Photosensitive resin composition, photosensitive element, printed wiring board, and method for manufacturing printed wiring board

A photosensitive resin composition with phenol-modified resins and inorganic fillers addresses the challenges of high resolution and thermal shock resistance in printed wiring boards, enhancing insulation properties for high-density applications.

JP2024150011APending Publication Date: 2024-10-23RESONAC CORP

Patent Information

Application Number
JP2023063213
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23

AI Technical Summary

Technical Problem

Existing permanent resists for printed wiring boards face challenges in achieving high resolution, thermal shock resistance, and insulation properties, particularly with the increasing density of printed wiring boards.

Method used

A photosensitive resin composition comprising phenol-modified resins with (meth)acryloyl groups, photopolymerization initiators, inorganic fillers, and optional elastomers, which form a permanent resist with excellent resolution, thermal shock resistance, and insulation properties.

Benefits of technology

The composition enables the formation of a permanent resist with improved resolution, thermal shock resistance, and insulation, suitable for high-density printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150011000002
    Figure 2024150011000002
  • Figure 2024150011000001
    Figure 2024150011000001
Patent Text Reader

Abstract

To provide a photosensitive resin composition capable of forming a permanent resist with superior resolution, thermal shock resistance and insulation properties, a photosensitive element including the photosensitive resin composition, a printed wiring board, and a method for manufacturing a printed wiring board.SOLUTION: A photosensitive resin composition according to the present disclosure includes (A) a phenol-modified resin with a (meth)acryloyl group and without a carboxy group, (B) a phenol-modified resin with both a (meth)acryloyl group and a carboxy group, (C) a photopolymerization initiator, and (D) an inorganic filler, where the component (B) is a reaction product of a compound having two or more phenolic hydroxy groups in one molecule, a compound having a cyclic ether group, a monocarboxylic acid having an α,β-ethylenically unsaturated group, and a polybasic acid anhydride.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a photosensitive resin composition for permanent resist, a photosensitive element, a printed wiring board, and a method for producing a printed wiring board. [Background technology]

[0002] In the field of printed wiring boards, permanent resists are formed on printed wiring boards. The permanent resists have the role of preventing corrosion of the conductor layer and maintaining electrical insulation between the conductor layers when the printed wiring board is used. In recent years, the permanent resists have also come to play the role of a solder resist film that prevents solder from adhering to unnecessary parts of the conductor layer of the printed wiring board in the process of flip-chip mounting or wire-bonding mounting of a semiconductor element on the printed wiring board via solder.

[0003] The permanent resist is formed by a screen printing method using a thermosetting resin composition, a photolithography method using a photosensitive resin composition, etc. For example, in flexible wiring boards using mounting methods such as FC (Flip Chip), TAB (Tape Automated Bonding), and COF (Chip On Film), a thermosetting resin paste is screen printed and thermally cured to form a permanent resist, except for IC chips, electronic components or LCD (liquid crystal display) panels, and connecting wiring parts (see, for example, Patent Document 1).

[0004] In semiconductor package substrates such as BGA (ball grid array) and CSP (chip size package) mounted on electronic components, it is necessary to remove the permanent resist from the bonding portion in order to (1) flip-chip mount a semiconductor element on the semiconductor package substrate via solder, (2) wire-bond the semiconductor element and the semiconductor package substrate, or (3) solder the semiconductor package substrate to a motherboard substrate. For this reason, a photolithography method is used for forming an image on the permanent resist, in which a photosensitive resin composition is applied and dried, and then selectively irradiated with active light such as ultraviolet light to harden the composition, and only the unirradiated portion is removed by development to form an image. The photolithography method is suitable for mass production due to its good workability, and is widely used in the electronic materials industry for forming images on photosensitive materials (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2003-198105 A [Patent Document 2] JP 2011-133851 A Summary of the Invention [Problem to be solved by the invention]

[0006] In response to the increasing density of printed wiring boards, even higher performance is being demanded of permanent resists, and in particular, there is a demand for a high degree of resolution (ability to form fine patterns), thermal shock resistance, and insulating properties.

[0007] An object of the present disclosure is to provide a photosensitive resin composition capable of forming a permanent resist excellent in resolution, thermal shock resistance, and insulation property, a photosensitive element and a printed wiring board using the photosensitive resin composition, and a method for producing a printed wiring board. [Means for solving the problem]

[0008] One aspect of the present disclosure relates to the following photosensitive resin composition, photosensitive element, printed wiring board, and method for producing a printed wiring board. [1] A photosensitive resin composition comprising: (A) a phenol-modified resin having a (meth)acryloyl group and no carboxy group; (B) a phenol-modified resin having a (meth)acryloyl group and a carboxy group; (C) a photopolymerization initiator; and (D) an inorganic filler, wherein the component (B) is a reaction product of a compound having two or more phenolic hydroxyl groups in one molecule, a compound having a cyclic ether group, a monocarboxylic acid having an α,β-ethylenically unsaturated group, and a polybasic acid anhydride. [2] The photosensitive resin composition according to the above [1], wherein the compound having a cyclic ether group includes at least one selected from the group consisting of alkylene oxide compounds and cyclic carbonate compounds. [3] The photosensitive resin composition according to the above [1] or [2], wherein the component (D) contains silica particles. [4] The photosensitive resin composition according to any one of the above [1] to [3], further comprising (E) an elastomer. [5] The photosensitive resin composition according to any one of the above [1] to [4], further comprising (F) a photopolymerizable monomer. [6] The photosensitive resin composition according to any one of the above [1] to [5], further comprising (G) a curing agent. [7] The photosensitive resin composition according to any one of the above [1] to [6], wherein the content of the component (B) is 20 mass % or more based on the total solid content of the photosensitive resin composition. [8] A photosensitive element comprising a support film and a photosensitive layer containing the photosensitive resin composition according to any one of the above [1] to [7]. [9] A printed wiring board comprising a permanent resist comprising a cured product of the photosensitive resin composition according to any one of [1] to [7] above.

[10] The printed wiring board according to [9] above, wherein the thickness of the permanent resist is 5 μm or more.

[11] A method for producing a printed wiring board, comprising the steps of: forming a photosensitive layer on a substrate using the photosensitive resin composition according to any one of [1] to [7] above or the photosensitive element according to [8] above; exposing and developing the photosensitive layer to form a resist pattern; and curing the resist pattern to form a permanent resist. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a photosensitive resin composition capable of forming a permanent resist excellent in resolution, thermal shock resistance and insulation property, a photosensitive element using the photosensitive resin composition, a printed wiring board, and a method for producing a printed wiring board. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a photosensitive element according to this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, one embodiment of the present disclosure will be specifically described, but the present disclosure is not limited thereto. In the following embodiment, the components (including element steps, etc.) are not essential unless otherwise specified, or considered to be obviously essential in principle. The same applies to the numerical values ​​and their ranges, and the present disclosure is not unduly limited.

[0012] In the present disclosure, a numerical range indicated using "~" indicates a range including the numerical values ​​described before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in the present disclosure, the upper or lower limit of a numerical range of a certain stage may be replaced with the upper or lower limit of a numerical range of another stage. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit of the numerical range may be replaced with a value shown in the Examples. In the present disclosure, the content of each component in the composition means the total content of the multiple substances present in the composition, unless otherwise specified, when there are multiple substances corresponding to each component. In the present disclosure, the "solid content" refers to the non-volatile content excluding volatile substances such as water and solvent contained in the resin composition, and refers to the components that remain without evaporating or volatilizing when the resin composition is dried, and also includes components that are liquid, syrup-like, or wax-like at room temperature (25°C, the same below). In the present disclosure, (meth)acrylate means acrylate or the corresponding methacrylate. The same applies to other similar expressions such as (meth)acryloyl.

