Antifogging film, packaging material, and package

A polypropylene film using bio-naphtha-derived propylene and specific additives maintains antifogging properties and stability over time, addressing environmental concerns and film degradation issues.

JP2024149367AInactive Publication Date: 2024-10-18OJI HLDG CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023216851
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-05
Filing Date
2023-12-22
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polypropylene films used in packaging materials face issues with color and strength changes over time, and there is a need to reduce the environmental impact by minimizing petrochemical materials.

Method used

A polypropylene film is produced using bio-naphtha-derived propylene, combined with specific amounts of an antifogging agent and phosphorous antioxidant, to maintain antifogging properties while reducing petrochemical use.

Benefits of technology

The film exhibits stable antifogging properties with minimal color and strength changes over time, while significantly reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149367000001
    Figure 2024149367000001
Patent Text Reader

Abstract

To provide an antifogging film that is produced using bionaphtha-derived propylene so as to reduce environmental loads which has less change in color and strength with time.SOLUTION: An antifogging film containing polypropylene produced using bionaphtha-derived propylene and an antifogging agent contains 10 mass% or more and 50 mass% or less of a unit based on the bionaphtha-derived propylene, 0.3 mass% or more and 1.0 mass% or less of the antifogging agent, and 300 mass ppm or more and 1,000 mass ppm or less of a phosphorus-based antioxidant, with respect to the mass of the antifogging film. The phosphorus-based antioxidant is preferably tris(2,4-di-t-butylphenyl)phosphite.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an anti-fog film produced using raw materials derived from bionaphtha, and a packaging material and a package using said anti-fog film. [Background technology]

[0002] Polypropylene films are widely used as packaging materials for foods, medicines, industrial products, etc., or as parts of industrial products. Examples of the forms of use include single-layer sheets made of a single layer of polypropylene film, and laminated sheets in which polypropylene film is laminated with other sheet materials. Examples of other sheet materials to be laminated with polypropylene film include polyester resin films, polyvinyl chloride films, and paper. For packaging materials, polypropylene films having anti-fogging properties are used as required.

[0003] In recent years, in order to reduce the environmental impact, attempts have been made to replace petroleum-based raw materials with non-petroleum-based raw materials in various industrial products and packaging materials. For example, Patent Document 1 proposes producing polyolefin resins from biological raw materials by cracking. However, when films were produced from the polyolefins obtained by cracking, the films showed changes in color and strength over time, and did not fully meet the needs of customers for industrial products and packaging materials. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2018-522087 Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention aims to provide a film material that has anti-fogging properties and exhibits little change in color and strength over time while reducing the amount of petrochemical materials used, thereby resolving the problem of the environmental load of plastic products. [Means for solving the problem]

[0006] The present inventors have thoroughly investigated methods for producing a film using non-petrochemical materials that have a small environmental impact as raw materials, and as a result have found that by adjusting the blend amount of a phosphorus-based antioxidant in the film to a specific range, a polypropylene film can be obtained that has anti-fog properties, is less susceptible to change in color and transparency over time, has excellent mechanical properties, and has a reduced environmental impact, thereby completing the present invention.

