Polymerizable composition and resin composition

By using drying oil homopolymers or copolymers in wet paper friction materials, flexibility and durability are improved, addressing the limitations of conventional phenolic resins to meet the demands of modern automobile engines.

JP2024147304APending Publication Date: 2024-10-16SUMITOMO BAKELITE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023060232
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-10-16

AI Technical Summary

Technical Problem

Existing wet friction materials face challenges in achieving sufficient flexibility and durability to handle the increased demands of modern automobile engines with higher rotation speeds and outputs, as conventional phenolic resins are hard and brittle, and drying oil-modified phenolic resins may not fully improve flexibility due to unbounded aliphatic hydrocarbon groups.

Method used

Employing a homopolymer or copolymer of drying oils, such as tung, perilla, linseed, or soybean oil, to enhance the flexibility and mechanical strength of wet paper friction materials, which are then impregnated into fiber bases and cured, optionally with solvents to adjust viscosity and include additives for improved properties.

Benefits of technology

The resulting wet paper friction materials exhibit enhanced flexibility, durability, and coefficient of friction, meeting the demands of high-performance automotive applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147304000001
    Figure 2024147304000001
  • Figure 2024147304000002
    Figure 2024147304000002
Patent Text Reader

Abstract

To provide a resin composition that yields a wet paper friction material with superior flexibility and durability.SOLUTION: The present invention provides a polymerizable composition including drying oil. The present invention also provides a resin composition including a homopolymer or copolymer of drying oil. The present invention further provides a resin composition including a cured product of a homopolymer or copolymer of drying oil and a phenolic resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polymerizable composition and a resin composition. More specifically, the present invention relates to a polymerizable composition and a resin composition used in the production of a wet friction material. [Background technology]

[0002] The transmission of an automatic vehicle normally incorporates a multi-plate clutch that alternates between multiple friction plates, which have a wet friction material bonded to the surface of a metal base plate (core plate), and a separator plate, which is a single metal plate or other friction mating material. These plates are pressed against each other and released in the ATF (automatic transmission fluid), which is used as a lubricant, to transmit or cut off driving force.

[0003] In recent automobile industry, various parts are being made lighter and more efficient in pursuit of energy saving and weight reduction. Meanwhile, automobile engines tend to have higher revolutions and power. In automatic transmissions, wet friction materials are required to have higher friction coefficients, heat resistance, and durability in order to meet the needs of higher revolutions and power output of automobile engines.

[0004] As wet friction materials, rubber-based friction materials and so-called paper friction materials using paper or organic fibers as a base material are used. Paper friction materials are generally manufactured by blending various friction modifiers with a base material such as natural pulp or organic synthetic fibers, obtaining paper by a wet papermaking method, and then impregnating and curing this paper with a thermosetting resin that acts as a binder such as phenolic resin. Liquid resol-type phenolic resin is generally used for wet paper friction materials. The required characteristics of the phenolic resin for wet paper friction materials are increasing year by year, and in particular, there is an increasing demand for improving the flexibility of the phenolic resin in order to improve the friction characteristics. However, while the cured product of general phenolic resin has excellent mechanical properties, it is hard and brittle, and it cannot be said that it has excellent flexibility.

[0005] In order to solve the above problems, a technique has been proposed in which a drying oil or the like is used as a modifier in the reaction for synthesizing a phenolic resin to improve flexibility (for example, Patent Document 1). Such drying oil-modified phenolic resins have a feature of being more flexible than unmodified phenolic resins because flexible aliphatic hydrocarbon groups are introduced into them. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 9-59599 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the drying oil-modified phenolic resin described in Patent Document 1 may not have sufficient flexibility improvement effect because some aliphatic hydrocarbon groups are not bonded to the phenolic structural unit. In addition, friction materials are required to have further improved friction characteristics and durability in order to respond to the recent improvement in fuel efficiency of vehicles and the increase in load on friction materials. Therefore, resins used for manufacturing friction materials are also required to have further improved mechanical strength in addition to flexibility.

