Coating composition with high solid content
A high solid content coating composition using polyaspartic acid ester, polyisocyanate, and epoxy group-containing silane coupling agent addresses weather and corrosion resistance issues, enhancing adhesion and reducing VOCs for metal applications.
Patent Information
- Application Number
- JP2023099738
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2023-06-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-06-19
AI Technical Summary
Existing high solid content coating compositions used for metal materials face challenges in achieving sufficient weather resistance, corrosion resistance, and coating hardness while complying with stringent VOC regulations and ensuring good workability.
A high solid content coating composition comprising polyaspartic acid ester, polyisocyanate compound, epoxy group-containing silane coupling agent, and polyol with specific molecular weight and hydroxyl value ranges, along with optional additives like pigments and zeolite, to enhance adhesion and crosslinking density.
The composition achieves excellent weather resistance, corrosion resistance, and coating hardness with improved metal adhesion, while reducing VOC emissions and maintaining good workability, suitable for direct application on metal materials.
Smart Images

Figure 2024146677000001 
Figure 2024146677000002 
Figure 2024146677000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a high solids coating composition which has excellent weather resistance and corrosion resistance and can be applied directly to metal substrates. [Background technology]
[0002] Conventionally, acrylic lacquer, acrylic urethane paint, amino acrylic resin paint, etc. have been used when painting industrial machinery, buildings, automobiles, structures, furniture (including steel), etc. In particular, when painting construction machinery or industrial machinery such as bulldozers, hydraulic excavators, wheel loaders, etc., acrylic urethane paint containing a hydroxyl group-containing acrylic resin and a polyisocyanate compound is mainly used because of its room temperature drying property, durability, etc.
[0003] Furthermore, in recent years, there has been a demand to reduce volatile organic compounds (VOCs) in paints due to their impact on the environment, including from an ESG perspective, and VOC regulations, including legislation, are being strengthened worldwide.
[0004] In one-coat coatings applied directly to metal materials for construction machinery and other applications, paint compositions containing acrylic resins and isocyanate compounds have been used to ensure weather resistance and corrosion resistance, but the paint solids concentration is generally low, and there have been limitations to VOC reduction.
[0005] Generally, coating compositions of polyamine compounds and isocyanate compounds have excellent coating film performance such as high corrosion resistance and chemical resistance, but their high reactivity results in a fast curing rate and a short pot life, which makes them difficult to handle, such as in terms of painting workability, and therefore they have not been put to practical use in painting construction machinery, etc.
[0006] Patent Document 1 discloses a high-solids coating composition characterized by using a polyisocyanate composition which is made from a base polyol containing a low molecular weight acrylic polyol or polyester polyol, and an aliphatic diisocyanate or an alicyclic diisocyanate as raw materials, and which has a content of components with a molecular weight of 700 or less of 20 to 60 mass%, a ratio of weight average molecular weight to number average molecular weight of 1.2 to 5.0, and a ratio of the viscosity of the polyisocyanate composition at 25°C (units: mPa.s) to the number average functionality of the isocyanate groups represented by a specific formula.
[0007] However, the high-solids coating composition described in Patent Document 1 is insufficient to satisfy the recently strengthened VOC regulation levels, and there are cases in which the coating workability is insufficient.
[0008] Patent Document 2 discloses a polyaspartic acid ester-based coating composition in which the dialkyl fumarate content is significantly reduced as a paint composition for producing a gloss-stable colored top coat.
[0009] However, the coating composition described in Patent Document 2 has insufficient corrosion resistance and weather resistance, and may lack the adhesion to metal materials required, particularly when directly applying the coating to metal materials. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2003-128989 A [Patent Document 2] Special Publication No. 2022-521250 Summary of the Invention [Problem to be solved by the invention]
[0011] The problem to be solved by the present invention is to provide a high solids coating composition which is excellent in weather resistance, corrosion resistance and coating hardness and which can be directly applied to metal substrates. [Means for solving the problem]
[0012] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by a high solids coating composition containing a polyaspartic acid ester (A), a polyisocyanate compound (B), an epoxy group-containing silane coupling agent (C), and a polyol (D) having a weight average molecular weight and hydroxyl value within a specific range, and have thus completed the present invention.
[0013] That is, the present invention provides: 1. A high solids coating composition comprising a polyaspartic acid ester (A), a polyisocyanate compound (B), an epoxy group-containing silane coupling agent (C), and a polyol (D) having a weight average molecular weight of 250 to 2,300 and a hydroxyl value in the range of 50 to 800.
[0014] 2. A high solids coating composition according to item 1, wherein the polyaspartic acid ester (A) contains a polyaspartic acid ester having a secondary amino group represented by the following formula (1):
[0015] [ka]
[0016] (In the formula, X is an n-valent cyclic or chain aliphatic hydrocarbon group or a polyoxyalkylene polyamine residue having a number average molecular weight of 25 to 5,000, and R 1 and R 2 are each independently an organic group inactive to an isocyanate group, and n is an integer of 2 or greater. 3. The high solids coating composition according to item 1 or 2, wherein the polyol (D) contains a polyester polyol and / or a polyether polyol.
[0017] 4. A high solid content coating composition according to any one of items 1 to 3 above, having a solid content concentration of 70 mass % or more.
[0018] 5. The high solids coating composition according to any one of items 1 to 4, further comprising a pigment.
[0019] 6. The high solids coating composition according to any one of items 1 to 5, wherein the polyisocyanate compound (B) contains a silyl group-containing modified polyisocyanate.
[0020] 7. The high solids coating composition according to item 6, wherein the silyl group-containing modified polyisocyanate is a reaction product made from raw materials including an alkoxysilane (a1) having a primary amino group, an alkyl carboxylate (a2) and a polyisocyanate (a3).
[0021] 8. The high solids coating composition according to any one of items 1 to 7, further comprising zeolite.
[0022] 9. A one-coat high solids coating composition according to any one of items 1 to 8.
[0023] 10. A coating method comprising coating a substrate with the high solids coating composition according to any one of items 1 to 8 above.
[0024] 11. A construction machine or industrial machine coated with the high solid content coating composition according to any one of items 1 to 8. Effect of the Invention
[0025] The coating composition of the present invention comprises as its components a polyaspartic acid ester, a polyisocyanate compound, an epoxy group-containing silane coupling agent, and a polyol having a low molecular weight and a high hydroxyl value, and therefore has low viscosity, a high VOC reduction effect, and excellent curing properties, and the resulting urea crosslinked coating film has excellent weather resistance and corrosion resistance.
[0026] It is also believed that the improved barrier properties due to the epoxy group-containing silane coupling agent result in improved metal adhesion, and the improved crosslink density due to the low molecular weight polyol further results in significant improvements in the levels of weather resistance, corrosion resistance and coating hardness.
[0027] Therefore, the coating composition of the present invention has the effect of providing a high solids coating composition which is extremely excellent in weather resistance, corrosion resistance and coating hardness, and has high metal adhesion, making it possible to apply the coating directly to metal materials, and which further has an excellent finished appearance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] The high solid content coating composition of the present invention (hereinafter sometimes simply referred to as the present coating composition) is a composition containing a polyaspartic acid ester (A), a polyisocyanate compound (B), an epoxy group-containing silane coupling agent (C), and a polyol (D). It will be described in detail below.
[0029] <Polyaspartic acid ester (A)> As the polyaspartic acid ester, from the viewpoints of reactivity and coating workability, a polyaspartic acid ester having a secondary amino group is preferred.
[0030] Specifically, the following formula (1)
[0031] [ka]
[0032] (In the formula, X is an n-valent cyclic or chain aliphatic hydrocarbon group or a polyoxyalkylene polyamine residue having a number average molecular weight of 25 to 5,000, and R 1 and R 2 are each independently an organic group inactive to an isocyanate group, and n is an integer of 2 or more.
