tire
The tire's inner liner, with a specific Ew/Es ratio, high crack growth index, and reduced thickness, enhances air retention by utilizing ionic bonds to prevent cracks and maintain air integrity.
Patent Information
- Application Number
- JP2023062962
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing pneumatic tires face challenges in maintaining air retention due to the difficulty of butyl-based rubber compositions in preventing air leakage, necessitating improvements in inner liners.
The tire incorporates an inner liner composed of a rubber composition with a specific ratio of complex modulus of elasticity when wet to dry (Ew/Es) of 0.95 or less, a crack growth index A of 190 or more, and a thickness of 2.0 mm or less, utilizing ionic bonds that can recombine to enhance air retention.
The configuration significantly improves air retention by suppressing crack formation and recombining ionic bonds, ensuring long-term air retention performance.
Smart Images

Figure 2024149220000003 
Figure 2024149220000004 
Figure 2024149220000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a tire. [Background technology]
[0002] A pneumatic tire is composed of various components such as an inner liner in addition to the tread that comes into contact with the road surface. The inner liner is a tire component that exhibits air retention by reducing the amount of air leaking from inside the tire to the outside (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-227494 A Summary of the Invention [Problem to be solved by the invention]
[0004] The inner liner is endowed with air-retaining properties by compounding butyl-based rubber such as butyl rubber, which is difficult for air to permeate, but further improvement is required.
[0005] An object of the present invention is to solve the above problems and to provide a tire with excellent air retention properties. [Means for solving the problem]
[0006] The present invention relates to a tire having an inner liner, The inner liner is made of a rubber composition having a ratio (Ew / Es) of a complex modulus of elasticity Ew (MPa) when wet to a complex modulus of elasticity Es (MPa) when dry of 0.95 or less, The rubber composition has a crack growth index A of 190 or more as measured by the following crack growth test, The tire relates to a tire in which the thickness G of the inner liner is 2.0 mm or less. <Crack growth test> (1) A rubber sheet formed from the rubber composition, measuring 100 mm in length, 50 mm in width, and 2.0 mm in thickness, is given an initial cut of 5.0 mm on both sides of the center in the longitudinal direction. (2) The sample with the initial scratch is bent at 40% strain using a De Mattia testing machine, and the number of times it is bent until it breaks is measured. (3) The number of flexions until fracture / 100 is the crack growth index A. Effect of the Invention
[0007] The present invention relates to a tire having an inner liner, the inner liner being composed of a rubber composition having a ratio (Ew / Es) of a complex modulus Ew (MPa) when wet to a complex modulus Es (MPa) when dry of 0.95 or less, the rubber composition having a crack growth index A measured in the crack growth test of 190 or more, and the inner liner having a thickness G of 2.0 mm or less, thereby improving air retention. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a schematic diagram showing a sample (rubber sheet) used in a crack growth test. [Diagram 2] 1 is a cross-sectional view showing a portion of a pneumatic tire. [Diagram 3] FIG. 3 is an enlarged cross-sectional view showing the vicinity of the tread of the tire of FIG. 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention relates to a tire having an inner liner, the inner liner is made of a rubber composition having a ratio (Ew / Es) of a complex modulus of elasticity Ew when wet to a complex modulus of elasticity Es when dry of 0.95 or less; The rubber composition has a crack growth index A of 190 or more as measured by the crack growth test, The inner liner has a thickness G of 2.0 mm or less.
[0010] The above-mentioned rubber composition provides the above-mentioned effects, and although the reason why such effects are obtained is not entirely clear, it is presumed to be as follows. Since the ratio (Ew / Es) of the complex modulus of elasticity Ew when wet with water to the complex modulus of elasticity Es when dry is 0.95 or less, it is believed that ionic bonds that are reversibly changed by water are generated in the rubber composition, and that these ionic bonds, unlike covalent bonds of sulfur and the like, are capable of recombining due to electric charge. In addition, since the crack growth index A is 190 or more, the occurrence of cracks in the rubber composition is suppressed, and it is believed that the rubber itself is also less likely to break. Moreover, by reducing the thickness G of the inner liner to 2.0 mm or less, it is possible to reduce the strain applied to the rubber surface, which is believed to further suppress the occurrence of cracks. From the above, it is believed that the inner liner is less likely to crack, and even if cracks do occur, they can rebond through ionic bonds, which means that cracks in the inner liner are suppressed for a long period of time and that the air retention performance after deterioration is improved. Therefore, it is presumed that the present invention can improve the air retention of a tire.
[0011] In this way, the problem (objective) of improving air retention is solved by adopting a configuration that satisfies the relationships of "Ew / Es is 0.95 or less," "crack growth index A is 190 or more," and "inner liner thickness G is 2.0 mm or less." In other words, the parameters "Ew / Es is 0.95 or less," "crack growth index A is 190 or more," and "inner liner thickness G is 2.0 mm or less" do not define the problem (objective); the problem of the present application is to improve air retention, and a configuration that satisfies these parameters is used as a means to achieve this.
[0012] In this specification, physical properties such as complex modulus (E*) and hardness (H) of a rubber composition refer to physical properties such as E* and H of the rubber composition after vulcanization.
[0013] In this specification, the complex modulus of elasticity Es in a dry state means the complex modulus of elasticity (E*) of a rubber composition (after vulcanization) in a dried state, and specifically means the complex modulus of elasticity (E*) of a rubber composition (after vulcanization) dried by the method described in the Examples. In this specification, the complex modulus of elasticity Ew when wetted with water means the complex modulus of elasticity (E*) of a rubber composition (after vulcanization) in a state wetted with water, and specifically means the complex modulus of elasticity (E*) of a rubber composition (after vulcanization) wetted with water by the method described in the Examples.
[0014] In this specification, the complex modulus (E*) of a rubber composition (after vulcanization) is the complex modulus measured under conditions of a temperature of 30° C., an initial strain of 10%, a dynamic strain of 2%, a frequency of 10 Hz, and an elongation mode.
[0015] In this specification, the dry hardness Hs means the hardness (H) of a rubber composition (after vulcanization) in a dried state, and specifically means the hardness (H) of a rubber composition (after vulcanization) dried by the method described in the Examples. In this specification, the water-wet hardness Hw means the hardness (H) of a rubber composition (after vulcanization) in a state wet with water, specifically, the hardness (H) of a rubber composition (after vulcanization) wetted with water by the method described in the Examples.
[0016] In this specification, the hardness (JIS-A hardness) of the rubber composition (after vulcanization) is measured at 25°C using a type A durometer in accordance with JIS K6253-3:2012 "Vulcanized rubber and thermoplastic rubber - Determination of hardness - Part 3: Durometer hardness".
[0017] In the above tire, the rubber composition (after vulcanization) constituting the inner liner has a ratio (Ew / Es) of the water-wet complex modulus Ew to the dry complex modulus Es of 0.95 or less, and from the viewpoint of obtaining a better effect, it is preferably 0.93 or less, more preferably 0.92 or less, and even more preferably 0.91 or less. The lower limit of Ew / Es is not particularly limited, but is preferably 0.50 or more, more preferably 0.70 or more, and even more preferably 0.75 or more.
[0018] The rubber composition (after vulcanization) has a complex elastic modulus Es (MPa) in a dry state of preferably 5.0 MPa or more, more preferably 8.0 MPa or more, and even more preferably 9.8 MPa or more. The upper limit is not particularly limited, but is preferably 15.0 MPa or less, more preferably 13.0 MPa or less, and even more preferably 11.7 MPa or less. When the hardness is within the above range, the effect can be suitably obtained.
[0019] From the viewpoint of obtaining the desired effect, it is preferable that the complex modulus (E*) of the rubber composition (after vulcanization) is reversibly changed by water.
[0020] In this specification, the complex modulus (E*) changes reversibly due to water means that the complex modulus (E*) of the rubber composition (after vulcanization) reversibly increases or decreases due to the presence of water. Note that, for example, when changing from dry to wet to dry, the complex modulus (E*) only needs to change reversibly, and the complex modulus (E*) does not need to be the same at the first drying time and the second drying time, and may be the same at the first drying time and the second drying time.
[0021] The relationship of "Ew / Es of 0.95 or less" of the rubber composition can be achieved by the rubber composition having a bond that can be reversibly cut and recombined by adding water and drying, such as a hydrogen bond or an ionic bond. To be more specific, for example, this can be achieved by using a rubber modified with an ionic functional group in combination with a compound having an opposite charge to the ionic functional group to form an ionic bond between them.
[0022] For example, when a rubber modified with an ionic functional group is used in combination with a compound having an opposite charge to the ionic functional group, the complex modulus (E*) when dry tends to increase if the ionic bond is strengthened by increasing the content of the ionic functional group, etc. Also, it can be adjusted by the type and amount of chemicals (especially rubber components, fillers, softeners such as oils) blended into the rubber composition; for example, reducing the amount of softener tends to increase E* when dry, and increasing the amount of filler tends to increase E* when dry.
[0023] The complex modulus (E*) when wetted with water can be lowered compared to when dry by, for example, forming a rubber composition crosslinked by ionic bonds in which some or all of the rubber molecules of the rubber component are crosslinked by ionic bonds, and E* when wetted with water can be adjusted. Specifically, by using a rubber modified with an ionic functional group in combination with a compound having an opposite charge to the ionic functional group, a rubber composition crosslinked by ionic bonds is formed, and E* when wetted with water can be lowered compared to when dry. In addition, it can be adjusted by the type and amount of chemicals (especially rubber components, fillers, softeners such as oils) blended into the rubber composition. For example, increasing the amount of fillers tends to increase E* when wetted with water, and decreasing the amount of softeners tends to increase E* when wetted with water.
[0024] Specifically, by adjusting the complex modulus (E*) of the dry state to within a desired range, and then using a rubber modified with an ionic functional group in combination with a compound having an opposite charge to the ionic functional group, the rubber composition can achieve a relationship of "Ew / Es of 0.95 or less" and a reversible change in E* caused by water. Also, the above-mentioned E* of the dry state can be achieved.
