New formulation for low-carbon construction binder, preparation method and construction material
A construction binder formulation using a raw clay matrix and deflocculant achieves comparable mechanical properties to Portland cement, addressing the industry's high carbon emissions by reducing greenhouse gas emissions and enhancing thermal comfort in construction materials.
Patent Information
- Application Number
- JP2024117977
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-02-08
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-23
AI Technical Summary
The cement industry contributes significantly to carbon emissions due to high energy consumption and CO2 release, and existing alternative binders either have high clinker content or insufficient mechanical properties, limiting their effectiveness as low-carbon replacements for Portland cement.
A construction binder formulation comprising a raw clay matrix and a deflocculant, with specific mineral species and peptizers, achieves mechanical properties comparable to Portland cement while reducing greenhouse gas emissions by 30-85%, particularly through the use of a raw clay matrix and an activator composition.
The formulation provides construction materials with mechanical properties comparable to Portland cement while significantly reducing carbon footprint, improving moisture-thermal properties, and allowing for the production of construction elements with enhanced comfort and reduced environmental impact.
Smart Images

Figure 2024150651000009 
Figure 2024150651000001 
Figure 2024150651000002
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of construction materials, more particularly to the field of binders that can be used in construction. The present invention relates to a formulation for a construction binder. The present invention also relates to a method for preparing a construction binder, the construction binder itself, as well as the use of such a binder in the manufacture of construction materials. [Background technology]
[0002] Cement is the second most consumed resource in the world, with over 4 billion tonnes of the material produced worldwide each year, and this consumption is constantly growing, driven by the growing demand for housing and infrastructure.
[0003] Cement is generally a hydraulic binder, which means that it hardens and sets when mixed with water. After hardening, cement maintains its strength and stability even when exposed to water. There is a wide variety of cements in use around the world. Nevertheless, all conventional cements contain clinker in percentages ranging from 5% for some blast-furnace cements to a minimum of 95% for Portland cement. Portland cement is the most widely used cement in the world today.
[0004] Clinker is the result of the calcination of a mixture of about 80% limestone and 20% aluminosilicates (such as clays). This calcination, clinkerization, takes place at temperatures of over 1200°C, so such a cement preparation process implies high energy consumption. Moreover, the chemical conversion of limestone to lime also releases carbon dioxide. As a result, the cement industry generates about 8% of the world's CO2 emissions. In response to this challenge, industry and researchers are looking for ways to reduce the impact of carbon dioxide emissions generated by the cement industry.
[0005] First solutions have involved the creation of cement plants that use a combination of waste-based alternative fuels and technologies related to the capture and storage of carbon emissions during cement production to achieve zero-emission status, but these solutions are not yet available on an industrial scale and require significant investments.
[0006] The recommended route is to find alternatives to Portland cement, which is too energy intensive. Indeed, the development of alternative construction binders that require less energy consumption in production could reduce the energy footprint of the entire construction industry (Maddalena et al., "Can Portland cement be replaced by low-carbon alternative materials? A study of the thermal properties and carbon emissions of innovative cements", Journal of Cleaner Production 186; 2018; 933-942).
[0007] For example, new hydraulic binders have been proposed that are similar to Portland cement but contain secondary components such as ash formed during coal combustion in power plants. However, the secondary components (ash, pozzolans, blast furnace slag) typically make up to 35% of the mixture, and this composite Portland cement contains at least 50% clinker. This is still too high a clinker content to be a true low-carbon alternative to Portland cement.
[0008] Metakaolin-based hydraulic binders, i.e. cements, have also been proposed. Metakaolin is a dehydroxylated alumina silicate of general composition Al2Si2O7, a largely amorphous dehydration product of kaolinite of general formula Al2(OH)4Si2O5 with strong pozzolanic activity. In general, the pozzolanic activity of a material can be defined as the ability of a material, which does not have binding properties, but which, in finely divided form, in the presence of moisture, reacts chemically with calcium hydroxide at room temperature to form compounds with binding properties. Kaolinite clay is widely available in the earth's crust, and heat treatment (e.g., at 600-800 °C for a short time, called "flash") dehydroxylates the kaolinite crystal structure to produce metakaolin. The mixture of lime or sodium hydroxide with metakaolin during the hydration of cement induces a pozzolanic reaction. This reaction enhances the binding properties of metakaolin-based cements. Due to these properties, metakaolin-based construction materials have been proposed, including flash metakaolin associated with sodium hydroxide, as described in documents FR3034094 or US10315115. The rheological properties of these construction binders can be improved by adding plasticizers or water reducers such as polyacrylates or lignosulfonates. However, such methods, which require high temperature rise, have a high energy consumption and therefore require improvement of the carbon footprint.
[0009] On the other hand, the use of uncalcined kaolinite or a wider use of raw clay matrix has been proposed for cements with a low carbon footprint (NA Hadi, "Geopolymerization of Kaolin and Metakaolin Incorporating NaOH and High Calcium Ash", Earth Science Research Vol. 5, No. 1; 2016). However, these cements either had too low physical properties such as improved mechanical strength, reduced capillary absorption or reduced liquid permeability, as described in document FR3016376, or required the partial addition of Portland cement to have acceptable mechanical properties.
[0010] Moreover, classically, it has been proposed to add construction binders to soils to form construction materials. Nevertheless, these construction materials have limited mechanical properties. Indeed, a publication by Ulrich Rohlen and Christof Ziegert entitled "Construire en terre crue, construction-renovation-finitions" (2013, editions le Moniteur ISBN 978-2-281-11567-3) shows that the compressive strength of soil concrete varies from 0.6 MPa up to 12 MPa, with typical values of about 3 MPa. Furthermore, a publication entitled "Traite de Construction en terre" measures the evolution of the compressive strength of soils stabilized with cement and shows that the compressive strength values of soil concretes containing, in particular, 7% cement (i.e. 50% cement in a binder made of cement and clay) do not exceed 12 MPa. This has always discouraged builders from using excessively high contents of raw clay in construction binders and, more generally, in construction materials requiring high compressive strength.
[0011] Therefore, there is a need for new formulations of construction binders with a low carbon footprint while producing mechanical properties of concrete at least equal to or better than those of concrete from cements commonly used in the construction sector such as CEM I, CEM II, CEM III, CEM IV, and CEM V cements, as defined in the NF EN197-1 standard. Summary of the Invention [Problem to be solved by the invention]
[0012] The present invention therefore aims to overcome the disadvantages of the prior art, in particular to provide a formulation for a construction binder, which on the one hand allows to obtain a construction material with mechanical properties at least comparable to those of Portland cement, and on the other hand improves the comfort of the inhabitants compared to concrete made from Portland cement.
[0013] The present invention also aims to provide a method for producing a construction binder, which reduces the emission of greenhouse gases, such as carbon dioxide, released during the preparation of such a binder, while maintaining the mechanical properties of said binder related to its use in the construction sector.The present invention also relates to the use of a construction binder for the production of construction elements, which allows improving the comfort of the inhabitants, in particular the hygrothermal properties of buildings, compared to conventional concrete. [Means for solving the problem]
[0014] To this end, the present invention relates to a construction binder formulation comprising, in dehydrated form, a raw clay matrix and a deflocculating agent.
[0015] This dehydrated mix is therefore intended to totally or partially replace traditional cements such as Portland cement, lime, or calcium aluminate cements ("calcium sulphoaluminate cements" - CSA in Anglo-Saxon terminology). As shown below, this mix allows to achieve the same mechanical performance as Portland cement (class C 25 / 30) while reducing greenhouse gas emissions by 30-85%, more commonly by around 50%.