[0013] [Photosensitive resin composition] The photosensitive resin composition according to this embodiment contains (A) a phenol-modified resin having a (meth)acryloyl group and no carboxy group (hereinafter also referred to as "(A) component"); (B) a phenol-modified resin having a (meth)acryloyl group and a carboxy group (hereinafter also referred to as "(B) component"); (C) a photopolymerization initiator (hereinafter also referred to as "(C) component"); and (D) an inorganic filler (hereinafter also referred to as "(D) component"). The (B) component is a reaction product of a compound having two or more phenolic hydroxyl groups in one molecule, a compound having a cyclic ether group, a monocarboxylic acid having an α,β-ethylenically unsaturated group, and a polybasic acid anhydride. The photosensitive resin composition according to this embodiment is a negative photosensitive resin composition, and a cured film of the photosensitive resin composition can be suitably used as a permanent resist.

[0014] <Component (A)> The photosensitive resin composition according to the present embodiment contains, as component (A), a phenol-modified resin having a (meth)acryloyl group and no carboxy group. By containing component (A), a permanent resist having excellent insulating properties and thermal shock resistance can be formed. The component (A) may be used alone or in combination of two or more.

[0015] The component (A) may be a reaction product of a compound having two or more phenolic hydroxyl groups in one molecule (hereinafter also referred to as "component (a)"), a compound having a cyclic ether group (hereinafter also referred to as "component (b)"), and a monocarboxylic acid having an α,β-ethylenically unsaturated group (hereinafter also referred to as "component (c)"). Since such a component (A) has a hydrophilic alkylene oxide group or a repeating structure thereof, when used in combination with the component (B) described below, the alkali developability tends to be good. Furthermore, by containing such a component (A), the insulating properties of the formed permanent resist are more excellent.

[0016] The component (a) may be, for example, a novolac type phenolic resin. The novolac type phenolic resin may be synthesized, for example, by a condensation reaction between a phenol and formaldehyde in the presence of an acid catalyst. Examples of the phenol include phenol, cresol, ethylphenol, propylphenol, butylphenol, hexylphenol, octylphenol, nonylphenol, phenylphenol, cumylphenol, bisphenol A, bisphenol F, and bixylenol. From the viewpoint of superior insulation properties, thermal shock resistance, and alkaline developability, the component (a) may be a bisphenol A type novolac resin obtained by using bisphenol A, or a bisphenol F type novolac resin obtained by using bisphenol F.

[0017] Examples of component (a), in addition to novolak-type phenolic resins, include condensates of phenols and aromatic aldehydes having a phenolic hydroxyl group, poly-p-hydroxystyrene, condensates of 1-naphthol or 2-naphthol and aldehydes (i.e., naphthol-type novolak resins), condensates of 1,2-, 1,3-, 1,4-, 1,5-, 1,6-, 2,3-, 2,6-, and 2,7-dihydroxynaphthalene and aldehydes, condensates of mononaphthol, the above-mentioned dihydroxynaphthalene and aldehydes, condensates of mono- or dihydroxynaphthalene and xylylene glycols, adducts of mono- or dihydroxynaphthalene and diene compounds, and condensates of phenols and bis(methoxymethyl)biphenyl.

[0018] The component (a) may have an average number of phenol nuclei of 3 or more. The component (a) may be used alone or in combination of two or more.

[0019] Examples of the (b) component include alkylene oxide compounds and cyclic carbonate compounds. Examples of the alkylene oxide compounds include ethylene oxide, propylene oxide, 1,2-butylene oxide, trimethylene oxide, tetrahydrofuran, and tetrahydropyran. Examples of the cyclic carbonate compounds include ethylene carbonate and propylene carbonate. The (b) component may be used alone or in combination of two or more. From the viewpoints of insulation, thermal shock resistance, and alkaline developability, the (b) component may be ethylene oxide, propylene oxide, or butylene oxide.

[0020] Examples of the (c) component include acrylic acid, a dimer of acrylic acid, methacrylic acid, β-styryl acrylic acid, β-furfuryl acrylic acid, a (meth)acrylic acid caprolactone adduct, and a half ester compound of a saturated or unsaturated dibasic acid anhydride and a hydroxyl group-containing (meth)acrylate. The (c) component may be used alone or in combination of two or more. From the viewpoints of photoreactivity and physical properties of the cured product, particularly thermal shock resistance, moisture absorption resistance, and insulating properties, the (c) component may be acrylic acid or methacrylic acid.

[0021] From the viewpoint of achieving superior resolution, thermal shock resistance, and insulating properties, the component (A) may be a reaction product of a bisphenol A novolak resin or a bisphenol F novolak resin with ethylene oxide or propylene oxide, and acrylic acid or methacrylic acid.

[0022] The (A) component can be obtained, for example, through a step of subjecting a compound (b) having a cyclic ether group to an addition reaction with some or all of the phenolic hydroxyl groups of a compound (a) having two or more phenolic hydroxyl groups in one molecule to obtain an alkylene oxide adduct having an alcoholic hydroxyl group (hereinafter also referred to as "Step 1"), and a step of subjecting the alcoholic hydroxyl group of the adduct to an esterification reaction with a monocarboxylic acid (c) having an α,β-ethylenically unsaturated group (hereinafter also referred to as "Step 2").

[0023] Step 1 is, for example, a method of carrying out a reaction by using an organic solvent in the presence of an alkali metal compound such as sodium hydroxide; a quaternary ammonium salt such as trimethylbenzylammonium hydroxide, tetramethylammonium hydroxide, or tetraethylammonium hydroxide; or a mixture of an alkali metal compound and a quaternary ammonium salt at 80 to 180° C. and normal pressure to 10 kg / cm 2The organic solvent may be at least one selected from the group consisting of acetates such as ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, etc.; ketones such as methyl ethyl ketone, cyclohexanone, methyl isobutyl ketone, etc.; aromatic hydrocarbons such as toluene, xylene, tetramethylbenzene, etc.; and mixed solvents thereof, or at least one selected from the group consisting of ketones, aromatic hydrocarbons, and mixed solvents thereof may be used.

[0024] The esterification reaction in step 2 may be carried out at a temperature of 50 to 150°C under reduced pressure, normal pressure or pressure. As the solvent, a known solvent may be used. As the catalyst, for example, sulfuric acid, hydrochloric acid, phosphoric acid, boron fluoride, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and cation exchange resin may be mentioned. The esterification reaction may be carried out in the presence of a polymerization inhibitor. As the polymerization inhibitor, for example, hydroquinone, methylhydroquinone, hydroquinone monomethyl ether, catechol, and pyrogallol may be mentioned.

[0025] The weight average molecular weight (Mw) of the component (A) may be 2,000 to 150,000 or 4,000 to 100,000.

