Polyester recovery method and polyester chemical recycling method
The method of heat-treating polyester with acidic treatment liquid and separation effectively addresses the challenge of separating hydrolyzable nitrogen-containing resins, enhancing productivity and quality in polyester recycling.
Patent Information
- Application Number
- JP2023103289
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-04
- Filing Date
- 2023-06-23
- Publication Date
- 2024-10-17
AI Technical Summary
Existing methods for recycling polyester are hindered by the difficulty in separating hydrolyzable nitrogen-containing resins such as nylon or polyurethane, which cause molecular weight decrease and quality deterioration during the recycling process, making it challenging to produce high-quality recycled polyester.
A method involving heat-treating a mixture of polyester and hydrolyzable nitrogen-containing resin with an acidic treatment liquid, followed by separation and depolymerization, using sulfuric acid, hydrochloric acid, or phosphoric acid to effectively remove the nitrogen-containing resin.
This method enables industrial-scale, cost-effective separation of hydrolyzable nitrogen-containing resins from polyester, resulting in high-quality recycled polyester production.
Smart Images

Figure 2024148127000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for recovering polyester, a method for chemically recycling polyester, and the like. [Background technology]
[0002] Traditionally, polyester (e.g., polyethylene terephthalate (PET)) has been widely used as fibers, films, clothing, resins, etc., due to its excellent properties. Due to the large amount of polyester used, the development of recycling technologies has been actively considered in recent years. In particular, chemical recycling, in which polyester is regenerated under basic conditions to the state of polyester monomers (e.g., bis(2-hydroxyethyl) terephthalate, dimethyl terephthalate, etc.) and then polycondensed again to produce recycled polyester, is known as a method for obtaining high-quality recycled polyester, and its application to recycled fibers, recycled bottles, recycled films, recycled containers, recycled rags, recycled automotive interior materials, etc. is being considered.
[0003] To obtain high-quality recycled polyester by chemical recycling, it is necessary to separate various additives such as coloring pigments, dyes, stabilizers, and antistatic agents, different materials such as nylon, urethane, cotton, and polyolefin, and other components from various recovered products. Here, low-molecular-weight components such as coloring pigments can be removed by washing with a cleaning solution or solvent, and non-hydrolyzable different materials such as cotton can be removed as solids by filtration when polyester is depolymerized to regenerate liquid polyester monomer (see Patent Documents 1 to 3).
[0004] In this specification, the polyester monomer refers to a dicarboxylic acid such as terephthalic acid or 2,6-naphthalenedicarboxylic acid obtained by alcoholysis or hydrolysis of a polyester, or an ester thereof. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-104847 A [Patent Document 2] JP 2019-104861 A [Patent Document 3] JP 2007-045874 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, if the recycled material containing polyester contains hydrolyzable nitrogen-containing resins such as nylon and urethane, the resins may be reduced in molecular weight during the regeneration process to obtain polyester monomers, making it difficult to separate them from the polyester monomers, or may cause quality degradation such as coloring, making it difficult to obtain high-quality recycled polyester. In order to avoid this, it is necessary to pre-sort and separate the hydrolyzable nitrogen-containing resins from the recycled material containing polyester before chemical recycling. Conventionally, such sorting and separation have been physically performed by manual visual inspection, but this requires a great deal of effort and cost, and improvements have been required.
[0007] Moreover, in recent years, there has been an increase in products in which polyester and hydrolyzable nitrogen-containing resins are composited in a form that is difficult to physically separate and sort. Examples of such products include blended yarns of polyester and polyurethane, laminated films of PET layers and gas-barrier nylon layers, etc. Therefore, there is a demand for the development of an industrially simple method for removing hydrolyzable nitrogen-containing resins contaminated in mixtures containing polyester, and there is a particularly strong demand for a method for removing hydrolyzable nitrogen-containing resins that have a large impact on the coloring of recycled polyester.
[0008] The present invention has been made in view of the above problems. An object of the present invention is to provide a method for recovering polyester, which is capable of industrially and easily separating a hydrolyzable nitrogen-containing resin from a mixture containing a polyester and a hydrolyzable nitrogen-containing resin, and is excellent in productivity and economy, and a chemical recycling method for polyester, which is capable of producing high-quality recycled polyester, and is excellent in productivity and economy, and the like. [Means for solving the problem]
[0009] As a result of intensive research aimed at solving the above problems, the present inventors have found that the above problems can be solved by heat-treating a mixture containing a polyester and a hydrolyzable nitrogen-containing resin with an acidic treatment solution, and have thus completed the present invention. That is, the present invention provides various specific embodiments as shown below.
[0010] <1> A step of impregnating a mixture containing a polyester and a hydrolyzable nitrogen-containing resin with an acidic treatment liquid to obtain an impregnated treatment mixture; heating the impregnation mixture to 50° C. or higher; and separating the polyester and the liquid component of the hydrolyzable nitrogen-containing resin from the impregnation treatment mixture. Methods for recovering polyester.
[0011] <2> The acid treatment liquid contains at least one selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid. <1> 2. The method for recovering polyester according to claim 1 .