[0016] Furthermore, the presence of the original clay matrix allows for better moisture heat transfer and therefore better cooling properties of constructions using binders resulting from this formulation.
[0017] Other optional features of the formulation include: - the original clay matrix comprises at least one mineral species selected from kaolinite, illite, smectite, bentonite, chlorite, montmorillonite, muscovite, halloysite, sepiolite, attapulgite, vermiculite and the so-called layered clays, which are complex combinations of several clays. The presence of one or more of these mineral species in the binder formulation allows to obtain a construction material with good mechanical properties, i.e. mechanical properties comparable to those of construction materials containing cement and, more generally, Portland cement. Preferably, the original clay matrix comprises at least one mineral species selected from kaolinite, illite, smectite and bentonite. - it contains at least 80% by weight of original clay matrix, preferably 80-99.5% by weight, more preferably 90-99% by weight. This amount of original clay matrix makes it possible to improve the mechanical properties of materials built with this formulation. the deflocculating agent is selected from: - non-ionic surfactants such as polyoxyethylene ethers; anionic agents such as anionic agents selected from alkylarylsulfonates, amino alcohols, carbonates, silicates, fatty acids, humates (e.g. sodium humate), carboxylic acids, lignosulfonates (e.g. sodium lignosulfonate), polyacrylates, phosphates or polyphosphates such as sodium hexametaphosphate, sodium tripolyphosphate, sodium orthophosphate, carboxymethylcellulose and mixtures thereof; - a polyacrylate, such as a polyacrylate selected from sodium polyacrylate or ammonium polyacrylate; - 2-amino-2-methyl-1-propanol; monoethanolamine, diethanolamine, or triethanolamine; amines such as amines selected from isopropanolamine (1-amino-2-propanol, diisopropanolamine and triisopropanolamine) and N-alkylated ethanolamines; or - A mixture of them. These deflocculants allow for good dispersion of the clay and are suitable for use in clay matrices that can be used in construction. the deflocculating agent represents at least 0.5% by weight of the original clay matrix, preferably between 0.5 and 20% by weight of the original clay matrix, more preferably between 1 and 10% by weight, such a concentration making it possible to improve the mechanical properties of the material made from this formulation; - it is, - 80-99.5% by weight of the original clay matrix, and - 0.5 to 20% by weight of a deflocculating agent, Such formulations for construction binders can achieve mechanical properties equivalent to Portland cement when such formulations are used in combination with an activator composition.
[0018] The present invention further relates to a construction binder comprising the components of the construction binder formulation according to the invention and an activator composition. In particular, the present invention further relates to a construction binder comprising a raw clay matrix, a deflocculating agent and an activator composition, characterized in that the construction binder comprises at least 30% by weight of the raw clay matrix. The activator composition makes it possible to impart the desired mechanical properties to the construction binder and in particular to structure the clay sheets.
[0019] According to other optional characteristics of the construction material: The construction binder comprises less than 30% by weight of metakaolin, preferably less than 26% by weight of metakaolin, more preferably less than 21% by weight of metakaolin, less than 17% by weight of metakaolin, less than 13% by weight of metakaolin, even more preferably less than 10% by weight of metakaolin, less than 5% by weight of metakaolin, for example no metakaolin. - the original clay matrix contains at least one mineral species selected from kaolinite, illite, smectite, bentonite, chlorite, montmorillonite, muscovite, halloysite, sepiolite, attapulgite, vermiculite and the so-called interlayer clays which are complex combinations of several clays; - the original clay matrix contains at least one mineral species selected from kaolinite, illite, smectite, bentonite, chlorite, montmorillonite, muscovite, halloysite, sepiolite, attapulgite, vermiculite and the so-called interlayer clays which are complex combinations of several clays; - It comprises at least 40% by weight of a raw clay matrix. the deflocculating agent is selected from: - non-ionic surfactants such as polyoxyethylene ethers; anionic agents such as anionic agents selected from alkylarylsulfonates, amino alcohols, carbonates, silicates, fatty acids, humates (e.g. sodium humate), carboxylic acids, lignosulfonates (e.g. sodium lignosulfonate), polyacrylates, phosphates or polyphosphates such as sodium hexametaphosphate, sodium tripolyphosphate, sodium orthophosphate, carboxymethylcellulose and mixtures thereof; - a polyacrylate, such as a polyacrylate selected from sodium polyacrylate or ammonium polyacrylate; - 2-amino-2-methyl-1-propanol; monoethanolamine, diethanolamine, or triethanolamine; amines such as amines selected from isopropanolamine (1-amino-2-propanol, diisopropanolamine and triisopropanolamine) and N-alkylated ethanolamines; or - A mixture of them. The deflocculating agent represents at least 0.25% by weight of the construction binder. The activator composition represents at least 10% by weight of the construction binder. The original clay matrix, deflocculating agent, and activator composition form a two-component or multi-component system. - it is, - 30-80% by weight of the original clay matrix, - 0.25 to 20% by weight of a deflocculating agent, and - 10 to 50% by weight of an activator composition, Includes. The activator composition is an alkaline activator composition. The alkaline composition may, for example, comprise a compound having a pKa greater than or equal to 10, more preferably greater than or equal to 12, even more preferably substantially equal to 14. The activator composition comprises an organophosphorus compound, such as sodium tripolyphosphate, preferably the organophosphorus compound represents at least 2% by weight of the construction binder. - it comprises at least 2% by weight of a metal oxide. In particular, the activator composition comprises a metal oxide. In particular, the metal oxide is present in a content of at least 2% by weight of the composition, preferably at least 5% by weight of the composition, even more preferably at least 10% by weight of the composition. Such a concentration makes it possible to improve the mechanical properties of the material made from this formulation. The metal oxide is selected from iron oxides such as FeO, Fe3O4, Fe2O3, alumina Al2O3, manganese(II) oxide MnO, titanium(IV) oxide TiO2 and mixtures thereof. The activator composition comprises a cement, preferably a Portland cement, which may be, for example, a CEM I type cement. It comprises a blast furnace slag composition, preferably the blast furnace slag composition represents at least 5% by weight of the construction binder. - it is, - 40-70% by weight of the original clay matrix, - 0.5 to 6% by weight of a deflocculating agent, - 5 to 20% by weight of an activator composition, and - 20-45% by weight of blast furnace slag, Includes. - it is, - 35-65% by weight of the original clay matrix, - 0.5 to 5% by weight of a deflocculating agent, - 31-49% by weight of Portland CEM 1 type cement, Includes. - it is, - 35-65% by weight of the original clay matrix, - 0.5 to 5% by weight of a deflocculating agent, - 10-30% by weight of blast furnace slag, and - 15-35% by weight of Portland CEM 1 type cement, Includes. - it is, - 45-70% by weight of the original clay matrix, - 0.5 to 6% by weight of a deflocculating agent, - 10 to 30% by weight of an activator composition, and - 15 to 35% by weight of metakaolin, Includes. - it is, - 45-70% by weight of the original clay matrix, - 0.5 to 5% by weight of a deflocculating agent, - 10 to 25% by weight of an activator composition, - 5-20% by weight of blast furnace slag, and - 15 to 30% by weight of metakaolin, Includes.
[0020] These amounts allow for mechanical properties comparable to Portland cement while significantly reducing the carbon footprint.
