Composition

A resin composition with polyphenylene sulfide, carbon-based particles, metal, and carbon fibers addresses the challenge of friction and wear stability in sliding parts, enhancing energy efficiency and mechanical element lifespan.

JP2024146813APending Publication Date: 2024-10-15LION IDEMITSU COMPOSITES CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024041693
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-15
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing resin compositions for sliding parts fail to achieve both stability of friction coefficient and wear resistance, particularly in high-load environments, and do not adequately address fluctuations in frictional force and wear.

Method used

A resin composition comprising 30 to 70% polyphenylene sulfide resin, 1 to 30% carbon-based particles, 5 to 40% metal fibers, and 5 to 40% carbon fibers, which provides excellent friction coefficient stability and wear resistance even in high-load conditions.

Benefits of technology

The composition exhibits stable friction coefficient and enhanced wear resistance, improving energy efficiency and mechanical element lifespan, and contributes to sustainable production by reducing frictional fluctuations and wear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146813000006
    Figure 2024146813000006
  • Figure 2024146813000001
    Figure 2024146813000001
  • Figure 2024146813000002
    Figure 2024146813000002
Patent Text Reader

Abstract

To provide a novel resin composition that enhances both friction coefficient stability and wear resistance.SOLUTION: A composition according to one embodiment of the present invention includes polyphenylene sulfide resin: 30-70 mass%, carbon-based particles: 1-30 mass%, metal fibers: 5-40 mass%, and carbon fibers: 5-40 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition which is excellent in both stability of the coefficient of friction and wear resistance. [Background technology]

[0002] The present invention relates to a resin composition that can be suitably used for sliding parts, such as shafts, bearings, and gears, where friction occurs, and to a molded article thereof.

[0003] The life of sliding parts is largely determined by the wear of the material, and therefore excellent wear resistance is required. In addition, when used as sliding parts of machines, it is preferable that the fluctuation of frictional force is small in transmitting power, and at the same time, it is preferable that the generated frictional force is low from the viewpoint of energy loss.

[0004] Metals and thermosetting resins that have been conventionally used for sliding parts exhibit sufficient heat resistance, but it is difficult to satisfy excellent friction and wear properties in addition to productivity and light weight.

[0005] Patent Document 1 describes a polyamide resin composition containing (A) a polyamide resin obtained from a mixed xylylenediamine consisting of 15 to 45 mol % of paraxylylenediamine and 85 to 55 mol % of metaxylylenediamine and an α,ω-linear aliphatic dibasic acid, (B) a fibrous reinforcing material, and (C) a solid lubricant, in which (B) is 8 to 65 wt % and (C) is 8 to 30 wt % relative to the total weight of (A) + (B) + (C), and the polyamide resin composition has excellent mechanical strength and sliding properties, and in particular, excellent friction and wear properties represented by a high limit PV value.

[0006] Patent Document 2 describes a polyphenylene sulfide resin composition capable of providing a molded article having high sliding properties and abrasion resistance as well as excellent mechanical properties such as tensile break strength, tensile break elongation, Charpy impact strength, and heat distortion temperature. The resin composition contains polyphenylene sulfide (A), a modified polyolefin composition (B), and a fibrous filler (C), and the content of the modified polyolefin composition (B) is 2 to 8 parts by mass per 100 parts by mass of the total of the polyphenylene sulfide (A), the modified polyolefin composition (B), and the fibrous filler (C).

[0007] Patent Document 3 describes a reel base with a torque limiter that transmits torque between first and second friction plates and a second rotating body, in which the first and second friction plates and the second rotating body are formed from a thermoplastic resin composition composed of a base resin and a first additive and a second additive that are added to the base resin, the base resin being a polyacetal resin or a polyphenylene sulfide resin, the first additive being one or more selected from an olefin-based polymer, a styrene-based polymer, and a fluorine-based polymer, and the second additive being one or more selected from a lubricating oil, a wax, a fatty acid, graphite, molybdenum disulfide, and a phosphate. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2006-45413 A [Patent Document 2] JP 2019-218568 A [Patent Document 3] Japanese Patent Application Publication No. 10-274252 Summary of the Invention [Problem to be solved by the invention]

[0009] However, Patent Documents 1 to 3 do not disclose both the variation in frictional force and the amount of wear, and do not consider compatibility between the stability of the friction coefficient and wear resistance. Therefore, the resin compositions of the above-mentioned conventional techniques are not sufficient in terms of compatibility between the stability of the friction coefficient and wear resistance, and there is room for improvement.

