Method of manufacturing laminate

The method improves the embeddability of optical waveguide cladding in opto-electrical composite substrates by using a cover film with controlled mechanical properties during lamination, addressing voids and resin leakage issues for enhanced optical performance.

JP2024146689APending Publication Date: 2024-10-15SUMITOMO BAKELITE CO LTD

Patent Information

Application Number
JP2023126867
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-08-03
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional methods for manufacturing opto-electrical composite substrates face challenges in fully embedding the optical waveguide cladding in through-holes of the substrate, leading to issues such as voids and resin leakage, which affect optical performance.

Method used

A method involving the use of a cover film with specific storage modulus and loss modulus properties to create a gap during lamination, allowing for improved embeddability and prevention of resin leakage, by stacking a cover film, substrate, and resin layer in a workpiece and heating and pressing under controlled conditions.

Benefits of technology

The method enhances the embeddability of the cladding layer in through-holes, reducing voids and resin leakage, thereby improving the optical performance and reliability of the opto-electrical composite substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146689000001_ABST
    Figure 2024146689000001_ABST
Patent Text Reader

Abstract

To provide a method of manufacturing a laminate that can yield a photoelectric composite substrate with improved embedment properties.SOLUTION: The present invention relates to a method of manufacturing a laminate comprising a substrate 110 having a through hole 140 and a first clad layer 20 of a light guide 100, and the method comprises at least: a process (A) of preparing a workpiece 400 having a cover film 330, the substrate 110, and a film 300 with a resin layer (a) 310 made of a resin composition to form the first clad layer 20, which are superposed on one another in this order; and a process (B) of heating and pressing the workpiece 400 to laminate the first clad layer 20 on the substrate 110.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a laminate. [Background technology]

[0002] 2. Description of the Related Art In recent years, there has been a demand for components capable of realizing more advanced information communication, such as larger capacity information and faster information communication speeds, in information and communication devices. As one such component, an optical / electrical composite substrate has been considered.

[0003] An example of the optical / electrical composite substrate is one in which an optical waveguide is provided on a substrate. Techniques relating to a method for manufacturing an optical waveguide include, for example, the techniques described in Patent Documents 1 to 3.

[0004] Patent Document 1 describes a method for producing an embedded polyimide optical waveguide, which is characterized in that an upper cladding between an arbitrary substrate and a ridge-type waveguide has the same heat resistance as the substrate and is bonded together with an adhesive with a lower refractive index than the core. According to the method for producing a polyimide optical waveguide described in Patent Document 1, it is described that a polyimide optical waveguide can be produced on any substrate.

[0005] Patent Document 2 describes an opto-electrical hybrid board comprising a flexible circuit board in which electrical wiring having mounting pads is formed on the surface of an insulating layer, an element mounted on the mounting pad, and an optical waveguide laminated on the back surface of the insulating layer, wherein the flexible circuit board is a flexible double-sided circuit board in which electrical wiring is also formed on the back surface of the insulating layer, and a metallic reinforcing layer is formed by plating on at least the portion of the electrical wiring on the back surface that corresponds to the mounting pad, and the optical waveguide is in contact with the metallic reinforcing layer. According to the optical-electrical hybrid board described in Patent Document 2, a metallic reinforcing layer is adhered to an insulating layer of a flexible circuit board without an adhesive layer, and it is described that an optical-electrical hybrid board can be provided in which elements are properly mounted while suppressing deformation due to a pressure load when the elements are mounted by the metallic reinforcing layer.

[0006] Patent Document 2 describes a method of preparing a substrate in which copper foil 21 is formed on the front and back surfaces of an insulating layer 1 made of a resin such as polyimide, and forming through holes 1a and via holes 1b for an optical path in the substrate (see paragraph 0023 of Patent Document 2). It also describes a flexible double-sided circuit board E in which a metallic reinforcing layer M is formed (see paragraph 0028 of Patent Document 2). The flexible double-sided circuit board E includes the above substrate. Furthermore, Patent Document 2 describes that an undercladding layer 6 is formed on the back side of a flexible double-sided circuit board E in contact with a metal reinforcing layer M that covers the electrical wiring 2B on the back side, and describes that examples of a molding material for the undercladding layer 6 include photosensitive resins and thermosetting resins (see paragraph 0029 of Patent Document 2). According to Figures 4 to 6 of Patent Document 2, it can be seen that the molding material for the undercladding layer 6 is filled into a recess formed in the flexible double-sided circuit board E on which the metal reinforcing layer M is formed.

[0007] Patent Document 3 describes an optoelectronic wiring board that is formed by integrating a rigid section in which conductor circuits and insulating layers are laminated on both sides of a substrate with one or more bendable flex sections, wherein the rigid section is formed with external connection terminals for mounting optical elements and / or package substrates on which optical elements are mounted, and at least one of the flex sections is formed with optical wiring. According to the optoelectronic wiring board of Patent Document 3, it is described that large-volume information processing and high-speed information processing can be suitably performed without increasing the size of the wiring board.

[0008] Patent Document 3 describes that the rigid section has an optical signal transmitting region formed therein, and that the optical signal transmitting region is filled with a resin composition (see claims 4 and 5 of Patent Document 3). Furthermore, Patent Document 3 describes that the optical signal transmitting region is formed so as to penetrate all of the substrates and insulating layers that constitute the rigid section (see claim 6 of Patent Document 3).

[0009] Furthermore, Patent Document 3 describes a substrate 221 consisting of an optical waveguide film 250 and a surrounding resin layer (insulating layer) 221a, and describes that the resin layer 221a constitutes part of the optical signal transmitting regions 242a, 242b (see paragraph 0033 of Patent Document 3). [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2000-321455 A [Patent Document 2] JP 2014-238455 A [Patent Document 3] JP 2006-140233 A Summary of the Invention [Problem to be solved by the invention]

[0011] In conventional technology relating to optoelectronic composite substrates, there are known optoelectronic composite substrates in which recesses and through holes formed in a substrate are filled with a resin composition (see, in particular, Patent Documents 2 and 3).

