Resin composition, cured product, resin film, prepreg, laminate, and printed wiring board
A resin composition with a specific copolymer structure addresses the high dielectric issues in conventional materials, achieving low dielectric constants, loss tangents, and improved dimensional stability for printed circuit boards.
Patent Information
- Application Number
- JP2024013227
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-01-31
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional resin compositions used in printed circuit boards have high dielectric constants and dielectric loss tangents, leading to limited information capacity and processing speed, and the addition of modifiers to reduce these properties results in deteriorated dimensional stability due to increased thermal expansion coefficients.
A resin composition comprising a copolymer of vinyl aromatic and conjugated diene compounds with specific molecular weights and structural configurations, along with a curing agent and radical initiator, to achieve low dielectric constants and loss tangents while maintaining small thermal expansion coefficients and excellent dimensional stability.
The resin composition provides printed circuit boards with low dielectric constants, low loss tangents, and improved dimensional stability, ensuring reduced warping and enhanced performance in electronic devices.
Smart Images

Figure 2024146752000001 
Figure 2024146752000002 
Figure 2024146752000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a cured product, a resin film, a prepreg, a laminate, and a printed wiring board. [Background technology]
[0002] 2. Description of the Related Art In recent years, with the remarkable progress in information network technology and the expansion of services utilizing information networks, electronic devices are required to have larger information capacities and faster processing speeds. In order to meet these demands, materials with low dielectric loss are required for various substrates such as printed circuit boards and flexible substrates.
[0003] 2. Description of the Related Art In order to obtain materials with small dielectric loss, resin cured products containing, as a main component, a thermosetting resin such as an epoxy resin, which has a low dielectric constant and a low dielectric tangent and excellent mechanical properties such as strength and heat resistance, or a thermoplastic resin such as a polyphenylene ether resin, have been studied and disclosed. However, the materials disclosed so far still have room for improvement in terms of low dielectric constant and low dielectric tangent, and when these materials are used in printed circuit boards, there is a problem that the amount of information and processing speed are limited.
[0004] To overcome these problems, various rubber components have been proposed as modifiers for the above-mentioned thermosetting resins and thermoplastic resins. For example, Patent Document 1 discloses at least one elastomer selected from the group consisting of block copolymers of vinyl aromatic compounds and olefin-based alkene compounds, hydrogenated products thereof, and homopolymers of vinyl aromatic compounds, as a modifier for lowering the dielectric tangent and dielectric constant of polyphenylene ether resin. Moreover, Patent Document 2 discloses a styrene-based elastomer as a modifier for lowering the dielectric tangent and dielectric constant of an epoxy resin. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2021-147486 [Patent Document 2] JP 2020-15861 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the resin compositions using the modifiers disclosed in Patent Documents 1 and 2 still do not have a sufficiently low dielectric constant and low dielectric loss tangent, and furthermore, the addition of the modifier deteriorates the coefficient of linear thermal expansion and reduces dimensional stability.
[0007] Therefore, an object of the present invention is to provide a resin composition which can give a cured product having a low dielectric constant, a low dielectric tangent, a small thermal expansion coefficient, and excellent dimensional stability, and to provide a cured product, a resin film, a prepreg, a laminate, and a printed wiring board which use the resin composition. [Means for solving the problem]
[0008] As a result of intensive research conducted by the present inventors in order to solve the problems of the conventional techniques described above, they have found that the above problems can be solved by a resin composition comprising copolymer (A) and copolymer (B), which are copolymers of a vinyl aromatic compound and a conjugated diene compound and have a predetermined structure, and at least one of a cured resin, a radical initiator, and a curing agent, and have thus completed the present invention. That is, the present invention is as follows.
[0009] [1] A copolymer (A) having vinyl aromatic monomer units and conjugated diene monomer units; a copolymer (B) having vinyl aromatic monomer units and conjugated diene monomer units; At least one component selected from the group consisting of the following components (I) to (III): Contains All of the following conditions (1) to (6) are met: Resin composition. Component (I): Cured resin (excluding copolymer (A) and copolymer (B)) Component (II): Radical initiator Component (III): Hardener (excluding component (I)) <Condition (1)>: The copolymer (A) has a number average molecular weight of 30,000 or less. <Condition (2)>: The copolymer (A) has at least one polymer block mainly composed of vinyl aromatic monomer units. <Condition (3)>: The copolymer (B) has at least one polymer block mainly composed of vinyl aromatic monomer units. <Condition (4)>: The copolymer (B) has a number average molecular weight of 50,000 or more. <Condition (5)>: The content (Sa) (mass%) of vinyl aromatic monomer units in the copolymer (A); The difference (ΔS) from the content (Sb) (mass %) of the vinyl aromatic monomer unit in the copolymer (B) satisfies the following relationship. ΔS=|Sa-Sb|≦25 <Condition (6)>: The average content of vinyl aromatic monomer units in the copolymer (A) and the copolymer (B) is 50% by mass or more. [2] The average hydrogenation rate (H) (%) of the unsaturated double bonds derived from the conjugated diene compound contained in the copolymer (A) and the copolymer (B) and the average vinyl bond amount (V) (%) are The resin composition according to [1] above, which satisfies the following relational formula: V+10≦H [3] The copolymer (B) is a block copolymer represented by any one of the following general structures: a1-b1-a2-c1, a1-b1-a2-b2, a1-c1-a2-c2, and a1-c1-a2-b1; the a1 block and the a2 block are polymer blocks mainly composed of vinyl aromatic monomer units, The b1 block and the b2 block are random polymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units, The c1 block and the c2 block are polymer blocks mainly composed of conjugated diene monomer units. The resin composition according to [1] or [2] above. [4] The resin composition according to any one of [1] to [3], wherein the ratio (Mnb / Mna) of the number average molecular weight (Mnb) of the copolymer (B) to the number average molecular weight (Mna) of the copolymer (A) is greater than 4. [5] The resin composition according to any one of [1] to [4] above, wherein the hydrogenation rate of the unsaturated double bonds derived from the conjugated diene in the copolymer (A) is 55% or more and 95% or less. [6] The resin composition according to any one of [1] to [5] above, wherein the hydrogenation rate of the unsaturated double bonds derived from the conjugated diene in the copolymer (B) is 55% or more and 95% or less. [7] The copolymer (A) is a block copolymer represented by the general structural formula: df, d is a polymer block mainly composed of vinyl aromatic monomer units, f is a polymer block mainly composed of conjugated diene monomer units; The resin composition according to any one of [1] to [6] above. [8] A cured product of the resin composition according to any one of [1] to [7] above. [9] A printed wiring board comprising the cured product according to [8] above.
[10] A resin film comprising the cured product described in [8].
[11] A substrate; The resin composition according to any one of [1] to [7] above, Prepreg is a composite material.
[12] A substrate; The cured product according to [8] above, Prepreg is a composite material.
[13] The prepreg according to
[11] above, wherein the base material is a glass cloth.
[14] The prepreg according to
[12] above, wherein the base material is a glass cloth.
[15] A cured product of the resin film according to
[10] above; Metal foil; A laminate having the following structure:
[16] A cured product of the prepreg according to
[11] above; Metal foil; A laminate having the following structure:
[17] A cured product of the prepreg according to
[12] above; Metal foil; A laminate having the following structure:
[18] A printed wiring board comprising the resin film according to
[10] above.
[19] A printed wiring board comprising the prepreg according to
[13] .
[20] A printed wiring board comprising the prepreg according to
[14] . Effect of the Invention
[0010] According to the present invention, a resin composition which gives a cured product having a low dielectric constant, a low dielectric dissipation factor, a small coefficient of linear thermal expansion, and excellent dimensional stability, a cured product using the resin composition, a resin film, a prepreg, a laminate, and a printed wiring board are obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention (hereinafter simply referred to as "the present embodiment") will be described in detail. It should be noted that the following embodiment is merely an example for explaining the present invention, and is not intended to limit the present invention to the following content, and the present invention can be implemented in various modified forms within the scope of its gist.
[0012] [Resin composition] The resin composition of the present embodiment is A copolymer (A) having vinyl aromatic monomer units and conjugated diene monomer units; a copolymer (B) having vinyl aromatic monomer units and conjugated diene monomer units; At least one component selected from the group consisting of the following components (I) to (III): and satisfies all of the following <Condition (1)> to <Condition (6)>. Component (I): Cured resin (excluding copolymer (A) and copolymer (B)) Component (II): Radical initiator Component (III): Hardener (excluding component (I)) <Condition (1)>: The copolymer (A) has a number average molecular weight of 30,000 or less. <Condition (2)>: The copolymer (A) has at least one polymer block mainly composed of vinyl aromatic monomer units. <Condition (3)>: The copolymer (B) has at least one polymer block mainly composed of vinyl aromatic monomer units. <Condition (4)>: The copolymer (B) has a number average molecular weight of 50,000 or more. <Condition (5)>: The content (Sa) (mass%) of vinyl aromatic monomer units in the copolymer (A); The difference (ΔS) from the content (Sb) (mass %) of the vinyl aromatic monomer unit in the copolymer (B) satisfies the following relationship. ΔS=|Sa-Sb|≦25 <Condition (6)>: The average content of vinyl aromatic monomer units in the copolymer (A) and the copolymer (B) is 50% by mass or more.
[0013] By virtue of having the above-described configuration, the resin composition of the present embodiment has a low dielectric constant and a low dielectric tangent, a small coefficient of linear thermal expansion, and is less likely to cause warping of a substrate during production, resulting in excellent dimensional stability. In this specification, when a polymerized monomer is incorporated into a constituent element of a polymer, it is referred to as a "monomer unit", and when it is in the form of a monomer before becoming a constituent element of a polymer, it is referred to as a "compound".
[0014] (Copolymer (A)) The thermosetting resin composition of the present embodiment contains a copolymer (A). The copolymer (A) is a copolymer having vinyl aromatic monomer units and conjugated diene monomer units. The copolymer (A) has a number average molecular weight (Mna) of 30,000 or less, and has at least one polymer block mainly composed of vinyl aromatic monomer units.
[0015] <Vinyl aromatic compounds> Examples of vinyl aromatic compounds forming the vinyl aromatic monomer units of the copolymer (A) include, but are not limited to, styrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylethylene, N,N-dimethyl-p-aminoethylstyrene, and N,N-diethyl-p-aminoethylstyrene. Among these, styrene, α-methylstyrene, and p-methylstyrene are preferred from the viewpoints of availability and productivity. These may be used alone or in combination of two or more.
[0016] <Conjugated diene compounds> The conjugated diene compound forming the conjugated diene monomer unit of the copolymer (A) may be any diolefin having a conjugated double bond, and may include, but is not limited to, 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, farnesene, and the like. Among these, 1,3-butadiene and isoprene are preferred from the viewpoints of availability and productivity. These may be used alone or in combination of two or more.
[0017] <Condition (1)> The number average molecular weight (Mna) of the copolymer (A) is 30,000 or less, preferably 5,000 or more and less than 30,000, and more preferably 5,000 or more and less than 25,000. When the number average molecular weight (Mna) of the copolymer (A) is 30,000 or less, the solubility of the copolymer (A) in the varnish tends to be good. The number average molecular weight (Mna) of the copolymer (A) can be measured by gel permeation chromatography (hereinafter referred to as GPC) using standard polystyrene as a calibration curve. Specifically, it can be measured by the method described in the examples below. The number average molecular weight (Mna) of the copolymer (A) can be controlled within the above numerical range by adjusting conditions such as the amount of monomer added and the amount of polymerization initiator added in the polymerization step.
[0018] <Condition (2)> The copolymer (A) has at least one polymer block mainly composed of vinyl aromatic monomer units. When the copolymer (A) has at least one polymer block mainly composed of vinyl aromatic monomer units, the solubility of the copolymer (A) in varnish tends to be improved.
[0019] In this specification, the term "mainly composed of" means that the target monomer unit is contained in the target polymer block at more than 70 mass% and no greater than 100 mass%, preferably at least 80 mass% and no greater than 100 mass%, and more preferably at least 90 mass% and no greater than 100 mass%. In this specification, the "amount of vinyl bonds" means the proportion of 1,2-bonds and 3,4-bonds among the 1,2-bonds, 3,4-bonds and 1,4-bonds incorporated in the conjugated diene before hydrogenation. The amount of vinyl bonds can be measured by nuclear magnetic resonance spectroscopy (NMR). The amount of vinyl bonds can be arbitrarily controlled by using a polar compound or the like, which will be described later.
[0020] In the copolymer (A), the content (BSa) of polymer blocks mainly composed of vinyl aromatic monomer units is preferably 10 mass % or more, more preferably 15 mass % or more, and even more preferably 20 mass % or more. When the content (BSa) of the polymer block mainly composed of vinyl aromatic monomer units in the copolymer (A) is 10 mass % or more, the solubility of the copolymer (A) in the varnish tends to be improved. The content of the polymer block mainly composed of vinyl aromatic monomer units can be measured by NMR, specifically, by the method described in the examples below. The content (BSa) of the polymer block mainly composed of vinyl aromatic monomer units in the copolymer (A) can be controlled within the above numerical range by adjusting the amount of monomer added in the polymerization step, the timing of addition, the polymerization time, etc.
[0021] The structure of the copolymer (A) is not limited, but it is preferable that the copolymer (A) has a structure represented by the following general formula, for example. de df (de) n (df) n ded dfd ef def df (de) m -Z (df) m -Z (def) m -Z (dfe) m -Z In the above formula, d, e, and f represent polymer blocks (d), (e), and (f), respectively. However, from the perspective of productivity, (de) n , (df) n is preferred, and de and df are more preferred. Moreover, from the viewpoint of the crack resistance of the resin composition of the present embodiment, it is more preferable that the copolymer (A) is df. When the copolymer (A) is df, the toughness of the resin composition of the present embodiment tends to be improved, and the crack resistance tends to be good. The copolymer (A) may be a mixture containing a plurality of types of structures represented by the above general formula in any ratio.
[0022] In each of the general formulae representing the copolymer (A) described above, d is a polymer block mainly composed of vinyl aromatic monomer units, e is a random copolymer block composed of vinyl aromatic monomer units and conjugated diene monomer units, and f is a polymer block mainly composed of conjugated diene monomer units. n is an integer of 1 or more, preferably an integer of 1 to 10, and more preferably an integer of 1 to 5. m is an integer of 2 or more, preferably an integer of 2-11, and more preferably an integer of 2-8. Z represents a coupling agent residue. Here, the coupling agent residue means a residue remaining after bonding of the coupling agent used for bonding between the polymer blocks (e) and between the polymer blocks (f). The coupling agent is not limited to the following, but examples thereof include polyhalogen compounds and acid esters, which will be described later.
[0023] The vinyl aromatic monomer units in the polymer block (e) may be distributed uniformly or in a tapered manner. Furthermore, the vinyl aromatic monomer units may have a plurality of uniformly distributed portions and / or a plurality of taperedly distributed portions. Furthermore, the polymer block (f) may have a plurality of portions with different contents of the vinyl aromatic monomer units.
[0024] The hydrogenation rate of the double bonds derived from the conjugated diene monomer units in the copolymer (A) is preferably 55% or more, more preferably 60% or more, and even more preferably 65% or more. If the hydrogenation rate of the double bonds derived from the conjugated diene monomer units in the copolymer (A) is 55% or more, the reactivity of the cured resin with the copolymer (A) can be controlled, and the solder heat resistance of the resin composition of this embodiment tends to be improved. The hydrogenation rate of the double bonds derived from the conjugated diene monomer units in the copolymer (A) is preferably 95% or less, more preferably 90% or less, and even more preferably 85% or less. If the hydrogenation rate of the double bonds derived from the conjugated diene monomer units in the copolymer (A) is 95% or less, the crosslinkability of the copolymer (A) is improved, and the solder heat resistance of the resin composition of this embodiment tends to be improved. The hydrogenation rate of the double bonds derived from the conjugated diene monomer units in the copolymer (A) can be measured by NMR, specifically, by the method described in the examples below. The hydrogenation rate of the double bonds derived from the conjugated diene monomer units in the copolymer (A) can be controlled within the above numerical range by adjusting the type and amount of hydrogenation catalyst, the amount of hydrogenation, and the hydrogenation time.
[0025] (Copolymer (B)) The copolymer (B) is a copolymer having vinyl aromatic monomer units and conjugated diene monomer units. The copolymer (B) has at least one polymer block mainly composed of vinyl aromatic monomer units and has a number average molecular weight (Mnb) of 50,000 or more.
[0026] <Vinyl aromatic compounds> Examples of vinyl aromatic compounds forming the vinyl aromatic monomer units constituting the copolymer (B) include, but are not limited to, styrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylethylene, N,N-dimethyl-p-aminoethylstyrene, and N,N-diethyl-p-aminoethylstyrene. Among these, styrene, α-methylstyrene, and p-methylstyrene are preferred from the viewpoints of availability and productivity. These may be used alone or in combination of two or more.
[0027] <Conjugated diene compounds> The conjugated diene compound forming the conjugated diene monomer units constituting the copolymer (B) may be any diolefin having a conjugated double bond, and examples thereof include, but are not limited to, 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, farnesene, and the like. Among these, 1,3-butadiene and isoprene are preferred from the viewpoints of availability and productivity. These may be used alone or in combination of two or more.
[0028] The copolymer (B) has at least one polymer block mainly composed of vinyl aromatic monomer units. When the copolymer (B) has a polymer block mainly composed of vinyl aromatic monomer units, the solubility of the copolymer (B) in the varnish tends to be improved.
[0029] In the copolymer (B), the content (BSb) of polymer blocks mainly composed of vinyl aromatic monomer units is preferably 10 mass % or more, more preferably 15 mass % or more, and even more preferably 20 mass % or more. When the content (BSb) of the polymer block mainly composed of vinyl aromatic monomer units in the copolymer (B) is 10 mass % or more, the solubility of the copolymer (B) in varnish tends to be improved. The content of the polymer block mainly composed of vinyl aromatic monomer units can be measured by NMR, specifically, by the method described in the examples below. The content (BSb) of the polymer block mainly composed of vinyl aromatic monomer units in the copolymer (B) can be controlled within the above numerical range by adjusting the amount of monomer added in the polymerization step, the timing of addition, the polymerization time, etc.