[0026] Mw can be measured by gel permeation chromatography (GPC). Mw can be measured, for example, under the following GPC conditions, and the value converted using a calibration curve of standard polystyrene can be used as Mw. The calibration curve can be created using a 5-sample set ("PStQuick MP-H" and "PStQuick B", manufactured by Tosoh Corporation) as standard polystyrene. GPC equipment: High-speed GPC equipment "HCL-8320GPC" (Tosoh Corporation) Detector: Differential refractometer or UV detector (Tosoh Corporation) Column: TSKgel SuperMultipore HZ-H (column length: 15 cm, column inner diameter: 4.6 mm) (manufactured by Tosoh Corporation) Eluent: Tetrahydrofuran (THF) Measurement temperature: 40℃ Flow rate: 0.35mL / min Sample concentration: 10mg / THF5mL Injection volume: 20μL

[0027] The content of the (A) component may be 5 parts by mass or more, 8 parts by mass or more, 10 parts by mass or more, 12 parts by mass or more, or 14 parts by mass or more from the viewpoint of thermal shock resistance and insulating property, and may be 50 parts by mass or less, 45 parts by mass or less, 40 parts by mass or less, or 35 parts by mass or less from the viewpoint of resolution, based on the total solid content of the photosensitive resin composition. The content of the (A) component may be 1% by mass or more, 3% by mass or more, or 5% by mass or more from the viewpoint of thermal shock resistance and insulating property, and may be 20% by mass or less, 18% by mass or less, 16% by mass or less, or 14% by mass or less from the viewpoint of resolution.

[0028] <(B) component> The photosensitive resin composition according to the present embodiment contains a phenol-modified resin having a (meth)acryloyl group and a carboxy group as the component (B). The component (B) is a reaction product of a compound having two or more phenolic hydroxyl groups in one molecule, a compound having a cyclic ether group, a monocarboxylic acid having an α,β-ethylenically unsaturated group, and a polybasic acid anhydride (hereinafter also referred to as "component (d)"). Such a component (B) has excellent compatibility with the component (A), and when used in combination with the component (A), it has excellent resolution. In addition, by containing the component (B), the developability, particularly the alkaline developability, tends to be improved. The component (B) can be used alone or in combination of two or more.

[0029] As the compound having two or more phenolic hydroxyl groups in one molecule, the compound having a cyclic ether group, and the monocarboxylic acid having an α,β-ethylenically unsaturated group, the components (a) to (c) listed in the above section on component (A) may each be used independently.

[0030] Examples of the component (d) include alicyclic dibasic acid anhydrides such as methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, nadic anhydride, 3,6-endomethylenetetrahydrophthalic anhydride, methylendomethylenetetrahydrophthalic anhydride, and tetrabromophthalic anhydride, aliphatic or aromatic dibasic acid anhydrides such as succinic anhydride, maleic anhydride, itaconic anhydride, octenylsuccinic anhydride, pentadodecenylsuccinic anhydride, phthalic anhydride, and trimellitic anhydride, and aliphatic or aromatic tetrabasic acid dianhydrides such as biphenyltetracarboxylic dianhydride, diphenylethertetracarboxylic dianhydride, butanetetracarboxylic dianhydride, cyclopentanetetracarboxylic dianhydride, pyromellitic anhydride, and benzophenonetetracarboxylic dianhydride. The component (d) can be used alone or in combination of two or more. From the viewpoints of resolution and heat resistance, an alicyclic dibasic acid anhydride may be used as the component (d).

[0031] The (B) component can be obtained, for example, through a step of subjecting a compound having a cyclic ether group to an addition reaction with some or all of the phenolic hydroxyl groups of a compound having two or more phenolic hydroxyl groups in one molecule to obtain an alkylene oxide adduct having an alcoholic hydroxyl group (hereinafter also referred to as "step i"), a step of subjecting the alcoholic hydroxyl group of the adduct to an esterification reaction with a monocarboxylic acid having an α,β-ethylenically unsaturated group (hereinafter also referred to as "step ii"), and a step of further reacting the obtained product with a polybasic acid anhydride (hereinafter also referred to as "step iii"). The reaction conditions of steps i and ii may be the same as those of steps 1 and 2 described above for the (A) component, respectively.

[0032] In step iii, the amount of component (d) used may be such that the acid value of the component (B) produced is 30 to 150 mgKOH / g or 50 to 120 mgKOH / g. The reaction in step iii may be carried out in the presence or absence of an organic solvent, in the presence of a polymerization inhibitor such as a hydroquinone compound and oxygen, at 50 to 150°C. If necessary, a catalyst may be used. Examples of the catalyst include tertiary amines such as triethylamine, quaternary ammonium salts such as triethylbenzylammonium chloride, imidazole compounds such as 2-ethyl-4-methylimidazole, and phosphorus compounds such as triphenylphosphine.

[0033] The acid value of component (B) may be 30 to 150 mgKOH / g or 50 to 120 mgKOH / g. When the acid value of component (B) is 30 mgKOH / g or more, the solubility in an alkaline aqueous solution is improved, and the formed coating film tends to be easily developed. When the acid value of component (B) is 150 mgKOH / g or less, development up to the surface of the exposed area can be suppressed regardless of the exposure conditions.

[0034] The weight average molecular weight of the (B) component may be 2000 to 150000 or 4000 to 100000. When the weight average molecular weight of the (B) component is 2000 or more, it is possible to prevent deterioration of tack-free performance, and also to prevent poor moisture resistance of the coating film after exposure, film loss during development, and significant deterioration in resolution. When the weight average molecular weight of the (B) component is 150000 or less, it is possible to prevent significant deterioration in developability and storage stability.

[0035] The content of the (B) component may be 20% by mass or more, or 25% by mass or more, or 50% by mass or less, 45% by mass or less, 40% by mass or less, or 35% by mass or less, based on the total amount of solids in the photosensitive resin composition. When the (B) component content is 20% by mass or more, the resolution is more excellent. When the (B) component content is 50% by mass or less, the acid value of the photosensitive resin composition is prevented from increasing, and the insulating property is prevented from decreasing.

[0036] The photosensitive resin composition according to the present embodiment may contain a carboxyl group-containing resin other than the component (B) as necessary, as long as the effect of the present disclosure is not impaired. Examples of such a carboxyl group-containing resin include those obtained by adding an acid anhydride to a reaction product of a novolac type and / or bisphenol type epoxy compound and an unsaturated monobasic acid.

[0037] <(C) component> The photosensitive resin composition according to this embodiment contains a photopolymerization initiator as component (C). The component (C) is not particularly limited as long as it can polymerize the photopolymerizable compound contained in the photosensitive resin composition according to this embodiment, and can be appropriately selected from commonly used photopolymerization initiators. The component (C) can be used alone or in combination of two or more.

[0038] Examples of the component (C) include benzoin compounds such as benzoin, benzoin methyl ether, and benzoin isopropyl ether; acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-methyl-1-[4-(methylthio) alkylphenone compounds such as phenyl-2-morpholino-1-propanone and N,N-dimethylaminoacetophenone; anthraquinone compounds such as 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and 2-aminoanthraquinone; 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; ketal compounds such as acetophenone dimethyl ketal and benzil dimethyl ketal; benzophenone compounds such as benzophenone, methylbenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bis(diethylamino)benzophenone, Michler's ketone, and 4-benzoyl-4'-methyldiphenyl sulfide; acridine compounds such as 9-phenylacridine and 1,7-bis(9,9'-acridinyl)heptane; 2,4,6- acylphosphine oxide compounds such as trimethylbenzoyldiphenylphosphine oxide; and oxime ester compounds such as 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(O-benzoyloxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone-1-(O-acetyloxime), and 1-phenyl-1,2-propanedione-2-[O-(ethoxycarbonyl)oxime].