[0033] In formula (1), X is an n-valent cyclic or chain aliphatic hydrocarbon group having a number average molecular weight of 25 to 5,000, or a polyoxyalkylene polyamine residue.
[0034] X is an n-valent group having a number average molecular weight of 25 to 5,000, and the number average molecular weight is preferably 50 to 3,000, and more preferably 100 to 2,000.
[0035] X is an aliphatic hydrocarbon group or a polyoxyalkylene polyamine residue.
[0036] The aliphatic hydrocarbon group may be an alicyclic hydrocarbon group, a chain hydrocarbon group, or a group having both an alicyclic portion and a chain portion.
[0037] The alicyclic hydrocarbon group may have a side chain. The chain hydrocarbon group may be a straight-chain hydrocarbon group or a branched hydrocarbon group.
[0038] X is preferably a divalent aliphatic hydrocarbon group. Examples of the divalent aliphatic hydrocarbon group include alkylene, cycloalkylene, cycloalkylalkylene, alkylcycloalkylene, alkylenebiscycloalkylene, alkylenebis(alkylcycloalkylene), and cycloalkylenebisalkylene.
[0039] Here, alkylene is preferably alkylene having 1 to 8 carbon atoms, cycloalkylene is preferably cycloalkylene having 5 to 6 carbon atoms, alkyl is preferably alkyl having 1 to 8 carbon atoms, and cycloalkyl is preferably cycloalkyl having 5 to 6 carbon atoms.
[0040] The polyoxyalkylene polyamine residue refers to a group obtained by removing primary amino groups at both ends from a polyoxyalkylene polyamine. The polyoxyalkylene polyamine residue may have a side chain. The polyoxyalkylene polyamine residue is preferably a polyoxyethylene polyamine residue, a polyoxypropylene polyamine residue, a polyoxybutylene polyamine residue, or a polyoxyethylene polyoxypropylene polyamine residue. The polyoxyalkylene polyamine residue is more preferably -(CH(CH 3 )-CH 2-O)x-CH 2 -CH(CH 3 )-(where x is an integer from 3 to 6).
[0041] In formula (1), R 1 and R 2 R is each independently an organic group that is inactive to an isocyanate group. 1 and R 2 is preferably alkyl having 1 to 15 carbon atoms, more preferably alkyl having 1 to 8 carbon atoms, further preferably methyl or ethyl, and most preferably ethyl.
[0042] In formula (1), n is an integer of 2 or more. n is preferably an integer of 2 to 6, more preferably an integer of 2 to 4, and most preferably 2.
[0043] Compounds of formula (1) can be synthesized, for example, by reacting an optionally substituted maleate or fumarate ester with a polyamine.
[0044] Specific examples of the compound represented by formula (1) include, but are not limited to, tetraethyl N,N'-[methylenebis(cyclohexane-4,1-diyl)]bisaspartate, tetraethyl N,N'-(hexane-1,6-diyl)bisaspartate, tetrabutyl N,N'-(2-methylpentane-1,5-diyl)bisaspartate, tetraethyl N,N'-[methylenebis(3-methylcyclohexane-4,1-diyl)]bisaspartate, tetraethyl N,N '-(bis-2-propyl)polypropylene glycol 300-O,O'-diylbisaspartate tetraethyl, N,N'-(butane-1,4-diyl)bisaspartate tetraethyl, N,N'-(2,2-dimethylpropane-1,3-diyl)bisaspartate tetraethyl, N,N'-(2,4-dimethylhexane-1,6-diyl)bisaspartate tetraethyl, and at least one selected from the group consisting of these. Among them, N,N'-[methylenebis(cyclohexane-4,1-diyl)]bisaspartate tetraethyl, N,N'-(2-methylpentane-1,5-diyl)bisaspartate tetrabutyl, and N,N'-[methylenebis(3-methylcyclohexane-4,1-diyl)]bisaspartate tetraethyl are preferred.
[0045] Commercially available polyaspartic acid esters (A) include "Desmophen NH1420", "Desmophen NH1423LF", "Desmophen NH 1520", and "Desmophen NH 1220" (all trade names, manufactured by Sumika Bayer), "FEISOARTIC F420", "FEISOARTIC F220", and "FEISOARTIC F520" (all trade names, manufactured by Feiyang Chemical Industry Co., Ltd.), and the like.
[0046] <Polyisocyanate compound (B)> As the polyisocyanate compound, those which have been conventionally used in the production of polyurethanes can be used.
[0047] Specific examples of the polyisocyanate compound include aliphatic polyisocyanate compounds, alicyclic polyisocyanate compounds, aromatic aliphatic polyisocyanate compounds, aromatic polyisocyanate compounds, crude products thereof, and modified products of these polyisocyanate compounds.
[0048] Examples of the modified products include biuret modified products, isocyanurate modified products, and mixtures of two or more of these.
[0049] Among the above, from the viewpoint of high solid content, aliphatic polyisocyanate compounds can be preferably used.
[0050] An aliphatic polyisocyanate compound is a compound that has a straight-chain or branched chain carbon skeleton and has two or more free isocyanate groups per molecule.
[0051] Specific examples of aliphatic polyisocyanate compounds include ethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, 1,6,11-undecane triisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2,6-diisocyanatomethyl caproate, bis(2-isocyanatoethyl) fumarate, bis(2-isocyanatoethyl) carbonate, and 2-isocyanatoethyl-2,6-diisocyanatohexanoate.
[0052] Specific examples of modified aliphatic polyisocyanate compounds include biuret-modified HDI and isocyanurate-modified HDI.
[0053] As the aliphatic polyisocyanate compound, from the viewpoints of curability and finished appearance, hexamethylene diisocyanate (HDI) and modified products of HDI can be suitably used.
[0054] Commercially available aliphatic polyisocyanate compounds (B) include, for example, TUL-100 (manufactured by Asahi Kasei Chemicals Corporation), Desmodur N3900 (manufactured by Sumika Covestro Urethanes), Desmodur N3600 (manufactured by Sumika Covestro Urethanes), Desmodur N3200 (manufactured by Sumika Covestro Urethanes), TOLONATE XF-800 (manufactured by Vencolex), and TOLONATE XF-450 (manufactured by Vencolex).
[0055] Specific examples of the alicyclic polyisocyanate compound include isophorone diisocyanate (IPDI), dicyclohexylmethane-4,4'-diisocyanate (hydrogenated MDI), cyclohexylene diisocyanate, methylcyclohexylene diisocyanate (hydrogenated TDI), bis(2-isocyanatoethyl)-4-cyclohexene-1,2-dicarboxylate, 2,5- and / or 2,6-norbornane diisocyanate, and the like.
[0056] Specific examples of the aromatic aliphatic polyisocyanate compound include m- and / or p-xylylene diisocyanate (XDI), α,α,α',α'-tetramethylxylylene diisocyanate (TMXDI), and the like.
[0057] Specific examples of the aromatic polyisocyanate compound include 1,3- and / or 1,4-phenylene diisocyanate, 2,4- and / or 2,6-tolylene diisocyanate (TDI), crude TDI, 2,4'- and / or 4,4'-biphenylmethane diisocyanate (MDI), 4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatodiphenylmethane, crude MDI, 1,5-naphthylene diisocyanate, 4,4',4''-triphenylmethane triisocyanate, m- and p-isocyanatophenylsulfonyl isocyanate, and the like.
[0058] Specific examples of modified polyisocyanate compounds other than the above-mentioned aliphatic polyisocyanate compounds include modified polyisocyanate compounds such as modified MDI (urethane-modified MDI, carbodiimide-modified MDI, trihydrocarbyl phosphate-modified MDI), urethane-modified TDI, and isocyanurate-modified IPDI; and mixtures of two or more of these [for example, a mixture of modified MDI and urethane-modified TDI].
[0059] Furthermore, as a modified polyisocyanate compound, a silyl group-containing modified polyisocyanate can be used for the purpose of improving corrosion resistance.
[0060] The silyl group-containing modified polyisocyanate can further improve the corrosion resistance without decreasing the gloss of the resulting coating film.
