Heat-shrinkable polyester-based film, heat-shrinkable label, and package

A heat-shrinkable polyester film with specific chemical and thermal properties ensures compatibility with PET bottles, addressing recycling issues by maintaining transparency and preventing pulsation in recycled PET resin production.

JP2024149713AActive Publication Date: 2024-10-18TOYOBO CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024131644
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-08-27
Filing Date
2024-08-08
Publication Date
2024-10-18
Estimated Expiration
2041-08-19

AI Technical Summary

Technical Problem

Conventional heat-shrinkable polyester films are not compatible with PET bottles, leading to issues such as loss of transparency and difficulty in recycling due to differences in crystallinity and material composition, causing problems like pulsation during the production of recycled PET resin.

Method used

A heat-shrinkable polyester film composed of 95 mol% or more dicarboxylic acid, 0-5 mol% isophthalic acid, 85-98 mol% ethylene terephthalate units, and 2-15 mol% diethylene glycol, with specific thermal shrinkage and crystallization properties, ensuring compatibility with PET bottles.

Benefits of technology

The film maintains high heat-shrinkage rates and compatibility with PET bottles, allowing for the production of high-quality recycled PET resin without impairing transparency or causing pulsation during the recycling process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149713000005
    Figure 2024149713000005
  • Figure 2024149713000006
    Figure 2024149713000006
  • Figure 2024149713000001
    Figure 2024149713000001
Patent Text Reader

Abstract

To provide a heat-shrinkable polyester-based film that has a high heat shrinkage rate in the main shrinkage direction and can be recycled together with used beverage plastic bottles to obtain good recycled PET resin.SOLUTION: A heat-shrinkable polyester-based film contains: in 100 mol% of the dicarboxylic acid component, dicarboxylic acid of 95 mol% or more and 100 mol% or less and isophthalic acid of 0 mol% or more and 5 mol% or less; in a total ester unit 100 mol%, an ethylene terephthalate unit of 85 mol% or more and 98 mol% or less; and in 100 mol% of a polyhydric alcohol component, diethylene glycol of 2 mol% or more and 15 mol% or less. heat-shrinkable polyester-based film having a predetermined hot water heat shrinkage rate, melts the film using a differential scanning calorimeter (DSC), and then quenches and heats the same again, and a melting peak temperature, a crystallization calorific value, and a melting calorimetric value are measured and all of these fall within a predetermined range.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a heat-shrinkable polyester film, and more particularly to a heat-shrinkable polyester film, a heat-shrinkable label, and a packaging material that can be mixed with PET bottles in the PET bottle recycling process to produce recycled PET resin that can be recycled without any problems. [Background technology]

[0002] In recent years, stretched films (so-called heat-shrinkable films) made of polyvinyl chloride resins, polystyrene resins, polyester resins, etc. have been widely used for label packaging, cap seals, and integrated packaging that serve to protect glass bottles, PET bottles, etc. and display products. Among such heat-shrinkable films, polyvinyl chloride films have problems such as low heat resistance, generation of hydrogen chloride gas when incinerated, and dioxin generation. In addition, polystyrene films have poor solvent resistance, and inks with special compositions must be used for printing, and they must be incinerated at high temperatures, which causes problems such as a large amount of black smoke accompanied by an unpleasant odor when incinerated. Therefore, polyester heat-shrinkable films, which have high heat resistance, are easy to incinerate, and have excellent solvent resistance, have been widely used as shrink labels, and their usage tends to increase with the increase in the distribution volume of PET containers.

[0003] Normal heat-shrinkable polyester films that shrink significantly in the width direction are widely used. The film is stretched by a tenter stretching method or the like to produce a wide master roll, which is then slit to any width and wound into a roll of any length to produce a film roll product. The film is given a design and is then printed in roll form for the purpose of product display. After printing, the film is slit again to the required width and wound into a roll, after which it is center-sealed by solvent bonding, made into a tube, and wound into a roll (to become a label roll).

[0004] The labels are made into tubular bags and wound up, then cut to the required length as they are unwound from the roll to become ring-shaped labels. The ring-shaped labels are attached to the packaged items by hand or other methods, and passed through a steam tunnel or hot air tunnel to shrink them and become labels.

[0005] In recent years, the demand for environmental protection has been growing. For example, PET bottle containers are recycled, regenerated as recycled PET resin, and used in various plastic products. Due to the growing demand for environmental protection, the amount of recycled PET resin used is increasing, and the recycling rate of PET bottles is also increasing.

[0006] PET beverage bottles are recycled once their contents have been emptied into recycled PET resin, but the labels that give the beverage bottles their decorative design are generally not recycled. The polystyrene-based heat-shrinkable film label described in Patent Document 1 is incompatible with PET, the raw material for PET bottles. Therefore, if polystyrene-based heat-shrinkable film is mixed in the process of making recycled PET resin, the transparency of the recycled PET resin will be lost, which is undesirable. The laminated film of polyester and polystyrene described in Patent Document 2 is also undesirable because it contains polystyrene, which is incompatible with PET, in the mixture. Patent Document 3 is an invention of a polyester-based heat-shrinkable film, but cyclic olefins and the like are mixed in to create voids, and as with the above, olefin-based raw materials that are incompatible with PET are mixed in, which is undesirable.

[0007] Patent Document 4 is an invention of a transparent polyester-based heat shrinkable film, which does not contain any raw materials that are incompatible with PET, so the transparency is not lost in the process of making recycled PET resin. However, polyester-based heat shrinkable films are generally produced from amorphous PET raw materials to which amorphous monomers have been added to express heat shrink properties. The raw materials used in PET bottles are homo-PET, which is a crystalline raw material. Therefore, if amorphous polyester-based heat shrinkable films are mixed in the process of making recycled PET resin, it becomes difficult to reuse the resulting recycled PET resin as a homo-PET raw material, and it cannot be used as a raw material to make PET bottles again. In addition, since the densities of crystalline and amorphous raw materials are different, in the process of mixing the two raw materials to make recycled resin, the amorphous raw material is not extruded uniformly, and problems such as pulsation and tow breakage are likely to occur in the die after melt extrusion, which is undesirable. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 5286763 [Patent Document 2] International Publication No. WO2020 / 021948 [Patent Document 3] Patent No. 5625912 [Patent Document 4] Patent No. 5633808 Summary of the Invention [Problem to be solved by the invention]

