Coating liquid and method for manufacturing article
A coating liquid with a low glass transition resin and amino resin fine particles addresses the issues of poor film-forming and adhesion in matte coatings, providing improved film formation and heat resistance.
Patent Information
- Application Number
- JP2023061962
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing coating liquids that impart matte properties to coatings lack adequate film-forming properties and adhesion, leading to issues such as poor appearance, film drop-off, and blocking when heated.
A coating liquid comprising a resin dispersion with a water-dispersible resin having a mass average glass transition point of 100°C or less, combined with amino resin fine particles, which can be dotted on the coating to improve film formation and adhesion.
The solution enhances film-forming properties and adhesion, allowing for a matte coating that maintains a good coating state even when heated, with improved uniformity and resistance to blocking.
Smart Images

Figure 2024148641000001 
Figure 2024148641000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating liquid and a method for producing an article. [Background technology]
[0002] Conventionally, for example, a coating may be provided on a substrate such as a printing medium for the purpose of protecting the substrate. As a method for providing a coating on a substrate, a method using a coating liquid containing a component for forming a coating is known. The coating liquid described in Patent Documents 1 and 2 contains a component such as silica that imparts matte properties to the coating. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2010-229302 A [Patent Document 2] JP 2005-272586 A Summary of the Invention [Problem to be solved by the invention]
[0004] There is a demand for improved film-forming properties in coating fluids that impart matte properties to coating films. [Means for solving the problem]
[0005] In order to solve the above problems, one aspect of the present invention is a coating liquid used for forming a coating on a substrate, the coating liquid comprising (A) a resin dispersion and (B) amino resin fine particles, the (A) resin dispersion containing (a) a water-dispersible resin that is a component that forms the coating, the (B) amino resin fine particles being capable of being scattered throughout the coating, and the (a) water-dispersible resin having a mass average glass transition point of 100°C or lower. Effect of the Invention
[0006] The present invention exhibits the effect of improving the film-forming properties in a coating liquid that imparts matte properties to a coating film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] An embodiment of the coating liquid and the method for producing an article will be described below. <Coating fluid> The coating liquid is used to form a coating film on a substrate. In this specification, a layer of the coating liquid before drying formed by applying the coating liquid to a substrate is referred to as a "coating layer", and a solid film obtained by drying the coating layer is referred to as a "coating".
[0008] Examples of substrates to which the coating liquid is applied include printing media and printed matter. For example, printing media has a substrate layer such as paper. When a coating is provided on the printing media, the coating can be used as a base layer (primer layer) for printing, and printing can be performed on the coating. A printed matter has a substrate layer and a printing layer provided on the substrate layer. When the substrate is a printed matter, a coating can be provided on the printing layer of the printed matter. The coating provided on the printed matter in this way can also be used as a base layer for printing.
[0009] The coating liquid contains (A) a resin dispersion and (B) amino resin fine particles. (A) The resin dispersion contains (a) a water-dispersible resin which is a component for forming a coating. (B) The amino resin fine particles can be scattered in the coating. (a) The water-dispersible resin has a mass average glass transition point of 100°C or lower.
[0010] <(A) Resin dispersion> The water-dispersible resin (a) of the resin dispersion (A) is a resin that can be dispersed in an aqueous dispersion medium. The resin dispersion (A) contains an aqueous dispersion medium that disperses the water-dispersible resin (a). When the aqueous dispersion medium is removed from the coating layer formed by applying the coating liquid, the water-dispersible resin (a) aggregates and adheres. The water-dispersible resin (a) aggregates and adheres in this manner to form a coating. At this time, the amino resin microparticles (B) in the coating layer are retained in the coating.
[0011] The mass average glass transition point of the (a) water-dispersible resin is 100° C. or less, preferably 95° C. or less, and more preferably 90° C. or less. When the mass average glass transition point of the (a) water-dispersible resin exceeds 100° C., the film-forming property of the film is not obtained. In detail, when the dispersion medium is removed from the coating layer, the (a) water-dispersible resin does not sufficiently adhere. This causes the appearance of the film to be poor, and the (B) amino resin fine particles and the like to fall off from the film.
[0012] Furthermore, when the mass average glass transition point of the (a) water-dispersible resin is 100° C. or lower, the adhesion of the coating to the substrate can be easily increased when the coating is heated. The mass average glass transition point of the (a) water-dispersible resin is preferably 50° C. or higher, more preferably 55° C. or higher, and even more preferably 60° C. or higher. When the mass average glass transition point of the (a) water-dispersible resin is 50° C. or higher, it is possible to suppress the occurrence of blocking, which is a phenomenon in which articles having a coating stick to each other via the coating when the articles having a coating are loaded. Furthermore, when the mass average glass transition point of the (a) water-dispersible resin is 50° C. or higher, it is possible to suppress changes in the state of the coating when the articles having a coating are heat-treated.
[0013] When multiple types of water-dispersible resins are used, the mass-average glass transition temperature is the average value of the glass transition temperatures of the multiple types of water-dispersible resins calculated on a mass basis. When one type of water-dispersible resin is used, the mass-average glass transition temperature is the glass transition temperature of that water-dispersible resin. The glass transition temperature of the water-dispersible resin can be measured by differential scanning calorimetry (DSC) or differential thermal analysis (DTA).
[0014] The content of the water-dispersible resin (a) in the coating liquid is preferably 30% by mass or more, more preferably 35% by mass or more, and even more preferably 40% by mass or more. When the content of the water-dispersible resin (a) in the coating liquid is 30% by mass or more, the film-forming properties of the coating can be further improved. This makes it easier to form a dense coating even on a substrate having a substrate layer with liquid absorption properties or a substrate having a water-repellent printing layer.
[0015] Examples of the types of (a) water-dispersible resin include (a1) (meth)acrylic resin, (a2) polyester resin, (a3) urethane resin, polyolefin resin, polyamide resin, vinyl acetate resin, vinyl chloride resin, ionomer, copolymers of these resins, etc. Only one type of (a) water-dispersible resin may be used, or two or more types may be used in combination.
[0016] The water-dispersible resin (a) preferably contains at least one selected from (a1) (meth)acrylic resin, (a2) polyester resin, and (a3) urethane resin. In this case, the print quality can be improved when printing is performed on the coating. In more detail, in general printing, inks such as water-based inks, volatile solvent inks, and oil-based inks, and toners such as liquid toners and powder toners contain a fixing component for the coloring material. Examples of fixing components for the coloring material contained in inks and toners generally include binder resins such as alkyd resins, polyester resins, (meth)acrylic resins, amide resins, and urethane resins, and (meth)acrylic monomers and their polymers, which are the main components of active energy ray-curable inks. The above (a1) (meth)acrylic resins, (a2) polyester resins, and (a3) urethane resins have high affinity for such fixing components for the coloring material, so that when a coating liquid is applied to a printed material, the fixation of the coating to the printed surface of the printed material can be improved. Furthermore, when printing is further performed on the coating of an article having a coating, the wettability of the fixing component of the coloring material to the coating becomes favorable, so that, for example, the printing becomes clear.