[0025] In the above tire, from the viewpoint of obtaining the desired effect, it is desirable that the rubber composition (after vulcanization) constituting the inner liner has a ratio (Hw / Hs) of the wet hardness Hw to the dry hardness Hs of less than 1.00. Hw / Hs is preferably 0.99 or less, more preferably 0.98 or less. The lower limit of Hw / Hs is not particularly limited, but is preferably 0.50 or more, more preferably 0.70 or more, and even more preferably 0.75 or more. When the hardness is within the above range, the effect can be preferably obtained.
[0026] Although the mechanism by which a greater effect is obtained when Hw / Hs is adjusted to less than 1.00 is unclear, it is believed that when Hw / Hs is less than 1.00, ionic bonds that are reversibly changed by water are generated in the rubber composition, and these ionic bonds can be recombined by electric charge. Therefore, it is presumed that the occurrence of cracks is suppressed for a long period of time, and the air retention performance after aging is improved.
[0027] The dry hardness Hs of the rubber composition (after vulcanization) is preferably 40 or more, more preferably 45 or more, and even more preferably 46 or more, and is preferably 50 or less, more preferably 49 or less, and even more preferably 48 or less. Within the above ranges, the effects tend to be favorably obtained.
[0028] The relationship of "Hw / Hs less than 1.00" of the rubber composition can be achieved by the rubber composition having a bond that can be reversibly cut and recombined by adding water and drying, such as a hydrogen bond or an ionic bond. To be more specific, for example, this can be achieved by using a rubber modified with an ionic functional group in combination with a compound having an opposite charge to the ionic functional group to form an ionic bond between them.
[0029] For example, when rubber modified with an ionic functional group is used in combination with a compound having an opposite charge to the ionic functional group, the dry hardness (H) tends to increase if the ionic bond is strengthened by increasing the content of the ionic functional group, etc. Also, it can be adjusted by the type and amount of chemicals (especially rubber components, fillers, softeners such as oils) blended into the rubber composition, and for example, it tends to increase when the amount of softener is reduced, the amount of filler is increased, and tends to decrease when the amount of softener is increased, the amount of filler is reduced, and the amount of sulfur is reduced.
[0030] The hardness (H) when wetted with water can be reduced compared to when dry by, for example, forming a rubber composition crosslinked by ionic bonds in which some or all of the rubber molecules of the rubber component are crosslinked by ionic bonds, and the hardness when wetted with water can be adjusted. Specifically, by using a rubber modified with an ionic functional group in combination with a compound having an opposite charge to the ionic functional group, a rubber composition crosslinked by ionic bonds is formed, and the hardness when wetted with water can be reduced compared to when dry. In addition, the hardness can be adjusted by the type and amount of chemicals (particularly rubber component, filler, softener, and sulfur) blended into the rubber composition. For example, the hardness tends to increase when the amount of softener is reduced, the amount of filler is increased, and the hardness tends to decrease when the amount of softener is increased, the amount of filler is reduced, and the hardness tends to decrease when the amount of softener is increased, the amount of filler is reduced, and the amount of sulfur is reduced.
[0031] Specifically, by adjusting the dry hardness (H) to within a desired range and using a rubber modified with an ionic functional group in combination with a compound having an opposite charge to the ionic functional group, the rubber composition can achieve a relationship of "Hw / Hs less than 1.00" and reversible hardness change due to water. Also, the above-mentioned dry hardness can be achieved.
[0032] In the above tire, the rubber composition (after vulcanization) constituting the inner liner has a crack growth index A measured by the following crack growth test of 190 or more. Note that the crack growth test is conducted in accordance with JIS K6260:2017 except for the following conditions. <Crack growth test> (1) A rubber sheet formed from the rubber composition, measuring 100 mm in length, 50 mm in width, and 2.0 mm in thickness, is given an initial cut of 5.0 mm on both sides of the center in the longitudinal direction. (2) The sample with the initial scratch is bent at 40% strain using a De Mattia testing machine, and the number of times it is bent until it breaks is measured. (3) The number of flexions until fracture / 100 is the crack growth index A.
[0033] FIG. 1 is a schematic diagram showing a sample (rubber sheet) used in a crack growth test. Specifically, as shown in FIG. 1, a rubber sheet (rubber composition (after vulcanization)) measuring 100 mm long x 50 mm wide x 2.0 mm thick (thickness not shown) is used, with a cut (initial flaw) of 5.0 mm made horizontally on each end of the lengthwise direction from the center (center, 50 mm position of 100 mm long), and the above crack growth test is performed with the sample gripped at 15 mm above the top end and 15 mm below the bottom end in the lengthwise direction.
[0034] From the viewpoint of obtaining a greater effect, the crack growth index A is preferably 260 or more, more preferably 322 or more, even more preferably 340 or more, particularly preferably 360 or more, and most preferably 370 or more. There is no particular upper limit, and a larger index is more desirable, but the crack growth index A may be 1000 or less, 800 or less, or 600 or less.
[0035] The "crack growth index A of 190 or more" of the rubber composition can be achieved by the rubber composition having a bond that can be reversibly cut and recombined by adding water and drying, such as a hydrogen bond or an ionic bond. To be more specific, for example, it can be realized by using a rubber modified with an ionic functional group in combination with a compound having an opposite charge to the ionic functional group to form an ionic bond between them. In addition, it can be adjusted by the type and amount of chemicals (especially rubber components, fillers, softeners such as oils) blended into the rubber composition. For example, the crack growth index tends to increase when the amount of the softener is increased, and the crack growth index tends to increase when the amount of the filler is decreased.
[0036] Hereinafter, chemicals that can be used for the rubber composition constituting the inner liner (rubber composition for inner liner) will be described.
[0037] The rubber composition for an inner liner contains a rubber component. Here, the rubber component is a component that contributes to crosslinking, and is generally a polymer with a weight average molecular weight (Mw) of 10,000 or more, and is a polymer component that is not extracted with acetone. The elastomer component is in a solid state at room temperature (25°C).
[0038] The weight average molecular weight of the rubber component is preferably 50,000 or more, more preferably 150,000 or more, even more preferably 200,000 or more, and particularly preferably 270,000 or more, and is preferably 2,000,000 or less, more preferably 1,500,000 or less, and even more preferably 1,000,000 or less. Within the above ranges, the effect tends to be better obtained.
[0039] In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) can be determined by standard polystyrene conversion based on the measured value obtained by gel permeation chromatography (GPC) (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMULTIPORE HZ-M manufactured by Tosoh Corporation).
[0040] Examples of the rubber component that can be used in the rubber composition include rubber that is crosslinked mainly with sulfur (sulfur crosslinkable rubber). Examples of the sulfur crosslinkable rubber include diene rubber. Examples of the diene rubber include isoprene rubber, butadiene rubber (BR), styrene butadiene rubber (SBR), styrene isoprene butadiene rubber (SIBR), ethylene propylene diene rubber (EPDM), chloroprene rubber (CR), and acrylonitrile butadiene rubber (NBR). Examples of the rubber component include butyl rubber and fluororubber. These may be used alone or in combination of two or more. These rubber components may be modified or hydrogenated as described below, and extended rubber extended with oil, resin, liquid rubber component, or the like may be used. Among these, butyl rubber and isoprene rubber are preferred, and butyl rubber is more preferred.
[0041] The rubber component may be a non-modified rubber or a modified rubber. The modified rubber may be a rubber having a functional group that interacts with a filler such as silica. For example, the modified rubber may be a terminal modified rubber (terminal modified rubber having the functional group at the terminal) in which at least one terminal of the rubber is modified with a compound (modifier) having the functional group, a main chain modified rubber having the functional group at the main chain, a main chain terminal modified rubber having the functional group at the main chain and terminal (for example, a main chain terminal modified rubber having the functional group at the main chain and at least one terminal modified with the modifier), or a terminal modified rubber modified (coupled) with a polyfunctional compound having two or more epoxy groups in the molecule and having a hydroxyl group or an epoxy group introduced therein.
[0042] Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), and an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms) are preferred.
[0043] As the butyl rubber, either a non-modified butyl rubber or a modified butyl rubber can be used. The modified butyl rubber may be a modified butyl rubber having the same functional group as the modified rubber introduced therein.
[0044] Specific examples of butyl-based rubbers include butyl rubber and halogenated butyl rubbers such as chlorinated butyl rubber (Cl-IIR), brominated butyl rubber (Br-IIR), and fluorinated butyl rubber (F-IIR). Commercially available butyl-based rubbers include ExxonMobil's Exprobutyl and Chlorobutyl HT1068. These may be used alone or in combination of two or more. Among these, brominated butyl rubber is preferred from the viewpoint of obtaining a greater effect.
[0045] Examples of isoprene-based rubber include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, and modified IR. Examples of NR include SIR20, RSS♯3, TSR20, and other rubber industry-standard rubbers. Examples of IR include IR2200 and other rubber industry-standard rubbers. Examples of modified NR include deproteinized natural rubber (DPNR), high-purity natural rubber (UPNR), and other rubbers. Examples of modified NR include epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), and grafted natural rubber. Examples of modified IR include epoxidized isoprene rubber, hydrogenated isoprene rubber, and grafted isoprene rubber. These may be used alone or in combination of two or more.
[0046] The BR is not particularly limited, and for example, high cis BR with a high cis content, BR containing syndiotactic polybutadiene crystals, BR synthesized using a rare earth catalyst (rare earth BR), etc. can be used. These may be used alone or in combination of two or more. In particular, the BR preferably contains high cis BR with a cis content of 90% by mass or more. The cis content is more preferably 95% by mass or more. The cis content can be measured by infrared absorption spectroscopy.
[0047] The cis amount of BR means the cis amount of the BR when there is one type of BR, and means the average cis amount when there are multiple types of BR. The average cis content of BR can be calculated by {Σ(content of each BR × cis content of each BR)} / total content of all BRs. For example, when 100% by mass of the rubber component contains 20% by mass of BR with a cis content of 90% by mass and 10% by mass of BR with a cis content of 40% by mass, the average cis content of BR is 73.3% by mass (=(20×90+10×40) / (20+10)).