[0030] The number average molecular weight (Mnb) of the copolymer (B) is 50,000 or more, preferably 60,000 or more, more preferably 80,000 or more, and even more preferably 100,000 or more. By containing the copolymer (A) and the copolymer (B) in the resin composition of this embodiment, the low dielectric constant and low dielectric loss tangent of the resin composition of this embodiment tend to be improved. On the other hand, the thermal expansion coefficients of the copolymer (A) and the copolymer (B) are higher than the thermal expansion coefficient of the cured resin. By making the number average molecular weight (Mnb) of the copolymer (B) 50,000 or more, the increase in the linear thermal expansion coefficient of the resin composition due to the addition of the copolymer (B) can be suppressed, which is preferable from the viewpoint of dimensional stability. In other words, the addition of such a copolymer (B) tends to improve the balance between dimensional stability and dielectric performance. The upper limit of the number average molecular weight (Mnb) of the copolymer (B) is preferably 500,000 or less, more preferably 300,000 or less, and even more preferably 200,000 or less, from the viewpoint of productivity. The number average molecular weight (Mnb) of the copolymer (B) can be measured by GPC. The number average molecular weight (Mnb) of the copolymer (B) can be controlled within the above-mentioned range by adjusting conditions such as the amount of monomer added in the polymerization step and the amount of polymerization initiator added.
[0031] The copolymer (B) is not limited to the following, but for example, it is preferable that it has a structure represented by the following general formula. (a1-b1) o (a1-c1) o a1-b1-a2 a1-c1-a2 a1-b1-c1 a1-b1-b2 a1-c1-c2 a1-c1-b1 a1-b1-c1-a2 a1-c1-b1-a2 a1-b1-c1-b2 a1-b1-a2-b2 a1-b1-a2-c1 a1-c1-a2-b1 a1-c1-a2-c2 [(a1-b1) o ]pZ [(a1-c1) o ]pZ (a1-b1-c1) p -Z (a1-c1-b1) p -Z
[0032] It is further preferred that the copolymer (B) is a block copolymer represented by any one of the general structures: a1-b1-a2-c1, a1-b1-a2-b2, a1-c1-a2-c2, and a1-c1-a2-b1. When copolymer (B) is a block copolymer represented by any one of the general structures: a1-b1-a2-c1, a1-b1-a2-b2, a1-c1-a2-c2, and a1-c1-a2-b1, the resin composition of this embodiment tends to have excellent copper adhesion. In the above formula, a1, a2, b1, b2, c1, and c2 represent polymer blocks (a1), (a2), (b1), (b2), (c1), and (c2), respectively. o is an integer of 1 or more, preferably an integer of 1 to 10, and more preferably an integer of 1 to 5. p is an integer of 2 or more, preferably an integer of 2 to 11, and more preferably an integer of 2 to 8. Z represents a coupling agent residue. Here, the coupling agent residue means a residue of a coupling agent used for bonding between polymer blocks (b) and between polymer blocks (c) after bonding.
[0033] The copolymer (B) is preferably one polymerized by sequential polymerization. "Polymerized by sequential polymerization" means that the copolymer is sequentially polymerized from one end of the final target polymer structure to the other end, without using a coupling reaction. It is preferable that the copolymer (B) does not contain any coupling agent residue, which can prevent unintended inclusion of uncoupled substances, etc.
[0034] The vinyl aromatic monomer units in the polymer block (b) may be distributed uniformly or in a tapered shape. Furthermore, the vinyl aromatic monomer units may have a plurality of uniformly distributed portions and / or a plurality of taperedly distributed portions. Furthermore, the polymer block (b) may have a plurality of portions with different contents of the vinyl aromatic monomer units.
[0035] In each of the general formulas representing the copolymer (B) described above, (a1) and (a2) are polymer blocks mainly composed of vinyl aromatic monomer units. (b1) and (b2) are random copolymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units. (c1) and (c2) are polymer blocks mainly composed of conjugated diene monomer units.
[0036] The hydrogenation rate (also referred to as hydrogenation ratio) of double bonds derived from conjugated diene monomer units in the copolymer (B) is preferably 55% or more, more preferably 60% or more, and even more preferably 65% or more. When the hydrogenation rate of the double bonds derived from the conjugated diene monomer units in the copolymer (B) is 55% or more, the reactivity of the component (I): the cured resin with the copolymer (B) can be controlled, and the solder heat resistance of the resin composition of this embodiment tends to be improved. The hydrogenation rate of the double bonds derived from the conjugated diene monomer units in the copolymer (B) is preferably 95% or less, more preferably 90% or less, and even more preferably 85% or less. When the hydrogenation rate of the double bonds derived from the conjugated diene monomer units in the copolymer (B) is 95% or less, the crosslinkability of the copolymer (B) is improved, and the solder heat resistance of the resin composition of this embodiment tends to be improved. The hydrogenation rate of the double bonds derived from the conjugated diene monomer units in the copolymer (B) can be measured by NMR, specifically, by the method described in the examples below. The hydrogenation rate of the double bonds derived from the conjugated diene monomer units in the copolymer (B) can be controlled within the above numerical range by adjusting the type and amount of hydrogenation catalyst, the amount of hydrogenation, and the hydrogenation time.
[0037] (Relationship between the contents of vinyl aromatic monomer units in copolymer (A) and copolymer (B)) <Condition (5)> In the resin composition of the present embodiment, the difference (ΔS) between the content (Sa) (mass%) of the vinyl aromatic monomer unit in the copolymer (A) and the content (Sb) (mass%) of the vinyl aromatic monomer unit in the copolymer (B) satisfies the following relationship. ΔS=|Sa-Sb|≦25 Moreover, ΔS is preferably 20 or less, and more preferably 15 or less. When the ΔS satisfies the above relational expression, the solubility of the copolymer (A) and the copolymer (B) in the varnish can be ensured. Since copolymer (B) has a relatively high molecular weight, it may be difficult to dissolve in varnish by itself depending on its molecular weight and structure, but by setting ΔS to a small value, it is possible to prevent the copolymer (B) from being difficult to dissolve in varnish. This is because copolymer (A) has a low molecular weight and tends to be highly soluble in varnish, and by satisfying |Sa-Sb|≦25 and improving the compatibility of copolymer (A) and copolymer (B), copolymer (A) acts like a compatibilizer and contributes to increasing the solubility of copolymer (B) in varnish. ΔS can be controlled within the above-mentioned numerical range by adjusting the amount of monomer added and the polymerization time in the polymerization step of copolymer (A) and copolymer (B).
[0038] (Relationship between number average molecular weights of copolymer (A) and copolymer (B)) The ratio (Mnb / Mna) of the number average molecular weight (Mnb) of the copolymer (B) to the number average molecular weight (Mna) of the copolymer (A) is preferably greater than 4, more preferably 5 or more, and even more preferably 6 or more. When (Mnb / Mna) is 4 or more, the resin composition of this embodiment tends to have a decreased coefficient of linear thermal expansion and improved dimensional stability.
[0039] (Content of vinyl aromatic monomer units in copolymer (A) and copolymer (B)) <Condition (6)> The average content of vinyl aromatic monomer units in the copolymer (A) and the copolymer (B) is 50% by mass or more, preferably 50% by mass to 90% by mass, more preferably 50% by mass to 85% by mass, even more preferably 55% by mass to 85% by mass, and even more preferably 60% by mass to 80% by mass. When the average content of the vinyl aromatic monomer unit in the copolymer (A) and the copolymer (B) is 50 mass% or more, the resin composition of the present embodiment tends to have improved solubility in varnish. In particular, when the resin composition of the present embodiment is made into a cured resin composition, even if maleimide is used as the cured resin (component (I)), the solubility in varnish is improved, so that a resin composition with excellent dimensional stability tends to be obtained. The vinyl aromatic monomer unit contents of the copolymer (A) and the copolymer (B) may be the same or different. If they are different, the contents of the vinyl aromatic monomer units of the copolymer (A) and the copolymer (B) may be set so that the vinyl aromatic monomer unit content (average vinyl aromatic monomer unit content) of the copolymer (A) and the copolymer (B) combined is 50% by mass or more, and the vinyl aromatic monomer unit contents of both polymers may be set so that the weighted average taking into account the molecular weight and the mixing ratio is 50% by mass or more. From the viewpoint of enhancing the compatibility of the two copolymers, it is preferable that the differences in the vinyl aromatic monomer unit content, vinyl bond amount and hydrogenation rate between the copolymer (A) and the copolymer (B) are small. The average content of the vinyl aromatic monomer units in the copolymer (A) and the copolymer (B) can be controlled within the above-mentioned numerical range by adjusting the amount of the monomer added in the polymerization process of the copolymer (A) and the copolymer (B).
[0040] (Amount of vinyl bonds in copolymer (A) and copolymer (B)) The vinyl bond content (V) of the conjugated diene monomer units of the copolymer (A) and the copolymer (B) is preferably 20% or more, more preferably 30% or more, and even more preferably 40% or more. When the vinyl bond content (V) of the conjugated diene monomer units of the copolymer (A) and the copolymer (B) is 20% or more, the resin composition of the present embodiment tends to have improved copper adhesion.
[0041] The vinyl bond content (V) of the conjugated diene monomer units of the copolymer (A) and the copolymer (B) is preferably 85% or less, more preferably 75% or less, and even more preferably 65% or less. When the vinyl bond amount (V) of the conjugated diene monomer units of the copolymer (A) and the copolymer (B) is 85% or less, the resin composition of the present embodiment tends to have excellent long-term storage stability. The vinyl bond amounts of the copolymers (A) and (B) may be the same or different. When they are different, the vinyl bond amounts of the two polymers may be set so that the combined state of the copolymers (A) and (B) has a preferable vinyl bond amount.
[0042] (Average vinyl bond content (V) and average hydrogenation ratio (H) of copolymer (A) and copolymer (B)) The copolymers (A) and (B) are preferably hydrogenated copolymers, and it is preferable that the average hydrogenation rate (H) (%) of the unsaturated double bonds derived from the conjugated diene compound contained in the copolymers and the average vinyl bond amount (V) (%) of the conjugated diene monomer units contained in the copolymers (A) and (B) satisfy the following relational formula: V+10≦H Here, the average hydrogenation ratio (H) refers to the average hydrogenation ratio of the copolymer (A) and the copolymer (B), and can be calculated from the results of NMR measurement according to the following formula. Average hydrogenation ratio (H) = (hydrogenation ratio of copolymer (A)) x (mass ratio of copolymer (A)) + (hydrogenation ratio of copolymer (B)) x (mass ratio of copolymer (B)) The average vinyl bond content (V) is the average vinyl bond content of the copolymer (A) and the copolymer (B), and can be calculated from NMR measurement according to the following formula. Average vinyl bond content (V) = (vinyl bond content of copolymer (A)) x (mass ratio of copolymer (A)) + (vinyl bond content of copolymer (B)) x (mass ratio of copolymer (B)) When the average hydrogenation ratio (H) of the copolymer (A) and the copolymer (B) satisfies the above formula, the resin composition of the present embodiment tends to have excellent long-term storage stability.
[0043] The average hydrogenation ratio (H) of the copolymer (A) and the copolymer (B) can be controlled, for example, by the amount of catalyst used during hydrogenation, and the hydrogenation rate can be controlled, for example, by the amount of catalyst used during hydrogenation, the amount of hydrogen feed, the pressure, the temperature, etc. The average hydrogenation ratio (H) of the copolymer (A) and the copolymer (B) can be measured by a nuclear magnetic resonance (NMR) spectrometer. The average vinyl bond content (V) of the copolymer (A) and the copolymer (B) can be controlled by, for example, the amount of the tertiary amine compound or the ether compound added, or the polymerization temperature. The average vinyl bond content (V) of the copolymer (A) and the copolymer (B) can be measured by a nuclear magnetic resonance (NMR) spectrometer.
[0044] When the copolymer (A) or (B) has a random copolymer block of a vinyl aromatic monomer unit and a conjugated diene monomer unit, the mass ratio (RS) of the vinyl aromatic monomer unit contained in the random copolymer block is preferably 70 mass% or less, more preferably 65 mass% or less, and even more preferably 60 mass% or less. When the mass ratio (RS) of the vinyl aromatic monomer unit contained in the random copolymer block of the copolymer (A) or the copolymer (B) is 70 mass% or less, the copolymer having a random copolymer block, the resin composition containing the copolymer, and the cured product thereof tend to have excellent copper adhesion.
[0045] (Relationship between molecular weights of polymer blocks mainly composed of vinyl aromatic monomer units in copolymers (A) and (B)) The ratio (MnS1 / MnS2) of the molecular weight (MnS1) of the polymer block mainly composed of vinyl aromatic monomer units in copolymer (A) to the molecular weight (MnS2) of the polymer block mainly composed of vinyl aromatic monomer units in copolymer (B) is preferably 0.9 or less, more preferably 0.8 or less, and even more preferably 0.7 or less. When (MnS1 / MnS2) is 0.9 or less, the resin composition of the present embodiment tends to have excellent copper adhesion. Incidentally, (MnS1) and (MnS2) can be controlled by adjusting the amount of monomer added during polymerization. MnS1 and MnS2 are calculated by the following method. MnS1 = Mn1 × BS1 MnS2 = Mn2 × BS2 ÷ f BS1: Proton nuclear magnetic resonance ( 1 The content (mass%) of the polymer block mainly composed of vinyl aromatic monomer units in the copolymer (A) determined by H-NMR BS2: Proton nuclear magnetic resonance ( 1 The content (mass%) of the polymer block mainly composed of vinyl aromatic monomer units in the copolymer (B) determined by H-NMR f: Degree of branching of copolymer (B) determined by GPC-light scattering method with a viscometer (Mn1) and (Mn2) can be measured by GPC using standard polystyrene as a calibration curve. (BS1) and (BS2) can be measured by NMR. (f) can be measured by a GPC-light scattering method equipped with a viscosity detector. The specific measurement method will be described later.
[0046] The method for measuring the mass proportions (RS1) and (RS2) of the vinyl aromatic monomer units in the random polymer blocks and the contents (BS1) and (BS2) of the polymer blocks mainly composed of vinyl aromatic monomer units will be specifically described by applying the NMR method, taking as an example a case in which the vinyl aromatic compound is styrene and the conjugated diene compound is 1,3-butadiene. Using samples prepared by dissolving 30 mg of copolymer (A) and copolymer (B) in 1 g of deuterated chloroform, 1 H-NMR was measured, and the content (BS) of the polymer block mainly composed of vinyl aromatic monomer units (styrene block in this case) was calculated from the ratio of the integrated value of the chemical shift from 6.9 ppm to 6.3 ppm to the total integrated value. Styrene block strength (b-St strength) = (integrated value of 6.9 ppm to 6.3 ppm) / 2 Random styrene strength (r-St strength) = (integrated value of 7.5 ppm to 6.9 ppm) - 3 × (b-St) Ethylene-butylene strength (EB strength) = Total integrated value - 3 x {(b-St intensity) + (r-St intensity)} / 8 Styrene block content (BS) =104×(b-St strength) / [104×{(b-St strength)+(r-St strength)}+56×(EB strength)] Mass fraction of styrene in random polymer block (RS) =104×(r-St strength) / {104×(r-St strength)+56×(EB strength)}
[0047] (Degree of branching (f) of copolymer (B)) The branching degree (f) of the copolymer (B) can be measured by a GPC-light scattering method equipped with a viscosity detector. Using the copolymer (B) as a sample, carry out GPC-light scattering measurement with a viscosity detector, and based on the standard polystyrene, determine the absolute molecular weight (M) from the results of the light scattering detector and RI detector, and the intrinsic viscosity ([η]) from the results of the RI detector and viscosity detector. Next, the reference intrinsic viscosity ([η]0) is calculated by the following formula. [η]0=a×M b a = -0.788 + 0.421 × (content of vinyl aromatic monomer units in copolymer (B)) -0.342×(RS2)-0.197×(BS2) b = 1.601 - 0.081 x (content of vinyl aromatic monomer units in copolymer (B)) +0.064×(RS2)+0.039×(BS2) RS2: Mass ratio of vinyl aromatic monomer units in the random polymer block of copolymer (B) BS2: Proton nuclear magnetic resonance ( 1 The content of polymer blocks mainly composed of vinyl aromatic monomer units in copolymer (B) determined by H-NMR M: Absolute molecular weight of copolymer (B) Next, the shrinkage factor g is calculated as the ratio of the intrinsic viscosity ([η]) of the copolymer (B) to the reference intrinsic viscosity ([η]0). Shrinkage factor (g)=[η] / [η]0 The resulting shrinkage factor (g) is then used to calculate the branching degree (f), which is defined as g=f / [(f+1)(f+2)] (f≧2).
[0048] (Method for Producing Copolymer (A) and Copolymer (B)) Examples of methods for producing the copolymer (A) and the copolymer (B) include, but are not limited to, methods described in JP-B-36-19286, JP-B-43-17979, JP-B-46-32415, JP-B-49-36957, JP-B-48-2423, JP-B-48-4106, JP-B-51-49567, and JP-A-59-166518.
[0049] Examples of the production method of copolymer (A) and copolymer (B) include, but are not limited to, (1) a method of solution polymerizing copolymer (A) and copolymer (B) respectively and mixing the solutions containing the polymers, (2) a method of removing the solvent and catalyst from copolymer (A) and copolymer (B) respectively and then mixing them, (3) a method of adding a polymerization initiator in two stages during the polymerization reaction, (4) a method of adding a protic reagent such as alcohol as a modifier or polymerization terminator that reacts with the living terminals during the polymerization reaction in a molar amount that is insufficient relative to the living terminals to terminate the reaction of some of the living terminals, and (5) a method of adding a protic reagent such as alcohol as a modifier or polymerization terminator in an equimolar amount to the living terminals after the polymerization reaction to terminate the reaction of all living terminals, and then adding a new polymerization initiator and monomer to the solution to carry out polymerization. In the method (1), either of the following methods can be applied: a method in which the polymerization solutions of copolymer (A) and copolymer (B) before the hydrogenation reaction are mixed and then the hydrogenation reaction is carried out, or a method in which the solutions of copolymer (A) and copolymer (B) are mixed after the respective hydrogenation reactions are carried out. The mixing ratio of copolymer (A) and copolymer (B) can be controlled by adjusting the concentration of each polymerization solution and the mixing amount of the solutions. In the method (3), the mixing ratio of the copolymer (A) and the copolymer (B) can be arbitrarily controlled by adjusting the feed rates of the vinyl aromatic compound and the conjugated diene compound, the amount of the polymerization initiator added in two stages, the timing of the second stage addition of the polymerization initiator, etc. In the method (4) above, the mixing ratio and structure of the copolymer (A) and the copolymer (B) can be arbitrarily controlled by adjusting the feed rate and feed composition of the vinyl aromatic compound and the conjugated diene compound, the amount of the modifier or polymerization terminator added midway and the timing of addition, etc. The copolymer (A) has a low molecular weight and is less entangled in molecules, so that mixing it before desolvation as in the above methods (1), (3), (4), and (5) enables the desolvation and finishing process to be carried out at a high rate. The methods (3) and (4) can simultaneously produce the copolymer (A) and the copolymer (B), and can reduce the number of production steps compared to the case where the copolymer (A) and the copolymer (B) are produced separately, thereby improving production efficiency.
