Glass cloth

The controlled heat cleaning and silane treatment of quartz glass cloth with a slow temperature increase and low dew point address the strength variations issue, producing a high-strength, low-loss-tangent glass cloth suitable for advanced communication substrates.

JP2024150218APending Publication Date: 2024-10-23SHIN ETSU CHEMICAL CO LTD

Patent Information

Application Number
JP2023063528
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23

AI Technical Summary

Technical Problem

Quartz glass cloth, with a composition of 95% by mass or more, exhibits low tensile strength and significant variations in tensile strength between the winding core side and the unwinding side due to microcracks caused by thermal expansion during heat cleaning, which limits its use in producing substrates for high-speed communication applications.

Method used

A manufacturing process involving a controlled heat cleaning method with a temperature increase rate of 100°C/h or less, a dew point of 15°C or lower, and treatment with a silane coupling agent to enhance tensile strength and reduce dielectric loss tangent, resulting in a glass cloth with 0.10 GPa or more tensile strength at both ends and a difference of 0.15 GPa or less between the core and unwinding sides.

Benefits of technology

The process produces quartz glass cloth with consistent tensile strength and low dielectric loss tangent, enhancing the reliability and productivity of substrates for 5G and 6G communication applications by minimizing tears and ensuring uniform strength across the roll.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150218000003
    Figure 2024150218000003
  • Figure 2024150218000001
    Figure 2024150218000001
  • Figure 2024150218000002
    Figure 2024150218000002
Patent Text Reader

Abstract

To provide a quartz glass cloth with small variation in tensile strength between the winding core side and the unwinding side in a roll while keeping a low dielectric tangent of a glass cloth having a SiO2 composition amount of 95 mass% or more, and a production method for the same.SOLUTION: A glass cloth is obtained by treating a glass cloth having a SiO2 composition amount of 95 mass% or more with a silane coupling agent, where the dielectric tangent at 10 GHz is 0.0008 or lower, the gas permeability is 75 cm3 / (cm2 s) or lower, the longitudinal tensile strengths at both ends of the winding core side and the unwinding side of the roll are each 0.10 GPa or higher, and the difference in tensile strength between both is 0.15 GPa or less when the glass cloth is wound into a roll state.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a quartz glass cloth wound into a roll having a small difference in tensile strength between the core side and the unwinding side, and a method for producing the same. [Background technology]

[0002] At present, with the high performance and high-speed communication of information terminals such as smartphones, the printed wiring boards used are becoming denser and thinner, and at the same time, the dielectric constant and the dielectric loss tangent are becoming lower. As an insulating material for the printed wiring board, a laminated board is widely used, which is made by laminating prepregs obtained by impregnating glass cloth with a thermosetting resin such as epoxy resin (hereinafter referred to as "matrix resin") and curing the prepreg by heating and pressing. It is known that the transmission loss of a signal in a board is improved as the dielectric constant (ε) and the dielectric loss tangent (tanδ) are smaller, as shown by the Edward A. Wolff formula: transmission loss ∝√ε×tanδ, and it is known that the contribution of the dielectric loss tangent to the transmission loss is large, particularly from the above formula. For this reason, a low dielectric loss tangent is required for the glass cloth, and glass cloths with improved dielectric properties have been proposed as described in Patent Documents 1 to 4. In particular, Patent Document 4 reports a quartz cloth with a very excellent dielectric loss tangent.

[0003] In addition, demand for circuit boards for future 5G and 6G communication applications is higher than ever before, and there is a need to increase the speed of circuit board production lines in order to improve productivity. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-292567 [Patent Document 2] Patent No. 3896636 [Patent Document 3] Patent No. 6866178 Summary of the Invention [Problem to be solved by the invention]

[0005] Since the tensile strength of glass cloth, which is a substrate raw material, is low, the coating of resin onto the glass cloth is a rate-limiting factor in the production of substrates. In particular, although quartz glass cloth has a large amount of SiO2 and a dielectric loss tangent superior to multi-component glass, it is hard and brittle, and therefore has low tensile strength. Furthermore, glass cloth is generally wound around a paper tube or a plastic tube, and the tensile strength of the quartz glass cloth is large within the same roll, and there is a problem that the tensile strength of the quartz glass cloth is broken at the part with weak tensile strength when it is continuously processed under the same conditions in the substrate production line. In particular, there is a problem that the tensile strength difference between both ends of the roll's core side and the unwinding side is large. In particular, for glass cloth with an SiO2 composition amount of 95% by mass or more, it is desired to improve the tensile strength while maintaining a low dielectric loss tangent. For this reason, the object is to provide a quartz glass cloth and a manufacturing method thereof, which has a small tensile strength variation between the core side and the unwinding side in the roll while maintaining a low dielectric loss tangent of glass cloth with an SiO2 composition amount of 95% by mass or more. [Means for solving the problem]

[0006] As a result of intensive research to achieve the above object, the present inventors have found that the cause of the decrease in tensile strength of glass cloth (hereinafter sometimes referred to as quartz glass cloth) having an SiO2 composition of 95 mass% or more is microcracks that occur when filaments of the quartz glass cloth rub against each other due to thermal expansion of the filaments caused by a sudden temperature change during the heat cleaning process to remove the sizing agent applied when the glass cloth is woven. In addition, they have found that the stress on the filaments due to thermal expansion is particularly large toward the inside of the roll of the quartz glass cloth wound into a roll during heat cleaning, causing a decrease in tensile strength, which causes variation in the tensile strength of the quartz glass cloth when made into a product.

