Laminated film

A laminated film with a base layer and coat layer using active energy ray-curable resin, filler, and leveling agent addresses glare and transmission clarity issues, providing enhanced optical and mechanical properties for improved display appearance.

JP2024146613APending Publication Date: 2024-10-15LINTEC CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023059620
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing laminated films for optical displays suffer from issues such as Newton's rings and glare, leading to deteriorated visibility and appearance quality, particularly under bright lighting conditions, and existing solutions compromise transmission clarity.

Method used

A laminated film with a base layer and a coat layer composed of active energy ray-curable resin, filler, and leveling agent, featuring specific surface shape and kurtosis parameters to prevent glare and maintain high transmission clarity.

Benefits of technology

The laminated film achieves excellent optical and mechanical properties, ensuring high transmission clarity and superior appearance quality, reducing graininess under bright lighting conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146613000007
    Figure 2024146613000007
  • Figure 2024146613000008
    Figure 2024146613000008
  • Figure 2024146613000009
    Figure 2024146613000009
Patent Text Reader

Abstract

To provide a laminated film having excellent optical properties and mechanical properties, high transmission clarity and excellent appearance quality and to provide an optical display having excellent appearance quality and comprising the laminated film.SOLUTION: There is provided a laminated film having a substrate layer and a coating layer. The coating layer is a layer formed from a composition for forming the coating layer containing (A) a component: an active energy ray-curable resin, (B) a component: a filler and (C) a component: a leveling agent, and when the surface shape of projections having a projection width of 10 μm or more which appear on the surface opposite to the substrate layer side of the coating layer is measured by an optical interference type surface shape observation device, the average value of θ(°) indicated by the following expression (1) is 0.4(°) or more, or the Kurtosis (Rku) on the surface opposite to the substrate layer side of the coating layer is 35 or more. (In the expression, when a surface on which the projection is not present is defined as a reference surface, dZ (μm) represents the height of the projection from the reference surface at a point (point B) of dX (μm) in a horizontal direction toward the center of the projection from the periphery (point A) of the projection and dX is 5 (μm) and represents a distance in the horizontal direction from the point A to the point B.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated film having high appearance quality that is suitable for use in optical displays. [Background technology]

[0002] In recent years, devices with a touch panel mounted on a display have come into widespread use as information terminals, etc. For example, in a resistive touch panel, which is known as one type of touch panel, a gap is provided between a transparent plastic film and a substrate, and input is performed by pressing the input surface with a finger, a pen, or the like to bring the transparent plastic film into partial contact with the substrate.

[0003] Here, when the transparent plastic film and the substrate come into contact during input, problems such as Newton's rings due to optical interference are generated on the transparent plastic film, which deteriorates the visibility and appearance of the display. In order to solve this problem, a layer on which fine irregularities are formed by fine particles or the like is laminated on one or both sides of the transparent plastic film (Patent Documents 1 to 3). However, laminating such a layer on which fine irregularities are formed also causes a problem of reduced transmission clarity. Specifically, when the display is placed in a bright place such as under a fluorescent lamp, a grainy texture (roughness) appears on the display surface, which may impair the appearance (appearance quality) of the display.

[0004] In relation to the present invention, Patent Document 4 proposes an optical film in which the antiglare properties and transmitted image clarity (transmitted image clarity), which are in a trade-off relationship, are improved by mixing a generally flat portion and a portion having an inclined angle on the film surface and controlling the diffuse reflection properties. However, the transmitted image clarity of the obtained optical film was far from satisfactory. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2012-203323 A [Patent Document 2] JP 2013-152396 A [Patent Document 3] JP 2013-171126 A [Patent Document 4] WO2009 / 001911 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above-mentioned circumstances, and has an objective of providing a laminate film to be laminated on a display, which not only prevents the occurrence of Newton rings and glare, but also has excellent optical properties and mechanical properties, high transmission clarity, and excellent appearance quality, as well as an optical display which includes the laminate film and has excellent appearance quality. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted extensive research into a laminate film having a base layer and a coating layer in order to solve the above problems. the result, (α) The present inventors have found that a laminate film in which the coating layer is a layer formed from a coating layer-forming composition containing component (A): an active energy ray-curable resin, component (B): a filler, and component (C): a leveling agent, and which satisfies the following (β1) and / or (β2), has excellent optical properties and mechanical properties, high transmission clarity, and excellent appearance quality, and can be suitably used for optical displays, particularly touch panels, etc., and have completed the present invention. (β1) When the surface shape of protrusions having a protrusion width of 10 μm or more appearing on the surface of the coating layer opposite the substrate layer side is measured using an optical interference type surface profile observation device, the average value of θ(°) of tan θ shown in equation (1) described below is 0.4(°) or more. (β2) The kurtosis (Rku) of the surface of the coating layer opposite to the substrate layer side is 35 or more.

[0008] Thus, according to the present invention, there are provided the following laminate films [1] to [8] and an optical display [9].

[0009] [1] A laminated film having a base layer and a coating layer, the coating layer being formed from a coating layer-forming composition containing component (A): an active energy ray-curable resin, component (B): a filler, and component (C): a leveling agent; A laminated film characterized in that, when the surface shape of protrusions having a width of 10 μm or more appearing on the surface of the coating layer opposite the substrate layer side is measured using an optical interference type surface shape observation device, the average value of θ (°) represented by the following formula (1) is 0.4 (°) or more.

[0010]

number

[0011] (In the formula, dZ (μm) represents the height of the protrusion from a reference plane at a point (point B) that is dX (μm) in the horizontal direction from the periphery (point A) of the protrusion toward the center of the protrusion, when the surface on which the protrusion does not exist is taken as the reference plane, and dX is 5 (μm) and represents the horizontal distance from point A to point B.)

[0012] [2] A laminated film having a base layer and a coating layer, the coating layer being formed from a coating layer-forming composition containing component (A): an active energy ray-curable resin, component (B): a filler, and component (C): a leveling agent; A laminate film, wherein the kurtosis (Rku) of the surface of the coating layer opposite the substrate layer side is 35 or more.

