Poly(METH)acrylic acid (SALT)-based water-absorbing resin
A high SAP mobility poly(meth)acrylic acid (salt)-based resin with inorganic fine particles ensures even distribution and efficient liquid absorption across the absorbent body, reducing liquid return in absorbent articles.
Patent Information
- Application Number
- JP2023060397
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
AI Technical Summary
Conventional poly(meth)acrylic acid (salt)-based water-absorbing resins used in absorbent articles like disposable diapers face challenges in efficiently absorbing liquid over the entire surface, leading to an insufficient reduction in liquid return on the absorbent surface.
A particulate poly(meth)acrylic acid (salt)-based water-absorbing resin with high SAP mobility, containing water-insoluble inorganic fine particles and specific surface area, is developed to enhance distribution and absorption efficiency, reducing liquid return by ensuring even distribution across the absorbent body.
The resin effectively absorbs liquid over the entire surface of absorbent articles, minimizing liquid return and improving the overall performance of absorbent materials.
Smart Images

Figure 2024147407000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a water-absorbing resin. More specifically, the present invention relates to a poly(meth)acrylic acid (salt)-based water-absorbing resin. [Background technology]
[0002] In recent years, water-absorbing resins have been widely used as water-absorbing agents in sanitary materials such as paper diapers, sanitary napkins, and incontinence pads from the viewpoint of absorbing body fluids. Examples of such water-absorbing resins include hydrolyzates of starch-acrylonitrile graft copolymers, neutralized products of starch-acrylic acid graft polymers, saponified products of vinyl acetate-acrylic acid ester copolymers, and crosslinked products of partially neutralized (meth)acrylic acid polymers. Among these, poly(meth)acrylic acid (salt)-based water-absorbing resins using (meth)acrylic acid and / or its salt as the main monomer component are most widely produced industrially from the viewpoint of water-absorbing performance.
[0003] As parameters indicating the desired characteristics of such poly(meth)acrylic acid (salt)-based water absorbent resins, many parameters are known, such as water absorption capacity without load (CRC), water absorption capacity under load (AAP), water absorption rate (FSR / vortex), liquid permeability without load, liquid permeability under load, impact resistance, urine resistance, fluidity, gel strength, coloring resistance, particle size, etc. Furthermore, many parameter measurement methods have been proposed from various viewpoints for the same parameter, for example, water absorption capacity without load. Water absorbent resins that have been developed with attention to these many characteristics have a problem that, even if the many characteristics (for example, "water absorption capacity without load (CRC)" and "water absorption capacity under load (AAP)" etc.) are controlled, it is still difficult to say that they exhibit sufficient performance when actually used in absorbents such as paper diapers.
[0004] Patent Document 1, for example, describes a technique for making a water-absorbent resin exhibit excellent performance even when actually used in an absorbent body such as a paper diaper. The absorbent composition solves the problem of exhibiting excellent performance such as swiftly absorbing liquid, maintaining high liquid diffusibility, and maintaining the amount of absorption per unit weight. The absorbent composition contains a water-absorbent resin that is a crosslinked polymer of a polyacrylate, and contains a predetermined amount of amorphous silicon dioxide and / or a predetermined amount of a polyamine compound with a weight-average molecular weight of 5,000 or more relative to the water-absorbent resin, and has a diffusion absorption index of 1.5 g / g min or more and a diffusion absorption index of 20 g / cm or more in a 0.9 wt % sodium chloride aqueous solution. 2 The absorbent composition has a diffusion absorption capacity of 25 g / g or more for a 0.9 wt % aqueous sodium chloride solution after 60 minutes from the start of absorption under a load of 100 g / g or more. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2010-142808 A Summary of the Invention [Problem to be solved by the invention]
[0006] The above-mentioned conventional techniques provide absorbent compositions that quickly absorb liquid and maintain high liquid diffusibility, but when used in absorbent articles such as disposable diapers that include a water-absorbent resin and a water-permeable substrate, the effects are still insufficient, and there is room for improvement, particularly in terms of reducing the amount of liquid return over the entire absorbing surface of the absorbent article.
[0007] One aspect of the present invention aims to provide a water-absorbent resin that can efficiently absorb liquid across the entire absorbent body of an absorbent article comprising a water-absorbent resin and a water-permeable substrate, thereby reducing the amount of liquid returning across the entire absorbent surface of the absorbent article. [Means for solving the problem]
[0008] One aspect of the present invention provides the following water-absorbent resin.
[0009] [1] A particulate poly(meth)acrylic acid (salt)-based water-absorbing resin, A poly(meth)acrylic acid (salt)-based water absorbent resin having a SAP mobility of 10% by mass or more, as determined by the following steps (1) to (4): (1) A nonwoven fabric cut into a rectangle measuring 4 cm x 12 cm is attached to the inclined surface of an acrylic resin inclined table with a surface inclined at 45 degrees, with its longitudinal direction perpendicular to the width direction of the inclined table. Here, the nonwoven fabric has a thickness of 3 mm and a basis weight of 41 g / m 2 It is an air-through nonwoven fabric made of a mixture of polyethylene, polypropylene and polyethylene terephthalate, the fiber diameter of the polyethylene and the fiber diameter of the polypropylene are 0.18 mm, and the fiber diameter of the polyethylene terephthalate is 0.27 mm; (2) A mark is made at a position 1 cm below the uppermost edge of the nonwoven fabric and 2 cm inside from the edge perpendicular to the uppermost edge of the nonwoven fabric, and 1.0 g of the water absorbent resin is dropped vertically upward from the mark over a period of 5 seconds from a height of 1 cm; (3) The water-absorbent resin that has moved and slid down on or within the nonwoven fabric and fallen into a tray installed at the bottom of the inclined platform is collected and its mass is measured; (4) Calculate the SAP mobility according to the following formula (1). SAP mobility [mass%] = mass of recovered water absorbent resin [g] / total mass of dropped water absorbent resin [g] × 100 Equation (1).
[0010] [2] The poly(meth)acrylic acid (salt)-based water-absorbing resin according to [1], which contains water-insoluble inorganic fine particles.
[0011] [3] The specific surface area of the water-insoluble inorganic fine particles is 100 m 2 / g or less.
[0012] [4] The poly(meth)acrylic acid (salt)-based water-absorbing resin according to any one of [1] to [3], which has a water-absorbing speed measured by a vortex method of less than 35 seconds. Effect of the Invention
[0013] According to one aspect of the present invention, it is possible to provide a water-absorbent resin that can efficiently absorb liquid across the entire absorbent body of an absorbent article comprising a water-absorbent resin and a water-permeable substrate, thereby reducing the amount of liquid returning across the entire absorbent surface of the absorbent article. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1003 is a cross-sectional view of the absorbent body for evaluation of the amount of liquid return, showing the procedure for preparing an absorbent body for evaluation. The figure shows a state in which a nonwoven fabric is placed on an adhesive tape, 1002 shows a state in which a water-absorbent resin has been sprayed onto the nonwoven fabric, as viewed from directly above. FIG. [Diagram 2] FIG. 2 is a schematic diagram of a roll-type crushing device used in the crushing step in one embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing a pair of rolls in a roll-type grinding device used in a grinding step in one embodiment of the present invention, where 2001 is a pair of rolls in which grooves are provided on the surface of both rolls, and 2002 is a pair of rolls in which grooves are provided on the surface of one roll and no grooves are provided on the surface of the other roll. [Figure 4] This is a cross-sectional view of an apparatus for evaluating SAP mobility, cut along a plane that includes the longitudinal centerline of a nonwoven fabric attached to an inclined table and is perpendicular to the horizontal plane. [Diagram 5] FIG. 2 is a perspective view showing the external configuration of a tilt table to which a nonwoven fabric is attached in a device for evaluating SAP mobility. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described below with reference to the best mode. It should be understood that the terms used in this specification are used in the sense commonly used in the art unless otherwise specified. Therefore, unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as commonly understood by those skilled in the art to which this invention belongs. In the event of a conflict, this specification (including definitions) shall prevail. The present invention is not limited to the following embodiments, and various modifications may be made within the scope of the claims.
[0016] [1] Definitions of terms (1-1) “Water-absorbing resin” The "water-absorbent resin" in the present invention refers to a water-swellable, water-insoluble polymer gelling agent that satisfies the following physical properties: "Water-swellable" refers to a polymer gelling agent that satisfies the physical properties of CRC of 5 g / g or more as specified in ERT441.2-02, and "water-insoluble" refers to a polymer gelling agent that satisfies the physical properties of Ext of 50 wt% or less as specified in ERT470.2-02.
[0017] The water-absorbing resin can be appropriately designed according to its application, and is not particularly limited, but is preferably a hydrophilic cross-linked polymer obtained by cross-linking an unsaturated monomer having a carboxyl group. The water-absorbing resin is not limited to a form in which the total amount (100% by weight) is a polymer, and may be a water-absorbing resin composition containing additives and the like within a range that satisfies the physical properties (CRC, Ext). Furthermore, the water-absorbing resin in the present invention is not limited to a final product, and may refer to an intermediate product in the manufacturing process of the water-absorbing resin (for example, a hydrogel-like cross-linked polymer after polymerization, a dried polymer after drying, a water-absorbing resin before surface cross-linking, a water-absorbing resin after surface cross-linking, a water-absorbing resin after granulation, etc.), and all of these are collectively referred to as "water-absorbing resin" together with the water-absorbing resin composition. The shape of the water-absorbing resin is not particularly limited, and examples thereof include sheet-like, fibrous, film-like, and particulate shapes, but particulate water-absorbing resins are preferred in the present invention.
[0018] (1-2) "Poly(meth)acrylic acid (salt)-based water-absorbent resin" In the present invention, the term "poly(meth)acrylic acid (salt)-based water-absorbing resin" refers to a water-absorbing resin that contains an arbitrary graft component and is mainly composed of a repeating unit derived from (meth)acrylic acid and / or a salt thereof (hereinafter referred to as "(meth)acrylic acid (salt)"). The poly(meth)acrylic acid (salt)-based water-absorbing resin is a water-absorbing resin that contains preferably 50 to 100 mol%, more preferably 70 to 100 mol%, further preferably 90 to 100 mol%, and particularly preferably substantially 100 mol% of (meth)acrylic acid (salt) relative to the total monomers (excluding crosslinking agents) used in polymerization.
[0019] (1-3) "EDANA" and "ERT" "EDANA" is an abbreviation of European Disposables and Nonwovens Associations, and "ERT" is an abbreviation of EDANA Recommended Test Methods, a European standard (almost a global standard) for measuring the properties of water-absorbent resins. In the present invention, unless otherwise specified, the physical properties of the water-absorbent resin are measured in accordance with the original ERT (revised in 2002 / publicly known document).