[0012] <3> The mixture contains, relative to 100 parts by mass of the mixture, 50 parts by mass or more and 99 parts by mass or less of the polyester and 1 part by mass or more and 40 parts by mass or less of the hydrolyzable nitrogen-containing resin. <1> or <2> 2. The method for recovering polyester according to claim 1 .
[0013] <4> The hydrolyzable nitrogen-containing resin includes at least one selected from the group consisting of nylon and polyurethane. <1> ~ <3> 13. The method for recovering polyester according to claim 12.
[0014] <5> The mixture includes one or more selected from the group consisting of fibers, fiber-reinforced resins, bottles, containers, films, and multilayer films; The polyester is included in one or more selected from the group consisting of a fiber, a fiber-reinforced resin, a bottle, a container, a film, and a multilayer film; The hydrolyzable nitrogen-containing resin is contained in one or more selected from the group consisting of fibers, fiber-reinforced resins, bottles, containers, films, and multilayer films. <1> ~ <4> 13. The method for recovering polyester according to claim 12.
[0015] <6> In the heating step, the impregnation mixture is heated to less than 150° C. <1> ~ <5> 13. The method for recovering polyester according to claim 12.
[0016] <7> In the heating step, the acidic treatment liquid is caused to flow through the mixture. <1> ~ <6> 13. The method for recovering polyester according to claim 12.
[0017] <8> The method further comprises a step of washing the polyester obtained by separating the liquid component with the acidic treatment liquid or water at a temperature of 50° C. or higher. <1> ~ <7> 13. The method for recovering polyester according to claim 12.
[0018] <9> A step of impregnating a mixture containing a polyester and a hydrolyzable nitrogen-containing resin with an acidic treatment liquid to obtain an impregnation treatment mixture; heating the impregnation mixture to 50° C. or higher; separating the polyester and the liquid component of the hydrolyzable nitrogen-containing resin from the impregnation treatment mixture; and a step of obtaining a polyester monomer by depolymerization using the polyester obtained by separating the liquid component as a depolymerization raw material. Chemical recycling methods for polyester. Here, the above <9> The polyester chemical recycling method described in <2> ~ <8> It is preferable that the present invention further has the technical features described in any one of the above. Effect of the Invention
[0019] According to the present invention, it is possible to easily separate the hydrolyzable nitrogen-containing resin from a mixture containing a polyester and a hydrolyzable nitrogen-containing resin on an industrial scale, thereby improving productivity and economic efficiency, and as a result, making it possible to produce a high-quality recycled polyester. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a flow chart showing a method for recovering polyester according to one embodiment and a method for chemically recycling polyester according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. However, the following embodiments are merely examples for explaining the present invention, and the present invention is not limited thereto. That is, the present invention can be practiced with any modifications within the scope of the gist of the present invention. In this specification, for example, the expression of a numerical range such as "1 to 100" includes both the lower limit "1" and the upper limit "100". The same applies to the expression of other numerical ranges.
[0022] [Polyester recovery method] Fig. 1 is a flow chart showing the polyester recovery method and the polyester chemical recycling method of this embodiment. The polyester recovery method of this embodiment includes at least a step (S12) of impregnating a mixture containing polyester and hydrolyzable nitrogen-containing resin with an acidic treatment liquid to obtain an impregnation treatment mixture, a step (S13) of heating the impregnation treatment mixture to 50°C or higher, and a step (S14) of separating the polyester and the liquid component of the hydrolyzable nitrogen-containing resin from the impregnation treatment mixture. Each step will be described in detail below.
[0023] <Preparation step of impregnation treatment mixture (S12)> In this step S12, the mixture containing the polyester and the hydrolyzable nitrogen-containing resin is impregnated with an acidic treatment liquid to obtain an impregnated treatment mixture. The mixture put into the acidic treatment liquid may take various forms. Examples include, but are not limited to, fibers, fiber-reinforced resins, bottles, containers, films, and multilayer films. The mixture put into the acidic treatment liquid may be any combination and ratio of two or more types selected from these forms.
[0024] In this specification, polyester means a material having an ester bond formed by dehydration condensation of a polycarboxylic acid and a polyol; an ester bond formed by dehydration condensation of a hydroxycarboxylic acid; an ester bond formed by dehydration condensation of a combination of these; or an ester exchange reaction of a polycarboxylic acid. Specific examples of polyester include polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), polybutylene naphthalate (PBN), glycol-modified polyethylene terephthalate (PETG), polyethylene succinate (PES), polybutylene succinate (PBS), polylactic acid, polyglycolic acid, polycaprolactone, and polyhydroxyalkanoate, but are not limited thereto. These may be used alone or in any combination and ratio of two or more.
[0025] In this specification, the hydrolyzable resin means a resin having a bond that can be hydrolyzed. The bond that can be hydrolyzed is not particularly limited, but includes a urethane bond, an amide bond, a carbonate bond, an ester bond, etc., and these are divided into resins that contain nitrogen and resins that do not contain nitrogen. In this specification, a hydrolyzable resin that contains nitrogen is referred to as a hydrolyzable nitrogen-containing resin, and a hydrolyzable resin other than polyester that does not contain nitrogen is referred to as a hydrolyzable nitrogen-free resin.