[0013] [3] The laminated film according to [1] or [2], wherein the component (B) is an acrylic fine particle.

[0014] [4] The laminate film according to [1] or [2], wherein the content of the (C) component is 0.3 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the (A) component.

[0015] [5] The laminate film according to [1], wherein the kurtosis (Rku) of the surface of the coating layer opposite the substrate layer side is 35 or more.

[0016] [6] The laminate film according to [1] or [2], wherein the kurtosis (Rku) of the surface of the coating layer opposite the substrate layer side is 300 or less.

[0017] [7] The laminate film according to [1] or [2], wherein the haze value of the surface of the coating layer opposite the substrate layer side is 5% or less.

[0018] [8] The laminate film according to [1] or [2], having a transmission clarity of 460 or more.

[0019] [9] An optical display comprising the laminate film according to [1] or [2]. Effect of the Invention

[0020] According to the present invention, there is provided a laminate film having excellent optical properties and mechanical properties, high transmission clarity, and excellent appearance quality. The laminate film of the present invention having such properties can be suitably used for optical displays, particularly touch panels. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a graph showing the relationship between the planar shape of protrusions P, which appear on a coating layer and have a protrusion width of 10 μm or more, and θ(°). [Diagram 2] FIG. 2 is a schematic diagram of protrusions on the surface of the laminated film of the present invention. [Diagram 3] FIG. 3 is a schematic diagram of protrusions on the surface of a conventional laminated film. [Figure 4]FIG. 4 is a cross-sectional view of one example (part) of an optical display including the laminate film of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present invention will be described in detail below, divided into the sections of 1) a laminate film and 2) an optical display.

[0023] 1) Laminated film The laminated film of the present invention is a laminated film having a substrate layer and a coating layer.

[0024] 1.Base material layer As the base layer of the laminated film of the present invention, a film appropriately selected from known resin films that have been conventionally used as optical films can be used.

[0025] Examples of the resin material constituting the resin film include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, viscose, diacetyl cellulose, triacetyl cellulose, acetyl cellulose butyrate, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polystyrene, polycarbonate, polymethylpentene, polysulfone, polyether ether ketone, polyether sulfone, polyether imide, polyimide, fluororesin, polyamide, acrylic resin, norbornene resin, cycloolefin resin, etc. Among these, polyethylene terephthalate (PET), polycarbonate, triacetyl cellulose, and cycloolefin resin are preferred, and polyethylene terephthalate and triacetyl cellulose are more preferred, from the viewpoint of excellent transparency and adhesion, excellent heat resistance, and mechanical strength, and from the viewpoint of easily satisfying the optical properties described below. In addition, from the viewpoint of SDGs, a material with a high biomass content may be used as the material constituting the resin film, or a material that can be recycled or reused, or a material that has been recycled or reused may be used.

[0026] When the substrate layer is a laminated film, it is preferable that the substrate layer satisfies the optical properties described below, and may be a single-layer or two or more-layer resin film. In addition, when a coating layer or the like is formed on the substrate layer, the surface of the substrate layer may be subjected to a physical treatment such as a corona discharge treatment or an oxidation treatment in order to improve adhesion.

[0027] The thickness of the substrate layer is not particularly limited, but in consideration of touch panel applications, it is preferably 25 to 500 μm, more preferably 40 to 400 μm, particularly preferably 60 to 300 μm, and even more preferably 80 to 200 μm, which tends to increase the scratch resistance and hardness of the laminated film.

[0028] 2. Coating layer The coating layer of the laminated film of the present invention (sometimes referred to as the "coating layer of the present invention" in this specification) is preferably a layer formed from a coating layer-forming composition containing component (A): an active energy ray-curable resin, component (B): a filler, and component (C): a leveling agent (sometimes referred to as the "coating layer-forming composition of the present invention" in this specification).

[0029] (1)Component (A) The coating layer forming composition according to the present invention preferably contains an active energy ray curable resin as component (A) (in this specification, the "active energy ray curable resin" may be referred to as "component (A)"). The component (A) is a compound that has the property of being crosslinked and cured by irradiation with active energy rays such as ultraviolet rays and electron beams.

[0030] The component (A) may be selected from conventionally known materials, and may be an active energy ray curable monomer, prepolymer, resin, or a mixture of two or more of these. Among these, from the viewpoint of kneadability with the component (B) and ease of adjusting optical properties to a desired range, polyfunctional (meth)acrylic monomers, (meth)acrylate prepolymers, organic-inorganic hybrid resins, etc. are preferred.

[0031] Here, the (meth)acrylic monomer means an acrylic monomer or a methacrylic monomer, the (meth)acrylate prepolymer means an acrylate prepolymer or a methacrylate prepolymer, and the (meth)acrylic acid means an acrylic acid or a methacrylic acid, and the same applies to other similar terms.

[0032] Examples of polyfunctional (meth)acrylic monomers include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphoric acid di(meth)acrylate, allylated cyclohexyl di(meth)acrylate, isocyanurate di(meth)acrylate, trimethylsilyl ether di(meth)acrylate, and the like. Examples of the polyfunctional (meth)acrylate include polymethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, propionic acid modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, propionic acid modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and caprolactone modified dipentaerythritol hexa(meth)acrylate. These monomers can be used alone or in combination of two or more.

[0033] Examples of the (meth)acrylate-based prepolymer include polyester acrylate-based prepolymer, epoxy acrylate-based prepolymer, urethane acrylate-based prepolymer, and polyol acrylate-based prepolymer.