[0017] (a1) (meth)acrylic resin refers to a polymer having a (meth)acrylic acid compound as a main constituent unit. (a1) (meth)acrylic resin refers to a (meth)acrylic acid polymer, a modified (meth)acrylic acid polymer, and a copolymer of a (meth)acrylic acid polymer or a modified (meth)acrylic acid polymer with another polymer. A modified (meth)acrylic acid polymer is a (meth)acrylic acid polymer in which a substituent has been introduced into the side chain or terminal group of the (meth)acrylic acid polymer.
[0018] Examples of the (a1) (meth)acrylic resin include poly(meth)acrylic acid and modified products thereof, ethylene (meth)acrylic acid copolymer, propylene (meth)acrylic acid copolymer, styrene (meth)acrylic acid copolymer, urethane (meth)acrylic acid copolymer, vinyl acetate acrylic acid copolymer, vinyl chloride acrylic acid copolymer, etc. From the viewpoint of the physical properties of the resulting coating film, the (a1) (meth)acrylic resin preferably contains a styrene (meth)acrylic acid copolymer.
[0019] (a2) polyester resin refers to a polymer having a compound having an ester bond as a main constituent unit. (a2) polyester resin refers to, for example, a polycondensation product of a polyhydric alcohol and a polycarboxylic acid, a polycondensation product of a polyhydric alcohol and a derivative of a polycarboxylic acid, a resin consisting of a modified product in which a substituent is introduced into the side chain or terminal group of these polycondensation products, and a resin consisting of a copolymer of these polycondensation products and other resins. (a2) polyester resins include, for example, saturated polyester resins, unsaturated polyester resins and modified products thereof, copolymers of saturated polyester resins and other resins, copolymers of unsaturated polyester resins and modified products thereof and other resins, etc. Examples of other resins constituting the copolymer include olefin-based resins, (meth)acrylic resins, amide-based resins, vinyl acetate-based resins, vinyl chloride-based resins, etc.
[0020] (a3) urethane resin refers to a polymer having a compound having a urethane bond as a main constituent unit. (a3) urethane resin specifically refers to, for example, a polycondensation product of a polyhydric alcohol, a polyisocyanate, and a derivative thereof, a polycondensation product of a polyhydric alcohol, a polycarboxylic acid, and a polyisocyanate, a resin consisting of a modified product in which a substituent is introduced into the end or side chain of these polycondensates, and a resin consisting of a copolymer of these polycondensates and other resins. (a3) urethane resins include, for example, ether-type urethane resins, ester-type urethane resins and modified products thereof, copolymers of ether-type urethane resins and other resins, copolymers of ester-type urethane resins and modified products thereof and other resins, etc. Examples of other resins constituting the copolymer include olefin-based resins, (meth)acrylic-based resins, amide-based resins, vinyl acetate-based resins, vinyl chloride-based resins, etc.
[0021] The dispersion medium contained in the (A) resin dispersion liquid is an aqueous dispersion medium containing water. The dispersion medium may contain an organic solvent compatible with water. When the dispersion medium contains an organic solvent, it is possible to improve the drying property and wettability of the coating liquid, and the film-forming property of the (a) water-dispersible resin. In addition, it is possible to suppress deformation of an article having a coating film and to suppress freezing of the coating liquid in a low-temperature environment.
[0022] Examples of organic solvents include methanol, ethanol, propanol, butanol, 3-methoxy-3-methyl-1-butanol, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, diethylene glycol monoisobutyl ether, diethylene glycol monoisobutyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, tripropylene glycol monomethyl ether, dipropylene glycol monopropyl ether, glycerin, triacetin, polyethylene glycol, polypropylene glycol, vinylpyrrolidone, 1,3-dioxolane, 1,3-dioxane, tetrahydrofuran, normal methylpyrrolidone, N,N-dimethylformamide, and acetone.
[0023] The content of the organic solvent in the dispersion medium is, for example, preferably 15% by mass or less, more preferably 10% by mass or less, and further preferably 5% by mass or less. Examples of the (A) resin dispersion include a resin dispersion prepared by emulsion polymerization, a resin dispersion obtained by dispersing a (a) water-dispersible resin in a dispersion medium by a dispersion means such as emulsification or suspension, etc. As the (A) resin dispersion, a commercially available resin dispersion to which a dispersion medium has been added as necessary can be used.
[0024] <(B) Amino resin fine particles> The (B) amino resin fine particles are fine particles of a resin obtained by polycondensation of a compound having an amino group and a compound having an aldehyde group. The (B) amino resin fine particles are dispersed in the dispersion medium of the (A) resin dispersion liquid. The (B) amino resin fine particles are dotted in the coating, forming a minute uneven structure on the surface of the coating. As a result, the coating is imparted with a matte finish by the uneven structure of the coating formed by the (B) amino resin fine particles. By imparting matte finish to the coating, a high-quality matte-toned coating can be obtained. The (B) amino resin fine particles may be present in the coating, or a portion of the (B) amino resin fine particles may be exposed from the surface of the coating.
[0025] The (B) amino resin fine particles can be appropriately selected and used from the viewpoints of dispersibility in the coating liquid, coating suitability of the coating liquid, stability of the coating liquid, etc. Examples of the (B) amino resin fine particles include urea resins, melamine resins, guanamine resins, aniline resins, sulfonamide resins, etc. The (B) amino resin fine particles may be used alone or in combination of two or more kinds.
[0026] From the viewpoint of good dispersibility in the coating liquid, the (B) amino resin fine particles are preferably at least one selected from (B1) a urea resin, (B2) a melamine resin, and (B3) a guanamine resin.
[0027] The content of (B) amino resin microparticles can be adjusted appropriately depending on the level of gloss required for the coating. By adjusting the content of (B) amino resin microparticles so that the gloss of the coating is similar to the inherent gloss of the substrate, an article that makes use of the inherent texture of the substrate can be obtained. In addition, by further suppressing the gloss of the substrate with (B) amino resin microparticles, it is possible to finish the article in a matte finish with a more luxurious feel.
[0028] The content of the (B) amino resin fine particles is preferably 30 parts by mass or less per 100 parts by mass of the (a) water-dispersible resin, from the viewpoint of improving the fluidity of the coating liquid, the dispersibility of the (a) water-dispersible resin, coatability, stability of the coating liquid, etc. The content of the (B) amino resin fine particles is more preferably 27.5 parts by mass or less, and even more preferably 25 parts by mass or less per 100 parts by mass of the (a) water-dispersible resin.
[0029] The shape of the (B) amino resin fine particles may be spherical or amorphous. The (B) amino resin fine particles are preferably spherical from the viewpoint of improving the uniformity of the unevenness of the surface of the coating film and thereby improving the appearance of the coating film.
[0030] The average particle size of the (B) amino resin fine particles is preferably in the range of 1 μm or more and 20 μm or less, more preferably in the range of 1 μm or more and 18 μm or less, and even more preferably in the range of 1 μm or more and 15 μm or less.
[0031] When the average particle diameter of the (B) amino resin fine particles is within the above range, a uniform gloss is imparted to the coating film, and a higher matte effect is obtained. The average particle diameter of the (B) amino resin fine particles is calculated by a dynamic light scattering method, a laser diffraction method, a microscope observation, etc. The above average particle diameter is preferably a particle diameter at 50% cumulative distribution or 90% cumulative distribution.
