ink

The ink formulation with a specific SP value and monomer composition addresses ink durability and stability issues, providing enhanced scratch resistance and circulation stability in inkjet recording devices.

JP2024146796APending Publication Date: 2024-10-15NIPPON KAYAKU CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024037155
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-11
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Inkjet recording devices face challenges with ink durability and circulation stability, particularly in commercial and office printing, where there is a need for inks with excellent scratch resistance and stability to prevent ink deterioration and colorant sedimentation.

Method used

An ink formulation containing an organic solvent and a binder with an SP value between 9.8 and 12.3, incorporating specific monomers like C1-C4 hydroxyalkyl (meth)acrylate, and a glass transition temperature of 35 to 150°C, along with a water-octanol partition coefficient of 2.00 to 3.50, enhances circulation stability and scratch resistance.

Benefits of technology

The ink exhibits improved circulation stability and scratch resistance, ensuring durable and stable ink performance in inkjet recording devices, particularly in non-absorbent recording materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146796000001
    Figure 2024146796000001
  • Figure 2024146796000002
    Figure 2024146796000002
  • Figure 2024146796000003
    Figure 2024146796000003
Patent Text Reader

Abstract

To provide an ink for various recording applications, particularly for inkjet printing, characterized by superior circulation stability and scratch resistances in printed materials, as well as printed materials containing the inkjet ink.SOLUTION: An ink includes an organic solvent and a binder, the binder having an SP value of 9.8 or more and 12.3 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ink that is suitable for use in a recording method using an inkjet printer (inkjet recording method). [Background technology]

[0002] In recent years, inkjet recording apparatuses have been increasingly used in the fields of commercial printing and office printing, where inks that produce images with excellent abrasion resistance are in demand. On the other hand, in order to prevent deterioration of the ink and sedimentation of the coloring material and to improve the ejection stability of the ink, inkjet recording devices equipped with ink-circulating inkjet heads have been increasingly used in recent years, and inks with excellent abrasion resistance and circulation stability are in demand. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. WO2022 / 203041 [Patent Document 2] JP 2021-021042 A [Patent Document 3] JP 2022-146196 A [Patent Document 4] Patent No. 6560846 [Patent Document 5] Patent No. 6391721 [Patent Document 6] JP 2017-185716 A [Patent Document 7] Patent Publication No. 2022-52563 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide an ink having good circulation stability and excellent abrasion resistance of printed matter, an inkjet recording method using the inkjet ink, an ink set comprising the inkjet ink, an ink media set comprising the inkjet ink or the ink set and a printed medium, and a printed medium to which the inkjet ink or each inkjet ink of the ink set is adhered. [Means for solving the problem]

[0005] Means for Solving the Problems The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved by an ink containing an organic solvent and a binder, wherein the SP value of the binder is in the range of 9.8 or more and 12.3 or less, and have thus completed the present invention.

[0006] That is, the present invention relates to the following 1) to 9). 1) An ink comprising an organic solvent and a binder, the SP value of the binder being in the range of 9.8 or more and 12.3 or less. 2) The ink according to 1), wherein the binder contains a (meth)acrylic monomer as a constituent monomer. 3) The ink according to 1) or 2), wherein the binder contains a C1-C4 hydroxyalkyl (meth)acrylate as a constituent monomer, and the content of the C1-C4 hydroxyalkyl (meth)acrylate is 0.1 to 25 mass% based on the total mass of the binder solids. 4) The ink according to any one of 1) to 3), wherein the acid value of the binder is 5 to 150 mgKOH / g. 5) The ink according to any one of 1) to 4), wherein the binder has a Tg of 35 to 150°C. 6) The ink according to any one of 1) to 5), wherein the binder has a weight average molecular weight of 30,000 to 120,000. 7) The ink according to any one of 1) to 6), wherein the organic solvent has a water-octanol partition coefficient of 2.00 or more and less than 3.50. 8) The ink according to any one of 1) to 7), wherein the organic solvent comprises a C4-C12 alkanediol. 9) The ink according to any one of 1) to 8), further comprising a wax, the content of the wax being 0.01 to 1.0% by mass relative to the total mass of the ink. 10) A set of an ink and an overcoat agent, the set comprising the ink according to any one of 1) to 9) above, and an overcoat agent containing an organic solvent and a binder, the SP value of the binder being in the range of 9.8 or more and 12.3 or less. 11) 10) A recording medium on which an image is formed using a set of the ink and overcoat agent described in 10). 12) A method for producing a recording medium, comprising forming an image on a recording medium using the ink according to any one of 1) to 9), and then covering a part or all of the image-formed portion with the overcoat agent according to 10). Effect of the Invention

[0007] The present invention provides an ink that has good circulation stability and excellent abrasion resistance of printed matter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, specific embodiments to which the present invention is applied will be described in detail. In this specification, "CI" means "Color Index." In addition, in this specification, including the examples, "%" and "parts" are all based on mass unless otherwise specified.

[0009] <Ink> The ink according to this embodiment contains an organic solvent and a binder, and the SP value of the binder is in the range of 9.8 to 12.3. The components contained in the ink according to this embodiment will be described in detail below. Note that each of the components described below may be used alone or in combination of two or more.

[0010] <Organic solvent> The ink contains an organic solvent as an essential component. The water-octanol partition coefficient of the organic solvent is preferably 2.00 or more and less than 3.50, more preferably 2.40 to 3.00. In this specification, the "water-octanol partition coefficient" refers to a ClogP value calculated using ChemDraw Professional ver.16.0 manufactured by Perkin Elmer. The number of decimal places of the calculated value is not constant. For this reason, in this specification, the third decimal place is rounded off and the value is described to the second decimal place. In addition, when the calculated value is to the second decimal place, the value is described as it is. In addition, when the calculated value does not have two decimal places, the values ​​of each digit to the second decimal place are regarded as "zero" and all are described to the second decimal place. Hereinafter, the "water-octanol partition coefficient" may be described as the "ClogP value".

[0011] Examples of organic solvents having a ClogP value of 2.00 or more and less than 3.50 include 1,2-nonanediol (2.11), 2-propylheptane-1,3-diol (2.31), ethylene glycol monoheptyl ether (2.43), ethylene glycol diisobutyl ether (2.55), dibutyl diglycol (2.63), 1,2-decanediol (2.64), 2-[2-(2-ethylhexyloxy)ethoxy]ethanol (2.65), diisobutyl Examples include ethylene glycol dibutyl ether (2.81), 2,6-dimethyl-4-heptanol (2.99), 3,5,5-trimethyl-1-hexanol (3.08), 2-butoxyethyl benzoate (3.43), and diethylene glycol monobutyl ether adipate (3.49). The values ​​in parentheses are ClogP values.

[0012] The content of the organic solvent having a ClogP value of 2.00 or more and less than 3.50 is usually preferably 0.1% by mass to 15.0% by mass, more preferably 0.4% by mass to 10.0% by mass, and even more preferably 0.8% by mass to 5.0% by mass, based on the total weight of the ink.

[0013] By containing 0.1 mass % to 15.0 mass % of an organic solvent having a ClogP value of 2.00 or more but less than 3.50, relative to the total weight of the ink, and by containing a binder within the range of the present invention, the drying behavior changes, resulting in a stronger film of the printed matter and significantly improved abrasion resistance.

[0014] [C4-C12 Alkanediol] The ink preferably contains a C4-C12 alkanediol, preferably a 1,2-(C4-C12) alkanediol. Alkanediols having C7 or more are generally considered to be poorly water-soluble. Specific examples thereof include 1,2-heptanediol, 1,2-octanediol, 5-methyl-1,2-hexanediol, 4-methyl-1,2-hexanediol, and 4,4-dimethyl-1,2-pentanediol. Among these, 1,2-octanediol is preferred. In addition, C6 or lower alkanediols are generally considered to be water-soluble. Specific examples include 1,2-hexanediol, 1,2-pentanediol, 1,2-butanediol, 4-methyl-1,2-pentanediol, 3,3-dimethyl-1,2-butanediol, etc. Although all of these are preferable, 1,2-hexanediol is more preferable in terms of less odor problems in the working environment. The content of the C4-C12 alkanediol in the total mass of the ink is usually 0.1 to 20%, preferably 0.5 to 18%, and more preferably 0.5 to 15%.