[0020] (1-4) “Water permeable base material” The "water-permeable substrate" in the present invention refers to a member that has a function of permeating and / or diffusing an introduced liquid and is in direct contact with a water-absorbent resin in an absorbent body used in absorbent articles such as disposable diapers. Specific examples include hydrophilic fibers (e.g., pulp fibers, etc.), hydrophilic fiber stacks, hydrophilic nonwoven fabrics containing hydrophilic fibers as constituent fibers, and nonwoven fabrics containing synthetic fibers as constituent fibers.
[0021] (1-5)Other In this specification, the range "X to Y" means "X or more and Y or less". In this specification, "weight" and "mass", "weight %" and "mass %, "parts by weight" and "parts by mass" are treated as synonyms. In this specification, unless otherwise specified, "ppm" means "ppm by mass". In this specification, "acid (salt)" means "acid and / or its salt", and "(meth)acrylic" means "acrylic and / or methacrylic". In this specification, the unit of volume "liter" may be written as "l" or "L".
[0022] [2] Water-absorbing resin (2-1)SAP mobility The present inventors have found that, in an absorbent article comprising a water-absorbent resin and a water-permeable substrate, by using a water-absorbent resin that is easily movable between or on the fibers of the water-permeable substrate, the water-absorbent resin can be distributed over the entire absorbent body, and the amount of liquid returning over the entire absorbing surface can be reduced, and have completed the present invention. In the present invention, the "SAP mobility" of a water-absorbent resin means the ratio of the mass of the water-absorbent resin that slides down to the bottom of the inclined platform to the total mass of the water-absorbent resin dropped when the water-absorbent resin (SAP / Super Absorbent polymer) is dropped from near the upper end of a water-permeable substrate placed on the inclined platform having a surface inclined at 45 degrees. Specifically, the SAP mobility is calculated by the following formula (1) using the measured value measured by the method described in the Examples. SAP mobility [mass%] = mass of recovered water absorbent resin [g] / total mass of dropped water absorbent resin [g] × 100 Equation (1) The SAP mobility of the water-absorbent resin according to one embodiment of the present invention is preferably 10% by mass or more, more preferably 12% by mass or more, and even more preferably 14% by mass or more. The upper limit of the SAP mobility is not particularly limited, but is preferably 50% by mass or less, and even more preferably 30% by mass or less. If the SAP mobility of the water-absorbent resin is 10% by mass or more, when the water-absorbent resin is used in an absorbent article comprising a water-absorbent resin and a water-permeable substrate, the water-absorbent resin can be distributed evenly over the entire surface of the absorbent body because the water-absorbent resin is easily moved between or on the fibers of the water-permeable substrate. Therefore, the liquid is efficiently absorbed over the entire surface of the absorbent body, so that the amount of liquid returning over the entire absorption surface can be reduced. On the other hand, when the water-absorbent resin is not evenly distributed over the entire surface of the absorbent body (when segregated), the liquid present in the part where the water-absorbent resin is not present returns, so that the amount of liquid returning increases. In addition, if the SAP mobility of the water-absorbent resin is 50% by mass or less, the yield is excellent during the production of an absorbent article comprising a water-absorbent resin and a water-permeable substrate, so that it is preferable.
[0023] Specifically, in the manufacturing process of absorbent articles, if the water-absorbent resin can be uniformly sprayed on a water-permeable substrate, the water-absorbent resin is sandwiched by a top sheet or wrapped by a core wrap sheet in a subsequent process, and the distribution state of the water-absorbent resin is fixed and maintained uniform. On the other hand, when segregation occurs in the spraying process of the water-absorbent resin, the non-uniform distribution state cannot be eliminated with a conventional water-absorbent resin, but with the water-absorbent resin of the present invention, which has a significantly high SAP mobility, it is possible to uniformly disperse the water-absorbent resin on the water-permeable substrate by performing an operation such as applying vibration before being fixed by a top sheet or a core wrap sheet.
[0024] (2-2) Shape of water-absorbent resin In one embodiment of the present invention, the shape of the water-absorbent resin is preferably particulate, and specific examples thereof include irregularly pulverized particles, spherical particles, football-shaped particles, aggregate particles, and granulated particles. Here, the spherical shape is not limited to a perfect sphere, and includes substantially spherical particles with an aspect ratio of 1.0 to 1.2. Among these, spherical particles, spherical aggregate particles, and spherical granulated particles are more preferable from the viewpoint of easy movement between or on the fibers of the water-permeable substrate.
[0025] (2-3) Additives In one embodiment of the present invention, the water-absorbent resin may contain additives to exhibit various functions. Examples of the additives include surfactants, compounds having phosphorus atoms, oxidizing agents, organic reducing agents, water-insoluble inorganic fine particles, organic powders (e.g., metal soaps, etc.), deodorants, antibacterial agents, pulp, thermoplastic fibers, etc.
[0026] Examples of the water-insoluble inorganic fine particles include silicic acid (salt) such as natural zeolite or synthetic zeolite; kaolin; talc; clay; bentonite; calcium phosphate; barium phosphate; silicic acid or its salt; clay; diatomaceous earth; silica gel; zeolite; hydroxyapatite; hydrotalcite; vermiculite; perlite; isolite; activated clay; quartz sand; silica stone; strontium ore; fluorite; bauxite; metal oxides such as silica (silicon dioxide) and titanium oxide; composite hydrated oxides containing zinc and silicon, or zinc and aluminum (for example, as exemplified in International Publication No. 2005 / 010102). The water-absorbent resin according to one embodiment of the present invention more preferably contains, among these water-insoluble inorganic fine particles, hydrotalcite; clay minerals such as kaolin, talc, and zeolite; calcium phosphate; barium phosphate; silicic acid (salt); and the like. When the hydrogen-absorbing resin containing these water-insoluble inorganic fine particles is used in an absorbent article, friction between the water-absorbent resin particles and the water-permeable substrate can be reduced to improve the slipperiness, and therefore the water-absorbent resin can easily move on or between the fibers of the water-permeable substrate, which is preferable.
[0027] The content of the water-insoluble inorganic fine particles is preferably 0.01 to 5.00 parts by weight, more preferably 0.05 to 3.00 parts by weight, further preferably 0.10 to 1.00 parts by weight, and particularly preferably 0.20 to 0.50 parts by weight, relative to 100 parts by weight of the water absorbent resin, from the viewpoint of reducing friction occurring between the water absorbent resin and the water-permeable substrate.
[0028] The water-insoluble inorganic fine particles have a size smaller than that of the water-absorbent resin particles. The average particle size of the water-insoluble inorganic fine particles is preferably 0.01 to 50.00 μm, and may be 0.10 to 30.00 μm, or 1.00 to 20.00 μm. Here, the average particle size can be measured by a pore electrical resistance method or a laser diffraction / scattering method depending on the characteristics of the particles.
[0029] The specific surface area of the water-insoluble inorganic fine particles is preferably 100 m 2 / g, more preferably less than 95m 2 / g, and more preferably less than 90m 2 / g, less than 80m 2 / g, and particularly preferably less than 50m 2 The lower limit of the specific surface area of the water-insoluble inorganic fine particles is not particularly limited, but is preferably less than 0.1 m 2 / g or more, more preferably 1.0m 2 The specific surface area can be measured by the BET method. 2 If the molecular weight is less than 1 / g, the friction generated between the water-absorbent resin and the water-permeable substrate can be reduced, which is preferable.
[0030] (2-4)CRC "CRC" is an abbreviation for Centrifuge Retention Capacity, and means the water absorption capacity of a water-absorbent resin under no pressure. In this specification, CRC is measured in accordance with the EDANA method (ERT441.2-02).
[0031] From the viewpoint of water absorption properties when used in sanitary materials, the CRC of the water absorbent resin according to one embodiment of the present invention is preferably 15 g / g or more, more preferably 20 g / g or more, and even more preferably 25 g / g or more. The upper limit of the CRC of the water absorbent resin is not particularly limited, but is preferably 50 g / g or less.
[0032] (2-5)Ext "Ext" is an abbreviation for Extractables, and means the amount of extractables extracted from a water-absorbent resin. In this specification, Ext is measured in accordance with the EDANA method (ERT470.2-02).
[0033] (2-6) AAP "AAP" is an abbreviation of Absorption Against Pressure, and means the water absorption capacity of a water absorbent resin under pressure. In the present invention, AAP is measured in accordance with the EDANA method (ERT442.2-02) except that the load condition is changed to 4.83 kPa (0.7 psi). Specifically, 0.9 g of a water absorbent resin is swollen under a pressure of 4.83 kPa for 1 hour using a 0.9 mass% sodium chloride aqueous solution, and then AAP (water absorption capacity against pressure) (unit: g / g) is measured.
[0034] The AAP of the water-absorbent resin according to one embodiment of the present invention is preferably 15 g / g or more, more preferably 18 g / g or more, and even more preferably 20 g / g or more, from the viewpoint of water absorption properties when used in sanitary materials. The upper limit of the AAP of the water-absorbent resin is not particularly limited, but is preferably 40 g / g or less.
[0035] (2-7) Moisture content "Moisture content" is measured in accordance with the EDANA method (ERT430.2-02), except that the sample amount is changed to 1.0 g and the drying temperature is changed to 180°C.
[0036] (2-8) Mass average particle diameter (D50) The "mass-average particle diameter (D50)" is measured in accordance with "(3) Mass-Average Particle Diameter (D50) and Logarithmic Standard Deviation (σζ) of Particle Diameter Distribution" described in columns 27 and 28 of U.S. Pat. No. 7,638,570.
[0037] The mass average particle diameter (D50) of the water-absorbent resin according to one embodiment of the present invention is preferably 250 μm to 800 μm, more preferably 300 μm to 700 μm, even more preferably 310 μm to 600 μm, and particularly preferably 320 μm to 500 μm, from the viewpoint that the water-absorbent resin is easily moved between or on the fibers of the water-permeable substrate in the absorbent article. The ratio of particles having a particle diameter of less than 150 μm, that is, the ratio of particles passing through a JIS standard sieve with an opening of 150 μm, is preferably 40 mass% or less, more preferably 30 mass% or less, even more preferably 20 mass% or less, and particularly preferably 10 mass% or less, from the viewpoint that it is preferable that the fine particles adhering to and remaining between or on the fibers of the water-permeable substrate in the absorbent article are small. If the mass average particle diameter is 250 μm or more, there is an advantage that the water-absorbent resin is easily moved between or on the fibers of the water-permeable substrate in the absorbent article, and further, there is little dust and the handling is good. Furthermore, if the mass average particle size is 800 μm or less, a decrease in the rate at which the particle absorbs body fluids (eg, urine, blood, etc.) is prevented, making the particle suitable for use in paper diapers and the like having a high water absorption rate.
