Inkjet ink
The inkjet ink formulation with specific surfactants and LogP-controlled aqueous medium addresses ejection stability and image quality issues by stabilizing the meniscus and optimizing pigment distribution, resulting in stable ejection and high-quality images.
Patent Information
- Application Number
- JP2023060848
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-17
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing inkjet inks fail to achieve optimal ejection stability, image density, and scratch resistance, as they suffer from hydrophobicity gradients leading to nozzle clogging and uneven pigment distribution.
Inkjet inks containing a pigment, a first surfactant represented by general formula (S1), a second surfactant represented by general formula (S2), and an aqueous medium with a specific octanol/water partition coefficient LogP of -0.52 to -0.19, which stabilizes the meniscus and optimizes pigment distribution.
The ink achieves excellent ejection stability and forms images with desired image density and scratch resistance by preventing nozzle clogging and ensuring appropriate pigment penetration into the recording medium.
Smart Images

Figure 2024148002000001 
Figure 2024148002000002 
Figure 2024148002000003
Abstract
Description
[Technical field]
[0001] The present invention relates to ink-jet inks. [Background technology]
[0002] Some inkjet recording devices use aqueous inkjet inks containing a pigment and an aqueous medium. Inkjet inks are required to have excellent ejection stability and to be capable of forming images having a desired image density and excellent abrasion resistance.
[0003] In response to such demands, for example, an inkjet ink has been proposed that contains a coloring material and alkyl polyols, the alkyl polyols including two or more first alkyl polyols having an octanol / water partition coefficient LogP of -0.7 or more and 0.01 or less and a normal boiling point of 180° C. or more and 250° C. or less (Patent Document 1). The inkjet ink described above is said to have excellent clogging recovery properties and continuous printing stability by containing an alkyl polyol having a predetermined octanol / water partition coefficient LogP. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-231107 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, even the inkjet ink described in Patent Document 1 does not fully satisfy the ejection stability, image density of the formed image, and abrasion resistance.
[0006] The present invention has been made in view of the above problems, and an object of the present invention is to provide an inkjet ink that has excellent ejection stability and is capable of forming an image having a desired image density and excellent abrasion resistance. [Means for solving the problem]
[0007] The inkjet ink according to the present invention contains a pigment, a first surfactant, a second surfactant, and an aqueous medium. The first surfactant is a compound represented by the following general formula (S1). The second surfactant is a compound represented by the following general formula (S2). The aqueous medium has an octanol / water partition coefficient LogP of -0.52 or more and -0.19 or less.
[0008] [ka]
[0009] In the general formula (S1), R 1 R represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 2 represents an alkyl group having 1 or more and 4 or less carbon atoms. n represents an integer of 2 or more and 5 or less. In the general formula (S2), m represents an integer of 12 or more and 20 or less. Effect of the Invention
[0010] The inkjet ink according to the present invention is excellent in ejection stability and can form images having a desired image density and excellent abrasion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described. In the following, the volume median diameter (D 50 ) is a value measured using a dynamic light scattering particle size distribution analyzer ("Zetasizer Nano ZS" manufactured by Malvern Instruments) unless otherwise specified. In this specification, acrylic and methacrylic may be collectively referred to as "(meth)acrylic".
[0012] The measured weight average molecular weight (Mw), unless otherwise specified, is a value measured using gel permeation chromatography.
[0013] Unless otherwise specified, the measured acid value is a value measured in accordance with "JIS (Japanese Industrial Standards) K0070-1992".
[0014] <Ink> An inkjet ink (hereinafter sometimes simply referred to as ink) according to an embodiment of the present invention will be described below. The ink of the present invention contains a pigment, a first surfactant, a second surfactant, and an aqueous medium. The first surfactant is a compound represented by the following general formula (S1). The second surfactant is a compound represented by the following general formula (S2). The octanol / water partition coefficient LogP (hereinafter sometimes simply referred to as "LogP") of the aqueous medium is -0.52 or more and -0.19 or less.
[0015] [ka]
[0016] In general formula (S1), R 1 R represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 2 represents an alkyl group having 1 or more and 4 or less carbon atoms. n represents an integer of 2 or more and 5 or less. In general formula (S2), m represents an integer of 12 or more and 20 or less.
[0017] In addition, in the general formula (S1), 1 may be the same or different.
[0018] The ink of the present invention, by being provided with the above-mentioned configuration, is excellent in ejection stability and can form an image having a desired image density and excellent abrasion resistance. The reason is presumed to be as follows. In the inkjet recording method using the known ink, when an image is formed and then image formation is performed again after a certain period of time, image defects are likely to occur. This image defect occurs when the meniscus of the known ink comes into contact with the air near the tip of the nozzle of the recording head (near the opening) and the known ink dries. When the known ink loses moisture due to drying, the content ratio of water-soluble organic solvent becomes relatively high and the hydrophobicity increases. On the other hand, this phenomenon does not occur inside the nozzle of the recording head (a part away from the tip of the nozzle). As a result, in the nozzle of the recording head, a hydrophobicity gradient occurs in which the known ink present near the tip of the nozzle is highly hydrophobic and the known ink present inside the nozzle is low in hydrophobicity. When such a hydrophobicity gradient occurs, the pigment contained in the known ink migrates from near the tip of the nozzle to the inside of the nozzle. As a result, the pigment concentration of the known ink decreases near the tip of the nozzle of the recording head and becomes transparent. Furthermore, inside the nozzles of the recording head, the pigment concentration of the known ink increases, causing the ink to thicken, which can lead to nozzle clogging. As a result, the inkjet recording method using the known inks produces the above-mentioned image defects.