[0007] Therefore, the present invention provides the following inventions. 1. A glass cloth having an SiO2 composition amount of 95 mass% or more is a glass cloth treated with a silane coupling agent, Dielectric tangent at 10GHz is 0.0008 or less, Ventilation rate is 75cm 3 / (cm 2 s) or less, The glass cloth is wound into a roll, A glass cloth having a longitudinal tensile strength of 0.10 GPa or more at both ends of the core side and the unwinding side of a roll, with the difference between the tensile strengths being 0.15 GPa or less. 2. The glass cloth according to 1, wherein the difference in tensile strength in the longitudinal direction is 0.10 GPa or less. 3. A prepreg comprising the glass cloth according to 1 or 2 and an organic resin. 4. A laminate comprising the glass cloth according to 1 or 2 and an organic resin. 5. A printed wiring board comprising the glass cloth according to 1 or 2 and an organic resin. 6. A heat cleaning method for removing a sizing agent adhering to the surface of a glass cloth having an SiO2 composition amount of 95 mass% or more, comprising the steps of: The glass cloth to which the sizing agent is attached is A heat cleaning method in which the material is heated from room temperature to a specified temperature at a rate of 100°C / h or less. 7. The heat cleaning method according to 6, wherein the glass cloth having the sizing agent adhered thereto is heated in an environment in which the dew point is 15°C or lower when the temperature is lowered. Effect of the Invention

[0008] It is possible to provide a quartz glass cloth having a low dielectric tangent of glass cloth with an SiO2 composition amount of 95 mass % or more, and having small variation in tensile strength within a roll, and a manufacturing method thereof. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic diagram showing a roll-shaped glass cloth of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [Glass cloth] The glass cloth of the present invention is a glass cloth having an SiO2 composition amount of 95 mass% or more, which is treated with a silane coupling agent, Dielectric tangent at 10GHz is 0.0008 or less, Ventilation rate is 75cm 3 / (cm 2 s) or less, The glass cloth is wound into a roll, The glass cloth has a longitudinal tensile strength of 0.10 GPa or more at both ends of the core side and the unwinding side of the roll, and the difference between the tensile strengths is 0.15 GPa or less. Hereinafter, the "glass cloth having an SiO2 composition amount of 95 mass% or more" may be referred to as a "quartz glass cloth", and the "glass cloth treated with a silane coupling agent" of the present invention may be referred to as a "silane-treated glass cloth".

[0011] [SiO2 composition] The silane-treated glass cloth of the present invention has a SiO2 composition amount of 95% by mass or more. From the viewpoints of electrical properties such as dielectric loss tangent and physical properties such as thermal expansion, the SiO2 composition amount is preferably 97% by mass or more, more preferably 99% by mass or more, and even more preferably 99.9% by mass or more.

[0012] [Dissipation factor] The silane-treated glass cloth of the present invention has a dielectric loss tangent at 10 GHz of 0.0008 or less, more preferably 0.0008 or less, more preferably 0.0006 or less, and even more preferably 0.0003 or less. The method for measuring the dielectric loss tangent is based on a resonance method, specifically based on the description of the examples described later. Since there is almost no change in the dielectric loss tangent between the core side and the unwinding side of the roll, the sampling location is not particularly limited, but the unwinding side is preferable from the viewpoint of workability. The measurement position on the unwinding side is 10 m from the unwinding, excluding the three layers on the surface wound in a roll shape.

[0013] [Breathability] The air permeability of the silane-treated glass cloth of the present invention is 75 cm3 / (cm 2 s) or less, 50cm 3 / (cm 2 s) or less is preferable, 30cm 3 / (cm 2 The lower limit is not particularly limited, and 0 ccm 3 / (cm 2 The glass cloth of the present invention may have an air permeability of 75 cm 3 / cm 2 If it is larger than / s, when resin is applied during the manufacture of prepregs, etc., the amount of resin in the gaps between the filaments varies, resulting in places where the resin is insufficient, which adversely affects the reliability of the board. The air permeability can be measured by the method described in JIS R3420. There is almost no difference in air permeability between the core side and the unwinding side of the roll, so the sampling location is not particularly limited, but the unwinding side is preferable from the viewpoint of workability. The measurement position on the unwinding side is 10 m into the unwinding, excluding the three layers on the surface wound in a roll shape.

[0014] [Rolled glass cloth] The glass cloth of the present invention is the glass cloth wound into a roll. The winding core is not particularly limited, and may be cylindrical. The diameter of the winding core is appropriately selected in the range of 50 to 400 mm, and more preferably in the range of 100 to 200 mm.

[0015] [Glass cloth length] The length of the silane-treated quartz glass cloth of the present invention is preferably 500 to 4,000 m, more preferably 1,000 to 2,000 m. If it is less than 500 m, the productivity decreases, and if it exceeds 4,000 m, the diameter and weight of the roll become too large, making it difficult to handle, and therefore inappropriate. As a method for measuring the length of the silane-treated quartz glass, it is preferable to measure it with a measuring device attached to a device that can rewind glass cloth, such as a fabric inspection machine or a rewinding machine. In particular, since glass cloth basically includes a fabric inspection process, it is preferable to measure the length at the same time as the fabric inspection using a fabric inspection machine. In addition, since the tensile strength of the quartz glass cloth of 0 to 100 m on the core side during heat cleaning is most likely to decrease, this portion may be removed as appropriate. When removing the quartz glass cloth, it is preferable to remove it after the silane treatment from the viewpoint of handling, and as a removal method, it can be removed by unwinding while measuring the actual length of the relevant portion with a device that can rewind glass cloth, such as a fabric inspection machine or a rewinding machine.

