Nonwoven fabric and wiping sheet including the same
The use of multilobed cross-section fibers in nonwoven fabrics addresses issues of water absorption, retention, and fiber shedding, enhancing wiping performance and reducing fuzzing, resulting in improved wiping sheets.
Patent Information
- Application Number
- JP2024057782
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-15
AI Technical Summary
Nonwoven fabrics used in wiping sheets face challenges with insufficient water absorption and retention, large fiber diameters, and issues with fuzzing and fiber shedding, particularly when using irregular cross-section fibers and splittable composite fibers.
Incorporation of multilobed cross-section fibers with at least three convex portions, where the width of the root portion is smaller than the tip, and a portion of these fibers can split or peel off, enhancing wiping performance and reducing fuzzing and fiber shedding.
The nonwoven fabric exhibits improved dirt collection and wiping properties with enhanced water absorption and retention, while minimizing fiber shedding and fuzzing, making it suitable for various wiping applications.
Smart Images

Figure 2024146925000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a nonwoven fabric, and in particular to a wiping sheet containing the nonwoven fabric. [Background technology]
[0002] Nonwoven fabrics are used in various wiping sheets for wiping dirt from the human body or objects. Various techniques have been proposed to improve the wiping effect of wiping sheets. Among them, fibers with irregular cross sections or ultrafine fibers may be used as fibers constituting wiping sheets. It has been reported that when fibers with irregular cross sections, that is, fibers with a cross section perpendicular to the fiber length direction, are used for wiping sheets, the wiping properties of the wiping sheets can be improved depending on the shape (see Patent Documents 1 and 2). However, irregular cross section fibers tend to have a large fiber diameter, and therefore it is considered that the water absorption and water retention properties may be insufficient.
[0003] As another method for improving the wiping property of a wiping sheet, it has been proposed to use splittable composite fibers (composite fibers with a cross section in which two wedge-shaped resin components are arranged alternately) as fibers constituting the nonwoven fabric used in the wiping sheet. When splittable composite fibers are used for the wiping sheet, it is known that the splittable composite fibers are split by subjecting the fiber web to a high-pressure water flow or other treatment in the process of producing the nonwoven fabric, thereby forming ultrafine fibers composed of each resin component (see, for example, Patent Documents 3 and 4).
[0004] Since the ultrafine fibers obtained by splitting the splittable composite fibers have a non-circular fiber cross section, they are not only highly effective at removing various types of dirt from the surface of the object to be wiped (skin or floor surface), but also have a larger specific surface area than fibers with a circular cross section, which makes the wiping sheet itself bulkier. In addition, the removed dirt is more likely to be collected inside the fibers or inside the wiping sheet, so wiping sheets based on nonwoven fabric containing splittable composite fibers have excellent wiping performance.
[0005] In the manufacturing process of nonwoven fabrics using splittable conjugate fibers, a fiber web is subjected to high-pressure water jet treatment, heat treatment, and mechanical entanglement treatment (needle punching treatment) to split the splittable conjugate fibers into resin components, generating ultrafine fibers. In order to increase the amount of ultrafine fibers contained in the resulting nonwoven fabric, it is preferable that the ratio (splitting rate) of ultrafine fibers generated from the splittable conjugate fibers is high. However, in nonwoven fabrics using splittable conjugate fibers, the splitting rate of the splittable conjugate fibers is usually at most about 60 to 80%, and at least about 40 to 20% of unsplittable conjugate fibers may be present in the nonwoven fabric. These unsplittable splittable conjugate fibers have a round fiber cross section and a large fineness (2.2 dtex or more), so that the wiping performance is not necessarily sufficient.
[0006] In addition, various wiping sheets are required to further suppress fuzzing and fiber shedding during use, and improvements are being made to improve these performances. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 2-234914 [Patent Document 2] Japanese Patent Application Publication No. 2-289220 [Patent Document 3] JP 2006-625 A [Patent Document 4] JP 2015-277 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention aims to provide a nonwoven fabric that has excellent dirt collection performance and higher wiping properties, and further aims to provide a nonwoven fabric that can further suppress fluffing and fiber shedding when used as a wiping sheet. [Means for solving the problem]
[0009] As a result of intensive research, the present inventors have found that when a specific multilobal cross-sectional fiber is used, (i) the fiber shape may be distorted by a high-pressure water flow (part of the convex portion may be split or peeled off), and (ii) even if the fiber cross-sectional shape is not changed by the high-pressure water flow, the fiber cross-section may have a moderate uneven shape. Furthermore, they have found that a nonwoven fabric containing such a fiber has improved wiping properties due to the ultrafine fiber-like parts that may be generated, and that the wiping properties are improved by the moderate uneven shape that the fiber cross-section may have, and that the nonwoven fabric is suitable for various wiping sheet applications, and have completed the present invention.
[0010] This specification includes the following embodiments. 1. A nonwoven fabric used as a base material for a wiping sheet for wiping the surface of an object, The nonwoven fabric contains 20% by mass or more of multilobal cross-section fibers, The multilobal cross-section fiber is a fiber having a fiber cross-section with a multilobal cross-section shape having at least three convex portions, At least one of the protrusions may have a generally curved tip portion, and a width (Wb) of a base portion toward the center of the fiber is smaller than a maximum width (Wt) of the tip portion; At least a portion of the multilobal cross-section fiber may include fibers derived from multilobal cross-section fibers formed by splitting or peeling off at least one of at least three protruding portions constituting the multilobal cross-section fiber, The fibers derived from the multilobal cross section fibers may be in the form of ultrafine fibers formed by splitting or peeling off at least one of the multiple protrusions contained in the multilobal cross section fibers. 2. The nonwoven fabric according to 1 above, wherein the multilobal cross section fiber has 3 or more and 8 or less convex portions in the fiber cross section. 3. The nonwoven fabric according to 1 or 2 above, wherein the maximum width Wt of the protrusions is 3.5 μm or more and 20 μm or less, and the length Lt is 4 μm or more and 25 μm or less. 4. The protrusion has a narrowed portion toward the center of the fiber, and the width (Wb) of the base portion of the protrusion is smaller than the maximum width (Wt) of the protrusion; The width Wb of the base portion of the protrusion is 2 μm or more and 12 μm or less, 4. The nonwoven fabric according to any one of 1 to 3 above, wherein the ratio Lt / Wb of the length Lt of the protrusions to the width Wb of the base portion is 1.0 or more and 3.5 or less, and the ratio Wt / Wb of the maximum width Wt to the width Wb of the base portion is greater than 1 and less than 3.5. 5. The multilobal cross-section fiber is a fiber made of a single resin component, The single resin component is a resin component containing 50% by mass or more of polypropylene resin, The fineness of the multilobal cross-section fiber is 0.5 dtex or more and 10 dtex or less, 5. The nonwoven fabric according to any one of 1 to 4 above, wherein the single resin component contains a hydrophilizing agent in an amount of 0.5% by mass or more and 10% by mass or less. 6. The nonwoven fabric contains, in addition to the multilobal cross-section fibers, hydrophilic fibers, and thermally adhesive fibers; When the combined mass of the multilobal cross-section fibers, the hydrophilic fibers, and the thermal adhesive fibers is taken as 100 mass%, the nonwoven fabric contains 20 mass% or more and 80 mass% or less of fibers derived from the multilobal cross-section fibers, 10 mass% or more and 50 mass% or less of the hydrophilic fibers, and 10 mass% or more and 40 mass% or less of the thermal adhesive fibers, 6. The nonwoven fabric according to any one of 1 to 5 above, wherein at least a part of the intersections of constituent fibers in the nonwoven fabric are thermally bonded by the thermal adhesive fiber. 7. The nonwoven fabric according to claim 6, wherein the hydrophilic fibers are cellulosic fibers. 8. The nonwoven fabric according to 6 or 7 above, wherein the thermal adhesive fiber is a composite fiber composed of a low melting point resin component and a high melting point resin component, and the melting point of the low melting point resin component is 145°C or lower. 9. The nonwoven fabric according to the above item 8, wherein the thermal adhesive fiber is a core-sheath type composite fiber having a low melting point resin component as a sheath component and a high melting point resin component as a core component. 10. The nonwoven fabric according to 8 or 9 above, wherein the low melting point resin component contained in the thermal adhesive fiber is a resin component containing 50 mass% or more of polyethylene resin. 11. The nonwoven fabric according to any one of 1 to 5 above, comprising one or more fiber layers containing the multilobal cross section fibers and at least one type selected from hydrophilic fibers and thermally adhesive fibers. 12. The nonwoven fabric described in 11 above, comprising one or more fiber layers containing the multilobal cross-section fibers and at least one type selected from hydrophilic fibers and thermally adhesive fibers, and further comprising one or more fiber layers in which the content of the multilobal cross-section fibers is less than 20 mass%. 13. A nonwoven fabric according to claim 12, comprising two fiber layers containing the multilobal cross-section fibers and at least one selected from hydrophilic fibers and thermally adhesive fibers, and one fiber layer having a multilobal cross-section fiber content of less than 20% by mass, wherein fiber layers containing the multilobal cross-section fibers and at least one selected from hydrophilic fibers and thermally adhesive fibers are laminated on both surfaces of the fiber layer having a multilobal cross-section fiber content of less than 20% by mass. 14. The nonwoven fabric according to claim 13, wherein the fiber layers containing multilobal cross-section fibers and at least one type selected from hydrophilic fibers and thermally adhesive fibers, laminated on both surfaces of a fiber layer having a multilobal cross-section fiber content of less than 20%, are not thermally bonded to each other. 15. The nonwoven fabric according to any one of the above items 6 to 10, which is a single-layered nonwoven fabric consisting only of the multilobal cross section fibers, the hydrophilic fibers, and the thermal adhesive fibers. 16. A wet wiping sheet using the nonwoven fabric described in any one of 1 to 14 above as a substrate, and impregnated with a liquid in a ratio within the range of 100 parts by mass or more and 1,000 parts by mass or less per 100 parts by mass of the substrate. Effect of the Invention
[0011] The nonwoven fabric of an embodiment of the present invention is a nonwoven fabric containing 20% by mass or more of specific multilobal cross-section fibers, and even if part of the cross-sectional shape of the specific multilobal cross-section fibers collapses, i.e., part of the convex portions in the fiber cross-section of the multilobal cross-section fibers separates or peels off, even if part of the cross-sectional shape of the specific multilobal cross-section fibers does not collapse, i.e., part of the convex portions in the fiber cross-section of the multilobal cross-section fibers do not separate or peel off, the nonwoven fabric has excellent dirt collection performance, and when used as various wiping sheets, a nonwoven fabric can be provided that easily produces a wiping sheet with better wiping properties. In addition, in a more preferred embodiment of the nonwoven fabric of the present invention, in addition to the specific multilobal cross-section fibers, thermally adhesive fibers are contained, and by thermally bonding the fibers with the thermal adhesive component, the degree of freedom of the fibers can be appropriately controlled, and pilling and fiber fall-off can be further suppressed when the nonwoven fabric is used as a wiping sheet. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 illustrates a schematic of a multilobal cross-section fiber according to the present invention. [Diagram 2] FIG. 2 shows scanning electron microscope (SEM) photographs of the surface (100x and 50x) and cross section (400x) of the nonwoven fabrics of Examples 1, 4 and 7. [Diagram 3] FIG. 3 shows SEM photographs of the surface (100x and 50x) and cross section (400x) of the nonwoven fabrics of Comparative Examples 3, 4 and 1. [Figure 4] FIG. 4 shows a scanning electron microscope (SEM) photograph of the cross section of the nonwoven fabric of Example 1, magnified 200 times, showing the cross-sectional shape of the multilobal cross-sectional fibers. [Diagram 5] FIG. 5 shows a scanning electron microscope (SEM) photograph of the cross section of the nonwoven fabric of Example 4, magnified 200 times, showing the cross-sectional shape of the multilobal cross-sectional fibers. [Figure 6] FIG. 6 shows a scanning electron microscope (SEM) photograph of the cross section of the nonwoven fabric of Comparative Example 4, magnified 200 times, showing the cross-sectional shape of the multilobal cross-sectional fibers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The nonwoven fabric of the present invention can be used for various applications where nonwoven fabrics are used, but can be suitably used as a substrate for wiping sheets for wiping the surface of an object. Wiping sheets are divided into personal wiping sheets, such as antiperspirant sheets and sheets for wiping bottoms, which are mainly used for wiping human skin (however, in the present invention, the personal wiping sheets include sheets used for wiping organisms other than humans, such as mammals), and object wiping sheets, which are used for wiping dirt and foreign objects that have fallen or adhered to the surface of an object, such as floors, window panes, furniture, and the surface of the body of a passenger car. In both the personal wiping sheets and object wiping sheets, they are used to wipe off foreign objects and dirt that have fallen or adhered to the surface to be wiped, so the performance of entangling foreign objects and dirt from the target surface (wiping performance) is important. Therefore, the configuration of the multi-lobate cross-section fiber that contributes to the wiping performance in the nonwoven fabric of the present invention and its action and effect will be described.
[0014] (multilobal cross-section fiber) The multilobal cross-section fiber contained in the nonwoven fabric of the present invention is a fiber having a multilobal cross-section shape having at least three convex portions in its fiber cross-section. The multilobal cross-section fiber will be described with reference to FIG. 1. The multilobal cross-section fiber 1 has a multilobal cross-section shape having three or more convex portions 2. At least one of the convex portions present in the fiber cross-section of the multilobal cross-section fiber may have a substantially curved tip portion, and the width Wb of the base portion toward the center of the fiber is smaller than the maximum width Wt of the tip portion. The number of convex portions 2 is preferably 3 to 8, more preferably 3 to 6, and particularly preferably 3 or 4. It is believed that the convex portions present in the fiber cross-section of the multilobal cross-section fiber improve the wiping performance of the nonwoven fabric containing the multilobal cross-section fiber, which removes and traps dirt from the surface of the target object by the convex portions.
[0015] In the multilobal cross-section fiber contained in the nonwoven fabric of the present invention, the protrusions 2 present in the cross section of the fiber are easily deformed because the width Wb of the base part of the protrusion is smaller than the maximum width Wt of the tip part. As will be described later, when manufacturing a nonwoven fabric, a force is applied to the fiber in the manufacturing process (for example, a carding process or a hydroentanglement process for hydroentangled nonwoven fabrics), and the applied force may cause at least a part of the protrusions to be split or peeled off from the multilobal cross-section fiber. As a result, at least a part of the multilobal cross-section fiber contains fibers derived from multilobal cross-section fiber that may be formed by splitting or peeling off at least one of the protrusions constituting the multilobal cross-section fiber. The fibers derived from the multilobal cross-section fiber are ultrafine fibers with a smaller fiber cross-sectional area than the multilobal cross-section fiber, since a part of the multilobal cross-section fiber (i.e., the protrusions 2) is split or peeled off from the main body of the multilobal cross-section fiber. Therefore, the nonwoven fabric of the present invention can contain fibers derived from multilobal cross-section fibers formed by splitting or peeling off at least one of the multiple convex portions contained in the multilobal cross-section fibers in at least a portion of the multilobal cross-section fibers contained in the nonwoven fabric, and at least a portion of the fibers derived from the multilobal cross-section fibers can be in the form of ultrafine fibers.