[0010] An object of one aspect of the present invention is to provide a novel resin composition that is excellent in both stability of the friction coefficient and wear resistance. [Means for solving the problem]

[0011] As a result of intensive research to solve the above problems, the present inventors have found for the first time that a composition containing a predetermined amount of polyphenylene sulfide resin, graphite, and metal fibers is excellent in both stability of friction coefficient and wear resistance not only in low load environments but also in high load environments, and have completed the present invention. That is, a composition according to one aspect of the present invention is configured to contain 30 to 70 mass % of polyphenylene sulfide resin, 1 to 30 mass % of carbon-based particles, 5 to 40 mass % of metal fibers, and 5 to 40 mass % of carbon fibers. Effect of the Invention

[0012] According to one aspect of the present invention, it is possible to provide a novel resin composition that is excellent in both stability of friction coefficient and wear resistance even in a high-load environment. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a diagram showing an outline of a friction and wear characteristic test carried out in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] One embodiment of the present invention will be described in detail below. In this specification, unless otherwise specified, "A to B" indicating a numerical range means "A or more and B or less."

[0015] <1. Composition> (overview) A composition according to one embodiment of the present invention includes 30 to 70 mass% of polyphenylene sulfide resin, 1 to 30 mass% of carbon-based particles, 5 to 40 mass% of metal fibers, and 5 to 40 mass% of carbon fibers. The composition according to one embodiment of the present invention includes a blend obtained by blending raw materials for the composition including the above-mentioned components, and a kneaded product obtained by melt-kneading the raw materials for the composition including the above-mentioned components.

[0016] The composition according to one embodiment of the present invention contains the polyphenylene sulfide resin, carbon-based particles, metal fibers, and carbon fibers in the above-mentioned predetermined amounts, and is a resin composition that has excellent friction coefficient stability and wear resistance not only in low load environments but also in high load environments. By using such a resin composition in sliding parts, the excellent friction coefficient stability can be improved, thereby improving the energy efficiency of sliding, and the excellent wear resistance can be improved, thereby improving the life of mechanical elements. Such effects also contribute to the achievement of, for example, Goal 12 of the Sustainable Development Goals (SDGs) proposed by the United Nations, "Responsible Consumption and Production."

[0017] (Use of the composition) The composition according to one embodiment of the present invention has excellent friction coefficient stability and wear resistance, and therefore can be suitably used as a material for sliding parts used on sliding surfaces. Therefore, the composition according to one embodiment of the present invention can be used as a composition for sliding parts. The composition according to one embodiment of the present invention can be suitably used as a composition for shafts, bearings, gears, etc. Therefore, the composition according to one embodiment of the present invention can be used as a composition for shafts, bearings, gears, etc.

[0018] In addition, the composition according to one embodiment of the present invention has excellent heat dissipation properties, and can therefore be more suitably used as a composition for sliding parts used under severe conditions such as high speeds.

[0019] (Polyphenylene sulfide resin) Polyphenylene sulfide resin (hereinafter also referred to as "PPS") is a polymer having a structural unit represented by the following formula (I).

[0020] [ka] (In formula (I), Ar represents a phenylene-containing group, and S represents sulfur.) If the structural unit represented by the above formula (I) is defined as 1 mole (basic mole), the PPS used in the present invention is a polymer containing this structural unit in an amount of usually 50 mol % or more, preferably 70 mol % or more, and more preferably 90 mol % or more.

[0021] In the above formula (I), Ar may have a group other than phenylene, and the phenylene may have a substituent. The number of carbon atoms in Ar is, for example, 6 to 20. Examples of Ar include the following structures. [ka]

[0022] PPS may be a homopolymer consisting of the same structural unit, a copolymer having two or more different structural units, or a mixture of these. The copolymer may be a random copolymer or a block copolymer.

[0023] The polymer chain of PPS may be partially substituted with other polymers within the scope of not impairing the effects of the present invention. Examples of the polymer to be substituted include polyester-based polymers, polyarylene ether-based polymers, polystyrene-based polymers, polyolefin-based polymers, fluorine-containing polymers, polyolefin-based elastomers, and silicone-based elastomers.

