GRINDING PLATE, GRINDING DEVICE, SURFACE PROCESSING METHOD, MANUFACTURING METHOD OF SINGLE CRYSTAL SiC SUBSTRATE, AND SINGLE CRYSTAL SiC SUBSTRATE

The grinding plate and device design using tribo-oxidation with metal oxide abrasive grains and a specific segment shape address non-uniform processing and warpage in large-diameter SiC substrates, enabling efficient mass production with minimal scratches and warpage, suitable for epitaxial growth and device applications.

JP2024149101APending Publication Date: 2024-10-18RESONAC CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023062778
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing methods for processing large-diameter single-crystal SiC substrates face challenges such as excessive trial and error, non-uniform processing, and difficulty in reducing thickness variations, surface roughness, and warpage, which hinder mass production and practical application.

Method used

A grinding plate and device design utilizing a tribo-oxidation effect with abrasive grains made of metal oxides or SiC, combined with a specific segment shape and arrangement, to achieve uniform processing without liquid coolant, addressing the issues of non-uniformity and warpage in large-diameter SiC substrates.

Benefits of technology

Enables uniform and efficient processing of large-diameter single-crystal SiC substrates with minimal scratches and warpage, facilitating mass production and reducing the process-affected layer to less than 1 μm, with surface roughness between 1 nm and 5 nm, suitable for subsequent epitaxial growth and device applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149101000001_ABST
    Figure 2024149101000001_ABST
Patent Text Reader

Abstract

To provide a grinding plate that can be applied to an existing device and is capable of suppressing the occurrence of minute scratches on a large-diameter substrate.SOLUTION: A grinding plate includes a grindstone segment on a base metal having a flat surface. The grindstone segment includes a soft pad in which abrasive grains are fixed on the surface or a resin bond grindstone which contains the abrasive grains and resin. The grindstone segment has a segment shape designed so as to be uniformly processed on the basis of the abrasive grain trajectory density within a processing object surface defined by the arrangement of the grinding plate and a processing object table and the relative speed between the abrasive grains and a processing object. The abrasive grain is composed of at least one kind or more of metal oxides softer than single crystal SiC and having a band gap, or SiC.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a grinding plate, a grinding device, a surface processing method, a method for manufacturing a single crystal SiC substrate, and a single crystal SiC substrate. [Background technology]

[0002] The semiconductor material SiC (silicon carbide) has a wider band gap than Si (silicon), which is currently widely used as a device substrate. Therefore, research is being conducted into using single crystal SiC substrates to create power devices, high frequency devices, high temperature operating devices, and the like.

[0003] The single crystal SiC substrate is formed, for example, by cutting a single crystal SiC ingot produced by a sublimation method, and then polishing both surfaces to a mirror finish (see, for example, Patent Document 1).

[0004] The cut substrate has warping, waviness, thickness variations, and processing distortion. These are reduced by, for example, grinding with diamond abrasive grains, and then the substrate is given a mirror finish by CMP (chemical mechanical polishing). However, because the processing speed of CMP is slow, it is desirable to make the depth of the processing distortion layer before CMP as small as possible (for example, see Non-Patent Document 1).

[0005] Also, it is desirable to have little thickness variation. Thickness variation is indicated by an index called TTV (Total Thickness Variations), and Patent Document 2 discloses SiC substrates with a diameter of 3 inches and TTVs of 0.623, 0.673, and 0.739 μm, while Patent Document 3 discloses SiC substrates with a diameter of 76 mm and a TTV of 1.7 μm and SiC substrates with a diameter of 100 mm and a TTV of 1.05 μm.

[0006] For mirror finishing of non-oxide ceramics such as SiC, there is a mechanochemical polishing technique that utilizes the mechanochemical effect. For example, Non-Patent Document 2 discloses a method of dry polishing using chromium oxide abrasive grains with an average grain size of 0.5 μm on a polishing disk molded from resins such as acrylonitrile or phenol, and the results of machining single crystal SiC.

[0007] In addition, Patent Document 4 discloses that, based on a hypothesis named tribocatalysis, a 3-inch diameter SiC substrate is mirror-finished, and the difference between the maximum and minimum values ​​of the substrate height corresponding to the TTV is 1.4 μm, and Non-Patent Document 3 discloses that a similar mirror-finish is performed on a 100 mm diameter SiC substrate, and the TTV is 1.8 μm. As a specific means, Patent Document 4 proposes a mechanism in which an abrasive grain made of a material having a band gap is given energy by mechanical sliding with the workpiece, and electrons on the abrasive grain surface are excited to generate electron-hole pairs, and highly oxidizing active species such as superoxide anion, hydroxyl radical, or atomic oxygen are generated to oxidize the sample surface in a similar mechanism to that described in the photocatalytic material, and a method for manufacturing a 3-inch diameter SiC substrate with a small TTV is disclosed. In addition, Non-Patent Document 3 discloses that a SiC substrate with a diameter of 100 mm and a small TTV was obtained by processing using the same principle as Patent Document 4.

[0008] As disclosed in Patent Document 5, the front surface of the single crystal SiC substrate needs to be a mirror surface for epitaxial growth in the next step, but the back surface preferably has a large surface roughness from the viewpoint of handling and the like.

[0009] Furthermore, when a single crystal SiC substrate is used as a seed crystal for the sublimation method, if there is damage such as foreign matter or polishing scratches on the crystal growth surface, the crystal growth is hindered and it is not possible to grow a high-quality silicon carbide single crystal. Therefore, as disclosed in Patent Document 6, for example, an etching process has been performed using hydrogen gas or the like before crystal growth to remove crystal growth inhibition factors such as dust and polishing scratches, promote lateral growth, and grow a high-quality silicon carbide single crystal with few crystal defects. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Patent No. 4499698 [Patent Document 2] JP 2012-214376 A [Patent Document 3] Special Publication No. 2016-501809 [Patent Document 4] Patent No. 6016301 [Patent Document 5] Patent No. 5560774 [Patent Document 6] JP 2010-111540 A [Non-patent literature]

[0011] [Non-Patent Document 1] Takanori Takado, Kazutoshi Hotta, Kenji Kawata, Masatake Nagaya, Hiroto Maeda, Yoshihiro Deguchi, Shogo Matsuda, Atsunori Takeda, Ryuichi Takanabe, Tomohiro Nakayama, Tomohisa Kato: Proceedings of the 21st Lecture of the SiC and Related Wide-Gap Semiconductors Study Group, pp. 72-73 [Non-Patent Document 2] Suga, Tadatomo: Machines and Tools, 35, 92-96 (1991) [Non-Patent Document 3] T. Kido, M. Nagaya, K. Kawata and T. Kato, Mater. Sci. Forum 778-780 (2014) 754-758 [Non-Patent Document 4] Keiji Nakayama: J. Vac. Soc. Jpn., 49, 618-623 (2006) [Non-Patent Document 5] Zhou Libo, Mitsuda Takahito, Shimizu Jun, Tian Bingye, Yamamoto Takeyuki: Journal of the Japanese Society for Abrasive Technology, 54, 45-49 (2010) [Non-Patent Document 6] Shinya Hirano, Kenji Kawata, Hiroshi Asamizu, Tomohisa Kato: Journal of the Japanese Society for Abrasive Technology, 60, 454-459 (2016) Summary of the Invention [Problem to be solved by the invention]

[0012] However, the contents disclosed in Patent Document 2 and Patent Document 3 do not mention a method for processing a SiC substrate, and in order to manufacture a substrate with a small TTV, trial and error beyond the level that a person skilled in the art would expect, or excessive trial and error, was required regarding processing conditions.