[0021] The present invention further relates to a method for preparing a construction binder. A method of preparing a construction binder may comprise the steps of mixing a raw clay matrix, a deflocculating agent and an activator composition, said construction binder comprising at least 30% by weight of the raw clay matrix.
[0022] In particular, the method for preparing a construction binder may in particular comprise the following steps: - preparing a clay suspension comprising at least one raw clay matrix, one deflocculating agent and water; - adding an activator composition to the clay suspension, said activator composition may be an alkaline activator composition and / or may include a metal oxide; - mixing to obtain a construction binder, said construction binder comprising at least 30% by weight of the original clay matrix.
[0023] According to other optional characteristics of the method: It comprises a step of mixing a clay suspension to obtain a peptized clay suspension, after which an activator composition is added. The construction binder comprises at least 50% by weight, preferably 50-80% by weight, of a raw clay matrix. It may also comprise at least 40% by weight, preferably 40 to 60% by weight, of a raw clay matrix. The deflocculating agent represents at least 0.25% by weight of the construction binder, preferably at least 0.5% by weight of the construction binder, more preferably between 0.5 and 10% by weight of the construction binder. The activator composition is present in a content of at least 10% by weight of the binder, for example the metal oxide is present in a content of at least 10% by weight of the binder.
[0024] The invention further relates to construction materials, such as mortars, coatings, plasters, insulation materials, lightweight concrete, prefabricated elements, etc., which comprise the construction binder according to the invention.
[0025] According to other optional characteristics of the construction material: - the construction binder comprises excavated soil, said excavated soil comprising a raw clay matrix. Indeed, in contrast to known construction materials, within the framework of the present invention it is possible to produce a construction binder, and thus, by extension, a construction material with sufficient compressive strength, directly from the excavated soil. The excavated soil may further comprise aggregates, such as, but not limited to, sand and / or gravel. - it further comprises one or more fillers, the fillers being for example selected from mineral or vegetable fillers. The fillers may be any fillers known to the person skilled in the art of construction materials. In particular, they may be selected from recycled or non-recycled aggregates, powders, sand, grit, gravel and / or fibres. The fibres may in particular be sawdust, wood chips and fibres, straw, flax, perlite, cork or even fibres of plant origin, such as kennebot. Preferably, the construction material according to the invention further comprises fibres of plant origin. - It contains pigments. - It further comprises a foaming or expanding agent such as aluminum powder.
[0026] According to another aspect, the invention relates to the use of a construction binder according to the invention for the production of covering elements, in particular floor coverings such as tiles, slabs, paving stones or edgings, interior or exterior facade elements, wall coverings such as cladding panels, planking elements or roof coverings of the tile type, for the production of extruded or moulded construction modules such as bricks or for the production of various extruded shapes.
[0027] The invention relates to the use of a construction binder according to the invention for the manufacture of composite materials such as construction panels of the prefabricated panel type, prefabricated blocks such as door or window lintels, prefabricated wall elements or any other prefabricated construction elements.
[0028] The present invention relates to the use of a construction binder according to the invention for the production of insulating modules, such as partition panels or lightweight insulating construction modules (having a density of less than 1.5 kg / L, preferably less than 1.2 kg / L, more preferably less than 1.0 kg / L, more preferably less than 0.7 kg / L).
[0029] The invention relates to the use of a construction binder according to the invention for the production of construction elements, buildings or houses, or decorative items by additive manufacturing, such as by means of a 3D printer.
[0030] The present invention relates to the use of a construction binder according to the invention for the production of a sealant, adhesive or grout in the form of a two-component system having either a composition in solid form on the one hand and a composition in liquid form on the other hand, or a composition in the form of two pastes.
[0031] The present invention also relates to the use of a deflocculating agent in combination with a raw clay matrix and an activator composition for the preparation of a construction binder, the raw clay matrix representing at least 30% by weight of the construction binder, and the activator composition being a composition for obtaining concrete having a minimum compressive strength of the cylinder at 28 days, measured according to the NF EN206-1 standard, of at least 20 MPa, preferably at least 25 MPa, more preferably at least 40 MPa.
[0032] Other advantages and features of the present invention will become apparent upon reading the following description, given by way of illustrative and non-limiting example, with reference to the attached figures, in which: [Brief description of the drawings]
[0033] [Figure 1] FIG. 1 shows a diagram of a method for preparing a construction binder according to the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] In the following description, the term "wt. %" with respect to the raw clay matrix, the mixture, the binder or the construction material is to be understood as a percentage based on the dry weight of the mixture, the binder or the construction material. The dry weight is the weight before adding water, which is necessary, for example, to form a construction binder.
[0035] The term "dehydrated" in the sense of the present invention corresponds to a formulation containing a reduced amount of water, for example a water content of less than 20% by weight, preferably less than 10% by weight, more preferably less than 5% by weight, for example less than 1% by weight. The water content can be measured by any method known in the art. For example, it can be measured according to the NF P 94 050 standard "Determination of the moisture content of materials: oven drying method" of September 1995.
[0036] By "clay matrix" is meant one or more rock materials based on hydrated silicates or aluminosilicates of lamellar structure, said clay matrix being composed of fine particles generally resulting from the alteration of silicates with a three-dimensional framework, such as feldspar. The clay matrix may therefore comprise a mixture of such rock materials, which may consist, for example, of kaolinite, illite, smectite, bentonite, chlorite, vermiculite, metakaolin or mixtures thereof. The expression "original clay matrix" corresponds within the meaning of the present invention to a clay matrix that has not undergone a calcination step. In particular, it has not undergone a prior heat treatment. For example, it corresponds to a clay matrix that has not undergone a temperature increase of more than 300°C, preferably more than 200°C, more preferably more than 150°C. In fact, the original clay matrix may undergo a heating step, which generally requires a temperature increase of less than or equal to 150°C, but does not undergo a calcination step.
[0037] "Debulker" or "Peptizer" means any compound that breaks up aggregates and colloids in an aqueous suspension. Deflocculants have been used, for example, in the context of oil drilling or extraction to make clays more fluid and easier to extract or drill.
[0038] By "active agent composition" is meant any composition that functions to promote the formation of compact structures, thereby enhancing the mechanical strength of a material incorporating such active agent composition.
[0039] The term "substantially equal" within the meaning of the present invention corresponds to a value that varies from a comparison value by less than 20%, preferably by less than 10%, and even more preferably by less than 5%.
[0040] The inventors have developed new formulations for construction binders that can be used advantageously, but not exclusively, as a replacement for Portland cement, lime or CSA. The formulations according to the invention, more particularly the construction binders according to the invention, have the advantage of having a carbon footprint at least two times lower than most of the construction binders most used in the world today, or hydraulic binders (i.e. Portland cement). In fact, the construction binders according to the invention are mainly composed of a clay matrix, also called raw clay matrix, which has not undergone a calcination process, an energy-consuming process that generates the emission of greenhouse gases, more particularly carbon dioxide.
[0041] Furthermore, the mix or construction binder according to the invention has a lower clinker content than comparable products and, for comparable mechanical properties, can reduce CO2 emissions and production costs.
[0042] Advantageously, as shown in the examples, the construction binder according to the invention allows the production of construction materials having mechanical properties at least equivalent to those of concrete formulated with Portland cement or with "low carbon" materials such as those mentioned above.
[0043] Thus, according to a first aspect, the present invention relates to a formulation of a construction binder comprising, in dehydrated form, a raw clay matrix and a deflocculating agent.
