Sustainable sound-absorbing nonwoven fabric

A nonwoven fabric using crushed fibers from textile waste, thermally bonded with core-sheath type binder fibers, addresses the challenges of non-uniformity and high weight in sustainable sound-absorbing materials, achieving high sound absorption and mechanical strength while reducing reliance on recycled PET.

JP2024148167AActive Publication Date: 2024-10-17CARL FREUDENBERG KG
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024060098
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-04
Filing Date
2024-04-03
Publication Date
2024-10-17
Estimated Expiration
2044-04-03

AI Technical Summary

Technical Problem

Existing sustainable sound-absorbing materials in the automotive industry face challenges with non-uniform appearance, low sound absorption capacity, and high basis weight, which contradicts the need for lightweight construction, and rely heavily on recycled PET fibers that may become scarce.

Method used

A sound-absorbing nonwoven fabric is developed using crushed framework staple fibers and core-sheath type binder fibers, thermally bonded to achieve good acoustic and mechanical properties without relying on r-PET fibers, utilizing a method that includes shredding textile waste to disrupt the structure and forming a nonwoven fabric through heat treatment.

Benefits of technology

The nonwoven fabric achieves a high flow resistance, sound absorption, and mechanical strength with a low basis weight, maintaining uniform appearance and sustainability by utilizing crushed fibers from textile waste, overcoming the limitations of recycled PET fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148167000001_ABST
    Figure 2024148167000001_ABST
Patent Text Reader

Abstract

To provide sustainable sound-absorbing nonwoven fabrics with a low area density, and a method for producing the same.SOLUTION: There is provided a thermally solidified sound-absorbing nonwoven fabric having a fluid resistance of 150 Ns / m3 to 5000 Ns / m3, measured in accordance with DIN EN 29053, May 1993, and an area density of 150 g / m2 to 600 g / m2. The nonwoven fabric includes c) structural staple fibers having a mean titer of 0.9 dtex to 8.8 dtex, in a proportion of 50 wt.-% to 90 wt.-% in relation to an overall weight of the nonwoven fabric, and d) core-sheath binding fibers in a proportion of 10 wt.-% to 50 wt.-% in relation to the overall weight of the nonwoven fabric. The structural staple fibers include a percentage of reprocessed structural staple fibers and the core-sheath binding fibers include a percentage of reprocessed core-sheath binding fibers.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sustainable sound absorbing nonwoven fabric with a low basis weight. The present invention further relates to a method for producing the same and to its use.

[0002] Sound absorbing nonwoven fabrics are used in a variety of applications. One important field of use is as sound absorbers in the automotive industry. EP 3246442 A1 states: a) at least one open-pore support layer comprising thick staple fibers having an average fineness of 3 dtex to 17 dtex and, as framework fibers, thin staple fibers having an average fineness of 0.3 dtex to 2.9 dtex, in particular 0.5 dtex to 2.9 dtex; b) a microporous flowable bed disposed on the support layer and including microfibers having a fiber diameter of less than 10 μm; The sound absorbing textile composite has a flow resistance of 250 Ns / m 3 ~5000Ns / m 3 , especially 250Ns / m 3 ~2000Ns / m 3 The support layer may contain sheath-core fibers as bonding fibers.

[0003] Advantageously, the sound absorbing material combines good acoustic properties with a low basis weight and is advantageously produced, at least in part, from sustainable resources.

[0004] One approach to producing sustainable sound absorbing materials is to use recycled fiber materials as raw materials. However, commercially available sound absorbing materials of this kind have a very uneven appearance. Furthermore, they generally have a low sound absorption capacity, usually weighing less than 600 g / m. 2 This runs counter to the increasing efforts to achieve desirable lightweight construction of automobiles.

[0005] Another approach is the use of r-PET fibers obtained from recycled PET bottles. This approach certainly allows the desired sound absorption to be achieved with lighter materials. However, since PET bottles will become an increasingly scarce resource in the future, other alternatives to sustainable fiber resources are needed to produce efficient sound absorbers. The object of the present invention is therefore to provide a sustainable sound absorber that does not require the use of r-PET fibers obtained from recycled PET bottles as a raw material source and has good acoustic and mechanical properties. A further object is to provide a method for producing said sound absorber and its use.

[0006] The challenge is to meet the 150 Ns / m2 load, measured according to DIN EN 29053, May 1993 edition. 3 ~5000Ns / m 3 , advantageously 150 Ns / m 3 ~3000Ns / m 3 , and even more preferably 150Ns / m 3 ~2000Ns / m 3 , especially 150Ns / m 3 ~1000Ns / m 3 and a flow resistance of 150g / m 2 ~600g / m 2 and a basis weight of the thermal bonded sound absorbing nonwoven fabric, the nonwoven fabric comprising: a) comprising 50% to 90% by weight, preferably 60% to 80% by weight, more preferably still 70% to 80% by weight, based on the total weight of the nonwoven fabric, of framework staple fibers having an average fineness of 0.9 dtex to 8.8 dtex, advantageously 0.9 dtex to 6.7 dtex, in particular 0.9 dtex to 3.3 dtex, and b) the nonwoven fabric contains core-sheath type binder fibers in an amount of 10% by weight to 50% by weight, preferably 20% by weight to 40% by weight, and more preferably 20% by weight to 30% by weight, based on the total weight of the nonwoven fabric; The problem is solved by a thermally bonded sound absorbing nonwoven fabric, in which the framework staple fibers include a proportion of chopped framework staple fibers, and the sheath-core binder fibers include a proportion of chopped sheath-core binder fibers.

[0007] It was found that the nonwoven fabric according to the invention has very good acoustic and mechanical properties, despite the proportion of chopped fibers. Chopped fibers are fibers obtained in a mechanical process (chopping) to break down the structure of textile waste. The observed good acoustic and mechanical properties were surprising, since usually the fibers are subjected to very high mechanical stresses in the chopping process, which results in partial destruction. In addition, the chopped fibers contained in the nonwoven fabrics of the prior art have a wide range of different fiber lengths, with a proportion of short fibers and a proportion of unbroken thread-like or sheet-like material pieces. This results in a strong change in the property profile compared to the primary fibers. As a result, in particular the acoustic properties were expected to be deteriorated. It was particularly surprising that the sheath of the chopped sheath-core binder fibers can be sufficiently remelted even a second time during the production of the nonwoven fabric, thereby allowing bonding.

[0008] As explained above, shredded fibres are fibres obtained from textile waste during a shredding process, which is a mechanical process aimed at breaking down the structure of the textile waste. The aim of this process is to recover the fibres contained in the textile waste and reuse them as raw material for new production cycles.

[0009] The crushing process is described, for example, in Hilmar Fuchs, Wilhelm Albrecht, Vliesstoffe: Rohstoffe, Herstellung, Anwendung, Eigenschaften, Pruefung (18. Juli 2012), zweite Ausgabe, Wiley VCH.

