Poly(METH)acrylic acid (SALT)-based water-absorbing resin

A particulate poly(meth)acrylic acid (salt)-based water-absorbing resin with enhanced absorption capacity against pressure fluctuations addresses the instability of conventional resins, ensuring stable performance in absorbent articles like disposable diapers.

JP2024147408APending Publication Date: 2024-10-16NIPPON SHOKUBAI CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023060399
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-10-16

AI Technical Summary

Technical Problem

Conventional poly(meth)acrylic acid (salt)-based water-absorbing resins exhibit insufficient absorption capacity under varying loads commonly encountered in absorbent articles like disposable diapers, as they are evaluated under static pressure conditions, failing to account for dynamic pressure fluctuations.

Method used

A particulate poly(meth)acrylic acid (salt)-based water-absorbing resin with a specific absorption capacity against pressure fluctuations of 76.0 g/g or more, incorporating water-insoluble inorganic fine particles, is developed to stabilize absorption performance under changing loads.

Benefits of technology

The resin ensures stable and excellent absorbency in absorbent articles by maintaining high absorption capacity even under varying loads, reducing liquid return and leakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147408000001_ABST
    Figure 2024147408000001_ABST
Patent Text Reader

Abstract

To provide a water-absorbing resin that achieves an absorbent article exhibiting stable and superior absorption performance during practical use when employed in an absorber of the absorbent article, such as a disposable diaper.SOLUTION: The present invention provides a particulate poly(meth)acrylic acid (salt)-based water-absorbing resin, having an absorption capacity under pressure variations of 76.0 g / g or higher.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a water-absorbing resin. More specifically, the present invention relates to a poly(meth)acrylic acid (salt)-based water-absorbing resin. [Background technology]

[0002] In recent years, water-absorbing resins have been widely used as water-absorbing agents in sanitary materials such as paper diapers, sanitary napkins, and incontinence pads from the viewpoint of absorbing body fluids. Examples of such water-absorbing resins include hydrolyzates of starch-acrylonitrile graft copolymers, neutralized products of starch-acrylic acid graft polymers, saponified products of vinyl acetate-acrylic acid ester copolymers, and crosslinked products of partially neutralized (meth)acrylic acid polymers. Among these, poly(meth)acrylic acid (salt)-based water-absorbing resins using (meth)acrylic acid and / or its salt as the main monomer component are most widely produced industrially from the viewpoint of water-absorbing performance.

[0003] As parameters indicating the desired characteristics of such poly(meth)acrylic acid (salt)-based water absorbent resins, many parameters are known, such as water absorption capacity without load (CRC), water absorption capacity under load (AAP), water absorption rate (FSR / vortex), liquid permeability without load, liquid permeability under load, impact resistance, urine resistance, fluidity, gel strength, coloring resistance, particle size, etc. Furthermore, many parameter measurement methods have been proposed from various viewpoints for the same parameter, for example, water absorption capacity without load. Water absorbent resins that have been developed with attention to these many characteristics have a problem that, even if the many characteristics (for example, "water absorption capacity without load (CRC)" and "water absorption capacity under load (AAP)" etc.) are controlled, it is still difficult to say that they exhibit sufficient performance when actually used in absorbents such as paper diapers.

[0004] As a technique for controlling absorbency against pressure (AAP), for example, Patent Document 1 discloses a pressure absorbency index, which is the sum of absorbency under four different pressure loads, and discloses a crosslinked, hydrophilic, highly swellable hydrogel based on a polymerized monomer or a graft polymer, which is characterized by having a pressure absorbency index of <100 and a vertical absorption of at least 12 g / g under a pressure of 1922.8 Pa. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2002-536471 Summary of the Invention [Problem to be solved by the invention]

[0006] However, when a water-absorbent resin is actually used as an absorbent body of an absorbent article such as a disposable diaper, loads of various magnitudes are applied and the loads change in a short period of time. Therefore, in the above-mentioned conventional water-absorbent resin, in which the total of evaluation results under a single pressure load condition is used as an index, there are cases where insufficient absorption capacity occurs during actual use, and there is room for improvement.

[0007] An object of one aspect of the present invention is to provide a water-absorbent resin that, when used in an absorbent body of an absorbent article such as a disposable diaper, can realize an absorbent article that exhibits stable and excellent absorption capacity even under various loads. [Means for solving the problem]

[0008] An embodiment of the present invention includes the following configuration.

[0009] [1] A particulate poly(meth)acrylic acid (salt)-based water-absorbing resin having an absorption capacity against pressure fluctuations calculated by the following formula (1) of 76.0 g / g or more.

[0010] Absorption capacity for pressure change [g / g] = {Absorption capacity for pressure change from 0.05 psi to 0.7 psi (A) [g / g]} + {Absorption capacity for pressure change from 0.7 psi to 0.05 psi (B) [g / g]} Equation (1) [2] The poly(meth)acrylic acid (salt)-based water-absorbing resin according to [1], which has an absorption capacity (A) of 34.0 g / g or more with respect to a pressure change from a pressure of 0.05 psi to a pressure of 0.7 psi.

[0011] [3] The poly(meth)acrylic acid (salt)-based water-absorbing resin according to [1] or [2], having an absorption capacity (B) of 44.0 g / g or more with respect to a pressure change from a pressure of 0.7 psi to a pressure of 0.05 psi.

[0012] [4] The poly(meth)acrylic acid (salt)-based water-absorbing resin according to any one of [1] to [3], which contains water-insoluble inorganic fine particles.

[0013] [5] The specific surface area of ​​the water-insoluble inorganic fine particles is 100 m 2 The poly(meth)acrylic acid (salt)-based water-absorbing resin according to any one of [1] to [4], wherein the water-absorbing capacity is less than 1000 g / g. Effect of the Invention

[0014] According to one aspect of the present invention, it is possible to provide a water-absorbent resin that can realize an absorbent article that exhibits stable and excellent absorption capacity when actually used in an absorbent body of an absorbent article such as a disposable diaper. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a perspective view showing the external configuration of an apparatus for measuring the absorption capacity against pressure fluctuations. [Diagram 2] FIG. 1 is a cross-sectional view showing an apparatus for measuring the absorption capacity against pressure fluctuations. [Diagram 3] 1A to 1C are plan views showing the process of producing an absorbent body for evaluation produced in an example. [Figure 4] FIG. 2 is a cross-sectional view of an absorbent body for evaluation produced in the examples. [Diagram 5] FIG. 2 is a schematic diagram of a roll-type crushing device used in the crushing step in one embodiment of the present invention. [Figure 6] FIG. 2 is a schematic diagram showing a pair of rolls in a roll-type grinding device used in a grinding step in one embodiment of the present invention, where 2001 is a pair of rolls in which grooves are provided on the surface of both rolls, and 2002 is a pair of rolls in which grooves are provided on the surface of one roll and no grooves are provided on the surface of the other roll. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will be described below with reference to the best mode. It should be understood that the terms used in this specification are used in the sense commonly used in the art unless otherwise specified. Therefore, unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as commonly understood by those skilled in the art to which this invention belongs. In the event of a conflict, this specification (including definitions) shall prevail. The present invention is not limited to the following embodiments, and various modifications may be made within the scope of the claims.

[0017] [1] Definitions of terms (1-1) “Water-absorbing resin” The "water-absorbent resin" in the present invention refers to a water-swellable, water-insoluble polymer gelling agent that satisfies the following physical properties: "Water-swellable" refers to a polymer gelling agent that satisfies the physical properties of CRC of 5 g / g or more as specified in ERT441.2-02, and "water-insoluble" refers to a polymer gelling agent that satisfies the physical properties of Ext of 50 wt% or less as specified in ERT470.2-02.

[0018] The water-absorbing resin can be appropriately designed according to its application, and is not particularly limited, but is preferably a hydrophilic cross-linked polymer obtained by cross-linking an unsaturated monomer having a carboxyl group. The water-absorbing resin is not limited to a form in which the total amount (100% by weight) is a polymer, and may be a water-absorbing resin composition containing additives and the like within a range that satisfies the physical properties (CRC, Ext). Furthermore, the water-absorbing resin in the present invention is not limited to a final product, and may refer to an intermediate product in the manufacturing process of the water-absorbing resin (for example, a hydrogel-like cross-linked polymer after polymerization, a dried polymer after drying, a water-absorbing resin before surface cross-linking, a water-absorbing resin after surface cross-linking, a water-absorbing resin after granulation, etc.), and all of these are collectively referred to as "water-absorbing resin" together with the water-absorbing resin composition. The shape of the water-absorbing resin is not particularly limited, and examples thereof include sheet-like, fibrous, film-like, and particulate shapes, but particulate water-absorbing resins are preferred in the present invention.

[0019] (1-2) "Poly(meth)acrylic acid (salt)-based water-absorbent resin" In the present invention, the term "poly(meth)acrylic acid (salt)-based water-absorbing resin" refers to a water-absorbing resin that contains an arbitrary graft component and is mainly composed of a repeating unit derived from (meth)acrylic acid and / or a salt thereof (hereinafter referred to as "(meth)acrylic acid (salt)"). The poly(meth)acrylic acid (salt)-based water-absorbing resin is a water-absorbing resin that contains preferably 50 to 100 mol%, more preferably 70 to 100 mol%, further preferably 90 to 100 mol%, and particularly preferably substantially 100 mol% of (meth)acrylic acid (salt) relative to the total monomers (excluding crosslinking agents) used in polymerization.

[0020] (1-3) "EDANA" and "ERT" "EDANA" is an abbreviation of European Disposables and Nonwovens Associations, and "ERT" is an abbreviation of EDANA Recommended Test Methods, a European standard (almost a global standard) for measuring the properties of water-absorbent resins. In the present invention, unless otherwise specified, the physical properties of the water-absorbent resin are measured in accordance with the original ERT (revised in 2002 / publicly known document).

[0021] (1-4)Other In this specification, the range "X to Y" means "X or more and Y or less". In this specification, "weight" and "mass", "weight %" and "mass %, "parts by weight" and "parts by mass" are treated as synonyms. In this specification, unless otherwise specified, "ppm" means "ppm by mass". In this specification, "acid (salt)" means "acid and / or its salt", and "(meth)acrylic" means "acrylic and / or methacrylic". In this specification, the unit of volume "liter" may be written as "l" or "L".

[0022] [2] Water-absorbing resin (2-1) Absorption capacity against pressure fluctuations The present inventors conducted intensive studies to solve the above problems, and came up with the idea of ​​using a new index called "absorbency against pressure fluctuations" assuming a state where various loads are applied and the loads change in a short time (when standing / sitting, or turning over in bed temporarily applies a high load to the absorbent body attachment site). The inventors then found that an absorbent article using a water-absorbent resin having a predetermined range of "absorbency against pressure fluctuations" can achieve stable absorbency during actual use, and completed the present invention. The "absorbency against pressure fluctuations" in the present invention is a physical property value that indicates absorbency assuming a state where the load changes during actual use, which is expressed as the sum of the absorbency (A) of the water-absorbent resin when the pressure changes from low pressure to high pressure (from 0.05 psi to 0.7 psi) and the absorbency (B) of the water-absorbent resin when the pressure changes from high pressure to low pressure (from 0.7 psi to 0.05 psi), and is specifically a value measured by the measurement method described in the examples.