[0019] In contrast, the ink of the present invention contains a first surfactant. The first surfactant is a surfactant that is generally used in applications such as cosmetics. The first surfactant has a high movement speed at the gas-liquid interface. Therefore, when a meniscus of the ink of the present invention is formed near the tip of the recording head, the first surfactant quickly moves to the meniscus to form a protective layer. As a result, the ink of the present invention is prevented from drying near the tip of the recording head, and can exhibit excellent ejection stability.
[0020] Furthermore, an image formed by an inkjet recording method has insufficient abrasion resistance if the pigment remains on the surface of the recording medium. On the other hand, an image formed by an inkjet recording method has insufficient image density if the pigment penetrates deep into the recording medium. In contrast, the ink of the present invention contains a second surfactant and an aqueous medium, thereby optimizing the position of the pigment in the formed image. Specifically, the second surfactant imparts an appropriate penetrability to the recording medium to the ink of the present invention. As a result, the ink of the present invention can quickly penetrate into the recording medium after landing on the recording medium. In addition, since the ink of the present invention contains a relatively highly hydrophobic aqueous medium (an aqueous medium with a LogP of -0.52 or more and -0.19 or less), the dispersion state of the pigment in the aqueous medium is somewhat unstable. Then, when the ink of the present invention penetrates into the recording medium, a speed difference occurs in which highly hydrophilic components (e.g., water and highly hydrophilic water-soluble organic solvent) penetrate quickly, and other components (e.g., highly hydrophobic water-soluble organic solvent and pigment) penetrate slowly. As a result, when the ink of the present invention penetrates into the recording medium, the highly hydrophobic water-soluble organic solvent and pigment are concentrated at a site relatively close to the surface of the recording medium, and the pigment aggregates. As a result, the ink of the present invention can form an image in which the pigment remains at a portion slightly penetrating from the surface of the recording medium (i.e., an image having a desired image density and excellent abrasion resistance). The ink of the present invention will be described in more detail below. Each of the components described below may be used alone or in combination of two or more.
[0021] [Pigment] In the ink of the present invention, the pigment constitutes a pigment particle together with, for example, a pigment-coated resin. The pigment particle is constituted, for example, by a core containing a pigment and a pigment-coated resin that coats the core. The pigment-coated resin exists, for example, in a state of being dispersed in a solvent. From the viewpoint of optimizing the color density, hue, or stability of the ink of the present invention, the volume median diameter of the pigment particles is preferably 30 nm or more and 200 nm or less, and more preferably 70 nm or more and 130 nm or less.
[0022] Examples of pigments include yellow pigments, orange pigments, red pigments, blue pigments, purple pigments, and black pigments. Examples of yellow pigments include CI Pigment Yellow (74, 93, 95, 109, 110, 120, 128, 138, 139, 151, 154, 155, 173, 180, 185, and 193). Examples of orange pigments include CI Pigment Orange (34, 36, 43, 61, 63, and 71). Examples of red pigments include CI Pigment Red (122 and 202). Examples of blue pigments include CI Pigment Blue (15, more specifically 15:3). Examples of purple pigments include CI Pigment Violet (19, 23, and 33). Examples of black pigments include CI Pigment Black (7).
[0023] In the ink of the present invention, the pigment content is preferably 0.50% by mass or more and 10.00% by mass or less, and more preferably 1.50% by mass or more and 5.00% by mass or less. By making the pigment content 0.50% by mass or more, the ink of the present invention can more easily form an image having a desired image density. In addition, by making the pigment content 10.00% by mass or less, the fluidity of the ink of the present invention can be ensured.
[0024] [Pigment-coated resin] The pigment coating resin is a resin that is soluble in the aqueous medium of the ink of the present invention. A part of the pigment coating resin is present, for example, on the surface of the pigment particle, optimizing the dispersibility of the pigment particle. A part of the pigment coating resin is present, for example, in a dissolved state in the aqueous medium of the ink of the present invention.
[0025] The pigment coating resin is preferably a styrene-acrylic resin. The styrene-acrylic resin is a copolymer of at least one monomer selected from the group consisting of an alkyl (meth)acrylate ester and (meth)acrylic acid, and styrene. The styrene-acrylic resin preferably has a repeating unit derived from (meth)acrylic acid ((meth)acrylic acid unit), a repeating unit derived from an alkyl (meth)acrylate ester ((meth)acrylic acid alkyl ester unit), and a styrene unit.
[0026] Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and octyl (meth)acrylate. The (meth)acrylic acid alkyl ester is preferably methyl methacrylate or butyl acrylate.