[0012] The manufacturing process of the photoelectric composite substrate includes, for example, a process of integrating a substrate having a through hole with a film for optical waveguide clad. In this process, the through hole formed in the substrate needs to be filled with the optical waveguide clad (hereinafter, "embedding property" refers to the property of how much the optical waveguide clad can be embedded in the through hole).

[0013] The present invention has been made in consideration of the above circumstances, and provides a method for producing a laminate that can provide an optoelectronic composite substrate with improved embeddability. [Means for solving the problem]

[0014] According to the present invention, there is provided a method for producing a laminate as described below.

[0015] [1] A method for manufacturing a laminate including a substrate having a through hole and a first clad layer of an optical waveguide, comprising the steps of: A step (A) of preparing a workpiece by stacking a cover film, the substrate, and a film having a resin layer (a) made of a resin composition for forming the first clad layer in this order; and (B) laminating the first clad layer onto the substrate by heating and pressing the work. [2] The method for producing a laminate according to [1] above, wherein the cover film has a storage modulus E' at 100°C of 0.10 GPa or more. [3] The method for producing a laminate according to [2] above, wherein the cover film has a storage modulus E' at 100°C of 0.10 GPa or more and 2.00 GPa or less. [4] The method for producing a laminate according to any one of the above [1] to [3], wherein the cover film has a loss modulus E'' at 100° C. of 0.1 MPa or more and 100 MPa or less. [5] The method for producing a laminate according to any one of the above [1] to [4], wherein the cover film includes at least one film selected from the group consisting of a resin film and a metal film. [6] The method for producing a laminate described in [5] above, wherein the cover film includes a resin film. [7] The method for producing a laminate described in [6] above, wherein the resin constituting the resin film includes at least one selected from the group consisting of polyethylene terephthalate, polypropylene, polybutylene terephthalate, polyethylene naphthalate, and polyimide. [8] The method for producing a laminate according to any one of the above [1] to [7], wherein the cover film has a thickness of 5 μm or more and 200 μm or less. [9] The method for producing a laminate according to any one of the above [1] to [8], wherein in the step (B), the work is heated to 80° C. or more and 180° C. or less and pressed.

[10] The method for producing a laminate according to any one of the above [1] to [9], wherein in the step (B), the work is pressed with a pressure of 0.1 MPa or more and 10.0 MPa or less.

[11] The method for producing a laminate according to any one of the above [1] to

[10] , wherein in the step (B), the work is heated and pressed under reduced pressure using a vacuum laminator.

[12] The method for producing a laminate according to

[11] above, wherein in the step (B), the degree of vacuum is 500 Pa or less.

[13] The method for producing a laminate according to any one of the above [1] to

[12] , further comprising a step (C) of removing the cover film from the workpiece after the step (B).

[14] The method for producing a laminate according to any one of the above [1] to

[13] , wherein T / R is 0.10 or more, where T [μm] is the thickness of the substrate and R [μm] is the hole diameter of the through hole.

[15] The method for producing a laminate according to any one of the above [1] to

[14] , wherein the through holes have a hole diameter of 10 μm or more and 1000 μm or less.

[16] The method for producing a laminate according to any one of the above [1] to

[15] , wherein the substrate has a thickness of 10 μm or more and 500 μm or less.

[17] The method for producing a laminate according to any one of the above [1] to

[16] , wherein the resin layer (a) has a thickness of 10 μm or less and 200 μm or less.

[18] The method for producing a laminate according to any one of the above [1] to

[17] , wherein the resin layer (a) has a thickness smaller than a thickness of the substrate.

[19] The method for producing a laminate according to any one of [1] to

[18] above, wherein, when the volume of the through hole in the laminate is taken as 100 volume %, 70 volume % or more of the through hole is filled with a resin composition for forming the first clad layer.

[20] The method for producing a laminate according to any one of [1] to

[19] above, wherein the laminate is an optical / electrical composite substrate further comprising a core layer and a second clad layer in this order on the first clad layer. Effect of the Invention

[0016] According to the present invention, it is possible to provide a method for producing a laminate that can provide an optoelectronic composite substrate with improved embeddability. [Brief description of the drawings]

[0017] [Figure 1] 1 is a cross-sectional view showing a schematic example of a structure of an optical / electrical composite substrate according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing a schematic example of a structure of a workpiece in step (A). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Furthermore, a numerical range of "A to B" means A or more and B or less unless otherwise specified.

[0019] 1 is a cross-sectional view showing a schematic example of the structure of an optoelectronic composite substrate according to the present embodiment, the drawing being a simplified view and not in accordance with the actual dimensional ratio. As shown in FIG. 1, the optical / electrical composite substrate 200 has an optical waveguide 100 provided on a substrate 110. The optical waveguide 100 has a first clad layer 20, a core layer 30, and a second clad layer 40 laminated in this order. A mirror 50 on the light-emitting element side and a mirror 60 on the light-receiving element side are formed on the optical waveguide 100. The substrate 110 has through-holes 140 (140a, 140b) (the through-hole 140 shown in FIG. 1 is filled with the first clad layer 20). A light-emitting element 120 and a light-receiving element 130 are provided on the side of the substrate 110 opposite to the optical waveguide 100 side.

[0020] The propagation path of light in the photoelectric composite substrate 200 will be specifically described with reference to Fig. 1. The light emitted from the light emitting portion of the light emitting element 120 passes through a through hole 140a formed in the substrate 110, enters the mirror 50 on the light emitting element side, and is transmitted through the core layer 30. Thereafter, it enters the mirror 60 on the light receiving element side, passes through a through hole 140b formed in the substrate 110, and enters the light receiving element 130. The arrows in Fig. 1 are a schematic representation of the propagation of light.

