Surface-treated aluminum material, production method thereof, and component for semiconductor processing device
A surface-treated aluminum material with a protective film of aluminum oxide and hydrated oxide addresses durability issues by enhancing corrosion resistance and preventing cracks, suitable for semiconductor manufacturing components.
Patent Information
- Application Number
- JP2023063321
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-23
AI Technical Summary
Components for semiconductor manufacturing equipment made of aluminum with an anodized film face issues of low durability against corrosive gases and plasma, with potential cracks and foreign matter generation due to incomplete closure of anodic oxide film pores.
A surface-treated aluminum material with a protective film comprising aluminum oxide and hydrated oxide, having a thickness of 2 μm or more, and a specific C_H/C_Al mass ratio of 0.2 to 0.7, formed by anodizing and sealing the anodic oxide film under controlled temperature and time conditions.
The material exhibits enhanced corrosion resistance against corrosive gases and plasma, suppressing crack formation, suitable for use in semiconductor manufacturing equipment.
Smart Images

Figure 2024150085000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-treated aluminum material, a manufacturing method thereof, and a member for semiconductor manufacturing equipment. [Background technology]
[0002] Aluminum materials made of aluminum or aluminum alloys are used in a variety of applications. An anodized coating may be provided on the surface of these aluminum materials for the purpose of protecting the surface.
[0003] For example, Patent Document 1 describes a component for a substrate processing apparatus that performs plasma processing on a substrate, the component having a coating formed on the surface of the component by anodizing treatment in which the component is connected to the anode of a DC power supply and immersed in a solution mainly containing an organic acid, and the coating is subjected to a semi-sealing treatment using boiling water. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2008-81815 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the part in Patent Document 1 has a problem in that the pores in the anodized film are not completely blocked, resulting in low durability against corrosive gases and plasma.
[0006] On the other hand, in order to improve the durability of the parts of Patent Document 1 against corrosive gases and plasma, a method of completely blocking the pores of the anodized film is considered. However, in this case, cracks are likely to occur in the anodized film when the temperature rises, and there is a risk of generating foreign matter consisting of small pieces of the anodized film. In order to prevent the generation of such foreign matter, it is desirable to further improve the heat resistance of aluminum materials having an anodized film on the surface.
[0007] The present invention has been made in view of the above background, and aims to provide a surface-treated aluminum material that has excellent corrosion resistance against corrosive gases and plasma and can suppress the occurrence of cracks, a manufacturing method thereof, and a component for semiconductor manufacturing equipment. [Means for solving the problem]
[0008] One aspect of the present invention is a method for manufacturing a semiconductor device, comprising: a protective coating formed on at least a portion of the surface of the base material, the protective coating including an oxide and a hydrated oxide of aluminum; The thickness of the protective coating is 2 μm or more, When the mass ratio of elements in the protective film is analyzed in the depth direction by glow discharge optical emission spectrometry, the integral value C of the mass ratio of aluminum atoms in the range from the surface of the protective film to a depth of 1 μm Al The integral value of the mass ratio of hydrogen atoms to H Ratio of C H / C Al The surface-treated aluminum material has a surface roughness of 0.2 or more and 0.7 or less.
[0009] Another aspect of the present invention is a method for producing a surface-treated aluminum material of the above aspect, an anodizing process for forming an anodized film having pores on the base material by anodizing the base material; and then a sealing step of immersing the base material in hot water to seal the pores in the anodized coating, thereby forming the protective coating on the base material, The method for producing a surface-treated aluminum material includes a step in which the product of the hot water temperature T [°C] and the immersion time t [hours] in the sealing step is more than 20°C·hours and less than 75°C·hours. Effect of the Invention
[0010] The surface of the base material in the surface-treated aluminum material (hereinafter referred to as "aluminum material") is provided with a protective film having a thickness of 2 μm or more and containing an oxide and a hydrated oxide of aluminum. The oxide and the hydrated oxide are determined by the integral value C Al The integral value of the mass ratio of hydrogen atoms to H Ratio of C H / C Al is distributed so as to be within the above-mentioned specific range. By providing such a protective coating on the base material, the aluminum material has high corrosion resistance and can suppress the occurrence of cracks.
[0011] In addition, in the manufacturing method of the aluminum material of the above aspect, the base material is anodized to form an anodized film, and then the pores of the anodized film are sealed under the specific conditions to form the protective film on the base material, thereby making it possible to easily obtain the aluminum material.