[0007] The present invention has the following aspects. [1] An anti-fog film comprising polypropylene produced using propylene derived from bionaphtha and an anti-fog agent, the anti-fog film containing, relative to the mass of the anti-fog film, 10% by mass or more and 50% by mass or less of units based on the propylene derived from the bionaphtha, 0.3% by mass or more and 1.0% by mass or less of the anti-fog agent, and 300 ppm by mass or more and 1,000 ppm by mass or less of a phosphorus-based antioxidant. [2] The anti-fog film according to [1], wherein the phosphorus-based antioxidant comprises tris(2,4-di-t-butylphenyl)phosphite. [3] A laminate having a plurality of layers laminated together, at least one of which is made of the anti-fog film according to [1] or [2] above. [4] A packaging material comprising the anti-fog film described in [1] or [2] above. [5] A package in which an item is packaged using the packaging material described in [4] above. [6] An anti-fog film comprising a polypropylene and an anti-fog agent, wherein the polypropylene comprises a first polypropylene (A) comprising units based on propylene derived from bionaphtha; The content of the propylene-based unit derived from the bionaphtha is 10% by mass or more and 50% by mass or less relative to the mass of the anti-fog film; The anti-fog agent is contained in an amount of 0.3% by mass to 1.0% by mass relative to the mass of the anti-fog film, An anti-fog film comprising a phosphorus-based antioxidant in an amount of 300 ppm by mass or more and 1000 ppm by mass or less relative to the mass of the anti-fog film. [7] The anti-fog film according to [6], wherein the first polypropylene (A) further contains units based on propylene derived from petroleum naphtha. [8] The anti-fog film according to [7], wherein the first polypropylene (A) contains units based on propylene derived from a mixture of bionaphtha and petroleum naphtha. [9] The anti-fog film according to any one of [6] to [8], wherein the bionaphtha-derived propylene-based units account for 20 to 90 mass % of all units of the first polypropylene (A).

[10] The anti-fog film according to any one of [6] to [9], wherein the polypropylene further comprises a second polypropylene (B) that contains units based on propylene derived from petroleum naphtha and does not contain units based on propylene derived from bionaphtha.

[11] The anti-fog film according to any one of [6] to

[10] , which has a core layer containing the first polypropylene (A) and a skin layer having a composition different from that of the core layer.

[12] The anti-fog film according to

[11] , wherein the core layer further comprises a second polypropylene (B) that contains units based on propylene derived from petroleum naphtha and does not contain units based on propylene derived from bionaphtha.

[13] The anti-fog film according to

[11] or

[12] , wherein the skin layer comprises a second polypropylene (B) that contains units based on propylene derived from petroleum naphtha and does not contain units based on propylene derived from bionaphtha. Effect of the Invention

[0008] According to the present invention, a polypropylene film having anti-fog properties and little change in color and strength over time can be obtained while reducing the amount of petrochemical materials used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] In this specification, the use of "to" indicating a range of values ​​means that the values ​​before and after it are included as the lower limit and upper limit. The lower and upper limits of the numerical ranges disclosed in this specification can be combined in any manner to create new numerical ranges.

[0010] <Anti-fog film> The anti-fog film according to one embodiment of the present invention is a polypropylene film having anti-fog properties (hereinafter, also referred to as "polypropylene film (F)"). The polypropylene film (F) contains polypropylene obtained by polymerization of propylene and an anti-fog agent. A part of the propylene is produced from a raw material derived from bionaphtha. In this specification, "bionaphtha" means naphtha produced using biomass as a raw material. "Petroleum naphtha" means naphtha produced using petroleum as a raw material.

[0011] The polypropylene film (F) contains 10% by mass or more and 50% by mass or less, preferably 10% by mass or more and 25% by mass or less, of units based on propylene produced from raw materials derived from bionaphtha (hereinafter also referred to as "bio-naphtha-derived P units"). If the content of the bionaphtha-derived P units is less than 10% by mass, the effect of reducing the environmental load is small. In addition, if the content of the bionaphtha-derived P units exceeds 50% by mass, the change in color and strength over time is easily noticeable, and the commercial value of the product is likely to decrease. The content of the bionaphtha-derived P units is preferably 40% by mass or less, and more preferably 30% by mass or less.

[0012] The polypropylene film (F) contains an anti-fog agent in an amount of 0.3% by mass or more and 1.0% by mass or less, preferably 0.4% by mass or more and 0.7% by mass or less. When the content of the anti-fog agent is 0.3% by mass or more, the anti-fog property is excellent. When the content of the anti-fog agent is 1.0% by mass or less, appearance defects such as whitening are unlikely to occur. Examples of the antifogging agent include glycerin fatty acid ester, alkyldiethanolamine, alkyldiethanolamine fatty acid ester, etc. The antifogging agent may be used alone or in combination of two or more kinds. In the polypropylene film (F), at least a part of the antifogging agent is preferably present on the surface or in the vicinity of the surface of the film. For example, it is preferable that the polypropylene film (F) is formed using a resin composition containing the antifogging agent, and then at least one of the front and back surfaces is subjected to a surface treatment such as a corona treatment to promote bleeding out of the antifogging agent.