[0015] <Binder> The ink contains a binder as an essential component. Examples of the binder include one or more selected from condensation polymers such as polyurethane and polyester; and vinyl polymers such as (meth)acrylic resins, styrene resins, acrylic-styrene resins, butadiene resins, styrene-butadiene resins, vinyl chloride resins, vinyl acetate resins, and acrylic silicone resins. From the viewpoints of ejection stability, drying properties, and abrasion resistance, it is preferable that the binder is a vinyl resin and the constituent monomer is a (meth)acrylic monomer.

[0016] The (meth)acrylic monomer is not particularly limited, and examples thereof include (meth)acrylic acid, carboxylic acids having a carbon-carbon double bond such as β-carboxyethyl acrylate, (meth)acrylic acid esters such as methyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate, (meth)acrylic acid esters having a hydroxyl group such as 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, (meth)acrylates having an allyl group such as allyl acrylate and allyl methacrylate, ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, and the like. di(meth)acrylate compounds linked by an alkyl chain, such as polyoxyethylene (2)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (4)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (5)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (6)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (7)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (8)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (9)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (10)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (11)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (12)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (13)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (14)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (15)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (16)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (17)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (18)-2,2-bis(4-hydroxyphenyl)propane di(meth)acrylate, polyoxyethylene (19 ... The binder preferably contains a C1-C4 hydroxyalkyl (meth)acrylate as a constituent monomer.

[0017] The SP value of the binder is in the range of 9.8 or more and 12.3 or less, more preferably in the range of 9.9 or more and 11.8 or less, even more preferably in the range of 10.0 or more and 11.3 or less, particularly preferably in the range of more than 10.0 and 11.3 or less, and extremely preferably in the range of 10.3 or more and 11.0 or less.

[0018] The SP value (solubility parameter) was introduced by Hildebrand and is a value defined by regular solution theory, and is a physical property that serves as a guide to compatibility. The evaporation energy per mole of liquid is ΔE V [Unit: kcal mol ー1 ] and its molar volume is Vm [unit: cm 3 mol ー1 ], then the SP value δ [unit: (cal / cm 3 ) 0.5 ] is defined by the following formula (A). δ = (ΔE V / Vm) 1 / 2 (A)

[0019] The δ value (SP value) is used as a physical and chemical constant that indicates the magnitude of intermolecular interactions in liquids. V The δ values ​​at room temperature calculated from the values ​​have been reported for many compounds (e.g., Hoy, KL, The Hoy Tables of Solubility Parameters, Union Carbide Corporation, Solvents and Coatings Materials Division, South Charlston, WV, 1985).

[0020] On the other hand, for substances that do not sublimate, such as resin particles, or for substances that have no observable boiling point, such as thermally decomposable compounds, the cohesion can be estimated by the group contribution method proposed by Hoy (Allan FM Barton, CRC Handbook of Solubility Parameters and Other Cohesion Parameters 2nd ed., CRC Press (1991), p. 165-167).

[0021] The SP value can also be experimentally measured by turbidimetric titration, which has been proposed by KW Suh, DHC Arke et al. in the following references 1 and 2. [Reference 1]: KWSuh, DHClarke, J. Polym. Sci., 1671, 1967 [Reference 2]:KWSuh,JMCorbett.J.Appl.Poym.Sci.,2359,1968

[0022] According to the above-mentioned turbidimetric titration method, the SP value can be measured, for example, in accordance with the following procedure (procedures 1 and 2).

[0023] [Step 1]: Hydrogenation of hydrophilic groups of resin particles (preparation of SP value measurement sample) (1) 200 mL of the resin particle dispersion is placed in a dialysis membrane (product name "MWCO's 0.5 m of 3.5-5 kD Biotech RC", manufactured by SPECTRUM LABORATORIES, Inc.) and immersed in 10 L of hydrochloric acid (pH 3 ± 0.5). The membrane is immersed for 24 hours with magnetic stirring to replace cations such as amines and alkali metals with hydrogen ions. (2) The resin particles are immersed in 12 L of ion-exchanged water (pH 7±0.5) while still in the dialysis membrane. The resin particles are neutralized by soaking for 24 hours with magnetic stirring. (3) After replacing the ion-exchanged water, immerse for an additional 6 hours with magnetic stirring and confirm that the pH of the ion-exchanged water is 7±0.5. (4) Immerse in 2 L of ethanol for 8 hours and remove moisture with magnetic stirring. (5) The resin particles removed from the dialysis membrane are placed in a dry 500 mL beaker and dried under reduced pressure for 6 hours while maintaining the temperature at 80°C to remove the ethanol. (6) The completely dried resin particles are ground to obtain a powder, which is used as a dry resin particle sample.

[0024] [Step 2]: Measuring the SP value (1) Weigh out 0.500 g ± 0.005 g of a dry resin particle sample into a 50 mL Erlenmeyer flask. (2) Add 10 mL of tetrahydrofuran (THF) and dissolve the dried resin particle sample to prepare a sample solution. (3) Cool the prepared sample solution with magnetic stirring and titrate the cloudiness point (mL) with n-hexane while maintaining the temperature at 25°C. Specifically, while keeping the Erlenmeyer flask containing the sample solution at 25°C, place it on some Ming font characters (12pt) printed on plain paper by electrophotography, and when viewed from above, the liquid layer becomes cloudy and the characters become blurred and illegible, which is the point at which this occurs. (4) Using the same procedure, titrate the turbidity point (mL) of ion-exchanged water. (5) The SP value δ (cal / cm) of the resin particles is calculated according to the following formulas (1) to (9). 3 ) 1 / 2 Calculate.

[0025] (formula) TIFF2024146796000001.tif224170

[0026] The meaning and value of each variable are as follows: L: Titration volume (mL) of low polarity solvent (n-hexane) H: Titration volume of highly polar solvent (water) (mL) φ SL : Volume fraction of dissolving solvent (THF) to the sum of dissolving solvent (THF) and titration solvent (n-hexane) φ L : Volume fraction of the titration solvent (n-hexane) to the sum of the dissolving solvent (THF) and the titration solvent (n-hexane) φ SH : Volume fraction of dissolving solvent (THF) to the sum of dissolving solvent (THF) and titration solvent (ion-exchanged water) φ H : Volume fraction of titration solvent (ion-exchanged water) to the sum of dissolution solvent (THF) and titration solvent (ion-exchanged water) V S : Molar volume of dissolving solvent (THF) [mL / mol] = 81.0 V L Molar volume of titration solvent (n-hexane) [mL / mol] = 132 V H Molar volume of titration solvent (ion-exchanged water) [mL / mol] = 18.0 δ S : SP value of dissolving solvent (THF) [(cal / cm 3 ) 1 / 2 〕=9.54 δ L : SP value of titration solvent (n-hexane) [(cal / cm 3 ) 1 / 2 〕=7.24 δ H : SP value of titration solvent (ion-exchanged water) [(cal / cm 3 ) 1 / 2 〕=23.5 δ SL : SP value of the mixed solution when titrated with the titration solvent (n-hexane) δ SH : SP value of the mixed solution when titrated with the titration solvent (ion-exchanged water) δ: SP value of resin particles [(cal / cm 3 ) 1 / 2 〕

[0027] [Step 1]: The purpose of hydrogenating the hydrophilic groups of resin particles (preparing a sample for measuring the SP value) is to obtain a dry powder of resin particles, so if this purpose can be achieved, the dry powder may be obtained by the following method: Drop the resin particle dispersion into a poor solvent to precipitate fine resin particles, filter, and then dry the particles to obtain a dry powder of resin particles by freeze-drying.

[0028] The SP value is 9.0 (cal / cm 3 ) 1 / 2 〕In the case of resin particles that are not easily dissolved in THF as shown below, it is recommended to use p-xylene or toluene instead of THF as a solvent to dissolve the dry resin particle sample. In this case, each variable changes as shown below.

