Silicon carbide single crystal and method for manufacturing the same
By controlling the growth of SiC single crystals with periodic variations in dopant gas flow rate to manage specific resistance, the method addresses the challenge of maintaining high growth rates and suppressing differently oriented crystals, enhancing yield and reducing costs.
Patent Information
- Application Number
- JP2023062933
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
AI Technical Summary
Existing methods for growing silicon carbide (SiC) single crystals face challenges in maintaining a high growth rate while suppressing the formation of differently oriented crystals, which leads to reduced product yield and increased costs due to the need for etching to remove these crystals.
A method involving a SiC single crystal manufacturing apparatus that controls the growth of SiC single crystals by periodically varying the specific resistance through adjustments in the flow rate of dopant gas, such as nitrogen, to suppress the formation of differently oriented crystals without etching, thereby maintaining a high growth rate.
This approach effectively suppresses the formation and expansion of differently oriented crystals, enhancing product yield and reducing manufacturing costs by maintaining a stable growth rate without the need for etching, thus improving the overall efficiency of SiC single crystal production.
Smart Images

Figure 2024149201000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to silicon carbide (hereinafter referred to as SiC) single crystal and a method for producing the same. [Background technology]
[0002] Conventionally, the gas growth method has been known in which SiC raw material gas is supplied to the growth surface of a seed crystal made of SiC single crystal, and SiC single crystal is grown on the seed crystal. In the gas growth method, in addition to the SiC raw material gas, H2 (hydrogen) gas, which acts as a carrier gas, and N2 (nitrogen) gas, which acts as a dopant to adjust the resistivity of the crystal, are introduced to produce SiC single crystal.
[0003] Increasing the growth rate of SiC single crystals is an effective way to reduce the cost of producing SiC single crystals. However, if the growth rate is too high, polycrystalline grains called misoriented crystals may appear within the SiC single crystal, and the misoriented crystals may expand as they grow.
[0004] Once a SiC single crystal ingot is obtained by growing the SiC single crystal, it is sliced and processed into wafers, and devices are fabricated on the wafer through semiconductor processes, but devices in areas where crystals with different orientations exist are defective. Therefore, even if high-speed growth is performed with the aim of reducing costs, the product yield decreases and costs end up being higher.
[0005] In response to this, Patent Document 1 proposes a technique for removing misorientation, in which the growing SiC single crystal is monitored, and if misorientation occurs, etching gas is introduced into the furnace to etch the entire SiC single crystal until the misorientation disappears. This makes it possible to suppress the generation of misorientated crystals and prevent a decrease in product yield. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2004-43211 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, with the technology of Patent Document 1, the SiC single crystal is etched during growth, which causes losses in the growth of the SiC single crystal due to the etching, resulting in a decrease in the effective growth rate and an increase in production costs.
[0008] An object of the present disclosure is to provide a method for producing a SiC single crystal that can suppress the formation of misoriented crystals while suppressing a decrease in growth rate, and a SiC single crystal in which the formation of misoriented crystals is suppressed. [Means for solving the problem]
[0009] A first aspect of the present disclosure is A SiC single crystal, At least in a portion of the crystal, resistivity repeatedly changes in the growth direction, with the resistivity gradually increasing and then decreasing.
[0010] In this way, the resistivity of the SiC single crystal increases and decreases gradually. Even if different orientation crystals are generated in such a SiC single crystal, they are not inherited during growth, and the expansion is suppressed. Therefore, the SiC single crystal can be made to have different orientation crystals suppressed.
[0011] A second aspect of the present disclosure is A method for producing a SiC single crystal, comprising the steps of: A pedestal (10) is placed in a crucible (9) having a hollow portion that constitutes a reaction chamber, and a seed crystal (2) for growing a SiC single crystal (3) is placed on one surface of the pedestal; supplying a SiC source gas (20) for growing the SiC single crystal on the surface of the seed crystal, a carrier gas (21), and a dopant gas (22) containing a dopant from below the pedestal, and heating and decomposing the source gas before supplying it to the seed crystal, thereby growing the SiC single crystal on the surface of the seed crystal, In growing the SiC single crystal, the resistivity of the SiC single crystal repeatedly increases and decreases gradually with respect to the growth distance, thereby growing the SiC single crystal.