[0013] The polypropylene film (F) contains a phosphorus-based antioxidant in an amount of 300 ppm or more and 1000 ppm or less, preferably 300 ppm or more and 700 ppm or less. If the content of the phosphorus-based antioxidant is 300 ppm or more, it is excellent in the effect of suppressing the change in color and strength over time. If the content of the phosphorus-based antioxidant exceeds 1000 ppm, the transparency and printing characteristics are likely to deteriorate due to bleed-out over time.

[0014] Examples of phosphorus-based antioxidants include tris(nonylphenyl)phosphite, tris(2,4-di-t-butylphenyl)phosphite, distearyl pentaerythritol diphosphite, bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite, bis(2,4-di-t-butyl-6-methylphenyl)pentaerythritol diphosphite, bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, and tetrakis(2,4-di-t-butylphenyl) 4,4'-diphenylenediphosnite, 2,2'-methylenebis(4,6-di-t-butylphenyl)2-ethylhexyl phosphite, 2,2'-ethylidenebis(4,6-di-t-butylphenyl)fluorophosphite, bis(2,4-di-t-butyl-6-methylphenyl)ethyl phosphite, 2-(2,4,6-tri-t-butylphenyl)-5-ethyl-5-butyl-1,3,2-oxaphosphorinane, 2,2',2''-nitrilo[triethyl-tris(3,3',5,5'-tetra-t-butyl-1,1'-biphenyl-2,2'-diyl)phosphite, etc. Among these, tris(2,4-di-t-butylphenyl)phosphite is particularly preferred. The phosphorus-based antioxidant preferably contains tris(2,4-di-t-butylphenyl)phosphite. The proportion of tris(2,4-di-t-butylphenyl)phosphite relative to the total mass of the phosphorus-based antioxidants contained in the polypropylene film (F) is preferably 80 mass% or more, more preferably 85 mass% or more, even more preferably 90 mass% or more, and particularly preferably 95 mass% or more. It may be 100 mass%.

[0015] The polypropylene film (F) may contain materials other than polypropylene and the anti-fogging agent depending on quality requirements, so long as the effects of the present invention are not impaired. Examples of other materials include pigments, dyes, lubricants, antiblocking agents, antistatic agents, UV absorbers, plasticizers, freshness-retaining agents, deodorizers, compatibilizers, resins other than polypropylene, and antioxidants other than phosphorus-based antioxidants. The total content of the other materials relative to the mass of the polypropylene film (F) is, for example, preferably 3 mass % or less, more preferably 2 mass % or less, and may be zero.

[0016] The polypropylene contained in the polypropylene film (F) is mainly composed of units based on propylene, and is a propylene homopolymer or a copolymer having 80 mass % or more of units based on propylene. The copolymer is, for example, a copolymer having units based on propylene and units based on one or more types of α-olefins, such as ethylene, 1-butene, 1-hexene, 1-octene, and 4-methyl-pentene-1. The proportion of propylene-based units relative to all the polypropylene units is preferably 85% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more. It may be 100% by mass.

[0017] [First polypropylene (A)] In a preferred embodiment of the polypropylene film (F), the polypropylene contained in the polypropylene film (F) includes a first polypropylene (A) containing bionaphtha-derived P units. The content of the bionaphtha-derived P units relative to all units of the first polypropylene (A) is preferably from 20 to 90 mass%, more preferably from 30 to 70 mass%, and even more preferably from 40 to 50 mass%.

[0018] The first polypropylene (A) preferably contains bionaphtha-derived P units and units based on propylene derived from petroleum naphtha (hereinafter also referred to as "petroleum-derived P units"). The content of the petroleum-derived P units relative to all units of the first polypropylene (A) is preferably from 10 to 80 mass%, more preferably from 30 to 70 mass%, and even more preferably from 50 to 60 mass%.

