Lubricating oil additive and lubricating oil composition

A block copolymer-based lubricating oil additive addresses the environmental and health concerns of conventional additives by reducing sulfur and metal content, enhancing lubricity and wear resistance in lubricating oils.

JP2024150269APending Publication Date: 2024-10-23OTSUKA CHEMICAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023063608
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23

AI Technical Summary

Technical Problem

Conventional lubricating oil additives containing sulfur, phosphorus, and metals cause corrosion and environmental issues while improving extreme pressure properties and wear resistance, posing health risks.

Method used

A lubricating oil additive composed of a block copolymer with an A block containing a polyorganosiloxane group and a B block with a polar group, which adsorbs metals and reduces friction and wear without sulfur, phosphorus, and metals.

Benefits of technology

The additive provides excellent lubricity and wear resistance while minimizing environmental impact and health hazards, suitable for lubricating oils used in metal processing, engine oils, and hydraulic oils.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150269000001
    Figure 2024150269000001
  • Figure 2024150269000002
    Figure 2024150269000002
  • Figure 2024150269000003
    Figure 2024150269000003
Patent Text Reader

Abstract

To provide a lubricating oil additive and a lubricating oil composition that can impart excellent lubricity and have high safety with reduced content of sulfur, phosphorus, and metals.SOLUTION: The lubricating oil additive of the present invention is characterized by comprising a block copolymer containing an A block including a structural unit (a-1) derived from a vinyl monomer (a) having a poly-organosiloxane group and a B block including a structural unit (b-1) derived from a vinyl monomer (b) containing a polar group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to lubricating oil additives and lubricating oil compositions. [Background technology]

[0002] Lubricants (lubricating oils) are used for various purposes such as metal processing oils, engine oils, drive system oils, hydraulic oils, etc. In recent years, the viscosity of lubricating oils has been reduced in order to improve the performance and size of various devices and to improve fuel efficiency. As a result, contact surfaces that require lubrication are increasingly subjected to higher pressure than ever before, which has led to problems with wear on the contact surfaces.

[0003] For example, Patent Document 1 discloses a lubricating oil containing one or more polyethers (E) represented by the following general formula (1), having an HLB of 4 or less and a weight average molecular weight of 500 to 10,000. R 1 -{(O-CH 2 CH 2 CH 2 CH 2 ) m / (OA) n}-OR 2 (1) [R in the formula 1 is a hydrocarbon group having 1 to 24 carbon atoms, R 2 is an alkyl group having 1 to 4 carbon atoms, A is at least one selected from alkylene groups having 1 to 4 carbon atoms excluding 1,4-butylene groups, and m and n are integers of 1 or more such that the weight average molecular weight of (E) is 500 to 10,000. 2 CH 2 CH 2 CH 2 The oxyalkylene groups (OA groups) may be bonded randomly or in a block form.

[0004] Patent Document 2 discloses an engine oil composition comprising a lubricating base oil containing, as component (A), 100 to 500 ppm by mass of zinc dithiophosphate having a specific structure in terms of phosphorus content, and, as component (B), 0.01 to 20% by mass of a reaction product of a divalent or higher hindered alcohol and a monocarboxylic acid having 8 or more carbon atoms.

[0005] Patent Document 3 discloses a lubricant composition comprising (A) a non-silicone base stock oil and (B) 0.5 to 50% by weight of a silicone oil based on the total weight of (A) + (B), wherein the viscosity index of the lubricant composition is at least 10% greater than the viscosity index of the non-silicone lubricant base oil (A) when measured according to ASTM D 2270-10e1, and the lubricant composition is shear stable when measured according to DIN 51350-6 (Method A). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2002-012881 A [Patent Document 2] JP 2005-325241 A [Patent Document 3] JP 2015-525827 A Summary of the Invention [Problem to be solved by the invention]

[0007] In lubricants (lubricating oils), additives are blended into the base oil for the purpose of improving various performances such as extreme pressure properties, wear resistance, and oxidation stability. Among them, additives that affect extreme pressure properties and wear resistance are used to counter wear of components under high load because they have the effect of reducing friction. Conventional lubricating oil additives aimed at improving extreme pressure properties contain elements such as sulfur, phosphorus, lead, zinc, and chlorine (see Patent Document 1 (paragraph 0024), Patent Document 2 (paragraph 0031), and Patent Document 3 (paragraph 0057)). As a result, there are corrosion of the lubricated surface, damage to human health, and environmental problems when discarded. An object of the present invention is to provide a lubricating oil additive and a lubricating oil composition which are capable of imparting excellent lubricity and have a high level of safety by reducing the contents of sulfur, phosphorus and metals. [Means for solving the problem]

[0008] The lubricating oil additive of the present invention, which has been able to solve the above problems, is characterized in that it comprises a block copolymer comprising an A block containing a structural unit (a-1) derived from a vinyl monomer (a) having a polyorganosiloxane group, and a B block containing a structural unit (b-1) derived from a vinyl monomer (b) containing a polar group. In the block copolymer used in the present invention, the highly polar B block forms an adsorbent portion that adsorbs to metals such as iron, steel, stainless steel, and aluminum, and the A block forms a lubricating portion that dissolves in the base oil. As a result, the block copolymer used in the present invention is considered to have an effect of reducing friction and wear. Therefore, it can be used as a lubricating oil additive (for example, an oiliness improver, an extreme pressure agent, a wear modifier, an anti-wear improver, etc.).

[0009] The lubricating oil composition of the present invention contains a base oil and the lubricating oil additive of the present invention.

[0010] The present invention includes a lubrication system in which a metallic material is in contact with the lubricating oil composition of the present invention. Effect of the Invention

[0011] According to the present invention, it is possible to provide a lubricating oil additive that can impart excellent lubricity and has a high level of safety by reducing the contents of sulfur, phosphorus, and metals, and a lubricating oil composition using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an example of a preferred embodiment of the present invention will be described. However, the following embodiment is merely an example, and the present invention is not limited to the following embodiment.

[0013] The lubricating oil additive of the present invention is characterized in that it comprises a block copolymer comprising an A block containing a structural unit (a-1) derived from a vinyl monomer (a) having a polyorganosiloxane group, and a B block containing a structural unit (b-1) derived from a vinyl monomer (b) containing a polar group.

[0014] In this specification, the term "A block" can be rephrased as "A segment" and the term "B block" can be rephrased as "B segment." The term "polyorganosiloxane group" refers to a -SiR 2 -[OSiR 2 ] n -R is a monovalent organic group (R is independently a monovalent organic group, and n is an integer of 2 or more). "Vinyl monomer" refers to a monomer having a radically polymerizable carbon-carbon double bond in the molecule. "Structural unit derived from vinyl monomer" refers to a structural unit in which the radically polymerizable carbon-carbon double bond of a vinyl monomer is polymerized to become a carbon-carbon single bond. "(Meth)acrylic" refers to "at least one of acrylic and methacrylic". "(Meth)acrylate" refers to "at least one of acrylate and methacrylate". "(Meth)acryloyl" refers to "at least one of acryloyl and methacryloyl".