[0016] [Glass cloth width] The width of the silane-treated quartz glass of the present invention is preferably 1,300 mm or less, and can be appropriately adjusted to 1,200 to 1,300 mm, 500 to 630 mm, etc. An example of a method for adjusting the cloth width is adjustment with a slitter. It is preferable to seal the pores with a thermoplastic resin, a thermosetting resin, or a UV-curable resin before slitting, and then cut the glass to the desired width with a slitter.

[0017] [Tensile strength of glass cloth] The glass cloth of the present invention has a longitudinal tensile strength of 0.10 GPa or more at both ends of the core side and the unwinding side of the roll. Here, the longitudinal direction refers to the unwinding direction of the cloth, and the transverse direction refers to the width direction of the cloth. The longitudinal length is the length of the glass cloth, and the longitudinal length is the width. The measurement position on the core side is within 10 m from the start of winding, excluding the three innermost layers wound in a roll, and usually a 1 m portion is used. The measurement position on the unwinding side is within 10 m from the end of unwinding the three layers of the surface wound in a roll, and usually a 1 m portion is used. The innermost and outermost three layers of the roll-shaped glass cloth are easily affected by external factors because they come into contact with the core and packaging material, and are easily weakened in strength. Therefore, the strength of the core side and the unwinding side in the present invention is applied excluding the three layers.

[0018] The longitudinal tensile strength of both ends of the core side and unwinding side of the roll is 0.10 GPa or more, preferably 0.12 GPa or more, and more preferably 0.15 GPa or more. The longitudinal direction here refers to the unwinding direction of the cloth, and the transverse direction refers to the width direction of the cloth. If the longitudinal tensile strength is less than 0.10 GPa, problems such as breakage during resin coating in the next process will occur. There is no particular upper limit, and it may be 0.5 GPa or more. In the transverse direction, 0.12 GPa or more is preferable, and 0.15 GPa or more is more preferable.

[0019] In addition, the difference in the longitudinal tensile strength between both ends of the core side and the unwinding side of the roll is 0.15 GPa or less, preferably 0.12 GPa or less, and more preferably 0.10 GPa or less. If it exceeds 0.15 GPa, problems such as the cloth suddenly breaking at the part with weak tensile strength during resin coating under the same conditions will occur. There is no particular restriction on the lower limit, and it may be 0 GPa. In the transverse direction, it is preferably 0.12 GPa or less, and more preferably 0.10 GPa or less. In addition, since the parts with strong and weak tensile strength of the glass cloth are switched between the core side and the unwinding side depending on the number of rewinds and inspections, it cannot be said that the tensile strength of the core side is weak in general.

[0020] [Method of manufacturing silane-treated quartz glass] The quartz glass cloth having an SiO2 content of 95 mass% or more, which is used in the manufacture of the silane-treated glass cloth of the present invention, can be manufactured, for example, by the following method. Quartz glass having a diameter of 50 to 500 mm is melted at 1,700 to 2,300°C, and the filamentous product is wound up to obtain a quartz fiber having a diameter of 200±100 μm. If the melting temperature is within this range, stable drawing is possible.

[0021] Since the strength of the quartz yarn is very weak, it is preferable to coat it with a coating agent before winding it up. As the coating agent, an acrylate resin with excellent curing properties that can be cured with UV is preferable. The thickness of the coating film is preferably 5 μm or more because a sufficient reinforcing effect can be obtained. The quartz filament can be formed into a desired filament diameter by, for example, heating the above quartz yarn with a mixed flame of oxygen and hydrogen at 1700 to 2,300°C. In the present invention, the filament diameter is 3 to 20 μm, and preferably 3 to 8 μm.

[0022] A quartz glass strand can be produced by bundling 30 to 250 quartz filaments, preferably 100 to 200 quartz filaments, and a bundling agent is used to bundle the strands. The bundling agent is mainly made of starch, and softeners and lubricants can be added to impart functionality. The bundling agent composition is generally called a sizing agent. Quartz glass yarn is obtained by twisting the strands produced as described above. The twisting frequency is preferably 10 to 30 times per meter.

[0023] The quartz glass cloth can be obtained by weaving quartz yarn. The quartz glass cloth of the present invention is not particularly limited, but has a basis weight of 10 to 100 g / m 2 The weaving method is not particularly limited, but examples thereof include weaving methods using an air jet loom, a water jet loom, a rapier loom, a shuttle loom, etc. When weaving is performed using an air jet loom, etc., polyvinyl alcohol (PVA) or starch can be attached as a secondary sizing agent to obtain further lubricity.

[0024] [Opening of glass cloth] The glass cloth is preferably subjected to an opening treatment after weaving in order to enhance the impregnation with the resin. The opening method is not particularly limited, but examples thereof include an opening treatment method using ultrasonic waves, a method using a high-pressure columnar water flow, a method of spraying a diffusion spray into the atmosphere, and a method using a gas-liquid mixed mist with an adjusted air-water volume ratio. In particular, the method using a gas-liquid mixed mist is preferable because it can efficiently open the fibers while suppressing misalignment and fluffing of the strands. The gas-liquid mixed mist is a gas-liquid mixed mist in which a gas is mixed with a liquid to atomize the liquid.

[0025] The liquid to be mixed (aqueous liquid W1) may be water or a liquid in which one or more selected from alcohol, surfactant, silane coupling agent, lubricant, and colloidal silica are blended with water. These may be appropriately selected depending on the glass type, surface condition, thickness, etc. of the glass cloth. In addition, the sizing agent attached to the glass fiber bundle may be dissolved. The proportion of water in the liquid to be mixed is preferably 10 to 100% by mass, more preferably 50 to 100% by mass, and the upper limit may be 95% by mass or 100% by mass.