[0027] Of all the repeating units contained in the pigment coating resin, the proportion of (meth)acrylic acid units is preferably 30% by mass or more and 50% by mass or less. Of all the repeating units contained in the pigment coating resin, the proportion of (meth)acrylic acid alkyl ester units is preferably 35% by mass or more and 55% by mass or less. Of all the repeating units contained in the pigment coating resin, the proportion of styrene units is preferably 5% by mass or more and 25% by mass or less. As the pigment coating resin, a resin having a repeating unit derived from methacrylic acid, a repeating unit derived from methyl methacrylate, a repeating unit derived from butyl acrylate, and a styrene unit is more preferable.
[0028] In the ink, the content of the pigment coating resin is preferably 0.10% by mass or more and 4.00% by mass or less, and more preferably 0.50% by mass or more and 2.00% by mass or less. By making the content of the pigment coating resin 0.10% by mass or more, the dispersibility of the pigment component can be further improved. By making the content of the pigment coating resin 4.00% by mass or less, the ejection stability of the ink of the present invention can be further optimized.
[0029] The acid value of the pigment coating resin is preferably from 30 mgKOH / g to 200 mgKOH / g, more preferably from 70 mgKOH / g to 130 mgKOH / g. By setting the acid value of the pigment coating resin to be from 30 mgKOH / g to 200 mgKOH / g, the dispersibility of the pigment can be further improved while optimizing the storage stability of the ink of the present invention.
[0030] The acid value of the pigment coating resin can be adjusted by changing the amount of monomer used in synthesizing the pigment coating resin. For example, the acid value of the pigment coating resin can be increased by using a monomer (more specifically, acrylic acid, methacrylic acid, etc.) having an acidic functional group (e.g., a carboxyl group) in synthesizing the pigment coating resin.
[0031] The Mw of the pigment coating resin is preferably from 10,000 to 50,000, and more preferably from 15,000 to 25,000. By setting the Mw of the pigment coating resin to be from 10,000 to 50,000, the image density of the formed image can be further optimized while suppressing an increase in the viscosity of the ink of the present invention.
[0032] The Mw of the pigment coating resin can be adjusted by changing the polymerization conditions for the pigment coating resin (more specifically, the amount of polymerization initiator used, polymerization temperature, polymerization time, etc.).
[0033] In the polymerization of the pigment-coated resin, the amount of the polymerization initiator used is preferably 0.001 to 5 mol, more preferably 0.01 to 2 mol, per mol of the monomer mixture. In the polymerization of the pigment-coated resin, for example, the polymerization temperature can be 50° C. to 70° C., and the polymerization time can be 10 to 24 hours. The polymerized pigment-coated resin is preferably neutralized with an equal amount of a basic compound before being used as a raw material for the ink of the present invention. The basic compound is preferably a hydroxide of an alkali metal ion (e.g., NaOH or KOH).
[0034] [First surfactant] The first surfactant is represented by the general formula (S1): The first surfactant optimizes the permeability of the ink of the present invention into a recording medium.
[0035] In general formula (S1), R 1 Examples of the alkyl group having 1 to 3 carbon atoms represented by the formula (S1) include a methyl group, an ethyl group, an n-propyl group, and an iso-propyl group. 1 preferably represents a hydrogen atom.
[0036] In general formula (S1), R 2 Examples of the alkyl group having 1 to 4 carbon atoms represented by the formula (S1) include a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, and a tert-butyl group. 2 preferably represents a methyl group.
[0037] In the general formula (S1), n preferably represents 2 or 3.
[0038] The first surfactant is preferably a compound represented by the following chemical formula (S1-1) or a compound represented by the following chemical formula (S1-2).
[0039] [ka]
[0040] The first surfactant can be obtained, for example, by reacting a compound represented by the following general formula (a) with a compound represented by the following general formula (b) in the presence of an acid. 1 , R 2 and n have the same meaning as in general formula (S1).
[0041] [ka]
[0042] In the ink of the present invention, the content of the first surfactant is preferably from 0.01% to 3.00% by mass, more preferably from 0.07% to 1.00% by mass, and even more preferably from 0.30% to 0.70% by mass. By setting the content of the first surfactant to be from 0.01% to 2.00% by mass, the permeability of the ink of the present invention into the recording medium can be further optimized.
[0043] [Second surfactant] The second surfactant is represented by the general formula (S2). The second surfactant suppresses drying of the ink of the present invention in the nozzle of the recording head. The second surfactant is called ceramide, and various compounds represented by the general formula (S2) are commercially available.
[0044] In formula (S2), m is preferably an even number, more preferably an integer of 14 or more and 18 or less, and further preferably 14, 16 or 18.
[0045] In the ink of the present invention, the content of the second surfactant is preferably from 0.01% to 2.00% by mass, more preferably from 0.03% to 0.70% by mass, and even more preferably from 0.05% to 0.20% by mass. By setting the content of the second surfactant to from 0.01% to 2.00% by mass, drying of the ink of the present invention can be more effectively suppressed.
[0046] [Other surfactants] The ink of the present invention may contain only the first surfactant and the second surfactant as surfactants, or may further contain a surfactant other than the first surfactant and the second surfactant (hereinafter, referred to as another surfactant). In the surfactant contained in the present invention, the total content ratio of the first surfactant and the second surfactant is preferably 60% by mass or more, and more preferably 80% by mass or more.