[0050] In the case of producing a styrene-butadiene copolymer by batch polymerization using a tank-type reactor equipped with a stirrer and a jacket, when the block structures of copolymer (A) are de and copolymer (B) are a1-b-a2-c, it is preferable that the c block and the e block have the same structure and the same molecular weight, the a2 block and the d block are preferably composed of the same vinyl aromatic compound, and the molecular weight of the a2 block is preferably larger than the molecular weight of the d block. Furthermore, when polymerization is carried out by the above method (3), the timing of adding the second-stage initiator depends on the ratio of the molecular weights of the a2 block and the d block, and it is preferable to add the initiator at a timing when the polymerization conversion rate of the vinyl aromatic compound in the a2 block reaches 100 × (molecular weight of the d block) / (molecular weight of the a2 block) (%).
[0051] <Classification of copolymer (A) and copolymer (B)> The resin composition of the present embodiment contains two components, copolymer (A) and copolymer (B), and therefore has two or more peaks in its GPC chart. Among these, copolymer (A) refers to all components having a number average molecular weight of 30,000 or less.
[0052] The copolymer before hydrogenation can be obtained, for example, by a method of carrying out living anionic polymerization using a predetermined monomer in a hydrocarbon solvent using a polymerization initiator such as an organic alkali metal compound, but is not limited to the following. The hydrocarbon solvent is not particularly limited, and examples thereof include aliphatic hydrocarbons such as n-butane, isobutane, n-pentane, n-hexane, n-heptane, and n-octane; alicyclic hydrocarbons such as cyclohexane, cycloheptane, and methylcycloheptane; and aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene.
[0053] As the polymerization initiator, an organic alkali metal compound that is generally known to have anionic polymerization activity toward conjugated diene compounds and vinyl aromatic compounds can be used. For example, there may be mentioned an aliphatic hydrocarbon alkali metal compound having 1 to 20 carbon atoms, an aromatic hydrocarbon alkali metal compound having 1 to 20 carbon atoms, an organic amino alkali metal compound having 1 to 20 carbon atoms, and the like. The alkali metal contained in the polymerization initiator is not limited to the following, but examples thereof include lithium, sodium, and potassium. One or more types of alkali metals may be contained in one molecule. Examples of the polymerization initiator include, but are not limited to, n-propyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, n-pentyllithium, n-hexyllithium, benzyllithium, phenyllithium, tolyllithium, a reaction product of diisopropenylbenzene and sec-butyllithium, and a reaction product of divinylbenzene, sec-butyllithium, and a small amount of 1,3-butadiene. Furthermore, 1-(t-butoxy)propyllithium disclosed in U.S. Patent No. 5,708,092 and lithium compounds into which one or several molecules of an isoprene monomer have been inserted to improve the solubility thereof, siloxy group-containing alkyllithiums such as 1-(t-butyldimethylsiloxy)hexyllithium disclosed in British Patent No. 2,241,239, amino group-containing alkyllithiums disclosed in U.S. Patent No. 5,527,753, diisopropylamide lithium, hexamethyldisilazide lithium and other aminolithiums can also be used.
[0054] The amount of the lithium compound used as a polymerization initiator depends on the molecular weight of the desired copolymer, but is preferably 0.005 to 6.4 phm (parts by mass per 100 parts by mass of monomer), and more preferably 0.005 to 2.6 phm.
[0055] When a conjugated diene compound and a vinyl aromatic compound are copolymerized using an organic alkali metal compound as a polymerization initiator, a tertiary amine compound or an ether compound can be added in order to adjust the content of vinyl bonds (1,2-bonds or 3,4-bonds) in the conjugated diene monomer units incorporated into the copolymer and to adjust the random copolymerizability of the conjugated diene compound and the vinyl aromatic compound.
[0056] The tertiary amine compound is not particularly limited, but examples thereof include compounds represented by the following formula: R1R2R3N (In the formula, R1, R2, and R3 are a hydrocarbon group having 1 to 20 carbon atoms or a hydrocarbon group having a tertiary amino group.) Examples of such compounds include, but are not limited to, trimethylamine, triethylamine, tributylamine, N,N-dimethylaniline, N-ethylpiperidine, N-methylpyrrolidine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetraethylethylenediamine, 1,2-dipiperidinoethane, trimethylaminoethylpiperazine, N,N,N',N'',N''-pentamethylethylenetriamine, N,N'-dioctyl-p-phenylenediamine, etc. Among these, N,N,N',N'-tetramethylethylenediamine is preferred.
[0057] As the ether compound, a linear ether compound or a cyclic ether compound can be used. Examples of the linear ether compound include dialkyl ether compounds of ethylene glycol, such as dimethyl ether, diethyl ether, diphenyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and ethylene glycol dibutyl ether; and dialkyl ether compounds of diethylene glycol, such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, and diethylene glycol dibutyl ether. Examples of cyclic ether compounds include tetrahydrofuran, dioxane, 2,5-dimethyloxolane, 2,2,5,5-tetramethyloxolane, 2,2-bis(2-oxolanyl)propane, and alkyl ethers of furfuryl alcohol.
[0058] The amount of the tertiary amine compound or ether compound used is preferably 0.1 to 4 (mol / mol of alkali metal), more preferably 0.2 to 3 (mol / mol of alkali metal), relative to the amount of the polymerization initiator of the organic alkali metal compound.
[0059] In the process for producing the copolymer (A) and the copolymer (B), sodium alkoxide may be present during copolymerization. The sodium alkoxide is not limited to the following, but examples thereof include compounds represented by the following formula: In particular, sodium alkoxides having an alkyl group having 3 to 6 carbon atoms are preferred, and sodium t-butoxide and sodium t-pentoxide are more preferred. NaOR (In the formula, R is an alkyl group having 2 to 12 carbon atoms.) The amount of sodium alkoxide used in the polymerization process of copolymers (A) and (B) is preferably 0.01 or more and less than 0.1 (molar ratio), more preferably 0.01 or more and less than 0.08 (molar ratio), even more preferably 0.03 or more and less than 0.08 (molar ratio), and even more preferably 0.04 or more and less than 0.06 (molar ratio), relative to the vinyl bond amount adjuster (tertiary amine compound or ether compound). When the amount of sodium alkoxide is within this range, it tends to be possible to produce at a high productivity a copolymer having a narrow molecular weight distribution, which has a copolymer block containing a conjugated diene monomer unit having a high vinyl bond amount and a polymer block mainly composed of a vinyl aromatic monomer unit having a narrow molecular weight distribution.
[0060] The method for copolymerizing a conjugated diene compound and a vinyl aromatic compound using an organic alkali metal compound as a polymerization initiator is not particularly limited, and may be batch polymerization, continuous polymerization, or a combination thereof. The polymerization temperature is not particularly limited, but is usually from 0 to 180°C, and preferably from 30 to 150°C. The time required for polymerization varies depending on the conditions, but is usually within 48 hours, and preferably 0.1 to 10 hours. It is also preferable to carry out the polymerization in an atmosphere of an inert gas such as nitrogen gas. The polymerization pressure is not particularly limited as long as it is within a pressure range sufficient to maintain the monomer and the solvent in a liquid phase within the above polymerization temperature range.
[0061] Furthermore, at the end of the polymerization, a required amount of a coupling agent having two or more functional groups may be added to carry out a coupling reaction. The coupling agent having two or more functional groups is not particularly limited, and any known coupling agent can be used. Examples of bifunctional coupling agents include, but are not limited to, dihalogen compounds such as dimethyldichlorosilane and dimethyldibromosilane, acid esters such as methyl benzoate, ethyl benzoate, phenyl benzoate, and phthalates. Examples of polyfunctional coupling agents having three or more functional groups include, but are not limited to, 1,1,1,2,2-pentachloroethane, perchloroethane, pentachlorobenzene, perchlorobenzene, octabromodiphenyl ether, decabromodiphenyl ether, polyalcohols having three or more functional groups, epoxidized soybean oil, polyfunctional epoxy compounds such as diglycidyl bisphenol A, epoxy group-containing compounds having two to six functional groups, carboxylic acid esters, polyvinyl compounds such as divinylbenzene, and compounds represented by the formula R1. (4-n) Six n (wherein R1 is a hydrocarbon group having 1 to 20 carbon atoms, X is a halogen, and n is an integer of 3 or 4), and a halogenated tin compound. Examples of halogenated silicon compounds include, but are not limited to, methylsilyl trichloride, t-butylsilyl trichloride, silicon tetrachloride, and brominated versions of these compounds. Examples of the tin halide compound include, but are not limited to, polyvalent halogen compounds such as methyltin trichloride, t-butyltin trichloride, tin tetrachloride, etc. Dimethyl carbonate, diethyl carbonate, etc. can also be used.
[0062] The copolymer (A) and the copolymer (B) may be obtained by subjecting the living terminal of the block copolymer obtained by the above-mentioned method to an addition reaction with a modifier that generates a functional group-containing atomic group. Examples of functional group-containing atomic groups include, but are not limited to, atomic groups containing at least one functional group selected from the group consisting of a hydroxyl group, a carbonyl group, a thiocarbonyl group, an acid halide group, an acid anhydride group, a carboxyl group, a thiocarboxyl acid group, an aldehyde group, a thioaldehyde group, a carboxylate group, an amide group, a sulfonic acid group, a sulfonate group, a phosphoric acid group, a phosphoric acid ester group, an amino group, an imino group, a nitrile group, a pyridyl group, a quinoline group, an epoxy group, a thioepoxy group, a sulfide group, an isocyanate group, an isothiocyanate group, a silicon halide group, a silanol group, an alkoxy silicon group, a tin halide group, an alkoxy tin group, and a phenyl tin group.
[0063] Modifiers that generate functional group-containing atomic groups include, but are not limited to, tetraglycidyl meta-xylylene diamine, tetraglycidyl-1,3-bisaminomethylcyclohexane, ε-caprolactone, δ-valerolactone, 4-methoxybenzophenone, γ-glycidoxyethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyldimethylphenoxysilane, bis(γ-glycidoxypropyl)methylpropoxysilane, 1,3-dimethyl-2-imidazolidinone, 1,3-diethyl-2-imidazolidinone, N,N'-dimethylpropyleneurea, and N-methylpyrrolidone. The amount of the modifying agent added is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, and further preferably 0.3 to 10 parts by mass, based on 100 parts by mass of the copolymer before modification. The temperature for the addition reaction of the modifying agent is preferably 0 to 150°C, more preferably 20 to 120°C. The time required for the modification reaction varies depending on the modification reaction conditions, but is preferably within 24 hours, and more preferably 0.1 to 10 hours.
[0064] The copolymer (A) is preferably produced by carrying out a hydrogenation step after the above-mentioned polymerization step or after the above-mentioned modification step. The hydrogenation catalyst used for producing the copolymer (A) is not particularly limited, and for example, the hydrogenation catalysts described in JP-B-42-8704, JP-B-43-6636, JP-B-63-4841, JP-B-1-37970, JP-B-1-53851, JP-B-2-9041, etc. can be used. Preferred hydrogenation catalysts include titanocene compounds and / or mixtures with reducing organometallic compounds. The titanocene compound is not particularly limited, but examples thereof include compounds described in JP-A-8-109219, and specific examples thereof include compounds having at least one ligand having a (substituted) cyclopentadienyl structure, an indenyl structure, and a fluorenyl structure, such as biscyclopentadienyltitanium dichloride and monopentamethylcyclopentadienyltitanium trichloride. The reducing organometallic compound is not particularly limited, but examples thereof include organoalkali metal compounds such as organolithium compounds, organomagnesium compounds, organoaluminum compounds, organoboron compounds, and organozinc compounds. The reaction temperature for the hydrogenation reaction is usually from 0 to 200°C, and preferably from 30 to 150°C. The pressure of hydrogen used in the hydrogenation reaction is preferably 0.1 to 15 MPa, more preferably 0.2 to 10 MPa, and further preferably 0.3 to 5 MPa. The reaction time for the hydrogenation reaction is usually 3 minutes to 10 hours, and preferably 10 minutes to 5 hours. The hydrogenation reaction can be carried out by any of a batch process, a continuous process, or a combination thereof.
[0065] The copolymer (B) is preferably produced by carrying out a hydrogenation step after the above-mentioned polymerization step or after the above-mentioned modification step. The hydrogenation catalyst used for producing the copolymer (B) is not particularly limited, and for example, the hydrogenation catalysts described in JP-B-42-8704, JP-B-43-6636, JP-B-63-4841, JP-B-1-37970, JP-B-1-53851, JP-B-2-9041, etc. can be used. Preferred hydrogenation catalysts include titanocene compounds and / or mixtures with reducing organometallic compounds. The titanocene compound is not particularly limited, but examples thereof include compounds described in JP-A-8-109219, and specific examples thereof include compounds having at least one ligand having a (substituted) cyclopentadienyl structure, an indenyl structure, and a fluorenyl structure, such as biscyclopentadienyltitanium dichloride and monopentamethylcyclopentadienyltitanium trichloride. The reducing organometallic compound is not particularly limited, but examples thereof include organoalkali metal compounds such as organolithium compounds, organomagnesium compounds, organoaluminum compounds, organoboron compounds, and organozinc compounds. The reaction temperature for the hydrogenation reaction is usually from 0 to 200°C, and preferably from 30 to 150°C. The pressure of hydrogen used in the hydrogenation reaction is preferably 0.1 to 15 MPa, more preferably 0.2 to 10 MPa, and further preferably 0.3 to 5 MPa. The reaction time for the hydrogenation reaction is usually 3 minutes to 10 hours, and preferably 10 minutes to 5 hours. The hydrogenation reaction may be carried out by any of a batch process, a continuous process, or a combination thereof.
[0066] If necessary, catalyst residues may be removed from the reaction solution after the hydrogenation step. The polymerization initiator used in producing the hydrogenated copolymer by anionic living polymerization and the compound containing a metal atom in the hydrogenation catalyst in the hydrogenation reaction described above tend to react with moisture in the air in the desolvation step, etc., to generate a specific metal compound that remains in the hydrogenated copolymer. When these compounds are contained in the resin composition of the present embodiment and the cured product thereof, the dielectric constant and dielectric loss tangent tend to increase, and further, ion migration tends to occur easily in electronic material applications. Examples of the remaining metal compounds include compounds of metals contained in the polymerization initiator and the hydrogenation catalyst, for example, oxides of each atom such as titanium oxide, amorphous titanium oxide, orthotitanic acid, metatitanic acid, titanium hydroxide, nickel hydroxide, nickel monoxide, lithium oxide, lithium hydroxide, cobalt oxide, and cobalt hydroxide, and composite oxides of each atom and a different metal such as lithium titanate, barium titanate, strontium titanate, nickel titanate, and nickel-iron oxide. From the viewpoint of lowering the dielectric constant, lowering the dielectric loss tangent, and making ion migration less likely to occur, the amount of the metal compound remaining in the copolymers (A) and (B) is preferably 150 ppm or less, more preferably 130 ppm or less, further preferably 100 ppm or less, and further more preferably 90 ppm or less, in terms of the amount of the remaining metal. Specific examples of the remaining metal include Ti, Ni, Li, Co, etc.
[0067] As a method for reducing the amount of residual metal in the resin composition of the present embodiment and its cured product, a conventionally known method can be applied, and is not particularly limited. For example, after the hydrogenation reaction of copolymers (A) and (B), a method of adding water and carbon dioxide gas to neutralize the hydrogenation catalyst residue; a method of adding water, carbon dioxide gas, and an acid to neutralize the hydrogenation catalyst residue can be mentioned. Specifically, the method described in Japanese Patent Application No. 2014-557427 can be applied. Even if these metal removal methods are used, water containing hydroxides of metal compounds is mixed in the solvent removal process of copolymers (A) and (B), so that about 1 to 15 ppm is generally contained. Therefore, it is preferable to remove 20% or more of the amount of metal added to copolymers (A) and (B), more preferably 30% or more, even more preferably 40% or more, even more preferably 50% or more, and even more preferably 60% or more.
[0068] In addition, the amount of residual metal in the copolymers (A) and (B) can be reduced by reducing the amount of polymerization initiator and hydrogenation catalyst added, but reducing the amount of polymerization initiator increases the molecular weight of the copolymers (A) and (B), and if the molecular weight of the copolymers (A) and (B) constituting the resin composition of this embodiment is outside the range of the requirements, the heat resistance of the cured product tends to decrease. In addition, when performing a hydrogenation reaction, reducing the amount of hydrogenation catalyst increases the hydrogenation reaction time and increases the hydrogenation reaction temperature, which tends to significantly reduce productivity.
[0069] Methods for separating the copolymers (A) and (B) from the solvent include, but are not limited to, a method in which a polar solvent that is a poor solvent for the copolymers (A) and (B), such as acetone or alcohol, is added to a solution of the copolymers (A) and (B) to precipitate and recover the copolymers (A) and (B); a method in which a solution of the copolymers (A) and (B) is poured into boiling water with stirring and the solvent is removed by steam stripping to recover the copolymers; and a method in which the solvent is distilled off by directly heating a solution of the copolymers (A) and (B).
[0070] The copolymer (A) and the copolymer (B) may contain an antioxidant on the surface and / or inside thereof, for example, by adding an antioxidant during the production. The following antioxidant may also be added to the resin composition of the present embodiment, which will be described later.