[0061] The silyl group-containing modified polyisocyanate is not particularly limited, and any modified polyisocyanate containing a silyl group can be used without limitation. In particular, a silyl group-containing modified polyisocyanate (X) which is a reaction product using as raw materials components including an alkoxysilane (a1) having a primary amino group, an alkyl carboxylate (a2), and a polyisocyanate (a3) can be preferably used.
[0062] The silyl group-containing modified polyisocyanate (X) is a modified polyisocyanate that is synthesized using a carboxylic acid alkyl ester (a2) as a modifier, can be stably diluted in an organic solvent, and has excellent storage stability.
[0063] Specific examples of the compound (a1) include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyl-methyldiethoxysilane, 3-aminopropyl-methyldimethoxysilane, 3-aminopropyl-ethyleneglycoloxymethoxysilane, 4-amino-3,3-dimethylbutyltrimethoxysilane, 4-amino-3,3-dimethylbutyltriethoxysilane, and combinations thereof. 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane are particularly preferred.
[0064] The carboxylic acid alkyl ester (a2) is preferably a saturated carboxylic acid alkyl ester.
[0065] Specific examples of saturated carboxylic acid alkyl esters include methyl acetate, ethyl acetate, n-propyl acetate, i-propyl acetate, n-butyl acetate, i-butyl acetate, n-pentyl acetate, i-pentyl acetate, cyclohexyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate, 1-methylpentyl acetate (also known as sec-hexyl acetate), 2-methoxyethyl acetate, 2-ethoxyethyl acetate, 3-methoxybutyl acetate, 3-ethoxybutyl acetate, methyl propionate, ethyl propionate, and propionate. n-Propyl pionate, i-Propyl propionate, n-Butyl propionate, i-Butyl propionate, n-Pentyl propionate, i-Pentyl propionate, Methyl butyrate, Ethyl butyrate, n-Propyl butyrate, i-Propyl butyrate, n-Butyl butyrate, i-Butyl butyrate, t-Butyl butyrate, Methyl valerate, Ethyl valerate, Methyl octanoate, Methyl laurate, Methoxypropyl acetate, Ethyl 3-ethoxypropionate, Butyl glycol acetate, Butyl diglycol acetate , methyl isovalerate, ethyl isovalerate, methyl 3,3,5-trimethylhexanoate, methyl isobutyrate, ethyl isobutyrate, i-butyl isobutyrate, n-butyl i-butyrate, t-butyl i-butyrate, methyl 2-ethylhexanoate, methyl pivalate, ethyl 2-hydroxy-2-methylpropionate, methyl neodecanoate, di-i-propyl fumarate, isobornyl acrylate, and combinations thereof.
[0066] Examples of the polyisocyanate (a3) include the polyisocyanate compounds described above as the polyisocyanate compound (B).
[0067] The method for producing the silyl group-containing modified polyisocyanate (X) may be a method of simultaneously reacting an alkoxysilane (a1) having a primary amino group, an alkyl carboxylate (a2), and a polyisocyanate (a3). However, a preferred method is a method of previously reacting an alkoxysilane (a1) with an alkyl carboxylate (a2) to obtain an N-position-modified alkoxysilane having a secondary amino group or a secondary amide group, and then reacting this with a polyisocyanate (a3).
[0068] The amount of isocyanate groups in the silyl group-containing modified polyisocyanate is preferably within the range of, for example, 1.0 mmol or more, 2.0 mmol or more, 5.5 mmol or less, and 5.0 mmol or less per gram of nonvolatile content of the modified polyisocyanate from the viewpoints of corrosion resistance, drying property, and the like.
[0069] The amount of isocyanate groups in a modified polyisocyanate can be determined, for example, by adding 10 ml of a 0.1 mol / L dibutylamine solution to 0.1 g of a sample to react with the NCO groups, and then titrating the remaining dibutylamine with an aqueous hydrochloric acid solution using bromophenol blue as a titration indicator.
[0070] The polyisocyanate compounds (B) may be used alone or in combination of two or more kinds.
[0071] From the viewpoints of curability and dryness to touch, the ratio of the amino group of the polyaspartic acid ester (A) to the isocyanate group of the polyisocyanate compound (B) is preferably within the range of 0.5 to 2.0 equivalents, particularly 0.8 to 1.5 equivalents, and more particularly 1.0 to 1.3 equivalents of the isocyanate group per equivalent of the amino group.
[0072] From the viewpoints of corrosion resistance and weather resistance, it is preferable that the polyaspartic acid ester (A) is within the range of 20 to 70 mass%, particularly 30 to 50 mass%, and the polyisocyanate compound (B) is within the range of 30 to 80 mass%, particularly 50 to 70 mass%, based on the total solid content of the polyaspartic acid ester (A) and the polyisocyanate compound (B).
[0073] When the polyisocyanate compound (B) contains a silyl group-containing modified polyisocyanate, from the viewpoints of corrosion resistance and dryness to touch, the solid content of the silyl group-containing modified polyisocyanate is preferably within the range of 1 to 100 mass%, particularly 5 to 70 mass%, and more particularly 5 to 50 mass%, based on the total solid content of the polyisocyanate compound (B).
[0074] <Epoxy group-containing silane coupling agent (C)> In the present invention, the epoxy group-containing silane coupling agent (C) is a component that contributes to improving the adhesion to metal materials, and thereby to improving the corrosion resistance, in particular, of the coating composition of the present invention.
[0075] The epoxy group-containing silane coupling agent (C) is a compound having both an alkoxysilyl group and an epoxy group in the molecule, and specific examples thereof include glycidoxymethyltrimethoxysilane, glycidoxymethyltriethoxysilane, β-glycidoxyethyltrimethoxysilane, β-glycidoxyethyltriethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyl(methyl)dimethoxysilane, γ-glycidoxypropyl(dimethyl)methoxysilane, γ-glycidoxypropyl(ethyl)dimethoxysilane, (3,4-epoxycyclohexyl)methyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and the like.
[0076] As the epoxy group-containing silane coupling agent (C), from the viewpoints of corrosion resistance and finished appearance, γ-glycidoxypropyltrimethoxysilane and γ-glycidoxypropylmethyldiethoxysilane can be suitably used.
[0077] From the viewpoint of the appearance of the coating film, the epoxy equivalent of the epoxy group-containing silane coupling agent (C) is preferably within the range of 100 to 1000 g / eq, particularly 100 to 500 g / eq.
[0078] The epoxy group-containing silane coupling agent (C) can be used alone or in combination of two or more kinds.
[0079] In the coating composition of the present invention, from the viewpoints of water resistance and coating film appearance, the amount of the epoxy group-containing silane coupling agent (C) is preferably 0.1 to 50 mass %, particularly preferably 0.5 to 30 mass %, and further particularly preferably 0.5 to 15 mass %, based on the total solid content of the polyaspartic acid ester (A) and the polyisocyanate compound (B).
[0080] <Polyol (D)> Specific examples of the polyol (D) include polyester polyol, polyether polyol, acrylic polyol, polyolefin polyol, fluorine polyol, polycarbonate polyol, polyurethane polyol, etc. The polyol (D) may contain one type alone or two or more types in combination.
[0081] Among these, as the polyol (D), from the viewpoints of dryness to touch and weather resistance, polyether polyols and polyether polyols are preferred.
[0082] 1. Polyester polyol The polyester polyol can be obtained, for example, by subjecting a dibasic acid and a polyhydric alcohol to a condensation reaction.
[0083] Examples of the dibasic acid include carboxylic acids such as succinic acid, adipic acid, dimer acid, maleic anhydride, phthalic anhydride, isophthalic acid, terephthalic acid, and 1,4-cyclohexanedicarboxylic acid.
[0084] Examples of the polyhydric alcohol include ethylene glycol, propylene glycol, diethylene glycol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, trimethylpentanediol, cyclohexanediol, trimethylolpropane, glycerin, pentaerythritol, 2-methylolpropanediol, and ethoxylated trimethylolpropane.