[0024] PPS can be produced by known methods, for example, as described in JP-B-45-3368, JP-B-52-12240, etc. PPS may be heated in air to increase its molecular weight, or may be chemically modified with a compound such as an acid anhydride.

[0025] The melt viscosity of PPS at a resin temperature of 310°C and a shear rate of 1000 (1 / sec) is preferably 10 to 1000 Pa·S, more preferably 20 to 300 Pa·S, and even more preferably 70 to 100 Pa·S. The melt viscosity of PPS is measured with a capillary rheometer.

[0026] The PPS may also contain a filler, such as glass fiber or carbon fiber.

[0027] (Actions and Effects of Polyphenylene Sulfide Resin) Since PPS is a crystalline resin, it has excellent chemical resistance. In addition, PPS also has excellent heat resistance. Therefore, when the composition according to one aspect of the present invention contains PPS, the chemical resistance and heat resistance of the composition can be improved. The composition according to one aspect of the present invention contains 30 to 70 mass % of PPS. When the content of PPS in the composition is within the above range, the chemical resistance and heat resistance of the composition can be sufficiently improved.

[0028] (Carbon-based particles) Carbon-based particles refer to particulate carbon materials. Carbon materials are materials whose main component is carbon atoms, for example, materials containing 95% by mass or more of carbon atoms. The type of carbon-based particles is not particularly limited. Examples of carbon-based particles include graphite, carbon black, and activated carbon. These may be used alone or in combination of two or more types in any ratio.

[0029] (Actions and Effects of Carbon-Based Particles) The composition according to one embodiment of the present invention contains carbon-based particles, which tends to improve the wear resistance. The composition according to one embodiment of the present invention contains 1 to 30 mass% of carbon-based particles. When the content of the carbon-based particles in the composition is within the above range, the wear resistance of the composition can be sufficiently improved.

[0030] (Preferred types of carbon-based particles) The carbon-based particles are preferably graphite particles. Graphite is also called graphite. Graphite is broadly classified into natural graphite and artificial graphite. Natural graphite is further classified into three types: amorphous graphite, scaly graphite, and massive (scaly) graphite. The graphite contained in the composition according to one embodiment of the present invention may be natural graphite or artificial graphite. By blending softer graphite among the carbon-based particles, wear of the sliding counterpart material is reduced and abrasive wear is suppressed. The graphite is preferably natural graphite.

[0031] (Preferable content of carbon-based particles) From the viewpoint of further improving the abrasion resistance, the content of the carbon-based particles in the composition according to one embodiment of the present invention is preferably 10% by mass or more, more preferably 15% by mass or more, and preferably less than 20% by mass. More preferably, it is 1% by mass or more and less than 20% by mass.

[0032] (Average particle size of carbon-based particles) The average particle size of the carbon-based particles is preferably 1 μm or more and 50 μm or less, more preferably 5 μm or more, and more preferably 20 μm or less. Here, in this specification, the "average particle size" refers to a value measured by a laser diffraction / scattering method and on a volume basis using a SALD-2300 manufactured by SHIMADZU.

[0033] (Metal Fiber) The type of metal fiber may be appropriately determined and is not particularly limited. For example, metal fibers containing soft metals such as brass, copper, phosphor bronze, and hard metals such as carbon steel can be mentioned. These may be used alone or in combination of two or more types in any ratio. Here, "soft metal" refers to a metal having a hardness of less than 200HV based on Vickers hardness. Also, "hard metal" refers to a metal having a hardness of 200HV or more based on Vickers hardness.

[0034] (Actions and Effects of Metal Fibers) The composition according to one embodiment of the present invention contains metal fibers, which tends to improve the stability of the friction coefficient of the composition. In addition, the composition according to one embodiment of the present invention contains metal fibers, which tends to improve the thermal conductivity. As a result of the improved thermal conductivity, the composition has excellent heat dissipation properties and is suppressed from softening or melting the resin, so that the composition can be more suitably used as a composition for sliding parts used under harsh conditions such as high speeds.

[0035] The composition according to one embodiment of the present invention contains 5 to 40 mass % of metal fibers. When the content of the metal fibers in the composition is within the above range, the effect of improving the stability of the friction coefficient and the thermal conductivity of the composition can be sufficiently obtained.