[0071] Examples of the antioxidant include, but are not limited to, phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, and amine-based antioxidants. Specifically, 2,6-di-t-butyl-4-methylphenol, n-octadecyl-3-(4'-hydroxy-3',5'-di-t-butyl-phenyl)propionate, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane], tris-(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, 4,4'-butylidene-bis-(3-methyl-6-t-butylphenol), 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methyl n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, pentaerythrityl-tetrakis[ 3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 3,5-di-t-butyl-4-hydroxybenzylphosphonate-diethyl ester, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis(3,5-di-t-butyl-4 -Hydroxybenzylphosphonic acid ethyl) calcium and polyethylene wax (50%) mixture, octylated diphenylamine, 2,4-bis[(octylthio)methyl]-o-cresol, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, butyric acid, 3,3-bis(3-t-butyl-4-hydroxyphenyl)ethylene ester, 1,1,3-tris-(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl) isocyanurate, 2-t-butyl-6-(3'-t-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenyl-acrylate, and 2-[1-(2-hydroxy-3,5-di-t-pentylphenyl)-ethyl]-4,6-di-t-pentylphenyl acrylate. From the viewpoint of insulation reliability, the above-mentioned antioxidant may be used as a pellet blocking inhibitor.
[0072] Examples of the polymerization terminator include, but are not limited to, water, various alcohols such as methanol, ethanol, isopropanol, 2-ethylhexanol, heptanol, and mixtures thereof.
[0073] The copolymer (B) and / or the copolymer (A) may be pelletized. These may be pelletized individually or in the form of a mixture. Examples of the pelletizing method include a method in which copolymer (B) and / or copolymer (A) are extruded in the form of strands from a single-screw or twin-screw extruder, and then cut in water with a rotary blade installed in front of a die section; a method in which copolymer (A) and / or copolymer (B) are extruded in the form of strands from a single-screw or twin-screw extruder, and then cooled with water or air, and then cut with a strand cutter; a method in which the copolymers are melt-mixed using an open roll or Banbury mixer, then formed into a sheet using a roll, and then the sheet is cut into strips, and then cut into cubic pellets using a pelletizer. The size and shape of the pellets of the copolymer (B) and / or the copolymer (A) are not particularly limited. If necessary, a pellet blocking inhibitor may be added to the pellets of the copolymer (B) and / or the copolymer (A) in order to prevent pellet blocking. Examples of pellet blocking inhibitors include, but are not limited to, calcium stearate, magnesium stearate, zinc stearate, polyethylene, polypropylene, ethylene bisstearylamide, talc, and amorphous silica. As the pellet blocking inhibitor, from the viewpoint of ion migration, EBS, polyethylene, and polypropylene are preferred. The amount of the pellet blocking inhibitor to be added is preferably 500 to 6000 ppm, more preferably 1000 to 5000 ppm, based on the copolymer (A) and / or (B). The pellet anti-blocking agent is preferably incorporated in a state in which it is attached to the surface of the pellet, but it may also be contained to some extent inside the pellet.
[0074] (Molecular weight distribution of copolymer (A) and copolymer (B)) The molecular weight distribution (Mwa / Mna) of the copolymer (A) is preferably 1.01 to 8.0, more preferably 1.01 to 6.0, and further preferably 1.01 to 5.0. When the molecular weight distribution is within the above range, the resin composition of the present embodiment tends to have good dimensional stability. The shape of the molecular weight distribution of the copolymer (A) measured by GPC is not particularly limited, and it may be a polymodal molecular weight distribution having two or more peaks, or a monomodal molecular weight distribution having one peak. The molecular weight distribution of the copolymer (A) is preferably monomodal. When the molecular weight distribution of the copolymer (A) is monomodal, the heat resistance tends to be excellent. The weight average molecular weight (Mwa) and molecular weight distribution [Mwa / Mna; the ratio of the weight average molecular weight (Mwa) to the number average molecular weight (Mna)] of the copolymer (A) can be determined by using the molecular weight of the peak of a chromatogram measured by GPC according to the method described in the Examples below, and a calibration curve (prepared using the peak molecular weight of the standard polystyrene) obtained by measuring commercially available standard polystyrene.
[0075] The molecular weight distribution (Mwb / Mnb) of the copolymer (B) is preferably 1.01 to 8.0, more preferably 1.01 to 6.0, and further preferably 1.01 to 5.0. When the molecular weight distribution is within the above range, the resin composition of the present embodiment tends to have good dimensional stability. The shape of the molecular weight distribution of the copolymer (B) measured by GPC is not particularly limited, and it may be a polymodal molecular weight distribution having two or more peaks, or a monomodal molecular weight distribution having one peak. The molecular weight distribution of the copolymer (B) is preferably monomodal. When the molecular weight distribution of the copolymer (B) is monomodal, the heat resistance tends to be excellent. The weight average molecular weight (Mwb) and molecular weight distribution (Mwb / Mnb; the ratio of the weight average molecular weight (Mwb) to the number average molecular weight (Mnb)) of the copolymer (B) can be determined by using the molecular weight of the peak of a chromatogram measured by GPC using the method described in the Examples below, and a calibration curve (prepared using the peak molecular weight of the standard polystyrene) obtained by measuring commercially available standard polystyrene.
[0076] (mass ratio of copolymer (A) to copolymer (B)) In the resin composition of the present embodiment, the mass ratio (A) / (B) of the contents of the copolymer (A) and the copolymer (B) is preferably from the viewpoint of productivity to 5 / 95 to 70 / 30, more preferably from 10 / 90 to 60 / 40, and further preferably from 15 / 85 to 50 / 50.
[0077] (Content of copolymer (A) and copolymer (B)) The total content of copolymer (A) and copolymer (B) in the resin composition of this embodiment is not particularly limited, but is preferably 5 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the resin solid content of the resin composition of this embodiment. Furthermore, from the viewpoint of achieving the effect of imparting flexibility to the resin composition of this embodiment, the lower limit of the total content of copolymer (A) and copolymer (B) is more preferably 6 parts by mass or more, and even more preferably 8 parts by mass or more. Furthermore, the upper limit of the total content of copolymer (A) and copolymer (B) is more preferably 50 parts by mass or less, and even more preferably 40 parts by mass or less, from the viewpoints of suppressing a decrease in the glass transition temperature of the resin composition of this embodiment and suppressing increased stickiness. The resin solid content refers to the components remaining after excluding the filler and the solvent from the resin composition.
[0078] (Components Constituting Resin Composition) The resin composition of the present embodiment contains the above-mentioned copolymer (A) and copolymer (B), and at least one component selected from the group consisting of the following components (I) to (III). Component (I): Cured resin (excluding copolymer (A) and copolymer (B)) Component (II): Radical initiator Component (III): Hardener (excluding component (I))
[0079] <Component (I): Cured resin (excluding copolymer (A) and copolymer (B))> The resin composition of this embodiment may contain the component (I) cured resin (excluding copolymer (A) and copolymer (B)) for the purpose of imparting performance such as heat resistance and adhesion to a substrate, within a range that does not impair the dielectric performance of the cured product. The component (I) cured resin has the effect of improving strength and heat resistance by crosslinking in the resin composition of this embodiment. Since the cured resin has a polar group, the resin composition and cured product of this embodiment tend to have excellent heat resistance. As the component (I): cured resin (excluding copolymer (A) and copolymer (B)), from the viewpoint of the heat resistance and adhesiveness of the resin composition of the present embodiment, at least one type selected from the group consisting of epoxy-based resins, polyimide-based resins, polyphenylene ether-based resins, liquid crystal polyester-based resins, and fluorine-based resins is preferred, and more preferred are epoxy-based resins, polyimide-based resins, and polyphenylene ether-based resins. In the process of preparing a varnish containing component (I): cured resin, when the cured resin is a polyimide resin, the copolymers (A) and (B) may be difficult to dissolve depending on the structure, but the average content of the vinyl aromatic monomer units of the copolymers (A) and (B) is 50% by mass or more, so that the solubility of the copolymers (A) and (B) in the varnish is high and preferable. That is, when the component (I) is a polyimide resin or when an epoxy resin and a polyimide resin are used in combination, the resin composition of this embodiment in which the average content of the vinyl aromatic monomer units of the copolymers (A) and (B) is 50% by mass or more is a preferred embodiment for the purpose of ensuring solubility in the varnish.
[0080] From the viewpoint of heat resistance of the resin composition of the present embodiment, the polyimide resin as component (I) may have imide bonds in the repeating unit and belong to the category called polyimide resin. Although not limited to the following, for example, a general polyimide structure obtained by polycondensation (imide bond) of tetracarboxylic acid or its dianhydride with diamine is included, and from the viewpoint of curability, it is preferable that the above-mentioned polyimide structure has an unsaturated group at the terminal. Examples of the polyimide resin having an unsaturated group at the terminal include maleimide type polyimide resin, nadiimide type polyimide resin, and allylnadiimide type polyimide resin. The tetracarboxylic acid or dianhydride thereof is not limited to the following, but examples thereof include aromatic tetracarboxylic acid dianhydrides, alicyclic tetracarboxylic acid dianhydrides, and aliphatic tetracarboxylic acid dianhydrides. These may be used alone or in combination of two or more. The diamine is not limited to the following, but examples thereof include aromatic diamines, alicyclic diamines, and aliphatic diamines that are commonly used in the synthesis of polyimides. These may be used alone or in combination of two or more. In addition, at least one of the tetracarboxylic acid or its dianhydride and diamine may have one or more functional groups selected from the group consisting of a fluorine group, a trifluoromethyl group, a hydroxyl group, a sulfone group, a carbonyl group, a heterocycle, a long-chain alkyl group, an allyl group, and the like, from the viewpoint of reducing the dielectric constant and the dielectric loss tangent of the cured product of the resin composition of the present embodiment. In addition, the component (I) may be a commercially available polyimide resin, and examples of the polyimide resin include Neoprim (registered trademark) C-3650 (manufactured by Mitsubishi Gas Chemical Co., Ltd., trade name), Neoprim C-3G30 (manufactured by Mitsubishi Gas Chemical Co., Ltd., trade name), Neoprim C-3450 (manufactured by Mitsubishi Gas Chemical Co., Ltd., trade name), Neoprim P500 (manufactured by Mitsubishi Gas Chemical Co., Ltd., trade name), BT (bismaleimide-triazine) resin (manufactured by Mitsubishi Gas Chemical Co., Ltd.), JL-20 (manufactured by New Japan Chemical Co., Ltd., trade name) (the varnishes of these polyimide resins may contain silica), Rikacoat SN20 and Rikacoat PN20, both manufactured by New Japan Chemical Co., Ltd., and IST Corporation, respectively. Examples of such products include Pyre-ML, Upia-AT, Upia-ST, Upia-NF, and Upia-LB manufactured by Ube Industries, PIX-1400, PIX-3400, PI2525, PI2610, HD-3000, and AS-2600 manufactured by Hitachi Chemical Co., Ltd., HPC-5000, HPC-5012, HPC-1000, HPC-5020, HPC-3010, HPC-6000, HPC-9000, HCI-7000, HCI-1000S, HCI-1200E, and HCI-1300 manufactured by Showa Denko K.K., BMI-2300 manufactured by Daiwa Kasei Kogyo Co., Ltd., and MIR-3000 manufactured by Shin Nippon Kayaku Co., Ltd.
[0081] The polyphenylene ether resin as component (I) may be any resin that belongs to the category of polyphenylene ether resins and contains phenylene ether units as repeating structural units. It may be a homopolymer having phenylene ether units, or a polymer containing other structural units other than phenylene ether units. In the homopolymer having a phenylene ether unit, the phenylene group in the phenylene unit may have a substituent, but is not particularly limited thereto. Examples of the substituent include an acrylic group such as an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, or a tert-butyl group; a cyclic alkyl group such as a cyclohexyl group; a vinyl group, an allyl group, an isopropenyl group, a 1-butenyl group, a 1-pentenyl group, a p-vinylphenyl group, a p-isopropenylphenyl group, a m-vinylphenyl group, or a m-isopropenylphenyl group. phenylphenyl group, o-vinylphenyl group, o-isopropenylphenyl group, p-vinylbenzyl group, p-isoproperbenzyl group, m-vinylbenzyl group, m-isopropenylbenzyl group, o-vinylbenzyl group, o-isopropenylbenzyl group, p-vinylphenylethenyl group, p-vinylphenylpropenyl group, p-vinylphenylbutenyl group, m-vinylphenylethenyl group, m-vinylphenylpropenyl group, m-vinylphenylbutenyl group, o-vinylphenylethenyl group, o- Unsaturated bond-containing substituents such as vinylphenylpropenyl group, o-vinylphenylbutenyl group, methacryl group, acrylic group, 2-ethylacrylic group, and 2-hydroxymethylacrylic group, hydroxyl group, carboxyl group, carbonyl group, thiocarbonyl group, acid halide group, acid anhydride group, carboxylic acid group, thiocarboxylic acid group, aldehyde group, thioaldehyde group, carboxylic acid ester group, amide group, sulfonic acid group, sulfonic acid ester group, phosphoric acid group, phosphoric acid ester group, amino group, imino group, nitrile group, pi Examples of functional group-containing substituents include a lysyl group, a quinoline group, an epoxy group, a thioepoxy group, a sulfide group, an isocyanate group, an isothiocyanate group, a halogenated silicon group, a silanol group, an alkoxysilicon group, a halogenated tin group, a boronic acid group, a boron-containing group, a boronate salt group, an alkoxytin group, and a phenyltin group. From the viewpoint of the curability of the resin composition of the present embodiment, it is preferable that the functional group-containing substituent has a predetermined polar group from the viewpoint of radical reactivity and / or reactivity with component (III): a curing agent, which will be described later. The molecular weight of the polyphenylene ether resin is preferably 100,000 or less, more preferably 50,000 or less, and even more preferably 10,000 or less, from the viewpoint of the curability of the resin composition of this embodiment. The polyphenylene ether resin may be linear or may have a crosslinked or branched structure.
[0082] The liquid crystal polyester resin as component (I) is a polyester that forms an anisotropic molten phase, and may be any resin that belongs to the category called liquid crystal polyester resin. Examples of such inks include "X7G" manufactured by Eastman Kodak Company, Xyday manufactured by Dartco, Econol manufactured by Sumitomo Chemical Co., Ltd., and Vectra manufactured by Celanese Corporation.
[0083] The epoxy resin as component (I) may be any resin that falls within the category of epoxy resins, and from the viewpoint of the strength of the resin composition of this embodiment, it preferably has two or more epoxy groups in one molecule. The epoxy resin may be used alone or in combination of two or more kinds. Examples of epoxy resins include bixylenol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidyl ester type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, tetraphenylethane type epoxy resins, and the like.
[0084] In addition, when an epoxy resin is used as component (I) from the viewpoint of reactivity, the resin composition of this embodiment preferably contains component (III): a curing agent, which will be described later. Examples of polar groups contained in component (III): a curing agent include a carboxy group, an imidazole group, a hydroxyl group, an amino group, a mercaptan group, a benzoxazine group, and a carbodiimide group. From the viewpoint of reactivity, a carboxy group, an imidazole group, a hydroxyl group, a benzoxazine group, and a carbodiimide group are preferred. From the viewpoint of low dielectric constant and low dielectric loss tangent of the resin composition of this embodiment and the cured product, a hydroxyl group, a carboxy group, an imidazole group, a benzoxazine group, and a carbodiimide group are more preferred, and a hydroxyl group, a carboxy group, an imidazole group, a benzoxazine group, and a carbodiimide group are even more preferred.
[0085] In addition, two or more polar resins having different radical reactivities may be used as component (I). In this case, from the viewpoint of the curability of the resin composition of the present embodiment, component (II): a radical initiator described later, and component (III): a curing agent described later can be used alone or in combination. For example, when a maleimide-type polyimide resin having excellent radical reactivity and a bisphenol A epoxy resin having no radical reactivity are used as component (I), component (II): a radical initiator and component (III): a curing agent can be added in combination from the viewpoint of the curability of the resin composition of the present embodiment.
[0086] When a polar resin having a high melting point and high rigidity is used as component (I), the composition may not contain component (III): a curing agent, which will be described later. Examples of resins having a high melting point and high rigidity include liquid crystal polyester resins and fluorine-based resins such as polytetrafluoroethylene. Since component (I) has a high melting point and high rigidity, the resin composition of the present embodiment tends to have heat resistance and / or strength required for practical use even when it does not contain component (III): a curing agent described below.
[0087] The content of component (I) in the resin composition of the present embodiment is preferably 10 parts by mass to 90 parts by mass, more preferably 15 parts by mass to 85 parts by mass, and even more preferably 20 parts by mass to 80 parts by mass, per 100 parts by mass of the resin solid content of the resin composition of the present embodiment, from the viewpoint of heat resistance. The resin solid content refers to the components remaining after excluding the filler and the solvent from the resin composition.
[0088] <Component (II): Radical initiator> As the component (II): radical initiator, any conventionally known initiator can be used, and a preferred example is a thermal radical initiator. Examples of the thermal radical initiator include, but are not limited to, hydroperoxides such as diisopropylbenzene hydroperoxide (Percumyl P), cumene hydroperoxide (Percumyl H), and t-butyl hydroperoxide (Perbutyl H); α,α-bis(t-butylperoxy-m-isopropyl)benzene (Perbutyl P), dicumyl peroxide (Percumyl D), 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane (Perhexa 25B), t-butylcumyl peroxide (Perbutyl C), di-t-butyl peroxide (Perbutyl ...t-butyl peroxide (Perbutyl H), and t-butyl peroxide (Perbutyl H). peroxyketals such as n-butyl 4,4-di-(t-butylperoxy)valerate (Perhexa V); diacyl peroxides; peroxydicarbonates; organic peroxides such as peroxyesters; and azo compounds such as 2,2-azobisisobutylnitrile, 1,1'-(cyclohexane-1-1carbonitrile), 2,2'-azobis(2-cyclopropylpropionitrile), and 2,2'-azobis(2,4-dimethylvaleronitrile). These may be used alone or in combination of two or more.