[0044] As mentioned above, the use of a raw clay matrix can reduce the environmental impact of construction binders.
[0045] Deflocculants are already used with clays, especially pottery and ceramics, where the preparation of a liquid, non-dehydrated slip may involve mixing the deflocculant with the clay matrix. This practice allows the clay to be liquefied and only the fine particles recovered; this practice is not intended for the preparation of construction binders.
[0046] Here, without being limited to theory, the deflocculating agent is able to locate itself at the interface of the sheets that make up the original clay matrix and break it down. The use of the deflocculating agent will therefore make it possible to obtain from the original clay matrix a formulation that contains a broken-down original clay matrix and that, in the presence of the activator composition, is able to form a more effective construction binder.
[0047] Such formulations can be prepared without prior preparation or can be prepared at a manufacturing site and optionally stored before being transported to the construction site.
[0048] Thus, the present invention relates to a formulation for a construction binder, for example comprising a raw clay matrix and a deflocculating agent, which can be stored and / or transported until it is mixed with an activator composition, thereby allowing the formation of a construction binder. In particular, the formulation can be stored in a container with a volume of between 0.5 L and 50 L.
[0049] The general and preferred properties of each component of the formulation according to the invention are presented in detail.
[0050] Raw clay matrix The original clay matrix may include at least one mineral species selected from, for example, kaolinite, illite, smectite, bentonite, chlorite, and vermiculite. Table 1 below shows the chemical properties of these mineral species. [Table 1]
[0051] Preferably, the formulation according to the invention comprises at least 80% by weight of the original clay matrix, more preferably at least 90% by weight of the original clay matrix. Indeed, the formulation of the construction binder according to the invention has the advantage that it can contain a large amount of the original clay matrix without altering the mechanical properties of the construction material, thus making it possible to produce a construction material with adequate mechanical performance.
[0052] Moreover, preferably, the formulation according to the invention comprises at most 98% by weight of the original clay matrix, more preferably at most 96% by weight of the original clay matrix. Indeed, the formulation for the construction binder according to the invention also comprises at least one deflocculating agent, thus limiting the proportion of the original clay matrix in the formulation.
[0053] Thus, in particular, the formulation according to the invention may comprise from 80 to 99.5% by weight of original clay matrix, preferably from 90 to 99% or from 80 to 98% by weight of original clay matrix, more preferably from 85 to 97% by weight of original clay matrix, even more preferably from 90 to 96% by weight of original clay matrix.
[0054] Deflocculating agent Many compounds can act as peptizers and many are commonly known to those skilled in the art.
[0055] In the context of the present invention, the deflocculating agent is in particular a non-ionic surfactant, such as a polyoxyethylene ether, which may be chosen, for example, from poly(oxyethylene) lauryl ether.
[0056] The peptizing agent may also be an anionic agent, such as an anionic surfactant. In particular, the anionic agent may be selected from alkylarylsulfonates, aminoalcohols, carbonates, silicates, fatty acids, humates (e.g., sodium humate), carboxylic acids, lignosulfonates (e.g., sodium lignosulfonate), polyacrylates, phosphates, or polyphosphates, such as sodium hexametaphosphate, sodium tripolyphosphate, sodium orthophosphate, carboxymethylcellulose, and mixtures thereof. The peptizer can also be a polyacrylate, which in turn can be selected, for example, from sodium polyacrylate and ammonium polyacrylate.
[0057] The peptizer can also be an amine selected from, for example, 2-amino-2-methyl-1-propanol; monoethanolamine, diethanolamine, or triethanolamine; isopropanolamine (1-amino-2-propanol, diisopropanolamine, and triisopropanolamine) and N-alkylated ethanolamines. The peptizer can also be a silicate, such as sodium silicate, sodium metasilicate, or sodium trisilicate.
[0058] Alternatively, the deflocculating agent can be a mixture of compounds, such as a mixture comprising at least two compounds selected from nonionic surfactants, anionic agents, polyacrylates, amines and organophosphorus compounds. In particular, the peptizer may be a mixture of sodium silicate and sodium carbonate. Preferably, the deflocculating agent is selected from lignosulfonates (eg, sodium lignosulfonate), polyacrylates, humates, and mixtures thereof.
[0059] The peptizer is preferably in the form of a salt. However, the present invention is not limited to the above deflocculating agents, and any type of deflocculating agent known to those skilled in the art may be used in place of the above deflocculating agents.
[0060] In particular, the deflocculating agent comprises at least 0.5% by weight of the original clay matrix, preferably at least 1% by weight of the original clay matrix, more preferably at least 2% by weight of the original clay matrix, even more preferably at least 3% by weight of the original clay matrix, for example at least 4% by weight of the original clay matrix. Indeed, with such a concentration of deflocculating agent, the binder formulation according to the present invention can then be used in combination with an activator composition to form a material having advantageous mechanical properties.
[0061] Furthermore, the deflocculating agent comprises at most 20% by weight of the original clay matrix, preferably at most 10% by weight of the original clay matrix. Indeed, too high a concentration is not necessary to form a material with advantageous mechanical properties.
[0062] In particular, the deflocculating agent comprises between 0.5 and 20% by weight of the original clay matrix, preferably between 1 and 10% by weight of the original clay matrix, more preferably between 3 and 10% by weight of the original clay matrix, and even more preferably between 4 and 10% by weight of the original clay matrix.
[0063] According to another aspect, the present invention further relates to a construction binder comprising the components of the construction binder formulation according to the invention and an activator composition.
[0064] It is the addition of an activator composition in combination with the original clay matrix and a deflocculating agent that gives the construction binder its desired mechanical properties.
[0065] The construction binder may advantageously be in the form of a two-component or multi-component system, i.e. it may contain its components in juxtaposition, in particular the original clay matrix, the deflocculating agent and the activator composition.
[0066] In particular, the construction binder can be prepared in such a way that the activator composition is not in contact with the original clay matrix and / or the deflocculating agent prior to the mixing step required for the actual use of the construction binder. Such a feature has the advantage that the stability of the construction binder can be improved prior to its use.
[0067] For example, a construction binder may correspond to a mixture corresponding to a binder formulation according to the invention in combination with an activator composition contained in another container. In a two-component or multi-component system, the components are not all in the same form (liquid, solid, paste, etc.), or the components are in paste form, or are contained in different containers.
[0068] Just before use, the construction binder can be mixed with water, or more generally with an aqueous solution that allows the components of the construction binder to be thoroughly mixed. Nevertheless, before the addition of this water, it may be in the form of a construction binder that is at least partially dehydrated.
[0069] As described below, the activator composition can be a liquid composition, so that the construction binder can be formed without the addition of water or additional aqueous solutions.
[0070] Advantageously, and as will be explained in detail, some of the components of the construction binder (the deflocculating agent and the clay matrix) can be mixed with water before adding the activator composition.
[0071] Nevertheless, construction binders can also be advantageously prepared in dehydrated form, in which case they can be mixed with an aqueous solution immediately prior to use, which allows for easier transport and packaging.
[0072] Without being limited by theory, it is believed that the activator composition allows the formation of a network between the clay sheets that gives the construction binder according to the invention its mechanical properties.