[0048] In addition, either unmodified or modified BR can be used as the BR. Modified BR includes modified BR in which functional groups similar to those of modified rubber have been introduced. In addition, hydrogenated butadiene polymer (hydrogenated BR) can also be used as the BR.
[0049] The SBR is not particularly limited, and for example, emulsion polymerized styrene butadiene rubber (E-SBR), solution polymerized styrene butadiene rubber (S-SBR), etc. can be used. These may be used alone or in combination of two or more kinds.
[0050] The styrene content of SBR is preferably 5% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more. The styrene content is preferably 60% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less. When it is within the above range, the effect tends to be better obtained. In this specification, the styrene content is 1 It can be measured by H-NMR measurement.
[0051] The styrene amount of SBR means the styrene amount of the SBR when there is one type of SBR, and means the average styrene amount when there are multiple types of SBR. The average styrene amount of SBR can be calculated by {Σ(content of each SBR × styrene amount of each SBR)} / total content of all SBRs. For example, when 100% by mass of the rubber component contains 85% by mass of SBR with a styrene amount of 40% by mass and 5% by mass of SBR with a styrene amount of 25% by mass, the average styrene amount of the SBR is 39.2% by mass (=(85×40+5×25) / (85+5)).
[0052] The vinyl bond content of SBR is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 7% by mass or more. When the vinyl bond content is within the above range, preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, the effect tends to be better. In this specification, the vinyl bond amount (1,2-bonded butadiene unit amount) can be measured by infrared absorption spectroscopy.
[0053] The vinyl content of SBR (amount of 1,2-bonded butadiene units) is the proportion of vinyl bonds when the total mass of the butadiene parts in SBR is taken as 100 (unit: mass%), and is calculated as vinyl content [mass%] + cis content [mass%] + trans content [mass%] = 100 [mass%]. When there is one type of SBR, it means the vinyl content of that SBR, and when there are multiple types, it means the average vinyl content. The average vinyl content of SBR can be calculated by Σ{content of each SBR × (100 [mass%] - styrene content of each SBR [mass%]) × vinyl content of each SBR [mass%]} / Σ{content of each SBR × (100 [mass%] - styrene content of each SBR [mass%])}. For example, in 100 parts by mass of the rubber component, there are 75 parts by mass of SBR with a styrene content of 40 mass% and a vinyl content of 30 mass%, 25 parts by mass of styrene, and 10 parts by mass of vinyl. In the case where SBR with a vinyl content of 20 mass% is 15 parts by mass and the remaining 10 parts by mass is a component other than SBR, the average vinyl content of the SBR is 28 mass% (={75 × (100 [mass%] - 40 [mass%]) × 30 [mass%] + 15 × (100 [mass%] - 25 [mass%]) × 20 [mass%])} / {75 × (100 [mass%] - 40 [mass%]) + 15 × (100 [mass%] - 25 [mass%])}.
[0054] Both unmodified and modified SBR can be used. Modified SBR includes modified SBR with the same functional groups as modified rubber. Hydrogenated styrene-butadiene copolymer (hydrogenated SBR) can also be used as SBR.
[0055] Among the above rubber components, a rubber crosslinked by ionic bonds (ionic bond rubber) can be preferably used. The ionic bond rubber is a rubber having an ionic functional group, and the ionic functional group can be an anionic functional group or a cationic functional group. The ionic bond rubber may have one ionic functional group or two or more ionic functional groups.
[0056] Examples of the anionic functional group include a halogen group and an acidic functional group. Examples of the halogen group include a fluoro group, a chloro group, a bromo group, and an iodo group. Examples of the acidic functional group include a carboxylic acid group, a sulfonic acid group, a sulfate group, a phosphonic acid group, a phosphoric acid group, a phosphinic acid group, a maleic acid group, an acid anhydride group (such as a maleic anhydride group), a fumaric acid group, an itaconic acid group, an acrylic acid group, a methacrylic acid group, and a mercapto group. Of these, a halogen group and a carboxylic acid group are preferred, and a halogen group is more preferred.
[0057] The cationic functional group may be a basic functional group. Examples of basic functional groups include amino groups, imino groups (=NH), ammonium bases, and heterocyclic groups having a basic nitrogen atom. The amino group may be any of primary amino groups (-NH2), secondary amino groups (-NHR), and tertiary amino groups (-NRR'). The R and R' are alkyl groups, phenyl groups, aralkyl groups, and the like, and preferably have 1 to 8 carbon atoms. Examples of ammonium bases include tertiary ammonium bases and quaternary ammonium bases. Examples of heterocyclic groups having a basic nitrogen atom include nitrogen-containing heterocyclic groups such as pyridine groups, pyrimidine groups, pyrazine groups, imidazole groups, imidazole groups containing thiols, triazole groups, and thiazole groups. In the case of heterocyclic groups, the presence of a double bond makes them easily dispersible in rubber. Among these, pyridine groups, imidazole groups, thiazole groups, and amino groups (amine groups) are preferred, and imidazole groups are more preferred.
[0058] Examples of the rubber into which the ionic functional group is introduced include the diene rubber described above in the sulfur crosslinkable rubber, as well as non-diene rubbers that do not contain diene compounds or that contain very little diene compounds, such as butyl rubber, urethane rubber, and silicone rubber. These may be used alone or in combination of two or more. Among these, non-diene rubbers are preferred, and butyl rubber is more preferred.
[0059] The ionic-bonding rubber is modified with an ionic functional group, and the content of the ionic functional group in 100% by mass of the ionic-bonding rubber is preferably 0.5% by mass or more, more preferably 0.8% by mass or more, and even more preferably 1.0% by mass or more, and is preferably 40% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less. Within the above ranges, the effect tends to be preferably obtained. The content of the ionic functional group can be measured by performing NMR measurement and calculating the content (mass %) based on the peak corresponding to the ionic functional group.
[0060] From the viewpoint of obtaining the desired effect, the rubber composition for the inner liner preferably contains the ionic-bonding rubber as a rubber component, and more preferably contains the ionic-bonding rubber and the sulfur-crosslinkable rubber, wherein the ionic-bonding rubber is preferably a halogenated butyl rubber, and the sulfur-crosslinkable rubber is preferably an isoprene-based rubber.
[0061] In the rubber composition for an inner liner, the content of the ionic bond rubber in 100% by mass of the rubber component is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 86% by mass or less. Within the above ranges, the effects tend to be favorably obtained.
[0062] In the rubber composition for the inner liner, the content (Bc) of the butyl rubber in 100% by mass of the rubber component is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 86% by mass or less. Within the above range, the effect tends to be preferably obtained. The content of the halogenated butyl rubber (BHc) in 100% by mass of the rubber component is also desirably in the same range.
[0063] In the rubber composition for the inner liner, the content of the isoprene-based rubber in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 14% by mass or more, and is preferably 50% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less. Within the above ranges, the effects tend to be favorably obtained.
[0064] When the rubber composition for an inner liner contains BR, the content of BR in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 8% by mass or more, even more preferably 10% by mass or more, and is preferably 30% by mass or less, more preferably 25% by mass or less, even more preferably 20% by mass or less. Within the above ranges, the effects tend to be favorably obtained.
[0065] When the rubber composition for the inner liner contains SBR, the content of SBR in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 8% by mass or more, even more preferably 10% by mass or more, and is preferably 30% by mass or less, more preferably 25% by mass or less, even more preferably 20% by mass or less. Within the above ranges, the effect tends to be preferably obtained.
[0066] From the viewpoint of obtaining a better effect, the rubber composition for the inner liner desirably contains an ionic compound having an ionic functional group 2 having an opposite charge to the ionic functional group (ionic functional group 1) of the ionic-bonding rubber. By using the ionic-bonding rubber and the ionic compound in combination, it becomes possible to form an ionic bond between the ionic-bonding rubber and the ionic compound. As a result, it becomes possible to realize "Ew / Es of 0.95 or less" and "crack growth index A of 190 or more", thereby improving air retention. In this specification, the ionic compounds are not considered to be fillers.
[0067] The ionic functional group 2 may be the same as the ionic functional group 1 described above. When the ionic functional group 2 is an anionic functional group, a halogen group or a carboxylic acid group is preferable, and a halogen group is more preferable. When the ionic functional group 2 is a cationic functional group, a pyridine group, an imidazole group, a thiazole group, or an amino group (amine group) is preferable, and an imidazole group is more preferable.
[0068] Examples of the ionic compound having an anionic functional group include dicarboxylic acids, specifically, aliphatic dicarboxylic acids (adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, etc.); aromatic dicarboxylic acids (terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodium sulfoisophthalic acid, hexahydroterephthalic acid, hexahydroisophthalic acid, etc.); alicyclic dicarboxylic acids (1,4-cyclohexanedicarboxylic acid, etc.); etc. Among them, from the viewpoint of crack growth resistance (self-repairing property), etc., aliphatic dicarboxylic acids are preferred, and suberic acid, adipic acid, sebacic acid, and dodecanedioic acid are more preferred.