[0012] In this way, by simply repeatedly gradually increasing and decreasing the resistivity during the growth of the SiC single crystal, it is possible to eliminate the misoriented crystals without etching and also to suppress a decrease in the substantial growth rate of the SiC single crystal. Therefore, it is possible to provide a method for producing a SiC single crystal that can suppress a decrease in the growth rate while suppressing the misoriented crystals.
[0013] Note that the reference symbols in parentheses attached to each component indicate an example of the correspondence between the component and specific components described in the embodiments described below. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a cross-sectional view of a SiC single crystal manufacturing apparatus according to a first embodiment. [Diagram 2] FIG. 13 is a diagram showing the variation in the flow rate of N2, which serves as a dopant gas, with respect to growth time. [Diagram 3] FIG. 3 is a binarized diagram of a microscope image when the resistivity is repeatedly increased and decreased by varying the flow rate of the dopant gas as shown in FIG. [Figure 4] FIG. 13 is a diagram showing a comparative example in which resistivity is changed in a pulsed manner with respect to growth distance. [Diagram 5] FIG. 11 is a diagram showing the variation in growth rate with respect to growth time described in another embodiment. [Figure 6]FIG. 13 is a diagram showing a case where resistivity is repeatedly and gradually increased and decreased with respect to the growth distance, which will be described in another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In the following embodiments, parts that are the same or equivalent to each other will be denoted by the same reference numerals.
[0016] (First embodiment) The SiC single crystal manufacturing apparatus 1 shown in Fig. 1 is used to manufacture a SiC single crystal ingot by long-length growth. Using this SiC single crystal manufacturing apparatus 1, a method for manufacturing a SiC single crystal that can increase the growth rate while suppressing differently oriented crystals is provided.
[0017] 1 faces the top and bottom, and supplies SiC raw material gas to the surface of seed crystal 2 made of a SiC single crystal substrate, causing SiC single crystal 3 to grow on the surface of seed crystal 2. Specifically, SiC single crystal manufacturing apparatus 1 is equipped with a gas supply unit 4, a gas introduction source 5, a gas exhaust port 6, a vacuum vessel 7, a heat insulating material 8, a heating vessel 9, a pedestal 10, a rotary pull-up mechanism 11, and first and second heating devices 12 and 13.
[0018] The gas supply unit 4 is provided below the SiC single crystal manufacturing apparatus 1, and introduces a raw material gas 20 containing various gases that serve as SiC raw materials from a gas introduction source 5, a carrier gas 21, and a dopant gas 22 into the SiC single crystal manufacturing apparatus 1.
[0019] The gas supply unit 4 includes a raw material gas supply unit 4a that supplies a raw material gas 20, a carrier gas supply unit 4b that supplies a carrier gas 21, and a dopant gas supply unit 4c that supplies a dopant gas 22. Although not shown in the figure, each of these gas supply units 4a to 4b is composed of components that constitute a supply path. The raw material gas supply unit 4a introduces the raw material gas 20 from a raw material gas source 5a, which will be described later, into the SiC single crystal manufacturing apparatus 1. The carrier gas supply unit 4b introduces the carrier gas 21 from a carrier gas source 5b, which will be described later, into the SiC single crystal manufacturing apparatus 1. The dopant gas supply unit 4c introduces the dopant gas 22 from a dopant gas source 5c, which will be described later, into the SiC single crystal manufacturing apparatus 1.
[0020] The gas introduction source 5 supplies gas containing a SiC raw material gas into the SiC single crystal manufacturing apparatus 1. In this embodiment, the gas introduction source 5 includes a raw material gas source 5a, a carrier gas source 5b, and a dopant gas source 5c.
[0021] The source gas source 5a supplies a source gas 20 including a SiC source gas containing Si and C, for example, a mixed gas of a silane-based gas such as silane and a hydrocarbon-based gas such as propane. The carrier gas source 5b supplies a carrier gas 21 such as H2. The dopant gas source 5c supplies a dopant gas 22 such as N2. Although not shown, each of these gas sources 5a to 5c is equipped with a heating device for controlling the temperature of each supply gas and a flow rate control device for controlling the flow rate, and the temperature and flow rate of each supply gas can be controlled according to the growth status of the SiC single crystal 3.