[0032] (B) The density of the amino resin microparticles is 1.0 g / cm 3 More than 1.6g / cm 3 It is preferable that the density is within the range of 1.2 g / cm or less. 3 More than 1.7g / cm 3 and more preferably within the range of 1.3 g / cm 3 More than 1.6g / cm 3 It is within the following range.
[0033] When the density of the (B) amino resin fine particles is within the above range, the (B) amino resin fine particles are appropriately oriented on the surface and inside of the coating, making it possible to obtain a higher matte effect without impairing the physical properties of the coating.
[0034] <Ingredients other than those listed above> The coating liquid may contain particles other than the amino resin particles (B). Examples of particles other than the amino resin particles (B) include acrylic resin particles, acrylic-styrene resin particles, polyethersulfone resin particles, polyolefin particles, polyamide particles, cellulose acetate particles, silica particles, alumina particles, titanium oxide particles, ceramic particles, glass particles, organic-inorganic composite particles such as acrylic-silica composite particles, and wax particles. The shape of the particles other than the amino resin particles (B) is preferably spherical from the viewpoint of not impairing the uniformity of the uneven structure formed by the amino resin particles (B). The softening point of the particles other than the amino resin particles (B) is preferably higher than the heat treatment temperature from the viewpoint of suppressing deterioration during the heat treatment described below.
[0035] The coating liquid may contain a surface tension adjuster as necessary. The surface tension adjuster is a compound capable of adjusting the surface tension of the coating liquid to a predetermined range. Some surface tension adjusters function as dispersants, which will be described later. Examples of surface tension adjusters include ionic surfactants, nonionic surfactants, and modified silicone oils.
[0036] The coating liquid may contain a dispersant as necessary. The dispersant is also called an emulsifier. It is a component that suppresses particle aggregation by physically or electrically repelling the water-dispersible resin (A) and the amino resin fine particles (B) in the coating liquid. Examples of the dispersant include surfactant-type dispersants, polymer-type dispersants, and low-molecular-weight dispersants.
[0037] The coating liquid may contain a pH adjuster for adjusting the pH of the coating liquid, if necessary. The pH adjuster adjusts the ionization state of the components contained in the coating liquid, and improves the stability of the properties of the coating liquid. Examples of pH adjusters include acids such as lactic acid and citric acid, and salts thereof, and bases such as alkanolamines, potassium carbonate, and sodium hydrogen carbonate.
[0038] The coating liquid may contain an antioxidant as required. The antioxidant suppresses oxidation of the components in the coating liquid. This can suppress the deterioration of the components in the coating liquid. Specifically, it can suppress the change in viscosity of the coating liquid and the separation of the components in the coating liquid. Furthermore, the antioxidant can suppress oxidation of the components of the coating in the coating. This can suppress discoloration of the coating, poor appearance such as cracking, and deterioration of physical properties. Examples of the antioxidant include hindered phenol-based antioxidants and hindered amine-based antioxidants.
[0039] The coating liquid may contain an ultraviolet absorbing agent as necessary. The ultraviolet absorbing agent suppresses deterioration of the coating film when the coating film is exposed to ultraviolet light. Specific examples of deterioration of the coating film include discoloration, poor appearance such as chalking, and deterioration of physical properties. Examples of ultraviolet absorbing agents include benzotriazole-based ultraviolet absorbing agents and amine-based ultraviolet absorbing agents.
[0040] The coating liquid may contain a fluorescent whitening agent as required. The fluorescent whitening agent adjusts the hue of the article by emitting pale fluorescence when the coating is exposed to light. Examples of the fluorescent whitening agent include benzoxazole-based fluorescent whitening agents and coumarin-based fluorescent whitening agents.
[0041] The coating liquid may contain a crosslinking agent as necessary. The crosslinking agent reacts with the functional groups of the coating film to increase the number of chemical bonding points, thereby improving physical properties such as heat resistance and abrasion resistance. Examples of crosslinking agents include isocyanate compounds, carbodiimide compounds, oxazoline compounds, and silane coupling agents.
[0042] The coating liquid may contain a viscosity modifier as necessary. The viscosity modifier is used, for example, to adjust the coating liquid to an appropriate viscosity depending on the coating device. This makes it possible to improve the applicability of the coating liquid by the coating device. Examples of the viscosity modifier include water-soluble polysaccharides such as carboxymethyl cellulose, water-soluble polymer compounds such as polyacrylates, and layered mineral compounds such as layered silicates.
[0043] The coating liquid may contain a preservative as necessary. The preservative suppresses the growth of microorganisms in the coating liquid, thereby suppressing changes in viscosity of the coating liquid, separation of components in the coating liquid, spoilage of components in the coating liquid, etc. Examples of the preservative include antibacterial agents and antifungal agents.
[0044] The coating liquid may contain a coloring material as necessary. The coloring material enhances the expressiveness of the article by adjusting the color tone of the coating. Examples of the coloring material include dyes and pigments.
[0045] The coating liquid may contain an antifoaming agent as necessary. The antifoaming agent exerts at least one of foam breaking, foam suppressing, and defoaming effects on the coating liquid, thereby suppressing deterioration of coatability due to foam inclusion. Examples of the antifoaming agent include silicone-based antifoaming agents, surfactant-based antifoaming agents, polyether-based antifoaming agents, higher alcohol-based antifoaming agents, and mineral oil-based antifoaming agents.
[0046] <Viscosity of coating fluid> The viscosity of the coating liquid measured with a Brookfield viscometer is preferably 1500 mPa·s or less at 20° C. This viscosity is preferably 10 mPa·s or more, more preferably in the range of 20 mPa·s or more and 1000 mPa·s or less, and even more preferably in the range of 30 mPa·s or more and 500 mPa·s or less.
[0047] By setting the viscosity of the coating liquid within the above range, it is possible to form a denser coating on the substrate. Furthermore, when the coating liquid is applied using a general-purpose coating device such as a roll coater or a screen printer, streaks and unevenness in the coating are suppressed, making it possible to obtain a more uniform coating.
[0048] <Preparation of coating liquid> The coating liquid can be prepared by stirring or kneading the above-mentioned raw materials. Examples of stirring or kneading devices include a blade type stirrer, an ultrasonic device, a roll mill, a bead mill, and the like. The coating liquid can also be filtered during preparation of the coating liquid or before use. By filtering the coating liquid, for example, foreign matter, aggregates of fine particles, and the like in the coating liquid can be removed. This makes it possible to further improve the quality of the coating film.
[0049] <Base material> The substrate to which the coating liquid is applied has a substrate layer. Examples of the substrate layer include substrate layers having liquid absorption properties. Examples of the material of the substrate layer having liquid absorption properties include paper and nonwoven fabric. Examples of the paper include coated paper, art paper, lightly coated paper, fine paper, Japanese paper, paperboard, and synthetic paper. Examples of the nonwoven fabric include nonwoven fabrics made of synthetic fibers, semi-synthetic fibers, or natural fibers.
[0050] The substrate layer may be a layer that does not have liquid absorption properties. Examples of the material of the substrate layer include resin, metal, glass, rubber, and ceramics. Examples of the resin of the substrate layer include polyethylene resin, polyester resin, polypropylene resin, acrylic resin, polyamide resin, polycarbonate resin, polystyrene resin, vinyl chloride resin, and metal deposition resin having a metal deposition layer provided on these resins. Examples of the shape of the resin include films, sheets, plates, and other molded products. Examples of the metal of the substrate layer include stainless steel, aluminum, iron, and copper. Examples of the shape of the metal include plates and other molded products.