[0012] As described above, according to the above-mentioned aspects, it is possible to provide a surface-treated aluminum material that has excellent corrosion resistance against corrosive gases and plasma and can suppress the occurrence of cracks, a manufacturing method thereof, and a member for semiconductor manufacturing equipment. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a cross-sectional view showing a main part of an aluminum material in the embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a main part of a base material after the anodizing treatment step is completed in the manufacturing process of the aluminum material of the embodiment. [Diagram 3] FIG. 3 is an explanatory diagram showing the profile of the mass ratio of hydrogen atoms in the depth direction in the protective coating of the test material S1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] (Aluminum material) The material of the base material in the aluminum material can be appropriately selected from the group consisting of aluminum and aluminum alloys depending on the application of the aluminum material. For example, when it is intended to reduce outgassing from the aluminum material, it is preferable that the base material is composed of 1000 series aluminum or 3000 series aluminum alloy. As the 3000 series aluminum alloy, for example, an aluminum alloy having a chemical composition containing Mn (manganese): 1.0 mass% to 1.5 mass%, and containing one or more elements selected from the group consisting of Si (silicon), Fe (iron), Cu (copper), Mg, Cr (chromium), Zn (zinc) and Ti (titanium) as optional components, with the balance being Al and unavoidable impurities, can be used.
[0015] More specifically, the 1000 series aluminum constituting the base material of the aluminum material can be, for example, aluminum having a chemical composition represented by alloy number AA1100, AA1100A, AA1200, AA1200A, AA1300, AA1110, AA1120, AA1230, AA1230A, AA1235, AA1435, AA1145, AA1345, AA1445, AA1150, AA1350, AA1350A, AA1450, AA1370, AA1275, AA1185, AA1285, AA1385, AA1188, AA1190, AA1290, AA1193, AA1198, or AA1199.
[0016] Examples of the 3000 series aluminum alloys constituting the base material of the aluminum material include alloy numbers AA3002, AA3102, AA3003, AA3103, AA3103A, AA3103B, AA3203, AA3403, AA3004, AA3004A, AA3104, AA3204, AA3304, AA3005, AA3005A, AA3105, AA3105A, AA3105B, AA3007, and AA3107. , AA3207, AA3207A, AA3307, AA3009, AA3010, AA3110, AA3011, AA3012, AA3012A, AA3013, AA3014, AA3015, AA3016, AA3017, AA3019, AA3020, AA3021, AA3025, AA3026, AA3030, AA3130, or AA3065 may be used.
[0017] In addition, when the strength of the aluminum material is to be increased, it is preferable that the base material is made of a 5000 series aluminum alloy or a 6000 series aluminum alloy. For example, the 5000 series aluminum alloy may be an aluminum alloy containing 0.5% by mass or more and 5.0% by mass or less of Mg (magnesium), one or more elements selected from the group consisting of Si, Fe, Cu, Mn, Cr, Zn, and Ti as optional components, and the balance being Al and unavoidable impurities. For example, the 6000 series aluminum alloy may be an aluminum alloy containing 0.3% by mass or more and 1.5% by mass or less of Mg, 0.2% by mass or more and 1.2% by mass or less of Si, one or more elements selected from the group consisting of Fe, Cu, Mn, Cr, Zn, and Ti as optional components, and the balance being Al and unavoidable impurities.
[0018] More specifically, examples of the 5000 series aluminum alloys constituting the base material of the aluminum material include alloy numbers AA5182, AA5183, AA5005, AA5005A, AA5205, AA5305, AA5505, AA5605, AA5006, AA5106, AA5010, AA5110, AA5110A, AA5210, AA5310, AA5016, AA5017, AA5018, AA5018A, AA5019, AA5019A, AA5 119, AA5119A, AA5021, AA5022, AA5023, AA5024, AA5026, AA5027, AA5028, AA5040, AA5140, AA5041, AA5042, AA5043, AA5049, AA5149, AA5249, AA5349, AA5449, AA5449A, AA5050, AA5050A, AA5050C, AA5150, AA5051, AA5051A, AA5151, AA5251, AA5251A, AA5351, AA5451, AA5052, AA5252, AA5352, AA5154, AA5154A, AA5154B, AA5154C, AA5254, AA5354, AA5454, AA5554, AA5654, AA 5654A, AA5754, AA5854, AA5954, AA5056, AA5356, AA5356A, AA5456, AA5456A, AA5456B, AA5556, AA5556A, AA5556B, AA5556C, Aluminum alloys having the chemical composition represented by AA5257, AA5457, AA5557, AA5657, AA5058, AA5059, AA5070, AA5180, AA5180A, AA5082, AA5182, AA5083, AA5183, AA5183A, AA5283, AA5283A, AA5283B, AA5383, AA5483, AA5086, AA5186, AA5087, AA5187, or AA5088 may be used.