[0089] When the above-mentioned component (I): curable resin is a resin having radical reactivity, the amount of component (II): radical initiator can be adjusted arbitrarily depending on the reactivity, or it can be omitted. The radically reactive resin as component (I) may be, for example, a homopolymer of a compound containing at least one vinyl group and / or halogen element in the polymer and / or a copolymer with any compound, and from the viewpoint of the low dielectric constant and low dielectric loss tangent of the resin composition and the cured product of this embodiment, the homopolymer and / or copolymer preferably has a vinyl group. Having a vinyl group may be a polymer consisting of a repeating unit having a vinyl group, or may be a polymer having a vinyl group obtained by reacting each polar group of a compound having a vinyl group and a polar group with a resin having a polar group. Examples of the compound having a vinyl group and a polar group include (meth)acrylic acid (in this specification, "(meth)acrylic" means "methacrylic or acrylic"), carboxyl group-containing vinyl monomers such as maleic acid, maleic acid monoalkyl esters, and fumaric acid, sulfone group-containing vinyl monomers such as vinyl sulfonic acid, (meth)allyl sulfonic acid, methyl vinyl sulfonic acid, and styrene sulfonic acid, hydroxyl group-containing vinyl monomers such as hydroxystyrene, N-methylol (meth)acrylamide, hydroxyethyl (meth)acrylate, and hydroxypropyl (meth)acrylate, phosphoric acid group-containing vinyl monomers such as 2-hydroxyethyl (meth)acryloyl phosphate, phenyl-2-acryloyloxyethyl phosphate, and 2-acryloyloxyethyl phosphonic acid, hydroxystyrene, N-methylol (meth)acrylamide, amide, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, polyethylene glycol (meth)acrylate, 1-butene-3-ol, and other hydroxy group-containing vinyl monomers; aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and other amino group-containing vinyl monomers; (meth)acrylamide, N-methyl (meth)acrylamide, N-butylacrylamide, and other amide group-containing vinyl monomers; (meth)acrylonitrile, cyanostyrene, cyanoacrylate, and other nitrile group-containing vinyl monomers; glycidyl methacrylate, tetrahydrofurfuryl (meth)acrylate, p-vinylphenyl phenyl oxide, and other epoxy group-containing vinyl monomers; and polyisocyanate group-containing vinyl monomers such as uretdione and isocyanurate. Examples of halogen-containing monomers include vinyl chloride, vinyl bromide, vinylidene chloride, allyl chloride, chlorostyrene, bromostyrene, dichlorostyrene, chloromethylstyrene, tetrafluorostyrene, and chloroprene.
[0090] When the radical reactivity of the cured resin (I) is low or absent, from the viewpoint of reactivity, it is preferable that the resin composition of this embodiment contains a curing agent (III) described later. The curing agent (III) usually has a function of reacting with the cured resin (I) to cure the resin composition. The "reaction" of the curing agents (I) and (III) means that the polar groups of each component have covalent bonding properties. When polar groups react with each other, for example, when OH of a carboxyl group is eliminated, the original polar group changes or disappears, but when a covalent bond is formed as a result, this is included in the definition that the polar groups are "reactive" with each other.
[0091] The content of component (II) in the resin composition of this embodiment is preferably 0.01 to 5 parts by mass, more preferably 0.02 to 4 parts by mass, and even more preferably 0.03 to 3 parts by mass, per 100 parts by mass of the resin solids of the resin composition of this embodiment, from the viewpoint of heat resistance. The resin solid content refers to the components remaining after excluding the filler and the solvent from the resin composition.
[0092] <Component (III): Hardener (excluding component (I))> From the viewpoint of curing function, it is preferable that the curing agent of component (III) has at least two polar groups in one molecular chain that are capable of reacting with the functional groups of the cured resin (component (I)). The component (III) may be used alone or in combination of two or more kinds. The type of polar group contained in component (I) and component (III) is not particularly limited. For example, Epoxy and carboxyl, carbonyl, ester, imidazole, hydroxyl, amino, mercaptan, benzoxazine, and carbodiimide groups; Amino and carboxyl groups, carbonyl groups, hydroxyl groups, acid anhydride groups, sulfonic acid, and aldehyde groups; Isocyanate groups, hydroxyl groups, carboxylic acids; Anhydride and hydroxyl groups; Silanol groups, hydroxyl groups, and carboxylic acid groups; Halogens and carboxylic acid groups, carboxylic ester groups, amino groups, phenol groups, thiol groups; Alkoxy and hydroxy groups, alkoxide groups, and amino groups; Maleimide and cyanate groups; etc. These polar groups can be arbitrarily selected as to whether they are the polar groups of component (I): the cured resin, or the polar groups of component (III): the curing agent.
[0093] In addition, cases where the polar group of component (I) does not react directly with the polar group of component (III), but can react by adding a curing accelerator such as a catalyst, are also included in the definition of "reactive." For example, when component (I) is a resin having an epoxy group and component (III) is a curing agent having an acid anhydride group, the reactivity between the epoxy group and the acid anhydride group is usually very low, but by adding a compound having an amino group as a curing accelerator, the epoxy group and the amino group of component (I) react, and some or all of the epoxy groups of component (III) become hydroxyl groups. The resin composition of this embodiment is cured by the reaction of the hydroxyl groups with the acid anhydride groups of the curing agent of component (III).
[0094] When component (I) is a curable resin having a polar group, the ratio of the amounts of the curing agents, component (I) and component (III), in terms of the molar ratio of the polar groups, is preferably (molar amount of polar groups in component (I)):(molar amount of polar groups in component (III))=1:0.01 to 1:20, more preferably 1:0.05 to 1:15, and even more preferably 1:0.1 to 1:10, from the viewpoint of reactivity. Specific examples of the component (III): curing agent are given below. Examples of curing agents having an ester group include EXB9451, EXB9460, EXB, 9460S, HPC8000-65T, HPC8000H-65TM, EXB8000L-65TM, EXB8150-65T, and EXB9416-70BK manufactured by DIC Corporation, and YLH1026, DC808, YLH1026, YLH1030, and YLH1048 manufactured by Mitsubishi Chemical Corporation.
[0095] Examples of curing agents having a hydroxyl group include, but are not limited to, MEH-7700, MEH-7810, MEH-7851, NHN, CBN, and GPH manufactured by Nippon Kayaku Co., Ltd., SN170, SN180, SN190, SN475, SN485, SN495, SN-495V, and SN375 manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and TD-2090, LA-7052, LA-7054, LA-1356, LA-3018-50P, and EXB-9500 manufactured by DIC Corporation.
[0096] Examples of the curing agent having a benzoxazine group include, but are not limited to, ODA-BOZ manufactured by JFE Chemical Corporation, HFB2006M manufactured by Showa Polymer Co., Ltd., and Pd and Fa manufactured by Shikoku Chemical Industry Co., Ltd.
[0097] Examples of curing agents having an isocyanate group include, but are not limited to, bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Commercially available products include PT30, PT60, ULL-950S, BA230, and BA230S75 manufactured by Lonza Japan.
[0098] The curing agent having a carbodiimide group is not limited to the following, but examples thereof include V-03 and V-07 manufactured by Nisshinbo Chemical Co., Ltd.
[0099] Examples of the curing agent having an amino group include, but are not limited to, 4,4'-methylenebis(2,6-dimethylaniline), diphenyldiaminosulfone, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenylether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino 4-hydroxyphenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, etc. Commercially available products include KAYABOND C-200S, KAYABOND C-100, Kayahard AA, Kayahard AB, Kayahard AS manufactured by Nippon Kayaku Co., Ltd., and Epicure W manufactured by Mitsubishi Chemical Corporation. From the viewpoint of reactivity, the curing agent having an amino group is preferably a primary amine and / or a secondary amine, more preferably a primary amine.
[0100] Examples of the curing agent having an acid anhydride group include, but are not limited to, phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, and benzophenone. Examples of such anhydrides include tetracarboxylic dianhydrides, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and polymeric acid anhydrides such as styrene-maleic acid resin, which is a copolymer of styrene and maleic acid.
[0101] In addition, a compound having at least two of the above-mentioned structures having radical reactivity also reacts with component (I) and has the function of curing the resin composition of this embodiment, and therefore can be used as component (III): a curing agent. Examples of compounds having at least two structures having radical reactivity include allyl monomers such as triallyl isocyanurate (Taikyu, manufactured by Mitsubishi Chemical Corporation), tris(2-hydroxyethyl) isocyanurate, diallyl fumarate, diallyl adipate, triallyl citrate, and diallyl hexahydrophthalate.
[0102] The content of component (III) in the resin composition of the present embodiment is preferably 10 parts by mass to 90 parts by mass, more preferably 15 parts by mass to 85 parts by mass, and even more preferably 20 parts by mass to 80 parts by mass, based on 100 parts by mass of the resin solid content of the resin composition of the present embodiment, from the viewpoint of heat resistance. The resin solid content refers to the components remaining after excluding the filler and the solvent from the resin composition.
[0103] <Component (IV): Additives> The resin composition of the present embodiment may further contain, as component (IV), a curing accelerator, a filler, a flame retardant, and other additives. Moreover, the additives contained in the copolymers (A) and (B) have the same meaning as the component (IV) of the resin composition.
[0104] The curing accelerator is added for the purpose of promoting the reactivity between the above-mentioned components, and may be any conventionally known accelerator, such as a phosphorus-based curing accelerator, an amine-based curing accelerator, an imidazole-based curing accelerator, a guanidine-based curing accelerator, or a metal-based curing accelerator. The curing accelerator may be used alone or in combination of two or more kinds.
[0105] Examples of phosphorus-based curing accelerators include, but are not limited to, triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, and the like, with triphenylphosphine and tetrabutylphosphonium decanoate being preferred.
[0106] Examples of the amine-based curing accelerator include, but are not limited to, trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, with 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene being preferred.
[0107] Examples of the imidazole-based curing accelerator include, but are not limited to, 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, and the like. Imidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazolidinediamine 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2 Examples of imidazole compounds include 1-dodecyl-2-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins. Of these, 2-ethyl-4-methylimidazole and 1-benzyl-2-phenylimidazole are preferred. As the imidazole-based curing accelerator, a commercially available product may be used, for example, P200-H50 manufactured by Mitsubishi Chemical Corporation.
[0108] Examples of the guanidine curing accelerator include, but are not limited to, dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, tetramethylguanidine, pentamethylguanidine, tetramethylguanidine, pentamethylguanidine, tetramethylguanidine, pentamethylguanidine, tetramethylguanidine, pentamethylguanidine, tetramethylguanidine, pentamethylguanidine, tri ... pentamethylguanidine, trimethylguanidine, pentamethylguanidine, trimethylguanidine, pentamethylguanidine, trimethylguanidine, pentamethylguanidine, trimethylguanidine, pentamethylguanidine, trimethylguanidine, pentamethylguanidine, trimethylguanidine, pentamethylguanidine, pentamethylguanidine, pentamethylguanidine, pentamethylguanidine, pentamethylguanidine Examples of the aryl biguanide include riazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide. Of these, dicyandiamide and 1,5,7-triazabicyclo[4.4.0]dec-5-ene are preferred.
[0109] Examples of metal-based curing accelerators include, but are not limited to, organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Examples of the organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of the organic metal salt include zinc octoate, tin octoate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.
[0110] Examples of the filler include, but are not limited to, inorganic fillers such as silica, calcium carbonate, magnesium carbonate, magnesium hydroxide, aluminum hydroxide, calcium sulfate, barium sulfate, carbon black, glass fiber, glass beads, glass balloons, glass flakes, graphite, titanium oxide, potassium titanate whiskers, carbon fiber, alumina, kaolin clay, silicic acid, calcium silicate, quartz, mica, talc, clay, zirconia, potassium titanate, alumina, and metal particles; and organic fillers such as wood chips, wood powder, pulp, and cellulose nanofibers. These may be used alone or in combination of two or more. The shape of these fillers is not particularly limited and may be any of scaly, spherical, granular, powdery, irregular, etc. From the viewpoint of the low dielectric constant and low dielectric tangent of the resin composition and the cured product of this embodiment, silica is preferred as the filler. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica.
[0111] Examples of the flame retardant include, but are not limited to, halogen-based flame retardants such as bromine compounds, phosphorus-based flame retardants such as aromatic compounds, and flame retardants containing aromatic bromine compounds such as metal hydroxides, alkylsulfonates, antimony trioxide, aluminum hydroxide, magnesium hydroxide, zinc borate, hexabromobenzene, decabromodiphenylethane, 4,4-dibromobiphenyl, and ethylenebistetrabromophthalimide. These flame retardants may be used alone or in combination of two or more. The above flame retardants also include so-called flame retardant auxiliaries, which have a low flame retardancy effect by themselves but exhibit a synergistic effect when used in combination with other flame retardants.
[0112] Fillers and flame retardants that have been previously surface-treated with a surface treatment agent such as a silane coupling agent can also be used. Examples of the surface treatment agent include, but are not limited to, a fluorine-containing silane coupling agent, an aminosilane coupling agent, an epoxysilane coupling agent, a mercaptosilane coupling agent, a silane coupling agent, an alkoxysilane, an organosilazane compound, and a titanate coupling agent. These may be used alone or in combination of two or more.
[0113] There are no particular limitations on the other additives, so long as they are generally used in compounding resin compositions and / or cured products. Examples of such other additives include, but are not limited to, pigments and / or colorants such as carbon black and titanium oxide; lubricants such as stearic acid, behenic acid, zinc stearate, calcium stearate, magnesium stearate, and ethylene bisstearamide; release agents; plasticizers such as organic polysiloxanes, fatty acid esters such as phthalate esters, adipic acid ester compounds, and azelaic acid ester compounds, and mineral oils; antioxidants such as hindered phenols and phosphorus-based heat stabilizers; hindered amine-based light stabilizers; benzotriazole-based ultraviolet absorbers; antistatic agents; organic fillers; thickeners; defoamers; leveling agents; resin additives such as adhesion-imparting agents; other additives, or mixtures thereof.
[0114] From the viewpoint of the low dielectric constant and low dielectric loss tangent of the resin composition and the cured product of the present embodiment, it tends to be preferable that no pigments, colorants, lubricants, release agents, or antistatic agents are contained.
[0115] The resin composition of this embodiment may be prepared by melt-kneading the components, or by dissolving and stirring the components in a solvent capable of dissolving them (hereinafter referred to as "varnish"). From the viewpoint of ease of handling, however, varnish is preferred. Examples of the solvent include, but are not limited to, ketones such as acetone, methyl ethyl ketone (MEK), and cyclohexanone; acetate esters such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate; carbitols such as cellosolve and butyl carbitol; aromatic hydrocarbons such as toluene and xylene; and amide solvents such as dimethylformamide, dimethylacetamide (DMAc), and N-methylpyrrolidone. The organic solvents may be used alone or in combination of two or more.
[0116] [Cured product] The cured product of the present embodiment is a cured product of the resin composition of the present embodiment, and is obtained by subjecting the resin composition of the present embodiment to a curing reaction at any temperature and time. The cured product of the present embodiment is a concept that includes not only a completely cured product, but also a form in which only a part of the resin composition is cured and contains uncured components (semi-cured product). In the process for producing the laminate described below, a step of further curing the cured product may be carried out. The reaction temperature in the curing step of the cured product of this embodiment is preferably 80° C. or higher, more preferably 100° C. or higher, and even more preferably 120° C. or higher. The reaction time is preferably from 10 to 240 minutes, more preferably from 20 to 230 minutes, and further preferably from 30 to 220 minutes. When the resin composition of the present embodiment is a varnish, it is preferable to carry out a curing reaction after removing the solvent. The drying method may be a conventionally known method such as heating or hot air blowing, and is preferably carried out at a temperature lower than the curing reaction temperature. The resin composition is dried so that the amount of the solvent in the resin composition is preferably 10% by mass or less, more preferably 5% by mass or less.
[0117] [Resin film] The resin film of the present embodiment is made of the resin composition of the present embodiment. The resin film of the present embodiment includes the cured product of the present embodiment. The resin film of the present embodiment can be obtained by spreading the varnish made of the resin composition of the present embodiment into a uniform thin film on a suitable support, and then drying the varnish as described above to remove the solvent. Such a resin film can be wound up into a roll and stored. The resin film of the present embodiment may be configured to have a predetermined protective film laminated thereon, and in such a case, the resin film can be used by peeling off the protective film. Examples of the support include a film made of a plastic material, a metal foil, and a release paper. Examples of films made of plastic materials that serve as supports include polyesters such as polyethylene terephthalate and polyethylene naphthalate, polycarbonate, acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, and the like. From the standpoint of availability and cost, polyethylene terephthalate and polyethylene naphthalate are preferred. Examples of the metal foil include copper foil and aluminum foil, and copper foil is preferred. The copper foil may be a foil made of a single metal such as copper, or may be a foil made of an alloy of copper and another metal (such as tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.). The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, an antistatic treatment, or a release treatment.
[0118] [Prepreg] The prepreg according to the present embodiment includes a substrate and the resin composition according to the present embodiment or a cured product thereof impregnated or applied to the substrate. That is, the prepreg according to the present embodiment is a composite of the resin composition according to the present embodiment or the cured product thereof and the substrate. The prepreg can be obtained, for example, by impregnating a substrate such as glass cloth with the varnish which is the resin composition of the present embodiment, and then removing the solvent by the drying method described above. Examples of the substrate include various glass cloths such as roving cloth, cloth, chopped mat, and surfacing mat; asbestos cloth, metal fiber cloth, and other synthetic or natural inorganic fiber cloths; woven or nonwoven fabrics obtained from liquid crystal fibers such as wholly aromatic polyamide fibers, wholly aromatic polyester fibers, and polybenzoxazole fibers; natural fiber cloths such as cotton cloth, linen cloth, and felt; natural cellulose-based substrates such as carbon fiber cloth, kraft paper, cotton paper, and cloth obtained from paper-glass blended fiber yarns; and polytetrafluoroethylene porous films. From the viewpoint of dielectric performance, glass cloth is preferred. These substrates may be used alone or in combination of two or more. The proportion of solids in the prepreg made of the resin composition of the present embodiment is preferably 30 to 80% by mass, more preferably 40 to 70% by mass. When the proportion is 30% by mass or more, the prepreg tends to have better insulation reliability when used for electronic substrates, etc. When the proportion is 80% by mass or less, the prepreg tends to have better mechanical properties such as rigidity when used for electronic substrates, etc.