[0085] In addition, polycaprolactones obtained by ring-opening polymerization of lactones such as ε-caprolactone with polyhydric alcohols can also be used as polyester polyols.
[0086] Furthermore, alcohol components other than the above polyhydric alcohols can also be used.
[0087] Specific examples of the alcohol include monoalcohols such as methanol, ethanol, propyl alcohol, butyl alcohol, stearyl alcohol, and 2-phenoxyethanol; alcohol compounds obtained by reacting a monoepoxy compound such as propylene oxide, butylene oxide, or neodecanoic acid glycidyl ester (a commercially available product is "Cardura E10P" (trade name, manufactured by HEXION, a glycidyl ester of synthetic highly branched saturated fatty acid)) with an acid; and esters of glycol and monobasic acid.
[0088] 2. Polyether polyol The polyether polyols are not particularly limited, but include, for example, the following (1) to (3).
[0089] (1) Polyether polyols obtained by random or block addition of an alkylene oxide or a mixture of alkylene oxides to a polyhydric hydroxy compound or a mixture of polyhydric hydroxy compounds using a catalyst.
[0090] Examples of the catalyst include hydroxides (lithium, sodium, potassium, etc.), strong basic catalysts (alcoholates, alkylamines, etc.), composite metal cyanide complexes (metal porphyrins, zinc hexacyanocobaltate complexes, etc.), and the like.
[0091] Examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, cyclohexene oxide, and styrene oxide.
[0092] (2) Polyether polyols obtained by reacting a polyamine compound with an alkylene oxide.
[0093] Examples of the polyamine compound include ethylenediamines.
[0094] Examples of the alkylene oxide include the same ones as those exemplified in (1).
[0095] (3) Polymer polyols obtained by polymerizing acrylamide or the like using the polyether polyols obtained in (1) or (2) as a medium.
[0096] Examples of the polyhydric hydroxy compound include the following compounds (i) to (vi).
[0097] (i) Diglycerin, ditrimethylolpropane, pentaerythritol, dipentaerythritol, etc.
[0098] (ii) Sugar alcohol compounds such as erythritol, D-threitol, L-arabinitol, ribitol, xylitol, sorbitol, mannitol, galactitol, and rhamnitol.
[0099] (iii) Monosaccharides such as arabinose, ribose, xylose, glucose, mannose, galactose, fructose, sorbose, rhamnose, fucose, and ribosaccharides.
[0100] (iv) Disaccharides such as trehalose, sucrose, maltose, cellobiose, gentiobiose, lactose, and melibiose.
[0101] (v) Trisaccharides such as raffinose, gentianose, and melezitose.
[0102] (vi) Tetrasaccharides such as stachyose.
[0103] 3. Acrylic polyol The acrylic polyol is not particularly limited, but examples thereof include those obtained by copolymerizing a single or mixture of an ethylenically unsaturated bond-containing monomer having a hydroxy group with a single or mixture of other ethylenically unsaturated bond-containing monomers copolymerizable therewith.
[0104] The ethylenically unsaturated bond-containing monomer having a hydroxy group is not particularly limited, but examples thereof include hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate. These may be used alone or in combination of two or more. Among them, hydroxyethyl acrylate or hydroxyethyl methacrylate is preferred.
[0105] Examples of other ethylenically unsaturated bond-containing monomers copolymerizable with the above monomers include the following (1) to (6), which may be used alone or in combination of two or more.
[0106] (1) Acrylic acid esters such as methyl acrylate, ethyl acrylate, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-hexyl acrylate, cyclohexyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, benzyl acrylate, and phenyl acrylate.
[0107] (2) Methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, benzyl methacrylate, and phenyl methacrylate.
[0108] (3) Unsaturated carboxylic acids, such as acrylic acid, methacrylic acid, maleic acid, and itaconic acid.
[0109] (4) Unsaturated amides such as acrylamide, methacrylamide, N,N-methylenebisacrylamide, diacetone acrylamide, diacetone methacrylamide, maleic acid amide, and maleimide.
[0110] (5) Vinyl monomers such as glycidyl methacrylate, styrene, vinyl toluene, vinyl acetate, acrylonitrile, and dibutyl fumarate.
[0111] (6) Vinyl monomers having a hydrolyzable silyl group, such as vinyltrimethoxysilane, vinylmethyldimethoxysilane, and γ-(meth)acryloxypropyltrimethoxysilane.
[0112] 4. Polyolefin polyol The polyolefin polyol is not particularly limited, but examples thereof include polybutadiene having two or more hydroxyl groups, hydrogenated polybutadiene, polyisoprene, and hydrogenated polyisoprene.
[0113] 5. Fluoropolyol In this specification, the fluorine polyol refers to a polyol containing fluorine in the molecule.Specific examples of the fluorine polyol include copolymers of fluoroolefin, cyclovinyl ether, hydroxyalkyl vinyl ether, monocarboxylic acid vinyl ester, etc., as disclosed in JP-A-57-34107 (Reference 1) and JP-A-61-275311 (Reference 2), etc.
[0114] From an ESG perspective, it is preferable not to use fluorine polyols.
[0115] 6. Polycarbonate polyol The polycarbonate polyol is not particularly limited, but examples thereof include the following (1) to (4).
[0116] (1) Dialkyl carbonates such as dimethyl carbonate; (2) Alkylene carbonates such as ethylene carbonate; (3) diaryl carbonates such as diphenyl carbonate; (4) A product obtained by condensation polymerization of low molecular weight carbonate compounds such as those described in (1) to (3) above.
[0117] 7. Polyurethane polyol The polyurethane polyol is not particularly limited, but can be obtained, for example, by reacting a polyol with an isocyanate component in a conventional manner.
[0118] Examples of the polyol include low molecular weight polyols such as ethylene glycol and propylene glycol, and high molecular weight polyols such as acrylic polyols, polyester polyols, and polyether polyols.
[0119] The hydroxyl value of the polyol (D) is preferably within a range of 50 to 800, particularly 100 to 700, and further particularly 150 to 600, from the viewpoints of drying properties, crosslink density, and weather resistance.
[0120] In the present invention, the hydroxyl value can be measured in accordance with JIS K1557.
[0121] The weight average molecular weight of the polyol (D) is preferably within a range of 250 to 2,300, particularly preferably 250 to 1,500, and further particularly preferably 250 to 1,000, from the viewpoints of drying properties, crosslink density, and weather resistance.
[0122] In the present invention, the "weight average molecular weight" is a value calculated based on the molecular weight of standard polystyrene from a chromatogram measured by gel permeation chromatography in accordance with the method described in JIS K 0124-2011.
[0123] The gel permeation chromatograph used was "HLC8120GPC" (manufactured by Tosoh Corporation). Four columns, "TSKgel G-4000HXL", "TSKgel G-3000HXL", "TSKgel G-2500HXL", and "TSKgel G-2000HXL" (all of which are product names manufactured by Tosoh Corporation), were used, and the measurements were performed under the following conditions: mobile phase: tetrahydrofuran, measurement temperature: 40°C, flow rate: 1 ml / min, and detector: RI.
[0124] In the coating composition of the present invention, from the viewpoints of drying property and crosslink density, the amount of polyol (D) is preferably 1 to 20 mass %, particularly preferably 1 to 10 mass %, and further particularly preferably 3 to 10 mass %, based on the total solid content of the polyaspartic acid ester (A) and the polyisocyanate compound (B).
[0125] In the coating composition of the present invention, the molar ratio of hydroxyl groups in the polyol (D) to isocyanate groups in the polyisocyanate composition (B) (hydroxyl groups / isocyanate groups) is preferably within the range of 0.5 to 2.0 equivalents, particularly 0.8 to 1.5 equivalents, and more particularly 1.0 to 1.3.