[0021] According to the study of the present inventors, it was found that in the conventional manufacturing method of the optical / electrical composite substrate, the first clad layer cannot be sufficiently embedded in the through-hole formed in the substrate, and thus a depression may occur on the surface of the optical waveguide clad opposite to the substrate side (i.e., the core layer side of the first clad layer) or a void may occur in the through-hole. The through-hole is a propagation path of light, and it was found that when the above-mentioned depression or void occurs in the optical / electrical composite substrate, an optical loss occurs at the interface of the depression or void. The present invention has been made in consideration of the above circumstances, and provides a method for producing a laminate that can provide an optoelectronic composite substrate with improved embeddability.

[0022] The method for manufacturing a laminate of the present embodiment is a method for manufacturing a laminate comprising a substrate having a through hole and a first clad layer of an optical waveguide, and comprises at least a step (A) of preparing a workpiece comprising a cover film, a substrate, and a film comprising a resin layer (a) made of a resin composition for forming the first clad layer, stacked in that order, and a step (B) of heating and pressing the workpiece to laminate the first clad layer onto the substrate.

[0023] The method for manufacturing the laminate of this embodiment includes a step (A) of preparing a workpiece by stacking a cover film, a substrate, and a film having a resin layer (a) in that order, and a step (B) of heating and pressing the workpiece. The inventors believe that by providing the workpiece with a cover film, an appropriate gap is generated between the cover film and the substrate when the workpiece is pressed, and this gap acts as a passage for air to escape, thereby suppressing the generation of voids in the through hole and improving embeddability. That is, according to the method for producing a laminate of the present embodiment, it is possible to provide a method for producing a laminate that can obtain an optoelectronic composite substrate with improved embeddability.

[0024] Furthermore, the inventors have found that when filling a through hole formed in a substrate with a resin composition for forming a first clad layer, the resin composition may leak onto the surface of the substrate opposite to the first clad layer (hereinafter, such a phenomenon will be referred to as "resin leakage"). Furthermore, the inventors have found that the more the embeddability improves, the more likely resin leakage occurs.

[0025] In view of the above circumstances, the present inventors have conducted extensive research and have found that in the method for producing a laminate according to the present embodiment, by setting the storage modulus E' of the cover film within an appropriate range, embeddability can be improved and resin leakage can be suppressed.

[0026] Hereinafter, each step of the method for producing the laminate of this embodiment will be specifically described.

[0027] [Work preparation process (A)] The method for manufacturing the laminate of this embodiment includes a step (A) of preparing a workpiece by stacking, in this order, a cover film, a substrate, and a film having a resin layer (a) made of a resin composition for forming a first clad layer.

[0028] 2 is a cross-sectional view showing a schematic example of the structure of the workpiece in step (A). Note that the drawing is a simplified drawing and does not correspond to the actual dimensional ratio. The workpiece 400 is formed by laminating, in this order, a cover film 330, a substrate 110, and a film 300 including a resin layer (a) made of a resin composition for forming a first clad layer. Here, a through hole 140 is formed in the substrate 110.

[0029] The workpiece 400 is preferably formed by stacking the cover film 330, the substrate 110, and the film 300 provided with the resin layer (a) in that order so that they are in direct contact with each other.

[0030] The film 300 having the resin layer (a) may be a single-layer film consisting of only the resin layer (a) 310, or may be a multi-layer film as shown in FIG. 2, but is preferably a film in which the resin layer (a) 310 and a base film 320 are laminated. When the film 300 having the resin layer (a) includes the base film 320, the film 300 having the resin layer (a) can be easily handled and contamination of the press device can be prevented. When the film 300 having the resin layer (a) is a multi-layer film, the workpiece 400 is placed on the substrate 110 with the film 300 having the resin layer (a) facing the substrate 110, with the resin layer (a) 310 being on the substrate 110 side.

[0031] There are no particular limitations on the substrate 110 as long as it is a substrate having a through hole. Examples of the substrate 110 include a printed circuit board and a flexible substrate, and the like. A flexible substrate is preferable, and a flexible double-sided copper-clad laminate is more preferable.

[0032] The thickness of substrate 110 is preferably 10 μm or more, more preferably 30 μm or more, even more preferably 40 μm or more, and even more preferably 45 μm or more, and from the viewpoint of miniaturizing the optoelectronic composite substrate, it is preferably 500 μm or less, more preferably 300 μm or less, even more preferably 200 μm or less, even more preferably 100 μm or less, and even more preferably 80 μm or less.

[0033] The substrate 110 has at least one through-hole 140 , and may have one through-hole 140 or may have two or more through-holes 140 . Specifically, for example, in the substrate 110 shown in FIG. 1 and FIG. 2, the through-hole 140 serves as a light propagation path, so the substrate 110 has a through-hole 140a on the light-emitting element side and a through-hole 140b on the light-receiving element side.

[0034] The hole diameter of the through hole 140 is preferably 10 μm or more, more preferably 30 μm or more, even more preferably 50 μm or more, even more preferably 70 μm or more, even more preferably 90 μm or more, and preferably 1000 μm or less, more preferably 800 μm or less, even more preferably 600 μm or less, even more preferably 500 μm or less, even more preferably 400 μm or less, even more preferably 350 μm or less, even more preferably 250 μm or less, even more preferably 200 μm or less, even more preferably 150 μm or less. Here, when the substrate 110 has a plurality of through holes 140, it is sufficient that the hole diameter of at least one of the through holes 140 is within the above range.

