Cement-based solidification material
A cement-based solidifying material incorporating fine bamboo charcoal powder addresses carbon emissions and bamboo decline by enhancing cement efficiency and maintaining strength and fluidity, providing a sustainable solution for soil stabilization.
Patent Information
- Application Number
- JP2023059612
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
The cement industry emits significant carbon dioxide during manufacturing, and there is a need to reduce greenhouse gas emissions while also addressing the decline of bamboo usage leading to biodiversity loss and natural disasters, necessitating new uses for bamboo materials.
A cement-based solidifying material is developed using a hydraulic composition containing Portland cement, blast furnace slag, gypsum, and fine bamboo charcoal powder, with a ratio of fine bamboo charcoal powder between 0.1 to 30 parts by mass, which enhances cement utilization efficiency and reduces carbon dioxide emissions.
The use of fine bamboo charcoal powder in cement-based solidifying materials effectively reduces carbon dioxide emissions and maintains strength and fluidity, offering a sustainable alternative to conventional cement-based agents.
Smart Images

Figure 2024146608000003 
Figure 2024146608000004 
Figure 2024146608000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a hydraulic composition containing Portland cement, blast furnace slag, and gypsum, and a cement-based solidification material containing fine bamboo charcoal powder. [Background technology]
[0002] Cement-based solidification materials used to solidify soil have been developed since the 1970s through the intensive research and development of various cement manufacturers, in response to soils for which the previously used cement and lime were unable to fully achieve the target properties, such as strength. Cement-based solidification materials are made by adding active ingredients to the base material Portland cement, such as pozzolanic materials such as blast furnace slag and fly ash, strength enhancers with special ingredients such as alumina cement and jet cement, and cement stimulants such as gypsum and sodium sulfate, to reinforce specific ingredients in the cement, adjust the particle size, and add effective ingredients according to the soil quality. Products such as general-purpose solidification materials (solidification materials for special soil and solidification materials for general soft soil), solidification materials for high organic soil, and dust-suppressing solidification materials are sold.
[0003] Cement-based solidification materials are used in a wide range of applications, including strengthening the bearing capacity of the foundations of civil engineering structures such as retaining walls, box culverts and caissons, roadbeds and subgrades, and the foundations of architectural structures in residential areas. In recent years, they have also been used as countermeasures against liquefaction on reclaimed land during earthquakes, and to strengthen embankments to prevent flooding from high tides and river flooding.
[0004] As mentioned above, various active ingredients are added to cement-based solidification materials depending on the purpose of improvement, so they are not included in the category of "cement" in the Japanese Industrial Standards. Therefore, among cement materials, there is a large degree of freedom in the selection of raw materials used in material design (Non-Patent Document 1).
[0005] In addition, when using cement-based solidification materials, the strength required varies depending on the magnitude of the load on the ground and the purpose of the improvement. Furthermore, unlike concrete, the fine and coarse aggregates are not always fixed, and the properties of the soil to be improved (grain size, water content, organic matter content that inhibits the reaction of cement, etc.) vary widely, so generally, before using it on site, soil is sampled from the ground to be improved, and a process is carried out to confirm the relationship between the amount of cement-based solidification material added and the strength, and then the amount to be used on site is determined. [Prior art documents] [Non-patent literature]
[0006] [Non-Patent Document 1] Japan Cement Association, "Ground Improvement Manual Using Cement-Based Solidification Materials (5th Edition)" (2021) Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, while there has been a demand to reduce greenhouse gas emissions, the cement industry emits a large amount of carbon dioxide during manufacturing, and there is a demand to reduce carbon dioxide emissions by reducing the amount of cement used.
[0008] On the other hand, the decline in bamboo use and the decline of forestry in recent years have led to the degradation of forests, which are contributing factors in natural disasters such as landslides. Of these, bamboo grows faster than trees and has been widely used as a building material, but the recent decline in bamboo use has become a serious problem of "bamboo damage" that leads to a decline in biodiversity. Therefore, since expanding the uses for which bamboo can be used will also help prevent bamboo damage, there is a need to find new and unprecedented ways to use bamboo that will lead to a reduction in carbon dioxide emissions in the cement industry. [Means for solving the problem]
[0009] The inventors have conducted extensive research to solve the above problems. As a result, they discovered that carbonizing bamboo into fine powder and using it as a cement-based solidification material could lead to a new way of using it, which led to the completion of this research.