[0126] It is believed that the polyol (D) improves the crosslink density, and in particular the weather resistance of the coating film.
[0127] The coating composition of the present invention may contain a curing catalyst, if necessary, for the purpose of promoting the reaction between the polyisocyanate compound (B) and the polyol (D). Examples of the curing catalyst include known urethane curing catalysts such as organometallic compounds, tertiary amines, and phosphoric acid compounds.
[0128] Examples of organometallic compounds include tin octoate, dibutyltin di(2-ethylhexanoate), dioctyltin di(2-ethylhexanoate), dioctyltin diacetate, dibutyltin dilaurate, dibutyltin oxide, dioctyltin oxide, dibutyltin fatty acid salts, lead 2-ethylhexanoate, zinc octoate, zinc naphthenate, zinc fatty acids, cobalt naphthenate, calcium octoate, copper naphthenate, and tetra(2-ethylhexyl)titanate.
[0129] The above curing catalysts can be used alone or in combination of two or more.
[0130] In the coating composition of the present invention, a coloring pigment can be used to obtain a desired color. Specific examples of the coloring pigment include titanium white, zinc molybdate, calcium molybdate, carbon black, graphite, iron black, Prussian blue, ultramarine, cobalt blue, copper phthalocyanine blue, indanthrone blue, yellow lead, synthetic yellow iron oxide, red iron oxide, transparent red iron oxide, bismuth vanadate, titanium yellow, zinc yellow, monoazo yellow, ochre, disazo, isoindolinone yellow, metal complex azo yellow, and quinophthalone. Examples of the pigments include yellow, benzimidazolone yellow, monoazo red, unsubstituted quinacridone red, azo lake (Mn salt), quinacridone magenta, anthranthrone orange, dianthraquinonyl red, perylene maroon, perylene red, diketopyrrolopyrrole chrome vermilion, chlorinated phthalocyanine green, brominated phthalocyanine green, pyrazolone orange, benzimidazolone orange, dioxazine violet, and perylene violet.
[0131] When a color pigment is used in the coating composition of the present invention, the amount used is preferably 5 to 100 mass %, particularly preferably 10 to 60 mass %, based on the total solid content of the polyaspartic acid ester (A) and the polyisocyanate compound (B), from the viewpoints of coating film appearance, weather resistance, and base hiding ability.
[0132] The coating composition of the present invention may contain an extender pigment, if necessary.
[0133] Examples of the extender pigment include clay, silica, barium sulfate, talc, calcium carbonate, white carbon, diatomaceous earth, and magnesium carbonate.
[0134] Of the above-mentioned body pigments, barium sulfate or calcium carbonate having an average particle size of 0.01 to 5 μm, preferably 0.05 to 4 μm, and more preferably 0.05 to 3 μm, can be suitably used from the viewpoints of reducing the paint viscosity, coating workability, and finished appearance.
[0135] Commercially available products of such extender pigments include, for example, barium sulfate, Varifine BF-20 (manufactured by Sakai Chemical Industry Co., Ltd., product name, barium sulfate having an average particle size of 0.03 μm), Variace B-33 (manufactured by Sakai Chemical Industry Co., Ltd., product name, barium sulfate having an average particle size of 0.3 μm), SPARWITE W-5HB (manufactured by Sino-Can Co., Ltd., product name, barium sulfate powder, average particle size: 1.6 μm), and BLANC FIXE MICRO (manufactured by Venator Materials Co., Ltd., product name, barium sulfate having an average particle size of 0.7 μm); Examples of calcium carbonate include Neolite SA-200 (trade name, manufactured by Takehara Chemical Industry Co., Ltd., calcium carbonate having an average particle size of 0.08 μm), Micro POWDER 3N (trade name, manufactured by Bihoku Funka Kogyo Co., Ltd., calcium carbonate having an average particle size of 1.1 μm), and Sunlite SL1500 (trade name, manufactured by Takehara Chemical Industry Co., Ltd., calcium carbonate having an average particle size of 2.5 μm).
[0136] In this specification, the average particle size is a value obtained by measuring particle size distribution by dynamic light scattering.
[0137] Specifically, the value is measured using, for example, UPA-EX250 (product name, manufactured by Nikkiso Co., Ltd., a particle size distribution measuring device using a dynamic light scattering method).
[0138] When a body pigment is used in the coating composition of the present invention, the amount of the body pigment used is preferably 10 to 200 mass %, particularly preferably 15 to 150 mass %, based on the total solid content of the polyaspartic acid ester (A) and the polyisocyanate compound (B), from the viewpoints of finished appearance and coating workability.
[0139] In addition, in the coating composition of the present invention, the amount of pigments (coloring pigments, extender pigments and other pigments) used is preferably within the range of 5 to 250 mass %, particularly 20 to 200 mass %, and more particularly 25 to 150 mass %, based on the total solid content of the polyaspartic acid ester (A) and the polyisocyanate compound (B), from the viewpoints of finished appearance and coating workability.
[0140] In the coating composition of the present invention, zeolite can further be used for the purpose of improving the pot life.
[0141] Zeolite is a general term for crystalline aluminosilicates, whose constituent elements are Al, Si, O, and cations (positive ions), and is SiO 4 and AlO 4 The tetrahedral structure (Si 4+ Or Al 3+ Zeolite is a compound with a basic structure of a tetrahedron (a tetrahedron formed around a center). These are connected in a complex and regular manner, forming one-, two-, or three-dimensional regular pores with diameters of several Å to several tens of Å, roughly the same size as small molecules. This is the characteristic of zeolites.
[0142] Zeolite has cations in its pores, and these cations are the basis of the zeolite's various functions. Only molecules smaller than the diameter of the zeolite pores can enter them, and because they can be screened out from larger molecules, some zeolites are called molecular sieves.
[0143] There are two types of zeolite: natural zeolite, which is mainly composed of hydrous aluminosilicate, and Na 2 O.Al 2 O 3 xSiO 2 ·yH 2 There is a synthetic zeolite whose main component is O. Synthetic zeolites are also called palmitites and are produced by the dry method of co-evaporating sodium carbonate, silica, alumina or kaolin, or by the wet method of combining sodium silicate and sodium aluminate to precipitate a gel.
[0144] Both natural and synthetic zeolites have ion exchange capacity, their crystal structure does not change even when dehydrated, and they have large adsorption capacity because they have molecular-sized pores after dehydration. Zeolites made by hydrothermal synthesis, which are crystallized from sodium aluminosilicate gel and dehydrated to obtain pores of a certain size, are generally called molecular sieves.
[0145] Zeolite generally referred to as molecular sieve can be preferably used from the viewpoint of pot life and corrosion resistance. Zeolite molded into powder or pellet form is commercially available, and molecular sieve 3A, molecular sieve 4A, molecular sieve 5A, molecular sieve 13X, etc. are commercially available depending on the type of raw material zeolite. The numbers indicate the approximate diameter (angstroms) of the pores, and the capital letters indicate the type of zeolite, with A representing LTA zeolite and X representing FAU zeolite.
[0146] Of the above molecular sieves, from the viewpoint of the finished appearance, molecular sieve 3A, molecular sieve 4A, and molecular sieve 5A are preferred, with molecular sieve 5A being particularly preferred.
[0147] The location and size of the metal cations near the pores of the molecular sieve crystals changes the effective diameter of the pores; for example, molecular sieve 5A is molecular sieve 4A in which the sodium ions are replaced by calcium ions.
[0148] From the viewpoint of finished appearance, the pore size (effective diameter of the pores) of the zeolite is preferably in the range of 0.50 nm or less, particularly preferably in the range of 0.10 to 0.50 nm, and further particularly preferably in the range of 0.20 to 0.50 nm.
[0149] The pore size of the zeolite can be measured by a nitrogen gas adsorption method.
[0150] When zeolite is used in the coating composition of the present invention, the amount used is preferably within the range of 0.1 to 30 mass %, particularly 3 to 30 mass %, and more particularly 5 to 20 mass %, based on the total solid content of the polyaspartic acid ester (A) and the polyisocyanate compound (B), from the viewpoints of pot life and finished appearance.