[0010] On the other hand, primary fibers are fibers according to the invention that have not been recycled by a crushing process. Crushed fibers can be distinguished from primary fibers in that they have a damaged fiber structure, which can be visually recognized. This is manifested, for example, in the crushed framework fibers, by an irregular or completely destroyed crimp structure and / or an uneven fiber length. Crushed binder fibers furthermore have binder components that are at least partially destroyed at least before being remelted, which is manifested by an irregular fiber profile. If the crushed sheath-core binder fibers are thermally bonded, as in the nonwoven fabric according to the invention, they can be distinguished, for example, from thermally bonded primary sheath-core binder fibers in that they have a more irregular structure, in which, for example, two cores are surrounded by a common sheath or the sheath is deformed, for example, agglomerated.

[0011] Figure 1 shows a photographic image of the primary framework fibers. The fibers have a strong and uniform crimp. Figure 2 shows a photographic image of the fractured framework fibers. The fibers are clearly less crimped and more irregular. Figure 3 shows an SEM image of the fused primary binder fibers. A relatively regular fiber profile is observed. The irregularity is only due to the binder components being melted and the framework fibers falling off in some places. This falling off is due to the sample preparation, where a part of the nonwoven fabric was cut off and the fibers were pulled out in this case. Figure 4 shows an SEM image of the fractured binder fibers (not refused). The partially destroyed binder components are clearly visible. Figure 5 shows an SEM image of the refused fractured binder fibers. It can be seen how the two cores are surrounded by a common sheath.

[0012] Furthermore, micrographs of examples of nonwoven fabrics according to the invention have revealed that the nonwoven fabrics according to the invention have a less uniform fiber distribution than nonwoven fabrics of the same structure containing only primary fibers. For example, the crushed sheath-core binder fibers have been found to form "webbed fibers" with a higher proportion of binder fibers than in the rest of the nonwoven fabric. Figure 6 shows a nonwoven fabric according to the invention with webbed fibers colored white. For comparison, Figure 7 shows a nonwoven fabric containing only primary fibers and no webbed fibers.

[0013] Nonwoven fabrics are structures made of fibers of definite length, continuous fibers (filaments) or chopped yarns of any type and origin bound in any way to form webs (fiber layers, fiber batts) which are then bound together in any way, excluding the crossing and entanglement of yarns as occurs in the manufacture of woven, warp knitted, weft knitted, laced, braided and tufted products. Nonwoven fabrics do not include films or papers. Nonwoven fabrics are described in DIN EN ISO 9092, August 2019 edition.

[0014] According to the invention, the nonwoven fabric comprises 50% to 90% by weight, preferably 60% to 80% by weight, even more preferably 70% to 80% by weight, of framework staple fibres having an average fineness of 0.9 dtex to 8.8 dtex, advantageously 0.9 dtex to 6.7 dtex, in particular 0.9 dtex to 3.3 dtex, relative to the total weight of the nonwoven fabric, the framework staple fibres comprising a proportion of chopped framework staple fibres.

[0015] Framework staple fibers should be understood to be staple fibers that are not present in the fused state of the binder fiber's binder component. This is the usual meaning of framework fibers. Preferably, the core-sheath binder fibers are also staple fibers. Staple fibers should be understood to be fibers that have a predetermined length, as opposed to theoretically infinite filaments, as is customary in the art.

[0016] According to the invention, the framework staple fibres comprise a proportion of crushed framework staple fibres, wherein the crushed framework staple fibres have an average fineness of 0.9 dtex to 8.8 dtex, advantageously 0.9 dtex to 6.7 dtex, in particular 0.9 dtex to 3.3 dtex. In a preferred embodiment of the invention, the crushed framework staple fibres have an average staple length of 5 mm to 60 mm, even more preferably 10 mm to 55 mm, in particular 10 mm to 50 mm.

[0017] In a further preferred embodiment of the present invention, the chopped framework staple fibers comprise at least one melt-spinnable polymer. Preferably, the polymer is selected from polyacrylonitrile, polyvinyl alcohol, viscose, polyamides, in particular polyamide 6 and polyamide 6.6, polyolefins and / or polyesters. Preference is given to polyolefins and / or polyesters. Very particular preference is given to polyesters.

[0018] Particularly preferably, the fractured framework staple fibers comprise at least one polyester selected from the group consisting of polyethylene terephthalate, polypropylene terephthalate, polytetramethylene terephthalate, poly(decamethylene) terephthalate, poly-1,4-cyclohexylene dimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyglycolic acid, polylactide, polycaprolactone, polyethylene adipate, polyhydroxyalkanoate, polyhydroxybutyrate, poly-3-hydroxybutyrate-co-3-hydroxyvalerate, polytrimethylene terephthalate, Vectran, polyethylene naphthalate, copolymers thereof and / or mixtures thereof. Particularly preferred polyesters are polyethylene terephthalate, polyethylene naphthalate and polybutylene terephthalate, mixtures and / or copolymers thereof. Particularly preferably, the fractured framework staple fibers comprise polyethylene terephthalate. In that case, the chopped framework staple fibers preferably comprise from 50% to 100% by weight, more preferably still from 70% to 100% by weight, more preferably still from 80% to 100% by weight of the aforementioned polymer, in particular polyethylene terephthalate, based on the total weight of the chopped framework staple fibers, and in particular consist of the polymers mentioned herein.

[0019] In a preferred embodiment, the nonwoven fabric comprises primary framework staple fibres in addition to the chopped framework staple fibres, the primary framework staple fibres advantageously having an average fineness of 0.9 dtex to 8.8 dtex, even more preferably 0.9 dtex to 6.7 dtex, in particular 0.9 dtex to 3.3 dtex. If present, the primary framework staple fibres preferably have an average staple length of 20 mm to 80 mm, even more preferably 25 mm to 80 mm, in particular 30 mm to 80 mm.

[0020] In a further preferred embodiment of the present invention, the primary framework staple fibers comprise at least one melt-spinnable polymer. Preferably, the polymer is selected from polyacrylonitrile, polyvinyl alcohol, viscose, polyamides, in particular polyamide 6 and polyamide 6.6, polyolefins and / or polyesters. Preference is given to polyolefins and / or polyesters. Very particular preference is given to polyesters.

[0021] Particularly preferably, the primary framework staple fibers comprise at least one polyester selected from the group consisting of polyethylene terephthalate, polypropylene terephthalate, polytetramethylene terephthalate, poly(decamethylene) terephthalate, poly-1,4-cyclohexylene dimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyglycolic acid, polylactide, polycaprolactone, polyethylene adipate, polyhydroxyalkanoate, polyhydroxybutyrate, poly-3-hydroxybutyrate-co-3-hydroxyvalerate, polytrimethylene terephthalate, Vectran, polyethylene naphthalate, copolymers thereof and / or mixtures thereof. Particularly preferred polyesters are polyethylene terephthalate, polyethylene naphthalate and polybutylene terephthalate, mixtures and / or copolymers thereof. Particularly preferably, the primary framework staple fibers comprise polyethylene terephthalate. In that case, the primary framework staple fibres preferably comprise from 50% to 100% by weight, more preferably still from 70% to 100% by weight, more preferably still from 80% to 100% by weight of the aforementioned polymer, in particular polyethylene terephthalate, based on the total weight of the primary framework staple fibres, and in particular consist of the polymers mentioned herein.