[0015] (Structural unit (a-1)) The block copolymer of the present invention has an A block having a structural unit (a-1) derived from a vinyl monomer (a) having a polyorganosiloxane group.

[0016] The vinyl monomer (a) is not particularly limited as long as it has a vinyl group and a polyorganosiloxane group in one molecule. From the viewpoint of polymerizability, the functional group equivalent (g / mol) of the vinyl group of the vinyl monomer is preferably 500 or more, more preferably 600 or more, even more preferably 700 or more, and is preferably 50,000 or less, more preferably 3,000 or less, and even more preferably 1,200. The number of vinyl groups that the vinyl monomer (a) has is not particularly limited, but is preferably 1.

[0017] The number average molecular weight (Mn) of the vinyl monomer (a) is preferably 500 or more, more preferably 600 or more, and even more preferably 700 or more, and is preferably 50,000 or less, more preferably 3,000 or less, and even more preferably 1,200. If the number average molecular weight (Mn) of the vinyl monomer (a) is within the above range, when the vinyl monomer (a) is mixed with a base oil, the copolymer component does not precipitate and compatibility is good.

[0018] Examples of the vinyl monomer (a) include (meth)acrylates having a polyorganosiloxane group, (meth)acrylamides having a polyorganosiloxane group, and the like. Of these, (meth)acrylates having a polyorganosiloxane group are preferred.

[0019] The vinyl monomer (a) is preferably a compound represented by the following general formula (1). [ka] [In the formula, R 11 R represents a hydrogen atom or a methyl group. 12 , R 13 , R 14 , R 15 and R 16 Q independently represents a saturated hydrocarbon group having 1 to 10 carbon atoms which may have a substituent. 1 represents a single bond or a divalent organic group. n represents an integer of 2 or more.

[0020] R 12 , R 13 , R 14 , R 15 and R 16 Examples of the substituent include a halogen atom and an alkoxy group having 1 to 10 carbon atoms.

[0021] R 12 , R 13 , R 14 , R 15 and R 16 are each independently a saturated hydrocarbon group having 1 to 10 carbon atoms which may have a substituent. As the saturated hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, an alkyl group or a fluoroalkyl group having 1 to 8 carbon atoms is preferred, a methyl group or a trifluoropropyl group is more preferred, and a methyl group is even more preferred. From the viewpoint of ease of synthesis, R 12 , R 13 , R 14 , R 15 and R 16 are preferably the same. Depending on the desired physical properties, different groups may be introduced into some of them.

[0022] Q 1 is a single bond or a divalent organic group. Examples of the divalent organic group include substituted or unsubstituted divalent saturated hydrocarbon groups having 1 to 10 carbon atoms which may have an ether group (-O-), an ester group (-C(=O)O- or -OC(=O)-), an amide group (-C(=O)NH-), or a urethane group (-NHC(=O)-O-) between carbon atoms. Examples of the substituent include halogen atoms and alkoxy groups having 1 to 10 carbon atoms.

[0023] n is preferably an integer of 2 or more, more preferably an integer of 6 or more, and is preferably an integer of 300 or less.

[0024] The vinyl monomer (a) forming the structural unit (a-1) is more preferably a compound represented by the following general formula (2). [ka] [In the formula, R 21 R represents a hydrogen atom or a methyl group. 22 represents an alkyl group having 1 to 4 carbon atoms; m1 is a number from 1 to 6; and m2 is a number from 20 to 300.

[0025] Specific examples of the vinyl monomer (a) having the formula (1) are commercially available from Shin-Etsu Chemical Co., Ltd. (modified silicone oil series) and JNC Corporation (Silaplane (registered trademark)). Shin-Etsu Chemical Co., Ltd.'s X-22-2404 [functional group equivalent (g / mol): 420] [number average molecular weight: 420], X-22-174ASX [functional group equivalent (g / mol): 900] [number average molecular weight: 900], X-22-174BX [functional group equivalent ( g / mol): 2,300][number average molecular weight: 2,300], KF-2012[functional group equivalent (g / mol): 4,600], X-22-2426[functional group equivalent (g / mol): 12,000][number average molecular weight: 12,000], FM-0711[number average molecular weight: 1,000], FM-0721[number average molecular weight: 5,000], FM-0725[number average molecular weight: 10,000] (all trade names) manufactured by JNC Corporation. The functional group equivalent is the functional group equivalent of 1 mole of vinyl group. When the vinyl monomer (a) is monofunctional, the functional group equivalent [g / mol] can be regarded as the number average molecular weight of the vinyl monomer (a) relative to 1 mole of siloxane.

[0026] The A block of the block copolymer used in the present invention may be composed essentially of the structural unit (a-1) derived from the vinyl monomer (a) having a polyorganosiloxane group, or may contain other structural units.

[0027] The content of the structural unit (a-1) derived from the vinyl monomer (a) having a polyorganosiloxane group in the A block is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and preferably 100% by mass or less, based on 100% by mass of the structural units constituting the A block. By setting the content of the structural unit (a-1) within the above range, the copolymer component does not precipitate when mixed with the base oil, and compatibility is good.

[0028] In addition, it is preferable that the A block does not substantially contain the structural unit (b-1) contained in the B block. That is, in the A block, the content of the structural unit (b-1) contained in the B block is preferably 10% by mass or less, more preferably 8% by mass or less, further preferably 5% by mass or less, and particularly preferably 2% by mass or less, based on 100% by mass of the structural units constituting the A block. The lower limit of the content is 0% by mass.

[0029] It is also preferred that the A block of the block copolymer used in the present invention consists essentially of the structural unit (a-1) derived from the vinyl monomer (a) having a polyorganosiloxane group.

[0030] (Structural unit (b-1)) The block B of the block copolymer used in the present invention has a structural unit (b-1) derived from a vinyl monomer (b) containing a polar group.

[0031] The polar group refers to a group containing a structure in which the difference in electronegativity between two adjacent atoms is large, and specific examples thereof include a hydroxy group, a carboxy group, an amino group, a sulfonic acid group, a phosphoric acid group, a phosphonic acid group, and a phosphinic acid group, and is preferably at least one type selected from the group consisting of a hydroxy group, a carboxy group, and an amino group.

[0032] The vinyl monomer (b) is preferably a compound represented by the following general formula (3). [ka] [In the formula, R 31 R represents a hydrogen atom or a methyl group. 32 represents a single bond or a divalent organic group. Y 3 represents a polar group.

[0033] In the general formula (3), the divalent organic group R 32 Examples of the alkylene group include an alkylene group, an arylene group, and -CO-NH-R 321 - group (amide group), -CO-OR 322 - group (ester group), and preferably -CO-NH-R 321 - groups and / or -CO-OR 322 - group, more preferably -CO-OR 322 The bonding direction of the amide group and the ester group is not particularly limited, but the bonding form of the amide group is C-CO-NH-R 321 -Y 3 is preferable, and the bonding form of the ester group is C-CO-OR 322 -Y 3 is preferred.