[0022] The gas outlet 6 discharges unreacted gas in the source gas 20 after being supplied to the seed crystal 2, the carrier gas 21, the dopant gas 22, and the like, as exhaust gas to the outside of the SiC single crystal manufacturing apparatus 1.
[0023] The vacuum vessel 7 is made of quartz glass or the like, has a hollow cylindrical shape, in this embodiment, and is structured to allow the introduction and discharge of the raw material gas 20, the carrier gas 21, and the dopant gas 22. The vacuum vessel 7 also accommodates other components of the SiC single crystal manufacturing apparatus 1, and is structured to allow the pressure of the internal space in which it is accommodated to be reduced by evacuating. As described above, the bottom of the vacuum vessel 7 is provided with the raw material gas supply unit 4a for supplying the raw material gas 20, the carrier gas supply unit 4b for supplying the carrier gas 21, and the dopant gas source 5c for supplying the dopant gas 22. A through hole 7a is formed in the upper part of the vacuum vessel 7, specifically, in the upper position of the side wall, and a gas outlet 6 for exhaust gas such as unreacted gas of the raw material gas 20 is fitted into the through hole 7a.
[0024] The heat insulating material 8 has a hollow cylindrical shape, and in this embodiment, is arranged coaxially with the vacuum vessel 7. The heat insulating material 8 has a cylindrical shape with a smaller diameter than the vacuum vessel 7, and is arranged inside the vacuum vessel 7 to suppress heat transfer from the space inside the heat insulating material 8 to the vacuum vessel 7. The heat insulating material 8 is made of, for example, graphite, but the surface may be coated with a high melting point metal carbide such as TaC (tantalum carbide) or NbC (niobium carbide) to make it difficult to be thermally etched. A through hole 8a is also formed in the upper part of the heat insulating material 8, specifically, in the upper position of the side wall, and the gas exhaust port 6 is fitted into this through hole 8a.
[0025] The heating vessel 9 constitutes a crucible serving as a reaction vessel, and is configured to have a tubular shape having a hollow portion, and in this embodiment, a cylindrical shape. The hollow portion of the heating vessel 9 constitutes a reaction chamber in which the SiC single crystal 3 is grown on the surface of the seed crystal 2. The heating vessel 9 is made of, for example, graphite, but the surface may be coated with a high melting point metal carbide such as TaC or NbC to make it difficult to be thermally etched. The heating vessel 9 is disposed so as to surround the pedestal 10. Then, exhaust gas such as unreacted gas in the raw material gas 20 is guided to the gas outlet 6 through the inner peripheral surface of the heating vessel 9 and the outer peripheral surfaces of the seed crystal 2 and the pedestal 10. The heating vessel 9 decomposes the SiC raw material gas in the raw material gas 20 before the raw material gas 20 from the raw material gas supply unit 4a is guided to the seed crystal 2. In addition, a through hole 9a is also formed in the upper part of the heating vessel 9, specifically, in the upper position of the side wall, and the gas outlet 6 is fitted into this through hole 9a.
[0026] The pedestal 10 is a member for mounting the seed crystal 2. The pedestal 10 has a circular surface on which the disk-shaped seed crystal 2 is mounted, and the central axis of the pedestal 10 is arranged coaxially with the central axis of the heating vessel 9 and the central axis of the shaft 11a of the rotary lifting mechanism 11 described later. The pedestal 10 is made of, for example, graphite, but the surface may be coated with a high melting point metal carbide such as TaC or NbC to make it difficult to be thermally etched. The seed crystal 2 is attached to one surface of the pedestal 10 on the side of the raw material gas supply unit 4a, and the SiC single crystal 3 is grown on the surface of the seed crystal 2. The pedestal 10 is connected to the shaft 11a on the surface opposite to the surface on which the seed crystal 2 is disposed, and is rotated with the rotation of the shaft 11a, and can be pulled up above the paper surface as the shaft 11a is pulled up.