[0016] In the nonwoven fabric of the present invention, at least a portion of the multilobal cross-section fibers contained in the nonwoven fabric may include fibers derived from multilobal cross-section fibers formed by splitting or peeling off at least one of the convex portions constituting the multilobal cross-section fibers, and at least a portion of the fibers derived from the multilobal cross-section fibers may be ultrafine fibers having a smaller cross-sectional area than the multilobal cross-section fibers. In the multilobal cross-section fibers whose cross-sections are not collapsed, the at least three convex portions have a high effect of entangling and removing dirt from the surface to be wiped, and the concave portions formed between the convex portions are likely to have an effect of retaining the entangled dirt. In addition, when the nonwoven fabric of the present invention is used as a wiping sheet (so-called wet wiping sheet) impregnated with a chemical solution, the concave portions have a high effect of absorbing and retaining the chemical solution, so that it is thought that a wiping sheet with excellent sustained release of the chemical solution is easily obtained. In addition, the multilobal cross-section fibers with collapsed fiber cross sections generate fibers derived from the multilobal cross-section fibers by convex parts that can be split and peeled off from the multilobal cross-section fibers, and at least a part of the fibers derived from the multilobal cross-section fibers can be in the form of ultrafine fibers. The fibers derived from the multilobal cross-section fibers have the original convex shape, i.e., a flat non-circular fiber cross-sectional shape, regardless of whether they are completely separated and peeled off from the original multilobal cross-section fibers, and therefore can enhance the effect of entangling and removing dirt from the surface to be wiped. As a result, the nonwoven fabric of the present invention contains fibers that have the effect of enhancing wiping performance, regardless of whether the cross-sectional shape of the multilobal cross-section fibers contained in the nonwoven fabric collapses or not, and therefore is more likely to exhibit higher wiping performance than nonwoven fabrics that must contain conventional splittable composite fibers.
[0017] The maximum width Wt of the tip of the convex portion 2 included in the fiber cross section of the multilobal cross-section fiber 1 included in the nonwoven fabric of the present invention is preferably 3.5 μm to 20 μm, more preferably 4.5 μm to 16 μm, and particularly preferably 5 μm to 14 μm. When the maximum width Wt of the tip of the convex portion 2 is within the above range, the effect of retaining the dirt caught in the concave portion 3 formed between the convex portions is easily obtained, and when the nonwoven fabric of the present invention is used as a wiping sheet impregnated with a chemical solution (a so-called wet wiping sheet), the effect of absorbing and retaining the chemical solution in the concave portion is high, so that a wiping sheet with excellent sustained release of the chemical solution is easily obtained.
[0018] The width Wb of the base of the protrusion 2 in the cross section of the multilobal cross-section fiber 1 contained in the nonwoven fabric of the present invention is preferably 2 μm or more and 12 μm or less, more preferably 3.0 μm or more and 10 μm or less, and particularly preferably 3.5 μm or more and 8 μm or less. When the width Wb of the base of the protrusion 2 is within the above range, the protrusion 2 is easily peeled off, fibrillated, or separated from the vicinity of its base due to various forces applied to the fiber in the manufacturing process of the nonwoven fabric, which makes it easier to generate fibers derived from the multilobal cross-section fiber, especially ultrafine fibers derived from the multilobal cross-section fiber, and the wiping performance of the obtained nonwoven fabric is easily improved. The protrusions in the cross section of the multilobal cross-section fiber 1 contained in the nonwoven fabric of the present invention have a portion that is narrowed toward the center of the fiber, and the width Wb of the base of the protrusion is smaller than the maximum width Wt of the protrusion. When the width Wb of the base portion of the protrusion is smaller than the maximum width Wt of the protrusion, the protrusion becomes more likely to peel off, fibrillate, or separate from near its base, making it easier to generate ultrafine fiber-like fibers derived from multi-lobal cross-section fibers.
[0019] In the protrusions 2 included in the fiber cross section of the multilobal cross-section fiber 1 included in the nonwoven fabric of the present invention, the maximum width (Wt) at the tip of the protrusion is indicated by Wt in FIG. 1, specifically, the maximum length when a line is drawn from the center of the fiber to the tip of the protrusion 2 and a perpendicular line is drawn from the line to the outer shape of the protrusion, and the width (Wb) at the base of the protrusion is indicated by Wb in FIG. 1, specifically, the length connecting both ends of the base of each of the adjacent protrusions. The ratio (Wt / Wb) of the maximum width Wt at the tip of the protrusion to the width Wb of the base is preferably greater than 1 and less than or equal to 3.5. When the ratio (Wt / Wb) of the maximum width Wt at the tip to the width Wb of the base satisfies the above range, not only is it easy for the protrusions 2 to peel off, fibrillate, or separate from the vicinity of their base, but also the multilobal cross-section fiber is easy to manufacture. The ratio (Wt / Wb) of the maximum width Wt at the tip of the protrusion to the width Wb at the base is more preferably 1.2 to 3, particularly preferably 1.4 to 2.5, and most preferably 1.4 to 2. The maximum width Wt at the tip of the protrusion and the width Wb at the base can be determined by enlarging the cross section of the produced nonwoven fabric with a scanning electron microscope or the like and averaging the values of any 15 multilobal cross-section fibers.
[0020] The length Lt of the convex portion 2 included in the fiber cross section of the multilobal cross-section fiber 1 included in the nonwoven fabric of the present invention (the distance from the center point of the root part of the convex portion to the tip) is preferably 4 μm or more and 25 μm or less, more preferably 6.5 μm or more and 20 μm or less, and particularly preferably 8.0 μm or more and 16 μm or less. If the length Lt of the convex portion is less than 4 μm, the convex portion 2 is difficult to deform from the root. If the length Lt of the convex portion exceeds 25 μm, in addition to the area of the convex portion becoming too large, the fineness of the multilobal cross-section fiber itself becomes too large, which may cause a decrease in the wiping performance of the nonwoven fabric containing it. If the length Lt of the convex portion is 4 μm or more and 25 μm or less, the convex portion 2 is more easily deformed from the root and has better wiping performance, which is preferable. The length Lt of the convex portion can be obtained by enlarging the cross section of the manufactured nonwoven fabric with a scanning electron microscope or the like and averaging the values of 15 arbitrary multilobal cross-section fibers.
[0021] In the multilobal cross-section fiber contained in the nonwoven fabric of the present invention, the ratio (Lt / Wb) of the length Lt of the protrusion 2 to the width Wb of the base portion is preferably 1 or more and 3.5 or less. When the ratio (Lt / Wb) of the length Lt of the protrusion to the width Wb of the base portion satisfies the above range, not only is it easy for the protrusion to peel off, fibrillate, or separate from the vicinity of its base, but also the production of the fiber becomes easy. The ratio (Lt / Wb) of the length Lt of the protrusion to the width Wb of the base portion is more preferably 1.2 or more and 3 or less, particularly preferably 1.4 or more and 2.7 or less, and most preferably 1.5 or more and 2.5 or less.
[0022] The multilobal cross-section fibers contained in the nonwoven fabric of the present invention may be fibers made of multiple resin components, for example, composite fibers made of two types of resin components, but are preferably single fibers made of a single resin component. If the multilobal cross-section fibers are single fibers made of a single resin component, the melt viscosity of the thermoplastic resin used as the raw material during fiber production can be easily adjusted, making it easier to produce multilobal cross-section fibers that meet a predetermined fiber cross-sectional shape.
[0023] The thermoplastic resin contained in the resin component, preferably the single resin component, is not particularly limited, and may be selected from any thermoplastic resin commonly used in fiber production.Specifically, one or more resins may be selected from the group consisting of polyolefin resins such as polyethylene, polypropylene, polybutene-1, polymethylpentene, ethylene-propylene copolymer, ethylene-vinyl alcohol copolymer, ethylene-vinyl acetate copolymer, ethylene-methacrylic acid copolymer, ethylene-acrylic acid copolymer, ethylene-methyl methacrylate copolymer, and ethylene-methyl acrylate copolymer; aromatic polyester resins such as polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; aliphatic polyester resins such as polylactic acid, polyethylene succinate, and polybutylene succinate; polyamide resins such as nylon 6 and nylon 66; polycarbonate resins; polyoxymethylene (polyacetal) resins; polyketone resins; polystyrene resins; vinylon resins; and acrylic resins. The raw materials of these thermoplastic resins are not particularly limited, and may be thermoplastic resins derived from petroleum, thermoplastic resins derived from biomass in which at least a part of the raw materials is derived from plants, or recycled (regenerated) thermoplastic resins obtained by crushing, melting, and re-pelletizing a thermoplastic resin product that has been used once. The single resin component constituting the multilobal cross-section fibers contained in the nonwoven fabric of the present invention is preferably a resin component containing 50% by mass or more of polypropylene resin, more preferably a resin component containing 75% by mass or more of polypropylene resin, and particularly preferably a resin component containing 80% by mass or more of polypropylene resin.
[0024] The polypropylene resin is not particularly limited as long as it is a polypropylene resin that can be melt-spun, but preferably, the melt mass flow rate of the polypropylene resin according to JIS K 7210 (measurement temperature 230°C, load 2.16 kgf (21.18 N) or less, also simply referred to as "MFR230") is in the range of 5 g / 10 min to 50 g / 10 min, more preferably in the range of 10 g / 10 min to 45 g / 10 min, and particularly preferably in the range of 20 g / 10 min to 35 g / 10 min. When MFR230 is within the above range, not only is yarn breakage unlikely to occur during spinning, but the shear stress of the molten polypropylene resin is appropriately large, so that the fiber cross-sectional shape immediately after melt spinning is easily maintained, and a multilobal cross-sectional fiber having a predetermined cross-sectional shape is easily obtained.
[0025] The fineness of the multilobal cross-section fiber contained in the nonwoven fabric of the present invention is not particularly limited, but is preferably 0.5 dtex to 10 dtex, more preferably 0.8 dtex to 5.6 dtex, and particularly preferably 1.0 dtex to 3.5 dtex. If the fineness of the multilobal cross-section fiber exceeds 10 dtex, when the nonwoven fabric containing the multilobal cross-section fiber is used as a wiping sheet, the surface of the target object may be damaged or the wiping sheet may have a poor usability. If the fineness of the multilobal cross-section fiber is less than 0.5 dtex, the carding property of the multilobal cross-section fiber is reduced, making it difficult to produce a nonwoven fabric containing the multilobal cross-section fiber. If the fineness of the multilobal cross-section fiber is 0.5 dtex to 10 dtex, a softer texture is easily produced, a more comfortable feel is obtained, and productivity is further improved.
[0026] The fiber length of the multilobal cross-section fibers contained in the nonwoven fabric of the present invention is not particularly limited, but is preferably 20 mm to 80 mm, more preferably 25 mm to 70 mm, and particularly preferably 30 mm to 65 mm. When the fiber length of the multilobal cross-section fibers contained in the nonwoven fabric of the present invention satisfies the above range, the nonwoven fabric of the present invention has excellent productivity and is less susceptible to fiber shedding.
[0027] The multilobal cross-section fiber contained in the nonwoven fabric of the present invention is preferably a single fiber made of a single resin component, and more preferably, the single resin component contains a hydrophilizing agent in order to increase the hydrophilicity of the multilobal cross-section fiber. In order to increase the hydrophilicity of the multilobal cross-section fiber, the method of adding a hydrophilizing agent to the single resin component constituting the multilobal cross-section fiber is not particularly limited. Specifically, the hydrophilizing agent can be added to the single resin component by a method of mixing inorganic particles with the single resin component, a method of mixing a hydrophilizing agent, etc. with the single resin component, or a method of mixing a modified polyolefin having a polar group with the single resin component. The hydrophilizing agent that can be added to the single resin component is not particularly limited, and examples of the inorganic particles include oxides, carbonates, or sulfates of at least one element selected from the group consisting of silicon, aluminum, calcium, magnesium, sodium, and potassium.
[0028] The hydrophilizing agent that can be added to the single resin component is not particularly limited as long as it is a compound having a hydrophilic group such as a hydroxyl group, a carbonyl group, a carboxyl group (also referred to as a carboxy group), or a sulfone group. Examples of the hydrophilizing agent include fatty acid glycerides (polyglycerin fatty acid esters having a glycerin polymerization degree of 1 to 10, such as monoglycerin fatty acid esters, diglycerin fatty acid esters, triglycerin fatty acid esters, and tetraglycerin fatty acid esters), alkylene oxide adducts of polyglycerin having a glycerin polymerization degree of 1 to 10, and POE alkyl (C8 to C10) containing an alkyl group having 8 to 18 carbon atoms. 18 ) phosphate, alkyl (C8-C 18 ) phosphate, alkyl (C8-C 18) phosphoric acid ester salts, alkoxylated alkylphenols, polyoxyalkylene fatty acid esters, and fatty acid diethanolamides. Examples of modified polyolefins having polar groups that can be added to the single resin component include resins obtained by graft-polymerizing maleic anhydride with polypropylene resins or polyethylene resins. The inorganic particles, hydrophilizing agents, modified polyolefins having polar groups, etc. can be mixed in a range that does not significantly impair spinnability or fiber properties, and are preferably added in a proportion of 0.1% by mass or more and 15% by mass or less, more preferably 0.5% by mass or more and 10% by mass or less, and particularly preferably 0.8% by mass or more and 8% by mass or less, when the mass of the entire single resin component (i.e., the mass of the entire fiber) is taken as 100% by mass.
[0029] A method for increasing the hydrophilicity of the multilobal cross-section fibers contained in the nonwoven fabric of the present invention is to attach a fiber treatment agent mainly composed of a surfactant to the surface of the multilobal cross-section fibers. The surfactant contained in the fiber treatment agent attached to the surface of the multilobal cross-section fibers is not particularly limited, and may be any ordinary surfactant used for the purpose of improving the hydrophilicity of synthetic fibers, such as phosphate ester surfactants such as alkyl phosphates such as octyl alkyl phosphate, decyl alkyl phosphate, lauryl alkyl phosphate, tridecyl alkyl phosphate, myristyl alkyl phosphate, cetyl alkyl phosphate, and stearyl alkyl phosphate, and metal salts thereof such as sodium or potassium.
[0030] In order to enhance the hydrophilicity of the multilobal cross-section fibers contained in the nonwoven fabric of the present invention, the multilobal cross-section fibers may be subjected to a hydrophilic treatment to improve the hydrophilicity. Examples of the hydrophilic treatment include a fluorine gas treatment, a plasma discharge treatment, and a corona discharge treatment. When a corona discharge treatment is performed, the discharge amount per one treatment is not particularly limited, but is preferably 50 W·min / m 2 More than 100W·min / m is preferable, and the total discharge rate is 100W·min / m 2 More than 5000W min / m 2The more preferable total discharge rate is 250W·min / m 2 More than 5000W min / m 2 The plasma treatment is not particularly limited, but is preferably a normal pressure plasma treatment, and may be performed under the conditions of a voltage of 50 kV to 250 kV and a frequency of 500 pps to 3000 pps. The normal pressure plasma treatment can be performed at a low voltage, which is convenient because it causes less deterioration of the fiber. The fluorine gas treatment is not particularly limited, but may be performed using a mixed gas containing fluorine gas and oxygen gas, or a mixed gas containing fluorine gas and sulfurous acid gas.