[0023] The "absorption capacity against pressure fluctuation" of the water-absorbent resin according to one embodiment of the present invention is preferably 76.0 g / g or more, more preferably 77.0 g / g or more, and even more preferably 78.0 g / g or more. The upper limit of the "absorption capacity against pressure fluctuation" is not particularly limited, but is preferably 90 g / g or less, and may be 85 g / g or less. If the "absorption capacity against pressure fluctuation" of the water-absorbent resin according to one embodiment of the present invention is 76.0 g / g or more, it is preferable because when such a water-absorbent resin is used as an absorbent body of an absorbent article and actually used, an absorbent article that exhibits stable and excellent absorption capacity even when various loads are applied can be realized.

[0024] The absorbency (A) of the water-absorbent resin according to one embodiment of the present invention against pressure fluctuation from low pressure to high pressure is preferably 34.0 g / g or more, more preferably 35.0 g / g or more, and even more preferably 36.0 g / g or more. The upper limit of the absorbency (A) is not particularly limited, but is preferably 45 g / g or less, and may be 40 g / g or less. The absorbency (B) of the water-absorbent resin according to one embodiment of the present invention against pressure fluctuation from high pressure to low pressure is preferably 44.0 g / g or more, more preferably 44.5 g / g or more, and even more preferably 45.0 g / g or more. The upper limit of the absorbency (B) is not particularly limited, but is preferably 55 g / g or less, and may be 50 g / g or less. When the absorbency (A) of the water-absorbent resin against pressure fluctuation from low pressure to high pressure is 34.0 g / g or more, and / or when the absorbency (B) of the water-absorbent resin against pressure fluctuation from high pressure to low pressure is 44.0 g / g or more, when such a water-absorbent resin is used in an absorbent body of an absorbent article and actually used, it is preferable because an absorbent article that exhibits stable and excellent absorbency even under various loads can be realized.

[0025] (2-2) Shape of water-absorbent resin In one embodiment of the present invention, the water absorbent resin is preferably in the form of particles, and specific examples thereof include particles in the form of irregularly crushed shapes, spherical particles, football-shaped particles, aggregated particles, granulated particles, etc. Here, the spherical shape is not limited to a perfect sphere, and also includes a nearly spherical shape with an aspect ratio of 1.0 to 1.2.

[0026] (2-3) Additives In one embodiment of the present invention, the water-absorbent resin may contain additives to exhibit various functions. Examples of the additives include surfactants, compounds having phosphorus atoms, oxidizing agents, organic reducing agents, water-insoluble inorganic fine particles, organic powders (e.g., metal soaps, etc.), deodorants, antibacterial agents, pulp, thermoplastic fibers, etc.

[0027] Examples of the water-insoluble inorganic fine particles include silicic acid (salt) such as natural zeolite and synthetic zeolite; kaolin; talc; clay; bentonite; calcium phosphate; barium phosphate; silicic acid or its salt; clay; diatomaceous earth; silica gel; zeolite; hydroxyapatite; hydrotalcite; vermiculite; perlite; isolite; activated clay; quartz sand; quartz stone; strontium ore; fluorite; bauxite; metal oxides such as silica (silicon dioxide) and titanium oxide; composite hydrated oxides containing zinc and silicon, or zinc and aluminum (for example, as exemplified in International Publication No. 2005 / 010102). The water-absorbing resin according to one embodiment of the present invention is more preferably, among these water-insoluble inorganic fine particles, particularly containing hydrotalcite; kaolin, talc, zeolite, etc. Hydrogen-absorbing resins containing these water-insoluble inorganic fine particles are preferred because they have a good water absorption capacity under pressure.

[0028] From the viewpoint of absorption performance under load, the content of the water-insoluble inorganic fine particles is preferably 0.01 to 5.00 parts by weight, more preferably 0.05 to 3.00 parts by weight, even more preferably 0.10 to 1.00 parts by weight, and particularly preferably 0.20 to 0.50 parts by weight, relative to 100 parts by weight of the water absorbent resin.

[0029] The water-insoluble inorganic fine particles have a size smaller than that of the water-absorbent resin particles. The average particle size of the water-insoluble inorganic fine particles is preferably 0.01 to 50.00 μm, and may be 0.10 to 30.00 μm, or 1.00 to 20.00 μm. Here, the average particle size can be measured by a pore electrical resistance method or a laser diffraction / scattering method depending on the characteristics of the particles.

[0030] The specific surface area of ​​the water-insoluble inorganic fine particles is preferably 100 m 2 / g, more preferably less than 95m 2 / g, and more preferably less than 90m 2 / g, less than 80m 2 / g, and particularly preferably less than 50m 2The lower limit of the specific surface area of ​​the water-insoluble inorganic fine particles is not particularly limited, but is preferably less than 0.1 m 2 / g or more, more preferably 1.0m 2 / g or more. Here, the specific surface area can be measured by the BET method. 2 If it is less than 1 / g, the absorption performance under load becomes good, which is preferable.

[0031] (2-4)CRC "CRC" is an abbreviation for Centrifuge Retention Capacity, and means the water absorption capacity of a water-absorbent resin under no pressure. In this specification, CRC is measured in accordance with the EDANA method (ERT441.2-02).

[0032] From the viewpoint of water absorption properties when used in sanitary materials, the CRC of the water absorbent resin according to one embodiment of the present invention is preferably 15 g / g or more, more preferably 20 g / g or more, and even more preferably 25 g / g or more. The upper limit of the CRC of the water absorbent resin is not particularly limited, but is preferably 50 g / g or less.

[0033] (2-5)Ext "Ext" is an abbreviation for Extractables, and means the amount of extractables extracted from a water-absorbent resin. In this specification, Ext is measured in accordance with the EDANA method (ERT470.2-02).

[0034] (2-6) AAP "AAP" is an abbreviation of Absorption Against Pressure, and means the water absorption capacity of a water absorbent resin under pressure. In the present invention, AAP is measured in accordance with the EDANA method (ERT442.2-02) except that the load condition is changed to 4.83 kPa (0.7 psi). Specifically, 0.9 g of a water absorbent resin is swollen under a pressure of 4.83 kPa for 1 hour using a 0.9 mass% sodium chloride aqueous solution, and then AAP (water absorption capacity against pressure) (unit: g / g) is measured.

[0035] The AAP of the water-absorbent resin according to one embodiment of the present invention is preferably 10 g / g or more, more preferably 12 g / g or more, and even more preferably 23 g / g or more, from the viewpoint of water absorption properties when used in sanitary materials. The upper limit of the AAP of the water-absorbent resin is not particularly limited, but is preferably 40 g / g or less.

[0036] (2-7) Moisture content "Moisture content" is measured in accordance with the EDANA method (ERT430.2-02), except that the sample amount is changed to 1.0 g and the drying temperature is changed to 180°C.

[0037] (2-8) Mass average particle diameter (D50) The "mass-average particle diameter (D50)" is measured in accordance with "(3) Mass-Average Particle Diameter (D50) and Logarithmic Standard Deviation (σζ) of Particle Diameter Distribution" described in columns 27 and 28 of U.S. Pat. No. 7,638,570.

[0038] The mass average particle diameter (D50) of the water absorbent resin according to one embodiment of the present invention is preferably 250 μm to 800 μm, more preferably 300 μm to 700 μm, even more preferably 310 μm to 600 μm, and particularly preferably 320 μm to 500 μm, from the viewpoint of ease of handling. In addition, the ratio of particles having a particle diameter of less than 150 μm is preferably 40 mass% or less, more preferably 30 mass% or less, even more preferably 20 mass% or less, and particularly preferably 10 mass% or less, from the viewpoint of reducing dust. If the mass average particle diameter is 250 μm or more, there is an advantage that there is even less dust and the handling is good. In addition, if the mass average particle diameter is 800 μm or less, a decrease in the rate of absorption of body fluids (e.g., urine, blood, etc.) is prevented, and the resin is suitable for use in paper diapers and the like having a high water absorption rate.

[0039] (2-9) Bulk density "Bulk density" is measured in accordance with the EDANA method (ERT460.2-02).

[0040] The water-absorbent resin according to one embodiment of the present invention has a bulk density of preferably 0.60 g / mL to 1.00 g / mL, more preferably 0.62 g / mL to 0.90 g / mL, and further preferably 0.64 g / mL to 0.80 g / mL. If the bulk density is 0.60 to 1.00 g / mL, a decrease in the absorption rate of body fluids (e.g., urine, blood, etc.) in the water-absorbent resin is prevented, and the water-absorbent resin is suitable for use in paper diapers with a high water absorption rate.

[0041] (2-10) Water absorption rate In the present invention, the "water absorption rate" of the water absorbent resin means the "water absorption rate by the Vortex method." The "water absorption rate by the Vortex method" means the time required for the stirrer tip to be covered with the test liquid when 2.0 g of the water absorbent resin is added to 50 g of a 0.9% by mass aqueous sodium chloride solution stirred at 600 rpm with a stirrer tip.

[0042] A water-absorbent resin having excellent "water absorption speed" is preferable because it can instantly absorb liquid and reduce the amount of liquid returning when used as an absorbent article. The water-absorbent resin according to one embodiment of the present invention has a water-absorption speed of preferably 45 seconds or less, more preferably 40 seconds or less, and even more preferably 30 seconds or less. There is no particular lower limit for the water-absorption speed, but it is 10 seconds or more, preferably 15 seconds or more, and even more preferably 20 seconds or more.

[0043] (2-11)Surface tension The "surface tension" of the water-absorbent resin is measured by the method described in WO2015 / 129917, specifically, the method described in the Examples.

[0044] The surface tension of the water absorbent resin powder according to one embodiment of the present invention is preferably in the range of 60 to 75 mN / m, more preferably in the range of 62 to 74 mN / m, and further preferably in the range of 65 to 72 mN / m.

[0045] [3] Method for producing water-absorbent resin The process for producing the water-absorbent resin according to one embodiment of the present invention will be described below.

[0046] (3-1) Monomer aqueous solution preparation process This step is a step of preparing an aqueous solution containing (meth)acrylic acid (salt) as a main component (hereinafter referred to as "aqueous monomer solution"). Note that, although a slurry liquid of a monomer can be used within a range in which the water absorption performance of the obtained water absorbent resin is not deteriorated, for the sake of convenience, the aqueous monomer solution will be described in this section.