[0019] The first polypropylene (A) may be a copolymer having other units based on monomers other than propylene. The total content of the bionaphtha-derived P units and the petroleum-derived P units relative to the total units of the first polypropylene (A) is preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. It may be 100% by mass.

[0020] The first polypropylene (A) preferably comprises propylene-based units produced from a mixture of bionaphtha and petroleum naphtha. The propylene produced from a mixture of bionaphtha and petroleum naphtha as the raw naphtha is a mixture of propylene derived from the bionaphtha and propylene derived from the petroleum naphtha. The ratio of propylene derived from the bionaphtha and propylene derived from the petroleum naphtha in the produced propylene is determined by the ratio of propylene derived from the bionaphtha and propylene derived from the petroleum naphtha in the raw naphtha. For example, propylene (50 / 50) produced from a mixture of 50 mass% bionaphtha and 50 mass% petroleum naphtha is a mixture of 50 mass% propylene derived from the bionaphtha and 50 mass% propylene derived from the petroleum naphtha. Based on all units of the polypropylene obtained by polymerizing propylene (50 / 50), the content of bionaphtha-derived P units is 50 mass %, and the content of petroleum-derived P units is 50 mass %.

[0021] The first polypropylene (A) contained in the polypropylene film (F) may be one type or two or more types. The content of the first polypropylene (A) in the polypropylene film (F) can be designed so that the bionaphtha-derived P unit is 10% by mass or more and 50% by mass or less with respect to the mass of the polypropylene film.

[0022] [Second polypropylene (B)] The polypropylene contained in the polypropylene film (F) preferably contains, in addition to the first polypropylene (A), a second polypropylene (B) that contains petroleum-derived P units and does not contain bionaphtha-derived P units. The second polypropylene (B) may be a copolymer having units based on monomers other than propylene. The content of the petroleum-derived P units relative to all units of the second polypropylene (B) is preferably 80% by mass or more, more preferably 85% by mass or more, further preferably 90% by mass or more, particularly preferably 95% by mass or more. It may be 100% by mass.

[0023] The second polypropylene (B) contained in the polypropylene film (F) may be one type or two or more types. The content of the second polypropylene (B) relative to the polypropylene film (F) can be designed so that the bionaphtha-derived P units in the first polypropylene (A) are 10 mass% or more and 50 mass% or less relative to the mass of the polypropylene film (F).

[0024] [film] The polypropylene film (F) preferably has a core layer and a skin layer which have different compositions. For example, the polypropylene film (F) may have a core layer comprising a mixture of the first polypropylene (A) and the second polypropylene (B), and a skin layer comprising the second polypropylene (B) and no first polypropylene (A). The skin layer may be provided on only one of the front side and the back side of the core layer, or on both sides.

[0025] The resin contained in the skin layer is not particularly limited, but ethylene-propylene-1-butene copolymers, propylene-α-olefin random copolymers, and mixtures thereof are preferred because they tend to effectively exhibit anti-fogging properties. Examples of the α-olefin include ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, and 1-decene.

[0026] In the polypropylene film (F) having a core layer and a skin layer, the anti-fog agent may be contained in the core layer, the skin layer, or both. It is preferable to perform a surface treatment such as a corona treatment on the surface to exhibit anti-fog properties to promote bleeding of the anti-fog agent.

[0027] The polypropylene film (F) may be uniaxially or biaxially stretched. The stretching ratio is preferably 3 to 6 times in the MD direction and 8 to 12 times in the TD direction. The density of the polypropylene film (F) is not particularly limited, but is, for example, 0.90 to 0.92 g / cm 3 The density is a value measured by a dry density meter, a density gradient tube, etc. The thickness of the polypropylene film (F) is not particularly limited, but is, for example, 15 μm to 80 μm.

[0028] <Anti-fog film manufacturing method> The polypropylene film (F) can be produced by forming a resin composition containing polypropylene into a sheet to obtain an unstretched sheet, and then biaxially stretching the unstretched sheet to obtain the polypropylene film (F). Among these, a tenter sequential biaxial stretching method is preferred. The polypropylene film (F) having a core layer and a skin layer is preferably produced by a tenter sequential biaxial stretching method using a co-extrusion die.