[0031] The nonwoven fabric of the present invention is a nonwoven fabric containing 20% by mass or more of the multilobal cross-sectional fiber. When the mass of the entire nonwoven fabric is taken as 100% by mass, the nonwoven fabric contains 20% by mass or more of the multilobal cross-sectional fiber having a predetermined fiber cross-sectional shape, and the nonwoven fabric can exhibit high wiping performance due to the wiping performance of the multilobal cross-sectional fiber itself (the ability to remove dirt and foreign matter from the surface of the target object by the convex portion) and the wiping performance of the multilobal cross-sectional fiber-derived fiber that can be generated from the multilobal cross-sectional fiber (particularly the wiping performance of the ultrafine fiber-like fiber that can be generated from the multilobal cross-sectional fiber). In the nonwoven fabric of the present invention, the upper limit of the proportion of the multilobal cross-sectional fiber is not particularly limited, and the nonwoven fabric may be made of only the multilobal cross-sectional fiber, but if the nonwoven fabric contains other fibers, the amount of fuzz generation and the amount of fallen fibers required for the wiping sheet can be reduced. Therefore, in the nonwoven fabric of the present invention, a nonwoven fabric containing multilobal cross section fibers, hydrophilic fibers and thermally adhesive fibers, which is a preferred embodiment when the nonwoven fabric contains fibers other than multilobal cross section fibers, will be described in detail.
[0032] One embodiment of the nonwoven fabric of the present invention, that is, the nonwoven fabric used as a substrate of a wiping sheet for wiping the surface of an object, is a nonwoven fabric containing 20% by mass or more of multilobal cross-section fibers, The multilobal cross-section fiber is a fiber having a fiber cross-section with a multilobal cross-section shape having at least three convex portions, At least one of the protrusions may have a generally curved tip portion, and a width (Wb) of a base portion toward the center of the fiber is smaller than a maximum width (Wt) of the tip portion; At least a portion of the multilobal cross-section fiber may include fibers derived from multilobal cross-section fibers formed by splitting or peeling off at least one of at least three protruding portions constituting the multilobal cross-section fiber, The fibers derived from the multilobal cross section fibers may be in the form of ultrafine fibers formed by splitting or peeling off at least one of a plurality of protrusions contained in the multilobal cross section fibers, The nonwoven fabric includes, in addition to the multilobal cross-section fibers, hydrophilic fibers, and thermally bondable fibers; When the combined mass of the multilobal cross-section fibers, the hydrophilic fibers, and the thermal adhesive fibers is taken as 100 mass%, the nonwoven fabric contains 20 mass% or more and 80 mass% or less of fibers derived from the multilobal cross-section fibers, 10 mass% or more and 50 mass% or less of the hydrophilic fibers, and 10 mass% or more and 40 mass% or less of the thermal adhesive fibers, At least some of the intersections of the constituent fibers in the nonwoven fabric are thermally bonded by the thermal adhesive fibers.
[0033] The present invention also provides a wet wiping sheet for personal use, which uses the nonwoven fabric as a substrate and is impregnated with a liquid in a ratio within the range of 100 parts by mass or more and 1,000 parts by mass or less per 100 parts by mass of the substrate.
[0034] One form of nonwoven fabric used as a substrate for the wiping sheet of the present invention is a nonwoven fabric containing hydrophilic fibers and thermally adhesive fibers in addition to multilobal cross-section fibers that satisfy a predetermined fiber cross-sectional shape, and the nonwoven fabric contains 20% by mass or more and 80% by mass or less of fibers derived from the multilobal cross-section fibers, 10% by mass or more and 50% by mass or less of the hydrophilic fibers, and 10% by mass or more and 40% by mass or less of the thermally adhesive fibers, when the combined mass of the multilobal cross-section fibers, the hydrophilic fibers, and the thermally adhesive fibers is taken as 100% by mass, and at least a portion of the intersections of the constituent fibers within the nonwoven fabric are thermally bonded by the thermally adhesive fibers. By making a nonwoven fabric containing a multilobal cross-section fiber contain a predetermined amount of hydrophilic fiber and thermal adhesive fiber, and by thermally bonding at least a part of the intersections of the constituent fibers constituting the nonwoven fabric with the thermal adhesive fiber, it is possible to improve the chemical liquid impregnation of the nonwoven fabric while maintaining the high wiping performance of the nonwoven fabric containing the multilobal cross-section fiber, and to reduce the amount of fiber shedding, and the nonwoven fabric is particularly suitable as a substrate for various wet wiping sheets that are used by impregnating the nonwoven fabric with a chemical liquid. Since the multilobal cross-section fiber contained in this nonwoven fabric has been explained, the hydrophilic fiber and thermal adhesive fiber, as well as the manufacturing method of the nonwoven fabric, will be further explained.
[0035] (hydrophilic fiber) The hydrophilic fiber plays a role of retaining a medicinal solution (e.g., a liquid cosmetic) impregnated in the nonwoven fabric, and also of supplying the retained liquid to the target object. In the present invention, the hydrophilic fiber is a fiber having an official moisture regain of 5% or more. The official moisture regain is shown in JIS L0105 (2006). When the official moisture regain is unknown, the value calculated from the following formula shall be used as the official moisture regain. Official moisture content (%) = [(W-W') / W'] x 100 Here, W is the mass (g) of the fiber in an environment with a temperature of 20° C. and a humidity of 65% RH, and W' is the mass (g) of the fiber when completely dry. The mass of the fiber in an environment with a temperature of 20° C. and a humidity of 65% RH means the mass of the fiber when it is left in an environment with a temperature of 20° C. and a humidity of 65% RH and reaches a certain mass, and the mass of the fiber when completely dry means the mass of the fiber when it is left in a dryer set at 105° C. and reaches a certain mass.
[0036] Specific examples of hydrophilic fibers include natural fibers such as pulp, cotton (also referred to simply as cotton fiber), hemp, silk, and wool, regenerated fibers such as viscose rayon, cupra, and solvent-spun cellulose fibers, and synthetic fibers having hydrophilic properties or synthetic fibers having hydrophobic properties (synthetic fibers with an official moisture regain of less than 5%) that have been subjected to a hydrophilization treatment. Examples of hydrophilization treatments include corona discharge treatment, sulfonation treatment, graft polymerization treatment, kneading a hydrophilizing agent into fibers, and applying a durable oil agent. The hydrophilic fibers are preferably cellulosic fibers. Cellulosic fibers include, for example, the above-mentioned natural fibers and regenerated fibers, and more specifically, 1) Pulp, such as mechanical pulp, recycled pulp and chemical pulp 2) Cotton, hemp and other natural plant fibers, 3) Regenerated fibers such as viscose rayon, cupra, and solvent-spun cellulose fibers (e.g., lentined lyocell® and Tencel®).
[0037] The pulp may be produced by conventional methods using softwood or hardwood. Generally, the pulp fibers have a fineness of 1.0 dtex to 4.0 dtex and a fiber length of 0.8 mm to 4.5 mm, although pulp fibers having a fineness and / or fiber length outside these ranges may be used.
[0038] When using regenerated fibers, the fineness is preferably about 0.1 dtex to 6 dtex, more preferably 0.3 dtex to 4.5 dtex, and particularly preferably 0.5 dtex to 3.5 dtex. Regenerated fibers with fineness within this range are suitable for ensuring flexibility. If the fineness of the regenerated fibers is too small, the carding property during the production of the fiber web may deteriorate, and the productivity of the nonwoven fabric may decrease. If the fineness of the regenerated fibers is too large, the nonwoven fabric may become coarse and the touch may be deteriorated.
[0039] The hydrophilic fiber is more preferably a regenerated fiber, and in particular, viscose rayon, because viscose rayon has a proven track record of use in the field of personal wet wipes, and is relatively inexpensive and easy to obtain. It should be noted that hydrophilic fibers do not include the multilobal cross section fibers described above.
[0040] (Thermo-adhesive fiber) The thermally adhesive fiber refers to a fiber that is at least partially melted by heat treatment. The heat treatment temperature can be appropriately selected depending on the components of the thermally adhesive fiber. At least some of the intersections between the constituent fibers that make up the nonwoven fabric of the present invention are thermally bonded (fixed) by such thermally adhesive fibers. The fact that the nonwoven fabric has a large number of thermally bonded fiber intersections (fixed points) contributes to improving the handling properties (mechanical strength, elasticity, etc., and ultimately the spreadability and elongation resistance in a wet state) of the finally obtained nonwoven fabric.
[0041] The thermal adhesive fiber is typically a synthetic fiber, and is preferably a composite fiber containing a thermoplastic resin component having a relatively high melting point (for example, above 140°C) (hereinafter, "high melting point component") and a thermoplastic resin component having a lower melting point (for example, below 140°C) (hereinafter, "low melting point component"), with the low melting point component occupying at least a part of the fiber surface. The melting point is the melting point of the resin after being made into a fiber, and can be obtained from a DSC curve measured in accordance with JIS K7121 (1987). By heat treating such a composite fiber at a temperature lower than the melting point of the high melting point component and higher than the melting point of the low melting point component, the low melting point component can be melted while leaving the high melting point component, and can be fused to other fibers, thereby firmly bonding the fibers together.
[0042] The high melting point component has a sufficient melting point difference with the low melting point component, preferably a melting point difference of 5°C or more, more preferably a melting point difference of 10°C or more, and is preferably one that does not deform due to heat at a temperature at which the low melting point component is melted. The high melting point component may be a polyolefin resin or a polyester resin, and the low melting point component may be a polyolefin resin having a lower melting point. Specific combinations of high melting point component / low melting point component include polypropylene / polyethylene, polypropylene / ethylene-propylene copolymer, polyethylene terephthalate / polyethylene, polyethylene terephthalate / ethylene-propylene copolymer, etc. Polyethylene includes high density polyethylene, low density polyethylene, linear low density polyethylene, etc.
[0043] More specifically, the thermal adhesive fiber may be a core-sheath type composite fiber. The core-sheath type composite fiber is a composite fiber composed of two different components in the core and sheath, and the arrangement of the core and sheath is not particularly limited. In other words, in the fiber cross section, it may be a single core in which the core component is present at one location, or a multi-core in which the core component is present at two or more locations. In addition, the positional relationship between the core component and the sheath component in the fiber cross section may be a concentric type in which the core component and the sheath component are concentrically arranged, an eccentric type in which the core component is biasedly arranged, or a parallel type (also called side-by-side) in which the core component and the sheath component are arranged side by side. In the nonwoven fabric for cosmetic-impregnated skin application sheet of the present invention, it is necessary to thermally bond the fibers uniformly and to a certain extent strongly throughout the nonwoven fabric with a smaller content of thermal adhesive fiber, so it is preferable to use a core-sheath type composite fiber having a concentric fiber cross section in which the low-melting point component is uniformly distributed on the fiber surface.
[0044] The core-sheath type composite fiber may be composed of, for example, a core containing a first polyolefin resin or polyester resin (high melting point component) and a sheath containing a second polyolefin resin or low melting point polyester resin (low melting point component) having a melting point lower than that of the first polyolefin resin or polyester resin (high melting point component). Specifically, the high melting point component may be polypropylene, polymethylpentene, polyethylene terephthalate, polytrimethylene terephthalate, polylactic acid, etc., preferably polypropylene, and the low melting point component may be high density polyethylene, low density polyethylene, linear low density polyethylene, ethylene-propylene copolymer, polybutene-1, polybutylene succinate, etc., preferably high density polyethylene.
[0045] The fineness of the sheath-core composite fiber is preferably thicker from the viewpoint of obtaining a high transparency. It is considered that a thicker fineness reduces the number of fibers and reduces diffuse reflection of light. However, if the fineness is too thick, the number of fiber intersections (fixing points) that are thermally bonded decreases, and the effect of improving handleability may be reduced. In addition, if the fineness of the sheath-core composite fiber is too thick, the touch of the nonwoven fabric may become hard, or the irritation (e.g., a prickly touch) may become strong when the nonwoven fabric is in contact with the skin, making it unsuitable as a base fabric for a wiping sheet for personal use. The fineness of the sheath-core composite fiber is preferably 0.5 dtex or more and 6 dtex or less, more preferably 0.8 dtex or more and 4.5 dtex or less, and particularly preferably 1 dtex or more and 3.5 dtex or less.
[0046] The thermal adhesive fiber may also be a fiber derived from a splittable conjugate fiber. A splittable conjugate fiber is a conjugate fiber composed of two or more components, and is a fiber that can form a plurality of smaller fibers from one fiber by splitting. The term "fiber derived from splittable conjugate fiber" refers to a single fiber formed by splitting a splittable conjugate fiber, which is composed of only one section before splitting, a fiber composed of two or more sections, and a fiber in which one splittable conjugate fiber is partially split but is not split at all in other parts. Alternatively, in the case where one splittable conjugate fiber is not split at all, as long as fibers formed by splitting a splittable conjugate fiber are included in the fibers derived from splittable conjugate fibers, the fibers include those in which the splittable conjugate fiber is not split at all.
[0047] Specifically, splittable composite fibers have a fiber cross-sectional structure in which at least one of the constituent components is divided into two or more components in the fiber cross-section, at least a portion of the constituent component is exposed on the fiber surface, and the exposed portion is formed continuously in the length direction of the fiber.
[0048] For example, the splittable composite fiber may be composed of a combination of a first polyolefin resin or polyester resin (high melting point component) and a second polyolefin resin or a low melting point polyester resin (low melting point component) having a melting point lower than that of the first polyolefin resin or polyester resin (high melting point component). Specifically, the high melting point component may be polypropylene, polymethylpentene, polyethylene terephthalate, polytrimethylene terephthalate, polylactic acid, etc., preferably polyethylene terephthalate, and the low melting point component may be high density polyethylene low density polyethylene, linear low density polyethylene, ethylene-propylene copolymer, polybutene-1, polybutylene succinate, etc., preferably high density polyethylene.
[0049] The fineness of the splittable conjugate fiber is not particularly limited as long as it gives ultrafine fibers having a fineness of 0.6 dtex or less, preferably 0.5 dtex or less, when split into each component (i.e., when each section becomes a single fiber). In the present invention, ultrafine fibers made of a low melting point component are included as fibers derived from the splittable conjugate fiber, and these heat-bond at least some of the intersections between the fibers. When the fineness of the ultrafine fibers made of a low melting point component is 0.6 dtex or less, the heat-bonding points are small, so that the nonwoven fabric is unlikely to become excessively hard, and the texture of the nonwoven fabric is unlikely to be impaired.
[0050] In order to generate such ultrafine fibers, the fineness of the splittable composite fiber is preferably 1 dtex or more and 6 dtex or less, more preferably 1.3 dtex or more and 4 dtex or less, and particularly preferably 1.5 dtex or more and 3 dtex or less. The number of divisions into each component in the splittable composite fiber (i.e., the number of sections in the composite fiber) is preferably 4 to 32, more preferably 4 to 20, and particularly preferably 6 to 16. If the number of divisions is small, it is necessary to reduce the fineness before division in order to form ultrafine fibers with a fineness of 0.6 dtex or less. The lower limit of the fineness of the ultrafine fiber is not particularly limited, but is preferably 0.05 dtex or more.