[0047] The "main component" means that the amount (content) of (meth)acrylic acid (salt) used is preferably 50 mol % or more, more preferably 70 mol % or more, and further preferably 90 mol % or more (upper limit: 100 mol %), based on the total monomers (excluding the internal crosslinking agent) used in the polymerization reaction of the water absorbent resin.

[0048] ((Meth)acrylic acid (salt)) In the method for producing a water-absorbent resin according to one embodiment of the present invention, from the viewpoints of the physical properties and productivity of the resulting water-absorbent resin, a (meth)acrylic acid (salt) is used as a monomer.

[0049] The "(meth)acrylic acid" may be any known (meth)acrylic acid, and may contain, as a polymerization inhibitor, preferably methoxyphenols, more preferably p-methoxyphenol, preferably at 200 ppm or less, more preferably 10 to 160 ppm, and even more preferably 20 to 100 ppm, from the viewpoint of the polymerizability of (meth)acrylic acid and the color tone of the water-absorbing resin. In addition, as for impurities in (meth)acrylic acid, the compounds described in U.S. Patent Application Publication No. 2008 / 0161512 are also applicable to the present invention.

[0050] The "(meth)acrylic acid salt" is a neutralized product obtained by neutralizing the (meth)acrylic acid with the following basic composition. As the (meth)acrylic acid salt, a commercially available (meth)acrylic acid salt (e.g., sodium (meth)acrylate, etc.) may be used, or a salt obtained by neutralization in a water absorbent resin manufacturing plant may be used.

[0051] (Basic Composition) In one embodiment of the present invention, the term "basic composition" refers to a composition containing a basic compound. Examples of basic compositions include commercially available aqueous sodium hydroxide solutions.

[0052] Specific examples of the basic compound include carbonates and hydrogen carbonates of alkali metals, hydroxides of alkali metals, ammonia, organic amines, etc. Among these, from the viewpoint of the physical properties of the resulting water absorbent resin, it is preferable that the basic compound is strongly basic. That is, it is preferable to use hydroxides of alkali metals (sodium hydroxide, potassium hydroxide, lithium hydroxide, etc.), and more preferable to use sodium hydroxide.

[0053] (neutralization) In one embodiment of the present invention, the neutralization can be selected from or used in combination with neutralization of (meth)acrylic acid (before polymerization) and neutralization of a hydrogel crosslinked polymer obtained by crosslinking and polymerizing (meth)acrylic acid (after polymerization) (hereinafter referred to as "post-neutralization"). These neutralization methods may be continuous or batch-wise, and are not particularly limited, but the continuous method is preferred from the viewpoint of production efficiency, etc.

[0054] Regarding the conditions such as the neutralization apparatus, neutralization temperature, and residence time, the conditions described in WO 2009 / 123197 and US Patent Application Publication No. 2008 / 0194863 are applied.

[0055] In one embodiment of the present invention, the neutralization rate is preferably 10 to 90 mol%, more preferably 40 to 85 mol%, further preferably 50 to 80 mol%, and particularly preferably 60 to 75 mol% based on the acid group of the monomer. If the neutralization rate is less than 10 mol%, the water absorption capacity may be significantly reduced. On the other hand, if the neutralization rate is more than 90 mol%, a water absorbent resin having a high water absorption capacity under pressure may not be obtained.

[0056] The neutralization rate is the same whether it is neutralized before or after polymerization. The neutralization rate of the water absorbent resin as a final product is also applied to the neutralization rate. Note that a neutralization rate of 75 mol% means a mixture of 25 mol% (meth)acrylic acid and 75 mol% (meth)acrylic acid salt. The mixture may also be referred to as a partially neutralized product of (meth)acrylic acid.

[0057] (Other monomers) In the present specification, the term "other monomer" refers to a monomer other than the (meth)acrylic acid (salt). The other monomer can be used in combination with the (meth)acrylic acid (salt) to produce a water-absorbing resin.

[0058] The other monomer may be a water-soluble unsaturated monomer or a hydrophobic unsaturated monomer. Specifically, the compounds described in U.S. Patent Application Publication No. 2005 / 0215734 (excluding (meth)acrylic acid) are also applicable to the present invention.

[0059] (Internal crosslinking agent) Examples of the internal crosslinking agent used in the present invention include N,N'-methylenebis(meth)acrylamide, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane di(meth)acrylate, glycerin tri(meth)acrylate, glycerin acrylate methacrylate, ethylene oxide modified trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, and the like. Examples of the internal crosslinking agent include hexa(meth)acrylate, triallyl cyanurate, triallyl isocyanurate, triallyl phosphate, triallylamine, poly(meth)allyloxyalkane, (poly)ethylene glycol diglycidyl ether, glycerol diglycidyl ether, ethylene glycol, polyethylene glycol, propylene glycol, glycerin, 1,4-butanediol, pentaerythritol, ethylenediamine, ethylene carbonate, propylene carbonate, polyethyleneimine, glycidyl (meth)acrylate, etc. From the viewpoint of reactivity, one or more types of the internal crosslinking agent can be selected.

[0060] From the viewpoint of the water absorption performance of the obtained water absorbent resin, the internal crosslinking agent is preferably a compound having two or more polymerizable unsaturated groups, more preferably a compound having two or more polymerizable unsaturated groups that are thermally decomposable at a drying temperature described later, and further preferably a compound having two or more polymerizable unsaturated groups that have a (poly)alkylene glycol structural unit.

[0061] The polymerizable unsaturated group is preferably an allyl group or a (meth)acrylate group. Among these, from the viewpoint of water absorption performance, a (meth)acrylate group is more preferable. The (poly)alkylene glycol structural unit is preferably a polyethylene glycol from the viewpoint of water absorption performance. The number n of the (poly)alkylene glycol structural unit is preferably 1 to 100, more preferably 6 to 50.

[0062] The amount of the internal crosslinking agent used is preferably 0.0001 to 10 mol%, more preferably 0.001 to 1 mol%, based on the total amount of monomers. By setting the amount used within the above range, a desired water absorbent resin can be obtained. When the amount used is 0.0001 mol% or more, the gel strength tends to increase and the water-soluble content tends to decrease, and when the amount used is 10 mol% or less, the water absorption capacity tends to increase, which is preferable.

[0063] In one embodiment of the present invention, the method of adding the internal crosslinking agent is not particularly limited, but includes a method of adding the internal crosslinking agent to a monomer aqueous solution in advance and causing a crosslinking reaction simultaneously with polymerization, a method of adding an internal crosslinking agent during or after polymerization and causing post-crosslinking, a method of radical crosslinking using a radical polymerization initiator, and a method of radiation crosslinking using active energy rays such as electron beams and ultraviolet rays. Among these, from the viewpoint of reactivity, a method of adding the internal crosslinking agent to a monomer aqueous solution in advance and causing a crosslinking reaction simultaneously with polymerization is preferred. The above methods may be used in combination as appropriate within a range that does not impair the effects of the present invention.

[0064] (Other substances added to the monomer aqueous solution) In one embodiment of the present invention, from the viewpoint of improving the physical properties of the resulting water-absorbent resin, the following substances may be added during preparation of the aqueous monomer solution.

[0065] Specifically, hydrophilic polymers such as starch, starch derivatives, cellulose, cellulose derivatives, polyvinyl alcohol, poly(meth)acrylic acid (salt), and crosslinked poly(meth)acrylic acid (salt) may be added in an amount of preferably 50% by weight or less, more preferably 20% by weight or less, even more preferably 10% by weight or less, and particularly preferably 5% by weight or less (the lower limit is 0% by weight) based on the total monomers used in the polymerization (excluding the crosslinking agent).

[0066] Furthermore, foaming agents such as carbonates, azo compounds, and bubbles, surfactants, chelating agents, chain transfer agents, etc. may be added in an amount of preferably 5% by weight or less, more preferably 1% by weight or less, and even more preferably 0.5% by weight or less (the lower limit is 0% by weight) based on the total monomers used in the polymerization (excluding the crosslinking agent).

[0067] The substance may be added to the aqueous monomer solution or during the polymerization. The above-mentioned adding forms may be used in combination as appropriate within the scope of not impairing the effects of the present invention.

[0068] When a water-soluble resin or a water-absorbent resin is used as the hydrophilic polymer, a graft polymer or a water-absorbent resin composition (e.g., a starch-acrylic acid polymer, a PVA-acrylic acid polymer, etc.) is obtained. These polymers and water-absorbent resin compositions are also included in the category of the water-absorbent resin of the present invention.

[0069] (monomer component concentration) In this step, when preparing the aqueous monomer solution, the above-mentioned substances are added. The concentration of the monomer component in the aqueous monomer solution is not particularly limited, but is preferably 10 to 80% by weight, more preferably 20 to 75% by weight, and further preferably 30 to 70% by weight, from the viewpoint of the physical properties of the water absorbent resin.

[0070] When aqueous solution polymerization or reversed-phase suspension polymerization is employed, a solvent other than water can be used in combination as necessary. In this case, the type of the solvent is not particularly limited.

[0071] The "concentration of the monomer component" is a value calculated by the following formula (2), and the weight of the aqueous monomer solution does not include the weight of a graft component such as starch, fine powder of a water absorbent resin generated from a production process and added for reuse, and the weight of a hydrophobic solvent in reversed-phase suspension polymerization.

[0072] Monomer component concentration (weight%) = {(weight of monomer component) / (weight of monomer aqueous solution)} × 100... Equation (2).

[0073] (3-2) Polymerization process This step is a step of polymerizing the aqueous monomer solution obtained in the aqueous monomer solution preparation step to obtain a hydrous gel crosslinked polymer (hereinafter referred to as "hydrous gel").

[0074] (Polymerization initiator) The polymerization initiator used in one embodiment of the present invention is not particularly limited since it is appropriately selected depending on the polymerization form, etc., but examples thereof include a thermally decomposable polymerization initiator, a photodecomposable polymerization initiator, or a redox-based polymerization initiator used in combination with a reducing agent that promotes the decomposition of these polymerization initiators. Specifically, one or more of the polymerization initiators disclosed in U.S. Pat. No. 7,265,190 are used. From the viewpoint of the handling of the polymerization initiator and the physical properties of the water-absorbing resin, preferably a peroxide or an azo compound, more preferably a peroxide, and even more preferably a persulfate is used.

[0075] The amount of the polymerization initiator used is preferably 0.001 to 1 mol %, more preferably 0.001 to 0.5 mol %, based on the total monomers used in the polymerization (excluding the crosslinking agent), and the amount of the reducing agent used is preferably 0.0001 to 0.02 mol %, based on the total monomers used in the polymerization (excluding the crosslinking agent).

[0076] Instead of the polymerization initiator, the polymerization reaction may be carried out by irradiation with active energy rays such as radiation, electron beams, and ultraviolet rays, and these active energy rays may be used in combination with the polymerization initiator.