[0010] That is, it is a cement-based solidification material characterized by containing a hydraulic composition including Portland cement, blast furnace slag, and gypsum, and bamboo charcoal fine powder.
[0011] The ratio of the bamboo charcoal fine powder to 100 parts by mass of the hydraulic composition is preferably 0.1 parts by mass or more and less than 30 parts by mass. In addition, the gypsum is preferably anhydrous gypsum or dihydrate gypsum. Effect of the Invention
[0012] According to the present invention, the use of bamboo charcoal fine powder contributes to the effective use of bamboo materials and the reduction of the amount of cement used as a cement-based solidification material, thereby contributing to the reduction of carbon dioxide emissions. Furthermore, by setting the ratio of bamboo charcoal fine powder to 0.1 parts by mass or more and less than 30 parts by mass, it is possible to provide a cement-based solidification material that does not suffer a significant decrease in strength compared to cement-based solidification materials that do not contain bamboo charcoal fine powder, and that ensures fluidity when made into a paste. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a diagram showing the relationship between the amount of bamboo charcoal fine powder per 100 parts by mass of a hydraulic composition and the paste flow. [Diagram 2] FIG. 2 shows the relationship between the amount of bamboo charcoal fine powder per 100 parts by mass of the hydraulic composition and the compressive strength of the mortar. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] An embodiment of the present invention will be described.
[0015] The cement-based solidification material of the present invention is characterized in that it contains a hydraulic composition containing Portland cement, blast furnace slag, and gypsum, and bamboo charcoal fine powder.
[0016] As the Portland cement used in the hydraulic composition in the cement-based solidification material of the present invention, any commercially available Portland cement can be used without restrictions. From the viewpoint of strength, ordinary Portland cement, high-early-strength Portland cement, and ultra-high-early-strength Portland cement are preferable, and from the viewpoint of economy, ordinary Portland cement is more preferable.
[0017] The blast furnace slag used in the hydraulic composition of the cement-based solidification material of the present invention can be any commercially available blast furnace slag without any restrictions. Among them, ground blast furnace slag used as a cement raw material or concrete admixture is more preferable. If it is difficult to procure blast furnace slag alone, commercially available blast furnace cement types A, B, and C may be used.
[0018] The gypsum used in the hydraulic composition in the cement-based solidification material of the present invention can be any commercially available anhydrous gypsum, hemihydrate gypsum, or dihydrate gypsum, without any particular restrictions. In addition, gypsum such as phosphate gypsum, hydrofluoric gypsum, flue gas desulfurization gypsum, titanic gypsum, refined gypsum, etc., can be used without any restrictions, regardless of the by-product process. When the cement-based solidification material is mixed with water and used in a paste form, it is preferable to use anhydrous gypsum or dihydrate gypsum, since the viscosity of the paste does not increase. Anhydrous gypsum and dihydrate gypsum may be used either alone or in combination. It is preferable to use anhydrous gypsum from the viewpoint of strength.
[0019] The bamboo charcoal fine powder used in the cement-based solidification material of the present invention can be any commercially available bamboo charcoal fine powder without any particular restrictions. The higher the carbonization temperature, the higher the carbon content and the greater the carbon dioxide reduction effect, so it is preferable to use bamboo charcoal produced at a high temperature of 800°C or higher, but this is not limiting. In addition, the smaller the average particle size of the bamboo charcoal fine powder, the lower the fluidity when the cement-based solidification material of the present invention is made into a paste, so the average particle size of the bamboo charcoal fine powder is preferably 75 μm or less, and more preferably 50 μm or less.
[0020] The mixing ratio of the above materials is preferably 0.1 parts by mass or more and less than 30 parts by mass of bamboo charcoal fine powder per 100 parts by mass of hydraulic composition containing Portland cement, blast furnace slag, and gypsum. The more the bamboo charcoal fine powder is used, the more difficult it becomes to obtain sufficient strength, but if the bamboo charcoal fine powder is less than 30 parts by mass, the strength is not significantly impaired. In addition, when the cement-based solidification material is made into a paste, there is no loss of fluidity. Furthermore, from the viewpoint of reducing carbon dioxide emissions as a cement-based solidification material by reducing the amount of Portland cement used, and of uniformly mixing the bamboo charcoal fine powder in the cement-based solidification material, the more the bamboo charcoal fine powder is used, and more preferably 5 parts by mass or more and less than 30 parts by mass.
