Curable resin composition and method for manufacturing printed circuit board using curable resin composition

A curable resin composition with specific properties and inorganic filler ratios ensures complete filling and smooth polishing of through holes in printed wiring boards, addressing the issue of dents and enhancing electromagnetic properties.

JP2024146833APending Publication Date: 2024-10-15TAIYO HOLDINGS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024048596
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-25
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing curable resin compositions used for filling through holes in printed wiring boards often fail to completely fill both sides of the board, leading to dents and uneven surfaces after polishing, especially with smaller diameter holes.

Method used

A curable resin composition containing a curable resin, curing agent, and inorganic filler, with specific ratios and properties, is used to fill through holes, ensuring that the cured material covers a sufficient area around the holes to facilitate smooth polishing and minimize dents, by adjusting the filling amount and curing conditions.

Benefits of technology

The composition allows for a smooth surface finish after polishing, reducing the occurrence of recesses in through holes, and can be tailored for electromagnetic noise suppression and inductor characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146833000001_ABST
    Figure 2024146833000001_ABST
Patent Text Reader

Abstract

To provide a curable resin composition capable of suppressing a depression from occurring in a polishing and smoothing step after charge into a through hole.SOLUTION: A curable resin composition includes a curable resin, a curing agent and an inorganic filler. A plurality of approximately cylindrical through holes 2 having a wall surface subjected to plating and having an inner diameter of 0.12 mm is provided at an equal interval of 1 mm in a substrate having a surface subjected to plating and having the total thickness of 1.6 mm; when charging the through holes 2 with the curable resin composition from the side of one main surface of the substrate to cure the curable resin composition, the main surface has a cured product coated area 4 in which the cured product of the curable resin composition coats the main surface of the substrate so as to cover a periphery of the individual through hole 2; and when setting the straight line longest distance of the individual cured product coated area 4 to rL (μm) and setting the straight line longest distance of a line segment going a center of a line segment of rL to rS (μm), the cured product coated area 4 satisfying 1≤rL / rS≤1.5 is 50% or more of the entire cured product coated area.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable resin composition, and more particularly to a curable resin composition that can be suitably used as a filler for filling penetrating holes such as through-holes in printed wiring boards, and a method for producing a printed wiring board using the curable resin composition. [Background technology]

[0002] As electronic devices become smaller and more functional, there is a demand for finer patterns on printed wiring boards, smaller mounting areas, and higher density component mounting. For this reason, multilayer boards such as double-sided boards with through holes that form interlayer connections to electrically connect different wiring layers, and build-up wiring boards in which an insulating layer and a conductor circuit are formed in sequence on a core material, and interlayer connections are made with via holes, etc., are being used.

[0003] In such printed wiring boards, recesses between conductor circuits on the surface, through holes with wiring layers formed on the inner wall surfaces, via holes, and other holes are generally filled with a thermosetting resin composition. As the thermosetting resin composition, a curable resin composition containing an epoxy resin as a curable resin component, an epoxy resin curing agent, and an inorganic filler is generally used. In addition, the hole filling process is performed by filling the holes in the substrate with the curable resin composition by means of screen printing or the like, curing the curable resin composition, and then polishing the excess cured material to smooth the substrate.

[0004] In recent years, with the trend toward smaller diameters of through-holes and via-holes, there has been an increasing demand for curable resin compositions to have excellent filling properties. For example, it is known that the filling properties can be improved by blending a specific inorganic filler into a curable resin composition (e.g., Patent Documents 1 and 2, etc.). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-235121 A [Patent Document 2] JP 2017-71656 A Summary of the Invention [Problem to be solved by the invention]

[0006] When a curable resin composition is filled into a through hole such as a through hole from one side of a printed wiring board by a printing means, in the case of a curable resin composition having excellent filling property as described above, the curable resin composition discharged from the through hole opening on the other side of the printed wiring board wets and spreads, and when the excess portion is polished after the curable resin composition is cured, the through hole is not completely filled and a dent is generated.

[0007] Accordingly, an object of the present invention is to provide a curable resin composition which can be smoothed by polishing after filling into a through-hole and which is less likely to produce a recess in the through-hole. [Means for solving the problem]

[0008] The present inventors have noticed that even if the curable resin composition spreads from the through-hole opening on the side opposite to the printed surface of the printed wiring board, the surface can be smoothed in a subsequent polishing step depending on the way the composition spreads. As a result of further investigation, the present inventors have found that the shape of the spread affects the smoothness after polishing. The present invention is based on this finding. That is, the gist of the present invention is as follows.

[0009] [1] A curable resin composition comprising a curable resin, a curing agent, and an inorganic filler, A printed wiring board having a thickness of 1.6 mm and a total thickness of 1.6 mm, the board having a plated surface and a plurality of substantially cylindrical through holes having an inner diameter of 0.12 mm and plated walls at equal intervals of 1 mm, is filled with the curable resin composition from one main surface of the printed wiring board, and the curable resin composition is then cured. When the main surface of the printed wiring board is viewed from the front on the main surface opposite to the filling side, the main surface has a cured product covering region in which a cured product of the curable resin composition covers the main surface of the board so as to cover the periphery of each through hole, The longest straight line distance of each hardened coating area is r L (μm), and L The longest straight line distance between the center of the line segment is r S (μm), 1≦r L / r S ≦1.5 A curable resin composition, characterized in that the cured product coating area satisfying the above requirement accounts for 50% or more of the total cured product coating area. [2] The curable resin composition according to [1], wherein the inorganic filler is contained in an amount of 40 to 90 mass % based on the total solid content of the curable resin composition. [3] The curable resin composition according to [1] or [2], wherein the inorganic filler has an average particle size of 0.1 to 20 μm. [4] The curable resin composition according to any one of [1] to [3], wherein the inorganic filler comprises a magnetic filler. [5] A method for producing a printed wiring board using the curable resin composition according to any one of [1] to [4], comprising the steps of: A printed wiring board having a plurality of substantially cylindrical through holes is prepared; filling the through-holes with the curable resin composition by printing from one main surface side of the printed wiring board; The filled curable resin composition is cured. Including, The method is characterized in that, when filling the curable resin composition, the curable resin composition is discharged from a through-hole on a main surface of the printed wiring board opposite to the printed side, and the filling amount of the curable resin composition is adjusted so that the curable resin composition does not come into contact with the curable resin composition discharged from an adjacent through-hole. [6] The method according to [5], further comprising polishing a main surface of the printed wiring board opposite to a printed side after the filled curable resin composition is cured. Effect of the Invention