[0051] The substrate is not limited to a printing medium or a printed matter. That is, an article having a coating film provided on a substrate may be an article having no printed layer. When the substrate is a printed matter, the printing method of the printed layer and the printed components are not particularly limited. Examples of the printing method include offset printing, flexographic printing, gravure printing, screen printing, toner printing, inkjet printing, pad printing, sublimation transfer printing, and the like. Examples of the printed components include water-based ink, volatile solvent ink, oil-based ink, active energy ray curable ink, sublimation ink, liquid toner, and powder toner. The coloring material and color tone of the printed components are also not particularly limited. For example, the ink may be a colored ink using dyes or pigments as coloring materials, or a transparent ink that does not contain coloring materials.
[0052] <Production method> Next, a method for producing an article using the above coating liquid will be described. The article includes a substrate and a coating disposed on the substrate. In the method of manufacturing the article, the substrate may include a coating disposed on one or both sides.
[0053] The method for manufacturing an article includes a coating step of applying a coating liquid to a substrate to provide a coating layer on the substrate, and a coating forming step of drying the coating layer to form a coating. As the coating device used in the coating step, for example, a roll coater, a screen printer, etc. can be used. The amount of coating in the coating step may be adjusted according to the thickness of the coating after the coating step. The thickness of the coating is preferably 1.0 μm or more, more preferably 2.0 μm, and even more preferably 4.0 μm or more. When the thickness of the coating is 1.0 μm or more, it is easy to suppress uneven coating. This makes it possible to suppress, for example, a decrease in print quality when printing is performed on the coating.
[0054] In the drying of the coating layer in the step of forming the coating film, the dispersion medium is removed from the coating layer. Examples of the method for drying the coating layer include air drying using hot or cold air, heating using a heater such as an infrared heater, etc. For example, a heating furnace equipped with a heater or the like may be used to dry the coating layer.
[0055] The drying temperature in the step of forming the coating is preferably T-90 [°C] or higher, more preferably T-80 [°C] or higher, and even more preferably T-70 [°C] or higher, when the mass average glass transition point of the (a) water-dispersible resin is T [°C]. In this case, for example, it is possible to shorten the film formation time. The drying temperature in the step of forming the coating is preferably T+200 [°C] or lower, more preferably T+150 [°C] or lower, and even more preferably T+100 [°C] or lower, when the mass average glass transition point of the (a) water-dispersible resin is T [°C]. In this case, the influence of heat on the substrate can be suppressed. The drying temperature referred to here refers to the environmental temperature, the surface temperature of the substrate, the blowing temperature during air drying, the heater temperature of the infrared heater, the set temperature of the heating furnace, and the like.
[0056] A cleaning process for cleaning the substrate beforehand can be carried out before the coating process. In the cleaning process, contaminants such as sebum and hydraulic oil adhering to the substrate are removed. By carrying out the cleaning process, the quality of the substrate is made uniform, so that it is possible to reduce the number of defective products. In addition, a surface modification process for modifying the surface of the substrate can be carried out before the process of applying the coating liquid to the substrate. Examples of the surface modification process include discharge treatments such as ultraviolet irradiation, corona treatment, and plasma treatment.
[0057] The method for manufacturing an article may further include a heat treatment step of heat-treating the coating. By carrying out the heat treatment step, the adhesion of the coating to the substrate can be improved. In the heat treatment step, for example, at least one of non-contact heating and contact heating can be used.
[0058] Non-contact heating can be performed, for example, by blowing hot air onto the coating, irradiating heat rays, etc. Examples of heat rays used in irradiating heat rays include infrared rays. The heating temperature in non-contact heating is preferably 150° C. or higher, more preferably 200° C. or higher. The heating temperature in non-contact heating is preferably 300° C. or lower, more preferably 250° C. or lower. The heating time in non-contact heating is, for example, within a range of 10 seconds or more and 30 seconds or less.
[0059] In contact heating, for example, a heating member is brought into contact with the coating. Examples of the heating member include a heater having a flat contact surface, a heat roller, and the like. The heating temperature in contact heating is preferably 100° C. or higher, and more preferably 110° C. or higher. The heating temperature in contact heating is preferably 180° C. or lower, and more preferably 160° C. or lower. When a heat roller is used, the heating time in contact heating is, for example, within the range of 0.5 m / min or higher and 25 m / min or lower.
[0060] From the viewpoints of productivity, thermal conductivity, and the like, the heat treatment method in the heat treatment step is preferably at least one of non-contact heating using heat rays and contact heating using a heat roller. The method for manufacturing an article may further include a printing step of providing a printing layer on the coating. The printing method in the printing step is not limited, but an inkjet method is preferred from the viewpoint of printability. The printing components and printing colors used in the printing step are not limited. The ink used in the printing step may be colored or colorless and transparent. In the printing step, it is preferable to use at least one of a volatile solvent ink and an active energy ray curable ink from the viewpoint of excellent curability of the ink.
[0061] When the method for producing an article includes the above-mentioned heat treatment step and the above-mentioned printing step, the heat treatment step may be performed before or after the printing step. The obtained article may be processed into a predetermined shape by cutting, creasing, or the like, as necessary. Examples of uses of the article include posters, recording media (product tags, etc.), packaging materials (cosmetic boxes, etc.), cards (greeting cards, business cards, etc.), stationery (pocket holders, etc.), etc.
[0062] <Actions and Effects of the Present Embodiment> Next, the operation and effects of this embodiment will be described. (1) The coating liquid is used for forming a coating on a substrate. The coating liquid contains (A) a resin dispersion and (B) amino resin fine particles. (A) The resin dispersion contains (a) a water-dispersible resin, which is a component for forming a coating. (B) The amino resin fine particles can be scattered in the coating. (a) The water-dispersible resin has a mass average glass transition point of 100°C or lower.
[0063] According to this configuration, a coating film having a matte finish can be obtained by the amino resin fine particles (B). In addition, since the mass average glass transition point of the water-dispersible resin (a) is 100° C. or less, the film-forming property can be improved. Therefore, the film-forming property can be improved in the coating liquid that imparts a matte finish to the coating film.
[0064] (2) The content of the (B) amino resin fine particles is preferably 30 parts by mass or less per 100 parts by mass of the (a) water-dispersible resin, which can improve the dispersibility of the (a) water-dispersible resin, coatability, stability of the coating liquid, etc.
[0065] (3) The amino resin fine particles (B) are preferably spherical fine particles. The average particle size of the amino resin fine particles (B) is preferably in the range of 1 μm or more and 20 μm or less. In this case, a uniform gloss is imparted to the coating film, and a higher matte effect is obtained.
[0066] (4) The amino resin fine particles (B) preferably contain at least one selected from the group consisting of (B1) urea resin fine particles, (B2) melamine resin fine particles, and (B3) guanamine resin fine particles, which can enhance the dispersibility of the amino resin fine particles (B) in the coating liquid.
[0067] (5)(B) The density of the amino resin microparticles is 1.0 g / cm 3 More than 1.6g / cm 3 It is preferable that the range is as follows: In this case, the (B) amino resin fine particles are appropriately oriented on the surface and inside of the coating, so that a higher matte effect can be obtained without impairing the physical properties of the coating.
