Adhesive film for metal terminal and manufacturing method thereof, metal terminal with adhesive film for metal terminal, exterior material for power storage device, kit including exterior material for power storage device and adhesive film for metal terminal, and power storage device and manufacturing method thereof
The adhesive film with a polypropylene layer and a 20% or less island ratio in the sea-island structure addresses moisture infiltration issues in power storage devices, enhancing adhesion and sealing performance.
Patent Information
- Application Number
- JP2024118944
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-25
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-23
AI Technical Summary
The increasing thickness of adhesive films between metal terminals and exterior materials in power storage devices leads to higher moisture infiltration, causing deterioration of the power storage device elements.
An adhesive film for metal terminals with a polypropylene layer featuring a sea-island structure and an island ratio of 20% or less is used to suppress water vapor permeation, enhancing adhesion between the metal terminal and the exterior material.
The adhesive film effectively reduces water vapor permeation into the power storage device, improving the sealing performance and preventing element deterioration.
Smart Images

Figure 2024150668000003 
Figure 2024150668000004 
Figure 2024150668000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an adhesive film for metal terminals and a method for producing the same, a metal terminal with an adhesive film for metal terminals, an exterior material for an electricity storage device, a kit including an exterior material for an electricity storage device and an adhesive film for metal terminals, and an electricity storage device and a method for producing the same. [Background technology]
[0002] Conventionally, various types of electricity storage devices have been developed, and in all electricity storage devices, exterior materials for electricity storage devices are essential components for sealing electricity storage device elements such as electrodes and electrolytes. Conventionally, metal exterior materials for electricity storage devices have been widely used as exterior materials for electricity storage devices, but in recent years, with the increasing performance of electric vehicles, hybrid electric vehicles, personal computers, cameras, mobile phones, etc., electricity storage devices are required to have a variety of shapes and are required to be thin and lightweight. However, conventionally widely used metal exterior materials for electricity storage devices have the disadvantages that it is difficult to keep up with the diversification of shapes and there is also a limit to the weight reduction.
[0003] In view of this, in recent years, a laminate sheet in which a base layer / adhesive layer / barrier layer / thermal adhesive resin layer are laminated in this order has been proposed as an exterior material for an electricity storage device that can be easily processed into various shapes and can realize a thinner and lighter weight. When such an exterior material for an electricity storage device in the form of a laminate film is used, the periphery of the exterior material for an electricity storage device is heat-sealed and thermally fused with heat sealing in a state in which the thermal adhesive resin layers positioned in the innermost layers of the exterior material for an electricity storage device face each other, thereby sealing the electricity storage device element with the exterior material for an electricity storage device.
[0004] A metal terminal protrudes from the heat-sealed portion of the exterior material for an electricity storage device, and the electricity storage device element sealed with the exterior material for an electricity storage device is electrically connected to the outside by the metal terminal electrically connected to the electrode of the electricity storage device element. That is, among the heat-sealed portions of the exterior material for an electricity storage device, the portion where the metal terminal is present is heat-sealed in a state where the metal terminal is sandwiched between the heat-sealable resin layer. Since the metal terminal and the heat-sealable resin layer are made of different materials, adhesion is likely to decrease at the interface between the metal terminal and the heat-sealable resin layer.
[0005] For this reason, an adhesive film is sometimes disposed between the metal terminal and the heat-sealable resin layer for the purpose of increasing the adhesion between them, etc. Examples of such adhesive films include those described in Patent Document 1. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-79638 A Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, with the increase in capacity of electricity storage devices, the thickness of the adhesive film disposed between the metal terminal and the exterior material for the electricity storage device tends to increase. As the thickness of the adhesive film increases, the amount of moisture (water vapor) penetrating into the electricity storage device through the adhesive film also tends to increase. When a large amount of moisture penetrates into the electricity storage device, various problems such as deterioration of the electricity storage device elements occur.