[0047] Other surfactants include, for example, acetylene glycol surfactants (surfactants containing acetylene glycol compounds), silicone surfactants (surfactants containing silicone compounds) and fluorine surfactants (surfactants containing fluorine resins or fluorine-containing compounds).Acetylene glycol surfactants include, for example, ethylene oxide adducts of acetylene glycol and propylene oxide adducts of acetylene glycol.
[0048] The content of the other surfactant in the ink of the present invention is preferably from 0.01% by mass to 1.00% by mass, and more preferably from 0.05% by mass to 0.20% by mass.
[0049] [Aqueous medium] The aqueous medium contained in the ink of the present invention is a medium containing water. The aqueous medium may function as a solvent or as a dispersion medium. Specific examples of the aqueous medium include aqueous media containing water and a water-soluble organic solvent.
[0050] The LogP of the aqueous medium is -0.52 or more and -0.19 or less, preferably -0.52 or more and -0.35 or less, and more preferably -0.52 or more and -0.45 or less. By making the LogP of the aqueous medium -0.52 or more, the dispersion stability of the pigment in the aqueous medium can be moderately destabilized. As a result, the ink of the present invention can optimize the image density of the image formed. By making the LogP of the aqueous medium -0.19 or less, the pigment can be prevented from becoming excessively unstable in the aqueous medium. As a result, the ink of the present invention can optimize the scratch resistance of the image formed. The LogP of the aqueous medium can be measured by various calculation software (for example, HSPiP described in the examples).
[0051] (water) In the ink of the present invention, the water content is preferably from 25.00% to 70.00% by mass, and more preferably from 45.00% to 55.00% by mass. By setting the water content to from 25.00% to 70.00% by mass, it becomes easier to adjust the LogP of the aqueous medium to the above range.
[0052] (Water-soluble organic solvent) Examples of the water-soluble organic solvent include glycol compounds, glycol ether compounds, lactam compounds, nitrogen-containing compounds, acetate compounds, thiodiglycol, glycerin, and dimethyl sulfoxide.
[0053] Examples of glycol compounds include ethylene glycol, 1,3-propanediol, propylene glycol, 1,3-butanediol, 1,2-pentanediol, 1,5-pentanediol, 1,2-octanediol, 1,8-octanediol, 3-methyl-1,3-butanediol, 3-methyl-1,5-pentanediol, diethylene glycol, triethylene glycol, and tetraethylene glycol.
[0054] Examples of glycol ether compounds include diethylene glycol diethyl ether, diethylene glycol monobutyl ether, ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monobutyl ether, and propylene glycol monomethyl ether.
[0055] Lactam compounds include, for example, 2-pyrrolidone and N-methyl-2-pyrrolidone.
[0056] Examples of nitrogen-containing compounds include 1,3-dimethylimidazolidinone, formamide, and dimethylformamide.
[0057] An example of the acetate compound is diethylene glycol monoethyl ether acetate.
[0058] The water-soluble organic solvent is preferably a glycol compound or a glycol ether compound, more preferably 3-methyl-1,3-butanediol, 1,2-pentanediol, 1,3-propanediol, propylene glycol, 1,3-butanediol, 3-methyl-1,5-pentanediol or triethylene glycol monobutyl ether, and further preferably the first mixed solvent, the second mixed solvent, the third mixed solvent or the fourth mixed solvent shown below.
[0059] The first mixed solvent contains only 3-methyl-1,3-butanediol, 1,2-pentanediol, propylene glycol, and triethylene glycol monobutyl ether. In this case, in the ink of the present invention, the content of 3-methyl-1,3-butanediol is preferably 9.00% by mass or more and 10.00% by mass or less. The content of 1,2-pentanediol is preferably 8.00% by mass or more and 10.00% by mass or less. The content of propylene glycol is preferably 18.00% by mass or more and 22.00% by mass or less. The content of triethylene glycol monobutyl ether is preferably 5.00% by mass or more and 7.00% by mass or less.
[0060] The second mixed solvent contains only 3-methyl-1,3-butanediol, 1,2-pentanediol, propylene glycol, triethylene glycol monobutyl ether, and 1,3-propanediol. In this case, in the ink of the present invention, the content of 3-methyl-1,3-butanediol is preferably 8.00% by mass or more and 9.00% by mass or less. The content of 1,2-pentanediol is preferably 8.00% by mass or more and 10.00% by mass or less. The content of propylene glycol is preferably 12.50% by mass or more and 14.00% by mass or less. The content of triethylene glycol monobutyl ether is preferably 10.00% by mass or more and 12.00% by mass or less. The content of 1,3-propanediol is preferably 2.00% by mass or more and 4.00% by mass or less.
[0061] The third mixed solvent contains only 1,2-pentanediol, propylene glycol, triethylene glycol monobutyl ether, 3-methyl-1,5-pentanediol, and 1,3-butanediol. In this case, in the ink of the present invention, the content of 1,2-pentanediol is preferably 8.00% by mass or more and 10.00% by mass or less. The content of propylene glycol is preferably 14.00% by mass or more and 16.00% by mass or less. The content of triethylene glycol monobutyl ether is preferably 7.00% by mass or more and 9.00% by mass or less. The content of 3-methyl-1,5-pentanediol is preferably 9.50% by mass or more and 11.50% by mass or less. The content of 1,3-butanediol is preferably 1.00% by mass or more and 3.00% by mass or less.