[0039] The (C) component may contain at least one selected from the group consisting of an alkylphenone compound, a thioxanthone compound, a benzophenone compound, an oxime ester compound, and an acylphosphine oxide compound. The (C) component can be selected according to the desired performance. The (C) component may contain an acylphosphine oxide compound from the viewpoint of improving the curing property of the bottom by photobleaching, and may contain an alkylphenone compound from the viewpoint of being less likely to volatilize and generate outgassing.

[0040] The alkylphenone compound can be classified into a benzil ketal compound having a benzil ketal structure, an α-hydroxyalkylphenone compound having a hydroxyl group at the α-position of the carbonyl group, and an α-aminoalkylphenone compound having a nitrogen atom at the α-position of the carbonyl group, and among these, an α-aminoalkylphenone compound is preferred. When the (C) component contains an alkylphenone compound, the content of the alkylphenone compound may be 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 85% by mass or more, or 90% by mass or more based on the total amount of the (C) component.

[0041] The content of component (C) is not particularly limited, and may be 0.1 mass% or more, 0.2 mass% or more, 0.4 mass% or more, or 0.6 mass% or more, and may be 15 mass% or less, 10 mass% or less, 5 mass% or less, or 1.5 mass% or less, based on the total solid content of the photosensitive resin composition. If the content of component (C) is 0.1 mass% or more, the exposed area tends to be less likely to dissolve during development, and if it is 15 mass% or less, heat resistance tends to be excellent.

[0042] The photosensitive resin composition according to this embodiment may further contain, in addition to the component (C), a photopolymerization initiation assistant such as N,N-dimethylaminobenzoic acid ethyl ester, N,N-dimethylaminobenzoic acid isoamyl ester, pentyl-4-dimethylaminobenzoate, triethylamine, triethanolamine, or other tertiary amines. The photopolymerization initiation assistant may be used alone or in combination of two or more.

[0043] <(D) component> The photosensitive resin composition according to the present embodiment contains an inorganic filler as component (D). By containing component (D), the formed permanent resist has excellent thermal shock resistance. The component (D) may be used alone or in combination of two or more.

[0044] Examples of component (D) include silica (SiO2), alumina (Al2O3), titania (TiO2), tantalum oxide (Ta2O5), zirconia (ZrO2), silicon nitride (Si3N4), barium titanate (BaO·TiO2), barium carbonate (BaCO3), magnesium carbonate (MgCO3), aluminum hydroxide (Al(OH)3), magnesium hydroxide (Mg(OH)2), lead titanate (PbO·TiO2), lead zirconate titanate (PZT), lead lanthanum zirconate titanate (PLZT), gallium oxide (Ga2O3), and spinel (MgO·Al2O3). , mullite (3Al2O3·2SiO2), cordierite (2MgO·2Al2O3 / 5SiO2), talc (3MgO·4SiO2·H2O), aluminum titanate (TiO2·Al2O3), yttria-containing zirconia (Y2O3·ZrO2), barium silicate (BaO·8SiO2), boron nitride (BN), calcium carbonate (CaCO3), barium sulfate (BaSO4), calcium sulfate (CaSO4), zinc oxide (ZnO), magnesium titanate (MgO·TiO2), hydrotalcite, mica, calcined kaolin, and carbon (C).

[0045] The (D) component may contain silica particles from the viewpoint of further improving the thermal shock resistance of the permanent resist. The content of the silica particles is not particularly limited, but may be 5% by mass or more, 10% by mass or more, 15% by mass or more, 20% by mass or more, 25% by mass or more, or 28% by mass or more, and may be 60% by mass or less, 55% by mass or less, or 50% by mass or less, based on the total solid content of the photosensitive resin composition. When the content of the silica particles is within the above range, the composition tends to have a low thermal expansion coefficient, solder heat resistance, adhesive strength, etc.

[0046] From the viewpoint of improving the dispersibility of the inorganic filler in the photosensitive resin composition by the aggregation prevention effect, the component (D) may be an inorganic filler that has been surface-treated in advance with alumina or an organosilane compound.

[0047] From the viewpoint of resolution, the average particle size of the component (D) may be 0.01 to 5 μm, 0.05 to 3 μm, 0.1 to 2 μm, or 0.15 to 1 μm.

[0048] The average particle size of the component (D) is the average particle size of the inorganic filler in a state dispersed in the photosensitive resin composition, and is a value obtained by measuring it by the following procedure. That is, after diluting the photosensitive resin composition 1000 times with a solvent (methyl ethyl ketone), a submicron particle analyzer (manufactured by Beckman Coulter, Inc., product name "N5") is used to measure the particle size distribution of the particles dispersed in the solvent at a refractive index of 1.38 in accordance with the international standard ISO13321. The particle size at an integrated value of 50% (volume basis) in the particle size distribution is taken as the average particle size. The average particle size of the component (D) contained in the photosensitive layer formed using the photosensitive resin composition and its cured film can also be measured by the same procedure.

[0049] The content of the (D) component is not particularly limited, and may be 20 mass% or more, 25 mass% or more, or 28 mass% or more, and may be 70 mass% or less, 65 mass% or less, or 60 mass% or less, based on the total solid content of the photosensitive resin composition. When the content of the (D) component is within the above range, the strength, thermal shock resistance, resolution, etc. of the cured product of the photosensitive resin composition tend to be superior.

[0050] <(E) component> The photosensitive resin composition according to this embodiment may further contain an elastomer as component (E). By containing component (E), it is possible to suppress a decrease in flexibility and adhesive strength caused by distortion (internal stress) inside the resin due to cure shrinkage, and it is possible to improve the flexibility and adhesive strength of the cured film formed by the photosensitive resin composition. By further containing component (E), the photosensitive resin composition according to this embodiment can be suitably used for semiconductor package substrates. The component (E) can be used alone or in combination of two or more.

[0051] Examples of the (E) component include styrene-based elastomers, olefin-based elastomers, urethane-based elastomers, polyester-based elastomers, polyamide-based elastomers, acrylic elastomers, and silicone-based elastomers. The (E) component may contain at least one selected from the group consisting of olefin-based elastomers, polyester-based elastomers, and acrylic elastomers. From the viewpoint of developability, the (E) component may contain an acrylic elastomer.

[0052] Examples of olefin-based elastomers include polymers or copolymers of α-olefins having 2 to 20 carbon atoms, such as ethylene, propylene, 1-butene, 1-hexene, and 4-methyl-pentene; copolymers of α-olefins having 2 to 20 carbon atoms and non-conjugated dienes having 2 to 20 carbon atoms, such as dicyclopentadiene, 1,4-hexadiene, cyclooctadiene, methylenenorbornene, ethylidenenorbornene, butadiene, and isoprene; and carboxylic acid-modified butadiene-acrylonitrile copolymers. Specific examples include polyethylene, polybutadiene, hydroxyl-containing polybutadiene, hydroxyl-containing polyisopropylene, ethylene-propylene copolymer (EPR), and ethylene-propylene-diene copolymer (EPDM).