[0077] (polymerization form) The polymerization form applied in one embodiment of the present invention is not particularly limited, but examples thereof include aqueous solution polymerization, reversed-phase suspension polymerization, droplet polymerization, bulk polymerization, precipitation polymerization, etc. Among these, aqueous solution polymerization or reversed-phase suspension polymerization is preferred from the viewpoints of ensuring good water absorption properties and easiness of polymerization control.

[0078] (3-3) Gel granulation process In this step, for example, when reverse phase suspension polymerization is employed, the hydrogel crosslinked polymer separated from the hydrophobic organic solvent after polymerization is sized using a gel sizing device having an extrusion section and a perforated plate. This results in a sized hydrogel crosslinked polymer (hereinafter, the hydrogel after gel sizing is referred to as "sized gel"). The gel sizing step is an optional step. By including the gel sizing step, it becomes easier to control the absorption capacity of the water absorbent resin against pressure fluctuations.

[0079] For gel sizing conditions and embodiments other than those described above, the contents disclosed in [2-5. Gel sizing process] of JP 2022-132183 A are preferably applied to the present invention.

[0080] (3-4) Gel crushing process In this step, for example, when aqueous solution polymerization is employed, the hydrogel obtained in the polymerization step is gel-pulverized with a gel pulverizer (e.g., a screw extruder such as a kneader or meat chopper, a cutter mill, etc.) to obtain a particulate hydrogel (hereinafter referred to as "particulate hydrogel"). When the polymerization step is kneader polymerization, the polymerization step and the gel-pulverization step are carried out simultaneously. Regarding gel-pulverization conditions and forms other than those described above, the contents disclosed in International Publication No. 2011 / 126079 are preferably applied to the present invention.

[0081] (3-5) Drying process This step is a step of drying the particulate hydrogel obtained in the polymerization step and / or gel granulation step and / or gel crushing step to a desired resin solid content to obtain a dry polymer. The resin solid content is determined from the loss on drying (weight change when 1 g of water-absorbent resin is heated at 180°C for 3 hours), and is preferably 80% by weight or more, more preferably 85 to 99% by weight, and even more preferably 90 to 98% by weight.

[0082] The method for drying the particulate hydrogel is not particularly limited, and examples thereof include heat drying, hot air drying, reduced pressure drying, fluidized bed drying, stirring drying, infrared drying, microwave drying, drum dryer drying, azeotropic dehydration with a hydrophobic organic solvent, high humidity drying using high temperature water vapor, etc. Among these, stirring drying is preferred from the viewpoints of drying efficiency and shape retention.

[0083] (3-6) Hydrophilic treatment process This process is a process of hydrophilizing the water-absorbent resin with an organic solvent. This can enhance the effect of the surface cross-linking process (increasing the absorbency of the water-absorbent resin under pressure and reducing the amount of reversion). In addition, the water absorption rate increases because the hydrophilicity of the surface of the water-absorbent resin increases. The hydrophilization process may be performed after the surface cross-linking process described below, or may be performed before the surface cross-linking process.

[0084] The specific hydrophilization method varies depending on the cause of the formation of hydrophobic parts on the surface of the water-absorbent resin. For example, when the water-absorbent resin is produced by reversed-phase suspension polymerization, the surfactant used as a dispersant during polymerization is the cause of the hydrophobicity, so it is preferable to wash it off, and more preferably to wash it off with an organic solvent.

[0085] The organic solvent is not particularly limited as long as it can wash the surfactant, but in order to enhance the washing effect, it is preferable to use an organic solvent that does not swell the water-absorbing resin. The preferred swelling ratio of the water-absorbing resin during the treatment is less than 2 times. As the organic solvent, not only hydrophilic organic solvents but also hydrophobic organic solvents can be used. Specific examples of hydrophilic organic solvents include lower alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, and t-butyl alcohol; ketones such as acetone; ethers such as dioxane and tetrahydrofuran; amides such as N,N-dimethylformamide; and sulfoxides such as dimethyl sulfoxide. Examples of hydrophobic organic solvents include aliphatic hydrocarbons such as n-pentane, n-heptane, n-hexane, and n-octane; alicyclic hydrocarbons such as cyclohexane, methylcyclohexane, cyclooctane, and decalin; halogenated hydrocarbons such as chlorobenzene, bromobenzene, carbon tetrachloride, and 1,2-dichloroethane; and aromatic hydrocarbons such as benzene, toluene, and xylene. Among these, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-heptane, n-hexane, and cyclohexane are preferably used.

[0086] In one embodiment of the present invention, when the water-absorbent resin is hydrophilized with the organic solvent, it is preferable to bring the organic solvent into contact with the water-absorbent resin in a heated state, since the absorbency under pressure and the reversion amount may be further improved. The heating temperature is preferably equal to or lower than the boiling point of the organic solvent, and is generally about 40 to 120°C, depending on the type of organic solvent used. The hydrophilization treatment is preferably performed in a state where the water-absorbent resin is dry. If the hydrophilization treatment is performed in a state where the water-absorbent resin is wetted with an organic solvent or water, the water-absorption speed or water-absorption capacity may be reduced when crosslinking is performed near the surface. Therefore, it is preferable to perform the hydrophilization treatment in a state where the water-absorbent resin obtained by reversed-phase suspension polymerization or aqueous solution polymerization is filtered and dried to remove the polymerization solvent and water.

[0087] (3-7) Crushing process The pulverization step is a step in which the particulate dried polymer obtained through the drying step is pulverized to adjust the particle size and shape to a desired value.

[0088] In one embodiment of the present invention, it is important to precisely control the grinding conditions in this grinding step.

[0089] (Crushing device) Various types of pulverizers can be used in this step, but in one embodiment of the present invention, it is preferable to use a specific roll-type pulverizer because it is easy to adjust the particulate dry polymer to an optimal shape. As the specific roll-type pulverizer, for example, a roll-type pulverizer consisting of a pair of rolls, at least one of the pair of rolls has a groove (longitudinal groove) extending parallel to the roll rotation direction on the surface, is used. By passing the particulate dry polymer through the clearance between the pair of rolls provided in this specific roll-type pulverizer, the particulate dry polymer is compressed, sheared, or compacted between the rolls, thereby pulverizing the particulate dry polymer. Examples of such specific roll-type pulverizers include a roll granulator (manufactured by Nippon Granulator Co., Ltd.), a roll granulator (manufactured by Kurimoto Iron Works Co., Ltd.), and a GRAN-U-LIZER (manufactured by MPE Co., Ltd.). If this specific roll-type pulverizer is used, the pulverizing force is mild, so that the generation of particles with crushed flat surfaces exposed can be suppressed. Therefore, a crushed product with a large surface area can be obtained. Therefore, a water-absorbent resin having a large surface area can be obtained. Such a water-absorbent resin having a large surface area has a high water absorption rate and can absorb liquid in a short time.

[0090] On the other hand, in the pair of rolls, those in which there are no grooves on the surfaces of both rolls, and those in which even if there are grooves, the grooves extend perpendicularly to the roll rotation direction, etc. are severely damaged, and hence many smooth surfaces are generated on the surface of the water absorbent resin after pulverization, which is not preferable.

[0091] Here, the pulverizing device used in the pulverizing step before forming a granulated product or an aggregate of primary particles of a water absorbent resin is not particularly limited, but it is preferable to select the specific roll type pulverizing device (e.g., roll granulator) described above.

[0092] FIG. 1 shows a schematic diagram of the specific roll-type grinding device used in the grinding step in one embodiment of the present invention. As shown in FIG. 1, the roll-type grinding device 200 includes a pipe 201 for supplying a particulate dried polymer to the device 200, an inlet 202 for supplying the dried polymer into the device 200, and a pair of rolls 203 for grinding the supplied dried polymer. These are arranged in this order in a direction from top to bottom. The "direction from top to bottom" is not limited to the vertical direction, but is a concept that may also include an oblique direction. The pair of rolls 203 is composed of two rolls 203a and 203b. In the roll-type grinding device, at least one pair (two rolls) of rolls may be provided, and for example, two pairs (four rolls) or more of rolls may be provided in a vertical arrangement. For example, when two pairs of rolls are arranged in a vertical arrangement, the dried polymer passes between the pair of rolls located at the top and is ground, and then passes between the pair of rolls located at the bottom and is ground.

[0093] The dried polymer 20a introduced between the rolls 203 passes between the rolls 203a and 203b of the pair of rolls 203, and becomes the water absorbent resin 20b which is a pulverized product of the dried polymer. Although not shown, the roll-type pulverizing device 200 may be provided with a feeder between the introduction port 202 and the pair of rolls 203 for quantitative supply.

[0094] The specific roll-type grinding device has grooves (uneven pattern) on the surface of at least one of the pair of rolls. The groove means unevenness on the roll surface, and in the present invention, means grooves arranged in a striped pattern. The grooves are arranged in a plurality of rows in the roll width direction (the direction of the rotation axis of the roll). That is, in the roll-type grinding device, a plurality of grooves (vertical grooves) extending parallel to the roll rotation direction are arranged in the roll width direction on the surface of at least one of the pair of rolls. Therefore, unevenness (concave and convex portions) is formed on the roll surface extending parallel to the roll rotation direction. As a result, the clearance between the pair of rolls does not substantially change due to the rotation of the rolls at any position in the roll width direction. Since the clearance between the rolls does not change at any position in the roll width direction, it is possible to apply an appropriate force to the dried polymer passing between the rolls, and it is presumed that the particle size of the resulting pulverized product is uniform and a pulverized product having a sharp particle size distribution is obtained. The clearance between the rolls means the distance between a pair of opposing rolls.

[0095] In a preferred embodiment of the manufacturing method of the present invention, grooves are provided on each of the two roll surfaces of the pair of rolls. In this case, it is believed that the clearance between the rolls can be made constant at any position in the roll width direction by meshing the corresponding concaves and convexes provided on the roll surfaces of the two rolls, and thus a constant force can be applied to the dried material being pulverized. Therefore, it is presumed that the particle size of the pulverized material obtained is more uniform, and a pulverized material having a sharper particle size distribution can be obtained. The pair of rolls may be the same shape (groove shape, diameter) or different shapes, but it is preferable to use rolls of the same shape (including symmetrical relationship).

[0096] For example, in one embodiment, the roll type crushing device 200 has grooves (concave and convex) extending parallel to the roll rotation direction on the roll surface of both of the pair of rolls 203. That is, as shown in 2001 in the figure, both of the pair of rolls 203 (rolls 203a, 203b) have concave and convex portions extending parallel to the roll rotation direction of the roll rotation axis A on their roll surfaces. Thus, the convex portions provided on the roll surface of one of the pair of rolls are configured to mesh with the concave portions provided on the roll surface of the other of the pair of rolls by rotation.