[0021] The cement-based solidification material of the present invention may contain concrete admixtures such as limestone fine powder, fly ash, silica fume, bentonite, etc., within the scope of not impairing the effect of the present invention.
[0022] The cement-based solidification material of the present invention can be produced by mixing a hydraulic composition containing Portland cement, blast furnace slag, and gypsum with bamboo charcoal fine powder. A commercially available cement-based solidification material may be used as the hydraulic composition. Portland cement, blast furnace slag, gypsum, and bamboo charcoal fine powder may be mixed instead of the hydraulic composition. Any mixer capable of mixing powders can be used for mixing without any restrictions. For example, a mixer that generally mixes mortar or concrete can be used. Specific examples include a pan-type mixer, a forced two-shaft mixer, a tilting mixer, and a mortar mixer. In addition, a mixer equipped with a mechanism capable of shearing at high speed, such as a chopper, may be used for the purpose of homogeneous mixing and dispersion. EXAMPLES
[0023] In order to explain the present invention more specifically, examples and comparative examples will be given below, but the present invention is not limited to these examples.
[0024] 1.Materials used (a) Hydraulic composition The hydraulic composition was a mixture of ordinary Portland cement, blast furnace slag, and anhydrous gypsum.
[0025] (b) Fine bamboo charcoal powder The bamboo charcoal fine powder used was commercially available.
[0026] 2.Paste flow test (1) Paste flow formula A paste flow test was conducted to confirm the fluidity when mixed with water. The mixture used in the paste flow test is shown in Table 1. The hydraulic composition and bamboo charcoal fine powder were mixed in advance with water to form a paste to prepare a cement-based solidification material. The mixing ratio of the cement-based solidification material to water was 1:0.5 by weight.
[0027] (2) Mixing A Hobart mixer was used for mixing. The cement-based solidification material was added to a predetermined amount of water that had been measured in advance in a mixing bowl, and mixed at low speed for 30 seconds. After mixing, the sample adhering to the paddle and inside the mixing bowl was scraped off for 30 seconds, and after the scraping, the mixture was mixed at low speed for another 2 minutes to prepare a paste sample.
[0028] (3) Paste flow test The paste flow test was performed according to the method described in Appendix 3.M-103 "Quality Criteria for Self-Leveling Materials" in JASS15 "Plastering Works" of the Standard Specifications for Building Construction and Commentary. A polyvinyl chloride pipe (capacity 100 ml) with an inner diameter of 50 mm and height of 51 mm was placed in the center of a polished glass plate 300 mm in length and width, and the mixed paste sample was filled into the pipe, which was then lifted up. After the spread had stopped, the diameters in two perpendicular directions were measured, and the average value was taken as the paste flow value.
[0029] (4) Paste flow The paste flow measurement results are shown in Table 1. For the cement-based solidification material that did not contain bamboo charcoal fine powder (Reference Example 1), the flow was 147.30 mm. For the bamboo charcoal fine powder only (Reference Example 2), the flow was 50.00 mm, the same as the inner diameter of the flow cone, and the flow did not spread. The particles of the bamboo charcoal fine powder are hollow, so they are highly absorbent, and it can be said that this is the reason why the paste flow did not spread.
[0030] In Examples 1 to 3, the paste flow became smaller as the amount of fine bamboo charcoal powder increased, but it spread further after the flow cone was removed.
[0031] Figure 1 shows the relationship between the amount of bamboo charcoal fine powder per 100 parts by mass of hydraulic composition and paste flow. As mentioned above, the more bamboo charcoal fine powder there is, the smaller the paste flow, and it can be seen that this result shows a correlation. Furthermore, an exponential approximation was performed on this correlation to estimate the bamboo charcoal fine powder content at which the paste flow would not spread (50.00 mm). As a result, it was predicted that the paste flow would not spread if the amount of bamboo charcoal fine powder was 30 parts by mass or more per 100 parts by mass of cement-based solidification material.
[0032] Since cement-based solidification materials are sometimes used in paste form, a larger flow value in the paste is preferable from the viewpoint of workability. Therefore, it is preferable to use less than 30 parts by mass of bamboo charcoal fine powder for 100 parts by mass of hydraulic composition containing Portland cement, blast furnace slag, and anhydrous gypsum.