[0053] As the polyester-based elastomer, a compound obtained by polycondensation of a dicarboxylic acid or its derivative with a diol compound or its derivative can be used. Examples of the dicarboxylic acid include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid; aliphatic dicarboxylic acids having 2 to 20 carbon atoms such as adipic acid, sebacic acid, and dodecanedicarboxylic acid; and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid. Examples of the diol compound include aliphatic diols such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, and 1,10-decanediol; alicyclic diols such as 1,4-cyclohexanediol; and aromatic diols such as bisphenol A, bis(4-hydroxyphenyl)methane, bis(4-hydroxy-3-methylphenyl)propane, and resorcin.

[0054] As the polyester-based elastomer, a multiblock copolymer having an aromatic polyester (e.g., polybutylene terephthalate) as a hard segment component and an aliphatic polyester (e.g., polytetramethylene glycol) as a soft segment component can be used. There are various grades of polyester-based elastomers depending on the type, ratio, and molecular weight of the hard and soft segments. Commercially available products of such multiblock copolymers include, for example, "Hytrel (registered trademark)" (manufactured by DuPont-Toray Co., Ltd.), "Pelprene (registered trademark)" (manufactured by Toyobo Co., Ltd.), "Espel (registered trademark)" and "Teslac (registered trademark)" (manufactured by Resonac Co., Ltd.).

[0055] The acrylic elastomer may be a compound containing a structural unit based on a (meth)acrylic acid ester as a main component. Examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, methoxyethyl (meth)acrylate, and ethoxyethyl (meth)acrylate. The acrylic elastomer may be a compound obtained by copolymerizing a (meth)acrylic acid ester with acrylonitrile, or may be a compound obtained by further copolymerizing a monomer having a functional group that serves as a crosslinking point. Examples of the monomer having a functional group include glycidyl methacrylate and allyl glycidyl ether.

[0056] Examples of acrylic elastomers include acrylonitrile-butyl acrylate copolymers, acrylonitrile-butyl acrylate-ethyl acrylate copolymers, methyl methacrylate-butyl acrylate-methacrylic acid copolymers, and acrylonitrile-butyl acrylate-glycidyl methacrylate copolymers.

[0057] The weight average molecular weight of the component (E) may be from 500 to 50,000, from 800 to 30,000, or from 1,000 to 20,000. When the weight average molecular weight of the component (E) is within the above range, the compatibility with the component (B) and the solubility of the unexposed areas in a developer tend to be excellent, and the resolution tends to be excellent.

[0058] The content of the component (E) may be 0.5 to 20 mass %, 1 to 15 mass %, 1.5 to 10 mass %, 2 to 6 mass %, or 2 to 4 mass % based on the total solid content of the photosensitive resin composition.

[0059] <(F) Component> The photosensitive resin composition according to the present embodiment may further contain a photopolymerizable monomer as component (F). Component (F) is not particularly limited as long as it is a monomer having a functional group exhibiting photopolymerizability (excluding components (A) and (B)). Examples of the functional group exhibiting photopolymerizability include groups having an ethylenically unsaturated bond, such as vinyl groups, allyl groups, propargyl groups, butenyl groups, ethynyl groups, phenylethynyl groups, maleimide groups, nadimide groups, and (meth)acryloyl groups. The component (F) may be used alone or in combination of two or more.

[0060] From the viewpoint of photosensitivity, the component (F) may contain a photopolymerizable monomer having a molecular weight of 1000 or less. Examples of photopolymerizable monomers having a molecular weight of 1000 or less include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; mono- or di(meth)acrylates of glycols such as ethylene glycol, methoxytetraethylene glycol, and polyethylene glycol; (meth)acrylamides such as N,N-dimethyl(meth)acrylamide and N-methylol(meth)acrylamide; aminoalkyl (meth)acrylates such as N,N-dimethylaminoethyl (meth)acrylate; hexanediol, trimethylolpropane, pentaerythritol, ditrimethylolpropane, and the like. Examples of the polyhydric alcohols include tyrolpropane, dipentaerythritol, tris-hydroxyethyl isocyanurate, and other polyhydric (meth)acrylates, or their ethylene oxide or propylene oxide adducts; (meth)acrylates of ethylene oxide or propylene oxide adducts of phenols, such as phenoxyethyl (meth)acrylate and polyethoxy di(meth)acrylate of bisphenol A; (meth)acrylates of glycidyl ethers, such as glycerin diglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; and melamine (meth)acrylate.

[0061] From the viewpoint of further improving the sensitivity, the (F) component may contain a polyvalent (meth)acrylate compound of the above-mentioned polyhydric alcohol or an ethylene oxide or propylene oxide adduct thereof. From the viewpoint of increasing the crosslink density by photocuring and further improving the heat resistance and insulating properties, the (F) component may contain a (meth)acrylate compound having three or more ethylenically unsaturated bonds in the molecule. Examples of such compounds include the above-mentioned polyvalent (meth)acrylate compounds. From the viewpoint of further improving the sensitivity, the polyvalent (meth)acrylate compound may contain dipentaerythritol tri(meth)acrylate.

[0062] The content of the component (F) may be 2 to 50 mass%, 3 to 20 mass%, or 3 to 10 mass% based on the total solid content of the photosensitive resin composition. When the content of the component (F) is 2 mass% or more, the photosensitivity tends to be improved and the exposed area tends to be less likely to dissolve during development, and when it is 50 mass% or less, the heat resistance tends to be improved.

[0063] <(G) component> The photosensitive resin composition according to the present embodiment may further contain a curing agent as component (G). Examples of component (G) include a compound that cures by itself with heat, ultraviolet light, etc., and a compound that cures by reacting with a carboxy group of component (B) with heat, ultraviolet light, etc. Use of component (G) can improve the heat resistance, adhesive strength, chemical resistance, etc. of the permanent resist.

[0064] Examples of the (G) component include thermosetting compounds such as epoxy compounds, melamine compounds, urea compounds, oxazoline compounds, blocked isocyanates, etc. The (G) component can be used alone or in combination of two or more.

[0065] Examples of epoxy compounds include bisphenol A type epoxy resins, bisphenol F type epoxy resins, hydrogenated bisphenol A type epoxy resins, brominated bisphenol A type epoxy resins, novolac type epoxy resins, bisphenol S type epoxy resins, biphenyl type epoxy resins, heterocyclic epoxy resins such as triglycidyl isocyanurate, and bixylenol type epoxy resins.

[0066] Examples of the melamine compound include triaminotriazine, hexamethoxymelamine, and hexabutoxylated melamine. Examples of the urea compound include dimethylol urea.

[0067] As the blocked isocyanate, for example, an addition reaction product of a polyisocyanate compound and an isocyanate blocking agent is used. As the polyisocyanate compound, for example, tolylene diisocyanate, xylylene diisocyanate, phenylene diisocyanate, naphthylene diisocyanate, bis(isocyanatemethyl)cyclohexane, tetramethylene diisocyanate, hexamethylene diisocyanate, methylene diisocyanate, trimethylhexamethylene diisocyanate, isophorone diisocyanate, etc., as well as their adducts, biuret forms, isocyanurates, etc., can be mentioned.

[0068] From the viewpoint of further improving the heat resistance of the cured film, the component (G) may contain at least one selected from the group consisting of epoxy compounds and blocked isocyanates.