[0034] Here, the polyester acrylate prepolymer can be obtained by esterifying the hydroxyl group of a polyester oligomer having hydroxyl groups at both ends obtained by condensation of a polyvalent carboxylic acid and a polyhydric alcohol with (meth)acrylic acid, or by esterifying the terminal hydroxyl group of an oligomer obtained by adding an alkylene oxide to a polyvalent carboxylic acid with (meth)acrylic acid. The epoxy acrylate prepolymer can be obtained by reacting (meth)acrylic acid with an oxirane ring of a relatively low molecular weight bisphenol type epoxy resin or novolac type epoxy resin to esterify it. The urethane acrylate prepolymer can be obtained by esterifying a polyurethane oligomer obtained by reacting a polyether polyol or a polyester polyol with a polyisocyanate with (meth)acrylic acid. The polyol acrylate prepolymer can be obtained by esterifying the hydroxyl group of a polyether polyol with (meth)acrylic acid. These prepolymers can be used alone or in combination of two or more. They may also be used in combination with the above-mentioned polyfunctional (meth)acrylic monomer.

[0035] Organic-inorganic hybrid resins are resins in which both inorganic and organic components exist in the same molecule, and are functional materials that combine the excellent properties of both inorganic components, such as hardness, heat resistance, and weather resistance, and organic components, such as flexibility, light weight, and processability. Examples of organic-inorganic hybrid resins include compounds obtained by bonding organic compounds having polymerizable unsaturated groups such as (meth)acryloyl groups, silanol groups, vinyl groups, and allyl groups to inorganic fine particles such as silica via a silane coupling agent, and silsesquioxane compounds obtained by hydrolyzing and polycondensing trifunctional silane compounds. Among these, in order to make the coating layer stronger after curing, compounds obtained by bonding organic compounds having polymerizable unsaturated groups to inorganic fine particles are preferred, compounds obtained by bonding organic compounds having polymerizable unsaturated groups to silica inorganic fine particles are more preferred, and compounds obtained by bonding organic compounds having (meth)acryloyl groups to silica inorganic fine particles are even more preferred.

[0036] The inorganic fine particles contained in the organic-inorganic hybrid resin do not correspond to a filler described later, but function as a binder and improve the hardness of the coating layer to be formed. The average particle size of the inorganic fine particles is preferably 5 to 100 nm, more preferably 10 to 90 nm, particularly preferably 15 to 80 nm, and further preferably 20 to 70 nm. This makes it easier to maintain the strength of the coating layer after curing. The average particle size of the inorganic fine particles is measured by a dynamic light scattering method.

[0037] The organic-inorganic hybrid resin is also preferably used in combination with other active energy ray curable components such as the above-mentioned polyfunctional (meth)acrylate monomers. When the organic-inorganic hybrid resin is used in combination with other active energy ray curable components, the content of the organic-inorganic hybrid resin relative to 100 parts by mass of the active energy ray curable components is preferably 10 to 200 parts by mass, more preferably 50 to 150 parts by mass, and particularly preferably 75 to 125 parts by mass. The organic-inorganic hybrid resin is also preferably in the form of an organosol (colloidal).

[0038] (2)(B) Component The composition for forming a coat layer according to the present invention preferably contains a filler as component (B) (in this specification, "filler" may be referred to as "component (B)"). By using a filler, an uneven shape is formed on the surface of the coating layer, and optical properties such as haze value can be easily adjusted to a desired value. The filler is not particularly limited, and examples thereof include inorganic fillers made of silica, calcium carbonate, aluminum hydroxide, magnesium hydroxide, clay, talc, titanium dioxide, etc.; organic fillers made of acrylic resins, acrylic-styrene copolymers, melamine resins, polycarbonate resins, polyethylene resins, polystyrene resins, benzoguanamine resins, epoxy resins, etc.; and organic-inorganic fillers made of silicon-containing compounds having an intermediate structure between inorganic and organic. These fillers may be used alone or in combination of two or more.

[0039] Among these, the filler used in the present invention is preferably an organic filler, and more preferably an acrylic filler made of an acrylic resin, from the viewpoint that it is likely to be unevenly distributed on the surface of the coating layer and therefore likely to exhibit good optical properties.

[0040] The shape of the filler may be a fixed shape such as a sphere, or may be an indefinite shape with no particular shape. From the viewpoint of more easily achieving the effects of the present invention, a fixed shape is preferable, a spherical shape is more preferable, and a perfect sphere is even more preferable.

[0041] The average particle size of the filler is preferably 0.1 to 10 μm, more preferably 0.5 to 8 μm, particularly preferably 1 to 6 μm, and further preferably 2 to 4 μm. The average particle size of the filler can be measured using a laser diffraction scattering type particle size distribution measuring device.

[0042] The refractive index of the filler is preferably 1.2 to 1.7, more preferably 1.3 to 1.6, and particularly preferably 1.35 to 1.5, which makes it easier to have desired optical properties.

[0043] The content of the (B) component is preferably 0.005 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, and even more preferably 0.02 to 3 parts by mass, relative to 100 parts by mass of the (A) component, which makes it easier to achieve the effects of the present invention.

[0044] (3)(C) component The composition for forming a coating layer according to the present invention preferably contains a leveling agent as component (C) (in this specification, the "leveling agent" may be referred to as "component (C)"). This makes it easier to adjust the θ(°) and kurtosis of the coating layer to be formed within the desired range, making it possible to obtain an optical display with excellent appearance quality.

[0045] Examples of the leveling agent include silicone-based leveling agents, fluorine-based leveling agents, acrylic-based leveling agents, vinyl-based leveling agents, etc. Among these, silicone-based leveling agents and fluorine-based leveling agents are preferred from the viewpoints of high leveling properties, excellent compatibility with other components used, and ease of adjusting the θ(°) and kurtosis of the coating layer to be formed within the desired range.

[0046] The silicone-based leveling agent preferably includes polydimethylsiloxane or modified polydimethylsiloxane. The fluorine-based leveling agent preferably includes a compound having a perfluoroalkyl group or a fluorinated alkenyl group in the main chain or side chain. The leveling agent can be used alone or in combination of two or more kinds.