[0013] The method disclosed in Non-Patent Document 2 requires a processing load of 0.34 MPa for a small single crystal sample, which is not practical for mass production, and is not applicable to the current efforts toward practical use of SiC power semiconductors targeting 6-inch or even 8-inch diameters. Therefore, in order to develop a mirror finish method based on the method disclosed in Non-Patent Document 2 that can be used for mass production of single crystal SiC substrates having mirror surfaces that can be used for devices, it was currently necessary to solve at least the problems of the processing load and the uniform processing of large-diameter substrates.

[0014] In both of the methods described in Patent Document 4 and Non-Patent Document 3, it is believed that excessive trial and error is required to uniformly process a SiC substrate having a diameter of 145 mm or more to obtain SiC with a small TTV.

[0015] However, in the method disclosed in Patent Document 5, a surface with large surface roughness usually has a deep process-affected layer, and a difference in residual stress occurs between the front and back surfaces, causing the substrate to warp due to the Twyman effect, which causes various problems. Therefore, it is difficult to reduce the warp of a single-crystal SiC substrate in which the processing conditions of both sides are different, one side is a mirror surface and the back surface is not a mirror surface, and it is particularly difficult to obtain a substrate with small warpage when the diameter of the substrate is large, such as 145 mm or more, or when the substrate is thin, which is greatly affected by the Twyman effect. Patent Document 5 discloses a technology for controlling the shape of a single-crystal SiC substrate using the Twyman effect, but since electrolytic etching is performed using hydrofluoric acid, which is difficult to handle, more careful consideration is required for safety and waste disposal than when CMP is performed, it is difficult to uniformly remove the process-affected layer of a single-crystal SiC substrate with a diameter of 145 mm or more with the disclosed substrate and cathode arrangement, and it can only be applied to n-type substrates, which are major obstacles to the practical application and dissemination of the technology.

[0016] However, the method described in Patent Document 6 has a problem in that it is extremely difficult to uniformly etch the surface of the single crystal SiC substrate used as a seed crystal when the diameter of the substrate is large, such as 145 mm or more. When the surface roughness of the single crystal SiC substrate is appropriately large, the flowing hydrogen gas is easily captured, and etching starts uniformly over the entire surface of the substrate, which is advantageous for uniform etching, but when diamond processing is performed, the processing-affected layer becomes large, making it difficult to remove crystallization-inhibiting factors.

[0017] The present invention aims to provide a highly practical grinding plate, grinding device, surface processing method and manufacturing method that can be applied to mass production processes by using an existing grinding device, i.e., a grinding device in which the center of rotation of the workpiece table is positioned so that it hits the outer periphery of the grinding plate, and that can uniformly process large-diameter single-crystal SiC substrates, such as those with a diameter of 145 mm or more, while suppressing the occurrence of micro-scratches, as well as a large-diameter single-crystal SiC substrate in which the occurrence of micro-scratches is suppressed. [Means for solving the problem]

[0018] In order to solve the above problems, the present inventors conducted extensive research and came up with the present invention.

[0019] The method disclosed in Patent Document 4 is advantageous for mirror-finishing SiC substrates, and the present invention utilizes this method. However, in the course of our investigations, we have come to understand the effective requirements for uniformly machining SiC substrates with diameters of 145 mm or more using a grinding device.

[0020] On the other hand, Patent Document 4 proposes a hypothesis that the generation of electron-hole pairs is the origin of the tribocatalysis, but we have come to the conclusion that the hypothesis that the origin is microplasma caused by discharge due to the high electric field of triboelectric charging, as disclosed in Non-Patent Document 4, is more valid. There is also a possibility that the mechanism is that electron-hole pairs are generated as a result of UV light being emitted. Therefore, water-based coolants are unnecessary because they are disadvantageous to triboelectric charging, even if they are pure water. In addition, oil-based coolants are dangerous because they may ignite. In other words, liquid coolants are not used in the present invention. In the following, this action will be called tribooxidation action in the present invention.

[0021] In the present invention, in order to easily apply the processing of large-diameter single crystal SiC substrates to mass production, it is necessary to be able to attach it to a grinding device and use it. Since processing using the tribo-oxidation effect of abrasive grains using a grinding device has not been performed on SiC substrates with a diameter of 145 mm or more, we have intensively studied grinding conditions that can effectively express the tribo-oxidation effect and perform uniform processing. As a result, we found that there are appropriate conditions and ranges for the type of abrasive grain, selection of grain size, type and shape of abrasive grain holding pad and bond material, rotation speed of the grinding plate, etc.

[0022] Patent Document 4 discloses a grinding plate in which a soft pad and a hard pad are attached in that order to a base metal having a flat surface, using a CMP pad as the base of the grinding plate. However, it has been found that if the segment shape is appropriate, a grinding plate with only a soft pad attached, or a grinding plate with a soft resin-bonded grinding wheel attached, can be used.

[0023] Furthermore, Patent Document 4 states that "There are various materials that have tribo-oxidation properties. For example, diamond and SiC are materials that have a band gap and therefore exhibit tribo-oxidation properties. However, they are not softer than single crystal SiC and will scratch the machined surface of the single crystal SiC, making them unsuitable." It also discloses "abrasive grains made of at least one type of metal oxide that is softer than single crystal SiC and has a band gap," but it was found that SiC abrasive grains, which are the same material as the workpiece, can also be used for mirror finishing.

[0024] The segment shape is important for uniform mirror finishing using a grinding device. Regarding the segment shape, Patent Document 4 only states that "In a normal grinding device, the center of rotation of the workpiece table is arranged so as to hit the outer periphery of the grinding plate, and the rotation direction of the workpiece table is opposite to that of the grinding plate. Therefore, if there are abrasive grains on the entire surface of the grinding plate, the abrasive grains will come into contact with the center of the workpiece more frequently, and only the center will be scraped off. Therefore, appropriate segmentation to prevent this is effective." In the examples, it states that "the workpiece is segmented into a right-angled triangle of 30 x 40 x 50 mm," and shows a drawing. When the segment shape in the drawing disclosed in Patent Document 4 was used for surface processing of a large-diameter single-crystal SiC substrate with a diameter of 145 mm or more, it was difficult to uniformly process the single-crystal SiC substrate. For SiC substrates with a diameter of up to 3 inches, the processing area is small so excessive trial and error is not required. However, to uniformly mirror-finish single crystal SiC substrates with a diameter of 145 mm or more, excessive trial and error is required, and based on the disclosure of Patent Document 4, it was not possible to find a segment shape that can uniformly process single crystal SiC substrates.

[0025] The inventors have discovered that it is effective to design the segment shape so that it can be machined uniformly based on the abrasive grain trajectory density on the workpiece surface, which is determined by the arrangement of the grinding plate and the workpiece table, and the relative speed between the abrasive grains and the workpiece.

[0026] The present invention provides the following means. (1) A grinding plate comprising a grinding wheel segment mounted on a base metal having a flat surface, the grinding wheel segment having a soft pad with abrasive grains fixed to its surface or a resin-bonded grinding wheel containing abrasive grains and resin, the grinding wheel segment having a segment shape designed to enable uniform processing based on the abrasive grain trajectory density in the workpiece surface determined by the arrangement of the grinding plate and a workpiece table and the relative speed of the abrasive grains and the workpiece, and the abrasive grains made of at least one metal oxide softer than single crystal SiC and having a band gap, or SiC.