[0008] The present invention has been made in view of the above problems, and provides a resin composition which can provide a wet paper friction material having excellent flexibility and durability. [Means for solving the problem]

[0009] The present inventors have discovered that by using a homopolymer or copolymer of drying oil as a thermosetting resin for friction materials, a paper friction material having an excellent coefficient of friction, high strength, and excellent flexibility can be obtained, and have thus completed the present invention.

[0010] According to the present invention, there are provided the following polymerizable composition and resin composition. [1] A polymerizable composition comprising a drying oil. [2] The polymerizable composition according to item [1], wherein the drying oil comprises at least one selected from tung oil, perilla oil, linseed oil, poppy oil, walnut oil, safflower oil, sunflower oil, castor oil, and soybean oil. [3] The polymerizable composition according to item [1] or [2], wherein the drying oil comprises tung oil. [4] A resin composition comprising a homopolymer or copolymer of a drying oil. [5] The resin composition according to item [4], further comprising a solvent. [6] The resin composition according to item [4] or [5], wherein the drying oil homopolymer or copolymer includes a homopolymer or copolymer of tung oil, perilla oil, linseed oil, poppy seed oil, walnut oil, safflower oil, sunflower oil, castor oil, or soybean oil. [7] The resin composition according to any one of items [4] to [6], wherein the drying oil homopolymer or copolymer comprises a tung oil homopolymer. [8] The resin composition according to any one of items [4] to [7], wherein the viscosity of the drying oil homopolymer or copolymer at 25°C is 0.5 Pa s or more and 50 Pa s or less. [9] The resin composition according to any one of items [4] to [8], wherein the weight average molecular weight of the homopolymer or copolymer of the drying oil is 10,000 or more and 500,000 or less.

[10] The resin composition according to any one of items [4] to [9], wherein the carbon residue rate of the homopolymer or copolymer of the drying oil measured in accordance with JIS K 6910 is 5 mass% or less.

[11] An article comprising a cured product of the resin composition according to any one of items [4] to

[10] .

[12] A wet paper friction material obtained by impregnating a fibrous base material with the resin composition described in any one of items [4] to

[10] , and then heating and curing the impregnated base material.

[13] A hardened homopolymer or copolymer of a drying oil, Phenol resin, A resin composition comprising:

[14] The resin composition according to item

[13] , wherein the cured product of the homopolymer or copolymer of the drying oil is dispersed in the phenolic resin.

[15] The resin composition according to item

[13] or

[14] , wherein the hardened homopolymer or copolymer of a drying oil is a hardened homopolymer or copolymer of tung oil, perilla oil, linseed oil, poppy seed oil, walnut oil, safflower oil, sunflower oil, castor oil, or soybean oil. Effect of the Invention

[0011] According to the present invention, there is provided a resin composition which can provide a wet paper friction material having excellent flexibility and durability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described. In this specification, the expression "a to b" in the explanation of a numerical range means "a or more and b or less" unless otherwise specified. For example, "5 to 90%" means "5% or more and 90% or less."

[0013] [Polymerizable composition] The polymerizable composition according to the first embodiment of the present invention includes a drying oil. The polymerizable composition of the present embodiment is used as a binder resin that is impregnated into a fiber base material and then cured by heat treatment in the production of a wet paper friction material, for example.

[0014] In this specification, drying oil refers to an oil or fat including an oil containing a fatty acid (palmitoleic acid, oleic acid, linoleic acid, linolenic acid, etc.) having an aliphatic hydrocarbon group having an ethylenic double bond, and having an iodine value of at least 130. Such drying oil has the property of solidifying and drying in a relatively short period of time when formed into a thin film and left in the air.

[0015] The polymerizable composition of the present embodiment can be suitably used as a material for an impregnation resin for producing a paper friction material. A wet paper friction material obtained by using the impregnation resin material obtained from such a polymerizable resin composition has high strength and desired flexibility.