[0062] The fourth mixed solvent contains 1,2-pentanediol, propylene glycol, triethylene glycol monobutyl ether, and 3-methyl-1,5-pentanediol. In this case, in the ink of the present invention, the content of 1,2-pentanediol is preferably 6.00% by mass or more and 8.00% by mass or less. The content of propylene glycol is preferably 11.50% by mass or more and 12.50% by mass or less. The content of triethylene glycol monobutyl ether is preferably 12.00% by mass or more and 14.00% by mass or less. The content of 3-methyl-1,5-pentanediol is preferably 11.50% by mass or more and 13.50% by mass or less.
[0063] The total content of the water-soluble organic solvents in the ink of the present invention is preferably from 35.00% by mass to 60.00% by mass, and more preferably from 40.00% by mass to 50.00% by mass.
[0064] [Other ingredients] The ink of the present invention may further contain known additives (for example, a dissolution stabilizer, a drying inhibitor, an antioxidant, a viscosity adjuster, a pH adjuster, and an anti-mold agent) as necessary.
[0065] [Ink manufacturing method] The ink of the present invention can be produced, for example, by uniformly mixing a pigment dispersion containing a pigment, a first surfactant, a second surfactant, and an aqueous medium with a stirrer. In producing the ink of the present invention, after the components are uniformly mixed, foreign matter and coarse particles may be removed with a filter (for example, a filter with a pore size of 5 μm or less).
[0066] (Pigment dispersion) The pigment dispersion is a dispersion containing a pigment. The pigment dispersion preferably further contains a pigment-coating resin. The dispersion medium of the pigment dispersion is preferably water.
[0067] The content of the pigment in the pigment dispersion is preferably from 5.0 to 30.0% by mass, more preferably from 15.0 to 25.0% by mass, and the content of the pigment coating resin in the pigment dispersion is preferably from 2.0 to 12.0% by mass, more preferably from 5.0 to 7.0% by mass.
[0068] The pigment dispersion can be prepared by wet-dispersing the pigment, the pigment-coated resin, a dispersion medium (e.g., water), and optional components (e.g., other surfactants) using a media-type wet disperser. In the wet dispersion using a media-type wet disperser, small-particle-size beads (e.g., D 50 The material of the beads is not particularly limited, but hard materials (for example, glass and zirconia) are preferable.
[0069] When the pigment dispersion is added in the production of the ink of the present invention, the ratio of the pigment dispersion to all the raw materials of the ink is, for example, 10.0% by mass or more and 40.0% by mass or less. EXAMPLES
[0070] Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0071] [Preparation of the first surfactant] The first surfactants, surfactants (S1-1) and (S1-2), were prepared by the following method.
[0072] (Surfactant (S1-1)) A round-bottom flask immersed in an oil bath was used as a reaction vessel. 42.06 g (0.4 mol) of 2-(2-aminoethoxy)ethanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., molecular weight 105.14), 70.49 g (0.8 mol) of ethyl acetate, and 0.33 g of phosphorous acid were added to the reaction vessel to obtain a reaction solution. The reaction solution was refluxed under a N2 atmosphere (first reflux treatment). After the first reflux treatment, excess ethyl acetate and ethanol (by-products) in the reaction vessel were distilled off by distillation.
[0073] The first reflux process was performed using an FT-IR spectrometer (Fourier transform infrared spectrophotometer) with a wave number of 1646 cm -1 The ratio of the specific peak present at the position (the ratio of the peak derived from the amide carbonyl structure generated by the reaction) was monitored during the first reflux treatment. During the first reflux treatment, the ratio of the specific peak increased as the reaction proceeded. When the increase in the ratio of the specific peak stopped, it was determined that the reaction had proceeded completely, and the first reflux treatment was terminated.
[0074] (Details of FT-IR equipment) FT-IR device: Nicolet iS10 (manufactured by Thermo Electron Co., Ltd.) ATR device: Attached device for single-reflection type ATR (using ZnSe crystal) Detector: DTGS detector
[0075] Next, 35.24 g (0.4 mol) of ethyl acetate was added to the reaction solution (ethyl acetate addition treatment). Next, the reaction solution was refluxed under a N2 atmosphere (second reflux treatment). After the second reflux treatment, excess ethyl acetate and ethanol (by-products) in the reaction vessel were distilled off (distillation treatment).
[0076] The second reflux treatment was carried out while monitoring the ratio of the specific peaks with the above-mentioned FT-IR device. During the second reflux treatment, the ratio of the specific peaks increased as the reaction proceeded. When the increase in the ratio of the specific peaks stopped, it was determined that the reaction had proceeded completely, and the second reflux treatment was terminated.
[0077] The series of processes of adding ethyl acetate, second refluxing and distillation was repeated several times until the increase in the ratio of the specific peak was no longer observed during the second refluxing. This allowed all of the 2-(2-aminoethoxy)ethanol in the reaction solution to react. The resulting reaction product was the surfactant (S1-1) represented by the above-mentioned chemical formula (S1-1).
