Coating composition and coating film protective coating material
A coating composition with polymer (A) and polyvinyl alcohol polymer (B) addresses the inefficiencies in applying protective coatings on complex shapes by minimizing sagging and ensuring uniform coverage, thereby protecting paint films on objects like automobile panels.
Patent Information
- Application Number
- JP2023061575
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-05
- Publication Date
- 2024-10-18
AI Technical Summary
Existing methods for protecting paint films on complex, three-dimensional objects such as automobile panels face challenges in efficient application and sagging, leading to potential damage during transportation and storage due to improper application of protective sheets or uneven coating thickness.
A coating composition comprising a polymer (A) and polyvinyl alcohol polymer (B) in an aqueous emulsion, with specific viscosity and composition, which can be applied using a slot die to form a high-quality protective coating that minimizes sagging and ensures efficient coverage.
The composition effectively forms a durable protective film that prevents damage to paint films on complex shapes by reducing sagging and ensuring uniform application, enhancing the protective properties of the coating material.
Smart Images

Figure 2024148445000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a paint film protective coating material and a coating composition for forming the paint film protective coating material. [Background technology]
[0002] There is a known technique for protecting a coating by attaching a protective sheet to the coating, for the purpose of preventing damage to the coating during transport, storage, curing, construction, etc. of an article having a coating (for example, painted automobiles and their parts, or metal sheets such as painted steel sheets and molded products thereof). The coating protective sheet used for such a purpose generally takes the form of a substrate-attached single-sided adhesive sheet having an adhesive (also referred to as a pressure-sensitive adhesive; the same applies below) layer on one side of a sheet-like substrate (support substrate), and is configured so that it can achieve its protective purpose by being attached to an adherend (object to be protected) via the adhesive. After completing its protective role, the coating protective sheet is then removed (re-peeled) from the adherend. Patent Document 1 can be cited as a technical document relating to coating protective sheets. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-111552 A [Patent Document 2] JP 2004-224874 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the case of objects to be protected that have a non-planar shape (particularly objects to be protected that have a complex three-dimensional shape such as the exterior panels of automobiles), it is difficult to efficiently attach a paint protective sheet to the object to be protected. If the paint protective sheet is not attached properly to the object to be protected, for example if the paint protective sheet is attached in a wrinkled state, the paint protective sheet may peel off when wind blows into the wrinkles during storage or transport of the object to be protected after attachment, and the paint protective sheet may no longer be able to fulfill its intended protective purpose.
[0005] On the other hand, it has also been proposed to directly apply a liquid composition for forming a protective film onto the coating film of the object to be protected, and then dry the liquid composition on the coating film to form a protective film. Patent Document 2 is an example of a document related to this type of technology. Patent Document 2 proposes a paint for pressure-fed roller coating, in which the paint is pressure-fed into the inside of a coating roller for coating. However, in general, in pressure-fed roller coating, it is difficult to control the amount of coating (and thus the thickness of the protective film formed after drying), and it is difficult to efficiently form a high-quality protective film. In addition, paints designed to be suitable for pressure-fed roller coating tend to sag when applied to a non-horizontal surface (especially a vertical surface), and this tendency becomes more pronounced as the amount of coating increases.
[0006] In view of the above circumstances, the present invention has an object to provide a coating composition for forming a paint film protective coating material, which is less likely to sag and can efficiently form a high-quality paint film protective coating material. Another related object is to provide a paint film protective coating material obtained from such a coating composition. [Means for solving the problem]
[0007] According to this specification, a coating composition for forming a coating film protective coating material is provided. The coating composition includes a polymer (A) as a base polymer, which is a polymer of a monomer component including an acrylic monomer. The coating composition is in the form of an aqueous emulsion in which the polymer (A) is dispersed in an aqueous solvent. The coating composition further includes a polyvinyl alcohol-based polymer (B). The polyvinyl alcohol-based polymer (B) has a degree of saponification of 80 mol % or more. The polyvinyl alcohol-based polymer (B) has a degree of polymerization of 1200 or less. The content of the polyvinyl alcohol-based polymer (B) is 0.3 parts by weight or more and 5.0 parts by weight or less relative to 100 parts by weight of the polymer (A). The coating composition has a viscosity of 25 Pa·s or more as measured by a BH type viscometer at 30°C and 2 rpm. A coating composition that includes an appropriate amount of the polyvinyl alcohol-based polymer (B) relative to the polymer (A) and has a BH viscosity of 25 Pa·s or more is less likely to sag, and can efficiently form a high-quality protective film. In the following, the viscosity measured by a BH type viscometer may be abbreviated as "BH viscosity."
[0008] In some embodiments of the technology disclosed herein (including a coating composition, a method for producing a coating composition, a coating film protection method, a coating film protection coating material, etc., the same applies below), the coating composition further contains a thickener. By using the thickener, a coating composition that satisfies the above BH viscosity can be preferably realized.
[0009] In some preferred embodiments of the coating composition, the monomer components constituting the polymer (A) include a carboxyl group-containing monomer. That is, the polymer (A) is preferably a polymer of monomer components containing a carboxyl group-containing monomer. The technology disclosed herein can be preferably implemented in an embodiment that includes the polymer (A) composed of monomer components of such a composition as a base polymer.
[0010] In some preferred embodiments of the coating composition, the monomer component constituting the polymer (A) contains a nitrogen atom-containing monomer. That is, the polymer (A) is preferably a polymer of a monomer component containing a nitrogen atom-containing monomer. The technology disclosed herein can be preferably implemented in an embodiment that contains a polymer (A) composed of monomer components of such a composition. The monomer component may be a composition containing a carboxyl group-containing monomer and a nitrogen atom-containing monomer.
[0011] This specification also provides a method for producing any of the coating compositions disclosed herein. The production method includes preparing a polymer emulsion containing an aqueous solvent, the polymer (A), and 0.3 parts by weight or more and 5.0 parts by weight or less of the polyvinyl alcohol-based polymer (B) relative to 100 parts by weight of the polymer (A), and having a viscosity of 1.0 Pa s or more and 4.5 Pa s or less at a solid content of 47% by weight measured at 30°C and 2 rpm using a BH viscometer; and adjusting the viscosity of the polymer emulsion so that the viscosity measured at 30°C and 2 rpm using a BH viscometer is 25 Pa s or more. The coating composition disclosed herein can be preferably produced by such a production method. The "viscosity at a solid content of 47% by weight" of a polymer emulsion refers to the viscosity of the polymer emulsion as is when the solid content of the polymer emulsion is within the range of 47% by weight ±1% by weight, and for a polymer emulsion whose solid content is outside the above range, refers to the viscosity when the solid content is adjusted to be within the range of 47% by weight ±1% by weight.
[0012] According to this specification, there is provided a coating film protective coating material (hereinafter, sometimes abbreviated as "coating material") formed from any of the coating compositions disclosed herein. The coating material can be formed, for example, by applying the coating composition onto a coating film to be protected and drying it. The coating material can be a dried film of any of the coating compositions disclosed herein.
[0013] This specification also provides a method for protecting a coating film, comprising: preparing any of the coating compositions disclosed herein; applying the coating composition onto a coating film of an object to be protected having the coating film; and drying the coating composition to form a coating film-protecting coating material that temporarily protects the coating film. The coating composition is less likely to sag or sag, and can efficiently form a high-quality coating material on the coating film of the object to be protected. According to the coating film protection method using such a composition, the coating film can be appropriately protected by the coating material. The coating composition can be preferably applied using a slot die.
[0014] In addition, any suitable combination of the elements described in this specification may also be included within the scope of the invention for which patent protection is sought by this application. [Brief description of the drawings]
[0015] [Figure 1] 1 is a cross-sectional view showing an example of an object protected by a paint film protective coating material according to the present invention. [Diagram 2] 1 is a block diagram showing one embodiment of a coating film protection method according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Preferred embodiments of the present invention will be described below. Matters necessary for carrying out the present invention other than those specifically mentioned in this specification can be understood by those skilled in the art based on the teachings on carrying out the invention described in this specification and the common general technical knowledge at the time of filing. The present invention can be carried out based on the contents disclosed in this specification and the common general technical knowledge in the relevant field. In the following drawings, the same reference numerals may be used to denote components or parts having the same function, and duplicated descriptions may be omitted or simplified. In addition, the embodiments shown in the drawings are schematic in order to clearly explain the present invention, and do not necessarily accurately represent the size or scale of the product actually provided.
[0017] In this specification, the term "acrylic monomer" is a general concept referring to monomers having at least one (meth)acryloyl group in one molecule (hereinafter also referred to as "(meth)acryloyl group-containing monomers") and (meth)acrylonitrile. In addition, in this specification, "(meth)acryloyl" refers to acryloyl and methacryloyl. Similarly, "(meth)acrylate" refers to acrylate and methacrylate, "(meth)acrylic" refers to acrylic and methacrylic, and "(meth)acrylonitrile" refers to acrylonitrile and methacrylonitrile.
[0018] In this specification, the term "polyvinyl alcohol polymer" (hereinafter sometimes referred to as PVA) refers to a polymer containing vinyl alcohol units (-CHCH(OH)) as its repeating units, and is a concept that refers comprehensively to unmodified PVA and modified PVA. Unmodified PVA is a polymer whose repeating units are vinyl alcohol units (-CHCH(OH)-) and vinyl ester units (-CHCH(OC(=O)R A -, where R A is an alkyl group, for example, an alkyl group having 1 to 10 carbon atoms, preferably an alkyl group having 1 to 6 carbon atoms, typically a methyl group.) Examples of modified PVA include PVA having a repeating unit (for example, a repeating unit having an anionic group) other than a vinyl ester unit (typically a vinyl acetate unit) and PVA having a structure in which at least a portion of the vinyl alcohol unit is acetalized and modified.
[0019] In this specification, the term "aqueous solvent" refers to water or a mixed solvent containing water as the main component (a component contained in excess of 50% by weight). The solvent other than water constituting this mixed solvent may be one or more selected from various organic solvents (such as lower alcohols) that can be uniformly mixed with water. In this specification, the aqueous solvent typically contains water in an amount of 90% by weight or more, preferably 95 to 100% by weight.
[0020] <Polymer (A)> The coating composition provided by this specification contains polymer (A) as a base polymer. Here, the term "base polymer" refers to a component that accounts for more than 50% by weight (typically 70% by weight or more, for example 90% by weight or more, and may be 95% by weight or more, or may be 100% by weight) of the polymer contained in the coating composition. The base polymer in the coating film protective coating material disclosed herein has the same meaning. The polymer (A) is a polymer of monomer components including an acrylic monomer. Thus, the polymer (A) is a polymer that contains monomer units derived from an acrylic monomer.
[0021] In the above polymer (A), the glass transition temperature (calculated Tg) calculated based on the composition of the monomer components constituting the polymer (A) may be, for example, -50°C or higher and 10°C or lower. In some embodiments, the calculated Tg of the polymer (A) is preferably 0°C or lower. The calculated Tg of the polymer (A) being 0°C or lower is advantageous from the viewpoint of the marking prevention properties of the coating material containing the polymer (A) as described below, and is also preferable from the viewpoint of easily realizing a coating material with a moderately large elongation at break, as described below. From the viewpoint of easily obtaining better marking prevention properties, in some embodiments, the calculated Tg of the polymer (A) may be, for example, -5°C or lower, -9°C or lower (e.g., -10°C or lower), or -15°C or lower. Lowering the calculated Tg of the polymer (A) is advantageous in terms of improving the peeling workability when peeling the coating material from the coating film in a low-temperature environment such as outdoors in winter (for example, suppressing peeling failure due to chipping or tearing of the coating material), and suppressing the occurrence of cracks in the coating material due to differences in the linear expansion coefficient between the coating material and the protected object when the protected object is exposed to temperature changes. On the other hand, from the viewpoint of peeling and peeling workability in high temperature ranges, the calculated Tg of the polymer (A) is suitably -40°C or higher, advantageously -35°C or higher, preferably -30°C or higher, and may be -25°C or higher or -20°C or higher. The technology disclosed herein can be preferably implemented in an embodiment using a polymer (A) having a calculated Tg of, for example, -25°C or higher to -10°C or lower.
[0022] Here, the calculated Tg of a polymer in this specification means the Tg calculated by the Fox formula based on the composition of the monomer components used in the synthesis of the polymer. The Fox formula is a relational expression between the Tg of a copolymer and the glass transition temperature Tgi of a homopolymer obtained by homopolymerizing each of the monomers constituting the copolymer, as shown below. 1 / Tg=Σ(Wi / Tgi) In the above Fox formula, Tg represents the glass transition temperature (unit: K) of the copolymer, Wi represents the weight fraction of monomer i in the copolymer (copolymerization ratio on a weight basis), and Tgi represents the glass transition temperature (unit: K) of the homopolymer of monomer i.