[0026] The types of gas to be mixed (G1) include air, nitrogen gas, and inert gas, and can be used alone or in combination of two or more. Among them, compressed air is preferred. As conditions for fiber-opening in the gas-liquid mixed mist, it is preferred that the liquid and gas are mixed at an air-water volume ratio V1 / V2 of the gas consumption amount V1 and the liquid spray amount V2 in the range of 5 to 150, the sum P1+P2 of the gas pressure P1 and the liquid pressure P2 is 0.2 to 2.0 MPa, and the pressure ratio P1 / P2 is 0.2 to 1.5. Such conditions are suitable in that the strands of the quartz glass cloth can be efficiently opened while suppressing misalignment and fluffing.

[0027] The liquid temperature of the liquid used in the gas-liquid mixture mist is preferably 20 to 90°C. By keeping the liquid temperature within the above range, the softening of the sizing agent attached to the glass fiber bundles is promoted, and the opening effect of the glass cloth in the above-mentioned opening treatment step can be improved.

[0028] In the present invention, the timing of the opening is preferably before heat cleaning. That is, in order to suppress a sudden temperature change during heat cleaning, the temperature rise rate is set to 100°C / h or less as described below, and further, by performing the opening treatment before heat cleaning, the contact area of ​​the filaments passing through is reduced, and the occurrence of microcracks is suppressed, thereby further reducing the variation in tensile strength.

[0029] The degree of fiber opening can be evaluated by measuring the air permeability, which can be measured according to the air permeability described in JIS R3420. 3 / (cm 2 s) or less, 50cm 3 / (cm 2 s) or less is preferable, 30cm 3 / (cm 2 ·s) or less is more preferable. By setting the above range, the contact area between the filaments is reduced during heat cleaning described below, thereby suppressing friction between the filaments due to thermal expansion of the filaments, and it is considered that the decrease in the tensile strength of the quartz glass cloth can be further suppressed. The air permeability of the glass cloth of the present invention is largely dependent on the fiber opening operation, and although the value of the air permeability varies slightly depending on post-operations such as silane treatment, the air permeability of the glass cloth before heat cleaning is 75 cm 3 / (cm 2 If the air permeability after silane treatment is less than 75 cm 3 / (cm 2 The measurement method is the same as that after silane treatment.

[0030] [Glass cloth heat cleaning process] The sizing agent remains on the surface of the quartz glass cloth after weaving, and the remaining sizing agent deteriorates the dielectric properties. In addition, the silane coupling agent treatment on the quartz glass cloth becomes insufficient, resulting in poor adhesion with the resin. Therefore, deoiling is generally performed after weaving to remove the adhering sizing agent. The deoiling process includes a method of washing with water or an organic solvent, and a method called a process of burning and removing organic matter, and the heat cleaning process, which is a heating process, is common because it can perform deoiling more reliably. This process can be performed using a flow or batch type heating furnace, but the flow type burns off the sizing agent at high temperature all at once, which causes problems such as a decrease in the tensile strength of the glass cloth and residual burnt sizing agent, and the batch type is common, in which organic matter is slowly burned off at 350 to 900 ° C. and removed. In the batch type heat cleaning, the glass cloth is wrapped around a metal tube and heated. The thermal expansion difference between quartz glass and metal is large, and if the quartz glass is wrapped around a metal tube as it is, the quartz glass cloth will break on the winding core side or the tensile strength will be significantly reduced. Therefore, by wrapping E-glass cloth between the metal tube and the quartz glass cloth as a buffer material, the thermal expansion difference can be alleviated and the quartz glass cloth can be prevented from breaking or from losing its tensile strength. The thickness of the E-glass wrapping is Winding thickness (mm) = (thermal expansion coefficient of metal tube (ppm / ℃) - thermal expansion coefficient of quartz glass (ppm / ℃)) x heating temperature (℃) x outer diameter of metal tube (mm) It is sufficient to make it so that the above is true.

[0031] [Heat cleaning temperature] In the present invention, the heat cleaning temperature is preferably 350 to 900°C. The higher the temperature, the more the reaction of SiO2+H2O⇔Si-OH leans to the left, and the dielectric tangent decreases, but the tensile strength decreases, so the temperature is preferably 400 to 700°C. If the temperature is less than 350°C, not only is the above reaction less likely to lean to the left, but the sizing agent remains unburned, which has an adverse effect on the dielectric tangent and silane treatment. If the temperature exceeds 900°C, the quartz glass filaments may fuse together, causing a significant decrease in tensile strength.

[0032] [Heat cleaning time] In the present invention, the heat cleaning time may be any time as long as the sizing agent is removed, and for example, the heating temperature (°C) x heating time (h) is 450°C·h or more.

[0033] [Heat cleaning temperature rise rate] In the present invention, the temperature rise rate during heat cleaning is preferably 100°C / h or less, more preferably 50°C / h or less, and even more preferably 25°C / h or less. When heating at 450°C or more, particularly 500°C or more, the thermal expansion value of the filament also increases, so a lower temperature rise rate is suitable at higher temperatures. Specifically, when the heating temperature exceeds 400°C, It is preferable to appropriately adjust the temperature rise rate so that it is (°C / h) = 100 (°C / h) - (heating temperature (°C) - 400°C) / 6 or less. There is no particular lower limit, but from the viewpoint of productivity, it is preferable to have a rate of 5°C / h or more. Furthermore, if it is within the above range, the temperature may be raised in multiple steps.