[0026] The hydrolyzable nitrogen-containing resin means a resin having a nitrogen-containing bond (nitrogen-containing repeating unit). The nitrogen-containing bond is not particularly limited, but may be a urethane bond (-O-CO-NH- bond) or an amide bond (-CO-NR- bond, where R is a hydrogen atom or any substituent, preferably an alkyl group). The hydrolyzable nitrogen-containing resin is not particularly limited, but may be polyurethane or nylon. Specific examples of hydrolyzable nitrogen-containing resins include polyurethane elastic fibers (spandex, elastane) obtained by polyaddition of polyisocyanate and polyol, nylon 6, nylon MXD6, nylon 6,6, nylon 6,6,6, nylon 7, nylon 8, nylon 9, nylon 10, nylon 11, nylon 12, nylon 6,10, nylon 10,10, nylon 6,9, nylon 4,6, nylon 4,10, nylon 5,6, nylon 5,10, nylon 6I, nylon 6T, nylon 6I / 6T, nylon 6-3-T, nylon 6 / MXDI, nylon 6 / 6I, polyamide 4, polyamide 6, and polyamide 7. Amide 10, polyamide 11, polyamide 12, polyamide 4,6, polyamide 6,6, polyamide 6,10, polyamide 6T, polyamide 9T, polyamide 6IT, polymetaxylylene adipamide (polyamide MXD6), isophthalic acid copolymerized polymetaxylylene adipamide (polyamide MXD6I), polymetaxylylene sebacamide (polyamide MXD10), polymetaxylylene dodecanamide (polyamide MXD12), poly 1,3-bisaminocyclohexane adipamide (polyamide BAC6), polyparaxylylene sebacamide (polyamide PXD10), etc. are included, but are not particularly limited thereto. These can be used alone or in any combination and ratio of two or more. It is more preferable that the hydrolyzable nitrogen-containing resin essentially contains polyurethane. The number of products using composite materials (e.g., blended fibers, etc.) containing polyester and polyurethane as a hydrolyzable nitrogen-containing resin is increasing, and the method of this embodiment has extremely high industrial utility value in that it is possible to easily separate polyester and polyurethane from such composite materials. In this case, nylon may or may not be further contained.
[0027] The polyester and the hydrolyzable nitrogen-containing resin may be contained in the mixture, and the mixed form is not particularly limited. For example, the polyester may be contained in any one of fibers, fiber-reinforced resins, bottles, containers, films, multilayer films, etc., or may be contained in two or more of these. Similarly, the hydrolyzable nitrogen-containing resin may be contained in any one of fibers, fiber-reinforced resins, bottles, containers, films, multilayer films, etc., or may be contained in two or more of these. In addition, the polyester and the hydrolyzable nitrogen-containing resin may be contained in the mixture as fibers such as blended yarns, blended yarns, and composite yarns, may be contained in the mixture as laminated films such as woven fabrics, woven cloths, and nonwoven cloths, or may be contained in the mixture as two-color molded bodies or multi-color molded bodies.
[0028] The content ratio in the mixture can be appropriately set in consideration of the composition of the recovered polyester, and is not particularly limited, but from the viewpoint of obtaining high-quality recycled polyester, it is preferable that the polyester is 50 parts by mass or more and 99 parts by mass or less, and the hydrolyzable nitrogen-containing resin is 1 part by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the mixture. More preferably, the polyester is 75 parts by mass or more and 99 parts by mass or less, and the hydrolyzable nitrogen-containing resin is 1 part by mass or more and 25 parts by mass or less, relative to 100 parts by mass of the mixture. Even more preferably, the polyester is 90 parts by mass or more and 99 parts by mass or less, and the hydrolyzable nitrogen-containing resin is 1 part by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the mixture.
[0029] The mixture may contain a hydrolyzable nitrogen-free resin other than polyester. The content of the hydrolyzable nitrogen-free resin is not particularly limited, but is preferably less than 8% by mass, more preferably less than 5% by mass, more preferably less than 3% by mass, and even more preferably less than 1% by mass, based on 100 parts by mass of the mixture. Specific examples of the hydrolyzable nitrogen-free resin include, but are not limited to, cotton, poly(meth)acrylic acid ester, acrylic, acetate, rayon, cupra, polycarbonate, etc.