[0097] In one embodiment, as shown in 2002 in FIG. 6 , one of the pair of rolls 203 (e.g., roll 203a) has grooves on the roll surface that extend parallel to the roll rotation direction of the roll rotation axis A of the roll, and the other of the pair of rolls (e.g., roll 203b) has a smooth surface (flat surface) without grooves on the roll surface.

[0098] Here, the clearance between the rolls will be described based on 2001 in FIG. 6 and 2002 in FIG. 6. As shown in 2001 in FIG. 6, when grooves are provided on the surfaces of the two rolls 203a and 203b, the clearance d has a constant value d at any position in the roll width direction. Also, as shown in 2002 in FIG. 6, when grooves are provided on the surface of one roll 203a and no grooves are provided on the surface of the other roll 203b, the clearance d has a maximum value (dmax) and a minimum value (dmin) depending on the position in the roll width direction. In both the form of 2001 in FIG. 6 and 2002 in FIG. 6, the grooves provided on the rolls are formed to extend parallel to the roll rotation direction, so that the clearance does not substantially change with the rotation of the rolls.

[0099] In addition, in the longitudinal groove structure, due to circumstances in the manufacture of the roll, transverse grooves (grooves extending in the roll width direction) or convex portions extending in the roll width direction may be formed in a part of the roll. Such grooves or convex portions cause cutouts in some of the longitudinal grooves of the roll. In this case, the presence of some cutouts formed in the longitudinal grooves of the roll causes a change in the clearance at any position in the roll width direction. Here, "not substantially changing with the rotation of the roll" includes "not changing the clearance over a length range of 70% or more of one rotation of the roll, preferably over a length range of 80% or more, more preferably over a length range of 90% or more, and even more preferably over a length range of 95% or more." Therefore, even if a cutout portion exists in a part of the longitudinal grooves of the roll, it is considered to be "not substantially changing with the rotation of the roll" if the above-mentioned provision is satisfied.

[0100] Here, in the embodiment of 2001 in Fig. 6, the clearance d is the same at any position in the roll width direction, whereas in the embodiment of 2002 in Fig. 6, the clearance d differs depending on the position in the roll width direction. In the present invention, even if the clearance d differs depending on the position in the roll width direction, it is sufficient that the clearance d does not substantially change at any position due to the rotation of the roll.

[0101] In the rolls shown in 2001 and 2002 in Fig. 6, the grooves are provided in a shape that extends substantially parallel (0 degrees) to the roll rotation direction. "Substantially parallel" means that grooves inclined at less than ±1° to the roll rotation direction are included in the configuration of the present invention. The inclination angle may be either in the positive or negative direction with respect to the roll rotation direction.

[0102] The minimum clearance value dmin between the rolls can be appropriately determined, and is not particularly limited, but is preferably more than 0 and 3 mm or less. The minimum clearance value dmin between the rolls is more preferably 0.05 to 3 mm, even more preferably 0.05 to 2.5 mm, even more preferably 0.1 to 2 mm, particularly preferably 0.1 to 1.5 mm, and most preferably 0.2 to 1 mm. By arranging a pair of rolls so that the minimum clearance value dmin between the rolls is within the above range, the effect of reducing particles with exposed flat surfaces in the pulverized product can be further exerted. Note that when the minimum clearance value dmin and the maximum clearance value dmax are the same (i.e., in the case of 2001 in FIG. 6), the clearance d is regarded as the minimum clearance value dmin. When two or more pairs of rolls are used in the pulverization process, it is sufficient that the minimum value of the minimum clearance values ​​provided between the rolls is within the above range.

[0103] In addition, when the clearance d varies depending on the position in the roll width direction, as shown by 2002 in Fig. 6, the clearance d at each position is calculated, and the difference between the maximum clearance dmax and the minimum clearance dmin is referred to as the "clearance difference." The clearance difference is not particularly limited, but is preferably 0 to 0.2 mm, more preferably 0 to 0.1 mm, and even more preferably 0 to 0.05 mm.

[0104] The pitch (spacing) of the grooves provided on the roll can be appropriately determined according to the size of the particles to be pulverized. When the pulverized particle size is large, it is preferable to select a large groove pitch, and when the pulverized particle size is small, it is preferable to select a small groove pitch. The groove pitch is not particularly limited, but is preferably 0.1 to 2 mm, more preferably 0.2 to 1.5 mm, and even more preferably 0.3 to 1.2 mm. Here, the groove pitch p means the interval between the crest of any groove and the crest of the adjacent groove, or the interval between the valley of any groove and the valley of the adjacent groove, as shown in 2001 in FIG. 6. For example, when a surface (hereinafter referred to as a "flat portion") parallel to the circumferential direction is provided between the crest and valley of the groove, it means the interval between the crest and crest of adjacent grooves, including the flat portion, or the interval between the valley of adjacent grooves. The pitch of the groove may be different on one roll, but is preferably constant over the entire roll width, and when grooves are provided on both of a pair of rolls, it is preferably constant over the entire pair of rolls.

[0105] The height of the grooves can be appropriately determined and is not particularly limited, but the grooves are preferably provided with a height of 0.1 to 2 mm, more preferably 0.2 to 1.5 mm, and even more preferably 0.3 to 1 mm. Here, the height of the grooves means the difference in height between the apex of the crest of any groove and the bottom of the valley of that groove, as shown in 2001 in Fig. 6.

[0106] (Water-absorbent resin before the grinding process) In one embodiment of the present invention, the dried polymer obtained in the drying step or the like and subjected to the pulverization step may be pulverized in its entirety in a pulverizer, preferably the specific roll-type pulverizer, but depending on the shape of the dried polymer, it may be subjected to another step, for example, a rough crushing step, or may be subjected to a classification step, before being pulverized in the pulverizer. The "rough crushing step" refers to a step of disintegrating (loosening) aggregated particles. Therefore, when the dried polymer is aggregated in a block shape or the like, the dried polymer may be roughly crushed in advance in order to efficiently perform pulverization in a pulverizer, preferably the specific roll-type pulverizer.

[0107] In one embodiment of the present invention, the particle size distribution of the dried polymer fed into the pulverizer, preferably the specific roll-type pulverizer, is such that the proportion of particles with a particle diameter of 850 μm or more (proportion of particles that did not pass through a sieve with an opening diameter of 850 μm) is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less in 100% by mass of the dried polymer. Also, the proportion of particles with a particle diameter of 1400 μm or more (proportion of particles that did not pass through a sieve with an opening diameter of 1400 μm) in 100% by mass of the dried polymer is preferably 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less.

[0108] In one embodiment of the present invention, the resin solid content of the dried polymer subjected to the pulverization step is, for example, preferably 80.0 to 99.0% by mass, more preferably 90.0 to 98.8% by mass, and even more preferably 95.0 to 98.5% by mass. That is, the moisture content of the dried polymer of the present invention is preferably 1.0 to 20% by mass, more preferably 1.2 to 10% by mass, and even more preferably 1.5 to 5% by mass. By setting the solid content rate of the dried polymer within the above range, the hardness of the dried polymer can be adjusted to be suitable for pulverization in the pulverization step, and the generation of particles with crushed and exposed flat surfaces can be suppressed in the obtained pulverized product. Therefore, a crushed product with a large surface area can be obtained. In addition, the obtained water-absorbing resin with a large surface area has a high water absorption rate and can absorb liquid in a short time. The method for determining the resin solid content of the dried polymer is as described in "(3-4) Drying step".

[0109] In one embodiment of the present invention, the relationship between the clearance between the pair of rolls and the mass average particle size of the dried polymer fed to the roll-type grinding device is preferably 1:0.3 to 1:10. In this case, an appropriate pressure that prevents the water absorbent resin from being crushed is applied to the dried polymer during grinding, and the generation of particles with crushed and exposed flat surfaces can be suppressed. The relationship between the clearance between the pair of rolls and the mass average particle size of the dried polymer fed to the roll-type grinding device is more preferably 1:0.5 to 1:5, and further preferably 1:0.9 to 1:3.

[0110] (3-8) Classification process The water absorbent resin (e.g., water absorbent resin powder) obtained through the pulverization step is further subjected to a classification step, if necessary. In one embodiment of the present invention, the particle size adjustment method in the classification step is not particularly limited, but examples thereof include sieve classification using a JIS standard sieve (JIS Z8801-1 (2000)) and air flow classification.

[0111] (3-9) Surface crosslinking process The water-absorbent resin (e.g., water-absorbent resin powder) obtained through the pulverization step (and any subsequent step) is preferably surface-crosslinked with a surface crosslinking agent. The surface crosslinking is a treatment for providing a portion with high crosslink density in the surface layer of the water-absorbent resin (a region from the surface of the water-absorbent resin to a depth of several tens of μm inside). By carrying out the surface crosslinking treatment, various water-absorbing properties can be improved. In this specification, the water-absorbent resin also includes a surface-crosslinked water-absorbent resin.

[0112] For example, when reversed-phase suspension polymerization is adopted, a surface crosslinking (also called a post-crosslinking reaction) is disclosed in a known patent document (e.g., JP-A-2006-176570) in which a hydrogel obtained after polymerization is stirred and dispersed in an inert organic solvent such as a hydrocarbon solvent before drying, a surface crosslinking agent (also called a post-crosslinking agent) described later is added, and a heat treatment is performed to crosslink the surface vicinity of the water-absorbent resin. In one embodiment of the present invention, it is preferable to perform a surface treatment on the powder after drying the hydrogel in order to increase the absorption capacity under pressure.

[0113] (Surface cross-linking agent) The surface cross-linking agent used in this step is not particularly limited, but may be an organic or inorganic surface cross-linking agent. Among them, from the viewpoint of the physical properties of the water-absorbent resin and the handling of the surface cross-linking agent, an organic surface cross-linking agent that reacts with a carboxyl group is preferred. For example, one or more surface cross-linking agents disclosed in U.S. Patent No. 7,183,456 may be mentioned. Specifically, polyhydric alcohol compounds, epoxy compounds, haloepoxy compounds, polyamine compounds or their condensates with haloepoxy compounds, oxazoline compounds, oxazolidinone compounds, polyvalent metal salts, alkylene carbonate compounds, cyclic urea compounds, etc. may be mentioned.

[0114] (3-10) Granulation process The method for producing a water-absorbent resin according to one embodiment of the present invention may include a granulation step for obtaining an aggregate of primary particles. For example, in the case of reversed-phase suspension polymerization, an aggregate of primary particles can be obtained by performing multiple reversed-phase suspension polymerization steps, adding an aggregating agent to the gel of primary particles after polymerization, and the like. Therefore, these steps can be said to be granulation steps. In the case of aqueous solution polymerization, the granulation step may include adding an aqueous liquid to fine particles of a water-absorbent resin passing through a JIS standard sieve with a mesh size of 150 μm, and stirring and mixing the mixture.