[0034] When the quartz glass cloth is heated at a temperature rise rate within this range, microcracks in the filaments due to sudden thermal expansion can be suppressed. The filaments facing the vertical direction are connected as a single strand from the winding core to the outside, so the longer the cloth is, the more likely cracks due to thermal expansion are to occur. The vertical direction here refers to the unwinding direction of the cloth, and the horizontal direction refers to the width direction of the cloth. Thermal expansion also occurs in the horizontal filaments, but the tensile strength is less likely to decrease compared to the vertical direction. The glass cloth of the present invention has a small difference in tensile strength between the vertical and horizontal directions, and can effectively suppress a decrease in the vertical tensile strength inside the winding core, especially during heat cleaning.

[0035] [Heat cleaning environment] In the present invention, when the quartz glass cloth is heat-cleaned, the dew point during heat cleaning can be controlled to not only reduce the dielectric tangent but also increase the tensile strength of the quartz glass cloth. At least during the temperature drop, it is preferable to perform the heat-cleaning in an environment with a dew point of 15°C or less. An example of an environment with a dew point of 15°C or less is a method of making the inside of the furnace a gas with a dew point of 15°C or less. Examples of such a gas include dry air and inert gas. The reaction of SiO2+H2O⇔Si-OH tends to lean to the right at 100 to 300°C. As a preferred method, at least during the temperature drop through the temperature range of 100 to 300°C, the air is filled with dry air with a dew point of 15°C or less, thereby preventing the increase of SiOH groups in the quartz glass cloth and obtaining a glass cloth with a superior dielectric tangent.

[0036] One method for filling the furnace with a dry atmosphere with a dew point of 15°C or less is to introduce dry air produced by a compressor or air dryer into the furnace. The dew point of the dry gas introduced should be 15°C or less (volume absolute humidity: 12.8 g / m 3 ) is preferred, and 0°C (volume absolute humidity: 4.85 g / m 3 ) or less is more preferable, and -20°C or less (volume absolute humidity: 1.07g / m 3 ) is more preferable, and −60° C. (volume absolute humidity: 0.0193 g / m 3 ) or less is particularly preferred. The timing of introducing dry air is at least when the temperature is decreasing, and it may be introduced when the temperature is increased and maintained as appropriate. The amount of dry air introduced is not particularly limited, but is preferably 0.5 to 20 times the volume of the drying furnace per hour, as a range that sufficiently decreases the dew point inside the furnace and keeps the temperature inside the furnace constant. The SiOH group on the surface affects not only the dielectric tangent but also the tensile strength. If there are many SiOH groups, the glass cloth softens and the tensile strength decreases.

[0037] [Silane coupling agent treatment] The glass cloth of the present invention is treated with a silane coupling agent, and can be obtained, for example, by surface-treating a glass cloth that has been deoiled by heat cleaning with a silane coupling agent. The dielectric tangent of the quartz glass cloth after the silane coupling agent treatment is preferably 1.5 times or less, more preferably 1.3 times or less, of the dielectric tangent of the quartz glass cloth before the silane coupling agent treatment.

[0038] The silane treatment liquid is not particularly limited, but from the viewpoint of productivity and environmental load, an aqueous solution in which 0.01 to 5 mass% of a silane coupling agent is dispersed is preferable, and the pH can be adjusted according to the type of silane coupling agent to be dispersed. The method of adjusting the pH is not particularly limited, but adjustment with acetic acid or ammonia according to the silane coupling agent used is preferable.

[0039] The silane coupling agent is represented by the general formula (1): R 1 X R 2 Y Si(OR 3 ) 4-X-Y (1) (In the formula, R 1 is a monovalent organic group having 1 to 20 carbon atoms, including an epoxy group, an amino group, an unsaturated group, a mercapto group, an isocyanate group, an acid anhydride group, or a hydroxyl group; R 2 is an alkyl group or an aryl group having 1 to 10 carbon atoms, R 3 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, X is 1 or 2, Y is 0 or 1, and X+Y is 1 or 2. For example, trimethylmethoxysilane, trimethylethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, methylphenyldimethoxysilane, methylphenyldiethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, trimethoxysilane, triethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, phenylmethylvinylethoxysilane, naphthyltrimethoxysilane, naphthyltriethoxysilane, 1,4-bis(methoxydimethylsilyl)benzene, tetramethoxysilane, tetraethoxysilane, xylsilane, n-propyltriethoxysilane, hexyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, 1,6-bis(trimethoxysilyl)hexane, vinyltrimethoxysilane, vinyltriethoxysilane, p-styryltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-Epoxycyclohexyl)ethylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-(vinylbenzyl) Examples of alkoxysilane compounds include alkoxysilane compounds such as N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane and its hydrochloride, N-(vinylbenzyl)-2-aminoethyl-3-aminopropylmethyldimethoxysilane and its hydrochloride, 3-isocyanatepropyltriethoxysilane, tris-(trimethoxysilylpropyl)isocyanurate, 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, and bis(trisethoxysilylpropyl)tetrasulfide, which may be used alone or in combination of two or more. In particular, Shin-Etsu Chemical's methacrylamide silane coupling agent X-12-1370 for low dielectric resins is preferred because it can maintain the dielectric tangent of the glass cloth low compared to 3-methacryloxypropyltrimethoxysilane. The method of applying the silane treatment solution is not particularly limited, but examples thereof include a method of impregnating glass fibers with the silane treatment solution, treatment by roll coating, etc. The method of drying the silane treatment solution is not particularly limited, but examples thereof include drying methods using hot air, infrared rays, and hot rolls.