[0038] (2-9) Bulk density "Bulk density" is measured in accordance with the EDANA method (ERT460.2-02).
[0039] The water-absorbent resin according to one embodiment of the present invention has a bulk density of preferably 0.60 g / mL to 1.00 g / mL, more preferably 0.62 g / mL to 0.90 g / mL, and further preferably 0.64 g / mL to 0.80 g / mL. If the bulk density is 0.60 to 1.00 g / mL, a decrease in the absorption rate of body fluids (e.g., urine, blood, etc.) in the water-absorbent resin is prevented, and the water-absorbent resin is suitable for use in paper diapers with a high water absorption rate.
[0040] (2-10) Water absorption rate In the present invention, the "water absorption rate" of the water absorbent resin means the "water absorption rate by the Vortex method." The "water absorption rate by the Vortex method" means the time required for the stirrer tip to be covered with the test liquid when 2.0 g of the water absorbent resin is added to 50 g of a 0.9% by mass aqueous sodium chloride solution stirred at 600 rpm with a stirrer tip.
[0041] A water-absorbent resin having excellent "water-absorption speed" is preferable because it can instantly absorb liquid and reduce the amount of liquid returning when used as an absorbent article. The water-absorbent resin according to one embodiment of the present invention has a water-absorption speed of preferably less than 45 seconds, more preferably less than 40 seconds, even more preferably less than 35 seconds, and particularly preferably less than 30 seconds. The lower limit of the absorption speed is not particularly limited, but may be 10 seconds or more, 15 seconds or more, or 20 seconds or more. If the absorption speed of the water-absorbent resin is less than 45 seconds, it can quickly absorb the liquid diffused by the water-permeable substrate, and therefore has excellent liquid retention properties and is suitable for use in paper diapers with high water-absorption speed.
[0042] The present inventors have found that, in an absorbent article comprising a water-absorbent resin and a water-permeable substrate, by using a water-absorbent resin having a predetermined SAP mobility, the water-absorbent resin can be distributed over the entire absorbent body, and the amount of liquid return over the entire absorbent surface can be reduced, and further, that when a water-absorbent resin having a superior water absorption speed is used, even if the water-absorbent resin has the same degree of SAP mobility, the amount of liquid return over the entire absorbent surface can be further reduced. In particular, if the absorption speed of the water-absorbent resin is less than 35 seconds, the amount of liquid return over the entire absorbent surface can be further reduced, which is preferable.
[0043] [3] Method for producing water-absorbent resin The process for producing the water-absorbent resin according to one embodiment of the present invention will be described below.
[0044] (3-1) Monomer aqueous solution preparation process This step is a step of preparing an aqueous solution containing (meth)acrylic acid (salt) as a main component (hereinafter referred to as "aqueous monomer solution"). Note that, although a slurry liquid of a monomer can be used within a range in which the water absorption performance of the obtained water absorbent resin is not deteriorated, for the sake of convenience, the aqueous monomer solution will be described in this section.
[0045] The "main component" means that the amount (content) of (meth)acrylic acid (salt) used is preferably 50 mol % or more, more preferably 70 mol % or more, and further preferably 90 mol % or more (upper limit: 100 mol %), based on the total monomers (excluding the internal crosslinking agent) used in the polymerization reaction of the water absorbent resin.
[0046] ((Meth)acrylic acid (salt)) In the method for producing a water-absorbent resin according to one embodiment of the present invention, from the viewpoints of the physical properties and productivity of the resulting water-absorbent resin, a (meth)acrylic acid (salt) is used as a monomer.
[0047] The "(meth)acrylic acid" may be any known (meth)acrylic acid, and may contain, as a polymerization inhibitor, preferably methoxyphenols, more preferably p-methoxyphenol, preferably at 200 ppm or less, more preferably 10 to 160 ppm, and even more preferably 20 to 100 ppm, from the viewpoint of the polymerizability of (meth)acrylic acid and the color tone of the water-absorbing resin. In addition, as for impurities in (meth)acrylic acid, the compounds described in U.S. Patent Application Publication No. 2008 / 0161512 are also applicable to the present invention.
[0048] The "(meth)acrylic acid salt" is a neutralized product obtained by neutralizing the (meth)acrylic acid with the following basic composition. As the (meth)acrylic acid salt, a commercially available (meth)acrylic acid salt (e.g., sodium (meth)acrylate, etc.) may be used, or a salt obtained by neutralization in a water absorbent resin manufacturing plant may be used.
[0049] (Basic Composition) In one embodiment of the present invention, the term "basic composition" refers to a composition containing a basic compound. Examples of basic compositions include commercially available aqueous sodium hydroxide solutions.
[0050] Specific examples of the basic compound include carbonates and hydrogen carbonates of alkali metals, hydroxides of alkali metals, ammonia, organic amines, etc. Among these, from the viewpoint of the physical properties of the resulting water absorbent resin, it is preferable that the basic compound is strongly basic. That is, it is preferable to use hydroxides of alkali metals (sodium hydroxide, potassium hydroxide, lithium hydroxide, etc.), and more preferable to use sodium hydroxide.
[0051] (neutralization) In one embodiment of the present invention, the neutralization can be selected from or used in combination with neutralization of (meth)acrylic acid (before polymerization) and neutralization of a hydrogel crosslinked polymer obtained by crosslinking and polymerizing (meth)acrylic acid (after polymerization) (hereinafter referred to as "post-neutralization"). These neutralization methods may be continuous or batch-wise, and are not particularly limited, but the continuous method is preferred from the viewpoint of production efficiency, etc.
[0052] Regarding the conditions such as the neutralization apparatus, neutralization temperature, and residence time, the conditions described in WO 2009 / 123197 and US Patent Application Publication No. 2008 / 0194863 are applied.
[0053] In one embodiment of the present invention, the neutralization rate is preferably 10 to 90 mol%, more preferably 40 to 85 mol%, further preferably 50 to 80 mol%, and particularly preferably 60 to 75 mol% based on the acid group of the monomer. If the neutralization rate is less than 10 mol%, the water absorption capacity may be significantly reduced. On the other hand, if the neutralization rate is more than 90 mol%, a water absorbent resin having a high water absorption capacity under pressure may not be obtained.
[0054] The neutralization rate is the same whether it is neutralized before or after polymerization. The neutralization rate of the water absorbent resin as a final product is also applied to the neutralization rate. Note that a neutralization rate of 75 mol% means a mixture of 25 mol% (meth)acrylic acid and 75 mol% (meth)acrylic acid salt. The mixture may also be referred to as a partially neutralized product of (meth)acrylic acid.
[0055] (Other monomers) In the present specification, the term "other monomer" refers to a monomer other than the (meth)acrylic acid (salt). The other monomer can be used in combination with the (meth)acrylic acid (salt) to produce a water-absorbing resin.
[0056] The other monomer may be a water-soluble unsaturated monomer or a hydrophobic unsaturated monomer. Specifically, the compounds described in U.S. Patent Application Publication No. 2005 / 0215734 (excluding (meth)acrylic acid) are also applicable to the present invention.
[0057] (Internal crosslinking agent) Examples of the internal crosslinking agent used in the present invention include N,N'-methylenebis(meth)acrylamide, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane di(meth)acrylate, glycerin tri(meth)acrylate, glycerin acrylate methacrylate, ethylene oxide modified trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, and the like. Examples of the internal crosslinking agent include hexa(meth)acrylate, triallyl cyanurate, triallyl isocyanurate, triallyl phosphate, triallylamine, poly(meth)allyloxyalkane, (poly)ethylene glycol diglycidyl ether, glycerol diglycidyl ether, ethylene glycol, polyethylene glycol, propylene glycol, glycerin, 1,4-butanediol, pentaerythritol, ethylenediamine, ethylene carbonate, propylene carbonate, polyethyleneimine, glycidyl (meth)acrylate, etc. From the viewpoint of reactivity, one or more types of the internal crosslinking agent can be selected.
[0058] From the viewpoint of the water absorption performance of the obtained water absorbent resin, the internal crosslinking agent is preferably a compound having two or more polymerizable unsaturated groups, more preferably a compound having two or more polymerizable unsaturated groups that are thermally decomposable at a drying temperature described later, and further preferably a compound having two or more polymerizable unsaturated groups that have a (poly)alkylene glycol structural unit.
[0059] The polymerizable unsaturated group is preferably an allyl group or a (meth)acrylate group. Among these, from the viewpoint of water absorption performance, a (meth)acrylate group is more preferable. The (poly)alkylene glycol structural unit is preferably a polyethylene glycol from the viewpoint of water absorption performance. The number n of the (poly)alkylene glycol structural unit is preferably 1 to 100, more preferably 6 to 50.
[0060] The amount of the internal crosslinking agent used is preferably 0.0001 to 10 mol%, more preferably 0.001 to 1 mol%, based on the total amount of monomers. By setting the amount used within the above range, a desired water absorbent resin can be obtained. When the amount used is 0.0001 mol% or more, the gel strength tends to increase and the water-soluble content tends to decrease, and when the amount used is 10 mol% or less, the water absorption capacity tends to increase, which is preferable.
[0061] In one embodiment of the present invention, the method of adding the internal crosslinking agent is not particularly limited, but includes a method of adding the internal crosslinking agent to a monomer aqueous solution in advance and causing a crosslinking reaction simultaneously with polymerization, a method of adding an internal crosslinking agent during or after polymerization and causing post-crosslinking, a method of radical crosslinking using a radical polymerization initiator, and a method of radiation crosslinking using active energy rays such as electron beams and ultraviolet rays. Among these, from the viewpoint of reactivity, a method of adding the internal crosslinking agent to a monomer aqueous solution in advance and causing a crosslinking reaction simultaneously with polymerization is preferred. The above methods may be used in combination as appropriate within a range that does not impair the effects of the present invention.
[0062] (Other substances added to the monomer aqueous solution) In one embodiment of the present invention, from the viewpoint of improving the physical properties of the resulting water-absorbent resin, the following substances may be added during preparation of the aqueous monomer solution.