[0016] Drying oils used in the polymerizable composition of the present embodiment include tung oil, perilla oil, linseed oil, poppy seed oil, walnut oil, safflower oil, sunflower oil, castor oil, and soybean oil, as well as combinations thereof. Among these, from the viewpoints of availability and price, it is preferable to use tung oil, linseed oil, castor oil, and soybean oil, and it is particularly preferable to use tung oil.

[0017] The polymerizable composition of the present embodiment is provided as a liquid composition by mixing the above-mentioned drying oil and, if necessary, a solvent.

[0018] [Resin composition] The resin composition according to the second embodiment of the present invention contains a homopolymer or copolymer of drying oil, and is preferably a liquid resin composition. In this specification, the homopolymer or copolymer of drying oil is referred to as "polymerized oil of drying oil" or simply "polymerized oil", and the resin composition according to the second embodiment is referred to as "polymerized oil-containing resin composition". The homopolymer / copolymer of drying oil (polymerized oil) plays a role as a binder resin that is impregnated into a fiber base material and then hardened by heat treatment in the production of a wet paper friction material, for example.

[0019] The drying oil used in the drying oil homopolymer or copolymer (polymerized oil) contained in the polymerized oil-containing resin composition of this embodiment is the above-mentioned drying oil used in the polymerizable composition according to the first embodiment. The drying oil homopolymer / copolymer refers to a polymer obtained by linking drying oils together through a polymerization reaction of the ethylenic double bonds contained in the aliphatic hydrocarbon groups they have. In this embodiment, the drying oil homopolymer refers to a polymer obtained by a polymerization reaction of the same type of drying oil, and the drying oil copolymer refers to a polymer obtained by a polymerization reaction of different types of drying oil.

[0020] The polymerized oil-containing resin composition of the present embodiment contains a homopolymer / copolymer of drying oil, and therefore can be suitably used as an impregnation resin for producing a paper friction material having high strength and excellent flexibility. In addition, the polymerized oil-containing resin composition of the present embodiment contains a plant-derived polymerized oil, so that the environmental load can be reduced.

[0021] In a preferred embodiment, the polymerized oil-containing resin composition comprises a homopolymer of tung oil or a copolymer of tung oil and linseed oil.

[0022] In one embodiment, the polymerized oil-containing resin composition may contain a solvent. By using a solvent, the viscosity of the obtained polymerized oil-containing resin composition can be adjusted to a level appropriate for the application to which it is used. The solvent used in the polymerized oil-containing resin composition of this embodiment is not particularly limited as long as it is a solvent in which the homopolymer / copolymer of drying oil can be dissolved or dispersed. Examples of solvents that can be used include, but are not limited to, ketone-based organic solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; alcohol-based organic solvents such as methanol, ethanol, propanol, and butanol; ether-based organic solvents such as propylene glycol methyl ether; and aromatic hydrocarbon solvents such as toluene.

[0023] The polymerized oil-containing resin composition of the present embodiment can be produced by a step of obtaining a homopolymer / copolymer of the drying oil by thermal polymerization at a temperature of, for example, 100 to 300° C., and a step of mixing the obtained homopolymer / copolymer with a solvent by a known method. From the viewpoint of handling, the polymerized oil-containing resin composition of the present embodiment is preferably provided in a liquid form.

[0024] The drying oil homopolymer / copolymer used in the polymerized oil-containing resin composition of this embodiment preferably has a weight average molecular weight of 10,000 to 500,000, more preferably 15,000 to 400,000. A drying oil homopolymer / copolymer having a weight average molecular weight in the above range is preferable because impregnated paper with excellent flexibility can be obtained when a resin composition containing the drying oil is impregnated into paper. The degree of polymerization and molecular weight of the drying oil homopolymer / copolymer can be appropriately adjusted by changing the conditions of the polymerization reaction of the drying oil (e.g., reaction temperature, reaction time).