[0023] The glass transition temperature of the homopolymer used to calculate the calculated Tg is a value described in a publicly known document. For example, for the monomers listed below, the following values are used as the glass transition temperatures of the homopolymers of the monomers. n-Butyl acrylate -55℃ Acrylonitrile 97℃ Vinyl acetate 32℃ Methyl methacrylate 105℃ Acrylic acid 106℃ For the glass transition temperature of homopolymers of monomers other than those exemplified above, the values described in "Polymer Handbook" (3rd edition, John Wiley & Sons, Inc., 1989) shall be used. If the Tg of the homopolymer is not described in the publicly known materials, the value obtained by the following measurement method shall be used. Specifically, 100 parts by weight of monomer, 0.2 parts by weight of azobisisobutyronitrile, and 200 parts by weight of ethyl acetate as a polymerization solvent are charged into a reactor equipped with a thermometer, a stirrer, a nitrogen inlet tube, and a reflux condenser, and stirred for 1 hour while passing nitrogen gas through. After removing oxygen from the polymerization system in this way, the temperature is raised to 63°C and reacted for 10 hours. Then, the mixture is cooled to room temperature to obtain a homopolymer solution with a non-volatile content concentration of 33% by weight. Then, the homopolymer solution is cast and applied onto a release liner, and dried to prepare a test sample (sheet-shaped homopolymer) with a thickness of about 2 mm. This test sample is punched out into a disk with a diameter of 7.9 mm, sandwiched between parallel plates, and the viscoelasticity is measured in shear mode using a viscoelasticity tester (TA Instruments Japan, model name "ARES") while applying a shear strain of 1 Hz at a temperature range of -70 to 150°C and a heating rate of 5°C / min. The peak top temperature of tan δ is taken as the Tg of the homopolymer.
[0024] In some embodiments, the SP value of the polymer (A) is greater than 9.5 (units [(cal / cm 3 ) 1 / 2]. The same applies below.) is suitable, and is preferably 10.0 or more. The polymer (A) having the above SP value can have an SP value that is far from (typically farther from) the SP value of the coating film to be protected. The coating film can be, for example, a urethane coating film formed by the reaction of a polyol (e.g., an acrylic polyol) with a polyisocyanate, or a coating film formed from an acid-epoxy crosslinked acrylic paint. By making the SP value of the polymer (A) far from the SP value of the coating film, the interaction between the coating material containing the polymer (A) and the coating film tends to decrease. This is advantageous from the viewpoint of suppressing the occurrence of peeling failure and the increase in the burden of peeling work due to the peel strength of the coating material from the coating film becoming too high, suppressing deformation (marking) of the coating film due to material transfer between the coating film and the coating material, etc. In some embodiments, the SP value of the polymer (A) may be more than 10.0, may be 10.5 or more, may be 10.8 or more, may be 11.2 or more, or may be 11.5 or more. The upper limit of the SP value of the polymer (A) is not particularly limited. From the viewpoint of easily forming a coating material with well-balanced properties, in some embodiments, the SP value of the polymer (A) is suitably about 14.0 or less, may be 13.5 or less, may be 13.0 or less, may be less than 12.5, may be 12.0 or less, may be less than 12.0, or may be 11.5 or less.
[0025] In this specification, the SP value refers to the value of the solubility parameter calculated from the basic structure of a compound by the method proposed by Fedors. The SP value of the polymer (A) can be adjusted by selecting the composition of the monomer components constituting the polymer (A), specifically, by selecting the types and amount ratios of the monomers contained in the monomer components.
[0026] In some embodiments, the SP value of the polymer (A) is suitably 0.2 or more higher than the SP value of the coating film to be protected, preferably 0.5 or more higher, more preferably 0.7 or more higher, and even more preferably 1.0 or more higher. By combining the polymer (A) and the coating film to be protected having such a difference in SP value, the coating material containing the polymer (A) is likely to achieve good peelability and good anti-marking properties.
[0027] The polymer (A) in the technology disclosed herein is a polymer of monomer components including one or more acrylic monomers. The ratio of the acrylic monomer in the monomer components may be, for example, 5 mol% or more, suitably 10 mol% or more, preferably 15 mol% or more, 25 mol% or more, 35 mol% or more, 45 mol% or more, more than 50 mol%, or more than 70 mol%. In some preferred embodiments, the ratio of the acrylic monomer in the monomer components may be 85 mol% or more, 90 mol% or more, 95 mol% or more, or 100 mol%. In some embodiments, the ratio of the acrylic monomer in the monomer components may be 50 mol% or less, 40 mol% or less, or 30 mol% or less.
[0028] In some embodiments, the monomer components constituting the polymer (A) include at least a (meth)acryloyl group-containing monomer as the acrylic monomer. The (meth)acryloyl group-containing monomer may be used alone or in combination of two or more. The ratio of the (meth)acryloyl group-containing monomer among the monomer components may be, for example, 5 mol% or more, suitably 10 mol% or more, preferably 15 mol% or more, more preferably 20 mol% or more, may be 30 mol% or more, may be 40 mol% or more, may be 45 mol% or more, may be 50 mol% or more, may be 55 mol% or more, or may be 60 mol% or more. The entire monomer component (i.e., 100 mol%) may be a (meth)acryloyl group-containing monomer. From the viewpoint of facilitating compatibility with a calculated Tg of a predetermined value or less and facilitating the formation of a coating material with well-balanced properties, in some embodiments, the proportion of the (meth)acryloyl group-containing monomer in the monomer components is preferably 95 mol% or less, more preferably 90 mol% or less, and may be 85 mol% or less, 80 mol% or less, 75 mol% or less, or 70 mol% or less. The technology disclosed herein can also be implemented in an embodiment in which the proportion of the (meth)acryloyl group-containing monomer in the monomer components is 65 mol% or less, 55 mol% or less, 45 mol% or less, or 35 mol% or less.
[0029] The monomer components constituting the polymer (A) preferably contain at least an alkyl (meth)acrylate as the (meth)acryloyl group-containing monomer. The alkyl (meth)acrylate can be useful for adjusting the storage modulus, adjusting the tensile properties, and adjusting the SP value described later, depending on the selection of the type and amount of use. The alkyl (meth)acrylate can be used alone or in combination of two or more.
[0030] As the alkyl(meth)acrylate, for example, a compound represented by the following formula (1) can be suitably used. CH2=C(R 1 )COOR 2 (1) Here, R in the above formula (1) 1 is a hydrogen atom or a methyl group. 2 is a chain alkyl group having 1 to 20 carbon atoms. Hereinafter, this range of carbon atoms will be referred to as "C 1-20 The chain alkyl group may be linear or branched.
[0031] R 2 C 1-20 Alkyl (meth)acrylate (C 1-20 Specific examples of the alkyl(meth)acrylate include, but are not limited to, methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, isopropyl(meth)acrylate, n-butyl(meth)acrylate, isobutyl(meth)acrylate, s-butyl(meth)acrylate, t-butyl(meth)acrylate, pentyl(meth)acrylate, isopentyl(meth)acrylate, hexyl(meth)acrylate, heptyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, octyl(meth)acrylate, acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.
[0032] Of these, at least C 4-20 Alkyl (meth)acrylate (preferably C 4-14 It is preferable to use at least C alkyl (meth)acrylate, since this can contribute to a decrease in the calculated Tg of the polymer (A). 4-9It is more preferable to use an alkyl acrylate. For example, it is preferable that the monomer component contains one or both of n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA), and it is more preferable that the monomer component contains at least BA.
[0033] Among the monomer components constituting polymer (A), C 1-20 The proportion of alkyl (meth)acrylate may be, for example, 5 mol% or more, suitably 10 mol% or more, preferably 15 mol% or more, 25 mol% or more, 35 mol% or more, 45 mol% or more, 55 mol% or more, or 60 mol% or more. In addition, from the viewpoint of easily realizing suitable film properties, C 1-20 The proportion of alkyl (meth)acrylate is suitably 95 mol % or less, preferably 90 mol % or less, may be 85 mol % or less, may be 80 mol % or less, may be 75 mol % or less, may be 70 mol % or less, or may be 65 mol % or less. 1-20 The ratio of alkyl (meth)acrylate may be 60 mol % or less, 50 mol % or less, 40 mol % or less, or 30 mol % or less.
[0034] The monomer component constituting polymer (A) is C 4-9 In the embodiment containing an alkyl acrylate, among the monomer components, C 4-9 The proportion of alkyl acrylate may be, for example, 5 mol% or more, suitably 10 mol% or more, and from the viewpoint of easily obtaining a lower calculated Tg, it is preferably 15 mol% or more, may be 25 mol% or more, may be 35 mol% or more, may be 40 mol% or more, or may be 45 mol% or more. On the other hand, from the viewpoint of easily obtaining a polymer (A) having a predetermined or higher SP value, C among the monomer components is 4-9The proportion of alkyl acrylate is suitably 80 mol % or less, preferably 70 mol % or less, may be 65 mol % or less, may be 60 mol % or less, or may be 55 mol % or less. 4-9 The ratio of alkyl acrylate may be 50 mol % or less, 40 mol % or less, 30 mol % or less, 25 mol % or less, or 20 mol % or less.
[0035] The monomer components constituting the polymer (A) may contain a combination of an alkyl (meth)acrylate and a monomer other than the alkyl (meth)acrylate. Some examples of monomers other than the alkyl (meth)acrylate include functional group-containing monomers such as carboxy group-containing monomers, hydroxyl group (OH group)-containing monomers, cyano group-containing monomers, amide group-containing monomers, amino group-containing monomers, monomers having a nitrogen atom-containing ring, acid anhydride group-containing monomers, epoxy group-containing monomers, keto group-containing monomers, and alkoxysilyl group-containing monomers. Appropriate use of functional group-containing monomers can increase the cohesive strength of the polymer (A). Functional group-containing monomers can also be useful for adjusting the storage modulus, adjusting tensile properties, and adjusting the SP value described later.
[0036] Examples of the carboxy group-containing monomer include acrylic acid (AA), methacrylic acid (MAA), carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid. Of these, AA and MAA are preferred. Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, etc.; polypropylene glycol mono(meth)acrylate, etc. Among them, preferred hydroxyl group-containing monomers include hydroxyalkyl (meth)acrylates in which the alkyl group is linear and has 2 to 4 carbon atoms.
[0037] Examples of the cyano group-containing monomer include acrylonitrile, methacrylonitrile, and 2-cyanoethyl (meth)acrylate. Among these, acrylonitrile and methacrylonitrile are preferred, and acrylonitrile is particularly preferred. Examples of amide group-containing monomers include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, and diacetone(meth)acrylamide. Examples of the amino group-containing monomer include aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate. Examples of monomers having a nitrogen atom-containing ring include monomers having a structure in which a substituent having a polymerizable functional group is bonded to a nitrogen atom-containing ring, such as N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-vinylmorpholine, N-vinylcaprolactam, and N-(meth)acryloylmorpholine. Other examples include maleimide ring-containing monomers such as N-isopropylmaleimide and N-cyclohexylmaleimide. An example of an isocyanate group-containing monomer is 2-(meth)acryloyloxyethyl isocyanate.
[0038] Examples of the acid anhydride group-containing monomer include maleic anhydride and itaconic anhydride. Examples of the keto group-containing monomer include diacetone (meth)acrylate, vinyl methyl ketone, vinyl ethyl ketone, allyl acetoacetate, and vinyl acetoacetate. Examples of the monomer having an epoxy group include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, and allyl glycidyl ether. Examples of the alkoxysilyl group-containing monomer include 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane.
[0039] The monomer components constituting the polymer (A) may contain other copolymerization components other than the above-mentioned monomers for the purpose of improving cohesive strength, etc. Examples of the other copolymerization components include vinyl ester monomers such as vinyl acetate (VAc), vinyl propionate, and vinyl laurate; aromatic vinyl compounds such as styrene, substituted styrenes (α-methylstyrene, etc.), and vinyl toluene; cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate, cyclopentyl (meth)acrylate, and isobornyl (meth)acrylate; aromatic ring compounds such as aryl (meth)acrylates (e.g., phenyl (meth)acrylate), aryloxyalkyl (meth)acrylates (e.g., phenoxyethyl (meth)acrylate), and arylalkyl (meth)acrylates (e.g., benzyl (meth)acrylate). olefin monomers such as ethylene, propylene, isoprene, butadiene, and isobutylene; chlorine atom-containing monomers such as vinyl chloride and vinylidene chloride; alkoxy group-containing monomers such as methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, and ethyl carbitol (meth)acrylate; vinyl ether monomers such as methyl vinyl ether and ethyl vinyl ether; polyfunctional monomers having two or more (e.g., three or more) polymerizable functional groups (e.g., (meth)acryloyl groups) in one molecule, such as 1,6-hexanediol di(meth)acrylate and trimethylolpropane tri(meth)acrylate; and the like.