[0069] Specific examples of ionic compounds having a cationic functional group include imidazoles (imidazole, N-isobutylimidazole, 1-methylimidazole, 2-methylimidazole, 2-ethylimidazole, 2-n-propylimidazole, 2-isopropylimidazole, 1-butylimidazole, 2-butylimidazole, 2-phenylimidazole, 4-methylimidazole, 4-ethylimidazole, 4-nitroimidazole, 4-phenylimidazole, 2-methyl-4-phenylimidazole, 4,5-dimethylimidazole, 1- isobutyl-2-methylimidazole, 2,4,5-trimethylimidazole, 2,4,5-triphenylimidazole, benzimidazole, 2-methylbenzimidazole, 2-phenylbenzimidazole, etc.; pyridines (pyridine, 2-isobutylpyridine, 3-isobutylpyridine, 3-methylpyridine, 4-methylpyridine, 2-ethylpyridine, 3-ethylpyridine, 4-ethylpyridine, 4-propylpyridine, 2-n-hexylpyridine, 3-n-hexylpyridine, 3,5-dimethylpyridine, 3,5-diethylpyridine, 2,6-di-tert-butylpyridine, 2-benzylpyridine, 4-benzylpyridine, 2-phenylpyridine, 3-phenylpyridine, 4-phenylpyridine, 2,6-diphenylpyridine, 2-(3-phenylpropyl)pyridine, 4-(3-phenylpropyl)pyridine, etc.; thiazoles (thiazole, 2-aminothiazole, 2-methylthiazole, 2-methoxythiazole, 2-ethoxythiazole, 2-isobutylthiazole, 2-trimethylsilylthiazole, 5-trimethylsilylthiazole, 4-methylthiazole, 4, 5-dimethylthiazole, 2-ethylthiazole, 2,4-dimethylthiazole, 2-amino-5-methylthiazole, 2-amino-4-methylthiazole, 2,4,5-trimethylthiazole, benzothiazole, 2-methylbenzothiazole, 2,5-dimethylbenzothiazole, etc.); alkylenediamines (methylenediamine, ethylenediamine, propylenediamine, butylenediamine, etc.); polyamines (diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, etc.); and the like.Among these, from the viewpoint of crack growth resistance (self-repairing property) and the like, imidazoles, pyridine, and ethylenediamine are preferred, imidazoles are more preferred, and methylimidazole and butylimidazole are even more preferred.
[0070] As the ionic compound, in addition to the above-mentioned compounds, metal salts can also be used. Examples of the metal salts include sodium acetate, sodium carbonate, potassium acetate, etc. Among them, sodium acetate is preferable.
[0071] Since the effect tends to be more favorably obtained, the ionic functional group 1 of the ionic bonding rubber is preferably an anionic functional group, and the ionic functional group 2 of the ionic compound is preferably a cationic functional group.
[0072] In the rubber composition for an inner liner, the content (Ic) of the above ionic compound is, from the viewpoint of self-repairing property, preferably 0.6 parts by mass or more, more preferably 0.9 parts by mass or more, even more preferably 1.2 parts by mass or more, and particularly preferably 1.8 parts by mass or more, per 100 parts by mass of the rubber component, and is preferably 6.5 parts by mass or less, more preferably 4.5 parts by mass or less, and even more preferably 2.4 parts by mass or less. The content (IIc) of imidazoles per 100 parts by mass of the rubber component is also desirably in the same range.
[0073] The rubber composition for the inner liner desirably contains a filler. The filler is not particularly limited, and materials known in the rubber field can be used, for example, inorganic fillers such as carbon black, silica, calcium carbonate, talc, alumina, clay, aluminum hydroxide, aluminum oxide, mica, biochar, poorly dispersible fillers, etc. Among them, carbon-derived fillers (carbon-containing fillers) such as carbon black, and silica are preferred from the viewpoint of obtaining a greater effect.
[0074] In the rubber composition for innerliner, the content of the filler (total amount of fillers such as silica, carbon black, etc.) is preferably 30 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 60 parts by mass or more, per 100 parts by mass of the rubber component, and is preferably 150 parts by mass or less, more preferably 120 parts by mass or less, and even more preferably 100 parts by mass or less. Within the above range, the effect tends to be better obtained.
[0075] In the rubber composition for the inner liner, usable carbon black is not particularly limited, but examples thereof include N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, and N762. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Co., Ltd., Lion Co., Ltd., Shin-Nichika Carbon Co., Ltd., Columbia Carbon Co., Ltd., and the like. These may be used alone or in combination of two or more. In addition to conventional carbon black made from mineral oils, carbon black made from biomass materials such as lignin may be used. Recycled carbon black obtained by decomposing rubber products and plastic products containing carbon black, such as tires, may be appropriately used by replacing the above carbon black in an equal amount.
[0076] The nitrogen adsorption specific surface area (N2SA) of carbon black is 5m 2 / g or more is preferable, and 10m 2 / g or more is more preferable, and 15m 2 / g or more is more preferable. 2 / g or less is preferable, and 50m 2 / g or less is more preferable, and 40m 2 Within the above range, there is a tendency that the effect is better obtained. The nitrogen adsorption specific surface area of carbon black can be determined in accordance with JIS K6217-2:2001.
[0077] The dibutyl phthalate oil absorption (DBP) of the carbon black is preferably 40 ml / 100 g or more, more preferably 60 ml / 100 g or more, and even more preferably 70 ml / 100 g or more. In addition, when the DBP is within the above range of preferably 200 ml / 100 g or less, more preferably 150 ml / 100 g or less, and even more preferably 100 ml / 100 g or less, the effect tends to be better. The DBP of carbon black is determined by the measurement method of JIS K6217-4:2001.
[0078] In the rubber composition for an inner liner, the content of carbon black is preferably 30 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 60 parts by mass or more, and is preferably 150 parts by mass or less, more preferably 120 parts by mass or less, and even more preferably 100 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0079] In the rubber composition for the inner liner, examples of silica that can be used include dry process silica (anhydrous silica) and wet process silica (hydrated silica). Among them, wet process silica is preferred because it has a large number of silanol groups. Commercially available products include those from Degussa, Rhodia, Tosoh Silica, Solvay Japan, and Tokuyama. These may be used alone or in combination of two or more.
[0080] As the silica, plant-derived silica can also be suitably used. Examples of plant-derived silica include silica derived from plants containing silica. Examples of plants containing silica include rice, corn, sugarcane, horsetail, wheat, barley, rye, pearl barley, millet, foxtail millet, Japanese barnyard millet, and Erianthus. In addition, the saccharification residue of the above-mentioned plants containing silica can also be used. Among them, rice husks and straws with high silica content are preferred, and rice husks are more preferred. In addition, the plant containing silica may be one that has been burned to ash or one that has been carbonized.
[0081] The nitrogen adsorption specific surface area (N2SA) of the silica is preferably 50 m 2 / g or more, more preferably 100m 2 / g or more, more preferably 150m 2 The upper limit of the N2SA of silica is not particularly limited, but is preferably 350 m 2 / g or less, more preferably 300m 2 / g or less, more preferably 250m 2 Within the above range, there is a tendency for the effect to be better obtained. The N2SA of silica is a value measured by the BET method in accordance with ASTM D3037-93.
[0082] When the rubber composition for an inner liner contains silica, the content of silica relative to 100 parts by mass of the rubber component is preferably 20 parts by mass or more, more preferably 50 parts by mass or more, even more preferably 70 parts by mass or more, and is preferably 150 parts by mass or less, more preferably 120 parts by mass or less, even more preferably 100 parts by mass or less. When it is within the above range, the effect tends to be better obtained.
[0083] Examples of the poorly dispersible filler include microfibrillated vegetable fibers, short fiber cellulose, gel compounds, etc. Among these, microfibrillated vegetable fibers are preferred.
[0084] The microfibrillated plant fiber is preferably cellulose microfibril, since it has good reinforcing properties. The cellulose microfibril is not particularly limited as long as it is derived from a natural product, and examples thereof include those derived from resource biomass such as fruits, grains, and root vegetables, wood, bamboo, hemp, jute, and kenaf, and pulp, paper, cloth, agricultural waste, waste biomass such as food waste and sewage sludge obtained from these as raw materials, unused biomass such as rice straw, wheat straw, and thinned wood, as well as cellulose produced by sea squirts, acetic acid bacteria, etc. These microfibrillated plant fibers may be used alone or in combination of two or more.
[0085] In this specification, cellulose microfibrils typically refer to cellulose fibers having an average fiber diameter of 10 μm or less, more typically cellulose fibers having a microstructure formed by the aggregation of cellulose molecules and an average fiber diameter of 500 nm or less. Typical cellulose microfibrils are formed, for example, as an aggregate of cellulose fibers having the above-mentioned average fiber diameter.
[0086] When the rubber composition for the inner liner contains a poorly dispersible filler, the content of the poorly dispersible filler is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less. Within the above range, the effect tends to be better obtained.
[0087] When the rubber composition for an inner liner contains silica, it is preferable that it further contains a silane coupling agent. The silane coupling agent is not particularly limited, and those known in the rubber field can be used. For example, bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl-N, Examples of such silylsilanes include sulfide-based silylsilanes such as N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, and 3-triethoxysilylpropyl methacrylate monosulfide; mercapto-based silylsilanes such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and Momentive's NXT and NXT-Z; vinyl-based silylsilanes such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based silylsilanes such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based silylsilanes such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based silylsilanes such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based silylsilanes such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. Commercially available products include those manufactured by Degussa, Momentive, Shin-Etsu Silicones, Tokyo Chemical Industry, Azumax, and Dow Corning Toray Co., Ltd. These may be used alone or in combination of two or more.
[0088] In the rubber composition for innerliner, the content of the silane coupling agent is preferably 0.1 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, and particularly preferably 7 parts by mass or more, based on 100 parts by mass of silica. The upper limit of the content is preferably 50 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and particularly preferably 10 parts by mass or less. Within the above range, the effect tends to be better obtained.
[0089] The rubber composition for the inner liner desirably contains a plasticizer. In this specification, the plasticizer is a material that imparts plasticity to the rubber component, and may be liquid or solid at room temperature (25° C.) These may be used alone or in combination of two or more kinds.
[0090] In the rubber composition for the inner liner, the content of the plasticizer (total amount of the plasticizer) is preferably 50 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the rubber component. The lower limit is not particularly limited, but is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more. Within the above range, the effect tends to be better obtained. The plasticizer content includes the amount of oil and resin contained in the oil-extended rubber and resin-extended rubber.
[0091] In the rubber composition for an inner liner, the content of the solid plasticizer in a solid state at room temperature (25° C.) is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and further preferably 3 parts by mass or less, per 100 parts by mass of the rubber component, and may be 0 parts by mass. When it is within the above range, the effect tends to be better.