[0151] A rheology control agent can be used in the coating composition of the present invention for the purpose of controlling the fluidity of the coating and improving the finished appearance and coating workability.
[0152] Specific examples of rheology control agents include clay minerals (e.g., metal silicates, montmorillonite), acrylic resins (e.g., those containing a structure consisting of an acrylic acid ester or methacrylic acid ester polymer or oligomer in the molecule), polyolefins (e.g., polyethylene, polypropylene, etc.), amides (higher fatty acid amides, polyamides, oligomers, etc.), polycarboxylic acids (including derivatives having at least two carboxyl groups in the molecule), cellulose (including various derivatives such as nitrocellulose, acetyl cellulose, cellulose ether, etc.), urethanes (polymers, oligomers, etc. containing a urethane structure in the molecule), ureas (polymers, oligomers, etc. containing a urea structure in the molecule), urethane ureas (polymers, oligomers, etc. containing a urethane structure and a urea structure in the molecule).
[0153] Of the above, from the viewpoint of the finished appearance, acrylic resin, urea and urethane urea are preferably used.
[0154] Commercially available rheology control agents include, for example, amide waxes such as Disparlon 6900 (Kusumoto Chemical Industries, Ltd.), Disparlon A603 (Kusumoto Chemical Industries, Ltd.), and Thixol W300 (Kyoeisha Chemical Industries, Ltd.); polyethylene waxes such as Disparlon 4200 (Kusumoto Chemical Industries, Ltd.); cellulose acetate butyrate (CAB, Eastman Chemical Products Co., Ltd.), hydroxyethyl cellulose (HEC), hydrophobized HEC, and carboxymethylcellulose (CMC). cellulose-based rheology control agents such as BYK-410, BYK-411, BYK-420, BYK-425 (all manufactured by BYK-Chemie Co., Ltd.); polyolefin-based rheology control agents such as Flonone SA-345HF (Kyoeisha Chemical Co., Ltd.); and higher fatty acid amide-based rheology control agents such as Flonone HR-4AF (Kyoeisha Chemical Co., Ltd.).
[0155] When a rheology control agent is used in the coating composition of the present invention, the amount used is preferably within the range of 0.1 to 20 mass %, particularly 0.5 to 15 mass %, and more particularly 0.8 to 10 mass %, based on the total solid content of the polyaspartic acid ester (A) and the polyisocyanate compound (C), from the viewpoints of finished appearance and coating workability.
[0156] The coating composition of the present invention may further contain, as necessary, pigment dispersants, surface conditioners, surfactants, defoamers, resins other than the polyaspartic acid ester (A) (e.g., epoxy resins, etc.), curing agents (excluding the polyisocyanate compound (B)), preservatives, antifreeze agents, etc.
[0157] This paint contains polyisocyanate compound (B) having free isocyanate groups as a constituent component, and therefore undergoes a crosslinking reaction with the base resin, polyaspartic acid ester (A), at room temperature. It is therefore a two-component paint consisting of a base agent containing component (A) and a curing agent containing component (B). In general, the base agent and curing agent are mixed immediately before application, and a solvent such as an organic solvent is added as necessary to adjust the viscosity, making it suitable for use.
[0158] In this case, it is generally preferred that the components used as required are contained in the base material. Mixing can be carried out using a mixer such as a disperser or homogenizer.
[0159] The coating composition of the present invention is a high solids coating composition, which can reduce the amount of volatile substances such as VOCs emitted during coating. Specifically, the concentration of solids (non-volatile matter) in the coating can be 70% by mass or more, particularly 80% by mass or more.
[0160] In this specification, the paint solids (non-volatile content) concentration at the time of painting can be determined by weighing 1.0 g of a sample immediately before painting, which has been adjusted to a viscosity suitable for painting under conditions of a temperature of 20°C and a humidity of 60%, into a tin dish, heating it at a temperature of 105°C for 3 hours to remove the volatile components, and calculating the remaining amount as a mass percentage.
[0161] The coating composition of the present invention can be applied by a coating method such as dip coating, brush coating, roll brush coating, spray coating, roll coating, spin coating, dip coating, bar coating, flow coating, electrostatic coating, airless coating, electrodeposition coating, die coating, or the like.
[0162] Examples of substrates include cold-rolled steel sheets, black-skinned steel sheets, galvanized alloy steel sheets, electrolytic galvanized steel sheets, etc., and construction or industrial machinery made of these materials, such as bulldozers, hydraulic excavators, wheel loaders, etc. These may be subjected to shot blasting, surface conditioning, surface treatment, etc., or may even be subjected to undercoating, if necessary.
[0163] The coating composition of the present invention is a high-solids coating composition that has excellent weather resistance and corrosion resistance and can be applied directly to metal substrates. Therefore, it can be suitably used as a topcoat coating that complies with VOC regulations from the ESG perspective for the above-mentioned substrate applications, in particular as a one-coat topcoat coating that is applied directly to metal substrates. EXAMPLES
[0164] The present invention will be described in more detail below with reference to Production Examples, Examples, and Comparative Examples, but the present invention is not limited thereto. In each example, "parts" means parts by mass, and "%" means % by mass.
[0165] Preparation of coating composition Example 1 Preparation of Coating Composition No. 1 Coating composition No. 1 was obtained by the following steps 1 and 2.
[0166] Process 1 Aspartic acid ester resin (A-1) 49.5 parts (solid content), polyol compound (D-1) 5.5 parts (solid content), Variace B-33 (Note 1) 18 parts, Typec CR-95 (Note 2) 8 parts, Carbon MA-100 (Note 3) 1 part, BYK-161 (Note 4) 3 parts, TINUVIN 400 (Note 5) 2 parts, TINUVIN 123 (Note 6) 2 parts, BYK-052N (Note 7) 0.01 parts, BYK-300 (Note 8) 0.05 parts were mixed and stirred, and the solid content concentration was adjusted with a solvent to obtain the main agent of paint composition No. 1 with a solid content of 80 mass%.
[0167] In the above, the extender pigment and color pigment were added and mixed as a pigment dispersion paste prepared using 20 parts of the aspartic acid ester resin (A-1).
[0168] Step 2: 45.1 parts of a polyisocyanate compound (D-1) and 7.0 parts of an epoxy group-containing silane coupling agent (B-1) were added to the base resin obtained in step 1 above, and the solid content was adjusted with a solvent to obtain coating composition No. 1 having a solid content of 80% by mass.
[0169] Examples 2 to 26 and Comparative Examples 1 to 4 Preparation of Coating Compositions Nos. 2 to 30 Coating composition Nos. 2 to 30 were obtained in the same manner as in Example 1, except for the formulations shown in Table 1. Coating composition Nos. 27 to 30 are comparative examples.
[0170] The raw material composition (values) in Table 1 are solid content masses.
[0171] [Table 1]
[0172] [Table 2]
[0173] [Table 3]
[0174] [Table 4]
[0175] [Table 5]
[0176] The raw materials in the table are as follows:
[0177] Polyaspartic acid ester compound (A) Polyaspartic acid ester (A-1): Desmophen NH-1420: Trade name, manufactured by Covestro, polyaspartic acid ester, amine value 201. Molecular weight 554.7, viscosity 1000 mPa·s Polyaspartic acid ester (A-2): Desmophen NH-1423LF: Trade name, manufactured by Covestro, polyaspartic acid ester, amine value 230, molecular weight 554.7, viscosity 1500 mPa·s Polyaspartic acid ester (A-3): Desmophen NH-1220: Trade name, manufactured by Covestro, polyaspartic acid ester, amine value 206, molecular weight 460.6, viscosity 100 mPa·s Polyisocyanate Compound (B) Polyisocyanate compound (B-1): Desmodur N 3900: Trade name, manufactured by Covestro, low viscosity HDI isocyanurate, NCO group content 23.5%. Viscosity at 23°C 700 mPa·s Polyisocyanate compound (B-2): Desmodur N 3600: Trade name, manufactured by Covestro, HDI isocyanurate, NCO group content 23%. Viscosity at 23°C: 1200 mPa·s Polyisocyanate compound (B-3): Desmodur N 3200: Trade name, manufactured by Covestro, HDI burette type isocyanate, NCO group content 23%. Viscosity at 23°C: 2500 mPa·s Polyisocyanate compound (B-4): TOLONATE XF-800: Trade name, manufactured by VENCOLEX, HDI modified aliphatic polyisocyanate, NCO group content 20.1%. Viscosity at 23°C 900 mPa·s Epoxy group-containing silane coupling agent (C) Epoxy group-containing silane coupling agent (C-1): "KBM-403": trade name, manufactured by Shin-Etsu Chemical Co., Ltd., γ-glycidoxypropyltrimethoxysilane, epoxy equivalent 236, molecular weight 236.