[0069] The content of the component (G) may be 2 to 40 mass%, 3 to 30 mass%, or 5 to 20 mass% based on the total solid content of the photosensitive resin composition. By setting the content of the component (G) within the above range, it is possible to further improve the heat resistance of the formed cured film while maintaining good developability.

[0070] <(H) component> The photosensitive resin composition according to the present embodiment may further contain a pigment as component (H) from the viewpoint of improving the appearance, such as by concealing the conductor pattern. As component (H), a colorant that develops a desired color when concealing the conductor pattern, etc., can be used. The component (H) may be used alone or in combination of two or more.

[0071] Examples of colorants include phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, carbon black, and naphthalene black.

[0072] The content of the (H) component is not particularly limited, but from the viewpoint of making the production equipment easier to identify and better concealing the conductor pattern, it may be 0.01 to 5.0 mass%, 0.03 to 3.0 mass%, or 0.05 to 2.0 mass% based on the total solid content of the photosensitive resin composition.

[0073] <Other ingredients> The photosensitive resin composition according to the present embodiment may contain a diluent such as an organic solvent to adjust the viscosity as necessary. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, butyl cellosolve acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha.

[0074] When a diluent is used, the amount of the diluent used may be appropriately selected from an amount that results in a total solid content of the photosensitive resin composition of 50 to 90 mass%, 60 to 80 mass%, or 65 to 75 mass%. When the photosensitive resin composition contains a diluent, the content of the diluent may be 10 to 50 mass%, 20 to 40 mass%, or 25 to 35 mass%. When the content of the diluent is within the above range, the coatability of the photosensitive resin composition is improved, and a more precise pattern can be formed. The photosensitive resin composition according to this embodiment may not contain a diluent.

[0075] The photosensitive resin composition according to the present embodiment may further contain various additives as necessary. Examples of additives include polymerization inhibitors such as k-quinone, methyl hydroquinone, hydroquinone monomethyl ether, catechol, and pyrogallol; thickeners such as bentone and montmorillonite; antifoaming agents such as silicone-based, fluorine-based, and vinyl resin-based; silane coupling agents; and flame retardants such as brominated epoxy compounds, acid-modified brominated epoxy compounds, antimony compounds, phosphate compounds of phosphorus-based compounds, aromatic condensed phosphate esters, and halogen-containing condensed phosphate esters. These may be used alone or in combination of two or more. The photosensitive resin composition according to the present embodiment may not contain the various additives.

[0076] The photosensitive resin composition according to the present embodiment can be produced by mixing the above-mentioned components. For the mixing, a device such as a roll mill or a bead mill can be used.

[0077] [Photosensitive element] The photosensitive element according to this embodiment includes a support film and a photosensitive layer containing the above-mentioned photosensitive resin composition. Fig. 1 is a cross-sectional view showing a schematic diagram of the photosensitive element according to this embodiment. As shown in Fig. 1, the photosensitive element 1 includes a support film 10 and a photosensitive layer 20 formed on the support film 10.

[0078] The photosensitive element 1 can be produced, for example, by applying the photosensitive resin composition according to this embodiment onto a support film 10 by a known method such as reverse roll coating, gravure roll coating, comma coating, or curtain coating, and then drying the coating to form a photosensitive layer 20. The coating can be dried by hot air drying, or drying using far infrared rays or near infrared rays. The drying temperature may be 60 to 120° C., 70 to 110° C., or 80 to 100° C. The drying time may be 1 to 60 minutes, 2 to 30 minutes, or 5 to 20 minutes.

[0079] Examples of the support film include polyester films such as polyethylene terephthalate and polybutylene terephthalate; and polyolefin films such as polypropylene and polyethylene. The thickness of the support film may be, for example, 5 to 100 μm. The thickness of the photosensitive layer may be, for example, 5 to 50 μm, 15 to 40 μm, or 20 to 30 μm.

[0080] The photosensitive layer 20 may further include a protective film 30 covering the photosensitive layer 20. The photosensitive element 1 may also have a protective film 30 laminated on the surface of the photosensitive layer 20 opposite to the surface in contact with the support film 10. As the protective film 30, for example, a polymer film such as polyethylene or polypropylene may be used. The protective film may be the same film as the support film or may be a different film.

[0081] [Printed wiring board] The printed wiring board according to the present embodiment includes a permanent resist containing a cured product of the photosensitive resin composition according to the present embodiment. The method for producing the printed wiring board according to the present embodiment includes a step of forming a photosensitive layer on a substrate using the above-mentioned photosensitive resin composition or the above-mentioned photosensitive element, a step of exposing and developing the photosensitive layer to form a resist pattern, and a step of curing the resist pattern to form a permanent resist. An example of each step will be described below.

[0082] First, a metal-clad laminate substrate is prepared as a substrate, and a photosensitive layer is formed on the substrate. When a photosensitive resin composition is used, the photosensitive resin composition may be applied on the substrate by a method such as screen printing, spraying, roll coating, curtain coating, or electrostatic coating, and the formed coating film may be dried at 60 to 110°C to form a photosensitive layer. The coating may be performed so that the thickness of the photosensitive layer obtained by drying is 5 μm or more, 10 to 200 μm, 15 to 150 μm, 20 to 100 μm, or 23 to 50 μm. When a photosensitive element is used, the photosensitive layer may be formed by thermally laminating the photosensitive layer of the photosensitive element on the substrate using a laminator.

[0083] Next, a negative mask is brought into contact with the photosensitive layer directly or through a transparent film such as a support film, and the layer is exposed to actinic rays, after which the unexposed areas are dissolved and removed with a developer to form a resist pattern. Examples of actinic rays include electron beams, ultraviolet rays, and X-rays, and ultraviolet rays are preferred. Examples of light sources that can be used include low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, and halogen lamps. The exposure dose is 10 to 2000 mJ / cm. 2 , 100~1500mJ / cm 2 , or 300 to 1000 mJ / cm 2 The developing method may be, for example, a dipping method or a spray method. As the developer, for example, an alkaline aqueous solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, tetramethylammonium hydroxide, or the like may be used.

[0084] Next, the formed resist pattern is subjected to at least one of post-exposure and post-heating treatment to sufficiently harden it to form a permanent resist. The exposure dose of the post-exposure is 100 to 5000 mJ / cm 2 , 500~2000mJ / cm 2 , or 700 to 1500 mJ / cm 2The heating temperature of the post-heating may be 100 to 200°C, 120 to 180°C, or 135 to 165°C. The heating time of the post-heating may be 5 minutes to 12 hours, 10 minutes to 6 hours, or 30 minutes to 2 hours. The thickness of the permanent resist may be 5 μm or more, 10 to 50 μm, 15 to 40 μm, or 20 to 30 μm. Thereafter, wiring is formed by etching to produce a printed wiring board.

[0085] The permanent resist according to this embodiment can be used as an interlayer insulating layer or a surface protective layer of a semiconductor element. A semiconductor element having an interlayer insulating layer or a surface protective layer formed from the cured film of the above-mentioned photosensitive resin composition, and an electronic device including the semiconductor element can be produced. The semiconductor element may be, for example, a memory, a package, etc. having a multilayer wiring structure, a rewiring structure, etc. Examples of electronic devices include mobile phones, smartphones, tablet terminals, personal computers, and hard disk suspensions. By providing a patterned cured film formed by the photosensitive resin composition according to this embodiment, a semiconductor element and an electronic device having excellent reliability can be provided. EXAMPLES

[0086] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples.