[0092] In the rubber composition for the inner liner, the content of the liquid plasticizer in a liquid state at room temperature (25°C) is preferably 50 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the rubber component. The lower limit is not particularly limited, but is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more. Within the above range, the effect tends to be better obtained. The liquid plasticizer content includes the amount of oil contained in the oil-extended rubber and the amount of liquid resin in the resin-extended rubber that has been extended with the liquid resin.
[0093] Examples of the plasticizer include oils, liquid polymers, resins, etc. These may be used alone or in combination of two or more kinds.
[0094] The oil is not particularly limited, and may be any conventionally known oil, such as paraffinic process oil, aromatic process oil, naphthenic process oil, low PCA (polycyclic aromatic) process oil such as TDAE and MES, vegetable-derived oil, and mixtures thereof. These may be used alone or in combination of two or more. From the viewpoint of life cycle analysis, lubricating oil or waste edible oil after use in a rubber mixing mixer or automobile engine may be used as appropriate.
[0095] Examples of the plant-derived oils (also called vegetable oils) include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil.
[0096] As the above oil, for example, products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., Japan Energy Co., Ltd., Orisoi Co., Ltd., H&R Co., Ltd., Toyokuni Oil Mills Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., Nisshin Oillio Group Co., Ltd., etc. can be used.
[0097] In the rubber composition for innerliner, the content of oil (total amount of oil) is preferably 50 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, per 100 parts by mass of the rubber component. The lower limit is not particularly limited, but is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more. Within the above range, the effect tends to be better obtained. The oil content includes the amount of oil contained in the oil-extended rubber.
[0098] Examples of the liquid polymer include liquid diene polymers (liquid rubber) and liquid farnesene polymers at 25°C. Examples of liquid rubber include liquid styrene butadiene copolymers (liquid SBR), liquid butadiene polymers (liquid BR), liquid isoprene polymers (liquid IR), liquid styrene isoprene copolymers (liquid SIR), liquid styrene butadiene styrene block copolymers (liquid SBS block polymers), and liquid styrene isoprene styrene block copolymers (liquid SIS block polymers). The ends or main chains of these may be modified with polar groups. Hydrogenated products of these may also be used.
[0099] The liquid diene polymer has a weight average molecular weight (Mw) of 1.0×10 in terms of polystyrene measured by gel permeation chromatography (GPC). 3 ~5.0×10 4 Preferably, it is 3.0×10 3 ~1.5×10 4 The lower or upper limit of Mw of the liquid diene polymer may be 4,500 or 8,500. In this specification, the Mw of the liquid diene-based polymer is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).
[0100] As the liquid diene polymer, for example, products available from Sartomer Co., Ltd., Kuraray Co., Ltd., etc. can be used.
[0101] The resin may be a resin that is commonly used as a tire compound, and may be liquid or solid at room temperature (25°C). Examples of the resin include aromatic vinyl polymers, coumarone-indene resins, coumarone resins, indene resins, phenolic resins, rosin resins, petroleum resins, terpene resins, and acrylic resins. The resin may also be a hydrogenated resin. These may be used alone or in combination of two or more. The resin itself may also be a copolymer of monomer components of multiple origins. Among these, aromatic vinyl polymers, petroleum resins, terpene resins, and hydrogenated resins thereof are preferred from the viewpoint of obtaining better effects.
[0102] When a resin that is solid at room temperature is used, the softening point of the resin is preferably 50°C or higher, more preferably 55°C or higher, even more preferably 60°C or higher, and particularly preferably 85°C or higher. Also, it is preferably 160°C or lower, more preferably 150°C or lower, even more preferably 140°C or lower, and particularly preferably 100°C or lower. Within the above range, the effect tends to be better. When the resin is liquid at room temperature, the softening point is preferably 20°C or lower, preferably 10°C or lower, and preferably 0°C or lower. The softening point of the resin is the temperature at which the ball drops when the softening point specified in JIS K6220-1:2001 is measured using a ring and ball softening point tester.
[0103] The aromatic vinyl polymer is a polymer containing an aromatic vinyl monomer as a structural unit. For example, it can be a resin obtained by polymerizing α-methylstyrene and / or styrene, and specifically, it can be a homopolymer of styrene (styrene resin), a homopolymer of α-methylstyrene (α-methylstyrene resin), a copolymer of α-methylstyrene and styrene, a copolymer of styrene and another monomer, etc.
[0104] The coumarone-indene resin is a resin containing coumarone and indene as main monomer components constituting the resin skeleton (main chain). Other monomer components contained in the skeleton besides coumarone and indene include styrene, α-methylstyrene, methylindene, vinyltoluene, etc.
[0105] The coumarone resin is a resin containing coumarone as a main monomer component constituting the skeleton (main chain) of the resin.
[0106] The indene resin is a resin containing indene as a main monomer component constituting the skeleton (main chain) of the resin.
[0107] The phenolic resin may be a known polymer obtained by reacting phenol with an aldehyde such as formaldehyde, acetaldehyde, or furfural in the presence of an acid or alkali catalyst. Among these, those obtained by reacting with an acid catalyst (such as novolac-type phenolic resin) are preferred.
[0108] Examples of the rosin resin include rosin-based resins such as natural rosin, polymerized rosin, modified rosin, ester compounds thereof, and hydrogenated products thereof.
[0109] Examples of the petroleum resin include C5 resin, C9 resin, C5 / C9 resin, dicyclopentadiene (DCPD) resin, C9 / DCPD resin, and hydrogenated versions of these resins. Among these, DCPD resin, hydrogenated DCPD resin, C9 / DCPD resin, and C9 / hydrogenated DCPD resin are preferred.
[0110] The terpene resin is a polymer containing terpene as a constituent unit. For example, polyterpene resin obtained by polymerizing a terpene compound, aromatic modified terpene resin obtained by polymerizing a terpene compound and an aromatic compound, etc. can be mentioned. As the aromatic modified terpene resin, terpene phenol resin made from terpene compounds and phenolic compounds, terpene styrene resin made from terpene compounds and styrene compounds, and terpene phenol styrene resin made from terpene compounds, phenolic compounds, and styrene compounds can also be used. In addition, examples of the terpene compound include α-pinene, β-pinene, etc., examples of the phenolic compound include phenol, bisphenol A, etc., and examples of the aromatic compound include styrene compounds (styrene, α-methylstyrene, etc.). Among them, aromatic modified terpene resin is preferable.
[0111] The acrylic resin is a polymer containing an acrylic monomer as a constituent unit. For example, a styrene-acrylic resin having a carboxyl group and obtained by copolymerizing an aromatic vinyl monomer component and an acrylic monomer component, such as a styrene-acrylic resin, can be used. Among them, a solventless carboxyl group-containing styrene-acrylic resin can be preferably used.
[0112] Examples of the resins that can be used include products from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Company, Exxon Mobil Corporation, KRATON, Nippon Paint Chemical Co., Ltd., Nippon Shokubai Co., Ltd., ENEOS Corporation, Arakawa Chemical Industries, Ltd., and Taoka Chemical Co., Ltd.
[0113] From the viewpoint of sustainability, it is desirable to use, as the plasticizer, a plant-derived plasticizer such as the plant-derived oil or farnesene-based polymer.
[0114] When the rubber composition for the inner liner contains a plant-derived plasticizer, the content of the plant-derived plasticizer in 100% by mass of the plasticizer is preferably 5% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more. The upper limit is not particularly limited and may be 100% by mass, but is preferably 80% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less. Within the above range, the effect tends to be better obtained, and it is also desirable from the viewpoint of sustainability.
[0115] Farnesene polymers are polymers obtained by polymerizing farnesene and have structural units based on farnesene. Farnesene has isomers such as α-farnesene ((3E,7E)-3,7,11-trimethyl-1,3,6,10-dodecatetraene) and β-farnesene (7,11-dimethyl-3-methylene-1,6,10-dodecatriene), but (E)-β-farnesene, which has the following structure, is preferred. [ka]
[0116] The farnesene-based polymer may be a homopolymer of farnesene (farnesene homopolymer) or a copolymer of farnesene and a vinyl monomer (farnesene-vinyl monomer copolymer). These may be used alone or in combination of two or more. Among them, a copolymer of farnesene and a vinyl monomer is preferred.
[0117] Examples of vinyl monomers include aromatic vinyl compounds such as styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-tert-butylstyrene, 5-t-butyl-2-methylstyrene, vinylethylbenzene, divinylbenzene, trivinylbenzene, divinylnaphthalene, tert-butoxystyrene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethylether, N,N-dimethylaminoethylstyrene, N,N-dimethylaminomethylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2-t-butylstyrene, 3-t-butylstyrene, 4-t-butylstyrene, vinylxylene, vinylnaphthalene, vinyltoluene, vinylpyridine, diphenylethylene, and tertiary amino group-containing diphenylethylene, as well as conjugated diene compounds such as butadiene and isoprene. These may be used alone or in combination of two or more. Among these, butadiene is preferred. That is, the farnesene-vinyl monomer copolymer is preferably a copolymer of farnesene and butadiene (farnesene-butadiene copolymer).
[0118] In the farnesene-vinyl monomer copolymer, the copolymerization ratio by mass of farnesene and vinyl monomer (farnesene / vinyl monomer) is preferably 40 / 60 to 90 / 10.
[0119] The farnesene-based polymer preferably has a weight average molecular weight (Mw) of 3000 or more and 300,000 or less. The Mw of the farnesene-based polymer is preferably 8000 or more, more preferably 10,000 or more, and is preferably 100,000 or less, more preferably 60,000 or less, and even more preferably 50,000 or less. Within the above ranges, the effect tends to be more preferably obtained.
[0120] The farnesene-based polymer may be either a liquid or solid polymer at room temperature (25° C.), and is preferably a liquid farnesene-based polymer that is a liquid at room temperature (25° C.).
[0121] When the rubber composition for an inner liner contains the liquid farnesene polymer, the content of the liquid farnesene polymer is preferably 0.1 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 6 parts by mass or more, and is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less, per 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better. When the content is within the above range, the effect tends to be better, and is also desirable from the viewpoint of sustainability.