[0040] In some embodiments, the monomer component constituting the polymer (A) includes a nitrogen atom-containing monomer. Examples of the nitrogen atom-containing monomer include at least one of the above-mentioned cyano group-containing monomer, amide group-containing monomer, amino group-containing monomer, and monomer having a nitrogen atom-containing ring. The nitrogen atom-containing monomer may be used alone or in combination of two or more. The monomer component preferably includes a combination of an alkyl (meth)acrylate and a nitrogen atom-containing monomer, and C 4-9It is more preferable to use a combination of an alkyl acrylate and a nitrogen atom-containing monomer. The nitrogen atom-containing monomer tends to have a relatively high SP value (for example, a higher SP value than alkyl (meth)acrylate) due to the inclusion of a structural portion containing nitrogen. By appropriately using the nitrogen atom-containing monomer, it becomes easier to obtain a polymer (A) having a predetermined or higher SP value. In addition, the nitrogen atom-containing monomer generally tends to have a high Tg of the homopolymer, and when a nitrogen atom-containing monomer is used as a monomer component constituting the polymer (A), the calculated Tg of the polymer (A) tends to increase. However, when the nitrogen atom-containing monomer and C are used, the calculated Tg of the polymer (A) tends to increase. 4-9 By using an appropriate combination with an alkyl acrylate, it is possible to suitably realize a polymer (A) that satisfies both a predetermined or higher SP value and a predetermined or lower Tg.
[0041] In the embodiment in which the monomer component constituting the polymer (A) contains a nitrogen atom-containing monomer, the ratio of the nitrogen atom-containing monomer in the monomer component can be set so as to obtain the desired effect of use.In some embodiments, the ratio of the nitrogen atom-containing monomer in the monomer component may be, for example, 1 mol% or more, suitably 5 mol% or more, preferably 10 mol% or more, more preferably 15 mol% or more, may be 20 mol% or more, may be 25 mol% or more, may be 30 mol% or more, or may be 35 mol% or more.On the other hand, from the viewpoint of making it easier to make the calculated Tg of the polymer (A) below a predetermined value, the ratio of the nitrogen atom-containing monomer in the monomer component is suitably 70 mol% or less, preferably 65 mol% or less, may be 60 mol% or less, may be 55 mol% or less, may be 50 mol% or less, may be 45 mol% or less, or may be 40 mol% or less.
[0042] In some preferred embodiments, the monomer components constituting the polymer (A) contain at least acrylonitrile as the nitrogen atom-containing monomer. By including acrylonitrile in the monomer components, it becomes easier to realize a coating material that has a good balance between good releasability and good anti-marking properties, and a coating composition that can form the coating material. The proportion of acrylonitrile in the nitrogen atom-containing monomers contained in the monomer components may be, for example, 25 mol% or more, 50 mol% or more, 70 mol% or more, 85 mol% or more, 95 mol% or more, or 100 mol%.
[0043] In an embodiment in which the monomer component constituting the polymer (A) contains acrylonitrile, the proportion of acrylonitrile in the monomer component may be, for example, 1 mol% or more, suitably 5 mol% or more, preferably 10 mol% or more, more preferably 15 mol% or more, may be 20 mol% or more, may be 25 mol% or more, may be 30 mol% or more, or may be 35 mol% or more. On the other hand, from the viewpoint of easily making the calculated Tg of the polymer (A) a predetermined value or less, the proportion of acrylonitrile in the monomer component is suitably 70 mol% or less, preferably 65 mol% or less, may be 60 mol% or less, may be 55 mol% or less, may be 50 mol% or less, may be 45 mol% or less, or may be 40 mol% or less.
[0044] The acid value of the polymer (A) is not particularly limited, and may be, for example, 60 mgKOH / g or less. In some embodiments, from the viewpoint of suppressing the peel strength from the coating film, the acid value of the polymer (A) is advantageously 20.0 mgKOH / g or less, preferably 15.0 mgKOH / g or less, more preferably 12.0 mgKOH / g or less, may be 11.0 mgKOH / g or less, or may be 10.0 mgKOH / g or less. The technology disclosed herein can also be implemented in an embodiment in which the acid value of the polymer (A) is 8.0 mgKOH / g or less, 6.0 mgKOH / g or less, 3.0 mgKOH / g or less, or 1.0 mgKOH / g or less. The acid value of the polymer (A) may be 0 mgKOH / g or higher than 0 mgKOH / g. In some embodiments, from the viewpoint of improving the strength (e.g., breaking strength) of the coating material, the acid value of the polymer (A) may be, for example, 1.0 mgKOH / g or more, 2.0 mgKOH / g or more, 4.0 mgKOH / g or more, or 7.0 mgKOH / g or more. Increasing the strength of the coating material can be advantageous from the viewpoint of improving the peeling workability (e.g., preventing tearing or chipping during peeling).
[0045] The acid value of the polymer (A) is measured according to the potentiometric titration method specified in JIS K0070:1992. As a sample for measuring the acid value, for the polymer (A) contained in the coating material, the coating material is put into chloroform, the resulting mixture is left to stand for 12 hours, and then the mixture is filtered through a filter, and a substance having a weight average molecular weight of 10,000 or more (measured by GPC) is used as a sample. The acid value of the polymer (A) contained in the coating composition is measured using a sample obtained in the same manner as the sample for measuring the acid value of the polymer (A) contained in the coating material after drying the coating composition at 80°C for 3 minutes to form a film (coating material) with a thickness of about 100 μm. The acid value of the polymer (A) contained in the aqueous emulsion of the polymer (A) described later is measured using a sample obtained in the same manner as the sample for measuring the acid value of the polymer (A) contained in the coating composition. More specifically, for example, a precisely weighed sample is added to 50 mL of a solvent obtained by mixing diethyl ether and ethanol in a volume ratio of 4:1, completely dissolved, and a phenolphthalein solution is added as an indicator to prepare a measurement solution. The measurement solution is subjected to potentiometric titration with a 0.1 mol / L potassium hydroxide ethanol solution, and the inflection point of the obtained titration curve is taken as the end point. The acid value is calculated from the following formula. In the examples described later, the acid value of the polymer (A) was measured by this method. Acid value (mgKOH / g)=(B×F×5.611) / S B: Amount of 0.1 mol / L potassium hydroxide ethanol solution added at the end point (mL) F: 0.1 mol / L potassium hydroxide ethanol solution (1.0) S: Amount of sample collected (g)
[0046] In some embodiments of the technology disclosed herein, the monomer component constituting the polymer (A) is a monomer (m T ) and a monomer (m L ) wherein the monomer (m T) may contain a nitrogen atom-containing monomer having a homopolymer Tg of 90° C. or higher. An example of a nitrogen atom-containing monomer having a homopolymer Tg of 90° C. or higher is acrylonitrile (homopolymer Tg: 97° C.). In this embodiment, the polymer (A) may contain a monomer (m L ) and a monomer (m T ) and may further contain other monomers. As the Tg of the homopolymer of each monomer, a value described in a publicly available document is used, as in the case of the glass transition temperature of the homopolymer used to calculate the calculated Tg described above. When the Tg of the homopolymer is not described in the publicly available document, the inflection point temperature of the loss modulus G" obtained by the above-mentioned measurement method is used.
[0047] Monomer (m L ) can be useful for appropriately lowering the calculated Tg of the polymer (A) and improving the mark-preventing properties of the coating material containing the polymer (A). Lowering the calculated Tg of the polymer (A) can also be advantageous from the viewpoint of improving the low-temperature properties of the coating material (e.g., performance such as suppressing crack generation at low temperatures and suppressing cracking or tearing when peeled off from a coating film at low temperatures). L The monomer (m) may have a homopolymer Tg of -30°C or less, and may be selected from, for example, the various monomers listed above, but is not limited thereto. L The monomers (m) may be used alone or in combination of two or more. L Specific non-limiting examples of monomers that can be used as the acrylate include n-butyl acrylate (BA), 2-ethylhexyl acrylate (2EHA), isooctyl acrylate, isononyl acrylate, isoamyl acrylate, 4-hydroxybutyl acrylate (4HBA), methoxyethyl acrylate, ethyl carbitol acrylate, ethoxy-diethylene glycol acrylate, and the like.
[0048] Monomer (m LThe lower limit of the Tg of the homopolymer of each monomer used as monomer (m) is not particularly limited, and may be, for example, −100° C. or higher, −90° C. or higher, or −80° C. or higher. In some embodiments, a monomer having a homopolymer Tg in the range of −60° C. or higher and −40° C. or lower is used as monomer (m L The monomer (m L ), the proportion of monomers having a homopolymer Tg in the range of -60°C or more and -40°C or less may be, for example, 50 mol% or more, 75 mol% or more, 85 mol% or more, 95 mol% or more, or 100 mol%.
[0049] Monomer (m T ) can be useful for improving the cohesive strength and high-temperature properties of the coating material (e.g., suppression of the decrease in storage modulus at high temperatures, peelability at high temperatures, etc.). T The monomers (m) may be used alone or in combination of two or more. T The monomer (m) may contain only one nitrogen atom-containing monomer, or may contain two or more nitrogen atom-containing monomers in combination, or may contain one or more nitrogen atom-containing monomers in combination with another monomer having a homopolymer Tg of 90° C. or higher (i.e., a monomer that does not fall under the category of a nitrogen atom-containing monomer. Hereinafter, this monomer may also be referred to as a "nitrogen atom-free monomer"). TAs the monomer (m), acrylonitrile may be used alone, or acrylonitrile may be used in combination with a nitrogen atom-free monomer having a homopolymer Tg of 90° C. or higher, or acrylonitrile may be used in combination with a nitrogen atom-free monomer having a homopolymer Tg of 90° C. or higher, and a nitrogen atom-containing monomer having a homopolymer Tg of 90° C. or higher (excluding acrylonitrile). The nitrogen atom-free monomer having a homopolymer Tg of 90° C. or higher may be appropriately selected from, for example, the various monomers mentioned above, but is not limited thereto. The above nitrogen atom-free monomer may be used alone or in combination with a nitrogen atom-containing monomer having a homopolymer Tg of 90° C. or higher (e.g., acrylonitrile). Monomer (m T The upper limit of the Tg of the homopolymer of each monomer used as the copolymer (a) is not particularly limited, and may be, for example, 250° C. or lower, 200° C. or lower, or 150° C. or lower.
[0050] Monomer (m T Non-limiting examples of non-nitrogen-containing monomers that can be used as monomer (m) include acrylic acid, methacrylic acid, methyl methacrylate, isobornyl acrylate, isobornyl methacrylate, dicyclopentanyl acrylate, dicyclopentanyl methacrylate, adamantyl acrylate, tert-butyl methacrylate, and the like, with preferred examples being acrylic acid (AA) and methyl methacrylate (MMA). T ) may be used, but are not limited to, acrylonitrile, methacrylonitrile, acryloylmorpholine, acrylamide, etc., with acrylonitrile being a preferred example.
[0051] Monomer (m T The content of the nitrogen atom-containing monomer in the monomer (m) may be, for example, 35 mol % or more, and from the viewpoint of easily realizing suitable film properties, it is appropriate that it is 50 mol % or more, and preferably 60 mol % or more. TThe content of the nitrogen atom-containing monomer in the monomer (m) may be more than 70 mol%, more than 80 mol%, more than 90 mol%, more than 93 mol%, or even 100 mol%. T The content of the nitrogen atom-containing monomer in the copolymer (a) may be 85 mol % or less, 75 mol % or less, 70 mol % or less, or 65 mol % or less.
[0052] In some embodiments, the monomer (m T In this embodiment, the nitrogen atom-containing monomer contained in the monomer (m) includes at least acrylonitrile. T The proportion of acrylonitrile in the nitrogen atom-containing monomer contained in the copolymer (a) may be, for example, 25 mol % or more, 50 mol % or more, 70 mol % or more, 85 mol % or more, 95 mol % or more, or 100 mol %.
[0053] Monomer (m T ) on the body surface containing acrolynitrile, the monomer (m T The content of acrylonitrile in the monomer (m) may be, for example, 35 mol % or more, and from the viewpoint of easily realizing suitable film properties, it is appropriate that it is 50 mol % or more, and preferably 60 mol % or more. T The content of acrylonitrile in the monomer (m) may be greater than 70 mol%, greater than 80 mol%, greater than 90 mol%, greater than 93 mol%, or even 100 mol%. T The acrylonitrile content in the copolymer (a) may be 85 mol % or less, 75 mol % or less, 70 mol % or less, or 65 mol % or less.