[0119] [Laminate] The laminate of the present embodiment has the above-mentioned resin film and metal foil. The laminate of the present embodiment includes the cured product of the prepreg described above and a metal foil. The laminate of the present embodiment can be produced, for example, through a step (a) of laminating a resin film made of the resin composition of the present embodiment onto a substrate to form a resin layer and obtain a prepreg, a step (b) of flattening the resin layer by heating and pressurizing it to obtain a cured prepreg, and a step (c) of further forming a predetermined wiring layer made of a metal foil on the resin layer. In the step (a), the method of laminating the resin film on the substrate is not particularly limited, but for example, a method of laminating using a multi-stage press, a vacuum press, a normal pressure laminator, a laminator that heats and presses under vacuum, etc. are mentioned, and the method of using a laminator that heats and presses under vacuum is preferred. According to the method of using this laminator, even if the target electronic circuit board has a fine wiring circuit on the surface, it is possible to fill the gap between the circuits with resin without voids. In addition, lamination may be a batch type or a continuous type using a roll or the like. The prepreg constituting the laminate of the present embodiment may be in a form having a substrate and a cured product of a resin composition.
[0120] Examples of the substrate of the laminate described above include the substrate constituting the prepreg described above, as well as a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a polyphenylene ether substrate, a fluororesin substrate, etc. The surface of the substrate on which the resin layer is laminated may be roughened in advance, and the number of substrate layers is not limited.
[0121] In the step (b), the resin film and the substrate laminated in the step (a) are heated and pressurized to be flattened. The conditions can be adjusted as desired depending on the type of substrate and the composition of the resin film, but preferably, for example, the temperature is 100 to 300° C., the pressure is 0.2 to 20 MPa, and the time is 30 to 180 minutes. In the step (c), a predetermined wiring layer made of a metal foil is further formed on the resin layer produced by heating and pressing the resin film and the substrate. The method of formation is not particularly limited and includes conventionally known methods, such as subtractive etching methods and semi-additive methods. The subtractive method is a method in which an etching resist layer having a shape corresponding to the desired pattern is formed on a metal layer, and then a development process is performed to dissolve and remove the metal layer from the areas where the resist has been removed using a chemical solution, thereby forming the desired wiring. The semi-additive method is a method in which a metal coating is formed on the surface of a resin layer by electroless plating, a plating resist layer having a shape corresponding to the desired pattern is formed on the metal coating, a metal layer is then formed by electrolytic plating, and the unnecessary electroless plating layer is then removed with a chemical solution or the like to form the desired wiring layer.
[0122] In addition, holes such as via holes may be formed in the resin layer as necessary, and the method for forming the holes is not particularly limited and may be any conventionally known method, such as an NC drill, a carbon dioxide gas laser, a UV laser, a YAG laser, or plasma.
[0123] [Metal-clad laminate] The laminate of the present embodiment described above may be in the form of a plate, or may be a flexible laminate having flexibility. The laminate of the present embodiment may be a metal-clad laminate. The metal-clad laminate is obtained by laminating and curing the resin composition of the present embodiment or the prepreg of the present embodiment with a metal foil, and has a configuration in which a portion of the metal foil has been removed from the metal-clad laminate. The metal-clad laminate preferably has a configuration in which a cured prepreg (also referred to as a "cured composite") and a metal foil are laminated and adhered to each other, and is suitably used as a material for electronic circuit boards.
[0124] Examples of the metal foil include aluminum foil and copper foil. Among these, copper foil is preferred because of its low electrical resistance. The cured prepreg to be combined with the metal foil may be one or more sheets, and depending on the application, a metal foil is placed on one or both sides of the cured composite to form a laminate. Examples of the method for producing the laminate include a method in which a prepreg composed of the resin composition of the present embodiment and a substrate is formed, this is layered on a metal foil, and the resin composition is cured to obtain a laminate in which the cured prepreg and the metal foil are laminated together. One particularly preferred application of the laminate is a printed wiring board, which is preferably a metal-clad laminate having at least a portion of the metal foil removed. The printed wiring board of this embodiment can be produced by a method of pressurizing and heating the prepreg of this embodiment described above. The substrate can be the same as that described above for the prepreg. The printed wiring board contains the resin composition of this embodiment, and thus has excellent strength and electrical properties (low dielectric constant and low dielectric tangent), and can suppress the fluctuation of electrical properties due to environmental changes, and has excellent insulation reliability and mechanical properties.
[0125] [Printed Wiring Board] The printed wiring board of the present embodiment includes a cured product of the resin composition of the present embodiment. The printed wiring board of this embodiment can be produced using the resin composition and / or varnish of this embodiment described above. The printed wiring board of the present embodiment includes at least one selected from the group consisting of a cured product of the resin composition described above, a resin film including the resin composition of the present embodiment or a cured product thereof, and a prepreg which is a composite of a substrate and the resin composition or the cured product thereof. The printed wiring board of this embodiment can be used in a form including a resin-coated metal foil. EXAMPLES
[0126] Hereinafter, the present embodiment will be described in detail with reference to specific examples and comparative examples, but the present invention is not limited to the following examples in any way. First, the evaluation methods and the methods for measuring physical properties applied to the examples and comparative examples are described below.
[0127] [Method of identifying the structures of copolymer (A) and copolymer (B) and method of measuring the physical properties] ((1) Content of vinyl aromatic monomer units (styrene) in the copolymer) The copolymer before hydrogenation was used to perform proton nuclear magnetic resonance ( 1 H-NMR spectroscopy was used to measure the The measurement equipment used was JNM-LA400 (manufactured by JEOL), the solvent was deuterated chloroform, the sample concentration was 50 mg / mL, the observation frequency was 400 MHz, tetramethylsilane was used as the chemical shift standard, the pulse delay was 2.904 seconds, the number of scans was 64, the pulse width was 45°, and the measurement temperature was 26°C. The styrene content was calculated using the integrated value of the total styrene aromatic signals from 6.2 to 7.5 ppm in the spectrum.
[0128] ((2) Amount of vinyl bonds in copolymer (A) and copolymer (B) The copolymer before hydrogenation was used to perform proton nuclear magnetic resonance ( 1 The vinyl bond content was measured by 1 H-NMR. The measurement conditions and the method of processing the measurement data were the same as those in (1) above. The amount of vinyl bonds in each of copolymers (A) and (B) is calculated by calculating the integral per 1H of each bond type from the integral values of the signals assigned to 1,4-bonds and 1,2-bonds, and dividing the integral value of the 1,2-bond by the sum of the integral values of the 1,4-bonds and 1,2-bonds (the 1,2-bond is in the case of butadiene, and the 3,4-bond is in the case of isoprene).
[0129] ((3) Mass ratio of vinyl aromatic monomer units in random polymer blocks (RS) and content of polymer blocks mainly composed of vinyl aromatic monomer units (BS) The definition is as follows: BSa: Content of polymer blocks mainly composed of vinyl aromatic monomer units in copolymer (A) BSb: Content of polymer blocks mainly composed of vinyl aromatic monomer units in copolymer (B) RSa: Mass ratio of vinyl aromatic monomer units in the random polymer block of copolymer (A) RSb: Mass ratio of vinyl aromatic monomer units in the random polymer block of copolymer (B) The hydrogenated block copolymer (A) and the hydrogenated copolymer (B) were used as the measurement samples. 1Using H-NMR (Joel Resonance Corporation ECS400), the vinyl aromatic monomer units contained in each were classified into those derived from the "polymer block mainly composed of vinyl aromatic monomer units" and those derived from the "random copolymer structure composed of vinyl aromatic compounds and conjugated diene compounds." Deuterated chloroform was used as the solvent, the sample concentration was 50 mg / mL, the observation frequency was 400 MHz, tetramethylsilane was used as the chemical shift standard, the pulse delay was 2.904 seconds, the number of scans was 256, and the measurement temperature was 23°C. The amount of random and block aromatic monomer units was calculated from the integral value per 1H of each bond type from the integrated intensity of the signal assigned to aromatics, and then the total styrene content was calculated, and the styrene mass ratio in the random polymer block (hereinafter referred to as the random styrene amount) (RSa) (RSb) and the styrene block content in the copolymer (BSa) (BSb) were calculated. The calculation method is as follows. Styrene block strength (b-St strength) = (integrated value of 6.9 ppm to 6.3 ppm) / 2 Random styrene strength (r-St strength) = (integrated value of 7.5 ppm to 6.9 ppm) - 3 × (b-St) Ethylene-butylene strength (EB strength) = Total integrated value - 3 x {(b-St intensity) + (r-St intensity)} / 8 Styrene block content (BS) =104×(b-St strength) / [104×{(b-St strength)+(r-St strength)}+56×(EB strength)] Random styrene content (RS) =104×(r-St strength) / {104×(r-St strength)+56×(EB strength)}
[0130] ((4) Number average molecular weight (Mn)) The number average molecular weights of the copolymer (A) and the copolymer (B) were measured using GPC (apparatus: Tosoh HLC8220, column TSKgel SuperH-RC x 2). The solvent used was tetrahydrofuran. The measurement was performed at a temperature of 35° C. A calibration curve was prepared using commercially available standard polystyrenes with known weight average molecular weights, and the number average molecular weight converted into polystyrene was determined using the calibration curve. In the table, the number average molecular weight of copolymer (A) is designated as (Mna), and the number average molecular weight of copolymer (B) is designated as (Mnb).
[0131] (Mass ratio of copolymer (A) and copolymer (B) in (5)) The ratio of copolymer (A) to copolymer (B) was measured using a mixture of copolymer (A) and copolymer (B) using GPC (instrument: Tosoh HLC8220, column TSKgel SuperH-RC x 2). The solvent used was tetrahydrofuran. The measurement was performed at a temperature of 35° C. The mass ratio of copolymer (A) to copolymer (B) was calculated from the area ratio of the peaks due to copolymer (A) and copolymer (B).
[0132] ((6) Hydrogenation rate) The hydrogenation rates of copolymer (A) and copolymer (B) were measured by a nuclear magnetic resonance spectrometer (BRUKER, DPX-400). The hydrogenated copolymer was used to perform proton nuclear magnetic resonance ( 1 H-NMR (H-NMR) measurements. Specifically, the integral values of the signals at 4.5 to 5.5 ppm derived from the residual double bonds and the signals attributable to the hydrogenated conjugated dienes were calculated, and the ratio thereof was calculated.
[0133] ((7) Calculation of average hydrogenation rate H (%) and average vinyl bond content (V) (%) The average hydrogenation ratio (H) and the average vinyl bond content (V) were calculated by the following formulas. Average hydrogenation ratio (H) = (hydrogenation ratio of copolymer (A)) x (mass ratio of copolymer (A)) + (hydrogenation ratio of copolymer (B)) x (mass ratio of copolymer (B)) Average vinyl bond content (V) = (vinyl bond content of copolymer (A)) x (mass ratio of copolymer (A)) + (vinyl bond content of copolymer (B)) x (mass ratio of copolymer (B))
[0134] (Separation of Copolymer (A) and Copolymer (B), which are Components of Co-assembly (X)) The resin composition was separated into a low molecular weight component, copolymer (A), and a high molecular weight component, copolymer (B), using GPC [apparatus: Waters ACQUITY UPLC H-Class, columns: Waters ACQUITY APC XT900 (2.5 μm, 4.6 × 150 mm), Waters ACQUITY APC XT200 (2.5 μm, 4.6 × 75 mm), Waters ACQUITY APC XT125 (2.5 mm, 4.6 × 75 mm) in series]. The solvent used was chloroform. Based on the GPC measurement chart, the low molecular weight peak and the high molecular weight peak were separated.
[0135] [Block copolymer and resin composition materials] (Preparation of hydrogenation catalyst) In the examples and comparative examples described later, the hydrogenation catalyst used in producing the block copolymer was prepared by the following method. A reaction vessel equipped with a stirrer was purged with nitrogen and charged with 1 liter of dried and purified cyclohexane. Next, 100 mmol of bis(η5-cyclopentadienyl)titanium dichloride was added. While thoroughly stirring, an n-hexane solution containing 200 mmol of trimethylaluminum was added and reacted at room temperature for about 3 days. This produced a hydrogenation catalyst.
[0136] (Copolymer (A) and Copolymer (B)) Copolymers (A1) to (A20), copolymers (B1) to (B20), and copolymer (X1) were produced as follows.
[0137] <Production example 1: Copolymer (A1)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.493 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 15 minutes. Subsequently, a cyclohexane solution containing 48 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 32 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 20 mass%, a styrene content (Sa) of 68 mass%, a random styrene amount (RSa) of 60 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 3,000, and a number average molecular weight (Mna) of 15,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A1).
[0138] <Production example 2: Copolymer (A2)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.291 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 15 minutes. Subsequently, a cyclohexane solution containing 48 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 32 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 20 mass%, a styrene content (Sa) of 68 mass%, a random styrene amount (RSa) of 60 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 5,000, and a number average molecular weight (Mna) of 25,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A2).
[0139] <Production Example 3: Copolymer (A3)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 1.07 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 48 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 32 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 20 mass%, a styrene content (Sa) of 68 mass%, a random styrene amount (RSa) of 60 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 1,400, and a number average molecular weight (Mna) of 7,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A3).
[0140] <Production Example 4: Copolymer (A4)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 60 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.641 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.6 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 50 minutes. Then, a cyclohexane solution containing 40 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 30 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 60 mass%, a styrene content (Sa) of 60 mass%, a random styrene amount (RSa) of 0 mass%, a styrene block content (BSa) of 60 mass%, a styrene block molecular weight (MnSa) of 7,200, and a number average molecular weight (Mna) of 12,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A4).
[0141] <Production Example 5: Copolymer (A5)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.582 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.6 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 24 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 56 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 20 mass%, a styrene content (Sa) of 44 mass%, a random styrene amount (RSa) of 30 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 3,000, and a number average molecular weight (Mna) of 15,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A5).
[0142] <Production Example 6: Copolymer (A6)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.712 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.9 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 10 minutes. Subsequently, a cyclohexane solution containing 56 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 24 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 20 mass%, a styrene content (Sa) of 76 mass%, a random styrene amount (RSa) of 70 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 2,000, and a number average molecular weight (Mna) of 10,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A6).
[0143] <Production Example 7: Copolymer (A7)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 60 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.641 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 45 minutes. Then, a cyclohexane solution containing 40 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 30 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 60 mass%, a styrene content (Sa) of 60 mass%, a random styrene amount (RSa) of 0 mass%, a styrene block content (BSa) of 60 mass%, a styrene block molecular weight (MnSa) of 7,200, and a number average molecular weight (Mna) of 12,000. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the copolymer to obtain a copolymer (A7).
[0144] <Production Example 8: Copolymer (A8)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 60 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.641 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 45 minutes. Then, a cyclohexane solution containing 40 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 30 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 60 mass%, a styrene content (Sa) of 60 mass%, a random styrene amount (RSa) of 0 mass%, a styrene block content (BSa) of 60 mass%, a styrene block molecular weight (MnSa) of 7,200, and a number average molecular weight (Mna) of 12,000. Further, the hydrogenation catalyst prepared as described above was added to the obtained copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C, and the hydrogenation reaction was stopped midway. The hydrogenation rate of the resulting hydrogenated copolymer was 70%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A8).
[0145] <Production Example 9: Copolymer (A9)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.291 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 48 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 32 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 20 mass%, a styrene content (Sa) of 68 mass%, a random styrene amount (RSa) of 60 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 5,000, and a number average molecular weight (Mna) of 25,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A9).
[0146] <Production Example 10: Copolymer (A10)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 60 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 40 parts by mass of butadiene (concentration: 20% by mass) were charged. Next, 0.534 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 60 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 20 mass%, a styrene content (Sa) of 60 mass%, a random styrene amount (RSa) of 0 mass%, a styrene block content (BSa) of 0 mass%, a styrene block molecular weight (MnSa) of 0, and a number average molecular weight (Mna) of 15,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the obtained hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the copolymer to obtain a copolymer (A10).
[0147] <Production Example 11: Copolymer (A11)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.183 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 10 minutes. Subsequently, a cyclohexane solution containing 48 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 32 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 20 mass%, a styrene content (Sa) of 68 mass%, a random styrene amount (RSa) of 60 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 8,000, and a number average molecular weight (Mna) of 40,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A11).
[0148] <Production Example 12: Copolymer (A12)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.582 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.5 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 10 minutes. Subsequently, a cyclohexane solution containing 24 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 56 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 20 mass%, a styrene content (Sa) of 44 mass%, a random styrene amount (RSa) of 30 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 3,000, and a number average molecular weight (Mna) of 15,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A12).
[0149] <Production Example 13: Copolymer (A13)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.356 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 10 minutes. Subsequently, a cyclohexane solution containing 56 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 24 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 20 mass%, a styrene content (Sa) of 68 mass%, a random styrene amount (RSa) of 60 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 4,000, and a number average molecular weight (Mna) of 20,000. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the copolymer to obtain a copolymer (A13).
[0150] <Production Example 14: Copolymer (A14)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.356 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 10 minutes. Subsequently, a cyclohexane solution containing 56 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 24 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 20 mass%, a styrene content (Sa) of 68 mass%, a random styrene amount (RSa) of 60 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 4,000, and a number average molecular weight (Mna) of 20,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A14).
[0151] <Production Example 15: Copolymer (A15)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.712 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 10 minutes. Subsequently, a cyclohexane solution containing 56 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 24 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 20 mass%, a styrene content (Sa) of 68 mass%, a random styrene amount (RSa) of 60 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 2,000, and a number average molecular weight (Mna) of 10,000. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the copolymer to obtain a copolymer (A15).
[0152] <Production Example 16: Copolymer (B1)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.061 part by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.8 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 42 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 28 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Subsequently, a cyclohexane solution containing 6 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 4 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Vb) of 20 mass%, a styrene content (Sb) of 68 mass%, a random styrene amount (RSb) of 60 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 12,000, and a number average molecular weight (Mnb) of 120,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B1).
[0153] <Production Example 17: Copolymer (B2)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.080 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.8 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 42 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 28 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Then, a cyclohexane solution containing 10 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Vb) of 30 mass%, a styrene content (Sb) of 62 mass%, a random styrene amount (RSb) of 53 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 12,000, and a number average molecular weight (Mnb) of 120,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B2).