[0073] The activator composition is present, for example, in a content of at least 10% by weight of the construction binder, preferably at least 15% by weight of the construction binder, more preferably at least 20% by weight of the construction binder, even more preferably at least 25% by weight of the construction binder, and for example at least 30% by weight of the construction binder. Further, the activator composition may comprise up to 50% by weight of the construction binder, preferably up to 45% by weight of the construction binder, and more preferably up to 40% by weight of the construction binder. In particular, the activator composition may comprise between 10 and 50% by weight of the construction binder, preferably between 15 and 50% by weight of the construction binder. More preferably, the activator composition comprises between 10 and 35% by weight of the construction binder, even more preferably between 15 and 30% by weight of the construction binder.
[0074] In particular, the activator composition may include a metal oxide and / or may be an alkaline activator composition. Preferably, the metal oxide is a transition metal oxide. More preferably, the metal oxide is selected from iron oxides such as FeO, Fe3O4, Fe2O3, alumina Al2O3, manganese(II) oxide MnO, titanium(IV) oxide TiO2 and mixtures thereof.
[0075] The metal oxides may preferably be derived from the composition of blast furnace slag, for example formed during the production of pig iron from iron ore.
[0076] The metal oxide is present in a content of at least 2% by weight of the construction binder, preferably at least 5% by weight of the construction binder, more preferably at least 10% by weight of the construction binder.
[0077] When the activator composition is an alkaline activator composition, the alkaline composition may preferably comprise a compound having a pKa of 10 or more, more preferably 12 or more, and even more preferably substantially equal to 14. It may be considered a strong base.
[0078] In particular, the activator composition may comprise a mixture of sodium hydroxide and sodium silicate. The activator composition may be used in solid form. It may also be used in liquid form, for example in the case of alkaline activator compositions. In this case, the percentages indicated in the formulations correspond to the weight of the liquid composition.
[0079] As regards the liquid alkaline activator composition, it may contain between 10 and 70%, preferably between 20 and 60%, more preferably between 30 and 50% of a mixture of sodium hydroxide and sodium silicate, based on grams of dry product of the total weight of the composition.
[0080] Alkaline compositions, and more broadly activator compositions, may include organophosphorus compounds such as, for example, sodium tripolyphosphate, designated by the acronym NaTPP.
[0081] Advantageously, the activator composition can be an alkaline activator composition further comprising a metal oxide.As shown in the examples, the construction binder prepared from such an activator composition has good mechanical properties.Therefore, preferably, the activator composition can comprise a metal oxide and at least one compound with a pKa of 10 or more.
[0082] The activator composition may be an aqueous composition. It may therefore preferably contain water. As explained below, its use may be combined with the addition of water in the formation of the construction binder according to the invention. However, alternatively, the activator composition may be in solid form, for example in powder form.
[0083] Preferably, the original clay matrix comprises at least 30% by weight of the construction binder, preferably at least 40% by weight of the construction binder, more preferably between 40 and 80% by weight, even more preferably between 45 and 65% by weight, even more preferably between 50 and 60% by weight.
[0084] Likewise, the deflocculating agent may represent at least 0.25% by weight of the construction binder, preferably at least 0.5% by weight of the construction binder, more preferably at least 1% by weight of the construction binder, even more preferably at least 1.5% by weight of the construction binder, and for example at least 2% by weight of the construction binder.
[0085] Furthermore, the peptizer may comprise up to 20% by weight of the construction binder, preferably up to 15% by weight of the construction binder, more preferably up to 10% by weight of the construction binder.
[0086] In particular, the deflocculating agent may represent between 0.25 and 10% by weight of the construction binder, preferably between 0.5 and 10% by weight of the construction binder, more preferably between 1 and 10% by weight of the construction binder, between 1 and 8% by weight of the construction binder, between 2 and 8% by weight of the construction binder, between 2 and 5% by weight of the construction binder, even more preferably, the deflocculating agent may represent between 0.5 and 6% by weight of the construction binder, between 1 and 4% by weight of the construction binder.
[0087] In a particular embodiment, the construction binder according to the invention comprises: - 30-80% by weight of the original clay matrix, - 0.25 to 20% by weight of a deflocculating agent, and - 10 to 50% by weight of an activator composition, Includes.
[0088] Preferably, the construction binder according to the invention comprises: - 45-60% by weight of the original clay matrix, - 0.25% to 5% by weight, preferably 1% to 4%, of a deflocculating agent, and - 10 to 50% by weight of an activator composition, Includes.
[0089] Preferably, the construction binder according to the invention comprises: - 30-80% by weight of the original clay matrix, - 1 to 10% by weight of a deflocculating agent, and - 10 to 50% by weight of an activator composition, Includes.
[0090] Preferably, the construction binder according to the invention comprises: - 50-75% by weight of the original clay matrix, - 1 to 10% by weight of a deflocculating agent, and - 15 to 50% by weight of an activator composition, Includes.
[0091] More preferably, the construction binder according to the invention comprises: - 50-75% by weight of the original clay matrix, - 2 to 5% by weight of a deflocculating agent, and - 15 to 45% by weight of an activator composition, Includes.
[0092] More preferably, the construction binder according to the invention comprises: - 50-60% by weight of the original clay matrix, - 2 to 5% by weight of a deflocculating agent, and - 25 to 45% by weight of a metal oxide, Includes.
[0093] Even more preferably, the construction binder according to the invention comprises - 30-80% by weight of the original clay matrix, - 1 to 10% by weight of a deflocculating agent, - 10 to 40% by weight of a metal oxide, and - 2 to 15% by weight of a strong base, Includes.
[0094] In addition to the original clay matrix, the deflocculating agent and the activator composition, the construction binder may contain metakaolin, flushed or unflushed, cement, lime and / or plaster. Moreover, as shown in the examples, some construction binder compositions may have mechanical performances equal to or better than Portland cement. Thus, even more preferably, the construction binder according to the invention comprises: - 45-70% by weight of the original clay matrix, - 0.5 to 6% by weight of a deflocculating agent, - 10 to 35% by weight of an activator composition, and - 15 to 30% by weight of metakaolin, Includes.
[0095] Even more preferably, the construction binder according to the invention comprises - 35-65% by weight of the original clay matrix, - 0.5 to 5% by weight of a deflocculating agent, - 10-30% by weight of blast furnace slag, and - 15-35% by weight of Portland CEM1 cement, Includes.
[0096] Even more preferably, the construction binder according to the invention comprises - 40-70% by weight of the original clay matrix, - 0.5 to 6% by weight of a deflocculating agent, - 5 to 20% by weight of an activator composition, and - 20-45% by weight of blast furnace slag, Includes.
[0097] Even more preferably, the construction binder according to the invention comprises - 40-70% by weight of the original clay matrix, - 0.5 to 5% by weight of a deflocculating agent, - 10 to 25% by weight of an activator composition, - 5-20% by weight of blast furnace slag, and - 15 to 30% by weight of metakaolin, Includes.
[0098] As mentioned above, the formulation is an open formulation and the construction binder may further comprise complementary compounds such as plasticizers or water reducers.
[0099] Furthermore, the water to dry matter weight ratio of the composition referred to herein as construction binder is controlled and is preferably less than 1 and advantageously substantially equal to 0.6.
[0100] According to another aspect, the present invention relates to a method for preparing a construction binder. Such a method according to the present invention, as shown in Figure 1, has the advantage of being a so-called low-carbon method, i.e. the greenhouse gas emissions, in particular carbon dioxide emissions, of the low-carbon method are reduced compared to the greenhouse gas emissions of known methods for preparing construction binders. Such a reduction in greenhouse gas emissions is in particular due to the absence of an energy-intensive calcination step.