[0019] Examples of the 6000 series aluminum alloys constituting the base material of the aluminum material include alloy numbers AA6101, AA6101A, AA6101B, AA6201, AA6201A, AA6401, AA6501, AA6002, AA6003, AA6103, AA6005, AA6005A, AA6005B, AA6005C, AA6105, AA6205, AA6305, AA6006, AA6106, AA6206, AA6306, AA6008, AA6009, AA6010, AA6110, AA6110A, AA6011, AA6111, AA6012, AA6012A, AA6013, AA6113, AA6014, AA6015, AA6016 , AA6016A, AA6116, AA6018, AA6019, AA6020, AA6021, AA6022, AA6023, AA6024, AA6025, AA6026, AA6027, AA6028, AA6031, AA6032, AA6033, AA6040, AA6041, AA6042, AA6043, AA6151, AA6351, AA6351A, AA6451, AA6951, AA6053, AA6055, AA6056, AA6156, AA6060, AA6160, AA6260, AA6360, AA6460, AA6460B, AA6560, AA6660, AA6061, AA6061A, AA6261, AA6361, AA6162, Aluminum alloys having a chemical composition represented by AA6262, AA6262A, AA6063, AA6063A, AA6463, AA6463A, AA6763, A6963, AA6064, AA6064A, AA6065, AA6066, AA6068, AA6069, AA6070, AA6081, AA6181, AA6181A, AA6082, AA6082A, AA6182, AA6091, or AA6092 may be used.
[0020] A protective film containing an oxide of aluminum and a hydrated oxide is provided on the base material. The protective film can be obtained, for example, by anodizing the base material to form a porous anodized film made of an oxide of aluminum and having many pores on the surface of the base material, followed by a sealing treatment to block the pores of the anodized film with a hydrated oxide of aluminum.
[0021] The thickness of the protective film is 2 μm or more. This can protect the base material from corrosive gases and plasma, and improve the corrosion resistance of the aluminum material. From the viewpoint of corrosion resistance, the upper limit of the thickness of the protective film is not particularly limited, and the thicker the protective film, the more the corrosion resistance of the aluminum material can be improved. From this viewpoint, the thickness of the protective film is preferably 5 μm or more, and more preferably 10 μm or more. The upper limit of the thickness of the protective film in manufacturing is, for example, 200 μm. From the viewpoint of suppressing the occurrence of cracks in the protective film, the thickness of the protective film is preferably 100 μm or less.
[0022] The aluminum oxide and hydrated oxide in the protective film are the integral value C of the mass ratio of aluminum atoms in the range from the surface of the protective film to a depth of 1 μm when the mass ratio of elements in the protective film is analyzed in the depth direction by glow discharge optical emission spectrometry. Al The integral value of the mass ratio of hydrogen atoms to H Ratio of C H / C Al The integral ratio C is distributed so that it is 0.20 or more and 0.70 or less. H / C Al indicates the amount of hydrated oxide present near the surface of the protective film, and the ratio C H / C Al A higher value means that a greater amount of hydrated oxide is present near the surface of the protective coating.
[0023] Therefore, the ratio of integral values C H / C Al In a protective film having a ratio C of 0.20 or more, it is considered that the pores generated by the anodizing treatment are sufficiently blocked by hydrated oxides. H / C Al By making the integral ratio C 0.20 or more, it is possible to suppress the intrusion of corrosive gases, plasma, etc. into the pores, and the corrosion resistance of the aluminum material can be improved. H / CAl The value of is preferably 0.22 or more, more preferably 0.24 or more, even more preferably 0.26 or more, particularly preferably 0.28 or more, and most preferably 0.30 or more.
[0024] On the other hand, the ratio of integral values C H / C Al If the ratio is less than 0.20, the blocking of pores is likely to be insufficient, which may lead to a decrease in the corrosion resistance of the aluminum material.