[0022] According to the present invention, the nonwoven fabric contains 10% by weight to 50% by weight, preferably 20% by weight to 40% by weight, and more preferably 20% by weight to 30% by weight of the core-sheath type binder fibers relative to the total weight of the nonwoven fabric, and the core-sheath type binder fibers contain a certain proportion of crushed core-sheath type binder fibers.

[0023] Binder fibers are to be understood as fibers having at least one binder component present in the form of a more or less modified fiber structure or a completely fused continuous phase. The binder component can bring about the adhesive bonding of the sheet-like construction. In core-sheath binder fibers, the sheath acts as the binder component.

[0024] Also preferably, the chopped sheath-core binder fibers have an average fineness in the range of 1.7 dtex to 6.7 dtex, advantageously 1.7 dtex to 5 dtex.

[0025] Preferably, the fractured core-sheath binder fibers have a core polymer (core polymer) different from the sheath polymer. After solidification, the core polymer may be partially or completely surrounded by the binder component. The quantitative ratio of the core polymer to the sheath polymer can be freely selected. A ratio of 90:10 to 10:90 (weight ratio of core:sheath in weight %), more preferably still 80:20 to 20:80, more preferably still 80:20 to 30:70, in particular 80:20 to 40:60 has proven to be particularly advantageous.

[0026] According to a particularly preferred embodiment, the sheath polymer of the fractured sheath-core binder fiber has a lower melting point than the core polymer of the fractured sheath-core binder fiber, in which case the difference between the melting temperature of the sheath polymer and the melting temperature of the core polymer is advantageously at least 5° C., preferably at least 8° C., particularly preferably at least 10° C. This difference in melting temperatures of the two polymers provides good temperature stability.

[0027] The core polymer of the fractured sheath-core binder fiber can comprise a wide variety of materials. Preferably, the core polymer is a melt-spinnable polymer. Preferably, the polymer is selected from polyacrylonitrile, polyvinyl alcohol, viscose, polyamide, in particular polyamide 6 and polyamide 6.6, polyolefins and / or polyesters. Preferred are polyolefins and / or polyesters. Very particularly preferred are polyesters.

[0028] Particularly preferably, the core polymer comprises at least one polyester selected from the group consisting of polyethylene terephthalate, polypropylene terephthalate, polytetramethylene terephthalate, poly(decamethylene) terephthalate, poly-1,4-cyclohexylene dimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyglycolic acid, polylactide, polycaprolactone, polyethylene adipate, polyhydroxyalkanoate, polyhydroxybutyrate, poly-3-hydroxybutyrate-co-3-hydroxyvalerate, polytrimethylene terephthalate, Vectran, polyethylene naphthalate, copolymers thereof and / or mixtures thereof. Preferred polyesters are polyethylene terephthalate, polyethylene naphthalate and polybutylene terephthalate, mixtures and / or copolymers thereof. Particularly preferably, the core polymer comprises polyethylene terephthalate. In that case, the core polymer comprises preferably 50% to 100% by weight, more preferably still 70% to 100% by weight, more preferably still 80% to 100% by weight of the aforementioned polymer, in particular polyethylene terephthalate, based on the total weight of the core polymer, and in particular consists of the polymers mentioned herein.

[0029] When the nonwoven fabric comprises primary sheath / core binder fibers, the core polymer of the chopped sheath / core binder fibers advantageously has the same polymer and / or polymers as the core polymer of the primary sheath / core binder fibers.

[0030] The sheath polymer of the fractured core-sheath binder fibers can likewise comprise a wide variety of materials. Preferably, the sheath polymer comprises a copolyester, in particular a copolyethylene terephthalate. Suitable copolymers are, for example, random, gradient, alternating, block or graft copolymers. The copolymers can consist of two, three, four or more different monomers (terpolymers, tetrapolymers). Particularly preferred further comonomers are the monomers of the following polymers: aromatic and aliphatic polyesters, aromatic and aliphatic polyamides, aromatic and aliphatic epoxides, aromatic and aliphatic polyurethanes, polysiloxanes, polyacrylates, polyacrylamides.

[0031] In this case, the sheath polymer of the fractured sheath-core binder fiber contains copolyethylene terephthalate in an amount of preferably 50% by weight to 100% by weight, more preferably 70% by weight to 100% by weight, and even more preferably 80% by weight to 100% by weight, based on the total weight of the sheath polymer of the fractured sheath-core binder fiber.

[0032] When the nonwoven fabric comprises primary sheath / core binder fibers, the sheath polymer of the chopped sheath / core binder fibers advantageously has the same polymer and / or polymers as the sheath polymer of the primary sheath / core binder fibers.

[0033] Preferably, the sheath polymer of the fractured core-sheath binder fibers has a melting point in the range of less than 250°C, even more preferably in the range of 70 to 235°C, even more preferably in the range of 125 to 225°C, and particularly preferably in the range of 150 to 225°C.

[0034] When the nonwoven fabric comprises primary framework fibers and / or primary sheath / core binder fibers, the chopped sheath / core binder fibers advantageously have the same average fineness and / or the same polymer as the primary sheath / core binder fibers and / or the chopped framework fibers have the same average fineness and / or the same polymer as the primary framework fibers.

[0035] In a preferred embodiment, the nonwoven fabric comprises primary sheath-core binder fibers.

[0036] The primary sheath-core binder fibers are preferably staple fibers, preferably having an average staple length of from 20 mm to 80 mm, even more preferably from 25 mm to 80 mm, especially from 30 mm to 80 mm.

[0037] Also preferably, the primary sheath-core binder fibers have an average fineness ranging from 1.7 dtex to 6.7 dtex, advantageously from 1.7 dtex to 5 dtex.

[0038] According to the invention, the primary sheath-core binder fiber preferably has a polymer (core polymer) in the core that is different from the sheath polymer. The quantitative ratio of the core polymer to the sheath polymer can be freely selected. A ratio of 90:10 to 10:90 (weight ratio of core:sheath in weight %), more preferably 80:20 to 20:80, even more preferably 80:20 to 30:70, in particular 80:20 to 40:60 has proven to be particularly advantageous.

[0039] According to a particularly preferred embodiment, the sheath polymer of the primary sheath-core binder fiber has a lower melting point than the core polymer of the primary sheath-core binder fiber, in which case the difference between the melting temperature of the sheath polymer and the melting temperature of the core polymer is advantageously at least 5° C., preferably at least 8° C., particularly preferably at least 10° C. This difference in melting temperatures of the two polymers provides good temperature stability.