[0051] The shape of the sections is not particularly limited. For example, the splittable conjugate fiber may be one in which wedge-shaped sections are arranged in a chrysanthemum shape. Alternatively, the splittable conjugate fiber may be one in which the sections are arranged in layers in the fiber cross section. In addition, the splittable conjugate fiber may be a so-called solid splittable conjugate fiber that does not have a continuous cavity in the length direction when the fiber cross section is observed, or may be a so-called hollow splittable conjugate fiber that has one or more continuous cavities in the length direction.
[0052] The volume ratio of the low melting point component and the high melting point component that constitute the above-mentioned core-sheath type composite fiber or splittable type composite fiber is not particularly limited, but is preferably, for example, 2:8 to 8:2 (volume of low melting point component:volume of high melting point component), more preferably 3:7 to 7:3 (volume of low melting point component:volume of high melting point component), and particularly preferably 35:65 to 65:35 (volume of low melting point component:volume of high melting point component). It should be noted that the thermally adhesive fibers do not include the multilobal cross section fibers described above.
[0053] (Non-woven fabric composition) In the nonwoven fabric of the present invention, when the nonwoven fabric is a nonwoven fabric containing hydrophilic fibers and thermal adhesive fibers in addition to multilobal cross-sectional fibers that satisfy a predetermined fiber cross-sectional shape, it is preferable that the nonwoven fabric contains 20% by mass or more and 80% by mass or less of fibers derived from the multilobal cross-sectional fibers, 10% by mass or more and 50% by mass or less of the hydrophilic fibers, and 10% by mass or more and 40% by mass or less of the thermal adhesive fibers, when the combined mass of the multilobal cross-sectional fibers, hydrophilic fibers, and thermal adhesive fibers contained in the nonwoven fabric is taken as 100% by mass. In the nonwoven fabric of the present invention, when the nonwoven fabric is a nonwoven fabric containing at least three types of fibers, multilobal cross-sectional fibers, hydrophilic fibers, and thermal adhesive fibers, by satisfying the above-mentioned ranges, the nonwoven fabric obtained not only has excellent wiping performance for entangling dirt and foreign matter from the target surface when used as a base fabric for various wiping sheets, but also has excellent impregnation of chemicals, and tends to have less fiber shedding during use. When the nonwoven fabric of the present invention contains three types of fibers, namely, multilobal cross-section fibers, hydrophilic fibers, and thermally adhesive fibers, the ratios are more preferably 25% to 70% by mass of fibers derived from multilobal cross-section fibers, 15% to 45% by mass of hydrophilic fibers, and 10% to 30% by mass of thermally adhesive fibers, and even more preferably 40% to 60% by mass of fibers derived from multilobal cross-section fibers, 20% to 40% by mass of hydrophilic fibers, and 15% to 25% by mass of thermally adhesive fibers. In addition to the multilobal cross-section fibers, hydrophilic fibers, and thermally adhesive fibers, the nonwoven fabric of the present invention can also contain other fibers, such as a single fiber with a round cross section made only of a high-melting thermoplastic resin to increase the rigidity (stiffness) of the nonwoven fabric, but this can complicate the production process, and is therefore preferable to be a nonwoven fabric made of three types of fibers, namely, multilobal cross-section fibers (including fibers derived from multilobal cross-section fibers), hydrophilic fibers, and thermally adhesive fibers.
[0054] The nonwoven fabric of the present invention may be a nonwoven fabric comprising the multilobal cross section fibers and one or more fiber layers containing at least one kind selected from the hydrophilic fibers and the thermally adhesive fibers. When the nonwoven fabric of the present invention contains the multilobal cross-section fibers and one fiber layer containing at least one type selected from the hydrophilic fibers and the thermally adhesive fibers, it may be a single-layer nonwoven fabric, and when it contains two or more of the above-mentioned fiber layers, it may be a nonwoven fabric containing two or more fiber layers. When the nonwoven fabric of the present invention is a nonwoven fabric containing the multilobal cross-section fibers and two or more fiber layers containing at least one type selected from the hydrophilic fibers and the thermally adhesive fibers, each of the fiber layers may be exactly the same in terms of the type of fiber used and the ratio of each fiber used, or the type of fiber used and the ratio of each fiber used in each fiber layer may be different.
[0055] The nonwoven fabric of the present invention may be a nonwoven fabric that contains the multilobal cross-section fibers and one or more fiber layers containing at least one fiber selected from hydrophilic fibers and thermally adhesive fibers, and further contains one or more fiber layers having a content of the multilobal cross-section fibers of less than 20% by mass. The fiber layer having a content of the multilobal cross-section fibers of less than 20% by mass may be a fiber layer containing at least one fiber selected from hydrophilic fibers and thermally adhesive fibers.
[0056] The nonwoven fabric of the present invention may be a single-layered nonwoven fabric, or a laminated nonwoven fabric (laminated nonwoven fabric) in which multiple fiber layers are laminated. When the nonwoven fabric of the present invention is a laminated nonwoven fabric, for example, a three-layered nonwoven fabric in which a fiber layer containing a hydrophilic fiber such as pulp, cotton, rayon, etc. and a fiber layer containing a multilobal cross-section fiber are laminated on both surfaces of the fiber layer, may be used as the fiber layer having a multilobal cross-section fiber content of less than 20 mass %.
[0057] The nonwoven fabric of the present invention includes a fiber layer including multilobal cross-section fibers. The fiber layer including multilobal cross-section fibers may include other fibers, and may include at least one selected from hydrophilic fibers and thermally adhesive fibers, or may include both. The nonwoven fabric of the present invention may include multiple fiber layers containing multilobal cross-section fibers, preferably having a multilobal cross-section fiber content of 20% by mass or more, more preferably having a multilobal cross-section fiber content of 30% or more, and may include other fiber layers having a multilobal cross-section fiber content of less than 20% by mass.
[0058] When the nonwoven fabric of the present invention is a single-layer nonwoven fabric comprising a fiber layer containing the multilobal cross-section fiber and at least one selected from hydrophilic fibers and thermally adhesive fibers, the nonwoven fabric may contain, for example, 20% by mass or more and 100% by mass or less of fibers derived from the multilobal cross-section fiber, 0% by mass or more and 80% by mass or less of the hydrophilic fiber, and 0% by mass or more and 80% by mass or less of the thermally adhesive fiber, assuming that the total mass of the multilobal cross-section fiber, hydrophilic fiber, and thermally adhesive fiber is 100% by mass. It is preferable that the fiber composition contains at most 25% by mass and at most 70% by mass of fibers derived from multilobal cross section fibers, at least 15% by mass and at most 45% by mass of hydrophilic fibers, and at least 10% by mass and at most 30% by mass of thermally adhesive fibers, and it is even more preferable that the fiber composition contains at least 40% by mass and at most 60% by mass of fibers derived from multilobal cross section fibers, at least 20% by mass and at most 40% by mass of hydrophilic fibers, and at most 15% by mass and at most 25% by mass of thermally adhesive fibers.
[0059] When the nonwoven fabric of the present invention is a single-layer nonwoven fabric comprising a fiber layer that contains the multilobal cross-section fiber and may contain at least one fiber selected from hydrophilic fibers and thermally adhesive fibers, the fiber layer that contains the multilobal cross-section fiber and contains at least one fiber selected from hydrophilic fibers and thermally adhesive fibers has a basis weight of, for example, 30 g / m 2 More than 200g / m 2 It is preferable that the thickness is less than 30 g / m 2 More than 100g / m 2 The weight per unit area is preferably 35 g / m or less. 2 It is also preferable that the weight is 40 g / m or more. 2 It is more preferable that the basis weight is 150 g / m or more. 2 It is also preferable that the weight is less than 100 g / m 2 It is more preferable that the basis weight is 30 g / m or less. The upper and lower limits of the basis weight can be selected depending on the application and usage of the nonwoven fabric. 2 More than 200g / m 2When the nonwoven fabrics listed below are used as the base fabric for various wiping sheets, wiping sheets with excellent usability are more likely to be obtained. The preferred basis weight of the nonwoven fabric is 35 g / m 2 More than 80g / m 2 The weight of the nonwoven fabric is preferably 35 g / m or less. 2 More than 70g / m 2 The following is the result.
[0060] When the nonwoven fabric of the present invention is a single-layered nonwoven fabric comprising a fiber layer that contains the multilobal cross-section fiber and may contain at least one fiber selected from hydrophilic fibers and thermally adhesive fibers, the thickness of the fiber layer that contains the multilobal cross-section fiber and contains at least one fiber selected from hydrophilic fibers and thermally adhesive fibers is not particularly limited, and varies depending on the ratio of the constituent fibers, the basis weight, the manufacturing conditions, etc. 2 The thickness when a load of 3 gf (2.94 cN) is applied per unit area is, for example, preferably 0.30 mm or more and 3.00 mm or less, more preferably 0.50 mm or more and 2.75 mm or less, and particularly preferably 0.60 mm or more and 2.50 mm or less. If the thickness of the nonwoven fabric is too small, the nonwoven fabrics tend to adhere to each other when folded in a wet state, and the usability and ease of use of the wet wiping sheet may be reduced. If the thickness of the nonwoven fabric is within the above range, the nonwoven fabrics are less likely to adhere to each other even when folded in a wet state, and the wet wiping sheet is more excellent in usability and ease of use.
[0061] When the nonwoven fabric of the present invention is a laminated nonwoven fabric containing the multilobal cross-section fibers, preferably containing 20% by mass or more of multilobal cross-section fibers, and containing at least one fiber selected from hydrophilic fibers and thermally adhesive fibers, or when the nonwoven fabric of the present invention is a laminated nonwoven fabric having a two-layer structure in which a fiber layer containing the multilobal cross-section fibers, preferably containing 20% by mass or more of multilobal cross-section fibers, and containing at least one fiber selected from hydrophilic fibers and thermally adhesive fibers, and a fiber layer having a multilobal cross-section fiber content of less than 20% by mass, the fiber layer containing the multilobal cross-section fibers can contain, for example, 20% by mass or more and 100% by mass of fibers derived from the multilobal cross-section fibers, 0% by mass or more and 80% by mass or less of the hydrophilic fibers, and 0% by mass or more and 80% by mass or less of the thermally adhesive fibers, when the total mass of the multilobal cross-section fibers, hydrophilic fibers, and thermally adhesive fibers is taken as 100% by mass. When the fiber layer containing multilobal cross-section fibers is a fiber layer containing multilobal cross-section fibers, hydrophilic fibers, and thermally adhesive fibers, it is preferable that the fiber layer contains 20% by mass or more and 80% by mass or less of fibers derived from the multilobal cross-section fibers, 10% by mass or more and 50% by mass or less of the hydrophilic fibers, and 10% by mass or more and 40% by mass or less of the thermally adhesive fibers.
[0062] When the nonwoven fabric of the present invention is a laminated nonwoven fabric containing the multilobal cross-section fibers, preferably containing 20% by mass or more of multilobal cross-section fibers, and containing at least one fiber selected from hydrophilic fibers and thermally adhesive fibers, or when the nonwoven fabric of the present invention is a laminated nonwoven fabric having a two-layer structure in which a fiber layer containing the multilobal cross-section fibers, preferably containing 20% by mass or more of multilobal cross-section fibers, and containing at least one fiber selected from hydrophilic fibers and thermally adhesive fibers, and a fiber layer in which the content of multilobal cross-section fibers is less than 20% by mass, the type of fiber other than the multilobal cross-section fibers to be used and the content of the fiber other than the multilobal cross-section fibers may be determined depending on the intended use of the nonwoven fabric.
[0063] If the nonwoven fabric of the present invention is mainly used for wiping the surface of glass products, wiping the surface of the body of various vehicles (for example, passenger cars used in general households), or wiping human skin such as makeup remover sheets, it is required that it is less irritating to the surface to be wiped and less likely to damage the surface to be wiped. When the nonwoven fabric of the present invention is used as a base fabric of a wiping sheet used for such purposes, the fiber layer containing the multilobal cross-section fiber is a fiber layer containing multilobal cross-section fiber and thermal adhesive fiber, and when the total mass of the multilobal cross-section fiber, hydrophilic fiber, and thermal adhesive fiber is 100 mass%, the fiber layer may contain, for example, 20 mass% to 80 mass% of the fiber derived from the multilobal cross-section fiber, 0 mass% to 60 mass% of the hydrophilic fiber, and 20 mass% to 80 mass% of the thermal adhesive fiber. At this time, it is preferable that at least a part of the thermal adhesive fiber is a split type composite fiber, and it is more preferable that the thermal adhesive fiber is a split type composite fiber. In addition, in the fiber layer containing this multi-lobal cross-section fiber, the fibers contained in the fiber layer may or may not be thermally bonded to each other, but if irritation to the target surface is to be suppressed, it is preferable that the fibers contained in the fiber layer are not thermally bonded.
[0064] When the nonwoven fabric of the present invention is used as a base fabric for wiping sheets that are required to be sufficiently impregnated with a liquid medicine and be able to wipe a wide area with a single sheet without drying up, such as sheets for wiping household floors, antiperspirant sheets, and sheets for wiping babies and elderly care, the fiber layer containing the multilobal cross section fiber is a fiber layer containing multilobal cross section fibers and hydrophilic fibers, and when the total mass of the multilobal cross section fibers, hydrophilic fibers, and thermal adhesive fibers in the fiber layer is taken as 100 mass%, the fiber layer may contain, for example, 20 mass% or more and 80 mass% or less of the fibers derived from the multilobal cross section fibers, 20 mass% or more and 80 mass% or less of the hydrophilic fibers, and 0 mass% or more and 60 mass% or less of the thermal adhesive fibers.
[0065] When the nonwoven fabric of the present invention is used as a base fabric for wiping sheets that vigorously rub the target surface, such as sheets used to wipe off burnt-on food around kitchen gas stoves or dirt stuck inside microwave ovens, or sheets (industrial wipers) used in factories to wipe off machines and tools soiled with grease, or for wiping sheets where strength is required, the fiber layer containing the multilobal cross-section fibers is a fiber layer containing multilobal cross-section fibers and thermally adhesive fibers, and when the total mass of the multilobal cross-section fibers, hydrophilic fibers, and thermally adhesive fibers is taken as 100 mass%, the fiber layer can contain, for example, 20 mass% or more and 80 mass% or less of fibers derived from the multilobal cross-section fibers, 0 mass% or more and 60 mass% or less of the hydrophilic fibers, and 20 mass% or more and 80 mass% or less of the thermally adhesive fibers. At this time, the thermal adhesive fiber is preferably a composite fiber (core-sheath type composite fiber) whose cross section is composed of a core component and a sheath component, and more preferably the thermal adhesive fiber is a core-sheath type composite fiber. In addition, the fiber layer containing this multilobal cross-section fiber may or may not be thermally bonded to each other, but since the base fabric is required to have strength that can withstand wiping work, it is preferable that the fibers contained in the fiber layer are at least partially thermally bonded to each other by the thermal adhesive fiber.