[0068] (6) (a) The water-dispersible resin preferably contains at least one selected from (a1) a (meth)acrylic resin, (a2) a polyester resin, and (a3) a urethane resin, which can improve the print quality when printing is performed on the coating of an article having a coating.
[0069] (7) The viscosity of the coating liquid measured with a Brookfield viscometer is preferably 1500 mPa s or less at 20°C. In this case, it is possible to form a dense coating on the substrate. In addition, in this case, when the coating liquid is applied using a general-purpose coating device such as a roll coater or a screen printer, streaks and unevenness in the coating are suppressed, making it possible to obtain a more uniform coating.
[0070] (8) The content of the water-dispersible resin (a) in the coating liquid is preferably 30% by mass or more. In this case, the film-forming properties of the coating can be further improved. As a result, even if the substrate has a substrate layer having liquid absorption properties or a printed layer having water repellency, a dense coating can be easily formed on the substrate layer or the printed layer. Therefore, it is possible to improve the fixation of the coating to the substrate.
[0071] More specifically, for example, on a water-repellent surface such as a printed surface using toner, the coating layer formed by applying a coating liquid may gradually shrink due to the repelling of water. By increasing the content of (a) water-dispersible resin, the rate at which the coating layer shrinks can be delayed. This makes it easier to form a uniform coating from (a) water-dispersible resin in the coating layer, for example.
[0072] In addition, for example, when a coating is formed on a substrate layer having liquid absorption properties such as bulky paper such as high-quality paper, a dense coating is easily formed. This makes it possible to suppress the ink from penetrating into the substrate layer having liquid absorption properties such as paper when printing is performed on the surface of the coating. Therefore, it is possible to improve the print quality when printing is performed on the coating. In addition, when an active energy ray curable ink is used as the ink, it is possible to suppress the ink from penetrating into the substrate layer having liquid absorption properties such as paper, and therefore it is possible to promote the curing of the ink.
[0073] (9) The substrate may have a substrate layer having liquid absorption properties. The above-mentioned coating liquid can form, for example, a coating having good adhesion and uniformity on the substrate layer having liquid absorption properties and the printed layer provided on the substrate layer. For example, by printing on the coating provided on the substrate layer having liquid absorption properties, it is possible to suppress the ink from penetrating into the substrate layer. This improves the color development of the ink. In addition, for example, when printing is performed on the coating using an active energy ray curable ink, the ink tends to remain on the surface of the coating, and therefore the curing of the ink can be promoted.
[0074] (10) The coating can be used as a base layer for printing. In this case, the coating exhibits good printability. Therefore, it is possible to improve the quality of printing on the coating. (11) The substrate may be a printed matter having a substrate layer and a printed layer provided on the substrate layer. A coating film may be provided on the printed layer of such a printed matter. The coating liquid has good coatability on the printed layer of the printed matter, and therefore the coating film has good adhesion to the printed layer.
[0075] In particular, when the substrate has a printed layer printed with powder toner, the printed layer often contains a thermoplastic resin and wax as printing components. Even in such a printed matter, the wettability of the coating liquid to the printed layer is ensured, making it possible to form a dense coating. This increases the contact area between the coating and the printed surface, thereby improving the fixability of the coating. Furthermore, by subjecting the coating to a heat treatment, the coating is fused to the printing components in the printed layer of the printed matter, making it possible to further improve the adhesion of the coating.
[0076] (12)(a) The water-dispersible resin has a mass-average glass transition point of 100° C. or less, and therefore the adhesion of the coating to the substrate can be improved when the substrate is heated. Therefore, even when a coating having a matte finish is heated, it is possible to obtain a coating that can maintain its good condition.
[0077] (13) In the coating liquid, for example, by adjusting the content of the amino resin fine particles (B), it is possible to adjust the matte effect of the coating film. In addition, since the amino resin fine particles (B) have good dispersibility in the aqueous dispersion medium of the resin dispersion medium (A), it is possible to obtain a relatively high matte effect even with a small content. In addition, the viscosity of the coating liquid containing the amino resin fine particles (B) is unlikely to increase even if the content of the amino resin fine particles (B) is increased. Therefore, it is possible to obtain a coating liquid with a viscosity range suitable for a general coating device. Therefore, it is possible to provide a coating liquid that can be used for a relatively wide range of applications. In addition, since the amino resin fine particles (B) are thermosetting resin particles, they are unlikely to change in quality during heat treatment of the coating film. Therefore, for example, it is possible to suppress changes in the gloss of the coating film after heat treatment.
[0078] (14)(a) The water-dispersible resin preferably has a mass-average glass transition point of 50° C. or higher. In this case, the occurrence of blocking can be suppressed. In addition, even if the coating is heated, the coating can be prevented from becoming undesirably sticky.
[0079] (15) A method for manufacturing an article includes a coating step of applying a coating liquid to a substrate to form a coating layer on the substrate, and a coating step of drying the coating layer to form a coating. According to this method, a coating having a matte property can be obtained, which can maintain its condition well even when heated.
[0080] (16) The method for producing an article may further include a printing step of providing a printed layer on the coating. In the printing step, it is preferable to use an inkjet method. In this case, a high-quality printed layer can be provided by utilizing the printability of the coating.
[0081] (17) In the printing step, it is preferable to use at least one of a volatile solvent ink and an active energy ray curable ink. In this case, since the ink has excellent curing properties, the productivity of an article having a printed layer on a coating film can be increased.
[0082] (18) The method for producing an article may further include a heat treatment step of heat treating the coating, which can improve, for example, the adhesion of the coating to the substrate. (19) In the heat treatment step, at least one of the following heating methods may be used: non-contact heating using blowing hot air or irradiating the coating with heat rays, and contact heating using a heating member in contact with the coating. For example, such a heating method can improve the adhesion of the coating to the substrate. EXAMPLES
[0083] Next, examples and comparative examples will be described. (Examples 1 to 11) In Examples 1 to 11, each raw material was placed in a container so as to obtain the composition shown in Table 1, and a dispersion was prepared by stirring at room temperature using a stirrer equipped with a dispersing blade until no aggregates were found. Next, a coating liquid was prepared by filtering the dispersion using a mesh strainer with a pore size of 100 μm (manufactured by Big Corporation, product name: Microstrainer 130UU). The viscosity of the obtained coating liquid was measured at 20° C. using a B-type viscometer (manufactured by Toki Sangyo Co., Ltd., product name: BLII).
[0084] In Table 1, the units of the numerical values showing the compositions are mass %. The abbreviations in Table 1 are as follows. "(A) Resin Dispersion A11" is a resin dispersion containing (a1) a (meth)acrylic resin and an aqueous dispersion medium (manufactured by GOO Chemical Industry Co., Ltd., product name: Plussize OP-905, resin content: 40 mass %, glass transition point: 65°C).
[0085] "(A) Resin Dispersion A12" is a resin dispersion containing (a1) a (meth)acrylic resin and an aqueous dispersion medium (manufactured by BASF, product name: JONCRYL PDX-7700, resin content: 48 mass%, glass transition point: 80°C).
[0086] "(A) Resin Dispersion A13" is a resin dispersion containing (a1) a (meth)acrylic resin and an aqueous dispersion medium (manufactured by BASF, product name: JONCRYL PDX-7777, resin content: 46 mass%, glass transition point: 40°C).