[0047] The content of the (C) component is preferably 0.3 to 10 parts by mass, more preferably 0.4 to 8 parts by mass, even more preferably 0.5 to 6 parts by mass, even more preferably 0.6 to 4 parts by mass, and particularly preferably 0.7 to 3 parts by mass, relative to 100 parts by mass of the (A) component. This allows the leveling effect described below to be sufficiently obtained, and makes it easy to adjust the θ(°) and kurtosis of the formed coating layer to the desired range. The obtained coating layer exhibits the desired optical properties and has excellent appearance quality.

[0048] (3) Other ingredients The composition for forming a coating layer according to the present invention may contain other components in addition to the components (A), (B), and (C). Preferred examples of the other components include a photopolymerization initiator.

[0049] By using a photopolymerization initiator, the amount of light irradiation can be reduced and the polymerization and curing time can be shortened when forming a coating layer. In particular, when crosslinking is performed by irradiation with active light such as ultraviolet light as active energy rays, it is preferable to have a photopolymerization initiator present.

[0050] The photopolymerization initiator is not particularly limited, and conventionally known ones can be used. For example, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, benzophenone, p-phenylbenzophenone, 2-methylanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, benzyl dimethyl ketal, p-dimethylaminobenzoic acid ester, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, etc. can be mentioned. The photopolymerization initiator can be used alone or in combination of two or more kinds.

[0051] When a photopolymerization initiator is used, the blending ratio thereof is preferably 0.1 to 20 parts by mass, more preferably 0.2 to 10 parts by mass, and even more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of component (A), which makes it easier for the coating layer to exhibit the desired scratch resistance and hardness.

[0052] The coating layer forming composition according to the present invention may further contain other additives such as antioxidants, ultraviolet absorbers, silane coupling agents, light stabilizers, defoamers, infrared absorbers, antistatic agents, colorants, dispersants, etc., as long as they do not affect the effects of the present invention.

[0053] (4) Coating layer formation The coating layer according to the present invention is preferably formed by applying the coating layer-forming composition according to the present invention to the surface of the substrate layer or another layer laminated on the substrate layer, and irradiating the resulting coating film with active energy rays to cure the coating film.

[0054] The composition for forming a coating layer according to the present invention is preferably prepared by adding the above-mentioned essential components (A) to (C) and, if desired, other components to an appropriate solvent and dissolving or dispersing these components.

[0055] Examples of the solvent to be used include aliphatic hydrocarbons such as hexane and heptane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; alcohols such as methanol, ethanol, 2-propanol, n-butanol, isobutyl alcohol (IBA), and n-octanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, 2-pentanone, diisobutyl ketone, cyclohexanone, isophorone, and cyclohexanone; ethyl acetate, butyl acetate, ethyl lactate, and γ-butyrolactone. esters; cellosolves such as methyl cellosolve, ethyl cellosolve, ethylene glycol mono n-butyl ether, ethylene glycol mono t-butyl ether, and propylene glycol monomethyl ether (PGM); glycol ethers such as 3-methoxy-3-methylbutanol, 3-methoxy-3-methylbutyl acetate, diethylene glycol monobutyl ether, and 1-ethoxy-2-propanol; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; etc. These solvents can be used alone or in combination of two or more.

[0056] The amount of the solvent used can be appropriately determined so that the composition for forming a coating layer according to the present invention has a state (concentration, viscosity) suitable for forming a coating film. When a solvent is used, the amount of the solvent used is preferably 10 to 500 parts by mass, more preferably 30 to 300 parts by mass, and even more preferably 50 to 200 parts by mass, relative to 100 parts by mass of the component (A).

[0057] The method for applying the composition for forming a coating layer according to the present invention to the surface of the substrate layer or other layers laminated on the substrate layer is not particularly limited, and any conventionally known method such as bar coating, knife coating, roll coating, blade coating, die coating, gravure coating, etc. is usable. The coating film is preferably dried at 40 to 120° C. for about 30 seconds to 5 minutes.

[0058] The coating film is then cured by irradiating it with active energy rays, and a coating layer can be formed. Examples of active energy rays used to cure the coating film include ultraviolet rays; electron beams; laser light such as semiconductor lasers, argon lasers, and He-Cd lasers; ionizing radiation such as α-rays, β-rays, γ-rays, neutron beams, X-rays, and accelerated electron beams; and the like. Among these, the active energy rays are preferably ultraviolet rays and electron beams, and more preferably ultraviolet rays, because they can be generated using a relatively simple device.

[0059] When ultraviolet rays are used as the active energy rays, the ultraviolet light source may be an ultra-high pressure mercury lamp, a high pressure mercury lamp, a low pressure mercury lamp, a carbon arc, a black light lamp, a metal halide lamp, or the like.

[0060] The amount of UV light is 50-1,000mJ / cm 2 is preferably 100 to 700 mJ / cm 2 It is more preferable that the illuminance of the ultraviolet light is usually 100 to 1000 mW / cm. 2 is preferably 200 to 700 mW / cm 2 The irradiation time is usually from 1 second to 1 hour, and the irradiation temperature is usually from 20 to 100°C.

[0061] The electron beam irradiation can be carried out by an electron beam accelerator, etc. The dose of the electron beam is preferably 10 to 1000 krad.

[0062] The irradiation with active energy rays can be carried out in an air atmosphere or an inert gas atmosphere, such as nitrogen, argon, or helium.

[0063] The thickness of the obtained coating layer is preferably 0.1 to 30 μm, more preferably 0.2 to 20 μm, particularly preferably 0.5 to 10 μm, further preferably 1 to 7 μm, and more preferably 2 to 5 μm. This makes it easier to form a coating layer having a desired range of θ(°) and kurtosis, and the obtained coating layer is more likely to exhibit the effects of the present invention. If the coating layer thickness is less than 0.1 μm, it may be difficult to obtain the hardness required for practical use.

[0064] The coating layer according to the present invention preferably satisfies the following requirements (β1) and / or (β2). <Requirements for (β1)> In the coating layer according to the present invention, protrusions resulting from the filler (B) appear on the surface of the coating layer opposite to the substrate layer side. When the surface shape of the protrusions having a width of 10 μm or more, preferably (the average particle size (μm) of the filler + 10) μm or more is measured by an optical interference type surface shape observation device, it is preferable that the average value of θ(°) shown in the following formula (1) is 0.4(°) or more.