[0036] (Preferred types of metal fibers) The metal fiber preferably contains a soft metal. By containing a soft metal, the metal fiber can suppress the wear of the mold during injection molding of the composition. In addition, when used as a sliding part, the wear of the sliding counterpart material is reduced, and abrasive wear is suppressed. From the viewpoint of the wear of the counterpart material and improvement of thermal conductivity, the soft metal is preferably copper or phosphor bronze.

[0037] (Preferable content of metal fibers) From the viewpoint of improving the stability of the friction coefficient and wear resistance of the composition, the content of the metal fiber in the composition according to one embodiment of the present invention is preferably 5 to 35 mass%, more preferably 10 to 33 mass%. From the viewpoint of improving the stability of the friction coefficient and wear resistance of the composition under a particularly high load environment such as the test condition of a load of 300 N in the friction and wear property test in the Examples described later, the content of the metal fiber in the composition according to one embodiment of the present invention is particularly preferably 10 to 15 mass%. In addition, from the viewpoint of improving the thermal conductivity (heat dissipation), the content of the metal fiber in the composition according to one embodiment of the present invention is preferably 11 to 40 mass%, more preferably 15 to 30 mass%.

[0038] (Average fiber diameter and length of metal fibers) The average fiber diameter and average fiber length of the metal fibers may be appropriately determined and are not particularly limited, but for reasons described below, it is more preferable to use short fibers having an average fiber length of 20 mm or less and an average fiber diameter of 150 μm or less, or short fibers having an average fiber length of 6 mm or less and an average fiber diameter of 100 μm or less, or short fibers having an average fiber length of 3 mm or less and an average fiber diameter of 40 μm or less. In this specification, the term "average fiber length" refers to the length of the fibers and means the average value when 50 or more fibers are measured using a KEYENCE VHX-5000 digital microscope.

[0039] When soft copper fibers or the like are used, if the average fiber length is within the above range, the fibers are less likely to be entangled with each other and feeding failures are less likely to occur. When the average fiber length of the metal fibers is 6 mm or less, the composition can be well kneaded, improving the mass productivity of the composition. In addition, in order to increase the contact area of ​​the metal fibers on the sliding surface, it is preferable that the average fiber diameter of the metal fibers is 100 μm or less. In this specification, the "average fiber diameter D" of the metal fibers represents the thickness of the fibers and means a value calculated from the specific gravity ρ of the metal fibers, the number N of the metal fibers (100 or more) and their weight W, the average fiber length L, and pi using the following formula. D = √{[(W / ρ) / N] / (π×L)}

[0040] Although there are no particular lower limits for the average fiber length and average fiber diameter of the metal fibers, from the viewpoint of preventing the metal fibers from falling off during the process of being subjected to friction, the average fiber length of the metal fibers is preferably 1.0 mm or more, more preferably 1.5 mm or more, and the average fiber diameter of the metal fibers is preferably 10 μm or more, more preferably 15 μm or more.

[0041] (Carbon Fiber) Carbon fiber refers to fiber with a carbon content of 90% or more obtained by baking organic fiber. The type of carbon fiber is not particularly limited and can be selected appropriately. From the viewpoint of improving strength or thermal conductivity, it is preferable that the carbon fiber has a density of 1.70 or more. For example, polyacrylonitrile (PAN)-based carbon fiber can be suitably used as such carbon fiber. One type of carbon fiber may be used alone, or two or more types may be used in any ratio.

[0042] (Actions and Effects of Carbon Fiber) The inclusion of carbon fibers in the composition according to one embodiment of the present invention tends to improve the wear resistance. In addition, the inclusion of carbon fibers in the composition according to one embodiment of the present invention tends to improve the mechanical strength (e.g., tensile strength, bending strength, etc.) and thermal conductivity of the composition.

[0043] The composition according to one embodiment of the present invention contains 5 to 40 mass % of carbon fiber. When the content of carbon fiber in the composition is within the above range, the wear resistance, mechanical strength, and thermal conductivity of the composition can be sufficiently improved.