[0115] The method for producing a water absorbent resin according to one embodiment of the present invention includes a granulation step, and may also include a crushing step of crushing the water absorbent resin obtained in the granulation step using the above-mentioned specific roll-type crushing device.

[0116] (3-11) Additive addition process The method for producing a water-absorbent resin according to one embodiment of the present invention preferably includes a step of adding an additive to impart various functions to the water-absorbent resin. As the additive, any of those described in "(2-2) Additives" can be used.

[0117] The method and timing of adding the additives are not particularly limited, and may be appropriately selected depending on the additives to be added.

[0118] From the viewpoint of providing a water-absorbent resin having a good water absorption capacity under pressure, the method for producing a water-absorbent resin according to one embodiment of the present invention preferably includes a step of adding water-insoluble inorganic fine particles. Here, the water-insoluble inorganic fine particles are as explained in "(2-2) Additives".

[0119] The timing of adding the water-insoluble inorganic fine particles is not particularly limited, but for example, it is preferable to add them after the pulverization step or the surface cross-linking step, or after the pulverization step or the surface cross-linking step and further after a classification step, a polishing step, a granulation step, a water-containing (water addition) step, a sizing step, etc. In addition, the method of adding the water-insoluble inorganic fine particles is not particularly limited, but examples thereof include a method of dry blending with a water-absorbent resin (e.g., water-absorbent resin powder), a method of adding as a dispersion to a water-absorbent resin (e.g., water-absorbent resin powder) and mixing, etc.

[0120] (3-12) Other processes The method for producing a water absorbent resin according to one embodiment of the present invention may include, in addition to the above-mentioned steps, a water-containing (rewetting) step, a step of adding other additives, a granulation step, and a fine powder reuse step, as necessary. In addition, the method may further include a transport step, a storage step, a packaging step, a keeping step, and the like.

[0121] (Rewetting process) This step, which is optionally performed, is a step of adding at least one kind of additive selected from the group consisting of a polyvalent metal salt, a cationic polymer, a chelating agent, an inorganic reducing agent, and an α-hydroxycarboxylic acid compound to the water absorbent resin (e.g., water absorbent resin particles) obtained in the surface cross-linking step.

[0122] The additive is preferably added to the water-absorbing resin (for example, water-absorbing resin particles) as an aqueous solution or a dispersion (slurry). The additive may be added and mixed simultaneously with the above-mentioned surface cross-linking agent solution.

[0123] Specifically, the method described in International Patent Publication No. 2015 / 053372, “(2-7) Rewetting Step”, is also applicable to the present invention.

[0124] (Sizing process) The "size regulation step" means a step of loosening the water absorbent resin loosely aggregated through the surface cross-linking step to regulate the particle size. This size regulation step includes a fine powder removal step and a classification step subsequent to the surface cross-linking step. The size regulation step is preferably carried out from the viewpoint of regulating the particle size of the water absorbent resin and obtaining stable water absorption properties.

[0125] (Fine powder reuse process) The "fine powder reuse step" means a step of supplying the fine powder generated by sieve classification or the like in each step to any of the steps as it is or after granulating the fine powder. The fine powder reuse step is preferably carried out from the viewpoint of reducing production loss of the water absorbent resin.

[0126] [4] Uses of water-absorbent resins The use of the water-absorbent resin according to one embodiment of the present invention is not particularly limited, but is preferably used as an absorbent body for absorbent articles such as paper diapers (for infants and adults), sanitary napkins, incontinence pads, etc. In particular, it can be suitably used as an absorbent body for paper diapers comprising a water-absorbent resin and a fibrous substrate. Other absorbent articles include, for example, soil water retention agents, seedling sheets, seed coating materials, condensation prevention sheets, drip absorbents, freshness-preserving materials, disposable hand warmers, cooling bandanas, ice packs, medical waste liquid solidifying agents, residual soil solidifying materials, water damage prevention waste liquid gelling agents, water-absorbing sandbags, disaster-use portable toilets, compresses, thickening agents for cosmetics, water-stopping materials for electric and electronic material communication cables, gasket packing, sustained-release agents for fertilizers, various sustained-release agents (space disinfectants, air fresheners, etc.), pet sheets, cat litter, wound protection dressing materials, condensation prevention building materials, oil moisture removers, paints, adhesives, resin additives (anti-blocking agents, light diffusing agents, matting agents, additives for decorative panels, additives for artificial marble, additives for toners, etc.), and the like. EXAMPLES

[0127] The present invention will be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to these examples. Examples obtained by appropriately combining the technical means described in each example are also included in the scope of the present invention. In the examples, the terms "parts" and "%" may be used, but unless otherwise specified, they represent "parts by mass" or "% by mass". Unless otherwise specified, each operation is performed at room temperature (23°C ± 2°C). For the electrical equipment used in the examples and comparative examples (including the measurement of the physical properties of the water-absorbent resin), a power supply of 200V or 100V, 60Hz was used unless otherwise noted.

[0128] 1. Evaluation Method [1-1] Centrifuge holding capacity (CRC) The centrifuge retention capacity (CRC) of the water-absorbent resin was measured in accordance with the EDANA method (ERT441.2-02).

[0129] Specifically, 0.2 g of the water-absorbent resin was placed in a nonwoven bag, and then immersed in a large excess of 0.9% by mass aqueous sodium chloride solution for 30 minutes to allow free swelling. Thereafter, the bag was centrifuged (250 G) for 3 minutes to remove water, and the water absorption capacity (unit: g / g) was determined.

[0130] [1-2] Absorption under pressure (AAP) The AAP (absorbency under pressure) of the water-absorbent resin was measured in accordance with the EDANA method (ERT442.2-02). Note that the load condition was changed to 4.83 kPa (0.7 psi).

[0131] [1-3] Moisture content The moisture content of the water-absorbent resin was measured in accordance with the EDANA method (ERT430.2-02). Note that, in the measurement, the mass of the sample (water-absorbent resin) was changed to 1.0 g, the drying temperature to 180° C., and the drying time to 3 hours.

[0132] Specifically, 1.0 g of a sample (water-absorbent resin or water-absorbent resin powder) was placed in an aluminum cup having a bottom diameter of 50 mm, and then the total mass W1 (g) of the sample and the aluminum cup was accurately weighed.

[0133] Next, the sample was placed in an aluminum cup and left to stand in an oven set at an atmospheric temperature of 180° C. After 3 hours, the sample was removed from the oven together with the aluminum cup, and the total mass W2 (g) of the dried sample and aluminum cup was accurately weighed. When the mass of the sample (water-absorbent resin) used in this measurement was M (1.0 g), the moisture content (mass%) of the sample was calculated according to the following formula (3): Moisture content (mass%) = {(W1-W2) / M}×100...Equation (3).

[0134] [1-4] Mass average particle diameter (D50) The mass-average particle diameter (D50) of the water-absorbent resin was measured according to the method described in “(3) Mass-Average Particle Diameter (D50) and Logarithmic Standard Deviation (σζ) of Particle Diameter Distribution” in columns 27 and 28 of U.S. Pat. No. 7,638,570.

[0135] [1-5] Surface tension The surface tension of the water-absorbent resin was measured by the method described in WO2015 / 129917.

[0136] Specifically, 50 ml of 0.90% by mass sodium chloride aqueous solution adjusted to 20°C was placed in a thoroughly washed 100 ml beaker, and the surface tension of the 0.90% by mass sodium chloride aqueous solution was measured using a surface tensiometer (K11 automatic surface tensiometer, manufactured by KRUSS). In this measurement, the surface tension value must be in the range of 71 to 75 [mN / m].

[0137] Next, a thoroughly washed cylindrical stirrer with a length of 25 mm and 0.500 g of water-absorbent resin were placed in a beaker containing the 0.90 mass% sodium chloride aqueous solution after the surface tension measurement, adjusted to 20°C, and stirred for 4 minutes at 500 rpm. After 4 minutes, the stirring was stopped, and the water-absorbent resin was allowed to settle, after which the surface tension of the supernatant was measured again by the same operation. In addition, in the measurement of the surface tension, a plate method using a platinum plate was adopted, and the plate was thoroughly washed with deionized water before each measurement, and heated and washed with a gas burner before use.

[0138] [1-6] Water absorption rate (Vortex method) 0.02 parts by mass of Food Blue No. 1, a food additive, was added to 1000 parts by mass of a 0.90% by mass aqueous solution of sodium chloride (physiological saline), and the liquid temperature was adjusted to 30° C. 50 ml of the physiological saline was measured out into a 100 ml beaker, and 2.0 g of the water-absorbent resin was added at once while stirring at 600 rpm using a cylindrical stirrer tip with a length of 40 mm and a cross section perpendicular to the length direction and a diameter of 8 mm and a magnetic stirrer. The time until the water-absorbent resin absorbed the physiological saline and covered the stirrer tip was measured as the water absorption speed (seconds).

[0139] [1-7] Absorption capacity against pressure fluctuations The absorption capacity against pressure fluctuation is expressed as the sum of the absorption capacity (A) against pressure fluctuation from low pressure to high pressure (from 0.05 psi to 0.7 psi) and the absorption capacity (B) against pressure fluctuation from high pressure to low pressure (from 0.7 psi to 0.05 psi), which are measured by the procedure described below. The absorption capacity against pressure fluctuation will be described with reference to Figs. 3 and 4.

[0140] [1-7-1] Absorption capacity for pressure changes from low to high (A) A weighed amount of 1.0 g of water-absorbent resin 16 was spread to a uniform thickness on the bottom 15 of a cell 11 having an inner diameter of 60 mm and a bottom 15 formed of a stainless steel wire net (opening 36 μm = 400 mesh). A piston 12 having a diameter of 59 mm and a weight of 96 g was mounted on the spread water-absorbent resin 16. At this time, a load of 0.05 psi was applied to the water-absorbent resin 16. After measuring the mass Wa [g] of the cell 11 with the piston 12 mounted thereon, the cell was placed in a 20 cm × 20 cm petri dish 13 containing 180 g of a 0.9% by mass sodium chloride aqueous solution at 25 ° C., and the water-absorbent resin 16 was allowed to absorb the 0.9% by mass sodium chloride aqueous solution for 5 minutes. Next, a weight 14 of 1249 g was further placed on the piston 12, and the 0.9% by mass sodium chloride aqueous solution was allowed to be absorbed for 5 minutes under a load of 0.7 psi. Five minutes after the weight 14 was placed, the measuring device set 10 was removed from the dish 13, the weight 14 was removed, and the mass Wb [g] (of the cell 11 with the piston 12 mounted thereon) was measured. The absorption capacity (A) in response to a pressure change from low to high pressure was then calculated according to the following equation (4).

[0141] Absorption capacity when pressure changes from low to high (A) [g / g] = {(Wb - Wa) / (weighed mass of water-absorbent resin)} Equation (4).

