Adhesive composition
The adhesive composition with thermosetting resin, thermoplastic resin particles, and curing agents addresses the challenge of unstable adhesive performance by enhancing cohesive failure resistance and adhesive strength, suitable for diverse materials.
Patent Information
- Application Number
- JP2021141613
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-08-31
- Publication Date
- 2024-10-17
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing adhesive compositions face challenges in achieving both high adhesive strength and stable cohesive failure, with interfacial failure leading to unstable adhesive performance due to variations in external force.
An adhesive composition comprising a thermosetting resin, thermoplastic resin particles, and a curing agent or curing accelerator, with specific conditions and ratios to enhance cohesive failure resistance and adhesive strength, including components with functional groups like hydroxy, carboxy, and glycidyl groups, and controlled thermal and mechanical properties.
The adhesive composition achieves high adhesive strength and improved cohesive failure resistance, suitable for bonding various materials including metals and resins, with enhanced fracture toughness and stability.
Smart Images

Figure 2024147843000002 
Figure 2024147843000003 
Figure 2024147843000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive composition. [Background technology]
[0002] Conventionally, various adhesive compositions have been used in various industrial fields such as automobiles and electronic materials. Adhesive compositions used in industrial fields are required to have stable adhesive performance in addition to high adhesive strength to adherend objects such as metal materials. Specifically, stable adhesive performance is a performance in which the variation in the magnitude of the external force that causes peeling during adhesion to the adherend object is small, the adherend object is adhered until the external force applied to the adhesive layer exceeds a certain magnitude, and when the magnitude is exceeded, the adhered adherend object peels off.
[0003] The known modes of adhesion failure when adherend objects peel off include interfacial failure, cohesive failure, and a mixture of these, and it is known that when the adhesion failure mode due to an external force is cohesive failure, the adhesive performance is stable (see, for example, Patent Document 1). On the other hand, even if an adhesive composition has high adhesive strength to an adherend object, if the adhesion failure mode is interfacial failure, there is a problem that the adhesive performance is not stable because there is a large variation in the external force when peeling occurs at the interface between the adhesive layer and the adherend object.
[0004] For example, Patent Document 2 discloses an epoxy resin adhesive containing an epoxy resin, a curing agent, and a polyolefin resin coated with silica. This adhesive composition has low shrinkage and high adhesiveness, but does not provide sufficient performance in terms of fracture morphology.
[0005] Furthermore, for example, Patent Document 3 discloses an adhesive composition containing an adhesive resin, core-shell polymer particles, and polymer particles, which improves adhesive performance by using two types of particles: special core-shell polymer particles having a size of several tens to several hundreds of nanometers, and polymer particles larger than the core-shell polymer particles. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 5-295340 [Patent Document 2] Patent No. 6526571 [Patent Document 3] International Publication No. 2019 / 189238 Summary of the Invention [Problem to be solved by the invention]
[0007] A primary object of the present invention is to provide an adhesive composition which achieves both high adhesive strength and an improved cohesive failure rate. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems. As a result, it has been found that, in an adhesive composition comprising a thermosetting resin as component (A), thermoplastic resin particles as component (B), a curing agent as component (C) and / or a curing accelerator as component (D), the fracture energy G per unit area of a cured product of a mixture of components (A), (B), (C) and (D) that satisfies the predetermined conditions (I) to (III) and further consists only of components (A), (C) and (D) is 0.01 to 0.15 times that of a cured product of the mixture. 1c The fracture energy per unit area of the cured product of a mixture consisting of only components (A), (B), (C) and (D) is 1c The present invention was completed based on this finding and further intensive research.
[0009] That is, the present invention provides the following configuration. Item 1. A thermosetting resin as component (A), Thermoplastic resin particles as component (B); a curing agent as component (C) and / or a curing accelerator as component (D); An adhesive composition comprising: The component (B) contains a resin having at least one selected from the group consisting of a hydroxy group, a carboxy group, a carboxylic anhydride group, an amino group, an amide group, and a glycidyl group, The adhesive composition has a fracture energy per unit area G of a cured product of a mixture consisting of only the components (A), (C) and (D), which is calculated by the following formula (2): 1c The fracture energy per unit area of the cured product of a mixture consisting of only components (A), (B), (C) and (D) is 1c The ratio is 2.5 to 6.0 times, Destructive Energy G 1c = (fracture toughness value K 1c ) 2 / Tensile modulus E (Equation 2) The adhesive composition, wherein the components (A), (B), (C) and (D) satisfy the following conditions (I) to (III): Condition (I): The value obtained by subtracting the heat generation initiation temperature of a mixture consisting of only the components (A), (C) and (D) from the melting point of the component (B) is -10°C to 60°C. Condition (II): The difference between the tensile modulus of a cured product of the mixture consisting only of the components (A), (C), and (D) and the tensile modulus of a cured product of the mixture consisting only of the components (A), (B), (C), and (D) is 0.3 GPa or more. Condition (III): The tensile strength of a laminate to be measured, which is a cured product of a mixture consisting of only the components (A), (C) and (D) and a film formed from the component (B), is 4 MPa or more, and the strain energy per unit volume is 100 kJ / m. 3 That's all. However, the blending ratios of the components (A), (B), (C) and (D) when measuring the above conditions (I) to (III) are as follows: The functional group equivalent (molar) ratio of component (C) to component (A) is 1:1. Component (D) is 3 parts by mass per 100 parts by mass of component (A). Component (B) is 30 parts by mass per 100 parts by mass of the total of components (A), (C), and (D). In addition, when component (C) is not included in the adhesive composition, component (B) is 30 parts by mass per 100 parts by mass of the total of components (A) and (D). (Measurement of condition (III)) A film of 1.5 mm width, 1 mm thickness, and 3 mm length formed from component (B) is placed in the center of a mold with a space of 90 mm width, 1 mm thickness, and 3 mm length, and a mixture consisting of only components (A), (C), and (D) is poured into both sides of the film. The mixture is cured in the mold by successively heating at 60°C for 60 minutes, at 100°C for 60 minutes, and at 150°C for 120 minutes, to obtain a test laminate in which the cured mixture consisting of only components (A), (C), and (D) is laminated on both sides of the film. A tensile test is performed on the test laminate under conditions of a gripper distance of 25 mm and a test speed of 0.5 mm / min to determine the tensile strength. The strain energy per unit volume is determined from the obtained stress-strain curve. Item 2. The adhesive composition according to Item 1, wherein component (A) is an epoxy resin. Item 3. The adhesive composition according to item 1 or 2, wherein the content of component (A) is 7 to 95 mass %. Item 4. The adhesive composition according to any one of Items 1 to 3, wherein component (B) has a volume average particle size of 2 to 30 μm. Item 5. The adhesive composition according to any one of Items 1 to 4, which is used for bonding any one of structural materials, composite materials, electric and electronic materials, substrate materials, laminate materials, coating materials, and paints. Item 6. A cured product of the adhesive composition according to any one of items 1 to 5. Item 7. A step of applying or casting the adhesive composition according to any one of items 1 to 5 onto a surface of an object to be adhered; curing the adhesive composition; A method for producing an adhesive layer comprising the steps of: Item 8. A step of applying the adhesive composition according to any one of items 1 to 5 to a surface of an object to be adhered and disposing the adhesive composition between at least two objects to be adhered; curing the adhesive composition; A method for producing a laminate in which at least two objects to be bonded are bonded, comprising: Item 9. A step of casting the adhesive composition according to any one of items 1 to 5 between at least two objects to be adhered; curing the adhesive composition; A method for producing a laminate in which at least two objects to be bonded are bonded, comprising: Effect of the Invention
[0010] According to the present invention, it is possible to provide an adhesive composition that achieves both high adhesive strength and improved cohesive failure rate. The adhesive composition of the present invention can be suitably used for adhesion applications in which adhesive compositions are used in various industrial fields, such as structural materials, composite materials, electric and electronic materials, substrate materials, laminate materials, coating materials, and paints. In particular, the adhesive composition of the present invention can be suitably used as an adhesive composition for adhering objects that are members made of metal materials such as iron, stainless steel, and aluminum alloys, or resin materials such as engineering plastics and carbon fiber reinforced plastics, either alone or in combination. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a schematic diagram of a laminate used in the measurement of condition (III). [Diagram 2] 1 is a graph showing integral values of a stress-strain curve. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The adhesive composition of the present invention is an adhesive composition comprising a thermosetting resin as component (A), thermoplastic resin particles as component (B), a curing agent as component (C) and / or a curing accelerator as component (D), wherein component (B) comprises a resin having at least one selected from the group consisting of a hydroxy group, a carboxy group, a carboxylic anhydride group, an amino group, an amide group and a glycidyl group, and the adhesive composition has a fracture energy G 1c = (fracture toughness value K 1c ) 2 Fracture energy G per unit area of a cured product of a mixture consisting of only components (A), (C) and (D) calculated by " / tensile modulus E (Equation 2)" 1c The fracture energy per unit area of the cured product of a mixture consisting of only components (A), (B), (C) and (D) is 1c is 2.5 to 6.0 times, and further, components (A), (B), (C) and (D) satisfy the following conditions (I) to (III). By satisfying all of these configurations, the adhesive composition of the present invention can achieve both high adhesive strength and an improved cohesive failure rate.