[0029] <Laminate> A laminate according to one embodiment of the present invention is a laminate in which a plurality of layers are laminated, at least one of which is made of a polypropylene film (F). For example, there may be mentioned a laminate in which a plurality of polypropylene films (F) are laminated together, and a laminate in which one or more layers of polypropylene film (F) are laminated with one or more layers made of a material different from that of the polypropylene film (F). Examples of the layer made of a material different from the polypropylene film (F) include resin films other than the polypropylene film (F), paper, and the like. Examples of methods for producing the laminate include methods of laminating with other films, such as dry lamination and hot melt lamination, etc. Among these, the dry lamination method using gravure roll coating equipment is preferred. It is preferable that the polypropylene film (F) is laminated so that the surface having antifogging properties is present on the outermost surface of the laminate.

[0030] <Packaging materials> The packaging material according to one embodiment of the present invention comprises a polypropylene film (F). The polypropylene film (F) may be used as a packaging material as it is, or may be processed to a packaging material by any known processing method. For example, the ends of the polypropylene film (F) may be bonded together with an adhesive or heat-sealed to form a bag-shaped packaging material. Also, the end of the polypropylene film (F) and the end of a packaging material other than the polypropylene film (F) may be bonded or heat-sealed to form a bag-shaped packaging material. For example, a packaging bag produced using a general bag making machine using a welding and sealing method can be exemplified.

[0031] <Package> A package according to one embodiment of the present invention is an article packaged with the packaging material according to the present invention. Examples of the goods include general merchandise, food, clothing, etc. As the packaging method, known packaging methods can be applied.

[0032] <Example> The present invention will be specifically described below with reference to examples. Note that the present invention is not limited to these examples. Note that, unless otherwise specified, the unit of content "%" is "mass%". Measurement and evaluation methods used in each example are shown below.

[0033] (1) Color The YI value of the film was measured using a spectral colorimeter / haze meter "COH7700 (product name)" manufactured by Nippon Denshoku Industries Co., Ltd. The film was stored at 23°C for 3 months, and the YI value at the start of storage (initial YI) and the YI value after 3 months (YI after 3 months) were measured, and the YI value change rate (unit: %) was calculated using the following formula. The effect of suppressing the change in color over time was evaluated according to the following criteria. YI value change rate = (YI after 3 months - initial YI) / initial YI x 100 ○: Change in YI value after 3 months at 23℃ is within 20% ×: When the rate of change in YI value after 3 months at 23℃ exceeds 20%

[0034] (2) Tensile strength The tensile strength in the machine direction was measured using a tensile tester in accordance with JIS K7127. Samples were cut to a size of 15 mm in the width direction × 200 mm in the machine direction, and the test was performed at a tensile speed of 200 mm / min. The strength was measured when the film broke. The film was stored at 90°C for one month, and the strength at the start of storage (initial strength) and the strength after one month (strength after one month) were measured, and the strength change rate (unit: %) was calculated using the following formula. The effect of suppressing the change in tensile strength over time was evaluated according to the following criteria. Strength change rate = (initial strength - strength after 1 month) / initial strength x 100 ○: Strength change rate within 20% after 1 month at 90℃ ×: When the strength change rate after 1 month at 90℃ exceeds 20%

[0035] (3) Transparency The transparency of the film was measured using a Clarity-Meter TM-1D transparency meter manufactured by Murakami Color Research Laboratory. The film was stored at 23°C for 3 months, and the transparency at the start of storage (initial transparency) and after 3 months (transparency after 3 months) were measured, and the transparency change rate (unit: %) was calculated using the following formula. The effect of suppressing the change in transparency over time was evaluated according to the following criteria. Transparency change rate = (initial transparency - transparency after 3 months) / initial transparency x 100 ○: Transparency change rate within 20% after 3 months at 23℃ ×: When the transparency change rate after 3 months at 23℃ exceeds 20%