[0065]

number

[0066] In the formula, dZ (μm) represents the height of the protrusion from a reference plane at a point (point B) dX (μm) in the horizontal direction from the periphery (point A) of the protrusion toward the center of the protrusion when the surface on which the protrusion does not exist is taken as the reference plane, and dX is 5 (μm) and represents the horizontal distance from point A to point B. FIG. 1 shows a schematic diagram showing the relationship between the cross-sectional shape of a protrusion P having a protrusion width of 10 μm or more that appears on the coating layer and θ (°). The protrusion width refers to the distance (μm) from the periphery (point A) of the protrusion to the periphery (point C) of the protrusion that is the furthest in the horizontal direction. In addition, in the present invention, the "average value of θ (°)" refers to the average value of the θ values ​​shown in the above formula (1) measured by an optical interference surface profile observation device for any three protrusions having a protrusion width of 10 μm or more.

[0067] The coating layer according to the present invention preferably has an average value of θ(°) of 0.4(°) or more, more preferably 0.5(°) or more, even more preferably 0.8(°) or more, particularly preferably 1.2(°) or more, of which 1.6(°) or more is preferable, and most preferably 2(°) or more. The upper limit of the average value of θ(°) is usually less than 90(°). From the viewpoint of compatibility with the optical properties and hardness required for the obtained laminated film, it is preferable that the average value of θ(°) is 20(°) or less, more preferably 15(°) or less, even more preferably 10(°) or less, particularly preferably 6(°) or less, and especially preferably 3(°) or less.

[0068] The laminate film of the present invention having a coating layer that satisfies the requirement (β1) is less likely to exhibit graininess (roughness) on the surface when placed in a bright place such as under a fluorescent lamp, and tends to have excellent appearance quality.

[0069] <Requirements for (β2)> In the coating layer according to the present invention, the kurtosis (Rku) of the surface of the coating layer opposite to the substrate layer is preferably 35 or more, more preferably 38 or more, even more preferably 45 or more, particularly preferably 55 or more, of which 65 or more is preferable, and most preferably 70 or more. The upper limit of the kurtosis (Rku) is not particularly limited, but from the viewpoint of compatibility with the optical properties and hardness required for the resulting laminated film, it is preferably 300 or less, more preferably 250 or less, even more preferably 200 or less, particularly preferably 150 or less, of which 100 or less and most preferably 90 or less are preferable.

[0070] Kurtosis (Rku) is a parameter indicating the sharpness (kurtosis) of the roughness profile, and the larger the value, the steeper the convex shape. In the present invention, the value of kurtosis (Rku) refers to the average value of values ​​measured at three different locations using an optical interference type surface profile observation device in accordance with JIS B0601. When the coating layer according to the present invention has the above-mentioned kurtosis (Rku) value, when the coating layer is placed in a bright place such as under a fluorescent lamp, the surface is less likely to have a grainy texture (roughness), and the coating layer is likely to have excellent appearance quality.

[0071] As described above, in the coating layer according to the present invention, the projections that appear on the surface and originate from component (B) have a narrow base, a steep protrusion gradient, and a large kurtosis. This is believed to be because the leveling agent of component (C) acts to surround the filler of component (B) in the resin of component (A).

[0072] This state is shown in FIG. 2. FIG. 3 shows a schematic diagram of a conventional laminated film. In FIGS. 2 and 3, 1a and 1b indicate coating layers, 2a and 2b indicate base layers, 3a and 3b indicate fillers, and 4 indicates a leveling agent. As shown in FIG. 2, in the coating layer 1a according to the present invention, the leveling agent 4 acts to surround the filler 3a in the resin, suppressing the spread of the base of the protrusions, and it is considered that protrusions with a higher degree of sharpness appear compared to the coating layer 1b in FIG. 3. It is considered that the laminated film of the present invention has such a surface, and thus has high transmission clarity and excellent appearance quality.

[0073] (5) Other layers The laminated film of the present invention may have other layers such as a hard coat layer, an optical adjustment layer, a primer layer, and an adhesive layer depending on the purpose. Among these, the other layer is preferably a hard coat layer, and is preferably provided on the surface of the substrate layer opposite to the surface having the coat layer in the laminated film of the present invention. The hard coat layer is preferably provided on the outermost surface of the touch panel, that is, the surface that is directly touched by fingers or a touch pen. This improves the durability of the touch panel of the laminated film of the present invention.

[0074] In the laminated film of the present invention, the primer layer may be provided between the substrate layer and the coating layer. This serves to enhance the adhesion between the substrate layer and the coating layer. The primer layer is formed, for example, by applying a reactive coating liquid consisting of polyester polyol or polyether polyol and polyisocyanate to the surface of the substrate layer in an amount of 0.5 to 2 g / m. 2 It can be formed by coating.

[0075] In the laminated film of the present invention, the adhesive layer may be provided on the surface of the base material layer opposite to the surface having the coating layer. This allows the adhesive layer to be well attached to a transparent conductive film such as an ITO film. The adhesive constituting the adhesive layer is not particularly limited, and known adhesives having a predetermined transparency, such as acrylic adhesives, rubber adhesives, silicone adhesives, and urethane adhesives, may be used. In addition, when the laminated film of the present invention includes an adhesive layer, a release film may be laminated on the surface of the adhesive layer. The release film has a role of protecting the surface of the adhesive layer and is peeled off and removed when used. The release film is not particularly limited as long as it has the desired releasability on its release surface (the surface in contact with the adhesive layer), and known release films may be used.

[0076] (6) Surface protection sheet The laminated film of the present invention may have a surface protective sheet on the coating layer for the purpose of protecting the surface of the coating layer until use. The surface protective sheet is peeled off and removed when used. As the surface protective sheet, a conventionally known resin film is preferably used.