[0035] When the thickness of substrate 110 is T [μm] and the hole diameter of through hole 140 is R [μm], T / R is preferably 0.10 or more, more preferably 0.13 or more, even more preferably 0.15 or more, even more preferably 0.20 or more, even more preferably 0.25 or more, even more preferably 0.30 or more, even more preferably 0.35 or more, even more preferably 0.40 or more, even more preferably 0.45 or more, and even more preferably 0.60 or more, and the upper limit is not particularly limited, and may be, for example, 2.00 or less, 1.50 or less, or 1.00 or less. Here, when the substrate 110 has a plurality of through holes 140, it is sufficient that the T / R of at least one of the through holes 140 falls within the above range. Generally, the larger the T / R, the more difficult it is to sufficiently fill the through-hole with the first clad layer. On the other hand, according to the method for manufacturing the laminate of the present embodiment, even when the T / R is large, it is possible to sufficiently fill the through-hole with the first clad layer.

[0036] A preferred embodiment of the film 300 including the cover film 330 and the resin layer (a) will be described later.

[0037] [Laminating process (B)] The method for producing a laminate in this embodiment includes a step (B) of laminating a first cladding layer onto a substrate by heating and pressing a workpiece. The substrate and the resin layer (a) can be laminated by heating and pressing the workpiece. Since the resin layer (a) is made of the resin composition for forming the first clad layer, in other words, the substrate and the first clad layer can be laminated by heating and pressing the workpiece.

[0038] The degree of vacuum in step (B) is not particularly limited, and the workpiece may be heated and pressed at normal pressure, or may be heated and pressed under reduced pressure. In step (B), the work is preferably heated and pressed under reduced pressure using a vacuum laminator. Here, reduced pressure means that the degree of vacuum is smaller than normal pressure (1013 hPa). In step (B), from the viewpoint of further improving embeddability, the degree of vacuum is preferably 500 Pa or less, more preferably 400 Pa or less, even more preferably 350 Pa or less, and even more preferably 320 Pa or less. The lower limit is not particularly limited, but may be, for example, 10 Pa or more, or 50 Pa or more.

[0039] In step (B), the pressure when pressing the workpiece is preferably 0.1 MPa or more, more preferably 0.3 MPa or more, and even more preferably 0.4 MPa or more, from the viewpoint of further improving embeddability, and is preferably 10.0 MPa or less, more preferably 8.0 MPa or less, even more preferably 6.0 MPa or less, even more preferably 5.0 MPa or less, even more preferably 3.0 MPa or less, and even more preferably 1.0 MPa or less, from the viewpoint of preventing damage to the substrate.

[0040] In step (B), the temperature of the workpiece when it is heated and pressed is, from the viewpoint of further improving embeddability, preferably 80°C or higher, more preferably 90°C or higher, even more preferably 100°C or higher, even more preferably 120°C or higher, and even more preferably 130°C or higher, and from the viewpoint of further improving embeddability, preferably 180°C or lower, more preferably 160°C or lower, and even more preferably 150°C or lower. When the temperature of the workpiece is equal to or higher than the lower limit, the resin composition for forming the first cladding layer is more easily softened, and the embeddability is further improved.When the temperature of the workpiece is equal to or lower than the upper limit, the storage modulus E' of the cover film at the workpiece temperature is more improved, and the embeddability is further improved. Here, the temperature of the workpiece may be considered to be the same as the set press temperature of the press device, because the workpiece is thin and therefore the temperature of the workpiece is considered to reach the same temperature as the set press temperature within a few seconds after being placed in the press device.

[0041] In step (B), the time for pressing the workpiece is, from the viewpoint of further improving embeddability, preferably 30 seconds or more, more preferably 60 seconds or more, even more preferably 90 seconds or more, even more preferably 120 seconds or more, even more preferably 150 seconds or more, even more preferably 180 seconds or more, and even more preferably 200 seconds or more, and from the viewpoint of further improving productivity, is preferably 500 seconds or less, more preferably 400 seconds or less, even more preferably 300 seconds or less, and even more preferably 250 seconds or less.

[0042] In the step (B), the method for heating and pressing the workpiece is not particularly limited, and may be a plate press or a roll press. In step (B), the method for pressing the workpiece is preferably a plate pressing method. In other words, in step (B), the workpiece is preferably sandwiched between two press plates and heated and pressed.

[0043] In step (B), the pressing device used when heating and pressing the workpiece is not particularly limited, but is preferably a vacuum laminating device. As the vacuum laminating device, for example, a diaphragm type laminator, a rubber press type laminator, or the like can be used. Specifically, examples of diaphragm-type laminators include CVP-300 (manufactured by Nikko Materials Co., Ltd.), MVLP-500 / 600-IIA (manufactured by Meiki Seisakusho Co., Ltd.), etc. Examples of rubber press-type laminators include CVP-600 (manufactured by Nikko Materials Co., Ltd.), CVP-700 (manufactured by Nikko Materials Co., Ltd.), etc.

[0044] [Cover film removal process (C)] The method for producing a laminate of the present embodiment preferably further includes, after the step (B), a step (C) of removing the cover film from the workpiece.

[0045] In step (C), the method for removing the cover film from the workpiece is not particularly limited, and examples thereof include a method for mechanically peeling the cover film from the workpiece; a method for chemically removing the cover film by dissolving the cover film in the workpiece with an organic solvent or the like; and the like. The method for mechanically peeling the cover film from the workpiece is preferred.

[0046] When the cover film is mechanically peeled off from the workpiece, the cover film may be peeled off from the workpiece by hand, or the cover film may be peeled off from the workpiece by a machine such as an automatic peeling machine.

[0047] [Other processes] The method for producing a laminate according to the present embodiment may include steps other than steps (A), (B) and (C).

[0048] As another example of the other step, there may be mentioned a step of heating and pressing the workpiece between the step (B) and the step (C). By further providing a step of heating and pressing the workpiece between steps (B) and (C), the embeddability can be further improved. In the step of heating and pressing the workpiece between step (B) and step (C), the degree of vacuum, the pressure when pressing the workpiece, the temperature of the workpiece, the pressing time, etc. may be appropriately set.