[0029] φ SL : Volume fraction of the dissolving solvent (p-xylene / toluene) relative to the sum of the dissolving solvent (p-xylene / toluene) and the titration solvent (n-hexane) φ L : Volume fraction of the titration solvent (n-hexane) relative to the sum of the dissolution solvent (p-xylene / toluene) and the titration solvent (n-hexane) φ SH : Volume fraction of the dissolving solvent (p-xylene / toluene) relative to the sum of the dissolving solvent (p-xylene / toluene) and the titration solvent (ion-exchanged water) φH : Volume fraction of titration solvent (ion-exchanged water) to the sum of dissolution solvent (p-xylene / toluene) and titration solvent (ion-exchanged water) V S : Molar volume of dissolving solvent (p-xylene / toluene) [mL / mol] = 123 / 106 δ S : SP value of dissolving solvent (p-xylene / toluene) [(cal / cm 3 ) 1 / 2 〕=8.80 / 8.91 The SP value in the present invention is influenced not only by the type of resin and the constituent monomers, but also by various factors such as the resin skeleton which changes due to the molecular weight and branching structure, the type and amount of the initiator used, the type and amount of the chain transfer agent, etc. Therefore, the SP value cannot be accurately derived by calculation, and an experimentally measured value must be used.

[0030] The glass transition temperature (Tg) of the binder is preferably 35 to 150° C., and more preferably 55 to 120° C. The glass transition temperature (Tg) of the resin is a value measured by a method such as differential scanning calorimetry (DSC).

[0031] The weight average molecular weight of the binder is preferably 30,000 to 120,000. The weight average molecular weight of the binder can be measured by gel permeation chromatography (GPC). Specifically, the measurement can be performed using HLC-8320GPC (manufactured by Tosoh Corporation) as a GPC device, two TSK gel Super Multipore HZ-H (manufactured by Tosoh Corporation, inner diameter 4.6 mm x 15 cm) columns, tetrahydrofuran as an eluent, and TSK Standard (manufactured by Tosoh Corporation) as a standard sample.

[0032] The acid value of the binder is preferably 5 to 150 mgKOH / g, more preferably 10 to 120 mgKOH / g, and further preferably 15 to 75 mgKOH / g. The acid value of a polymer represents the number of mg of KOH required to neutralize 1 g of the polymer, and can be measured according to JIS-K3054.

[0033] Examples of the binder having the SP value, glass transition temperature (Tg) and weight average molecular weight within the above ranges include those containing C1-C4 alkyl (meth)acrylate, C1-C4 hydroxyalkyl (meth)acrylate and C6-C10 alkyl (meth)acrylate as constituent monomers, etc. Examples of the binder having an acid value of 5 to 150 mgKOH / g include those containing carboxylic acid having a carbon-carbon double bond as constituent monomers.

[0034] The alkyl portion of the C1-C4 alkyl (meth)acrylate may be linear or branched, and is preferably linear. Two or more types of C1-C4 alkyl (meth)acrylate may be mixed and used. As the C1-C4 alkyl (meth)acrylate, C1-C3 alkyl (meth)acrylate is preferred, C1-C2 alkyl (meth)acrylate is more preferred, and methyl methacrylate is even more preferred.

[0035] The hydroxyalkyl portion of the C1-C4 hydroxyalkyl (meth)acrylate may be linear or branched, and is preferably linear. Two or more types of C1-C4 hydroxyalkyl (meth)acrylate may be mixed and used. As the C1-C4 hydroxyalkyl (meth)acrylate, C1-C3 hydroxyalkyl (meth)acrylate is preferred, C1-C2 hydroxyalkyl (meth)acrylate is more preferred, and 2-hydroxyethyl (meth)acrylate is even more preferred.

[0036] The alkyl portion of the C6-C10 alkyl acrylate may be linear or branched, and is preferably branched. As the C6-C10 alkyl acrylate, C7-C9 alkyl acrylate is preferred, C8 alkyl acrylate is more preferred, and 2-ethylhexyl acrylate is even more preferred.

[0037] Examples of the carboxylic acid having a carbon-carbon double bond include acrylic acid, methacrylic acid, and β-carboxyethyl acrylate, with methacrylic acid being more preferred.

[0038] When the binder contains, as constituent monomers, a C1-C4 alkyl (meth)acrylate, a C1-C4 hydroxyalkyl (meth)acrylate, a C6-C10 alkyl (meth)acrylate, and a carboxylic acid having a carbon-carbon double bond, the ratio of the four constituent monomers, C1-C4 alkyl (meth)acrylate, C1-C4 hydroxyalkyl (meth)acrylate, C6-C10 alkyl (meth)acrylate, and a carboxylic acid having a carbon-carbon double bond, is 55 to 9. The content is preferably 5 mass%, 0.1 to 25 mass%, 0 to 45 mass%, and 2 to 15 mass%, and more preferably 65 to 90 mass%, 3 to 10 mass%, 0 to 31 mass%, and 4 to 10 mass%, and it is preferable that the total amount falls within these ranges to be 100 mass%, and when the content of methyl methacrylate is X and the content of 2-hydroxyethyl (meth)acrylate is Y in the total mass of the constituent monomers, the value represented by X / Y is preferably in the range of 2.5 to 75.0, and more preferably in the range of 5.5 to 35.0.

[0039] The binder preferably contains, as constituent monomers, a C1-C4 alkyl (meth)acrylate and a C6-C10 alkyl (meth)acrylate, the respective contents of which are 55 to 95% by mass and 0.1 to 45% by mass relative to the total mass of the binder solids.

[0040] The constituent monomers of the binder include non-(meth)acrylic monomers such as propylene, butadiene, styrene chloride, maleic acid, styrene, chlorostyrene, or α-methylstyrene. For example, there are vinyl monomer units having crosslinking properties, specifically aromatic divinyl compounds such as divinylbenzene, divinylnaphthalene, etc.; (meth)acrylates having an allyl group such as allyl acrylate, allyl methacrylate, etc.; diacrylate compounds bonded with alkyl chains such as ethylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butanediol diacrylate, 1,5-pentanediol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, and the above compounds in which the acrylate is replaced with methacrylate; diacrylate compounds bonded with alkyl chains containing ether bonds such as diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol# 400 diacrylate, polyethylene glycol #600 diacrylate, dipropylene glycol diacrylate, and compounds in which the acrylate of the above compounds is replaced with a methacrylate; diacrylate compounds linked by chains containing aromatic groups and ether compounds, such as polyoxyethylene (2)-2,2-bis(4-hydroxyphenyl)propane diacrylate, polyoxyethylene (4)-2,2-bis(4-hydroxyphenyl)propane diacrylate, and compounds in which the acrylate of the above compounds is replaced with a methacrylate; polyfunctional crosslinking agents include pentaerythritol triacrylate, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, oligoester acrylate, and compounds in which the acrylate of the above compounds is replaced with a methacrylate; triallyl cyanurate, triallyl trimellitate, and the like. The binder preferably contains, as its constituent monomers, methyl methacrylate and 2-ethylhexyl acrylate. When the total mass of the methyl methacrylate and the total mass of the 2-ethylhexyl acrylate as constituent monomers in the binder are X2 and Y2, respectively, the value calculated by Y2 / X2 is preferably 0 or more and 1 or less, more preferably 0 or more and 0.5 or less, even more preferably 0 or more and 0.3 or less, particularly preferably 0 or more and 0.1 or less, and extremely preferably 0.

[0041] The binder is preferably a water dispersion, and the average particle size thereof is preferably 50 nm to 5 μm, and more preferably 100 nm to 1 μm, in order to prevent clogging of the inkjet head.

[0042] The content of the binder in the ink (content as solid content) is usually 0.1 to 14 mass %, preferably 0.5 to 12 mass %, and more preferably 2 to 10 mass %, relative to the total mass of the ink.

[0043] The ink may further contain a colorant. The colorant is not particularly limited, but examples thereof include pigments and disperse dyes.

[0044] Examples of the pigment include inorganic pigments, organic pigments, extender pigments, hollow particles, and the like. Examples of inorganic pigments include carbon black, metal oxides, metal hydroxides, metal sulfides, metal ferrocyanides, and metal chlorides.

[0045] When the ink according to the present embodiment is a black ink and the colorant is an inorganic pigment, the inorganic pigment contained in the black ink is preferably carbon black such as thermal black, acetylene black, oil furnace black, gas furnace black, lamp black, gas black, channel black, etc. Specific examples of carbon black include the Raven series manufactured by Columbia Carbon Co., the Monarch series, Regal series, and Mogul series manufactured by Cabot Corporation, the HiBlack series, ColorBlack series, Printex series, SpecialBlack series, and Nerox series manufactured by Orion Engineered Carbons, and the MA series, MCF series, No. 25, No. 33, No. 40, No. 47, No. 52, No. 900, and No. 2300 manufactured by Mitsubishi Chemical Corporation.