[0054] The monomer component constituting the polymer (A) is the monomer (m T ) and monomer (m LIn an embodiment including the above, the proportion of the nitrogen atom-containing monomer having a homopolymer Tg of 90° C. or more in the entire monomer components may be, for example, 20 mol% or more, and from the viewpoint of easily realizing suitable film properties, it is appropriate to be 25 mol% or more (for example, 28 mol% or more), and it is preferably 30 mol% or more, and it may be 35 mol% or more, or it may be 40 mol% or more. The technology disclosed herein can be preferably implemented in an embodiment in which the proportion of the nitrogen atom-containing monomer having a homopolymer Tg of 90° C. or more in the entire monomer components constituting the polymer (A) is more than 50 mol%. In addition, from the viewpoint of flexibility of the coating material, the proportion of the nitrogen atom-containing monomer having a homopolymer Tg of 90° C. or more is appropriately 60 mol% or less, and it is preferably less than 60 mol%. In some embodiments, the proportion of the nitrogen atom-containing monomer having a homopolymer Tg of 90° C. or more may be 57 mol% or less, or it may be 56 mol% or less. The technology disclosed herein can also be practiced in an embodiment in which the proportion of nitrogen atom-containing monomers having a Tg of 90° C. or higher in the homopolymer is 53 mol % or less, 50 mol % or less, or even 40 mol % or less.
[0055] The monomer component constituting the polymer (A) is the monomer (m T ) and monomer (m LIn an embodiment including the above, the content of acrylonitrile in the entire monomer components may be, for example, 20 mol% or more, and from the viewpoint of easily realizing suitable film properties, it is appropriate to be 25 mol% or more (for example, 28 mol% or more), and it is preferably 30 mol% or more, and it may be 35 mol% or more, or it may be 40 mol% or more. The technology disclosed herein can be preferably implemented in an embodiment in which the content of acrylonitrile in the entire monomer components constituting the polymer (A) is more than 50 mol%. In addition, from the viewpoint of flexibility of the coating material, the content of acrylonitrile is appropriately 60 mol% or less, and it is preferably less than 60 mol%. In some embodiments, the content of acrylonitrile may be 57 mol% or less, or may be 56 mol% or less. The technology disclosed herein can also be implemented in an embodiment in which the content of acrylonitrile is 53 mol% or less, 50 mol% or less, or even 40 mol% or less.
[0056] The monomer (m T ) and the above monomer (m L ) molar ratio (m T / m L ) is not particularly limited, and may be, for example, about 0.05 to 3.00, or about 0.10 to 2.00. T / m L ) is, for example, 0.60 or more and 1.50 or less, it is easy to obtain a coating material having a storage modulus in the above range at each temperature. In some embodiments, the ratio (m T / m L ) is preferably less than 1.5, more preferably 1.4 or less, may be 1.35 or less, may be 1.30 or less, may be less than 1.30 (e.g., 1.29 or less), may be 1.28 or less, or may be 1.25 or less. In some embodiments, the ratio (m T / m L) is preferably 0.70 or more, more preferably 0.75 or more, may be 0.90 or more, may be 1.0 or more, or may be more than 1.0. This makes it possible to realize a coating material that has a good balance between good releasability from the coating film and good peeling workability at a high level. T / m L ) may be 1.1 or more, 1.15 or more, 1.20 or more, 1.22 or more, or 1.25 or more.
[0057] The monomer components constituting the polymer (A) are monomers (m T ) and monomer (m L Monomers other than those having a homopolymer glass transition temperature of higher than -30°C and lower than 90°C (hereinafter, monomers (m I The monomer (m I The monomer (m) may be selected from the various monomers mentioned above, but is not limited thereto, so long as the glass transition temperature of the homopolymer falls within the above range. I The monomers (m) may be used alone or in combination of two or more. I Specific non-limiting examples of monomers that can be used as the copolymer include ethyl acrylate (EA), ethyl methacrylate, methyl acrylate (MA), n-butyl methacrylate, isobutyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, vinyl acetate, N-vinyl-2-pyrrolidone, and the like.
[0058] Monomer (m I The amount of monomer (m T ) and monomer (m L In some embodiments, the amount of the monomer (m IThe amount of monomer (m) used is suitably not more than 80 mol % (for example, not more than 40 mol %) of the total monomer components, advantageously not more than 30 mol %, preferably not more than 20 mol %, and more preferably not more than 15 mol %. I The amount of monomer (m) used is preferably 0 mol % or more and less than 10 mol %, for example, 0 mol % or more and less than 5 mol %, of the total monomer components. I The use amount of the monomer (m) is 0 mol % of the total monomer components. I ) is not used.
[0059] <Synthesis of Polymer (A)> The method for obtaining the polymer (A) from the monomer components as described above is not particularly limited. For example, known polymerization methods such as emulsion polymerization, solution polymerization, bulk polymerization, and suspension polymerization can be appropriately adopted. Alternatively, active energy ray irradiation polymerization such as photopolymerization (typically carried out in the presence of a photopolymerization initiator) performed by irradiating light such as UV rays, and radiation polymerization performed by irradiating radiation such as β rays and γ rays may be adopted. Since it is easy to prepare a coating composition in the form of an aqueous emulsion in which the polymer (A) is dispersed in an aqueous solvent, in some preferred embodiments, the polymer (A) is obtained by emulsion polymerization of the monomer components having the composition as described above. As a monomer supply method in the emulsion polymerization method, a lump-feed method in which all the monomer raw materials are supplied at once, a continuous supply (dropping) method, a divided supply (dropping) method, and the like can be appropriately adopted. A part or all of the monomer components may be mixed with water and an emulsifier in advance to emulsify, and the emulsion may be supplied to a polymerization vessel.
[0060] The polymerization temperature can be appropriately selected depending on the type of monomer and solvent used, the type of polymerization initiator, etc. The polymerization temperature is suitably about 20°C or higher, preferably about 40°C or higher, more preferably about 50°C or higher, and may be about 60°C or higher, about 65°C or higher, or even about 70°C or higher. The polymerization temperature is suitably about 170°C or lower (typically about 140°C or lower), and preferably about 95°C or lower (for example, about 85°C or lower). In emulsion polymerization, the polymerization temperature is preferably about 95°C or lower (for example, about 85°C or lower).
[0061] In the polymerization, a known or commonly used thermal polymerization initiator or photopolymerization initiator can be used depending on the polymerization method, polymerization mode, etc. The polymerization initiator can be used alone or in appropriate combination of two or more kinds.
[0062] The thermal polymerization initiator is not particularly limited, but for example, an azo-based polymerization initiator, a peroxide-based initiator, a redox-based initiator formed by combining a peroxide with a reducing agent, a substituted ethane-based initiator, etc. can be used. Examples of azo initiators include 2,2'-azobisisobutyronitrile, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]hydrate, 2,2'-azobis(2-methylpropionamidine)disulfate, 2,2'-azobis(2-methylpropionamidine)dihydrochloride, 2,2'-azobis(2-methylpropionamidine)dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane]dihydrochloride, and 2,2'-azobis(N,N'-dimethyleneisobutylamidine)dihydrochloride. Examples of peroxide initiators include persulfates such as potassium persulfate and ammonium persulfate; benzoyl peroxide, t-butyl hydroperoxide, di-t-butyl peroxide, dicumyl peroxide, dilauroyl peroxide, di-n-octanoyl peroxide, di(4-methylbenzoyl) peroxide, t-butyl peroxybenzoate, t-butyl peroxyisobutyrate, t-hexyl peroxypivalate, t-butyl peroxypivalate, di(2-ethylhexyl) peroxide, and the like. Examples of suitable peroxycarbonates include di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butylperoxydicarbonate, t-butylperoxyneodecanoate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclododecane, 1,1-bis(t-hexylperoxy)cyclohexane, and hydrogen peroxide. Examples of redox initiators include a combination of a peroxide and ascorbic acid (e.g., a combination of hydrogen peroxide and ascorbic acid), a combination of a peroxide and an iron (II) salt (e.g., a combination of hydrogen peroxide and an iron (II) salt), a combination of a persulfate and a metabisulfite (e.g., a combination of ammonium persulfate and sodium metabisulfite), a combination of a persulfate and a hydrogensulfite (e.g., sodium hydrogensulfite), and the like.
[0063] The photopolymerization initiator is not particularly limited, but examples of the photopolymerization initiator that can be used include ketal-based photopolymerization initiators, acetophenone-based photopolymerization initiators, benzoin ether-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzyl-based photopolymerization initiators, benzophenone-based photopolymerization initiators, and thioxanthone-based photopolymerization initiators.
[0064] The amount of the polymerization initiator used is not particularly limited and may be a normal amount depending on the polymerization method, polymerization mode, etc. For example, about 0.001 to 5 parts by weight (typically about 0.01 to 2 parts by weight, for example about 0.01 to 1 part by weight) of the polymerization initiator can be used relative to 100 parts by weight of the monomer to be polymerized.
[0065] In the polymerization, various conventionally known chain transfer agents (which may also be understood as molecular weight regulators or polymerization degree regulators) may be used as necessary. The chain transfer agents may be used alone or in combination of two or more. As the chain transfer agent, mercaptans such as n-dodecyl mercaptan, t-dodecyl mercaptan, and thioglycolic acid may be used. Alternatively, a chain transfer agent that does not contain a sulfur atom (non-sulfur chain transfer agent) may be used. Specific examples of non-sulfur chain transfer agents include anilines such as N,N-dimethylaniline and N,N-diethylaniline; terpenoids such as α-pinene and terpinolene; styrenes such as α-methylstyrene and α-methylstyrene dimer; compounds having a benzylidenyl group such as dibenzylideneacetone, cinnamyl alcohol, and cinnamylaldehyde; hydroquinones such as hydroquinone and naphthohydroquinone; quinones such as benzoquinone and naphthoquinone; olefins such as 2,3-dimethyl-2-butene and 1,5-cyclooctadiene; alcohols such as phenol, benzyl alcohol, and allyl alcohol; and benzyl hydrogens such as diphenylbenzene and triphenylbenzene. When a chain transfer agent is used, the amount used may be, for example, about 0.01 to 1 part by weight based on 100 parts by weight of the monomer components. The technology disclosed herein may also be preferably carried out in an embodiment in which no chain transfer agent is used.
[0066] Emulsion polymerization is usually carried out in the presence of an emulsifier. The emulsifier for emulsion polymerization is not particularly limited, and known anionic emulsifiers, nonionic emulsifiers, etc. can be used. The emulsifier can be used alone or in combination of two or more kinds.
[0067] Non-limiting examples of anionic emulsifiers include sodium lauryl sulfate, ammonium lauryl sulfate, sodium dodecylbenzenesulfonate, sodium polyoxyethylene lauryl sulfate, sodium polyoxyethylene alkyl ether sulfate, ammonium polyoxyethylene alkyl phenyl ether sulfate, sodium polyoxyethylene alkyl phenyl ether sulfate, sodium polyoxyethylene alkyl sulfosuccinate, etc. Non-limiting examples of nonionic emulsifiers include polyoxyethylene alkyl ether, polyoxyethylene alkyl phenyl ether, polyoxyethylene fatty acid ester, polyoxyethylene polyoxypropylene block polymer, etc. Emulsifiers having reactive functional groups (reactive emulsifiers) may be used. Examples of reactive emulsifiers include radical polymerizable emulsifiers having a structure in which a radical polymerizable functional group such as a propenyl group or an allyl ether group is introduced into the above-mentioned anionic emulsifier or nonionic emulsifier.
[0068] The amount of the emulsifier used in emulsion polymerization may be, for example, 0.2 parts by weight or more, 0.5 parts by weight or more, 1.0 parts by weight or more, or 1.5 parts by weight or more, relative to 100 parts by weight of the monomer component. In some embodiments, the amount of the emulsifier used is usually suitably 10 parts by weight or less, preferably 5 parts by weight or less, and may be 3 parts by weight or less, relative to 100 parts by weight of the monomer component.
[0069] In some preferred embodiments, the emulsion polymerization can be carried out in the presence of a protective colloid. Examples of the protective colloid include polyvinyl alcohol polymers (PVA); cellulose derivatives such as hydroxyethyl cellulose, hydroxypropyl cellulose, and carboxymethyl cellulose salts; and natural polysaccharides such as guar gum. The protective colloid can be used alone or in combination of two or more.
[0070] The amount of protective colloid used is suitably 0.1 parts by weight or more relative to 100 parts by weight of monomer components, advantageously 0.3 parts by weight or more, preferably 0.5 parts by weight or more (e.g. 0.7 parts by weight or more), may be 1.0 parts by weight or more, 1.5 parts by weight or more, 2.0 parts by weight or more, or 2.5 parts by weight or more. The amount of protective colloid used relative to 100 parts by weight of monomer components may be, for example, 10 parts by weight or less, 5.0 parts by weight or less, 4.0 parts by weight or less, 3.5 parts by weight or less, 3.0 parts by weight or less, or 2.5 parts by weight or less.