[0063] Specifically, hydrophilic polymers such as starch, starch derivatives, cellulose, cellulose derivatives, polyvinyl alcohol, poly(meth)acrylic acid (salt), and crosslinked poly(meth)acrylic acid (salt) may be added in an amount of preferably 50% by weight or less, more preferably 20% by weight or less, even more preferably 10% by weight or less, and particularly preferably 5% by weight or less (the lower limit is 0% by weight) based on the total monomers used in the polymerization (excluding the crosslinking agent).
[0064] Furthermore, foaming agents such as carbonates, azo compounds, and bubbles, surfactants, chelating agents, chain transfer agents, etc. may be added in an amount of preferably 5% by weight or less, more preferably 1% by weight or less, and even more preferably 0.5% by weight or less (the lower limit is 0% by weight) based on the total monomers used in the polymerization (excluding the crosslinking agent).
[0065] The substance may be added to the aqueous monomer solution or during the polymerization. The above-mentioned adding forms may be used in combination as appropriate within the scope of not impairing the effects of the present invention.
[0066] When a water-soluble resin or a water-absorbent resin is used as the hydrophilic polymer, a graft polymer or a water-absorbent resin composition (e.g., a starch-acrylic acid polymer, a PVA-acrylic acid polymer, etc.) is obtained. These polymers and water-absorbent resin compositions are also included in the category of the water-absorbent resin of the present invention.
[0067] (Monomer component concentration) In this step, when preparing the aqueous monomer solution, the above-mentioned substances are added. The concentration of the monomer component in the aqueous monomer solution is not particularly limited, but is preferably 10 to 80% by weight, more preferably 20 to 75% by weight, and further preferably 30 to 70% by weight, from the viewpoint of the physical properties of the water absorbent resin.
[0068] When aqueous solution polymerization or reversed-phase suspension polymerization is employed, a solvent other than water can be used in combination as necessary. In this case, the type of the solvent is not particularly limited.
[0069] The "concentration of the monomer component" is a value calculated by the following formula (2), and the weight of the aqueous monomer solution does not include the weight of a graft component of a hydrophilic polymer (e.g., starch, etc.), fine powder of a water absorbent resin generated from a production process and added for reuse, and the weight of a hydrophobic solvent in reversed-phase suspension polymerization.
[0070] Monomer component concentration (weight%) = {(weight of monomer component) / (weight of monomer aqueous solution)} × 100... Equation (2).
[0071] (3-2) Polymerization process This step is a step of polymerizing the aqueous monomer solution obtained in the aqueous monomer solution preparation step to obtain a hydrous gel crosslinked polymer (hereinafter referred to as "hydrous gel").
[0072] (Polymerization initiator) The polymerization initiator used in one embodiment of the present invention is not particularly limited since it is appropriately selected depending on the polymerization form, etc., but examples thereof include a thermally decomposable polymerization initiator, a photodecomposable polymerization initiator, or a redox-based polymerization initiator used in combination with a reducing agent that promotes the decomposition of these polymerization initiators. Specifically, one or more of the polymerization initiators disclosed in U.S. Pat. No. 7,265,190 are used. From the viewpoint of the handling of the polymerization initiator and the physical properties of the water-absorbing resin, preferably a peroxide or an azo compound, more preferably a peroxide, and even more preferably a persulfate is used.
[0073] The amount of the polymerization initiator used is preferably 0.001 to 1 mol %, more preferably 0.001 to 0.5 mol %, based on the total monomers used in the polymerization (excluding the crosslinking agent), and the amount of the reducing agent used is preferably 0.0001 to 0.02 mol %, based on the total monomers used in the polymerization (excluding the crosslinking agent).
[0074] Instead of the polymerization initiator, the polymerization reaction may be carried out by irradiation with active energy rays such as radiation, electron beams, and ultraviolet rays, and these active energy rays may be used in combination with the polymerization initiator.
[0075] (polymerization form) The polymerization form applied in one embodiment of the present invention is not particularly limited, but examples thereof include aqueous solution polymerization, reversed-phase suspension polymerization, droplet polymerization, bulk polymerization, precipitation polymerization, etc. Among these, aqueous solution polymerization or reversed-phase suspension polymerization is preferred from the viewpoints of ensuring good water absorption properties and easiness of polymerization control.
[0076] When reversed-phase suspension polymerization is used, particles with high sphericity can be produced, so that a water-absorbent resin that easily moves between or on the fibers of a water-permeable substrate can be suitably produced. In addition, the water-absorbent resin produced by aqueous solution polymerization tends to have an irregular shape, but in the subsequent process, the corners can be removed by polishing to make the particles smooth on the surface, so that a water-absorbent resin that has a small frictional force with the water-permeable substrate and easily moves between or on the fibers can be suitably produced.
[0077] (3-3) Gel crushing process This step is a step of gel-crushing the hydrogel obtained in the polymerization step with a gel crusher (e.g., a screw extruder such as a kneader or meat chopper, a cutter mill, etc.) to obtain a particulate hydrogel (hereinafter referred to as a "particulate hydrogel"). When the polymerization step is kneader polymerization, the polymerization step and the gel-crushing step are carried out simultaneously. When a particulate hydrogel is obtained directly in the polymerization process, such as droplet polymerization or reversed-phase suspension polymerization, the gel-crushing step may not be carried out.
[0078] As for the gel crushing conditions and forms other than those described above, the contents disclosed in WO 2011 / 126079 are preferably applied to the present invention.
[0079] (3-4) Drying process This step is a step of drying the particulate hydrogel obtained in the polymerization step and / or gel crushing step to a desired resin solid content to obtain a dry polymer. The resin solid content is determined from the loss on drying (weight change when 1 g of the water-absorbent resin is heated at 180°C for 3 hours), and is preferably 80% by weight or more, more preferably 85 to 99% by weight, and even more preferably 90 to 98% by weight.
[0080] The method for drying the particulate hydrogel is not particularly limited, and examples thereof include heat drying, hot air drying, reduced pressure drying, fluidized bed drying, stirring drying, infrared drying, microwave drying, drum dryer drying, azeotropic dehydration with a hydrophobic organic solvent, high humidity drying using high temperature water vapor, etc. Among these, stirring drying is preferred from the viewpoints of drying efficiency and shape retention.
[0081] (3-5) Crushing process The pulverization step is a step in which the particulate dried polymer obtained through the drying step is pulverized to adjust the particle size and shape to a desired value.
[0082] In one embodiment of the present invention, it is important to precisely control the grinding conditions in this grinding step.
[0083] (Crushing device) As the pulverizing device used in this step, various pulverizing devices can be mentioned, but in one embodiment of the present invention, it is preferable to use a specific roll-type pulverizing device because it is easy to adjust the particulate dry polymer to an optimal shape. As the specific roll-type pulverizing device, for example, a roll-type pulverizing device consisting of a pair of rolls, at least one of the pair of rolls has a groove (longitudinal groove) extending parallel to the roll rotation direction on the surface, is used. By passing the particulate dry polymer through the clearance between the pair of rolls provided in this specific roll-type pulverizing device, the particulate dry polymer is compressed, sheared or compacted between the rolls, and the particulate dry polymer is pulverized. As such a specific roll-type pulverizing device, for example, a roll granulator (manufactured by Nippon Granulator Co., Ltd.), a roll granulator (manufactured by Kurimoto Iron Works Co., Ltd.), a GRAN-U-LIZER (manufactured by MPE Co., Ltd.), etc. can be mentioned. If this specific roll-type pulverizing device is used, the pulverizing force is mild, so that the water absorbent resin is prevented from being crushed, and a pulverized product with a rounded and high sphericity can be obtained. Furthermore, generation of fine powder is also suppressed. Therefore, a water-absorbent resin that easily moves between or on the fibers of a water-permeable substrate can be suitably produced.
[0084] On the other hand, in the pair of rolls, rolls having no grooves on the surface of either roll, or rolls having grooves extending perpendicularly to the direction of roll rotation, are not preferred because they are subject to severe damage and produce a large amount of non-rounded crushed material and fine powder.
[0085] FIG. 2 shows a schematic diagram of the specific roll-type grinding device used in the grinding step in one embodiment of the present invention. As shown in FIG. 2, the roll-type grinding device 200 includes a pipe 201 for supplying a particulate dried polymer to the device 200, an inlet 202 for supplying the dried polymer into the device 200, and a pair of rolls 203 for grinding the supplied dried polymer. These are arranged in this order in a direction from top to bottom. The "direction from top to bottom" is not limited to the vertical direction, but is a concept that may also include an oblique direction. The pair of rolls 203 is composed of two rolls 203a and 203b. In the roll-type grinding device, at least one pair (two rolls) of rolls may be provided, and for example, two pairs (four rolls) or more of rolls may be provided in a vertical arrangement. For example, when two pairs of rolls are arranged in a vertical arrangement, the dried polymer passes between the pair of rolls located at the top and is ground, and then passes between the pair of rolls located at the bottom and is ground.
[0086] The dried polymer 20a introduced between the rolls 203 passes between the rolls 203a and 203b of the pair of rolls 203, and becomes the water absorbent resin 20b which is a pulverized product of the dried polymer. Although not shown, the roll-type pulverizing device 200 may be provided with a feeder between the introduction port 202 and the pair of rolls 203 for quantitative supply.
[0087] The specific roll-type grinding device has grooves (uneven pattern) on the surface of at least one of the pair of rolls. The groove means unevenness on the roll surface, and in the present invention, means grooves arranged in a striped pattern. The grooves are arranged in a plurality of rows in the roll width direction (the direction of the rotation axis of the roll). That is, in the roll-type grinding device, a plurality of grooves (vertical grooves) extending parallel to the roll rotation direction are arranged in the roll width direction on the surface of at least one of the pair of rolls. Therefore, unevenness (concave and convex portions) is formed on the roll surface extending parallel to the roll rotation direction. As a result, the clearance between the pair of rolls does not substantially change due to the rotation of the rolls at any position in the roll width direction. Since the clearance between the rolls does not change at any position in the roll width direction, it is possible to apply an appropriate force to the dried polymer passing between the rolls, and it is presumed that the particle size of the resulting pulverized product is uniform and a pulverized product having a sharp particle size distribution is obtained. The clearance between the rolls means the distance between a pair of opposing rolls.
[0088] In a preferred embodiment of the manufacturing method of the present invention, grooves are provided on each of the two roll surfaces of the pair of rolls. In this case, it is believed that the clearance between the rolls can be made constant at any position in the roll width direction by meshing the corresponding concaves and convexes provided on the roll surfaces of the two rolls, and thus a constant force can be applied to the dried material being pulverized. Therefore, it is presumed that, particularly in the pulverization of spherical particles, the particle size of the pulverized product obtained is more uniform, and a pulverized product having a sharper particle size distribution can be obtained. The pair of rolls may be the same shape (groove shape, diameter) or different shapes, but it is preferable to use rolls of the same shape (including symmetrical relationship).