[0034] R 321 is preferably an alkylene group (-R 3211 - group) or ester group (-R 3212 -O-CO-R 3213 -group), and more preferably an ester group. The bonding direction of the ester group is not particularly limited, but the bonding mode of the ester group is preferably -R 3212 -O-CO-R 3213 -Y 3 is preferred.

[0035] R 3211 is preferably a linear alkylene group or a branched alkylene group, more preferably a linear alkylene group having 1 to 10 carbon atoms or a branched alkylene group having 3 to 10 carbon atoms, and even more preferably a linear alkylene group having 1 to 4 carbon atoms. Specific examples include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, and a heptamethylene group.

[0036] R 3212 is preferably a linear alkylene group or a branched alkylene group, more preferably a linear alkylene group having 1 to 10 carbon atoms or a branched alkylene group having 3 to 10 carbon atoms, and even more preferably a linear alkylene group having 1 to 4 carbon atoms. Specific examples include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, and a heptamethylene group.

[0037] R 3213 is preferably a linear alkylene group, a branched alkylene group, a cyclic alkylene group or an arylene group, more preferably a linear alkylene group having 1 to 10 carbon atoms, a branched alkylene group having 3 to 10 carbon atoms, a cyclic alkylene group having 6 to 10 carbon atoms or an arylene group having 6 to 10 carbon atoms, and further preferably a linear alkylene group having 1 to 4 carbon atoms. Specific examples include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, a heptamethylene group, a cyclohexylene group, a phenylene group, and the like.

[0038] R 322 is preferably an alkylene group (-R 3221 - group) or ester group (-R 3222 -O-CO-R 3223 -group), and more preferably an ester group. The bonding direction of the ester group is not particularly limited, but the bonding mode of the ester group is preferably -R 3222 -O-CO-R 3223 -Y 3 is preferred.

[0039] R 3221is preferably a linear alkylene group or a branched alkylene group, more preferably a linear alkylene group having 1 to 10 carbon atoms or a branched alkylene group having 3 to 10 carbon atoms, and even more preferably a linear alkylene group having 1 to 4 carbon atoms. Specific examples include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, and a heptamethylene group.

[0040] R 3222 is preferably a linear alkylene group or a branched alkylene group, more preferably a linear alkylene group having 1 to 10 carbon atoms or a branched alkylene group having 3 to 10 carbon atoms, and even more preferably a linear alkylene group having 1 to 4 carbon atoms. Specific examples include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, and a heptamethylene group.

[0041] R 3223 is preferably a linear alkylene group, a branched alkylene group, a cyclic alkylene group or an arylene group, more preferably a linear alkylene group having 1 to 10 carbon atoms, a branched alkylene group having 3 to 10 carbon atoms, a cyclic alkylene group having 6 to 10 carbon atoms or an arylene group having 6 to 10 carbon atoms, and further preferably a linear alkylene group having 1 to 4 carbon atoms. Specific examples include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, a heptamethylene group, a cyclohexylene group, a phenylene group, and the like.

[0042] Y 3 Examples of the polar group represented by the formula (I) include a hydroxy group, a carboxy group, an amino group, a sulfonic acid group, a phosphoric acid group, a phosphonic acid group, and a phosphinic acid group, and preferably at least one selected from the group consisting of a hydroxy group, a carboxy group, and an amino group.

[0043] Examples of vinyl monomers having a hydroxy group include hydroxyl group-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate.

[0044] Examples of vinyl monomers having a carboxy group include (meth)acrylic acid and (meth)acrylates having a carboxy group.

[0045] Examples of the (meth)acrylate having a carboxy group include 2-acryloyloxyethyl hydrogen succinate, 2-methacryloyloxyethyl hydrogen succinate, 2-(acryloyloxy)ethyl hydrogen hexahydrophthalate, 2-(methacryloyloxyethyl) hydrogen hexahydrophthalate, 2-acryloyloxyethyl hydrogen phthalate, 2-methacryloyloxyethyl hydrogen phthalate, caprolactone adduct of acrylic acid, and caprolactone adduct of methacrylic acid.

[0046] Examples of vinyl monomers having an amino group include dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, dimethylaminobutyl (meth)acrylate, ethylaminoethyl (meth)acrylate, ethylaminopropyl (meth)acrylate, ethylaminobutyl (meth)acrylate, diethylaminoethyl (meth)acrylate, diethylaminopropyl (meth)acrylate, diethylaminobutyl (meth)acrylate, propylaminoethyl (meth)acrylate, propylaminopropyl (meth)acrylate, propylaminobutyl (meth)acrylate, dipropylaminoethyl (meth)acrylate, dipropylaminopropyl (meth)acrylate, dipropylaminobutyl (meth)acrylate, tert-butylaminoethyl (meth)acrylate, and dimethylaminopropyl (meth)acrylamide.

[0047] The content of the structural unit (b-1) is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, based on 100% by mass of the structural units constituting the B block. The upper limit of the content of the structural unit (b-1) is preferably 100% by mass or less, more preferably 98% by mass or less, and even more preferably 95% by mass or less. By setting the content of the structural unit (b-1) within the above range, it becomes possible to sufficiently adsorb to the substrate.

[0048] The B block may be composed of only the structural unit (b-1), or may contain other structural units. It is preferable that the B block does not substantially contain the structural unit (a-1) contained in the A block. That is, in the B block, the content of the structural unit (a-1) contained in the A block is preferably 6% by mass or less, and more preferably 4% by mass or less, based on 100% by mass of the structural units constituting the B block. The lower limit of the content is 0% by mass.

[0049] The block copolymer used in the present invention may contain structural units derived from another vinyl monomer (c) copolymerizable with the vinyl monomer (a) and the vinyl monomer (b), as long as the effects of the present invention are not impaired.

[0050] Examples of the other vinyl monomers (c) include (meth)acrylates having a chain alkyl group, (meth)acrylates having a cyclic alkyl group, and (meth)acrylates having an aromatic group.

[0051] Examples of the (meth)acrylate having a chain alkyl group include (meth)acrylates having a linear alkyl group and (meth)acrylates having a branched alkyl group. The (meth)acrylate having a linear alkyl group is preferably a (meth)acrylate having a linear alkyl group with a carbon number of 1 to 20, and more preferably a (meth)acrylate having a linear alkyl group with a carbon number of 1 to 10. Examples of the (meth)acrylate having a linear alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, n-lauryl (meth)acrylate, and n-stearyl (meth)acrylate.

[0052] The (meth)acrylate having a branched alkyl group is preferably a (meth)acrylate having a branched alkyl group with a carbon number of 3 to 20, and more preferably a (meth)acrylate having a branched alkyl group with a carbon number of 3 to 10. Examples of the (meth)acrylate having a branched alkyl group include isopropyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isononyl (meth)acrylate, and isodecyl (meth)acrylate.