[0071] In some preferred embodiments, emulsion polymerization is carried out in the presence of PVA. The aqueous emulsion of polymer (A) obtained by such emulsion polymerization tends to exhibit the thickening effect by adding a thickener. By using such an aqueous emulsion of polymer (A), a coating composition showing good viscosity characteristics with good sagging prevention properties can be suitably prepared. Carrying out emulsion polymerization in the presence of PVA can be advantageous from the viewpoint of easily obtaining a coating composition showing good viscosity characteristics suitable for slot die coating. As PVA, those corresponding to polymer (B) described later can be preferably used, but are not limited thereto, and PVA not corresponding to polymer (B) may be used, or PVA corresponding to polymer (B) and PVA not corresponding to polymer (B) may be used in combination. In some preferred embodiments, emulsion polymerization for obtaining polymer (A) is carried out in the presence of PVA, and 50% by weight or more (preferably 70% by weight, more preferably 90% by weight or more, and may be 100% by weight) of the PVA is PVA corresponding to polymer (B). The polymer (B) used in this manner during emulsion polymerization is preferably one or more types selected from the group consisting of unmodified PVA and anionic PVA (for example, carboxy-modified PVA).
[0072] The protective colloid (e.g., PVA corresponding to polymer (B)) may be used in combination with the emulsifier as described above, or the protective colloid may be used without using an emulsifier. In some preferred embodiments, the emulsifier and the protective colloid as described above are used in combination. For example, emulsion polymerization can be performed in such a manner that water and a protective colloid are placed in a polymerization vessel, and a part or all of the monomer components are mixed with water and an emulsifier in advance to form an emulsion, which is then fed to the polymerization vessel. When an anionic protective colloid (e.g., anion-modified PVA) is used in combination with an emulsifier, it is preferable to use one or more emulsifiers selected from the group consisting of anionic emulsifiers and nonionic emulsifiers, from the viewpoint of polymerization stability, etc.
[0073] <Polyvinyl alcohol polymer (B)> In the technology disclosed herein, one or more types of PVA having a predetermined degree of saponification and polymerization are used as the polyvinyl alcohol-based polymer (B) (hereinafter, sometimes abbreviated as "polymer (B)"). The use of polymer (B) can improve film-forming properties (e.g., suppression of cracking) and sagging prevention properties when forming a coating film protective coating material from a coating composition in the form of an aqueous emulsion.
[0074] The degree of saponification of the PVA used as the polymer (B) is preferably 80 mol% or more, more preferably 82 mol% or more, and may be 84 mol% or more, 85 mol% or more, 86 mol% or more, 87 mol% or more, 88 mol% or more, 90 mol% or more, or 93 mol% or more, from the viewpoint of drying property when forming a coating film protective coating material from a coating composition in the form of an aqueous emulsion. In some embodiments, as the polymer (B), a PVA having a degree of saponification of 95 mol% or more (e.g., 96 mol% or more, 98 mol% or more, or 99 mol% or more), which is generally referred to as a fully saponified PVA, may be used. In some embodiments, the degree of saponification of the PVA used as the polymer (B) may be, for example, less than 99 mol%, 98 mol% or less, 97 mol% or less, 90 mol% or less (e.g., less than 90 mol%), 89 mol% or less, or 88 mol% or less, from the viewpoint of the above-mentioned film-forming property, etc. A degree of saponification that is not too high can also be advantageous from the standpoint of emulsion stability.
[0075] The degree of polymerization of the PVA used as the polymer (B) is suitably 1200 or less, preferably 1000 or less, and may be 900 or less, 800 or less, 700 or less, 600 or less, or 500 or less, from the viewpoint of the drying property and emulsion stability. The lower limit of the degree of polymerization of the PVA is not particularly limited, and may be appropriately selected so that the effect of use is appropriately exhibited. In some embodiments, the degree of polymerization of the PVA used as the polymer (B) is suitably 200 or more, preferably 300 or more, and may be 400 or more, or may be 500 or more.
[0076] The degree of saponification and degree of polymerization of PVA are measured based on JIS K6726: 1994. When nominal values are provided by the manufacturer or dealer, these values may be used.
[0077] The PVA used as the polymer (B) may be modified or unmodified. One or more modified PVAs may be used in combination with one or more unmodified PVAs. Examples of modified PVAs include anionic modified PVAs having anionic groups such as carboxyl groups, sulfonic acid groups, and phosphoric acid groups introduced therein; cationic modified PVAs having cationic groups such as quaternary ammonium salts introduced therein; and nonionic modified PVAs having an oxyalkylene (e.g., oxyethylene, oxypropylene, etc.) or a polyoxyalkylene structure consisting of repetitions thereof introduced in the side chain. Anionic modified PVAs are obtained, for example, by saponifying a copolymer of a monomer having an anionic group and a vinyl ester (e.g., vinyl acetate). Carboxy groups and sulfonic acid groups are preferred as the anionic groups in the anionic modified PVAs. In some preferred embodiments, one or more selected from the group consisting of unmodified PVAs and anionic modified PVAs (e.g., carboxyl modified PVAs, sulfonic acid modified PVAs, etc.) are used as the polymer (B).
[0078] The polymer (B) contained in the coating composition disclosed herein may be used as a protective colloid when synthesizing the polymer (A) by emulsion polymerization. The polymer (B) contained in the coating composition disclosed herein may be added after the aqueous emulsion of the polymer (A) obtained by emulsion polymerization in the absence of the polymer (B), or may be added during or after the preparation of an aqueous emulsion in which the polymer (A) obtained by a method other than emulsion polymerization (e.g., solution polymerization method) is dispersed in an aqueous solvent. In some preferred embodiments, at least a part of the polymer (B) contained in the coating composition is used as a protective colloid during the emulsion polymerization. The proportion of the polymer (B) used as the protective colloid in the total amount of the polymer (B) contained in the coating composition is, for example, 50% by weight or more, preferably 70% by weight or more, more preferably 90% by weight or more, and may be 100% by weight.
[0079] In the coating composition disclosed herein, the content of polymer (B) relative to 100 parts by weight of polymer (A) (when two or more types of PVA are used as polymer (B), the total content thereof) is suitably 0.3 parts by weight or more, advantageously 0.5 parts by weight or more (for example, 0.7 parts by weight or more), preferably 1.0 parts by weight or more, may be 1.5 parts by weight or more, may be 2.0 parts by weight or more, or may be 2.5 parts by weight or more, from the viewpoint of drying property of the coating composition, etc., the content of polymer (B) relative to 100 parts by weight of polymer (A) is suitably 5.0 parts by weight or less, preferably 4.0 parts by weight or less, may be 3.5 parts by weight or less, may be 3.0 parts by weight or less, or may be 2.5 parts by weight or less. The above-mentioned content of polymer (B) can also be applied to the amount of polymer (B) present relative to 100 parts by weight of the monomer component when polymer (A) is obtained by emulsion polymerization in the presence of polymer (B). It can be advantageous from the viewpoint of polymerization stability when polymer (A) is obtained by emulsion polymerization in the presence of polymer (B) and the stability of the obtained emulsion, etc., if the amount of polymer (B) is not too large.
[0080] The coating composition disclosed herein may further contain a PVA that does not fall under the polymer (B) in addition to the polymer (B). From the viewpoint of making it easier to appropriately exert the effect of using the polymer (B), the content of the PVA that does not fall under the polymer (B) is suitably less than 50% by weight of the total PVA (i.e., the total amount of the PVA that falls under the polymer (B) and the PVA that does not fall under the polymer (B)), preferably less than 20% by weight, and more preferably less than 10% by weight (e.g., less than 5% by weight). The coating composition may be substantially free of the PVA that does not fall under the polymer (B).
[0081] <Other ingredients> The coating composition disclosed herein may contain other optional components as desired. Examples of such optional components include additives such as known thickeners, thixotropic agents, dispersants, defoamers, and inorganic powders. For example, various additives may be added to the aqueous emulsion (polymerization reaction liquid) of polymer (A) obtained by emulsion polymerization as described above to prepare a coating composition in the form of an aqueous emulsion containing the additives. In addition, for example, when an aqueous emulsion of polymer (A) is obtained by emulsion polymerization in the presence of polymer (B), the aqueous emulsion may be used as it is, or may be used after pH adjustment (e.g., adding ammonia water to adjust the pH to about 6 to 8) and / or concentration adjustment (e.g., adding water to adjust the solid content to about 40 to 60% by weight) as a coating composition.
[0082] (Thickener) The thickener can be useful for adjusting the viscosity characteristics of the coating composition.As the thickener, known thickeners such as urethane-based thickeners, cellulose-based thickeners, polyether-based thickeners, and acrylic-based thickeners can be used.The thickener can be used alone or in combination of two or more. Examples of commercially available urethane thickeners include BYK's product names "RHEOBYK-H 3300VF", "RHEOBYK-T 1010", and "RHEOBYK-L 1400", ADEKA's product names "ADEKA NOL UH-450VF", "ADEKA NOL UH-420", "ADEKA NOL UH-462", "ADEKA NOL UH-472", "ADEKA NOL UH-540", "ADEKA NOL UH-756VF", and "ADEKA NOL UH-814N", and San Nopco's "SN Thickener 612", "SN Thickener 621N", "SN Thickener 625N", "SN Thickener 627N", and "SN Thickener 660T". In some embodiments, a urethane association type thickener may be preferably used as the urethane thickener. Suitable examples of the urethane associative thickener include BYK products sold under the trade names "RHEOBYK-H 3300VF," "RHEOBYK-T 1010," and "RHEOBYK-L 1400," and ADEKA products sold under the trade names "ADEKA NOL UH-450VF" and "ADEKA NOL UH-420."
[0083] Examples of the cellulose-based thickener include hydroxyethyl cellulose, carboxymethyl cellulose, methyl cellulose, etc. An example of a commercially available product is "SANHEC L" manufactured by Sansho Corporation. Examples of polyether thickeners include polyethylene glycol, polyether dialkyl ester, polyether dialkyl ether, polyether epoxy modified products, etc. Commercially available products include, for example, the trade name "POLYOX WSR N-80" manufactured by Dow Chemical Company. Examples of acrylic thickeners include acrylic acid polymers such as sodium polyacrylate. Commercially available products include Primal ASE-60, Primal TT-615, and Primal RM-5 manufactured by Rohm and Haas, and SN Thickener 613, SN Thickener 618, SN Thickener 630, SN Thickener 634, and SN Thickener 636 manufactured by San Nopco.
[0084] The amount of the thickener used is not particularly limited, and can be appropriately adjusted so as to obtain the desired viscosity characteristics (for example, BH viscosity measured under conditions of 30 ° C. and 2 rpm). From the viewpoint of suppressing excessive influence on the film properties, in some embodiments, the amount of the thickener used relative to 100 parts by weight of the polymer (A) is suitably 15 parts by weight or less, preferably 10 parts by weight or less, more preferably 5.0 parts by weight or less (for example, 3.0 parts by weight or less), and may be 2.5 parts by weight or less, 2.0 parts by weight or less, or 1.5 parts by weight or less. The lower limit of the amount of the thickener used is not particularly limited, and may be, for example, 0.01 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, 0.3 parts by weight or more, or 0.5 parts by weight or more relative to 100 parts by weight of the polymer (A).
[0085] (Inorganic powder) By adding an inorganic powder to the coating composition, a coating material containing the inorganic powder is formed. With such a coating material, the inorganic powder can block light such as ultraviolet light, and photodegradation of the coating material itself and the coating film protected by the coating material can be suppressed. As the inorganic powder, oxides such as titanium oxide, zinc oxide, magnesium oxide, alumina, and silica; carbonates such as calcium carbonate; sulfates such as barium sulfate; and the like can be used. Inorganic powders that can color the coating film protective coating material white are preferred. With a white coating film protective coating material, the deterioration of the coating material and the coating film can be better suppressed by, for example, suppressing the temperature rise caused by irradiation with sunlight.
[0086] The amount of inorganic powder used relative to 100 parts by weight of polymer (A) can be, for example, 0.5 parts by weight or more, and from the viewpoint of light shielding effect, it is appropriate to set it to 1 part by weight or more, preferably 2 parts by weight or more, more preferably 3 parts by weight or more, and may be 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, or may be 20 parts by weight or more. Also, the amount of inorganic powder used relative to 100 parts by weight of polymer (A) can be, for example, 100 parts by weight or less, and from the viewpoint of strength and film-forming property of the coating material, it is appropriate to set it to 80 parts by weight or less, advantageously 60 parts by weight or less, preferably 50 parts by weight or less, may be 40 parts by weight or less, or may be 30 parts by weight or less.