[0010] According to the present invention, it is possible to provide a curable resin composition which can be polished to smooth the through-hole after filling, and which is less likely to cause recesses in the through-hole. [Brief description of the drawings]

[0011] [Figure 1a] FIG. 2 is a schematic diagram illustrating a process for producing a printed wiring board in which holes are filled with the curable resin composition of the present invention. [Figure 1b] FIG. 2 is a schematic diagram illustrating a process for producing a printed wiring board in which holes are filled with the curable resin composition of the present invention. [Figure 1c] FIG. 2 is a schematic diagram illustrating a process for producing a printed wiring board in which holes are filled with the curable resin composition of the present invention. [Figure 1d] FIG. 2 is a schematic diagram illustrating a process for producing a printed wiring board in which holes are filled with the curable resin composition of the present invention. [Diagram 2] This is a front view of the main surface of a printed wiring board opposite the printed side, in which a plurality of through holes are provided at regular intervals, and a curable resin composition filled in each through hole is cured. [Diagram 3] 3 is a cross-sectional view taken along the line XX' in FIG. 2. [Figure 4] This is an enlarged view of any one of the through holes shown in FIG. 3 (when 1≦rL / rS≦1.5). [Diagram 5] This is an enlarged view of any one of the through holes shown in FIG. 3 (when rL / rS≧1.5). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] <Curable resin composition> The curable resin composition of the present invention contains a curable resin, a curing agent, and an inorganic filler as essential components. In the present invention, when a printed wiring board having a thickness of 1.6 mm and a total thickness of 1.6 mm and a plurality of substantially cylindrical through holes having an inner diameter of 0.12 mm and plated on the wall surface are provided at equal intervals of 1 mm in a substrate having a plated surface and the through holes are filled with the curable resin composition from one main surface side of the printed wiring board, and the curable resin composition is cured, When the main surface of the printed wiring board is viewed from the front on the main surface opposite to the filling side, the main surface has a cured product covering region in which a cured product of the curable resin composition covers the main surface of the board so as to cover the periphery of each through hole, The longest straight line distance of each hardened coating area is r L (μm), and L The longest straight line distance between the center of the line segment is r S (μm), 1≦r L / r S ≦1.5 By preparing a curable resin composition such that the cured product coating area satisfying the above requirement accounts for 50% or more of the total cured product coating area, it is possible to obtain a printed wiring board having a smooth surface free of dents after surface polishing in a printed wiring board in which the through-holes are filled with the cured product of the curable resin composition. The following will explain in detail with reference to the drawings.

[0013] 1a to 1d are schematic diagrams illustrating a process for filling a through-hole in a printed wiring board with a curable resin composition. First, a printed wiring board 1 having a through-hole 2 is prepared (FIG. 1a). The printed wiring board 1 is prepared by providing copper foil (wiring layer) 102 on both sides of an insulating layer 101, forming a through-hole 2 on the surface of the board using a drill or the like, and plating the inner wall 201 of the through-hole 2 and the surface of the wiring layer 102 to form a plating layer 103.

[0014] The insulating layer 101 may be a resin substrate such as a glass epoxy substrate, a polyimide substrate, a bismaleimide-triazine resin substrate, or a fluororesin substrate, or a copper-clad laminate of these resin substrates, a ceramic substrate, or a metal substrate.

[0015] The copper foil 102 is provided on both sides of the insulating layer 101, each having a thickness of 18 μm. The surface of the copper foil 102 is preferably subjected to buffing or the like and then acid washing.

[0016] The plating process involves electroless plating and electrolytic plating for thick plating, forming a plating layer 103 on the surface of the substrate 10. The thickness of the plating layer 103 is 30 μm. Copper plating is preferred as the electroless plating and electrolytic plating. Conventionally known methods can be suitably applied as the electroless plating and electrolytic plating methods.

[0017] The total thickness of the printed wiring board 1, i.e., the thickness including the insulating layer 101, the wiring layer 102, and the plating layer 103, is 1.6 mm, and the through holes 2 are provided perpendicular to the main surface of the printed wiring board 1. The inner walls 201 of each through hole 2 are plated, and the through holes 2 have a generally cylindrical shape with an inner diameter of 0.12 mm. The printed wiring board 1 has a plurality of through holes 2 of the above-mentioned shape provided at equal intervals of 1 mm.

[0018] Next, the through-holes 2 are filled with the curable resin composition 3 by printing from one of the main surfaces S1 of the printed wiring board (FIG. 1b). At this time, the filling amount of the curable resin composition 3 during printing is adjusted so that the curable resin composition is discharged from the through-holes on the main surface S2 side (hereinafter, sometimes referred to as the ejection surface side) opposite the main surface S1 side (hereinafter, sometimes referred to as the printing surface side) of the main surfaces S1 and S2 of the printed wiring board 1, and a bulge 4 is formed. Specifically, the curable resin composition 3 is discharged from the ejection surface side S2 of the through-holes 2 of the printed wiring board 1, but the filling amount of the curable resin composition is adjusted so that the curable resin composition does not come into contact with the curable resin composition discharged from the adjacent through-holes. More specifically, the curable resin composition is discharged to a depth of 0.04±0.01 mm per through-hole. 3 The through-holes are filled with the compound in an amount of 1000g / g.