[0087] [Synthesis Example 1: Synthesis of A-1] (Step 1: Addition reaction) In a flask equipped with a cooling tube and a stirrer, 456 parts by mass of bisphenol F, 228 parts by mass of water, and 649 parts by mass of 37% formalin were charged, and while maintaining the temperature at 40°C or less, 228 parts by mass of 25% aqueous sodium hydroxide solution was added, and the reaction was carried out at 50°C for 10 hours. The solution after the reaction was cooled to 40°C, and while maintaining the temperature at 40°C or less, it was neutralized with 37.5% aqueous phosphoric acid solution until the pH reached 4. The solution was left to stand, and the organic layer and the aqueous layer were separated. 300 parts by mass of methyl isobutyl ketone was added to the obtained organic layer and dissolved uniformly, and then washed three times with 500 parts by mass of distilled water. After washing, water, solvent, etc. were removed under reduced pressure at a temperature of 50°C to obtain product A. The obtained product A was dissolved in 550 parts by mass of methanol, and 1230 parts by mass of a solution of product A was obtained. A part of the obtained solution of product A was dried at room temperature using a vacuum dryer, and the solid content concentration was 55.2% by mass.

[0088] 500 parts by mass of the obtained solution of product A and 440 parts by mass of 2,6-xylenol were charged into a flask equipped with a cooling tube and a stirrer, and were dissolved uniformly at 50°C. Then, methanol was removed under reduced pressure at a temperature of 50°C. Next, 8 parts by mass of oxalic acid was added, and the reaction was carried out at 100°C for 10 hours. Then, the distillate distilled out at 180°C and reduced pressure of 50 mmHg was removed, and 550 parts by mass of novolac resin A was obtained.

[0089] In an autoclave equipped with a thermometer, a nitrogen introduction device / alkylene oxide introduction device, and a stirrer, 130 parts by mass of novolac resin A, 2.6 parts by mass of a 50% aqueous sodium hydroxide solution, and 100 parts by mass of toluene / methyl isobutyl ketone (mass ratio = 2 / 1) were charged, and the inside of the system was replaced with nitrogen while stirring. Next, the temperature was increased to 150°C, and the mixture was cooled to 150°C and 8 kg / cm 2 45 parts by mass of ethylene oxide was gradually introduced and reacted at a gauge pressure of 0.0 kg / cm. 2The reaction was continued for about 4 hours until the reaction reached a state where the reaction mixture was dissolved in water. The reaction solution was cooled to room temperature, and 3.3 parts by mass of a 36% aqueous hydrochloric acid solution was added to the reaction solution and mixed to neutralize the sodium hydroxide. The neutralized solution was diluted with toluene and washed with water three times. The solvent was then removed using an evaporator to obtain product B (ethylene oxide adduct of novolac resin A; hydroxyl group equivalent: 175 g / eq). Product B was one in which ethylene oxide was added on average to one equivalent of phenolic hydroxyl group.

[0090] (Step 2: Esterification reaction) In a reactor equipped with a stirrer, a thermometer and an air inlet tube, 175 parts by mass of product B, 73 parts by mass of acrylic acid, 3.0 parts by mass of p-toluenesulfonic acid, 0.1 parts by mass of hydroquinone monomethyl ether and 130 parts by mass of toluene were charged, and the mixture was stirred while blowing in air, heated to 115°C, and reacted for 4 hours while distilling off the water generated by the reaction as an azeotropic mixture with toluene. Then, the mixture was cooled to room temperature, and the reaction solution obtained was washed with 5% NaCl aqueous solution, and the toluene was removed by distillation under reduced pressure. Then, diethylene glycol monoethyl ether acetate was added to obtain a solution of phenol-modified resin A-1 having an acryloyl group and no carboxy group (solid concentration: 70% by mass).

[0091] [Synthesis Example 2: Synthesis of A-2] The same procedure as in Synthesis Example 1 was carried out except that bisphenol F in Step 1 of Synthesis Example 1 was changed to bisphenol A, thereby obtaining a solution of phenol-modified resin A-2 having an acryloyl group and no carboxy group (solid concentration: 69% by mass).

[0092] [Synthesis Example 3: Synthesis of B-1] Except for changing the amount of acrylic acid in step 2 of Synthesis Example 1 to 50 parts by mass, the same procedure as in Synthesis Example 1 was performed to obtain a solution of phenol-modified resin A-3 having an acryloyl group and no carboxy group (solid concentration: 68% by mass).

[0093] Next, 312 parts by mass of the solution of A-3, 0.1 parts by mass of hydroquinone monomethyl ether, and 0.3 parts by mass of triphenylphosphine were charged into a four-neck flask equipped with a stirrer and a reflux condenser, and the resulting mixture was heated to 110°C, and 45 parts by mass of tetrahydrophthalic anhydride were added and reacted for 4 hours. After that, the mixture was cooled to obtain a solution of phenol-modified resin B-1 having an acryloyl group and a carboxy group (solid content concentration: 73% by mass; solid content acid value: 50 mgKOH / g).

[0094] [Synthesis Example 4: Synthesis of B-2] The same procedure as in Synthesis Example 1 was carried out except that bisphenol F in step 1 of Synthesis Example 1 was changed to bisphenol A and the amount of acrylic acid in step 2 was changed to 50 parts by mass, thereby obtaining a solution of phenol-modified resin A-4 having an acryloyl group and no carboxy group.

[0095] Next, 312 parts by mass of the solution of A-4, 0.1 parts by mass of hydroquinone monomethyl ether, and 0.3 parts by mass of triphenylphosphine were charged into a four-neck flask equipped with a stirrer and a reflux condenser, and the resulting mixture was heated to 110°C, and 45 parts by mass of tetrahydrophthalic anhydride was added and reacted for 4 hours. After that, the mixture was cooled to obtain a solution of phenol-modified resin B-2 having an acryloyl group and a carboxy group (solid content concentration: 69% by mass; solid content acid value: 52 mgKOH / g).

[0096] [Synthesis Example 5: Synthesis of B'-1] In a flask equipped with a stirrer, a reflux condenser and a thermometer, 350 parts by mass of bisphenol F novolac type epoxy resin (manufactured by DIC Corporation, product name "EXA-7376"), 70 parts by mass of acrylic acid, 0.5 parts by mass of methyl hydroquinone and 120 parts by mass of carbitol acetate were mixed with stirring at 90 ° C. The resulting mixture was cooled to 60 ° C., 2 parts by mass of triphenylphosphine was added, and the mixture was reacted at 100 ° C. until the acid value of the solution became 1 mg KOH / g or less. 98 parts by mass of tetrahydrophthalic anhydride and 85 parts by mass of carbitol acetate were added to the reaction solution, and the mixture was heated to 80 ° C. and reacted for 6 hours. Thereafter, the reaction solution was cooled to room temperature to obtain a solution of carboxyl group-containing resin (B'-1) (solid concentration: 73 mass%; solid acid value: 65 mg KOH / g).