[0044] (Preferable carbon fiber content) The carbon fiber content in the composition according to one embodiment of the present invention is preferably 10% by mass or more, more preferably 20% by mass or more, from the viewpoint of mechanical strength. Also, from the viewpoint of molding, it is preferably 35% by mass or less. When a PPS composition containing carbon fiber as a filler is used as the PPS raw material, the carbon fiber content in the composition according to one embodiment of the present invention is the total amount including the amount of carbon fiber contained in the PPS raw material.

[0045] The total content of the carbon fiber and the metal fiber in the composition according to one embodiment of the present invention is preferably 50% by mass or less of the composition. This can prevent the fluidity of the composition from decreasing, and can improve the mass productivity of the composition. The mass ratio of the carbon fiber and the metal fiber is not particularly limited, but from the viewpoint of improving the thermal conductivity of the composition, it is preferable to use a larger amount of the metal fiber than the carbon fiber. In addition, the total content of the carbon fiber and the metal fiber in the composition according to one embodiment of the present invention is preferably 10% by mass or more of the composition, and more preferably 20% by mass or more.

[0046] (Average fiber diameter and average fiber length of carbon fibers) The average fiber length and average fiber diameter of the carbon fiber may be appropriately determined and are not particularly limited. For example, chopped fibers having an average fiber length of 20 mm or less and an average fiber diameter of 30 μm or less can be suitably used as the carbon fiber. From the viewpoint of mechanical strength and thermal conductivity, the average fiber length of the carbon fiber is preferably 3 mm or more and 10 mm or less, and more preferably 3 mm or more and 7 mm or less. In addition, from the viewpoint of increasing the contact area with the counter material and increasing the carbon fibers supporting the sliding interface, the average fiber diameter of the carbon fiber is preferably 1 μm or more and 20 μm or less. In this specification, when the carbon fiber is a chopped fiber, the average fiber length may be referred to as the "cut length". In this specification, the "average fiber length" of the carbon fiber represents the length of the fiber and means the average value when 50 or more fibers are measured with a KEYENCE digital microscope VHX-5000, and the "average fiber diameter" of the carbon fiber means the average value when 50 or more fibers are measured with an electron microscope.

[0047] (Other Ingredients) In addition to the above-mentioned components, the composition according to one aspect of the present invention may contain any additives such as antioxidants, nucleating agents, plasticizers, release agents, flame retardants, pigments, and antistatic agents, as long as the additives do not impair the effects of the present invention. For example, an antioxidant may be added in an amount of about 1% by mass of the total amount in order to increase the thermal stability of the composition. The additives may be any additives commonly used in the relevant technical field.

[0048] (Production method of the composition) The method for producing the composition according to one embodiment of the present invention is not particularly limited, and the composition can be produced by a known method. For example, the above-mentioned components may be mixed at room temperature (e.g., 20°C to 30°C), and then kneaded by various methods such as melt kneading, and the method is not particularly limited.

[0049] Among the mixing and kneading methods, melt kneading using a twin screw extruder is preferably used. In the melt kneading using a twin screw extruder, it is preferable to knead at 300°C or higher from the viewpoint of mass productivity. Also, it is preferable to knead at 350°C or lower from the viewpoint of minimizing thermal decomposition of the raw materials of the composition.

[0050] <2. Molded body> The present invention also includes a molded article obtained by molding the composition according to one aspect of the present invention. The composition according to one aspect of the present invention in the molded article according to one aspect of the present invention has already been described, and will not be repeated here.

[0051] (Method of Manufacturing Molded Product) The molded article according to one embodiment of the present invention can be produced by a production method including a molding step of molding the composition according to one embodiment of the present invention. In the molding step, the method of molding the composition according to one embodiment of the present invention is not particularly limited. Known molding methods such as injection molding and extrusion molding can be used. Among them, injection molding is preferably used.

[0052] The molding temperature during injection molding is preferably 300° C. or higher from the viewpoint of molding flowability, and is preferably 350° C. or lower from the viewpoint of minimizing thermal decomposition of the components in the composition.

[0053] (Use of Molded Body) The molded article obtained by molding the composition according to one embodiment of the present invention has excellent friction coefficient stability and wear resistance, and therefore can be suitably used as a sliding part used on a sliding surface. The sliding part using the molded article according to one embodiment of the present invention can be suitably used as a sliding part of a machine element such as a shaft, a bearing, or a gear, which requires a stable friction coefficient and wear resistance.