[0019] Thereafter, the printed wiring board 1 is heated at a predetermined temperature for a predetermined time to cure the filled curable resin composition (FIG. 1c). Although the curing method here is not limited in any way, in the present invention, the printed wiring board 1 filled with the curable resin composition 3 is placed so that the board main surface is at an angle of 90°±10° with respect to the placement surface, and the temperature is raised from room temperature to 130°C in 10 minutes and held at 130°C for 45 minutes, and then the temperature is raised from 130°C to 150°C in 10 minutes and held at 150°C for 60 minutes to cure the filled curable resin composition 3.

[0020] Next, unnecessary portions of the bulge 4 protruding from the printing surface S1 of the through-hole 2 of the printed wiring board 1 and the ejection surface S2 are removed by polishing to make the surface flat (FIG. 1d). Polishing can be suitably performed by using a belt sander, buff polishing, or the like.

[0021] FIG. 2 is a front view of the discharge surface S2 of the printed wiring board 1 in a state in which the curable resin composition 3 filled in each through hole 2 of the printed wiring board 1, in which a plurality of through holes 2 are provided at regular intervals, is cured. FIG. 3 is a cross-sectional view of the X-X' line in FIG. 2. As described above, the surface of the discharge surface S2 of the printed wiring board 1 has the bulges 4 of the curable resin composition 3 discharged from the through holes 2 cured as they are. The shapes of the bulges 4 are different for each through hole 2. That is, it can be said that the main surface of the printed wiring board 1 opposite to the printed side has a cured product covering region 4 in which the cured product of the curable resin composition 3 covers the board main surface S2 so as to cover the periphery of each through hole 2.

[0022] 4 is an enlarged view of any one of the through holes 2 shown in FIG. 2. That is, it is an enlarged view of the ejection surface S2 of the printed wiring board 1 as viewed from the front. L (μm), r L The longest straight line distance between the center of the line segment is r S (μm), 1≦r L / r S ≦1.5 The cured product-coated area that satisfies is 50% or more of the total cured product-coated area. When the through-hole 2 is approximately cylindrical, the through-hole 2 is approximately circular when viewed from the front, but when the cured product-coated area is in the shape of a concentric circle, r L / r S On the other hand, as shown in FIG. 5, when the cured product-covered region 4 has an irregular shape, particularly a shape extending in one direction, r L / r S In the present invention, each of the cured product-covered regions 4 may have any shape, but 1≦r L / r S By making the cured product coating area satisfying ≦1.5 account for 50% or more of the total cured product coating area, it is possible to obtain a printed wiring board having a smooth surface free of dents after surface polishing in a printed wiring board in which through-holes are filled with a cured product of the curable resin composition.

[0023] That is, when the unnecessary part of the bulge 4 protruding from the surface of the through-hole 2 is removed by polishing to flatten it, the more the cured product coating area has a shape similar to the opening shape of the through-hole (i.e., approximately circular), the lower the probability of a dent occurring after polishing, and a smooth surface without any recesses can be obtained. The reason for this is unclear, but when the cured product coating area has an approximately circular shape, the shape in the thickness direction also tends to be a symmetrical convex shape, so when polished, only the bulging parts of the convex shape are polished and smoothed. On the other hand, when the shape of the cured product coating area is different from a circle (for example, an ellipse, etc.), the shape in the thickness direction of the cured product coating area is not a symmetrical convex shape but becomes an irregular shape, and it can be assumed that the thin part of the cured product coating area is peeled off or scraped off as a lump during polishing, causing a dent. In particular, when the shape in the thickness direction of the cured product coating area is not a symmetrical convex shape but is eccentric, the position of the top of the convex shape is shifted from the center of the through-hole, so that a dent is likely to occur on the through-hole. In addition, since it is difficult to polish the thin portions of the cured product-coated region, multiple polishing processes are required, and the portions may be polished excessively, resulting in dents. L / r S The "cured product-coated region satisfying 1 ≦ r ≦ 1.5" refers to the cured product-coated region 4 among the individual cured product-coated regions 4 described above. L / r S The term "total cured product-coated regions" refers to the total number of regions that satisfy the condition ≦1.5, and "total cured product-coated regions" refers to the total number of the individual cured product-coated regions 4 described above. In addition, when the individual cured product-coated regions of adjacent through-holes are connected to each other and are continuous, the relevant regions are not counted.

[0024] From the viewpoint of obtaining a printed wiring board having a smooth surface without dents after surface polishing, the above-mentioned 1≦r L / r S The area covered with the cured product which satisfies the condition ≦1.5 is preferably 60% or more, and more preferably 70% or more of the entire area covered with the cured product.

[0025] In order to obtain the above-described cured product-covered region in a printed wiring board in which the through-holes are filled with the cured product of the curable resin composition, the composition of the curable resin composition, printing conditions (filling conditions), curing conditions, etc. may be appropriately adjusted. The composition of the curable resin composition will be described in detail below.

[0026] [Curable resin] The curable resin composition according to the present invention includes a curable resin, which is a curable component. As the thermosetting resin, any resin that can be cured by heat can be used without any particular limitation, but epoxy resins can be preferably used. As the epoxy resin, any resin having two or more epoxy groups in one molecule can be used without any limitation. For example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, hydrogenated bisphenol A type epoxy resin, brominated bisphenol A type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, biphenyl type epoxy resin, naphthol type epoxy resin, naphthalene type epoxy resin, dicyclopentadiene type epoxy resin, triphenylmethane type epoxy resin, alicyclic epoxy resin, aliphatic chain epoxy resin, phosphorus-containing epoxy resin, anthracene type epoxy resin, norbornene type epoxy resin, adamantane type epoxy resin, fluorene type epoxy resin, aminophenol type epoxy resin, aminocresol type epoxy resin, alkylphenol type epoxy resin, etc. can be mentioned. The above-mentioned epoxy resins can be used alone or in combination of two or more.