[0040] The core polymer of the primary sheath-core binder fiber can comprise a wide variety of materials. Preferably, the core polymer is a melt-spinnable polymer. Preferably, the polymer is selected from polyacrylonitrile, polyvinyl alcohol, viscose, polyamide, in particular polyamide 6 and polyamide 6.6, polyolefins and / or polyesters. Preferred are polyolefins and / or polyesters. Very particular preferred are polyesters.

[0041] Particularly preferably, the core polymer comprises at least one polyester selected from the group consisting of polyethylene terephthalate, polypropylene terephthalate, polytetramethylene terephthalate, poly(decamethylene) terephthalate, poly-1,4-cyclohexylene dimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyglycolic acid, polylactide, polycaprolactone, polyethylene adipate, polyhydroxyalkanoate, polyhydroxybutyrate, poly-3-hydroxybutyrate-co-3-hydroxyvalerate, polytrimethylene terephthalate, Vectran, polyethylene naphthalate, copolymers thereof and / or mixtures thereof. Particularly preferred polyesters are polyethylene terephthalate, polyethylene naphthalate and polybutylene terephthalate, mixtures and / or copolymers thereof. Particularly preferably, the core polymer comprises polyethylene terephthalate. In that case, the core polymer comprises preferably 50% to 100% by weight, more preferably still 70% to 100% by weight, more preferably still 80% to 100% by weight of the aforementioned polymer, in particular polyethylene terephthalate, based on the total weight of the core polymer, and in particular consists of the polymers mentioned herein.

[0042] The sheath polymer of the primary sheath-core binder fibers can likewise comprise a wide variety of materials. Preferably, the sheath polymer comprises a copolyester, in particular a copolyethylene terephthalate. Suitable copolymers are, for example, random, gradient, alternating, block or graft copolymers. The copolymers can consist of two, three, four or more different monomers (terpolymers, tetrapolymers). Particularly preferred further comonomers are the monomers of the following polymers: aromatic and aliphatic polyesters, aromatic and aliphatic polyamides, aromatic and aliphatic epoxides, aromatic and aliphatic polyurethanes, polysiloxanes, polyacrylates, polyacrylamides.

[0043] In this case, the sheath polymer of the primary sheath / core binder fiber contains copolyethylene terephthalate in an amount of preferably 50% by weight to 100% by weight, more preferably 70% by weight to 100% by weight, and even more preferably 80% by weight to 100% by weight, based on the total weight of the sheath polymer of the primary sheath / core binder fiber.

[0044] Preferably, the sheath polymer of the primary sheath-core binder fibers has a melting point in the range of less than 250°C, even more preferably in the range of 70 to 235°C, even more preferably in the range of 125 to 225°C, and particularly preferably in the range of 150 to 225°C.

[0045] In a preferred embodiment of the present invention, the nonwoven fabric contains chopped fibers in an amount of 8% to 100% by weight, more preferably 10% to 80% by weight, even more preferably 15% to 70% by weight, and in particular 20% to 60% by weight, based on the total weight of the sound-absorbing nonwoven fabric. A high proportion of chopped fibers is advantageous in terms of sustainability.

[0046] In a further embodiment of the invention, the nonwoven fabric comprises primary fibers in an amount of less than 15% by weight, preferably less than 10% by weight, in particular less than 5% by weight, each relative to the total weight of the sound-absorbing nonwoven fabric. In a further embodiment of the invention, the nonwoven fabric does not comprise primary fibers.

[0047] In a further embodiment of the invention, the nonwoven fabric comprises framework staple fibers having an average fineness between 0.9 dtex and 8.8 dtex, advantageously between 0.9 dtex and 6.7 dtex, in particular between 0.9 dtex and 3.3 dtex, in a proportion of 60% to 80% by weight, more preferably still 70% to 80% by weight, relative to the total weight of the nonwoven fabric.

[0048] In a further embodiment of the invention, the nonwoven fabric comprises sheath-core binder fibers in a proportion of 20% to 40% by weight, and even more preferably 20% to 30% by weight, based on the total weight of the nonwoven fabric.

[0049] In a further preferred embodiment of the present invention, the nonwoven fabric comprises primary fibers in an amount of 5% by weight to 92% by weight, more preferably still 20% by weight to 90% by weight, more preferably still 30% by weight to 85% by weight, in particular 40% by weight to 80% by weight, each relative to the total weight of the sound-absorbing nonwoven fabric.

[0050] More preferably, the proportion of chopped framework staple fibers relative to the total weight of framework staple fibers is 10 to 100% by weight, preferably 15% to 80% by weight, even more preferably 20% to 70% by weight, especially 20% to 60% by weight.

[0051] Also preferably, the proportion of the crushed sheath-core binder fibers to the total weight of the sheath-core binder fibers is 10% by weight to 100% by weight, preferably 20% by weight to 75% by weight, even more preferably 30% by weight to 80% by weight, and particularly preferably 40% by weight to 80% by weight.

[0052] In a further preferred embodiment, the nonwoven fabric comprises 5% to 90% by weight of crushed framework staple fibers, more preferably still 10% to 80% by weight, more preferably still 15% to 70% by weight, more preferably still 20% to 60% by weight, in particular 20% to 50% by weight, based on the total weight of the sound-absorbing nonwoven fabric.

[0053] In a further preferred embodiment, the nonwoven fabric comprises 1% by weight to 50% by weight of crushed sheath-core binder fibers, more preferably 5% by weight to 40% by weight, even more preferably 7.5% by weight to 30% by weight, and particularly preferably 10% by weight to 20% by weight, based on the total weight of the sound absorbing nonwoven fabric.

[0054] In a further preferred embodiment, the nonwoven fabric comprises, based on the total weight of the nonwoven fabric, a) from 0% to 70% by weight, advantageously from 10% to 65% by weight, even more preferably from 20% to 55% by weight, in particular from 30% to 45% by weight of primary framework staple fibers; b) 0% to 70% by weight, advantageously 5% to 60% by weight, even more preferably 10% to 50% by weight, in particular 15% to 40% by weight of primary sheath-core binder fibers, c) 5% to 90% by weight, even more preferably 10% to 80% by weight, even more preferably 15% to 70% by weight, even more preferably 20% to 60% by weight, especially 20% to 50% by weight of crushed framework staple fibers; d) 1% to 50% by weight, more preferably 5% to 40% by weight, even more preferably 7.5% to 30% by weight, particularly preferably 10% to 20% by weight of crushed sheath-core binder fibers; Includes.

[0055] The nonwoven fabric according to the invention has a compressive strength of 150 Ns / m2, measured according to DIN EN 29053, May 1993 edition. 3 ~5000Ns / m 3 , advantageously 150 Ns / m 3 ~3000Ns / m 3 , and even more preferably 150Ns / m 3 ~2000Ns / m 3 , especially 150Ns / m 3 ~1000Ns / m 3 It has a flow resistance of .

[0056] The nonwoven fabric according to the invention further preferably has a sound absorption coefficient, measured in Alphacabin (DIN EN ISO 354:2003) at 1000 Hz at a thickness of 10 to 50 mm, even more preferably 10 to 35 mm, in particular 10 mm, of more than 0.35, preferably more than 0.4.