[0046] When the ink according to the present embodiment is a white ink and the colorant is an inorganic pigment, examples of the inorganic pigment contained in the white ink include oxides, nitrides, and oxynitrides of metals such as zinc, silicon, aluminum, titanium, strontium, and zirconium; inorganic compounds such as glass and silica; etc. Among these, titanium dioxide and zinc oxide are preferred.

[0047] Examples of organic pigments include various pigments such as azo, disazo, phthalocyanine, quinacridone, isoindolinone, dioxazine, perylene, perinone, thioindigo, anthraquinone, and quinophthalone.

[0048] Specific examples of organic pigments include yellow pigments such as CI Pigment Yellow 1, 2, 3, 12, 13, 14, 16, 17, 24, 55, 73, 74, 75, 83, 93, 94, 95, 97, 98, 108, 114, 128, 129, 138, 139, 150, 151, 154, 155, 180, 185, 193, 199, 202, and 213; Red pigments such as 5, 7, 12, 48, 48:1, 57, 88, 112, 122, 123, 146, 149, 150, 166, 168, 177, 178, 179, 184, 185, 202, 206, 207, 254, 255, 257, 260, 264, 269, 272; blue pigments such as CI Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 22, 25, 60, 66, 80; violet pigments such as CI Pigment Violet 19, 23, 29, 37, 38, 50; orange pigments such as CI Pigment Orange 13, 16, 43, 68, 69, 71, 73; CI Pigment Green 7, 36, 54, and other green pigments; and CI Pigment Black 1, and other black pigments. Among these, CI Pigment Blue 15:4 is preferred.

[0049] Examples of the extender pigment include silica, calcium carbonate, talc, clay, barium sulfate, white carbon, etc. The extender pigment is often used in combination with other colorants.

[0050] As the hollow particles, known hollow particles described in, for example, U.S. Pat. No. 4,880,465, Japanese Patent No. 3,562,754, Japanese Patent No. 6,026,234, Japanese Patent No. 5,459,460, JP-A-2003-268694, Japanese Patent No. 4,902,216, etc. can be used, and they are particularly preferably used as white pigments.

[0051] As disperse dyes, for example, dyes selected from CI Dispers are preferred. Specific examples thereof include yellow dyes such as CI Dispers Yellow 9, 23, 33, 42, 49, 54, 58, 60, 64, 66, 71, 76, 79, 83, 86, 90, 93, 99, 114, 116, 119, 122, 126, 149, 160, 163, 165, 180, 183, 186, 198, 200, 211, 224, 226, 227, 231, and 237; red dyes such as CI Dispers Red 60, 73, 88, 91, 92, 111, 127, 131, 143, 145, 146, 152, 153, 154, 167, 179, 191, 192, 206, 221, 258, and 283; and CI Dispers Orange. Orange dyes such as 9, 25, 29, 30, 31, 32, 37, 38, 42, 44, 45, 53, 54, 55, 56, 61, 71, 73, 76, 80, 96, 97, etc.; violet dyes such as CI Dispers Violet 25, 27, 28, 54, 57, 60, 73, 77, 79, 79:1, etc.; blue dyes such as CI Dispers Blue 27, 56, 60, 79:1, 87, 143, 165, 165:1, 165:2, 181, 185, 197, 202, 225, 257, 266, 267, 281, 341, 353, 354, 358, 364, 365, 368, etc.;

[0052] The average particle size of the colorant is preferably 30 to 300 nm, and more preferably 50 to 250 nm. In this specification, the average particle size refers to the average particle size of particles measured by a laser light scattering method.

[0053] The content of the colorant relative to the total mass of the ink according to this embodiment is preferably 1 to 30 mass %, more preferably 1 to 10 mass %, and even more preferably 2 to 8 mass %.

[0054] The colorant may further contain other dyes in addition to the pigment and the disperse dye. Examples of the other dyes include solvent dyes, direct dyes, acid dyes, and reactive dyes.

[0055] When the ink contains a plurality of types of colorants, the mixing ratio of the colorants can be set arbitrarily according to the purpose. When the ink contains other dyes in addition to the colorants, the mixing ratio of the total amount of the colorants to the total amount of the other dyes can also be set arbitrarily.

[0056] The ink may further contain water. The water is preferably water with a low content of impurities such as metal ions, i.e., ion-exchanged water, distilled water, etc. The content of water is 60 to 90% by mass, and preferably 70 to 90% by mass, based on the total mass of the ink according to this embodiment.

[0057] [wax] The ink may contain wax.

[0058] The form of the wax is preferably a wax emulsion, and particularly preferably an aqueous wax emulsion. As the wax emulsion, natural wax and chemically synthesized wax can be used. As the natural wax, an emulsion in which petroleum wax such as paraffin wax and microcrystalline wax, lignite wax such as montan wax, or vegetable wax such as carnauba wax and candelilla wax, animal and vegetable wax such as beeswax and lanolin are dispersed in an aqueous medium; as the chemically synthesized wax, an emulsion in which homopolymer wax such as polyethylene wax and polypropylene wax, oxidized polyalkylene waxes thereof, Fischer-Trop, copolymer wax such as ethylene vinyl acetate and ethylene acrylic acid are dispersed in an aqueous medium, and the like can be mentioned. Among these waxes, polyalkylene wax, oxidized polyalkylene wax, and paraffin wax are preferred. These waxes may be used alone or in combination.

[0059] The amount of wax added is usually 0.01 to 1.0% by mass, and more preferably 0.1 to 0.7% by mass, based on the total weight of the ink. The amount of wax added refers to the solid content of the wax contained in the ink.

[0060] [Dispersant] The ink preferably contains one or more dispersants to disperse the colorant. Another embodiment of the present invention is to use a self-dispersing colorant as the colorant, thereby dispersing the colorant without using a dispersant. The dispersant is not particularly limited, and known dispersants such as polymer dispersants can be used. The polymer dispersant is other than the binder and wax, and examples thereof include copolymers composed of at least two monomers (preferably at least one of which is a hydrophilic monomer) selected from monomers such as styrene and its derivatives; vinyl naphthalene and its derivatives; aliphatic alcohol esters of α,β-ethylenically unsaturated carboxylic acids; (meth)acrylic acid and its derivatives; maleic acid and its derivatives; itaconic acid and its derivatives; faric acid and its derivatives; vinyl acetate, vinyl alcohol, vinyl pyrrolidone, acrylamide, and their derivatives. Examples of such copolymers include styrene-(meth)acrylic acid copolymers, styrene-(meth)acrylic acid-(meth)acrylic acid ester copolymers, (meth)acrylic acid ester-(meth)acrylic acid copolymers, polyethylene glycol (meth)acrylate-(meth)acrylic acid copolymers, and styrene-maleic acid copolymers. Among these, styrene-(meth)acrylic acid copolymers, styrene-(meth)acrylic acid-(meth)acrylic acid ester copolymers, and (meth)acrylic acid ester-(meth)acrylic acid copolymers are preferred, (meth)acrylic acid ester-(meth)acrylic acid copolymers are more preferred, and methacrylic acid ester-methacrylic acid copolymers are even more preferred. Examples of types of copolymers include block copolymers, random copolymers, and graft copolymers. These copolymers may be in the form of a salt.

[0061] Dispersants can be commercially available or synthesized.

[0062] Examples of commercially available dispersants include Joncyrl 62, 67, 68, 678, and 687 (styrene-acrylic copolymers manufactured by BASF); Movinyl S-100A (modified vinyl acetate copolymer manufactured by Japan Coating Resins Co., Ltd.); and Julimer AT-210 (polyacrylic acid ester copolymer manufactured by Toa Gosei Co., Ltd.).

[0063] Examples of dispersants obtained by synthesis include the AB block polymer disclosed in WO 2013 / 115071. The monomer constituting the A block of the AB block polymer disclosed in WO 2013 / 115071 is at least one monomer selected from (meth)acrylic acid and linear or branched C4 alkyl (meth)acrylate, preferably at least one monomer selected from methacrylic acid and n-butyl methacrylate, and more preferably these two monomers are used in combination. The monomer constituting the B block of the AB block polymer disclosed in WO 2013 / 115071 is at least one monomer selected from benzyl methacrylate and benzyl acrylate, preferably benzyl methacrylate. Specific examples of the AB block polymer include the block copolymers disclosed in Synthesis Examples 3 to 8 of WO 2013 / 115071.