[0027] The above-mentioned epoxy resins are classified into solid, semi-solid and liquid epoxy resins before curing. These can be used alone or in combination of two or more. The term "liquid" refers to a liquid state having fluidity at 20°C, and the term "semi-solid" refers to a solid state having no fluidity at 20°C, but a liquid state having fluidity at 40°C.

[0028] Examples of solid epoxy resins include epoxidized products of condensation products of phenols and aromatic aldehydes having a phenolic hydroxyl group (trisphenol type epoxy resins), such as EPPN-502H (trisphenol epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; dicyclopentadiene aralkyl type epoxy resins, such as EPICLON HP-7200H (dicyclopentadiene skeleton-containing multifunctional solid epoxy resin) manufactured by DIC Corporation; EPICLON N660, EPICLON Novolac type epoxy resins such as N690 and EOCN-104S manufactured by Nippon Kayaku Co., Ltd.; phenol novolac type epoxy resins such as DEN431 manufactured by Dow Chemical Japan Co., Ltd.; biphenyl type epoxy resins such as YX-4000 manufactured by Mitsubishi Chemical Corporation; phosphorus-containing epoxy resins such as TX0712 manufactured by Nippon Steel Chemical & Materials Co., Ltd.; tris(2,3-epoxypropyl)isocyanurates such as TEPIC manufactured by Nissan Chemical Co., Ltd.; and bisphenol A type epoxy resins such as jER1001 manufactured by Mitsubishi Chemical Corporation.

[0029] Examples of semi-solid epoxy resins include bisphenol A type epoxy resins such as EPICLON 860, EPICLON 900-IM, EPICLON EXA-4816, and EPICLON EXA-4822 manufactured by DIC Corporation, Epotohto YD-134 manufactured by Nippon Steel Chemical & Material Co., Ltd., jER834 and jER872 manufactured by Mitsubishi Chemical Corporation, and ELA-134 manufactured by Sumitomo Chemical Co., Ltd.; and phenol novolac type epoxy resins such as EPICLON N-740 manufactured by DIC Corporation.

[0030] Liquid epoxy resins include ZX-1059 (a mixture of bisphenol A and bisphenol F epoxy resins) manufactured by Nippon Steel Chemical & Material Co., Ltd., jER828 (bisphenol A epoxy resin), jER807, and jER4004P (bisphenol F epoxy resin) manufactured by Mitsubishi Chemical Corporation, R710 (bisphenol E epoxy resin) manufactured by Air Water Inc., TETRAD-X (aromatic amine epoxy resin) manufactured by Mitsubishi Gas Chemical Co., Ltd., and jER630 (aminophenol epoxy resin) manufactured by Mitsubishi Chemical Corporation. Examples of suitable epoxy resins include ED-509S (tert-butylphenyl glycidyl ether) manufactured by ADEKA Corporation, EP-3300E (hydroxybenzophenone type liquid epoxy resin) manufactured by ADEKA Corporation, ELM-100 (para-aminophenol type liquid epoxy resin) manufactured by Sumitomo Chemical Co., Ltd., jER604 (glycidylamine type epoxy resin) manufactured by Mitsubishi Chemical Corporation, Epotohto YH-434 (glycidylamine type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd., and Sumiepoxy ELM-120 manufactured by Sumitomo Chemical Co., Ltd.

[0031] The amount of the epoxy resin in the total solid content is preferably 5 to 70% by volume, and more preferably 10 to 60% by volume, based on the total solid content of the curable resin composition.

[0032] In addition, in consideration of the film-forming property of the curable resin composition, that is, the coatability such as printability, the epoxy resin used in the present invention is preferably liquid rather than solid. In particular, the viscosity of the epoxy resin is preferably 50 Pa·s or less, more preferably 20 Pa·s or less, and even more preferably 5 Pa·s or less. The viscosity here refers to the viscosity measured at 25±1°C, rotor speed of 5.0 rpm, and 30-second value using a cone-plate viscometer (manufactured by Toki Sangyo Co., Ltd., TV-33H, rotor 3°×R9.7 or rotor 1°34'×R24) in accordance with JIS K8803:2011 "10 Viscosity measurement method using a cone-plate type rotational viscometer".

[0033] [Hardening agent] The curable resin composition of the present invention includes a curing agent for curing the above-mentioned curable resin. The curing agent can be used without any particular limitation as long as it has the effect of promoting the curing reaction of the epoxy resin. For example, amines, imidazoles, polyfunctional phenols, acid anhydrides, isocyanates, and polymers containing these functional groups may be used in combination as necessary. The amines include dicyandiamide, diaminodiphenylmethane, and the like. The imidazoles include alkyl-substituted imidazoles, benzimidazoles, and the like. The imidazole compound may also be an imidazole latent curing agent such as an imidazole adduct. The polyfunctional phenols include hydroquinone, resorcinol, bisphenol A and its halogen compounds, and further, novolacs and resol resins which are condensates of these with aldehydes. The acid anhydrides include phthalic anhydride, hexahydrophthalic anhydride, methylnadic anhydride, and benzophenonetetracarboxylic acid. The isocyanates include tolylene diisocyanate, isophorone diisocyanate, etc., and these isocyanates may be used after being masked with phenols, etc. These curing agents may be used alone or in combination of two or more kinds.