[0027] The rotary pull-up mechanism 11 rotates and pulls up the pedestal 10 via a shaft 11a made of a pipe material or the like. In this embodiment, the shaft 11a is configured in a straight line extending up and down, with one end connected to the surface of the pedestal 10 opposite to the surface to which the seed crystal 2 is attached, and the other end connected to the main body of the rotary pull-up mechanism 11. This shaft 11a is also made of, for example, graphite, but the surface may be coated with a high-melting point metal carbide such as TaC or NbC to make it difficult to be thermally etched. With this configuration, the pedestal 10, the seed crystal 2, and the SiC single crystal 3 can be rotated and pulled up, and the growth surface of the SiC single crystal 3 can be adjusted to a temperature suitable for growth while the growth surface of the SiC single crystal 3 has a desired temperature distribution.
[0028] The first and second heating devices 12 and 13 are configured with heating coils such as induction heating coils and direct heating coils, and are arranged to surround the vacuum vessel 7. In the present embodiment, the first and second heating devices 12 and 13 are configured with induction heating coils. The first and second heating devices 12 and 13 are configured to be able to independently control the temperature of the target locations, with the first heating device 12 being arranged at a position corresponding to the lower position of the heating vessel 9, and the second heating device 13 being arranged at a position corresponding to the pedestal 10. Therefore, the first heating device 12 can control the temperature of the lower portion of the heating vessel 9 to heat and decompose the SiC raw material gas. In addition, the second heating device 13 can control the temperatures around the pedestal 10, the seed crystal 2, and the SiC single crystal 3 to temperatures suitable for the growth of the SiC single crystal 3.
[0029] Thus, the SiC single crystal manufacturing apparatus 1 is configured. Next, a method for manufacturing a SiC single crystal 3 using the SiC single crystal manufacturing apparatus 1 according to this embodiment will be described.
[0030] First, the seed crystal 2 is attached to one surface of the pedestal 10. The surface of the seed crystal 2 opposite to the pedestal 10, that is, the growth surface of the SiC single crystal 3, is an off-substrate having a predetermined off-angle, such as 4° or 8°, with respect to the (0001) C-plane. Next, the pedestal 10 and the seed crystal 2 are placed in the heating vessel 9. Then, the first and second heating devices 12 and 13 are controlled to provide a desired temperature distribution. That is, the temperature distribution is set so that the SiC raw material gas contained in the raw material gas 20 is thermally decomposed and supplied to the surface of the seed crystal 2, and the SiC raw material gas is recrystallized on the surface of the seed crystal 2, while the sublimation rate is higher than the recrystallization rate in the heating vessel 9. In this way, the temperature of the bottom of the heating vessel 9 can be set to a high temperature of 2000° C. or higher, for example, 2400° C., and the temperature of the surface of the seed crystal 2 can be set to a temperature lower than the bottom of the heating vessel 9 and suitable for recrystallization of the SiC single crystal 3, for example, about 2200° C.
[0031] Furthermore, while the vacuum vessel 7 is maintained at a desired pressure, a source gas 20 containing a SiC source gas is introduced through the source gas supply unit 4a. As a result, the source gas 20 is supplied to the seed crystal 2 as shown by the arrow in FIG. 1, and a SiC single crystal 3 is grown on the surface of the seed crystal 2 based on this gas supply. Furthermore, a carrier gas 21 is introduced through the carrier gas supply unit 4b, and a dopant gas 22 is introduced through the dopant gas supply unit 4c. As a result, the carrier gas 21 and the dopant gas 22 are caused to flow inside the heating vessel 9, and the SiC single crystal 3 is doped with N contained in the dopant gas 22.
[0032] Then, the rotary pull-up mechanism 11 rotates the pedestal 10, the seed crystal 2, and the SiC single crystal 3 via the shaft 11a while pulling them up in accordance with the growth rate of the SiC single crystal 3. This keeps the height of the growth surface of the SiC single crystal 3 almost constant, making it possible to control the temperature distribution of the growth surface with good controllability.
