Adhesive composition
The adhesive composition with specific thermoplastic resin properties addresses unstable adhesive performance by enhancing cohesive failure resistance, ensuring strong and reliable bonding across diverse materials.
Patent Information
- Application Number
- JP2021141614
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-08-31
- Publication Date
- 2024-10-17
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing adhesive compositions face issues with unstable adhesive performance due to variations in cohesive and interfacial failure, leading to inconsistent adhesion strength and reliability, particularly when subjected to external forces.
An adhesive composition comprising a thermosetting resin, thermoplastic resin particles, a curing agent, and/or a curing accelerator, where the thermoplastic resin particles have a tensile modulus of 1 GPa or less and a strain energy per unit volume of 20000 kJ/m³, ensuring high adhesive strength and improved cohesive failure resistance.
The composition achieves both high adhesive strength and improved cohesive failure resistance, suitable for bonding various materials including metals and resins, with enhanced stability under external forces.
Smart Images

Figure 2024147844000002 
Figure 2024147844000001
Abstract
Description
[Technical Field]
[0001] The present invention relates to an adhesive composition. [Background technology]
[0002] Conventionally, various adhesive compositions have been used in various industrial fields such as automobiles and electronic materials. Adhesive compositions used in industrial fields are required to have stable adhesive performance in addition to high adhesive strength to adherends such as metal materials. Specifically, stable adhesive performance refers to a performance in which there is little variation in the magnitude of the external force that causes peeling when adhering to an adherend, and the adherend remains adhered until the external force applied to the adhesive layer exceeds a certain magnitude, and when this magnitude is exceeded, the adhered adherend peels off.
[0003] Known modes of adhesion failure when adherends peel off include interfacial failure, cohesive failure, and a mixture of these, and it is known that when the mode of adhesion failure due to an external force is cohesive failure, adhesive performance is stable (see, for example, Patent Document 1). On the other hand, even if an adhesive composition has high adhesive strength to adherends, if the mode of adhesion failure is interfacial failure, there is a problem in that the external force that causes peeling at the interface between the adhesive layer and the adherend varies greatly, resulting in unstable adhesive performance.
[0004] For example, Patent Document 2 discloses an epoxy resin adhesive containing an epoxy resin, a curing agent, and a polyolefin resin coated with silica. This adhesive composition has low shrinkage and high adhesiveness, but does not provide sufficient performance in terms of fracture morphology.
[0005] Furthermore, for example, Patent Document 3 discloses an adhesive composition containing an adhesive resin, core-shell polymer particles, and polymer particles. These compositions improve adhesive performance by using two types of particles: special core-shell polymer particles measuring several tens to several hundreds of nanometers, and polymer particles larger than the core-shell polymer particles, and therefore there is room for improvement from an industrial perspective. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 5-295340 [Patent Document 2] Patent No. 6526571 [Patent Document 3] International Publication No. 2019 / 189238 Summary of the Invention [Problem to be solved by the invention]
[0007] A primary object of the present invention is to provide an adhesive composition that achieves both high adhesive strength and an improved cohesive failure rate. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems. As a result, they have discovered that an adhesive composition containing a thermosetting resin, thermoplastic resin particles, and a curing agent and / or a curing accelerator has a tensile modulus of elasticity of a dumbbell test piece formed from the thermoplastic resin particles of 1 GPa or less and a strain energy per unit volume of 20,000 kJ / m 3 It has been found that, when the above conditions are met, both high adhesive strength and an improved rate of cohesive failure can be achieved. The present invention has been completed based on this finding and through further intensive research.
[0009] That is, the present invention provides the following configuration. Item 1. A thermosetting resin as component (A), Thermoplastic resin particles as component (B); a curing agent as component (C) and / or a curing accelerator as component (D); An adhesive composition comprising: The component (B) is a material having a tensile modulus of 1 GPa or less when a No. 7 dumbbell test piece molded to a width of 2 mm and a thickness of 1 mm in accordance with the provisions of JIS K7161, and a strain energy per unit volume calculated from the stress-strain curve of the test piece of 20,000 kJ / m 3 The adhesive composition is a thermoplastic resin particle as described above. Item 2. The adhesive composition according to Item 1, wherein component (A) is an epoxy resin. Item 3. The adhesive composition according to Item 1 or 2, wherein the content of component (A) is 7 to 95 mass% based on the total amount of components (A), (B), (C), and (D). Item 4. The adhesive composition according to any one of Items 1 to 3, wherein the volume average particle size of component (B) is 2 to 30 μm. Item 5. The adhesive composition according to any one of Items 1 to 4, which is used for bonding any of structural materials, composite materials, electrical and electronic materials, substrate materials, laminate materials, coating materials, and paints. Item 6. A cured product of the adhesive composition according to any one of items 1 to 5. Item 7. A step of applying or casting the adhesive composition according to any one of items 1 to 5 onto a surface of an object to be adhered; curing the adhesive composition; A method for producing an adhesive layer, comprising: Item 8. A step of applying the adhesive composition according to any one of items 1 to 5 to a surface of an object to be adhered and disposing the adhesive composition between at least two objects to be adhered; curing the adhesive composition; A method for producing a laminate in which at least two objects to be bonded are bonded, comprising: Item 9. A step of casting the adhesive composition according to any one of items 1 to 5 between at least two objects to be adhered; curing the adhesive composition; A method for producing a laminate in which at least two objects to be bonded are bonded, comprising: [Effects of the Invention]
[0010] According to the present invention, an adhesive composition can be provided that achieves both high adhesive strength and an improved cohesive failure rate. The adhesive composition of the present invention can be suitably used for bonding applications in which adhesive compositions have been used in various industrial fields, such as structural materials, composite materials, electrical and electronic materials, substrate materials, laminate materials, coating materials, and paints. In particular, the adhesive composition of the present invention can be suitably used as an adhesive composition for bonding objects made of metal materials such as iron, stainless steel, and aluminum alloys, or resin materials such as engineering plastics and carbon fiber reinforced plastics, either alone or in combination. [Brief explanation of the drawings]
[0011] [Figure 1] 1 is a graph showing integral values of a stress-strain curve. DETAILED DESCRIPTION OF THE INVENTION
[0012] The adhesive composition of the present invention is an adhesive composition comprising a thermosetting resin as component (A), thermoplastic resin particles as component (B), and a curing agent as component (C) and / or a curing accelerator as component (D), wherein component (B) is an adhesive composition having a tensile modulus of 1 GPa or less when a No. 7 dumbbell test piece molded to a width of 2 mm and a thickness of 1 mm in accordance with the provisions of JIS K7161 is used, and the strain energy per unit volume calculated from the stress-strain curve of the test piece is 20,000 kJ / m 3 The adhesive composition of the present invention is characterized by the above-mentioned. By satisfying all of the above-mentioned components, it is possible to achieve both high adhesive strength and an improved cohesive failure rate.