[0040] The effects of silane coupling agents are generally known to be that they increase the tensile strength of the glass cloth and increase the affinity with the resin when the resin is applied in the next process. However, since the silane coupling agent in the silane treatment solution itself contains SiOH groups, it is important to apply an appropriate amount to the quartz glass cloth. The reaction between the silane coupling agent and the glass cloth is silane treatment by reacting the SiOH group of the silane coupling agent with the SiOH group on the surface of the glass cloth. Since the quartz glass cloth in the present invention has fewer SiOH groups on the surface than general glass cloth by suppressing the dew point low, the amount of the silane coupling agent attached in the present invention is preferably more than 0 and 0.2 mass% or less with respect to the glass cloth, and more preferably 0.01 to 0.1 mass%. In such a range, the affinity with the resin can be improved while maintaining the low dielectric tangent of the quartz glass cloth. If it is less than 0.01 mass%, the affinity with the resin may be poor when the resin is applied to prepare a substrate in a later process, and the reliability of the substrate may be significantly reduced. If 0.3 mass% or more of the coupling agent is attached to the glass cloth, the Si-OH group of the silane coupling agent itself becomes excessive, and the dielectric tangent of the quartz glass cloth deteriorates. The amount of the silane coupling agent attached can be measured by the ignition loss described in JIS R3420. Since the amount of the silane coupling agent attached is almost the same between the core side and the unwinding side of the roll, there is no particular restriction on the sampling location, but the unwinding side is preferable from the viewpoint of workability. The tensile strength of the quartz glass cloth after the silane coupling agent treatment is not particularly limited, but it is preferable that it is at least 1 times that before the silane coupling agent treatment when applying a resin in a later process.

[0041] [Prepreg for printed circuit boards] The glass cloth of the present invention has high tensile strength and excellent dielectric properties, so that a prepreg for printed circuit boards that is thinner, has high tensile strength, and has excellent dielectric properties can be obtained. Examples of the prepreg for printed circuit boards include a prepreg containing the above-mentioned glass cloth and an organic resin. The organic resin is not particularly limited, and examples thereof include cyanate ester resin, bismaleimide-cyanate ester resin, epoxy resin, polyfunctional maleimide resin, unsaturated group-containing polyphenylene ether resin, PTFE, etc., and can be used alone or in combination of two or more. The amount of the organic resin used is within a known range.

[0042] [Laminate] Since the glass cloth of the present invention has high tensile strength and excellent dielectric properties, a thinner laminate having high tensile strength and excellent dielectric properties can be obtained. Examples of the laminate include those containing the above glass cloth and an organic resin.

[0043] [Printed circuit board] The glass cloth of the present invention has high tensile strength and excellent dielectric properties, so that a thinner printed circuit board having high tensile strength and excellent dielectric properties can be obtained. The printed circuit board can be one containing the above glass cloth and an organic resin. The method for producing the printed circuit board is not particularly limited, and a general method for producing a printed circuit board can be applied. EXAMPLES

[0044] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0045] [Preparation of quartz glass cloth] A quartz glass ingot containing 99.9% SiO2 was heated and drawn while winding a quartz thread with a diameter of 200 μm, and the obtained quartz thread was heated to 2,000 °C in a mixed flame of oxygen and hydrogen to produce a quartz glass filament with a diameter of 5.3 μm. A quartz glass fiber sizing agent (starch 3.0% by mass, beef tallow 0.5% by mass, emulsifier 0.1% by mass, remaining water) was applied to this quartz filament fiber with an applicator, and then the fiber was bundled with a bundler and wound up to produce a quartz glass strand with 200 quartz glass filaments. The wound quartz glass strand was twisted at 24 T / m to produce a quartz glass yarn.

[0046] An aqueous solution consisting of 1.5% by mass of partially saponified polyvinyl acetate and 1.5% by mass of starch was applied to the obtained quartz glass yarn as a secondary bundling agent, and then an IPC Standard 1078 quartz glass cloth with a width of 1,285 mm and a length of 1,500 m was produced using an air jet loom (SQ1).

[0047] [Example 1] The resulting 1,500 m of SQ1 was subjected to a fiber-opening process using a PSN slit nozzle manufactured by Ikeuchi Co., Ltd., with tap water at 25°C and 0.3 MPa and compressed air at 0.5 MPa, so that the air-water volume ratio was V2 / V1 = 100. The air permeability of the resulting quartz glass cloth was 25 cm 3 / (cm 2 The fiber-opening process was wound around an iron pipe with an outer diameter of 400Φ, which was wrapped with 20 mm thick E-glass cloth (IPC standard 2116) manufactured by Sakai Sangyo Co., Ltd., and heat-cleaned at 500°C for 24 hours using a Nemus electric furnace B80×85×200-3Z12-10 to remove the sizing agent, obtaining a desized quartz glass cloth. The starting temperature for heating was 20°C, the heating rate was 50°C / h, and the temperature was lowered to 50°C in 30 hours. During this process, dry air with a dew point of -70°C, produced by a CKD Corporation Super Heatless Dryer SHD3025, was fed in at 10 times the volume of the electric furnace per hour from heating to cooling, and heating was performed in a dry state. The obtained quartz glass cloth was immersed in an aqueous solution containing 0.2% by mass of methacrylamide silane coupling agent X-12-1370 manufactured by Shin-Etsu Chemical Co., Ltd. and 0.1% by mass of acetic acid, and then dried at 110°C for 3 minutes using a silane treatment machine manufactured by Hirano Techseed Co., Ltd. to perform silane treatment, obtaining a silane-treated quartz glass cloth with an adhesion amount of 0.05% by mass of silane coupling agent. Next, a fray prevention treatment agent consisting of 100 parts by mass of tricyclodecane dimethanol diacrylate, a bifunctional acrylate, and 0.5 parts by mass of Omnirad819 (an α-hydroxyacetophenone compound manufactured by IGM Co., Ltd.) as a photopolymerization initiator was applied to both widthwise edges with a coating width of 10 mm using a slitter (LP11A-00K-001) manufactured by Shin-Etsu Engineering Co., Ltd., and an integrated light amount of 500 mJ / cm 365 nm ultraviolet LED was applied. 2 After hardening the anti-fraying agent, the width was adjusted to 1,270 mm. This was wound up on a cylindrical paper tube manufactured by Showa Marutsutsu Co., Ltd., with an inner diameter of 76 mm, a diameter of 183 mm, and a width of 1,320 mm, using a Cortec inspection machine, to obtain a roll of silane-treated quartz glass cloth with a length of 1,450 m, including process losses along the way.