[0064] The acid value of the dispersant is usually from 90 to 200 mgKOH / g, preferably from 100 to 150 mgKOH / g, and more preferably from 100 to 120 mgKOH / g.

[0065] A neutralizing agent may be used to disperse the dispersant uniformly in water. Examples of the neutralizing agent include ammonia, hydroxides of alkali metals, hydroxides of alkaline earth metals, aliphatic amine compounds, and alkanolamine compounds. Among these, ammonia and hydroxides of alkali metals are preferred, and ammonia is more preferred. The amount of the neutralizing agent to be used is usually 30 to 300% neutralization degree, preferably 50 to 200%, assuming that the neutralization degree is 100% when the dispersant is neutralized with the theoretical equivalent of the acid value of the dispersant.

[0066] The mass average molecular weight of the dispersant is usually 10,000 to 60,000, preferably 10,000 to 40,000, more preferably 15,000 to 30,000, and further preferably 20,000 to 25,000. The mass average molecular weight of the dispersant can be measured by gel permeation chromatography (GPC). Specifically, the measurement can be performed using HLC-8320GPC (manufactured by Tosoh Corporation) as a GPC device, two TSK gel Super Multipore HZ-H (manufactured by Tosoh Corporation, inner diameter 4.6 mm x 15 cm) columns, tetrahydrofuran as an eluent, and TSK Standard (manufactured by Tosoh Corporation) as a standard sample.

[0067] The PDI (mass average molecular weight / number average molecular weight) of the dispersant is preferably about 1.29 to 1.49. By setting it in this range, the dispersibility and storage stability of the first ink composition tend to be improved.

[0068] The dispersant may be used in a state where it is mixed with the colorant, or in a state where a part or the whole of the surface of the colorant is coated with the dispersant, or both of these states may be used in combination.

[0069] The ratio of the total mass of the dispersants to the total mass of the colorants is usually 0.01 to 1.0, preferably 0.05 to 0.6, and more preferably 0.1 to 0.5.

[0070] Furthermore, the ink may contain ink modifiers such as, for example, humectants, antiseptics, antifungals, pH adjusters, chelating agents, rust inhibitors, water-soluble UV absorbers, water-soluble polymeric compounds, antioxidants and / or surfactants.

[0071] Specific examples of moisturizing agents include polyols such as glycerin, ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, polypropylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2,6-hexanetriol, and pentaerythritol; cyclic amides such as 2-pyrrolidone and N-methyl-2-pyrrolidone; ureas such as urea, thiourea, ethyleneurea, and 1,3-dimethylimidazolidinones; lactams such as ε-caprolactam; solid glycerins such as trimethylolpropane and trimethylolethane; and sugars such as maltitol, sorbitol, gluconolactone, and maltose.

[0072] Specific examples of antiseptic and antifungal agents include organic sulfur-based, organic nitrogen sulfur-based, organic halogen-based, haloarylsulfone-based, iodopropargyl-based, haloalkylthio-based, nitrile-based, pyridine-based, 8-oxyquinoline-based, benzothiazole-based, isothiazolin-based, dithiol-based, pyridine oxide-based, nitropropane-based, organic tin-based, phenol-based, quaternary ammonium salt-based, triazine-based, thiazine-based, anilide-based, adamantane-based, dithiocarbamate-based, brominated indanone-based, benzyl bromoacetate-based, and inorganic salt-based compounds.

[0073] A specific example of the organic halogen compound is sodium pentachlorophenol, and a specific example of the pyridine oxide compound is sodium 2-pyridinethiol-1-oxide.

[0074] Examples of isothiazoline compounds include 1,2-benzisothiazolin-3-one, 2-n-octyl-4-isothiazolin-3-one, 5-chloro-2-methyl-4-isothiazolin-3-one, 5-chloro-2-methyl-4-isothiazolin-3-one magnesium chloride, 5-chloro-2-methyl-4-isothiazolin-3-one calcium chloride, and 2-methyl-4-isothiazolin-3-one calcium chloride.

[0075] Other specific examples of antiseptic and antifungal agents include anhydrous sodium acetate, sodium sorbate, sodium benzoate, ethyl p-hydroxybenzoate, and Arch Chemical's trade names Proxel GXL(S) and Proxel XL-2(S).

[0076] Any substance can be used as the pH adjuster as long as it can control the pH of the ink within the above range without adversely affecting the ink being prepared. Specific examples of the pH adjuster include the neutralizing agents mentioned above; alkali metal carbonates such as lithium carbonate, sodium carbonate, sodium hydrogencarbonate, and potassium carbonate; alkali metal salts of organic acids such as sodium silicate and potassium acetate; and inorganic bases such as disodium phosphate.

[0077] Specific examples of the chelating agent include disodium ethylenediaminetetraacetate, sodium nitrilotriacetate, sodium hydroxyethylethylenediaminetriacetate, sodium diethylenetriaminepentaacetate, and sodium uracildiacetate.

[0078] Specific examples of the rust inhibitor include acid sulfite, sodium thiosulfate, ammonium thioglycolate, diisopropylammonium nitrite, pentaerythritol tetranitrate, and dicyclohexylammonium nitrite.

[0079] Examples of the water-soluble ultraviolet absorber include sulfonated benzophenone compounds, benzotriazole compounds, salicylic acid compounds, cinnamic acid compounds, and triazine compounds.

[0080] Specific examples of the water-soluble polymer compound include those other than the above-mentioned binders, waxes, and dispersants, such as polyethylene glycol, polyvinyl alcohol, cellulose derivatives, polyamines, and polyimines.

[0081] Examples of the antioxidant include various organic and metal complex-based anti-fading agents. Examples of the organic anti-fading agents include hydroquinones, alkoxyphenols, dialkoxyphenols, phenols, anilines, amines, indanes, chromans, alkoxyanilines, and heterocycles.

[0082] Examples of the surfactant include known anionic, cationic, amphoteric, nonionic, silicone-based and fluorine-based surfactants, and one or more of these can be selected and used.

[0083] Examples of anionic surfactants include alkyl sulfocarboxylates, α-olefin sulfonates, polyoxyethylene alkyl ether acetates, N-acylamino acids or salts thereof, N-acyl methyl taurines, alkyl sulfates, polyoxyalkyl ether sulfates, alkyl sulfates, polyoxyethylene alkyl ether phosphates, rosin acid soaps, castor oil sulfates, lauryl alcohol sulfates, alkylphenol phosphates, alkyl phosphates, alkylaryl sulfonates, diethyl sulfosuccinates, diethylhexyl sulfosuccinates, and dioctyl sulfosuccinates.

[0084] Examples of the cationic surfactant include 2-vinylpyridine derivatives and poly(4-vinylpyridine) derivatives.

[0085] Examples of amphoteric surfactants include lauryl dimethylaminoacetate betaine, 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine, coconut oil fatty acid amidopropyl dimethylaminoacetate betaine, polyoctyl polyaminoethyl glycine, and imidazoline derivatives.

[0086] Examples of nonionic surfactants include ether surfactants such as polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene dodecylphenyl ether, polyoxyethylene oleyl ether, polyoxyethylene lauryl ether, and polyoxyethylene alkyl ether; polyoxyethylene oleate, polyoxyethylene distearate, sorbitan laurate, sorbitan monostearate, sorbitan monooleate, sorbitan sesquioleate, and polyoxyethylene Examples of such polyglycol ethers include ester-based polyoxyethylene stearate and monooleate; acetylene glycol (alcohol)-based polyoxyethylene stearate and monooleate; acetylene glycol (alcohol)-based polyoxyethylene stearate and monooleate; Surfynol 104, 105PG50, 82, 420, 440, 465, 485, and Olfin STG (trade names) manufactured by Nissin Chemical Industry Co., Ltd.; and TergItol 15-S-7 and other polyglycol ether-based polyoxyethylene stearate and monooleate (trade name) manufactured by SIGMA-ALDRICH.

[0087] Examples of silicone surfactants include polyether-modified siloxane, polyether-modified polydimethylsiloxane, etc. Examples of such surfactants include Dynol 960 and Dynol 980 manufactured by Air Products Co., Ltd., Silface SAG001, Silface SAG002, Silface SAG003, Silface SAG005, Silface SAG503A, Silface SAG008, Silface SAG009, Silface SAG010 manufactured by Nissin Chemical Industry Co., Ltd., and BYK-345, BYK-347, BYK-348, BYK-349, BYK-3450, BYK-3451, BYK-3455, etc. manufactured by BYK-Chemie Co., Ltd., and various types of products can be easily purchased.