[0009] The heat-shrinkable polyester film of the present invention has a high heat shrinkage rate in the main shrinkage direction, and also has an objective of providing a heat-shrinkable polyester film which, even when recycled together with used PET beverage bottles, can yield good recycled PET resin. [Means for solving the problem]

[0010] The present invention, which has solved the above problems, has the following configuration. 1. A heat-shrinkable polyester film containing 95 mol% or more and 100 mol% or less of dicarboxylic acid and 0 mol% or more and 5 mol% or less of isophthalic acid out of 100 mol% of dicarboxylic acid components, and containing 85 mol% or more and 98 mol% or less of ethylene terephthalate units out of 100 mol% of all ester units, and containing 2 mol% or more and 15 mol% or less of diethylene glycol out of 100 mol% of polyhydric alcohol components, wherein the heat-shrinkable polyester film satisfies the following requirements (1) to (5): (1) When the film is immersed in 90°C hot water for 10 seconds, the hot water shrinkage rate is 40% or more and 70% or less in the width direction of the film. (2) When the film is immersed in 90°C hot water for 10 seconds, the hot water heat shrinkage rate is between -5% and 15% in the longitudinal direction of the film. (3) Using a differential scanning calorimeter (DSC), the film is heated to 300°C, melted, then rapidly cooled, and heated again to 300°C. The endothermic peak temperature due to melting is 245°C or higher and 260°C or lower. (4) Using a differential scanning calorimeter (DSC), the film is heated to 300°C, melted, then rapidly cooled, and heated again to 300°C, resulting in crystallization with a heat generation of 10 mJ / mg or more. (5) Using a differential scanning calorimeter (DSC), the film is heated to 300°C, melted, then rapidly cooled, and heated again to 300°C. The amount of heat absorbed by melting is 10 mJ / mg or more. 2. The film density is 1.33g / cm 3 More than 1.39g / cm 3 1. The heat-shrinkable polyester film according to 1., characterized in that: 3. The heat-shrinkable polyester film according to 1 or 2, characterized in that the haze at a film thickness of 20 μm is 2% or more and 10% or less. 4. A heat-shrinkable label using the heat-shrinkable polyester film described in any one of 1. to 3. 5. A package formed by covering at least a part of the outer periphery of an object to be packaged with the heat-shrinkable label described in 4. above and then heat-shrinking it. 6. The heat-shrinkable polyester film according to any one of 1. to 3. above, which is used for a heat-shrinkable label and then used as a raw material for recycling PET bottles. Effect of the Invention

[0011] The heat-shrinkable polyester film of the present invention has a high heat shrinkage rate in the main shrinkage direction, and the raw material components used are similar to those used in PET beverage bottles. In addition, the melting point, heat generation amount, and heat absorption amount of the film measured by a differential scanning calorimeter (hereinafter sometimes referred to as DSC) are similar to those of the raw materials used in PET bottles. Therefore, recycled PET resin can be obtained even if the heat-shrinkable polyester film is recycled at the same time as PET bottles. [Brief description of the drawings]

[0012] [Figure 1] 1 shows an example of measurement of the endothermic peak temperature, the amount of heat generated by crystallization, and the amount of heat absorbed by melting of a film using DSC in the present invention. [Diagram 2] 1 is an example (top view) of a TD (transverse direction stretching) pattern in a process for producing a heat-shrinkable polyester film of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The heat-shrinkable polyester film of the present invention will be described in detail below. The manufacturing method of the heat-shrinkable polyester film will be described in detail later, but the heat-shrinkable film is usually obtained by conveying and stretching the film using rolls or the like. In this case, the conveying direction of the film is called the longitudinal direction, and the direction perpendicular to the longitudinal direction is called the film width direction. Therefore, the width direction of the heat-shrinkable polyester film shown below is the direction perpendicular to the roll unwinding direction, and the film longitudinal direction is the direction parallel to the roll unwinding direction.

[0014] The heat-shrinkable polyester film of the present invention is a heat-shrinkable polyester film that contains 85 mol% or more and 98 mol% or less of ethylene terephthalate units out of 100 mol% of all ester units, contains 95 mol% or more and 100 mol% or less of dicarboxylic acid and 0 mol% or more and 5 mol% or less of isophthalic acid out of 100 mol% of dicarboxylic acid components, and contains 2 mol% or more and 15 mol% or less of diethylene glycol out of 100 mol% of polyhydric alcohol components, and is characterized in that the heat-shrinkable polyester film satisfies the following requirements (1) to (5). (1) When the film is immersed in 90°C hot water for 10 seconds, the hot water shrinkage rate is 40% or more and 70% or less in the width direction of the film. (2) When the film is immersed in 90°C hot water for 10 seconds, the hot water heat shrinkage rate is between -5% and 15% in the longitudinal direction of the film. (3) Using a differential scanning calorimeter (DSC), the film is heated to 300°C, melted, then rapidly cooled, and heated again to 300°C. The endothermic peak temperature due to melting is 245°C or higher and 260°C or lower. (4) Using a differential scanning calorimeter (DSC), the film is heated to 300°C, melted, then rapidly cooled, and heated again to 300°C, resulting in crystallization with a heat generation of 10 mJ / mg or more. (5) Using a differential scanning calorimeter (DSC), the film is heated to 300°C, melted, then rapidly cooled, and heated again to 300°C. The amount of heat absorbed by melting is 10 mJ / mg or more.

[0015] The present inventor analyzed the raw material composition of commercially available PET beverage bottles (PET beverage bottles sold by Coca-Cola, Suntory, Itoen, Kirin, and Asahi) using 1H-NMR (varian, UNITY50). Of 100 mol% of dicarboxylic acid components, 97-98.5 mol% of dicarboxylic acid and 1.5-3 mol% of isophthalic acid were contained. In addition, of 100 mol% of ester units, 97-99 mol% of ethylene terephthalate units were contained, and of 100 mol% of polyhydric alcohol components, 1-3 mol% of diethylene glycol was contained. It is believed that isophthalic acid is intentionally added to prevent whitening of the neck of the PET bottle during PET bottle molding. Diethylene glycol is believed to be a by-product during raw material polymerization.