[0025] In addition, the ratio of the integral values C H / C Al If the value of is excessively high, the protective coating may be prone to cracking when the temperature of the aluminum material rises. The reason for this is not entirely clear, but the following reasons are considered, for example. H / C Al If the value of is too high, it is considered that the protective film contains too much hydrated oxide or the crystallinity of the hydrated oxide is too high. H / C Al If the value of is excessively high, it is believed that the difference in the thermal expansion coefficients of the base material, the aluminum oxide, and the aluminum hydrated oxide will cause non-uniform thermal expansion within the protective coating, making cracks more likely to occur when the temperature rises.
[0026] From the viewpoint of suppressing the occurrence of cracks in the protective film, the integral ratio C H / C Al The value of the ratio C is set to 0.70 or less. H / C Al The value is preferably 0.68 or less, more preferably 0.66 or less, and even more preferably 0.64 or less.
[0027] Ratio of integral values in protective coating C H / C Al In forming the preferable range of the integral ratio C H / C AlThe upper and lower limits of can be arbitrarily combined. For example, the integral ratio C H / C Al The preferable range of may be 0.22 or more and 0.68 or less, 0.24 or more and 0.68 or less, 0.26 or more and 0.66 or less, 0.28 or more and 0.66 or less, or 0.30 or more and 0.64 or less.
[0028] The ratio of the integrals in the protective coating, C H / C Al Specifically, the calculation method of is as follows. First, the surface of the aluminum material is cleaned, and then a glow discharge optical emission spectrometer (for example, "GD750" manufactured by SPECTRUMA Analytik GmbH) is used to obtain a profile of the emission intensity of aluminum atoms and hydrogen atoms in the depth direction of the protective coating. At this time, the measurement conditions of the glow discharge optical emission spectrometer are anode diameter: 2.5 mm, output: 25 W, gas pressure: 3.5 hPa, and the capture interval of the emission intensity is 0.2 to 0.24 seconds. When measured under these conditions, the sputtering rate of the protective coating is about 50 to 90 nm / second.
[0029] The thus obtained profile of the emission intensity in the depth direction of aluminum atoms and hydrogen atoms is converted into a profile of mass ratio based on a calibration curve prepared in advance. Then, the mass ratio of each atom is integrated over a range from the surface of the protective coating to a position at a depth of 1 μm, and the integral value C of the mass ratio of hydrogen atoms is calculated. H and the integral value of the mass ratio of aluminum atoms, C Al The integral value C of the mass ratio of hydrogen atoms obtained above is calculated. H The integral value of the mass ratio of aluminum atoms, C Al By dividing by, the ratio of integral values C H / C Al can be calculated.
[0030] When a sealing test was performed according to the method specified in JIS H8683-2:2013, the mass loss per unit area of the aluminum material was 0.2 g / dm 2In this case, the corrosion resistance of the aluminum material can be further improved.
[0031] The specific method for the sealing test is as follows. First, 35 mL of phosphoric acid and 20 g of chromic anhydride are dissolved in water to prepare 1 L of test liquid. Next, a test piece including a protective film is taken from the aluminum material, and the area of the protective film on the test piece is measured. After removing any dirt from the surface of the test piece, the mass of the test piece is measured. Then, the test piece is immersed in the test liquid maintained at a temperature of 38°C ± 1°C for 15 minutes ± 5 seconds.
[0032] After the immersion of the test piece in the test solution is completed, the test piece is washed with running water and then washed with deionized water or distilled water. After the washed test piece is thoroughly dried, the mass of the test piece is measured.
[0033] The area A of the protective coating of the test piece obtained by the above (unit: dm 2 ), the mass m1 (unit: g) of the test piece before immersion in the test liquid, and the mass m2 (unit: g) of the test piece after immersion in the test liquid were used to calculate the mass loss per unit area δ based on the following formula (1): A (Unit: g / dm 2 ) can be calculated. δ A =(m1-m2) / A (1)
[0034] As described above, the aluminum material has excellent corrosion resistance against corrosive gases and plasmas, and can suppress the occurrence of cracks in the protective film even when the temperature rises. Therefore, the aluminum material is suitable for applications such as cover members provided around the fans of cooking appliances and members for semiconductor manufacturing equipment. More specifically, the aluminum material is suitable for use in, for example, chambers in semiconductor manufacturing equipment such as film formation equipment and etching equipment, and parts arranged in the chambers. Examples of film formation equipment include PVD (physical vapor deposition) equipment and CVD (chemical vapor deposition) equipment. Examples of etching equipment include dry etching equipment.