[0013] Condition (I): The value obtained by subtracting the heat generation initiation temperature of a mixture consisting of only the components (A), (C) and (D) from the melting point of the component (B) is -10°C to 60°C.
[0014] Condition (II): The difference between the tensile modulus of a cured product of the mixture consisting only of the components (A), (C), and (D) and the tensile modulus of a cured product of the mixture consisting only of the components (A), (B), (C), and (D) is 0.3 GPa or more.
[0015] Condition (III): The tensile strength of a laminate of a cured product of a mixture consisting of only the components (A), (C) and (D) and a film formed from the component (B) is 4 MPa or more, and the strain energy per unit volume is 100 kJ / m, as measured by the following method. 3 That's all.
[0016] However, the blending ratios of the components (A), (B), (C) and (D) when measuring the above conditions (I) to (III) are as follows: Component (C) is used such that the functional group equivalent (molar) ratio with component (A) is 1:1. Component (D) is used in an amount of 3 parts by mass per 100 parts by mass of component (A). Component (B) is used in an amount of 30 parts by mass per 100 parts by mass of the total of components (A), (C), and (D). When component (C) is not included in the adhesive composition, component (B) is used in an amount of 30 parts by mass per 100 parts by mass of the total of components (A) and (D).
[0017] (Measurement of condition (III)) The film formed from the component (B) to a width of 1.5 mm, a thickness of 1 mm, and a length of 3 mm is placed in the center of a mold with a space of 90 mm in width, 1 mm in thickness, and 3 mm in length, and a mixture consisting of only the components (A), (C), and (D) is poured into both sides of the film, and the mixture is cured in the mold by successively heating at 60°C for 60 minutes, at 100°C for 60 minutes, and at 150°C for 120 minutes to obtain a test laminate in which the cured mixture consisting of only the components (A), (C), and (D) is laminated on both sides of the film. A tensile test is performed on the test laminate under conditions of a gripper distance of 25 mm and a test speed of 0.5 mm / min to determine the tensile strength. The strain energy per unit volume is determined from the obtained stress-strain curve.
[0018] The adhesive composition of the present invention will be described in detail below. In this specification, the term "comprising" includes "consisting essentially of" and "consisting of".
[0019] In addition, in this specification, a numerical value connected with "~" means a numerical range including the numerical values before and after "~" as the lower limit and upper limit. When multiple lower limit values and multiple upper limit values are listed separately, any lower limit value and upper limit value can be selected and connected with "~".
[0020] The adhesive composition of the present invention contains a thermosetting resin as component (A) and thermoplastic resin particles as component (B), and further contains at least one of a curing agent as component (C) and a curing accelerator as component (D). That is, the adhesive composition of the present invention may be a composition containing components (A), (B), (C) and (D), a composition containing components (A), (B) and (C) but not containing component (D), or a composition containing components (A), (B) and (D) but not containing component (C).
[0021] <Component (A): Thermosetting resin> Examples of component (A) include thermosetting resins such as epoxy resins, acrylic resins, and silicone resins, and from the viewpoints of adhesiveness, insulating properties, and mechanical properties, epoxy resins are preferred. As these thermosetting resins, known resins used in epoxy resin adhesives, acrylic resin adhesives, silicone resin adhesives, and the like can be used. The resin of component (A) contained in the adhesive composition of the present invention may be one type, or two or more types.
[0022] The epoxy resin may be any epoxy resin that has an epoxy group and is curable, and examples thereof include monoepoxy compounds and polyepoxy compounds.
[0023] Specific examples of monoepoxy compounds include butyl glycidyl ether, hexyl glycidyl ether, phenyl glycidyl ether, allyl glycidyl ether, para-butylphenyl glycidyl ether, para-xylyl glycidyl ether, glycidyl acetate, glycidyl butyrate, glycidyl hexoate, and glycidyl benzoate.
[0024] Examples of the polyhydric epoxy compound include bisphenol type epoxy resins, epoxy resins obtained by glycidylating polyhydric phenol compounds, novolac type epoxy resins, aliphatic ether type epoxy resins, ether ester type epoxy resins, ester type epoxy resins, amine type epoxy resins, and alicyclic epoxy resins.
[0025] Among the polyfunctional epoxy compounds, specific examples of bisphenol-type epoxy resins include epoxy resins obtained by glycidylating bisphenols such as bisphenol A, bisphenol F, bisphenol AD, bisphenol S, tetramethylbisphenol A, tetramethylbisphenol F, tetramethylbisphenol AD, tetramethylbisphenol S, tetrabromobisphenol A, tetrachlorobisphenol A, and tetrafluorobisphenol A.
[0026] Specific examples of epoxy resins obtained by glycidylating polyhydric phenol compounds include epoxy resins obtained by glycidylating dihydric phenol compounds such as biphenol, dihydroxynaphthalene, and 9,9-bis(4-hydroxyphenyl)fluorene; epoxy resins obtained by glycidylating trisphenol compounds such as 1,1,1-tris(4-hydroxyphenyl)methane; and epoxy resins obtained by glycidylating tetrakisphenol compounds such as 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane.
[0027] Specific examples of novolac type epoxy resins include epoxy resins obtained by glycidylating novolac compounds such as phenol novolac type, cresol novolac type, bisphenol A novolac type, brominated phenol novolac type, and brominated bisphenol A novolac type.
[0028] Specific examples of aliphatic ether type epoxy resins include epoxy resins obtained by glycidylating polyhydric alcohols such as glycerin and polyethylene glycol.
[0029] Specific examples of ether ester type epoxy resins include epoxy resins obtained by glycidylating hydroxycarboxylic acids such as paraoxybenzoic acid.
[0030] Specific examples of ester-type epoxy resins include epoxy resins obtained by glycidylating polycarboxylic acids such as phthalic acid and terephthalic acid.
[0031] Specific examples of amine-type epoxy resins include epoxy resins obtained by glycidylating amine compounds such as 4,4'-diaminodiphenylmethane and m-aminophenol.
[0032] Specific examples of alicyclic epoxy resins include 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexane carboxylate, 1,2-epoxy-4-vinylcyclohexane, bis(3,4-epoxycyclohexylmethyl)adipate, 1-epoxyethyl 3,4-epoxycyclohexane, limonene diepoxide, and 3,4-epoxycyclohexylmethanol.
[0033] Among these epoxy resins, polyfunctional epoxy compounds are preferred, bisphenol type epoxy resins and amine type epoxy resins are more preferred, and among these, bisphenol A type epoxy resins and bisphenol F type epoxy resins are even more preferably used.
[0034] In the adhesive composition of the present invention, the blending amount of component (A) is preferably 7 to 95 mass %, more preferably 10 to 90 mass %, and even more preferably 30 to 80 mass %, based on the total adhesive composition.