[0034] As the amines, aliphatic polyamines and alicyclic polyamines are preferably used, and examples of the aliphatic polyamines include alkylenediamines having 2 to 6 carbon atoms, such as ethylenediamine and propylenediamine, polyalkylenepolyamines having 2 to 6 carbon atoms, such as diethylenetriamine and triethylenetriamine, and aromatic ring-containing aliphatic polyamines having 8 to 15 carbon atoms, such as xylylenediamine. Commercially available examples of modified aliphatic polyamines include Fujicure FXE-1000, Fujicure FXR-1020, Fujicure FXR-1030, Fujicure FXR-1080, and Fujicure FXR-1090M2 (manufactured by T&K TOKA Corporation), Ancamine 2089K, Sanmaid P-117, Sanmaid X-4150, Ancamine 2422, Surwet R, Sanmaid TX-3000, and Sanmaid A-100 (manufactured by Evonik Japan Co., Ltd.). Examples of alicyclic polyamines include isophorone diamine, 1,3-bis(aminomethyl)cyclohexane, bis(4-aminocyclohexyl)methane, norbornene diamine, 1,2-diaminocyclohexane, and laromine. Commercially available modified alicyclic polyamines include, for example, Ancamine 1618, Ancamine 2074, Ancamine 2596, Ancamine 2199, Sanmaido IM-544, Sanmaido I-544, Ancamine 2075, Ancamine 2280, Ancamine 1934, Ancamine 2228 (manufactured by Evonik Japan Co., Ltd.), Daitoclar F-5197, Daitoclar B-1616 (manufactured by Daito Sangyo Co., Ltd.), Fujicure FXD-821, Fujicure 4233 (manufactured by T&K TOKA Co., Ltd.), jER Cure 113 (manufactured by Mitsubishi Chemical Co., Ltd.), and Laromine C-260 (manufactured by BASF Japan Co., Ltd.). Other examples of polyamine-type curing agents include EH-5015S (manufactured by ADEKA Co., Ltd.).

[0035] The imidazoles include, for example, reaction products of epoxy resins and imidazole, etc. Examples of the imidazoles include 2-methylimidazole, 4-methyl-2-ethylimidazole, 2-phenylimidazole, 4-methyl-2-phenylimidazole, 1-benzyl-2-methylimidazole, 2-ethylimidazole, 2-isopropylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, etc. Examples of commercially available imidazole compounds include imidazoles such as 2E4MZ, C11Z, C17Z, and 2PZ, imidazole AZINE compounds such as 2MZ-A and 2E4MZ-A, imidazole isocyanurates such as 2MZ-OK and 2PZ-OK, and imidazole hydroxymethyl compounds such as 2PHZ and 2P4MHZ (all manufactured by Shikoku Chemical Industry Co., Ltd.). Examples of commercially available imidazole-type latent curing agents include Cureduct P-0505 (manufactured by Shikoku Chemical Industry Co., Ltd.).

[0036] The amount of the curing agent is preferably 1 to 100 parts by mass, more preferably 2 to 50 parts by mass, and particularly preferably 5 to 20 parts by mass, when the total solid content of the curable resin is 100 parts by mass. In particular, when the amount of the curing agent is 5 parts by mass or more, the pre-curing speed of the resin composition is generally not slowed down, and the composition in the deep part of the hole is sufficiently cured, so that the occurrence of cracks can be prevented. In addition, when the amount of the curing agent is 50 parts by mass or less, the storage stability is good, and the pre-curing speed of the resin composition is generally not too fast, so that voids are less likely to remain in the cured product, which is preferable.

[0037] [Inorganic filler] The curable resin composition according to the present invention contains an inorganic filler. By blending an inorganic filler, it is possible to adjust the linear expansion coefficient and to alleviate stress due to cure shrinkage when the curable resin composition is filled into a through hole such as a through hole of a printed wiring board and then cured. As the inorganic filler, a known inorganic filler used in a normal resin composition can be used. Specifically, for example, nonmetallic fillers such as silica, barium sulfate, calcium carbonate, silicon nitride, aluminum nitride, boron nitride, alumina, magnesium oxide, aluminum hydroxide, magnesium hydroxide, titanium oxide, mica, talc, and organic bentonite, and metallic fillers such as copper, gold, silver, palladium, and silicone can be mentioned. These inorganic fillers may be used alone or in combination of two or more kinds.

[0038] Among these inorganic fillers, calcium carbonate, silica, barium sulfate, and aluminum oxide, which are excellent in low moisture absorption and low volume expansion, are preferably used, and silica and calcium carbonate are more preferably used. Silica may be either amorphous or crystalline, or a mixture of these. In particular, amorphous (fused) silica is preferable. Calcium carbonate may be either natural heavy calcium carbonate or synthetic precipitated calcium carbonate.

[0039] Also, a magnetic filler can be used as the inorganic filler. By including a magnetic filler, noise electromagnetic waves in the near electromagnetic field can be suppressed or absorbed, so that an electronic component having excellent characteristics such as noise suppression can be obtained even when a plurality of circuit elements are mounted. Also, it can be suitably used as an insulating material for a high-frequency inductor element that requires a high relative permeability at 1 MHz to 200 MHz. In particular, by including a magnetic filler in the curable resin composition filled in the through hole, the characteristics of an inductor can be imparted to the through hole, which can contribute to making the board lighter, thinner, shorter, and smaller.

[0040] The magnetic filler can be used without any particular limitation, and examples thereof include spinel type ferrites such as Mg-Zn ferrite, Mn-Zn ferrite, Mn-Mg ferrite, Mn ferrite, Cu-Zn ferrite, Mg-Mn-Sr ferrite, Ni-Zn-Cu ferrite, and Ni-Zn ferrite; hexagonal type ferrites such as Ba-Zn ferrite, Ba-Mg ferrite, Ba-Ni ferrite, Ba-Co ferrite, and Ba-Ni-Co ferrite; and garnet type ferrites such as magnetite and Y ferrite. and conductive magnetic materials such as Fe alloys such as pure iron powder, Fe-Si alloy powder, Fe-Si-Al alloy powder, Ni powder, Fe-Ni alloy powder, Fe-Ni-Mo alloy powder, Fe-Ni-Mo-Cu alloy powder, Fe-Co alloy powder, Fe-Ni-Co alloy powder, Fe-Cr alloy powder, Fe-Cr-Si alloy powder, Fe-Ni-Cr alloy powder, or Fe-Cr-Al alloy powder, Ni alloys, High-Si alloys, and amorphous alloys such as Fe-based amorphous and Co-based amorphous.