[0178] Epoxy group-containing silane coupling agent (C-2): "KBE-402": trade name, manufactured by Shin-Etsu Chemical Co., Ltd., γ-glycidoxypropylmethyldiethoxysilane, epoxy equivalent 248, molecular weight 248.
[0179] Epoxy group-containing silane coupling agent (C-3): "MP-200": trade name, manufactured by Momentive Corporation, condensation product of γ-glycidoxypropyltrimethoxysilane, epoxy equivalent 205.
[0180] Epoxy resin (1): "JER-828": product name, manufactured by Mitsubishi Chemical Corporation, bisphenol A type liquid epoxy resin, epoxy equivalent 188.
[0181] Polyol Compounds (D) Polyol compound (D-1): "Desmophen XP-2488": Trade name, manufactured by Covestro, polyester polyol, hydroxyl value 528. Molecular weight 1400 Polyol compound (D-2): "EXCENOL 750ED": trade name, manufactured by AGC Corporation, polyester polyol, hydroxyl value 760, molecular weight 300.
[0182] Polyol compound (D-3): "Joncryl 507": trade name, manufactured by BASF, hydroxyl group-containing acrylic resin, hydroxyl value 140. Molecular weight 2200.
[0183] Polyol compound (D-4): "TA22-981": trade name, manufactured by Resonac Corporation, polyester polyol, hydroxyl value 55, molecular weight 2000.
[0184] Polyol compound (D-5): "Sannyx GP-3000": trade name, manufactured by Sanyo Chemical Industries, Ltd., polyether polyol, hydroxyl value 56, molecular weight 3000.
[0185] (Note 1) Variace B-33: Sakai Chemical Industry Co., Ltd., product name, barium sulfate, average particle size 0.3 μm (Note 2) Tipaque CR-95: Product name, titanium dioxide, manufactured by Ishihara Sangyo Kaisha, Ltd. (Note 3) Carbon MA-100: Product name, carbon black, manufactured by Mitsubishi Chemical Corporation (Note 4) BYK-161: Product name, wetting and dispersing agent, manufactured by BYK-Chemie Co., Ltd. (Note 5) TINUVIN400: BASF product name, hydroxyphenyltriazine ultraviolet absorber (Note 6) TINUVIN123: BASF product name, hindered amine light stabilizer (Note 7) BYK-052N: BYK Co., Ltd., product name, defoamer, alkyl vinyl ether copolymer (Note 8) BYK-300: Product name, silicone-based surface conditioner manufactured by BYK Co., Ltd. (Note 9) Neostan U-100: Product name, dibutyltin dilaurate, urethane curing catalyst, manufactured by Nitto Kasei Co., Ltd. (Note 10) Silyl group-containing modified polyisocyanate X1: 89.5 parts of 3-aminopropyltrimethoxysilane and 0.04 parts of methoquinone were placed in a flask and heated to 80°C, and air was introduced into the liquid and bubbled while stirring. 110 parts of di-i-propyl fumarate were added dropwise over 2 hours, and then the mixture was kept at 80°C for 1 hour and aged at 50°C for 1 week to obtain 199 parts of a mixture containing 95% of 3-(N-(1,2-bis(i-propoxycarbonyl)ethyl)amino)propyltrimethoxysilane. In another flask, 280 parts of mineral spirits, 224 parts of "Swasol 1000" (naphtha-based solvent, Maruzen Petrochemical Co., Ltd., product name), and 550 parts of "Duranate TSA-100" (hexamethylene diisocyanate-based modified isocyanurate-type polyisocyanate, Asahi Kasei Corporation, product name, isocyanate group content 20.6 wt%) were placed and stirred at room temperature. 108 parts of a mixture containing 95% 3-(N-(1,2-bis(i-propoxycarbonyl)ethyl)amino)propyltrimethoxysilane was added dropwise to the mixture over 2 hours, and the mixture was then kept at 60°C for 1 hour and cooled to room temperature to obtain a silyl group-containing modified polyisocyanate X1 solution with a non-volatile content of 56%. The concentration of isocyanate groups in 1 g of the solution was 2.09 mmol / g (3.72 mmol / g in terms of non-volatile content).
[0186] (Note 11) Silyl group-containing modified polyisocyanate X2: 89.5 parts of 3-aminopropyltrimethoxysilane, 0.04 parts of methoquinone, and 4 parts of "Swasol 1000" (naphtha-based solvent, Maruzen Petrochemical Co., Ltd., trade name) were placed in a flask, and air was introduced into the liquid to bubble and stir, and 104 parts of isobornyl acrylate was added dropwise over 2 hours, and then the mixture was kept at 50°C for 1 hour. The mixture was further aged at 50°C for 1 week to obtain 198 parts of a mixture containing 3-(N-(2-(isobornyloxycarbonyl)ethyl)amino)propyltrimethoxysilane / 3-aminopropyltrimethoxysilane / 3-(N,N-di(2-(isobornyloxycarbonyl)ethyl)amino)propyltrimethoxysilane in a molar ratio of 74 / 13 / 13. The total amount of (primary amino group + secondary amino group) in 1 g of the mixture was 2.20 mmol.
[0187] In another flask, 273 parts of mineral spirits, 223 parts of "Swasol 1000" (naphtha-based solvent, Maruzen Petrochemical Co., Ltd., trade name), and 500 parts of "Duranate TSA-100" were placed and stirred at room temperature. 111 parts of a mixture containing 3-(N-(2-(isobornyloxycarbonyl)ethyl)amino)propyltrimethoxysilane / 3-aminopropyltrimethoxysilane / 3-(N,N-di(2-(isobornyloxycarbonyl)ethyl)amino)propyltrimethoxysilane in a molar ratio of 74 / 13 / 13 were added dropwise over 2 hours, and the mixture was kept at 60°C for 2 hours and cooled to room temperature to obtain a silyl group-containing modified polyisocyanate X2 solution with a non-volatile content of 55%. The concentration of isocyanate groups contained in 1 g of the solution was 1.99 mmol / g (3.62 mmol / g in terms of non-volatile content).
[0188] (Note 12) Silyl group-containing modified polyisocyanate X3: In a flask under a nitrogen atmosphere, 89 parts of methyl acetate, which is a linear saturated ester, and 179 parts of 3-aminopropyltrimethoxysilane were placed and stirred at room temperature. 0.58 parts of a 28% methanol solution of sodium methoxide was added as a catalyst, and the mixture was stirred and heated to 70°C and aged for one day. The reaction rate of 3-aminopropyltrimethoxysilane was 97%, and methanol was by-produced in an amount almost equimolar to the reacted 3-aminopropyltrimethoxysilane. Then, 1.1 parts of bis(2-ethylhexyl)phosphoric acid was added as an acidic compound, and the mixture was concentrated by removing methanol and remaining methyl acetate under reduced pressure at 50°C to 70°C, resulting in 222 parts of crude 3-acetamidopropyltrimethoxysilane containing catalyst-derived residue as an N-position acyl modified intermediate. In another flask under a nitrogen atmosphere, 62 parts of butyl acetate and 500 parts of "Duranate TSA-100" were placed and stirred at room temperature. 55 parts of crude 3-acetamidopropyltrimethoxysilane was added to this, and the mixture was heated at 110°C for 7 hours to adduct the secondary amide group to the isocyanate group, thereby obtaining a silyl group-containing modified polyisocyanate X3 solution with a non-volatile content of 90%. The concentration of isocyanate groups in 1 g of the solution was 3.49 mmol / g (3.88 mmol / g in terms of non-volatile content).