[0142] [1-7-2] Absorption capacity for pressure changes from high to low pressure (B) A weighed amount of 1.0 g of the water-absorbent resin 16 was spread to a uniform thickness on the bottom 15 of the cell 11 having an inner diameter of 60 mm, the bottom 15 of which was formed of a stainless steel wire net (opening 36 μm = 400 mesh). A piston 12 having a diameter of 59 mm and a weight of 96 g was mounted on the water-absorbent resin 16, and the mass Wc [g] of the cell 11 with the piston 12 mounted thereon was measured. Then, a weight 14 of 1249 g was mounted on the piston 12. At this time, a load of 0.7 psi was applied to the water-absorbent resin 16. The measuring device set 10 was placed in a 20 cm x 20 cm petri dish 13 containing 180 g of a 0.9% by mass sodium chloride aqueous solution at 25 ° C., and the water-absorbent resin 16 was allowed to absorb the 0.9% by mass sodium chloride aqueous solution for 5 minutes. Next, the weight 14 on the piston 12 was removed, and the 0.9% by mass sodium chloride aqueous solution was allowed to absorb for 5 minutes under a load of 0.05 psi. Five minutes after removing the weight 14, the entire measuring device without the weight 14 was removed from the petri dish 13, and its mass Wd [g] was measured. Then, the absorption capacity (B) in response to a pressure change from high pressure to low pressure was calculated according to the following formula (5).

[0143] Absorption capacity when pressure changes from high to low (B) [g / g] = {(Wd-Wc) / (weighed mass of water-absorbent resin)} Equation (5).

[0144] [1-8] Absorber performance evaluation (1) Preparation of absorber As shown in Figs. 3 and 4, an adhesive tape 302 (vinyl tape No. 21S manufactured by NITTO DENKO) cut to 10 cm x 20 cm was placed with the adhesive side facing up, and 2.5 g of water-absorbing resin 301 was evenly spread on the adhesive surface of the adhesive tape 302 inwardly by 2 cm from each end of the four sides, i.e., in a 6 cm x 16 cm area in the center of the adhesive tape 302. Then, a 10 cm x 20 cm piece of nonwoven fabric 303 (3 mm thick and 41 g / m2 in weight) was placed on top of the adhesive tape 302. 2The fiber diameter of the polyethylene and polypropylene is 0.18 mm, and the fiber diameter of the polyethylene terephthalate is 0.27 mm.) was placed on the absorbent body 300 and attached to the adhesive surfaces on all four sides to prepare an absorbent body 300 for evaluation.

[0145] (2) Absorber evaluation under conditions involving pressure fluctuations In order to clearly confirm the effect of the present invention, an absorbent body was evaluated with an amount of liquid added that was in excess of that expected in actual use.

[0146] (2-1) The sum of the amount of liquid return and the amount of liquid leakage from the absorbent body under conditions involving pressure fluctuations from high to low pressure (1) After measuring the total mass K1 (g) of kitchen paper (Oji Nepia kitchen towels) cut into a size of 23 cm x 40 cm and stacked in 10 sheets, this was laid on a flat table, and an acrylic plate measuring 10 cm x 20 cm and 1.3 cm thick was placed on top of it, and the absorbent for evaluation, a wire mesh measuring 8 cm x 16 cm, and an acrylic plate measuring 28 cm x 48 cm equipped with a liquid injection tube were placed on top of it in that order. The acrylic plate equipped with a liquid injection tube had a liquid injection tube with an inner diameter of 2 cm at its center, and was placed on the wire mesh so that the liquid injection tube was located at the center of the absorbent for evaluation. The acrylic plate equipped with a liquid injection tube has a mass that applies a load of 0.06 psi to the absorbent.

[0147] A weight with a mass sufficient to apply a load of 0.7 psi to the absorbent was placed on the acrylic plate equipped with the uppermost liquid injection tube, and 20 g of a 0.9% by mass aqueous sodium chloride solution at 20°C was added from the liquid injection tube over a period of 30 seconds (first liquid addition).

[0148] Five minutes after the start of the first liquid addition, the weight was removed, and with a load of 0.06 psi applied to the absorbent body, 20 g of a 0.9% by mass aqueous sodium chloride solution at 20°C was added from the liquid injection tube over a period of 30 seconds (second liquid addition).

[0149] Immediately after 5 minutes had elapsed since the start of the second liquid addition, the acrylic plate and wire mesh equipped with the liquid injection tube were removed, and 20 sheets of kitchen paper (kitchen towels manufactured by Oji Nepia Co., Ltd.) cut to a size of 11 cm x 23 cm and stacked together to a total mass of K2 (g) were placed on the absorbent body, and a stainless steel tray with a bottom surface measuring 20 cm x 18 cm and a weight of 10 kg was placed inside, in that order, and the absorbent body was left to stand for 1 minute with the weight applied.

[0150] The total mass (K1') of the kitchen paper cut into a size of 23 cm x 40 cm and stacked in 10 sheets was measured, and the total mass (K2') of the kitchen paper cut into a size of 11 cm x 23 cm and stacked in 20 sheets was measured. The amount of liquid that could not be absorbed by the absorbent body in the series of evaluations, that is, "the sum of the amount of liquid return and the amount of liquid leakage from the absorbent body under conditions involving pressure fluctuations from high to low pressure (1)" was calculated based on the following formula (6).

[0151] The sum of the amount of liquid return and the amount of liquid leakage [g] = (K1' - K1) + (K2' - K2) Equation (6).

[0152] (2-2) The sum of the amount of liquid return and the amount of liquid leakage from the absorbent body under conditions involving pressure fluctuations from low to high pressure (2) The same procedure as in (2-1) was carried out, except that the load applied in the first liquid addition was 0.06 psi and the load applied in the second liquid addition was 0.7 psi, and the "sum of the amount of liquid return and the amount of liquid leakage of the absorbent body under conditions involving a pressure change from low to high pressure (2)" was calculated based on the above formula (6).

[0153] [1-9] Measuring the thickness of nonwoven fabric The thickness of the nonwoven fabric was measured using a large-type dial thickness gauge (thickness measuring device) (manufactured by Ozaki Manufacturing Co., Ltd., model number: JB, measuring probe: anvil top and bottom φ50 mm). The upper measuring probe of the thickness measuring device was brought close to a height of 2 to 3 mm from the nonwoven fabric, and then the hand was slowly released from the handle so as to apply as little pressure as possible to the nonwoven fabric, and the thickness of the nonwoven fabric was measured.

[0154] Example 1 800 g of n-heptane was placed in a 2000 mL four-neck separable flask equipped with a stirrer, reflux condenser, thermometer, nitrogen gas inlet tube, and dropping funnel, and 0.88 g of maleic anhydride-modified ethylene-propylene copolymer (product name: Hiwax (registered trademark) HW2203A, manufactured by Mitsui Chemicals, Inc.) was added and dissolved as a dispersant. Nitrogen gas was then blown in to expel the dissolved oxygen.

[0155] Separately, in a flask, an aqueous monomer solution (1) was prepared consisting of 127 g of sodium acrylate, 36 g of acrylic acid, 0.077 g of polyethylene glycol diacrylate (n=9), 0.008 g of pentasodium diethylenetriaminepentaacetate, 0.67 g of hydroxyethylcellulose as a thickener, and 215 g of ion-exchanged water, and nitrogen gas was blown in to expel the dissolved oxygen from the aqueous solution.

[0156] Next, 1.2 g of a 15% aqueous solution of sodium persulfate was added to the aqueous monomer solution (1) in the flask, and the entire amount was added to the separable flask and dispersed by stirring at 210 rpm. The bath temperature was then raised to 60° C. to initiate a polymerization reaction, and the bath temperature was maintained at 60° C. for 2 hours, after which the organic solvent was removed by suction filtration to obtain a hydrous gel-like crosslinked polymer (1).

[0157] The hydrogel crosslinked polymer (1) was heated to 90° C., then charged into a gel sieving device having a screw and a perforated plate with a hole diameter of 0.8 mm, and discharged from the gel sieving device to obtain a sieved gel (1).

[0158] Next, the granulated gel (1) was dried using a cylindrical container rotary dryer. Specifically, the granulated gel (1) was supplied to the cylindrical container rotary dryer while rotating the rotary container of the cylindrical container rotary dryer at 75 rpm in an atmosphere at a temperature of 200° C., and dried until the moisture content reached 10% by mass, to obtain a dried polymer (1).

[0159] The dried polymer (1) was added to a flask containing methanol in an amount 10 times the mass of the dried polymer (1), and the mixture was stirred at 60°C for 1 hour. The methanol was then filtered off, and the residue was air-dried at room temperature to perform a hydrophilization treatment.

[0160] Subsequently, the hydrophilically treated dried polymer (1) was pulverized using a roll granulator (manufactured by Nippon Granulator Co., Ltd., roll size: diameter 115 mm × length 100 mm) as a pulverizing device, and further classified using a JIS standard sieve with an opening of 150 μm, and fine powder that passed through the sieve was removed to obtain a water absorbent resin powder (1). Here, in the roll granulator, a pair of rolls was installed in the first stage, and one-stage pulverization was performed. Note that, as the pair of rolls, a groove having a V-shaped cross section was provided on the roll surface of each of the rolls in a direction parallel to the roll rotation direction (clearance difference: 0). Specifically, the grooves were provided over the entire circumference of the roll surface, and a plurality of grooves were provided continuously at equal intervals from one end to the other end of the roll. The pitch (spacing) of the grooves of the pair of rolls was the same for both rolls. In addition, the grooves in each roll were arranged so that the crest of the groove of one roll and the valley of the groove of the other roll were at the same position in the axial direction of the rolls, as shown in 2001 in Figure 6, and the clearance between the rolls was constant. Note that the clearance between the rolls means the distance between the two rolls, as mentioned above.

[0161] Roll speed: 565 / 462 rpm (inner rotation) Groove height (groove inclination angle): 1.0mm (45°) Groove pitch: 2.0mm Clearance between rolls: 1.0mm.

[0162] A surface crosslinking agent solution consisting of 0.03 part by mass of ethylene glycol diglycidyl ether, 0.385 part by mass of ethylene carbonate, 0.644 part by mass of propylene glycol and 2.6 parts by mass of ion-exchanged water was uniformly mixed with 100 parts by mass of the water absorbent resin powder (1), and the mixture was subjected to a heat treatment at 195°C for 25 minutes. The powder temperature was then forcibly cooled to 60°C, thereby obtaining a surface-crosslinked water absorbent resin powder (1).