[0048] [Example 2] A silane-treated quartz glass cloth was obtained in the same manner as in Example 1, except that the temperature rise rate was 10° C. / h. The amount of the silane coupling agent attached was 0.05% by mass, and the finished amount was 1,450 m.

[0049] [Example 3] A silane-treated quartz glass cloth was obtained in the same manner as in Example 1, except that the heating rate in Example 1 was 100°C / h up to 400°C, and 10°C / h from 400 to 500°C. The temperature was lowered to 50°C in 22 hours. The amount of the silane coupling agent attached was 0.05% by mass, and the finished amount was 1,450 m.

[0050] [Example 4] A silane-treated quartz glass cloth was obtained in the same manner as in Example 1, except that the heating conditions were 900°C for 1 hour and the temperature increase rate was 10°C / h. The temperature was decreased to 50°C in 40 hours. The amount of the silane coupling agent attached was 0.03 mass%, and the finished amount was 1,450 m.

[0051] [Example 5] A silane-treated quartz glass cloth was obtained in the same manner as in Example 1, except that the heating conditions were 350°C for 96 hours and the temperature increase rate was 100°C / h. The temperature was decreased to 50°C in 18 hours. The amount of the silane coupling agent attached was 0.12 mass%, and the finished amount was 1,450 m.

[0052] [Example 6] A silane-treated quartz glass cloth was obtained in the same manner as in Example 1, except that dry air was introduced only when the temperature was lowered. The amount of the silane coupling agent attached was 0.05% by mass, and the finished amount was 1,450 m.

[0053] [Example 7] A silane-treated quartz glass cloth was obtained in the same manner as in Example 1, except that dry air was not introduced in Example 1. The temperature was lowered to 50°C in 35 hours. The amount of the silane coupling agent attached was 0.10 mass%, and the finished amount was 1,450 m.

[0054] [Example 8] Silane-treated quartz glass cloth was produced in the same manner as in Example 4. When rewinding the cloth onto a paper core using a Cortec fabric inspection machine, 100 m of the area corresponding to the winding core was removed during heat cleaning. The amount of silane coupling agent attached was 0.05% by mass, and the finished length was 1,350 m.

[0055] [Example 9] 1,500 m of SQ1 was opened using a PSN slit nozzle manufactured by Ikeuchi Co., Ltd., with tap water at 25°C and 0.2 MPa and compressed air at 0.6 MPa, so that the air-water volume ratio was V2 / V1 = 185. The air permeability of the obtained quartz glass cloth was 72 cm 3 / (cm 2 The obtained spread quartz glass cloth was subjected to silane treatment in the same manner as in Example 1. The amount of the silane coupling agent attached was 0.05 mass %, and the finished length was 1,450 m.

[0056] [Comparative Example 1] A silane-treated quartz glass cloth was obtained in the same manner as in Example 1, except that the temperature rise rate was 150° C. / h. The amount of the silane coupling agent attached was 0.05 mass %, and the finished amount was 1,450 m.

[0057] [Comparative Example 2] 1,500 m of SQ1 was opened using a PSN slit nozzle manufactured by Ikeuchi Co., Ltd., with tap water at 25°C and 0.1 MPa and compressed air at 0.6 MPa, so that the air-water volume ratio was V2 / V1 = 205. The air permeability of the obtained quartz glass cloth was 103 cm 3 / (cm 2 The obtained spread quartz glass cloth was subjected to silane treatment in the same manner as in Example 1. The amount of the silane coupling agent attached was 0.05 mass %, and the finished length was 1,450 m.

[0058] [Comparative Example 3] The heating conditions in Example 1 were 300°C, 100 hours, and a temperature rise rate of 100°C / h. The temperature was lowered to 50°C in 24 hours. The quartz glass cloth taken out was colored, and the sizing agent was still burnt. The silane treatment was then carried out in the same manner as in Example 1 to obtain a silane-treated quartz glass cloth. The total amount of the sizing agent residue and the silane coupling agent was 0.23 mass%, and the finished amount was 1,450 m.

[0059] [Comparative Example 4] The heating conditions in Example 1 were 1,000°C for 1 hour, and the heating rate was 10°C / h. The temperature was lowered to 50°C in 48 hours. When silane treatment was performed in the same manner as in Example 1, the length of the silane-treated quartz glass cloth that was broken during the silane treatment and could be recovered was 530 m, and the amount of the silane coupling agent attached was 0.01 mass%. The above-described glass cloth was evaluated by the following methods, and the results are shown in the table.

