pattern exposure 1 However, after the photosensitive transfer material and the substrate are laminated together, the photosensitive transfer material is exposed to light using a Stouffer 21-step tablet as a mask, and then developed. The exposure dose S at which the maximum number of remaining film steps becomes 6 is 0 The exposure is 80% or less of the above. A method for manufacturing a laminate.

2. The method for producing a laminate according to claim 1 , wherein the photosensitive transfer material has a transmittance of 70% or more at a wavelength of maximum sensitivity.

3. The method for producing a laminate according to claim 1 or 2, wherein the exposure step is a step of performing pattern exposure by further interposing an ND filter between the photosensitive resin layer and an exposure light source.

4. The method for producing a laminate according to claim 3 , wherein the ND filter has a reflectance of 30% or less.

5. The method for producing a laminate according to claim 3, wherein the transmittance of the ND filter is 25% to 75%.

6. The method for producing a laminate according to claim 1 or 2, wherein an exposure method used in the exposure step is a contact exposure method.

7. The method for producing a laminate according to claim 1 or 2, wherein the photosensitive resin layer has a thickness of 5 μm or less.

8. The method for producing a laminate according to claim 1 or 2, wherein the photopolymerization initiator is a hexaarylbisimidazole-based photopolymerization initiator.

9. The method for producing a laminate according to claim 1 or 2, wherein the photosensitive resin layer further contains a sensitizer.

10. The method for producing a laminate according to claim 9, wherein a value obtained by dividing a content of the photopolymerization initiator in the photosensitive resin layer by a content of the sensitizer in the photosensitive resin layer is 20 or more and 300 or less on a mass basis.

11. The method for producing a laminate according to claim 9 , wherein the sensitizer is a benzophenone-based sensitizer.

12. 10. The method for producing a laminate according to claim 9, wherein when a film thickness of the photosensitive resin layer is X μm and a solid content of the sensitizer in the photosensitive resin layer is Y mass%, a value obtained by multiplying the value of X by the value of Y and further multiplying the result by 10 is 0.5 to 5.

0.

13. The exposure amount S 0 , but 60 mJ / cm 2 The method for producing a laminate according to claim 1 or 2, wherein:

14. The method for producing a laminate according to claim 1 or 2, further comprising the step of: providing an intermediate layer between the temporary support and the photosensitive resin layer.

15. The method for producing a laminate according to claim 14 , wherein the intermediate layer has a water-soluble resin layer.

16. The method for producing a laminate according to claim 14 , wherein the intermediate layer has a thermoplastic resin layer and a water-soluble resin layer.

17. The method for producing a laminate according to claim 1 or 2, further comprising a step of removing the temporary support between the laminating step and the exposure step.

18. The method for producing a laminate according to claim 1 or 2, wherein an opening width Wr of the resin pattern is wider than a light shielding width Wm of a light shielding pattern of the photomask.

19. The method for producing a laminate according to claim 18 , wherein an opening width Wr of the resin pattern is 20 μm or less.

20. the substrate has a metal layer on a surface in contact with the photosensitive transfer material, a step of performing an etching process on the metal layer in an area where the resin pattern is not formed after the developing step, and then removing the resin pattern to form a metal pattern layer, or a step of performing a plating process on the metal layer in an area where the resin pattern is not formed, and then removing the resin pattern, and performing an etching process on the metal layer exposed by removing the resin pattern to form a metal pattern layer. A method for producing the laminate according to claim 1 or 2.

21. the substrate is a metal substrate having a first surface and a second surface opposite the first surface; a step of performing an etching process on the metal substrate in an area where the resin pattern is not formed after the developing step to form a through hole penetrating the metal substrate, and then removing the resin pattern to form a metal pattern layer. A method for producing the laminate according to claim 1 or 2.

22. The method for producing a laminate according to claim 21, wherein the metal substrate contains an iron-nickel alloy.

23. The method for producing a laminate according to claim 21 , wherein the metal pattern layer has a rectangular through-hole.

24. The method for producing a laminate according to claim 21 , wherein the laminate is a metal mask.

25. The method for producing a laminate according to claim 20 , wherein the laminate is a semiconductor package.

Citation Information

Patent Citations

  • Photosensitive element, method for forming resist pattern, and method for producing printed circuit board

    WO2012081680A1

Cited By

  • Photosensitive resin composition, photosensitive element, method for forming resist patterns, and method for manufacturing printed circuit boards

    JP7952319B2

  • Photosensitive resin composition, photosensitive element, method for forming resist pattern, and method for producing printed wiring board

    JPWO2025115820A1