[0087] "(A) Resin Dispersion A14" is a resin dispersion containing (a1) a (meth)acrylic resin and an aqueous dispersion medium (manufactured by BASF, product name: JONCRYL PDX-7177, resin content: 36 mass%, glass transition point: 113°C).
[0088] "(A) Resin dispersion A2" is a resin dispersion containing (a2) polyester resin and an aqueous dispersion medium (manufactured by Takamatsu Oil Co., Ltd., product name: PESRESIN A-645GH, resin content: 30 mass %, glass transition point: 55°C).
[0089] "(A) Resin Dispersion A3" is a resin dispersion containing (a3) a urethane resin and an aqueous dispersion medium (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name: Superflex 870, resin content: 30 mass %, glass transition point: 78°C).
[0090] "(A) Resin Dispersion A4" is (a) a resin dispersion containing a vinyl chloride resin and an aqueous dispersion medium (manufactured by Nissin Chemical Industry Co., Ltd., product name: Vinyblan 900, resin content: 40 mass %, glass transition point: 70°C).
[0091] "(B) Amino resin microparticles B11" are spherical microparticles of urea resin (manufactured by Deuteron, product name: MK-F6, D50 particle size: 3.5 μm, D90 particle size: 6.5 μm, density: 1.47 g / cm 3 ).
[0092] "(B) Amino resin microparticles B12" are spherical microparticles of urea resin (manufactured by Deuteron, product name: SF505, D50 particle size: 7 μm, D90 particle size: 13 μm, density: 1.47 g / cm 3 ).
[0093] "(B) Amino resin microparticles B2" are spherical microparticles of melamine resin (manufactured by Nippon Shokubai Co., Ltd., product name: Eposter S12, D50, particle size: 1.2 μm, density: 1.5 g / cm 3 ). "(B) Amino resin microparticles B31" are spherical microparticles of guanamine resin (manufactured by Nippon Shokubai Co., Ltd., Eposter M05, D50, particle size: 5 μm, density: 1.4 g / cm 3 ).
[0094] "(B) Amino resin microparticles B32" are spherical microparticles of guanamine resin (manufactured by Nippon Shokubai Co., Ltd., product name: Eposter L15, D50, particle size: 9 μm, density: 1.4 g / cm 3 ). In addition, ion-exchanged water was added as a dispersion medium for adjusting the concentration, as necessary, in the amounts shown in the "ion-exchanged water" column of Table 1.
[0095] The mass average glass transition temperature in Table 1 is the average value of the glass transition temperature of the water-dispersible resin (a) contained in the coating liquid of each example, calculated on a mass basis, and is represented by the following formulas (1-1) and (1-2).
[0096] T P [℃]=(P / D)×P t …(1-1) T P [℃]: The glass transition temperature of water-dispersible resin P by mass among water-dispersible resins P, Q, R, etc. P: Content of water-dispersible resin P in the coating liquid [mass%] D: Total amount of water-dispersible resin in the coating liquid [mass%] P t : Glass transition temperature of water-dispersible resin P [℃] The content [mass %] of water-dispersible resin P is calculated by: content P1 [mass %] of resin dispersion containing water-dispersible resin P in the coating fluid × resin content P2 [mass %] in the resin dispersion / 100.
[0097] For the water-dispersible resins Q and R blended in the coating liquid, T Q [℃], T R Calculate [°C]···. Mass average glass transition temperature [℃] = (T P +T Q +T R +···)…(1-2) The content ratio [parts by mass] of (B) amino resin fine particles in Table 1 is the part by mass of the total amount of (B) amino resin fine particles when the total amount of (A) water-dispersible resin in the coating liquid is 100 parts by mass, and is expressed by the following formula (2).
[0098] (B) Content of amino resin fine particles [parts by mass] = (B) Total amount of amino resin fine particles [% by mass] / (A) Total amount of water-dispersible resin [% by mass] × 100 ... (2) (Comparative Examples 1 to 4) In Comparative Examples 1 to 4, coating solutions were prepared and the viscosities were measured in the same manner as in Examples 1 to 11, except that the compositions were changed as shown in Table 2.
[0099] In Table 2, the units of the numerical values showing the compositions are mass %. The abbreviations in Table 2 are as follows. "Microparticles C1" are microparticles other than the (B) amino resin microparticles, and are polyamide spherical microparticles (manufactured by ARKEMA, trade name: ORGASOL2001 UD NAT1, D50 particle size: 5 μm).
[0100] "Microparticles C2" are microparticles other than (B) amino resin microparticles, and are polyamide spherical microparticles (manufactured by ARKEMA, product name: ORGASOL2002 E53 NAT3, D50 particle size: 30 μm).
[0101] "Microparticles C3" are microparticles other than (B) amino resin microparticles, and are amorphous silica microparticles (manufactured by Nippon Aerosil Co., Ltd., trade name: AEROSIL200, D50 particle size: 12 μm).
[0102] In addition, ion-exchanged water was added as a dispersion medium for adjusting the concentration, as necessary, in the amounts shown in the "ion-exchanged water" column of Table 1. The total content ratio of fine particles in Table 2 [parts by mass] is the total amount of (B) amino resin fine particles and other fine particles when the total amount of (A) water-dispersible resin in the coating liquid is 100 parts by mass, and is expressed by the following formula (3).
[0103] Total content of fine particles [parts by mass] = (B) Total amount of amino resin fine particles and other fine particles [mass%] / (A) Total amount of water-dispersible resin [mass%] × 100...(3) (Preparation of evaluation samples) A partial print sample was obtained by printing a solid black image on half of a substrate (printing media, manufactured by Oji F-Tex, product name: OK Musilinter C) using a dry toner printer (manufactured by Xerox, product name: Versant 180 Press). This substrate has liquid absorption properties. The partial print sample has a portion consisting of only the substrate layer and a portion in which the substrate layer and the printing layer are laminated.
[0104] A coating liquid was applied to this partial print sample using a bar coater to provide a coating layer, and then the coating layer was dried by blowing hot air onto it so that the surface temperature of the substrate became 35°C, thereby obtaining an evaluation sample having a coating. The amount of coating liquid applied was adjusted to a coating amount that would result in a coating thickness of 2 μm.
[0105] In the following description, the "coating on the printed surface" of the evaluation sample refers to the coating provided on the printed portion of the evaluation sample where a solid black image is printed, and the "coating on the non-printed surface" refers to the coating provided on the portion where a solid black image is not printed.
[0106] (Evaluation of film-forming properties) The appearance of the coating of the evaluation sample obtained by the above method was visually observed, and the presence or absence of any adhesion to the finger when the surface of the coating was stroked with the pad of a finger was confirmed, and the film-forming property was evaluated according to the following evaluation criteria. The results are shown in Tables 1 and 2.
[0107] If the appearance of the coating was normal and no residue was found on the fingers when the surface of the coating was rubbed with the pads of the fingers, the coating was evaluated as having excellent film-forming properties (◯). When any part that was not in the form of a film was confirmed by external observation, and when the surface of the coating was rubbed with the pad of a finger and a powdery residue was found on the finger, the coating was evaluated as having poor film-forming properties (×).