[0057] Furthermore, the nonwoven fabric according to the present invention has a fiber density of 150 g / m 2 ~600g / m 2 , advantageously 200 g / m 2 ~550g / m 2 , and even more preferably 250 g / m 2 ~500g / m 2 It has a weight of

[0058] Advantageously, the nonwoven fabric according to the invention has a thickness, measured in accordance with DIN EN ISO 9073-2 (1997-02), methods B and C, of ​​between 10 and 50 mm, even more preferably between 10 and 35 mm.

[0059] Further preferably, the nonwoven fabric according to the invention has a maximum tensile strength in the longitudinal direction (according to DIN EN ISO 9073-2, 2022-05) of 25N to 100N, even more preferably 30N to 100N, in particular 40N to 100N and / or a maximum tensile strength in the transverse direction (according to DIN EN ISO 9073-2, 2022-05) of 25N to 100N, even more preferably 30N to 100N, in particular 40N to 100N.

[0060] More preferably, the nonwoven fabric according to the invention has an internal nonwoven strength, measured according to DIN 54310 1980, of more than 0.5 N / 5cm, for example from 0.5 N / 5cm to 10 N / 5cm, and / or from 0.5 N / 5cm to 3 N / 5cm, and / or from 0.5 N / 5cm to 2.5 N / 5cm.

[0061] In a further preferred embodiment, the sound-absorbing nonwoven fabric is produced from textile waste treated in a crushing process, the crushing process being carried out so that the treated textile waste contains at least 70% by weight of textile single fibers, advantageously 70% to 100% by weight, more preferably 80% to 100% by weight, more preferably 90% to 100% by weight, based on the total amount of treated textile waste. To determine the amount of textile single fibers, single fibers are manually separated from a sample (10 g) of treated textile waste. At least 10 samples are taken and the results are averaged.

[0062] More preferably, the sound-absorbing nonwoven fabric is manufactured from textile waste treated in a crushing process, the crushing process being carried out so that the amount of undisintegrated textile residues, such as neps and sheet-like material pieces, contained in the treated textile waste is less than 30% by weight, advantageously 0% to 30% by weight, advantageously 0% to 20% by weight, and even more preferably 0% to 10% by weight, based on the total amount of the treated textile waste. To determine the amount of undisintegrated textile residues, the undisintegrated textile residues are manually separated from a sample (10 g) of the treated textile waste. At least 10 samples are taken and the results are averaged.

[0063] More preferably, the sound-absorbing nonwoven fabric is produced from textile waste that contains nonwoven fabric and has been treated in a crushing process, and particularly preferably, from textile waste that contains more than 90% by weight of nonwoven fabric, for example 90% to 100% by weight, and even more preferably 95% to 100% by weight. Particularly preferably, the sound-absorbing nonwoven fabric is produced from textile waste that has been treated in a crushing process and is present in a state of being sorted by type.

[0064] In a further preferred embodiment, the sound absorbing nonwoven fabric is produced from treated textile waste, the treated textile waste comprising: a) comprising 50% to 90% by weight, preferably 60% to 80% by weight, more preferably still 70% to 80% by weight, of framework staple fibres with an average fineness of 0.9 dtex to 8.8 dtex, advantageously 0.9 dtex to 6.7 dtex, in particular 0.9 dtex to 3.3 dtex, based on the total weight of the treated textile waste, and b) The core-sheath type binder fibers are contained in an amount of 10% to 50% by weight, preferably 20% to 40% by weight, and more preferably 20% to 30% by weight, based on the total weight of the treated textile waste.

[0065] A further subject of the invention is a material having a resistance of 150 Ns / m, measured according to DIN EN 29053 of the May 1993 edition. 3 ~5000Ns / m 3 , advantageously 150 Ns / m 3 ~3000Ns / m 3 , and even more preferably 150Ns / m 3 ~2000Ns / m 3 , especially 150Ns / m 3 ~1000Ns / m 3 and a flow resistance of 150g / m 2 ~600g / m 2 A method for producing a sound absorbing nonwoven fabric having a basis weight of I. Providing textile waste, the textile waste comprising: a) comprising 50% to 90% by weight, preferably 60% to 80% by weight, more preferably still 70% to 80% by weight, of framework staple fibres with an average fineness of 0.9 dtex to 8.8 dtex, advantageously 0.9 dtex to 6.7 dtex, in particular 0.9 dtex to 3.3 dtex, based on the total weight of the textile waste, and b) a step of including a core-sheath type binder fiber in an amount of 10% by weight to 50% by weight, preferably 20% by weight to 40% by weight, and more preferably 20% by weight to 30% by weight, based on the total weight of the textile waste; II. at least partially disintegrating the textile structure of the textile waste in a crushing process to obtain a treated textile waste comprising a proportion of crushed framework staple fibers and a proportion of crushed sheath-core binder fibers; III. Forming a nonwoven fabric from the treated textile waste; IV. A step of heat-treating the nonwoven fabric to obtain a sound-absorbing nonwoven fabric; The method includes:

[0066] The process steps I) to IV) are preferably carried out successively.

[0067] Advantageously, by the method according to the invention, a thermally bonded sound-absorbing nonwoven fabric is produced, which nonwoven fabric comprises: a) comprising 50% to 90% by weight, preferably 60% to 80% by weight, more preferably still 70% to 80% by weight, based on the total weight of the nonwoven fabric, of framework staple fibers having an average fineness of 0.9 dtex to 8.8 dtex, advantageously 0.9 dtex to 6.7 dtex, in particular 0.9 dtex to 3.3 dtex, and b) the nonwoven fabric contains core-sheath type binder fibers in an amount of 10% by weight to 50% by weight, preferably 20% by weight to 40% by weight, and more preferably 20% by weight to 30% by weight, based on the total weight of the nonwoven fabric; The framework staple fibers include a proportion of crushed framework staple fibers, the sheath-core binder fibers include a proportion of crushed sheath-core binder fibers, and the sound absorbing nonwoven fabric has a density of 150 g / m 2 ~600g / m 2 Thus, a thermally bonded sound absorbing nonwoven fabric having a basis weight of

[0068] More preferably, the method according to the present invention produces a thermally bonded acoustic nonwoven fabric according to one or more of the embodiments described herein.

[0069] The method according to the present invention Process I. The method comprises providing a textile waste, which comprises framework staple fibres with an average fineness of 0.9 dtex to 8.8 dtex, advantageously 0.9 dtex to 6.7 dtex, in particular 0.9 dtex to 3.3 dtex, in a proportion of 50% to 90% by weight, preferably 60% to 80% by weight, more preferably 70% to 80% by weight, based on the total weight of the textile waste, and core-sheath binder fibres in a proportion of 10% to 50% by weight, preferably 20% to 40% by weight, more preferably 20% to 30% by weight, based on the total weight of the textile waste. A wide variety of textile wastes are suitable for the method according to the invention. Preferably, the textile waste comprises fibres according to one or more of the embodiments described for the sound-absorbing nonwoven fabric according to the invention.