[0097] The following materials were prepared as components (C) to (H). C-1: 2-methyl-[4-(methylthio)phenyl]morpholino-1-propanone (manufactured by IGM Resins BV, trade name "Ominirad 907") C-2: 4,4'-bis(diethylamino)benzophenone (Hodogaya Chemical Co., Ltd.) D-1: Silica particles (manufactured by Denka Co., Ltd., product name "SFP20M", average particle size: 0.3 μm) E-1: Polyester resin (manufactured by Resonac Corporation, product name "SP1108") F-1: Dipentaerythritol hexaacrylate (manufactured by Nippon Kayaku Co., Ltd., trade name "DPHA") G-1: Tetramethylbisphenol F type epoxy resin (bisphenol type crystalline epoxy resin; Nippon Steel Chemical & Material Co., Ltd., product name "YSLV-80XY") G-2: Novolac-type multifunctional epoxy resin (manufactured by Nippon Kayaku Co., Ltd., product name "RE-306") H-1: Phthalocyanine pigment (manufactured by Sanyo Pigment Co., Ltd.)

[0098] [Photosensitive resin composition] The components were mixed in the amounts (parts by mass, solid content equivalent) shown in Table 1 and kneaded using a three-roll mill. Carbitol acetate was then added so that the solid content concentration became 70% by mass, to obtain a photosensitive resin composition.

[0099] [Photosensitive element] A polyethylene terephthalate film (manufactured by Toyobo Film Solutions Co., Ltd., product name "G2-25", thickness 25 μm) was prepared as a support film. A solution obtained by diluting a photosensitive resin composition with methyl ethyl ketone was applied onto the support film so that the thickness after drying was 25 μm, and the solution was dried at 75° C. for 30 minutes using a hot air convection dryer to form a photosensitive layer. Next, a polyethylene film (manufactured by Tamapoly Co., Ltd., product name "NF-15") was attached as a protective film to the surface of the photosensitive layer opposite to the side in contact with the support film, to obtain a photosensitive element.

[0100] (Resolution) The protective film was peeled off and removed from the photosensitive element, and the exposed photosensitive layer was laminated onto a 0.6 mm thick copper-clad laminate substrate (manufactured by Resonac Corporation, product name "MCL-E-67") using a press-type vacuum laminator (manufactured by Meiki Seisakusho Corporation, product name "MVLP-500") at 80°C to obtain a laminate having a support film, a photosensitive layer, and a copper-clad laminate substrate.

[0101] Next, a negative mask having an opening pattern of a predetermined size (opening diameter size: 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 150, 200 μm) was attached to the support film of the laminate, and the photosensitive layer was exposed to light using an ultraviolet exposure device (manufactured by Oak Co., Ltd., product name "EXM-1201") at an exposure amount that would result in 13 complete curing steps on a step tablet (manufactured by Resonac Co., Ltd.). Thereafter, the support film was peeled off from the photosensitive layer, and the layer was exposed to light using a 1% by mass aqueous solution of sodium carbonate for 60 seconds at 1.765×10 5 The unexposed areas were then developed by spraying at a pressure of 2000 mJ / cm 2 using an ultraviolet exposure device. 2After the photosensitive layer was exposed to light at an exposure dose of 100 nm, it was heated at 170° C. for 1 hour to prepare a test piece 1 having a cured film on a copper-clad laminate substrate in which an opening pattern of a predetermined size was formed.

[0102] The above test piece 1 was observed using an optical microscope and evaluated according to the following criteria. S: The minimum mask opening diameter was 60 μm or less. A: The minimum opening diameter of the mask was more than 60 μm and was 100 μm or less. B: The minimum mask opening diameter was greater than 100 μm and less than 200 μm. C: The opening size of 200 μm was not opened.

[0103] (Thermal shock resistance) A temperature cycle test was carried out on the above test piece 1, with one cycle being -65°C for 30 minutes and 150°C for 30 minutes. At the 1000th and 1500th cycles, test piece 1 was observed visually and with an optical microscope, and evaluated according to the following criteria. A: No cracks were observed after 1500 cycles. B: No cracks were observed at 1000 cycles, but cracks were observed at 1500 cycles. C: Cracks were observed after 1000 cycles. D: The opening pattern was not formed and could not be evaluated.

[0104] (Insulating) Test piece 2 was produced in the same manner as test piece 1, except that a bismaleimide triazine substrate on which a comb-shaped electrode (line / space=10 / 10 μm) was formed was used instead of the copper-clad laminate substrate in the production of test piece 1. Test piece 2 was exposed to conditions of 135° C., 85% RH, and 3.3 V, and the change in resistance value was measured using a migration tester (manufactured by Kusumoto Chemicals Co., Ltd., product name "SIR13"). Thereafter, the degree of migration occurrence was observed using an optical microscope and evaluated according to the following criteria. A: Even after 200 hours, the resistance remains at 10 -7 It never dropped below Ω. B: Less than 200 hours, resistance value is 10 -7 It dropped below Ω.

[0105] [Table 1] [Explanation of symbols]

[0106] 1...photosensitive element, 10...support film, 20...photosensitive layer, 30...protective film.

Claims

1. (A) a phenol-modified resin having a (meth)acryloyl group and no carboxy group, (B) a phenol-modified resin having a (meth)acryloyl group and a carboxy group, (C) a photopolymerization initiator, and (D) an inorganic filler, The component (B) is a photosensitive resin composition which is a reaction product of a compound having two or more phenolic hydroxyl groups in one molecule, a compound having a cyclic ether group, a monocarboxylic acid having an α,β-ethylenically unsaturated group, and a polybasic acid anhydride.

2. The photosensitive resin composition according to claim 1, wherein the compound having a cyclic ether group comprises at least one compound selected from the group consisting of an alkylene oxide compound and a cyclic carbonate compound.

3. The photosensitive resin composition according to claim 1 , wherein the component (D) comprises silica particles.

4. The photosensitive resin composition according to claim 1 , further comprising (E) an elastomer.

5. The photosensitive resin composition according to claim 1 , further comprising (F) a photopolymerizable monomer.

6. The photosensitive resin composition according to claim 1 , further comprising (G) a curing agent.

7. 2. The photosensitive resin composition according to claim 1, wherein the content of the component (B) is 20 mass % or more based on the total solid content of the photosensitive resin composition.

8. A support film; A photosensitive element comprising a photosensitive layer comprising the photosensitive resin composition according to any one of claims 1 to 7.

9. A printed wiring board comprising a permanent resist comprising a cured product of the photosensitive resin composition according to any one of claims 1 to 7.

10. 10. The printed wiring board according to claim 9, wherein the permanent resist has a thickness of 5 μm or more.

11. forming a photosensitive layer on a substrate using the photosensitive resin composition according to any one of claims 1 to 7; exposing and developing the photosensitive layer to form a resist pattern; and hardening the resist pattern to form a permanent resist.

12. forming a photosensitive layer on a substrate using the photosensitive element of claim 8; exposing and developing the photosensitive layer to form a resist pattern; and hardening the resist pattern to form a permanent resist.

Citation Information

Patent Citations

  • Resin paste and flexible wiring board using the same

    JP2003198105A

  • Black matrix composition with high light-shielding property and improved adhesive force to substrate

    JP2011133851A

Cited By

  • Alkali-developable photosensitive resin composition, dry film, cured product, and printed wiring board

    JP2025152188A

  • Alkali-developable photosensitive resin composition, dry film, cured product, and printed wiring board

    JP7772857B2

  • Alkali developable photosensitive resin composition, dry film, cured product, and printed wiring board