[0025] The viscosity of the drying oil homopolymer / copolymer used in the polymerized oil-containing resin composition of this embodiment at 25°C is preferably 0.5 Pa·s or more and 50 Pa·s or less, more preferably 1 Pa·s or more and 30 Pa·s or less. A drying oil homopolymer / copolymer having a viscosity at 25°C within the above range is preferred because impregnated paper with excellent flexibility can be obtained when a resin composition containing the drying oil is impregnated into paper. The viscosity of the drying oil homopolymer / copolymer can be appropriately adjusted by changing the conditions of the polymerization reaction of the drying oil (e.g., reaction temperature, reaction time) to adjust the molecular weight.

[0026] The drying oil homopolymer / copolymer used in the polymerized oil-containing resin composition of this embodiment has a carbon residue rate of 5 mass % or less, preferably 3 mass % or less, and more preferably 1 mass % or less. The lower the carbon residue rate of the homopolymer / copolymer of drying oil, the less tar-like decomposition products are generated when exposed to a high-temperature environment. Therefore, friction materials manufactured using such homopolymer / copolymer of drying oil do not clog during use, and as a result, have excellent durability. Here, the carbon residue rate of the homopolymer / copolymer of drying oil is the carbon residue rate at a temperature of 800°C measured in accordance with JIS K6910.

[0027] When the polymerized oil-containing resin composition of the present embodiment is provided as a liquid resin containing a solvent, the drying oil homopolymer / copolymer is blended in an amount of, for example, 20% by mass to 80% by mass, preferably 25% by mass to 75% by mass, more preferably 30% by mass to 70% by mass, based on the entire resin composition. By blending the drying oil homopolymer / copolymer in the amount within the above range, the resulting resin composition has a suitable viscosity and is excellent in workability when impregnating the paper for wet friction materials.

[0028] The polymerized oil-containing resin composition of the present embodiment may further contain other additives, such as thermosetting resins such as phenolic resins and epoxy resins, elastomers, surfactants, flame retardants, antioxidants, colorants, etc., within the scope of not impairing the effects of the present invention.

[0029] (Application) The polymerized oil-containing resin composition of the present embodiment can be used as a material for producing various articles by curing.

[0030] (Wet paper friction material) The wet paper friction material of this embodiment can be manufactured using the polymerized oil-containing resin composition. Specifically, the wet paper friction material can be manufactured by impregnating the polymerized oil-containing resin composition into a fiber substrate and then curing it by heat treatment. As the fiber substrate, fibers such as natural fibers, metal fibers, carbon fibers, and chemical fibers can be used. Specifically, natural fibers such as natural pulp fibers and linter pulp; inorganic fibers such as glass fibers; carbon fibers such as polyacrylonitrile (PAN)-based carbon fibers and pitch-based carbon fibers; chemical fibers such as aramid fibers and phenol fibers can be used. These may be used alone or in combination of two or more. The form of the fiber is not particularly limited, but nonwoven fabrics, woven fabrics, etc. can be used.

[0031] The wet paper friction material obtained by using the polymerized oil-containing resin composition of the present embodiment has excellent heat resistance and durability as well as high flexibility. As a result, the wet paper friction material of the present embodiment has a high friction coefficient and therefore a high torque capacity.

[0032] [Resin composition] A resin composition according to a third embodiment of the present invention includes a cured product of a drying oil homopolymer / copolymer and a phenolic resin. In this specification, the resin composition according to the third embodiment is referred to as a "cured product-containing resin composition."

[0033] As the drying oil used in the cured product of the drying oil homopolymer / copolymer contained in the cured product-containing resin composition of this embodiment, the above-mentioned drying oil used in the polymerizable composition according to the first embodiment is used. The cured product of the drying oil homopolymer / copolymer refers to a cured product obtained by heat-treating the above-mentioned drying oil homopolymer / copolymer.