[0049] The other steps include, for example, a step of laminating another layer after step (C).

[0050] [Laminate] The laminate of this embodiment includes a substrate having a through hole and a first clad layer of an optical waveguide. The laminate of the present embodiment may further include other layers, and may be, for example, a laminate including a substrate, a first clad layer, and a base film in this order. In the laminate of this embodiment, the first clad layer is conceptually understood to include the resin layer (a).

[0051] The laminate of this embodiment is preferably an optoelectronic composite substrate further comprising a core layer and a second clad layer in this order on the first clad layer, i.e., the optoelectronic composite substrate comprises a substrate, a first clad layer, a core layer, and a second clad layer in this order. The optical / electrical composite substrate of this embodiment may further include a polyimide base material on the surface of the second cladding layer opposite to the core layer.

[0052] The optoelectronic composite substrate of this embodiment can be produced, for example, as follows. First, steps (A), (B) and (C) of this embodiment are carried out to obtain a laminate having a substrate, a first cladding layer and a base film in this order. Thereafter, the base film is peeled off from the laminate having the substrate, the first clad layer, and the base film in that order, and a film for forming a core layer is laminated to form the core layer, and then a film for forming a second clad layer is laminated to form the second clad layer. In addition, the method may appropriately include a step of forming a waveguide pattern in the core layer, a step of forming a mirror on the optical waveguide, and the like.

[0053] In the laminate of this embodiment, when the volume of the through hole formed in the substrate is taken as 100 volume %, from the viewpoint of further suppressing the propagation loss of the optical waveguide, it is preferable that 70 volume % or more of the through hole is filled with the resin composition for forming the first clad layer. The proportion of the resin composition for forming the first cladding layer filled in the through hole, when the volume of the through hole is taken as 100 volume%, from the viewpoint of further suppressing the propagation loss of the optical waveguide, is more preferably 75 volume% or more, even more preferably 80 volume% or more, even more preferably 85 volume% or more, even more preferably 90 volume% or more, even more preferably 95 volume% or more, even more preferably 98 volume% or more, even more preferably 99 volume% or more, and is, for example, 100 volume% or less. The resin composition for forming the first clad layer is a resin composition derived from the resin layer (a) of the film having the resin layer (a).

[0054] [Cover film] The cover film of this embodiment will be specifically described.

[0055] The cover film of the present embodiment is not particularly limited, but preferably includes at least one selected from the group consisting of a resin film and a metal film, and more preferably includes a resin film.

[0056] In the cover film of this embodiment, the resin constituting the resin film is not particularly limited, but from the viewpoint of further improving embeddability, it preferably contains at least one selected from the group consisting of polyethylene terephthalate, polypropylene, polybutylene terephthalate, polyethylene naphthalate, and polyimide, more preferably contains at least one selected from the group consisting of polyethylene terephthalate and polypropylene, and even more preferably contains polyethylene terephthalate. In the cover film of the present embodiment, the resin constituting the resin film preferably contains polypropylene, from the viewpoints of further improving embeddability and suppressing resin leakage.

[0057] In the cover film of this embodiment, the resin film may be subjected to a stretching treatment such as uniaxial stretching or biaxial stretching. The cover film of the present embodiment preferably contains a biaxially oriented polypropylene film from the viewpoints of further improving embeddability and suppressing resin leakage.

[0058] In the cover film of the present embodiment, the metal film may be, for example, a metal foil. The metal constituting the metal film is not particularly limited, and examples thereof include stainless steel, aluminum, and copper.

[0059] The layer structure of the cover film of the present embodiment is not particularly limited, and may be a single-layer film or a multi-layer film.

[0060] The storage modulus E' at 100°C of the cover film of this embodiment is, from the viewpoint of further suppressing the generation of voids in the through holes and further improving embeddability, preferably 0.10 GPa or more, more preferably 0.30 GPa or more, even more preferably 0.50 GPa or more, even more preferably 0.70 GPa or more, even more preferably 1.00 GPa or more, even more preferably 1.30 GPa or more, even more preferably 1.50 GPa or more, even more preferably 1.70 GPa or more, even more preferably 2.00 GPa or more, even more preferably 2.10 GPa or more, and even more preferably 2.20 GPa or more, and the upper limit is not particularly limited, and may be, for example, 5.00 GPa or less, 4.00 GPa or less, 3.00 GPa or less, or 2.50 GPa or less.

[0061] The storage modulus E' of the cover film of this embodiment at the temperature when pressed is, from the viewpoint of further suppressing the generation of voids in the through holes and further improving embeddability, preferably 0.03 GPa or more, more preferably 0.05 GPa or more, even more preferably 0.10 GPa or more, even more preferably 0.15 GPa or more, even more preferably 0.30 GPa or more, and even more preferably 0.50 GPa or more, and the upper limit is not particularly limited, but may be, for example, 1.00 GPa or less or 0.80 GPa or less. Here, the storage modulus E' at the temperature when pressing means the storage modulus E' at the temperature of the workpiece when the workpiece is pressed in step (B).

[0062] The present inventors consider that if the cover film of this embodiment is within the above-mentioned range of storage modulus E', when the workpiece is pressed in step (B), a suitable gap is more likely to be generated between the cover film and the substrate, and this gap becomes an air passage, so that the generation of voids in the through-hole can be suppressed and the embeddability is further improved. Note that, if the cover film of this embodiment has a storage modulus E' smaller than the preferable lower limit, the present inventors consider that in step (B), the cover film will excessively follow the substrate, making it difficult to generate a suitable gap between the cover film and the substrate. That is, the present inventors have found that the storage modulus E' of the cover film is an effective measure for further improving embeddability.