[0087] In some preferred embodiments, the inorganic powder contains at least titanium oxide (TiO2). Titanium oxide may be used in combination with one or more other inorganic powders (e.g., calcium carbonate). The type of titanium oxide is not particularly limited, and any crystal type of titanium oxide, such as rutile type, anatase type, or brookite type, may be used. Among them, rutile type titanium oxide is preferable. Titanium oxide whose particle surface has been subjected to a coating treatment may be used. The material for coating the titanium oxide particles is not particularly limited, and may be, for example, an inorganic oxide such as silica, alumina, or zinc oxide. A suitable example is a highly weather-resistant type titanium oxide (typically rutile type titanium oxide) whose particle surface is coated with Si-Al2O3 or the like.
[0088] The amount of titanium oxide used relative to 100 parts by weight of polymer (A) can be, for example, 0.1 parts by weight or more, and from the viewpoint of light shielding effect, it is appropriate to make it 0.5 parts by weight or more, preferably 1 part by weight or more, more preferably 2 parts by weight or more, and may be 3 parts by weight or more. Also, the amount of titanium oxide used relative to 100 parts by weight of polymer (A) can be, for example, 30 parts by weight or less, and is appropriate to make it 20 parts by weight or less, preferably 15 parts by weight or less, may be 10 parts by weight or less, or may be 8 parts by weight or less.
[0089] The average particle size of the inorganic powder is not particularly limited. For example, from the viewpoint of obtaining a good light shielding effect, the average particle size of the inorganic powder is preferably 150 nm or more, more preferably 180 nm or more, may be 220 nm or more, or may be 250 nm or more. On the other hand, from the viewpoint of dispersibility in the resin component, the average particle size of the inorganic powder is suitably 2000 nm or less, preferably 1500 nm or less, more preferably 1000 nm or less (e.g., 800 nm or less), may be 500 nm or less, may be 400 nm or less, or may be 350 nm or less. For example, titanium oxide particles having an average particle size of about 250 to 350 nm can be preferably used.
[0090] (thixotropic agent) The thixotropic agent can be useful for adjusting the viscosity characteristics of the coating composition. The thixotropic agent can be, for example, an inorganic material such as bentonite, modified bentonite, montmorillonite, hectorite, etc. The thixotropic agent can be used alone or in combination of two or more kinds. The amount of the thixotropic agent used is not particularly limited, and can be appropriately adjusted to obtain the desired viscosity characteristics. From the viewpoint of suppressing excessive influence on the film properties, in some embodiments, the amount of the thixotropic agent used relative to 100 parts by weight of the polymer (A) is suitably 10 parts by weight or less, preferably 5.0 parts by weight or less, may be 3.0 parts by weight or less, may be 2.5 parts by weight or less, or may be 2.0 parts by weight or less. The lower limit of the amount of the thixotropic agent used is not particularly limited, and may be, for example, 0.01 parts by weight or more, 0.05 parts by weight or more, or 0.1 parts by weight or more relative to 100 parts by weight of the polymer (A).
[0091] The thixotropic agent may also function as a thickener. The thickener and the thixotropic agent as described above may be used in combination, or only one of them may be used. When the thickener and the thixotropic agent are used in combination, the total amount of them used may be, for example, 15 parts by weight or less, 10 parts by weight or less, 5.0 parts by weight or less, 4.0 parts by weight or less, 3.0 parts by weight or less, 2.5 parts by weight or less, 2.0 parts by weight or less, or 1.5 parts by weight or less, relative to 100 parts by weight of the polymer (A). The total amount of the thickener and the thixotropic agent used may be, for example, 0.01 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, 0.3 parts by weight or more, or 0.5 parts by weight or more, relative to 100 parts by weight of the polymer (A), and may be 0.7 parts by weight or more, 1.0 parts by weight or more, or 1.5 parts by weight or more.
[0092] <Properties of Coating Composition> (BH viscosity) The coating composition disclosed herein has a viscosity (V B2 ) is suitably 25 Pa·s or more, advantageously 30 Pa·s or more (e.g. 32 Pa·s or more), preferably 40 Pa·s or more (e.g. 45 Pa·s or more), and more preferably 50 Pa·s or more (e.g. 55 Pa·s or more. As the viscosity measured under such low shear rate conditions increases, the sagging prevention properties of the coating composition applied to the object to be protected (e.g. sagging prevention properties when applied to a vertical surface) tend to improve. On the other hand, from the viewpoint of the defoaming property and leveling property of the coating composition, the viscosity (V B2 ) is suitably 200 Pa·s or less, preferably 150 Pa·s or less, and more preferably 100 Pa·s or less (for example, 80 Pa·s or less).
[0093] In the coating composition disclosed herein, the viscosity (V B20 ) is not particularly limited and may be, for example, about 5 Pa·s to 50 Pa·s. B20) is in the above range, the viscosity (V B2 ) in the above-mentioned range is easily obtained.
[0094] The viscosity of the coating composition measured by a BH viscometer (BH viscosity) is measured at 30°C and at 2 rpm and 20 rpm using a BH viscometer. The rotor used for the measurement is appropriately selected depending on the viscosity. For example, when the measuring device has a scale of 0 to 100, a rotor that falls within the range of 10 to 90 on the scale can be selected for measurement.
[0095] (Rheometer Viscosity) In some embodiments, the coating composition has a shear rate of 100 sec -1 Viscosity at (V R100 The viscosity (V) measured under such high shear rate conditions is preferably 1.0 Pa·s or more, more preferably 1.3 Pa·s or more, may be 1.5 Pa·s or more, may be 2.0 Pa·s or more, or may be 2.3 Pa·s or more. R100 By setting the viscosity (V) to a certain level or higher, the applicability (die coating ability) using a slot die can be improved. R100 The upper limit of the viscosity is not particularly limited, but from the viewpoints of compatibility with defoaming properties, ease of liquid delivery, etc., it is appropriate that the viscosity is 15 Pa·s or less, preferably 10 Pa·s or less, and may be 8.5 Pa·s or less, or may be 6.0 Pa·s or less. The viscosity of the coating composition measured by the rheometer (rheometer viscosity) is measured using a commercially available rheometer (for example, a rheometer viscometer "Rheo Stress 1" manufactured by Haake or an equivalent product) and a cone-type rotor (cone diameter: 35 mm, cone angle: 0.5 deg.) at a shear rate of 0.1 to 2000 sec at 30°C. -1 From the viscosity when it is continuously changed, the shear rate is 100sec -1 The viscosity can be measured by reading the viscosity at
[0096] (pH) The pH of the coating composition disclosed herein is suitably 5.5 or more (preferably 6.5 or more, e.g., 7.0 or more) from the viewpoints of dispersion stability and storage stability of the composition. Also, the pH of the coating composition is suitably 11.0 or less, preferably 10.0 or less, and more preferably 9.0 or less (e.g., 8.0 or less) from the viewpoints of handling of the composition and corrosion inhibition of a coater.
[0097] (solid content) In some embodiments of the coating composition disclosed herein, the solid content of the coating composition is suitably 25% by weight or more (e.g., 35% by weight or more) from the viewpoint of drying efficiency, coatability, etc., and is preferably 40% by weight or more, more preferably 44% by weight or more, from the viewpoint of film-forming properties. In addition, the solid content of the coating composition is suitably 70% by weight or less, preferably 60% by weight or less, and may be 55% by weight or less, or may be 50% by weight or less, from the viewpoint of coatability, emulsion dispersion stability, etc. The solid content of the coating composition can be adjusted by the amount of aqueous solvent used, etc. For example, the solid content of the coating composition can be adjusted by adjusting the amount of aqueous solvent used in emulsion polymerization or by adding water after the completion of emulsion polymerization.
[0098] <Production of Coating Composition> The coating composition disclosed herein can be produced, for example, by a method that includes at least the steps of preparing a polymer emulsion that contains an aqueous solvent, a polymer (A), and a polymer (B) and has a viscosity of 15 Pa·s or less when the solid content is 47% by weight, as measured with a BH viscometer at 30°C and 2 rpm, and adjusting the viscosity of the polymer emulsion so that the viscosity is 25 Pa·s or more, as measured with a BH viscometer at 30°C and 2 rpm. The content of polymer (B) in the polymer emulsion relative to 100 parts by weight of polymer (A) contained in the polymer emulsion may be, for example, 0.05 parts by weight or more, 0.1 parts by weight or more, 0.2 parts by weight or less, or 0.3 parts by weight or more. When the content of polymer (B) relative to 100 parts by weight of polymer (A) contained in the above polymer emulsion is less than 0.3 parts by weight, the content of polymer (B) relative to 100 parts by weight of polymer (A) contained in the final coating composition can be adjusted to any of the above-mentioned ranges (e.g., 0.3 parts by weight or more and 5.0 parts by weight or less) by adding polymer (B) to the polymer emulsion.
[0099] The above polymer emulsion suitably has a viscosity of 0.5 Pa·s or more when the solid content is 47% by weight, as measured by a BH type viscometer at 30°C and 2 rpm, and from the viewpoint of thickening, the viscosity is preferably 1.0 Pa·s or more, and more preferably 1.2 Pa·s or more (e.g., 1.5 Pa·s or more). From the viewpoint of polymerization stability when synthesizing polymer (A) by emulsion polymerization, the above polymer emulsion suitably has a viscosity of 10 Pa·s or less when the solid content is 47% by weight, as measured by a BH type viscometer at 30°C and 2 rpm, advantageously 7.0 Pa·s or less, preferably 5.0 Pa·s or less, and more preferably 4.5 Pa·s or less (e.g., 4.0 Pa·s or less).
[0100] From the viewpoint of dispersion stability and storage stability of the emulsion, the pH of the polymer emulsion is suitably in the range of 5.5 or more (preferably 6.5 or more, for example 7.0 or more) and 9.0 or less (preferably 8.0 or less). A polymer emulsion having the above viscosity at such a pH is preferred. For example, a polymer emulsion having the above viscosity and a pH of about 7.0 to 8.0 (for example about 7.5) is preferred.
[0101] In some embodiments, the solid content of the polymer emulsion is suitably 25% by weight or more or 35% by weight or more, preferably 40% by weight or more, more preferably 44% by weight or more, and suitably 70% by weight or less, preferably 60% by weight or less, may be 55% by weight or less, or may be 50% by weight or less, from the viewpoint of making it easy to make the solid content of the coating composition obtained by using the polymer emulsion fall within any of the above ranges. The solid content of the polymer emulsion can be adjusted by the amount of aqueous solvent used, etc. For example, the solid content of the polymer emulsion can be adjusted by adjusting the amount of aqueous solvent used in emulsion polymerization, or by adding water after the emulsion polymerization is completed.
[0102] <Paint film protection coating material> According to this specification, a coating film protective coating material (hereinafter, sometimes abbreviated as "coating material") formed from any of the coating compositions disclosed herein is provided. The coating material disclosed herein is prepared, for example, by applying (preferably applying by a slot die) the coating composition onto a coating film of an object to be protected and drying it. As a result, for example, as shown in FIG. 1, a coating film protective coating material 10 formed from the coating composition can be provided on a coating film 22 of an object to be protected 20 having the coating film 22.
[0103] Examples of methods for applying the coating composition onto the coating film of the object to be protected include application by a coater such as a die coater or a spray coater, roller application, dip coating, etc. Application by the die coater may be performed by a coating system including a robot arm equipped with a slit die. For example, by controlling the robot arm so that the slit die moves along the shape of the object to be protected while discharging the coating composition in the form of a continuous liquid film (ribbon), the coating composition can be applied efficiently and accurately to the object to be protected even if the object to be protected has a non-planar shape (for example, a complex three-dimensional shape such as the outer panel of an automobile).
[0104] The applied coating composition is preferably dried under heating from the viewpoints of efficient formation of the coating material, high precision, etc. The drying temperature can be, for example, about 40°C to 100°C, and is usually preferably about 60°C to 90°C.
[0105] The thickness of the coating film protective coating material is not particularly limited, but is suitably 20 μm or more from the viewpoint of enhancing the protective effect, and is preferably 50 μm or more from the viewpoint of strength, peeling workability, etc., and is more preferably 70 μm or more (e.g., 85 μm or more), may be 100 μm or more, or may be 120 μm or more. The thickness of the coating material can be adjusted by the application amount and solid content of the coating composition. From the viewpoint of drying property of the applied composition and prevention of dripping, the thickness of the coating material is suitably 300 μm or less, preferably 200 μm or less, and more preferably 180 μm or less (e.g., 150 μm or less).