[0027] (2) In the grinding plate of (1) above, the abrasive grains may be made of at least one metal oxide selected from the group consisting of cerium oxide, titanium oxide, silicon oxide, aluminum oxide, iron oxide, zirconium oxide, zinc oxide, and tin oxide.

[0028] (3) In the grinding plate of (1) above, the abrasive grains may be made of SiC.

[0029] (4) A grinding device having a grinding plate according to any one of (1) to (3) above.

[0030] (5) A surface processing method comprising mounting the grinding plate according to any one of (1) to (3) above on a grinding device and processing a surface of a single crystal SiC substrate having a diameter of 145 mm or more without using a liquid coolant.

[0031] (6) A method for producing a single crystal SiC substrate, comprising the step of processing the surface of a substrate by the surface processing method according to (5) above.

[0032] (7) A single crystal SiC substrate having a C-face processed layer of 1 μm or less, a surface roughness Sa within the range of more than 1 nm and 5 nm or less, and a diameter of 145 mm or more.

[0033] In this specification, the term "single crystal SiC substrate" is used commonly to refer to any of the substrates before, during, and after surface grinding. Effect of the Invention

[0034] According to the present invention, by using an existing grinding device, i.e., a grinding device in which the center of rotation of the workpiece table is positioned so that it hits the outer periphery of the grinding plate, it is possible to provide a highly practical grinding plate, grinding device, surface processing method and manufacturing method that can be applied to mass production processes and can uniformly process large-diameter single crystal SiC substrates, such as those with a diameter of 145 mm or more, while suppressing the occurrence of micro-scratches, as well as a large-diameter single crystal SiC substrate in which the occurrence of micro-scratches is suppressed. [Brief description of the drawings]

[0035] [Figure 1] FIG. 2 is a cross-sectional view showing the structure of a grinding plate according to the present invention. [Diagram 2] FIG. 2 is a plan view showing the structure of a grinding plate according to the present invention. [Diagram 3] 3 is a plan view showing a modified example of the grinding plate in FIG. 2. [Figure 4] 3 is a plan view showing another modified example of the grinding plate in FIG. 2. FIG. [Diagram 5] FIG. 13 is a plan view showing the structure of a grinding plate according to a comparative example of the present invention. [Figure 6] 1 is a cross-sectional view showing a structure of a grinding device according to the present invention. [Figure 7] FIG. 1 is a perspective view showing the structure of a grinding device in Non-Patent Document 5. [Figure 8] FIG. 13 is a diagram showing the density of abrasive grain tracks on the surface of a workpiece according to Non-Patent Document 5. [Figure 9] 5 is a schematic diagram for explaining a process for determining the shape of the grinding wheel segments in the grinding plate of the present invention. FIG. [Figure 10] 1A to 1C are diagrams for explaining a process for determining the shape of the grinding wheel segments in the grinding plate of the present invention. [Figure 11] 1A to 1C are diagrams for explaining a process for determining the shape of the grinding wheel segments in the grinding plate of the present invention. [Figure 12] 1A to 1C are diagrams for explaining a process for determining the shape of the grinding wheel segments in the grinding plate of the present invention. [Figure 13] 3 is an optical microscope photograph of a substrate surface before surface processing in Example 1 and Comparative Example 1. [Figure 14] 3 is an optical microscope photograph of the substrate surface after surface processing in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] Hereinafter, the configurations of a grinding plate, a grinding device, a surface processing method, a method for manufacturing a single crystal SiC substrate, and a single crystal SiC substrate, which can be used for surface processing of a large diameter single crystal SiC substrate such as a diameter of 145 mm, to which the present invention is applied, will be described with reference to the drawings. Note that the drawings used in the following description may show characteristic parts in an enlarged manner for the sake of convenience in order to make the characteristics easier to understand, and the dimensional ratios of each component may not necessarily be the same as the actual ones. In addition, the materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited to them, and can be appropriately changed and implemented within the scope of the present invention.

[0037] (Grinding plate and grinding device) Fig. 1 is a schematic diagram and cross-sectional view showing an example of a grinding plate for surface processing according to an embodiment of the present invention. Fig. 2 is a plan view of the grinding plate of Fig. 1. Although details will be described later, the plan view of the grinding plate may have a configuration as shown in Fig. 3 or Fig. 4. Fig. 5 is a plan view showing the structure of a grinding plate of a comparative example. In Fig. 2, an example of the rotation direction of the grinding plate is shown by an arrow for convenience of explanation, but the rotation direction may be the opposite direction to the arrow shown in the figure.

[0038] The grinding plate 10A shown in Fig. 1 and Fig. 2 has a grinding wheel segment on a base metal 1 having a flat surface S, and includes a grinding wheel segment 2A. The grinding wheel segment 2A has a soft pad with abrasive grains fixed to its surface or a resin-bonded grinding wheel containing abrasive grains and resin, for example, a soft pad or a resin-bonded grinding wheel. The grinding wheel segment 2A has a segment shape designed to enable uniform processing based on the abrasive grain trajectory density in the workpiece surface determined by the arrangement of the grinding plate 10A and the workpiece table, and the relative speed of the abrasive grains and the workpiece, and the abrasive grains are made of at least one or more metal oxides that are softer than single crystal SiC and have a band gap, or SiC.

[0039] First, an example in which the grindstone segment is a soft pad having abrasive grains fixed to its surface will be described below. The grinding plate 10A comprises a base metal 1 having a flat surface S, and a soft pad 2a attached thereon, and the soft pad 2a has abrasive grains made of at least one metal oxide that is softer than single crystal SiC and has a band gap or abrasive grains made of SiC (not shown) fixed to its surface. The base metal 1 has a circular ring shape in a plan view in a cross section perpendicular to the direction perpendicular to the flat surface S. For example, in the direction perpendicular to the flat surface S, the base metal 1 has an inner diameter larger at the end opposite the grinding wheel segment 2A than at the end on the grinding wheel segment 2A side.

[0040] In this example, the grinding wheel segment 2A is composed of four soft pads 2a segmented into a shape designed to enable uniform processing based on the abrasive grain trajectory density on the workpiece surface determined by the arrangement of the grinding plate 10A and the workpiece table, and the relative speed between the abrasive grains and the workpiece.

[0041] The grindstone segment 2A is laminated on the flat surface S of the base metal 1. The grindstone segment 2A is composed of multiple members, and each member is arranged in rotation symmetry with respect to the axial center of the flat surface S of the base metal 1. The grindstone segment 2A may be four-fold rotationally symmetric as shown in Fig. 2, or may be six-fold rotationally symmetric, eight-fold rotationally symmetric, etc.