[0063] The storage modulus E' at 100°C of the cover film of this embodiment is, from the viewpoint of further improving embeddability and further suppressing resin leakage, preferably 0.10 GPa or more, more preferably 0.20 GPa or more, even more preferably 0.40 GPa or more, even more preferably 0.50 GPa or more, even more preferably 0.60 GPa or more, and even more preferably 0.70 GPa or more, and from the viewpoint of further improving embeddability and further suppressing resin leakage, preferably 2.00 GPa or less, more preferably 1.80 GPa or less, even more preferably 1.60 GPa or less, even more preferably 1.40 GPa or less, even more preferably 1.20 GPa or less, and even more preferably 1.00 GPa or less.

[0064] The storage modulus E' of the cover film of this embodiment at the temperature when pressed is preferably 0.10 GPa or more, more preferably 0.20 GPa or more, even more preferably 0.40 GPa or more, even more preferably 0.50 GPa or more, even more preferably 0.60 GPa or more, and even more preferably 0.70 GPa or more, from the viewpoint of further improving embeddability and suppressing resin leakage, and is preferably 2.00 GPa or less, more preferably 1.80 GPa or less, even more preferably 1.60 GPa or less, even more preferably 1.40 GPa or less, even more preferably 1.20 GPa or less, and even more preferably 1.00 GPa or less, from the viewpoint of further improving embeddability and suppressing resin leakage.

[0065] According to the study by the present inventors, it was found that if the storage modulus E' of the cover film is too large, the embeddability is improved, but resin leakage may occur depending on the conditions such as the hole diameter of the through hole. The present inventors have studied diligently and found that the measure of the storage modulus E' of the cover film is effective from the viewpoint of suppressing resin leakage. And, it was found that by setting the storage modulus E' of the cover film within the above numerical range, the embeddability can be improved and the resin leakage can be further suppressed.

[0066] From the viewpoint of further improving embeddability, the glass transition temperature Tg of the cover film of this embodiment is preferably 50°C or higher, more preferably 70°C or higher, even more preferably 80°C or higher, even more preferably 90°C or higher, and even more preferably 100°C or higher. The upper limit is not particularly limited, but may be, for example, 400°C or lower, 300°C or lower, or 200°C or lower. When the glass transition temperature Tg of the cover film of this embodiment is at least the above lower limit, the storage modulus E' at 100° C. and the storage modulus E' at the pressing temperature can be easily adjusted to preferred numerical ranges.

[0067] The loss modulus E'' at 100°C of the cover film of this embodiment is, from the viewpoint of further improving embeddability and further suppressing resin leakage, preferably 0.1 MPa or more, more preferably 0.5 MPa or more, even more preferably 1.0 MPa or more, even more preferably 5.0 MPa or more, and even more preferably 8.0 MPa or more, and from the viewpoint of further improving embeddability and further suppressing resin leakage, is preferably 100 MPa or less, more preferably 80 MPa or less, and even more preferably 50 MPa or less. The present inventors have found that, from the viewpoint of further improving embeddability and further suppressing resin leakage, a measure called the loss modulus E'' of the cover film is also effective.

[0068] The storage modulus E', loss modulus E'' and glass transition temperature Tg of the cover film of this embodiment refer to values ​​measured by the method described in the Examples. That is, the storage modulus E', loss modulus E'' and glass transition temperature Tg of the cover film of this embodiment refer to values ​​measured by heating from 30°C to 160°C using a dynamic viscoelasticity measuring device under conditions of air atmosphere, frequency: 1 Hz, mode: tensile mode, heating rate: 5°C / min, and amplitude: 5 μm.

[0069] The storage modulus E', loss modulus E'' and glass transition temperature Tg of the cover film of this embodiment can be set to the desired numerical range, for example, by using a resin film as the cover film and appropriately adjusting the type and content of the resin constituting the resin film.

[0070] From the viewpoint of further improving the handleability and embeddability of the cover film, the thickness of the cover film in this embodiment is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 20 μm or more, even more preferably 25 μm or more, even more preferably 30 μm or more, even more preferably 35 μm or more, and is preferably 200 μm or less, more preferably 190 μm or less, even more preferably 150 μm or less, even more preferably 100 μm or less, even more preferably 70 μm or less.

[0071] The cover film of the present embodiment may be surface-treated, for example, the surface of the cover film may be subjected to a release treatment. If the surface of the cover film is subjected to a release treatment, it is preferable because this makes it easier to peel the cover film from the work in step (C).

[0072] [Film having resin layer (a)] The film having the resin layer (a) made of a resin composition for forming the first clad layer of this embodiment will be specifically described.

[0073] From the viewpoint of further improving embeddability, the thickness of the resin layer (a) is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more, and from the viewpoint of further improving the light propagation efficiency of the optical waveguide, the thickness is preferably 200 μm or less, more preferably 150 μm or less, even more preferably 100 μm or less, even more preferably 80 μm or less, even more preferably 60 μm or less, even more preferably 40 μm or less, and even more preferably 30 μm or less.

[0074] The thickness of the resin layer (a) is preferably smaller than the thickness of the substrate. The thickness of the resin layer (a), when the thickness of the substrate is taken as 100%, is preferably 80% or less, more preferably 70% or less, even more preferably 60% or less, and even more preferably 55% or less, and may be, for example, 10% or more, or 15% or more.

[0075] Here, the thickness of the resin layer (a) in this specification means the thickness of the resin layer (a) in step (A). That is, in the method for producing a laminate of this embodiment, the work is pressed in step (B), but the thickness of the resin layer (a) in this specification does not mean the thickness after pressing.

[0076] There are no particular limitations on the resin constituting the resin layer (a), and it may be any resin that can be used to form a cladding layer of an optical waveguide. Examples of the resin constituting the resin layer (a) include norbornene-based resins, polyimide resins, compounds having a cyclic ether structure, and copolymers of styrene-based monomers and diene-based monomers.