[0030] The mixture may contain components other than the polyester and the hydrolyzable resin (hereinafter, these may be referred to as "impurity components"). The content of the impurity components is not particularly limited, but from the viewpoint of obtaining high-quality recycled polyester, it is preferably less than 50% by mass, more preferably less than 40% by mass, even more preferably less than 35% by mass, even more preferably less than 10% by mass, particularly preferably less than 5% by mass, and most preferably less than 1% by mass, relative to 100 parts by mass of the mixture. It goes without saying that the lower limit is 0% by mass or more. Examples of impurity components include, but are not limited to, fiber materials other than polyester and hydrolyzable resin (e.g., cotton, rayon, hemp, silk, wool, etc.), resin materials other than polyester and hydrolyzable resin (polyolefin, polyvinyl alcohol, polystyrene, etc.), metals, paper, inorganic fillers, higher fatty acids, higher fatty acid esters, higher fatty acid amides, higher fatty acid metal salts, polysiloxanes, fluororesins, and other release improvers; colorants such as dyes and pigments; organic fillers; antioxidants; heat stabilizers; light stabilizers; ultraviolet absorbers; flame retardants; antistatic agents; surfactants; rust inhibitors; defoamers; fluorescent agents, surface finishing agents, etc. Note that cellulose such as cotton and rayon, acrylic, hemp, silk, wool, etc., as impurity components, can be pulverized by an acid treatment solution or solubilized by a chemical reaction, etc., so that when the method of this embodiment is applied, these can be separated as fine powder or liquid components. Therefore, the method of the present embodiment has extremely high industrial utility even when separating a mixture containing a hydrolyzable nitrogen-free resin, polyester, and polyurethane into a hydrolyzable nitrogen-free resin such as cotton, rayon, or cellulose such as hemp, an acrylic, silk, or wool, a polyester, and a polyurethane.
[0031] The acid treatment liquid is impregnated into the mixture described above to make it possible to separate the polyester and the hydrolyzable nitrogen-containing resin. The acid treatment liquid is not particularly limited, but a solution containing an inorganic acid such as sulfuric acid, hydrochloric acid, nitric acid, or phosphoric acid is preferably used from the viewpoint of solubility and liquefaction of the hydrolyzable nitrogen-containing resin. Among these, nitric acid and phosphoric acid are more preferable from the viewpoint of low corrosiveness, and phosphoric acid is particularly preferable. In particular, phosphoric acid, unlike hydrochloric acid, can separate polyester and polyurethane, and can also separate hydrolyzable nitrogen-free resins such as cellulose such as cotton and rayon, acrylic, and wool. Therefore, the method of the present embodiment has extremely high industrial utility value when separating a mixture containing a hydrolyzable nitrogen-free resin, polyester, and polyurethane into a hydrolyzable nitrogen-free resin such as cellulose such as cotton and rayon, acrylic, hemp, silk, and wool, polyester, and polyurethane. In addition, the solvent for the inorganic acid is not particularly limited, but water, methanol, ethanol, isopropyl alcohol, or a mixture thereof is preferable, and from the viewpoint of solubility and economic efficiency, an aqueous solvent containing at least water is more preferable, and water is even more preferable. The concentration of the acid treatment solution is preferably 40% or more, although it varies depending on the type of acid used. For example, in the case of sulfuric acid, the acid concentration is preferably 40% or more, more preferably 45% or more, and although the upper limit is not particularly limited, it is preferably 80% or less, more preferably 70% or less. In the case of phosphoric acid, the acid concentration is more preferably 50% or more, even more preferably 60% or more, and although the upper limit is not particularly limited, it is preferably 90% or less, more preferably 85% or less. In the case of nitric acid, the acid concentration is more preferably 45% or more, even more preferably 55% or more, and although the upper limit is not particularly limited, it is preferably 75% or less, more preferably 70% or less.
[0032] The method of impregnating the mixture with the acidic treatment liquid may be any method and is not particularly limited. For example, the acidic treatment liquid may be sprayed or applied to the mixture. From the viewpoints of solubility and economy, a method of immersing the mixture in a bath of the acidic treatment liquid is preferred. By impregnating the mixture containing the polyester and the hydrolyzable nitrogen-containing resin with the acidic treatment liquid, an impregnated treatment mixture can be obtained.
[0033] It is preferable to have a step S12a of crushing or cutting the mixture prior to preparation of the impregnation treatment mixture. By crushing or cutting the mixture in this way, the volume of the mixture can be reduced, and the treated surface area increases, which tends to promote decomposition or liquefaction of the hydrolyzable nitrogen-containing resin. The crushing or cutting of the mixture can be performed using a known method. In this case, known processing devices such as a crusher, ball mill, bead mill, flake crusher, hammer mill, pin mill, bantam mill, jet mill, cyclone mill, fret mill, pan mill, edge runner, roller mill, mix miller, vibration mill, sample mill, raikaiki, cutter, shredder, air cutter, cutter, etc. can also be used.
[0034] In addition, prior to preparation of the impregnation treatment mixture, before crushing or impregnation of the mixture, or after crushing or impregnation, an elution treatment S12b may be performed to extract impurities such as disperse dyes and halogen atoms from the mixture with a solvent. By performing this solvent extraction treatment in advance, it is possible to produce a higher quality recycled polyester. In the solvent extraction treatment, known solvents such as methylene chloride, xylene, and alkylene glycol can be used. In addition, the treatment temperature is not particularly limited, and the optimal temperature varies depending on the type of extraction solvent used, but is preferably 120°C to 210°C, and more preferably 120°C to 180°C. The solvent extraction treatment may be either a batch type or a countercurrent continuous type.