[0122] From the viewpoints of crack resistance, ozone resistance, and the like, the rubber composition for an inner liner preferably contains an antioxidant.
[0123] The antiaging agent is not particularly limited, and examples thereof include naphthylamine-based antiaging agents such as phenyl-α-naphthylamine; diphenylamine-based antiaging agents such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, Examples of the antioxidant include p-phenylenediamine antioxidants such as amines; quinoline antioxidants such as polymerized 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Among these, p-phenylenediamine antioxidants and quinoline antioxidants are preferred, and N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and polymerized 2,2,4-trimethyl-1,2-dihydroquinoline are more preferred. Commercially available products include, for example, products from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd.
[0124] In the rubber composition for an inner liner, the content of the antioxidant is preferably 0.2 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1.0 part by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 7.0 parts by mass or less, and more preferably 4.0 parts by mass or less.
[0125] The rubber composition for the inner liner preferably contains stearic acid. In the rubber composition for an inner liner, the content of stearic acid is preferably 0.5 parts by mass or more, more preferably 1.5 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, per 100 parts by mass of the rubber component.
[0126] As the stearic acid, any conventionally known product can be used, for example, products available from NOF Corp., Kao Corp., Fujifilm Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., and the like.
[0127] The rubber composition for an inner liner preferably contains zinc oxide. In the rubber composition for an inner liner, the content of zinc oxide is preferably 0.5 parts by mass or more, more preferably 1.5 parts by mass or more, and preferably 5 parts by mass or less, more preferably 3 parts by mass or less, per 100 parts by mass of the rubber component.
[0128] As the zinc oxide, any known zinc oxide can be used, for example, products available from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc.
[0129] The rubber composition for the inner liner may contain wax. In the rubber composition for an inner liner, the wax content is preferably 0.5 parts by mass or more, more preferably 2 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, per 100 parts by mass of the rubber component.
[0130] The wax is not particularly limited, and examples thereof include petroleum waxes, natural waxes, etc. Also, synthetic waxes obtained by refining or chemically treating multiple waxes can be used. These waxes may be used alone or in combination of two or more kinds.
[0131] Examples of petroleum waxes include paraffin wax and microcrystalline wax. Examples of natural waxes are not particularly limited as long as they are derived from resources other than petroleum, and include, for example, vegetable waxes such as candelilla wax, carnauba wax, Japan wax, rice wax, and jojoba wax; animal waxes such as beeswax, lanolin, and spermaceti; mineral waxes such as ozokerite, ceresin, and petrolactam; and refined products thereof. Examples of commercially available products include products from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., and Seiko Chemical Co., Ltd.
[0132] It is preferable to compound sulfur into the rubber composition for the inner liner in that it forms an appropriate amount of crosslinked chains in the polymer chains and imparts good performance.
[0133] In the rubber composition for an inner liner, the content of sulfur is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 5.0 parts by mass or less, more preferably 3.0 parts by mass or less, and even more preferably 2.0 parts by mass or less.
[0134] Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0135] The rubber composition for an inner liner preferably contains a vulcanization accelerator. In the rubber composition for the inner liner, the content of the vulcanization accelerator is not particularly limited and may be freely determined according to the desired vulcanization speed and crosslink density, but is preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and even more preferably 1.1 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 8.0 parts by mass or less, more preferably 6.0 parts by mass or less, and even more preferably 5.0 parts by mass or less.
[0136] The type of vulcanization accelerator is not particularly limited, and commonly used ones can be used. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, and N-cyclohexyl-2-benzothiazyl sulfenamide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, Nt-butyl-2-benzothiazolyl sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine-based vulcanization accelerators such as diphenylguanidine, di-orthotolyl guanidine, and orthotolyl biguanidine. These may be used alone or in combination of two or more. Among them, sulfenamide-based, guanidine-based and benzothiazole-based vulcanization accelerators are preferred.
[0137] In addition to the above-mentioned components, the rubber composition for an inner liner may contain compounding agents generally used in the tire industry, such as materials such as a mold release agent, as appropriate.
[0138] The rubber composition for the inner liner can be produced, for example, by kneading the above-mentioned components using a rubber kneading device such as an open roll or a Banbury mixer, and then vulcanizing the mixture.
[0139] As for the kneading conditions, in the base kneading step in which additives other than the crosslinking agent (vulcanizing agent) and the vulcanization accelerator are kneaded, the kneading temperature is preferably 100°C or higher, more preferably 120°C or higher, and also preferably 180°C or lower, more preferably 170°C or lower. In the finish kneading step in which the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is preferably 80°C or higher, and also preferably 120°C or lower, more preferably 110°C or lower. In addition, the composition kneaded with the vulcanizing agent and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is preferably 140°C or higher, more preferably 150°C or higher, and also preferably 190°C or lower, more preferably 185°C or lower.
[0140] In particular, the rubber composition for an inner liner is desirably produced by a production method including a step of kneading at least the ion-bonding rubber and the ionic compound to prepare a master batch.
[0141] The above step can be carried out, for example, by kneading at least the ionic rubber and the ionic compound at a temperature of 130° C. or less (preferably 120° C. or less). The kneading time is not particularly limited and may be appropriately set, but is preferably 2 to 6 minutes, more preferably 2 to 5 minutes.
[0142] The kneading method in the above step is not particularly limited, and a kneader generally used in the rubber industry, such as a Banbury mixer or an open roll, can be used.
[0143] The master batch containing the ion-bonding rubber and the ionic compound produced in the above process is kneaded and vulcanized with the other components described above by a known method, thereby producing the rubber composition (after vulcanization).
[0144] The rubber composition for an inner liner is used for an inner liner of a tire component. The inner liner is a member that is formed to form the inner surface of the tire cavity, and this member reduces the amount of air permeating therethrough and is capable of maintaining the internal pressure of the tire.
[0145] The tire of the present invention is manufactured by a normal method using the above-mentioned rubber composition for innerliner. That is, the composition, which contains various additives as necessary, is extruded to match the shape of the innerliner while still unvulcanized, molded by a normal method on a tire building machine, and laminated together with other tire components to form an unvulcanized tire, which is then heated and pressurized in a vulcanizer to manufacture the tire.
[0146] The tire is not particularly limited, and examples thereof include pneumatic tires, solid tires, airless tires, etc. Among these, pneumatic tires are preferred.
[0147] The above tires are suitably used as passenger car tires, large passenger car tires, large SUV tires, truck and bus tires, motorcycle tires, racing tires, winter tires (studless tires, snow tires, studded tires), all-season tires, run-flat tires, aircraft tires, mining tires, etc.
[0148] In the tire, the inner liner has a thickness G (mm) of 2.0 mm or less. G is preferably 1.8 mm or less, more preferably 1.5 mm or less. The lower limit is preferably 0.2 mm or more, more preferably 0.5 mm or more, and even more preferably 0.7 mm or more. Within the above range, the effect tends to be preferably obtained.
[0149] In this specification, the thickness G of the inner liner refers to the thickness of the inner liner on the tire equatorial plane in the tire radial cross section. Specifically, the thickness of the inner liner is the linear distance measured along the tire equatorial plane from the outer surface to the inner surface in the tire radial direction of the inner liner on the tire equatorial plane.
[0150] In the above tire, the ratio (A / G) of the crack growth index A in the rubber composition for innerliner (after vulcanization) to the thickness G (mm) of the innerliner is desirably greater than 100 in order to obtain a greater effect. A / G is preferably at least 130, more preferably at least 161, even more preferably at least 170, and particularly preferably at least 185. The upper limit is preferably at most 300, more preferably at most 250, and even more preferably at most 230. Within the above range, the effect tends to be favorably obtained.
[0151] The mechanism by which greater effectiveness is achieved when A / G is adjusted to exceed 100 is not clear, but it is presumed that by increasing the crack growth index A, the occurrence of cracks is suppressed and the rubber itself is less likely to be destroyed, and by reducing the thickness G of the inner liner, the strain applied to the rubber surface is reduced, suppressing the occurrence of cracks and improving the air retention performance after deterioration.
[0152] In the above tire, the ratio (Bc / G) of the content (Bc) of the above butyl-based rubber in 100 mass% of the rubber component in the rubber composition for the inner liner to the thickness G (mm) of the inner liner is desirably greater than 30 in order to obtain a greater effect. Bc / G is preferably at least 35, more preferably at least 40, and even more preferably at least 43. The upper limit is preferably at most 70, more preferably at most 60, and even more preferably at most 55. Within the above range, the effect tends to be favorably obtained. The ratio (BHc / G) of the content (BHc) of the halogenated butyl rubber in 100% by mass of the rubber component in the rubber composition for an inner liner to the thickness G (mm) of the inner liner is also desirably in the same range.
[0153] Although the mechanism by which a greater effect is obtained when the Bc / G is adjusted to a certain level or higher is not clear, it is believed that the air retention is improved by increasing the amount of butyl rubber B, and the strain applied to the rubber surface is reduced by reducing the thickness G of the inner liner, thereby suppressing the occurrence of cracks. Therefore, it is presumed that the air retention performance after deterioration is improved.
[0154] In the above tire, the ratio (Ic / G) of the content (Ic) of the ionic compound per 100 parts by mass of the rubber component in the rubber composition for the inner liner to the thickness G (mm) of the inner liner is desirably 0.8 or more in order to obtain a greater effect. Ic / G is preferably 1.0 or more, more preferably 1.2 or more, and even more preferably 1.3 or more. The upper limit is preferably 2.5 or less, more preferably 2.0 or less, and even more preferably 1.8 or less. Within the above range, the effect tends to be preferably obtained. The ratio (IIc / G) of the content (IIc) of the imidazoles per 100 parts by mass of the rubber component in the rubber composition for an inner liner to the thickness G (mm) of the inner liner is also desirably in the same range.
[0155] Although the mechanism by which the effect of adjusting Ic / G to a certain level or higher is unclear, it is believed that the air retention is improved by increasing the amount of ionic compounds IcB, and the strain applied to the rubber surface is reduced by reducing the thickness G of the inner liner, suppressing the occurrence of cracks. Therefore, it is presumed that the air retention performance after aging is improved.