[0066] When the nonwoven fabric of the present invention is a laminated nonwoven fabric, it is preferable that the laminated nonwoven fabric has a three-layer structure in which a fiber layer containing multilobal cross-section fibers is laminated on both surfaces of a fiber layer containing less than 20% by mass of multilobal cross-section fibers. In the laminated nonwoven fabric, the fiber layers that do not constitute both surfaces of the laminated nonwoven fabric, in other words, the inside of the nonwoven fabric that does not contact the target surface in the wiping sheet, are made into fiber layers that are more likely to be impregnated with liquid, so that the inside of the nonwoven fabric absorbs more chemical liquid, and both surfaces of the nonwoven fabric can be made into fiber layers with wiping performance suited to the application of the wiping sheet. When the nonwoven fabric of the present invention is a laminated nonwoven fabric with a three-layer structure in which a fiber layer containing multilobal cross-section fibers is laminated on both surfaces of a fiber layer containing less than 20% by mass of multilobal cross-section fibers, it is preferable that the fiber layer containing less than 20% by mass of multilobal cross-section fibers is a fiber layer containing a hydrophilic fiber layer from the viewpoint of absorbing more chemical liquid. The fiber layer containing the hydrophilic fiber may be a fiber layer containing 50% by mass or more and 100% by mass or less of hydrophilic fiber, preferably 75% by mass or more and 100% by mass or less of hydrophilic fiber, more preferably 80% by mass or more and 100% by mass or less of hydrophilic fiber. The fiber layer containing the hydrophilic fiber contains hydrophilic fiber, and as long as the content of multilobal cross section fiber is less than 20% by mass, other fibers contained therein are not particularly limited, and various fibers can be used according to the application and purpose. For example, if the nonwoven fabric is to have strength, it can contain thermal adhesive fiber, and if a bulkier nonwoven fabric is required, it can contain composite fiber that can exhibit three-dimensional shrinkage (one example is eccentric core-sheath type composite fiber) or synthetic fiber made of a single thermoplastic resin.
[0067] When the nonwoven fabric of the present invention is a three-layer laminated nonwoven fabric in which fiber layers (first fiber layer and third fiber layer) containing multilobal cross-section fibers are laminated on both surfaces of a fiber layer (middle fiber layer or second fiber layer) containing hydrophilic fibers and having a multilobal cross-section fiber content of 20 mass% or less, the ratio of the basis weight of the layer containing hydrophilic fibers (middle fiber layer or second fiber layer) to the basis weight of the fiber layers (first fiber layer and third fiber layer) containing multilobal cross-section fibers (first fiber layer / second fiber layer / third fiber layer) may be, for example, 0.1-20 / 1 / 0.1-20, 0.3-12 / 1 / 0.3-12, 0.5-7 / 1 / 0.5-7, or 0.5-5.0 / 1 / 0.5-5.0. When the ratio of the basis weights is 0.1-20 / 1 / 0.1-20, the basis weights of the fiber layer containing hydrophilic fibers (intermediate fiber layer) and the fiber layers containing multilobal cross-section fibers (first fiber layer and third fiber layer) are appropriately balanced. For example, when the nonwoven fabric of the present invention is used as a base fabric for a wet wiping sheet for humans or a wet wiping sheet for objects, which are used by impregnating various chemical solutions, the fiber layer containing hydrophilic fibers (intermediate fiber layer) constituting the nonwoven fabric absorbs a sufficient amount of chemical solution, and the multilobal cross-section fibers located on both surfaces of the fiber layer containing hydrophilic fibers (intermediate fiber layer) absorb a sufficient amount of chemical solution. When the fiber layer containing cross-sectional fibers has an appropriate basis weight, the amount of chemical solution released from the fiber layer containing hydrophilic fibers (intermediate fiber layer) to the nonwoven fabric surface is appropriate; in other words, the chemical solution is excellent in sustained release from the fiber layer containing hydrophilic fibers (intermediate fiber layer) to the nonwoven fabric surface. Therefore, when the target surface is wiped using various wet wiping sheets using the nonwoven fabric as a base fabric, the chemical solution gradually seeps out onto the nonwoven fabric surface, which has the advantageous effect of making it possible to wipe a wider area with a single wiping sheet.
[0068] When the nonwoven fabric of the present invention is a three-layer laminated nonwoven fabric in which two fiber layers containing multilobal cross-section fibers (first fiber layer and third fiber layer) are laminated on both surfaces of a fiber layer (intermediate fiber layer or second fiber layer) containing hydrophilic fibers and having a multilobal cross-section fiber content of 20 mass% or less, the ratio of the thickness of the layer containing hydrophilic fibers (intermediate fiber layer or second fiber layer) to the thickness of the fiber layer containing multilobal cross-section fibers (first fiber layer and third fiber layer) (first fiber layer / second fiber layer / third fiber layer) may be, for example, 0.1-20 / 1 / 0.1-20, 0.3-12 / 1 / 0.3-12, 0.5-7 / 1 / 0.5-7, or 0.5-5.0 / 1 / 0.5-5.0. When the thickness ratio is 0.1-20 / 1 / 0.1-20, the balance of the thickness of the fiber layer containing hydrophilic fibers (intermediate fiber layer) and the fiber layer containing multilobal cross section fibers (first fiber layer and third fiber layer) is appropriate. For example, when the nonwoven fabric of the present invention is used as a base fabric for a wet wiping sheet for humans or a wet wiping sheet for objects, which is impregnated with various chemical solutions, the distance from the fiber layer containing hydrophilic fibers (intermediate fiber layer) to the surface of the nonwoven fabric is appropriate, so that the amount of chemical solution released from the fiber layer containing hydrophilic fibers (intermediate fiber layer) to the surface of the nonwoven fabric is appropriate. When the target surface is wiped, the chemical solution gradually seeps out onto the surface of the nonwoven fabric, which advantageously enables a wider area to be wiped with one wiping sheet.
[0069] As long as the nonwoven fabric of the present invention can be obtained, the basis weight of the nonwoven fabric is not particularly limited, but is preferably 30 g / m 2 More than 200g / m 2 When a nonwoven fabric having a basis weight in this range is used as a base fabric for various wiping sheets, it is easier to obtain a wiping sheet that is excellent in feel when used. A more preferable basis weight of the nonwoven fabric is 35 g / m 2 More than 80g / m 2 The weight of the nonwoven fabric is preferably 35 g / m or less. 2 More than 70g / m 2 The following is the result.
[0070] As long as the nonwoven fabric of the present invention can be obtained, the thickness of the nonwoven fabric is not particularly limited, and varies depending on the ratio of the constituent fibers, the basis weight, the manufacturing conditions, etc. 2 The thickness when a load of 3 gf (2.94 cN) is applied per unit area is, for example, preferably 0.30 mm or more and 3.00 mm or less, more preferably 0.50 mm or more and 2.75 mm or less, and particularly preferably 0.60 mm or more and 2.50 mm or less. If the thickness of the nonwoven fabric is too small, the nonwoven fabrics tend to adhere to each other when folded in a wet state, and the usability and ease of use of the wet wiping sheet may be reduced. If the thickness of the nonwoven fabric is within the above range, the nonwoven fabrics are less likely to adhere to each other even when folded in a wet state, and the wet wiping sheet is more excellent in usability and ease of use.
[0071] (Nonwoven fabric manufacturing method) The nonwoven fabric of the present invention is obtained by preparing a fiber web containing multilobal cross-section fibers and entangling the fibers constituting the fiber web. The nonwoven fabric may be mixed with other fibers depending on the application of the nonwoven fabric, and a preferred embodiment of the nonwoven fabric is a nonwoven fabric containing multilobal cross-section fibers, hydrophilic fibers and thermally adhesive fibers. The nonwoven fabric containing multilobal cross-section fibers, hydrophilic fibers and thermally adhesive fibers is produced by preparing a fiber web containing multilobal cross-section fibers, hydrophilic fibers and thermally adhesive fibers, subjecting the fiber web to a fiber entanglement treatment, and then thermally bonding the fibers with thermally adhesive fibers (preferably a low-melting point component constituting the fiber surface of a core-sheath type composite fiber). The fiber web is produced by mixing the constituent fibers. The form of the fiber web may be any form selected from parallel webs, cross webs, card webs such as semi-random webs and random webs, air-laid webs, wet-laid paper webs, and spunbond webs, but is preferably a card web such as a parallel web, cross web, semi-random web and random web.
[0072] When producing a carded web, the fiber length of the constituent fibers is preferably 20 mm to 80 mm, more preferably 25 mm to 70 mm, and particularly preferably 30 mm to 65 mm. When producing a carded web, if all of the constituent fibers satisfy the above fiber length range, neps are unlikely to occur in the process of producing the carded web, and the nonwoven fabric can be stably produced.
[0073] In the production of the nonwoven fabric of the present invention, the entanglement treatment applied to the fiber web is not particularly limited and can be performed by a known entanglement treatment, such as a hydroentanglement treatment (spunlace treatment) or a needle punching treatment, but hydroentanglement treatment is preferred. According to the hydroentanglement treatment, the fibers are densely entangled with each other to obtain a nonwoven fabric with a uniform and flat surface, and by applying a high-pressure water stream to the multilobal cross-section fibers contained in the fiber web, a part of the convex parts present in the fiber cross section of the multilobal cross-section fibers is peeled off and separated from the multilobal cross-section fibers, thereby generating ultrafine fibers derived from the multilobal cross-section fibers.
[0074] The hydroentanglement treatment is carried out by placing the fiber web or laminated fiber webs on a support and spraying a columnar water stream onto the support. The support is a 0.2 mm2 opening so that the surface of the nonwoven fabric is flat and has no irregularities. 2 It is preferable that the support does not have an opening exceeding 100 mesh and that no protrusions or patterns are formed. For example, the support is preferably a plain weave support having a mesh size of 80 mesh or more and 100 mesh or less.
[0075] The hydroentanglement treatment may be carried out by spraying water at a pressure of 1 MPa to 15 MPa from a nozzle having orifices with a hole diameter of 0.05 mm or more and 0.5 mm or less arranged at intervals of 0.3 mm to 1.5 mm onto the front and back surfaces of the fiber web 1 to 5 times each. The water pressure is preferably 1 MPa to 10 MPa, more preferably 1 MPa to 7 MPa.
[0076] The fiber web after the entanglement treatment is subjected to a thermal bonding treatment as necessary. The thermal bonding treatment is preferably carried out at a temperature at which only the thermally adhesive fiber (preferably, when the thermally adhesive fiber contains two or more components, the lower melting point component) melts. When the entanglement treatment is a hydroentanglement treatment, the thermal bonding treatment may also serve as a drying treatment for removing moisture from the fiber web. Alternatively, the thermal bonding treatment and the drying treatment may be carried out separately.
[0077] In the thermal bonding process, if fiber components other than the low melting point component melt, the number of bonding points increases or large bonding points are formed, and the flexibility of the nonwoven fabric is impaired, so the temperature is selected so that only the low melting point component melts. For example, when the thermally adhesive fiber is made of a combination of polyethylene terephthalate / polyethylene (polyethylene is the low melting point component), the thermal bonding process is preferably performed at a temperature of 130°C or higher and 150°C or lower. Also, when the thermally adhesive fiber is made of a combination of polypropylene / polyethylene (polyethylene is the low melting point component), the thermal bonding process is preferably performed at a temperature of 130°C or higher and 145°C or lower. The degree of thermal bonding by the low melting point component can also be changed by adjusting the heat treatment temperature. The degree of thermal bonding affects the strength, flexibility, and texture of the nonwoven fabric.
[0078] After the fiber entanglement treatment and before the thermal bonding treatment, the nonwoven fabric may be subjected to a width-spreading treatment using a width-spreading roll, if necessary. By performing the width-spreading treatment, the number of fibers oriented in the CD direction can be increased, and the stress at 10% elongation of the nonwoven fabric can be improved.
[0079] The nonwoven fabric of the present invention may be completed by thermal bonding treatment. The nonwoven fabric of the present invention is impregnated with a liquid to form a wet sheet. The liquid to be impregnated and the amount of impregnation are appropriately selected depending on the application. For example, when the wet sheet is provided as a wet wiping sheet for personal use or a wet wiping sheet for objects, water or an aqueous solution containing a cleaning component may be impregnated in an amount of 100 parts by mass or more and 1000 parts by mass or less per 100 parts by mass of the nonwoven fabric. More specifically, the wet wiping sheet for personal use is provided as, for example, a hand wipe, a diaper wipe, a makeup remover sheet, a face wash sheet, an antiperspirant sheet, and a nail remover. Wet wiping sheets for objects include, for example, various types of household wet wiping sheets, more specifically, wet wiping sheets for floors, which are divided into those for flooring and those for tatami mats, wet wiping sheets for glass products, wet wiping sheets for cleaning general household appliances, wet wiping sheets intended for wiping sanitary ware such as washbasins and toilet bowls, wiping sheets for cooking utensils primarily intended for wiping off oil splashes and burnt-on food, wet wiping sheets for vehicles intended for wiping the bodies of various vehicles including passenger cars, as well as industrial wipers for removing oil stains such as grease adhering to machines. EXAMPLES
[0080] The present invention will be specifically and in detail explained below with reference to examples and comparative examples. However, these examples are merely one embodiment of the present invention, and the present invention is not limited to these examples in any way. In the description of the examples, unless otherwise specified, parts by weight and percentages by weight are based on the parts not taking into account the solvent.
[0081] [Example 1] A polypropylene resin (manufactured by Japan Polypropylene Co., Ltd., SA03 (trade name), melting point: 160°C, MFR230: 30g / 10min) was prepared. This was melt-extruded at a spinning temperature of 270°C using a spinning nozzle having a four-leaf nozzle hole shape, and taken up at a take-up speed of 1000m / min to produce a spun filament (undrawn) with a fineness of 4dtex. The spun filament was wet-drawn 2.7 times in warm water at 90°C, and a fiber treatment agent (a fiber treatment agent mainly composed of C12 alkyl phosphate ester potassium salt) was attached so that the active ingredient of the fiber treatment agent was attached at 0.3 mass% relative to the mass of the fiber. The continuous fiber was then cut to a fiber length of 51mm to obtain fiber 1-1 with a fineness of 1.7dtex (fiber diameter when the area of the fiber cross section is converted into a round cross section fiber with the same area: about 15.5μm).
[0082] Fiber 1-1 had a four-lobe fiber cross-sectional shape having four convex portions as shown in FIG. 1, and the convex portions had a substantially curved tip portion, and the width of the root portion toward the center of the fiber was smaller than the maximum width of the tip portion. The maximum width Wt at the tip portion of the convex portion was 8.6 μm, the width Wb at the root portion was 4.8 μm, the ratio Wt / Wb of the maximum width Wt of the convex portion to the width Wb of the root portion was 1.79, the length Lt of the convex portion (the length from the center point of the root portion of the convex portion to the tip) was 9.4 μm, and the ratio Lt / Wb of the length Lt of the convex portion to the width Wb of the root portion was 1.96. Some of the convex portions were deformed from the root, the distance between adjacent convex portions was not constant, and in some fibers, part of the root portion of the convex portion was peeled off.