[0033] At this time, when growing the SiC single crystal 3, the flow rate of the dopant gas 22 is periodically and repeatedly changed as shown in Fig. 2 to change the N2 content in the SiC single crystal manufacturing apparatus 1 and periodically vary the resistivity in the SiC single crystal 3. Specifically, the dopant gas 22 introduced from the dopant gas supply unit 4c into the heating vessel 9 is periodically increased or decreased by adjusting the flow rate at the dopant gas source 5c. Here, the dopant gas 22 is periodically increased or decreased in a sinusoidal manner.
[0034] In this way, it was experimentally confirmed that by periodically varying the resistivity within the SiC single crystal 3, the misoriented crystals disappear at the micro-sized stage during growth, meaning that they are no longer inherited by the growing crystal. When the resistivity periodically changes, the amount of N introduced as a dopant gradually changes in the process of the resistivity gradually increasing or decreasing, and during this change, the misoriented crystals can be eliminated at the micro-sized stage.
[0035] This is shown in Figure 3. In the SiC single crystal 3, the color changes according to the resistivity, with a light color for high resistivity and a dark color for low resistivity. As shown in this figure, the color gradually changes from light to dark and from dark to light for each fluctuation period C1 along the growth direction A1 of the SiC single crystal 3. It can also be seen that misoriented crystals 30 are generated during the growth of the SiC single crystal 3, but as the color changes, the misoriented crystals 30 are no longer inherited even as the SiC single crystal 3 grows, and disappear from the subsequently grown crystal.
[0036] As a result of various verifications, such a phenomenon occurred when the resistivity was repeatedly increased and decreased gradually, but did not occur in a process in which the resistivity was not gradually increased or decreased. For example, there has been a marking doping technique in which the resistivity is changed in a pulsed manner during growth as shown in FIG. 4 by changing the amount of N2 introduced as a dopant in a pulsed manner, but the misoriented crystals 30 could not be eliminated even if the amount of N2 introduced in a pulsed manner was changed in this way. This is because, even if the resistivity is simply changed in a pulsed manner, the misoriented crystals 30 are generated in both cases where the resistivity is high and where the resistivity is low, and in both cases, the misoriented crystals 30 expand when the resistivity does not change. Therefore, it can be said that it is necessary to repeatedly increase and decrease the resistivity gradually in order to eliminate the misoriented crystals 30. It is acceptable for there to be a portion that grows without changing the resistivity temporarily, and the growth amount of that portion should be tolerable even if the misoriented crystals 30 are generated and expanded in that portion.
[0037] To obtain the effect of eliminating the misoriented crystals 30, a certain degree of resistivity fluctuation is sufficient, and for example, it is preferable that the fluctuation range, i.e., the ratio of fluctuation to the median resistivity, is 0.5% or more. Also, if the resistivity fluctuation range becomes too large, it can cause defects such as heterogeneous polymorphism and dislocations. For this reason, it is preferable to make the resistivity fluctuation range 50% or less.
[0038] Furthermore, when the relationship between the change period of resistivity and the annihilation effect of the differently oriented crystal 30 was investigated, it was confirmed that if the change period of resistivity is too large, the size of the generated polycrystal becomes large and it may become impossible to annihilate it. It was found that such a phenomenon occurs when the change period of resistivity is greater than 500 μm in terms of the length of the SiC single crystal 3. When the change period of resistivity is converted into the length of the SiC single crystal 3, it is expressed as cycle time × growth rate = change period, and the change period is the value obtained by multiplying the time for one cycle shown as the growth time in Figure 2 by the growth rate of the SiC single crystal 3 at that time.
[0039] Furthermore, if the period of change in resistivity is too large, the thickness of the substrate cut from the SiC single crystal ingot is set to about 300 μm or 500 μm, and the resistivity of the wafer varies due to the period of change in resistivity. In other words, if the resistivity changes multiple times in the thickness of the wafer, the resistivity of each wafer will be averaged regardless of the position of the SiC single crystal ingot at which the wafer is cut. However, if the period of change in resistivity is large, the resistivity of the wafer will vary depending on the position at which the SiC single crystal ingot is cut, which will also cause variation in the characteristics of the final device.