[0156] In this specification, dimensions such as thickness are measured with the bead portion of the tire aligned to the standard rim width. During measurement, the tire is cut out in the tire radial direction, and both bead ends of the sample are fixed in a state where they are aligned to the standard rim width.
[0157] In this specification, unless otherwise specified, the dimensions of each part of the tire are values measured under normal conditions. In this specification, the term "normal condition" refers to a condition in which the tire is mounted on a normal rim (not shown), inflated to normal internal pressure, and no load is applied.
[0158] When it is not possible to measure with the tire mounted on a regular rim, the dimensions and angles of each part in the meridian section of the tire are measured by cutting the tire along a plane including the axis of rotation, and the distance between the left and right beads in the cross section is measured so that it corresponds to the distance between the beads of the tire mounted on a regular rim.
[0159] "Genuine rim" refers to the rim that is specified for each tire by the standard system that includes the standard on which the tire is based, for example, "Standard rim" in the applicable size listed in the "JATMA YEAR BOOK" for JATMA (Japan Automobile Tire Manufacturers Association), "Measuring Rim" in the "STANDARDS MANUAL" for ETRTO (The European Tire and Rim Technical Organization), and "Design Rim" in the "YEAR BOOK" for TRA (The Tire and Rim Association, Inc.). Refer to JATMA, ETRTO, and TRA in that order, and follow the standard if there is an applicable size at the time of reference. In the case of a tire not specified in the standard, it refers to the rim that can be assembled to the rim and can hold internal pressure, that is, the rim with the smallest rim diameter and the next narrowest rim width among the rims that do not leak air from between the rim and tire.
[0160] "Regular internal pressure" refers to the air pressure specified for each tire by each standard in the standard system including the standard on which the tire is based. For JATMA, it refers to the "Maximum Air Pressure", for ETRTO, it refers to the "INFLATION PRESSURE", and for TRA, it refers to the maximum value listed in the table "TIRE LOAD LIMITS AT VARIOUS COLD INFLATION PRESSURES". As with "regular rims", it refers to JATMA, ETRTO, TRA in that order and follows those standards. For tires not specified in the standard, it refers to the regular internal pressure (250kPa or more) of another tire size (specified in the standard) that is specified with the regular rim as the standard rim. Note that if multiple regular internal pressures of 250kPa or more are specified, it refers to the smallest value among them.
[0161] In this specification, the term "normal load" refers to the load that is determined for each tire by each standard in the standard system including the standard on which the tire is based, and is the maximum load capacity in the case of JATMA, the "LOAD CAPACITY" in the case of ETRTO, and the maximum value listed in the table "TIRE LOAD LIMITS AT VARIOUS COLD INFLATION PRESSURES" in the case of TRA. As in the case of the "normal rim" and "normal internal pressure" mentioned above, JATMA, ETRTO, and TRA are referred to in that order and their standards are followed. In the case of a tire not determined by a standard, the normal load W is calculated as follows: L Request. V = {(Dt / 2) 2 -(Dt / 2-Ht) 2}×π×Wt W L =0.000011×V+175 W L :Normal load (kg) V: Virtual volume of the tire (mm 3 ) Dt: Tire outer diameter (mm) Ht: Section height of the tire (mm) Wt: tire section width (mm)
[0162] The "section width Wt (mm)" of a tire is the maximum width between the outer surfaces of the sidewalls when the tire is in its normal condition, excluding any patterns or lettering on the sidewalls.
[0163] The "outer diameter Dt (mm)" of a tire refers to the outer diameter of the tire under normal conditions.
[0164] The "section height Ht (mm)" of a tire refers to the radial height of the tire at its radial cross section, and corresponds to half the difference between the tire's outer diameter Dt and the rim diameter R, where R is the tire's rim diameter (mm). In other words, the section height Ht can be calculated by (Dt-R) / 2.
[0165] An example of a tire according to the present invention will be described below with reference to the drawings, but the present invention is not limited to this embodiment.
[0166] FIG. 2 is a cross-sectional view showing a part of a pneumatic tire. 2, the up-down direction is the radial direction of the tire 2, the left-right direction is the axial direction of the tire 2, and the direction perpendicular to the paper surface is the circumferential direction of the tire 2. The tire 2 is symmetrical. The tread 4 includes a cap layer 30 and a base layer 28.
[0167] Although FIG. 2 shows an example of a two-layer tread 4 made up of a cap layer 30 and a base layer 28, a single-layer tread or a tread having a structure of three or more layers may also be used.
[0168] In the tire 2, each sidewall 6 extends substantially radially inward from an end of the tread 4. A radially outer portion of each sidewall 6 is joined to the tread 4. A radially inner portion of each sidewall 6 is joined to a clinch 10. Each sidewall 6 can prevent damage to the carcass 14.
[0169] 2 is located between the tread 4 and the sidewall 6. The wing 8 is joined to the tread 4 and the sidewall 6, respectively.
[0170] Each clinch 10 is located approximately radially inward of the sidewall 6 and has at least one or more portions that come into contact with the rim.
[0171] The carcass 14 includes a carcass ply 36. In the tire 2, the carcass 14 is made up of one carcass ply 36, but may be made up of two or more carcass plies.
[0172] In the tire 2, the carcass ply 36 is laid between the bead cores 32 on both sides and extends along the tread 4 and the sidewall 6. The carcass ply 36 is folded back from the inside to the outside in the axial direction around each bead core 32. By this folding back, the carcass ply 36 is formed with a main portion 36a and a pair of folded back portions 36b. That is, the carcass ply 36 includes the main portion 36a and a pair of folded back portions 36b.
[0173] Each bead core 32 includes a bead apex 34 extending radially outward from the bead core 32. The bead core 32 is preferably ring-shaped and includes a wound non-stretchable wire. The bead apex 34 tapers radially outward.
[0174] Although not shown, the carcass ply 36 is preferably made of a number of parallel cords and a topping rubber. The absolute value of the angle that each cord makes with respect to the equatorial plane CL is preferably 75° to 90°. In other words, the carcass 14 preferably has a radial structure.
[0175] The belt layer 16 in FIG. 2 is located radially inward of the tread 4. The belt layer 16 is laminated with the carcass 14. The belt layer 16 reinforces the carcass 14. In the tire 2 in FIG. 2, the belt layer 16 is composed of an inner layer 38 and an outer layer 40. As is clear from FIG. 2, it is desirable that the width of the inner layer 38 is slightly larger than the width of the outer layer 40 in the axial direction. In this tire 2, the axial width of the belt layer 16 is preferably 0.6 times or more and 0.9 times or less of the cross-sectional width of the tire 2.
[0176] Each of the inner layer 38 and the outer layer 40 is preferably made of a number of parallel steel cords and a topping rubber. In other words, the belt layer 16 includes a number of parallel steel cords.
[0177] The band 18 in Fig. 2 is located radially outside the belt layer 16. In the axial direction, the band 18 has a width equal to the width of the belt layer 16. The band 18 may also have a width greater than the width of the belt layer 16.
[0178] Although not shown, the band 18 is preferably made of a cord and a topping rubber. The cord is wound in a spiral shape. This band 18 has a so-called jointless structure. The cord extends substantially in the circumferential direction. The angle of the cord with respect to the circumferential direction is preferably 5° or less, and more preferably 2° or less. Since the belt layer 16 is restrained by the cord, lifting of the belt layer 16 is suppressed.
[0179] The belt layer 16 and the band 18 in Fig. 2 constitute a reinforcing layer. The reinforcing layer may be constituted by the belt layer 16 alone.
[0180] The inner liner 20 is located inside the carcass 14. The inner liner 20 is joined to the inner surface of the carcass 14. The inner liner 20 holds the internal pressure of the tire 2.
[0181] In the tire 2 of FIG. 2, the inner liner 20 is made of the above-mentioned rubber composition (after vulcanization).
[0182] Each chafer 22 is located adjacent to a bead 12. In this embodiment, the chafer 22 is preferably made of fabric with rubber impregnated into the fabric. The chafer 22 may be integral with the clinch 10.
[0183] In the tire 2, the tread 4 has a main groove 42 as the groove 26. As shown in FIG. 2, a plurality of main grooves 42, specifically three main grooves 42, are formed in the tread 4. These main grooves 42 are arranged at intervals in the axial direction. The three main grooves 42 are formed in the tread 4, thereby forming four ribs 44 extending in the circumferential direction. In other words, the spaces between the ribs 44 constitute the main grooves 42.
[0184] Each of the main grooves 42 extends in the circumferential direction. The main grooves 42 are continuous in the circumferential direction without interruption. The main grooves 42 facilitate the drainage of water present between the road surface and the tire 2, for example, in rainy weather. Therefore, even if the road surface is wet, the tire 2 can make sufficient contact with the road surface.
[0185] FIG. 3 is an enlarged cross-sectional view showing the vicinity of the tread 4 of the tire of FIG. The tire in FIG. 3 includes an inner liner 20, and in this case, the thickness G of the inner liner 20 refers to the linear distance from the outer surface to the inner surface in the tire radial direction of the inner liner 20 on the tire equatorial plane (CL) in the radial cross section of the tire.
[0186] In the tire 2 of Figures 2 and 3, the complex modulus of elasticity Ew (MPa) when wet, the complex modulus of elasticity Es (MPa) when dry, the hardness Hw when wet, the hardness Hs when dry, the crack growth index A, the butyl rubber content Bc (mass %), and the ionic compound content Ic (parts by mass) of the rubber composition constituting the inner liner 20 satisfy Ew / Es of 0.95 or less, A of 190 or more, and G of 2.0 mm or less, and it is preferable that Es, Hw / Hs, Hs, Bc, Ic, A / G, Bc / G, and Ic / G are in the ranges described above. EXAMPLES
[0187] In the following, examples (embodiments) that are considered to be preferable for carrying out the present invention will be shown, but the scope of the present invention is not limited to the examples.