[0070] Here, the textile waste can come from a wide variety of areas, such as clothing and technical textiles. Preferably, the textile waste comprises nonwoven fabrics. Particularly preferably, the textile waste comprises nonwoven fabrics in a proportion of more than 90% by weight, for example 90% to 100% by weight, even more preferably 95% to 100% by weight, based on the total weight of the textile waste. The textile waste can also comprise woven and / or warp knitted fabrics. The textile waste is furthermore advantageously present in a sorted state. Furthermore, the textile waste can also be present as post-consumer textiles, as residues of filaments or yarns or also as strip-like material from the production of sheet-like materials. Mixtures of different forms are also possible.

[0071] After step I, Optional Step I.1 in which the textile waste is pre-shredded, advantageously by shredding.

[0072] Furthermore, after step I or step I.1, Optional Step I.2 This can be followed by a process in which the pre-shredded textile waste is optionally moistened and / or oiled, which favors the subsequent structure collapse. Furthermore, it can reduce fiber friction, thereby reducing energy costs and fiber damage.

[0073] The method Process II. comprises at least partially disrupting the textile structure of the textile waste in a crushing step to obtain treated textile waste.

[0074] In a preferred embodiment, the crushing process is carried out in a crusher, the operating principle of which is that the textile waste is fed through a draw-in system, which has a conveying and at the same time a clamping action, to a crushing unit, advantageously a rotating drum, in which crushing elements are arranged. The rotating drum is advantageously a crushing drum. The crushing elements are preferably pin-, hook- or tooth-shaped. Preferably, the crushing elements are formed as a sawtooth set. The crushing elements grip the textile waste clamped by the draw-in system and at least partially crush its structure under the effect of tensile stress.

[0075] The textile waste can be subjected to the shredding process one or more times. Here, it is also possible to subject only a part of the textile waste to the shredding process several times. Advantageously, the shredding process comprises at least two shredding processes. For this purpose, the textile waste can be fed again to the same shredding unit after one shredding process in the shredding unit. However, it is also possible to arrange several shredding units in series. The transfer of material between the shredding units can be effected, for example, by a sieve drum. In a preferred embodiment of the invention, the number and fineness of the shredding elements arranged in the various shredding units are adapted to the progression of the structural disintegration of the textile waste.

[0076] The drawing system can comprise a pair of rolls or a combination of a rotating roll and a rigid trough. Preferably, the drawing system is configured as a trough drawing machine, in which the clamping points of the material are located at the corners of the trough. This is advantageous, since it allows the clamping points of the material to be closer to the effective range of the crushing elements.

[0077] By adjusting various parameters of the crushing process, in particular the number of crushing units through which the textile waste passes, the desired structural breakdown of the textile waste can be adjusted.

[0078] Preferably, the textile structure of the textile waste is disintegrated to such an extent that the treated textile waste contains at most 30% by weight of undisintegrated textile residues such as neps and sheet-like material pieces, advantageously 0% to 30% by weight, even more preferably 0% to 20% by weight, even more preferably 0% to 10% by weight. Advantageously, the textile structure of the textile waste is disintegrated to such an extent that the treated textile waste contains at least 70% by weight of textile single fibers, advantageously 70% to 100% by weight, even more preferably 80% to 100% by weight, even more preferably 90% to 100% by weight, based on the total weight of the treated textile waste. As a result, the treated textile waste obtained in step II. advantageously contains at least 70% by weight, even more preferably 70% to 100% by weight, even more preferably 80% to 100% by weight, even more preferably 90% to 100% by weight of textile single fibers. More preferably, the treated textile waste obtained in step II. contains undisintegrated textile residues, such as neps and sheet-like material pieces, in a proportion of less than 30% by weight, advantageously 0% to 30% by weight, even more preferably 0% to 20% by weight, even more preferably 0% to 10% by weight, based on the total amount of treated textile waste. To determine the proportion of undisintegrated textile residues, the undisintegrated textile residues are manually separated from the sample (10 g). At least 10 samples are taken and the results are averaged.

[0079] The treated textile waste obtained in step II. can be post-treated to improve its quality. For example, extensive cleaning can be carried out to reduce the proportion of short fibres and / or to separate coarse and foreign matter. Furthermore, desired textile treatments can be carried out, such as flame-retardant, mould-proof and / or antistatic treatments.

[0080] In a preferred embodiment of the present invention, the treated textile waste obtained in step II. is a) comprising 50% to 90% by weight, preferably 60% to 80% by weight, more preferably still 70% to 80% by weight, of framework staple fibres with an average fineness of 0.9 dtex to 8.8 dtex, advantageously 0.9 dtex to 6.7 dtex, in particular 0.9 dtex to 3.3 dtex, based on the total weight of the treated textile waste, and b) The core-sheath type binder fibers are contained in an amount of 10% to 50% by weight, preferably 20% to 40% by weight, and more preferably 20% to 30% by weight, based on the total weight of the treated textile waste.

[0081] In a further preferred embodiment of the present invention, the treated textile waste obtained in step II. is a) 5% to 90% by weight, more preferably still 10% to 80% by weight, more preferably still 15% to 70% by weight, more preferably still 20% to 60% by weight, in particular 20% to 50% by weight of crushed framework staple fibers having an average fineness of 0.9 dtex to 8.8 dtex, advantageously 0.9 dtex to 6.7 dtex, in particular 0.9 dtex to 3.3 dtex; b) 1% to 50% by weight, more preferably 5% to 40% by weight, more preferably 7.5% to 30% by weight, and especially 10% to 20% by weight of crushed sheath-core binder fibers; Includes.

[0082] After step II, Optional Step II.1 The process may be followed by a step II.1, which comprises mixing the treated textile waste obtained in step II. with primary framework staple fibers and / or primary sheath-core binder fibers to obtain a treated textile waste comprising primary fibers. Preferably, step II.1 produces a mixture of the following components by weight of the treated textile waste: a) from 0% to 70% by weight, advantageously from 10% to 65% by weight, even more preferably from 20% to 55% by weight, in particular from 30% to 45% by weight of primary framework staple fibers; b) 0% to 70% by weight, advantageously 5% to 60% by weight, even more preferably 10% to 50% by weight, in particular 15% to 40% by weight of primary sheath-core binder fibers, c) 5% to 90% by weight, even more preferably 10% to 80% by weight, even more preferably 15% to 70% by weight, even more preferably 20% to 60% by weight, especially 20% to 50% by weight of crushed framework staple fibers; d) 1% to 50% by weight, more preferably 5% to 40% by weight, even more preferably 7.5% to 30% by weight, particularly preferably 10% to 20% by weight of crushed sheath-core binder fibers; A treated textile waste comprising:

[0083] The method according to the present invention Process III. In step II. or II.1, the treated textile waste is formed into a nonwoven fabric, which can be formed by various methods known to those skilled in the art, such as the carding method.