[0016] Therefore, for the heat-shrinkable polyester film, a raw material containing only dicarboxylic acid and isophthalic acid as dicarboxylic acid components and only ethylene terephthalate units and diethylene glycol as ester units is preferable because it makes recycling with PET bottles easier. The weight ratio of the PET bottle to the label was also compared using a 500ml PET beverage bottle. The weight ratio of the label was low, ranging from 0.05 to 0.2, assuming that the PET bottle was 1. Thus, the inventors found that, even though the weight ratio of the label is low when the PET bottle and the label are mixed and recycled, the composition and characteristics of the label are factors that cause fluctuations in the resin size and the like during the recycling process.

[0017] In order to obtain high shrinkability in heat-shrinkable polyester films, it is common to copolymerize other polyvalent carboxylic acid components or other polyhydric alcohol components with homopolymers (PET) made of, for example, ethylene terephthalate. As polyhydric alcohol components to be used as copolymerized components, for example, neopentyl glycol and 1,4-cyclohexanediethanol are considered and widely used. In the case of films copolymerized with these components, the raw material composition is different from the raw material of the above-mentioned PET bottles for beverages, and therefore the recyclability with PET bottles is poor, which is undesirable.

[0018] As a polymerization method for polyethylene terephthalate (hereinafter, sometimes simply referred to as PET), any production method can be used, such as a direct polymerization method in which terephthalic acid is directly reacted with ethylene glycol, and, if necessary, other dicarboxylic acid components and diol components, and an ester exchange method in which a dimethyl ester of terephthalic acid (containing, if necessary, a methyl ester of another dicarboxylic acid) is subjected to an ester exchange reaction with ethylene glycol (containing, if necessary, another diol component).

[0019] Examples of dicarboxylic acid components other than terephthalic acid that constitute polyester include aromatic dicarboxylic acids such as isophthalic acid, naphthalenedicarboxylic acid, and orthophthalic acid, aliphatic dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, and decanedicarboxylic acid, and alicyclic dicarboxylic acids. In the heat-shrinkable polyester film of the present invention, it is preferable to use isophthalic acid, which is the same component as the raw material of PET bottles. The content of the isophthalic acid component is 0 mol% or more, preferably 1 mol% or more, out of 100 mol% of the polyvalent carboxylic acid component, and more preferably 1.5 mol% or more, which is the same composition as the raw material of PET bottles. At the upper limit, since the weight of the label is 5 to 20% of the PET bottle, 15 mol%, which is 5 times the content of isophthalic acid in the PET bottle, is not preferable. Isophthalic acid is amorphous, and if there is a large amount of isophthalic acid, the amorphousness becomes high, which is not preferable because problems such as pulsation occur when mixing with PET bottles to prepare recycled PET raw materials. The content of isophthalic acid is 5 mol % or less, preferably 4 mol % or less, and more preferably 3 mol % or less, the same as that of the raw material for PET bottles.

[0020] It is necessary that diethylene glycol accounts for 2 mol % or more and 15 mol % or less of 100 mol % of the polyhydric alcohol component constituting the polyester used in the film of the present invention. If the diethylene glycol content is less than 2 mol %, it is not preferable since it becomes difficult to exhibit the shrinkage properties required for a heat shrinkable film.The diethylene glycol content is preferably 3 mol % or more, and more preferably 4 mol % or more. On the other hand, as mentioned above, the upper limit is 5-20% of the label weight of the PET bottle. Therefore, even if it is mixed with the PET bottle in the recycling process, the diethylene glycol will be 1 / 5-1 / 20 or less. As mentioned above, the diethylene glycol contained in the raw material of the PET bottle is 1-3 mol%, so if the diethylene glycol in the recycled PET resin is 15 mol% or less, it will be within the range of diethylene glycol in PET bottle resin when it becomes recycled PET resin. Diethylene glycol is preferably 13 mol% or less, and more preferably 11 mol% or less.

[0021] It is preferable not to contain a diol having 8 or more carbon atoms (e.g., octanediol, etc.) or a polyhydric alcohol having a valence of 3 or more (e.g., trimethylolpropane, trimeritolethane, glycerin, diglycerin, etc.). A heat-shrinkable polyester film obtained using a polyester containing such a diol or polyhydric alcohol is difficult to achieve the required high shrinkage.

[0022] Various additives, such as waxes, antioxidants, antistatic agents, crystal nucleating agents, viscosity reducers, heat stabilizers, coloring pigments, coloring inhibitors, and ultraviolet absorbers, may be added to the resin forming the heat-shrinkable polyester film of the present invention, as necessary.

[0023] In the resin forming the heat-shrinkable polyester film of the present invention, it is preferable to add fine particles as a lubricant to improve the workability (slipperiness) of the film. Any fine particles can be selected, but for example, inorganic fine particles can be silica, alumina, titanium dioxide, calcium carbonate, kaolin, barium sulfate, etc., and organic fine particles can be acrylic resin particles, melamine resin particles, silicone resin particles, crosslinked polystyrene particles, etc. The average particle size of the fine particles can be appropriately selected as needed within the range of 0.05 to 3.0 μm (measured with a Coulter counter).

[0024] The method of blending the above particles into the resin forming the heat-shrinkable polyester film can be, for example, addition at any stage of the production of the polyester resin, but it is preferable to add the particles as a slurry dispersed in ethylene glycol or the like at the stage of esterification or after the completion of the transesterification reaction and before the start of the polycondensation reaction, and proceed with the polycondensation reaction. It is also preferable to blend a slurry of the particles dispersed in ethylene glycol or water or the like with the polyester resin raw material using a vented kneading extruder, or to blend the dried particles with the polyester resin raw material using a kneading extruder.

[0025] It is preferable that the heat shrinkable polyester film of the present invention, when treated in 90°C hot water for 10 seconds under no load, has a heat shrinkage rate in the main shrinkage direction of the film (i.e., hot water heat shrinkage rate at 90°C) calculated from the lengths before and after shrinkage according to the following formula 1 of 40% or more and 70% or less. Heat shrinkage rate = {(length before shrinkage - length after shrinkage) / length before shrinkage} × 100 (%) Formula 1

[0026] If the hot water shrinkage rate in the main shrinkage direction at 90°C is less than 40%, when the film is used for beverage labels or lunch box packaging, the shrinkage amount is small, which is undesirable because it causes label wrinkles and sagging after heat shrinkage. The hot water shrinkage rate at 90°C is more preferably 43% or more, particularly preferably 46% or more, and most preferably 50% or more. There is no problem if the hot water heat shrinkage rate in the main shrinkage direction at 90°C is higher than 70%, but in the present invention, it was not possible to obtain a film with a hot water heat shrinkage rate at 90°C of higher than 70%, so the upper limit was set at 70%.