[0041] In addition, commercially available magnetic fillers can be used as the magnetic filler. Specific examples of commercially available magnetic fillers include "AW2-08PF3FG" manufactured by Epson Atmix Corporation, "KNI-106" and "KNI-109" manufactured by JFE Chemical Corporation, "BSN-125", "BSN-714", and "BSN-828" manufactured by Toda Kogyo Co., Ltd., and "M10S", "M03S", "NZ03S", "E03S", "M001", and "E001" manufactured by Powdertech Co., Ltd. One type of magnetic powder may be used alone, or two or more types may be used in combination.

[0042] The shape of the inorganic filler is not particularly limited, and examples thereof include spherical, needle-like, plate-like, scaly, hollow, irregular, hexagonal, cubic, and flaky shapes. From the viewpoint of a high content of the inorganic filler, the spherical shape is preferred.

[0043] In addition, in consideration of the dispersibility of the inorganic filler, the filling property in the hole, the smoothness when the wiring layer is formed in the filled part, etc., the average particle diameter of the inorganic filler is preferably 0.1 μm to 20 μm, more preferably 0.1 μm to 15 μm, and even more preferably 0.1 μm to 10 μm. The average particle diameter means the volume cumulative 50% particle diameter (D50 volume%) including not only the particle diameter of the primary particles but also the particle diameter of the secondary particles (aggregates), and can be obtained as the median diameter (D50, volume basis) by cumulative distribution from the measured value of the particle size distribution by the laser diffraction / scattering method using a laser diffraction scattering type particle size distribution measuring device (MT3300EX manufactured by Microtrack Bell Co., Ltd.). The average particle diameter of the inorganic filler refers to the value measured as described above for the powder before preparing (pre-stirring, kneading) the resin composition.

[0044] The inorganic filler may be surface-treated. For example, the surface of the magnetic powder may be treated with a coupling agent having a curable reactive group as an organic group. As the coupling agent, a silane-based, titanate-based, aluminate-based, zircoaluminate-based coupling agent may be used. Examples of such silane-based coupling agents include vinyltrimethoxysilane, vinyltriethoxysilane, N-(2-aminomethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-anilinopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, etc., which may be used alone or in combination. It is preferable that these silane coupling agents are immobilized in advance on the surface of the inorganic filler by adsorption or reaction.

[0045] The curable reactive group is preferably a thermosetting reactive group. Examples of the thermosetting reactive group include a hydroxyl group, a carboxyl group, an isocyanate group, an amino group, an imino group, an epoxy group, an oxetanyl group, a mercapto group, a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, an ethoxyethyl group, and an oxazoline group. Among these, at least one of an amino group and an epoxy group is preferable.

[0046] In addition, the surface-treated inorganic filler may be contained in the curable resin composition in a surface-treated state, and the inorganic filler and the surface treatment agent may be separately blended into the curable resin composition to surface-treat the inorganic filler in the curable resin composition, but it is preferable to blend an inorganic filler that has been surface-treated in advance. By blending an inorganic filler that has been surface-treated in advance, it is possible to prevent a decrease in crack resistance, etc. due to the surface treatment agent that was not consumed in the surface treatment, which may remain when blended separately. When performing surface treatment in advance, it is preferable to blend a preliminary dispersion in which the inorganic filler is pre-dispersed in a solvent component or a resin component, and the surface-treated inorganic filler is pre-dispersed in a solvent component or a resin component, and the preliminary dispersion is blended into the composition, or it is more preferable to sufficiently surface-treat the inorganic filler when pre-dispersing it in a solvent component or a resin component, and then blend the preliminary dispersion into the curable resin composition.

[0047] The more inorganic filler is used, the better the magnetic properties of the cured product will be. From the viewpoint of achieving both insulating properties and the ability to fill small holes and narrow gaps, however, the inorganic filler is preferably contained in an amount of 40 to 90 mass %, and more preferably 50 to 90 mass %, based on the total solid content of the curable resin composition.

[0048] [Other ingredients]

[0049] The curable resin composition of the present invention may further contain an oxazine compound having an oxazine ring obtained by reacting a phenolic compound, formalin, and a primary amine, if necessary. By containing the oxazine compound, when electroless plating is performed on the cured product formed after curing the curable resin composition filled in the hole of a printed wiring board, roughening of the cured product by an aqueous potassium permanganate solution or the like can be facilitated, and peel strength with plating can be improved.

[0050] In addition, known colorants such as phthalocyanine blue, phthalocyanine green, iodine green, disazo yellow, crystal violet, titanium oxide, carbon black, and naphthalene black, which are used in ordinary screen printing resist inks, may be added.

[0051] Further, in order to impart storage stability during storage, known thermal polymerization inhibitors such as hydroquinone, hydroquinone monomethyl ether, tert-butylcatechol, pyrogallol, and phenothiazine can be added, and known thickeners and thixotropic agents such as clay, kaolin, and montmorillonite can be added in order to adjust the viscosity, etc. In addition, known additives such as silicone-based, fluorine-based, and polymer-based defoamers, leveling agents, and adhesion-imparting agents such as thiazole-based and triazole-based agents can be added.

[0052] In the curable resin composition of the present invention, it is not always necessary to use a dilution solvent. However, in order to adjust the viscosity of the curable resin composition, a dilution solvent may be added to the extent that no voids are generated.

[0053] Examples of diluting solvents include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, and acetate esters of the above glycol ethers; alcohols such as ethanol, propanol, ethylene glycol, and propylene glycol; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha.

[0054] The viscosity of the curable resin composition of the present invention at 25±1° C. is preferably in the range of 100 to 1000 dPa·s, more preferably 200 to 800 dPa·s, and particularly preferably 200 to 600 dPa·s. By setting the viscosity in such a range, the holes can be easily filled, and the recesses and through holes can be filled well without the generation of voids. The viscosity here refers to the viscosity measured at 25° C., at a rotor rotation speed of 5.0 rpm, and at a value of 30 seconds using a cone-plate type viscometer (manufactured by Toki Sangyo Co., Ltd., TV-33H, rotor 3°×R9.7) in accordance with the viscosity measurement method using a cone-plate type rotational viscometer of JIS K8803:2011 10.