[0034] The cured product-containing resin composition of the present embodiment contains a cured product of a drying oil homopolymer / copolymer, and thus has high strength and excellent flexibility.

[0035] The phenolic resin to be blended in the cured product-containing resin composition of the present embodiment includes resol-type phenolic resin and novolac-type phenolic resin. Among them, it is preferable to use novolac-type phenolic resin. Novolac-type phenolic resin is a phenolic resin obtained by reacting phenols and aldehydes under an acid catalyst. Specific examples of novolac-type phenolic resin include phenol novolac-type resin, cresol novolac-type resin, resorcin novolac-type resin, xylenol novolac-type resin, alkylphenol novolac-type resin, naphthol novolac-type resin, bisphenol A novolac-type resin, phenol aralkyl novolac-type resin, phenol diphenyl aralkyl novolac-type resin, phenol naphthalene novolac-type resin, phenol dicyclopentadiene novolac-type resin, and novolac-type modified phenolic resin using cashew nut oil, terpene, tall oil, rosin, rubber, etc.

[0036] In a preferred embodiment, the cured product of the drying oil homopolymer / copolymer is dispersed in the phenolic resin. Here, the fact that the cured product of the drying oil homopolymer / copolymer is dispersed in the phenolic resin means that, for example, fine particles of the cured product of the drying oil homopolymer / copolymer having a particle size of about 1 μm to 30 μm are present in the phenolic resin without reacting with the phenolic resin.

[0037] In one embodiment, the amount of the cured product of the drying oil homopolymer / copolymer in the cured product-containing resin composition is from 1 mass % to 60 mass %, preferably from 5 mass % to 50 mass %, and more preferably from 10 mass % to 40 mass %, based on the total resin material.

[0038] (Method of producing cured product-containing resin composition) The cured product-containing resin composition of this embodiment can be produced by a process of heating the polymerized oil-containing resin composition according to the second embodiment to cure the homopolymer / copolymer of drying oil contained in the resin composition, and a process of mixing the obtained cured product of the homopolymer / copolymer of drying oil with a phenolic resin. Preferably, the cured product-containing resin composition of this embodiment can be produced by the steps of: mixing the polymerized oil-containing resin composition according to the second embodiment with a phenolic resin to obtain a mixture containing a drying oil homopolymer / copolymer and a phenolic resin; and heating the obtained mixture to cure the drying oil homopolymer / copolymer, thereby obtaining a resin composition in which the cured product of the drying oil homopolymer / copolymer is dispersed in the phenolic resin.

[0039] (Application) The cured product-containing resin composition of this embodiment is used as a molding material for friction materials such as brake pads, brake linings, clutch facings, etc., grinding wheels, industrial heat-resistant materials, etc. Such articles can be produced by heating the cured product-containing resin composition of this embodiment under pressure, for example, by filling it into a mold, subjecting it to heat compression molding at 130°C to 180°C and 10 to 100 MPa for 5 to 20 minutes, and then subjecting it to post-cure treatment at 160°C to 250°C as necessary.

[0040] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. EXAMPLES

[0041] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these.

[0042] [Preparation of polymerized oil] (Preparation of Polymerized Oil 1) 1000 parts by mass of tung oil was added to a reaction vessel equipped with a stirrer, reflux condenser, and thermometer, and the mixture was heated to 180°C and reacted with stirring until the viscosity reached 8 Pa s. In this way, 1000 parts by mass of tung oil polymer (polymerized oil 1) was obtained. The weight average molecular weight (Mw) of the obtained polymerized oil 1 was 46,000.

[0043] (Preparation of Polymerized Oil 2) 800 parts by weight of tung oil and 200 parts by weight of linseed oil were added to a reaction vessel equipped with a stirrer, reflux condenser, and thermometer, and the mixture was heated to 180°C and reacted with stirring until the viscosity reached 6 Pa s. In this way, 1,000 parts by weight of tung oil and linseed oil polymer (polymerized oil 2) was obtained. The weight average molecular weight (Mw) of the obtained polymerized oil 2 was 29,000.