[0053] The cyclic alkyl group includes a cyclic alkyl group having a monocyclic structure (for example, a cycloalkyl group) and a cyclic alkyl group having a bridged ring structure (for example, an adamantyl group, a norbornyl group, and an isobornyl group). The (meth)acrylate having a cyclic alkyl group with a monocyclic structure is preferably a (meth)acrylate having a cyclic alkyl group with a monocyclic structure in which the cyclic alkyl group has a carbon number of 6 to 12. Specific examples of the (meth)acrylate having a cyclic alkyl group with a monocyclic structure include cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, and cyclododecyl (meth)acrylate.

[0054] The (meth)acrylate having a cyclic alkyl group having a bridged ring structure is preferably a (meth)acrylate having a bridged ring structure in which the carbon number of the bridged ring structure is 6 to 12. Specific examples of the (meth)acrylate having a cyclic alkyl group having a bridged ring structure include isobornyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, 2-ethyl-2-adamantyl (meth)acrylate, etc.

[0055] The (meth)acrylate having an aromatic group is preferably a (meth)acrylate having an aromatic group with a carbon number of 6 to 12. Examples of the aromatic group include an aryl group, and the aromatic group may have a chain portion such as an alkylaryl group, an aralkyl group, or an aryloxyalkyl group. Specific examples of the (meth)acrylate having an aromatic group include benzyl (meth)acrylate, phenyl (meth)acrylate, and phenoxyethyl (meth)acrylate.

[0056] The block copolymer used in the present invention is preferably composed of the above-mentioned structural units and does not contain a sulfur atom in the main chain or side chain.

[0057] (Block Copolymer) The block copolymer used in the present invention has the A block and the B block. The structure of the block copolymer is preferably at least one selected from the group consisting of (AB)m type, (AB)mA type, and (BA)mB type (m is an integer of 1 or more, for example, an integer of 1 to 3). Among these, the block copolymer is preferably an AB type diblock copolymer from the viewpoints of handling during processing and physical properties of the composition. The block copolymer may have other blocks in addition to the A block and the B block.

[0058] The content of the A block is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, and is preferably 99% by mass or less, more preferably 95% by mass or less, and even more preferably 90% by mass or less, based on 100% by mass of the structural units constituting the block copolymer. This is because by adjusting the content of the A block within the above range, a block copolymer having a desired function can be prepared.

[0059] The content of the B block is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on 100% by mass of the structural units constituting the block copolymer. By adjusting the content of the B block within the above range, a block copolymer having a desired function can be prepared.

[0060] In the block copolymer, the mass ratio of the A block to the B block (A block / B block) is preferably 50 / 50 or more, more preferably 60 / 40 or more, and even more preferably 70 / 30 or more, and is preferably 99 / 1 or less, more preferably 95 / 5 or less, and even more preferably 90 / 10 or less. This is because, as long as the mass ratio (A block / B block) is within the above range, a block copolymer having a desired function can be prepared.

[0061] The number average molecular weight (Mn) of the block copolymer is preferably 5,000 or more, more preferably 7,000 or more, even more preferably 10,000 or more, and is preferably 100,000 or less, more preferably 800,000 or less, and even more preferably 50,000 or less, because if the number average molecular weight is within the above range, it can be mixed with the base oil without precipitating when mixed with the base oil.

[0062] The molecular weight distribution (D) of the block copolymer is preferably 2.5 or less, more preferably 2.3 or less, and even more preferably 2.0 or less. If the molecular weight distribution is 2.5 or less, the block copolymer is easily dissolved in the base oil and adsorbed to the base material. In the present invention, the molecular weight distribution (D) is calculated by (weight average molecular weight (Mw) of the block copolymer) / (number average molecular weight (Mn) of the block copolymer). The smaller the Mw / Mn, the narrower the molecular weight distribution width, and the copolymer has a uniform molecular weight, and when the value is 1.0, the molecular weight distribution width is the narrowest. If the molecular weight distribution (D) of the block copolymer exceeds 2.5, it will include those with low molecular weights and those with high molecular weights.

[0063] The weight average molecular weight and number average molecular weight are measured by gel permeation chromatography (hereinafter referred to as "GPC").

[0064] (Method of Producing Block Copolymer) Examples of methods for producing the block copolymer include a method in which an A block is first produced by a polymerization reaction of a vinyl monomer, and then a monomer for a B block is polymerized onto the A block; a method in which a B block is first produced, and then a monomer for an A block is polymerized onto the B block; and a method in which the A block and the B block are produced separately, and then the A block and the B block are coupled together.

[0065] The polymerization method is not particularly limited, but living radical polymerization is preferred. That is, the block copolymer is preferably one polymerized by living radical polymerization. In conventional radical polymerization methods, not only initiation reactions and propagation reactions, but also termination reactions and chain transfer reactions cause deactivation of the growth end, and tend to produce a mixture of polymers with various molecular weights and non-uniform compositions. In contrast, living radical polymerization methods are preferred in that they maintain the simplicity and versatility of conventional radical polymerization methods, while being less likely to cause termination reactions and chain transfer reactions, and the growth end grows without being deactivated, making it easy to precisely control the molecular weight distribution and produce polymers with uniform composition.

[0066] Living radical polymerization methods include a method using a compound capable of generating a nitroxide radical (nitroxide method; NMP method) depending on the method of stabilizing the polymer growth terminal; a method using a metal complex such as copper or ruthenium to polymerize a halogenated compound as a polymerization initiator compound in a living manner from the polymerization initiator compound (ATRP method); a method using a dithiocarboxylate or xanthate compound (RAFT method); a method using an organic tellurium compound (TERP method); a method using an organic iodine compound (ITP method); a method using an iodine compound as a polymerization initiator compound and an organic compound such as a phosphorus compound, a nitrogen compound, an oxygen compound, or a hydrocarbon as a catalyst (reversible transfer catalyst polymerization; RTCP method, reversible catalyst-mediated polymerization; RCMP method), etc. Among these methods, the TERP method is preferable from the viewpoint of the diversity of monomers that can be used, molecular weight control in the polymer region, uniform composition, or coloring.

[0067] The TERP method is a method in which an organic tellurium compound is used as a chain transfer agent to polymerize a radically polymerizable compound (vinyl monomer), and is a method described, for example, in WO 2004 / 14848, WO 2004 / 14962, WO 2004 / 072126, and WO 2004 / 096870.

[0068] Specific polymerization methods of the TERP method include the following (a) to (d). (a) A method of polymerizing a vinyl monomer using an organotellurium compound represented by formula (4): (b) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by formula (4) and an azo-based polymerization initiator. (c) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by formula (4) and an organoditelluride compound represented by formula (5). (d) A method of polymerizing a vinyl monomer using a mixture of an organotellurium compound represented by formula (4), an azo-based polymerization initiator, and an organoditelluride compound represented by formula (5).