[0008] The main object of the present disclosure is to provide an adhesive film for a metal terminal, which is interposed between a metal terminal electrically connected to an electrode of an electricity storage device element and an exterior material for an electricity storage device that seals the electricity storage device element, and which, when the adhesive film for a metal terminal is disposed between the metal terminal and the exterior material for an electricity storage device, suppresses water vapor permeation through the adhesive film for a metal terminal into the interior of the electricity storage device.Furthermore, the present disclosure also aims to provide a method for producing the adhesive film for a metal terminal, a metal terminal with an adhesive film for a metal terminal, an exterior material for an electricity storage device, a kit including the exterior material for an electricity storage device and the adhesive film for a metal terminal, an electricity storage device, and a method for producing the electricity storage device. [Means for solving the problem]
[0009] The inventors of the present disclosure conducted intensive studies to solve the above problems. As a result, they found that an adhesive film for metal terminal, which is interposed between a metal terminal electrically connected to an electrode of an electricity storage device element and an exterior material for an electricity storage device that seals the electricity storage device element, includes at least a polypropylene layer, in which a sea-island structure is observed in a cross-sectional image obtained by a scanning electron microscope for a cross section of the polypropylene layer in a direction parallel to the TD and in the thickness direction, and in which the island ratio of the sea-island structure of the polypropylene layer is 20% or less, when the adhesive film for metal terminal is disposed between the metal terminal and the exterior material for an electricity storage device, water vapor permeation through the adhesive film for metal terminal into the inside of the electricity storage device is suppressed. The present disclosure has been completed through further studies based on such findings.
[0010] That is, the present disclosure provides the inventions of the following aspects. An adhesive film for a metal terminal, which is interposed between a metal terminal electrically connected to an electrode of an electricity storage device element and an exterior material for an electricity storage device that encapsulates the electricity storage device element, The adhesive film for metal terminals includes at least a polypropylene layer, A sea-island structure is observed in a cross-sectional image of the polypropylene layer taken in a direction parallel to the TD and in a thickness direction thereof using a scanning electron microscope; An adhesive film for metal terminal, wherein the island ratio of the sea-island structure of the polypropylene layer is 20% or less. Effect of the Invention
[0011] According to the present disclosure, it is possible to provide an adhesive film for a metal terminal, which is interposed between a metal terminal electrically connected to an electrode of an electricity storage device element and an exterior material for an electricity storage device that seals the electricity storage device element, and when the adhesive film for a metal terminal is disposed between the metal terminal and the exterior material for an electricity storage device, water vapor permeation through the adhesive film for a metal terminal into the inside of the electricity storage device is suppressed.Furthermore, the present disclosure also aims to provide a method for manufacturing the adhesive film for a metal terminal, a metal terminal with an adhesive film for a metal terminal, an exterior material for an electricity storage device, a kit including an exterior material for an electricity storage device and an adhesive film for a metal terminal, and an electricity storage device and a method for manufacturing the same. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic plan view of the electricity storage device of the present disclosure. [Diagram 2] 2 is a schematic cross-sectional view taken along line AA' in FIG. 1. [Diagram 3] 2 is a schematic cross-sectional view taken along line BB' in FIG. 1. [Figure 4] 1 is a schematic cross-sectional view of an adhesive film for metal terminals according to the present disclosure. [Diagram 5] 1 is a schematic cross-sectional view of an adhesive film for metal terminals according to the present disclosure. [Figure 6] 1 is a schematic cross-sectional view of an adhesive film for metal terminals according to the present disclosure. [Figure 7] 1 is a schematic cross-sectional view of an adhesive film for metal terminals according to the present disclosure. [Figure 8] 1 is a schematic cross-sectional view of an exterior material for an electricity storage device according to the present disclosure. [Figure 9]FIG. 2 is a schematic diagram for explaining a method for measuring the water vapor permeability of an adhesive film for a metal terminal according to the present disclosure. [Figure 10] FIG. 2 is a schematic diagram for explaining a method for measuring the adhesive strength between an adhesive film and an exterior material. [Figure 11] FIG. 2 is a schematic diagram for explaining a method for measuring the adhesive strength between an adhesive film and an exterior material. [Figure 12] FIG. 2 is a schematic diagram for explaining a method for measuring the adhesive strength between an adhesive film and an exterior material. [Figure 13] FIG. 2 is a schematic diagram for explaining a method for measuring the adhesive strength between an adhesive film and an exterior material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The adhesive film for metal terminal of the present disclosure is an adhesive film for metal terminal that is interposed between a metal terminal electrically connected to an electrode of an electricity storage device element and an exterior material for an electricity storage device that seals the electricity storage device element, and is characterized in that the adhesive film for metal terminal includes at least a polypropylene layer, and a sea-island structure is observed in a cross-sectional image obtained using a scanning electron microscope for a cross-section of the polypropylene layer in a direction parallel to the TD and in the thickness direction, and the island ratio of the sea-island structure of the polypropylene layer is 20% or less.