[0188] Various chemicals used in the examples and comparative examples will be collectively described below. Natural rubber: TSR20 Brominated butyl rubber: Cl-IIR (Bromobutyl 2255 manufactured by Exxonmobil, butyl rubber having an anionic functional group (bromo group), anionic functional group: 1.03% by mass) Imidazole: 1-butylimidazole (cationic compound) manufactured by Tokyo Chemical Industry Co., Ltd. Master batch: mixture of Cl-IIR and 1-butylimidazole (production example below, compounding ratio in Table 1) Carbon black: Diablack N660 (N2SA:28m) manufactured by Mitsubishi Chemical Corporation 2 / g, DBP absorption: 84ml / 100g) Anti-aging agent: Nocrac RD (poly(2,2,4-trimethyl-1,2-dihydroquinoline)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Stearic acid: NOF Corporation's "Tsubaki" stearic acid Oil: PS-32 (mineral oil) manufactured by Idemitsu Kosan Co., Ltd. Zinc oxide: Zinc oxide No. 1 manufactured by Mitsui Mining & Smelting Co., Ltd. Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Co., Ltd. Vulcanization accelerator CZ: Noccela CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator DM: Noccela DM (di-2-benzothiazolyl disulfide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0189] <Production example: Masterbatch production> According to the compounding ratio of Cl-IIR and 1-butylimidazole shown in Table 1, Cl-IIR and 1-butylimidazole are charged into a 1.7 L sealed Banbury mixer, kneaded for 4 minutes until the temperature reaches 115°C, and discharged when the temperature reaches 120°C to obtain a mixture (master batch) of Cl-IIR and 1-butylimidazole.
[0190] <Examples and Comparative Examples> According to the compounding recipe shown in Table 1, the chemicals other than sulfur and the vulcanization accelerator are kneaded for 5 minutes at 150°C using a 1.7 L Banbury mixer to obtain a kneaded mixture. Sulfur and a vulcanization accelerator are added to the kneaded mixture, and the mixture is kneaded for 5 minutes at 80° C. using an open roll to obtain an unvulcanized rubber composition. The unvulcanized rubber composition is vulcanized at 170° C. for 15 minutes to obtain a vulcanized rubber composition. In addition, the unvulcanized rubber composition is used to mold the inner liner into a shape that matches the shape of the inner liner, and is laminated together with other tire components to prepare an unvulcanized tire. The tire is then vulcanized at 170°C for 15 minutes to obtain a test tire (size: 195 / 65R15, specifications: Table 1).
[0191] The vulcanized rubber composition and the test tire were evaluated as follows. The results are shown in Table 1.
[0192] <Viscoelasticity test> A viscoelasticity measurement sample of 40 mm in length × 3 mm in width × 0.5 mm in thickness is taken from each vulcanized rubber composition, and the complex modulus (E*) of the vulcanized rubber composition is measured using a TA Instruments RSA series under the conditions of a temperature of 30°C, an initial strain of 10%, a dynamic strain of 1%, a frequency of 10 Hz, an extension mode, and a measurement time of 30 minutes, and the measured value is obtained 30 minutes after the start of the measurement.
[0193] (Dry complex elastic modulus Es) The viscoelasticity measurement sample is dried under normal temperature and pressure conditions until it reaches a constant weight. The complex modulus of the sample after drying is measured by the above-mentioned viscoelasticity test method, and is defined as the complex modulus of elasticity in the dry state, Es.
[0194] (Complex modulus of elasticity Ew when wet with water) The complex modulus of elasticity Ew when wetted with water is determined by measuring the viscoelasticity in water using the RSA immersion measurement jig and the above-mentioned viscoelasticity test method. The water temperature is set to 30°C.
[0195] <Hardness measurement> For test pieces (cuboid shape of 30 mm x 30 mm x 4 mm) made from each vulcanized rubber composition, the Shore hardness (H) is measured using a Type A durometer in accordance with JIS K6253-3:2012 "Vulcanized rubber and thermoplastic rubber - Determination of hardness - Part 3: Durometer hardness" (JIS-A hardness). Measurements are carried out at 25°C for both dry hardness (Hs) and wet hardness (Hw). Values are the average of five measurements. (Test piece treatment conditions) Drying: Dry the test piece at 80℃ and 1kPa or less under reduced pressure until it reaches a constant weight. When wet with water: Test piece is immersed in 20 ml of water at 25°C for 6 hours
[0196] <Crack growth test> The following crack growth test is performed on each vulcanized rubber composition to measure the crack growth index A. The crack growth test is performed in accordance with JIS K6260:2017 except for the following conditions. <Crack growth test> (1) A rubber sheet of 100 mm length × 50 mm width × 2.0 mm thickness formed from each vulcanized rubber composition was given an initial cut of 5.0 mm on both sides of the center in the longitudinal direction (sample shown in FIG. 1). (2) The sample with the initial scratch is bent at 40% strain using a De Mattia testing machine (manufactured by Toyo Seiki Co., Ltd.) and the number of times it is bent until it breaks is measured. (3) The number of flexions until fracture / 100 is the crack growth index A.
[0197] <Air retention> Each test tire is mounted on a JIS standard rim 15x6JJ, inflated to an initial pressure of 200Kpa, and left at room temperature for 90 days to calculate the rate of decrease in air pressure (% / month). The result is expressed as an index, with Comparative Example 2 set as the standard (100). The higher the index, the better the air retention.
[0198] [Table 1]
[0199] The present invention (1) is a tire having an inner liner, The inner liner is made of a rubber composition having a ratio (Ew / Es) of a complex modulus of elasticity Ew (MPa) when wet to a complex modulus of elasticity Es (MPa) when dry of 0.95 or less, The rubber composition has a crack growth index A of 190 or more as measured by the following crack growth test, In the tire, the thickness G of the inner liner is 2.0 mm or less. <Crack growth test> (1) A rubber sheet formed from the rubber composition, measuring 100 mm in length, 50 mm in width, and 2.0 mm in thickness, is given an initial cut of 5.0 mm on both sides of the center in the longitudinal direction. (2) The sample with the initial scratch is bent at 40% strain using a De Mattia testing machine, and the number of times it is bent until it breaks is measured. (3) The number of flexions until fracture / 100 is the crack growth index A.
[0200] The present invention (2) is the tire according to the present invention (1), in which the Ew / Es is 0.91 or less.
[0201] The present invention (3) is the tire according to the present invention (1) or (2), in which the crack growth index A is 360 or more.
[0202] The present invention (4) is a tire in any combination with any of the present inventions (1) to (3), in which the ratio (A / G) of the crack growth index A to the thickness G (mm) of the inner liner exceeds 100.
[0203] The present invention (5) is the tire according to the present invention (4), wherein the A / G is 170 or more.
[0204] The present invention (6) is a tire in any combination with any of the present inventions (1) to (5), in which the ratio (Hw / Hs) of the wet hardness Hw to the dry hardness Hs of the rubber composition is 0.98 or less.
[0205] The present invention (7) is directed to a rubber composition comprising a butyl rubber, The tire is any combination with any of the present inventions (1) to (6), in which the ratio (Bc / G) of the content of butyl-based rubber in 100% by mass of the rubber component in the rubber composition to the thickness G (mm) of the inner liner is 40 or more.
[0206] The present invention (8) further provides a rubber composition comprising an ionic compound, The tire is any combination with any of the present inventions (1) to (7), in which the ratio (Ic / G) of the content of the ionic compound (Ic) per 100 parts by mass of the rubber component in the rubber composition to the thickness G (mm) of the inner liner is 0.8 or more. [Explanation of symbols]
[0207] 2 Tires 4 Tread 6 Sidewall 8 Wing 10. Clinch 12 Beads 14 Carcass 16 Belt Layer 18 Bands 20 Inner Liner 22 Chafer 24 Tread Surface 26 Groove 28 Base Layer 30 Cap Layer 32 Bead core 34 Bead Apex 36 Carcass ply 36a Main part 36b Folded part 38 Inner layer 40 outer layer 42 Main groove 44 Ribs CL Tire equatorial plane G Inner liner thickness
Claims
1. A tire having an inner liner, the inner liner is made of a rubber composition having a ratio (Ew / Es) of a complex modulus of elasticity Ew (MPa) when wet to a complex modulus of elasticity Es (MPa) when dry of 0.95 or less; The rubber composition has a crack growth index A of 190 or more as measured by the following crack growth test, The tire, wherein the thickness G of the inner liner is 2.0 mm or less. <Crack growth test> (1) A rubber sheet made of the rubber composition and measuring 100 mm in length, 50 mm in width, and 2.0 mm in thickness is given an initial scratch of 5.0 mm on both sides of the center in the longitudinal direction. (2) The sample with the initial damage is bent at 40% strain using a De Mattia testing machine, and the number of times it is bent until it breaks is measured. (3) The number of flexions until breakage / 100 is defined as the crack growth index A.
2. 2. The tire according to claim 1, wherein the Ew / Es is 0.91 or less.
3. 2. The tire according to claim 1, wherein the crack growth index A is 360 or greater.
4. The tire according to claim 1 , wherein a ratio (A / G) of the crack growth index A to a thickness G (mm) of the inner liner exceeds 100.
5. 5. The tire according to claim 4, wherein the A / G is 170 or greater.
6. The tire according to claim 1, wherein the rubber composition has a ratio (Hw / Hs) of wet hardness Hw to dry hardness Hs of 0.98 or less.
7. The rubber composition includes a butyl-based rubber, The tire according to claim 1, wherein a ratio (Bc / G) of a content (Bc) of the butyl-based rubber in 100% by mass of the rubber component in the rubber composition to a thickness G (mm) of the inner liner is 40 or more.
8. The rubber composition contains an ionic compound, The tire according to claim 1, wherein a ratio (Ic / G) of a content (Ic) of the ionic compound per 100 parts by mass of the rubber component in the rubber composition to a thickness G (mm) of the inner liner is 0.8 or more.
Citation Information
Patent Citations
Rubber composition for inner liner, and pneumatic tire
JP2014227494A