[0089] For example, in one embodiment, the roll type crushing device 200 has grooves (concave and convex) extending parallel to the roll rotation direction on the roll surface of both of the pair of rolls 203. That is, as shown in 2001 in FIG. 3, both of the pair of rolls 203 (rolls 203a, 203b) have concave and convex portions extending parallel to the roll rotation direction of the roll rotation axis A on their roll surfaces. Thus, the convex portions provided on one roll surface of the pair of rolls are configured to mesh with the concave portions provided on the other roll surface of the pair of rolls by rotation.
[0090] In one embodiment, as shown in 2002 in FIG. 3, one of the pair of rolls 203 (e.g., roll 203a) has grooves on the roll surface that extend parallel to the roll rotation direction of the roll rotation axis A of the roll, and the other of the pair of rolls (e.g., roll 203b) has a smooth surface (flat surface) without grooves on the roll surface.
[0091] Here, the clearance between the rolls will be described based on 2001 in FIG. 3 and 2002 in FIG. 3. As shown in 2001 in FIG. 3, when grooves are provided on the surfaces of the two rolls 203a and 203b, the clearance d has a constant value d at any position in the roll width direction. Also, as shown in 2002 in FIG. 3, when grooves are provided on the surface of one roll 203a and no grooves are provided on the surface of the other roll 203b, the clearance d has a maximum value (dmax) and a minimum value (dmin) depending on the position in the roll width direction. In both of the forms 2001 in FIG. 3 and 2002 in FIG. 3, the grooves provided on the rolls are formed to extend parallel to the roll rotation direction, so that the clearance does not substantially change with the rotation of the rolls.
[0092] In addition, in the longitudinal groove structure, due to circumstances in the manufacture of the roll, transverse grooves (grooves extending in the roll width direction) or convex portions extending in the roll width direction may be formed in a part of the roll. Such grooves or convex portions cause cutouts in some of the longitudinal grooves of the roll. In this case, the presence of some cutouts formed in the longitudinal grooves of the roll causes a change in the clearance at any position in the roll width direction. Here, "not substantially changing with the rotation of the roll" includes "not changing the clearance over a length range of 70% or more of one rotation of the roll, preferably over a length range of 80% or more, more preferably over a length range of 90% or more, and even more preferably over a length range of 95% or more." Therefore, even if a cutout portion exists in a part of the longitudinal grooves of the roll, it is considered to be "not substantially changing with the rotation of the roll" if the above-mentioned provision is satisfied.
[0093] Here, in the embodiment of 2001 in Fig. 3, the clearance d is the same at any position in the roll width direction, whereas in the embodiment of 2002 in Fig. 3, the clearance d differs depending on the position in the roll width direction. In the present invention, even if the clearance d differs depending on the position in the roll width direction, it is sufficient that the clearance d does not substantially change at any position due to the rotation of the roll.
[0094] In the rolls shown in 2001 and 2002 in Fig. 3, the grooves are provided in a shape that extends substantially parallel (0 degrees) to the roll rotation direction. "Substantially parallel" means that grooves inclined at less than ±1° to the roll rotation direction are included in the configuration of the present invention. The inclination angle may be either in the positive or negative direction with respect to the roll rotation direction.
[0095] The minimum clearance value dmin between the rolls can be appropriately determined, and is not particularly limited, but is preferably more than 0 and 3 mm or less. The minimum clearance value dmin between the rolls is more preferably 0.05 to 3 mm, even more preferably 0.05 to 2.5 mm, even more preferably 0.1 to 2 mm, particularly preferably 0.1 to 1.5 mm, and most preferably 0.2 to 1 mm. By arranging a pair of rolls so that the minimum clearance value dmin between the rolls is within the above range, the effect of reducing the pulverized particles can be further exerted. Note that when the minimum clearance value dmin and the maximum clearance value dmax are the same (i.e., in the case of 2001 in FIG. 3), the clearance d is regarded as the minimum clearance value dmin. When two or more pairs of rolls are used in the pulverization process, it is sufficient that the minimum value of the minimum clearance values set between the rolls is within the above range.
[0096] In addition, when the clearance d varies depending on the position in the roll width direction, as shown by 2002 in Fig. 3, the clearance d at each position is calculated, and the difference between the maximum clearance dmax and the minimum clearance dmin is referred to as the "clearance difference." The clearance difference is not particularly limited, but is preferably 0 to 0.2 mm, more preferably 0 to 0.1 mm, and even more preferably 0 to 0.05 mm.
[0097] The pitch (spacing) of the grooves provided on the roll can be appropriately determined according to the size of the particles to be pulverized. When the pulverized particle size is large, it is preferable to select a large groove pitch, and when the pulverized particle size is small, it is preferable to select a small groove pitch. The groove pitch is not particularly limited, but is preferably 0.1 to 2 mm, more preferably 0.2 to 1.5 mm, and even more preferably 0.3 to 1.2 mm. Here, the groove pitch p means the interval between the crest of any groove and the crest of the adjacent groove, or the interval between the valley of any groove and the valley of the adjacent groove, as shown in 2001 in FIG. 3. For example, when a surface (hereinafter referred to as a "flat portion") parallel to the circumferential direction is provided between the crest and valley of the groove, it means the interval between the crest and crest of adjacent grooves, including the flat portion, or the interval between the valley of adjacent grooves. The groove pitch may be different on one roll, but is preferably constant over the entire roll width, and when grooves are provided on both of a pair of rolls, it is preferably constant over the entire pair of rolls.
[0098] The height of the grooves can be appropriately determined and is not particularly limited, but the grooves are preferably provided to a height of 0.1 to 2 mm, more preferably 0.2 to 1.5 mm, and even more preferably 0.3 to 1 mm. Here, the height of the grooves means the difference in height between the apex of the crest of any groove and the bottom of the valley of that groove, as shown in 2001 in Fig. 3.
[0099] (Water-absorbent resin before the grinding process) In one embodiment of the present invention, the dried polymer obtained in the drying step or the like and subjected to the pulverization step may be pulverized in its entirety in a pulverizer, preferably the specific roll-type pulverizer, but depending on the shape of the dried polymer, it may be subjected to another step, for example, a rough crushing step, or may be subjected to a classification step, before being pulverized in the pulverizer. The "rough crushing step" refers to a step of disintegrating (loosening) aggregated particles. Therefore, when the dried polymer is aggregated in a block shape or the like, the dried polymer may be roughly crushed in advance in order to efficiently perform pulverization in a pulverizer, preferably the specific roll-type pulverizer.
[0100] In one embodiment of the present invention, the particle size distribution of the dried polymer fed into the pulverizer, preferably the specific roll-type pulverizer, is such that the proportion of particles with a particle diameter of 850 μm or more (proportion of particles that did not pass through a sieve with an opening diameter of 850 μm) is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less in 100% by mass of the dried polymer. Also, the proportion of particles with a particle diameter of 1400 μm or more (proportion of particles that did not pass through a sieve with an opening diameter of 1400 μm) in 100% by mass of the dried polymer is preferably 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less.
[0101] In one embodiment of the present invention, the resin solid content of the dried polymer subjected to the pulverization step is, for example, preferably 80.0 to 99.5% by mass, more preferably 90.0 to 99.0% by mass, and even more preferably 95.0 to 98.5% by mass. That is, the water content of the dried polymer of the present invention is preferably 0.5 to 20% by mass, more preferably 1.0 to 10% by mass, and even more preferably 1.5 to 5% by mass. By setting the solid content rate of the dried polymer within the above range, the hardness of the dried polymer can be adjusted to be suitable for pulverization in the pulverization step, and the obtained pulverized product can have a rounded sphericity. The method for determining the resin solid content of the dried polymer is as described in "(3-4) Drying step".
[0102] In one embodiment of the present invention, the relationship between the clearance between the pair of rolls and the mass average particle size of the dried polymer fed to the roll-type grinding device is preferably 1:0.3 to 1:10. In this case, an appropriate pressure that prevents the water absorbent resin from being crushed is applied to the dried polymer during grinding, and a ground product with a rounded shape and high sphericity can be obtained. The relationship between the clearance between the pair of rolls and the mass average particle size of the dried polymer fed to the roll-type grinding device is more preferably 1:0.5 to 1:5, and further preferably 1:0.9 to 1:3.
[0103] (3-6) Classification process The water absorbent resin (e.g., water absorbent resin powder) obtained through the pulverization step is further subjected to a classification step, if necessary. In one embodiment of the present invention, the particle size adjustment method in the classification step is not particularly limited, but examples thereof include sieve classification using a JIS standard sieve (JIS Z8801-1 (2000)) and air flow classification.
[0104] (3-7) Surface crosslinking process The water-absorbent resin (e.g., water-absorbent resin powder) obtained through the pulverization step (and any subsequent step) is preferably surface-crosslinked with a surface crosslinking agent. The surface crosslinking is a treatment for providing a portion with high crosslink density in the surface layer of the water-absorbent resin (a region from the surface of the water-absorbent resin to a depth of several tens of μm inside). By carrying out the surface crosslinking treatment, various water-absorbing properties can be improved. In this specification, the water-absorbent resin also includes a surface-crosslinked water-absorbent resin.
[0105] (Surface cross-linking agent) The surface cross-linking agent used in this step is not particularly limited, but may be an organic or inorganic surface cross-linking agent. Among them, from the viewpoint of the physical properties of the water-absorbent resin and the handling of the surface cross-linking agent, an organic surface cross-linking agent that reacts with a carboxyl group is preferred. For example, one or more surface cross-linking agents disclosed in U.S. Patent No. 7,183,456 may be mentioned. Specifically, polyhydric alcohol compounds, epoxy compounds, haloepoxy compounds, polyamine compounds or their condensates with haloepoxy compounds, oxazoline compounds, oxazolidinone compounds, polyvalent metal salts, alkylene carbonate compounds, cyclic urea compounds, etc. may be mentioned.
[0106] (3-8) Granulation process The method for producing a water-absorbent resin according to one embodiment of the present invention may include a granulation step for obtaining an aggregate of primary particles. For example, in the case of reversed-phase suspension polymerization, an aggregate of primary particles can be obtained by performing multiple reversed-phase suspension polymerization steps, adding an aggregating agent to the gel of primary particles after polymerization, and the like. Therefore, these steps can be said to be granulation steps. In the case of aqueous solution polymerization, the granulation step may include adding an aqueous liquid to fine particles of a water-absorbent resin passing through a JIS standard sieve with a mesh size of 150 μm, and stirring and mixing the mixture.