[0027] The heat-shrinkable polyester film of the present invention preferably has a hot water shrinkage rate at 90°C in the longitudinal direction perpendicular to the main shrinkage direction of -5% to 15%. If the hot water shrinkage rate at 90°C in the longitudinal direction is less than -5%, when used for beverage labeling, the label will stretch and the label height on the PET bottle will be increased, which is not preferable. The hot water shrinkage rate at 90°C in the longitudinal direction is more preferably -4% or more, and particularly preferably -3% or more. If the hot water shrinkage rate at 90°C in the longitudinal direction is more than 15%, when used for beverage labeling, the label will shrink and the label height on the PET bottle will be shortened, which is undesirable. It may also cause distortion of the label after shrinkage. The hot water shrinkage rate at 90°C in the longitudinal direction is more preferably 13% or less, even more preferably 11% or less, particularly preferably 8% or less, and most preferably 5% or less.

[0028] The heat-shrinkable polyester film of the present invention is preferably heated to 300°C using a differential scanning calorimeter (hereinafter referred to as DSC) to melt, cooled, and then heated again to 300°C, and the endothermic peak temperature due to melting is preferably 245°C to 260°C. When a PET bottle was measured by the same method, the peak of the heat of fusion was in the range of 250 to 260°C. Therefore, if the peak of the heat of fusion is significantly different from that of a PET bottle, problems such as pulsation will occur in the melt extrusion process when producing a recycled PET resin, which is not preferable. It is more preferable that the temperature is 247°C to 260°C, and particularly preferable that the temperature is 250°C to 255°C.

[0029] The heat shrinkable polyester film of the present invention is heated to 300°C using a DSC to melt it, then cooled and heated again to 300°C to obtain a heat generation amount due to crystallization of preferably 10 mJ / mg or more. When a PET bottle was measured using the same method, the heat generation amount was in the range of 25 to 55 mJ / mg. If the amorphous amount of the heat shrinkable polyester film is high, it does not show a heat generation amount, and therefore, when producing a recycled PET resin, problems such as pulsation occur in the melt extrusion process, which is not preferable. Therefore, the amount of heat generated by crystallization is preferably 10 mJ / mg or more, more preferably 20 mJ / mg or more, and particularly preferably 25 mJ / mg or more. There is no specific upper limit on the amount of heat generated by crystallization, but it will not exceed 60 mJ / mg for polyester raw materials.

[0030] The heat shrinkable polyester film of the present invention is preferably endothermic by melting, which is obtained by heating to 300°C using a DSC, cooling, and then heating to 300°C again, of 10 mJ / mg or more. When a PET bottle is measured by the same method, the endothermic amount is in the range of 30 to 65 mJ / mg. If the amorphous content of the heat shrinkable polyester film is high, it does not show an endothermic amount, and therefore problems such as pulsation occur in the melt extrusion process when producing recycled PET resin, which is not preferable. Therefore, the amount of heat absorbed by melting is preferably 10 mJ / mg or more, more preferably 20 mJ / mg or more, and particularly preferably 30 mJ / mg or more. There is no particular upper limit for the amount of heat absorbed by melting, but for polyester raw materials, it will not exceed 70 mJ / mg.

[0031] The heat-shrinkable polyester film of the present invention has a density of 1.33 g / cm 3 It is preferable that the density is equal to or higher than the above. Many reports have been made on the density as an index of the degree of crystallinity. Therefore, a low density indicates low crystallinity and a large amount of amorphous matter. Density is 1.33g / cm 3 If it is less than 1.34 g / cm, problems such as pulsation will occur during the melt extrusion process when producing recycled PET resin, which is not preferable. 3 More preferably, it is 1.35 g / cm or more. 3 More preferably, it is equal to or greater than this. On the other hand, if the density is too high, it will crystallize and the shrinkage characteristics described above will not be obtained, which is not preferable. 3 More preferably, it is 1.37 g / cm or less. 3 It is particularly preferred that:

[0032] The thickness of the heat-shrinkable polyester film of the present invention is not particularly limited, but is preferably 15 to 50 μm for use as a heat-shrinkable film for label applications or lunch box packaging applications. If the film thickness is less than 15 μm, the stiffness of the film is significantly reduced, which is undesirable since the roll is prone to wrinkles. On the other hand, even if the film thickness is thick, there is no problem as a film roll, but it is preferable to make the film thinner from the viewpoint of cost. The film thickness is more preferably 17 to 45 μm, and particularly preferably 20 to 40 μm.

[0033] The heat-shrinkable polyester film of the present invention preferably has a haze value of 2% or more and 10% or less at a thickness of 20 μm. Since the heat-shrinkable film is a film that provides design, if the haze value is higher than 10%, the contents will not be clearly visible when the film is used as a label for a PET bottle, and the design will be reduced, which is not preferable. The haze value at a film thickness of 20 μm is more preferably 8% or less, and particularly preferably 6% or less. Although there is no problem with a haze of less than 2% when the film thickness is 20 μm, in the present invention, when the haze value is less than 2%, the slipperiness of the film deteriorates, so the lower limit is set to 2%.

[0034] The heat-shrinkable polyester film of the present invention can be obtained by melt-extruding the above-mentioned polyester raw material with an extruder to form an unstretched film, and then stretching the unstretched film in the width direction. The polyester can be obtained by polycondensing the above-mentioned suitable dicarboxylic acid component and diol component by a known method. In addition, chip-shaped polyester is usually used as the raw material for the film.

[0035] When melt extruding the raw resin, it is preferable to dry the polyester raw material using a dryer such as a hopper dryer or a paddle dryer, or a vacuum dryer. After drying the polyester raw material in this way, it is melted at a temperature of 230 to 270°C and extruded into a film using an extruder. For extrusion, any existing method such as a T-die method or a tubular method can be used.