[0069] [ka] [In formula (4), R 41 R represents an alkyl group having 1 to 8 carbon atoms, an aryl group, or an aromatic heterocyclic group. 42 and R 43 R each independently represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. 44 represents an alkyl group having 1 to 8 carbon atoms, an aryl group, a substituted aryl group, an aromatic heterocyclic group, an alkoxy group, an acyl group, an amido group, an oxycarbonyl group, a cyano group, an allyl group, or a propargyl group. In formula (5), R 41 represents an alkyl group having 1 to 8 carbon atoms, an aryl group, or an aromatic heterocyclic group.]

[0070] Specific examples of the organic tellurium compound represented by formula (4) include ethyl 2-methyl-2-n-butyltellanyl-propionate, ethyl 2-n-butyltellanyl-propionate, (2-hydroxyethyl) 2-methyl-methyltellanyl-propionate, and the organic tellurium compounds described in WO 2004 / 14848, WO 2004 / 14962, WO 2004 / 072126, and WO 2004 / 096870. Specific examples of the organic ditelluride compound represented by formula (5) include dimethyl ditelluride, dibutyl ditelluride, and the like. The azo polymerization initiator can be any azo polymerization initiator used in normal radical polymerization without any particular limitation. Examples of the azo polymerization initiator include 2,2'-azobis(isobutyronitrile) (AIBN), 2,2'-azobis(2,4-dimethylvaleronitrile) (ADVN), 1,1'-azobis(1-cyclohexanecarbonitrile) (ACHN), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) (V-70), and the like.

[0071] In the polymerization step, a vinyl monomer and an organic tellurium compound of formula (4) are mixed in a vessel purged with an inert gas, and for the purpose of promoting the reaction and controlling the molecular weight and molecular weight distribution according to the type of vinyl monomer, an azo-based polymerization initiator and / or an organic ditelluride compound of formula (5) are further mixed. Examples of the inert gas include nitrogen, argon, and helium. Argon and nitrogen are preferable. The amounts of the vinyl monomers (a) and (b) used may be appropriately adjusted depending on the physical properties of the desired copolymer.

[0072] The polymerization reaction can be carried out without a solvent, but may be carried out by stirring the mixture using an aprotic solvent or a protic solvent generally used in radical polymerization. Examples of aprotic solvents that can be used include acetonitrile, methyl ethyl ketone, anisole, benzene, toluene, propylene glycol monomethyl ether acetate, ethyl acetate, tetrahydrofuran (THF), N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), N-methyl-2-pyrrolidone (NMP), acetone, dioxane, chloroform, and carbon tetrachloride. Examples of protic solvents include water, methanol, ethanol, isopropanol, n-butanol, ethyl cellosolve, butyl cellosolve, 1-methoxy-2-propanol, hexafluoroisopropanol, and diacetone alcohol. The solvent may be used alone or in combination of two or more kinds. The amount of the solvent used may be appropriately adjusted, and is preferably 0.01 ml to 50 ml per 1 g of vinyl monomer, for example. The reaction temperature and reaction time may be appropriately adjusted depending on the molecular weight or molecular weight distribution of the resulting copolymer, but typically, the reaction is carried out at 0°C to 150°C for 1 minute to 100 hours. The pressure is typically normal, but may be increased or decreased. After the polymerization reaction is completed, the solvent used and residual vinyl monomers are removed from the resulting reaction mixture by a typical separation and purification means, and the target copolymer can be separated.

[0073] The growing end of the copolymer obtained by the polymerization reaction is -TeR derived from the tellurium compound. 41(In the formula, R 41 is the same as above), and is deactivated by handling in air after the polymerization reaction is completed, but tellurium atoms may remain. Since copolymers with tellurium atoms remaining at the terminals are colored and have poor thermal stability, it is preferable to remove the tellurium atoms. Methods for removing tellurium atoms include radical reduction methods, adsorption methods using activated carbon, and adsorption of metals using ion exchange resins, and these methods can also be used in combination. The other end of the copolymer obtained by the polymerization reaction (the end opposite to the growing end) is formed of -CR derived from the tellurium compound. 42 R 43 R 44 (In the formula, R 42 , R 43 and R 44 is R in Eq. (4). 42 , R 43 and R 44 (same as above.)

[0074] The present invention includes a lubricating oil composition containing a base oil and the lubricating oil additive of the present invention.

[0075] Examples of base oils include mineral oils such as paraffinic mineral oil, naphthenic mineral oil, and refined mineral oils obtained by refining these through hydrorefining, solvent deasphalting, solvent extraction, solvent dewaxing, hydrodewaxing, catalytic dewaxing, hydrocracking, alkali distillation, sulfuric acid washing, clay treatment, etc.; synthetic oils such as poly-α-olefins, ethylene-α-olefin copolymers, polybutenes, alkylbenzenes, alkylnaphthalenes, polyphenyl ethers, alkyl-substituted diphenyl ethers, polyol esters, dibasic acid esters, hindered esters, monoesters, and GTL (Gas to Liquids); and mixed oils of mineral oils and synthetic oils.

[0076] The content of the lubricating oil additive made of the block copolymer of the present invention is preferably 1 part by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, and preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 13 parts by mass or less, relative to 100 parts by mass of base oil. If the content of the lubricating oil additive made of the block copolymer is within the above range, when mixed with the base oil, the copolymer component does not precipitate and it is possible to maintain lubricating performance.

[0077] (Other additives) In addition to the above-mentioned additives, other additives may be added to the lubricating oil composition of the present invention, so long as the effects of the present invention are not impaired. Examples of the other additives include antioxidants, friction reducers, oiliness improvers, detergents, dispersants, viscosity index improvers, pour point depressants, rust inhibitors, corrosion inhibitors, and antifoaming agents, and it is preferable that the additives do not contain sulfur atoms.