[0013] The adhesive composition of the present invention will be described in detail below. As used herein, the term "comprising" includes "consisting essentially of" and "consisting of".
[0014] In addition, in this specification, numerical values connected with "~" mean a numerical range that includes the numerical values before and after "~" as the lower limit and upper limit. When multiple lower limit values and multiple upper limit values are listed separately, any lower limit value and upper limit value can be selected and connected with "~".
[0015] The adhesive composition of the present invention comprises a thermosetting resin as component (A) and thermoplastic resin particles as component (B), and further comprises at least one of a curing agent as component (C) and a curing accelerator as component (D). That is, the adhesive composition of the present invention may be a composition containing components (A), (B), (C), and (D), a composition containing components (A), (B), and (C) but not containing component (D), or a composition containing components (A), (B), and (D) but not containing component (C).
[0016] <Component (A): Thermosetting resin> Examples of component (A) include thermosetting resins such as epoxy resins, acrylic resins, and silicone resins, with epoxy resins being preferred from the viewpoints of adhesiveness, insulating properties, and mechanical properties. Known resins used in epoxy resin adhesives, acrylic resin adhesives, silicone resin adhesives, and the like can be used as these thermosetting resins. The resin component (A) contained in the adhesive composition of the present invention may be one type, or two or more types.
[0017] The epoxy resin may be any epoxy resin that has an epoxy group and is curable, and examples thereof include monoepoxy compounds and polyepoxy compounds.
[0018] Specific examples of monoepoxy compounds include butyl glycidyl ether, hexyl glycidyl ether, phenyl glycidyl ether, allyl glycidyl ether, para-butylphenyl glycidyl ether, para-xylyl glycidyl ether, glycidyl acetate, glycidyl butyrate, glycidyl hexoate, and glycidyl benzoate.
[0019] Examples of polyhydric epoxy compounds include bisphenol-type epoxy resins, epoxy resins obtained by glycidylating polyhydric phenol compounds, novolac-type epoxy resins, aliphatic ether-type epoxy resins, ether ester-type epoxy resins, ester-type epoxy resins, amine-type epoxy resins, and alicyclic epoxy resins.
[0020] Among the polyfunctional epoxy compounds, specific examples of bisphenol-type epoxy resins include epoxy resins obtained by glycidylating bisphenols such as bisphenol A, bisphenol F, bisphenol AD, bisphenol S, tetramethylbisphenol A, tetramethylbisphenol F, tetramethylbisphenol AD, tetramethylbisphenol S, tetrabromobisphenol A, tetrachlorobisphenol A, and tetrafluorobisphenol A.
[0021] Specific examples of epoxy resins obtained by glycidylating polyhydric phenol compounds include epoxy resins obtained by glycidylating dihydric phenol compounds such as biphenol, dihydroxynaphthalene, and 9,9-bis(4-hydroxyphenyl)fluorene, epoxy resins obtained by glycidylating trisphenol compounds such as 1,1,1-tris(4-hydroxyphenyl)methane, and epoxy resins obtained by glycidylating tetrakisphenol compounds such as 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane.
[0022] Specific examples of novolac-type epoxy resins include epoxy resins obtained by glycidylating novolac compounds such as phenol novolac, cresol novolac, bisphenol A novolac, brominated phenol novolac, and brominated bisphenol A novolac.
[0023] Specific examples of aliphatic ether type epoxy resins include epoxy resins obtained by glycidylating polyhydric alcohols such as glycerin and polyethylene glycol.
[0024] Specific examples of ether ester type epoxy resins include epoxy resins obtained by glycidylating hydroxycarboxylic acids such as parahydroxybenzoic acid.
[0025] Specific examples of ester-type epoxy resins include epoxy resins obtained by glycidylating polycarboxylic acids such as phthalic acid and terephthalic acid.
[0026] Specific examples of amine-type epoxy resins include epoxy resins obtained by glycidylating amine compounds such as 4,4'-diaminodiphenylmethane and m-aminophenol.
[0027] Specific examples of alicyclic epoxy resins include 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate, 1,2-epoxy-4-vinylcyclohexane, bis(3,4-epoxycyclohexylmethyl)adipate, 1-epoxyethyl 3,4-epoxycyclohexane, limonene diepoxide, and 3,4-epoxycyclohexylmethanol.