[0044] (Preparation of Polymerized Oil 3) 500 parts by weight of tung oil and 500 parts by weight of linseed oil were added to a reaction vessel equipped with a stirrer, reflux condenser, and thermometer, and the mixture was heated to 180°C and reacted with stirring until the viscosity reached 6 Pa s. In this way, 1000 parts by weight of tung oil and linseed oil polymer (polymerized oil 3) was obtained. The weight average molecular weight (Mw) of the obtained polymerized oil 3 was 38,000.

[0045] (Preparation of Cardanol Polymer 1) 1000 parts by mass of cardanol and 20 parts by mass of paratoluenesulfonic acid were added to a reaction vessel equipped with a stirrer, a reflux condenser, and a thermometer, and the mixture was heated to 140°C and reacted with stirring for 4 hours to obtain cardanol polymer 1. 300 parts by mass of methyl ethyl ketone (MEK) was added to the mixture, which was then dissolved and cooled. In this way, 1300 parts by mass of an MEK solution of cardanol polymer 1 with a non-volatile content of 45% was obtained. The weight average molecular weight (Mw) of the obtained cardanol polymer 1 was 30,000.

[0046] (Preparation of Cardanol Polymer 2) 1000 parts by mass of cardanol and 20 parts by mass of paratoluenesulfonic acid were added to a reaction vessel equipped with a stirrer, a reflux condenser, and a thermometer, and the mixture was heated to 140°C and reacted with stirring for 3.5 hours to obtain cardanol polymer 2. 300 parts by mass of methyl ethyl ketone was added thereto, dissolved, and cooled. In this way, 1300 parts by mass of a MEK solution of cardanol polymer 2 with a non-volatile content of 45% was obtained. The weight average molecular weight (Mw) of the obtained cardanol polymer 2 was 24,000.

[0047] (Preparation of Cardanol Polymer 3) 1000 parts by mass of cardanol and 20 parts by mass of paratoluenesulfonic acid were added to a reaction vessel equipped with a stirrer, a reflux condenser, and a thermometer, and the mixture was heated to 140°C and reacted with stirring for 3 hours to obtain cardanol polymer 3. 300 parts by mass of methyl ethyl ketone was added to the mixture, dissolved, and cooled. In this manner, 1300 parts by mass of a MEK solution of cardanol polymer 3 with a non-volatile content of 45% was obtained. The weight average molecular weight (Mw) of the obtained cardanol polymer 3 was 21,000.

[0048] (Preparation of Unmodified Phenolic Resin 1) In an inverted vessel equipped with a stirrer, reflux condenser, and thermometer, 1000 parts by mass of phenol, 740 parts by mass of aqueous formalin solution (formalin content: 37% by mass) and 20 parts by mass of triethylamine were added so that the molar ratio of the phenol to the phenol was 1, and the mixture was reacted at 100°C for 30 minutes while stirring. Next, while performing dehydration under a reduced pressure of 91 kPa, when the temperature in the system reached 65°C, 1000 parts by mass of methyl ethyl ketone (MEK) was added to dissolve the reactants, and then the mixture was cooled. In this way, 2100 parts by mass of a liquid MEK solution of unmodified resol type phenolic resin 1 (non-volatile content (solid content): 45% by mass) was obtained. The resulting liquid unmodified resol type phenolic resin 1 had a weight average molecular weight (Mw) of 200 and a dispersity (Mw / Mn) of 2.5.

[0049] [Table 1]

[0050] [Measurement of physical properties of polymerized oil] The weight average molecular weight, viscosity at 25°C, and carbon residue rate of the polymerized oil, cardanol polymer, and unmodified phenolic resin obtained above were measured. Note that for cardanol polymers 1 to 3 and unmodified phenolic resin 1, the physical properties of the individual samples before adding MEK were measured. The results are shown in Table 1. (viscosity) The measurement was performed using an E-type viscometer at a liquid temperature of 25°C. (residual coal rate) The residual carbon rate of the resin was measured according to JIS K 6910.