[0083] Rayon (Corona (registered trademark), manufactured by Daiwabo Rayon Co., Ltd.) was prepared as fiber 2. The fineness of fiber 2 was 1.7 dtex (fiber diameter when the cross-sectional area of the fiber is converted into a circular cross-sectional fiber with the same area: about 12 μm). A core-sheath type composite fiber (PP / HDPE) (manufactured by Daiwa Boseki Co., Ltd., NBF (registered trademark) (H) (product name)) with a core of polypropylene (melting point: 160°C) and a sheath of high-density polyethylene (melting point: 133°C) was prepared as fiber 3. The fineness of fiber 3 was 1.7 dtex (fiber diameter: about 15.5 μm).
[0084] 50% by mass of fiber 1-1, 30% by mass of fiber 2, and 20% by mass of fiber 3 were mixed and carded using a parallel carding machine to a web target weight of about 50 g / m 2 A parallel web was produced by the above method. This web was subjected to a hydroentanglement treatment to entangle the fibers. The hydroentanglement treatment was performed by spraying a columnar water stream of 3.0 MPa once onto one side of the web and once onto the other side, using a nozzle having orifices with a hole diameter of 0.08 mm spaced at 0.6 mm intervals. It is believed that at least a part of fiber 1-1 (a part of the convex portion) peeled off during this hydroentanglement treatment. The web after hydroentanglement was subjected to a heat treatment at 135° C., whereby drying and heat bonding were simultaneously performed. By the heat treatment, only the high density polyethylene of the fiber 3 was melted, and the fibers were thermally bonded to each other by the high density polyethylene, thereby producing the nonwoven fabric of Example 1.
[0085] [Example 2] In the melt spinning process described in Example 1, a spun filament (undrawn) having a fineness of 4.5 dtex was produced by setting the take-up speed to 900 m / min. The spun filament was wet-drawn 2.0 times in warm water at 90°C, and the same method as that described in Example 1 was used to obtain fiber 1-2 having a fineness of 2.6 dtex (fiber diameter when the fiber cross-sectional area is converted into a round cross-sectional fiber having the same area: about 19 μm). Fiber 1-2 was tetralobal like fiber 1-1. The maximum width Wt at the tip of the protrusion was 9.7 μm, the width Wb at the base was 5.4 μm, the ratio Wt / Wb of the maximum width Wt of the protrusion to the width Wb at the base was 1.80, the length Lt of the protrusion (the length from the center point of the base of the protrusion to the tip) was 10.2 μm, and the ratio Lt / Wb of the length Lt of the protrusion to the width Wb at the base was 1.89. The nonwoven fabric of Example 2 was produced in the same manner as described in Example 1, except that Fiber 1-2 was used instead of Fiber 1-1.
[0086] [Example 3] In the melt spinning process described in Example 1, instead of the raw polypropylene resin, a polypropylene resin to which a hydrophilizing agent (potassium salt of alkyl phosphate ester having 12 carbon atoms) was added so that the ratio of the hydrophilizing agent was 1.0% by mass when the total mass of the polypropylene resin and the hydrophilizing agent was 100% by mass was used as the raw material, and a take-up speed was set to 1350 m / min to produce a spun filament (undrawn) having a fineness of 3.5 dtex. The spun filament was wet-drawn 2.6 times in 90°C warm water using the same method as that described in Example 1 to obtain fiber 1-3 having a fineness of 1.5 dtex (fiber diameter when converted into a round cross-sectional fiber having the same area as the fiber cross-sectional area: about 14.6 μm). Fiber 1-3 was tetralobal like fiber 1-1. The maximum width Wt at the tip of the protrusion was 8.3 μm, the width Wb at the base was 4.9 μm, the ratio Wt / Wb of the maximum width Wt of the protrusion to the width Wb at the base was 1.69, the length Lt of the protrusion (the length from the center point of the base of the protrusion to the tip) was 9.6 μm, and the ratio Lt / Wb of the length Lt of the protrusion to the width Wb at the base was 1.96. The nonwoven fabric of Example 3 was produced using a method similar to that described in Example 1, except that fiber 1-3 was used instead of fiber 1-1.
[0087] [Example 4] In the melt spinning process described in Example 1, a polypropylene resin to which a hydrophilizing agent (potassium salt of an alkyl phosphate ester having 12 carbon atoms) was added so that the proportion of the hydrophilizing agent was 1.0 mass% when the sum of the mass of the polypropylene resin and the mass of the hydrophilizing agent was 100 mass% was used instead of the raw polypropylene resin, and a fiber 1-4 having a fineness of 1.7 dtex (fiber diameter when the fiber cross-sectional area is converted into a circular cross-section fiber with the same area: about 15.5 μm) was obtained using a method similar to that described in Example 1. Fiber 1-4 was tetralobal like fiber 1-1. The maximum width Wt at the tip of the protrusion was 8.7 μm, the width Wb at the base was 5.5 μm, the ratio Wt / Wb of the maximum width Wt of the protrusion to the width Wb at the base was 1.58, the length Lt of the protrusion (the length from the center point of the base of the protrusion to the tip) was 9.0 μm, and the ratio Lt / Wb of the length Lt of the protrusion to the width Wb at the base was 1.64. The nonwoven fabric of Example 4 was produced using a method similar to that described in Example 1, except that fiber 1-4 was used instead of fiber 1-1.
[0088] [Example 5] In the melt spinning process described in Example 1, instead of the raw polypropylene resin, a polypropylene resin to which a hydrophilizing agent (potassium salt of alkyl phosphate ester having 12 carbon atoms) was added so that the ratio of the hydrophilizing agent was 1.0% by mass when the total mass of the polypropylene resin and the hydrophilizing agent was 100% by mass was used as the raw material, and a take-up speed was set to 900 m / min to produce a spun filament (undrawn) having a fineness of 4.5 dtex. The spun filament was wet-drawn 2.3 times in 90°C warm water using the same method as that described in Example 1 to obtain fiber 1-5 having a fineness of 2.2 dtex (fiber diameter when converted into a round cross-sectional fiber having the same area of the fiber cross section: about 17.5 μm). Fiber 1-5 was tetralobal like fiber 1-1. The maximum width Wt at the tip of the protrusion was 8.4 μm, the width Wb at the base was 5.0 μm, the ratio Wt / Wb of the maximum width Wt of the protrusion to the width Wb at the base was 1.68, the length Lt of the protrusion (the length from the center point of the base of the protrusion to the tip) was 10.5 μm, and the ratio Lt / Wb of the length Lt of the protrusion to the width Wb at the base was 2.10. The nonwoven fabric of Example 5 was produced using a method similar to that described in Example 1, except that fiber 1-5 was used instead of fiber 1-1.
[0089] [Example 6] Fiber 1-6 having a fineness of 2.6 dtex (fiber diameter when the fiber cross-sectional area is converted to a round cross-sectional fiber having the same area: about 19.0 μm) was obtained using a method similar to that described in Example 2, except that in the melt spinning process described in Example 2, a polypropylene resin to which a hydrophilizing agent (potassium salt of an alkyl phosphate ester having 12 carbon atoms) was added so that the proportion of the hydrophilizing agent was 1.0 mass% when the sum of the mass of the polypropylene resin and the mass of the hydrophilizing agent was 100 mass% was used instead of the raw polypropylene resin as the raw material. Fiber 1-6 was tetralobal like fiber 1-1. The maximum width Wt at the tip of the protrusion was 9.3 μm, the width Wb at the base was 6.2 μm, the ratio Wt / Wb of the maximum width Wt of the protrusion to the width Wb at the base was 1.50, the length Lt of the protrusion (the length from the center point of the base of the protrusion to the tip) was 11.5 μm, and the ratio Lt / Wb of the length Lt of the protrusion to the width Wb at the base was 1.85. The nonwoven fabric of Example 6 was produced using a method similar to that described in Example 1, except that fiber 1-6 was used instead of fiber 1-1.
[0090] [Example 7] Fiber 1-7 having a fineness of 1.7 dtex (fiber diameter when the fiber cross-sectional area is converted to a round cross-sectional fiber having the same area: about 15.5 μm) was obtained using a method similar to that described in Example 1, except that in the melt spinning process described in Example 1, a polypropylene resin to which a hydrophilizing agent (potassium salt of an alkyl phosphate ester having 12 carbon atoms) was added so that the proportion of the hydrophilizing agent was 6.0 mass% when the sum of the mass of the polypropylene resin and the mass of the hydrophilizing agent was 100 mass% was used instead of the raw polypropylene resin as the raw material. Fiber 1-7 was tetralobal like fiber 1-1. The maximum width Wt at the tip of the protrusion was 8.6 μm, the width Wb at the base was 4.8 μm, the ratio Wt / Wb of the maximum width Wt of the protrusion to the width Wb at the base was 1.79, the length Lt of the protrusion (the length from the center point of the base of the protrusion to the tip) was 9.4 μm, and the ratio Lt / Wb of the length Lt of the protrusion to the width Wb at the base was 1.96. The nonwoven fabric of Example 7 was produced using a method similar to that described in Example 1, except that fiber 1-7 was used instead of fiber 1-1.
[0091] [Example 8] In the melt spinning process described in Example 5, a polypropylene resin to which a hydrophilizing agent (potassium salt of an alkyl phosphate ester having 12 carbon atoms) was added so that the proportion of the hydrophilizing agent was 6.0% by mass when the sum of the mass of the polypropylene resin and the mass of the hydrophilizing agent was 100% by mass was used instead of the raw polypropylene resin, and a fiber 1-8 having a fineness of 2.2 dtex (fiber diameter when the fiber cross-sectional area is converted to a round cross-section fiber with the same area: about 17.5 μm) was obtained using a method similar to that described in Example 5. Fiber 1-8 was tetralobal like fiber 1-1. The maximum width Wt at the tip of the protrusion was 8.4 μm, the width Wb at the base was 5.0 μm, the ratio Wt / Wb of the maximum width Wt of the protrusion to the width Wb at the base was 1.68, the length Lt of the protrusion (the length from the center point of the base of the protrusion to the tip) was 10.5 μm, and the ratio Lt / Wb of the length Lt of the protrusion to the width Wb at the base was 2.10. The nonwoven fabric of Example 8 was produced using a method similar to that described in Example 1, except that fiber 1-8 was used instead of fiber 1-1.
[0092] [Example 9] Fiber 1-9 having a fineness of 2.6 dtex (fiber diameter when the fiber cross-sectional area is converted to a circular cross-sectional fiber having the same area: about 19.0 μm) was obtained using a method similar to that described in Example 2, except that in the melt spinning process described in Example 2, a polypropylene resin to which a hydrophilizing agent (potassium salt of an alkyl phosphate ester having 12 carbon atoms) was added so that the proportion of the hydrophilizing agent was 6.0 mass% when the sum of the mass of the polypropylene resin and the mass of the hydrophilizing agent was 100 mass% was used instead of the raw polypropylene resin as the raw material. Fiber 1-9 was tetralobal like fiber 1-1. The maximum width Wt at the tip of the protrusion was 10.3 μm, the width Wb at the base was 6.2 μm, the ratio Wt / Wb of the maximum width Wt of the protrusion to the width Wb at the base was 1.66, the length Lt of the protrusion (the length from the center point of the base of the protrusion to the tip) was 11.0 μm, and the ratio Lt / Wb of the length Lt of the protrusion to the width Wb at the base was 1.77. The nonwoven fabric of Example 9 was produced using a method similar to that described in Example 1, except that fiber 1-9 was used instead of fiber 1-1.
[0093] [Example 10] The nonwoven fabric of Example 10 was produced in the same manner as in Example 3, except that the hydroentanglement treatment was performed with a columnar water flow of 1.5 MPa on both sides of the nonwoven fabric.
[0094] [Example 11] The nonwoven fabric of Example 11 was produced using the same method as that described in Example 1, except that in the manufacturing method of the nonwoven fabric described in Example 3, the hydroentanglement treatment was performed with a columnar water flow of 4.5 MPa on both sides.
[0095] [Example 12] The nonwoven fabric of Example 12 was produced using a method similar to that described in Example 4, except that in the nonwoven fabric production method described in Example 4, 30 mass% of fibers 1-4, 50 mass% of fiber 2, and 20 mass% of fiber 3 were mixed to produce a parallel web.
[0096] [Example 13] The nonwoven fabric of Example 13 was produced using a method similar to that described in Example 4, except that in the nonwoven fabric production method described in Example 4, 70 mass% of fibers 1-4, 10 mass% of fiber 2, and 20 mass% of fiber 3 were mixed to produce a parallel web.
[0097] [Example 14] The nonwoven fabric of Example 14 was produced using a method similar to that described in Example 4, except that a parallel web was produced using only fibers 1-4 in the nonwoven fabric production method described in Example 4.
[0098] [Comparative Example 1] Instead of fiber 1-1, fiber 1'-1 (T1281 (product name) manufactured by Toray Industries, Inc.) having a flat PET fineness of 1.7 dtex (fiber diameter 13.0 μm) was used. A nonwoven fabric of Comparative Example 1 was produced in the same manner as described in Example 1, except that fiber 1'-1 was used instead of fiber 1-1.
[0099] [Comparative Example 2] A fiber 1'-2 having a fineness of 1.4 dtex (fiber diameter: 14.6 µm) was obtained in the same manner as in Example 1, except that a spinning nozzle having a round nozzle hole shape was used. A nonwoven fabric of Comparative Example 2 was produced in the same manner as described in Example 1, except that fiber 1'-2 was used instead of fiber 1-1.
[0100] [Comparative Example 3] Fiber 1'-3 having a fineness of 1.5 dtex (fiber diameter: 14.6 μm) was obtained using a method similar to that described in Example 1, except that a spinning nozzle having a round nozzle hole shape was used and 1.0 mass% of a hydrophilizing agent (potassium salt of an alkyl phosphate ester having 12 carbon atoms) was attached to the fiber after dry drawing. A nonwoven fabric of Comparative Example 3 was produced in the same manner as described in Example 1, except that Fiber 1'-3 was used instead of Fiber 1-1.
[0101] [Comparative Example 4] Instead of fiber 1-1, a PET fiber with a shuriken-shaped cross section (PZ-FS (product name) manufactured by Tainan Boseki Co., Ltd., fineness: 1.6 dtex, fiber diameter when converted to a round cross section fiber with the same area: approximately 12.5 μm, fiber length: 38 mm) was prepared and used as fiber 1'-4 to make a nonwoven fabric. Fiber 1'-4 was tetralobal but shuriken-shaped. The maximum width Wt at the tip of the protrusion was 6.4 μm, the width Wb at the base was 7.9 μm, the ratio Wt / Wb of the maximum width Wt of the protrusion to the width Wb at the base was 0.81, the length Lt of the protrusion (the length from the center point of the base to the tip of the protrusion) was 5.8 μm, and the ratio Lt / Wb of the length Lt of the protrusion to the width Wb at the base was 0.73. A nonwoven fabric of Comparative Example 4 was produced in the same manner as described in Example 1, except that Fiber 1'-4 was used instead of Fiber 1-1.