[0035] <(B) Thermoplastic resin particles> Component (B) is a thermoplastic resin particle containing a resin having at least one selected from the group consisting of a hydroxy group, a carboxy group, a carboxylic anhydride group, an amino group, an amide group, and a glycidyl group, and may be a thermoplastic resin particle that satisfies the conditions (I) to (III). By containing a resin having the reactive group described above in component (B), the adhesive composition of the present invention has a better adhesive strength. Among these, from the viewpoint of reactivity with component (A) and component (C), it is preferable to contain at least one of a carboxy group, a carboxylic anhydride group, an amino group, and a glycidyl group. The type of thermoplastic resin constituting component (B) may be any type as long as it has these reactive functional groups, and representative examples of the thermoplastic resin include polyolefin resins, nylon resins, polyester resins, polyvinyl alcohol resins, and thermoplastic polyurethane resins.
[0036] Examples of polyolefin resins include copolymer resins of olefins and other monomers, partially saponified copolymer resins of olefins and other monomers, and acid-modified polymers of olefins.
[0037] Examples of the olefin constituting the copolymer resin of an olefin and another monomer include ethylene, propylene, and styrene. Examples of the other monomer include, among the monomers copolymerizable with the olefin, α,β-unsaturated carboxylic acid, α,β-unsaturated carboxylic anhydride, metal salt of α,β-unsaturated carboxylic acid, and α,β-unsaturated carboxylic ester. Examples of the α,β-unsaturated carboxylic acid include (meth)acrylic acid. Here, (meth)acrylic acid means "methacrylic acid" and "acrylic acid". The same applies to (meth)acrylic below. Examples of the α,β-unsaturated carboxylic anhydride include maleic anhydride, and examples of the metal salt of α,β-unsaturated carboxylic acid include sodium salt and magnesium salt of (meth)acrylic acid. Examples of the α,β-unsaturated carboxylic ester include hydroxy(meth)acrylate and glycidyl(meth)acrylate. These olefins and other monomers may be used alone or in combination of two or more.
[0038] Specific examples of the copolymer resin of the above-mentioned olefin with another monomer include ethylene / (meth)acrylic acid copolymer, ethylene / maleic anhydride copolymer, propylene / maleic anhydride copolymer; ethylene / (meth)acrylic acid ester copolymers such as ethylene / glycidyl (meth)acrylate copolymer; ethylene / (meth)acrylic acid ester / maleic anhydride copolymers such as ethylene / methyl (meth)acrylate / maleic anhydride copolymer, and resins of metal salts thereof.
[0039] Examples of the partially saponified copolymer resin of an olefin and another monomer include a partially saponified copolymer resin of an olefin and a vinyl ester, and a partially saponified copolymer resin of an olefin and an α,β-unsaturated carboxylic acid ester.
[0040] Specific examples of the partially saponified product of the copolymer resin of the olefin and another monomer include a partially saponified product of an ethylene / vinyl acetate copolymer, a partially saponified product of an ethylene / methyl methacrylate copolymer, a partially saponified product of an ethylene / ethyl methacrylate copolymer, a partially saponified product of an ethylene / methyl acrylate copolymer, and a partially saponified product of an ethylene / ethyl acrylate copolymer.
[0041] Examples of the acid-modified olefin polymer include acid-modified polyolefins such as maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, and maleic anhydride-modified styrene-ethylene-butylene-styrene (SEBS) copolymer.
[0042] Examples of nylon resins include -[NH(CH2)5CO]-, -[NH(CH2)4NHCO(CH2)4CO]-, -[NH(CH2)6NHCO(CH2)4CO]-, -[NH(CH2)6NHCO(CH2)8CO]-, -[NH(CH2) 10 CO]- and -[NH(CH2) 11 Specific examples of such nylon resins include nylon 6, nylon 46, nylon 66, nylon 610, nylon 11, nylon 12, and copolymers thereof, as well as nylon elastomers which are copolymers with polyesters or polyalkylene ether glycols.
[0043] In the present invention, the polyolefin resin, nylon resin, polyester resin, polyvinyl alcohol resin, and thermoplastic polyurethane resin may be used either alone or in combination of two or more kinds.
[0044] Among these, preferred components (B) are, from the viewpoint of being more flexible than component (A) and containing reactive functional groups, thermoplastic resin particles containing ethylene / (meth)acrylic acid copolymer, ethylene / glycidyl methacrylate copolymer, maleic anhydride-modified polyethylene, and nylon elastomer.
[0045] The volume average particle size of component (B) according to the present invention is, for example, 1 μm to 100 μm, and preferably 2 to 30 μm. If it is smaller than 1 μm, it is difficult to handle, and the viscosity increases in the process of mixing with component (A), which may impair workability. If it is larger than 100 μm, it may be easily separated when mixed with a curable resin, which may result in poor dispersion stability. By being 2 μm to 30 μm, the addition effect is more likely to be fully exerted without impairing workability.
[0046] The volume average particle diameter of component (B) is the volume average particle diameter determined by the electrical detection zone method (pore electrical resistance method). A specific device for measuring the volume average particle diameter by the pore electrical resistance method is, for example, an electrical detection type particle size distribution measuring device (trade name "Coulter Multisizer" manufactured by Beckman Coulter, Inc.). The aperture diameter used for the measurement is of various sizes, and each aperture diameter has a measurement range (volume average particle diameter) suitable for the measurement. The aperture diameter can be selected so as to cover the particle diameter present in the particles to be measured, and in the examples described below, an aperture diameter of 100 μm was used based on this policy. When measuring particles having a particle diameter smaller than the measurement range suitable for an aperture diameter of 100 μm, an aperture diameter smaller than 100 μm can be selected, and when measuring particles having a particle diameter larger than the measurement range suitable for an aperture diameter of 100 μm, an aperture diameter larger than 100 μm can be selected.
[0047] The shape of component (B) according to the present invention is not particularly limited as long as workability is not impaired, and examples thereof include spherical, irregular, scaly, etc. From the viewpoints of easy dispersion in the adhesive composition and suppression of viscosity increase, a spherical shape is preferred.
[0048] Component (B) according to the present invention can also contain inorganic particles such as alumina and silica, metal powders such as iron, copper, nickel and cobalt, and organic substances such as ultraviolet absorbers and heat stabilizers within or on the surface of the particles.
[0049] In the adhesive composition of the present invention, the amount of component (B) is adjusted so as to satisfy the above-mentioned fracture energy per unit area G 1c The amount of component (B) is preferably 3 to 300 parts by mass, more preferably 5 to 200 parts by mass, and even more preferably 10 to 80 parts by mass, per 100 parts by mass of component (A).
[0050] <Component (C): Hardener> The curing agent as component (C) is one that reacts with component (A), which is a thermosetting resin, to obtain a cured product, and may be any curing agent that satisfies the conditions (I) to (III). Component (C) may be used alone or in combination of two or more types. When component (C) is used in combination of two or more types, the mixture of the mixed curing agents is regarded as one component (C).
[0051] Examples of component (C) include amine-based curing agents, amide-based curing agents, acid anhydride-based curing agents, phenol-based curing agents, mercaptan-based curing agents, isocyanate-based curing agents, active ester-based curing agents, and cyanate ester-based curing agents.
[0052] Examples of the amine-based curing agent include chain aliphatic amines such as ethylenediamine, diethylenetriamine, triethylenetetramine, and tetraethylenepentamine; alicyclic amines such as isophoronediamine, bis(4-aminocyclohexyl)methane, and bis(aminomethyl)cyclohexane; and aromatic amines such as metaphenylenediamine, diaminodiphenylmethane, diethyltoluenediamine, and diethyldiaminodiphenylmethane.
[0053] Examples of the amide-based curing agent include dicyandiamide and its derivatives, polyamide resins (polyaminoamide, etc.), and the like.
[0054] Examples of the acid anhydride curing agent include aliphatic acid anhydrides such as maleic anhydride and dodecenylsuccinic anhydride; aromatic acid anhydrides such as phthalic anhydride, trimellitic anhydride and pyromellitic anhydride; and alicyclic acid anhydrides such as methylnadic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride and 4-methylhexahydrophthalic anhydride.
[0055] Examples of phenol-based curing agents include phenol novolac resins, cresol novolac resins, biphenyl novolac resins, triphenylmethane phenol resins, naphthol novolac resins, phenol biphenylene resins, phenol aralkyl resins, biphenyl aralkyl phenol resins, modified polyphenylene ether resins, and compounds having a benzoxazine ring.