[0106] Although not particularly limited, the storage modulus (G'(70)) at 70°C of the coating material disclosed herein may be, for example, 0.40 MPa or more. A coating material having a G'(70) of a predetermined value or more can be appropriately peeled off from a coating film without excessive softening even at a temperature higher than room temperature, such as when a protected object provided with the coating material is placed outdoors in summer. From the viewpoint of improving peelability at high temperatures, in some embodiments, G'(70) is advantageously 0.50 MPa or more, preferably 0.60 MPa or more, may be 0.70 MPa or more, may be 0.80 MPa or more, or may be 0.90 MPa or more. The technology disclosed herein can also be implemented in an embodiment in which G'(70) is 1.0 MPa or more, 1.1 MPa or more, or 1.2 MPa or more. In addition, it is preferable that the G'(70) of the coating material is a predetermined value or less from the viewpoint of easily preventing marks on the coating film. The coating material disclosed herein may have a G'(70) of, for example, 1.30 MPa or less, 1.20 MPa or less, 1.10 MPa or less, or 1.00 MPa or less. The technology disclosed herein may also be implemented in an embodiment in which the coating material has a G'(70) of 0.90 MPa or less or 0.80 MPa or less.
[0107] Although not particularly limited, the storage modulus (G'(23)) at 23°C of the coating material disclosed herein may be, for example, 250 MPa or more, 300 MPa or more, 350 MPa or more, 450 MPa or more, or 500 MPa or more. A coating material having a G'(23) of a predetermined value or more is less likely to tear or stretch excessively when peeled off from a coating film at room temperature. This is advantageous from the viewpoint of improving peelability. On the other hand, it is advantageous from the viewpoint of suppressing marks on the coating film if G'(23) is not too high. In addition, it is also preferable from the viewpoint of peeling workability, since it is easy to perform an operation that triggers peeling when peeling off the coating material from the coating film (for example, an operation of scratching the edge of the coating material with a fingernail or the like to lift it from the coating film). In some embodiments, the G'(23) of the coating material can be, for example, 800 MPa or less, 750 MPa or less, 700 MPa or less, 600 MPa or less, 500 MPa or less, or 400 MPa or less.
[0108] In some embodiments of the coating material disclosed herein, the storage modulus of the coating material at -30°C (G'(-30)) is, from the viewpoint of mark-prevention properties, suitably "for example, less than 2200 MPa. From the viewpoint of easily realizing better mark-prevention properties, G'(-30) is preferably 2000 MPa or less, more preferably 1900 MPa or less, may be 1800 MPa or less, may be 1700 MPa or less, or may be 1600 MPa or less. There is no particular lower limit for G'(-30). From the viewpoint of easily forming a coating material in which G'(70) and G'(23) are in an appropriate range, in some embodiments, G'(-30) is suitably 500 MPa or more, preferably 800 MPa or more, more preferably 1000 MPa or more, may be 1200 MPa or more, 1300 MPa or more, or may be 1400 MPa or more.
[0109] The storage modulus (G'(70), G'(23), G'(-30)) of the coating material is measured by the following method. That is, a laminated film with a thickness of about 1 mm is prepared by stacking a plurality of coating materials to be evaluated and integrating them by pressing. The laminated film is punched into a disk shape with a diameter of 7.9 mm to prepare a measurement sample, which is sandwiched between parallel plates, and the viscoelasticity is measured in a shear mode at a temperature range of -70 to 150°C and a heating rate of 5°C / min while applying a shear strain of a frequency of 1 Hz using a viscoelasticity tester, and the storage modulus G' at each temperature is obtained. The above-mentioned coating material is obtained by applying a coating composition to the painted surface (on the coating film) of a coated steel plate, drying it, and then peeling it off from the coated steel plate at room temperature. As the above-mentioned coated steel plate, for example, a coated steel plate prepared by coating a steel plate with an acid epoxy crosslinking type acrylic paint (manufactured by Kansai Paint Co., Ltd., product name "KINO1210TW") is suitably used. As the viscoelasticity tester, a TA Instruments device named "ARES G2" or an equivalent device can be used.
[0110] In some embodiments of the coating material, the glass transition temperature (hereinafter also referred to as "RSA-Tg"), which is determined as the temperature corresponding to the inflection point of the loss modulus G" in viscoelasticity measurement, is suitably 5°C or higher, preferably 15°C or higher, and more preferably 20°C or higher. Furthermore, the RSA-Tg may be, for example, 40°C or lower, 35°C or lower, or 30°C or lower (e.g., 25°C or lower). A coating material having an RSA-Tg within the above range makes it easy to obtain a coating material in which one or more of the above-mentioned G'(70), G'(23), and G'(-30) are within an appropriate range.
[0111] In some embodiments, the breaking strength of the coating material disclosed herein is, for example, suitably 12 N / 25 mm or more, advantageously 15 N / 25 mm or more, preferably 20 N / 25 mm or more, and more preferably 25 N / 25 mm or more (e.g., 30 N / 25 mm or more). For example, a coating material having a breaking strength in the above range at a thickness of about 100 μm to 150 μm (e.g., about 100 μm) is preferred.
[0112] In some embodiments, the elongation at break of the coating material disclosed herein is suitably 100% or more, advantageously 150% or more, preferably 200% or more, may be 220% or more, or may be 250% or more. Such a coating material can disperse stress by being moderately deformed when peeled off from the coating film, so that the break of the coating material due to local stress concentration can be suppressed. The upper limit of the elongation at break is not particularly limited, but is suitably 500% or less, may be 450% or less, or may be 400% or less. It can be advantageous from the viewpoint of increasing the work efficiency at the time of peeling off if the elongation at break is not too large. For example, a coating material having an elongation at break in the above range at a thickness of about 100 μm to 150 μm (for example, a thickness of about 100 μm) is preferred.
[0113] The breaking strength and elongation at break of the coating material are measured by the following method. That is, a measurement sample is prepared from the coating material to be evaluated in the form of a strip with a width of 25 mm (for example, a strip with a width of 25 mm and a length of 100 mm). The measurement sample is set in a tensile tester under an environment of 23°C and 50% RH, and a tensile test is performed with a gauge length of 50 mm and a tensile speed of 0.3 m / min to measure the breaking strength [N / 25 mm] and the elongation at break. The measurement sample can be obtained, for example, by applying a coating composition to the painted surface (on the paint film) of a painted steel plate, drying it, peeling it off from the painted steel plate at room temperature, and cutting it to an appropriate size. As the painted steel plate, for example, a painted steel plate prepared by painting an acid epoxy crosslinking acrylic paint (manufactured by Kansai Paint Co., Ltd., product name "KINO1210TW") on a steel plate is suitable. As a tensile tester, a device named "Tensilon" manufactured by Shimadzu Corporation or an equivalent product can be used.
[0114] In order to obtain good releasability from the coating film, the coating material according to some embodiments of the technology disclosed herein suitably has a peel strength, as measured by the following method, of less than 4.0 N / 25 mm, and preferably less than 2.5 N / 25 mm. [Peel strength measurement] A steel plate coated with an acid epoxy crosslinking acrylic paint (Kansai Paint Co., Ltd., product name "KINO1210TW") is held horizontally with the coated surface facing up. A coating composition is applied to the coated surface (on the coating film) of the coated steel plate so that the thickness of the coating composition is 100 μm in terms of solid content, and the coating composition is dried at 80° C. for 3 minutes to form a film (coating film protective coating material). The coated steel plate is then carried into a thermostatic chamber at 70° C. and held there for 7 days. The coated steel plate is removed from the thermostatic chamber and held in an environment of 23° C. and 50% RH for 30 minutes or more. Two linear cuts (25 mm apart) and a cut perpendicular to the cuts are then made in the film on the coating film, and the film is partially peeled off from the latter cut and set in a tensile tester, and peeled off in a 180° direction at a tensile speed of 0.3 m / min, to measure the peel strength [N / 25 mm] of the film from the coated steel plate. As the tensile tester, for example, a "Tensilon" manufactured by Shimadzu Corporation or an equivalent product can be used.
[0115] In some embodiments, the peel strength is more preferably 2.0 N / 25 mm or less, even more preferably 1.5 N / 25 mm or less, and may be 1.2 N / 25 mm or less, or may be 1.0 N / 25 mm or less. A low peel strength is preferable from the viewpoint of reducing the work load during peeling, and is also advantageous from the viewpoint of suppressing tearing or chipping of the coating material during peeling. In addition, from the viewpoint of obtaining a suitable adhesion to the coating film, the peel strength is appropriately 0.1 N / 25 mm or more, preferably 0.2 N / 25 mm or more, may be 0.3 N / 25 mm or more, may be 0.5 N / 25 mm or more, or may be 0.7 N / 25 mm or more. It is preferable that the peel strength is not too low from the viewpoint of preventing the coating material from being unintentionally peeled off from the coating film during the protection period of the coating film.
[0116] In some embodiments, the breaking strength [N / 25mm] is suitably 5 times or more than the peel strength [N / 25mm], advantageously 8 or more, and preferably 10 or more. When the breaking strength / peel strength ratio is large, there is a tendency that tearing or chipping is less likely to occur when peeling from the coating film to be protected. From this viewpoint, the breaking strength / peel strength ratio may be 15 or more, 20 or more, 25 or more, 30 or more, 35 or more, or 40 or more. The upper limit of the breaking strength / peel strength ratio is not particularly limited, but from the viewpoint of easily achieving both a moderate peel strength and good mark prevention properties, it is suitable to be 100 or less, 80 or less, 70 or less, or 60 or less.
[0117] <Paint film protection method> According to this specification, there is provided a coating film protection method including preparing any of the coating compositions disclosed herein, applying the coating composition onto a coating film of an object to be protected having the coating film, and drying the coating composition to form a coating film protective coating material that temporarily protects the coating film.
[0118] One embodiment of the coating film protection method will be described with reference to FIG. 2. That is, any of the coating compositions disclosed herein is prepared (step S10). This coating composition is applied (for example, by using a slot die) onto a coating film of an object to be protected (step S20). The applied coating composition is dried to form a coating film protective coating material that temporarily protects the coating film (step S30). By providing a coating material on the coating film in this manner, the coating film can be protected from damage and deterioration. The coating material that has completed its protective role is peeled off (for example, by peeling off) from the coating film at a desired timing (step S40).
[0119] The matters disclosed in this specification include the following. [1] A coating composition for forming a coating film protective coating material, The coating composition includes a polymer (A) as a base polymer, which is a polymer of a monomer component including an acrylic monomer, and is in the form of an aqueous emulsion in which the polymer (A) is dispersed in an aqueous solvent; The coating composition further comprises a polyvinyl alcohol-based polymer (B), The polyvinyl alcohol-based polymer (B) has a degree of saponification of 80 mol % or more, The polyvinyl alcohol-based polymer (B) has a degree of polymerization of 1200 or less, The content of the polyvinyl alcohol-based polymer (B) is 0.3 parts by weight or more and 5.0 parts by weight or less based on 100 parts by weight of the polymer (A), The coating composition has a viscosity of 25 Pa·s or more as measured at 30° C. and 2 rpm using a BH type viscometer. [2] The coating composition according to [1] above, further comprising a thickener. [3] The coating composition according to the above [1] or [2], wherein the monomer component constituting the polymer (A) includes a carboxy group-containing monomer. [4] The coating composition according to any one of the above [1] to [3], wherein the monomer component constituting the polymer (A) includes a nitrogen atom-containing monomer. [5] A method for producing the coating composition according to any one of [1] to [4] above, comprising the steps of: preparing a polymer emulsion comprising an aqueous solvent, the polymer (A), and 0.3 parts by weight or more and 5.0 parts by weight or less of the polyvinyl alcohol-based polymer (B) per 100 parts by weight of the polymer (A), the polymer emulsion having a viscosity of 1.0 Pa s or more and 4.5 Pa s or less at a solid content of 47% by weight as measured with a BH type viscometer under conditions of 30°C and 2 rpm; and adjusting the viscosity of the polymer emulsion so that the viscosity, measured using a BH type viscometer at 30°C and 2 rpm, is 25 Pa s or more; A method for producing a coating composition comprising: [6] Preparing the coating composition according to any one of [1] to [4] above; applying the coating composition onto a coating of an object to be protected; and drying the coating composition to form a coating protective coat that temporarily protects the coating; A coating protection method comprising the steps of: [7] The method for protecting a coating film according to the above [6], wherein the coating composition is applied using a slot die. [8] A coating film protective coating material formed from the coating composition according to any one of [1] to [4] above. EXAMPLES
[0120] Below, several experimental examples related to the present invention will be described, but it is not intended that the present invention be limited to those specific examples. In the following description, "parts" and "%" representing the amount used or the content are based on weight unless otherwise specified. In addition, unless otherwise specified, the amount of each material used is based on the amount of active ingredient.