[0054] 〔summary〕 The composition according to the first aspect of the present invention comprises 30 to 70 mass % of polyphenylene sulfide resin, 1 to 30 mass % of carbon-based particles, 5 to 40 mass % of metal fibers, and 5 to 40 mass % of carbon fibers.

[0055] In the composition according to the second aspect of the present invention, in the above-mentioned first aspect, the content of the carbon-based particles is preferably 1% by mass or more and less than 20% by mass.

[0056] In the composition according to the third aspect of the present invention, in the above-mentioned first or second aspect, the content of the metal fibers is preferably 5 to 35 mass %.

[0057] In the composition according to a fourth aspect of the present invention, in any one of the first to third aspects, the carbon fibers preferably have a density of 1.70 or more.

[0058] In the composition according to a fifth aspect of the present invention, in any one of the first to fourth aspects, the carbon-based particles preferably have an average particle size of 20 μm or less.

[0059] In the composition according to a sixth aspect of the present invention, in any one of the first to fifth aspects, the carbon-based particles are preferably graphite.

[0060] In the composition according to a seventh aspect of the present invention, in the sixth aspect, the graphite is preferably natural graphite.

[0061] A composition according to an eighth aspect of the present invention, in any one of the first to seventh aspects, preferably has the metal fibers containing a soft metal.

[0062] A composition according to a ninth aspect of the present invention, in the above eighth aspect, is preferably such that the soft metal is copper or phosphor bronze.

[0063] In the composition according to a tenth aspect of the present invention, in any one of the above aspects 1 to 9, the metal fibers preferably have an average fiber length of 6 mm or less and an average fiber diameter of 100 μm or less.

[0064] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in the respective embodiments are also included in the technical scope of the present invention. EXAMPLES

[0065] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0066] <Raw materials for the composition> The raw materials of the compositions used in the examples and comparative examples are as follows: Polyphenylene sulfide resin (PPS): DSP T-3G manufactured by DIC Corporation was used. These PPS are crosslinked PPS, and have a melt viscosity of 72 to 98 Pa·S at a resin temperature of 310°C and a shear rate of 1000 (1 / sec). Carbon fiber (CF): Polyacrylonitrile (PAN) carbon fiber (density 1.82) (manufactured by Mitsubishi Chemical Corporation, TR06U B4E, average fiber diameter 6 μm, average fiber length 6 mm) was used. The average fiber diameter and average fiber length of the carbon fiber were measured by the measurement method described above. Metal fiber: Copper fiber (KC Metal Fiber C1100, average fiber diameter 23 μm, average fiber length 1.7 mm, manufactured by Kogi Co., Ltd.) was used. The average fiber diameter and average fiber length of the copper fiber were measured by the measurement method described above. Metal fiber: Phosphor bronze fiber (manufactured by Kogi Co., Ltd., PBC2C, average fiber diameter 16 μm, average fiber length 1.7 mm) was used. The average fiber diameter and average fiber length of the phosphor bronze fiber were measured by the measurement method described above. Carbon-based particles: Natural graphite (ACP-1000, average particle size 14 μm, manufactured by Nippon Graphite Co., Ltd.) was used. The average particle size of the graphite was measured by the measurement method described above.

[0067] Example 1 The components were mixed according to the mixing ratios shown in Table 2, and melt-kneaded at 320°C using a TEM-37SS-13 / 3V (twin-screw kneading extruder, manufactured by Shibaura Machine Co., Ltd.) to obtain a resin composition of Example 1. The obtained resin composition was injection molded into a hollow cylindrical test piece 1 for friction and wear property testing, as shown in Fig. 1. As indicated by 1001 in Fig. 1, the test piece 1 has three hemispherical protrusions 10 with a radius of 1.0 mm on the upper surface (sliding surface) of the hollow cylinder.

[0068] [Examples 2 to 6, Comparative Examples 1 to 5] Test pieces of Examples 2 to 6 and Comparative Examples 1 to 5 were prepared in the same manner as in Example 1, except that the components were mixed according to the mixing ratios shown in Tables 1 to 3.