[0056] Examples of mercaptan-based curing agents include trimethylolpropane tris(3-mercaptopropionate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, pentaerythritol tetrakis(3-mercaptopropionate), tetraethylene glycol bis(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), 1,4-bis(3-mercaptobutyryloxy)butane, trimethylolpropane tris(3-mercaptobutyrate), trimethylolethane tris(3-mercaptobutyrate), and polysulfide polymers.
[0057] Examples of the isocyanate curing agent include hexamethylene diisocyanate, 1,4-tetramethylene diisocyanate, 2-methylpentane-1,5-diisocyanate, lysine diisocyanate, isophorone diisocyanate, and norbornane diisocyanate.
[0058] The active ester curing agent is a compound having one or more ester groups per molecule that react with the (A) thermosetting resin, and examples of such an active ester curing agent include phenyl esters, naphthyl esters, thiophenyl esters, N-hydroxyamine esters, and heterocyclic hydroxy compound esters.
[0059] Examples of the cyanate ester curing agent include bisphenol type cyanate resins such as novolac type cyanate resin, bisphenol A type cyanate resin, bisphenol E type cyanate resin, and tetramethylbisphenol F type cyanate resin.
[0060] In the adhesive composition of the present invention, it is preferable to use, as component (C), at least one selected from the group consisting of an amine-based curing agent, an acid anhydride-based curing agent, an amide-based curing agent, and a phenol-based curing agent, and an amine-based curing agent or an acid anhydride-based curing agent is more preferable.
[0061] In the adhesive composition of the present invention, the amount of component (C) is set to be within the range of the fracture energy G 1c The amount of component (C) is preferably such that the equivalent of the reactive functional group in component (C) is 0.1 to 5 equivalents per equivalent of the reactive functional group (e.g., epoxy group) in component (A), which is usually a thermosetting resin. The equivalent of the reactive functional group in component (C) is more preferably 0.3 to 3 equivalents, and even more preferably 0.5 to 2 equivalents.
[0062] <(D) Curing accelerator> The curing accelerator as component (D) is a component that accelerates the curing of component (A), which is a thermosetting resin. In addition, by using component (D) in combination with component (C), it is possible to increase the curing reaction speed and increase the strength of the obtained cured product. Note that component (D) can accelerate the curing of component (A) even without using it in combination with component (C). Component (D) may be used alone or in a mixture of two or more types. Note that when two or more types of component (D) are used in a mixture, the mixture of the mixed curing accelerators is regarded as one component (D).
[0063] Examples of the component (D) include imidazole compounds such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 1,2-dimethylimidazole, and 1-benzyl-2-methylimidazole; secondary amines such as piperidine; tertiary amines such as DBU (1,8-diazabicyclo(5,4,0)-undecene-7), DBN (1,5-diazabicyclo(4,3,0)-nonene-5), 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, triethylenediamine, 2-(dimethylaminomethyl)phenol, and 4-dimethylaminopyridine; phosphorus compounds such as triphenylphosphine and tetraphenylphosphonium tetraphenylborate, Lewis acid compounds, and cationic polymerization initiators.
[0064] In the adhesive composition of the present invention, it is preferable to use as component (D) at least one selected from the group consisting of imidazole compounds, tertiary amines, phosphorus-based compounds, and cationic polymerization initiators.
[0065] In the adhesive composition of the present invention, the amount of component (D) is set to be within the range of the fracture energy G 1c The blending amount may be such that the ratio of the above is 2.5 to 6.0 times. For example, the blending amount is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.5 to 5 parts by mass, per 100 parts by mass of component (A).
[0066] In the adhesive composition of the present invention, the total content of components (A), (B), (C) and (D) is preferably 10 mass% or more, more preferably 30 mass% or more, even more preferably 50 mass% or more, still more preferably 70 mass% or more, and may be 100 mass%.
[0067] In the present invention, components (A), (B), (C) and (D) satisfy the following conditions (I) to (III).
[0068] (Mixing ratio of components (A), (B), (C) and (D) in the measurements under conditions (I) to (III)) Component (C) is used such that the functional group equivalent (molar) ratio with component (A) is 1:1. Component (D) is used in an amount of 3 parts by mass per 100 parts by mass of component (A). Component (B) is used in an amount of 30 parts by mass per 100 parts by mass of the total of components (A), (C), and (D). In addition, when component (C) is not included in the adhesive composition, component (B) is used in an amount of 30 parts by mass per 100 parts by mass of the total of components (A) and (D).
[0069] <Condition (I)> The condition (I) is that the value obtained by subtracting the heat generation initiation temperature of a mixture consisting of only components (A), (C) and (D) from the melting point of component (B) is -10°C to 60°C. The condition (I) is a condition related to the thermal performance of component (B) which is a thermoplastic resin particle. Specifically, it is the temperature difference between the melting point (or endothermic peak top temperature) of component (B) and the heat generation initiation temperature of a mixture consisting of only components (A), (C) and (D) which does not contain component (B) (a mixture consisting of only components (A) and (D) when the adhesive composition does not contain component (C), and a mixture consisting of only components (A) and (C) when the adhesive composition does not contain component (D)). When this temperature difference is -10 to 60°C, the intermolecular interaction near the interface between component (A) which is a thermosetting resin and component (B) which is a thermoplastic resin particle becomes active. When the interaction between component (A) and component (B) becomes active, the cured product has excellent fracture resistance and improves fracture toughness. The lower limit of the temperature difference is preferably -5°C, more preferably -2°C. The upper limit is preferably 55°C, more preferably 50°C.
[0070] (Measurement of melting point and heat generation onset temperature) The melting point (or endothermic peak top temperature) and heat generation initiation temperature of each mixture and particle are measured by the following method. The temperature is measured at a temperature rise rate of 5°C / min using a differential scanning calorimeter (DSC6220, Hitachi High-Tech Science Co., Ltd.). The heat generation initiation temperature is defined as the point (Ta) at which the so-called DSC curve, which is a curve plotting the amount of heat (mW / mg) per 1 mg of sample at each measurement temperature during temperature rise, starts to deviate from the baseline.
[0071] <Condition (II)> Condition (II) is that the difference between the tensile modulus of a cured product of a mixture consisting only of components (A), (C) and (D) and the tensile modulus of a cured product of a mixture consisting only of components (A), (B), (C) and (D) is 0.3 GPa or more. Condition (II) is a condition showing the difference in tensile modulus depending on the presence or absence of component (B), which is a thermoplastic resin particle. Specifically, the difference in tensile modulus between a cured product of a mixture consisting of only components (A), (C) and (D) without component (B) (a mixture of only components (A) and (D) when the adhesive composition does not contain component (C), or a mixture of only components (A) and (C) when the adhesive composition does not contain component (D)) and a cured product of a mixture consisting of only components (A), (B), (C) and (D) (a mixture of only components (A), (B) and (D) when the adhesive composition does not contain component (C), or a mixture of only components (A), (B) and (C) when the adhesive composition does not contain component (D)) is 0.3 GPa or more. This difference in tensile modulus of elasticity of 0.3 GPa or more improves the strength of the interaction between components (A) and (B) as well as the effect of alleviating internal stress caused by distortion, etc. The lower limit of the difference in tensile elastic modulus is preferably 0.6 GPa, more preferably 0.8 GPa, and the upper limit is preferably 2.5 GPa.
[0072] (Measurement of tensile modulus) A mixture consisting of only components (A), (C) and (D) is prepared, and the resulting mixture is poured into a mold (length 90 mm, width 20 mm, thickness 2 mm), heated at 60°C for 60 minutes, heated to 100°C at 2°C / min, heated at 100°C for 60 minutes, heated to 150°C at 2.5°C / min, and heated at 150°C for 120 minutes in succession to cure, and then cut into rectangular cured product test pieces (length 80 mm, width 5 mm, thickness 2 mm). The obtained cured product test pieces are each subjected to a tensile test under the conditions of a gripping distance of 25 mm and a test speed of 0.5 mm / min, and the tensile stress (σ) and strain (ε) are measured to determine the tensile modulus. The tensile modulus is calculated according to the method specified in JIS K7161, specifically, from the gradient of the straight line at small strain (Equation 1). E = (σ2-σ1) / (ε2-ε1) (Equation 1) σ2: Tensile stress measured at ε2 = 0.0025 σ1: Tensile stress measured at ε1=0.0005 The tensile modulus of a cured product of a mixture consisting only of components (A), (B), (C) and (D) is also measured in a similar manner by a tensile test, and the difference in the tensile modulus is calculated.