[0036] (4) Anti-fogging properties A film cut into a square with a length of 140 mm in the MD direction and a length of 140 mm in the TD direction was used as a sample. About 20 ml of water was poured into a 100 ml beaker, and the sample was placed over the opening so that the measurement surface (the surface of the first skin layer or the surface of the second skin layer) was facing down, and the periphery was secured with a rubber band, and the sample was left to stand in a low-temperature incubator at 4°C for 60 minutes. The appearance of the sample was visually observed immediately after it was removed from the low-temperature incubator. The anti-fogging property was evaluated according to the following criteria. 〇: No cloudiness on the measurement surface ×: The measurement surface is cloudy

[0037] (5) Reducing environmental impact ○: Contains polypropylene derived from bio-naphtha, so the environmental impact is small. ×: The product has a large environmental impact because it does not contain polypropylene derived from bionaphtha.

[0038] (6) The content of phosphorus-based antioxidants in polypropylene films was measured by extracting the antioxidants in the films and performing HPLC-PDA analysis.

[0039] (7) The content of bionaphtha-derived P units in the polypropylene film was calculated based on the content of bionaphtha-derived P units in each raw material resin composition and the blending ratio of each raw material resin composition. It can also be measured by measuring the C14 concentration using accelerator mass spectrometry (AMS).

[0040] <Raw materials> [Raw material resin composition containing first polypropylene (A)] The following Bio-PPs (A1) to (A3) are all resin compositions that contain polypropylene obtained by polymerizing propylene produced from raw naphtha, which is a mixture of 50% by mass of bio-naphtha and 50% by mass of petroleum naphtha, and tris(2,4-di-t-butylphenyl)phosphite, a phosphorus-based antioxidant, but do not contain an anti-fogging agent. The content of P units derived from bio-naphtha is 50% by mass relative to the total units of polypropylene. Bio-PP (A1): 99.20% by mass of polypropylene, 0.10% by mass of phosphorus-based antioxidant, 0.70% by mass of additives other than phosphorus-based antioxidants. Bio-PP (A2): 99.19% by mass of polypropylene, 0.01% by mass of phosphorus-based antioxidant, 0.80% by mass of additives other than phosphorus-based antioxidants. Bio-PP (A3): 98.90% by mass of polypropylene, 0.40% by mass of phosphorus-based antioxidant, 0.70% by mass of additives other than phosphorus-based antioxidants.

[0041] [Raw material resin composition containing second polypropylene (B)] The following petroleum PP (B1) and (B2) are both resin compositions containing polypropylene obtained by polymerizing propylene produced from 100% petroleum naphtha as a raw material, and tris(2,4-di-t-butylphenyl)phosphite, a phosphorus-based antioxidant. Petroleum PP (B1): Polypropylene 99.16% by mass, phosphorus-based antioxidant 0.04% by mass, additives other than phosphorus-based antioxidants 0.80% by mass. Petroleum PP (B2): 99.17% by mass of polypropylene, 0.03% by mass of phosphorus-based antioxidant, 0.80% by mass of additives other than phosphorus-based antioxidants. The following Petroleum PP (B3) is a resin composition that contains an ethylene-propylene-1-butene copolymer derived from petroleum raw materials and tris(2,4-di-t-butylphenyl)phosphite, which is a phosphorus-based antioxidant, but does not contain an anti-fogging agent. Petroleum PP (B3): 99.65% by mass of ethylene-propylene-1-butene copolymer, 0.10% by mass of phosphorus-based antioxidant, 0.25% by mass of additives other than phosphorus-based antioxidant.

[0042] [Anti-fogging agent] Anti-fogging agent (C1): A mixture of 30% by mass of glycerin fatty acid ester, 20% by mass of alkyldiethanolamine, and 50% by mass of alkyldiethanolamine fatty acid ester.