[0101] In particular, the method comprises a step 110 of preparing a clay suspension comprising at least one raw clay matrix, a deflocculating agent and water. As before, the raw clay matrix may comprise at least one mineral species selected from kaolinite, illite, smectite, bentonite, chlorite, montmorillonite, muscovite, halloysite, sepiolite, attapulgite, vermiculite and the so-called layered clays, which are complex combinations of several clays. Advantageously, the preparation step 110 starts with a dehydrated premix comprising the raw clay matrix and the deflocculating agent.
[0102] In the preparation of the suspension step 110, water can be added such that the ratio of the mass of water to the mass of the construction binder is less than 1, for example between 0.4 and 0.8. Furthermore, water can be advantageously added after dry mixing of the raw clay matrix and the deflocculating agent.
[0103] Advantageously, the raw clay matrix used during the clay suspension preparation step 110 may be obtained from excavated soil near the construction site. Thus, the method for preparing a construction binder may comprise a step of excavating soil comprising the raw clay matrix prior to the clay suspension preparation step 110. Furthermore, in this case, the method may comprise a step of preparing the excavated soil, said preparation may comprise, for example, drying, grinding, sieving, storing.
[0104] Thus, the preparation of the construction binder according to the invention may allow the preparation of in-situ concrete made at least in part from raw materials from the construction site, such properties further reducing the environmental footprint of the produced concrete.
[0105] Preferably, following preparation of the clay suspension, the method according to the invention may include a step 120 of mixing the clay suspension to obtain a dispersed or deflocculated clay suspension.
[0106] This step 120 of mixing the clay suspension can be advantageously, but not exclusively, carried out in equipment selected from a mixer and a truck mixer, or more generally in any equipment adapted to mix clay suspensions for the manufacture of construction binders. Ultrasonic dispersion equipment can also be used.
[0107] This step 120 of mixing the clay suspension prior to adding the activator composition may be carried out for a period of at least 10 seconds, preferably at least 30 seconds, and more preferably at least 60 seconds.
[0108] Furthermore, this step 120 of mixing the clay suspension prior to adding the activator composition may be carried out for a period of up to 24 hours, preferably up to 12 hours, and more preferably up to 6 hours.
[0109] The method also includes adding an activator composition to the clay suspension at step 130. As detailed above, the activator composition may include a metal oxide and / or may be an alkaline activator composition.
[0110] The method includes a homogenization or mixing step 140 to obtain a construction binder.
[0111] Before, simultaneously with, or after the addition of the activator composition, the method according to the invention may include the addition of additives or materials for modifying the mechanical properties of the final construction material.
[0112] The added material may be, for example, recycled or non-recycled aggregates selected from fillers, powders, sand, grit, gravel, and / or fibers, and optionally pigments.
[0113] The method may also include the addition of a plasticizer, which may be, for example, a polyacrylate, a polynaphthalenesulfonate, a polycarboxylate, or a polyphosphonate.
[0114] The method may also include the addition of fibers, for example selected from vegetable fibers such as cotton, flax, hemp, cellulose, bamboo, miscanthus fibers, synthetic fibers such as metal, glass, carbon, polypropylene fibers, and mixtures thereof. The presence of fibers may allow the formation of a construction material with improved mechanical and thermal insulation properties.
[0115] The method may also include the addition of aggregate, for example selected from gravel, crushed concrete, recycled concrete, and mixtures thereof.
[0116] The method may also include the addition of additives, for example selected from synthetic or natural rheology retention agents, shrinkage prevention agents, water retention agents, air entrainment agents, synthetic resins, and mixtures thereof.
[0117] In particular, the preparation of a construction binder according to the invention will include the addition of sand and water. The sand may possibly be obtained from excavated material, especially in the case of "in situ" concrete. The sand may be desert sand.
[0118] The resulting construction material may be selected, for example, from a mortar, a coating, or a plaster.
[0119] Therefore, according to another aspect, the present invention relates to a construction material formed from the construction binder according to the present invention.
[0120] Furthermore, the present invention relates to a construction binder obtainable from the process according to the invention.The present invention relates to a construction material obtainable from the process according to the invention.
[0121] The invention in particular enables the production of: - Thermal insulating construction materials: from construction binders according to the invention with the addition of lightweight aggregates of the "vegetable or porous" type; - lightweight concrete: from construction binders according to the invention with the addition of a foaming agent of the aluminum powder type, which allows air to be trapped in the material, improving its insulating properties; - prefabricated elements: production of concrete blocks or slabs in factories from construction binders according to the invention; and - Thermal insulation module.
[0122] The invention therefore also relates to the use of the structural binder according to the invention for the manufacture of covering elements, for the manufacture of extruded or moulded structural modules or more generally for the manufacture of various extruded shapes.
[0123] The covering elements can be chosen, for example, from floor coverings such as tiles, flagstones, paving stones or borders, wall coverings such as interior or exterior facade elements, cladding panels, planking elements or roof coverings of the tile type. As regards extruded or moulded construction blocks, they are, for example, bricks.
[0124] The present invention also relates to the use of the construction binder according to the invention for the production of composite materials, prefabricated blocks.
[0125] The composite material is, for example, a construction panel of the prefabricated panel type, and the prefabricated block is, for example, a door or window lintel, a prefabricated wall element or any other prefabricated construction element.
[0126] The present invention also relates to the use of the structural binder according to the invention for the manufacture of insulating modules, such as partition panels or lightweight insulating structural modules, which have for example a density of less than 1.5 kg / L, preferably less than 1.2 kg / L, more preferably less than 1.0 kg / L, even more preferably less than 0.7 kg / L.
[0127] The present invention also relates to the use of the construction binder according to the invention for carrying out additive manufacturing. In particular, the carrying out of additive manufacturing can be carried out using automated 3D construction systems such as 3D printers. Such additive manufacturing can be used to manufacture construction elements, buildings or houses, or decorative items.
[0128] More generally, the present invention also relates to the use of a deflocculating agent in combination with a raw clay matrix and an activator composition for the preparation of a construction binder, in which the raw clay matrix represents at least 30% by weight of the construction binder and the activator composition is a composition for obtaining concrete having a minimum compressive strength at 28 days, measured according to the ISO 1920-4:2005 standard (Testing of concrete - Part 4: Strength of hardened concrete), of at least 20 MPa, preferably at least 25 MPa, preferably at least 40 MPa.
[0129] The present invention also relates to the use of a deflocculating agent in combination with a raw clay matrix and an activator composition for the preparation of a construction binder, in which the raw clay matrix represents at least 30% by weight of the construction binder and the activator composition is a composition for obtaining concrete having a minimum compressive strength at 28 days, measured according to the NF EN 197-1 standard, of at least 20 MPa, preferably at least 25 MPa, more preferably at least 40 MPa.
[0130] As shown in the examples below, the present invention provides a solution based on a mixture of raw clay matrix, deflocculating agent, and activator compositions to provide a construction binder with similar mechanical properties to standard ones while reducing the carbon footprint. EXAMPLES
[0131] Preparation of the construction binder: In all the examples given below, the formulations according to the invention are prepared according to the same protocol, i.e. a dry premix is made between the raw clay matrix and the deflocculating agent in the given amounts, then water is added and the solution is mixed at low speed, i.e. at approximately 600 revolutions per minute for 30 seconds, then the activator composition is added to the premix and then the premix is mixed at high speed, i.e. at approximately 1500 revolutions per minute for 3 minutes.