[0108] (Evaluation of blocking resistance) Six evaluation samples obtained by the above method were stacked with the coating surface facing up to obtain a laminate. A 5 mm thick, 5 cm square glass plate was placed on the coating of the printed surface of the evaluation sample of the top layer of the laminate, and a 1 kg weight was placed on the glass plate. In this state, it was left in an environment of 40°C for 7 days. After 7 days, the weight and glass plate were removed, and the blocking resistance was evaluated according to the following evaluation criteria for the parts of the glass plate of the test sample, which are the second to sixth layers from the top of the laminate, where the load was applied. The results are shown in Tables 1 and 2.
[0109] When the evaluation samples were not stuck to each other, they were evaluated as having excellent blocking resistance (◯). When the evaluation samples were found to be stuck to each other in one or more places, the blocking resistance was evaluated as poor (×).
[0110] (Evaluation of printing surface coatability) The appearance of the coating on the printed surface of the evaluation samples obtained by the above method was visually observed, and the coatability of the coating liquid on the printed surface was evaluated according to the following evaluation criteria. The results are shown in Tables 1 and 2.
[0111] When the coating on the printed surface had no visible streaks or repelling and had a uniform appearance, it was evaluated as having excellent print surface coating properties (◯). When slight streaks or repelling were visually observed in the coating on the printed surface, the coating property on the printed surface was evaluated as slightly poor (Δ).
[0112] When obvious streaks or repelling were visually observed in the coating on the printed surface, the coating property on the printed surface was evaluated as poor (×). (Evaluation of adhesion of coating) The coating on the non-printed side and the coating on the printed side of the evaluation sample were rubbed with a finger, and the appearance of the coating was visually observed, and the fixation of the coating was evaluated according to the following evaluation criteria. The results are shown in Tables 1 and 2.
[0113] When the coating on the non-printed surface and the coating on the printed surface were rubbed, and there was no lifting or peeling of the coating, the coating was evaluated as having excellent fixability (◯). When the coating on the non-printed surface or the coating on the printed surface was rubbed, if the coating on the non-printed surface or the coating on the printed surface lifted or peeled off, the fixability was evaluated as poor (×).
[0114] (Evaluation of heat treatment suitability) The evaluation sample was subjected to a heat treatment by passing it through a heat roller laminator (manufactured by Meiko Shoji Co., Ltd., product name: MS Pouch THS330, set temperature: 130°C, speed setting: 6). The appearance of the coating of the obtained evaluation sample was observed, and the heat treatment suitability was evaluated according to the following criteria. The results are shown in Tables 1 and 2.
[0115] When no change in the appearance of the coating of the evaluation sample was observed before and after the heat treatment, the sample was evaluated as having excellent heat treatment suitability (◯). When the coating was transferred to the heat roller during heat treatment, the heat treatment suitability was evaluated as poor (×).
[0116] In the following, the term "evaluation sample after heat treatment" refers to an evaluation sample obtained by heat treatment using the above-mentioned heat roller laminator. (Evaluation of adhesion of coating after heat treatment) After the heat treatment, the evaluation sample was cooled to room temperature, and cellophane tape (manufactured by Nichiban Co., Ltd., product name: CT-15) was applied to the coating on the non-printed side and the coating on the printed side. Next, the state of the coating was observed when the cellophane tape was peeled off at 180 degrees, and the adhesion of the coating after the heat treatment was evaluated according to the following criteria. The results are shown in Tables 1 and 2.
[0117] When the coating did not peel off, it was evaluated as having excellent adhesion (◯). When the coating peeled off together with the cellophane tape, the adhesion was evaluated as poor (×). The evaluation samples after the heat treatment that were evaluated as being poor (×) in terms of the heat treatment suitability were not evaluated (−).
[0118] (Evaluation of coating uniformity) The uniformity of the surface shape of the coating of the evaluation sample was visually observed, and the feel of the coating when the surface was stroked with the pad of a finger was confirmed. The results are shown in Tables 1 and 2.
[0119] When the surface of the coating of the evaluation sample was not rough when stroked with the pad of a finger and the appearance of unevenness was uniform, it was evaluated as having excellent uniformity (◯). When the surface of the coating of the evaluation sample was stroked with the pad of a finger, it was rough in some places due to protrusions, and there were scattered areas with different appearance unevenness, in which case the sample was rated as having slightly poor uniformity (△).
[0120] When the surface of the coating of the evaluation sample was rubbed with the pad of a finger and was obviously rough and had a clearly uneven appearance, the coating was rated as having poor uniformity (×). The evaluation samples after the heat treatment were also evaluated in the same manner according to the above criteria. Samples that were evaluated as poor (×) in terms of heat treatment suitability were not evaluated (-).
[0121] (Evaluation of the mattness of the coating) The 60° gloss of the coating on the printed surface of the evaluation sample was measured using a gloss meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name: PG-II), and the matteness of the coating was evaluated according to the following criteria. The results are shown in Tables 1 and 2.
[0122] When the 60° gloss level was less than 25, it was evaluated as having excellent matte properties (good). When the 60° gloss level was 25 or more, the matte properties were evaluated as poor (×). In order to evaluate the effectiveness of the matting components under the same conditions, the evaluation of the matting properties was performed only on samples in which the content of (B) the amino resin fine particles and the total content of the fine particles were each within the range of 7.8 parts by mass or more and 8.0 parts by mass or less. Samples that were not evaluated were not evaluated (-).
[0123] The evaluation samples after the heat treatment were also evaluated in the same manner according to the above criteria. Samples that were evaluated as poor (×) in terms of heat treatment suitability were not evaluated (-).
[0124] (Evaluation of printability) On the coating of the non-printed side of the evaluation sample, 12pt alphabet characters and a 10cm square solid image were printed with an ink thickness of 30μm using an active energy ray curable inkjet ink printer (manufactured by Duplo, product name: DDC-810). The printed image was visually inspected and the printability of the coating was evaluated according to the following criteria. The results are shown in Tables 1 and 2.
[0125] When the characters and solid images were printed without bleeding and the solid images were printed smoothly over the entire surface, the printability was evaluated as excellent (◯). When blurred characters due to ink bleeding or indentations in the image due to dot-like or line-like printing voids were observed, the printability was evaluated as somewhat poor (Δ).
[0126] When the ink penetrated into the substrate and did not harden or dry, the printability was evaluated as poor (×). The samples for evaluation after heat treatment that were evaluated as excellent (◯) in terms of heat treatment suitability were also evaluated according to the above criteria. Samples that were evaluated as poor (×) in terms of heat treatment suitability were not evaluated (-).
[0127] [Table 1]
[0128] [Table 2] As shown in Table 1, the coating liquid of each example can provide a coating film having a matte finish due to the inclusion of amino resin fine particles. It is also clear that the coating liquid of each example has excellent film-forming properties.
[0129] As shown in Table 2, the film-forming property was poor in the coating liquid of Comparative Example 1. The coating films obtained from the coating liquids of Comparative Examples 2 to 4 were poor in matte properties. It is seen that the coating liquid of each Example has excellent printing surface coating properties, and the resulting coating film has excellent fixation. It is seen that the coating films obtained from the coating liquids of Examples 1 to 9 and 11 have excellent uniformity. It is seen that the coating films obtained from the coating liquids of Examples 1 to 8 and 11 have excellent printability.