[0040] Taking these factors into consideration, it is preferable that the period of change in resistivity is 500 μm or less when converted into the length of the SiC single crystal 3. Furthermore, taking into consideration the variation in resistivity when made into a wafer, it is preferable that the fluctuation width of the resistivity is 0.5% or more and less than 10%, and the period of change in resistivity is 100 μm or less when converted into the length of the SiC single crystal 3.
[0041] The periodic variation in resistivity does not necessarily have to be present in the entire region of the SiC single crystal ingot to be effective; if it is present in any region, it is possible to suppress the formation of misoriented crystals 30 in that region, and the effective region during device fabrication can be expanded. In particular, it is effective to impart periodic variation in resistivity to crystal regions and facet regions created under high-speed growth conditions in which misoriented crystals 30 are likely to be generated. For example, by varying the flow rate of the dopant gas 23 while supplying the source gas 20, carrier gas 21, and dopant gas 23 intensively to the facet region, periodic variation can be imparted to the resistivity in the facet region.
[0042] As described above, the SiC single crystal 3 of this embodiment has a resistivity that is gradually and repeatedly increased and decreased periodically. Even if differently oriented crystals 30 are generated in such a SiC single crystal 3, they are not inherited during growth, and the expansion is suppressed. Therefore, the SiC single crystal 3 can have differently oriented crystals 30 suppressed.
[0043] Furthermore, by manufacturing the SiC single crystal 3 by periodically and gradually repeatedly increasing and decreasing the resistivity according to this embodiment, even if misoriented crystals 30 are generated during the growth of the SiC single crystal 3, the expansion of the misoriented crystals 30 can be suppressed and they can disappear during the growth. Furthermore, there is no need to perform etching to remove the misoriented crystals 30.
[0044] When the SiC single crystal 3 is manufactured without varying the resistivity or by varying it in a pulsed manner, if the differently oriented crystals 30 are generated, the differently oriented crystals 30 will expand as they grow. For this reason, even if the SiC single crystal ingot obtained by growing the SiC single crystal 3 is cut out and processed into a wafer, and a device is manufactured on the wafer through a semiconductor process, the device in the region where the differently oriented crystals 30 exist will be defective. And, the more the range where the differently oriented crystals 30 exist expands, the more devices will become defective, and the lower the product yield will be. On the other hand, when the differently oriented crystals 30 are generated, it is possible to remove the differently oriented crystals 30 by etching the SiC single crystal 3, but the generation of the differently oriented crystals 30 must be monitored, and the etching causes a loss in the growth of the SiC single crystal 3, which reduces the actual growth rate and increases the product cost.
[0045] In contrast, according to the present embodiment, it is possible to eliminate the misoriented crystals 30 without etching, and also to suppress a decrease in the substantial growth rate of the SiC single crystal 3, simply by periodically and gradually and repeatedly increasing and decreasing the resistivity during the growth of the SiC single crystal 3. This also improves the product yield and reduces the manufacturing cost.
[0046] (Other embodiments) Although the present disclosure has been described based on the above-described embodiment, it is not limited to the embodiment, and includes various modifications and modifications within the equivalent range. In addition, various combinations and forms, and other combinations and forms including only one element, more than one element, or less than one element, are also within the scope and concept of the present disclosure.
[0047] For example, in the above first embodiment, the flow rate of the dopant gas 22 is repeatedly changed periodically to gradually increase and decrease the resistivity of the SiC single crystal 3, but this can also be achieved by a method other than adjusting the flow rate of the dopant gas 22.
[0048] That is, as shown in Fig. 5, even if the growth rate is gradually increased or decreased with respect to the growth time, the amount of dopant taken up changes, and the resistivity of the SiC single crystal 3 can be periodically varied. For example, under the condition that the flow rate of the dopant gas 22 is constant, the growth rate of the SiC single crystal 3 can be increased by increasing the flow rate of the source gas 20, increasing the partial pressure of the source gas 20, lowering the surface temperature of the SiC single crystal 3, or the like. Therefore, by adjusting one or more of the flow rate or partial pressure of the source gas 20, the surface temperature of the SiC single crystal 3, etc., the growth rate of the SiC single crystal 3 can be gradually increased or decreased periodically, and the resistivity of the SiC single crystal 3 can be periodically varied.