[0078] Examples of the antioxidant include 2,6-di-t-butylphenol, 2,6-di-t-butyl-p-cresol, 2,6-di-t-butyl-4-methylphenol, 2,6-di-t-butyl-4 -Ethylphenol, 2,4-dimethyl-6-t-butylphenol, 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-bis(2,6-di-t-butylphenol), 4,4'-bis(2-methyl-6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 4,4'-butylidenebis(3-methyl-6-t-butylphenol), 4,4'-isopropylidenebis(2,6-di-t-butylphenol), 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-methylenebis(4-methyl-6-nonylphenol), 2,2'-isobutylidenebis(4,6-dimethylphenol), 2,6- Bis(2'-hydroxy-3'-t-butyl-5'-methylbenzyl)-4-methylphenol, 3-t-butyl-4-hydroxyanisole, 2-t-butyl-4-hydroxyanisole, 3-(4-hydroxy-3,5-di-t-butylphenyl) octyl propionate, 3-(4-hydroxy-3,5-di-t-butylphenyl) stearyl propionate, 3-(4-hydroxy-3,5-di-t-butylphenyl) oleyl propionate, 3-(4-hydroxy-3,5-di-t-butylphenyl) dodecyl propionate, 3-(4-hydroxy-3,5-di-t-butylphenyl) decyl propionate, 3-(4-hydroxy-3,5-di-t-butylphenyl) octyl propionate, tetrakis{3-(4- hydroxy-3,5-di-t-butylphenyl)propionyloxymethyl}methane, 3-(4-hydroxy-3,5-di-t-butylphenyl)propionic acid glycerol monoester, 3-(4-hydroxy-3,5-di-t-butylphenyl)propionic acid and glycerol monooleyl ether ester, 3-(4-hydroxy-3,5-di-t-butylphenyl)propionic acid butylene glycol diester, 3-(4-hydroxy-3,5-di-t-butylphenyl)propionic acid thiodiglycol diester, 4,4'-thiobis(3-methyl-6-t-butylphenol), 4,4'-thiobis(2-methyl-6-t-butylphenol), 2,2'-thiobis(4-methyl-6-t-butylphenol), 2,6-di-t-butyl-α-dimethylamino-p-cresol, 2,6-di-t-butyl-4-(N,N'-dimethylaminomethylphenol), bis(3,5-di-t-butyl-4-hydroxybenzyl)sulfide, tris{(3,5-di-t-butyl-4-hydroxyphenyl)propionyl-oxyethyl}isocyanurate, tris(3,5-di-t-butyl-4-hydroxyphenyl)isocyanurate, 1,3,5-tris(3,5-di-t-butyl- 4-hydroxybenzyl) isocyanurate, bis{2-methyl-4-(3-n-alkylthiopropionyloxy)-5-t-butylphenyl}sulfide, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl) isocyanurate, tetraphthaloyl-di(2,6-dimethyl-4-t-butyl-3-hydroxybenzyl sulfide), 6-(4-hydroxy-3,5-di-t-butylanilino)-2,4-bis( Octylthio)-1,3,5-triazine, 2,2-thio-{diethyl-bis-3-(3,5-di-t-butyl-4-hydroxyphenyl)}propionate, N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinamide), 3,5-di-t-butyl-4-hydroxy-benzyl-phosphate diester, bis(3-methyl-4-hydroxy-5-t-butylbenzyl sulfide, 3 ,9-Bis[1,1-dimethyl-2-{β-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}ethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis{3,phenolic antioxidants such as 3'-bis-(4'-hydroxy-3'-t-butylphenyl)butyric acid glycol esters; 1-naphthylamine, phenyl-1-naphthylamine, p-octylphenyl-1-naphthylamine, p-nonylphenyl-1- naphthylamine-based antioxidants such as naphthylamine, p-dodecylphenyl-1-naphthylamine, and phenyl-2-naphthylamine; phenylenediamine-based antioxidants such as N,N'-diisopropyl-p-phenylenediamine, N,N'-diisobutyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine, N,N'-di-β-naphthyl-p-phenylenediamine, N-phenyl-N'-isopropyl-p-phenylenediamine, N-cyclohexyl-N'-phenyl-p-phenylenediamine, N-1,3-dimethylbutyl-N'-phenyl-p-phenylenediamine, dioctyl-p-phenylenediamine, phenylhexyl-p-phenylenediamine, and phenyloctyl-p-phenylenediamine; dipyridylamine, diphenylamine, p,p'-di-n Examples of the antioxidant include diphenylamine-based antioxidants such as p,p'-butyldiphenylamine, p,p'-di-t-butyldiphenylamine, p,p'-di-t-pentyldiphenylamine, p,p'-dioctyldiphenylamine, p,p'-dinonyldiphenylamine, p,p'-didecyldiphenylamine, p,p'-didodecyldiphenylamine, p,p'-distyryldiphenylamine, p,p'-dimethoxydiphenylamine, 4,4'-bis(4-α,α-dimethylbenzoyl)diphenylamine, p-isopropoxydiphenylamine, and dipyridylamine; phenothiazine-based antioxidants such as phenothiazine, N-methylphenothiazine, N-ethylphenothiazine, 3,7-dioctylphenothiazine, phenothiazine carboxylic acid ester, and phenoselenazine; and zinc dithiophosphate. The amount of the antioxidant to be blended is preferably 0.01 to 5 parts by mass relative to 100 parts by mass of the base oil. ,

[0079] Examples of the friction reducer include organic molybdenum compounds such as sulfurized oxymolybdenum dithiocarbamate, sulfurized oxymolybdenum dithiophosphate, etc. The amount of the friction reducer to be added is preferably 0.003 to 0.2 parts by mass in terms of molybdenum content per 100 parts by mass of the base oil.

[0080] Examples of the oiliness improver include higher alcohols such as oleyl alcohol and stearyl alcohol, fatty acids such as oleic acid and stearic acid, esters such as oleyl glycerin ester, steryl glycerin ester, and lauryl glycerin ester, amides such as laurylamide, oleylamide, and stearylamide, amines such as laurylamine, oleylamine, and stearylamine, and ethers such as lauryl glycerin ether and oleyl glycerin ether. The amount of the oiliness improver to be blended is preferably 0.1 to 5 parts by mass per 100 parts by mass of the base oil.

[0081] Examples of detergents include sulfonates, phenates, salicylates, phosphates, and overbased salts of calcium, magnesium, barium, etc. Among these, overbased salts are preferred, and among overbased salts, those with a TBN (total basic number) of 30 mgKOH / g to 500 mgKOH / g are more preferred. Furthermore, salicylate-based detergents without phosphorus or sulfur atoms are preferred. The amount of detergent blended is preferably 0.5 to 10 parts by mass per 100 parts by mass of base oil.

[0082] Examples of dispersants include succinimide, succinic acid ester, benzylamine, or boron-modified products thereof, to which an alkyl group or alkenyl group having a weight average molecular weight of 500 to 3,000 has been added. The amount of the dispersant to be added is preferably 0.5 to 10 parts by mass relative to 100 parts by mass of the base oil.

[0083] Examples of viscosity index improvers include poly(C1-C18) alkyl (meth)acrylate, (C1-C18) alkyl acrylate / (C1-18) alkyl (meth)acrylate copolymer, diethylaminoethyl (meth)acrylate / (C1-C18) alkyl (meth)acrylate copolymer, ethylene / (C1-1C8) alkyl (meth)acrylate copolymer, polyisobutylene, polyalkylstyrene, ethylene / propylene copolymer, styrene / maleic acid ester copolymer, and styrene / hydrogenated isoprene copolymer. Alternatively, a dispersant or multifunctional viscosity index improver having dispersing properties may be used. The average molecular weight is preferably about 10,000 to 1,500,000. The amount of the viscosity index improver to be blended is preferably 0.1 to 20 parts by mass relative to 100 parts by mass of the base oil.

[0084] Examples of pour point depressants include polyalkyl (meth)acrylates, polyalkylstyrenes, polyvinyl acetates, etc. The pour point depressant preferably has a weight average molecular weight of 1,000 to 100,000. The pour point depressant is preferably added in an amount of 0.005 to 3 parts by mass relative to 100 parts by mass of the base oil.