[0163] 100 parts by mass of the surface-crosslinked water-absorbent resin powder (1) was uniformly mixed with 10.0 parts by mass of water, and the mixture was passed through a JIS standard sieve with an opening of 1000 μm to size the particles. Then, 100 parts by mass of the size-sized mixture was mixed with hydrotalcite (product name: DHT-6, manufactured by Kyowa Chemical Industry Co., Ltd., Mg 6 Al 2 (OH)16CO 3 4H 2 O, specific surface area=16m 2 The physical properties of the water-absorbent resin (1) are shown in Tables 1 and 2.

[0164] Example 2 An aqueous monomer solution (2) was prepared in the same manner as in Example 1, except that the amount of polyethylene glycol diacrylate (n=9) used in Example 1 was changed to 0.097 g and the thickener hydroxyethyl cellulose was not used. Nitrogen gas was then blown in to expel the dissolved oxygen from the aqueous solution.

[0165] Next, 1.2 g of a 15% aqueous solution of sodium persulfate was added to the monomer aqueous solution (2) in the flask, and the entire amount was added to the separable flask and dispersed by stirring at 230 rpm. The bath temperature was then raised to 60° C. to initiate a polymerization reaction, and the bath temperature was maintained at 60° C. for 2 hours. The organic solvent was then filtered off by suction filtration, and the residue was air-dried at room temperature overnight to obtain a hydrogel-like crosslinked polymer (2).

[0166] Thereafter, under the same conditions as in Example 1, a gel granulation step, a drying step using a cylindrical container rotary dryer, a hydrophilization treatment, a pulverization step, and a classification step were carried out to obtain a water absorbent resin powder (2).

[0167] A surface crosslinking agent solution consisting of 0.015 part by mass of ethylene glycol diglycidyl ether, 0.193 part by mass of ethylene carbonate, 0.322 part by mass of propylene glycol and 1.3 parts by mass of ion-exchanged water was uniformly mixed with 100 parts by mass of the water absorbent resin powder (2), and the mixture was subjected to a heat treatment at 180°C for 30 minutes. The powder temperature was then forcibly cooled to 60°C, thereby obtaining a surface-crosslinked water absorbent resin powder (2).

[0168] The surface-crosslinked water-absorbent resin powder (2) was subjected to the same procedures as in Example 1, including adding water, sizing, and adding hydrotalcite (product name: DHT-6, manufactured by Kyowa Chemical Industry Co., Ltd., Mg 6 Al 2 (OH)16CO 3 4H 2 O, specific surface area=16m 2 / g) was added to obtain a water-absorbent resin (2). The physical properties of the obtained water-absorbent resin (2) are shown in Tables 1 and 2.

[0169] Comparative Example 1 After adding 1.2 g of a 15% aqueous solution of sodium persulfate to the aqueous monomer solution (2) of Example 2, the entire amount was added to the separable flask and dispersed by stirring at 210 rpm. The bath temperature was then raised to 60° C. to initiate a polymerization reaction, and the bath temperature was maintained at 60° C. for 2 hours. The organic solvent was then filtered off by suction filtration, and the residue was air-dried at room temperature overnight to obtain a comparative hydrous gel-like crosslinked polymer (1).

[0170] Thereafter, the gel granulation step, the drying step using a cylindrical container rotary dryer, and the hydrophilization treatment were carried out under the same conditions as in Example 1, thereby obtaining a hydrophilized comparative dried polymer (1).

[0171] Next, the comparative dried polymer (1) that had been hydrophilically treated was pulverized using a roll mill (WML type roll pulverizer, manufactured by Inokuchi Giken Co., Ltd.) as a pulverizing device, and further classified using a JIS standard sieve with an opening of 150 μm, and the fine powder that passed through the sieve was removed to obtain a comparative water absorbent resin powder (1). Here, in the roll mill, a pair of rolls was installed in the first stage, and one-stage pulverization was performed. Note that, as the pair of rolls, a groove having a V-shaped cross section was provided on the roll surface of each of the rolls in a direction approximately perpendicular to the roll rotation direction. On the roll surface, one groove was provided continuously from one end of the roll to the other end (i.e., continuously in the roll width direction), and a plurality of grooves were provided continuously at equal intervals in a row around the entire circumference. The roll grooves (groove tooth shape) of the pair of rolls were both the same.

[0172] Roll speed: 480 / 200 rpm Groove pitch: 1.15mm Clearance between rolls: 1.0mm.

[0173] The comparative water absorbent resin powder (1) was subjected to surface crosslinking, water addition, granulation, and hydrotalcite (product name: DHT-6, manufactured by Kyowa Chemical Industry Co., Ltd., Mg 6 Al 2 (OH)16CO 3 4H 2 O, specific surface area=16m 2 / g) was added to obtain a comparative water-absorbing resin (1). The physical properties of the obtained comparative water-absorbing resin (1) are shown in Tables 1 and 2.

[0174] Comparative Example 2 A comparative water absorbent resin (2) was obtained by carrying out the same operations as in Comparative Example 1, except that the hydrophilization treatment was not carried out in Comparative Example 1, and that in the pulverization step, a roll granulator was used instead of a roll mill as a pulverization device, and pulverization was carried out under the same conditions as in Example 1. The physical properties of the obtained comparative water absorbent resin (2) are shown in Tables 1 and 2.

[0175] Comparative Example 3 The comparative dried polymer (1) subjected to hydrophilic treatment in Comparative Example 1 was pulverized under the same conditions as in Example 1 using a roll granulator as a pulverizing device, and further classified using a JIS standard sieve with an opening of 150 μm. The fine powder that passed through the sieve was removed to obtain a comparative water absorbent resin powder (3). The comparative water absorbent resin powder (3) was subjected to surface cross-linking under the same conditions as in Example 2 to obtain a surface cross-linked water absorbent resin powder (3). 100 parts by mass of the surface cross-linked water absorbent resin powder (3) was uniformly mixed with 10.0 parts by mass of water, and the mixture was passed through a JIS standard sieve with an opening of 1000 μm for sieving, and then fine particles of silica (trade name: Aerosil (registered trademark) 200, manufactured by Nippon Aerosil Co., Ltd., specific surface area = 200 m) were added to 100 parts by mass of the sieved product. 2 The comparative water-absorbing resin (3) was obtained by uniformly mixing 0.3 parts by weight of each of the above ingredients (100% by weight / g). The physical properties of the comparative water-absorbing resin (3) are shown in Tables 1 and 2.

[0176] Comparative Example 4 A comparative monomer aqueous solution (4) was prepared with the same composition as in Example 1, except that 26.4 mg of ethylene glycol diglycidyl ether was used instead of the polyethylene glycol diacrylate (n=9) in Example 1, and the thickener hydroxyethyl cellulose was not used. Nitrogen gas was then blown into the aqueous solution to remove dissolved oxygen.

[0177] Next, 1.2 g of a 15% aqueous solution of sodium persulfate was added to the comparative monomer aqueous solution (4) in the flask, and the entire amount was added to the separable flask and dispersed by stirring at 210 rpm. The bath temperature was raised to 60° C. to initiate the polymerization reaction, and the bath temperature was maintained at 60° C. for 2 hours, after which water was removed from the obtained hydrous gel-like material by azeotropic distillation.

[0178] To the dehydrated hydrogel, 6.08 g of a 2% by mass aqueous solution of ethylene glycol diglycidyl ether was added as a surface crosslinking agent, and the bath temperature was maintained at 80° C. for 2 hours to perform surface crosslinking. Thereafter, n-heptane was evaporated to remove it from the system, thereby obtaining a comparative hydrogel polymer (4).

[0179] Subsequently, the same hydrophilization treatment and pulverization steps as in Example 1 were carried out to obtain a comparative water absorbent resin powder (4).

[0180] 100 parts by mass of the obtained comparative water absorbent resin powder (4) was mixed with hydrotalcite (product name: DHT-6, manufactured by Kyowa Chemical Industry Co., Ltd., Mg 6 Al 2 (OH)16CO 3 4H 2 O, specific surface area=16m 2 0.3 parts by mass of 100% water-absorbent resin (1 / g) was added and mixed to obtain a comparative water-absorbent resin (4). The physical properties of the obtained comparative water-absorbent resin (4) are shown in Tables 1 and 2.

[0181] [Table 1]

[0182] [Table 2]

[0183] From Table 2, in the absorbent bodies using the water-absorbent resins of Examples 1 and 2, which show excellent values ​​of absorption capacity (A+B) against pressure fluctuation, even in the evaluation in which excess liquid was poured in compared to the amount of liquid assumed in practical use, the amount of liquid return and the amount of liquid leakage were suppressed to a small amount, compared to the absorbent resins of Comparative Examples 1 to 4. From these results, it is found that the water-absorbent resins having excellent absorption capacity against pressure fluctuation can be suitably used for absorbent articles exposed to various pressures in practical use. [Industrial Applicability]

[0184] The water-absorbent resin according to one embodiment of the present invention can realize stable absorption capacity during practical use of absorbent articles using the same, and can therefore be suitably used in sanitary materials (sanitary products) such as paper diapers, sanitary napkins, adult incontinence products (incontinence pads), and pet sheets. [Explanation of symbols]

[0185] 10. Apparatus for measuring absorption capacity against pressure fluctuations 11 Cell 12 Piston 13 Petri dish 14 Weight 15 Bottom 16 Water-absorbing resin 300 Evaluation absorbent 301 Water-absorbing resin 302 Adhesive tape 303 Nonwoven fabric 20a Dry polymer 20b Dried polymer pulverized material (water-absorbent resin powder) 200 Roller type grinding device 201 Piping 202 Inlet 203, 203a, 203b Roll

Claims

1. A particulate poly(meth)acrylic acid (salt)-based water-absorbing resin having an absorption capacity against pressure fluctuations calculated by the following formula (1) of 76.0 g / g or more. Absorption capacity against pressure change [g / g]={Absorption capacity against pressure change from 0.05 psi to 0.7 psi (A) [g / g]}+{Absorption capacity against pressure change from 0.7 psi to 0.05 psi (B) [g / g]}...Equation (1)

2. 2. The poly(meth)acrylic acid (salt) water absorbent resin according to claim 1, which has an absorption capacity (A) of 34.0 g / g or more with respect to a pressure change from 0.05 psi to 0.7 psi.

3. 3. The poly(meth)acrylic acid (salt)-based water-absorbent resin according to claim 1 or 2, which has an absorption capacity (B) of 44.0 g / g or more with respect to a pressure change from a pressure of 0.7 psi to a pressure of 0.05 psi.

4. The poly(meth)acrylic acid (salt)-based water-absorbing resin according to any one of claims 1 to 3, which contains water-insoluble inorganic fine particles.

5. The specific surface area of ​​the water-insoluble inorganic fine particles is 100 m 2 The poly(meth)acrylic acid (salt)-based water-absorbing resin according to claim 4, wherein the water-absorbent property is less than 1 / g.

Citation Information

Patent Citations

  • Crosslinked, hydrophilic, highly swellable hydrogels, methods of making and uses thereof

    JP2002536471A