[0077] The resin layer (a) may contain, in addition to the resin component, appropriate components such as a curing agent, an antioxidant, a surfactant, and the like.

[0078] The film having the resin layer (a) of this embodiment preferably further has a base film, and more preferably the resin layer (a) is provided on the base film. The base film may be, for example, a resin film. The resin constituting the base film is not particularly limited, but preferably contains at least one or more types selected from the group consisting of polyimide and polyethylene terephthalate, and more preferably contains polyethylene terephthalate.

[0079] From the viewpoint of further improving the handleability of the film, the thickness of the base film in this embodiment is preferably 10 μm or more, more preferably 15 μm or more, even more preferably 20 μm or more, preferably 30 μm or more, and is preferably 100 μm or less, more preferably 80 μm or less, even more preferably 60 μm or less, even more preferably 40 μm or less.

[0080] The substrate film of the present embodiment may be subjected to a surface treatment such as an antistatic treatment or a release treatment.

[0081] The film having the resin layer (a) of this embodiment can be obtained, for example, by applying a resin composition for forming the first clad layer onto a substrate film, drying it, and forming the resin layer (a). When applying the resin composition for forming the first clad layer onto the substrate film, the resin composition is preferably a varnish-like resin composition containing an organic solvent. The organic solvent in the resin composition is removed in the drying process. Examples of the coating method include direct coating methods using various coater devices such as a pin coater, a die coater, a comma coater, and a curtain coater, and printing methods such as screen printing.

[0082] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES

[0083] The present embodiment will be described in detail below based on examples, but the present embodiment is not limited to the descriptions of these examples.

[0084] [Preparation of film having resin layer (a)] First, a film having a resin layer (a) made of a resin composition for forming a first clad layer will be described. To 95.9 parts by mass (solid content) of Avatrel 2590 (Promerus, norbornene resin, 20 wt% 2-heptanone solution), 2.9 parts by mass of Curesol C11z (Shikoku Kasei, imidazole compound), 1.0 part by mass of Irganox 1076 (BASF, hindered phenol antioxidant), and 0.2 parts by mass of Irgafos 168 (BASF, phosphorus antioxidant) were added and mixed to obtain a coating liquid for forming a resin layer (a). This coating liquid for forming resin layer (a) was applied as a varnish using an applicator onto a 38 μm thick antistatic treated polyethylene terephthalate substrate (manufactured by Nippa Corporation, product name: PET38×1-TR1-ASQ, hereafter referred to as PET substrate) so that the dried thickness of the resin layer (a) would be 25 μm. The substrate was then dried at 45° C. for 15 minutes, and finally an OPP cover film (manufactured by Oji F-Tex Corporation, product name: E201F-50 μm) was attached to the surface of the resin layer (a) to obtain a film having a resin layer (a).

[0085] [Cover film] The cover film used in the examples will be described in detail below. The thickness, storage modulus E', glass transition temperature Tg, and loss modulus E'' of the cover film are shown in Table 1. Film 1 (PET film with silicone release treatment, manufactured by Mitsui Chemicals Tohcello Co., Ltd., product name: SP-PET38) Film 2 (multi-layer resin film, manufactured by Sumitomo Bakelite Co., Ltd., product name: SUMILITE CEL-E920C) Film 3 (OPP film, manufactured by Nippa Corporation, product name: OPP60×1J0) Film 4 (OPP film, manufactured by Oji F-Tex Co., Ltd., product name: Alphan E-201F) Film 5 (antistatic PET film, manufactured by Nippa Corporation, product name: PET38×1-TR1-ASQ) Film 6 (multi-layer resin film, manufactured by Sumitomo Bakelite Co., Ltd., product name: SUMILITE CEL-E911B) Film 7 (multi-layer resin film, manufactured by Sumitomo Bakelite Co., Ltd., product name: SUMILITE CEL-E915E)

[0086] [Examples 1 to 9] <Work preparation process (A)> First, a double-sided copper-clad laminate (CCL) with through holes was placed on the cover film. Next, the OPP cover film was peeled off from the film with the resin layer (a), and the double-sided copper-clad laminate and the resin layer (a) of the film with the resin layer (a) were in contact with each other to prepare a workpiece in which the cover film, the substrate, and the film with the resin layer (a) were layered in this order. The layer structure of the workpiece was "cover film / double-sided copper-clad laminate / resin layer (a) / PET substrate". The types of cover films are shown in Table 1. The thickness of the resin layer (a) of the film having the resin layer (a), the thickness T of the double-sided copper-clad laminate, the hole diameter R of the through hole, and T / R are also shown in Table 1.

[0087] <Laminating process (B)> Using the 1st stage of a diaphragm-type laminator (manufactured by Nikko Materials Co., Ltd., product name: CVP-300), the workpiece was pressed based on the conditions of step (B) in Table 1 to laminate the resin layer (a) onto the double-sided copper-clad laminate. The diaphragm-type laminator (manufactured by Nikko Materials Co., Ltd., product name: CVP-300) is a laminator equipped with a flattening stage as the second stage, but pressing was not performed using the second stage.

[0088] <Process (C) of removing the cover film> After step (B), the cover film was peeled off from the workpiece to obtain the laminates of Examples 1 to 9. The layer structure of the laminates of Examples 1 to 9 was "double-sided copper-clad laminate / first clad layer (resin layer (a)) / PET substrate."

[0089] [Measurement and Evaluation] <Storage modulus E', loss modulus E'' and glass transition temperature Tg of cover film> The cover film was heated from 30°C to 160°C under the conditions of air atmosphere (nitrogen: about 78%, oxygen: about 21%, argon: about 1%), frequency: 1Hz, mode: tensile mode, heating rate: 5°C / min, amplitude: 5μm, and the storage modulus E', loss modulus E'' and tanδ against temperature were measured using a dynamic viscoelasticity measuring device (manufactured by TA Instruments, product name: Q800). From the obtained storage modulus E', the storage modulus E' [GPa] at 100°C and the storage modulus E' [GPa] at 140°C of the cover film were calculated. Furthermore, the loss modulus E'' [MPa] at 100°C of the cover film was calculated. In addition, the glass transition temperature Tg [°C] of the cover film was calculated from the top peak of the obtained tanδ.