[0078] (Surfactant (S1-2)) Surfactant (S1-2) was prepared in the same manner as in the preparation of surfactant (S1-1), except that 0.4 mol of 2-"2-(2-aminoethoxy)ethoxy"ethanol (molecular weight 149.19) was used instead of 2-(2-aminoethoxy)ethanol.
[0079] [Preparation of the second surfactant] As the second surfactant, the following surfactants (S2-1) to (S2-3) were prepared. Surfactant (S2-1): Fujifilm Wako Pure Chemical Corporation's "C14 ceramide" (a compound represented by the general formula (S2) where m is 14) Surfactant (S2-2): Fujifilm Wako Pure Chemical Corporation's "C16 ceramide" (a compound represented by the general formula (S2) where m is 16) Surfactant (S2-3): Fujifilm Wako Pure Chemical Corporation's "C18 ceramide" (a compound represented by the general formula (S2) where m is 18)
[0080] [Preparation of cyan pigment dispersion] A cyan pigment dispersion was prepared for use in preparing the ink. In preparing the cyan pigment dispersion, first, a pigment coating resin solution containing the pigment coating resin (R) and water was prepared.
[0081] (Preparation of pigment coated resin solution) An alkali-soluble resin having a repeating unit derived from methacrylic acid (MAA unit), a repeating unit derived from methyl methacrylate (MMA unit), a repeating unit derived from butyl acrylate (BA unit), and a repeating unit derived from styrene (ST unit) was prepared. This alkali-soluble resin had a mass average molecular weight (Mw) of 20,000 and an acid value of 100 mg KOH / g. The mass ratio of each repeating unit in this alkali-soluble resin was "MAA unit: MMA unit: BA unit: ST unit = 40: 15: 30: 15". This alkali-soluble resin was mixed with an aqueous potassium hydroxide solution (KOH concentration: 10 mass%) (neutralization treatment). The alkali-soluble resin was neutralized with an equal amount of KOH by the neutralization treatment. As a result, a pigment-coated resin solution containing a pigment-coated resin (R) and water was obtained.
[0082] The Mw of the above-mentioned alkali-soluble resin was measured under the following conditions using gel permeation chromatography ("HLC-8020GPC" manufactured by Tosoh Corporation). A calibration curve was prepared using TSKgel standard polystyrenes F-40, F-20, F-4, F-1, A-5000, A-2500, and A-1000 manufactured by Tosoh Corporation and n-propylbenzene.
[0083] (Conditions for measuring mass average molecular weight) Column: Tosoh Corporation's "TSKgel SuperMultiporeHZ-H" (4.6mm I.D. x 15cm semi-microcolumn) Number of columns: 3 Eluent: Tetrahydrofuran ·Flow rate: 0.35mL / min Sample injection volume: 10μL ·Measurement temperature: 40℃ Detector: IR detector
[0084] [Preparation of cyan pigment dispersion] In order to obtain the composition shown in Table 1 below, a cyan pigment ("Lionol (registered trademark) Blue FG-7330" manufactured by Toyo Color Co., Ltd., component: copper phthalocyanine, color index: pigment blue 15:3), the above-mentioned pigment coating resin solution containing the pigment coating resin (R), an acetylene glycol surfactant "Olfine (registered trademark) E1010" manufactured by Nissin Chemical Industry Co., Ltd. (ethylene oxide adduct of acetylene glycol), and ion-exchanged water were added to the vessel of a media-type wet disperser ("DYNO (registered trademark)-MILL" manufactured by Willy & Bachofen (WAB)).
[0085] The content of "water" in Table 1 below indicates the total content of the ion-exchanged water charged into the vessel described above and the water contained in the pigment-coated resin solution (more specifically, the water contained in the aqueous sodium hydroxide solution used for neutralizing the alkali-soluble resin, and the water generated by the neutralization reaction of the alkali-soluble resin and potassium hydroxide).
[0086] [Table 1]
[0087] Next, the contents of the vessel were wet-dispersed. Zirconia beads (particle diameter 1.0 mm) were used as media. The amount of media added was 70 volume % of the capacity of the vessel. The dispersion conditions were a temperature of 10°C and a peripheral speed of 8 m / sec. As a result, a cyan pigment dispersion was obtained.
[0088] The volume median diameter (D 50 Specifically, the obtained cyan pigment dispersion was diluted 300 times with ion-exchanged water to prepare a measurement sample. The D of the pigment particles in the measurement sample was measured using a dynamic light scattering particle size distribution measurement device (Malvern Zetasizer Nano ZS). 50 The D of the pigment particles in the measurement sample was 50 of pigment particles contained in the cyan pigment dispersion 50 The measurement was carried out 10 times, and the average of the measurement results was taken as the D of the pigment particles.50 The D of the pigment particles contained in the cyan pigment dispersion was adopted. 50 was 100 nm.
[0089] <Ink Preparation> Inks of Examples 1 to 11 and Comparative Examples 1 to 9 were prepared by the following method.