[0077] (7) Layer composition Examples of the layer structure of the laminated film of the present invention include, but are not limited to, the following. In the following, the following symbols are used. BL: Base material layer Coat: Coat layer PL: Primer layer HC: Hard coat layer RF: Release film AL: Adhesive layer SP: Surface protection sheet

[0078] BL / COAT, BL / COAT / SP, HC / BL / COAT, HC / BL / COAT / SP, BL / PL / COAT, BL / PL / COAT / SP, HC / BL / PL / COAT, HC / BL / PL / COAT / SP, RF / AL / BL / COAT, RF / AL / BL / COAT / SP, RF / AL / BL / PL / COAT, RF / AL / BL / PL / COAT / SP

[0079] 3. Characteristics of laminated film (1) Total light transmittance The total light transmittance of the laminated film of the present invention is preferably 85% or more, more preferably 90% or more, and even more preferably 91% or more. The upper limit of the total light transmittance is usually 100%. This allows the image displayed on the display to have excellent visibility. The total light transmittance can be measured using a haze meter in accordance with JIS K 7361-1.

[0080] (2) Haze value The haze value of the coating layer surface of the laminated film of the present invention is preferably 5% or less. Furthermore, it is more preferably 0.1 to 5%, further preferably 0.3 to 5%, and particularly preferably 0.5 to 3%. This provides excellent visibility of the displayed image on the resulting display. The haze value can be measured using a haze meter in accordance with JIS K 7136:2000.

[0081] (3) Transparency The transmission clarity of the laminated film of the present invention is preferably 460 or more, more preferably 465 or more. The upper limit of the transmission clarity is not particularly limited, but is usually 500. The transmission clarity is an index of visibility, and when this value satisfies the above range, good display image quality (visibility) is easily obtained. The transmission clarity can be determined in accordance with JIS K 7374 by using an image clarity tester in a transmission mode, irradiating light from the coating layer side, and calculating the total image clarity value of 5 combs (comb width: 0.125 mm, 0.25 mm, 0.5 mm, 1.0 mm, 2.0 mm).

[0082] (4) Water contact angle In the laminated film of the present invention, the water contact angle of the coating layer surface is preferably 50 to 120°, more preferably 60 to 110°, particularly preferably 70 to 100°, further preferably 78 to 92°, and more preferably 80 to 88°. This allows the obtained laminated film to be suitably processed with ITO and easily satisfies the desired optical properties. In addition, the appearance of the obtained display is easily maintained. The water contact angle can be measured by the method described in the Examples.

[0083] (5)Pencil hardness In the laminated film of the present invention, the pencil hardness of the coating layer surface is preferably B or more, more preferably HB or more, particularly preferably F or more, and even more preferably H or more. The upper limit of the pencil hardness is not particularly limited, but from the viewpoint of improving the touch feeling of the touch panel, it is usually preferably 9H or less, more preferably 7H or less, particularly preferably 5H or less, particularly preferably 3H or less, and even more preferably 2H or less. This makes it easier to obtain a display with excellent scratch resistance and high appearance quality. The pencil hardness can be measured according to JIS K 5600 by the method described in the examples.

[0084] (6) Scratch resistance In the laminated film of the present invention, the coating layer surface has hard coat properties in terms of excellent scratch resistance. This makes it easier to maintain the appearance quality of the display when used in a display, and also makes it easier to provide a good touch feeling for the touch panel. Excellent scratch resistance can be confirmed by the absence of any change in appearance in a scratch resistance test using steel wool. Specifically, the coating layer surface was subjected to a scratch resistance test using #0000 steel wool at 250 g / cm in accordance with JIS K5600-5-10. 2 The scratch resistance can be confirmed by the number of scratches that appear on the surface after rubbing 10 times back and forth at a load of 10 cm. In the scratch resistance test, the number of scratches confirmed on the surface of the coating layer is preferably 10 or less, more preferably 3 or less, and particularly preferably 0.

[0085] (7)Surface tension In the laminated film of the present invention, the surface tension of the coating layer surface is preferably 15 to 50 mN / m, more preferably 18 to 42 mN / m, particularly preferably 20 to 30 mN / m, further preferably 22 to 25 mN / m, and of these, preferably 23 to 24 mN / m. This makes it easier to satisfy the water contact angle described above, and ITO processing can be performed well on the coating layer surface of the obtained laminated film. In addition, it also makes it easier to satisfy optical properties well, and in particular, it is easier to maintain the appearance of the obtained display well. The surface tension can be measured in accordance with the wetting tension test method of "JIS K6768:1999".

[0086] (8) Appearance quality The laminated film of the present invention has excellent appearance quality. That is, even when placed in a bright place such as under a fluorescent lamp, the surface is unlikely to have a grainy feel (roughness). Therefore, when used in a display, even when the display is placed in a bright place such as under a fluorescent lamp, the surface is unlikely to have a grainy feel (roughness), resulting in excellent appearance quality. The excellent appearance quality can be confirmed by the method described in the examples.

[0087] 4. Use of laminated film As described above, the laminated film of the present invention has excellent optical properties, mechanical properties, high transmission clarity, and excellent appearance quality, and is therefore suitable for use in various optical displays such as liquid crystal displays and organic electroluminescence (EL) displays, particularly for improving the appearance quality of touch panels (displays).

[0088] For example, the laminated film of the present invention is preferably used by laminating it to a transparent conductive film [ITO (indium tin oxide) film] of a resistive touch panel component. A schematic cross-sectional view showing an example of a touch panel using the laminated film of the present invention [a part of a touch panel] is shown in FIG. 4. In FIG. 4, 10 indicates the laminated film of the present invention, 10a indicates a base layer, 10b indicates a coating layer, 11a and 11b indicate ITO films, 12 indicates a dot spacer, 13 indicates a transparent substrate, and 14 indicates a liquid crystal display (LCD). The arrow indicates the direction of pressing the touch panel surface with a finger, pen, or the like. A hard coat layer is preferably laminated on the surface (the surface pressed by a finger, pen, or the like) of the laminated film 10 of the present invention. By laminating the laminated film of the present invention in this way, the obtained touch panel is less likely to have a grainy feel (roughness) on the outermost surface even when placed in a bright place such as under a fluorescent lamp, and has excellent appearance quality.