[0036] The extruded sheet-like molten resin can then be quenched to obtain an unstretched film. As a method for quenching the molten resin, a method in which the molten resin is cast from a die onto a rotating drum and rapidly cooled and solidified to obtain a substantially unoriented resin sheet can be suitably adopted.

[0037] The unstretched film thus obtained can be stretched in the width direction under predetermined conditions to obtain the heat-shrinkable polyester film of the present invention. Preferred stretching methods for obtaining the heat-shrinkable polyester film of the present invention are described below.

[0038] A typical heat-shrinkable polyester film is produced by stretching an unstretched film in the direction in which it is desired to shrink. In the present invention, the film is biaxially stretched within the range of the stretch ratio described below, since stretching in the longitudinal direction also increases the production speed and improves productivity.

[0039] It is preferable to perform the longitudinal stretching by roll stretching using rolls with different speeds. The rolls are preheated with a surface temperature of Tg or higher and Tg+20°C or lower, and stretched at a ratio of 1.1 to 1.3 times. If the surface temperature is below Tg, the stretching stress becomes high and the film breaks, which is not preferable. Also, if the temperature is higher than Tg+20°C, the film will stick to the roll, which may cause scratches on the film, which is not preferable. The roll surface temperature is preferably Tg+3°C or higher and Tg+17°C or lower, and particularly preferably Tg+5°C or higher and Tg+15°C or lower. A stretching ratio of less than 1.1 times is not preferable because the improvement in productivity is small. A stretching ratio of 1.15 times or more is preferable, and 1.2 times or more is particularly preferable. A stretching ratio in the longitudinal direction of more than 1.3 times is not preferable because the shrinkage rate in the longitudinal direction becomes high. A stretching ratio of 1.28 times or less is preferable, and 1.25 times or less is particularly preferable.

[0040] For widthwise stretching, the film stretched in the longitudinal direction is introduced into a tenter device capable of heating the film by holding both ends of the film with clips, and the film is heated to a predetermined temperature with hot air. After that, the film is stretched by increasing the distance between the clips while being transported in the longitudinal direction. The preheating temperature of the longitudinally stretched film is preferably Tg+30°C or more +80°C or less. If it is less than Tg+30°C, the preheating temperature is insufficient, which increases the stretching force and makes the film more likely to break, which is not preferred. If it is heated at a temperature higher than Tg+80°C, the stretching force in the width direction of the unstretched sheet decreases, which is not preferred because it worsens the thickness accuracy (thickness deviation) in the width direction. More preferably, it is Tg+40°C or more +70°C or less.

[0041] The film temperature during widthwise stretching is preferably Tg+5°C or more and Tg+30°C or less. If the film temperature is less than Tg+5°C, the stretching force becomes too high, which is undesirable as the film is prone to breakage. If the film temperature exceeds Tg+30°C, the stretching force is too low, which is undesirable as the thermal shrinkage in the widthwise direction measured at 90°C as described above becomes low. More preferably, the film temperature is Tg+8°C or more and Tg+25°C or less.

[0042] The stretching ratio in the width direction is preferably 3.4 times or more and 5 times or less. If the stretching ratio is less than 3.4 times, the stretching force is insufficient, and the thickness accuracy in the width direction of the film (so-called uneven thickness) is deteriorated. If the stretching ratio exceeds 5 times, the risk of breakage during film production increases and the equipment becomes long and large, which is not preferable. More preferably, it is 3.5 times or more and 4.8 times or less. Although not particularly limited, after stretching in the width direction, heat treatment may be performed to adjust the shrinkage rate.

[0043] When stretching in the width direction, it is preferable to stretch in two or more stages. In the present invention, a crystalline polyester raw material is weakly stretched in the longitudinal direction, and then the film is stretched in the width direction. It is common that the molecules of the film are oriented in the stretching direction, and the molecular orientation in the direction perpendicular to the stretching direction is reduced. Therefore, by first stretching in the width direction at a low stretching ratio of 1.2 to 1.7 times, the molecular orientation in the longitudinal direction of the film can be reduced, and the thermal shrinkage rate in the longitudinal direction can be reduced. Furthermore, if the film is relaxed in the width direction by 5% to 20% in the width direction in a tenter device (so-called TD relaxation), the molecules in the longitudinal direction are also relaxed, and the effect of reducing the thermal shrinkage rate in the longitudinal direction is increased. It is preferable that the film is made to a fixed length in the tenter device after relaxation in the width direction, and then the second stage of stretching is performed at 2 to 4.2 times. After the second stage stretching, it is preferable to heat treat the film in a tenter device at a temperature between the stretching temperature and stretching temperature +18°C. If the heat treatment temperature is lower than the stretching temperature, the purpose of the heat treatment step, which is to relax the molecular chains, will not be achieved. If the heat treatment temperature is higher than the stretching temperature +18°C, the heat shrinkage rate will decrease, which is not preferable for a heat shrinkable film. More preferably, it is between the stretching temperature +1°C and stretching temperature +15°C. EXAMPLES

[0044] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the embodiments of the examples, and can be modified as appropriate without departing from the spirit of the present invention.

[0045] The film was evaluated as follows.

[0046] [Intrinsic viscosity (IV)] 0.2 g of polyester was dissolved in 50 ml of a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (60 / 40 (weight ratio)), and the viscosity was measured using an Ostwald viscometer at 30° C. The unit is dl / g.

[0047] [Composition analysis] Each sample was dissolved in a solvent in which chloroform D (manufactured by Eurisopp) and trifluoroacetic acid D1 (manufactured by Eurisopp) were mixed at a ratio of 10:1 (volume ratio) to prepare a sample solution, and the NMR of the protons in the sample solution was measured using an NMR "GEMINI-200" (manufactured by Varian) at a temperature of 23°C and an accumulation number of 64. In the NMR measurement, the peak intensity of a specified proton was calculated, and the amount of the component in 100 mol% of the diacid component and the amount of the component in 100 mol% of the polyhydric alcohol component were measured.