[0090] [Example 1] 20.00 parts by mass of cyan pigment dispersion, 0.50 parts by mass of surfactant (S1-1), 0.10 parts by mass of surfactant (S2-1), 35.00 parts by mass of ion-exchanged water, 9.50 parts by mass of 3-methyl-1,3-butanediol, 9.00 parts by mass of 1,2-pentanediol, 19.90 parts by mass of propylene glycol, and 6.00 parts by mass of triethylene glycol monobutyl ether were added to a beaker. The contents of the beaker were mixed at a rotation speed of 400 rpm using a stirrer ("Three-One Motor BL-600" manufactured by Shinto Scientific Co., Ltd.) to obtain a mixed liquid. The mixed liquid was filtered using a filter (pore size 5 μm) to remove foreign matter and coarse particles contained in the mixed liquid. In this manner, the ink of Example 1 was obtained.
[0091] The octanol / water partition coefficient LogP of the aqueous medium (water, 3-methyl-1,3-butanediol, 1,2-pentanediol, propylene glycol, and triethylene glycol monobutyl ether) contained in the ink of Example 1 was calculated. In the calculation, calculation software "Hansen Solubility Parameter in Practice (HSPiP) Ver. 5.2.06" (developer: Prof. Steven Abbott et al.) was used. The octanol / water partition coefficient LogP of the aqueous medium contained in the ink of Example 1 was -0.50.
[0092] [Examples 2 to 11 and Comparative Examples 1 to 9] Inks of Examples 2 to 11 and Comparative Examples 1 to 9 were prepared in the same manner as in the preparation of the ink of Example 1, except that the types and amounts of each component were changed as shown in Tables 2 to 4. In Comparative Example 9, a surfactant (X) ("Surfynol (registered trademark) 420" manufactured by Nissin Chemical Industry Co., Ltd., an acetylene-based surfactant) was used as a surfactant different from the first surfactant and the second surfactant.
[0093] In Tables 2 to 4, the numerical value of each component indicates the content ratio. "MB" indicates 3-methyl-1,3-butanediol. "TEGMBE" indicates triethylene glycol monobutyl ether. "MPD" indicates 3-methyl-1,5-pentanediol.
[0094] [Table 2]
[0095] [Table 3]
[0096] [Table 4]
[0097] <Evaluation> The inks of Examples 1 to 11 and Comparative Examples 1 to 9 were evaluated for image density and abrasion resistance of the images formed, and for ejection stability, using the following methods. The evaluation results are shown in the following Tables 5 to 6. The evaluations were performed at a temperature of 25°C and a humidity of 60% RH, unless otherwise specified.
[0098] [Evaluation machine] A line head type inkjet recording device (a test machine manufactured by Kyocera Document Solutions Inc.) was used as the evaluation machine. The evaluation machine was equipped with a piezoelectric type recording head and a conveying table. The evaluation machine was equipped with a cleaning function for cleaning the nozzles of the recording head. The recording head was set so that the volume per ink droplet was 11 pL. The recording head was filled with the ink to be evaluated (specifically, any of the inks of Examples 1 to 11 and Comparative Examples 1 to 9).
[0099] [Image Density] In the evaluation of image density, A4-sized plain paper (FUJIFILM Business Innovation Co., Ltd.'s "C 2 ", PPC paper) was used. A solid image (size: length 10 cm, width 10 cm, printing rate: 100%) was formed on the recording medium using an evaluation machine. The recording medium on which the image was formed was left to stand for 1 hour in an environment with a temperature of 25°C and a humidity of 60% RH. After standing, the image density was measured at 10 randomly selected points on the solid image using a reflection densitometer (X-Rite "RD-19"). The average value of the image density measured at the 10 points was taken as the ID value. The image density was judged according to the following criteria.
[0100] (Image density standard) A (good): ID value was 1.20 or higher. B (bad): The ID value was less than 1.20.
[0101] [Discharge stability] After forming a solid image in the evaluation of image density, the recording head of the evaluation machine was cleaned by the nozzle cleaning function in an environment with a temperature of 25°C and a humidity of 10% RH. After cleaning, the evaluation machine was left to stand for one hour in an environment with a temperature of 25°C and a humidity of 10% RH. Next, using the evaluation machine after standing, a solid image was formed again on the above-mentioned recording medium. In the evaluation machine using ink with low ejection stability, the ink dried in the nozzles of the recording head of the evaluation machine during the one-hour standing, making it impossible to form a solid image. The ejection stability was judged according to the following criteria.
[0102] (Standard for discharge stability) A (good): The ink did not dry in the nozzles of the recording head, and a solid image could be formed. B (Fail): The ink dried in the nozzles of the recording head, and a solid image could not be formed.
[0103] [Abrasion resistance] In the evaluation of the abrasion resistance, copy paper ("CC90" manufactured by Mondi) was used as the recording medium. A solid image (size: 10 cm x 10 cm) was formed on the recording medium using an evaluation machine. Next, an unused recording medium (evaluation paper) was placed on top of the recording medium on which the solid image was formed. Next, a 1 kg rectangular weight was placed on the evaluation paper. At this time, the weight was placed so that the center of gravity of the weight was located at the center of the solid image. Next, with the weight placed, both ends of the evaluation paper were held, and the evaluation paper was moved back and forth 10 times in a certain direction to rub the solid image with the evaluation paper (load 1 kg). Next, the image density of the stain image transferred from the solid image to the evaluation paper was measured with a reflection densitometer ("eXact" manufactured by X-Rite). In detail, the image density of 10 randomly selected points in the stain image was measured with a reflection densitometer, and the arithmetic average value of the image densities of the 10 points was taken as the evaluation value (ID value) of the abrasion resistance. The abrasion resistance was judged according to the following criteria.