[0085] Examples of the rust inhibitor include sodium nitrite, oxidized paraffin wax calcium salt, oxidized paraffin wax magnesium salt, tallow fatty acid alkali metal salt, alkaline earth metal salt or amine salt, alkenylsuccinic acid or alkenylsuccinic acid half ester (the molecular weight of the alkenyl group is about 100 to 300), sorbitan monoester, nonylphenol ethoxylate, lanolin fatty acid calcium salt, etc. The amount of the rust inhibitor to be blended is preferably 0.01 to 3 parts by mass per 100 parts by mass of the base oil.

[0086] Examples of the corrosion inhibitor include benzotriazole, benzimidazole, benzothiazole, benzothiadiazole, tetraalkylthiuram disulfide, etc. The amount of the corrosion inhibitor to be added is preferably 0.01 to 3 parts by mass with respect to 100 parts by mass of the base oil.

[0087] Examples of the antifoaming agent include polydimethyl silicone, trifluoropropylmethyl silicone, colloidal silica, polyalkyl acrylate, polyalkyl methacrylate, alcohol ethoxy / propoxylate, fatty acid ethoxy / propoxylate, sorbitan partial fatty acid ester, etc. The amount of the antifoaming agent to be blended is preferably 0.001 to 0.1 parts by mass relative to 100 parts by mass of the base oil.

[0088] The lubricating oil composition of the present invention can be used as a lubricating oil composition for a lubrication system that comes into contact with metal materials such as iron, steel, stainless steel, aluminum, etc., and can be used particularly suitably in cold environments. Examples of such lubricating oil compositions include metal processing oils, engine oils, drive system oils, hydraulic oils, etc. EXAMPLES

[0089] The present invention will be described in more detail below with reference to specific examples. The present invention is not limited to the following examples, and can be modified as appropriate within the scope of the present invention.

[0090] PDMSMA: methacrylate having a polydimethylsiloxane group (X-174ASX manufactured by Shin-Etsu Chemical Co., Ltd., functional group equivalent (g / mol): 900, number average molecular weight: 900) MOESA: 2-Methacryloyloxyethyl hydrogen succinate SMA: Stearyl methacrylate HEMA: Hydroxymethyl methacrylate BTEE: Ethyl 2-methyl-2-n-butyltellanyl propionate DBDT: Dibutyl ditelluride AIBN: 2,2'-azobis(isobutyronitrile) BuAc: butyl acetate

[0091] [Evaluation method] (Polymerization rate) Using a nuclear magnetic resonance (NMR) measuring device (Bruker, model: AVANCE500 (frequency 500 MHz)), 1 H-NMR was measured (solvent: deuterated chloroform, internal standard: tetramethylsilane). From the obtained NMR spectrum, the integral ratio of the peaks of the vinyl group derived from the monomer and the ester side chain derived from the polymer was calculated, and the polymerization rate of the monomer was calculated.

[0092] (Weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (D)) The molecular weight was determined by gel permeation chromatography (GPC) using a high performance liquid chromatograph (Tosoh, model: HLC-8320). A column of SHODEX GPC KF-603 (Φ6.0mm×150mm) (Showa Denko) was used, a 30mmol / L lithium bromide-30mmol / L acetate-N-methylpyrrolidone solution was used as the mobile phase, and a differential refractometer was used as the detector. The measurement conditions were: column temperature 40°C, sample concentration 10mg / mL, sample injection amount 10μL, and flow rate 0.2mL / min. A calibration curve was created using polystyrene (molecular weight 70,500, 37,900, 19,920, 10,200, 4,290, 2,630, 1,150) as the standard substance, and the weight average molecular weight (Mw) and number average molecular weight (Mn) were measured. From these measured values, the molecular weight distribution (D=Mw / Mn) was calculated.

[0093] (friction coefficient measurement) The friction coefficient was measured using an automatic friction and wear analyzer TS500 manufactured by Kyowa Interface Science. Specifically, 10 parts by mass of lubricant additive was added to 100 parts by mass of poly-α-olefin as base oil to prepare a lubricant. 20 μl of the base oil solution was dropped onto a steel plate, and measurements were repeated 50 times under point contact conditions while applying a load of 50 g using SUS beads. In the case of cooling measurements, the steel plate was cooled to -10°C, and measurements were repeated 10 times in the same manner.

[0094] <Production of copolymer> (Synthesis Example 1) In a 50 mL reactor purged with argon, 12.00 g of PDMSMA, 0.30 mg of BTEE, 0.18 mg of DBDT, 33 mg of AIBN, and 12.00 g of BuAc, which had been previously purged with argon, were charged and reacted at 60° C. for 24 hours. The polymerization rate was 99%.

[0095] To this reaction solution, 2.00 g of MOESA and 2.00 g of BuAc, which had been replaced with argon in advance, were added and reacted at 60°C for 24 hours. After the reaction was completed, the reaction solution was poured into methanol under stirring. The precipitated polymer was suction filtered and dried to obtain Copolymer 1. The polymerization rate was 97%, the number average molecular weight (Mn) was 14,430, and the molecular weight distribution (D) was 1.38.

[0096] (Synthesis Examples 2 to 4) Copolymers 2 to 4 were prepared in the same manner as in Synthesis Example 1. Table 1 shows the monomers, organotellurium compounds, organoditellurium compounds, azo-based polymerization initiators, solvents, reaction temperatures, reaction times, and polymerization rates used. Table 2 shows the composition, number average molecular weight (Mn), and molecular weight distribution (D) of each copolymer. The content of each structural unit in the copolymer was calculated from the charge ratio of the monomers used in the polymerization reaction and the polymerization rate.

[0097] [Table 1]

[0098] [Table 2]

[0099] Example 1 Copolymer 1 obtained in Synthesis Example 1 was dissolved in 11.1 parts by mass per 100 parts by mass of poly-α-olefin base oil. 20 μl of this solution was dropped onto an SS400 substrate, and a SUJ-2 (3 mm, grade G-20) with a load of 50 g was used to move the substrate 4 mm at a speed of 0.2 mm / s. This measurement was repeated 50 times at 23°C to measure the friction coefficient.

[0100] Example 2 The same measurements as in Example 1 were carried out, except that Copolymer 2 obtained in Synthesis Example 2 was used instead of Copolymer 1.

[0101] Example 3 The same measurements as in Example 1 were carried out, except that Copolymer 3 obtained in Synthesis Example 3 was used instead of Copolymer 1.

[0102] Comparative Example 1 The same measurements as in Example 1 were carried out, except that silicone oil (KF-96-50CS manufactured by Shin-Etsu Chemical Co., Ltd.) was used instead of Copolymer 1.

[0103] Comparative Example 2 The same measurements as in Example 1 were carried out, except that Copolymer 4 obtained in Synthesis Example 4 was used instead of Copolymer 1.

[0104] Example 4 Copolymer 3 obtained in Synthesis Example 5 was dissolved in 11.1 parts by mass per 100 parts by mass of poly-α-olefin base oil. The solution was cooled to -10°C and a SUJ-2 (3 mm, grade G-20) with a 50 g load was moved 4 mm at a speed of 0.2 mm / s. This measurement was repeated 50 times to measure the friction coefficient.