[0069] <Friction and wear characteristic test> The shape of the test specimen was as shown in Figure 1, and the test was conducted in accordance with JIS K7218 Method A (1986) except that the number of measurement points was 1. The test material used was a steel equivalent to S45C as specified in JIS-G4051 (2016).

[0070] (Wear amount) The amount of wear was measured at room temperature (20 to 30°C) under a thrust load of 50N, 150N or 300N at a test speed of 0.5m / s for 3km. The amount of wear was calculated using the following formula. Wear amount (Δh) = h2-h1 In the above formula, h2 represents the height of the hemispherical projection 10a after the test as shown by 1003 in FIG. 1, and h1 represents the height of the hemispherical projection 10 before the test as shown by 1002 in FIG.

[0071] The height h1 of the hemispherical projection 10 was obtained by sandwiching the upper and lower surfaces of the test piece 1 before the test between two metal circular flat plates and measuring the center (i.e., the center of the circle) of the circular flat plate abutting the upper surface side with a Digimatic Indicator (ID-C112, manufactured by Mitutoyo Corporation). Similarly, the height h2 of the hemispherical projection 10a was obtained by measuring the center (i.e., the center of the circle) of the circular flat plate abutting the upper surface side of the test piece 1 after the test with a Digimatic Indicator.

[0072] Based on the measurement results of the amount of wear, the wear resistance was evaluated with a three-level score of 1 to 3 according to the following criteria. 3: Wear amount Δh (mm) is less than 0.19 (150N Comparative Example 5 reference) 2: Wear amount Δh (mm) is 0.19 or more and less than 0.40 1: Wear amount Δh (mm) is 0.40 or more (150N Comparative Example 3 reference) A score of 1 indicates poor abrasion resistance, a score of 2 indicates good abrasion resistance and a score of 3 indicates extremely good abrasion resistance.

[0073] (friction coefficient Δμ) The friction coefficient Δμ was recorded as the difference between the average value of the friction coefficient μ for approximately 10 minutes from the start of the test (the average value of the values ​​measured at a sampling rate of 3 seconds) and the average value of the friction coefficient μ for approximately 10 minutes immediately before the end of the test (the average value of the values ​​measured at a sampling rate of 3 seconds). The absolute value of the friction coefficient (Δμ) = (average value for about 10 minutes immediately before the end of the test - average value for about 10 minutes from the start of the test) was recorded.

[0074] Based on the measurement results of the friction coefficient Δμ, the stability of the friction coefficient was evaluated with a three-level score of 1 to 3 according to the following criteria. 3: Friction coefficient Δμ is less than 0.05 2: Friction coefficient Δμ is 0.05 or more and less than 0.1 (150N, see Comparative Example 5) 1: Friction coefficient Δμ is 0.1 or more (150N, see Comparative Example 3) A score of 1 indicates poor coefficient of friction stability, a score of 2 indicates good coefficient of friction stability, and a score of 3 indicates exceptional coefficient of friction stability.

[0075] <Thermal conductivity measurement test> Plates (60 mm square, 2 mm thick) for thermal conductivity measurement tests were molded by injection molding each of the resin compositions of Examples 1 to 3 and Comparative Examples 4 to 5. The thermal conductivity of each sample plate was measured using a hot disk method thermal property measurement device (TPA-501, manufactured by Kyoto Electronics Manufacturing Co., Ltd.).

[0076] Based on the results of the thermal conductivity measurements, the heat dissipation performance was evaluated using a three-level score of 1 to 3 according to the following criteria. 3: Thermal conductivity (W / m K) exceeds 5.0 2: Thermal conductivity (W / m K) is 2.0 or more and 5.0 or less (see Comparative Example 5) 1: Thermal conductivity (W / m K) is less than 2.0 (see Comparative Example 4) A score of 1 indicates poor heat dissipation, a score of 2 indicates good heat dissipation, and a score of 3 indicates exceptionally good heat dissipation.

[0077] <Result> The results are shown in Tables 1 to 3. In the tables, "-" means that the component was not blended.

[0078] [Table 1]

[0079] [Table 2]

[0080] [Table 3]

[0081] A comparison between Comparative Example 1 and Comparative Example 3 showed that the amount of wear was significantly reduced by blending carbon fibers.