[0089] 2) Optical Display The optical display of the present invention comprises the laminate film of the present invention.

[0090] For example, as shown in FIG. 4, an optical display including the laminated film of the present invention can be obtained by bonding (laminating) an ITO film 11a of a touch panel and a coating layer 10b of the laminated film of the present invention directly or via another layer such as an adhesive layer.

[0091] The surface of the obtained optical display of the present invention, equipped with the laminate film of the present invention, is less likely to exhibit graininess (roughness) even when placed in a bright place such as under a fluorescent lamp, and has excellent appearance quality.

[0092] The above-described embodiments are described for the purpose of facilitating understanding of the present invention, and are not described for the purpose of limiting the present invention. Therefore, each element disclosed in the above embodiment is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.

[0093] In this specification, when it is written "α to β" (α and β are any numerical values), it means "α or more and β or less", and also means "preferably greater than α" or "preferably smaller than β", unless otherwise specified. Furthermore, when it is written "α or more" (α is any numerical value), it means "preferably greater than α", unless otherwise specified, and when it is written "β or less" (β is any numerical value), it also means "preferably smaller than β", unless otherwise specified. EXAMPLES

[0094] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0095] Example 1 As the active energy ray-curable compound of component (A), 50 parts by mass (solid content equivalent; the same applies below) of a nanosilica-containing urethane acrylate [trade name: Opstar Z7530, manufactured by Arakawa Chemical Industries, Ltd. (represented as "A1" in the table below)] and 50 parts by mass of a polyfunctional acrylate not containing nanosilica [trade name: Beamset 575CB, manufactured by Arakawa Chemical Industries, Ltd. (represented as "A2" in the table below)] were used. As the filler of component (B), crosslinked polymethyl methacrylate [trade name A coating layer-forming composition was prepared by uniformly mixing 0.025 parts by mass of Techpolymer SSK-103, average particle size 3.0 μm, refractive index: 1.49, particle shape: spherical, manufactured by Sekisui Chemical Co., Ltd. (represented as "B1" in the table below)), 0.5 parts by mass of a silicone leveling agent as component (C) (trade name: SH28, manufactured by Dow-Toray Industries, Inc. (represented as "C1" in the table below)), and 3 parts by mass of a photopolymerization initiator (trade name: PI-150, manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd.) using a solvent.

[0096] The composition for forming a coating layer was applied with a Mayer bar onto a PET film (product name: Lumirror PET125U403, thickness: 125 μm, manufactured by Toray Industries, Inc.) as a substrate layer to form a coating film. The composition was then placed in an oven maintained at 70° C. for 1 minute to dry. Next, in a nitrogen atmosphere, an ultraviolet ray irradiation device (Eigrantage ECS-401GX type, manufactured by I-Graphics Co., Ltd.) was used to irradiate the film with a high-pressure mercury lamp as a light source at an illuminance of 200 mW / cm. 2 , Light intensity: 250mJ / cm 2 The coating was cured by irradiating it with ultraviolet rays under the irradiation conditions above, to prepare a laminated film (laminated film 1) having a coating layer with a thickness of 1.5 μm.

[0097] The θ(°) and kurtosis (Rku) shown in the formula (1) were measured for the surface of the coating layer of the laminated film 1. The average value of θ(°) was 0.59(°), and the kurtosis (Rku) was 38.1. Here, the average value of θ(°) refers to the average value of the values ​​measured for any three protrusions on the coating layer, each having a protrusion width of 10 μm or more, using an optical interference type surface profiler (manufactured by Hitachi High-Tech Science Corporation). In addition, the kurtosis (Rku) refers to the average value of the values ​​measured for three locations on the coating layer using an optical interference type surface profiler (manufactured by Hitachi High-Tech Science Corporation) in accordance with JIS B0601.

[0098] (Examples 2 to 6, Comparative Examples 1 to 6) In Example 1, laminate films 2 to 6 and 1r to 6r were produced in the same manner as in Example 1, except that the types of components (A), (B), and (C) and the photopolymerization initiator shown in Table 1 below were used in the amounts shown in Table 1 below. For the resulting laminate films 2 to 6 and 1r to 6r, the average value of θ (°) shown in the above formula (1) and kurtosis (Rku) of the coating layer surface were measured (calculated) in the same manner as in Example 1. The results are shown in Table 1 below.

[0099] In Table 1 below, C2 to C5 indicate the following. C2: Futergent 602A (fluorine-based leveling agent, manufactured by Neos Co., Ltd.) C3: Megafac RS-90 (fluorine-based surfactant, manufactured by DIC) C4: X-62-5408 (epoxy modified silicone resin, manufactured by Shin-Etsu Chemical Co., Ltd.) C5: BYK-3550 (silicone-based leveling agent, manufactured by BYK)

[0100] [Table 1]

[0101] The obtained laminated films 1 to 6 and 1r to 6r were subjected to the following tests.

[0102] [Appearance quality] The laminated films 1 to 6 and 1r to 6r were placed on a black plate so that the surface of the coating layer was in contact with the black plate. The laminated films placed on the black plate were then placed under a fluorescent lamp, and the appearance was visually observed and evaluated as follows. The results are shown in Table 2 below. ⊚: Almost no graininess is felt, and the appearance is good. ◯: A slight sense of grain is observed, but the appearance is at an acceptable level for use in an optical display. ×: Grainy texture is felt, and the appearance is unacceptable for use in an optical display.

[0103] [Total light transmittance] For the laminated films 1 to 6 and 1r to 6r, the total light transmittance (%) was measured using a haze meter ("NDH-5000", manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K 7361-1, by irradiating light from the coating layer side after blank correction. The results are shown in Table 2.