[0107] The method for producing a water absorbent resin according to one embodiment of the present invention includes a granulation step, and may also include a crushing step of crushing the water absorbent resin obtained in the granulation step by using the specific roll type crushing device described above.
[0108] (3-9) Polishing process The method for producing a water absorbent resin according to one embodiment of the present invention may include a step of polishing the surface of the water absorbent resin (e.g., water absorbent resin powder) obtained in the pulverization step. In particular, when aqueous solution polymerization is used as the polymerization form, the sphericity of the water absorbent resin (e.g., water absorbent resin powder) obtained through the pulverization step tends to be lower than that of the reversed-phase suspension polymerization, so that it is preferable to perform a polishing treatment as necessary.
[0109] The method for performing the polishing treatment is not particularly limited, but examples thereof include a method of putting a water-absorbent resin (e.g., water-absorbent resin powder) into a container together with glass beads and shaking the container, and a method of subjecting the container to a known stirring device such as a homogenizer or a pin mill.
[0110] (3-10) Additive addition process The method for producing a water-absorbent resin according to one embodiment of the present invention preferably includes a step of adding an additive to impart various functions to the water-absorbent resin. As the additive, any of those described in "(2-2) Additives" can be used.
[0111] The method and timing of adding the additives are not particularly limited, and may be appropriately selected depending on the additives to be added.
[0112] The method for producing a water-absorbent resin according to one embodiment of the present invention preferably includes a step of adding water-insoluble inorganic fine particles, from the viewpoint of reducing friction between the water-absorbent resin particles and the water-permeable substrate, improving the slipperiness, and facilitating the movement of the water-absorbent resin on or between the fibers of the water-permeable substrate. Here, the water-insoluble inorganic fine particles are as described in "(2-2) Additives". As described above, among the water-insoluble inorganic fine particles, it is more preferable to add hydrotalcite; clay minerals such as kaolin, talc, and zeolite; calcium phosphate; barium phosphate, and the like.
[0113] The timing of adding the water-insoluble inorganic fine particles is not particularly limited, but for example, it is preferable to add them after the pulverization step or the surface cross-linking step, or after the pulverization step or the surface cross-linking step and further after a classification step, a polishing step, a granulation step, a water-containing (water addition) step, a sizing step, etc. In addition, the method of adding the water-insoluble inorganic fine particles is not particularly limited, but examples thereof include a method of dry blending with a water-absorbent resin (e.g., water-absorbent resin powder), a method of adding as a dispersion to a water-absorbent resin (e.g., water-absorbent resin powder) and mixing, etc.
[0114] (3-11) Other processes The method for producing a water absorbent resin according to one embodiment of the present invention may include, in addition to the above-mentioned steps, a water-containing (rewetting) step, a step of adding other additives, a granulation step, and a fine powder reuse step, as necessary. In addition, the method may further include a transport step, a storage step, a packaging step, a keeping step, and the like.
[0115] (Rewetting process) This step, which is optionally performed, is a step of adding at least one kind of additive selected from the group consisting of a polyvalent metal salt, a cationic polymer, a chelating agent, an inorganic reducing agent, and an α-hydroxycarboxylic acid compound to the water absorbent resin (e.g., water absorbent resin particles) obtained in the surface cross-linking step.
[0116] The additive is preferably added to the water-absorbing resin (for example, water-absorbing resin particles) as an aqueous solution or a dispersion (slurry). The additive may be added and mixed simultaneously with the above-mentioned surface cross-linking agent solution.
[0117] Specifically, the method described in International Patent Publication No. 2015 / 053372, “(2-7) Rewetting Step”, is also applicable to the present invention.
[0118] (Sizing process) The "size regulation step" means a step of loosening the water absorbent resin loosely aggregated through the surface cross-linking step to regulate the particle size. This size regulation step includes a fine powder removal step and a classification step subsequent to the surface cross-linking step. The size regulation step is preferably carried out from the viewpoint of regulating the particle size of the water absorbent resin and obtaining stable water absorption properties.
[0119] (Fine powder reuse process) The "fine powder reuse step" means a step of supplying the fine powder generated by sieve classification or the like in each step to any of the steps as it is or after granulating the fine powder. The fine powder reuse step is preferably carried out from the viewpoint of reducing production loss of the water absorbent resin.
[0120] [4] Uses of water-absorbent resins The use of the water-absorbent resin according to one embodiment of the present invention is not particularly limited, but is preferably used as an absorbent body for absorbent articles such as paper diapers (for infants and adults), sanitary napkins, incontinence pads, etc. In particular, it can be suitably used as an absorbent body for paper diapers that include a water-absorbent resin and a water-permeable substrate. Other absorbent articles include, for example, soil water retention agents, seedling sheets, seed coating materials, condensation prevention sheets, drip absorbents, freshness-preserving materials, disposable hand warmers, cooling bandanas, ice packs, medical waste liquid solidifying agents, residual soil solidifying materials, water damage prevention waste liquid gelling agents, water-absorbing sandbags, disaster-use portable toilets, compresses, thickening agents for cosmetics, water-stopping materials for electric and electronic material communication cables, gasket packing, sustained-release agents for fertilizers, various sustained-release agents (space disinfectants, air fresheners, etc.), pet sheets, cat litter, wound protection dressing materials, condensation prevention building materials, oil moisture removers, paints, adhesives, resin additives (anti-blocking agents, light diffusing agents, matting agents, additives for decorative panels, additives for artificial marble, additives for toners, etc.), and the like. EXAMPLES
[0121] The present invention will be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to these examples. Examples obtained by appropriately combining the technical means described in each example are also included in the scope of the present invention. In the examples, the terms "parts" and "%" may be used, but unless otherwise specified, they represent "parts by mass" or "% by mass". Unless otherwise specified, each operation is performed at room temperature (23°C ± 2°C) and at a relative humidity of 40 to 50% RH. In addition, the electrical equipment used in the examples and comparative examples (including the measurement of the physical properties of the water-absorbent resin) was powered by a power source of 200V or 100V, 60Hz, unless otherwise noted.
[0122] 1. Evaluation Method [1-1] Centrifuge holding capacity (CRC) The centrifuge retention capacity (CRC) of the water-absorbent resin was measured in accordance with the EDANA method (ERT441.2-02).
[0123] Specifically, 0.2 g of the water-absorbent resin was placed in a nonwoven bag, and then immersed in a large excess of 0.9% by mass aqueous sodium chloride solution for 30 minutes to allow free swelling. Thereafter, the bag was centrifuged (250 G) for 3 minutes to remove water, and the water absorption capacity (unit: g / g) was determined.
[0124] [1-2] Absorption capacity under pressure (AAP) The absorbency under pressure (AAP) of the water-absorbent resin was measured in accordance with the EDANA method (ERT442.2-02). Note that the load condition was changed to 4.83 kPa (0.7 psi).
[0125] [1-3] Moisture content The moisture content of the water-absorbent resin was measured in accordance with the EDANA method (ERT430.2-02). Note that, in the measurement, the mass of the sample (water-absorbent resin) was changed to 1.0 g, the drying temperature to 180° C., and the drying time to 3 hours.
[0126] Specifically, 1.0 g of a sample (water-absorbent resin or water-absorbent resin powder) was placed in an aluminum cup having a bottom diameter of 50 mm, and then the total mass W1 (g) of the sample and the aluminum cup was accurately weighed.
[0127] Next, the sample was placed in an aluminum cup and left to stand in an oven set at an atmospheric temperature of 180° C. After 3 hours, the sample was removed from the oven together with the aluminum cup, and the total mass W2 (g) of the dried sample and aluminum cup was accurately weighed. When the mass of the sample (water-absorbent resin) used in this measurement was M (1.0 g), the moisture content (mass%) of the sample was calculated according to the following formula (3): Moisture content (mass%) = {(W1-W2) / M}×100...Equation (3).
[0128] [1-4] Mass average particle diameter (D50) The mass-average particle diameter (D50) of the water-absorbent resin was measured according to the method described in “(3) Mass-Average Particle Diameter (D50) and Logarithmic Standard Deviation (σζ) of Particle Diameter Distribution” in columns 27 and 28 of U.S. Pat. No. 7,638,570.
[0129] [1-5] Bulk density The bulk density of the water-absorbent resin was measured in accordance with the EDANA method (ERT460.2-02).
[0130] [1-6] Surface tension The surface tension of the water-absorbent resin was measured by the method described in paragraph 0244 of WO2015 / 129917.
[0131] Specifically, 50 ml of 0.90% by mass sodium chloride aqueous solution adjusted to 20°C was placed in a thoroughly washed 100 ml beaker, and the surface tension of the 0.90% by mass sodium chloride aqueous solution was measured using a surface tensiometer (K11 automatic surface tensiometer, manufactured by KRUSS). In this measurement, the surface tension value must be in the range of 71 to 75 [mN / m].
[0132] Next, a thoroughly washed cylindrical stirrer with a length of 25 mm and 0.500 g of water-absorbent resin were placed in a beaker containing the 0.90 mass% sodium chloride aqueous solution after the surface tension measurement, adjusted to 20°C, and stirred for 4 minutes at 500 rpm. After 4 minutes, the stirring was stopped, and the water-absorbent resin was allowed to settle, after which the surface tension of the supernatant was measured again by the same operation. In addition, in the measurement of the surface tension, a plate method using a platinum plate was adopted, and the plate was thoroughly washed with deionized water before each measurement, and heated and washed with a gas burner before use.
[0133] [1-7] SAP mobility The SAP mobility of the water-absorbent resin was measured by the following procedure.
[0134] As shown in Figs. 4 and 5, an inclined table 10 made of acrylic resin having a surface inclined at 45 degrees to the horizontal plane was placed on a flat and horizontal table, and a nonwoven fabric 11 (having a thickness of 3 mm and a basis weight of 41 g / m2) cut into a rectangle of 4 cm x 12 cm was placed on the inclined surface of the inclined table 10. 2 The nonwoven fabric is an air-through nonwoven fabric made of a mixture of polyethylene, polypropylene, and polyethylene terephthalate, and the fiber diameter of the polyethylene and the fiber diameter of the polypropylene are 0.18 mm, and the fiber diameter of the polyethylene terephthalate is 0.27 mm.) was attached using double-sided tape in a direction perpendicular to the width direction of the inclined table 10. A tray 12 was placed at the bottom of the inclined table 10. A mark 13 was made at a position 1 cm below the top edge of the nonwoven fabric 11 and 2 cm inside the side perpendicular to the top edge of the nonwoven fabric 11, and 1.0 g of water-absorbent resin was dropped over 5 seconds from a height of 1 cm vertically upward from the mark 13. The water-absorbent resin moved on or within the nonwoven fabric 11 and slid down, falling to the tray 12. The dropped water-absorbent resin was collected and its mass was measured, and then the SAP mobility was calculated according to the following formula (1). In addition, the phrase "moving within the nonwoven fabric 11" means that the water-absorbent resin that has entered the nonwoven fabric moves between the fibers of the nonwoven fabric.