[0042] The grinding wheel segment 2A shown in Fig. 2 has at least two sides extending from the inner peripheral end E1 side toward the outer peripheral end E2 side of the flat surface S. Both of the two sides extending from the inner peripheral end E1 side toward the outer peripheral end E2 side of the grinding wheel segment 2A are aligned with the rotation direction of the grinding plate 10A, or both of them face the rotation direction of the grinding plate 10A. Fig. 2 shows an example in which the sides are aligned with the rotation direction of the grinding plate 10A. Each of the plurality of members constituting the grindstone segment 2A is provided so as to intersect with the inner peripheral end E1 and the outer peripheral end E2 of the base metal 1 at two points, for example. Each of the multiple members constituting the grindstone segment 2A has a width that decreases, for example, as it moves away from the axial center of the flat surface S in the extension direction. In the example shown in Fig. 2, the grindstone segment extending in the x direction has a smaller size in the y direction as it moves away from the axial center of the flat surface S in the x direction, and the grindstone segment extending in the y direction has a smaller size in the x direction as it moves away from the axial center of the flat surface S in the y direction. Here, among the members constituting the grindstone segment 2A, the ends in the radial direction are located on a locus of points that are the same distance from the center of the metal base 1. In other words, the ends in the radial direction are located on the same circular arc. As shown in FIG. 2, for example, the grindstone segment 2A rotates counterclockwise when viewed from above from the substrate side, which is the workpiece.

[0043] The abrasive grains with a band gap become charged by friction during surface grinding of the single crystal SiC substrate, and discharge occurs in a small area, resulting in a high-energy state. This generates highly oxidizing active species such as superoxide anions, hydroxyl radicals, and atomic oxygen, which oxidize the sample surface, resulting in the formation of SiO 2 nH 2 The O is removed by the abrasive grains, creating a tribo-oxidation effect that allows the surface of the single-crystal SiC substrate to be processed.

[0044] Metal oxides, in particular, are materials having a band gap that causes tribo-oxidation, and are softer than single crystal SiC, and most of them have a band gap, so they can be used preferably because powders having tribo-oxidation are available industrially for use as abrasives, pigments, photocatalysts, etc. SiC also has a band gap and is an industrially available material at low cost, so it can be used preferably.

[0045] More preferably usable powders are at least one metal oxide powder selected from cerium oxide, titanium oxide, silicon oxide, aluminum oxide, iron oxide, zirconium oxide, zinc oxide, and tin oxide, or SiC powder, in view of their industrial availability and the fact that they have a band gap and therefore have a tribo-oxidation effect.

[0046] The most preferably usable metal oxide powder is cerium oxide powder or SiC powder, in view of their industrial availability, their tribo-oxidation effect due to their being semiconductor materials having a band gap, and the performance they exhibit.

[0047] The grinding plate 10A includes a base metal 1, and can be mounted on a grinding device for use with the grinding device. A known material can be used as the base metal 1, and for example, an aluminum alloy such as silumin can be used.

[0048] This base metal 1 has a flat surface S facing the workpiece, and the grinding plate 10A has a structure in which a soft pad 2a or a resin-bonded grindstone is attached to this flat surface S. By providing the grinding plate 10A with the grindstone segment 2A having such a structure, surface-based processing is possible, and scratches generated on the surface of the single crystal SiC substrate, which is the workpiece, can be minimized.

[0049] The soft pad 2a may be made of nonwoven fabric or suede. Specifically, the soft pad 2a may be a nonwoven fabric pad such as a SUBA pad or a suede pad such as a Supreme pad. The soft pad 2a may also be a nonwoven fabric pad or suede pad provided with waterproof abrasive paper.

[0050] The outermost surface of the soft pad 2a, which is used for surface processing of the substrate using the grinding plate 10A, has abrasive grains made of at least one metal oxide that is softer than single crystal SiC and has a band gap or abrasive grains made of SiC fixed to the surface of the soft pad 2a. The abrasive grains can be fixed to the surface of the soft pad 2a using a binder or adhesive. The abrasive grains can be fixed by adhering a fixed abrasive grain film, such as commercially available waterproof abrasive paper, to the soft pad, or by fixing the abrasive grains to the soft pad 2a with at least one of a binder and an adhesive.

[0051] Also, instead of the soft pad 2a, a resin-bonded grindstone in which abrasive grains made of at least one metal oxide that is softer than single crystal SiC and has a band gap or abrasive grains made of SiC are bonded with a resin that is as soft as the soft pad can be used. Even when a resin-bonded grindstone is used instead of the soft pad 2a, the segment shape of the grindstone segment 2A can be the same as when the soft pad 2a is used.

[0052] As described above, Fig. 3 and Fig. 4 are plan views showing modified examples of the grinding plate in Fig. 2. The grinding plates 10B, 10C shown in Fig. 3 and Fig. 4 differ from the grinding wheel segment 2A of the grinding plate 10A only in the segment shapes of the grinding wheel segments 2B, 2C, and other configurations can be the same as those of the grinding plate 10A. The grinding wheel segment 2B has a segment shape obtained by expanding the four members constituting the grinding wheel segment 2B in the rotation direction of the grinding plate 10B. The grinding wheel segment 2C has a shape with a radius. Fig. 5 is a plan view showing the structure of a grinding plate of a comparative example of the present invention. A grinding plate 10X shown in Fig. 5 also differs from the grinding plate 10A only in the segment shape of the grinding wheel segment 2X.

[0053] Each of the members constituting the grindstone segments 2B and 2C extends from the inner peripheral end E1 side of the base metal 1 toward the outer peripheral end E2 side, and is provided so as to intersect with the inner peripheral end E1 and the outer peripheral end E2 at two points, similar to each of the members constituting the grindstone segment 2A. Also, each of the members constituting the grindstone segments 2B and 2C, like each of the members constituting the grindstone segment 2A, has a smaller width as it moves away from the axial center of the flat surface S in the extension direction. Here, the width refers to the length in the direction intersecting with the extension direction. As described above, the radial ends of each of the multiple members constituting the grindstone segments 2B and 2C are located on a locus of points that are the same distance from the center of the base metal 1. That is, the radial ends of each of the multiple members constituting the grindstone segments 2B and 2C are provided on the same arc.

[0054] The grindstone segment 2B has, for example, at least two sides extending from the inner peripheral end E1 side of the flat surface S toward the outer peripheral end E2 side, one of which is along the rotation direction of the grinding plate 10B and the other of which is opposite to the rotation direction. The grindstone segment 2C has two curved lines extending from the inner peripheral end E1 side of the flat surface S toward the outer peripheral end E2 both of which are opposite to the rotation direction of the grinding plate 10C or both of which are along the rotation direction.

[0055] In contrast, the grindstone segments 2X of the grinding plate 10X according to the comparative example are designed without taking into consideration the relative speed of the abrasive grains and the workpiece, and therefore the outer peripheral ends, which are the outer radial ends of each of the grindstone segments 2X, are the apexes of the corners.

[0056] (Surface processing method for single crystal SiC substrate) The surface processing method according to one embodiment of the present invention is a method for processing the surface of a single crystal SiC substrate having a large diameter, for example, 145 mm or more, and the grinding plate 10A according to the above embodiment is attached to a grinding device, and the surface of a single crystal SiC substrate having a diameter of 145 mm or more is processed without using a liquid coolant. The surface processing method of the single crystal SiC substrate according to this embodiment is, for example, to generate oxidation products using the grinding plate, and grind the surface while removing the oxidation products.

[0057] The grinding device to which the grinding plate is attached may be a known existing grinding device, that is, a grinding device arranged so that the center of rotation of the workpiece table abuts on the outer periphery of the grinding plate.