[0035] (Aluminum material manufacturing method) The method for producing the aluminum material includes: an anodizing process for forming an anodized film having pores on the base material by anodizing the base material; Thereafter, the method includes a sealing step of immersing the base material in hot water to seal the pores in the anodized film, thereby forming the protective film on the base material. In addition, the product of the hot water temperature T (unit: °C) and the immersion time t (unit: hour) in the sealing step is more than 20°C·hour and less than 75°C·hour.
[0036] In the anodizing process, a direct current is passed between the base material and the counter electrode while the base material and the counter electrode are immersed in an electrolyte to form an anodized film on the surface of the base material. The anodized film thus formed has a dense barrier layer formed on the base material and a porous layer formed on the barrier layer and having a large number of pores. The barrier layer and the porous layer are made of an oxide of aluminum such as alumina.
[0037] The electrolytic solution used in the anodizing process may be, for example, an acidic electrolytic solution containing an electrolyte such as sulfuric acid or phosphoric acid, or an alkaline electrolytic solution containing an electrolyte such as sodium metaborate. From the viewpoint of more easily forming an anodized film having a desired structure in the anodizing process and thus more easily forming the protective film, the electrolytic solution used in the anodizing process is preferably an acidic electrolytic solution, more preferably an acidic electrolytic solution containing an inorganic acid as an electrolyte, and even more preferably an acidic electrolytic solution containing sulfuric acid as an electrolyte. Note that anions derived from the electrolyte may be incorporated into the oxide film formed on the surface of the aluminum material by the anodizing process, and for example, an oxide film containing sulfur derived from sulfate ions is formed in an anodizing process using sulfuric acid.
[0038] The current density of the direct current in the anodizing process is, for example, 1 mA / cm 2More than 20mA / cm 2 The temperature of the electrolytic solution in the anodizing treatment step can be appropriately set within the range of 0° C. or more and 40° C. or less.
[0039] The thickness of the anodized film formed in the anodizing treatment step is preferably 2 μm or more. By making the thickness of the anodized film 2 μm or more, the thickness of the protective film after the sealing step can be more easily made 2 μm or more.
[0040] In the pore sealing step, the base material on which the anodized film was formed in the anodized treatment step is immersed in hot water. When the anodized film is immersed in hot water, the aluminum oxide constituting the anodized film reacts with water to form a hydrated oxide. This hydrated oxide blocks the pores in the anodized film, and the anodized film becomes the protective film.
[0041] In the sealing step, the base material is immersed in hot water so that the product of the temperature T (unit: °C) of the hot water in which the base material is immersed and the immersion time t (unit: hours) is more than 20 °C·hours and less than 75 °C·hours, preferably 21 °C·hours or more and 73 °C·hours or less, more preferably 23 °C·hours or more and 71 °C·hours or less. By immersing the base material in hot water so that the product of the hot water temperature and the immersion time is greater than 20 °C·hours, the aluminum oxide constituting the anodized film can be sufficiently reacted with the hot water, and the pores of the anodized film can be sufficiently blocked. This makes it possible to form a protective film with excellent corrosion resistance. If the product of the hot water temperature and the immersion time is 20 °C·hours or less, the reaction between the aluminum oxide and the hot water is insufficient, and the pores are likely to be insufficiently blocked. Therefore, in this case, there is a risk of the corrosion resistance of the aluminum material being reduced. From the standpoint of more reliably obtaining a protective film having excellent corrosion resistance, the product of the hot water temperature and the immersion time is preferably 21°C·hours or more, and more preferably 23°C·hours or more.
[0042] On the other hand, if the product of the hot water temperature and the immersion time is too high, cracks may easily occur in the protective film when the temperature of the aluminum material rises. This may be caused by excessive reaction between aluminum oxide and hot water. From the viewpoint of suppressing the occurrence of cracks in the protective film and improving the heat resistance of the aluminum material, the product of the hot water temperature and the immersion time is less than 75°C·hours. From the same viewpoint, the product of the hot water temperature and the immersion time is preferably 73°C·hours or less, and more preferably 71°C·hours or less.
[0043] The temperature T of the hot water in the sealing step is preferably 50°C or higher, more preferably 60°C or higher, and even more preferably 70°C or higher. By using high-temperature hot water in the sealing step, the immersion time required to achieve a desired degree of sealing can be easily shortened. As a result, the productivity of the aluminum material can be further improved. The upper limit of the temperature T of the hot water in the sealing step is 150°C. That is, in the sealing step, the base material may be immersed in boiling water, or superheated steam may be brought into contact with the base material.