[0088] Examples of fluorine-based surfactants include perfluoroalkyl sulfonic acid compounds, perfluoroalkyl carboxylic acid compounds, perfluoroalkyl phosphate compounds, perfluoroalkyl ethylene oxide adducts, and polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups on the side chains, etc. Examples of such surfactants include Zonyl TBS, FSP, FSA, FSN-100, FSN, FSO-100, FSO, FS-300, and Capstone, manufactured by DuPont. Examples of the polymerizable monomers include FS-30 and FS-31; PF-151N and PF-154N manufactured by Omnova; F-114, F-410, F-444, EXP.TF-2066, EXP.TF-2148, EXP.TF-2149, F-430, F-477, F-552, F-553, F-554, F-555, F-556, F-557, F-558, F-559, F-561, F-562, R-40, R-41, RS-72-K, RS-75, RS-76-E, RS-76-NS, RS-77, EXP.TF-1540, and EXP.TF-1760 manufactured by DIC; and BYK-3440 and BYK-3441 manufactured by BYK-Chemie.

[0089] Among these, it is preferable to select at least one surfactant selected from nonionic or silicone surfactants.

[0090] In all of the above-mentioned components, contents, content ratios, etc., a combination of preferred components is more preferable, and a combination of more preferred components is even more preferable. The same applies to combinations of preferred components and more preferred components.

[0091] The method for preparing the ink is not particularly limited. One example is a method in which a dispersion liquid is prepared from a colorant and a dispersant, the binder and the organic solvent are added thereto, and water and the ink preparation agent are further added as necessary to prepare an ink composition.

[0092] The ink composition may be prepared using only one type of dispersion liquid, or two or more types of dispersion liquids.

[0093] When the ink contains a colorant, the method of dispersing the colorant to prepare a dispersion liquid includes a method using a sand mill (bead mill), a roll mill, a ball mill, a paint shaker, an ultrasonic disperser, a microfluidizer, etc., among which a sand mill (bead mill) is preferable. In addition, when preparing a colorant dispersion liquid using a sand mill (bead mill), it is preferable to use small beads (0.01 to 1 mm in diameter) and treat under conditions that increase the dispersion efficiency by increasing the bead packing rate, etc. By carrying out dispersion under such conditions, the particle size of the colorant can be reduced, and a dispersion liquid with good dispersibility can be obtained. In addition, after preparing the dispersion liquid, it is also preferable to remove components such as pigments with large particle sizes by filtration and / or centrifugation. In addition, in order to suppress foaming during the preparation of the dispersion liquid, a very small amount of a silicone-based, acetylene glycol-based, or other defoaming agent may be added. However, some defoaming agents inhibit dispersion and microparticulation, and it is preferable to use one that does not affect dispersion or stability after dispersion.

[0094] The colorant in the dispersion may be a microencapsulated colorant in which the surface of the colorant is coated with a dispersant, or may not be microencapsulated, but is preferably a microencapsulated colorant in which the colorant is uniformly coated with a dispersant.

[0095] The methods of uniformly covering the colorant surface with a dispersant to form a microencapsulation are roughly divided into two methods: physical / mechanical methods and chemical methods. As the latter chemical methods, surface precipitation, kneading, interfacial polymerization, etc. have been proposed. The surface precipitation method is a method of precipitating a dispersant on the colorant surface by utilizing pH adjustment or differences in solubility in a medium, and includes acid precipitation and phase inversion emulsification. The interfacial polymerization method is a method of adsorbing a monomer, oligomer, or pigment derivative on the colorant surface and then carrying out a polymerization reaction, and is also called the surface polymerization method. In the present invention, either method may be used, but the surface precipitation method is preferred, and the colored dispersion obtained by the phase inversion emulsification method is more preferred.

[0096] The phase inversion emulsification method is a method in which a colorant, a dispersant, and an organic solvent are mixed and dispersed, and water is further added to uniformly adsorb the dispersant onto the colorant surface. Specific manufacturing methods include the following five types of manufacturing methods.

[0097] 1. A manufacturing method in which a solution of a dispersant that disperses or dissolves in water and has a colorant dispersed in it is mixed with a liquid whose main component is water, and then the solvent is removed. 2. A manufacturing method in which a solution of a colorant dispersed in a hydrophilic organic solvent and a dispersant that disperses or dissolves in water by neutralization is mixed with a mixed liquid containing water and a neutralizing agent, and then the solvent is removed. 3. A manufacturing method in which a mixed solution of a hydrophilic organic solvent and a hydrophobic organic solvent in which a colorant is dispersed and a dispersant that disperses or dissolves in water is mixed with a liquid whose main component is water, and then the solvent is removed. 4. A manufacturing method in which a solution of a mixed solvent of a hydrophilic organic solvent and a hydrophobic organic solvent in which a colorant is dispersed and in which the dispersant disperses or dissolves in water by neutralization is mixed with a mixed liquid containing water and a neutralizing agent, and then the solvent is removed. 5. A manufacturing method in which a colorant is mixed with a solution of a mixed solvent whose main components are water and a hydrophilic organic solvent of a dispersant that disperses or dissolves in water, the pigment is dispersed in the solution, and then the solvent is removed.

[0098] The above-mentioned dispersion can be obtained by the above-mentioned manufacturing method, but a coated colorant dispersion can also be obtained by a different manufacturing method. An example of the manufacturing method is a manufacturing method in which a solution of a hydrophobic organic solvent in which a dispersant is dissolved is mixed with a liquid mainly composed of water containing a neutralizing agent to prepare an emulsion (emulsion or microemulsion), a colorant is added thereto and mixed / dispersed, and then water is further added to remove the solvent.

[0099] Although the dispersion liquid composed of colorant particles whose surfaces are covered with a dispersant has been described in detail, by using the above method, it is possible to easily obtain a dispersion liquid composed of colorant particles having a dispersant on the surface and an average particle size of 200 nm or less. In particular, it is more preferable to set the average particle size to 50 to 180 nm by selecting the type of colorant and the type of dispersant used, the acid value, the molecular weight, etc. Here, in this specification, the average particle size refers to the average particle size of particles measured using a laser light scattering method.

[0100] In preparing the dispersion, a neutralizing agent can be used, such as an alkali metal hydroxide, an alkaline earth metal hydroxide, an aliphatic amine compound, or an alcohol amine compound. These neutralizing agents can be used alone or in combination. In preparing the dispersion, the amount of the neutralizing agent is not limited. The degree of neutralization is 100% when the neutralization is performed with the theoretical equivalent of the acid value of the dispersing agent, and the neutralizing agent can be used in an amount exceeding the theoretical amount. The degree of neutralization is usually 0 to 150%, preferably 30 to 100%, and more preferably 50 to 70%.

[0101] Alkali metal hydroxides include, for example, lithium hydroxide, sodium hydroxide, and potassium hydroxide. Examples of the hydroxides of alkaline earth metals include beryllium hydroxide, magnesium hydroxide, calcium hydroxide, and strontium hydroxide. Of these, lithium hydroxide or sodium hydroxide is preferred.

[0102] Examples of the alcohol amine compound include monoethanolamine, diethanolamine, triethanolamine, monopropanolamine, dipropanolamine, tripropanolamine, methylethanolamine, dimethylethanolamine, and N-methyldiethanolamine. Among these, tertiary amines are preferred, and triethanolamine is more preferred.

[0103] Examples of the aliphatic amine compound include ammonia, monomethylamine, dimethylamine, trimethylamine, monoethylamine, dimethylamine and trimethylamine. Of these, ammonia or triethylamine is preferred.

[0104] The pH of the ink is usually pH 5 to 11, preferably pH 7 to 10, for the purpose of improving storage stability. The surface tension of the ink is usually 10 to 50 mN / m, preferably 20 to 40 mN / m. The viscosity of the ink is usually 30 mPa s or less, preferably 20 mPa s or less. The pH and surface tension of the ink can be appropriately adjusted by using ink regulators such as a pH adjuster and a surfactant.