[0132] The weight ratio of water to dry matter of the composition (also called construction binder) is adjusted to a value substantially equal to 0.6.
[0133] The resulting construction binder is then poured into molds and left to harden for 28 days at room temperature, i.e., about 20 degrees Celsius.
[0134] Methodology for measuring mechanical properties of construction binders: Once maturation is complete, the mechanical strength is measured. By mechanical strength of the construction binder is meant the compressive strength measured according to the NF EN 196-1 standard on a prism with a side of 40 millimeters and a length of 160 millimeters, expressed in megapascals (MPa).
[0135] Comparison of the construction binder according to the invention with known construction binders: Table 2 below shows known formulations and formulations according to the invention for different types of construction binders. The masses of the components associated with each formulation are expressed as a percentage of the total mass (dry weight) of the construction binder.
[0136] [Table 2]
[0137] Thus, Table 2 shows the mechanical strength of known construction binders (CEM1, HP2A1, CMT binders) that are not part of the present invention, such as the CEM1 type construction binder, better known under the name "Portland" cement, the compressive strength of which is of the order of 45 MPa.
[0138] The HP2A1 formulation is available according to the teachings of patent application FR3034094. The construction binder type HP2A1 contains 35% by weight of metakaolin obtained by calcining kaolin, 65% by weight of an activator composition. The relative strength of such a construction binder is therefore of the order of 42 MPa, which is lower than that of Portland type construction binders.
[0139] Finally, the CMT construction binder obtained by following the teachings of patent application FR3016376 comprises 75% by weight of original clay matrix, 10% by weight of an activator composition, in particular containing lime, and 15% by weight of Portland type cement. The mechanical strength associated with such a binder, which comprises a large proportion of original clay matrix, is according to patent application FR3016376 of the order of 25 MPa, and therefore has a substantially lower compressive strength than Portland or HP2A1 type construction binders. Nevertheless, the reproduction of these tests by the applicant has not been able to obtain strengths of more than 10 MPa. Thus, in the presence of a high concentration of original clay matrix and in the absence of a deflocculating agent, the construction binder will not produce a concrete with adequate mechanical properties.
[0140] Table 2 also shows the MUP1 formulation according to the invention. It is important to note that this formulation, containing 3% deflocculator, has a mechanical strength similar to that of Portland cement, even though it contains a large proportion (55%) of the original clay matrix.
[0141] The importance of deflocculating agents Table 3 below shows a known formulation HP2A_X02 and three formulations according to the invention MUP2, MUP S9-1 and MUP S10-1.
[0142] [Table 3]
[0143] A construction binder of the HP2A2 type comprises 54% by weight of a raw clay matrix, 23% by weight of an activator composition (alkali silicate solution and / or NaTPP), 18% by weight of metakaolin and 5% of BFS. In particular, such a formulation can be derived from the teachings of patent application FR3034094. The mechanical strength associated with such a binder is of the order of 27 MPa.
[0144] In contrast, the MUP2 binder obtained according to the invention and having a similar composition except for the presence of 3% deflocculating agent has a mechanical strength of 43 MPa, such a strength can be considered as equivalent to Portland cement.
[0145] Similarly, the MUPS9-1 binder obtained according to the invention and having a similar composition except for the presence of 1.5% deflocculating agent has a mechanical strength of 46 MPa, such a strength can be considered equivalent to Portland cement.
[0146] These results confirm the relevance of the construction binder according to the invention and highlight the advantage conferred on the compressive strength by the presence of metal oxides, for example from blast furnace slags.
[0147] Table 4A below shows MUP1, a formulation according to the invention already presented, and an equivalent formulation without added deflocculator.
[0148] [Table 4]
[0149] This comparison shows that the mechanical strength of the mix according to the invention can reach 45 MPa, while the mechanical strength of the same mix without deflocculating agent (CMT2), according to patent application FR3016376, is only 25 MPa. Moreover, as mentioned above, the Applicant's replication of these tests did not allow to obtain strengths of more than 10 MPa in the CMT2 test. Thus, in the presence of a high concentration of the original clay matrix and in the absence of a deflocculating agent, the construction binder does not produce concrete with adequate mechanical properties. As mentioned above, the presence of a deflocculating agent in combination with the original clay matrix and the activator composition makes it possible to improve the mechanical strength of the construction binder.
[0150] Table 4B below shows formulations according to the present invention, MUPS8-1 and MUPS12-1, compared to a reference formulation with no added deflocculator.
[0151] [Table 5]
[0152] This comparison shows that the mechanical strength of the formulations according to the invention can reach 40 MPa or more, whereas the mechanical strength of the same formulations without deflocculating agent (MUPS8-2 or MUPS11-3) does not reach 30 MPA. As explained in the previous paragraph, the presence of a deflocculating agent in combination with the original clay matrix, the activator composition and optionally metakaolin allows the mechanical strength of the construction binders herein to be improved by about 30% or more.
[0153] Table 4C below details the formulations of some construction binders according to the invention compared to reference binders (MUPS2-1 and MUPS2-2), which differ in particular in that the construction binders according to the invention contain a deflocculating agent.
[0154] [Table 6]
[0155] Table 4C shows formulations where the cement acts as the activator composition. The equivalent formulations where the deflocculator is removed have poor mechanical strength.
[0156] Conversely, by combining raw clay with a content of 50% or more with cement and deflocculating agents, strengths of over 20 MPa can be achieved. The resulting mechanical properties are more than tripled.
[0157] Use of a combination of metal oxide and alkaline activator composition: Table 5 below details the formulations of some construction binders according to the invention, in particular, these construction binders differ in that some contain an alkaline activator composition (in this case a solution containing NaTPP) and others contain Portland cement.
[0158] [Table 7]
[0159] Table 5 shows - Blast furnace slag (BFS) containing metal oxides; sodium tripolyphosphate, The mechanical strength of the compound containing the mixture is shown to be 45 MPa.
[0160] An equivalent formulation in which the alkaline activator composition is replaced by CEM1 cement has similar mechanical strength.
[0161] Furthermore, the MUPS5-1 composition without BFS has acceptable but lower compressive strength values. This composition shows that thanks to the present invention it is possible to reach mechanical strength values of more than 20 MPa for these construction binders containing more than 50% original clay matrix.
[0162] Concrete mixes from the construction binder according to the invention: Table 6 below details several concrete formulations, including a reference concrete made from Portland cement (B Portland) and concretes made from construction binders according to the invention (MUP_BA1, MUP_BA2, MUP_BA3), which differ in particular by the nature of the original clay matrix, the nature of the deflocculating agent and the activating composition used.
[0163] [Table 8]
[0164] As shown in Table 6, the concrete of the invention has a compressive strength comparable to that obtained with concrete formed with Portland cement. The invention therefore makes it possible to form, from a raw clay matrix, a low-carbon construction binder with sufficient mechanical properties to make it a construction material that will meet the majority of the sector's needs.
Claims
1. A construction binder comprising a raw clay matrix, a deflocculating agent and an activator composition, characterized in that said construction binder comprises at least 30% by weight of the raw clay matrix.
2. 2. Construction binder according to claim 1, characterized in that it contains less than 30% by weight of metakaolin.
3. 3. A construction binder according to claim 1 or 2, characterized in that it contains at least 40% by weight of a raw clay matrix.