[0073] <Condition (III)> The condition (III) is that the tensile strength of a laminate to be measured, which is a cured product of a mixture consisting of only the components (A), (C) and (D) and a film formed from the component (B), is 4 MPa or more, and the strain energy per unit volume is 100 kJ / m 3 or more. Condition (III) is a condition related to the strength of the interface between a film formed from component (A) which is a thermosetting resin and component (B) which is a thermoplastic resin particle. Specifically, a laminate for measurement made of a cured product of a mixture consisting of only components (A), (C) and (D) without component (B) (a mixture of only components (A) and (D) when the adhesive composition does not contain component (C), and a mixture of only components (A) and (C) when the adhesive composition does not contain component (D)) and a film formed from component (B) must have a tensile strength of 4 MPa or more and a strain energy per unit volume of 100 kJ / m 3The tensile strength is 4 MPa or more, which is considered to indicate that the interface between component (A) and component (B) has an interaction. In addition, the strain energy per unit volume is 100 kJ / m 3 It is believed that the interfacial interaction between component (A) and component (B) is strengthened by satisfying the above numerical values. By satisfying the above numerical values, the adhesive composition used will fully exert the effect of adding component (B) to the adhesive layer, improving fracture toughness. The lower limit of the tensile strength is preferably 5 MPa, more preferably 6 MPa, and the upper limit is preferably 50 MPa, more preferably 20 MPa. The lower limit of the strain energy per unit volume is preferably 150 kJ / m 3 , more preferably 200 kJ / m 3 The upper limit is preferably 20000 kJ / m 3 , more preferably 5000 kJ / m 3 It is.
[0074] (Measurement of condition (III)) The component (B) is molded and cut into a film having a width of 1.5 mm, a thickness of 1 mm, and a length of 3 mm. The film is placed in the center of a mold having a space of 90 mm in width, 1 mm in thickness, and 3 mm in length. A mixture consisting of only the components (A), (C), and (D) is poured into both sides of the film, and the mixture is cured in the mold by heating at 60°C for 60 minutes, increasing the temperature to 100°C at 2°C / min, heating at 100°C for 60 minutes, increasing the temperature to 150°C at 2.5°C / min, and heating at 150°C for 120 minutes in succession, thereby obtaining a test laminate in which the cured mixture consisting of only the components (A), (C), and (D) is laminated on both sides of the film. A tensile test is performed on the test laminate under the conditions of a gripper distance of 25 mm and a test speed of 0.5 mm / min to determine the tensile strength. The strain energy per unit volume is determined from the stress-strain curve shown in Figure 2. The strain energy per unit volume is the area enclosed from the start point of the tensile test to the break point, and is calculated from the integral of the tensile stress from the start point of the tensile test to the break point, with the strain as a variable. The integral is calculated by calculating the area of the smallest rectangle obtained at the minimum tensile stress within the strain width for each 0.0001 [mm / mm] strain width from the start of tension, and then summing up the areas of all the rectangles up to the break point.
[0075] The film of component (B) is formed according to the following guidelines. It is formed by pressing for 30 seconds at a temperature 25°C higher than the melting point of component (B) using a heat press (e.g., a manual hydraulic vacuum heating press (manufactured by Imoto Manufacturing Co., Ltd.) at a pressure of 0.2 MPa. For example, when the melting point of component (B) is 97°C, it is formed by pressing for 30 seconds at a temperature of 130°C and a pressure of 0.2 MPa. When the melting point of component (B) is 175°C, it is formed by pressing for 30 seconds at a temperature of 200°C and a pressure of 0.2 MPa.
[0076] The adhesive composition of the present invention has a fracture energy per unit area G of a cured product of a mixture consisting of only the components (A), (C) and (D), which is calculated by the following formula (2): 1cThe fracture energy per unit area of the cured product of a mixture consisting of only components (A), (B), (C) and (D) is 1c The ratio of the fracture energy G is 2.5 to 6.0 times. By setting the ratio to 2.5 to 6.0 times, an adhesive composition capable of achieving both high adhesiveness and a high cohesive failure rate is obtained. 1c The lower limit of this ratio is preferably 3, and the upper limit is preferably 5. From the viewpoint of suitably adjusting the ratio to 2.5 to 6.0, the adhesive composition of the present invention preferably contains the components in such a mass ratio that component (A):component (B):component (C):component (D) satisfies the relationship of 1:0.03-3:0-2:0-0.1 (excluding the case where the mass ratios of components (C) and (D) are simultaneously 0).
[0077] Destructive Energy G 1c = (fracture toughness value K 1c ) 2 / Tensile modulus E (Equation 2)
[0078] (Destructive energy G 1c (Measurement of the ratio of A mixture consisting of only components (A), (C) and (D) (a mixture of only components (A) and (D) when the adhesive composition does not contain component (C), or a mixture of only components (A) and (C) when the adhesive composition does not contain component (D)) is poured into a mold (length 90 mm, width 20 mm, thickness 3 mm), heated at 60°C for 60 minutes, heated to 100°C at 2°C / min, heated at 100°C for 60 minutes, heated to 150°C at 2.5°C / min, and heated at a temperature of 150°C for 120 minutes in succession to cure the mixture in the mold and prepare a rectangular cured product test piece. The obtained cured product test piece is cut to a size of 60 mm in length, 3 mm in width and 10 mm in thickness, and mechanically processed to a depth of 5 mm in the thickness direction at the center of the length direction using a PCB cutter or the like. Furthermore, a scratch with a depth of 0.1 mm in the thickness direction is made with a razor at the mechanically processed tip of the cured material. The total crack length is a = 5.1 mm. After that, a three-point bending test is performed in the compression direction at a speed of 1 mm / min and a support distance S = 40 mm using a tensile testing machine (AGS-X, Shimadzu Corporation), and the K value of ASTM E399 is obtained.1C In accordance with the provisions of the law, the fracture toughness value (K 1C (MPa m 1 / 2 ) is calculated by the following formula (3): Q is the load (N). K 1C ={(P Q ×S) / (B×W 3 / 2 )}×f(a / W) (Equation 3) f(a / W)=(3(a / W) 1 / 2 [1.99-(a / W)(1-a / W){2.15-3.93(a / W)+2.7(a / W) 2}]) / [2{1+2(a / W)}{1-(a / W)} 3 / 2 ] (Formula 4)
[0079] The obtained fracture toughness value (K 1C ) and the tensile modulus (E) calculated by (Equation 1), the fracture energy per unit area (G 1C ) is calculated.
[0080] Similarly, the fracture toughness (K 1C (MPa m 1 / 2 )) and calculate the fracture energy G 1c Calculate the ratio to.
[0081] In the adhesive composition of the present invention, the fracture energy per unit area G of a cured product of a mixture consisting of only components (A), (B), (C) and (D) is 1c is preferably 500 to 20,000 J / m 2 , more preferably 700 to 8000 J / m 2 , and more preferably 900 to 5000 J / m 2 The fracture energy per unit area G of the cured product of the mixture consisting of only components (A), (C) and / or (D) is 1c is preferably 200 to 3500 J / m 2 , more preferably 250 to 1500 J / m 2 , and more preferably 300 to 1000 J / m 2 It is.
[0082] <Additives that may be included in the adhesive composition> The adhesive composition of the present invention may contain other additives as necessary, provided that the additives do not impair the object and effect of the present invention.
[0083] Examples of additives include organic fillers not included in component (B), thermoplastic resins, rubbers, elastomers, composite particles, inorganic fillers, conductive particles, carbon black, antioxidants, inorganic phosphors, lubricants, ultraviolet absorbers, heat and light stabilizers, antistatic agents, polymerization inhibitors, defoamers, solvents, antiaging agents, radical inhibitors, adhesion improvers, flame retardants, surfactants, storage stability improvers, ozone antioxidants, thickeners, plasticizers, radiation shielding agents, nucleating agents, coupling agents, conductivity imparting agents, phosphorus-based peroxide decomposers, pigments, metal deactivators, and physical property adjusters.