[0049] In the above, the resistivity of the SiC single crystal 3 is varied periodically, but it is not necessary to vary it at a constant period. For example, as shown in Fig. 6, if the resistivity repeatedly varies in such a way that the resistivity gradually increases and gradually decreases with respect to the growth distance of the SiC single crystal 3, the variation in resistivity may not be regular. Even in this case, it is sufficient that the variation period of each repeated increase and decrease is 500 µm or less when converted into the length of the SiC single crystal 3.
[0050] In the above first embodiment, the SiC single crystal manufacturing apparatus 1 has been described as being of an upflow type, in which the source gas 20 is supplied to the growth surface of the SiC single crystal 3, passes by the outer peripheral surface of the SiC single crystal 3 and the side of the pedestal 10, and is then discharged further upward. However, the present invention is not limited to this, and may be of a return flow type, in which the source gas 20 is supplied to the growth surface of the SiC single crystal 3, and then returned in the same direction as the supply direction. Alternatively, the present invention may be of a side flow type, in which the source gas 20 is supplied to the growth surface of the SiC single crystal 3, and then discharged in the outer peripheral direction of the heating vessel 9. [Explanation of symbols]
[0051] 1. SiC single crystal manufacturing equipment 2 seed crystals 3. SiC single crystal 4 Gas supply source 5 Gas introduction source 9 Heating container 10 Pedestal 20 Raw gas 21 Carrier gas 22 Dopant Gas
Claims
1. A silicon carbide single crystal, A silicon carbide single crystal, in which at least a portion of the crystal undergoes repeated resistivity fluctuations in the growth direction, in which the resistivity gradually increases and then decreases.
2. 2. The silicon carbide single crystal according to claim 1, wherein the resistivity fluctuation range is 0.5% or more and 50% or less.
3. 2. The silicon carbide single crystal according to claim 1, wherein a period of the repeated increase and decrease in resistivity is 500 μm or less when converted into a length of the crystal.
4. 2. The silicon carbide single crystal according to claim 1, wherein a fluctuation range of the resistivity is 0.5% or more and 10% or less, and a fluctuation period of repeated increases and decreases in the resistivity is 100 μm or less when converted into a length of the crystal.
5. 5. The silicon carbide single crystal according to claim 1, wherein the repeated variation in resistivity occurs in a facet region.
6. A method for producing a silicon carbide single crystal, comprising the steps of: A pedestal (10) is placed in a crucible (9) having a hollow portion constituting a reaction chamber, and a seed crystal (2) for growing a silicon carbide single crystal (3) is placed on one surface of the pedestal; supplying a silicon carbide source gas (20) for growing the silicon carbide single crystal on the surface of the seed crystal from below the pedestal, a carrier gas (21), and a dopant gas (22) containing a dopant, and heating and decomposing the source gas before supplying it to the seed crystal, thereby growing the silicon carbide single crystal on the surface of the seed crystal; a silicon carbide single crystal grown by repeatedly increasing and decreasing the resistivity with respect to a growth distance of the silicon carbide single crystal, thereby growing the silicon carbide single crystal.
7. 7. The method for producing a silicon carbide single crystal according to claim 6, wherein, in growing the silicon carbide single crystal, a flow rate of the dopant gas is periodically varied so that a gradual increase and a gradual decrease in resistivity with respect to a growth distance of the silicon carbide single crystal are repeated.
8. 7. The method for producing a silicon carbide single crystal according to claim 6, wherein, in growing the silicon carbide single crystal, a gradual increase and a gradual decrease in resistivity with respect to a growth distance of the silicon carbide single crystal are repeated by varying one or more of a flow rate or a partial pressure of the source gas, and a temperature of a growth surface of the silicon carbide single crystal.
Citation Information
Patent Citations
Manufacturing method of sic single crystal
JP6050053B2
PROCESS AND APPARATUS FOR PREPARING SiC SINGLE CRYSTAL
JP2004043211A