[0102] [Comparative Example 5] The nonwoven fabric of Comparative Example 5 was produced using a method similar to that described in Comparative Example 1, except that the parallel web was produced using only fiber 1'-1 in the nonwoven fabric manufacturing method described in Comparative Example 1.
[0103] [Comparative Example 6] The nonwoven fabric of Comparative Example 5 was produced using a method similar to that described in Comparative Example 1, except that in the nonwoven fabric manufacturing method described in Comparative Example 4, only fiber 1'-4 was used to produce a parallel web.
[0104] [Comparative Example 7] The nonwoven fabric of Comparative Example 7 was produced using a method similar to that described in Comparative Example 5, except that in the manufacturing method of the nonwoven fabric described in Comparative Example 5, instead of fiber 1'-1, a parallel web was produced using only a commercially available split composite fiber (DF-1 (product name) manufactured by Yamato Boseki Co., Ltd., a 16-split fiber with a circular cross section in which polyethylene terephthalate resin and polypropylene resin are combined and 8 pieces of each resin component are arranged alternately, for a total of 16 resin components) only.
[0105] The physical properties of the nonwoven fabrics and fibers 1-1 to 1'-4 of the above-mentioned Examples 1 to Comparative Example 4 are summarized in Tables 1 to 3. The methods for measuring the physical properties of fibers 1-1 to 1'-4 are as follows.
[0106] [Single fiber size] The single fiber fineness was measured in accordance with the measurement of corrective fineness by the vibration method described in Appendix JB of JIS L 1015:2021 8.5.2 Measurement of fineness by the ISO method.
[0107] [Single fiber strength and breaking elongation] According to JIS L 1015, a tensile tester was used to measure the load and elongation at fiber breakage when the sample was gripped at a distance of 20 mm, and these were taken as single fiber strength and breaking elongation, respectively.
[0108] [140℃ dry heat shrinkage rate] The resulting multi-lobal cross section fiber was looped to a length of 10 cm, and the ends of the yarn were tied to obtain a sample (the total fineness of the sample consisting of multiple bundled fibers was adjusted to 55.6 dtex). An initial load of 0.26 cN / dtex was applied to the sample, and the sample was heated from room temperature to 170°C at a heating rate of 60°C / min using a thermal stress tester KE-2LS (manufactured by Kanebo Engineering Co., Ltd.) in displacement measurement mode, while the sample was continuously heated to 170°C at a heating rate of 60°C / min. The heat treatment shrinkage of the sample at 140°C was recorded as the 140°C dry heat shrinkage of the multi-lobal cross section fiber.
[0109] [Measurement of the shape of multi-lobed cross-section fibers] In the cross-section of the multi-lobal cross-section fiber, the maximum width (Wt) at the tip of the protrusion, the length (Lt) of the protrusion, the maximum width (Wt) at the tip of the protrusion, and the width (Wb) at the base of the protrusion were measured using the following procedure. First, a nonwoven fabric containing multilobal cross-section fibers is prepared, and the nonwoven fabric is cut with a sharp blade in a direction perpendicular to the machine direction (MD) of the nonwoven fabric. The cut surface obtained by the above operation was observed with a scanning electron microscope (SEM, acceleration voltage: 5.00 kV, magnification: 200 times). From the SEM images taken, five arbitrary multilobal cross-section fibers were selected from one SEM photograph. The selected fibers were measured using image analysis software WinROOF (manufactured by Mitani Shoji Co., Ltd.) to measure the length (Lt) of the convex portion, the maximum width (Wt) of the convex portion, and the distance of the width (Wb) of the base part of the convex portion shown in the fiber cross-section schematic diagram of the multilobal cross-section fiber in Figure 1. The measurements were performed on a total of three SEM images, and the values for each point in the 15 pieces were averaged.
[0110] The methods for measuring the physical properties of the nonwoven fabrics of Examples 1 to Comparative Example 4 are as follows. Thickness The thickness of the nonwoven fabric was measured as follows. A thickness gauge (THICKNESS GAUGE Model CR-60A (product name) manufactured by Daiei Scientific Instruments Manufacturing Co., Ltd.) was used to measure the thickness of the nonwoven fabric at 0.3 kPa (1 cm 2 3g per cm) and 1.96kPa (1cm) on nonwoven fabric 2 The thickness of the nonwoven fabric was measured under a load of 20 g per unit area.
[0111] [Metaku] The basis weight of a nonwoven fabric was calculated by measuring the mass of a sample piece of a specified size without wetting it with cosmetics, water, etc. That is, a sample of 15 cm length (MD direction, flow direction) x 15 cm width (CD direction, machine direction) was taken from the nonwoven fabric for which the basis weight was to be measured, and its mass was measured. The measured mass of the nonwoven fabric sample and the area of the sample (225 cm 2 The basis weight of the nonwoven fabric was calculated from the weight per unit area. Three samples were taken from the same nonwoven fabric, and the average of the basis weights measured for each sample was taken as the basis weight (actual measured value) of the nonwoven fabric.
[0112] [Specific volume] The specific volume was measured as follows. First, the basis weight of the nonwoven fabric for which the specific volume is to be measured is calculated by the above-mentioned method. Next, the thickness of the nonwoven fabric sample used for calculating the basis weight is measured by the above-mentioned method. The specific volume of the nonwoven fabric was calculated from the measured basis weight and thickness. As with the basis weight measurement, the specific volume was measured by taking three samples of the same nonwoven fabric, and the average value of the specific volumes measured for each sample was taken as the specific volume (actual measured value) of the nonwoven fabric.
[0113] [Bulk density] Bulk density was measured as follows. First, the basis weight of the nonwoven fabric to be measured for bulk density is calculated by the above-mentioned method. Next, the thickness of the nonwoven fabric sample used for calculating the basis weight is measured by the above-mentioned method. The specific volume of the nonwoven fabric was calculated from the measured basis weight and thickness. For the measurement of bulk density, similar to the measurement of basis weight, three samples to be measured were taken from the same nonwoven fabric, and the average value of the specific volume measured for each sample was taken as the bulk density (actual measured value) of the nonwoven fabric.
[0114] [Thickness reduction rate] The thickness reduction rate was measured as follows. First, three nonwoven fabric samples for measuring the thickness reduction rate are prepared. Next, when measuring the thickness of the nonwoven fabric, the load applied to the nonwoven fabric is 0.3 kPa (1 cm 2 The thickness (T 0.3 ) is measured. Next, the thickness was measured at a different location and the load applied to the nonwoven fabric was changed to 1.96 kPa (1 cm 2 20g weight per unit) and measure the thickness (T 1.96 ). The thickness (T 0.3 ) and the thickness (T 1.96 ) and calculate the thickness reduction rate of the nonwoven fabric using the following formula. ·Thickness reduction rate (%)=100×(T 0.3 -T 1.96 ) / T 0.3 The thickness reduction rate of the nonwoven fabric was measured three times, and the average value was regarded as the thickness reduction rate of the nonwoven fabric.
[0115] [Strength and elongation in dry state] The strength and elongation (breaking strength, breaking elongation, 10% modulus strength) of the nonwoven fabric in a dry state was measured in accordance with JIS L 1913:2010 6.3 as described below. First, three measurement samples are taken from the nonwoven fabric for measuring the strength and elongation in a dry state. Next, a constant-speed tension tensile tester was used to perform a tensile test under the conditions of a sample width of 5 cm, a gripping distance of 10 cm, and a tensile speed of 30±2 cm / min, and the load value at break (tensile strength), elongation percentage, and 10% modulus strength (the force required to elongate by 10%, also called the stress at 10% elongation) were measured. The tensile test was performed in the machine direction (MD) and cross direction (CD) of the nonwoven fabric as the tensile direction. The evaluation results were all the average values measured for three samples.
[0116] [Amount of fluff shedding] The amount of fuzz shedding was evaluated by measuring the amount (mg) of fibers that had fallen off from the nonwoven fabric by the following method. a) A disk (diameter 70 mm, 350 g) whose surface is covered with urethane foam (manufactured by INOAC Corporation, product name Malt Filter (registered trademark), product number: MF-30, ester-based polyurethane, number of cells 30, average cell diameter 410 μm, average coefficient of friction (MIU) 0.69, variation in average coefficient of friction (MMD) 0.043, thickness 5 mm) is attached to a rotating shaft so that the rotating shaft is shifted 20 mm from the center of the disk. b) Place the same urethane foam as above on top and fix the nonwoven fabric on the table so that one side of the nonwoven fabric is exposed. c) Place the disk on the nonwoven fabric. At this time, the only load applied to the nonwoven fabric is the disk's own weight. d) Rotate the rotating shaft and rotate the disk on the nonwoven fabric. Seven sets of three rotations clockwise and three rotations counterclockwise are performed. The rotation speed is about 3 seconds per rotation. e) After seven sets of rotation, collect the fibers that have fallen out of the nonwoven fabric and attached to the surface of the urethane foam covering the disk, and measure their mass (mg). f) The above operations a) to e) are carried out for three nonwoven fabric samples. For each of the three nonwoven fabric samples, the mass of the fallen fibers is measured and the average value is taken as the amount of fallen fuzz (mg).
[0117] [Collectivity] The foreign matter collection ability (dust, sesame, dust) required when the nonwoven fabric was used as various wiping sheets was evaluated as follows.
[0118] [Dust collection ability] First, a white acrylic plate (55 cm long, 65 cm wide) is prepared, and a rectangular area measuring 5 cm long x 15 cm wide at approximately the center of the plate is designated as the dust dispersion area. Next, 0.20 g of test powder (seven types) conforming to JIS Z 8901 is collected. The collected test powder is then dispersed and sprinkled evenly over the dust dispersion area of the white acrylic plate. A sample of nonwoven fabric with a length of 29 cm and a width of 21 cm was taken to evaluate the dust collection ability, and its mass (M D0 The mass of the nonwoven fabric was then measured, and the test powder on the dust-dispersed area was wiped off. The test powder was wiped off with a commercially available flooring wiper tool (manufactured by Kao Corporation, product name: Quickle Wiper (registered trademark); head part of the tool body was used) attached so that the area contributing to wiping was 26 cm vertically and 16 cm horizontally, and the top surface of the nonwoven fabric (the surface onto which the water jet was last sprayed during the water jet entanglement process) was the wiping surface, and a load of 400 gf was applied. Wiping was performed by moving the wiper back and forth once on the surface of the white acrylic plate. The wiping action is as follows. Place the wiper in the center of the dust distribution area so that the vertical direction of the wiper coincides with the vertical direction of the dust distribution area; From there, move the wiper 250 mm toward the left end of the dust dispersion area to rub the dust (white acrylic plate). Then, move the wiper 500 mm toward the right end of the dust dispersion area, The wiper was then moved 250 mm in the direction toward the left end of the dust dispersion area and made one stroke. After one stroke of the wiper, the mass of the nonwoven fabric used for wiping (M D ) is measured. The mass of the nonwoven fabric before and after wiping (M D0 , M D) and the mass (0.2g) of the test powder scattered on the white acrylic plate, the dust collection efficiency (%) was calculated using the following formula. Dust collection efficiency (%) = 100 × (M D -M D0 ) / 0.2 For the nonwoven fabrics to be evaluated for dust collection ability, the wiping surface of the nonwoven fabric was renewed, the white acrylic plate was washed with tap water, and after drying, the same wiping test was carried out three times. The average of the obtained measured values was regarded as the dust collection rate of the nonwoven fabric.
[0119] [Hair collection ability (wet)] As an evaluation of the performance when the nonwoven fabric was used as a wiping sheet, the hair collecting ability was evaluated by the following method. First, five strands of hair (approximately 5 cm long) were placed on a commercially available flooring board (three flooring boards, 14 cm long and 90 cm wide, joined together to make a flooring board 42 cm long and 90 cm wide), with three strands arranged horizontally and two arranged vertically, spaced 2 cm apart. Next, three samples measuring 29 cm in length and 21 cm in width were taken from the nonwoven fabric to evaluate its hair-collecting ability in a wet state, and hair was wiped off using the taken pieces of nonwoven fabric. The wiping is carried out in a wet state in which 100 parts by mass of the nonwoven fabric is impregnated with 300 parts by mass of distilled water. The hair that has fallen onto the flooring is wiped off by the following procedure. First, the nonwoven fabric moistened by the above method was attached to a commercially available flooring wiper tool (manufactured by Kao Corporation, product name: Quickle Wiper (registered trademark); the head part of the tool body was used) so that the area contributing to wiping was 26 cm vertically and 16 cm horizontally, and the top surface of the nonwoven fabric (the surface onto which the water jet was last sprayed during the water jet entanglement process) was the wiping surface, and a load of 400 gf was applied. Wiping was performed in the same manner as in the evaluation of the dust collection ability, by moving the wiper back and forth once over the flooring on which the hair had fallen. After wiping, the capture rate (%) was calculated from the number of hairs wiped off the flooring. For the nonwoven fabrics to be evaluated for hair collection ability (wet state), the wiping surface of the nonwoven fabric was renewed, the flooring board was wiped clean, and the same wiping test was carried out three times. The average of the measured values obtained was regarded as the hair collection rate (wet state) of the nonwoven fabric being evaluated.
[0120] [Sesame capture ability (wet condition)] As an evaluation of the performance when the nonwoven fabric was used as a wiping sheet, the sesame seed collection ability was evaluated by the following method. First, ten sesame seeds were arranged in three rows (3-4-3 rows, spaced 2 cm apart) on a commercially available flooring board (three flooring boards, each 14 cm long and 90 cm wide, were joined together to make a flooring board 42 cm long and 90 cm wide). Next, three samples measuring 29 cm in length and 21 cm in width were taken from the nonwoven fabric to evaluate its ability to capture sesame seeds in a wet state, and the taken pieces of nonwoven fabric were used to wipe off the sesame seeds. The wiping is carried out in a wet state in which 100 parts by mass of the nonwoven fabric is impregnated with 300 parts by mass of distilled water. The sesame seeds that have fallen onto the flooring are wiped off by the following procedure. First, the nonwoven fabric moistened by the above method was attached to a commercially available flooring wiper tool (Kao Corporation, product name: Quickle Wiper (registered trademark), head part of the tool body was used) so that the area contributing to wiping was 26 cm vertically and 16 cm horizontally, and the upper surface of the nonwoven fabric (the surface onto which the water jet was last sprayed during the water jet entanglement process) was the wiping surface, and a load of 400 gf was applied. Wiping was performed by moving the wiper back and forth once over the flooring on which sesame seeds had been dropped, using the same operating method as that used in the evaluation of dust collection ability. After wiping, the capture rate (%) was calculated from the number of sesame seeds wiped off the flooring. For the nonwoven fabrics to be evaluated for sesame capture (wet state), the wiping surface of the nonwoven fabric was renewed, the flooring board was wiped clean, and the same wiping test was carried out three times. The average of the measured values was regarded as the sesame capture rate (wet state) of the nonwoven fabrics to be evaluated.