[0084] The method according to the present invention Process IV. The nonwoven fabric obtained in step III is heat-treated to a strength of 150 Ns / m, measured according to the May 1993 edition of DIN EN 29053. 3 ~5000Ns / m 3 , advantageously 150 Ns / m 3 ~3000Ns / m 3 , and even more preferably 150Ns / m 3 ~2000Ns / m 3 , especially 150Ns / m 3 ~1000Ns / m 3 and a flow resistance of 150g / m 2 ~600g / m 2 A sound absorbing nonwoven fabric having a basis weight of 110° C. to 220° C. is obtained. As known to those skilled in the art, the basis weight can be adjusted by appropriately setting the basis weight when laminating the nonwoven fabric. The heat treatment is preferably carried out at a temperature of 110° C. to 220° C., preferably 120° C. to 200° C. The heat treatment is more preferably carried out in a forced air oven.

[0085] A further subject of the invention is a sound-absorbing nonwoven fabric produced by the method according to the invention.

[0086] A further subject of the invention is the use of the sound-absorbing nonwoven fabric according to the invention for sound absorption in the automotive sector, in particular in automotive interiors. [Brief description of the drawings]

[0087] [Figure 1] FIG. 1 shows a photographic image of the primary framework fibers. [Diagram 2] FIG. 1 shows a photographic image of fractured framework fibers. [Diagram 3] FIG. 13 shows an SEM image of fused primary binder fibers. [Figure 4] FIG. 1 shows an SEM image of crushed binder fibers (not refused). [Diagram 5] FIG. 13 shows an SEM image of re-fused crushed binder fibers. [Figure 6] FIG. 1 shows a nonwoven fabric according to the present invention having nested fibers. [Figure 7] FIG. 1 illustrates a nonwoven fabric that contains only primary fibers and no nested fibers. [Figure 8] FIG. 1 shows the sound absorption coefficient of the nonwoven fabric according to the present invention in Alpha Cabin.

[0088] To determine the parameters used according to the invention, the following measurement methods are used: Test method for measuring sound absorption coefficient in a reverberation chamber (Alpha Cabin) The measurements are carried out in accordance with DIN EN ISO 354:2003 in the Alpha Cabin. The test sample is placed directly on the floor and measured using a frame.

[0089] Determination of the percentage of crushed framework staple fibers and crushed sheath-core binder fibers in treated textile waste Take at least 10 samples (5 g) from the treated textile waste. Separate the fibers by hand using tweezers. Sheath-core binder fibers with at least partially destroyed binder components are considered to be disrupted sheath-core binder fibers. Framework staple fibers with irregular or completely destroyed crimp structure are considered to be disrupted framework staple fibers.

[0090] Determining the percentage of crushed framework staple fibers and crushed sheath-core binder fibers in nonwoven fabrics Cut out at least five samples from the nonwoven fabric. 2 ) are observed under a microscope (resolution shown in Figure 3). Sheath-core binder fibers that have an irregular structure, e.g., two cores surrounded by a common sheath, or the sheath is deformed, e.g., agglomerated, are considered to be disrupted sheath-core binder fibers. Framework staple fibers that have an irregular or completely disrupted crimp structure are considered to be disrupted framework staple fibers.

[0091] Test method for nonwoven fabrics to measure basis weight The measurement is based on ISO 9073-1 (1989-07) and the area of ​​the measurement sample is 100 mm x 100 mm.

[0092] Nonwoven fabric test method for measuring thickness Complies with methods B and C of DIN EN ISO 9073-2 (1997-02).

[0093] Fiber fineness measurement Measure the fiber diameter using a microscope and corresponding software according to DIN 53810 (1981-02) (Fineness of spun yarns - Terminology and measurement principle). Prepare 4 micropreparations from a total of more than 20 single fibers. For each micropreparation, shorten the fibers with scissors to a length of approximately 2-3 mm and place them on a microscope slide using a specimen pin. Then measure the fiber diameter in μm using the appropriate software and take the average. The averaged fiber diameter is then calculated using the following formula: Tt[dtex]=(π×d 2 ×ρ) / 400 This can be converted to fiber fineness Tt by: d is the fiber diameter (μm), ρ is the fiber density (g / cm 3 ).

[0094] Staple length measurement Select 10 fiber bundles from the existing fiber sample, take one single fiber from each of the 10 fiber bundles using tweezers, and measure the fiber length of the 10 single fibers by clamping one free fiber end in one of the two clamps and the other fiber end in the remaining clamp. Stretch the fiber by turning the hand wheel until it is straight. Read the fiber length from the scale on the measuring device and record it in mm. The average of all the recorded results gives the staple length: SP[mm]=(ΣL) / n ΣL Sum of individual fiber lengths n The number of random samples.

[0095] Melting point determination According to DIN EN ISO 11357-3 (2018-07) "Differential scanning calorimetry (DSC) - Part 3: Determination of melting and crystallization temperatures and enthalpies of melting and crystallization" with a heating rate of 10 K / min.

[0096] Maximum transverse / longitudinal tensile force (according to DIN EN ISO 9073-3, 2022-05) The maximum tensile force is measured as follows: A tensile testing machine according to DIN 51220 (2003) and DIN EN ISO 7500 (2018) and a punch of 260 x 50 mm are used.

[0097] Sample preparation: Measurement samples are punched out from the existing test sample evenly across the width of the fabric, 10 cm from each edge in both the machine and machine directions.

[0098] implementation: After the measurement sample is clamped evenly vertically in the center, the test is carried out according to the machine-specific operating instructions, and the sample is pulled at the specified pulling speed = 200 mm / min with a preload of 0.5 N.

[0099] Internal strength of nonwoven fabric according to DIN 54310 (1980) Unlike the standard, the nonwoven is separated parallel to the face so that the resulting legs can be clamped in the clamps of the tensile tester.

[0100] Test method for measuring flow resistance According to DIN EN 29053 (1993-05), method A (cocurrent air method), the effective sample diameter corresponds to 100 mm and an air pressure of 1000 mbar.

[0101] The present invention will now be described in more detail with reference to the following non-limiting examples.

[0102] Example 1: The textile waste used is a sound absorbing material consisting of 80% by weight of 1.7 dtex PET fibers (framework staple fibers, 38 mm) and 20% by weight of 4.4 dtex PET / CoPET (core-sheath binder fibers). The textile waste is moistened and re-fibered in a shredding process in a shredder equipped with a sawtooth set as the shredding element to obtain treated textile waste. The treated textile waste contains less than 15% by weight of undisintegrated textile residue. A nonwoven fabric is formed from the treated textile waste using a carding machine and is thermally treated to obtain a nonwoven fabric having a density of 250 g / m2. 2 , and a new sound-absorbing material with a thickness of 10 mm is manufactured. The obtained sound-absorbing material has a sound resistance of 153 Ns / m 3and has a sound absorption coefficient, measured in Alpha Cabin (DIN EN ISO 354:2003), shown in Figure 8. Furthermore, the sound absorber has a uniform appearance and good mechanical properties. The sound absorber has a maximum lateral tensile force of 62 N (according to DIN EN ISO 9073-2, 2022-05) and a nonwoven internal strength of 1.28 N / 5 cm, measured according to DIN 54310 1980.