[0048] [Heat shrinkage rate (hot water heat shrinkage rate)] The film was cut into a 10 cm x 10 cm square and immersed in warm water of a specified temperature ±0.5°C for 10 seconds without load to allow it to shrink, then immersed in water at 25°C ±0.5°C for 10 seconds and pulled out of the water to measure the longitudinal and transverse dimensions of the film, and the thermal shrinkage rate was calculated according to the following formula (1). The direction with the largest thermal shrinkage rate was determined as the main shrinkage direction. Heat shrinkage rate = {(length before shrinkage - length after shrinkage) / length before shrinkage} x 100 (%) Formula 1

[0049] [Tg (glass transition temperature)] Tg was determined according to JIS-K7121-1987 using a differential scanning calorimeter (model: DSC220) manufactured by Seiko Electronics Co., Ltd. In detail, 10 mg of unstretched film was heated from -40°C to 120°C at a heating rate of 10°C / min, and an endothermic curve was measured. Tangent lines were drawn before and after the inflection point of the obtained endothermic curve, and the intersection point was determined as the glass transition point (Tg; °C).

[0050] [Endothermic peak temperature][Amount of heat absorbed] The calorific value was determined according to JIS-K7121-1987 using a differential scanning calorimeter (model: DSC220) manufactured by Seiko Electronics Co., Ltd. 5 mg of the film after film formation was placed in a sample pan, the pan was covered, and the temperature was raised to 300°C at a heating rate of 10°C / min under a nitrogen gas atmosphere, and the temperature was maintained at 300°C for 2 minutes after the temperature was raised. The sample pan was then removed and quenched with liquid nitrogen. The sample after quenching was returned to room temperature, and again heated to 30°C to 300°C at a heating rate of 10°C / min using a differential scanning calorimeter, and DSC was measured. The endothermic peak at which the sample melted was taken as the endothermic peak temperature. The endothermic amount of melting was also determined from the endothermic peak area. If there was no melting peak, there was no melting peak temperature and the endothermic amount was taken as 0.

[0051] [Heat output] The calorific value was determined according to JIS-K7121-1987 using a differential scanning calorimeter (model: DSC220) manufactured by Seiko Denshi Kogyo Co., Ltd. 5 mg of the film after film formation was placed in a sample pan, the pan was covered, and the temperature was raised to 300°C at a heating rate of 10°C / min under a nitrogen gas atmosphere, and the temperature was maintained at 300°C for 2 minutes after the temperature was raised. The sample pan was then removed and quenched with liquid nitrogen. The sample after quenching was returned to room temperature, and again heated to 30°C to 300°C at a heating rate of 10°C / min using a differential scanning calorimeter, and DSC was measured. The calorific value was determined from the area of ​​the exothermic peak where the sample was heated. If there was no exothermic peak, there was no exothermic peak temperature, and the calorific value was set to 0.

[0052] [Film thickness] The measurement was performed using a dial gauge in accordance with JIS K7130-1999 Method A.

[0053] [Film Density] The density of a sample approximately 3 mm square was measured using an aqueous calcium nitrate solution according to the density gradient tube method of JIS-K-7112.

[0054] [Film Haze] In accordance with JIS K7361-1, the film was cut into a square shape with each side being 10 cm long, and the haze was measured using a haze meter NDH2000 manufactured by Nippon Denshoku Co., Ltd. Measurements were performed at three locations, and the average value was taken as the actual haze measurement value, and the haze converted into 20 μm was calculated using the following formula (2). Haze = measured haze value x 20 / film thickness (% / 20μm) Formula 2

[0055] [Shrinkage finish] The ends of the heat-shrinkable film were welded with an impulse sealer (manufactured by Fuji Impulse Co., Ltd.) to obtain a cylindrical label with the width direction as the circumferential direction. The diameter of the label in the shrink direction was 68 mm. This label was placed on a commercially available 500 ml PET bottle (containing contents; body diameter 62 mm, minimum diameter of neck 25 mm) and heat-shrunk by passing through steam using a steam tunnel (model: SH-1500-L) manufactured by Fuji Astec Inc. adjusted to 90°C (tunnel passing time: 5 seconds). The shrink finish of the label was visually evaluated according to the following criteria. It was visually evaluated on a 5-point scale according to the following criteria. The defects described below refer to jumping up, wrinkles, insufficient shrinkage, folding of the label end, whitening due to shrinkage, etc. 3 or more was considered to be acceptable. 5: Best finish (no defects) 4: Good finish (one defect) 3: There are two defects 2: 3 to 5 defects 1: Many defects (6 or more)

[0056] [Variation in recycled PET resin] The contents of the 500 ml PET bottle from which the shrink finish was evaluated as described above were removed and washed with water. The PET bottle and label were then crushed into pieces 8 to 10 mm in size using a crusher (Model 48, manufactured by Fujitex Co., Ltd.) to produce fluff. The obtained fluff was melted at 280℃ in a pelletizer (Nihon Yuki SRH-V55 / 48) and pellets were produced at a discharge rate of 120 kg per hour for 30 minutes to produce recycled PET resin. The recycled PET resin was cut to a length of 3±0.8 mm (2.2-3.8 mm) and a particle weight of 30±10 mg / piece (20-40 mg / piece). 300 particles of the recycled PET resin were sampled 5 minutes, 15 minutes, and 25 minutes after the start of granulation (total of 900 particles) and the size of the recycled PET resin was measured. The evaluation was performed using the following method, with ◯ being considered as passing. Good: Resin that is out of size (length, grain weight) is less than 10% of the total, and there are no problems during granulation due to pulsation, etc. △: Resin with the wrong size (length, grain weight) accounts for less than 30% of the total, and problems during granulation due to pulsation, etc. occurred less than twice. ×: Resin that is out of size (length, grain weight) is more than 30% of the total, and problems during granulation due to pulsation, etc. occurred three or more times.

[0057] <Preparation of polyester raw materials> [Synthesis Example 1] In a stainless steel autoclave equipped with a stirrer, a thermometer and a partial reflux condenser, 100 mol% of dimethyl terephthalate (DMT) as a dicarboxylic acid component and 100 mol% of ethylene glycol (EG) as a polyhydric alcohol component were charged so that the molar ratio of ethylene glycol was 2.2 times that of dimethyl terephthalate, 0.05 mol% (relative to the acid component) of zinc acetate as an ester exchange catalyst and 0.225 mol% (relative to the acid component) of antimony trioxide as a polycondensation catalyst were added, and an ester exchange reaction was carried out while distilling off the produced methanol outside the system. Thereafter, a polycondensation reaction was carried out under reduced pressure conditions of 26.7 Pa at 280°C to obtain polyester A with an intrinsic viscosity of 0.75 dl / g. The composition is shown in Table 1.