[0084] The additive may be contained in an amount of, for example, 0 to 90% by mass based on the entire adhesive composition. If the additive is contained in an amount exceeding 90% by mass, the stability of the entire composition is impaired, and the object and effect of the present invention cannot be fully achieved. The content of the additive in the adhesive composition of the present invention is preferably 70% by mass or less, more preferably 50% by mass or less, and even more preferably 30% by mass or less, and may not be contained.
[0085] <Method of manufacturing adhesive composition> The adhesive composition of the present invention can be produced by mixing component (A), component (B), component (C) and / or component (D), and further, if necessary, other additives.
[0086] The mixing method is not particularly limited as long as it can mix the components uniformly. For example, mixing and stirring with a paddle blade, mixing and stirring with a homomixer, mixing and stirring with a planetary mixer, etc. can be mentioned.
[0087] The adhesive composition of the present invention has a low viscosity and can be prepared without adding a solvent; however, if necessary, a solvent (e.g., toluene, xylene, methyl ethyl ketone, acetone, cyclohexanone, methylcyclohexane, cyclohexane, etc.) may be added within a range that does not affect the effects of the present invention.
[0088] A cured product can be obtained by curing the adhesive composition of the present invention. The curing method is not particularly limited and may be appropriately selected depending on the type of curing reaction of the curable resin. For example, the curing method can be performed by heating the composition. For example, in the case of curing by heating, the curing temperature is usually room temperature (25°C) to 250°C, and the curing time varies depending on the composition liquid and can usually be set in a wide range from 30 seconds to 1 week. Considering the influence on the thermal properties of the (B) component of the present invention and the interaction with other components, and from the viewpoint of preventing deterioration due to thermal history, it is preferable to set the curing temperature to 40°C to 200°C and the curing time to 1 minute to 12 hours.
[0089] The adhesive composition of the present invention can be suitably used for bonding structural materials, composite materials, electric and electronic materials, substrate materials, laminate materials, coating materials, paints, etc. Examples of adhesives for structural materials include adhesives for bonding metal materials, polymeric materials, inorganic materials, etc. used in automobiles and vehicles (bullet trains, trains), aircraft, the space industry, etc. Examples of adhesives for electric and electronic materials, substrate materials, and laminate materials include adhesives, sealants, and underfills for use between layers of multilayer substrates, for semiconductors, and for mounting.
[0090] <Cured product of adhesive composition> The cured product of the adhesive composition of the present invention is obtained by curing the above-mentioned adhesive composition of the present invention. The method for curing the adhesive composition of the present invention is not particularly limited, but includes a method of heating the adhesive composition of the present invention as described above.
[0091] <Method of manufacturing adhesive layer> The adhesive layer of the present invention can be produced by a production method including a step of applying or casting the adhesive composition of the present invention onto the surface of an object to be adhered, and a step of curing the adhesive composition. The method of curing the adhesive composition of the present invention is as described above.
[0092] <Method of manufacturing laminate> The method for producing a laminate of the present invention includes a step of applying the adhesive composition to the surface of an object to be adhered, disposing the adhesive composition between at least two objects to be adhered, and a step of curing the adhesive composition. The method for producing a laminate of the present invention also includes a step of casting the adhesive composition between at least two objects to be adhered, and a step of curing the adhesive composition. The method for curing the adhesive composition of the present invention is as described above. Also, the objects to be adhered may be those mentioned above. EXAMPLES
[0093] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0094] <Component (A): Thermosetting resin> As the component (A), the following thermosetting resins (A-1) and (A-2) were prepared. [Thermosetting resin A-1] Bisphenol F type epoxy resin (jER806; manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: 167) was used as component (A-1). [Thermosetting resin A-2] Bisphenol A type epoxy resin (jER828; manufactured by Mitsubishi Chemical Corporation, epoxy equivalent: 186) was used as component (A-2).
[0095] <Component (B): Thermoplastic resin particles> As the component (B), the following thermoplastic resin particles (B-1) to (B-6) were prepared.
[0096] [Thermoplastic resin particles B-1] As a resin having a carboxy group, an ethylene / acrylic acid copolymer (volume average particle size 10 μm, melting point 97° C., Flow Beads EA209 manufactured by Sumitomo Seika Chemicals) was used as thermoplastic resin particles B-1.
[0097] [Thermoplastic resin particles B-2] As a resin having a carboxy group, an amino group, and an amide group, 12 nylon (volume average particle size 20 μm, melting point 175° C., Orgasol 2002D manufactured by Arkema) was used as thermoplastic resin particles B-2.
[0098] [Thermoplastic resin particles B-3] In a pressure-resistant autoclave with an internal volume of 1 liter equipped with a turbine-type stirring blade with a diameter of 50 mm, 160 g of ethylene / glycidyl methacrylate copolymer resin (GMA content 19% by mass), 224 g of deionized water, and 16 g of ethylene oxide / propylene oxide copolymer (weight average molecular weight 15,500, ethylene oxide content 80% by mass) as an emulsifier were charged and sealed. Next, the inside of the autoclave was heated to 150°C while stirring at 500 revolutions per minute. After stirring for another 30 minutes while maintaining the internal temperature at 150°C, the contents were cooled to 25°C to obtain an aqueous dispersion of ethylene / glycidyl methacrylate copolymer. Next, the aqueous dispersion was filtered with filter paper, washed with water, and dried in a vacuum dryer at 40°C for 24 hours to obtain ethylene / glycidyl methacrylate copolymer particles as thermoplastic resin particles (B-3). The volume average particle diameter of the thermoplastic resin particles B-3 was 13 μm, and the melting point was 88°C.
[0099] [Thermoplastic resin particles B-4] In a pressure-resistant autoclave with an internal volume of 1 liter equipped with a turbine-type stirring blade with a diameter of 50 mm, 160 g of maleic anhydride-modified polyethylene resin (maleic anhydride content 0.5% by mass), 224 g of deionized water, and 16 g of ethylene oxide / propylene oxide copolymer (weight average molecular weight 15,500, ethylene oxide content 80% by mass) as an emulsifier were charged and sealed. Next, the inside of the autoclave was heated to 160°C while stirring at 500 revolutions per minute. After stirring for another 30 minutes while maintaining the internal temperature at 160°C, the contents were cooled to 25°C to obtain an aqueous dispersion of maleic anhydride-modified polyethylene. Next, the aqueous dispersion was filtered with filter paper, washed with water, and dried in a vacuum dryer at 60°C for 24 hours to obtain maleic anhydride-modified polyethylene particles as thermoplastic resin particles (B-4). The volume average particle diameter of the thermoplastic resin particles B-4 obtained here was 25 μm, and the melting point was 120°C.
[0100] [Thermoplastic resin particles B-5] In a pressure-resistant autoclave with an internal volume of 1 liter equipped with a turbine-type stirring blade with a diameter of 50 mm, 160 g of 12 nylon / polyalkylene ether glycol copolymer resin, 224 g of deionized water, and 16 g of ethylene oxide / propylene oxide copolymer (weight average molecular weight 15,500, ethylene oxide content 80% by mass) were charged and sealed. Next, the inside of the autoclave was heated to 180°C while stirring at 500 revolutions per minute. After stirring for another 30 minutes while maintaining the internal temperature at 180°C, the contents were cooled to room temperature to obtain an aqueous dispersion of 12 nylon / polyalkylene ether glycol copolymer. Next, the aqueous dispersion was filtered with filter paper, washed with water, and dried in a vacuum dryer at 60°C for 24 hours to obtain 12 nylon / polyalkylene ether glycol copolymer particles as thermoplastic resin particles (B-5). The volume average particle diameter of the thermoplastic resin particles B-5 obtained here was 11 μm, and the melting point was 140°C.
[0101] [Thermoplastic resin particles B-6] As thermoplastic resin particles having no functional group, polypropylene (volume average particle size 5 μm, melting point 145° C., PPW-5 manufactured by Seishin Enterprise Co., Ltd.) was used as thermoplastic resin particles (B-6).
[0102] <Component (C): Hardener> As the component (C), the following curing agent (C-1) and curing agent (C-2) were prepared. [Hardening agent C-1] An acid anhydride-based hardener (RIKACID MH700; a liquid alicyclic acid anhydride whose main component is 4-methylhexahydrophthalic anhydride, manufactured by New Japan Chemical Co., Ltd.) was used as the hardener (C-1). [Hardening agent C-2] An amine-based curing agent (Kayahard AA; diethyldiaminodiphenylmethane, manufactured by Nippon Kayaku Co., Ltd.) was used as the curing agent (C-2).