[0104] (Abrasion resistance standard) Good (A): The ID value is less than 0.008. Poor (B): ID value is 0.008 or more.
[0105] [Table 5]
[0106] [Table 6]
[0107] As shown in Tables 1 to 6, the inks of Examples 1 to 11 contained a pigment, a first surfactant, a second surfactant, and an aqueous medium. The first surfactant was a compound represented by general formula (S1). The second surfactant was a compound represented by general formula (S2). The LogP of the aqueous medium was -0.52 or more and -0.19 or less. The inks of Examples 1 to 11 were excellent in ejection stability, and were able to form images having desired image density and excellent abrasion resistance.
[0108] On the other hand, the ink of Comparative Example 1 had an excessively high LogP of the aqueous medium. It is considered that the pigment dispersion state of the ink of Comparative Example 1 is unstable, and the pigment quickly aggregates on the surface of the recording medium after landing on the recording medium. It is also considered that the pigment aggregates and causes nozzle clogging when the ink of Comparative Example 1 is exposed to drying conditions in the nozzle. As a result, the ink of Comparative Example 1 had poor ejection stability and abrasion resistance of the formed image.
[0109] The ink of Comparative Example 2 had an excessively low LogP of the aqueous medium. It is considered that the pigment dispersion state of the ink of Comparative Example 2 is excessively stable, and the pigment penetrates into the inside of the recording medium after landing on the recording medium. As a result, the ink of Comparative Example 2 formed an image with poor image density. The ink of Comparative Example 2 also formed an image with poor abrasion resistance.
[0110] The inks of Comparative Examples 3, 4, and 8 did not contain a second surfactant having a drying suppression effect. As a result, the inks of Comparative Examples 3, 4, and 8 had poor ejection stability. In addition, the inks of Comparative Examples 3, 4, and 8 also had poor at least one of the image density and abrasion resistance of the formed images.
[0111] The inks of Comparative Examples 5 to 7 did not contain a first surfactant that imparts penetrability to a recording medium to the ink. As a result, the inks of Comparative Examples 5 to 7 formed images with poor abrasion resistance. In addition, the inks of Comparative Examples 5 to 7 also had poor ejection stability and / or poor image density of the formed images.
[0112] The ink of Comparative Example 9 did not contain either the first or second surfactant, but instead contained a general surfactant (acetylene-based surfactant). The ink of Comparative Example 9 was poor in all of the ejection stability, image density, and abrasion resistance. [Industrial Applicability]
[0113] The inks of the present invention can be used to form images.
Claims
1. The ink composition includes a pigment, a first surfactant, a second surfactant, and an aqueous medium, The first surfactant is a compound represented by the following general formula (S1): The second surfactant is a compound represented by the following general formula (S2): The ink-jet ink, wherein the aqueous medium has an octanol / water partition coefficient Log P of -0.52 or more and -0.19 or less. 【Chemistry 1】 (In the general formula (S1), R 1 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 2 represents an alkyl group having 1 to 4 carbon atoms, n represents an integer of 2 to 5, In the general formula (S2), m represents an integer of 12 or more and 20 or less.
2. The ink-jet ink according to claim 1 , wherein a content of the first surfactant is from 0.01% by mass to 3.00% by mass.
3. The ink-jet ink according to claim 1 , wherein a content of the second surfactant is from 0.01% by mass to 2.00% by mass.
4. 3. The ink-jet ink according to claim 1, wherein the first surfactant is a compound represented by the following chemical formula (S1-1) or a compound represented by the following chemical formula (S1-2). 【Chemistry 2】
5. The ink-jet ink according to claim 1 or 2, wherein in formula (S2), m represents 14, 16 or 18.
6. The aqueous medium contains water and a water-soluble organic solvent, the water-soluble organic solvent is a first mixed solvent, a second mixed solvent, a third mixed solvent, or a fourth mixed solvent; the first mixed solvent contains only 3-methyl-1,3-butanediol, 1,2-pentanediol, propylene glycol, and triethylene glycol monobutyl ether; the second mixed solvent contains only 3-methyl-1,3-butanediol, 1,2-pentanediol, propylene glycol, triethylene glycol monobutyl ether, and 1,3-propanediol; the third mixed solvent contains only 1,2-pentanediol, propylene glycol, triethylene glycol monobutyl ether, 3-methyl-1,5-pentanediol, and 1,3-butanediol; 3. The ink-jet ink according to claim 1, wherein the fourth mixed solvent contains only 1,2-pentanediol, propylene glycol, triethylene glycol monobutyl ether, and 3-methyl-1,5-pentanediol.
Citation Information
Patent Citations
Ink for inkjet recording and recording method
JP2013231107A