[0028] Among these epoxy resins, polyvalent epoxy compounds are preferred, bisphenol type epoxy resins and amine type epoxy resins are more preferred, and among these, bisphenol A type epoxy resins and bisphenol F type epoxy resins are even more preferably used.
[0029] In the adhesive composition of the present invention, the amount of component (A) blended is preferably 7 to 95 mass%, more preferably 10 to 90 mass%, and even more preferably 30 to 80 mass%, relative to 100 mass% of the total amount of components (A), (B), (C), and (D).
[0030] <Component (B): Thermoplastic resin particles> The adhesive composition of the present invention contains thermoplastic resin particles as component (B). Component (B) has a tensile modulus of 1 GPa or less when a No. 7 dumbbell test piece molded to a width of 2 mm and a thickness of 1 mm conforming to the provisions of JIS K7161 is used. Furthermore, component (B) has a strain energy per unit volume of 20,000 kJ / m2 calculated from the stress-strain curve of the test piece. 3 That's all.
[0031] The tensile modulus of component (B) is calculated as follows: The thermoplastic resin particles of component (B) are pressed and molded into a film using a hot press under conditions of a temperature of 130 to 200°C, a pressure of 0.2 MPa, and a time of 30 seconds, and a No. 7 dumbbell test piece with a width of 2 mm and a thickness of 1 mm is prepared. The tensile modulus of the prepared test piece is measured by a tensile test in accordance with the provisions of JIS K7161. Specifically, the tensile test is performed under conditions of a gripping distance of 10 mm and a test speed of 0.5 mm / min, whereby the tensile stress (σ) and tensile strain (ε) are measured, and the tensile modulus is calculated from the gradient of the line at small strain (the following formula). E=(σ2-σ1) / (ε2-ε1) σ2: Tensile stress measured at ε2 = 0.0025 σ1: Tensile stress measured at ε1=0.0005
[0032] When the tensile modulus calculated by the above measurement is 1 GPa or less, component (B) can relieve the stress generated at the interface between the adhesive layer and the substrate when the adhesive composition is prepared, thereby increasing the adhesive strength. From the viewpoint of obtaining a higher adhesive strength, it is preferably 0.7 GPa or less, and more preferably 0.2 GPa or less. The lower limit of the tensile modulus is, for example, 0.01 GPa.
[0033] The strain energy per unit volume of the component (B) is calculated by the following method. A stress-strain curve is obtained from the tensile test in which the tensile modulus is calculated, and the strain energy per unit volume is determined. The strain energy per unit volume is the area enclosed from the start point of the tensile test to the break point, and the integral value of the tensile stress from the start point of the tensile test to the break point is calculated using the strain as a variable. As shown in Figure 1, the integral value is calculated by calculating the area of the smallest rectangle obtained at the minimum tensile stress within the strain width for each 0.0001 [mm / mm] strain width from the start of tension, and then summing the areas of all the rectangles up to the break point.
[0034] The strain energy per unit volume calculated from the stress-strain curve calculated in the above measurement is 20,000 kJ / m 3 By satisfying this condition, the effect of adding component (B) is fully exerted on the adhesive layer when the adhesive composition used is broken, and fracture toughness is improved. From the viewpoint of further improving fracture toughness, the strain energy per unit volume of the test piece is set to 30,000 kJ / m 3 It is preferable that the concentration is 100,000 kJ / m or more. 3 The upper limit of the strain energy is, for example, 2,000,000 kJ / m or more. 3 is.
[0035] The type of thermoplastic resin for component (B) is particles synthesized from a resin having thermoplastic properties, and the tensile modulus of elasticity of the dumbbell test piece and the strain energy per unit volume calculated from the stress-strain curve described above may be within a certain range. Representative examples of thermoplastic resins include polyolefin resins, nylon resins, polyester resins, polyvinyl alcohol resins, and thermoplastic polyurethane resins.
[0036] When the elastic modulus of component (B) is lower than that of the cured product formed by (A) the thermosetting resin and (C) the curing agent and / or (D) the curing accelerator, the component (B) has the effect of alleviating stress generated during curing, particularly distortion at the interface between the adhesive layer and the adherend, thereby achieving excellent adhesive strength.
[0037] Examples of the polyolefin resin include polyolefin resins, copolymer resins of olefins and other monomers, and polystyrene resins.
[0038] Examples of the polyolefin resin include olefin homopolymers, copolymers, and acid-modified polymers thereof. Examples of olefin homopolymers include polyethylene and polypropylene. Examples of olefin copolymers include ethylene-propylene copolymer, ethylene-1-butene copolymer, ethylene-1-octene copolymer, and ethylene-1-hexene copolymer. Examples of acid-modified olefin homopolymers and copolymers include maleic anhydride-modified polyethylene and maleic anhydride-modified polypropylene.
[0039] Examples of olefins constituting the copolymer resin of an olefin and another monomer include ethylene and propylene. The other monomers are not particularly limited as long as they are copolymerizable with the olefin, and examples include vinyl esters, α,β-unsaturated carboxylic acids, α,β-unsaturated carboxylic anhydrides, metal salts of α,β-unsaturated carboxylic acids, and α,β-unsaturated carboxylic esters. Examples of vinyl esters include vinyl acetate. Examples of α,β-unsaturated carboxylic acids include (meth)acrylic acid. Examples of α,β-unsaturated carboxylic anhydrides include maleic anhydride, and examples of metal salts of α,β-unsaturated carboxylic acids include sodium salts and magnesium salts of (meth)acrylic acid. Examples of α,β-unsaturated carboxylic esters include methyl (meth)acrylate, ethyl (meth)acrylate, hydroxyethyl (meth)acrylate, and glycidyl (meth)acrylate. These olefins and other monomers may be used alone or in combination of two or more.