[0103] Example 2: The treated textile waste from Example 1 is mixed with primary framework staple fibers and primary sheath-core binder fibers to obtain a treated textile waste containing primary fibers, which has the same composition as the original textile waste from Example 1 in terms of the proportion of framework fibers and binder fibers (80% by weight of 1.7 dtex PET fibers (38 mm) and 20% by weight of 4.4 dtex PET / CoPET fibers), where the treated textile waste contains a) 25% by weight and b) 50% by weight of reopened fibers.

[0104] The treated textile waste is carded into a nonwoven fabric, which is then heat-treated to a thickness of 250 g / m 2 The resulting sound absorbers, containing 25% and 50% by weight of reopened fibre, respectively, have a sound absorption strength of 160 Ns / m 3 and has the sound absorption coefficient shown in Figure 8. The sound absorbing material has a uniform appearance throughout and excellent mechanical properties.

Claims

1. 150 Ns / m measured according to DIN EN 29053, May 1993 edition 3 ~5000Ns / m 3 and a flow resistance of 150 g / m 2 Up to 600 g / m 2 A thermal bonded sound absorbing nonwoven fabric having a basis weight of a) framework staple fibers having an average fineness of 0.9 dtex to 8.8 dtex are contained in a proportion of 50% to 90% by weight based on the total weight of the nonwoven fabric; and b) A thermal bonded sound absorbing nonwoven fabric containing a core-sheath type binder fiber in an amount of 10% by weight to 50% by weight based on the total weight of the nonwoven fabric, 1. A thermally bonded acoustic nonwoven fabric, comprising: said framework staple fibers comprising a percentage of chopped framework staple fibers; and said sheath-core binder fibers comprising a percentage of chopped sheath-core binder fibers.

2. 2. The thermally bonded sound absorbing nonwoven fabric of claim 1, wherein the nonwoven fabric comprises primary framework staple fibers, the primary framework staple fibers having an average fineness of 0.9 dtex to 8.8 dtex and / or an average staple length of 20 mm to 80 mm.

3. 3. The thermally bonded sound absorbing nonwoven fabric according to claim 1 or 2, characterized in that the nonwoven fabric comprises primary sheath-core binder fibers, the primary sheath-core binder fibers being staple fibers, preferably having an average staple length of 20 mm to 80 mm.

4. 4. A thermally bonded sound absorbing nonwoven fabric according to claim 1, characterized in that the nonwoven fabric comprises primary framework staple fibers and / or primary sheath-core binder fibers, the chopped sheath-core binder fibers advantageously having the same average fineness and / or the same polymer as the primary sheath-core binder fibers and / or the chopped framework fibers having the same average fineness and / or the same polymer as the primary framework fibers.

5. 5. The thermally bonded sound absorbing nonwoven fabric according to claim 1, characterized in that the proportion of the chopped framework staple fibers to the total weight of the framework staple fibers is 10 to 100% by weight and / or the proportion of the chopped sheath-core binder fibers to the total weight of the core-sheath binder fibers is 10 to 100% by weight.

6. The nonwoven fabric is a) from 0% to 70% by weight, preferably from 10% to 65% by weight, of primary framework staple fibers; b) 0% to 70% by weight, preferably 5% to 60% by weight, of primary sheath-core binder fibers; c) 5% to 90% by weight of chopped framework staple fibers; d) 1% to 50% by weight, and even more preferably 5% to 40% by weight, of chopped sheath-core binder fibers; 6. The thermally bonded sound absorbing nonwoven fabric according to claim 1, comprising:

7. 7. A thermally bonded sound-absorbing nonwoven fabric according to claim 1, characterized in that the nonwoven fabric is produced from textile waste that has been treated in a crushing process, the crushing process being carried out in such a way that the treated textile waste contains undisintegrated textile residues, in particular neps and sheet-like material pieces, in a proportion of less than 30% by weight relative to the total amount of the treated textile waste.

8. 150Ns / m 3 ~5000Ns / m 3 and a flow resistance of 150 g / m 2 Up to 600 g / m 2 A method for producing a sound absorbing nonwoven fabric having a basis weight of I. Providing textile waste, said textile waste comprising: a) framework staple fibers having an average fineness of 0.9 dtex to 8.8 dtex in a proportion of 50% to 90% by weight based on the total weight of the textile waste; and b) comprising a core-sheath binder fiber in an amount of 10% by weight to 50% by weight based on the total weight of the textile waste; II. At least partially disintegrating the textile structure of the textile waste in a crushing process to obtain a treated textile waste comprising a proportion of crushed framework staple fibers and a proportion of crushed sheath-core binder fibers; III. Forming a nonwoven fabric from the treated textile waste; IV. A step of heat-treating the nonwoven fabric to obtain a sound-absorbing nonwoven fabric. A method comprising:

9. 9. The method of claim 8, further comprising the step I.2 of moistening the textile waste.

10. 10. The method according to claim 8 or 9, characterized in that the crushing process is carried out in a crusher, the operating principle of which is that the textile waste is fed through an intake system having a conveying and simultaneously clamping action into a crushing unit, preferably a rotating drum in which crushing elements are arranged, the crushing elements being formed as a sawtooth set.

11. 11. The method according to any one of claims 8 to 10, characterized in that the textile waste is subjected to the shredding process multiple times.

12. 12. The method according to any one of claims 8 to 11, characterized in that the disintegration of the textile structure of the textile waste in step II. is carried out to such an extent that the treated textile waste contains at most 30% by weight of undisintegrated textile residues such as neps and pieces of sheet-like material and / or the treated textile waste contains at least 70% by weight of textile single fibers based on the total weight of the treated textile waste.

13. 13. The method of any one of claims 8 to 12, further comprising blending the treated textile waste obtained in step II. with primary framework staple fibers and / or primary sheath-core binder fibers.

14. 14. A method according to any one of claims 8 to 13, characterized in that it produces a nonwoven fabric according to any one of claims 1 to 7.

15. A sound absorbing nonwoven fabric produced by the method according to any one of claims 8 to 13.

16. 20. Use of the sound-absorbing nonwoven fabric according to any one of claims 1 to 7 or 15 for sound absorption in the automotive sector.

Citation Information

Patent Citations

  • Soundproofing material and its use

    JP2001513217A

  • Mat and method for producing same

    JP2003301360A

  • Formed article consisting of crushed pieces of solid fiber made of polyester and method for producing the same

    JP2004156188A

  • Sound-absorbing material for vehicle interior trim and method of manufacturing the same

    JP2011051566A

  • Nonwoven textiles manufactured from short fibers

    JP2012511108A