[0044] The base material used in the anodizing process may be prepared by any method. For example, the method for producing an aluminum material further includes a casting step of producing an ingot made of aluminum or an aluminum alloy; a homogenization treatment step in which the ingot is subjected to homogenization treatment by holding the ingot at a temperature of 500° C. or more and 560° C. or less for 5 hours or more and 10 hours or less; The method may further include a hot rolling step of hot rolling the ingot that has been subjected to the homogenization treatment at a temperature of 500° C. or more and 560° C. or less to produce the base material.
[0045] As a casting method in the casting step, for example, DC casting can be adopted. The thickness of the ingot obtained in the casting step is not particularly limited, but the ingot may have a thickness of, for example, 600 mm or more.
[0046] In the homogenization process, the ingot obtained in the casting process is held at a temperature of 500°C to 560°C for 5 hours to 10 hours to perform homogenization. By setting the holding temperature and holding time in the homogenization process within the above-mentioned specific ranges, the structure of the ingot can be sufficiently homogenized. Then, by hot rolling such an ingot, a base material containing desired second phase particles can be obtained.
[0047] In the hot rolling process, the ingot that has been subjected to the homogenization treatment is hot rolled at a temperature of 500°C to 560°C. This allows the base material to be obtained. If the starting temperature in hot rolling is too low, the ingot will have high deformation resistance, which may cause cracks in the ingot during rolling or lead to poor productivity. On the other hand, if the starting temperature in hot rolling is too high, the ingot may melt locally due to processing heat during hot rolling.
[0048] In the manufacturing method, the base material obtained as described above may be directly subjected to anodizing treatment. The manufacturing method may also include a heat treatment step of subjecting the base material to heat treatment such as annealing, if necessary, after the hot rolling step and before the anodizing step.
[0049] Furthermore, the manufacturing method may include a pretreatment step of pretreating the base material after the hot rolling step and before the anodizing step. Examples of the pretreatment of the base material include degreasing treatment such as alkaline degreasing treatment, and polishing treatment such as mechanical polishing, chemical polishing, and electrolytic polishing. In the pretreatment step, one of the above pretreatments may be performed alone or two or more pretreatments may be appropriately combined depending on the desired characteristics of the aluminum material.
[0050] When an alkaline degreasing treatment is performed in the pretreatment step, the gloss of the anodized film obtained after anodizing treatment can be reduced, and an aluminum material having a matte appearance can be obtained. When a polishing treatment is performed in the pretreatment step, the gloss of the anodized film obtained after anodizing treatment can be increased, and an aluminum material having a glossy appearance can be obtained. From the viewpoint of further increasing the gloss of the aluminum material, it is preferable to perform an electrolytic polishing treatment on the base material in the pretreatment step. EXAMPLES
[0051] An embodiment of the surface-treated aluminum material and its manufacturing method will be described with reference to Figs. 1 to 3. As shown in Fig. 1, the surface-treated aluminum material 1 of this embodiment has a base material 2 made of aluminum or an aluminum alloy, and a protective coating 3 containing an oxide and a hydrated oxide of aluminum and formed on at least a part of the surface of the base material 2. The thickness of the protective coating 3 is 2 µm or more. When the mass ratio of elements in the protective coating 3 is analyzed in the depth direction by glow discharge optical emission spectrometry, the integral value C of the mass ratio of aluminum atoms in the range from the surface of the protective coating 3 to a depth of 1 µm is Al The integral value of the mass ratio of hydrogen atoms to H Ratio of C H / C Al is between 0.2 and 0.7.
[0052] Table 1 shows specific examples of the aluminum material 1 (test materials S1 to S5). The manufacturing method of the test materials S1 to S5 is, for example, as follows. First, an aluminum plate having a chemical composition represented by alloy number A6016 and a thickness of 1.1 mm is prepared as the base material 2. This base material 2 is subjected to a pretreatment for anodizing. Specifically, as the pretreatment, an alkali etching treatment is performed by immersing the base material 2 in a sodium hydroxide aqueous solution having a concentration of 5 mass% and a temperature of 55°C. Then, the base material 2 is immersed in nitric acid having a concentration of 30 mass% to perform a desmutting treatment. Then, the base material 2 is immersed in a mixed solution of phosphoric acid and sulfuric acid at a volume ratio of phosphoric acid:sulfuric acid = 7:3 at a temperature of 85°C to perform a chemical polishing treatment. After the chemical polishing treatment, a desmutting treatment is performed again under the same conditions as those described above.