[0040] Specific examples of the copolymer resin of the olefin with another monomer include ethylene / vinyl acetate copolymer, partially saponified ethylene / vinyl acetate copolymer, ethylene / (meth)acrylic acid copolymer, ethylene / maleic anhydride copolymer, propylene / maleic anhydride copolymer; ethylene / methyl methacrylate copolymer, partially saponified ethylene / methyl methacrylate copolymer, ethylene / ethyl methacrylate copolymer, partially saponified ethylene / ethyl methacrylate copolymer, ethylene / methyl acrylate copolymer, partially saponified ethylene / methyl acrylate copolymer, ethylene / ethyl acrylate copolymer, ethylene / ethyl acrylate copolymer. ethylene / (meth)acrylic acid ester copolymers such as ethylene / glycidyl (meth)acrylate copolymer and partially saponified products thereof; ethylene / (meth)acrylic acid ester / (meth)acrylic acid ester copolymers such as ethylene / glycidyl (meth)acrylate / methyl (meth)acrylate copolymer; ethylene / (meth)acrylic acid ester / vinyl acetate copolymers such as ethylene / glycidyl (meth)acrylate / vinyl acetate copolymer and ethylene / (meth)acrylic acid ester / maleic anhydride copolymer, as well as resins of metal salts thereof.
[0041] Examples of nylon resins include -[NH(CH2)5CO]-, -[NH(CH2)4NHCO(CH2)4CO]-, -[NH(CH2)6NHCO(CH2)4CO]-, -[NH(CH2)6NHCO(CH2)8CO]-, -[NH(CH2) 10 CO]- and -[NH(CH2) 11 [CO]-. Specific examples of such nylon resins include nylon 6, nylon 46, nylon 66, nylon 610, nylon 11, nylon 12, and polyamide elastomers, which are copolymers of these with polyester or polyalkylene ether glycol.
[0042] Examples of polyester resins include polyester resins obtained by polycondensation of acid components including terephthalic acid and isophthalic acid with diol components including ethylene glycol, butylene glycol, diethylene glycol, polyethylene glycol, 1,4-butanediol, and 1,6-hexanediol. Specific examples include terephthalic acid / ethylene glycol copolymer polyester resin, terephthalic acid / butylene glycol copolymer polyester resin, terephthalic acid / isophthalic acid / 1,4-butanediol copolymer polyester resin, terephthalic acid / isophthalic acid / 1,6-hexanediol copolymer polyester resin, terephthalic acid / isophthalic acid / polyethylene glycol copolymer polyester resin, terephthalic acid / isophthalic acid / ethylene glycol / 1,4-butanediol copolymer polyester resin, terephthalic acid / isophthalic acid / adipic acid / 1,4-butanediol copolymer polyester resin, and terephthalic acid / isophthalic acid / 1,4-butanediol / diethylene glycol copolymer polyester resin. Furthermore, examples of the polyester resin include polyester thermoplastic elastomers, which are copolymers of the copolymer polyester resin and polyalkylene ether glycol.
[0043] In the present invention, the polyolefin resin, nylon resin, polyester resin, polyvinyl alcohol resin, and thermoplastic polyurethane resin may be used either alone or in combination of two or more.
[0044] Among the above resins, preferred ones include polyolefin resins, nylon copolymers, nylon elastomers, and thermoplastic polyurethane resins, which are more flexible than curable resins and have a high plastic deformation capacity, and more preferred ones include polyethylene, ethylene / vinyl acetate copolymers, ethylene / (meth)acrylic acid copolymers, ethylene / (meth)acrylic acid ester copolymers, ethylene / glycidyl methacrylate copolymers, and 12 nylon elastomers.
[0045] The volume average particle size of component (B) is, for example, 1 μm to 100 μm, and preferably 2 μm to 30 μm. If it is smaller than 1 μm, it is difficult to handle, and the viscosity increases during the process of mixing with component (A), which may impair workability. If it is larger than 100 μm, it is prone to separation when mixed with a curable resin, resulting in poor dispersion stability. By being 2 μm to 30 μm, the effect of addition is more likely to be fully exerted without impairing workability.
[0046] The volume average particle size of component (B) is a volume average particle size determined by the electrical detection zone method (pore electrical resistance method).
[0047] A specific example of an apparatus for measuring the volume average particle diameter by the pore electrical resistance method is an electrical detection particle size distribution analyzer (trade name "Coulter Multisizer" manufactured by Beckman Coulter, Inc.). Aperture diameters used for measurement vary, and each aperture diameter has a measurement range (volume average particle diameter) suitable for measurement. The aperture diameter can be selected to cover the particle diameters present in the particles to be measured, and in the examples described below, an aperture diameter of 100 μm was used based on this principle. When measuring particles with particle diameters smaller than the measurement range suitable for an aperture diameter of 100 μm, an aperture diameter smaller than 100 μm can be selected, and when measuring particles with particle diameters larger than the measurement range suitable for an aperture diameter of 100 μm, an aperture diameter larger than 100 μm can be selected.
[0048] The shape of component (B) according to the present invention is not particularly limited as long as workability is not impaired, and examples include spherical, irregular, scaly, etc. From the viewpoints of facilitating dispersion in the adhesive composition and suppressing an increase in viscosity, a spherical shape is preferred.