[0103] <Component (D): Curing accelerator> As the component (D), the following curing accelerator (D-1) and curing accelerator (D-2) were prepared. [Cure Accelerator D-1] An imidazole-based curing accelerator (Curezol 1B2MZ; 1-benzyl-2-methylimidazole, manufactured by Shikoku Kasei Co., Ltd.) was used as component (D-1). [Cure Accelerator D-2] An imidazole-based curing accelerator (Curezol 2E4MZ; 2-ethyl-4-methylimidazole, manufactured by Shikoku Kasei Co., Ltd.) was used as component (D-2).
[0104] <Preparation of each composition> [Example 1: Adhesive composition (1)] In the following procedure, 38.4 parts by mass of component (A-1) (functional group equivalent: 0.23) was used to prepare the composition shown in Table 1. 37.3 parts by mass of component (C-1) (functional group equivalent: 0.23), which had been adjusted to have an equivalent functional group equivalent, 1.2 parts by mass of component (D) (3 parts by mass per 100 parts by mass of epoxy resin), and 23.1 parts by mass of component (B-1) were weighed into a plastic container and stirred at 2000 rpm for 1 minute and degassed at 2200 rpm for 1 minute using a Foam Remover Rentaro (ARE-310, manufactured by Shinki Corporation), to prepare an adhesive composition (1).
[0105] [Examples 2-8 and Comparative Examples 1-7: Adhesive Compositions (2)-(15)] Adhesive compositions (2)-(15) were prepared by mixing and stirring component (A), component (B), component (C) and / or component (D) so as to obtain the compositions shown in Table 1.
[0106] Regarding the components (A), (B), (C) and (D) used in producing the adhesive compositions (1)-(15), the blending ratios of the components (A), (B), (C) and (D) when measuring the following conditions (I) to (III) were as follows. Note that, since the same components (A) to (D) were used in Examples 1 to 4, the measured values under the following conditions (I) to (III) were also the same. The same applies to Comparative Examples 1, 2 and 4.
[0107] (Mixing ratio of components (A), (B), (C) and (D) in the measurements under conditions (I) to (III)) Component (C) is used such that the functional group equivalent (molar) ratio with component (A) is 1:1. Component (D) is used in an amount of 3 parts by mass per 100 parts by mass of component (A). Component (B) is used in an amount of 30 parts by mass per 100 parts by mass of the total of components (A), (C), and (D). When component (C) is not included in the adhesive composition, component (B) is used in an amount of 30 parts by mass per 100 parts by mass of the total of components (A) and (D).
[0108] [Condition (I): Melting point - Heat generation onset temperature] For each of the adhesive compositions (1)-(7) and (9)-(15), the melting point of component (B) minus the heat generation initiation temperature of a mixture consisting only of components (A), (C), and (D) was measured using the following procedure. As for adhesive composition (8), since it does not contain component (C), the value obtained by subtracting the heat generation initiation temperature of a mixture consisting only of components (A) and (D) from the melting point of component (B) was measured using the following procedure.
[0109] A mixture consisting of only components (A), (C) and (D) in the above blending ratio, not including component (B), or a mixture consisting of only components (A) and (D) was prepared, and the heat generation start temperature of the obtained mixture was measured at a heating rate of 5°C / min using a differential scanning calorimeter (DSC6220, Hitachi High-Tech Science Co., Ltd.). The heat generation start temperature was the point at which the so-called DSC curve, which is a curve plotting the amount of heat (mW / mg) in 1 mg of sample at each measurement temperature during heating, begins to move away from the baseline. In addition, in order to specify the melting point of component (B), a differential scanning calorimeter (DSC6220, Hitachi High-Tech Science Co., Ltd.) was used to measure the melting point (endothermic peak top temperature) at a heating rate of 5°C / min. The value of melting point - heat generation start temperature was calculated from the obtained heat generation start temperature and melting point. The results are shown in Table 1.
[0110] [Condition (II): Difference in tensile modulus] For adhesive compositions (1)-(7) and (9)-(15), the difference in tensile modulus between the cured product of a mixture consisting of only components (A), (C), and (D) and the cured product of a mixture consisting of only components (A), (B), (C), and (D) was measured by the following procedure. For adhesive composition (8), the difference in tensile modulus between the cured product of a mixture consisting of only components (A) and (D) and the cured product of a mixture consisting of only components (A), (B), and (D) was measured by the following procedure. A mixture consisting of only components (A), (C) and (D) in the above blending ratio, or a mixture consisting of only components (A) and (D) was prepared in each of the above blending ratios, except that component (B) was not included, and the resulting mixture was poured into a polymethylpentene mold (length 90 mm, width 20 mm, thickness 2 mm), heated at 60°C for 60 minutes, heated to 100°C at 2°C / min, heated at 100°C for 60 minutes, heated to 150°C at 2.5°C / min, and heated at 150°C for 120 minutes in succession to be cured, and a rectangular cured product test piece (length 80 mm, width 5 mm, thickness 2 mm) was produced. The obtained cured product test piece was subjected to a tensile test under the conditions of a gripper distance of 25 mm and a test speed of 0.5 mm / min, and the tensile stress (σ) and strain (ε) were measured to determine the tensile modulus. The tensile modulus was calculated according to the method specified in JIS K7161, specifically, from the gradient of the straight line at small strain (Equation 1). E = (σ2-σ1) / (ε2-ε1) (Equation 1) σ2: Tensile stress measured at ε2 = 0.0025 σ1: Tensile stress measured at ε1=0.0005 The tensile modulus of the cured product of the mixture consisting of only components (A), (B), (C) and (D) was also measured by a tensile test in the same manner, and the difference in the tensile modulus was calculated. The results are shown in Table 1.
[0111] [Condition (III): Tensile strength and strain energy] For adhesive compositions (1)-(7) and (9)-(15), the tensile strength and strain energy per unit volume of a laminate of a cured product of a mixture consisting of only components (A), (C), and (D) and a film formed from component (B) were measured by the following procedure. For adhesive composition (8), the tensile strength and strain energy per unit volume of a laminate of a cured product of a mixture consisting of only components (A) and (D) and a film formed from component (B) were measured by the following procedure. For component (B), a film was molded at a temperature 25°C higher than the melting point of component (B), at a pressure of 0.2 MPa, and for 30 seconds, and cut to a width of 1.5 mm, a thickness of 1 mm, and a length of 3 mm. The film was placed in the center of a polymethylpentene mold having a space of width 90 mm, thickness 1 mm, and length 3 mm, and a mixture consisting of only the components (A), (C), and (D) (components (A) and (D) for adhesive composition (8)) was poured on both sides of the film, and the mixture was cured in the mold by heating at 60°C for 60 minutes, increasing the temperature to 100°C at 2°C / min, heating at 100°C for 60 minutes, increasing the temperature to 150°C at 2.5°C / min, and heating at 150°C for 120 minutes. A measurement laminate was obtained in which a cured product of a mixture consisting of only the components (A), (C), and (D) (components (A) and (D) for adhesive composition (8)) was laminated on both sides of a film formed from component (B). A tensile test was performed on this measurement laminate under conditions of a gripper distance of 25 mm and a test speed of 0.5 mm / min to determine the tensile strength. The strain energy per unit volume was calculated from the obtained stress-strain curve. The strain energy per unit volume was calculated by using the strain as a variable and calculating the integral value of the tensile stress from the start point of the tensile test to the breaking point. The integral value was calculated by calculating the area of the smallest rectangle obtained at the minimum tensile stress within the strain width for every 0.0001 [mm / mm] of strain width from the start of tension, and then adding up the areas of all the rectangles up to the breaking point. The results are shown in Table 1.