[0058] [Synthesis Examples 2 to 5] Polyesters B to D shown in Table 1 were obtained by the same method as in Synthesis Example 1. When producing polyester B, SiO2 (Silysia 266 manufactured by Fuji Silysia Corporation; average particle size 3 μm) was added as a lubricant at a ratio of 20,000 ppm to the polyester. The intrinsic viscosity of the polyesters was all 0.75 dl / g. Each polyester was appropriately cut into chips. The composition of each polyester is shown in Table 1.

[0059] [Table 1]

[0060] [Example 1] The above-mentioned polyester A, polyester B, and polyester C were mixed in a weight ratio of 67:3:30 and fed into an extruder. The mixed resin was then melted at 273°C using a four-screw, extruded from a T-die while cooling to 260°C, and rapidly cooled by being wound around a rotating metal roll cooled to a surface temperature of 20°C to obtain an unstretched film with a thickness of 201 μm. The Tg of the unstretched film was 65°C. The unstretched film was introduced into a longitudinal stretching machine, preheated with a roll having a surface temperature of Tg+10°C (75°C), and stretched 1.2 times in the longitudinal (longitudinal) direction by utilizing the speed difference between the rolls. The film uniaxially stretched in the longitudinal direction was introduced into a tenter, and preheated until the film temperature reached Tg+45°C (110°C) while both ends of the film were held by clips. Thereafter, the film was stretched 1.5 times in the transverse direction in the first stage at a temperature of Tg+10°C (75°C), and then relaxed 10% in the width direction at Tg+10°C (75°C). The film after relaxation in the width direction was stretched 3.1 times (total stretch ratio 4.2 times) in the second stage at Tg+10°C (75°C). The film after stretching in the width direction was heat set at Tg+12°C (77°C). Both edges of the stretched film were cut and removed to continuously produce a biaxially stretched film of about 40 μm over a predetermined length, thereby obtaining a film roll made of a heat-shrinkable polyester film. The properties of the obtained film were evaluated by the above-mentioned method. The film-forming conditions are shown in Table 2, and the evaluation results are shown in Table 3. The film had no practical problems with shrink finish or variation in recycled PET.

[0061] [Example 2] Polyester A, polyester B, and polyester C were mixed in a weight ratio of 77:3:20 and fed into an extruder to obtain an unstretched film having a thickness of 201 μm in the same manner as in Example 1. The Tg of the unstretched film was 70° C. The unstretched film was stretched in the same manner as in Example 1 to obtain a film roll made of a heat-shrinkable polyester film having a thickness of 40 μm. However, the temperature conditions for stretching were changed to Tg+10°C (80°C), Tg+45°C (115°C), and Tg+12°C (82°C) because Tg was different from that in Example 1. The properties of the obtained film were evaluated by the above-mentioned method. The film formation conditions are shown in Table 2, and the evaluation results are shown in Table 3. The film had no practical problems with shrink finish or variation in recycled PET.

[0062] [Example 3] Polyester A, polyester B, and polyester C were mixed in a weight ratio of 92:3:5 and fed into an extruder to obtain an unstretched film having a thickness of 201 μm in the same manner as in Example 1. The Tg of the unstretched film was 74° C. The unstretched film was stretched in the same manner as in Example 1 to obtain a film roll made of a heat-shrinkable polyester film having a thickness of 40 μm. However, the temperature conditions for stretching were changed to Tg+10°C (84°C), Tg+45°C (119°C), and Tg+12°C (86°C) because Tg was different from that in Example 1. The properties of the obtained film were evaluated by the above-mentioned method. The film formation conditions are shown in Table 2, and the evaluation results are shown in Table 3. The film had no practical problems with shrink finish or variation in recycled PET.

[0063] [Example 4] Polyester A, polyester B, polyester C, and polyester D were mixed in a weight ratio of 52:3:5:40 and fed into an extruder to obtain an unstretched film having a thickness of 201 μm in the same manner as in Example 1. The Tg of the unstretched film was 74° C. The unstretched film was stretched in the same manner as in Example 1 to obtain a film roll made of a heat-shrinkable polyester film having a thickness of 40 μm. However, the temperature conditions for stretching were changed to Tg+10°C (84°C), Tg+45°C (119°C), and Tg+12°C (86°C) because Tg was different from that in Example 1. The properties of the obtained film were evaluated by the above-mentioned method. The film formation conditions are shown in Table 2, and the evaluation results are shown in Table 3. The film had no practical problems with shrink finish or variation in recycled PET.

[0064] [Example 5] Polyester A, polyester B, polyester C, and polyester D were mixed in a weight ratio of 57:3:30:10 and fed into an extruder to obtain an unstretched film having a thickness of 201 μm in the same manner as in Example 1. The Tg of the unstretched film was 65° C. The unstretched film was stretched in the same manner as in Example 1 to obtain a film roll made of a heat-shrinkable polyester film having a thickness of 40 μm. The film formation conditions are shown in Table 2, and the evaluation results are shown in Table 3. The film had no practical problems with shrink finish or variation in recycled PET.

[0065] [Example 6] Polyester A, polyester B, polyester C, and polyester D were mixed in a weight ratio of 67:3:20:10 and fed into an extruder to obtain an unstretched film having a thickness of 201 μm in the same manner as in Example 1. The Tg of the unstretched film was 70° C. The unstretched film was stretched in the same manner as in Example 1 to obtain a film roll made of a heat-shrinkable polyester film having a thickness of 40 μm. However, the temperature conditions for stretching were changed to Tg+10°C (80°C), Tg+45°C (115°C), and Tg+12°C (82°C) because Tg was different from that in Example 1. The properties of the obtained film were evaluated by the above-mentioned method. The film formation conditions are shown in Table 2, and the evaluation results are shown in Table 3. The film had no practical problems with shrink finish or variation in recycled PET.