[0135] SAP mobility [mass%] = mass of recovered water absorbent resin [g] / total mass of dropped water absorbent resin [g] × 100 Equation (1) [1-8] Water absorption rate (vortex method) 0.02 parts by mass of Food Blue No. 1, a food additive, was added to 1000 parts by mass of a 0.90% by mass aqueous solution of sodium chloride (physiological saline), and the liquid temperature was adjusted to 30° C. 50 ml of the physiological saline was measured out into a 100 ml beaker, and 2.0 g of the water-absorbent resin was added at once while stirring at 600 rpm using a cylindrical stirrer tip with a length of 40 mm and a cross section perpendicular to the length direction and a diameter of 8 mm and a magnetic stirrer. The time until the water-absorbent resin absorbed the physiological saline and covered the stirrer tip was measured as the absorption rate (seconds).
[0136] [1-9] Liquid return amount of absorbent (1) Preparation of absorber An adhesive tape 100 (vinyl tape No. 21S manufactured by NITTO DENKO) cut to 6 cm x 9 cm was placed on the bottom of a rectangular polystyrene case (bottom surface 6 cm x 9 cm, depth 1 cm (both dimensions of the case inner surface)) with the adhesive surface facing up, and nonwoven fabric 11 (thickness 3 mm, basis weight 41 g / m2) cut to 4 cm x 7 cm was placed on the area surrounded by four sides located 1 cm inward from the ends of the four sides of the adhesive surface of the adhesive tape 100, as shown by 1001 in FIG. 2 The nonwoven fabric was an air-through nonwoven fabric made of a mixture of polyethylene, polypropylene, and polyethylene terephthalate, the fiber diameter of the polyethylene and the fiber diameter of the polypropylene being 0.18 mm, and the fiber diameter of the polyethylene terephthalate being 0.27 mm.) was placed on the nonwoven fabric. The same nonwoven fabric as that used in the measurement of SAP mobility described above (1-7) was used as the nonwoven fabric. On the nonwoven fabric 11, as shown in 1002 in FIG. 1, the water absorbent resin 10 was sprayed in a strip shape with a width of 1 cm along the longitudinal direction of the nonwoven fabric 11 from the midpoint of one short side of the nonwoven fabric 11 to the midpoint of the other short side. Thereafter, the case was placed on a flat and horizontal table, and the water absorbent resin 10 sprayed in a strip shape was diffused on the nonwoven fabric 11 by performing an operation of reciprocating 10 times over a distance of 6 cm in a horizontal direction and in a direction perpendicular to the longitudinal direction of the nonwoven fabric 11 (the direction shown by the arrow in 1002 in FIG. 1) for 1 second. Next, as shown in 1003 of FIG. 1, a liquid-permeable nonwoven fabric 110 (air-laid nonwoven fabric, basis weight 46.6 g / m) of 6 cm×9 cm was applied onto the nonwoven fabric 11 in which the water-absorbent resin 10 was dispersed. 2 ) was placed on the absorbent sheet and attached to the adhesive surfaces on all four sides to prepare absorbent core 1 for evaluation.
[0137] (2) Measurement of the amount of liquid returning The absorbent for evaluation was placed on a flat and horizontal table with the liquid-permeable nonwoven fabric on the upper surface. 12 g of 0.9% by mass sodium chloride aqueous solution at 20° C. was weighed into a 50 mL glass beaker, and the liquid was added to the entire absorption surface of the absorbent for evaluation over 10 seconds. 30 seconds after the start of the liquid addition, a kitchen paper (kitchen towel manufactured by Oji Nepia Co., Ltd.) cut to 6 cm×9 cm and stacked in 24 sheets with a total mass K1 (g) and an acrylic plate of 6 cm×9 cm and mass 22 g were placed on the absorbent for evaluation in this order. 10 seconds after the kitchen paper and the acrylic plate were placed, the kitchen paper and the acrylic plate were removed, and the total mass K2 (g) of the 24 stacked kitchen paper sheets was measured, and the amount of liquid return of the absorbent for evaluation was calculated based on the following formula (4): Amount of liquid return (g) = K2 - K1... Equation (4).
[0138] [1-10] Dispersion of water-absorbent resin in absorbent body The state of dispersion of the water-absorbent resin in the absorbent core for evaluation was visually observed.
[0139] [1-11] Measuring the thickness of nonwoven fabric The thickness of the nonwoven fabric was measured using a large-type dial thickness gauge (thickness measuring device) (manufactured by Ozaki Manufacturing Co., Ltd., model number: JB, measuring probe: anvil top and bottom φ50 mm). The upper measuring probe of the thickness measuring device was brought close to a height of 2 to 3 mm from the nonwoven fabric, and then the hand was slowly released from the handle so as to apply as little pressure as possible to the nonwoven fabric, and the thickness of the nonwoven fabric was measured.
[0140] Example 1 800 g of n-heptane was placed in a 2000 mL four-neck separable flask equipped with a stirrer, reflux condenser, thermometer, nitrogen gas inlet tube, and dropping funnel, and 0.88 g of maleic anhydride-modified ethylene-propylene copolymer (product name: Hiwax (registered trademark) HW2203A, manufactured by Mitsui Chemicals, Inc.) was added and dissolved as a dispersant. Nitrogen gas was then blown in to expel the dissolved oxygen.
[0141] Separately, in a flask, an aqueous monomer solution (1) consisting of 127 g of sodium acrylate, 36 g of acrylic acid, 0.077 g of polyethylene glycol diacrylate (n=9), 0.008 g of pentasodium diethylenetriaminepentaacetate, 0.67 g of hydroxyethylcellulose as a thickener, and 215 g of ion-exchanged water was prepared, and nitrogen gas was blown in to expel the dissolved oxygen from the aqueous solution.
[0142] Next, 1.2 g of a 15% aqueous solution of sodium persulfate was added to the monomer aqueous solution (1) in the flask, and the entire amount was added to the separable flask and dispersed by stirring at 210 rpm. The bath temperature was then raised to 60° C. to initiate a polymerization reaction, and the bath temperature was maintained at 60° C. for 2 hours. The organic solvent was then filtered off by suction filtration, and the residue was air-dried at room temperature overnight to obtain a hydrogel-like crosslinked polymer (1).
[0143] Next, the hydrogel crosslinked polymer (1) was dried using a cylindrical container rotary dryer. Specifically, the rotary container of the cylindrical container rotary dryer was rotated at 75 rpm in an atmosphere at a temperature of 200° C., and the hydrogel polymer (1) was supplied to the cylindrical container rotary dryer and dried until the moisture content reached 10% by mass, thereby obtaining a dried polymer (1).
[0144] Subsequently, the dried polymer (1) was pulverized using a roll granulator (manufactured by Nippon Granulator Co., Ltd., roll size: diameter 115 mm × length 100 mm) as a pulverizing device, and further classified using a JIS standard sieve with an opening of 150 μm, and the fine powder that passed through the sieve was removed, thereby obtaining a water absorbent resin powder (1). Here, in the roll granulator, a pair of rolls was installed in the first stage, and one-stage pulverization was performed. Note that, as the pair of rolls, a groove having a V-shaped cross section was provided on the roll surface of each of the rolls in a direction parallel to the roll rotation direction (clearance difference: 0). Specifically, the grooves were provided over the entire circumference of the roll surface, and a plurality of grooves were provided continuously at equal intervals from one end to the other end of the roll. The pitch (spacing) of the grooves of the pair of rolls was the same for both rolls. In addition, the grooves in each roll were arranged so that the crest of the groove of one roll and the valley of the groove of the other roll were at the same position in the axial direction of the rolls, as shown in 2001 in Figure 3, and the clearance between the rolls was constant. Note that the clearance between the rolls means the distance between the two rolls, as mentioned above.
[0145] Roll speed: 565 / 462 rpm (inner rotation) Groove height (groove inclination angle): 1.0mm (45°) Groove pitch: 1.2mm Clearance between rolls: 0.6mm.
[0146] A surface crosslinking agent solution consisting of 0.03 parts by mass of ethylene glycol diglycidyl ether, 0.385 parts by mass of ethylene carbonate, 0.644 parts by mass of propylene glycol, and 2.6 parts by mass of ion-exchanged water was uniformly mixed with 100 parts by mass of the water absorbent resin powder (1), and subjected to a heat treatment at 195° C. for 25 minutes. Thereafter, the powder temperature was forcibly cooled to 60° C., thereby obtaining a surface-crosslinked water absorbent resin powder (1).
[0147] 100 parts by mass of the surface-crosslinked water-absorbent resin powder (1) was uniformly mixed with 10.0 parts by mass of water, and the mixture was classified using JIS standard sieves with openings of 1000 μm and 150 μm to obtain a sized product that passed through the JIS standard sieve with openings of 1000 μm and remained on the JIS standard sieve with openings of 150 μm. Thereafter, hydrotalcite (product name: DHT-6, manufactured by Kyowa Chemical Industry Co., Ltd., Mg6Al2(OH)16CO3·4H2O, specific surface area = 16 m) was added to 100 parts by mass of the sized product. 2 The physical properties of the water-absorbent resin (1) are shown in Table 1.
[0148] Example 2 7.5 g of polyethylene glycol diacrylate (n=9) was dissolved in 5500 g of an aqueous solution of sodium acrylate having a neutralization rate of 75 mol% (monomer concentration 38 mass%) to prepare an aqueous monomer solution (2). Next, the aqueous monomer solution (2) was fed into a reactor formed by attaching a lid to a jacketed stainless steel double-arm kneader having an internal volume of 10 L and two sigma-type blades, and the system was purged with nitrogen gas while maintaining the liquid temperature at 30°C to remove dissolved oxygen.
[0149] Next, 29.8 g of a 10% by mass aqueous solution of sodium persulfate and 1.5 g of a 1% by mass aqueous solution of L-ascorbic acid were added while stirring the aqueous monomer solution (2), and polymerization started about 1 minute later. The polymerization peak temperature reached 86°C 17 minutes after the start of polymerization, and the hydrogel polymer (2) was taken out 60 minutes after the start of polymerization.