[0058] Fig. 6 is a schematic cross-sectional view showing the structure of a portion of a grinding apparatus 100 equipped with a grinding plate 10A of the present invention, which grinds a single crystal substrate. The grinding plate 10A shown in Figs. 1 and 2 is attached to a grindstone flange 12 of a drive unit 11, which is rotated by a motor (not shown). The grinding plate 10A is attached to the grindstone flange 12 by, for example, screwing. The single crystal SiC substrate W is fixed to the workpiece table 14 by vacuum suction using a vacuum chuck device (not shown). The outer peripheral end of the grindstone segment 2A is aligned with the axial center C of the workpiece table 14. 15 The driving unit 11 rotates the grinding plate 10A and drives the grinding plate 10A to approach the substrate holder 15 which rotates together with the workpiece table 14, thereby grinding the substrate W. The outer peripheral end of the grindstone segment 2A is aligned with the axial center C of the workpiece table 14. 15 It is driven while maintaining the above arrangement.

[0059] By appropriately selecting the grinding conditions, the tribo-oxidation action of the grinding plate on the single crystal SiC can be manifested, generating oxidation products.

[0060] The rotation speed of the grinding plate 10A is preferably 300 rpm to 3000 rpm. If the rotation speed is lower than 300 rpm, triboelectric charging may be insufficient and tribo-oxidation may not occur, whereas if the rotation speed is higher than 3000 rpm, problems such as heat generation and device vibration may become significant.

[0061] The rotation speed of the grinding plate 10A is more preferably 500 rpm to 2000 rpm. By setting the rotation speed to 500 rpm or more, it is possible to generate tribo-oxidation more sufficiently, and by setting the rotation speed to 2000 rpm or less, it is possible to more reliably avoid problems such as heat generation and device vibration.

[0062] By segmenting the soft pad or resin-bonded grinding wheel, i.e., by separating it into appropriate sizes and attaching it to the base metal 1 as grinding wheel segments 2A, it is possible to control the frequency of contact between the abrasive grains on the grinding plate and the surface of the workpiece, and it is possible to prevent uneven processing, such as the central part of the workpiece being cut more than the other parts. In a normal grinding device, the center of rotation of the workpiece table is arranged to hit the outer periphery of the grinding plate, so when there are abrasive grains on the entire surface of the grinding plate, that is, when the soft pad or resin-bonded grinding wheel is arranged so that the base metal 1 is not exposed when the grinding plate is viewed in a plan view from the -z direction, the frequency of contact of the abrasive grains with the central part of the workpiece increases, and only the central part is cut, so appropriate segmentation to prevent this is effective. The rotation speed of the workpiece table 14 is preferably 30 rpm to 500 rpm. If the rotation speed is less than 30 rpm or more than 500 rpm, the operation will be outside the specifications of a normal grinding machine, and the amount of removal from the machined surface may become non-uniform.

[0063] In the present invention, in consideration of the mechanism of frictional electrification and discharge, as described above, liquid coolant, whether water-based or oil-based, is not used. When cooling is required, air or nitrogen gas can be blown near the processing part, and the operation can be continuous or intermittent.

[0064] The appropriate segment shape of the grinding wheel segment 2A is designed so as to perform uniform machining based on the density of abrasive grain tracks in the workpiece surface, which is determined by the arrangement of the grinding plate and the workpiece table, and the relative speed of the abrasive grains and the workpiece. An example of shape design is shown below. The shape design of the grinding plate 10A of the present invention employs a method that applies a conventional in-feed grinding model.

[0065] Conventionally, it has been considered that an in-feed grinding model is useful for analyzing the density of abrasive grain tracks within the surface of a workpiece (for example, Non-Patent Document 5). Figure 7 is a perspective view showing the structure of the grinding device in Non-Patent Document 5. As shown in Figure 7, Non-Patent Document 5 shows the arrangement of the grinding plate and the workpiece in a commonly used grinding device. The interference between the grinding plate and the workpiece within the surface of the workpiece at this time is shown in Figure 8, and the following discussion is developed.

[0066] Specifically, Non-Patent Document 5 states the following: Consider the amount of removal from the wafer for a very small area dr, distance r from the wafer center, as shown in Figure 8. If the average cutting width of one abrasive grain is a, the cutting depth is δ, and the length of the abrasive grain cutting path is ds, then the amount of removal is a δ ds. When integrated over a range corresponding to one circumference of the wafer, the removal volume is given by equation (1).

number

[0067] In the formula (1), h is the average depth of the wafer that is actually removed within the range dr. Also, m is the number of abrasive grains involved in cutting per wafer rotation, and the working area of ​​the grinding wheel is A 0、 Effective cutting edge area density is m 0 The rotation speed ratio of the wafer and the grindstone is n 1 / n 2 Then, m=A 0 m 0 n 1 / n 2 From equation (1), the actual removal depth h for the set cutting depth δ is given by equation (2).

number

[0068] However, Non-Patent Document 5 itself deals with Si, not SiC, as the workpiece. Furthermore, Non-Patent Document 5 takes an approach in which the grindstones are fixed to the outer periphery of the grinding plate, and therefore the abrasive grain track density remains uneven, and high flatness Si wafer processing is performed by optimizing the machine rigidity and the tilt angle accordingly. Also, Non-Patent Document 5 takes an approach in which the radius R 1 The grinding wheel exists only on the circumference of the circle, and the grinding wheel working area A 0 is set as a constant, but with such an arrangement of the grindstones, the vicinity of the center of the substrate is easily scraped. Therefore, the method of Non-Patent Document 5 cannot be said to be able to appropriately control the abrasive grain track density, and it is necessary to avoid a situation in which the vicinity of the center of the substrate is easily scraped. In addition, as will be described later, the method of Non-Patent Document 5 does not take into account the relative speed of the abrasive grains and the workpiece.

[0069] In order to solve the above problems, the present invention employs the following means. Specifically, first, the density of the abrasive grains is appropriately controlled. Basically, the symbols defined in Fig. 8 are followed, but r in Non-Patent Document 5 is replaced with x to express the function representing the grinding wheel segment shape in polar coordinates (r, θ) with C as the origin.

[0070] 9 to 12 are diagrams for explaining the process of determining the shape of the grindstone segments in the grinding plate of the present invention. In Fig. 9, it is considered that four segments are arranged in four-fold symmetry. The radius of the board is R 2 Therefore, the radius R of the grinding wheel circle C is2 -R 1 The grindstone does not act on the substrate in the following area. Therefore, for example, the radius R of the grindstone circle C shown by the dashed line in FIG. 2 -R 1 By determining another contour of the segment that has the arc of the octant and the X-axis as part of the contour and combining it with the one performed in the opposite direction about the X-axis, in this case, it is possible to determine the shape of the segment that is linearly symmetric with respect to the X-axis and four-fold symmetric with respect to the origin C. Let the arc length in the circumferential direction of the grinding wheel included in the segment at a point on the X-axis that is a distance x from the center of the substrate be a function of x, f(x), and consider determining an appropriate f(x), i.e., f(x) that eliminates 1 / x from the abrasive grain trajectory density parameter. Under the above assumptions, the grinding wheel area is not a constant but a function A(f(x)) of f(x). The area of ​​the wheel segment acting on the infinitesimal portion dx is the radius R of the wheel circle C. 1 -x to R 1 Since this is the region, integrating f(t) over this region gives the following equation (3).

number

number

[0071] Consider polar coordinates (r, θ) with C in Figure 10 as the origin. a = (π / 4) × {(R 1 -R 2 ) / R2},r=R 1 -x R 1 -R 2 ≦r≦R 1 The length of the arc of the thick two-dot chain line in Figure 10 at the radius r of the grinding wheel ring is (π / 4) × (R 1 -R 2 ) Therefore, the angle θ of the thick two-dot chain line in Figure 10 0 (r) is 2π×(π / 4)×{(R 1 -R 2 ) / 2πr}=(π / 4)×{(R 1 -R 2 ) / r}. Therefore, the thick solid line in Figure 10 is θ=π-θ 0 (r)(R 1 -R 2 ≦r≦R 1 ) That is, θ = π-(π / 4) × (R 1 -R 2 ) / r (R 1 -R 2 ≦r≦R 1 ).