[0104] [Haze value] For the laminated films 1 to 6 and 1r to 6r, the haze value (%) was measured using a haze meter ("NDH-5000", manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K 7136:2000, after blank correction, by irradiating light from the coating layer side. The results are shown in Table 2.

[0105] [Transmission clarity] For the laminated films 1 to 6 and 1r to 6r, light was irradiated from the coating layer side in transmission mode using an image clarity tester ("ICM-1T", manufactured by Suga Test Instruments Co., Ltd.) in accordance with JIS K 7374, and the total image clarity value of five combs (comb widths: 0.125 mm, 0.25 mm, 0.5 mm, 1.0 mm, 2.0 mm) was calculated, and the calculated value was taken as the transmission clarity. The results are shown in Table 2.

[0106] [Water contact angle] The water contact angle of the coating layer surface was measured for the laminated films 1 to 6 and 1r to 6r. That is, a glass plate was attached to the substrate layer side surface of the laminated film, and then the laminated film with the glass plate was placed on the test stand of a contact angle meter ("DH350 test stand", manufactured by KYOWA) with the glass plate side facing down. Next, 2 μL of water was dropped onto the coating layer surface of the laminated film with the glass plate, and the contact angle (°) immediately after the drop was measured with the contact angle meter, which was taken as the water contact angle (°). The results are shown in Table 2.

[0107] [Pencil hardness] The pencil hardness of the coating layer surface of the laminated films 1 to 6 and 1r to 6r was measured in accordance with JIS K 5600. That is, pencils with different hardnesses of the pencil cores ("Mitsubishi Pencil UNI", manufactured by Mitsubishi Pencil Co., Ltd.) were moved 7 mm at an angle of 45° while applying a load of 750 g, and the degree of damage to the surface was visually observed. This was carried out five times for each, and the hardness of the hardest pencil core that did not damage the surface four or more times was taken as the pencil hardness. The results are shown in Table 2.

[0108] [Scratch resistance] The scratch resistance of the coating layer surface was evaluated for the laminate films 1 to 6 and 1r to 6r. That is, the coating layer surface was scratched with #0000 steel wool at 250 g / cm in accordance with JIS K5600-5-10. 2 The coating layer was rubbed back and forth 10 times with a sliding distance of 10 cm under a load of 1000 g. The presence or absence of scratches on the surface of the coating layer was then visually confirmed under a three-wavelength fluorescent lamp and evaluated according to the following criteria. The results are shown in Table 2. ◎: 0 scratches found ○: 1 to 3 scratches confirmed △: 4 to 10 scratches confirmed ×: 11 or more scratches found

[0109] <Surface tension> For the laminate films 1 to 6 and 1r to 6r, the surface tension (mN / m) of the coating layer was measured in accordance with the wet tension test method of JIS K6768:1999.

[0110] [Table 2]

[0111] From Table 2, it can be seen that the laminated film of the present invention (Laminated Film 1-6) has excellent appearance quality, a transmitted light clarity of 460 or more, a high total light transmittance, and excellent hardness and scratch resistance.

[0112] On the other hand, the comparative laminate films 1r to 6r having small θ and kurtosis (Rku) had hardness and excellent scratch resistance, but were inferior in transmitted light clarity and in appearance quality. [Industrial Applicability]

[0113] As described above in detail, the laminated film of the present invention has high transmission clarity, excellent optical properties and mechanical properties, and also has excellent appearance quality. Therefore, it is expected to be suitably applied to optical displays such as touch panels that require high appearance quality. [Explanation of symbols]

[0114] 1a, 1b: Coating layer 2a, 2b...Base material layer 3a, 3b: Filler 4. Leveling agent 10. Laminated film 10a...Base material layer 10b Coating layer 11a, 11b...ITO film 12 Dot spacer 13 Transparent substrate 14 LCD

Claims

1. A laminated film having a base layer and a coating layer, the coating layer is a layer formed from a coating layer-forming composition containing an active energy ray-curable resin (A), a filler (B), and a leveling agent (C); A laminated film characterized in that, when the surface shape of protrusions having a protrusion width of 10 μm or more appearing on the surface of the coating layer opposite the substrate layer side is measured using an optical interference type surface shape observation device, the average value of θ (°) represented by the following formula (1) is 0.4 (°) or more. [0010] [In the formula, dZ (μm) represents the height of the protrusion from a reference plane at a point (point B) that is dX (μm) in the horizontal direction from the periphery (point A) of the protrusion toward the center of the protrusion, when a surface on which the protrusion does not exist is used as a reference plane, and dX is 5 (μm) and represents the horizontal distance from point A to point B.]

2. A laminated film having a base layer and a coating layer, the coating layer is a layer formed from a coating layer-forming composition containing an active energy ray-curable resin (A), a filler (B), and a leveling agent (C); A laminated film, characterized in that the kurtosis (Rku) of the surface of the coating layer opposite to the substrate layer side is 35 or more.

3. The laminated film according to claim 1 or 2, wherein the component (B) is an acrylic filler.

4. 3. The laminate film according to claim 1, wherein the content of the component (C) is from 0.3 parts by mass to 10 parts by mass with respect to 100 parts by mass of the component (A).

5. The laminated film according to claim 1 , wherein the kurtosis (Rku) of the surface of the coating layer opposite to the substrate layer side is 35 or more.

6. 3. The laminate film according to claim 1, wherein the kurtosis (Rku) of the surface of the coating layer opposite to the substrate layer side is 300 or less.

7. 3. The laminate film according to claim 1, wherein the haze value of the surface of the coating layer opposite to the substrate layer side is 5% or less.

8. 3. The laminated film according to claim 1, having a transmission clarity of 460 or more.

9. An optical display comprising the laminate film according to claim 1 or 2.

Citation Information

Patent Citations

  • Newton ring prevention sheet

    JP2012203323A

  • Newton ring prevention sheet

    JP2013152396A

  • Newton ring prevention sheet

    JP2013171126A

  • Optical film and its production method, and glare-proof polarizer using same and display apparatus