[0189] (Note 13) Molecular sieve 3A: Union Showa Co., Ltd., product name, sodium calcium aminosilicate, pore size 0.25 nm (Note 14) Molecular sieve 5A: Union Showa Co., Ltd., product name, sodium calcium aminosilicate, pore size 0.42 nm (Note 15) Molecular sieve 13X: Union Showa Co., Ltd., product name, sodium calcium aminosilicate, pore size 1.0 nm The test panels were prepared and the performance was evaluated according to the following procedure. The results are shown in Table 1.
[0190] Creating test panels Each of the coating compositions No. 1 to No. 30 was air spray coated (pressure 0.4 MPa) onto shot-blasted general structural rolled steel SS-400 (size 2.3 × 150 × 300 mm, Ra: 3.9 μm, Ry: 34 μm, Rz: 23 μm) so that the dry film thickness was 80 μm. After setting at 20°C for 10 minutes, the coating was dried by heating at 60°C for 30 minutes using an electric hot air dryer, and further aged at 20°C for 168 hours to obtain test panels of each of the coating compositions No. 1 to No. 30.
[0191] Performance evaluation Each of the coating compositions Nos. 1 to 30 and the test panels of each coating composition were subjected to performance tests for the following test items, and performance evaluation was performed according to the following evaluation criteria. The performance evaluation results are also shown in Table 1.
[0192] Finished appearance: The appearance of the coated surface of each test panel was evaluated visually and by gloss value. ◎: Good smoothness and 60 degree gloss value of 80 or more. ◯: Good smoothness and 60 degree gloss value of 70 or more and less than 80. Δ: At least one deterioration in the finished appearance selected from side edges, wavy edges, dullness, and chipped skin is observed, or the 60 degree gloss value is 60 or more and less than 70. ×: At least one of the finished appearances selected from side wrinkles, wavy wrinkles, dullness, and chipped skin is significantly deteriorated, or the 60 degree gloss value is less than 60.
[0193] Pencil hardness: According to JIS K 5600-5-4, a pencil lead was placed at an angle of about 45 degrees against the test plate surface, and the pencil lead was moved forward at a uniform speed for about 10 mm while being pressed against the test plate surface hard enough not to break the lead. The hardness symbol of the hardest pencil that did not break the coating was recorded as the pencil hardness. ◎:2H or more ○: H or more and less than 2H △: Above F and below H ×: Less than F Touch-drying property: Each coating composition was sprayed onto a tinplate in a constant temperature and humidity chamber at a temperature of 20°C and a humidity of 50% to give a dry film thickness of 60 μm, and the touch-drying time until the paint no longer remained on the finger was measured. ◎: Drying time less than 20 minutes ○: Drying time is 20 minutes or more and less than 30 minutes △: 30 minutes or more and less than 45 minutes ×: 45 minutes or more Corrosion resistance: In accordance with JIS K 5600-7-1, each test coated plate had a cross cut made in the test coating surface that reached the base material, and was sprayed with a 5% aqueous sodium chloride solution with a pH adjusted to 7.0 in an atmosphere of 35°C for 168 hours, after which the width of the blister on one side from the cut was evaluated. ◎: Less than 1.0mm ○: 1.0mm or more and less than 2.0mm △: 2.0mm or more and less than 3.0mm ×: 3.0mm or more Weather resistance: A Super Xenon Weather-O-Meter (product name, manufactured by Suga Test Instruments) specified in JIS B 7754 was used for each test panel. One cycle consisted of 1 hour 42 minutes of exposure to a xenon arc lamp and 18 minutes of exposure to the same lamp under rainfall conditions for two hours. After 1,500 hours (750 cycles) of repeated testing, the 60 degree gloss retention (GR%) and color difference (ΔE) of each counterfeit panel (initially painted panel) were measured and evaluated according to the following criteria. ◎: 60 degree gloss retention (GR%) is 80 or more and color difference (ΔE) is less than 2.0. ○: 60 degree gloss retention (GR%) is 70 or more and less than 80, or color difference (ΔE) is 2.0 or more and less than 3.0. △: 60 degree gloss retention (GR%) is 50 or more and less than 70, or color difference (ΔE) is 3.0 or more and less than 5.0. ×: 60 degree gloss retention (GR%) is less than 50 or color difference (ΔE) is 5.0 or more.
[0194] Pot life: For coating compositions Nos. 23 to 26 containing zeolite (molecular sieve), the pot life was evaluated in comparison with coating composition No. 16 in terms of the thickening rate.
[0195] When the viscosity of each paint composition was measured in an Iwata cup, the viscosity increase rate after one hour (Iwata cup viscosity after one hour (seconds) / initial Iwata cup viscosity (seconds)) was 4.0 for No. 16, 1.4 for No. 23, 1.3 for No. 24, 1.1 for No. 25, and 1.2 for No. 26. [Industrial Applicability]
[0196] It is possible to provide a high solids coating composition which has excellent weather resistance, corrosion resistance and coating film hardness and can be applied directly to metal substrates.
Claims
1. A high solids coating composition comprising a polyaspartic acid ester (A), a polyisocyanate compound (B), an epoxy group-containing silane coupling agent (C), and a polyol (D) having a weight average molecular weight of 250 to 2,300 and a hydroxyl value in the range of 50 to 800.
2. 2. The high solids coating composition according to claim 1, wherein the polyaspartic acid ester (A) contains a polyaspartic acid ester having a secondary amino group represented by the following formula (1): [Formula 1] (In the formula, X is an n-valent cyclic or chain aliphatic hydrocarbon group or a polyoxyalkylene polyamine residue having a number average molecular weight of 25 to 5,000, and R 1 and R 2 are each independently an organic group inactive to an isocyanate group, and n is an integer of 2 or more.
3. 3. The high solids coating composition according to claim 1, wherein the polyol (D) contains a polyester polyol and / or a polyether polyol.
4. The high solids coating composition according to any one of claims 1 to 3, having a solids concentration of 70 mass% or more.
5. The high solids coating composition according to any one of claims 1 to 4, further comprising a pigment.
6. The high solids coating composition according to any one of claims 1 to 5, wherein the polyisocyanate compound (B) contains a silyl group-containing modified polyisocyanate.
7. The high solids coating composition according to claim 6, wherein the silyl group-containing modified polyisocyanate is a reaction product made from components including an alkoxysilane (a1) having a primary amino group, an alkyl carboxylate (a2) and a polyisocyanate (a3) as raw materials.
8. The high solids coating composition according to any one of claims 1 to 7, further comprising a zeolite.
9. The one-coat high solids coating composition according to any one of claims 1 to 8.
10. A coating method comprising coating a substrate with the high solids coating composition according to any one of claims 1 to 8.
11. A construction machine or industrial machine coated with the high solids coating composition according to any one of claims 1 to 8.
Citation Information
Patent Citations
High-functional polyisocyanate containing allophanate group and silane group
JP2011074390A
Printing ink, method for producing polyurethane polyurea resin, and printed matter
JP2017149858A
Modified polyaspartic acid ester and curable resin composition
WO2016063884A1
Polyaspartic coating composition, coating film, and coated article
WO2018163953A1
High-solid coating composition
JP2003128989A
Cited By
Aqueous coating composition, coating film, and coated article
JP2026044945A
Water-based paint composition, coating film and coated article
JP7806159B1