[0072] In the above operation, the equation of the contour line is obtained by considering a clockwise circular arc based on the X-axis. Next, if we consider a counterclockwise arc based on the X-axis and perform the same operation, the equation of the contour line is θ=π+π / 4×(R 1 -R 2 ) / r (R 1 -R 2 ≦r≦R 1 ).

[0073] By rotating these by π / 2 in sequence, the contours of the shape shown by the thick solid lines in Figure 11 are obtained with four-fold symmetry. These contours and the circle r=R shown by the two-dot chain line are 1 -R 2 and the grey circle r=R 1 By arranging the grindstone in the area surrounded by the upper arc, the density of the abrasive grain tracks on the substrate can be made constant. However, this shape still does not solve the problem of the central part of the substrate being largely removed. This means that the problem cannot be solved by simply eliminating 1 / x from the abrasive grain track density parameter.

[0074] Unlike mechanical grinding using diamond wheels, the grinding process of the present invention utilizes tribo-oxidation reaction, so the removal depth h may be a function of the relative speed between the minute part dx and the grinding wheel. Therefore, the relative speed between the abrasive grains and the workpiece is considered as follows. In grinding, the rotation speed of the grinding wheel is overwhelmingly higher than the rotation speed of the substrate, and based on Preston's equation in polishing, it is assumed that the removal depth h is proportional to the abrasive velocity as well as the abrasive track density at dx. The grain velocity is also a function of x, and the distance from the center of the grain circle r=R 1 Since it increases in proportion to -x, if the arc length in the circumferential direction of the grinding wheel where h is constant is a function of x, then we obtain the following equation (5).

number

[0075] Therefore, if a is a constant in equation (5), it becomes equation (6).

number

[0076] The above-mentioned shape design is just one example, and various variations are possible. Figure 3 shows the shape obtained in Figure 12, Figure 2 shows an example in which the folded part is eliminated and the area is halved, and Figure 4 shows an example in which the initial reference line is an angled straight line instead of the X-axis. In the above, it has been assumed that the removal depth h is proportional to the abrasive grain velocity as well as the abrasive grain track density at dx, but even if it is more generally assumed to be proportional to the pth power of the abrasive grain velocity, the segment shape can be determined by treating it in the same way. In order to uniformly process large-diameter single crystal SiC substrates, the exponent p of the abrasive grain velocity is a real number equal to or greater than 1, and is preferably in the range of 1 to 3, and more preferably in the range of 1 to 2. By adopting this segment shape, it has become possible to uniformly process large-diameter single-crystal SiC substrates.

[0077] Based on the above-mentioned concept, the following items (a) and (b) are essential requirements for appropriate segment shape and arrangement. (a) The segments that contribute to the machining are on the grinding plate, with a concentric radius R 1 -R 2 The radius R of the circle is the same as the outside of the circle. 1 circle, i.e., inside the circumference of the grinding plate. (b) Draw a circle of radius r that is concentric with the grinding plate. 1 -R 2 From R 1 When the radius R 1 -R 2 Let L be the sum of the arc lengths of the overlapping parts of the circle and the segment, and let the sum of the arc lengths of the overlapping parts of the concentric circle of radius r and the segment be L × (R 1 -R 2 ) / r.

[0078] In addition, since the grinding plate rotates at high speed, it is desirable to satisfy the following item (c). (c) The shape and arrangement of the segments must have a reasonable degree of symmetry so that the grinding plate does not become imbalanced during rotation. Although not an essential requirement, it is desirable to satisfy the following item (d) from the practical aspect of actually producing the grinding plate. (ii) Even if the contours other than the circular arcs are approximated by straight lines to produce the grinding plate, the segment shape will not substantially affect the effect of the invention.

[0079] (Manufacturing method for single crystal SiC substrate) A method for manufacturing a single crystal SiC substrate according to one embodiment of the present invention includes a step of processing the surface of a substrate by the surface processing method according to the above embodiment. The method of the present invention utilizes oxidation on the SiC surface, and is therefore preferably applicable to the C-face of the (0001) surface of a SiC substrate, taking into account the height of the oxidation barrier and the properties of the oxidation product.

[0080] (Single crystal SiC substrate) The single crystal SiC substrate obtained by the means described in the above embodiment has a mirror surface with a small damaged layer. Specifically, the single crystal SiC substrate according to this embodiment has a C-face damaged layer of 1 μm or less, a surface roughness Sa in the range of more than 1 nm to 5 nm or less, and a diameter of 145 mm or more. The single crystal SiC substrate according to this embodiment has a surface roughness one order of magnitude greater than that of a mirror surface obtained by CMP, for example. The surface roughness of the single crystal SiC substrate according to this embodiment is preferably 2 nm or more and 5 nm or less, more preferably 2 nm or more and 3 nm or less. The conductivity type of the single crystal SiC substrate may be n-type, p-type, or semi-insulating.

[0081] The mirror surface can be confirmed by visual observation or optical microscope observation. The smallness of the processing-affected layer can be confirmed by warping due to the Twyman effect. The Si surface of a commercially available SiC substrate is usually processed by CMP, so the processing-affected layer is 1 μm or less. When the C surface of an as-received SiC substrate is diamond-ground as the starting surface to which the present invention is applied, the processing-affected layer of the C surface is large, so that the C surface side has a convex shape due to the Twyman effect. If the surface processing of the present invention is subsequently applied to the C surface, the C surface side has a concave shape. Therefore, the processing-affected layer obtained by the present invention is at least 1 μm or less, and preferably 0.5 μm or less.

[0082] The surface roughness can be confirmed, for example, by using a scanning white light interferometer. In Non-Patent Document 6, the surface roughness of CMP is 0.1 nm or less, and it can be confirmed that the surface roughness is one order of magnitude larger than this value.

[0083] In the present invention, the single crystal SiC substrate having a diameter of 145 mm or more and having a C-face that has been finally processed has a process-affected layer of 1 μm or less on the C-face and a surface roughness Sa in the range of more than 1 nm and less than 5 nm, and is therefore suitable as a substrate with small warpage due to the Twyman effect. If the process-affected layer is greater than 1 μm, the warpage due to the Twyman effect may be large, and if the surface roughness Sa is 1 nm or less, the preferable effects of identifying the front and back of the substrate, facilitating sensing of the substrate in an automatic substrate transport mechanism, and preventing slippage when the substrate is placed horizontally may be hindered. In addition, in the present invention, the single crystal SiC substrate having a diameter of 145 mm or more and having a C-face that has been finally processed preferably has a process-affected layer of 0.5 μm or less on the C-face and a surface roughness Sa of 2 nm or more and less than 5 nm. This configuration is even more suitable as a substrate with smaller warpage due to the Twyman effect, as required in Patent Document 5. Having the processing-affected layer on surface C be 0.5 μm or less makes it possible to prevent greater risk of warping due to the Twyman effect, and having a surface roughness Sa of 2 nm or more is even more preferable since it makes it possible to more easily identify the front and back of the substrate, to more easily sense the substrate in an automatic substrate transport mechanism, and to prevent slipping when the substrate is placed horizontally.