[0051] (Examples 1 to 3, Comparative Examples 1 to 4) (Preparation of polymerized oil-containing resin composition) For each of the Examples and Comparative Examples, the components were mixed according to the blending amounts shown in Table 2 below to obtain a varnish-like resin composition with a solid content of 30 mass %.

[0052] (Production of wet paper friction material) The above resin composition was impregnated into an aramid fiber substrate having a size of 120 mm×10 mm×thickness of 1 mm, and then dried and cured in an oven at 200° C. for 30 minutes to obtain a wet friction material (impregnated paper) as a test piece.

[0053] The obtained test pieces of the wet friction material were evaluated for the following items. The results are shown in Table 2 below together with the above-mentioned blending amounts.

[0054] <Tensile elongation at break (before heat treatment)> The tensile elongation at break of the obtained test piece of the wet friction material was measured by a method conforming to JIS P 8113. The unit is %. The measurement conditions were a precision universal testing machine AG-IS 5kN (manufactured by Shimadzu Corporation) at room temperature and normal pressure, and a test speed of 1mm / min. The higher the tensile elongation at break value, the more flexible the test piece. <Tensile elongation at break (after heat treatment)> The obtained test pieces of the wet friction material were heated in an oven at 220°C for 30 minutes, and then the tensile elongation at break was measured in the same manner as that for the test pieces before heat treatment. The higher the tensile elongation at break (after heat treatment), the better the heat resistance and flexibility of the test pieces.

[0055] [Table 2]

Claims

1. A polymerizable composition comprising a drying oil.

2. 10. The polymerizable composition of claim 1, wherein the drying oil comprises at least one selected from tung oil, perilla oil, linseed oil, poppy oil, walnut oil, safflower oil, sunflower oil, castor oil, and soybean oil.

3. 10. The polymerizable composition of claim 1, wherein the drying oil comprises tung oil.

4. A resin composition comprising a homopolymer or copolymer of a drying oil.

5. The resin composition according to claim 4 , further comprising a solvent.

6. The resin composition of claim 4, wherein the drying oil homopolymer or copolymer comprises a homopolymer or copolymer of tung oil, perilla oil, linseed oil, poppy oil, walnut oil, safflower oil, sunflower oil, castor oil, or soybean oil.

7. 5. The resin composition of claim 4, wherein the drying oil homopolymer or copolymer comprises a tung oil homopolymer.

8. The resin composition according to claim 4, wherein the viscosity of the homopolymer or copolymer of the drying oil at 25°C is 0.5 Pa·s or more and 50 Pa·s or less.

9. The resin composition according to claim 4, wherein the weight average molecular weight of the homopolymer or copolymer of the drying oil is 10,000 or more and 500,000 or less.

10. The resin composition according to claim 4, wherein the homopolymer or copolymer of the drying oil has a carbon residue rate of 5 mass% or less as measured in accordance with JIS K 6910.

11. An article comprising a cured product of the resin composition according to any one of claims 4 to 10.

12. A wet paper friction material obtained by impregnating a fibrous base material with the resin composition according to any one of claims 4 to 10, and then heating and curing the impregnated base material.

13. a cured homopolymer or copolymer of a drying oil; Phenol resin, A resin composition comprising:

14. The resin composition according to claim 13, wherein the cured homopolymer or copolymer of the drying oil is dispersed in the phenolic resin.

15. The resin composition according to claim 13, wherein the hardened homopolymer or copolymer of drying oil is a hardened homopolymer or copolymer of tung oil, perilla oil, linseed oil, poppy oil, walnut oil, safflower oil, sunflower oil, castor oil, or soybean oil.

Citation Information

Patent Citations

  • Wet frictional material