[0053] After the base material 2 has been pretreated as described above, the base material 2 is anodized to form an anodized film 30 on the surface of the base material 2. The electrolyte used in the anodization is an aqueous sulfuric acid solution with a concentration of 15% by mass, and the temperature of the electrolyte is 5° C. The current density in the anodization is 10 mA / cm 2 The treatment time is 60 minutes. The anodic oxide film 30 thus formed is a so-called porous type anodic oxide film, and as shown in Fig. 2, it has a barrier layer 31 formed on the base material 2, and a porous layer 32 formed on the barrier layer 31 and having a large number of pores 321. The thickness of the anodic oxide film 30 formed by anodizing under the above-mentioned conditions is approximately 15 µm.
[0054] After the anodizing treatment, the base material is immersed in hot water under the conditions shown in Table 1 to perform a sealing treatment. In this manner, test materials S1 to S5 shown in Table 1 can be obtained. Note that test materials R1 to R3 shown in Table 1 are test materials for comparison with test materials S1 to S5. The manufacturing method of test materials R1 to R3 is the same as that of test materials S1 to S5, except that the hot water temperature and immersion time in the sealing treatment were changed as shown in Table 1.
[0055] Next, the methods for evaluating the various properties of the test materials S1 to S5 and the test materials R1 to R3 shown in Table 1 will be described.
[0056] [Distribution of hydrogen atoms and aluminum atoms] After cleaning the surface of each test material, a glow discharge optical emission spectrometer (SPECTRUMA Analytik GmbH, "GD750") is used to obtain a profile of the emission intensity of aluminum atoms and hydrogen atoms in the depth direction of the protective film. The measurement conditions for the glow discharge optical emission spectrometer are anode diameter: 2.5 mm, output: 25 W, gas pressure: 3.5 hPa, and the emission intensity capture interval is 0.2 to 0.24 seconds. Note that when measured under these conditions, the sputtering rate of the protective film is approximately 50 to 90 nm / second.
[0057] The thus obtained profile of the emission intensity in the depth direction of aluminum atoms and hydrogen atoms is converted into a mass ratio profile based on a calibration curve prepared in advance. FIG. 3 shows an example of a profile of the mass ratio of hydrogen atoms in test material S1. The vertical axis of FIG. 3 is the mass ratio of hydrogen atoms (unit: mass%), and the horizontal axis is the depth from the surface of the protective coating (unit: μm). In the thus obtained profile, the mass ratio of each atom is integrated over a range from the surface of the protective coating to a depth of 1 μm, and the integral value C of the mass ratio of hydrogen atoms is calculated. H and the integral value of the mass ratio of aluminum atoms, C Al The integral value C of the mass ratio of hydrogen atoms obtained above is calculated. H The integral value of the mass ratio of aluminum atoms, C Al By dividing by the ratio C H / C Al Calculate.
[0058] [Sealing degree of protective film] A sealing test is conducted according to the method specified in JIS H8683-2:2013, and the mass loss per unit area of each test material is measured.
[0059] [Heat resistance] Heat resistance is evaluated based on the exposure rate of the base material, which is measured by the following method. First, the test material is heated for 4 hours in an oven set at 200°C. After the test material is removed from the oven and cooled to room temperature, an evaluation area is set on the protective film, and the rest of the surface of the test material other than the evaluation area is covered with silicone resin.
[0060] Next, a 5% by mass NaCl aqueous solution and a 99.7% by mass acetic acid are prepared, and acetic acid is added to the NaCl aqueous solution so that the volume ratio of the NaCl aqueous solution to the acetic acid is NaCl aqueous solution:acetic acid = 1000:1 to prepare a measurement solution. The test piece, counter electrode, and reference electrode electrically connected to the potentiostat are immersed in this solution, and left to stand for 30 minutes to stabilize the potential of the measurement section. For example, an Ag / AgCl electrode can be used as the reference electrode.
[0061] After the potential of the measurement part is stabilized, a voltage is applied between the test piece and the counter electrode using a potentiostat, and the potential of the measurement part is swept at a sweep rate of 20 mV / min until the potential of the measurement part reaches -2000 mV with respect to the reference electrode. The polarization curve of the test material after heating is obtained by measuring the current density flowing through the measurement part at this time. In addition, the polarization curve of the base material is obtained by performing the same measurement using the base material after the pretreatment of the anodizing treatment by the above-mentioned method.
[0062] Next, the center of the potential region showing the hydrogen diffusion limiting current is determined in the polarization curve of the base material. Then, the current density in the center of the potential region is calculated. In addition, in the polarization curve of the heated test material, the current density in the same potential as the center of the potential region in the polarization curve of the base material is calculated.