[0150] The hydrogel crosslinked polymer (2) was gel-pulverized using a meat chopper (No. 32 type, manufactured by Hiraga Seisakusho Co., Ltd.) equipped with a die having a die hole diameter of 9.5 mm to obtain hydrogel crosslinked polymer particles (2). The gel pulverization was performed by feeding the hydrogel crosslinked polymer (2) at 2.4 kg / min and water vapor at 5.0 kg / h into the meat chopper with the screw shaft rotation speed of the meat chopper set to 130 rpm.
[0151] Subsequently, the obtained hydrogel-like crosslinked polymer particles (2) were dried using the same cylindrical container rotary dryer as in Example 1. The particles were fed into the cylindrical container rotary dryer set at the same temperature and rotation speed as in Example 1, and dried until the moisture content reached 1% by mass, to obtain a dried polymer (2).
[0152] Subsequently, the dried polymer (2) was pulverized under the same pulverization conditions as those for pulverizing the dried polymer (1) in Example 1, except that the groove pitch was changed to 2.0 mm and the clearance was changed to 1 mm, using a roll granulator (manufactured by Nippon Granulator Co., Ltd., roll size: diameter 115 mm × length 100 mm) as a pulverizing device, and the dried polymer (2) was passed through a JIS standard sieve with an opening of 850 μm, to obtain a water absorbent resin powder (2) having a mass average particle diameter (D50) of 360 μm.
[0153] Thereafter, 30 g of the water absorbent resin powder (2) and 10 g of glass beads having a diameter of 6 mm were placed in a glass container with a lid having a diameter of 6 cm and a height of 11 cm, and the container was attached to a paint shaker (Toyo Seiki Seisakusho; Product No. 488). The container was then shaken at 800 cycles / min (CPM) for 30 minutes to obtain a water absorbent resin powder (2) having a polished surface.
[0154] 0.7 parts by mass of a surface crosslinking agent aqueous solution consisting of 0.1 parts by mass of ethylene glycol diglycidyl ether, 0.3 parts by mass of propylene glycol, and 0.3 parts by mass of water was uniformly mixed with 100 parts by mass of the surface-polished water absorbent resin powder (2), and the mixture was heat-treated for 20 minutes at 210° C. Thereafter, the powder was forcibly cooled to 60° C., and granulated by passing through a JIS standard sieve with an opening of 850 μm, to obtain a surface-crosslinked water absorbent resin powder (2).
[0155] 100 parts by mass of the surface-crosslinked water-absorbent resin powder (2) was mixed with hydrotalcite (product name: DHT-6, manufactured by Kyowa Chemical Industry Co., Ltd., MgAl(OH)CO·4HO, specific surface area = 16 m 2 The physical properties of the water-absorbent resin (2) are shown in Table 1.
[0156] Comparative Example 1 In Example 1, except that the amount of polyethylene glycol diacrylate (n=9) used was changed to 0.097 g, a polymerization reaction was carried out under the same conditions as the polymerization reaction of the aqueous monomer solution (1) in Example 1. The organic solvent was then removed by suction filtration, and the residue was air-dried at room temperature overnight to obtain a comparative hydrous gel-like crosslinked polymer (1).
[0157] Subsequently, the comparative hydrogel-like crosslinked polymer (1) was dried using the same cylindrical container rotary dryer as in Example 1. Specifically, the comparative hydrogel-like crosslinked polymer (1) was supplied to the cylindrical container rotary dryer set at the same temperature and rotation speed as in Example 1, and dried until the moisture content reached 10 mass %, to obtain a comparative dried polymer (1).
[0158] Next, the comparative dried polymer (1) was pulverized using a roll mill (WML type roll pulverizer, manufactured by Inokuchi Giken Co., Ltd.) as a pulverizing device to obtain a comparative water absorbent resin powder (1). Here, in the roll mill, a pair of rolls was installed in the first stage, and one-stage pulverization was performed. The pair of rolls used had a groove with a V-shaped cross section provided on the roll surface in a direction approximately perpendicular to the roll rotation direction. Specifically, one groove was provided continuously from one end of the roll to the other end (i.e., continuously in the roll width direction) on the roll surface, and multiple grooves were provided continuously and side by side at equal intervals over the entire circumference. The roll grooves (groove tooth shape) of the pair of rolls were the same for both.
[0159] Roll speed: 480 / 200 rpm Groove pitch: 1.15mm Clearance between rolls: 1.0mm.
[0160] A surface crosslinking agent solution consisting of 0.1 part by mass of ethylene glycol diglycidyl ether, 1.0 part by mass of isopropyl alcohol, and 3.0 parts by mass of ion-exchanged water was uniformly mixed with 100 parts by mass of the comparative water absorbent resin powder (1), and the mixture was heat-treated for 40 minutes at 100° C. The powder temperature was forcibly cooled to 60° C., thereby obtaining a surface-crosslinked comparative water absorbent resin powder (1).
[0161] 100 parts by mass of the surface-crosslinked comparative water-absorbent resin powder (1) was uniformly mixed with 5.0 parts by mass of water, and the mixture was passed through a JIS standard sieve with a mesh size of 300 μm to size the mixture. Then, 100 parts by mass of the size-sized mixture was mixed with hydrotalcite (product name: DHT-6, manufactured by Kyowa Chemical Industry Co., Ltd., Mg6Al2(OH)16CO3·4H2O, specific surface area = 16 m 2 0.3 parts by mass of each of the above powders (1 / g) was mixed uniformly to obtain a comparative water-absorbing resin (1). The physical properties of the comparative water-absorbing resin (1) are shown in Table 1.
[0162] Comparative Example 2 In Example 1, fine particle silica (product name: Aerosil (registered trademark) 200, manufactured by Nippon Aerosil Co., Ltd., specific surface area = 200 ± 25 m) was used instead of hydrotalcite. 2 A comparative water-absorbing resin (2) was obtained in the same manner as in Example 1, except that 0.3 parts by mass of 1,000g / g of the water-absorbing agent was mixed uniformly. The physical properties of the comparative water-absorbing resin (2) are shown in Table 1.
[0163] Comparative Example 3 In Comparative Example 1, fine particle silica (product name: Aerosil (registered trademark) 200, manufactured by Nippon Aerosil Co., Ltd., specific surface area = 200 ± 25 m) was used instead of hydrotalcite. 2 A comparative water-absorbing resin (3) was obtained in the same manner as in Comparative Example 1, except that 0.3 parts by mass of 1,000g / g of the cellulose acylate was uniformly mixed. The physical properties of the comparative water-absorbing resin (3) are shown in Table 1.
[0164] [Table 1]
[0165] Comparison between the Examples and Comparative Examples reveals that the water-absorbent resin with high SAP mobility is uniformly dispersed in the absorbent body, and the amount of liquid return of the absorbent body for evaluation, i.e., the amount of liquid return over the entire absorbing surface of the absorbent body, is reduced. It was also shown that the water-absorbent resin with high SAP mobility and excellent water absorption speed reduces the amount of liquid return of the absorbent body for evaluation. [Industrial Applicability]
[0166] According to the water-absorbent resin of one embodiment of the present invention, it is possible to provide a water-absorbent resin that can efficiently absorb liquid over the entire absorbent surface of an absorbent article comprising a water-absorbent resin and a water-permeable substrate, thereby reducing the amount of liquid returning over the entire absorbing surface of the absorbent article. Therefore, it can be suitably used in sanitary materials (sanitary products) such as paper diapers, sanitary napkins, adult incontinence products (incontinence pads), and pet sheets. [Explanation of symbols]
[0167] 1. Absorbent material for evaluation 10 Water-absorbing resin 11 Nonwoven fabrics 100 Adhesive Tape 110 Liquid permeable nonwoven fabric 20a Dry polymer 20b Dried polymer pulverized material (water-absorbent resin powder) 200 Roller type crusher 201 Piping 202 Inlet 203, 203a, 203b Roll 12 Saucer 13 marks 14 Slope
Claims
1. A particulate poly(meth)acrylic acid (salt)-based water-absorbing resin, A poly(meth)acrylic acid (salt)-based water-absorbing resin having a SAP mobility of 10% by mass or more, as determined by the following steps (1) to (4): (1) A nonwoven fabric cut into a rectangle measuring 4 cm x 12 cm is attached to the inclined surface of an acrylic resin inclined table having a surface inclined at 45 degrees, with the longitudinal direction of the rectangle perpendicular to the width direction of the inclined table. Here, the nonwoven fabric has a thickness of 3 mm and a basis weight of 41 g / m 2 and an air-through nonwoven fabric made of a mixture of polyethylene, polypropylene and polyethylene terephthalate, the fiber diameter of the polyethylene and the fiber diameter of the polypropylene being 0.18 mm, and the fiber diameter of the polyethylene terephthalate being 0.27 mm; (2) A mark is made at a position 1 cm below the uppermost edge of the nonwoven fabric and 2 cm inside from the edge perpendicular to the uppermost edge of the nonwoven fabric, and 1.0 g of the water-absorbent resin is dropped vertically upward from the mark over a period of 5 seconds from a height of 1 cm; (3) The water-absorbing resin that has moved and slid down on or within the nonwoven fabric and fallen into a tray installed at the bottom of the inclined platform is collected, and its mass is measured; (4) Calculate the SAP mobility according to the following formula (1): SAP mobility [mass %]=mass [g] of recovered water-absorbent resin / total mass [g] of added water-absorbent resin×100 Formula (1).
2. The poly(meth)acrylic acid (salt)-based water-absorbing resin according to claim 1, further comprising water-insoluble inorganic fine particles.
3. The specific surface area of the water-insoluble inorganic fine particles is 100 m 2 The poly(meth)acrylic acid (salt)-based water-absorbing resin according to claim 2, wherein the water-absorbent capacity is less than 1000 g / g.
4. The poly(meth)acrylic acid (salt)-based water-absorbing resin according to any one of claims 1 to 3, which has a water-absorbing speed measured by a vortex method of less than 35 seconds.
Citation Information
Patent Citations
Method for producing water absorbent
JP2022011517A
Method for producing water-absorbing resin
JP2022145483A
Poly(METH)acrylic acid (SALT)-based water-absorbing resin, and absorber
JP2022175089A
Poly(METH)acrylic acid (SALT)-based particulate absorbent, and production method
WO2015129917A1
Particulate water absorbing agent
WO2017170605A1
Cited By
System and control method
EP4703703A1