[0105] The ink is excellent in circulation stability, storage stability, ejection stability, wet spreadability on a recording material, and drying property, and a printed matter obtained using the ink of the present invention is excellent in abrasion resistance, adhesion, color development, etc. Furthermore, in terms of abrasion resistance, the ink is excellent in both dry abrasion resistance and wet abrasion resistance.

[0106] When the ink is used as an inkjet ink, it is preferable to reduce the content of inorganic impurities such as chlorides of metal cations (e.g., sodium chloride) and sulfates (e.g., sodium sulfate). The content of inorganic impurities is preferably 1% or less based on the total mass of the colorant, and the lower limit may be below the detection limit of an analytical instrument, i.e., 0%. Examples of methods for producing colorants with low inorganic impurities include a method of exchanging and adsorbing inorganic impurities with an ion exchange resin.

[0107] The present invention also includes an ink set combining a plurality of the above inks, an ink set combining the above inks with an ink other than the above inks, an inkjet recording method in which droplets of the above inks are ejected from an inkjet head to record on a print medium, and a printed matter printed using the above ink.The present invention also includes a set of ink and an overcoat agent containing the above ink and an overcoat agent described below, a recording medium on which an image is formed using the set of ink and overcoat agent, and a method for producing a recording medium, which includes forming an image on a recording medium using the ink and then covering a part or all of the image forming portion with the overcoat agent. The overcoat agent is not particularly limited as long as it can coat a part or all of the ink on the recording material, but it preferably contains an organic solvent and a binder, and the SP value of the binder is in the range of 9.8 to 12.3. The organic solvent and the binder contained in the overcoat agent may be the same as those described in the ink, including the preferred ones. The overcoat agent may contain a single binder resin or multiple binder resins. In addition, when the overcoat agent contains a binder resin, the binder resin may be the same as or different from the binder resin contained in the ink. The overcoat agent may also contain a wax, and the wax may be the same as those described in the ink, including the preferred ones.

[0108] The overcoat agent can be applied by various known application means, such as inkjet printing, a method using a coater, etc. The overcoat agent may be applied to a part or the whole of the area where the ink prints an image.

[0109] As the inkjet recording method, there is mentioned an inkjet recording method in which droplets of the ink are ejected in response to a recording signal and adhered to a recording material, thereby performing recording. The ink is poured into a container called an "ink tank" or an "ink cartridge", which is then loaded into a predetermined position of an inkjet printer and used for inkjet recording.

[0110] Examples of the inkjet method include a charge control method; a drop-on-demand method (pressure pulse method) that uses the vibration pressure of a piezoelectric element; an acoustic inkjet method; and a thermal inkjet, ie, a bubble jet (registered trademark) method. The ink can be used in any of these systems.

[0111] The recording material is not particularly limited, but a recording material that is non-absorbent or poorly absorbent to ink is preferred. Specific examples include coated paper such as lightly coated paper, art paper, coated paper, matte paper, and cast paper. Coated paper is paper that has a coating applied to its surface to enhance its aesthetic appearance and smoothness. Examples of the coating include various clays such as talc, pyrophyllite, and kaolin; mixtures of titanium oxide, magnesium carbonate, calcium carbonate, and the like with starch and / or polyvinyl alcohol; and the like. For example, paint can be applied to paper using a coater during the paper manufacturing process. There are two types of coaters: in-line type, which is directly connected to the papermaking machine to combine papermaking and coating in one process, and offline type, which is a separate process from papermaking. Lightly coated paper is paper with a coating weight of 12 g / m2. 2 The following paper is referred to. Art paper is a high-quality paper made of 100% chemical pulp with a thickness of 40 g / m 2 This refers to paper that has been coated with paint on the front and back. Coated paper and matte paper are 20 to 40 g / m 2 It refers to paper that has been coated with a coating of paint to a degree of gloss. Cast paper refers to paper that has been finished by applying pressure to the surface of art paper or coated paper using a machine such as a casting drum to enhance its gloss and recording effect. The above ink exhibits the effects of the present invention extremely favorably when used for recording on such non-absorbent or poorly absorbent recording materials.

[0112] Examples of the recording material include ordinary paper, none of which has an ink-receiving layer, media used in gravure printing or offset printing, etc.; paper and film exclusively for inkjet printing, which have an inkjet receiving layer, glossy paper and glossy film, etc.; fibers and cloths such as cellulose, nylon, and wool; leather; and substrates for color filters. Here, among plain papers not having an ink receiving layer, there are those that have low ink receiving properties similar to the non-absorbent non-recording material described above. Even when such plain papers are used, the effects obtained by the present invention are extremely effectively exhibited. EXAMPLES

[0113] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples. The average particle size was measured using a dynamic light scattering particle size distribution analyzer, Nanotrac Wave, manufactured by Nikkiso Co., Ltd. The solid content in the aqueous solution was measured using MS-70 manufactured by A&D Co., Ltd. by the dry weight method.

[0114] [Preparation Example 1]: Preparation of Dispersion 1. A block copolymer described in Synthesis Example 3 of International Publication No. 2013 / 115071 was prepared. 5.4 parts of the obtained polymer dispersant was dissolved in 20 parts of 2-butanone to obtain a uniform solution. A solution in which 0.2 parts of sodium hydroxide, 0.45 parts of ROCIMA 640 (manufactured by Dow Chemical Co.), and 0.06 parts of BYK1770 (manufactured by Big Chemie Japan Co., Ltd.) were dissolved in 56 parts of ion-exchanged water was added to this liquid, and the mixture was stirred for 1 hour to prepare an emulsified solution. 18 parts of CI Pigment Red 122 (Ink Jet Magenta E02, manufactured by Clariant Japan Co., Ltd.) were added to this, and dispersion was performed using a sand grinder. Dispersion was performed for 6 hours under conditions of 1500 rpm. Subsequently, 100 parts of ion-exchanged water was dropped, and the dispersion beads were separated by filtration. Further, 2-butanone and water were distilled off under reduced pressure using an evaporator so that the pigment solid content became 12.2%, to obtain a dispersion liquid having an average pigment particle size of 150 nm. This is designated as "Dispersion Liquid 1".

[0115] [Synthesis Examples 1 to 6]: Synthesis of Binders 1 to 6 Binders 1 to 6 were synthesized according to the method described below. The amounts of raw materials added were as shown in Table 1. A condenser, a thermometer, and a nitrogen inlet were attached to a glass reaction vessel (capacity 500 milliliters) equipped with a stirrer, and ion-exchanged water and Neopelex G-65 (Kao Corporation) were added. After replacing the air inside with nitrogen, the internal temperature was adjusted to 65°C while stirring. A 500 milliliter beaker was prepared separately, and ion-exchanged water, Neopelex G-65 (Kao Corporation), methyl methacrylate, 2-ethylhexyl acrylate, methacrylic acid, 2-hydroxyethyl methacrylate, and 1-dodecanethiol were added, and the mixture was stirred for 5 minutes at a stirring speed of 3000 rpm using a homogenizer to create an emulsion. An aqueous solution of ammonium persulfate dissolved in ion-exchanged water in a 30 milliliter beaker was added to the glass reaction vessel, and the emulsion created immediately thereafter was continuously dripped into the glass reaction vessel over 3 hours using a diaphragm pump. During the dropwise addition, the reaction was carried out at 65°C while introducing nitrogen. After the dropwise addition was completed, the mixture was stirred at 65°C for an additional 2 hours. After the reaction was completed, the mixture was cooled to below 40°C. After cooling, the mixture was filtered through a 325 mesh wire screen (opening: 0.043 mm) to obtain a binder sample with a solids concentration of 40% and the physical properties shown in Table 2.