[0063] The current density calculated based on the polarization curve of the test material after heating can be used as an index of the contact area between the base material and the measurement solution in the test material after heating, and the larger the current density value, the larger the contact area between the base material and the measurement solution. Therefore, the ratio of the current density calculated using the test piece after heating to the current density calculated using the base material can be used as an index of the increase rate of the exposed area of the base material due to heating. More specifically, for example, when defects such as cracks are formed in the protective film of the test material after heating, the base material may be exposed by the cracks. Therefore, in this case, the current density ratio of the test material after heating to the base material becomes large. Table 1 shows the current density ratio of each test material.
[0064] [Table 1]
[0065] As shown in Table 1, the test materials S1 to S5 were subjected to the sealing treatment so that the product of the hot water temperature and the immersion time in the sealing treatment step was within the above-mentioned specific range. Therefore, the integral value C of the mass ratio of aluminum atoms in these test materials Al The integral value of the mass ratio of hydrogen atoms toH Ratio of C H / C Al is within the above-mentioned specific range. Furthermore, these test materials have a low mass loss in a sealing test and are excellent in corrosion resistance against corrosive gases, plasma, etc. Furthermore, these test materials have a low current density ratio and can suppress the occurrence of cracks in the protective coating even when the temperature rises.
[0066] On the other hand, in the case of test materials R1 and R3, the product of the hot water temperature and the immersion time in the sealing treatment is higher than the specific range, so the hydration reaction between the aluminum oxide and the hot water proceeds excessively. Therefore, the current density ratio of test materials R1 and R3 is higher than that of test materials S1 to S5, and cracks are more likely to occur when the temperature rises.
[0067] In the case of test material R2, the product of the hot water temperature and the immersion time in the sealing treatment was lower than the specific range, so the pores in the anodized film were not sufficiently blocked, and therefore test material R2 had a higher mass loss in the sealing test and was inferior in corrosion resistance compared to test materials S1 to S5.
[0068] The above describes aspects of the surface-treated aluminum material and the manufacturing method thereof according to the present invention based on the examples. However, the specific aspects of the surface-treated aluminum material and the manufacturing method thereof according to the present invention are not limited to the aspects of the examples, and the configurations can be changed as appropriate within the scope of the invention without impairing the spirit of the invention. [Explanation of symbols]
[0069] 1. Surface-treated aluminum material 2 Base material 3 Protective Coating
Claims
1. A base material made of aluminum or an aluminum alloy; a protective coating formed on at least a portion of the surface of the base material, the protective coating including an oxide and a hydrated oxide of aluminum; The thickness of the protective coating is 2 μm or more, When the mass ratio of elements in the protective film is analyzed in the depth direction by glow discharge optical emission spectrometry, the integral value C of the mass ratio of aluminum atoms in the range from the surface of the protective film to a depth of 1 μm Al The integral value C of the mass ratio of hydrogen atoms to H Ratio C H / C Al A surface-treated aluminum material, wherein the refractive index is 0.2 or more and 0.7 or less.
2. When a sealing test was performed according to the method specified in JIS H8683-2:2013, the mass loss per unit area was 0.2 g / dm 2 The surface-treated aluminum material according to claim 1, wherein:
3. A semiconductor manufacturing equipment member comprising the surface-treated aluminum material according to claim 1 or 2.
4. A method for producing a surface-treated aluminum material according to claim 1 or 2, an anodizing process for forming an anodized film having pores on the base material by anodizing the base material; and then a sealing step of immersing the base material in hot water to seal the pores in the anodized coating, thereby forming the protective coating on the base material. The method for producing a surface-treated aluminum material, wherein the product of the hot water temperature T [° C.] and the immersion time t [hours] in the sealing step is more than 20° C.-hours and less than 75° C.-hours.
Citation Information
Patent Citations
Component for substrate treating apparatus and method for forming film
JP2008081815A
Cited By
Surface-treated aluminum materials, components for semiconductor manufacturing equipment, and electrostatic chucks
JP2026133245A
Surface-treated aluminum material and method for manufacturing the same
JP2026133247A
Method for manufacturing surface-treated aluminum material and method for manufacturing components for plasma processing apparatus
JP2026133249A
Method for manufacturing surface-treated aluminum material and method for manufacturing components for plasma processing apparatus
JP7833581B1
Manufacturing method for surface-treated aluminum material
JP7842267B1