[0121] <Polyvinyl alcohol polymer used> PVA-1: Partially saponified anion-modified polyvinyl alcohol (Mitsubishi Chemical Corporation, product name "Gosenex L-3266") PVA-2: Partially saponified polyvinyl alcohol (Kuraray Co., Ltd., product number 3-80) PVA-3: Partially saponified polyvinyl alcohol (Kuraray Co., Ltd., product number 3-88) PVA-4: Partially saponified polyvinyl alcohol (Denka Co., Ltd., product number B-05) PVA-5: Partially saponified polyvinyl alcohol (Kuraray Co., Ltd., product number 9-88) PVA-6: Partially saponified polyvinyl alcohol (Kuraray Co., Ltd., product number 22-88) PVA-7: Partially saponified polyvinyl alcohol (Kuraray Co., Ltd., product number L-8) PVA-8: Completely saponified anion-modified polyvinyl alcohol (Mitsubishi Chemical Corporation, product name "Gosenex CKS-50") PVA-9: Fully saponified polyvinyl alcohol (Kuraray Co., Ltd., product number 3-98) PVA-10: Fully saponified polyvinyl alcohol (Denka Co., Ltd., product number K-05)
[0122] <Example 1> (Preparation of polymer emulsion) A reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer was charged with 75 parts of ion-exchanged water, and 2.0 parts of PVA-1 was added as a polyvinyl alcohol polymer. After dissolving at room temperature while introducing nitrogen gas, the temperature was raised to 70°C and maintained at that temperature. In a separate container, 25 parts of ion-exchanged water was placed, and 100 parts of monomer components consisting of 44 mol% n-butyl acrylate (BA), 55 mol% acrylonitrile (AN), and 1 mol% acrylic acid (AA) were added to a surfactant solution containing 2 parts of polyoxyalkylene alkenyl ether (Kao Corporation, product name "Latemul PD-420") and 0.5 parts of sodium dodecylbenzenesulfonate (Kao Corporation, product name "Neopelex G-65") dissolved therein, followed by stirring and mixing to prepare a monomer emulsion. The monomer emulsion (containing 100 parts of monomer components), 0.3 parts of sodium metabisulfite aqueous solution (based on solids), and 0.3 parts of ammonium persulfate aqueous solution (based on solids) were added to the reaction vessel over a period of 5 hours while maintaining the system at approximately 70°C, and an emulsion polymerization reaction was carried out. After completion of the addition, the mixture was kept at the same temperature for another 3 hours for aging. The reaction mixture obtained was cooled to room temperature, and then the pH was adjusted to 7.5 by adding 10% ammonium water to obtain a polymer emulsion E1 (solids content 47%) in which the polymer (A), which is a polymer of the monomer, is dispersed in water. The polymer (A) has a calculated Tg of -18.8°C based on the composition of the monomer components, and an SP value of 11.8. The acid value of the polymer (A) was measured by the above-mentioned method, and was found to be 4 mgKOH / g.
[0123] (Preparation of Coating Composition) The obtained polymer emulsion E1 was mixed with 1.0 part of a thickener (manufactured by ADEKA CORPORATION, product name "ADEKA NOL UH-420") per 100 parts of the polymer (A) contained in the polymer emulsion E1 to obtain a coating composition C1 according to this example.
[0124] <Examples 2 to 12 and Comparative Examples 1 to 3> Except for changing the type and amount of polyvinyl alcohol-based polymer used as shown in Table 1, the preparation of polymer emulsion E1 according to Example 1 was similar to that of polymer emulsion E1, and polymer emulsions corresponding to each example were obtained. Coating compositions corresponding to each example were obtained in the same manner as in the preparation of coating composition C1 according to Example 1, except that polymer emulsions corresponding to each example were used instead of polymer emulsion E1.
[0125] <Comparative Example 4> The polymer emulsion of this example was obtained in the same manner as in the preparation of the polymer emulsion E1 of Example 1, except that no polyvinyl alcohol-based polymer was used. A coating composition according to this example was obtained in the same manner as in the preparation of the coating composition C1 according to Example 1, except that the polymer emulsion according to this example was used instead of the polymer emulsion E1. The polymer emulsions according to the above-mentioned respective Examples and Comparative Examples were adjusted to have a solid content of 47% by adding ion-exchanged water as appropriate.
[0126] <Measurement and Evaluation> [Viscosity measurement using a BH type viscometer] Using a BH type viscometer (manufactured by TOKIMEC), the BH viscosity (viscosity before the addition of the thickener) of the polymer emulsion and the BH viscosity (viscosity after the addition of the thickener) of the coating composition according to each example were measured at 30° C. and 2 rpm. The rotors used for the measurement were a No. 2 rotor for the polymer emulsion and a No. 4 rotor for the coating composition.
[0127] [Thickening] Based on the results of the viscosity measurements, the increase in viscosity was calculated using the following formula. Viscosity increase [Pa s] = (viscosity before adding thickener [Pa s]) - (viscosity after adding thickener [Pa s]) Based on the obtained viscosity increase amount, the viscosity increase property was evaluated according to the following three levels. G (Good): Viscosity increase of 30 Pa s or more A (Acceptable): Viscosity increase is 20 Pa s or more but less than 30 Pa s P(Poor): Viscosity increase is less than 20 Pa s
[0128] [Polymerization stability] The polymer emulsion obtained in each example was filtered at room temperature with a 150 mesh nylon filter (bag-shaped) at atmospheric pressure and then used to prepare the coating composition according to each example. Based on the filterability when the atmospheric filtration was performed on about 1 liter of the polymer emulsion, the polymerization stability was evaluated according to the following three levels. G (Good): No emulsion lumps remain on the filter and the filtration speed does not decrease. A (Acceptable): Emulsion lumps or deposits are observed on the filter, but the filtration speed does not decrease. P (Poor): Many emulsion clumps remain on the filter, causing the filtration speed to decrease midway.
[0129] [Film forming property] A steel plate coated with an acid epoxy crosslinking acrylic paint (manufactured by Kansai Paint Co., Ltd., product name "KINO1210TW") was held horizontally with the coated surface facing up. The coating composition according to each example was applied to the coated surface (on the coating film) of the coated steel plate in a square shape of 100 mm length and 100 mm width using an applicator manufactured by TP Giken Co., Ltd., and dried at 80°C for 5 minutes to form a film (coating film protective coating material). The amount of coating composition applied was set so that the thickness in terms of solid content was 120 μm. The film thus formed on the coating surface was visually observed and the film-forming properties were evaluated according to the following three standards. G (Good): No cracks observed. A (Acceptable): Minor cracks are observed, but do not penetrate the film. P (Poor): Obvious cracks are observed, penetrating the film.
[0130] [Drying] In the above film-forming property evaluation, the film was dried at 80° C. for 5 minutes, and then the film was observed and the drying property was evaluated according to the following three levels. Note that if the aqueous solvent remains, the film becomes cloudy. G (Good): No cloudiness (opaqueness) of the film is observed. A (Acceptable): The film is slightly cloudy, but can be peeled off cleanly from the coated steel plate. P (Poor): The film is cloudy and cannot be cleanly peeled off from the coated steel plate.
[0131] [Anti-sagging] A steel plate coated with an acid epoxy crosslinking acrylic paint (manufactured by Kansai Paint Co., Ltd., product name "KINO1210TW") was held horizontally with the coated surface facing up. In an environment of 23°C, the coating composition according to each example was applied to the coated surface of the coated steel plate in a strip shape of 100 mm width and a wet thickness of 400 μm using an applicator manufactured by TP Giken Co., Ltd. Immediately after application, the coated steel plate was stood vertically, and the state of the coating (the composition coated on the coated steel plate) after leaving it for 1 minute was visually observed. Based on the results, the sagging prevention property was evaluated according to the following three levels. G (Good): No sagging or sagging is observed. A (Acceptable): Sagging is observed, but no sagging occurs. P (Poor): Dripping is occurring.
[0132] [Table 1]
[0133] As shown in Table 1, the coating compositions of Examples 1 to 12 had good polymerization stability during synthesis of the polymer (A) contained in the composition, and were all good in the thickening of the polymer emulsion, the drying properties of the composition, film-forming properties, and sagging prevention properties, and were suitable for efficiently forming a high-performance protective film. In contrast, Comparative Examples 1 and 3 had low polymerization stability, and Comparative Examples 2 and 3 had low drying properties. In addition, Comparative Example 4, in which no polyvinyl alcohol-based polymer was used during polymerization, had insufficient thickening properties, film-forming properties, and sagging prevention properties.
[0134] A coating composition was prepared in the same manner as in Example 1, except that 0.1 parts of an antifoaming agent (San Nopco Ltd., Nopco NXZ) was further added to 100 parts of the polymer (A) contained in the polymer emulsion E1. The viscosity of the composition before thickening was 1.9 Pa·s and the viscosity after thickening was 44 Pa·s. The film-forming property, drying property, and sagging prevention property of the coating composition with a viscosity of 44 Pa·s were evaluated by the above-mentioned method, and all were good (evaluation G). On the other hand, a coating composition was prepared in the same manner as in Comparative Example 4, except that 2.0 parts of PVA-3 was further added to 100 parts of the polymer contained in the polymer emulsion obtained in Comparative Example 4. The viscosity before thickening was 0.8 Pa·s and the viscosity after thickening was 13 Pa·s. When the film-forming, thickening, drying and sagging resistance of this coating composition with a viscosity of 13 Pa s was evaluated using the methods described above, the drying properties were good (Grade G), but the film-forming and sagging resistance were insufficient (Grade P).
[0135] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above. [Industrial Applicability]
[0136] The coating composition provided by the technology described in this specification is suitable as a coating composition for forming a coating film protective coating material that is applied to a coating film of an object to be protected to protect the coating film from damage or deterioration such as scratches or stains, and is peeled off from the object to be protected after completing such protective role. The object to be protected may be, for example, a coated metal plate (for example, a coated steel plate used for housing materials, building materials, ships, railway vehicles, automobiles, and other transport equipment) having a coating film on the surface of a metal plate (steel plate, stainless steel plate, aluminum plate, etc.), a synthetic resin plate having a coating film, or a molded product thereof. The coating film protective coating material formed from the above coating composition can be preferably used for protecting a coating film of an article to be protected (an article having a coating film formed by the above coating treatment, for example, a metal plate such as a steel plate or a molded product thereof) that has been painted with a paint of various compositions, such as an acrylic paint, a polyester paint, an alkyd paint, a melamine paint, a urethane paint, an acid-epoxy crosslinking paint, or a composite system thereof (for example, an acrylic-melamine paint, an alkyd-melamine paint), by providing the coating film. [Explanation of symbols]
[0137] 10. Coating protection materials 20 Protected Objects 22 Paint film
Claims
1. A coating composition for forming a paint film protective coating material, The coating composition contains, as a base polymer, a polymer (A) which is a polymer of a monomer component including an acrylic monomer, and is in the form of an aqueous emulsion in which the polymer (A) is dispersed in an aqueous solvent; The coating composition further comprises a polyvinyl alcohol-based polymer (B), The polyvinyl alcohol-based polymer (B) has a degree of saponification of 80 mol % or more, The polyvinyl alcohol-based polymer (B) has a degree of polymerization of 1,200 or less, The content of the polyvinyl alcohol-based polymer (B) is 0.3 parts by weight or more and 5.0 parts by weight or less based on 100 parts by weight of the polymer (A), The coating composition has a viscosity of 25 Pa·s or more as measured by a BH type viscometer at 30° C. and 2 rpm.
2. The coating composition of claim 1 further comprising a thickener.
3. The coating composition according to claim 1 or 2, wherein the monomer component constituting the polymer (A) includes a carboxy group-containing monomer.
4. The coating composition according to claim 1 or 2, wherein the monomer component constituting the polymer (A) comprises a nitrogen atom-containing monomer.
5. 3. A method for producing the coating composition of claim 1 or 2, comprising: preparing a polymer emulsion comprising an aqueous solvent, the polymer (A), and 0.3 parts by weight or more and 5.0 parts by weight or less of the polyvinyl alcohol-based polymer (B) relative to 100 parts by weight of the polymer (A), the polymer emulsion having a viscosity of 1.0 Pa s or more and 4.5 Pa s or less at a solid content of 47% by weight measured at 30°C and 2 rpm using a BH type viscometer; and adjusting the viscosity of the polymer emulsion so that the viscosity, measured using a BH type viscometer at 30° C. and 2 rpm, is 25 Pa s or more; A method for producing a coating composition comprising:
6. Providing a coating composition according to claim 1 or 2; applying the coating composition onto a coating of an object to be protected; and drying the coating composition to form a coating protective coat that temporarily protects the coating; A coating protection method comprising the steps of:
7. The method for protecting a coating according to claim 6, wherein the coating composition is applied by a slot die.
8. A coating film protective coating material formed from the coating composition according to claim 1 or 2.
Citation Information
Patent Citations
Coating for force-feed type roller coating use
JP2004224874A
Coating film protective sheet
JP2011111552A
Coating film protective coat material and coating composition
JP2022176896A
Coating film protective coat material and coating composition
JP2022176897A
Coating film protective coat material and acrylic coating composition
JP2022176898A