[0112] [Fracture energy ratio] For adhesive compositions (1)-(7) and (9)-(15), the fracture energy G per unit area of a cured product of a mixture consisting only of components (A), (C) and (D) is calculated by the following formula (2): 1c The fracture energy per unit area of the cured product of a mixture consisting of only components (A), (B), (C) and (D) is 1c The ratio of the fracture energy G per unit area of the cured product of the mixture consisting of only components (A) and (D) of adhesive composition (8) was calculated using the following formula (2): 1c The fracture energy per unit area G of a mixture consisting of only components (A), (B) and (D) 1c The ratio was calculated. Destructive Energy G 1c = (fracture toughness value K 1c ) 2 / Tensile modulus E (Equation 2)
[0113] Specifically, a mixture consisting of only components (A), (C) and (D) (components (A) and (D) for adhesive composition (8)) was poured into a mold (length 90 mm, width 20 mm, thickness 3 mm), heated at 60°C for 60 minutes, heated to 100°C at 2°C / min, heated at 100°C for 60 minutes, heated to 150°C at 2.5°C / min, and heated at 150°C for 120 minutes in succession to cure the mixture in the mold and prepare a rectangular cured product test piece. The obtained cured product test piece had a length of 60 mm, a width B=3 mm and a thickness W=10 mm, and was mechanically processed to a depth of 5 mm in the thickness direction at the center in the length direction. Furthermore, a scratch was made with a razor at the mechanically processed tip of the cured product to a depth of 0.1 mm in the thickness direction. The total crack length a=5.1 mm. After that, a three-point bending test was performed using a tensile testing machine (AGS-X, Shimadzu Corporation) at a speed of 1 mm / min in the compression direction and a support distance of S = 40 mm. 1C In accordance with the provisions of the law, the fracture toughness value (K 1C (MPa m 1 / 2 ) was calculated. P in the following (Equation 3) Q is the load (N). K 1C ={(P Q ×S) / (B×W3 / 2 )}×f(a / W) (Equation 3) f(a / W)=(3(a / W) 1 / 2 [1.99-(a / W)(1-a / W){2.15-3.93(a / W)+2.7(a / W) 2}]) / [2{1+2(a / W)}{1-(a / W)} 3 / 2 ] (Formula 4)
[0114] The obtained fracture toughness value (K 1C ) and the tensile modulus (E) calculated by (Equation 1), the fracture energy per unit area (G 1C ) was calculated.
[0115] Similarly, for adhesive compositions (1)-(7) and (9)-(15), the fracture toughness values (K 1C (MPa m 1 / 2 )) and calculate the fracture energy G 1c The ratio of the fracture energy per unit area G of the cured product of the mixture consisting of only components (A), (B), (C) and (D) was calculated. The results are shown in Table 1. For the adhesive composition (1) of Example 1, the fracture energy per unit area G 1c is 1904 J / m 2 , the fracture energy per unit area G of the cured product of a mixture consisting only of components (A), (C) and (D) 1c is 373 J / m 2 and the ratio was 5.1.
[0116] <Evaluation of adhesive strength and cohesive failure rate> Each of the adhesive compositions (1)-(15) was applied to an aluminum plate (JIS H4000 A1050P, size 3 mm x 25 mm x 100 mm) that had been pretreated so that the adhesive area was a rectangle of 12.5 mm x 25 mm, and another aluminum plate was attached to the plate, which was then heated at 60°C for 60 minutes, heated at 2°C / min to 100°C, heated at 100°C for 60 minutes, heated at 2.5°C / min to 150°C, and heated at 150°C for 120 minutes in succession to be cured to prepare a tensile shear adhesion test specimen. The pretreatment here refers to a treatment method in which the plate was sandblasted and then immersed in an organic solvent and an alkaline bath at 70°C. The obtained tensile shear adhesion test specimens were subjected to a tensile shear adhesion test using a tensile testing machine (AGS-X, Shimadzu Corporation) with a gripping distance of 100 mm and a test speed of 2 mm / min. The measured values of the maximum breaking strength (N) and the area of the adhesive joint (mm 2 The tensile shear adhesive strength (MPa) to the aluminum plate was calculated from the measured values of the bond strength (MPa) and the fracture surface of the test piece after the tensile shear adhesive test was visually inspected, and the ratio of the area of the fracture surface where the adhesive remained on the metal substrate surface to the area of the adhesive joint was calculated. The results are shown in Table 1.
[0117] [Table 1]
Claims
1. A thermosetting resin as component (A); Thermoplastic resin particles as component (B); a curing agent as component (C) and / or a curing accelerator as component (D); An adhesive composition comprising: The component (B) contains a resin having at least one selected from the group consisting of a hydroxy group, a carboxy group, a carboxylic anhydride group, an amino group, an amide group, and a glycidyl group, The adhesive composition has a fracture energy per unit area G of a cured product of a mixture consisting of only the components (A), (C) and (D), which is calculated by the following formula (2): 1c The fracture energy G per unit area of the cured product of a mixture consisting of only components (A), (B), (C) and (D) 1c is 2.5 to 6.0 times, Destructive Energy G 1c = (fracture toughness value K 1c ) 2 / tensile modulus E (Equation 2) The adhesive composition, wherein the components (A), (B), (C) and (D) satisfy the following conditions (I) to (III): Condition (I): The value obtained by subtracting the heat generation initiation temperature of a mixture consisting of only the components (A), (C) and (D) from the melting point of the component (B) is -10°C to 60°C. Condition (II): The difference between the tensile modulus of a cured product of the mixture consisting only of the components (A), (C), and (D) and the tensile modulus of a cured product of the mixture consisting only of the components (A), (B), (C), and (D) is 0.3 GPa or more. Condition (III): The tensile strength of a laminate to be measured, which is a cured product of a mixture consisting of only the components (A), (C) and (D) and a film formed from the component (B), is 4 MPa or more, and the strain energy per unit volume is 100 kJ / m, as measured by the following method. 3 That's all. However, the blending ratios of the components (A), (B), (C) and (D) when measuring the above conditions (I) to (III) are as follows: The functional group equivalent (molar) ratio of component (C) to component (A) is 1:
1. Component (D) is 3 parts by mass per 100 parts by mass of component (A). Component (B) is 30 parts by mass per 100 parts by mass of the total of components (A), (C), and (D). In addition, when component (C) is not included in the adhesive composition, component (B) is 30 parts by mass per 100 parts by mass of the total of components (A) and (D). (Measurement of condition (III)) A film of 1.5 mm width, 1 mm thickness, and 3 mm length formed from component (B) is placed in the center of a mold with a space of 90 mm width, 1 mm thickness, and 3 mm length, and a mixture consisting of only components (A), (C), and (D) is poured into both sides of the film, and the mixture is cured in the mold by successively heating at 60°C for 60 minutes, at 100°C for 60 minutes, and at 150°C for 120 minutes to obtain a measurement laminate in which the cured mixture consisting of only components (A), (C), and (D) is laminated on both sides of the film. A tensile test is performed on the measurement laminate under conditions of a gripper distance of 25 mm and a test speed of 0.5 mm / min to determine the tensile strength. The strain energy per unit volume is determined from the obtained stress-strain curve.
2. 2. The adhesive composition according to claim 1, wherein component (A) is an epoxy resin.
3. The adhesive composition according to claim 1 or 2, wherein the content of component (A) is 7 to 95 mass %.
4. The adhesive composition according to any one of claims 1 to 3, wherein the volume average particle size of component (B) is 2 to 30 µm.
5. The adhesive composition according to any one of claims 1 to 4, which is used for bonding any one of structural materials, composite materials, electric and electronic materials, substrate materials, laminate materials, coating materials, and paints.
6. A cured product of the adhesive composition according to any one of claims 1 to 5.
7. A step of applying or casting the adhesive composition according to any one of claims 1 to 5 onto a surface of an object to be adhered; curing the adhesive composition; A method for producing an adhesive layer comprising the steps of:
8. A process for applying the adhesive composition according to any one of claims 1 to 5 to a surface of an object to be adhered and disposing the adhesive composition between at least two objects to be adhered; curing the adhesive composition; A method for producing a laminate in which at least two objects to be bonded are bonded, comprising:
9. A step of casting the adhesive composition according to any one of claims 1 to 5 between at least two objects to be adhered; curing the adhesive composition; A method for producing a laminate in which at least two objects to be bonded are bonded, comprising:
Citation Information
Patent Citations
Adhesive composition
JP1993295340A
Epoxy resin adhesive
JP6526571B2
Adhesive composition
WO2019189238A1