[0049] The thermoplastic resin particles (component (B)) used in the present invention may contain inorganic pigments such as alumina and silica, metal powders such as iron, copper, nickel and cobalt, and organic substances such as ultraviolet absorbers and heat stabilizers within or on their surfaces.
[0050] In the adhesive composition of the present invention, the amount of component (B) blended is preferably 5 to 50 mass %, and more preferably 10 to 40 mass %, relative to 100 mass % of the total amount of components (A), (B), (C), and (D).
[0051] <Component (C): Hardener> The curing agent as component (C) may be any that reacts with component (A), a thermosetting resin, to produce a cured product. Component (C) may be used alone or in combination with two or more types. When two or more types of component (C) are used in combination, the mixture of the curing agents is considered to be a single component (C).
[0052] Examples of component (C) include amine-based curing agents, amide-based curing agents, acid anhydride-based curing agents, phenol-based curing agents, mercaptan-based curing agents, isocyanate-based curing agents, active ester-based curing agents, and cyanate ester-based curing agents.
[0053] Examples of amine-based curing agents include chain aliphatic amines such as ethylenediamine, diethylenetriamine, triethylenetetramine, and tetraethylenepentamine; alicyclic amines such as isophoronediamine, bis(4-aminocyclohexyl)methane, and bis(aminomethyl)cyclohexane; and aromatic amines such as metaphenylenediamine, diaminodiphenylmethane, diethyltoluenediamine, and diethyldiaminodiphenylmethane.
[0054] Examples of amide-based curing agents include dicyandiamide and its derivatives, polyamide resins (such as polyaminoamides), and the like.
[0055] Examples of acid anhydride curing agents include aliphatic acid anhydrides such as maleic anhydride and dodecenyl succinic anhydride; aromatic acid anhydrides such as phthalic anhydride, trimellitic anhydride and pyromellitic anhydride; and alicyclic acid anhydrides such as methylnadic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride and 4-methylhexahydrophthalic anhydride.
[0056] Examples of phenol-based curing agents include phenol novolac resins, cresol novolac resins, biphenyl novolac resins, triphenylmethane phenol resins, naphthol novolac resins, phenol biphenylene resins, phenol aralkyl resins, biphenyl aralkyl phenol resins, modified polyphenylene ether resins, and compounds having a benzoxazine ring.
[0057] Examples of mercaptan curing agents include trimethylolpropane tris(3-mercaptopropionate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, pentaerythritol tetrakis(3-mercaptopropionate), tetraethylene glycol bis(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), 1,4-bis(3-mercaptobutyryloxy)butane, trimethylolpropane tris(3-mercaptobutyrate), trimethylolethane tris(3-mercaptobutyrate), and polysulfide polymers.
[0058] Examples of the isocyanate curing agent include hexamethylene diisocyanate, 1,4-tetramethylene diisocyanate, 2-methylpentane-1,5-diisocyanate, lysine diisocyanate, isophorone diisocyanate, and norbornane diisocyanate.
[0059] The active ester curing agent is a compound having one or more ester groups per molecule that react with the (A) thermosetting resin, and examples thereof include phenyl ester, naphthyl ester, thiophenyl ester, N-hydroxyamine ester, and heterocyclic hydroxy compound ester.
[0060] Examples of cyanate ester curing agents include bisphenol type cyanate resins such as novolac type cyanate resin, bisphenol A type cyanate resin, bisphenol E type cyanate resin, and tetramethylbisphenol F type cyanate resin.
[0061] In the adhesive composition of the present invention, it is preferable to use, as component (C), at least one selected from the group consisting of amine-based curing agents, acid anhydride-based curing agents, amide-based curing agents, and phenol-based curing agents, with amine-based curing agents and acid anhydride-based curing agents being more preferred.
[0062] In the adhesive composition of the present invention, the amount of component (C) is not particularly limited. It is preferable that the amount of reactive functional groups in component (C) is 0.1 to 5 equivalents per equivalent of reactive functional groups (e.g., epoxy groups) in component (A), which is a thermosetting resin. The equivalent weight of the reactive functional groups in component (C) is more preferably 0.3 to 3 equivalents, and even more preferably 0.5 to 2 equivalents.
[0063] <Component (D): Curing accelerator> The curing accelerator as component (D) is a component that accelerates the curing of component (A), which is a thermosetting resin. Furthermore, by using component (D) in combination with component (C), it is possible to increase the curing reaction rate and improve the strength of the resulting cured product. Note that component (D) can accelerate the curing of component (A) even without using it in combination with component (C). Component (D) may be used alone or in a mixture of two or more types. Note that when two or more types of component (D) are used in combination, the mixture of the curing accelerators is considered to be a single component (D).
[0064] Examples of component (D) include imidazole compounds such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 1,2-dimethylimidazole, and 1-benzyl-2-methylimidazole; secondary amines such as piperidine; tertiary amines such as DBU (1,8-diazabicyclo(5,4,0)-undecene-7), DBN (1,5-diazabicyclo(4,3,0)-nonene-5), 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, triethylenediamine, 2-(dimethylaminomethyl)phenol, and 4-dimethylaminopyridine; phosphorus compounds such as triphenylphosphine and tetraphenylphosphonium tetraphenylborate, Lewis acid compounds, and cationic polymerization initiators.
[0065] In the adhesive composition of the present invention, it is preferable to use as component (D) at least one selected from the group consisting of imidazole compounds, tertiary amines, phosphorus-based compounds, and cationic polymerization initiators.