[0116] [Table 1]

[0117] [Synthesis Example 7]: Synthesis of Binder 7 A condenser, a thermometer, and a nitrogen inlet were attached to a glass reaction vessel (capacity 500 milliliters) equipped with a stirrer, and 152.59 (g) of ion-exchanged water and 7.46 (g) of Neo-Perex G-65 (Kao Corporation) were added. After replacing the air inside with nitrogen, the inside temperature was adjusted to 65°C while stirring. A 500 milliliter beaker was prepared separately, and 130.71 (g) of ion-exchanged water, 0.23 (g) of Neo-Perex G-65 (Kao Corporation), 100.00 (g) of styrene, 2.90 (g) of 2-ethylhexyl acrylate, 9.21 (g) of methacrylic acid, and 80.40 (g) of α-methylstyrene were added, and the mixture was stirred for 5 minutes at a stirring speed of 3000 rpm using a homogenizer to create an emulsion. An aqueous solution of 1.50 (g) ammonium persulfate dissolved in 15.00 (g) ion-exchanged water was added to a glass reactor, and the emulsion was then continuously added dropwise to the glass reactor over a period of 3 hours using a diaphragm pump. During the addition, the reaction was carried out at 65°C while introducing nitrogen. After the addition was completed, the mixture was stirred at 65°C for an additional 2 hours. After the reaction was completed, the mixture was cooled to below 40°C. After cooling, the mixture was filtered through a 325 mesh wire screen (opening: 0.043 mm) to obtain a binder sample with a solids concentration of 40% and the physical properties shown in Table 2.

[0118] [Table 2]

[0119] [Examples 1 to 6]: Preparation of inks. Using Dispersion 1 obtained in Preparation Example 1 and any of the binders obtained in Synthesis Examples 1 to 5, the components shown in Table 3 below were added and mixed with stirring to obtain a liquid. The obtained liquid was filtered through a membrane filter with a pore size of 3 μm to obtain the inks of Examples 1 to 6, respectively. In Table 3, the numerical value of each component indicates the number of parts, and "balance" indicates that ion-exchanged water was added to adjust the total amount of the ink composition to 100 parts.

[0120] [Comparative Examples 1-2]: Preparation of comparative inks. Comparative inks of Comparative Examples 1 and 2 were obtained in the same manner as in Examples 1 to 6, except that the binders obtained in Synthesis Examples 6 to 7 were used.

[0121] The abbreviations in Table 3 below represent the following. In addition, blank spaces in Table 3 indicate 0 parts. AQ513: AQUACER 513 (manufactured by BYK Japan Co., Ltd., solid content: 34.6%). TEX: 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate (also known as Texanol). PG: Propylene glycol. 1,2HD: 1,2-hexanediol. BYK349: BYK-349 (manufactured by BYK Japan Co., Ltd.).

[0122] [Table 3]

[0123] [Abrasion resistance] 50 μl of each of the inks obtained in the examples and comparative examples was measured and coated with OK topcoat + 127.9 g / m2 (Oji Paper Co., Ltd.) at a speed of 200 mm / sec using a No. 3 bar coater in a PI-1210 automatic coating device (Tester Sangyo Co., Ltd.). 2 The resulting test print was then dried at 70°C for 2 minutes to produce a test print for abrasion resistance. The test print obtained was compared with an uncoated Oji Paper OK topcoat + 127.9 g / m2 test print using a Gakushin tester manufactured by Yasuda Seiki Seisakusho Co., Ltd. with a load of 900 g. 2 The coated paper was rubbed 13 times. The rubbed and unrubbed areas of the test print were visually compared and rated on a 5-point scale as follows. The evaluation results are shown in Table 4 below. -Evaluation criteria- A: Almost no discoloration can be seen. B: Very slight discoloration is observed. C: A slight discoloration is observed. D: Discoloration is clearly observed. E: The color of the abraded area has peeled off.

[0124] [Circulatory stability] 0.3 L of each of the inks obtained in the examples and comparative examples was prepared and circulated for 100 minutes at a flow rate of 0.3 L / min using a diaphragm pump NF60 manufactured by KNF Co., Ltd. 50 g of the circulated ink was filtered through a nylon filter with a mesh size of 10 μm (nylon mesh, mesh size 10 μm, #500 / 520 manufactured by Tanley Co., Ltd.) with an effective filtration area of ​​0.13 cm 2 Filtration was performed at 40°C and it was confirmed whether the ink passed through completely. If the ink passed through completely within 5 minutes (i.e., the entire 0.3 L volume was filtered), the result was recorded as "O", and if the ink did not pass through completely (i.e., the entire 0.3 L volume could not be filtered), the result was recorded as "X".

[0125] [Table 4]

[0126] As is clear from the results in Table 4, it was confirmed that the inks of the respective examples had good abrasion resistance and circulation resistance.

[0127] [Preparation Examples 2 to 6]: Preparation of overcoat agents. Using any of the binders obtained in Synthesis Examples 1 to 5 above, the components shown in Table 5 below were added and mixed with stirring to obtain a liquid. The resulting liquid was filtered through a membrane filter with a pore size of 3 μm to obtain the overcoat agents of Preparation Examples 2 to 6, respectively. The abbreviations in Table 5 below represent the following. W950: Chemipearl W950 (polyethylene water-based wax emulsion, manufactured by Mitsui Chemicals)

[0128] 50 μl of each of the inks in Examples 1 to 5 was measured and coated with OK Topcoat + 127.9 g / m (Oji Paper Co., Ltd.) at a speed of 200 mm / sec using a No. 3 bar coater in a PI-1210 automatic coating device (Tester Sangyo Co., Ltd.). 2(coated paper) and an image was formed. Then, it was dried at 70 degrees for 2 minutes. 50 μl of the overcoat agent of Preparation Examples 2 to 6 was coated at a speed of 200 mm / sec using a No. 3 bar coater in a PI-1210 automatic coater (manufactured by Tester Sangyo Co., Ltd.) so as to overlap the image-formed part of the obtained test print. Then, it was dried at 70 degrees for 2 minutes to obtain a test print. The obtained test print was compared with the uncoated Oji Paper OK topcoat + 127.9g / m using a Gakushin tester manufactured by Yasuda Seiki Seisakusho Co., Ltd. with a load of 900g. 2 The coated paper was rubbed 13 times. The rubbed and unrubbed areas of the test print were visually compared and rated on a 5-point scale as follows. The evaluation results are shown in Table 6 below. -Evaluation criteria- A: Almost no discoloration can be seen. B: Very slight discoloration is observed. C: A slight discoloration is observed. D: Discoloration is clearly observed. E: The color of the abraded area has peeled off.

[0129] [Table 5]

[0130] [Table 6]

[0131] As the results in Table 6 show, the test prints produced by combining the example inks and overcoat agents have excellent abrasion resistance. [Industrial Applicability]

[0132] The ink of the present invention has good circulation stability and good abrasion resistance of printed matter, and therefore can be suitably used in an inkjet recording apparatus equipped with an ink-circulation type inkjet head.

Claims

1. An ink comprising an organic solvent and a binder, the SP value of the binder being in the range of 9.8 or more and 12.3 or less.

2. The ink according to claim 1 , wherein the binder contains a (meth)acrylic monomer as a constituent monomer.

3. 3. The ink according to claim 1, wherein the binder contains a C1-C4 hydroxyalkyl (meth)acrylate as a constituent monomer, and the content of the C1-C4 hydroxyalkyl (meth)acrylate is 0.1 to 25 mass % relative to the total mass of the binder solids.

4. 3. The ink according to claim 1, wherein the binder has an acid value of 5 to 150 mg KOH / g.

5. The ink according to claim 1 or claim 2, wherein the binder has a Tg of 35 to 150°C.

6. 3. The ink according to claim 1 or claim 2, wherein the weight average molecular weight of the binder is from 30,000 to 120,000.

7. 3. The ink according to claim 1, wherein the organic solvent has a water-octanol partition coefficient of 2.00 or more and less than 3.

50.

8. The ink according to claim 1 or 2, comprising a C4-C12 alkanediol as the organic solvent.

9. 3. The ink according to claim 1, further comprising a wax, the content of the wax being 0.01 to 1.0% by mass relative to the total mass of the ink.

10. A set of an ink and an overcoat agent, comprising the ink according to claim 1 and an overcoat agent, the overcoat agent containing an organic solvent and a binder, and the SP value of the binder being in the range of 9.8 or more and 12.3 or less.

11. A recording medium on which an image is formed using the set of the ink and the overcoat agent according to claim 10.

12. A method for producing a recording medium, comprising forming an image on a recording medium using the ink according to claim 1, and then covering a part or all of the image-forming portion with an overcoat agent contained in the set of the ink and the overcoat agent according to claim 10.

Citation Information

Patent Citations

  • JP146196A

  • Voltage supervisory circuit

    JP1988091721A

  • Ink circulation device and inkjet recording device

    JP2017185716A

  • Inkjet ink and inkjet recording system

    JP2021021042A

  • Ink circulation system and inkjet printer

    JP2022052563A