[0043] <Example 1> An anti-fog film was produced using the raw material composition shown in Table 1. Using three extruders, the raw material composition for the core layer, the raw material composition for the first skin layer, and the raw material composition for the second skin layer were melt-kneaded at 230°C by each extruder, and the three layers were co-extruded so that the thickness ratio of the first skin layer / core layer / second skin layer was 5 / 90 / 5 to obtain a laminated sheet. The raw material composition for the core layer was a mixture of petroleum PP (B1), bio-PP (A1), and anti-fog agent (C1). The laminated sheet was cooled by contacting with a roll at 30°C, stretched longitudinally at 4.7 times at 140°C, and then stretched transversely at 10 times at 165°C. The first skin layer was subjected to a corona treatment to give a thickness of 30 µm and a density of 0.9 g / cm. 3 A biaxially oriented polypropylene film (anti-fogging film) was obtained. In this example, the content of the bionaphtha-derived P unit is 10 mass %, the content of the anti-fogging agent is 0.5 mass %, and the content of the phosphorus-based antioxidant is 340 ppm, relative to the mass of the polypropylene film.

[0044] <Example 2> A biaxially oriented polypropylene film was produced in the same manner as in Example 1, except that the raw material composition was changed so that the content of bionaphtha-derived P units was 25 mass%.

[0045] <Example 3> A biaxially oriented polypropylene film was produced in the same manner as in Example 1, except that both the first skin layer and the second skin layer were simultaneously subjected to corona treatment.

[0046] <Comparative Example 1> A biaxially oriented polypropylene film was produced in the same manner as in Example 1, except that the raw material composition was changed so that the content of the phosphorus-based antioxidant was 230 ppm.

[0047] <Comparative Example 2> A biaxially oriented polypropylene film was produced in the same manner as in Example 1, except that the raw material composition was changed so that the content of the phosphorus-based antioxidant was 1570 ppm.

[0048] <Comparative Example 3> A biaxially oriented polypropylene film was produced in the same manner as in Example 1, except that the raw material composition was changed so that the content of bionaphtha-derived P units was 0%.

[0049] <Evaluation> The polypropylene films obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were evaluated for the items shown in the tables. The results are shown in Table 1.

[0050] [Table 1]

[0051] As shown in the above results, the polypropylene films of Examples 1 to 3 had anti-fogging properties, low environmental impact, and small changes in color, mechanical properties, and transparency over time. In particular, Example 3, in which the polypropylene film was subjected to corona treatment on both sides, had anti-fogging properties on both sides. On the other hand, the polypropylene film of Comparative Example 1 had anti-fogging properties and a small environmental impact, but the color and mechanical properties changed significantly over time, raising concerns about problems in use. The polypropylene film of Comparative Example 2 had anti-fogging properties, a small environmental load, and little change in color and mechanical properties over time, but the transparency deteriorated over time. The polypropylene film of Comparative Example 3 had anti-fogging properties and showed little change in color, mechanical properties, and transparency over time, but had a large environmental impact because it did not use bionaphtha-derived polypropylene as a raw material. [Industrial Applicability]

[0052] The polypropylene film of the present invention is an excellent anti-fog film that has anti-fog properties, reduces the amount of petrochemical materials used, and is less susceptible to deterioration in color and strength over time, and is useful as an excellent packaging material.

Claims

1. An anti-fog film comprising polypropylene produced using propylene derived from bionaphtha and an anti-fog agent, the anti-fog film containing, relative to the mass of the anti-fog film, 10% by mass or more and 50% by mass or less of units based on the propylene derived from the bionaphtha, 0.3% by mass or more and 1.0% by mass or less of the anti-fog agent, and 300 ppm by mass or more and 1,000 ppm by mass or less of a phosphorus-based antioxidant.

2. 2. The anti-fog film of claim 1, wherein the phosphorus-based antioxidant comprises tris(2,4-di-t-butylphenyl)phosphite.

3. A laminate comprising a plurality of layers, at least one of which comprises the anti-fog film according to claim 1 or 2.

4. A packaging material comprising the anti-fog film according to claim 1 or 2.

5. A package in which an article is packaged with the packaging material according to claim 4.

Citation Information

Patent Citations

  • Antifogging film for food packaging

    JP1990219839A

  • Polypropylene resin composition and film made by using it

    JP1996081588A

  • Polyolefin resin composition and film made of the same

    JP2002069248A

  • Polypropylene based antifogging film

    JP2006231899A

  • Packaging film and package

    JP2008114514A