[0035] <Heating step of impregnation treatment mixture (S13)> In this step S13, the impregnation mixture obtained as described above is heated to 50°C or higher. In this method, the hydrolyzable nitrogen-containing resin in the mixture can be decomposed or liquefied at a relatively low temperature. The heat treatment temperature at this time is not particularly limited as long as it is 50°C or higher, but from the viewpoints of productivity and economy, it is more preferably 60°C or higher, even more preferably 70°C or higher, and most preferably 80°C or higher. The upper limit of the heat treatment temperature is not particularly limited, but from the viewpoints of productivity and economy, it is preferably less than 150°C, more preferably less than 140°C, even more preferably less than 130°C, and particularly preferably 120°C. In addition, the heat treatment time at this time is not particularly limited, but from the viewpoints of productivity and economy, it is preferably 48 hours or less, more preferably 12 hours or less, even more preferably 6 hours or less, and most preferably 3 hours or less. The heat treatment of the impregnation mixture may be either a batch type or a countercurrent continuous type.
[0036] In order to promote the decomposition or liquefaction of the hydrolyzable nitrogen-containing resin and to improve productivity and economy, it is preferable to heat the impregnation mixture while immersing the mixture in a bath of the acidic treatment liquid and flowing the acidic treatment liquid through the mixture. The method of flowing the treatment liquid can be carried out using a known method such as a stirring blade. The rotation speed of the stirring blade is not particularly limited, but is preferably 10 to 150 rpm.
[0037] After the heat treatment of the impregnation mixture, for example, a washing treatment S13a may be performed as necessary. The washing treatment may be performed based on a conventional method, and the type is not particularly limited. When the heat treatment is performed using an aqueous solution of an inorganic acid, it is preferable to perform a water washing treatment from the viewpoints of removing the inorganic acid and cooling.
[0038] The mechanism by which the polyester remains solid while the hydrolyzable nitrogen-containing resin becomes partially or entirely liquid by the acid treatment at a relatively low temperature as described above is unclear, but since the hydrolyzable nitrogen-containing resin hardly progresses in its molecular weight reduction, it is presumed that the hydrolyzable nitrogen-containing resin has a low Tg or is easily dispersible due to the addition of a large amount of acid (Tg: glass transition temperature). However, the function of the present invention is not limited to these presumptions.
[0039] <Polyester separation process (S14)> In this step S14, the polyester is separated from the impregnation mixture after the heat treatment. The impregnation mixture after the heat treatment contains, in addition to the polyester, liquid components of hydrolyzable nitrogen-containing resin, and liquid components or fine powder of impurity components. Therefore, by removing the liquid components and fine powder from the impregnation mixture after the heat treatment, a polyester with reduced hydrolyzable nitrogen-containing resin can be obtained. At this time, known solid-liquid separation methods such as pressure filtration using a pressure filter or nitrogen gas, vacuum suction filtration, and centrifugal separation can be applied.
[0040] In this specification, the polyester obtained after the polyester separation step (S14) refers to a solid component containing polyester recovered from the impregnation treatment mixture. This solid component is not particularly limited, but may contain polyester and hydrolyzable non-nitrogen-containing resin and / or impurity components. These hydrolyzable non-nitrogen-containing resin and / or impurity components can be separated from polyester as liquid components or fine powders by applying a known solid-liquid separation method such as pressure filtration using a pressure filter or nitrogen gas, vacuum suction filtration, and centrifugation.
[0041] In this polyester separation step, in order to prevent recontamination of the mixed components present in a liquid state, the separation operation is preferably carried out at 50° C. or higher, more preferably 60° C. or higher, even more preferably 70° C. or higher, particularly preferably 80° C. or higher, and most preferably 90° C. or higher. The upper limit of the treatment temperature is not particularly limited, but from the viewpoints of productivity and economy, it is preferably less than 150° C., more preferably less than 140° C., even more preferably less than 130° C., and particularly preferably less than 120° C. For the same reason, when performing solid-liquid separation such as filtration or centrifugation, it is preferable to perform hot filtration, and in that case, it is preferable to wash with water or the above-mentioned acid treatment liquid under a temperature condition of 50° C. or higher as described above.
[0042] After the polyester separation step, a washing treatment S14a and / or a drying treatment may be performed as necessary. The washing treatment may be performed based on a conventional method, and the type is not particularly limited. When the separation operation is performed using water or an acidic treatment liquid, a water washing treatment is preferable from the viewpoint of removing inorganic acid. Then, if necessary, the washed polyester may be subjected to a drying treatment at 50°C or more and 150°C or less as necessary.
[0043] The polyester thus obtained has a particularly reduced content of hydrolyzable nitrogen-containing resin, and is industrially important as a raw material for recycled polyester. The content of polyester in the obtained polyester can be appropriately set according to the desired performance, and is not particularly limited, but is preferably 70 parts by mass or more, more preferably 80 parts by mass or more, and even more preferably 90 parts by mass or more, relative to a total of 100 parts by mass. The content of components other than polyester can be appropriately set according to the desired performance, and is not particularly limited, but is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, relative to a total of 100 parts by mass.