[0154] <Production Example 18: Copolymer (B3)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 30 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.128 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.8 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 30 minutes. Subsequently, a cyclohexane solution containing 30 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Subsequently, a cyclohexane solution containing 30 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 30 minutes. Then, a cyclohexane solution containing 10 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 10 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond content (Vb) of 60 mass%, a styrene content (Sb) of 60 mass%, a random styrene content (RSb) of 0 mass%, a styrene block content (BSb) of 60 mass%, a styrene block molecular weight (MnSb) of 6,000, and a number average molecular weight (Mnb) of 60,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate (H) of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B3).
[0155] <Production Example 19: Copolymer (B4)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.075 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 21 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 49 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Subsequently, a cyclohexane solution containing 3 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 7 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Vb) of 20 mass%, a styrene content (Sb) of 52 mass%, a random styrene amount (RSb) of 40 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 12,000, and a number average molecular weight (Mnb) of 120,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B4).
[0156] <Production Example 20: Copolymer (B5)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.046 part by mass of n-butyllithium per 100 parts by mass of the total monomers and 1.1 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 49 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 21 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Subsequently, a cyclohexane solution containing 7 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 3 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 20 minutes. The polymer obtained as described above had a vinyl bond amount (Vb) of 20 mass%, a styrene content (Sb) of 76 mass%, a random styrene amount (RSb) of 70 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 15,000, and a number average molecular weight (Mnb) of 150,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B5).
[0157] <Production Example 21: Copolymer (B6)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 30 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.128 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 1 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 40 minutes. Subsequently, a cyclohexane solution containing 30 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 30 minutes. Subsequently, a cyclohexane solution containing 30 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 40 minutes. Then, a cyclohexane solution containing 10 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 10 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond content (Vb) of 60 mass%, a styrene content (Sb) of 60 mass%, a random styrene content (RSb) of 0 mass%, a styrene block content (BSb) of 60 mass%, a styrene block molecular weight (MnSb) of 6,000, and a number average molecular weight (Mnb) of 60,000. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B6).
[0158] <Production Example 22: Copolymer (B7)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 30 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.128 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 1 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 40 minutes. Subsequently, a cyclohexane solution containing 30 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 30 minutes. Subsequently, a cyclohexane solution containing 30 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 40 minutes. Then, a cyclohexane solution containing 10 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond content (Vb) of 60 mass%, a styrene content (Sb) of 60 mass%, a random styrene content (RSb) of 0 mass%, a styrene block content (BSb) of 60 mass%, a styrene block molecular weight (MnSb) of 6,000, and a number average molecular weight (Mnb) of 60,000. Further, the hydrogenation catalyst prepared as described above was added to the obtained copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C, and the hydrogenation reaction was stopped midway. The hydrogenation rate of the resulting hydrogenated copolymer was 70%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B7).
[0159] <Production Example 23: Copolymer (B8)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.061 part by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.8 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 48 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 32 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Next, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 10 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Vb) of 20 mass%, a styrene content (Sb) of 68 mass%, a random styrene amount (RSb) of 60 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 12,000, and a number average molecular weight (Mnb) of 120,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B8).
[0160] <Production Example 24: Copolymer (B9)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.083 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.8 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 42 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 28 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Subsequently, a cyclohexane solution containing 6 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 4 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond content (Vb) of 20 mass%, a styrene content (Sb) of 68 mass%, a random styrene content (RSb) of 60 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 9,000, and a number average molecular weight (Mnb) of 90,000. Further, the hydrogenation catalyst prepared as described above was added to the obtained copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C, and the hydrogenation reaction was stopped midway. The hydrogenation rate of the resulting hydrogenated copolymer was 50%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B9).
[0161] <Production Example 25: Copolymer (B10)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 30 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.061 part by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.8 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 40 minutes. Subsequently, a cyclohexane solution containing 30 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 30 minutes. Subsequently, a cyclohexane solution containing 30 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 40 minutes. Then, a cyclohexane solution containing 10 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 10 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond content (Vb) of 60 mass%, a styrene content (Sb) of 60 mass%, a random styrene content (RSb) of 0 mass%, a styrene block content (BSb) of 60 mass%, a styrene block molecular weight (MnSb) of 9,000, and a number average molecular weight (Mnb) of 90,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B10).
[0162] <Production Example 26: Copolymer (B11)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 60 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 40 parts by mass of butadiene (concentration: 20% by mass) were charged. Next, 0.065 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.8 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 80 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond content (Vb) of 20 mass%, a styrene content (Sb) of 60 mass%, a random styrene content (RSb) of 60 mass%, a styrene block content (BSb) of 0 mass%, a styrene block molecular weight (MnSb) of 0, and a number average molecular weight (Mnb) of 120,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate (H) of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B11).
[0163] <Production Example 27: Copolymer (B12)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.183 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.8 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 10 minutes. Subsequently, a cyclohexane solution containing 42 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 28 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Next, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 10 minutes. Subsequently, a cyclohexane solution containing 6 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 4 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond content (Vb) of 20 mass%, a styrene content (Sb) of 68 mass%, a random styrene content (RSb) of 60 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 4,000, and a number average molecular weight (Mnb) of 40,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate (H) of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B12).
[0164] <Production Example 28: Copolymer (B13)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.107 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.6 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 48 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 32 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Vb) of 20 mass%, a styrene content (Sb) of 68 mass%, a random styrene amount (RSb) of 60 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 7,000, and a number average molecular weight (Mnb) of 70,000. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B13).
[0165] <Production Example 29: Copolymer (B14)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.107 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.6 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 48 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 32 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Vb) of 20 mass%, a styrene content (Sb) of 68 mass%, a random styrene amount (RSb) of 60 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 7,000, and a number average molecular weight (Mnb) of 70,000. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B14).
[0166] <Production Example 30: Copolymer (B15)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.107 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.6 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 42 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 28 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Subsequently, a cyclohexane solution containing 6 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 4 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Vb) of 20 mass%, a styrene content (Sb) of 68 mass%, a random styrene amount (RSb) of 60 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 7,000, and a number average molecular weight (Mnb) of 70,000. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer relative to 100 parts by mass of the copolymer to obtain a copolymer (B15).
[0167] <Production Example 31: Copolymer (X1)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 7.4 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.053 part by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.8 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 10 minutes. Subsequently, a cyclohexane solution containing 29.4 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 19.6 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 4.8 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Next, a cyclohexane solution containing 7.7 parts by mass of styrene (concentration 20% by mass), 0.153 parts by mass of n-butyllithium per 100 parts by mass of total monomers, and 0.6 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added and polymerized for 20 minutes. Subsequently, a cyclohexane solution containing 18.6 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 12.4 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above was separated by chromatography into low molecular weight components (copolymer (A)) and high molecular weight components (copolymer (B)) and analyzed. Copolymer (A) had a vinyl bond amount (Va) of 20% by mass, a styrene content (Sa) of 68% by mass, a random styrene amount (RSa) of 60% by mass, a styrene block content (BSa) of 20% by mass, a styrene block molecular weight (MnSa) of 3000, and a number average molecular weight (Mna) of 15,000. Copolymer (B) had a vinyl bond amount (Vb) of 20% by mass, a styrene content (Sb) of 68% by mass, a random styrene amount (RSb) of 60% by mass, a styrene block content (BSb) of 20% by mass, a styrene block molecular weight (MnSb) of 12000, and a number average molecular weight (Mnb) of 150,000. The content ratio of copolymer (A) to copolymer (B) was (A) / (B)=30 / 70. Further, the hydrogenation catalyst prepared as described above was added to the resulting copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C. The hydrogenation rate (H) of the resulting hydrogenated copolymer was 98%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer relative to 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (X1) which is a mixture of copolymer (A) and copolymer (B).
[0168] <Production Example 32: Copolymer (A16)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.493 parts by mass of n-butyllithium per 100 parts by mass of the total monomers, 1.2 moles of N,N,N',N'-tetramethylethylenediamine per mole of n-butyllithium, and 0.02 moles of sodium t-pentoxide per mole of n-butyllithium were added, and polymerization was carried out at 70°C for 15 minutes. Subsequently, a cyclohexane solution containing 48 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 32 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 40 mass%, a styrene content (Sa) of 68 mass%, a random styrene amount (RSa) of 60 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 3,000, and a number average molecular weight (Mna) of 15,000. Further, the hydrogenation catalyst prepared as described above was added to the obtained copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C, and the hydrogenation reaction was stopped midway. The hydrogenation rate of the resulting hydrogenated copolymer was 75%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A16).
[0169] <Production Example 33: Copolymer (A17)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.493 parts by mass of n-butyllithium per 100 parts by mass of the total monomers, 1.2 moles of N,N,N',N'-tetramethylethylenediamine per mole of n-butyllithium, and 0.02 moles of sodium t-pentoxide per mole of n-butyllithium were added, and polymerization was carried out at 70°C for 15 minutes. Subsequently, a cyclohexane solution containing 48 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 32 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 40 mass%, a styrene content (Sa) of 68 mass%, a random styrene amount (RSa) of 60 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 3,000, and a number average molecular weight (Mna) of 15,000. Further, the hydrogenation catalyst prepared as described above was added to the obtained copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C, and the hydrogenation reaction was stopped midway. The hydrogenation rate of the resulting hydrogenated copolymer was 90%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A17).
[0170] <Production Example 34: Copolymer (A18)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 20 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.493 parts by mass of n-butyllithium per 100 parts by mass of the total monomers, 1.2 moles of N,N,N',N'-tetramethylethylenediamine per mole of n-butyllithium, and 0.02 moles of sodium t-pentoxide per mole of n-butyllithium were added, and polymerization was carried out at 70°C for 15 minutes. Subsequently, a cyclohexane solution containing 48 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 32 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 45 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 40 mass%, a styrene content (Sa) of 68 mass%, a random styrene amount (RSa) of 60 mass%, a styrene block content (BSa) of 20 mass%, a styrene block molecular weight (MnSa) of 3,000, and a number average molecular weight (Mna) of 15,000. Further, the hydrogenation catalyst prepared as described above was added to the obtained copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C, and the hydrogenation reaction was stopped midway. The hydrogenation rate of the resulting hydrogenated copolymer was 60%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A18).
[0171] <Production Example 35: Copolymer (A19)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 60 parts by mass of styrene (concentration: 20% by mass) was added. Next, 1.07 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 45 minutes. Then, a cyclohexane solution containing 40 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 30 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 60 mass%, a styrene content (Sa) of 60 mass%, a random styrene amount (RSa) of 0 mass%, a styrene block content (BSa) of 60 mass%, a styrene block molecular weight (MnSa) of 4,200, and a number average molecular weight (Mna) of 7,000. Further, the hydrogenation catalyst prepared as described above was added to the obtained copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C, and the hydrogenation reaction was stopped midway. The hydrogenation rate of the resulting hydrogenated copolymer was 70%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A19).
[0172] <Production Example 36: Copolymer (A20)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 40 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.8 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.7 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 45 minutes. Subsequently, a cyclohexane solution containing 60 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 30 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Va) of 60 mass%, a styrene content (Sa) of 40 mass%, a random styrene amount (RSa) of 0 mass%, a styrene block content (BSa) of 40 mass%, a styrene block molecular weight (MnSa) of 4,800, and a number average molecular weight (Mna) of 12,000. Further, the hydrogenation catalyst prepared as described above was added to the obtained copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C, and the hydrogenation reaction was stopped midway. The hydrogenation rate of the resulting hydrogenated copolymer was 70%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (A20).
[0173] <Production Example 37: Copolymer (B16)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.061 parts by mass of n-butyllithium per 100 parts by mass of the total monomers, 1.2 moles of N,N,N',N'-tetramethylethylenediamine per mole of n-butyllithium, and 0.02 moles of sodium t-pentoxide per mole of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 42 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 28 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Subsequently, a cyclohexane solution containing 6 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 4 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Vb) of 40 mass%, a styrene content (Sb) of 68 mass%, a random styrene amount (RSb) of 60 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 12,000, and a number average molecular weight (Mnb) of 120,000. Further, the hydrogenation catalyst prepared as described above was added to the obtained copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C, and the hydrogenation reaction was stopped midway. The hydrogenation rate of the resulting hydrogenated copolymer was 75%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B16).
[0174] <Production Example 38: Copolymer (B17)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.061 parts by mass of n-butyllithium per 100 parts by mass of the total monomers, 1.2 moles of N,N,N',N'-tetramethylethylenediamine per mole of n-butyllithium, and 0.02 moles of sodium t-pentoxide per mole of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 42 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 28 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Subsequently, a cyclohexane solution containing 6 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 4 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Vb) of 40 mass%, a styrene content (Sb) of 68 mass%, a random styrene amount (RSb) of 60 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 12,000, and a number average molecular weight (Mnb) of 120,000. Further, the hydrogenation catalyst prepared as described above was added to the obtained copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C, and the hydrogenation reaction was stopped midway. The hydrogenation rate of the resulting hydrogenated copolymer was 90%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B17).
[0175] <Production Example 39: Copolymer (B18)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.061 parts by mass of n-butyllithium per 100 parts by mass of the total monomers, 1.2 moles of N,N,N',N'-tetramethylethylenediamine per mole of n-butyllithium, and 0.02 moles of sodium t-pentoxide per mole of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 42 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 28 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Subsequently, a cyclohexane solution containing 6 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 4 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Vb) of 40 mass%, a styrene content (Sb) of 68 mass%, a random styrene amount (RSb) of 60 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 12,000, and a number average molecular weight (Mnb) of 120,000. Further, the hydrogenation catalyst prepared as described above was added to the obtained copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C, and the hydrogenation reaction was stopped midway. The hydrogenation rate of the resulting hydrogenated copolymer was 60%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B18).
[0176] <Production Example 40: Copolymer (B19)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.080 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.8 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 42 parts by mass of styrene (concentration: 20% by mass) and a cyclohexane solution containing 28 parts by mass of butadiene (concentration: 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Then, a cyclohexane solution containing 10 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond amount (Vb) of 30 mass%, a styrene content (Sb) of 62 mass%, a random styrene amount (RSb) of 53 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 12,000, and a number average molecular weight (Mnb) of 120,000. Further, the hydrogenation catalyst prepared as described above was added to the obtained copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C, and the hydrogenation reaction was stopped midway. The hydrogenation rate of the resulting hydrogenated copolymer was 70%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B19).
[0177] <Production Example 41: Copolymer (B20)> Batch polymerization was carried out using a tank-type reactor (internal volume: 10 L) equipped with a stirrer and a jacket. A cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added. Next, 0.078 parts by mass of n-butyllithium per 100 parts by mass of the total monomers and 0.6 mol of N,N,N',N'-tetramethylethylenediamine per 1 mol of n-butyllithium were added, and polymerization was carried out at 70°C for 20 minutes. Subsequently, a cyclohexane solution containing 35 parts by mass of styrene (concentration 20% by mass) and a cyclohexane solution containing 35 parts by mass of butadiene (concentration 20% by mass) were added and polymerization was carried out for 60 minutes. Subsequently, a cyclohexane solution containing 10 parts by mass of styrene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Then, a cyclohexane solution containing 10 parts by mass of butadiene (concentration: 20% by mass) was added and polymerization was carried out for 20 minutes. Thereafter, methanol was added to terminate the polymerization reaction. The polymer obtained as described above had a vinyl bond content (Vb) of 30 mass%, a styrene content (Sb) of 55 mass%, a random styrene content (RSb) of 44 mass%, a styrene block content (BSb) of 20 mass%, a styrene block molecular weight (MnSb) of 12,000, and a number average molecular weight (Mnb) of 120,000. Further, the hydrogenation catalyst prepared as described above was added to the obtained copolymer in an amount of 100 ppm (Ti standard) per 100 parts by mass of the copolymer, and a hydrogenation reaction was carried out at a hydrogen pressure of 0.7 MPa and a temperature of 80°C, and the hydrogenation reaction was stopped midway. The hydrogenation rate of the resulting hydrogenated copolymer was 70%. Next, 0.3 parts by mass of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate was added as a stabilizer based on 100 parts by mass of the hydrogenated copolymer to obtain a copolymer (B20).
[0178] <Production Example 42: Polyphenylene ether (PPE)> As a polar resin, polyphenylene ether resin (PPE) was polymerized as follows. In a 1.5-liter jacketed reactor equipped with a sparger for introducing oxygen-containing gas at the bottom of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor, 0.2512 g of cupric chloride dihydrate, 1.1062 g of 35% hydrochloric acid, 3.6179 g of di-n-butylamine, 9.5937 g of N,N,N',N'-tetramethylpropanediamine, 211.63 g of methanol and 493.80 g of n-butanol, and 180.0 g of 2,6-dimethylphenol containing 5 mol% of 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane were placed. The composition mass ratio of the solvent used was n-butanol:methanol=70:30. Then, oxygen was introduced into the reactor through the sparger at a rate of 180 ml / min with vigorous stirring, and the polymerization temperature was adjusted to maintain 40°C by passing a heat medium through the jacket. The polymerization solution gradually took on the form of a slurry. When the polyphenylene ether reached the desired number average molecular weight, the oxygen-containing gas was stopped and the resulting polymerization mixture was heated to 50° C. Then, hydroquinone (a reagent manufactured by Wako Pure Chemical Industries, Ltd.) was added little by little, and the mixture was kept warm at 50° C. until the slurry-like polyphenylene ether turned white. Then, 720 g of a methanol solution containing 6.5 mass % of 36% hydrochloric acid was added, filtered, and repeatedly washed with methanol to obtain wet polyphenylene ether. Then, the mixture was vacuum dried at 100°C to obtain dry polyphenylene ether. ηsp / c was 0.103 dl / g, and the yield was 97%. The ηsp / c was measured by dissolving the polyphenylene ether in chloroform at 0.5 g / dl and measuring the reduced viscosity (ηsp / c) at 30°C using an Ubbelohde viscometer. The unit is dl / g. The resulting polyphenylene ether was modified as follows. 152.5g of polyphenylene ether and 152.5g of toluene were mixed and heated to about 85°C. 2.1g of dimethylaminopyridine was then added. When all the solids had dissolved, 18.28g of methacrylic anhydride was slowly added. The resulting solution was maintained at 85°C for 3 hours with continuous mixing. The solution was then cooled to room temperature to obtain a toluene solution of methacrylate-capped polyphenylene ether. The resulting toluene solution was added dropwise to a cylindrical 3L SUS container equipped with a homogenizer for stirring, and 1000mL of 10°C methanol was added dropwise in small portions. The resulting powder was filtered, washed with methanol, and dried at 85° C. under nitrogen for 18 hours.