[0105] Comparative Example 3 The same measurements as in Example 4 were carried out, except that Copolymer 4 obtained in Synthesis Example 4 was used instead of Copolymer 3.

[0106] The evaluation results for each lubricating oil are shown in Table 3. [Table 3]

[0107] The results in Table 3 show that the lubricating oil of the present invention, which contains a lubricating oil additive consisting of a block copolymer containing an A block containing structural unit (a-1) derived from a vinyl monomer (a) having a polyorganosiloxane group, and a B block containing structural unit (b-1) derived from a vinyl monomer (b) containing a polar group, has a small coefficient of friction.

[0108] A comparison between Example 1 and Example 2 shows that the friction coefficient of a lubricating oil containing a lubricating oil additive made of a block copolymer having a B block containing a structural unit (b-1) derived from a vinyl monomer having a carboxyl group as the vinyl monomer (b) containing a polar group is smaller than that of a lubricating oil containing a block copolymer having a B block containing a structural unit (b-1) derived from a vinyl monomer having a hydroxyl group. A comparison between Example 4 and Comparative Example 3 shows that the effect of the lubricating oil additive of the present invention is remarkable in the low temperature range. [Industrial Applicability]

[0109] The lubricating oil additive of the present invention can be suitably applied to lubricating oils for various applications such as metal processing oils, engine oils, drive system oils, hydraulic oils, etc. Furthermore, the lubricating oil additive of the present invention does not contain sulfur and has a small environmental impact.

[0110] A preferred embodiment (1) of the present invention is a lubricating oil additive characterized by comprising a block copolymer including an A block containing a structural unit (a-1) derived from a vinyl monomer (a) having a polyorganosiloxane group, and a B block containing a structural unit (b-1) derived from a vinyl monomer (b) containing a polar group.

[0111] A preferred embodiment (2) of the present invention is the lubricating oil additive according to embodiment (1), in which the vinyl monomer (a) is a (meth)acrylate having a polyorganosiloxane group and / or a (meth)acrylamide having a polyorganosiloxane group.

[0112] A preferred embodiment (3) of the present invention is the lubricating oil additive according to the embodiment (1) or (2), wherein the vinyl monomer (a) has a number average molecular weight of 500 to 50,000.

[0113] A preferred embodiment (4) of the present invention is the lubricating oil additive according to any one of the embodiments (1) to (3), in which the vinyl monomer (b) is represented by general formula (3). [ka] [In the formula, R 31 R represents a hydrogen atom or a methyl group. 32 represents a single bond or a divalent organic group. Y 3 represents a polar group.

[0114] A preferred embodiment (5) of the present invention is the lubricating oil additive according to any one of the embodiments (1) to (4), in which the polar group is at least one selected from the group consisting of a hydroxy group, a carboxy group, and an amino group.

[0115] A preferred embodiment (6) of the present invention is the lubricating oil additive according to any one of the embodiments (1) to (5), wherein the mass ratio of the A block to the B block (A block / B block) in the block copolymer is 50 / 50 to 99 / 1.

[0116] A preferred embodiment (7) of the present invention is the lubricating oil additive according to any one of the embodiments (1) to (6), wherein the block copolymer has a number average molecular weight of 5,000 to 100,000.

[0117] A preferred embodiment (8) of the present invention is the lubricating oil additive according to any one of the embodiments (1) to (7), wherein the block copolymer is obtained by living radical polymerization and has a molecular weight distribution of 2.5 or less.

[0118] A preferred embodiment (9) of the present invention is the lubricating oil additive according to any one of the embodiments (1) to (8), wherein the block copolymer does not contain a sulfur atom in the main chain or a side chain.

[0119] A preferred embodiment (10) of the present invention is a lubricating oil composition containing a base oil and the lubricating oil additive according to any one of the embodiments (1) to (9).

[0120] A preferred embodiment (11) of the present invention is the lubricating oil composition according to the embodiment (10), wherein the base oil is at least one selected from the group consisting of mineral oils and synthetic oils.

[0121] A preferred embodiment (12) of the present invention is the lubricating oil composition according to embodiment (10) or (11), wherein the lubricating oil additive is blended in an amount of 1 to 20 parts by mass per 100 parts by mass of the base oil.

[0122] A preferred embodiment (13) of the present invention is a lubrication system in which a metal material is contacted with the lubricating oil composition according to any one of the embodiments (10) to (12).

Claims

1. A lubricating oil additive comprising a block copolymer including an A block containing a structural unit (a-1) derived from a vinyl monomer (a) having a polyorganosiloxane group, and a B block containing a structural unit (b-1) derived from a vinyl monomer (b) containing a polar group.

2. 2. The lubricating oil additive according to claim 1, wherein the vinyl monomer (a) is a (meth)acrylate having a polyorganosiloxane group and / or a (meth)acrylamide having a polyorganosiloxane group.

3. 2. The lubricating oil additive according to claim 1, wherein the vinyl monomer (a) has a number average molecular weight of 500 to 50,000.

4. The lubricating oil additive according to claim 1, wherein the vinyl monomer (b) is represented by the general formula (3): [Formula 1] [In the formula, R 31 R represents a hydrogen atom or a methyl group. 32 represents a single bond or a divalent organic group. 3 represents a polar group.

5. 2. The lubricating oil additive according to claim 1, wherein the polar group is at least one selected from the group consisting of a hydroxy group, a carboxy group, and an amino group.

6. 2. The lubricating oil additive according to claim 1, wherein the mass ratio of the A block to the B block (A block / B block) in the block copolymer is from 50 / 50 to 99 / 1.

7. 2. The lubricating oil additive according to claim 1, wherein the block copolymer has a number average molecular weight of 5,000 to 100,000.

8. 2. The lubricating oil additive according to claim 1, wherein the block copolymer is obtained by living radical polymerization and has a molecular weight distribution of 2.5 or less.

9. 2. The lubricating oil additive according to claim 1, wherein the block copolymer does not contain a sulfur atom in the main chain or in a side chain.

10. A lubricating oil composition comprising a base oil and the lubricating oil additive according to any one of claims 1 to 9.

11. The lubricating oil composition according to claim 10, wherein the base oil is at least one selected from the group consisting of mineral oils and synthetic oils.

12. The lubricating oil composition according to claim 10, wherein the lubricating oil additive is blended in an amount of 1 to 20 parts by mass per 100 parts by mass of the base oil.

13. A lubrication system in which a metallic material is in contact with the lubricating oil composition of claim 10.

Citation Information

Patent Citations

  • Viscosity index improver and lubricant composition

    JP2016028138A

  • Polymeric inorganic particles useful as lubricant additives

    JP2019527280A

  • Lubricating oil additive and lubricating oil composition

    JP2023140298A

  • Antifoaming agent, lubricating oil composition containing antifoaming agent, and machine using the lubricating oil composition

    JP7099659B1

  • Antifoaming agent, lubricating oil composition containing said antifoaming agent, and machine using said lubricating oil composition

    JP7616493B2