[0044] [Chemical recycling method for polyester] In addition, the polyester chemical recycling method of this embodiment uses the polyester obtained by the above-mentioned polyester recovery method as a depolymerization raw material and performs depolymerization to obtain a polyester monomer. That is, the polyester chemical recycling method of this embodiment includes at least a step (S12) of impregnating a mixture containing a polyester and a hydrolyzable nitrogen-containing resin with an acidic treatment liquid to obtain an impregnation treatment mixture, a step (S13) of heating the impregnation treatment mixture to 50°C or higher, a step (S14) of separating the polyester and the liquid component of the hydrolyzable nitrogen-containing resin from the impregnation treatment mixture, and a step (S21) of depolymerizing the polyester as a depolymerization raw material to obtain a polyester monomer. Steps S12 to S14 have already been described, so duplicated descriptions will be omitted, and step S21 will be described in detail below.
[0045] <Polyester depolymerization step (S21)> In this step S21, the polyester obtained as described above is used as a raw material for recycled polyester, i.e., as a raw material for depolymerization, and the polyester is depolymerized to obtain a polyester monomer.
[0046] The depolymerization of polyester can be carried out by any known method, and is not particularly limited. For example, known methods such as a method of reacting an alcohol under acid or alkaline conditions, a method of transesterification with methanol in the presence of a transesterification catalyst, a method of reacting an amine compound in the presence of a catalyst, a method of reacting a supercritical or subcritical fluid (water or methanol), and a method of hydrolysis in the presence of an enzyme can be applied. After the depolymerization step of polyester, terephthalic acid, dimethyl terephthalate, alkylene glycol, etc. can be purified by a purification method such as distillation, crystallization, and activated carbon treatment to obtain high-purity products.
[0047] As described above in detail, according to the polyester recovery method of the present embodiment, it is possible to easily separate the polyester and the hydrolyzable nitrogen-containing resin from a mixture containing the polyester and the hydrolyzable nitrogen-containing resin on an industrial scale, and it is possible to save a great deal of effort and cost compared to the conventional technology. Therefore, the polyester recovery method of the present embodiment is excellent in productivity and economy on an industrial scale. And, by chemically recycling the polyester (recovered polyester) with reduced hydrolyzable nitrogen-containing resin in this way, it is possible to obtain high-quality regenerated polyester with excellent productivity and economy. EXAMPLES
[0048] The features of the present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. That is, the materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. In addition, the values of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limits in the embodiment of the present invention, and the preferred numerical range may be a range defined by a combination of the above-mentioned upper or lower limit and the values of the following examples or the values of the examples.
[0049] Example 1 2.0 g of polyester and polyurethane blended fiber (manufactured by AEON Co., Ltd., product number TV158SA3302C, polyester 90% by mass, polyurethane 10% by mass) was weighed and placed in a glass flask together with a stirrer. Next, 10 mL of 75% phosphoric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., food additive grade) was weighed with a measuring cylinder and placed in the glass flask to obtain an impregnation treatment mixture. After that, the glass flask was heated in an oil bath set at 110 ° C. and stirred for 180 minutes, and the flask contents became a cloudy liquid containing polyester-containing solids. After the heat treatment was completed, the flask contents were filtered while hot, washed with ultrapure water at room temperature, and the solids were collected by filtration. The collected solids were air-dried overnight, and then dried in a dryer set at 80 ° C. for 2 hours, and the mass of the polyester-containing solids after drying was measured. Table 1 shows the ratio (%) of the mass of the polyester-containing solids after drying to the mass of the blended fiber before addition.
[0050] Example 2 The treatment was carried out in the same manner as in Example 1, except that the blended fiber used was changed to 2.0 g of a blended fiber of polyester and polyurethane (manufactured by UNIQLO Co., Ltd., product number 444128, polyester 88 mass%, polyurethane 12 mass%). The flask contents after heating were a cloudy white liquid containing polyester-containing solids. The ratio (%) of the mass of the polyester-containing solids after drying to the mass of the blended fiber before addition is shown in Table 1.
[0051] (Examples 3 to 5) The treatment was carried out in the same manner as in Example 1, except that the treatment conditions were changed as shown in Table 1. However, in Examples 4 and 5, the flask contents were filtered while hot after the heat treatment was completed, washed with phosphoric acid at 80°C, and then washed with ultrapure water at 80°C to filter and recover the solid content. The flask contents after heating were a cloudy white liquid containing polyester-containing solid content. The ratio (%) of the mass of the polyester-containing solid content after drying to the mass of the blended fibers before addition is shown in Table 1.
[0052] Example 6 The treatment was carried out in the same manner as in Example 1, except that a three-layer laminate film (PET / MX nylon / PET, containing 5% by mass of MX nylon, MX nylon is polyamide MXD6 resin manufactured by Mitsubishi Gas Chemical Company, Inc.) was used instead of the blended fiber, and the treatment conditions were changed to those shown in Table 1. The flask contents after heating were a cloudy white liquid containing polyester-containing solids. The ratio (%) of the mass of the polyester-containing solids after drying to the mass of the three-layer laminate film before addition is shown in Table 1.