[0066] [Comparative Example 1] The above-mentioned polyester A, polyester B, and polyester C were mixed in a weight ratio of 47:3:50 and fed into an extruder. The mixed resin was then melted at 273°C using a four-screw, extruded from a T-die while cooling to 260°C, and rapidly cooled by being wound around a rotating metal roll cooled to a surface temperature of 20°C to obtain an unstretched film with a thickness of 201 μm. The Tg of the unstretched film was 58°C. The unstretched film was introduced into a longitudinal stretching machine, preheated with a roll having a surface temperature of Tg+10°C (68°C), and stretched 1.2 times in the longitudinal (longitudinal) direction by utilizing the speed difference between the rolls. The film uniaxially stretched in the longitudinal direction was introduced into a tenter, and preheated until the film temperature reached Tg+45°C (103°C) while both ends of the film were held by clips. Thereafter, the film was stretched 1.5 times in the transverse direction in the first stage at a temperature of Tg+10°C (68°C), and then relaxed 10% in the width direction at Tg+10°C (68°C). The film after relaxation in the width direction was stretched 3.1 times (total stretch ratio 4.2 times) in the second stage at Tg+10°C (68°C). The film after stretching in the width direction was heat set at Tg+12°C (70°C). Both edges of the stretched film were cut and removed to continuously produce a biaxially stretched film of about 40 μm over a predetermined length, thereby obtaining a film roll made of a heat-shrinkable polyester film. The properties of the obtained film were evaluated by the above-mentioned method. The film-forming conditions are shown in Table 2, and the evaluation results are shown in Table 3. The shrinkage finish was a film with no practical issues, but the recycled PET resin mixed with PET bottles had a large variation in size, and there was one defect where a problem occurred during granulation due to pulsation.

[0067] [Comparative Example 2] Polyester B, Polyester C, and Polyester D were mixed in a weight ratio of 3:7:90 and fed into an extruder to obtain an unstretched film having a thickness of 201 μm in the same manner as in Example 1. The Tg of the unstretched film was 73° C. The unstretched film was stretched in the same manner as in Example 1 to obtain a film roll made of a heat-shrinkable polyester film having a thickness of 40 μm. However, the temperature conditions for stretching were changed to Tg+10°C (83°C), Tg+45°C (118°C), and Tg+12°C (85°C) because Tg was different from that in Example 1. The properties of the obtained film were evaluated by the above-mentioned method. The film formation conditions are shown in Table 2, and the evaluation results are shown in Table 3. The shrinkage finish was a film with no practical issues, but the recycled PET resin mixed with PET bottles had a large variation in size, and there were two defects where problems occurred during granulation due to pulsation.

[0068] [Comparative Example 3] Polyester A, polyester B, polyester C, and polyester E were mixed in a weight ratio of 12:3:5:80 and fed into an extruder to obtain an unstretched film having a thickness of 201 μm in the same manner as in Example 1. The Tg of the unstretched film was 74° C. The unstretched film was stretched in the same manner as in Example 1 to obtain a film roll made of a heat-shrinkable polyester film having a thickness of 40 μm. However, the temperature conditions for stretching were changed to Tg+10°C (83°C), Tg+45°C (118°C), and Tg+12°C (85°C) because Tg was different from that in Example 1. The properties of the obtained film were evaluated by the above-mentioned method. The film formation conditions are shown in Table 2, and the evaluation results are shown in Table 3. The shrink finish was good, but the recycled PET resin mixed with PET bottles had a large variation in size, and there were repeated defects due to pulsation problems during granulation.

[0069] [Table 2A]

[0070] [Table 2B]

[0071] [Table 3] [Industrial Applicability]

[0072] The heat-shrinkable polyester film of the present invention has a high heat shrinkage rate, but the raw material components used are similar to those used in PET beverage bottles. Therefore, even if the heat-shrinkable polyester film used as a label is mixed in the process of recycling PET bottles to produce recycled PET resin, recycled PET resin can be produced with stable quality.

Claims

1. A heat-shrinkable polyester film containing 95 mol% or more and 100 mol% or less of dicarboxylic acid and 0 mol% or more and 5 mol% or less of isophthalic acid out of 100 mol% of dicarboxylic acid components, and containing 85 mol% or more and 98 mol% or less of ethylene terephthalate units out of 100 mol% of all ester units, and containing 2 mol% or more and 15 mol% or less of diethylene glycol out of 100 mol% of polyhydric alcohol components, the heat-shrinkable polyester film being characterized by satisfying the following requirements (1) to (5). (1) When the film is immersed in 90°C hot water for 10 seconds, the hot water heat shrinkage rate is 40% or more and 70% or less in the width direction of the film. (2) When the film is immersed in 90°C hot water for 10 seconds, the hot water heat shrinkage rate is -5% or more and 15% or less in the longitudinal direction of the film. (3) Using a differential scanning calorimeter (DSC), the film is heated to 300°C, melted, then rapidly cooled, and heated again to 300°C. The endothermic peak temperature due to melting is 245°C or higher and 260°C or lower. (4) Film thickness is 15 μm or more and 50 μm or less (5) Using a differential scanning calorimeter (DSC), the film is heated to 300°C, melted, then rapidly cooled, and heated again to 300°C, and the amount of heat absorbed by melting is 10 mJ / mg or more.

2. The density of the film is 1.33 g / cm 3 1.39g / cm or more 3 2. The heat-shrinkable polyester film according to claim 1, wherein the heat-shrinkable polyester film has the following properties:

3. 3. The heat-shrinkable polyester film according to claim 1, which has a haze of 2% or more and 10% or less when the film has a thickness of 20 μm.

4. A heat-shrinkable label using the heat-shrinkable polyester film according to any one of claims 1 to 3.

5. A method for producing a package, comprising covering at least a part of the outer periphery of an object to be packaged with the heat-shrinkable label according to claim 4 and heat-shrinking the object.

6. 4. The heat-shrinkable polyester film according to claim 1, which is used for a heat-shrinkable label and then used as a raw material for recycling PET bottles.

Citation Information

Patent Citations

  • Heat-shrinkable polyester-based film

    JP2002103545A

  • Heat-shrinkable polyester film, and method for producing the same

    JP2008274160A

  • Heat-shrinkable polyester film, packaging body thereof, the method for producing heat-shrinkable polyester film

    WO2011114934A1

  • Heat-shrinkable polyester film and packaging

    WO2018025801A1

  • Crystallizable shrinkable films and thermoformable sheets made from resin blends

    WO2020076749A1