[0066] In the adhesive composition of the present invention, the amount of component (D) to be blended is not particularly limited. For example, it is preferably blended in an amount of 0.01 to 10 parts by mass per 100 parts by mass of component (A). It is more preferably 0.1 to 5 parts by mass, and even more preferably 0.5 to 5 parts by mass.
[0067] In the adhesive composition of the present invention, the total content of component (A), component (B), component (C), and component (D) is preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, still more preferably 70% by mass or more, and may be 100% by mass.
[0068] <Additives that may be included in the adhesive composition> The adhesive composition of the present invention may contain other additives as needed, provided that the additives do not impair the object and effect of the present invention.
[0069] Examples of additives include organic fillers not included in component (B), thermoplastic resins, rubbers, elastomers, composite particles, inorganic fillers, conductive particles, carbon black, antioxidants, inorganic fluorescent materials, lubricants, ultraviolet absorbers, heat and light stabilizers, antistatic agents, polymerization inhibitors, antifoaming agents, solvents, antioxidants, radical inhibitors, adhesion improvers, flame retardants, surfactants, storage stability improvers, ozone antioxidants, thickeners, plasticizers, radiation shielding agents, nucleating agents, coupling agents, conductivity imparting agents, phosphorus-based peroxide decomposers, pigments, metal deactivators, and physical property adjusters.
[0070] The additives may be contained in an amount of, for example, 0 to 90% by mass relative to the total adhesive composition. If the additives are contained in an amount exceeding 90% by mass, the stability of the entire composition is impaired, and the objects and effects of the present invention cannot be fully achieved. The content of the additives in the adhesive composition of the present invention is preferably 70% by mass or less, more preferably 50% by mass or less, and even more preferably 30% by mass or less, and may not be present at all.
[0071] <Method of manufacturing adhesive composition> The adhesive composition of the present invention can be produced by mixing component (A), component (B), component (C) and / or component (D), and, if necessary, other additives.
[0072] The mixing method is not particularly limited as long as it can mix the components uniformly, and examples include mixing and stirring with a paddle blade, mixing and stirring with a homomixer, and mixing and stirring with a planetary mixer.
[0073] The adhesive composition of the present invention has a low viscosity and can be prepared without adding a solvent; however, if necessary, a solvent (e.g., toluene, xylene, methyl ethyl ketone, acetone, cyclohexanone, methylcyclohexane, cyclohexane, etc.) may be added within a range that does not affect the effects of the present invention.
[0074] A cured product can be obtained by curing the adhesive composition of the present invention. The curing method is not particularly limited and may be selected appropriately depending on the type of curing reaction of the curable resin. For example, the curing method can be performed by heating the composition. When curing by heating, the curing temperature is usually room temperature (25°C) to 250°C, and the curing time varies depending on the composition liquid and can usually be set over a wide range from 30 seconds to 1 week. In consideration of the thermal properties of component (B) of the present invention and its influence on interactions with other components, and from the perspective of preventing deterioration due to thermal history, it is preferable to set the curing temperature to 40°C to 200°C and the curing time to 1 minute to 12 hours.
[0075] The adhesive composition of the present invention can be suitably used for bonding structural materials, composite materials, electrical and electronic materials, substrate materials, laminate materials, coating materials, paints, etc. Examples of adhesives for structural materials include adhesives for bonding metal materials, polymeric materials, inorganic materials, etc. used in automobiles and vehicles (bullet trains, trains), aircraft, the aerospace industry, etc. Examples of adhesives for electrical and electronic materials, substrate materials, and laminate materials include adhesives for interlayer bonding in multilayer substrates, for semiconductors, for mounting, etc., as well as sealants and underfills.
[0076] <Cured product of adhesive composition> The cured product of the adhesive composition of the present invention is obtained by curing the above-described adhesive composition of the present invention. The method for curing the adhesive composition of the present invention is not particularly limited, but as described above, a method of heating the adhesive composition of the present invention is one example.
[0077] <Method of manufacturing adhesive layer> The adhesive layer of the present invention can be produced by a production method including the steps of applying or casting the adhesive composition of the present invention onto the surface of an object to be adhered and curing the adhesive composition. The method for curing the adhesive composition of the present invention is as described above.
[0078] <Method of manufacturing laminate> The method for producing a laminate of the present invention includes the steps of applying an adhesive composition to the surface of an object to be adhered, disposing the adhesive composition between at least two objects to be adhered, and curing the adhesive composition. The method for producing a laminate of the present invention also includes the steps of casting the adhesive composition between at least two objects to be adhered, and curing the adhesive composition. The method for curing the adhesive composition of the present invention is as described above. Examples of objects to be adhered include those described above. [Example]
[0079] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0080] <Component (A): Thermosetting resin> As the component (A), the following thermosetting resins (A-1) and (A-2) were prepared. [Thermosetting resin A-1] Bisphenol F type epoxy resin (jER806: manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight 167) was used as component (A-1). [Thermosetting resin A-2] Bisphenol A type epoxy resin (jER828: manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight 186) was used as component (A-2).
[0081] <Component (B): Thermoplastic resin particles> As the component (B), the following thermoplastic resin particles (B-1) to (B-7) were prepared.