[0053] Comparative Example 1 The treatment was carried out in the same manner as in Example 1, except that 2.0 g of polyester white cloth (attached white cloth for dye fastness test, compliant with JIS L0803) was used instead of the blended fiber, and the treatment conditions were changed to those shown in Table 1. The flask contents after heating were a colorless, transparent liquid containing the polyester white cloth in the same shape as when it was added. The ratio (%) of the mass of the solid content recovered after drying to the mass of the polyester white cloth before addition is shown in Table 1.
[0054] Comparative Example 2 The treatment was carried out in the same manner as in Comparative Example 1, except that 1.0 g of polyurethane yarn (Lycra, T-127, manufactured by Toray Opelontech Co., Ltd.) was used instead of the blended fiber and the treatment conditions were changed to those shown in Table 1. After heating, the content of the flask was a colorless, transparent liquid containing a swollen solid.
[0055] Comparative Example 3 The treatment was carried out in the same manner as in Example 1, except that 2.0 g of polyester white cloth (attached white cloth for dye fastness test, compliant with JIS L0803) was used instead of the blended fiber, and the treatment conditions were changed to those shown in Table 1. The flask contents after heating were a colorless, transparent liquid containing the polyester white cloth in the same shape as when it was added. The ratio (%) of the mass of the solid content recovered after drying to the mass of the polyester white cloth before addition is shown in Table 1.
[0056] Comparative Example 4 The treatment was carried out in the same manner as in Comparative Example 3, except that 1.0 g of polyurethane yarn (Lycra, T-127, manufactured by Toray Opelontech Co., Ltd.) was used instead of the blended fiber and the treatment conditions were changed to those shown in Table 1. The flask contents after heating were a colorless, transparent liquid containing polyurethane yarn that maintained the shape before it was added. The ratio (%) of the mass of the solid content recovered after drying to the mass of the polyurethane yarn before it was added is shown in Table 1.
[0057] [Table 1]
[0058] As is clear from Table 1, it was confirmed that polyurethane, which is a hydrolyzable nitrogen-containing resin, can be liquefied and removed from blended fibers of polyester and polyurethane by various acid treatments. Also, as is clear from Comparative Examples 1 and 4, it was confirmed that polyurethane (Lycra) could hardly be removed by acid treatment using acetic acid or hydrochloric acid.
[0059] Next, in order to know the behavior of the treatment performance of each resin alone, the following experiment was carried out.
[0060] (Reference example 1) The treatment was carried out in the same manner as in Example 1, except that 2 g of polyester white cloth (attached white cloth for dye fastness test, compliant with JIS L0803) was used instead of the blended fiber and the treatment conditions were changed to those shown in Table 2. The flask contents after heating were a colorless, transparent liquid containing the polyester white cloth in the same shape as when it was added. The ratio (%) of the mass of the solid content recovered after drying to the mass of the polyester white cloth before addition is shown in Table 2.
[0061] (Reference examples 2~18) The treatment was carried out in the same manner as in Reference Example 1, except that the resins (white nylon cloth (white cloth attached for dye fastness test, compliant with JIS L0803), nylon pellets (Sigma-Aldrich, product number 181110), MX nylon pellets (Mitsubishi Gas Chemical Company, Inc., polyamide MXD6 resin, S6000 series)) and treatment conditions were changed as shown in Table 2. The ratio (%) of the mass of the solid content recovered after drying to the mass of the resin before addition is shown in Table 2.
[0062] Table 2 shows the treatment conditions and the measurement results. [Table 2]
[0063] As is clear from Table 2, it was confirmed that polyester could hardly be removed by various acid treatments. On the other hand, it was confirmed that hydrolyzable nitrogen-containing resin could be liquefied and removed by a specific acid treatment. In addition, as is clear from Reference Examples 15 and 18, it was confirmed that polyurethane (Lycra) could hardly be removed by acid treatment using acetic acid or hydrochloric acid.
[0064] Example 7 1.01 g of a blended fiber of polyester, acrylic, rayon and polyurethane (manufactured by Uniqlo Co., Ltd., product number 450528, polyester 39 mass%, polyurethane 8 mass%, rayon 21 mass%, acrylic 32 mass%) was weighed and placed in a glass vial together with a stirrer. Next, 30 mL of 85% phosphoric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent) was weighed with a measuring cylinder and placed in the glass vial to obtain an impregnation treatment mixture. After that, the glass vial was heated in a water bath set at 90 ° C. and stirred for 180 minutes, and the vial contents became a mixture containing polyester-containing solids. After the heat treatment was completed, the vial contents were hot filtered through a 60 mesh PTFE mesh with a mesh size of 0.2 mm, washed with 85% phosphoric acid at 80 ° C., and then further washed with ultrapure water at 80 ° C. to filter and recover the fibrous solids. The collected filamentous solid was air-dried overnight, and then dried for 2 hours in a dryer set at 80° C., and the mass of the polyester-containing filamentous solid after drying was measured. Table 3 shows the ratio (%) of the mass of the polyester-containing filamentous solid after drying to the mass of the blended fiber before addition, and the ratio (%) of the difference between the mass of the blended fiber before addition and the mass of the polyester-containing filamentous solid after drying to the total mass of impurities contained in the blended fiber before addition.