[0082] In addition, a comparison between Comparative Example 1 and Comparative Example 2, or a comparison between Comparative Example 4 and Comparative Example 5, showed that the amount of wear was reduced by adding graphite. This is believed to be because the addition of soft graphite reduced the wear of the mating material, suppressing abrasive wear.

[0083] In Comparative Examples 1 to 5, the amount of wear was greater under a load of 150 N compared to a load of 50 N. In contrast, in Examples 1 to 3, which contained all of carbon fiber, graphite, and copper fiber, the amount of wear was smaller under both a load of 50 N and a load of 150 N. This demonstrates that the resin compositions of Examples 1 to 3 have excellent wear resistance.

[0084] In addition, a comparison between Comparative Example 5 and Examples 1 to 3 showed that in Examples 1 to 3, which further contained copper fiber together with a certain amount of carbon fiber and graphite, the friction coefficient fluctuation (friction coefficient Δμ) during sliding was reduced. Thus, it was shown that the resin compositions of Examples 1 to 3 have excellent stability of the friction coefficient. By containing copper fiber together with a certain amount of carbon fiber and graphite, it was possible to further reduce the amount of resin wear even under a load of 150N, and also to further reduce the friction coefficient fluctuation during sliding. Thus, it was shown that the resin compositions of Examples 1 to 3 have excellent stability of the friction coefficient and wear resistance even under a high load environment.

[0085] Furthermore, a comparison between Comparative Examples 4-5 and Examples 1-3 showed that Examples 1-3, which contain copper fibers together with a certain amount of carbon fibers and graphite, have high thermal conductivity, and the thermal conductivity tends to increase as the copper fiber content increases. Therefore, it was shown that the resin compositions of Examples 1-3 have excellent heat dissipation properties.

[0086] As for Examples 4 to 6 in which phosphor bronze fibers were used instead of copper fibers as metal fibers, Examples 4 to 6 in which all of carbon fibers, graphite, and phosphor bronze fibers were included showed results of small wear amounts under both loads of 50 N and loads of 150 N, and also showed results of reduced friction coefficient fluctuations (friction coefficient Δμ) during sliding. Thus, it was demonstrated that the resin compositions of Examples 1 to 3 were excellent in wear resistance. Thus, it was demonstrated that the resin compositions of Examples 4 to 6 in which phosphor bronze fibers were used instead of copper fibers also showed excellent wear resistance and stability of the friction coefficient.

[0087] In a particularly high load environment, such as a test condition of a load of 300 N, Example 4 exhibited the most excellent wear resistance and stability of the friction coefficient.

[0088] The above results show that a composition containing 30 to 70 mass% polyphenylene sulfide resin, 1 to 30 mass% carbon-based particles, 5 to 40 mass% metal fibers, and 5 to 40 mass% carbon fibers has excellent friction coefficient stability and wear resistance even in a high-load environment. [Industrial Applicability]

[0089] The composition according to one aspect of the present invention can be suitably used as a resin composition for sliding parts. [Explanation of symbols]

[0090] 1 Test piece 10, 10a hemispherical process

Claims

1. A composition comprising 30 to 70 mass% of polyphenylene sulfide resin, 1 to 30 mass% of carbon-based particles, 5 to 40 mass% of metal fibers, and 5 to 40 mass% of carbon fibers.

2. The composition according to claim 1 , wherein the content of the carbon-based particles is 1% by mass or more and less than 20% by mass.

3. 3. The composition according to claim 1, wherein the content of the metal fibers is 5 to 35% by mass.

4. The composition according to claim 1 or 2, wherein the carbon fibers have a density of 1.70 or more.

5. 3. The composition according to claim 1 or 2, wherein said carbon-based particles have an average particle size of 20 μm or less.

6. 3. The composition of claim 1 or 2, wherein said carbon-based particles are graphite.

7. The composition of claim 6, wherein said graphite is natural graphite.

8. The composition of claim 1 or 2, wherein the metal fibers comprise a soft metal.

9. The composition of claim 8, wherein the soft metal is copper or phosphor bronze.

10. 3. The composition according to claim 1, wherein the metal fibers have an average fiber length of 6 mm or less and an average fiber diameter of 100 μm or less.

Citation Information

Patent Citations

  • Torque limiter

    JP1998274252A

  • Polyamide resin composition excellent in slidability

    JP2006045413A

  • Resin composition and molded article thereof

    JP2019218568A