[0082] [Thermoplastic resin particles B-1] Low-density polyethylene (volume average particle diameter 10 μm, melting point 106°C, Flowbeads CL2080 manufactured by Sumitomo Seika Chemicals Co., Ltd.) was used as thermoplastic resin particles (B-1). The particles were formed into a film using a heat press (manual hydraulic vacuum heating press manufactured by Imoto Manufacturing Co., Ltd.) at a temperature of 130°C, a pressure of 0.2 MPa, and a time of 30 seconds. Dumbbell No. 7 test specimens were then prepared using a punching machine (SD-type lever-type sample cutter SDL-100 manufactured by Dumbbell Co., Ltd.). The prepared test specimens were subjected to a tensile test using a tensile tester (AGS-X manufactured by Shimadzu Corporation) at a gripping distance of 10 mm and a test speed of 0.5 mm / min, and a stress-strain curve was obtained. The tensile modulus, determined according to the method specified in JIS K7161, was 0.2 GPa. The strain energy per unit volume determined from the stress-strain curve was 76,204 kJ / m. 3 It was.
[0083] [Thermoplastic resin particles B-2] High density polyethylene (volume average particle diameter 10 μm, melting point 130°C, Flow Beads HE3040 manufactured by Sumitomo Seika Chemicals Co., Ltd.) was used as thermoplastic resin particles (B-2). The tensile modulus and strain energy per unit volume were measured in the same manner as for thermoplastic resin particles (B-1), except that the temperature of the heat press was changed to 160°C. The measurement results showed a tensile modulus of 1 GPa and strain energy per unit volume of 30,702 kJ / m 3 It was.
[0084] [Thermoplastic resin particles B-3] A 1-liter pressure-resistant autoclave equipped with a 50 mm diameter turbine-type stirring blade was charged with 160 g of ethylene / methyl methacrylate copolymer resin (MMA content 10% by mass), 224 g of deionized water, and 16 g of ethylene oxide / propylene oxide copolymer (weight average molecular weight 15,500, ethylene oxide content 80% by mass) as an emulsifier, and then sealed. The autoclave was then heated to 150°C while stirring at 500 rpm. After stirring for an additional 30 minutes while maintaining the internal temperature at 150°C, the contents were cooled to 25°C to obtain an aqueous dispersion of ethylene / methyl methacrylate copolymer. The aqueous dispersion was filtered through filter paper, washed with water, and dried in a vacuum dryer at 60°C for 24 hours to obtain ethylene / methyl methacrylate copolymer particles as thermoplastic resin particles B-3. The volume-average particle diameter of the resulting ethylene / methyl methacrylate copolymer particles was 13 μm and the melting point was 100°C. The tensile modulus and strain energy per unit volume were measured using the same method as for the thermoplastic resin particles (B-1). The results were a modulus of elasticity of 0.1 GPa and a strain energy per unit volume of 591,702 kJ / m 3 It was.
[0085] [Thermoplastic resin particles B-4] Ethylene / acrylic acid copolymer (AA content 7% by mass, volume average particle size 10 μm, melting point 97° C., Flowbeads EA209 manufactured by Sumitomo Seika Chemicals Co., Ltd.) was used as thermoplastic resin particles (B-4). The tensile modulus and strain energy per unit volume were measured using the same method as for the thermoplastic resin particles (B-1). The results were a modulus of elasticity of 0.1 GPa and a strain energy per unit volume of 572,789 kJ / m 3 It was.
[0086] [Thermoplastic resin particles B-5] A 1-liter pressure-resistant autoclave equipped with a 50 mm diameter turbine-type stirring blade was charged with 160 g of ethylene / glycidyl methacrylate copolymer resin (GMA content: 19% by mass), 224 g of deionized water, and 16 g of ethylene oxide / propylene oxide copolymer (weight average molecular weight: 15,500, ethylene oxide content: 80% by mass) as an emulsifier, and then sealed. The autoclave was then heated to 150°C while stirring at 500 rpm. After stirring for an additional 30 minutes while maintaining the internal temperature at 150°C, the contents were cooled to 25°C to obtain an aqueous dispersion of ethylene / glycidyl methacrylate copolymer. The aqueous dispersion was then filtered through filter paper, washed with water, and dried in a vacuum dryer at 40°C for 24 hours to obtain ethylene / glycidyl methacrylate copolymer particles as thermoplastic resin particles B-5. The volume average particle diameter of the resulting ethylene / glycidyl methacrylate copolymer particles was 13 μm and the melting point was 88°C. The tensile modulus and strain energy per unit volume were measured using the same method as for the thermoplastic resin particles (B-1). The results were a modulus of elasticity of 0.1 GPa and a strain energy per unit volume of 23037 kJ / m 3 It was.
[0087] [Thermoplastic resin particles B-6] 12 nylon (volume average particle size 20 μm, melting point 175° C., Orgasol 2002D manufactured by Arkema) was used as thermoplastic resin particles B-6. The tensile modulus and strain energy per unit volume were measured in the same manner as for the thermoplastic resin particles (B-1), except that the temperature of the heat press was changed to 200°C. The measurement results showed a modulus of elasticity of 1.2 GPa and a strain energy per unit volume of 125055 kJ / m 3 It was.
[0088] [Thermoplastic resin particles B-7] Polymethyl methacrylate (volume average particle diameter 10 μm, microspheres manufactured by Matsumoto Oil & Fat Co., Ltd.) was used as thermoplastic resin particles B-7. The tensile modulus and strain energy per unit volume were measured in the same manner as for thermoplastic resin particles (B-1), except that the temperature of the heat press was changed to 200°C. The measurement results showed a modulus of elasticity of 2.6 GPa and a strain energy per unit volume of 8661 kJ / m 3 It was.