[0121] [Sustained release / liquid residual rate] The sustained release was measured as follows. The initial release amount and residual liquid rate were measured by preparing a nonwoven fabric of the same size as that used in the dirt collection test (length 29 cm, width 21 cm) and measuring the weight of the nonwoven fabric when dry (NW d Measure. Next, 100 parts by mass of the nonwoven fabric was impregnated with 300 parts by mass of distilled water, and the weight NWw of the nonwoven fabric when impregnated with the liquid was measured. Next, the nonwoven fabric was attached to a commercially available flooring wiper tool (manufactured by Kao Corporation, product name: Quickle Wiper (registered trademark); the head part of the tool body was used) so that the area contributing to wiping was 26 cm vertically and 16 cm horizontally, and the top surface of the nonwoven fabric (the surface onto which the water jet was last sprayed during the water jet entanglement process) would be the wiping surface. With a load of 400 gf applied, the nonwoven fabric was placed on the conveyor so that the conveyor's direction of travel was aligned with the horizontal direction of the nonwoven fabric (parallel to the 16 cm width), and the conveyor was operated at a speed of 5 m / min. The conveyor was rotated once (0.5 tatami mats = 0.81 m 2 ) weight of nonwoven fabric NW 0.5 The initial release amount RA1 was calculated from the following formula: ·Initial release amount (RA1 (g))=NWw-NW 0.5 Subsequently, the nonwoven fabric was similarly placed on the conveyor, and the weight of the nonwoven fabric was measured after the 2nd, 4th, 6th and 8th revolutions of the conveyor (NW2, NW4, NW6 and NW8) to determine the residual liquid rate in the nonwoven fabric. RR2=100-((NW w -NW2) / (NW w -N.W. d )×100) RR4=100-((NW w -NW4) / (NW w -N.W. d )×100) RR6=100-((NW w -NW6) / (NW w -N.W. d )×100) RR8=100-((NW w -NW8) / (NW w -N.W. d )×100)
[0122] [SEM photo] SEM photographs of the surfaces and cross sections of the nonwoven fabrics of Examples 1, 4 and 7 and Comparative Examples 3, 4 and 1 were taken and are shown in FIG. 2 and FIG. Rows (A), (B), and (C) in FIG. 2 show SEM photographs of the nonwoven fabrics of Examples 1, 4, and 7. The SEM photographs in columns (1) to (3) in each row of FIG. 2 show SEM photographs of three surfaces of each nonwoven fabric at 100 times magnification. The SEM photographs in columns (4) to (6) in each row of FIG. 2 show SEM photographs of three surfaces of each nonwoven fabric at 50 times magnification. The SEM photograph in column (7) in each row of FIG. 2 shows SEM photographs of the cross section of each nonwoven fabric at 400 times magnification. It can be seen that the nonwoven fabrics of Examples 1, 4, and 7 have a kinked and sharply curved fiber structure. Furthermore, it can be seen that some fibers may peel off to produce finer fibers. Rows (D), (E), and (F) in FIG. 3 show SEM photographs of the nonwoven fabrics of Comparative Examples 3, 4, and 1. The SEM photographs in columns (1) to (3) in each row of FIG. 3 show SEM photographs of three surfaces of each nonwoven fabric at 100 times magnification. The SEM photographs in columns (4) to (6) in each row of FIG. 3 show SEM photographs of three surfaces of each nonwoven fabric at 50 times magnification. The SEM photograph in column (7) in each row of FIG. 3 shows SEM photographs of the cross section of each nonwoven fabric at 400 times magnification. It can be seen that the nonwoven fabrics of Comparative Examples 3, 4, and 1 have almost no crimped or sharply curved fiber structure, but have a gently curved structure. It can also be seen that some fibers have peeled off and no ultrafine fibers have been produced.
[0123] [Table 1]
[0124] [Table 2]
[0125] [Table 3]
[0126] [Table 4]
[0127] None of the nonwoven fabrics of Examples 1 to 14 had particularly poor physical properties, and the physical properties were well-balanced and excellent overall. On the other hand, the nonwoven fabrics of Comparative Examples 1 to 7 had some poor physical properties, and as a whole, the balance of physical properties was inferior to that of the Examples.
[0128] [Example 15] As the fiber 1, the above-mentioned fiber 1-1 was used, which had a tetralobal cross-sectional shape with four projections, a fineness of 1.7 dtex, and a fiber diameter of 15.5 μm. Fiber 2 was not used. As fiber 3, a splittable composite fiber (DFS(SH) (product name) manufactured by Yamato Boseki Co., Ltd., hereinafter also referred to as PET / PE splittable composite fiber) with a round cross section and no hollow portion, which is made of a combination (PET / PE) of polyethylene terephthalate (melting point: 255°C) and high density polyethylene (melting point: 133°C), has a cross section in which polyethylene terephthalate sections (number of sections: 4) and high density polyethylene sections (number of sections: 4) are alternately arranged in a chrysanthemum shape, and has a total of 8 sections, was prepared. The fiber 3 had a fineness of 2.2 dtex and a fiber diameter of 16.0 μm. 50% by mass of fiber 1-1 and 50% by mass of PET / PE splittable composite fiber were mixed and carded into a web target weight of about 30 g / m using a parallel carding machine. 2 A parallel web was produced by the above method. This web was used as the first fibrous layer and the third fibrous layer.
[0129] On the other hand, the above-mentioned rayon (Corona (registered trademark), manufactured by Daiwabo Rayon Co., Ltd.) was prepared as a hydrophilic fiber. Its fineness was 1.7 dtex and its fiber diameter was 12 μm. Using 100% by mass of this hydrophilic fiber, a parallel carding machine was used to obtain a web target weight of about 10 g / m 2 A parallel web was produced by the above method. This web was used as the middle layer (second fibrous layer).
[0130] A middle layer is sandwiched between the first and third fiber layers, and the target weight is 70 g / m 2 A laminated fiber web of Example 15 was obtained. This web was subjected to a hydroentanglement treatment to entangle the fibers. The hydroentanglement treatment was performed by spraying a columnar water stream of 3.0 MPa twice on one side of the web using a nozzle having orifices with a hole diameter of 0.08 mm arranged at intervals of 0.6 mm, and spraying a columnar water stream of 3.0 MPa twice on the other side. The hydroentangled fiber web was dried using a dryer set at 80 ° C. so that the high-density polyethylene contained in the fiber web would not melt, and a nonwoven fabric of Example 15 was obtained. The evaluation results are shown in Table 5.
[0131] [Comparative Example 8] Using 100% by mass PET / PE splittable composite fiber, a parallel card machine was used to card the web at a target weight of approximately 30 g / m 2 A parallel web was produced. A nonwoven fabric of Comparative Example 8 was obtained in the same manner as in Example 15, except that this web was used as the first fibrous layer and the third fibrous layer. The evaluation results are shown in Table 5.
[0132] [Table 5]
[0133] The physical properties of the nonwoven fabric of Example 15, particularly with respect to fiber shedding, foreign matter collection (hair, sesame seeds, dust), and sustained release of the impregnated chemical solution, which are important when the nonwoven fabric is used as a base fabric for a wiping sheet, were not evaluated as having extremely low performance, and the physical properties were well balanced overall. The wiping properties showed better collection properties for foreign matter of different types and sizes such as hair, sesame seeds, and dust, especially dust collection properties, due to the expression of ultrafine fibers by the split fibers and the multilobal cross-section fibers and the effect of the inter-fiber voids by the multilobal cross-section fibers, by combining the split fibers and the multilobal cross-section fibers. Furthermore, the results showed better sustained release properties than the nonwoven fabric of Comparative Example 8, in which fiber layers not containing multilobal cross-section fibers were located on both surfaces. This is thought to be due to the effect of the inter-fiber voids by the multilobal cross-section fibers and the liquid retention properties derived from their shape. On the other hand, when the nonwoven fabric of Comparative Example 8, in which fiber layers composed only of ultrafine fibers and not containing multilobal cross-section fibers were arranged on both surfaces of the nonwoven fabric, was used as the base fabric of a wiping sheet, some physical properties assumed for wiping performance were poor, and the balance of physical properties as a whole was inferior to that of the nonwoven fabric of Example 15. This is because, when the nonwoven fabric of Comparative Example 8 was used as the base fabric of a wiping sheet, the first or third fiber layer constituting the wiping surface was a fiber layer composed only of split fibers, and therefore, although wiping performance was improved by ultrafine fibers with noncircular cross-sectional shapes generated by the entanglement and splitting treatment using a high-pressure water flow, the generation of ultrafine fibers reduced the inter-fiber voids inside the fiber layer, resulting in lower performance than that of Example 15. [Industrial Applicability]
[0134] The nonwoven fabric according to the embodiment of the present invention is a nonwoven fabric containing 20% by mass or more of specific multilobal cross-sectional fibers, and has excellent dirt collection performance even when the cross-sectional shape of the specific multilobal cross-sectional fibers is partially distorted, i.e., when some of the convex portions in the cross-section of the multilobal cross-sectional fibers are separated or peeled off, and even when the cross-sectional shape of the specific multilobal cross-sectional fibers is not partially distorted, i.e., when some of the convex portions in the cross-section of the multilobal cross-sectional fibers are not separated or peeled off. When the nonwoven fabric is used as various wiping sheets, wiping sheets with higher wiping properties can be easily obtained. Furthermore, when the nonwoven fabric contains thermally adhesive fibers in addition to specific multi-lobal cross-section fibers, the degree of freedom of the fibers can be appropriately controlled by thermally bonding the fibers with the thermal adhesive component, thereby further suppressing pilling and fiber shedding when used as a wiping sheet. [Explanation of symbols]
[0135] 1: Multilobular cross-section fiber 2: Convex part Wt: Maximum width of the tip of the convex part Wb: Width of the base of the protrusion Lt: Length of the convex part
Claims
1. A nonwoven fabric used as a substrate for a wiping sheet for wiping the surface of an object, The nonwoven fabric contains 20% by weight or more of multilobal cross-section fibers, The multilobal cross-section fiber is a fiber having a fiber cross-section with a multilobal cross-sectional shape having at least three convex portions, At least one of the protrusions may have a generally curved tip portion, and a width (Wb) of a base portion toward the center of the fiber is smaller than a maximum width (Wt) of the tip portion; At least a portion of the multilobal cross-section fiber may include fibers derived from multilobal cross-section fibers formed by splitting or peeling off at least one of at least three convex portions constituting the multilobal cross-section fiber, The fibers derived from the multilobal cross section fibers may be in the form of ultrafine fibers formed by splitting or peeling off at least one of the multiple protrusions contained in the multilobal cross section fibers.
2. 2. The nonwoven fabric according to claim 1, wherein the multilobal cross section fiber has a number of protrusions in a fiber cross section of 3 to 8.
3. 2. The nonwoven fabric according to claim 1, wherein the maximum width Wt of the protrusions is 3.5 μm or more and 20 μm or less, and the length Lt of the protrusions is 4 μm or more and 25 μm or less.
4. The protrusion has a narrowed portion toward the center of the fiber, and a width (Wb) of a base portion of the protrusion is smaller than a maximum width (Wt) of the protrusion, The width Wb of the base portion of the protrusion is 2 μm or more and 12 μm or less, 2. The nonwoven fabric according to claim 1, wherein the ratio Lt / Wb of the length Lt of the protrusions to the width Wb of the base portion is 1.0 or more and 3.5 or less, and the ratio Wt / Wb of the maximum width Wt to the width Wb of the base portion is greater than 1 and less than 3.
5.
5. The multilobal cross-section fiber is a fiber made of a single resin component, The single resin component is a resin component containing 50% by mass or more of a polypropylene resin, The fineness of the multilobal cross-section fiber is 0.5 dtex or more and 10 dtex or less, The nonwoven fabric according to claim 1 , wherein the single resin component contains a hydrophilizing agent in an amount of 0.5% by mass to 10% by mass.
6. The nonwoven fabric includes, in addition to the multilobal cross-section fibers, hydrophilic fibers, and thermally bondable fibers; the nonwoven fabric contains 20% by mass or more and 80% by mass or less of fibers derived from the multilobal cross-section fibers, 10% by mass or more and 50% by mass or less of the hydrophilic fibers, and 10% by mass or more and 40% by mass or less of the thermal adhesive fibers, when the combined mass of the multilobal cross-section fibers, the hydrophilic fibers, and the thermal adhesive fibers is taken as 100% by mass; The nonwoven fabric according to claim 1 , wherein at least a portion of the intersections of the constituent fibers in the nonwoven fabric are thermally bonded by the thermally adhesive fibers.
7. The nonwoven fabric of claim 6 , wherein the hydrophilic fibers are cellulosic fibers.
8. 7. The nonwoven fabric according to claim 6, wherein the thermal adhesive fiber is a composite fiber composed of a low melting point resin component and a high melting point resin component, and the melting point of the low melting point resin component is 145°C or lower.
9. 9. The nonwoven fabric according to claim 8, wherein the thermal adhesive fiber is a core-sheath type composite fiber having a low melting point resin component as a sheath component and a high melting point resin component as a core component.
10. The nonwoven fabric according to claim 8 , wherein the low melting point resin component contained in the thermal adhesive fiber is a resin component containing 50% by mass or more of a polyethylene resin.
11. The nonwoven fabric according to claim 1 , comprising one or more fiber layers containing the multilobal cross section fibers and at least one type selected from hydrophilic fibers and thermally adhesive fibers.
12. 12. The nonwoven fabric according to claim 11, further comprising one or more fiber layers containing the multilobal cross-section fibers and at least one selected from hydrophilic fibers and thermally adhesive fibers, and further comprising one or more fiber layers having a content of the multilobal cross-section fibers of less than 20 mass%.
13. The fabric includes two fiber layers containing the multilobal cross-section fiber and at least one fiber selected from a hydrophilic fiber and a thermally adhesive fiber, A nonwoven fabric comprising one fiber layer having a multilobal cross-section fiber content of less than 20% by mass, 13. The nonwoven fabric according to claim 12, wherein a fiber layer having a content of the multilobal cross-section fibers of less than 20 mass% has a fiber layer laminated on both surfaces thereof, the fiber layer containing the multilobal cross-section fibers and at least one fiber selected from hydrophilic fibers and thermally adhesive fibers.
14. 14. The nonwoven fabric according to claim 13, wherein the fiber layer containing multilobal cross-section fibers and at least one selected from hydrophilic fibers and thermally adhesive fibers is laminated on both surfaces of a fiber layer having a multilobal cross-section fiber content of less than 20%, and the fibers contained in the fiber layer are not thermally bonded to each other.
15. 7. The nonwoven fabric according to claim 6, which is a single-layered nonwoven fabric consisting of only the multilobal cross-section fibers, the hydrophilic fibers, and the thermal adhesive fibers.
16. A wet wiping sheet using the nonwoven fabric according to any one of claims 1 to 15 as a substrate, the substrate being impregnated with a liquid in an amount ranging from 100 parts by mass to 1,000 parts by mass per 100 parts by mass of the substrate.
Citation Information
Patent Citations
Polyester fiber, having durability and excellent in water absorptivity
JP1990234914A
Fabric for wiping cloth
JP1990289220A
Wiping sheet
JP2006000625A
Wiper and method for manufacturing the same
JP2015000277A
Cited By
Modified cross-section composite fiber, method for producing same, and nonwoven fabric