4. The deflocculating agent is - non-ionic surfactants, such as polyoxyethylene ethers; anionic agents such as anionic agents selected from alkylarylsulfonates, amino alcohols, carbonates, silicates, fatty acids, humates (e.g. sodium humate), carboxylic acids, lignosulfonates (e.g. sodium lignosulfonate), polyacrylates, phosphates or polyphosphates such as sodium hexametaphosphate silicate, sodium tripolyphosphate, sodium orthophosphate, carboxymethylcellulose and mixtures thereof; a polyacrylate, such as a polyacrylate chosen from sodium polyacrylate or ammonium polyacrylate; amines such as amines selected from 2-amino-2-methyl-1-propanol; monoethanolamine, diethanolamine, or triethanolamine; isopropanolamine (1-amino-2-propanol, diisopropanolamine and triisopropanolamine) and N-alkylated ethanolamines; or - Mixtures thereof 4. The construction binder according to claim 1, wherein the binder is selected from the group consisting of:
5. A construction binder according to any one of claims 1 to 4, characterized in that said deflocculating agent represents at least 0.25% by weight of said construction binder.
6. A construction binder according to any one of claims 1 to 5, characterized in that the activator composition represents at least 10% by weight of the construction binder.
7. A construction binder according to any one of claims 1 to 6, characterized in that the original clay matrix, the deflocculating agent and the activator composition form a two-component or multi-component system.
8. The construction binder comprises: - 30 to 80% by weight of a raw clay matrix, - 0.25 to 20% by weight of a deflocculating agent, and - 10 to 50% by weight of an activator composition, 8. A construction binder according to claim 1, comprising:
9. The construction binder according to any of claims 1 to 8, characterized in that the activator composition is an alkaline activator composition.
10. 10. Construction binder according to any of the preceding claims, characterized in that the activator composition comprises an organophosphorus compound such as sodium tripolyphosphate, preferably comprising at least 2% by weight of the construction binder.
11. A construction binder according to any one of the preceding claims, characterized in that it contains at least 2% by weight of metal oxide.
12. The metal oxide is FeO, Fe 3 O 4 , Fe 2 O 3 Iron oxides such as iron oxide, alumina Al 2 O 3 , manganese oxide (II) MnO, titanium oxide (IV) TiO 2 12. Construction binder according to claim 11, characterized in that it is selected from the group consisting of:
13. A construction binder according to any of the preceding claims, characterized in that it comprises a blast furnace slag composition, preferably which represents at least 5% by weight of the construction binder.
14. A construction binder according to any of the preceding claims, characterized in that the activator composition comprises Portland cement.
15. Construction binder according to any of the preceding claims, characterized in that the activator composition comprises metakaolin.
16. - 40 to 70% by weight of a raw clay matrix, - 0.5 to 6% by weight of a deflocculating agent, - 5 to 20% by weight of an activator composition, and - 20 to 45% by weight of blast furnace slag, A construction binder according to any one of claims 1 to 13, characterized in that it comprises
17. - 35 to 65% by weight of a raw clay matrix, - 0.5 to 5% by weight of a deflocculating agent, 31-49% by weight of Portland CEM1 cement A construction binder according to any one of claims 1 to 14, characterized in that it comprises
18. - 35 to 65% by weight of a raw clay matrix, - 0.5 to 5% by weight of a deflocculating agent, - 10 to 30% by weight of blast furnace slag, and 15-35% by weight of Portland CEM1 cement A construction binder according to any one of claims 1 to 14, characterized in that it comprises
19. - 45 to 70% by weight of a raw clay matrix, - 0.5 to 6% by weight of a deflocculating agent, - 10 to 35% by weight of an activator composition, and 15-30% by weight of metakaolin 16. A construction binder according to claim 1, comprising:
20. - 45 to 70% by weight of a raw clay matrix, - 0.5 to 5% by weight of a deflocculating agent, - 10 to 25% by weight of the activator composition, - 5 to 20% by weight of blast furnace slag, and 15-30% by weight of metakaolin 16. A construction binder according to claim 1, comprising:
21. A method (100) for preparing a construction binder, comprising: - preparing a clay suspension (110) comprising at least one raw clay matrix, one deflocculating agent and water; - adding (130) an activator composition to the clay suspension, which may be an alkaline activator composition and / or may include a metal oxide; - mixing (140) to obtain said construction binder, said construction binder comprising at least 30% by weight of a raw clay matrix; 13. A method for preparing a construction binder comprising:
22. 22. A method for preparing a construction binder according to claim 21, comprising a step (120) of mixing said clay suspension to obtain a peptized clay suspension, characterized in that after said mixing step (120) the activator composition is added.
23. A preparation method according to claim 21 or 22, characterized in that the construction binder comprises at least 50% by weight, preferably 50-80% by weight, of a raw clay matrix.
24. A preparation method according to any of claims 21 to 23, characterized in that said deflocculating agent represents at least 0.25% by weight of the construction binder, preferably at least 0.5% by weight of the construction binder, more preferably between 0.5 and 10% by weight of the construction binder.
25. A preparation method according to any of claims 21 to 24, characterized in that the activator composition is present in a content of at least 10% by weight of the binder.
26. Construction materials such as mortars, coatings, plasters, insulation materials, lightweight concrete, prefabricated elements, etc., comprising a construction binder according to any one of claims 1 to 20.
27. 27. The construction material of claim 26, characterized in that the construction binder comprises excavated soil containing the original clay matrix.
28. 28. A construction material according to claim 26 or 27, characterized in that it further comprises one or more fillers, said fillers being for example selected from mineral or vegetable fillers.
29. A construction material according to any one of claims 26 to 28, characterized in that it further comprises a foaming or expanding agent, such as aluminium powder.
30. Use of a construction binder according to any of claims 1 to 20 for the production of covering elements, in particular floor coverings such as tiles, stone slabs, paving stones or edgings, interior or exterior facade elements, wall coverings such as cladding panels, planking elements or roof coverings of the tile type, for the production of extruded or moulded construction modules such as bricks or for the production of various extruded shapes.
31. Use of a construction binder according to any of claims 1 to 20 for the manufacture of composite materials such as construction panels of the prefabricated panel type, prefabricated blocks such as door or window lintels, prefabricated wall elements or any other prefabricated construction elements.
32. 21. Use of a construction binder according to any of claims 1 to 20 for the production of insulating modules, such as partition panels or lightweight insulating construction modules, having a density of less than 1.5 kg / L, preferably less than 1.2 kg / L, more preferably less than 1.0 kg / L, more preferably less than 0.7 kg / L.
33. 21. Use of a construction binder according to any of claims 1 to 20 for the production of construction elements, buildings or houses, or decorative articles by additive manufacturing, such as by means of a 3D printer.
34. 21. Use of a construction binder according to any of claims 1 to 20 for the production of a sealant, adhesive or grout in the form of a two-component system having either a composition in solid form on the one hand and a composition in liquid form on the other hand, or two compositions in the form of pastes.
35. 1. Use of a deflocculating agent in combination with a raw clay matrix and an activator composition for the preparation of a construction binder, said raw clay matrix comprising at least 30% by weight of said construction binder, and said activator composition being a composition for obtaining a concrete having a minimum cylinder compressive strength at 28 days, measured according to NF EN 206-1 standard, of at least 20 MPa, preferably at least 25 MPa, more preferably at least 40 MPa.
Citation Information
Patent Citations
Plasticizing material, method for producing the same and grouting material using the plasticizing material
JP2002212559A
Cement composition
JP2003055024A
Composition for metakaolin construction material, related method for manufacturing said composition, and use for producing construction elements