[0033] [Table 1]
[0034] 3. Mortar compressive strength test (1) Mortar Mixture To confirm the effect of bamboo charcoal fine powder, a strength test was conducted using mortar. The ratio of hydraulic composition and bamboo charcoal fine powder in the cement-based solidification material was the same as the ratio in the paste flow test shown in Table 1. The hydraulic composition and bamboo charcoal fine powder were mixed in advance to make the cement-based solidification material. The mortar was mixed in a ratio of 100 parts by mass of cement-based solidification material, 300 parts by mass of fine aggregate, and 50 parts by mass of water. Tap water was used as the water, and standard sand for cement strength tests (sold by: General Incorporated Association Cement Association) was used as the fine aggregate.
[0035] (2) Mixing The mixing was carried out in accordance with JIS R 5201 (physical testing method for cement). The mixing method is explained below.
[0036] A Hobart mixer was used for mixing. After adding water and cement-based solidification material to the mixing bowl, the mixer was started at low speed. Thirty seconds after starting the mixer, fine aggregate was added at a steady rate over a period of 30 seconds. Next, the mixture was mixed at high speed for 30 seconds, followed by a 90-second pause. During the first 30 seconds of the pause, any mortar adhering to the mixing bowl and paddle was scraped off with a spoon. After the pause, the mixture was mixed again at high speed for 60 seconds.
[0037] (3) Molding The molding was carried out in accordance with JIS R 5201 (physical testing method for cement). The molding method is explained below.
[0038] A 40 x 40 x 160 mm formwork was used, and the mortar was immediately poured into the formwork after mixing. A table vibrator was used for pouring. The pouring method was as follows: The first layer of mortar was filled to about half the height of the formwork in 15 seconds from the start of vibration. After a 15-second interval, the remaining amount of mortar was filled in over the same 15 seconds as the first layer. Vibration was continued for a further 75 seconds. Finally, the excess was carefully scraped off so as not to damage the specimen, and the top surface was smoothed.
[0039] (4)Curing After molding, the mixture was covered with an iron plate for 24 hours after mixing to prevent moisture from evaporating and stored at 20°C. After 24 hours had passed, the mixture was removed from the mold and then cured in water at 20°C for the specified period.
[0040] (5) Compressive strength measurement The compressive strength was measured according to JIS R 5201 (physical testing method for cement). The ages of the materials measured were 7 and 28 days.
[0041] (6) Mortar compressive strength The measurement results of the mortar compressive strength are shown in Table 2. Reference Example 1 shows the measurement results when 100 parts by mass of a hydraulic composition was used as a cement-based solidification material without containing bamboo charcoal fine powder. The mortar compressive strength was 22.0 N / mm at 7 days of age. 2 , 46.4N / mm at 28 days 2 Moreover, Reference Example 2 is the measurement result when only bamboo charcoal fine powder was used, which does not contain a hydraulic composition, and the strength could not be measured at both 7 and 28 days of age. Reference Example 2 collapsed when it was removed from the formwork, and the compressive strength could not be measured. The reason for this is that bamboo charcoal fine powder alone does not have hydraulic properties.
[0042] In Examples 1 to 3, bamboo charcoal fine powder was mixed into the hydraulic composition. The more the bamboo charcoal fine powder was added, the smaller the mortar compressive strength became. However, even in Example 3, the compressive strength was 16.6 N / mm at 7 days old. 2 , 36.2N / mm at 28 days 2It can be said that the hardened mortar has sufficient compressive strength.
[0043] Figure 2 shows the relationship between the amount of bamboo charcoal fine powder per 100 parts by mass of hydraulic composition and the compressive strength of mortar. It can be said that there is a correlation between the amount of bamboo charcoal fine powder and the compressive strength of mortar. It can be said that sufficient compressive strength is obtained when the amount of bamboo charcoal fine powder is less than 30 parts by mass, which is enough to obtain a flow value in the paste flow test.
[0044] [Table 2]
Claims
1. A cement-based solidification material comprising a hydraulic composition containing Portland cement, blast furnace slag, and gypsum, and bamboo charcoal fine powder.
2. 2. The cement-based solidification material according to claim 1, wherein the ratio of the bamboo charcoal fine powder is 0.1 parts by mass or more and less than 30 parts by mass per 100 parts by mass of the hydraulic composition.
3. 2. The cement-based solidification material according to claim 1, characterized in that the gypsum is anhydrous gypsum or dihydrate gypsum.