[0055] The multilayer printed wiring board in which the holes and recesses are filled with the curable resin composition is heated, for example, at 80 to 160°C for about 30 to 180 minutes, whereby the curable resin composition is cured to form a cured product. From the viewpoint of easily removing unnecessary parts of the cured product that protrude from the substrate surface after filling the holes by physical polishing, the curing of the curable resin composition may be performed in two stages. That is, the curable resin composition can be pre-cured at a lower temperature and then main curing (finish curing). The pre-curing conditions are preferably heating at 80 to 130°C for about 30 to 180 minutes. Since the hardness of the pre-cured cured product is relatively low, unnecessary parts that protrude from the substrate surface can be easily removed by physical polishing, and a flat surface can be obtained. Then, the product is heated to main curing. The main curing conditions are preferably heating at 140 to 180°C for about 30 to 180 minutes.

[0056] Curing can be carried out in both the preliminary curing and the main curing using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, etc. (a method in which hot air in a dryer is brought into countercurrent contact using a heat source of an air heating method using steam, or a method in which hot air is blown onto the object to be cured from a nozzle). Among these, a hot air circulation drying oven is particularly preferred. In this case, the cured product hardly expands or shrinks due to its low expansion, and the final cured product has good dimensional stability, low moisture absorption, adhesion, electrical insulation, etc. The hardness of the preliminary cured product can be controlled by changing the heating time and heating temperature of the preliminary curing.

[0057] After the curable resin composition is cured as described above, unnecessary parts (bulging parts) of the cured product protruding from the surface of the printed wiring board are removed by a known physical polishing method, and the surface is flattened, and then the wiring layer on the surface is patterned into a predetermined pattern to form a predetermined circuit pattern. If necessary, the surface of the cured product may be roughened with an aqueous potassium permanganate solution or the like, and then a wiring layer may be formed on the cured product by electroless plating or the like. EXAMPLES

[0058] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples. In the following, "parts" and "%" are all based on mass unless otherwise specified.

[0059] <Preparation of Curable Resin Composition> The various components shown in Table 1 below were mixed in the ratios (parts by mass) shown in each table, and uniformly mixed and dispersed using a three-roll mill to prepare the curable resin compositions of Examples 1 to 6 and Comparative Examples 1 to 3.

[0060] In addition, *1 to *16 in Table 1 represent the following components. *1: Bisphenol A type epoxy resin (Mitsubishi Chemical Corporation, jER-828) *2: Metaxylenediamine type epoxy resin (Mitsubishi Gas Chemical Co., Ltd., TETRAD-X) *3: Triglycidyl-p-aminophenol resin (Mitsubishi Chemical Corporation, jER-630) *4: 4-tert-Butylphenyl glycidyl ether (ADEKA Corporation, ED-509S) *5: Imidazole-based curing agent (Shikoku Kasei Co., Ltd., 2MZA-PW) *6: Silica particles (Admatechs Co., Ltd., FE920A-SQ, average particle size 5.6 μm) *7: Silica particles (manufactured by Admatechs Co., Ltd., SC6500-SQ, average particle size 2.1 μm) *8: Silica particles (manufactured by Jiangsu NOVORAY New Materials Co., Ltd., NQ1110H, average particle diameter 6.2 μm) *9: Calcium carbonate particles (Softon 3200, average particle size 3.2 μm, manufactured by Bihoku Funka Kogyo Co., Ltd.) *10: Calcium carbonate particles (Bihoku Funka Kogyo Co., Ltd., Softon 1800, average particle size 1.8 μm) *11: Magnetic filler particles (M10S, Powder Tech Co., Ltd., average particle size 4.0 μm) *12: Titanium oxide particles (manufactured by Ishihara Sangyo Kaisha, Ltd., Typec CR-58, average particle size 0.3 μm) *13: Silane coupling agent (Shin-Etsu Chemical Co., Ltd., KBM-403) *14: Defoamer (KS-66, manufactured by Shin-Etsu Chemical Co., Ltd.) *15: Bentonite (Olben M, manufactured by Shiraishi Kogyo Co., Ltd.) *16: Wetting and dispersing agent (Big Chemie Japan Co., Ltd., DISPERBYK-111)

[0061] <Preparation of printed wiring board> The curable resin composition was degassed using an agitation degassing machine (ARE-310, manufactured by Thinky Corporation) under conditions of MIXING mode at 2000 rpm for 8 minutes and then DEFORM mode at 2200 rpm for 2 minutes. Note that, only in Example 3, the curable resin composition was degassed using an agitation degassing machine (ARE-310, manufactured by Thinky Corporation) under conditions of MIXING mode at 1800 rpm for 2 minutes and then DEFORM mode at 1800 rpm for 1 minute. Next, a glass epoxy board (FR-4 board: a glass epoxy board having through-holes with a conductor layer formed by panel plating, 150 mm × 290 mm × thickness 1.6 mm / through-hole diameter 0.12 mm (after plating) / pitch 1 mm) was washed with acid and then dried at 150 ° C for 15 minutes in a hot air circulation dryer (DF612 manufactured by Yamato Scientific Co., Ltd.). Next, the curable resin compositions of each of the Examples and Comparative Examples were filled into the through-holes by screen printing from one side of the substrate using a semi-automatic printer (SSA-PC660A, manufactured by Ceria Corporation) under the following printing conditions: During filling, the curable resin composition was discharged from the through-hole on the opposite side to the printed side, but the filling amount of the curable resin composition was adjusted so that it did not come into contact with the curable resin composition discharged from the adjacent through-hole, and the injection amount of the curable resin composition per through-hole was 0.04±0.01 mm. 3 It was decided. Next, after filling with the curable resin composition, the substrate was placed on a substrate rack so that the main surface of the substrate was at an angle of 90°±10° to the mounting surface, and then heated from room temperature to 130°C in 10 minutes in a hot air circulating drying furnace and held at 130°C for 45 minutes. Thereafter, the temperature was raised from 130°C to 150°C in 10 minutes and held at 150°C for 60 minutes to cure the curable resin composition, thereby producing an evaluation substrate.