[0179] [Examples and Comparative Examples Using Maleimide Resin as Curable Resin] (Examples 1 to 28, Comparative Examples 1 to 9) In addition to the above-mentioned components, the following components were further used to prepare resin compositions according to the following preparation method. <Component (I): Cured resin> [Polyimide resin] Bis(3-ethyl-5-methyl-4-maleimidophenyl)methane (BMI-70) (K.I. Chemicals Co., Ltd.) 4,4'-Bismaleimidodiphenylmethane (BMI-H) (K.I. Chemicals Co., Ltd.) <Component (III): Hardener> Cyanate ester curing agent 2,2-bis(4-cyanatephenyl)propane (Tokyo Chemical Industry Co., Ltd.)
[0180] The blending amounts of copolymer (A) and copolymer (B) are expressed as mass fractions (% by mass) relative to the total amount (100% by mass) of copolymer (A) and copolymer (B). The amounts of the components (I) to (III) are expressed in parts by mass when the total amount of the copolymer (A) and the copolymer (B) is taken as 100 parts by mass.
[0181] The ratios of the components used in the examples and comparative examples, and their respective physical properties, are shown in the table below. First, the polyimide resin (curable resin) and the cyanate ester curing agent were dissolved at 160°C in the mixing ratio shown in the table below, and reacted for 6 hours with stirring to obtain a bismaleimide-triazine resin oligomer. The obtained bismaleimide-triazine resin oligomer was dissolved in toluene, and the remaining components were added and stirred to dissolve, to prepare a varnish with a concentration of 20% by mass to 50% by mass. The varnish of the resin composition was impregnated into a glass substrate (L2116, #2116 type, "L Glass", manufactured by Asahi Kasei Corporation), and then heated and dried at 130°C for 50 minutes to obtain a prepreg. Six of the obtained prepregs were stacked together, heated to 200°C at a heating rate of 5°C / min, and heated and pressurized at 200°C for 2 hours at a pressure of 3 MPa to obtain a cured prepreg with a thickness of 0.7 mm.
[0182] (Evaluation Criteria for Examples 1 to 28 and Comparative Examples 1 to 9) <(1) Varnish solubility> Toluene was added to resin compositions prepared according to the formulations shown in the table below so that the solid content concentrations were 20% by mass and 50% by mass, respectively, and the mixture was stirred at 40° C. for 120 minutes. These solutions were used as evaluation samples and were evaluated according to the following three-level scale. [Evaluation Criteria] ◯: No residual solids were found in either solution with a solid content of 20% by mass or 50% by mass. △: Only the solution with a solid content of 20% by mass had no residual solids. ×: Residual residues remain in both solutions.
[0183] <(2) Storage stability of varnish> The varnishes of the resin compositions of the Examples and Comparative Examples prepared as described above were left to stand at 30°C / 50% RH, and their condition was observed. The number of days until layer separation and / or precipitation of a gel-like component occurred and the presence or absence of such separation were evaluated according to the following criteria. In the table, "-" indicates that the varnish could not be evaluated because some of the varnish remained undissolved during preparation. [Evaluation Criteria] ◎: 720 hours or more (including no precipitation) ○: 360 to less than 720 hours △:24~360 hours ×: Less than 24 hours
[0184] <(3) Dielectric properties> The dielectric loss tangent of the obtained prepreg at 10 GHz was measured by a cavity resonance method. The measurement devices used were a network analyzer (N5230A, manufactured by Agilent Technologies) and a cavity resonator (Cavity Resonator CP series) manufactured by Kanto Electronics Application Development Co., Ltd. The measurement samples were test pieces measuring 2.6 mm wide x 80 mm long cut out from the cured prepreg described in the preparation method described above. The evaluation was based on the difference in dielectric tangent and dielectric constant between Comparative Example 9, which does not contain copolymer (A) and copolymer (B), and each Example or Comparative Example (Comparative Example 9 - Example or Comparative Example). In the table, "-" indicates that the varnish could not be evaluated because some of the varnish remained undissolved during preparation. [Evaluation Criteria] Dissipation factor (Df) ◎: 0.001 or more ○: 0.0007 or more, less than 0.001 △: 0.0005 or more, less than 0.0007 ×: Less than 0.0005 Dielectric constant (Dk) ◎: 0.1 or more ○: 0.07 or more, less than 0.1 △: 0.04 or more, less than 0.07 ×: Less than 0.04
[0185] <(4) CTE measurement (coefficient of linear thermal expansion)> The CTE of the resin composition was measured in a temperature range of 50 to 250° C. in a direction perpendicular to the thickness direction. The measurements were performed using the thermal mechanical analysis method (TMA method) based on IPC TM650 2.4.41. The evaluation was performed based on the ratio of CTE of each Example or Comparative Example to that of Comparative Example 9 not containing the copolymer (A) or the copolymer (B) (Example or Comparative Example ÷ Comparative Example 9). In the table, "-" indicates that the varnish could not be evaluated because some of the varnish remained undissolved during preparation. [Evaluation Criteria] ◎: Less than 110% ○: 110% or more, less than 115% △: 115% or more, less than 120% ×: 120% or more
[0186] <(5) Adhesion to copper foil (peel strength)> Each resin composition described below was applied to a polyimide film, the solvent was dried off, and then a 35 μm thick copper foil was placed on top of the polyimide film. The resulting film was heated and pressed at 100° C. and 1 MPa for 2 minutes to laminate the copper foil, producing a laminate consisting of a polyimide film, resin composition, and copper foil. The laminate was heated at 180° C. for 1 hour to cure the resin composition, and the cured laminate was used as an adhesive sample. A 1 cm wide cut was made in the laminate, and a peel strength test was performed in which the copper foil was peeled off in a 90° direction at a pulling speed of 50 mm / min. A higher peel strength value indicates higher adhesion. The measurement results were evaluated according to the following criteria. In the table, "-" indicates that the varnish could not be evaluated because some of the varnish remained undissolved during preparation. [Evaluation Criteria] ◎:0.8N / mm or more ○: 0.6N / mm or more, less than 0.8N / mm △: 0.4N / mm or more, less than 0.6N / mm ×: Less than 0.4N / mm
[0187] <(6) Presence or absence of cracks> The varnish of the resin composition obtained above was applied to a low dielectric glass cloth having a thickness of 0.069 mm by impregnation, and then heated and dried at 165°C for 5 minutes using a dryer (a pressure-resistant explosion-proof steam dryer manufactured by Takasugi Seisakusho Co., Ltd.) to obtain a prepreg having a resin composition content of 30% by mass. Two sheets of this prepreg were stacked, 12 μm copper foil (3EC-M3-VLP, manufactured by Mitsui Mining & Smelting Co., Ltd.) was placed on both sides, and a pressure of 30 kg / cm was applied. 2 The laminate was vacuum pressed at a temperature of 210° C. for 150 minutes to obtain a copper-clad laminate (metal foil-clad laminate) having a thickness of 0.2 mm.
[0188] Two of the obtained copper-clad laminates were stacked together, with a 0.1 mm thick aluminum foil placed on top and a 1.5 mm thick paper-based phenolic resin laminate (FL-101, manufactured by Futamura Chemical Co., Ltd.) placed underneath. Using a drill with a diameter of 0.2 mm (ND-1V212, manufactured by Hitachi Via Mechanics Co., Ltd.), five via holes were created at random locations under conditions of a rotation speed of 160 krpm, a feed speed of 2 m / min, and a chip load of 12.5 μm / rev, and the presence or absence of cracks was evaluated by SEM observation.
[0189] [Whether or not cracks occur] The occurrence of cracks at the bottom of the five via holes was observed from SEM images. The fewer the cracks, the better the drilling workability was, and the evaluation was performed as follows. In the table, "-" indicates that the varnish could not be evaluated because some of the varnish remained undissolved during preparation. 〇: No cracks Δ: A few cracks remain, but the number of cracks is reduced as compared with Comparative Example 9 which does not contain the copolymer (A) or the copolymer (B). ×: Cracks were observed, and the number of cracks was equal to or greater than that in Comparative Example 9 which did not contain the copolymer (A) or the copolymer (B).
[0190] <(7) Solder heat resistance> The copper-clad laminate obtained above was immersed in a solder bath at 288°C, and the time required for the copper-clad laminate to develop appearance defects such as swelling and peeling was measured and evaluated according to the following evaluation criteria. In the table, "-" indicates that the varnish could not be evaluated because some of the varnish remained undissolved during preparation. ○: After immersion, appearance or worse appears within 30 seconds. △: After immersion, appearance worse than normal occurs within 30 seconds to less than 1 minute. ×: No visible damage occurred for 1 minute or more after immersion.
[0191] The evaluation results of Examples 1 to 28 and Comparative Examples 1 to 9 are shown in the following table. In the table below, the block structure is shown below. a, d: Polymer blocks mainly composed of vinyl aromatic monomer units b1, b2, e: Random polymer blocks consisting of vinyl aromatic monomer units and conjugated diene monomer units c1, c2, f: polymer blocks mainly composed of conjugated diene monomer units
[0192] [Table 1]
[0193] [Table 2]
[0194] [Table 3]
[0195] [Table 4]
[0196] [Table 5]
[0197] [Examples and Comparative Examples Using PPE as the Cured Resin] (Examples 29 to 34, Comparative Examples 10 to 11) Resin compositions were prepared using the following components according to the following preparation method. <Copolymer (A)> Copolymers (A1) to (A4) prepared in Production Examples 1 to 4 <Copolymer (B)> Copolymers (B1) to (B3) prepared in Production Examples 16 to 18 <Component (I): Cured resin> PPE produced in Example 42 <Component (II): Radical initiator> Perbutyl P (NOF Corporation) <Component (III): Hardener> Triallyl isocyanurate (TAIC TM ) (Mitsubishi Chemical Corporation)
[0198] The blending amounts of copolymer (A) and copolymer (B) are expressed as mass fractions (% by mass) relative to the total amount (100% by mass) of copolymer (A) and copolymer (B). The amounts of the components (I) to (III) are expressed in parts by mass when the total amount of the copolymer (A) and the copolymer (B) is taken as 100 parts by mass.
[0199] <Preparation of resin composition and varnish> Using the above-mentioned copolymer (A) and copolymer (B), and also using the above-mentioned components (I), (II), and (III), each component was measured out into a container in the proportions shown in the table below, dissolved in toluene (manufactured by Wako Pure Chemical Industries, Ltd.), and stirred to prepare a varnish containing a resin composition. When preparing the film, the viscosity was adjusted by changing the amount of toluene added. At that time, the concentration of the resin composition in the varnish was adjusted to 40 to 60% by mass.
[0200] <Preparation of prepreg using varnish and cured prepreg> A varnish of a resin composition prepared according to the formulation shown in the table below was impregnated into a glass substrate (L2116, #2116 type, "L Glass", manufactured by Asahi Kasei Corporation), and then heated and dried at 130°C for 50 minutes to obtain a prepreg. Six of the obtained prepregs were stacked together, heated to 200°C at a heating rate of 5°C / min, and heated and pressurized at 200°C for 2 hours at a pressure of 3 MPa to obtain a cured prepreg with a thickness of 0.7 mm.
[0201] (Evaluation Criteria for Examples 29 to 34 and Comparative Examples 10 to 11) <(1) Varnish solubility> Toluene was added to each of the resin compositions prepared according to the formulations shown in the table below so that the solid content concentrations were 20% by mass and 50% by mass, respectively, and the mixture was stirred at 40° C. for 120 minutes to obtain a solution. The solutions were rated on a three-point scale. In the table, "-" indicates that the varnish could not be evaluated because some of the varnish remained undissolved during preparation. [Evaluation Criteria] ◯: No residual solids were found in either solution with a solid content of 20% by mass or 50% by mass. △: Only the solution with a solid content of 20% by mass had no residual solids. ×: Residual residues remain in both solutions.
[0202] <(2) Dielectric properties> The dielectric loss tangent of the obtained prepreg at 10 GHz was measured by the cavity resonance method. A network analyzer (N5230A, manufactured by Agilent Technologies) and a cavity resonator (Cavity Resonator CP series) manufactured by Kanto Electronics Application Development Co., Ltd. were used as measuring devices, and a test piece of 2.6 mm wide x 80 mm long was cut out from the cured film described in the preparation method above and measured. The evaluation was based on the difference in dielectric tangent and dielectric constant between Comparative Example 11, which does not contain copolymer (A) and copolymer (B), and each Example or Comparative Example (Comparative Example 11 - Example or Comparative Example). In the table, "-" indicates that the varnish could not be evaluated because some of the varnish remained undissolved during preparation. [Evaluation Criteria] Dissipation factor (Df) ◎: 0.0013 or more ○: 0.0011 or more, less than 0.0013 △: 0.0009 or more, less than 0.0011 ×: Less than 0.0009 Dielectric constant (Dk) ◎: 0.20 or more ○: 0.15 or more, less than 0.20 △: 0.10 or more, less than 0.15 ×: Less than 0.10
[0203] ((3) CTE measurement (coefficient of linear thermal expansion)) The CTE of the resin composition was measured in a temperature range of 50 to 250° C. in a direction perpendicular to the thickness direction. The measurements were performed using the thermal mechanical analysis method (TMA method) based on IPC TM650 2.4.41. The evaluation was performed based on the ratio of CTE of each Example or Comparative Example to Comparative Example 11 not containing the copolymer (A) or the copolymer (B) (Example or Comparative Example ÷ Comparative Example 11). In the table, "-" indicates that the varnish could not be evaluated because some of the varnish remained undissolved during preparation. [Evaluation Criteria] ◎: Less than 110% ○: 110% or more, less than 115% △: 115% or more, less than 120% ×: 120% or more
[0204] In the table below, the block structure is shown below. a, d: Polymer blocks mainly composed of vinyl aromatic monomer units b1, b2, e: Random polymer blocks consisting of vinyl aromatic monomer units and conjugated diene monomer units c1, c2, f: polymer blocks mainly composed of conjugated diene monomer units
[0205] [Table 6]
[0206] [Table 7]
[0207] It was found that the cured product obtained by combining the copolymer (A) and the copolymer (B) of the embodiment had an excellent balance of dielectric performance and heat resistance. It was found that the cured product of the present invention is suitable for use in printed wiring boards using glass cloth and metal laminates. [Industrial Applicability]
[0208] The resin composition and cured product of the present invention have industrial applicability as materials for films, prepregs, electronic circuit boards, and next-generation communication boards.
Claims
1. A copolymer (A) having vinyl aromatic monomer units and conjugated diene monomer units; A copolymer (B) having vinyl aromatic monomer units and conjugated diene monomer units; At least one component selected from the group consisting of the following components (I) to (III): Contains All of the following conditions (1) to (6) are met. Resin composition. Component (I): Cured resin (excluding copolymer (A) and copolymer (B)) Component (II): Radical initiator Component (III): Curing agent (excluding component (I)) <Condition (1)>: The number average molecular weight of the copolymer (A) is 30,000 or less. <Condition (2)>: The copolymer (A) has at least one polymer block mainly composed of vinyl aromatic monomer units. <Condition (3)>: The copolymer (B) has at least one polymer block mainly composed of vinyl aromatic monomer units. <Condition (4)>: The number average molecular weight of the copolymer (B) is 50,000 or more. <Condition (5)>: The content (Sa) (mass%) of vinyl aromatic monomer units in the copolymer (A); The difference (ΔS) between the content (Sb) (mass%) of the vinyl aromatic monomer unit of the copolymer (B) is The following relationship is satisfied. ΔS=|Sa−Sb|≦25 <Condition (6)>: The average content of vinyl aromatic monomer units in the copolymer (A) and the copolymer (B) is 50 mass % or more.
2. The average hydrogenation rate (H) (%) of the unsaturated double bonds derived from the conjugated diene compound contained in the copolymer (A) and the copolymer (B) and the average vinyl bond content (V) (%) are The following relationship is satisfied: The resin composition according to claim 1. V+10≦H
3. The copolymer (B) is a block copolymer represented by any one of the general structures: a1-b1-a2-c1, a1-b1-a2-b2, a1-c1-a2-c2, and a1-c1-a2-b1, The a1 block and the a2 block are polymer blocks mainly composed of vinyl aromatic monomer units, The b1 block and the b2 block are random polymer blocks composed of vinyl aromatic monomer units and conjugated diene monomer units, The c1 block and the c2 block are polymer blocks mainly composed of conjugated diene monomer units. The resin composition according to claim 1.
4. The ratio (Mnb / Mna) of the number average molecular weight (Mnb) of the copolymer (B) to the number average molecular weight (Mna) of the copolymer (A) is greater than 4; The resin composition according to claim 1.
5. The hydrogenation rate of the unsaturated double bonds derived from the conjugated diene in the copolymer (A) is 55% or more and 95% or less. The resin composition according to claim 1.
6. The hydrogenation rate of the unsaturated double bonds derived from the conjugated diene in the copolymer (B) is 55% or more and 95% or less. The resin composition according to claim 1.
7. The copolymer (A) is a block copolymer represented by the general structural formula: d-f, d is a polymer block mainly composed of vinyl aromatic monomer units, f is a polymer block mainly composed of conjugated diene monomer units; The resin composition according to claim 1.
8. A cured product of the resin composition according to any one of claims 1 to 7.
9. A printed wiring board comprising the cured product according to claim 8.
10. A resin film comprising the cured product according to claim 8.
11. A substrate; The resin composition according to any one of claims 1 to 7, Prepreg is a composite material.
12. A substrate; The cured product according to claim 8 , Prepreg is a composite material.
13. The substrate is a glass cloth. The prepreg according to claim 11.
14. The substrate is a glass cloth. The prepreg according to claim 12.
15. A cured product of the resin film according to claim 10; Metal foil; A laminate having the following structure:
16. A cured product of the prepreg according to claim 11; Metal foil; A laminate having the following structure:
17. A cured product of the prepreg according to claim 12; Metal foil; A laminate having the following structure:
18. A printed wiring board comprising the resin film according to claim 10.
19. A printed wiring board comprising the prepreg of claim 13.
20. A printed wiring board comprising the prepreg of claim 14.
Citation Information
Patent Citations
Resin composition
JP2020015861A
Polyphenylene ether resin composition
JP2021147486A