[0089] <Component (C): Hardener> As the component (C), the following curing agents (C-1) and (C-2) were prepared. [Curing agent C-1] An acid anhydride curing agent (Rikacid MH700; a liquid alicyclic acid anhydride whose main component is 4-methylhexahydrophthalic anhydride, manufactured by New Japan Chemical Co., Ltd.) was used as curing agent C-1. [Hardening agent C-2] An amine-based curing agent (Kayahard AA; diethyldiaminodiphenylmethane, manufactured by Nippon Kayaku Co., Ltd.) was used as curing agent C-2.
[0090] <Component (D): Curing accelerator> As the component (D), the following curing accelerators (D-1) and (D-2) were used. [Curing Accelerator D-1] An imidazole-based curing accelerator (Curezol 1B2MZ; 1-benzyl-2-methylimidazole, manufactured by Shikoku Chemical Industries, Ltd.) was used as curing accelerator D-1. [Curing accelerator D-2] An imidazole-based curing accelerator (Curezol 2E4MZ; 2-ethyl-4-methylimidazole, manufactured by Shikoku Chemical Industry Co., Ltd.) was used as curing accelerator D-2.
[0091] <Preparation of each composition> Example 1 Adhesive composition (1) was prepared by weighing 38.7 parts by mass of component (A-1) (functional group equivalent: 0.23), 23 parts by mass of component (B-1), 37.7 parts by mass of component (C-1), and 0.6 parts by mass of component (D-1) into a plastic container so as to obtain the composition shown in Table 1, and then stirring the mixture at 2000 rpm for 1 minute and degassing it at 2200 rpm for 1 minute using an Awatori Rentaro (ARE-310, manufactured by Thinky Corporation) according to the following procedure.
[0092] (Examples 2-8, Comparative Examples 1-7: Adhesive Compositions (2)-(15)) Component (A), component (B), component (C) and / or component (D) were weighed into a plastic container so as to obtain the compositions shown in Table 1, and the mixture was stirred at 2000 rpm for 1 minute and then degassed at 2200 rpm for 1 minute using an Awatori Rentaro (ARE-310, manufactured by Thinky Corporation), to prepare adhesive compositions (2)-(15).
[0093] <Evaluation of adhesive strength and cohesive failure rate> (1) Tensile shear adhesive strength and cohesive failure rate against aluminum plate Adhesive compositions (1)-(15) were each applied to a pretreated aluminum plate (JIS H4000 A1050P, size 3mm x 25mm x 100mm) with a 12.5mm x 25mm rectangular adhesive joint. Another aluminum plate was attached to the plate and the plate was heated at 60°C for 60 minutes, then heated at 2°C / min to 100°C, heated at 100°C for 60 minutes, heated at 2.5°C / min to 150°C, and heated at 150°C for 120 minutes. Tensile shear adhesive test specimens were then prepared. The pretreatment included sandblasting and immersion in an alkaline bath containing an organic solvent at 70°C. The obtained tensile shear adhesive test specimens were subjected to a tensile shear adhesive test using a tensile testing machine (AGS-X, manufactured by Shimadzu Corporation) under the conditions of a gripping distance of 100 mm and a test speed of 2 mm / min, and the measured value of the maximum breaking strength (N) and the area of the adhesive joint (mm 2 The tensile shear adhesive strength (MPa) to the aluminum plate was calculated from the measured values. After the tensile shear adhesive test, the fracture surface of the test piece was visually inspected, and the ratio of the area of the fracture surface where adhesive remained on the metal substrate surface to the area of the adhesive joint was calculated. The results are shown in Table 1.
[0094] [Table 1]
Claims
1. A thermosetting resin as component (A); Thermoplastic resin particles as component (B); a curing agent as component (C) and / or a curing accelerator as component (D); An adhesive composition comprising: The component (B) has a tensile modulus of elasticity of a No. 7 dumbbell test piece molded to a width of 2 mm and a thickness of 1 mm according to the provisions of JIS K7161 of 1 GPa or less, and a strain energy per unit volume calculated from the stress-strain curve of the test piece of 20,000 kJ / m 3 The adhesive composition is the thermoplastic resin particles described above.
2. The adhesive composition according to claim 1 , wherein the component (A) is an epoxy resin.
3. 3. The adhesive composition according to claim 1, wherein the content of the component (A) is 7 to 95 mass% with respect to the total amount of the components (A), (B), (C), and (D).
4. The adhesive composition according to any one of claims 1 to 3, wherein the volume average particle diameter of the component (B) is 2 to 30 µm.
5. The adhesive composition according to any one of claims 1 to 4, which is used for bonding any one of structural materials, composite materials, electric and electronic materials, substrate materials, laminate materials, coating materials, and paints.
6. A cured product of the adhesive composition according to any one of claims 1 to 5.
7. A step of applying or casting the adhesive composition according to any one of claims 1 to 5 onto a surface of an object to be adhered; curing the adhesive composition; A method for producing an adhesive layer comprising the steps of:
8. A process for applying the adhesive composition according to any one of claims 1 to 5 to a surface of an object to be adhered and disposing the adhesive composition between at least two objects to be adhered; curing the adhesive composition; A method for producing a laminate in which at least two objects to be bonded are bonded, comprising:
9. A step of casting the adhesive composition according to any one of claims 1 to 5 between at least two objects to be adhered; curing the adhesive composition; A method for producing a laminate in which at least two objects to be bonded are bonded, comprising:
Citation Information
Patent Citations
Adhesive composition
JP1993295340A
Epoxy resin adhesive
JP6526571B2
Adhesive composition
WO2019189238A1