[0065] Example 8 The treatment was carried out in the same manner as in Example 7, except that a glass flask was used instead of a glass vial, an oil bath was used instead of a water bath, and the treatment conditions were changed as shown in Table 3. Table 3 shows the ratio (%) of the mass of the polyester-containing fibrous solid content after drying to the mass of the blended fiber before addition, and the ratio (%) of the difference between the mass of the blended fiber before addition and the mass of the polyester-containing fibrous solid content after drying to the total mass of impurity components contained in the blended fiber before addition.
[0066] (Reference example 19) The treatment was carried out in the same manner as in Example 1, except that 2.07 g of white cotton cloth (attached white cloth for dye fastness test, compliant with JIS L0803) was used instead of the blended fiber, and the treatment conditions were changed to those shown in Table 3. The flask contents after heating were a yellow, transparent, homogeneous liquid. Table 3 shows the ratio (%) of the mass of the cloth recovered after drying to the mass of the white cotton cloth before addition.
[0067] (Reference examples 20~30) The treatment was carried out in the same manner as in Reference Example 1, except that the resins (white rayon cloth (Nishimura Shoji Shoten, Miyako crepe plain cut cloth, 100% by mass of rayon), white acrylic cloth (white cloth for dyeing test, acrylic muslin), white wool cloth (attached white cloth for dye fastness test, JIS L0803 compliant), polyester and cotton blended fiber (AEON Co., Ltd., product number TV2793A1233R, 55% by mass of cotton, 45% by mass of polyester) and treatment conditions shown in Table 3 were changed. Table 3 shows the ratio (%) of the mass of the resin recovered after drying to the mass of the resin before addition, and the ratio (%) of the difference between the mass of the resin before addition and the mass of the polyester-containing thread-like solid content after drying to the total mass of impurities contained in the resin before addition.
[0068] Table 3 shows the treatment conditions and the measurement results. [Table 3] [Industrial Applicability]
[0069] According to the present invention, it is possible to easily separate the polyester and the hydrolyzable nitrogen-containing resin from a mixture containing the polyester and the hydrolyzable nitrogen-containing resin on an industrial scale, thereby improving productivity and economic efficiency. As a result, it is possible to produce high-quality recycled polyester, and therefore the present invention can be widely and effectively used in the field of recycled polyester materials.
Claims
1. A step of impregnating a mixture containing a polyester and a hydrolyzable nitrogen-containing resin with an acidic treatment liquid to obtain an impregnated treatment mixture; heating the impregnation mixture to 50° C. or higher; and separating the polyester and the liquid component of the hydrolyzable nitrogen-containing resin from the impregnation treatment mixture. Methods for recovering polyester.
2. The acid treatment liquid contains at least one selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid. The method for recovering polyester according to claim 1.
3. The mixture contains, relative to 100 parts by mass of the mixture, 50 parts by mass or more and 99 parts by mass or less of the polyester and 1 part by mass or more and 40 parts by mass or less of the hydrolyzable nitrogen-containing resin. The method for recovering polyester according to claim 1.
4. The hydrolyzable nitrogen-containing resin includes at least one selected from the group consisting of nylon and polyurethane. The method for recovering polyester according to claim 1.
5. The mixture includes one or more selected from the group consisting of fibers, fiber-reinforced resins, bottles, containers, films, and multilayer films; The polyester is included in one or more selected from the group consisting of a fiber, a fiber-reinforced resin, a bottle, a container, a film, and a multilayer film; The hydrolyzable nitrogen-containing resin is included in one or more selected from the group consisting of fibers, fiber-reinforced resins, bottles, containers, films, and multilayer films. The method for recovering polyester according to claim 1.
6. In the heating step, the impregnation mixture is heated to less than 150° C. The method for recovering polyester according to claim 1.
7. In the heating step, the acidic treatment liquid is caused to flow through the mixture. The method for recovering polyester according to claim 1.
8. The method further comprises a step of washing the polyester obtained by separating the liquid component with the acidic treatment liquid or water at a temperature of 50° C. or higher. The method for recovering polyester according to claim 1.
9. A step of impregnating a mixture containing a polyester and a hydrolyzable nitrogen-containing resin with an acidic treatment liquid to obtain an impregnation treatment mixture; heating the impregnation mixture to 50° C. or higher; separating the polyester and the liquid component of the hydrolyzable nitrogen-containing resin from the impregnation treatment mixture; and a step of obtaining a polyester monomer by depolymerization using the polyester obtained by separating the liquid component as a depolymerization raw material. Chemical recycling methods for polyester.
Citation Information
Patent Citations
Method for recovering effective component from dyed polyester fiber
JP2007045874A
Reinforced-fiber recovery apparatus and method for using the same
JP2017104847A