[0090] <Embeddability evaluation> For the laminates of Examples 1 to 9, the through holes of the substrate were observed using a microscope from the surface of the substrate opposite to the first cladding layer, and were evaluated according to the following criteria. A: The resin composition was able to fill the through-holes, and no voids remained in the through-holes. B: The through-holes are filled with the resin composition to a certain extent, but some voids remain in the through-holes. C: Many voids remain in the through hole.

[0091] <Resin leakage evaluation> The laminates of Examples 1 to 9 were observed in the same manner as in the embeddability evaluation, and were evaluated for resin leakage according to the following criteria. A: The resin composition does not protrude outside the through-hole. B: The resin composition protrudes to the outside of the through hole.

[0092] The results of the embeddability evaluation and the resin leakage evaluation are shown in Table 1.

[0093] [Table 1]

[0094] It can be seen from Table 1 that the laminate obtained by the manufacturing method of the example has a good embeddability evaluation. That is, according to the manufacturing method of the laminate of the present embodiment, a laminate that can produce an optoelectronic composite substrate with improved embeddability can be obtained.

[0095] Furthermore, when comparing Examples 3 to 9, which were all the same except for the type of cover film, the laminates obtained by the manufacturing methods of Examples 5 and 6 had good embeddability and resin leakage evaluations. That is, by adjusting the storage modulus E' to an appropriate range, a laminate can be obtained that can provide an optoelectronic composite substrate with improved embeddability and suppressed resin leakage. [Explanation of symbols]

[0096] 20 First cladding layer 30 Core Layer 40 Second Cladding Layer 50 Light emitting element side mirror 60 Mirror on the light receiving element side 100 optical waveguide 110 Substrate 120 Light emitting element 130 Photodetector 140a, 140b through hole 200 Photoelectric composite board 300 Film having resin layer (a) 310 Resin layer (a) 320 Base film 330 Cover Film 400 Work

Claims

1. A method for manufacturing a laminate including a substrate having a through hole and a first clad layer of an optical waveguide, comprising the steps of: A step (A) of preparing a workpiece by stacking a cover film, the substrate, and a film having a resin layer (a) made of a resin composition for forming the first clad layer in this order; and (B) laminating the first clad layer onto the substrate by heating and pressing the work.

2. The method for producing a laminate according to claim 1, wherein the cover film has a storage modulus E' at 100°C of 0.10 GPa or more.

3. The method for producing a laminate according to claim 2, wherein the cover film has a storage modulus E' at 100°C of 0.10 GPa or more and 2.00 GPa or less.

4. The method for producing a laminate according to claim 1 or 2, wherein the cover film has a loss modulus E'' at 100°C of 0.1 MPa or more and 100 MPa or less.

5. The method for producing a laminate according to claim 1 or 2, wherein the cover film includes at least one film selected from the group consisting of a resin film and a metal film.

6. The method for producing a laminate according to claim 5 , wherein the cover film includes a resin film.

7. The method for producing a laminate according to claim 6, wherein a resin constituting the resin film includes at least one selected from the group consisting of polyethylene terephthalate, polypropylene, polybutylene terephthalate, polyethylene naphthalate, and polyimide.

8. The method for producing a laminate according to claim 1 or 2, wherein the cover film has a thickness of 5 μm or more and 200 μm or less.

9. The method for producing a laminate according to claim 1 or 2, wherein in the step (B), the work is heated to 80° C. or more and 180° C. or less and pressed.

10. 3. The method for producing a laminate according to claim 1, wherein in the step (B), the work is pressed at a pressure of 0.1 MPa or more and 10.0 MPa or less.

11. 3. The method for producing a laminate according to claim 1, wherein in the step (B), the work is heated and pressed under reduced pressure using a vacuum laminator.

12. The method for producing a laminate according to claim 11, wherein the degree of vacuum in the step (B) is 500 Pa or less.

13. The method for producing a laminate according to claim 1 or 2, further comprising a step (C) of removing the cover film from the workpiece after the step (B).

14. 3. The method for producing a laminate according to claim 1, wherein when the thickness of the substrate is T [μm] and the hole diameter of the through hole is R [μm], T / R is 0.10 or more.

15. The method for producing a laminate according to claim 1 or 2, wherein the through holes have a hole diameter of 10 μm or more and 1000 μm or less.

16. The method for producing a laminate according to claim 1 or 2, wherein the thickness of the substrate is 10 μm or more and 500 μm or less.

17. The method for producing a laminate according to claim 1 or 2, wherein the resin layer (a) has a thickness of 10 μm or less and 200 μm or less.

18. The method for producing a laminate according to claim 1 or 2, wherein a thickness of the resin layer (a) is smaller than a thickness of the substrate.

19. 3. The method for producing a laminate according to claim 1, wherein, when the volume of the through hole is 100 volume %, 70 volume % or more of the through hole is filled with a resin composition for forming the first clad layer.

20. 3. The method for producing a laminate according to claim 1, wherein the laminate is an optical / electrical composite substrate further comprising a core layer and a second clad layer in this order on the first clad layer.

Citation Information

Patent Citations

  • Production of polyimide optical waveguide

    JP2000321455A

  • Optical and electrical wiring board and device for optical communication

    JP2006140233A

  • Photo-electric hybrid substrate

    JP2014238455A

Cited By

  • Thermally assisted magnetic recording and reproducing apparatus and method for adjusting same

    CN121641082A