[0084] In the present invention, the single crystal SiC substrate having a diameter of 145 mm or more, in which the C-face is finally processed, has a process-affected layer of 1 μm or less on the C-face, and a surface roughness Sa in the range of more than 1 nm and less than 5 nm, and is therefore suitable as a seed crystal. If the process-affected layer is greater than 1 μm, it may be difficult to remove factors that inhibit crystal growth, and if the surface roughness Sa is less than 1 nm, it may be difficult to perform uniform etching, and if it is greater than 5 nm, the surface roughness of the etched surface may become large and abnormal nuclei may be easily generated. In addition, the single crystal SiC substrate having a diameter of 145 mm or more, in which the C-face is finally processed, has a process-affected layer of 0.5 μm or less on the C-face, and a surface roughness Sa of 2 nm or more and less than 5 nm, and is therefore even more suitable as a seed crystal as required by Patent Document 6. If the process-affected layer is less than 0.5 μm, it is possible to prevent the factors that inhibit crystal growth from becoming difficult to remove, and if the surface roughness Sa is more than 2 nm, it is even more suitable. EXAMPLES

[0085] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0086] Example 1 Wheel radius R 2 = 150mm, radius R of 6 inch board 1 = 75 mm, and the power exponent of the abrasive grain velocity p = 1 were applied, and a polar coordinate plot was performed in Excel to obtain the segment shape of the grinding wheel segment shown in Figures 3 and 4. The segment shape obtained from the polar coordinate plot is called the effective segment shape. In order to avoid the acute angle of the segment, an area of ​​5 mm that does not contact the substrate is added to the effective segment shape toward the center of the circle. That is, the grindstone segment produced in Example 1 is not the inner peripheral end of the effective segment obtained by the polar coordinate plot, but has an area of ​​5 mm added (that is, an extra grindstone segment is provided 5 mm radially inward from the effective segment shape). In the following explanation, the inner peripheral end, which is the radially inner end of the grindstone segment, refers to the inner peripheral end of the segment actually produced. When attaching the segment to the base metal, since the outer diameter of the base metal is 300 mm and the inner diameter is 120 mm, the outer peripheral end of the grindstone segment and the outer peripheral end E2 of the base metal are aligned, and the inner peripheral end of the grindstone segment and the inner peripheral end E1 of the base metal are aligned. The surface of a ring-shaped aluminum alloy base metal with an outer diameter of 300 mm, which was prepared so that it could be attached to a Tokyo Seimitsu HRG300, was machined flat to face the workpiece, and four Nitta Haas Corporation CMP pads SUBA600 (soft pads) segmented into a shape that reproduces the shape shown in Figure 3 were attached to create a grinding plate base. This grinding plate base was trued using a conditioner CMP-MP100A manufactured by Asahi Diamond Industrial Co., Ltd. A waterproof abrasive paper (grain size: #1000, abrasive: C (SiC abrasive grains) manufactured by Trusco Nakayama Co., Ltd., which was also segmented into the shape shown in Figure 3, was attached to the trued SUBA600 segment surface to produce a grinding plate for surface processing of single crystal SiC substrates with tribo-oxidation properties.

[0087] Next, the prepared grinding plate was mounted on the grinding device HRG300, and a 6-inch diameter n-type (000-1) 4H-SiC (4° off) single crystal SiC substrate (C-face) made of SICC, which had been ground flat in advance with a vitrified bond diamond wheel (No. 2000) made by Tokyo Seimitsu Co., Ltd., was fixed to the workpiece table using a vacuum chuck, and surface processing was performed. That is, in the embodiment, surface processing was performed using a grinding device equipped with a grindstone segment having a segment shape designed to perform uniform processing based on the abrasive grain trajectory density in the workpiece surface determined by the arrangement of the grinding plate and the workpiece table, and the relative speed of the abrasive grain and the workpiece. In the surface processing, the grinding plate was driven while maintaining the arrangement in which the outer peripheral end of the grindstone segment was on the axial center of the workpiece table. The grinding plate rotated counterclockwise at a rotation speed of 1000 rpm, and the workpiece table rotated counterclockwise at a rotation speed of 400 rpm, with air blowing for cooling. The infeed of the grinding plate was performed by manually feeding it gradually, so that the increase in the motor current for rotating the grinding wheel was within the range of 0.8 to 1.1 A. Processing was performed intermittently, and the total processing time was 10 minutes.

[0088] The amount of removal from the single crystal SiC substrate was calculated by measuring the thickness of the substrate before and after processing at five points on the surface using a Mitutoyo height meter, and the average was 3.0 μm. The processing speed was a high 0.3 μm / min. The average substrate thickness after processing was 471.4 μm, with a difference between the maximum and minimum values ​​of 1.1 μm, indicating that processing was uniform.

[0089] FIG. 13 shows the results of differential interference contrast observation of the substrate surface before processing, and FIG. 14 shows the results of differential interference contrast observation of the substrate surface after processing, using an Olympus optical microscope. The countless grinding marks caused by #2000 diamond abrasive grains that were observed on the substrate before processing had completely disappeared, and a mirror surface without processing distortion had been achieved.

[0090] In addition, when the warpage of the processed single crystal SiC substrate was measured using a high-precision wafer shape and thickness measuring instrument Flat Master MSP manufactured by Tropel, the C-face was warped concavely, and the warpage value was small at 49.9 μm. Since the Si-face on the back side is an epi-ready surface of an as-received, the processing-affected layer is 1 μm or less. Since the C-face warps concavely, it means that the processing-affected layer on the C-face is even smaller, and it was shown to be 1 μm or less. For further confirmation, the back side of this substrate, i.e., the Si-face, was processed using a grindstone that has been confirmed to have a processing-affected layer of 0.5 μm or less by the step polishing method described in Non-Patent Document 1. When the warpage of this substrate was measured, the C-face was also warped concavely, and the warpage value was slightly larger at 72.9 μm. This confirmed that the processing-affected layer on the C-face was 0.5 μm or less.

[0091] Furthermore, the surface roughness of the processed substrate surface was measured using a Zygo New View 7300 scanning white light interferometer. The objective lens was set to 10X, and to extract the roughness components, the band pass filter was set as described in the manual, with a value of 1 / 4 of the "Size Y" input in the "Filter Low Wavelen" and a value three times the "Camera Res" input in the "Filter High Wavelen". The resulting surface roughness Sa was 2 nm, more than an order of magnitude higher than the surface roughness Sa obtained by CMP.

[0092] (Comparative Example) 5 shows a shape that is the first step in determining a segment shape for uniformly processing a 6-inch substrate by trial and error with reference to the drawing shown in Patent Document 4. That is, in the comparative example, surface processing was performed on a single crystal SiC substrate using a grindstone segment having a segment shape that is not designed to perform uniform processing based on the relative speed of the abrasive grains and the workpiece. In the comparative example, grinding was performed in the same manner as in the example, except that the SUBA600 and waterproof abrasive paper were segmented into a shape that reproduced the shape shown in Figure 5, and the amount of removal of the single crystal substrate was calculated in the same manner as in the example. The average value was 3.6 μm. The difference between the maximum and minimum thicknesses of the substrate after processing was 3.2 μm, indicating that processing was not uniform. This was not a problem with substrates of small area, but it was shown that the burden of trial and error increases as the area increases. In the comparative example, the central portion of the surface-processed single crystal SiC substrate was hardly scraped off, the process-affected layer in that portion was larger than 1 μm, and the surface roughness was 14 nm.