[0060] 1. Measurement of air permeability Before heat cleaning, the open-fiber-treated glass cloth and the silane-treated glass cloth were sampled from the unwinding side of the roll and measured for air permeability according to the method for measuring cloth air permeability in JIS R 3420. The measurement position on the unwinding side was a 10m section of the unwound material, excluding the top three layers wound in roll form.

[0061] 2. Dew point measurement The dew point was measured using an Orion dew point monitor MG-40.

[0062] 3. Measurement of basis weight The basis weight was measured according to the method for measuring the mass of cloth and mats specified in JIS R 3420. Sampling locations were the same as the following items used in calculating the basis weight.

[0063] 4. Tensile strength The silane-treated glass cloth wound around a cardboard tube was unwound using a Cortec fabric inspection machine, and three layers were removed from each of the core side and unwinding side of the roll. A 1 m sample was taken from the removed area, and the tensile strength was measured in the longitudinal and transverse directions using an autograph AGS-X manufactured by Shimadzu Corporation according to the tensile strength measurement method of JIS R 3420. The strength difference in tensile strength was calculated by recording the lower and higher values ​​on the core side and unwinding side. In this example, the tensile strength on the unwinding side was lower than that of the core. Tensile strength (GPa) = [Tensile strength (N / 25mm) / 25] / [Weight (g / m 2 ) / specific gravity of quartz glass 2.2 (g / cm 3 )] should be used.

[0064] 5. Amount of silane coupling agent attached A sample of silane-treated quartz glass cloth was taken from the unwinding side of the roll and measured according to the ignition loss method described in JIS R 3420. However, since the remaining sizing agent was included in Comparative Example 3, the amount was essentially the amount of silane coupling agent attached + the amount of remaining sizing agent.

[0065] 6. Measurement of dielectric tangent The dielectric loss tangent of the silane-treated glass cloth at 10 GHz was measured using a cavity resonator (TE011 mode) manufactured by AET Corporation. The thickness of the glass cloth was measured using the theoretical thickness. Theoretical film thickness t (μm) = Area weight (g / m 2 ) / specific gravity (g / cm 3 ) Calculated from. As for the sampling location, samples were taken from a 10m section of the roll, excluding the top three layers.

[0066] 7. Measuring the finished length The actual length of the silane-treated glass cloth was measured while rewinding it using a Cortec inspection machine.

[0067] 8. Reliability of the board The silane-treated glass cloth obtained in the examples and comparative examples was immersed in a 55% by mass toluene solution of SLK-3000 (trade name of Shin-Etsu Chemical Co., Ltd.) and dried at 110°C for 10 minutes to form a prepreg. Three layers of prepreg were stacked and cured by vacuum pressing to obtain a substrate. The obtained substrate was boiled at 100°C for 2 hours, the moisture on the surface was wiped off, and the substrate was submerged in a solder bath heated to 260°C for 30 seconds, and then submerged in a cooling material of -78°C consisting of acetone and dry ice for 30 seconds. Three sets of operations of submerging in a solder bath of 260°C and acetone of -78°C were performed. Three samples were prepared for each example and comparative example, and those that did not peel between the quartz glass cloth and the resin in any of the three samples were marked as "◯", those that had one or two peels were marked as "△", and those that all peeled were marked as "X".

[0068] [Table 1]

[0069] [Table 2]

[0070] Within the scope of the present invention, it is possible to provide a quartz glass cloth that has a low dielectric tangent while having little variation in tensile strength within a roll and is highly reliable, which has the remarkable effect of significantly improving the productivity of substrates for future 5G and 6G communication applications, etc.

[0071] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]

[0072] 1 Winding core

Claims

1. SiO 2 The glass cloth having a composition amount of 95 mass% or more is a glass cloth treated with a silane coupling agent, A dielectric tangent of 0.0008 or less at 10 GHz, Ventilation is 75cm 3 / (cm 2 s) or less, The glass cloth is wound into a roll, A glass cloth having a longitudinal tensile strength of 0.10 GPa or more at both ends of a core side and an unwinding side of a roll, with the difference between the tensile strengths being 0.15 GPa or less.

2. 2. The glass cloth according to claim 1, wherein the difference in tensile strength in the machine direction is 0.10 GPa or less.

3. A prepreg comprising the glass cloth according to claim 1 or 2 and an organic resin.

4. A laminate comprising the glass cloth according to claim 1 or 2 and an organic resin.

5. A printed wiring board comprising the glass cloth according to claim 1 or 2 and an organic resin.

6. SiO 2 A heat cleaning method for removing a sizing agent adhering to a surface of a glass cloth having a composition amount of 95% by mass or more, comprising the steps of: The glass cloth to which the sizing agent is attached is A heat cleaning method in which the substrate is heated from room temperature to a predetermined temperature at a rate of 100° C. / h or less.

7. 7. The heat cleaning method according to claim 6, wherein the glass cloth having the sizing agent adhered thereto is heated in an environment in which the dew point is 15[deg.] C. or less when the temperature is lowered.

Citation Information

Patent Citations

  • Core material for heat cleaning treatment

    JP2014122446A

  • Aqueous size agent

    JP2016216860A

  • Annealed quartz glass cloth and manufacturing method thereof

    JP2021195689A

  • Low dielectric resin substrate

    JP2022011534A

  • Glass cloth, prepreg, and printed wiring board

    JP2023006294A

Cited By

  • Electronic-grade quartz glass fiber cloth and preparation method thereof

    CN119800695A