[0130] It is clear that the coating films obtained from the coating fluids of Examples 1 to 10 have excellent suitability for heat treatment. It is also clear that the coating films obtained from the coating fluids of Examples 1 to 10 have excellent adhesion after heat treatment.
[0131] <Additional Notes> The technical ideas that can be understood from the above-described embodiment and modified examples will be described. (Appendix 1) A coating fluid used for forming a coating on a substrate, the coating fluid comprising: (A) a resin dispersion; and (B) amino resin fine particles, the (A) resin dispersion containing (a) a water-dispersible resin that is a component that forms the coating, the (B) amino resin fine particles being capable of being scattered throughout the coating, and the (a) water-dispersible resin having a mass average glass transition point of 100°C or lower.
[0132] (Appendix 2) The coating fluid according to (Appendix 1), wherein the content of the (B) amino resin fine particles is 30 parts by mass or less per 100 parts by mass of the (a) water-dispersible resin. (Appendix 3) The coating fluid according to (Appendix 1) or (Appendix 2), wherein the (B) amino resin fine particles are spherical fine particles, and the average particle diameter of the (B) amino resin fine particles is within the range of 1 μm or more and 20 μm or less.
[0133] (Appendix 4) The coating fluid according to any one of (Appendix 1) to (Appendix 3), wherein the (B) amino resin fine particles include at least one selected from the group consisting of (B1) urea resin fine particles, (B2) melamine resin fine particles, and (B3) guanamine resin fine particles.
[0134] (Note 5) The density of the amino resin fine particles (B) is 1.0 g / cm 3 More than 1.6g / cm 3 A coating fluid according to any one of (Appendix 1) to (Appendix 4), which is within the following range: (Appendix 6) The coating fluid according to any one of (Appendix 1) to (Appendix 5), wherein the (a) water-dispersible resin includes at least one selected from the group consisting of (a1) a (meth)acrylic resin, (a2) a polyester resin, and (a3) a urethane resin.
[0135] (Appendix 7) The coating fluid according to any one of (Appendix 1) to (Appendix 6), wherein the coating fluid has a viscosity measured with a Brookfield viscometer of 1500 mPa·s or less at 20°C. (Appendix 8) The coating fluid according to any one of (Appendix 1) to (Appendix 7), wherein the content of the water-dispersible resin (a) in the coating fluid is 30 mass % or more.
[0136] (Appendix 9) The coating fluid according to any one of (Appendix 1) to (Appendix 8), wherein the substrate has a substrate layer having liquid-absorbent properties. (Appendix 10) The coating solution according to any one of (Appendix 1) to (Appendix 9), wherein the coating serves as a base layer for printing.
[0137] (Additional Note 11) The substrate has a substrate layer and a printing layer provided on the substrate layer, The coating solution according to any one of (Appendix 1) to (Appendix 9), wherein the coating is provided on the printing layer.
[0138] (Appendix 12) A method for producing an article having a substrate and a coating film provided on the substrate, the method comprising: a coating step of applying a coating liquid to the substrate to provide a coating layer on the substrate; and a coating step of drying the coating layer to form the coating film, the coating liquid containing (A) a resin dispersion and (B) amino resin fine particles, the (A) resin dispersion containing (a) a water-dispersible resin that is a component that forms the coating film, the (B) amino resin fine particles being capable of being scattered throughout the coating film, and the (a) water-dispersible resin having a mass average glass transition point in the range of 50°C or higher and 100°C or lower.
[0139] (Appendix 13) The method for producing an article according to (Appendix 12), further comprising a printing step of providing a printing layer on the coating, the printing step using an inkjet method. (Appendix 14) The method for producing an article according to (Appendix 13), wherein at least one of a volatile solvent ink and an active energy ray curable ink is used in the printing step.
[0140] (Appendix 15) The method for manufacturing an article according to any one of (Appendix 12) to (Appendix 14), further comprising a heat treatment step of heat treating the coating.
[0141] (Appendix 16) In the heat treatment step, The method for producing an article according to (Appendix 15) uses at least one of a non-contact heating method in which hot air is blown onto the coating or a heat ray is irradiated onto the coating, and a contact heating method in which a heating member is brought into contact with the coating.
Claims
1. A coating liquid used to form a coating on a substrate, (A) a resin dispersion liquid; and (B) amino resin fine particles, The (A) resin dispersion contains (a) a water-dispersible resin which is a component that forms the coating film, The amino resin fine particles (B) can be scattered in the coating film, The water-dispersible resin (a) has a mass average glass transition temperature of 100° C. or lower.
2. The coating fluid according to claim 1 , wherein a content of the amino resin fine particles (B) is 30 parts by mass or less per 100 parts by mass of the water-dispersible resin (a).
3. The amino resin fine particles (B) are spherical fine particles, The coating fluid according to claim 1 , wherein the average particle diameter of the amino resin fine particles (B) is within a range of 1 μm or more and 20 μm or less.
4. The coating fluid according to claim 1 , wherein the amino resin fine particles (B) include at least one selected from the group consisting of urea resin fine particles (B1), melamine resin fine particles (B2), and guanamine resin fine particles (B3).
5. The density of the amino resin fine particles (B) is 1.0 g / cm 3 Above, 1.6g / cm 3 The coating fluid according to claim 1, wherein the viscosity is within the following range:
6. The coating fluid according to claim 1 , wherein the water-dispersible resin (a) comprises at least one selected from the group consisting of (a1) a (meth)acrylic resin, (a2) a polyester resin, and (a3) a urethane resin.
7. The coating fluid according to claim 1 , wherein the coating fluid has a viscosity measured with a Brookfield viscometer of 1500 mPa·s or less at 20° C.
8. The coating fluid according to claim 1 , wherein a content of the water-dispersible resin (a) in the coating fluid is 30% by mass or more.
9. The coating solution according to claim 1 , wherein the substrate has a substrate layer having liquid-absorbent properties.
10. The coating solution according to claim 1 , wherein the coating serves as a base layer for printing.
11. The substrate has a substrate layer and a printing layer provided on the substrate layer, The coating solution according to claim 1 , wherein the coating is provided on the printed layer.
12. A method for producing an article having a substrate and a coating disposed on the substrate, comprising the steps of: a coating step of applying a coating liquid to the substrate to form a coating layer on the substrate; and a coating forming step of drying the coating layer to form the coating. The coating liquid contains (A) a resin dispersion and (B) amino resin fine particles, The (A) resin dispersion contains (a) a water-dispersible resin which is a component that forms the coating film, The amino resin fine particles (B) can be scattered in the coating film, The method for producing an article, wherein the water-dispersible resin (a) has a mass average glass transition temperature of 100° C. or lower.
13. Further comprising a printing step of providing a printing layer on the coating, The method for manufacturing an article according to claim 12 , wherein the printing step uses an inkjet method.
14. The method for manufacturing an article according to claim 13 , wherein at least one of a volatile solvent ink and an active energy ray curable ink is used in the printing step.
Citation Information
Patent Citations
Water-based matting surface-treatment agent composition and polyvinyl chloride resin product having coating film layer thereof
JP2010121027A
Binder
JP2015527413A
Water-based ink composition for surface printing and article with printed layer
JP7093461B1
Microstructured Paint
US20150353755A1
Non aqueous crosslinkable composition
WO2022268669A1