[0093] Example 2 The C-side of a 6-inch substrate was processed in the same manner as in Example 1, except that the segment shape of the grinding wheel segment was changed to that shown in Figure 2 and that the Si-side and C-side of the substrate were processed in advance, and evaluation was performed in the same manner as in Example 1. Specifically, in Example 2, when the Si surface of the substrate was pre-processed, a grindstone was used that was confirmed to have a processing-induced layer of 0.5 μm or less by the step polishing method described in Non-Patent Document 1. Also, when the C surface of the substrate was pre-processed, diamond abrasive grains with a grit size of 4000 were used. The C surface was pre-processed to be flat using the above diamond abrasive grains. The removal amount of the single crystal SiC substrate was 1.7 μm on average. The processing speed was high at 0.17 μm / min. The average substrate thickness after processing was 489.0 μm, and the difference between the maximum and minimum values ​​was 0.6 μm, indicating that the substrate was processed uniformly. In addition, the warpage of the single crystal SiC substrate after processing was still concave on the C-face, and the warpage value was somewhat large at 84.5 μm. This confirmed that the processing-affected layer on the C-face was 0.5 μm or less. Furthermore, the surface roughness Sa of the processed substrate was 2 nm, which was more than one order of magnitude higher than the surface roughness Sa obtained by CMP.

[0094] Example 3 The C-side of a 6-inch substrate was processed in the same manner as in Example 2, except that the waterproof abrasive paper was formed into a segment shape obtained by assuming a power exponent p=1.5 of the abrasive grain speed, and was evaluated in the same manner as in Example 2. In this segment shape, if the arc length at the inner peripheral end of the segment shape shown in FIG. 2 is the same, the arc length at the outer peripheral end is about 0.7 times that of the segment shape shown in FIG. 2. Therefore, waterproof abrasive paper having a segment shape in which the arc length at the inner peripheral end of the segment shape shown in FIG. 2 is left unchanged, the arc length at the outer peripheral end is set to 0.7 times, and the other two sides of the contour are linearly approximated was prepared. A grinding plate was produced by attaching the waterproof abrasive paper having a segment shape obtained by assuming a power exponent p=1.5 of the abrasive grain speed onto a SUBA pad so as not to protrude from the pad, and processing and evaluation were performed. The removal amount of the single crystal SiC substrate was 2.7 μm on average. The processing speed was high at 0.27 μm / min. The average substrate thickness after processing was 471.8 μm, with a difference between the maximum and minimum values ​​of 1.9 μm, indicating that processing was uniform. In addition, the warpage of the single crystal SiC substrate after processing was still concave on the C-face, and the warpage value was somewhat large at 89.0 μm. This confirmed that the processing-affected layer on the C-face was 0.5 μm or less. Furthermore, the surface roughness Sa of the processed substrate was 2.8 nm, which was more than one order of magnitude higher than the surface roughness Sa obtained by CMP.

[0095] Example 4 The C-side of a 6-inch substrate was processed in the same manner as in Example 2, except that the waterproof abrasive paper was formed into a segment shape obtained by assuming a power exponent p=2.0 of the abrasive grain speed, and was evaluated in the same manner as in Example 2. In this segment shape, if the arc length at the inner peripheral end of the segment shape shown in FIG. 2 is the same, the arc length at the outer peripheral end is about 0.5 times that of the segment shape shown in FIG. 2. Therefore, waterproof abrasive paper having a segment shape in which the arc length at the inner peripheral end of the segment shape shown in FIG. 2 is left unchanged, the arc length at the outer peripheral end is set to 0.5 times, and the other two sides of the contour are linearly approximated was prepared. A grinding plate was produced by attaching the waterproof abrasive paper having a segment shape obtained by assuming a power exponent p=2.0 of the abrasive grain speed onto a SUBA pad so as not to protrude from the pad, and processing and evaluation were performed. The removal amount of the single crystal SiC substrate was 2.5 μm on average. The processing speed was high at 0.25 μm / min. The average substrate thickness after processing was 461.4 μm, and the difference between the maximum and minimum values ​​was 0.7 μm, indicating that processing was uniform. In addition, the warpage of the single crystal SiC substrate after processing was still concave on the C-face, and the warpage value was somewhat large at 91.0 μm. This confirmed that the processing-affected layer on the C-face was 0.5 μm or less. Furthermore, the surface roughness Sa of the processed substrate was 2.8 nm, which was more than one order of magnitude higher than the surface roughness Sa obtained by CMP. [Industrial Applicability]

[0096] The surface processing method for a single crystal SiC substrate, the manufacturing method thereof, and the grinding plate for surface processing of a single crystal SiC substrate of the present invention can be used to produce a single crystal SiC substrate or a seed crystal, and can also be used in a process of processing the back surface of a substrate after a device has been formed thereon to thin the substrate. [Explanation of symbols]

[0097] 1 base money 2A, 2B, 2C, 2X Grindstone Segments 10A, 10B, 10C, 10X Grinding Plate 11 Drive unit 12 Grindstone flange 14 Workpiece table 15 Board holding part W Single crystal SiC substrate

Claims

1. A grinding plate comprising: The grinding plate includes a grindstone segment on a base metal having a flat surface, The grindstone segment has a soft pad having abrasive grains fixed to a surface thereof or a resin-bonded grindstone containing abrasive grains and a resin; The grindstone segments have a segment shape designed to perform uniform machining based on the density of abrasive grain tracks in the surface of the workpiece determined by the arrangement of the grinding plate and the workpiece table, and the relative speed of the abrasive grains and the workpiece, The grinding plate is characterized in that the abrasive grains are made of at least one metal oxide that is softer than single crystal SiC and has a band gap, or SiC.

2. 2. The grinding plate according to claim 1, wherein the abrasive grains are made of at least one metal oxide selected from the group consisting of cerium oxide, titanium oxide, silicon oxide, aluminum oxide, iron oxide, zirconium oxide, zinc oxide, and tin oxide.

3. 2. The grinding plate of claim 1, wherein the abrasive grains are made of SiC.

4. A grinding device comprising the grinding plate according to any one of claims 1 to 3.

5. A surface processing method comprising: mounting the grinding plate according to any one of claims 1 to 3 on a grinding device; and processing a surface of a single crystal SiC substrate having a diameter of 145 mm or more without using a liquid coolant.

6. A method for producing a single crystal SiC substrate, comprising the step of processing a surface of a substrate by the surface processing method according to claim 5.

7. A single crystal SiC substrate having a C-face process-affected layer of 1 μm or less, a surface roughness Sa of more than 1 nm and 5 nm or less, and a diameter of 145 mm or more.

Citation Information

Patent Citations

  • Operation control valve for agricultural tractor

    JP1980060774A

  • Superimposed vibratory cutting method

    JP1985016301A

  • Method for growing silicon carbide single crystal, seed crystal, and silicon carbide single crystal

    JP2010111540A

  • Seventy five millimeter silicon carbide wafer with low warp, bow, and ttv

    JP2012214376A

  • Flat SiC semiconductor substrate

    JP2016501809A