[0062] (Printing conditions) Squeegee: Squeegee thickness 20mm, flat squeegee (hardness 70°) Screen: PET 200 mesh bias screen, aperture diameter 600 μm (dot pattern), emulsion thickness 30 μm Printing pressure: 60kg Squeegee speed: 5mm / sec Squeegee angle: 93° (attack angle 3°) Screen plate clearance: 1.5mm Drop amount (the distance the squeegee is lowered from the position where the distance between the squeegee and the substrate is zero when printing): 7 mm

[0063] <1≦r L / r S Calculation of ratio ≦1.5> The principal surface of the evaluation board prepared as described above, opposite to the printed side, was observed at 200x magnification using a microscope (VHX-6000, manufactured by Keyence Corporation). The longest linear distance r of the cured product-covered region covering the principal surface of the evaluation board so as to cover the periphery of each through-hole was L (μm), r L The longest straight line distance r that crosses the center of the line segment S (μm), r L / r S was calculated. r of all cured coated areas L / r S Calculate and make sure that 1≦r L / r S The percentage of the cured product-covered area that was within the range of ≦1.5 was calculated.

[0064] <Smoothness after polishing> The main surface of the evaluation board opposite to the printed side was physically polished with a buff polisher equipped with a single axis of Hi-Cut Buff 19 (SFBR-♯320, manufactured by Sumitomo 3M Co., Ltd.) set on one side until the resin was completely removed. The polished surface was then observed from the front at 200x magnification using a laser microscope (VK-X100, manufactured by Keyence Co., Ltd.) to check for dents on the surface of the through-holes filled with the cured material, and the distance from the surface of the glass epoxy board to the deepest dent was measured using the shape measurement mode. The smoothness after polishing was evaluated according to the following evaluation criteria. ◎: Dent depth is 5μm or less ○: Dent depth is more than 5 μm and less than 10 μm ×: Dent depth exceeds 10 μm The evaluation results are shown in Table 1 below.

[0065] <Magnetic properties> Magnetic properties were evaluated to confirm properties such as noise suppression. Each of the curable resin compositions of the examples and comparative examples was applied to copper foil using an applicator with a gap of 100 μm, and the curable resin composition was cured by heating at 150° C. for 30 minutes in a hot air circulation drying oven (DF610 manufactured by Yamato Scientific Co., Ltd.). The curable resin composition was then cut into a size of 1 cm×3 cm to be used as an evaluation board. Next, the complex permeability (μ), real part (μ′), imaginary part (μ″), and imaginary number (j) of each evaluation board at a temperature of 25° C. and 10 MHz to 1 GHz GHz were measured using an ENA network analyzer (E5071C manufactured by Keysight Corporation). The relationship between each item is expressed as μ=μ′-jμ″. The average value of 11 points around 100 MHz was used as an index. It is to be noted that if μ′>1.0, it can be said to have magnetism. Yes:μ'>1.0 None:μ'=1.0 The evaluation results are shown in Table 1 below.

[0066] [Table 1]

[0067] As is clear from the evaluation results in Table 1, 1≦r L / r S It can be seen that in the curable resin compositions (Examples 1 to 7) in which the cured product coating area satisfying ≦1.5 was 50% or more of the total cured product coating area, the surfaces of the through-holes filled with the cured product after polishing had small depressions and were smooth. On the other hand, 1≦r L / r S It can be seen that the curable resin compositions (Comparative Examples 1 to 3) in which the cured product coating area satisfying ≦1.5 was more than 50% of the total cured product coating area had large depressions on the surfaces of the through-holes filled with the cured product after polishing.

Claims

1. A curable resin composition comprising a curable resin, a curing agent, and an inorganic filler, When a printed wiring board having a thickness of 1.6 mm and a total thickness of 1.6 mm and a plurality of substantially cylindrical through holes having an inner diameter of 0.12 mm and plated walls are provided at equal intervals of 1 mm in a substrate having a plated surface, the through holes are filled with the curable resin composition from one main surface side of the printed wiring board, and the curable resin composition is cured, When the main surface of the printed wiring board is viewed from the front on a main surface opposite to a filling side, the main surface has a cured product covering region in which a cured product of the curable resin composition covers the main surface of the board so as to cover the periphery of each through hole, The longest straight line distance of each cured product coating area is r L (μm), and L The longest straight line distance between the center of the line segment is r S When (μm), 1≦r L / r S ≦1.5 A curable resin composition, characterized in that the cured product coating area satisfying the above requirement accounts for 50% or more of the total cured product coating area.

2. The curable resin composition according to claim 1, wherein the inorganic filler is contained in an amount of 40 to 90 mass% based on the total solid content of the curable resin composition.

3. The curable resin composition according to claim 1, wherein the inorganic filler has an average particle size of 0.1 to 20 μm.

4. The curable resin composition according to claim 1 , wherein the inorganic filler comprises a magnetic filler.

5. A method for producing a printed wiring board using the curable resin composition according to any one of claims 1 to 4, comprising the steps of: A printed wiring board having a plurality of substantially cylindrical through holes is prepared; filling the through-holes with the curable resin composition by printing from one main surface side of the printed wiring board; The filled curable resin composition is cured. Including, The method is characterized in that, when filling the curable resin composition, the curable resin composition is discharged from a through-hole on a main surface of the printed wiring board opposite to the printed side, and the filling amount of the curable resin composition is adjusted so that the curable resin composition does not come into contact with the curable resin composition discharged from an adjacent through-hole.

6. The method according to claim 5 , further comprising polishing a main surface of the printed wiring board opposite to a printed side after the filled curable resin composition is cured.

Citation Information

Patent Citations

  • Method of manufacturing resin filled substrate

    JP2007235121A

  • Paste composition for through hole filling, and printed wiring board prepared therewith