[0014] Because the adhesive film for metal terminals of the present disclosure has these characteristics, when the adhesive film for metal terminals is disposed between a metal terminal and an exterior material for an electricity storage device, water vapor transmission through the adhesive film for metal terminals into the interior of the electricity storage device is suppressed.
[0015] The electricity storage device of the present disclosure is also an electricity storage device comprising at least an electricity storage device element having a positive electrode, a negative electrode, and an electrolyte, an exterior material for an electricity storage device that seals the electricity storage device element, and metal terminals electrically connected to each of the positive electrode and the negative electrode and protruding outside the exterior material for an electricity storage device, and is characterized in that an adhesive film for metal terminals of the present disclosure is interposed between the metal terminals and the exterior material for an electricity storage device.
[0016] The adhesive film for metal terminal and its manufacturing method, and the electricity storage device and its manufacturing method according to the present disclosure will be described in detail below.
[0017] In this specification, the numerical range indicated by "~" means "more than or equal to" or "less than or equal to". For example, the expression "2-15 mm" means 2 mm or more and 15 mm or less. In the numerical ranges described in the present disclosure in stages, the upper limit or lower limit described in a certain numerical range may be replaced with the upper limit or lower limit of another numerical range described in stages. In addition, the upper limit and the upper limit, the upper limit and the lower limit, or the lower limit and the lower limit described separately may be combined to form a numerical range. In addition, in the numerical ranges described in the present disclosure, the upper limit or the lower limit described in a certain numerical range may be replaced with a value shown in the examples.
[0018] In addition, as a method for confirming the MD of the adhesive film for metal terminals, there is a method of observing the cross section of the adhesive film for metal terminals with an electron microscope to confirm the sea-island structure. In this method, the direction parallel to the cross section in which the average diameter of the island shape in the direction perpendicular to the thickness direction of the adhesive film for metal terminals was the largest can be determined as the MD. Specifically, the cross sections in the length direction of the adhesive film for metal terminals and each cross section (10 cross sections in total) in which the angle is changed by 10 degrees from the direction parallel to the cross section in the length direction to the direction perpendicular to the cross section in the length direction are observed with an electron microscope to confirm the sea-island structure. Next, the shape of each individual island is observed in each cross section. For each island shape, the straight line distance connecting the leftmost end in the direction perpendicular to the thickness direction of the adhesive film for metal terminals and the rightmost end in the perpendicular direction is defined as the diameter y. In each cross section, the average of the diameters y of the top 20 island shapes in descending order of the diameter y is calculated. The direction parallel to the cross section in which the average diameter y of the island shape was the largest is determined as the MD. Also, for example, the adhesive film for metal terminal can be left in a 150° C. environment for 2 minutes and then the thermal shrinkage rate is measured, and the larger shrinkage rate can be determined as MD.
[0019] 1. Adhesive film for metal terminals The adhesive film for metal terminal of the present disclosure is interposed between a metal terminal electrically connected to an electrode of an electricity storage device element and an exterior material for an electricity storage device that seals the electricity storage device element. Specifically, as shown in, for example, Fig. 1 to Fig. 3, the adhesive film for metal terminal 1 of the present disclosure is interposed between a metal terminal 2 electrically connected to an electrode of an electricity storage device element 4 and an exterior material for an electricity storage device 3 that seals the electricity storage device element 4. The metal terminal 2 protrudes outside the exterior material for an electricity storage device 3, and is sandwiched by the exterior material for an electricity storage device 3 via the adhesive film for metal terminal 1 at a peripheral portion 3a of the heat-sealed exterior material for an electricity storage device 3.
[0020] In the present disclosure, the temporary adhesion step of the adhesive film for metal terminal to the metal terminal is performed, for example, under conditions of a temperature of about 140 to 160°C, a pressure of about 0.01 to 1.0 MPa, a time of about 3 to 15 seconds, and a number of times of about 3 to 6, while the main adhesion step is performed, for example, under conditions of a temperature of about 160 to 240°C, a pressure of about 0.01 to 1.0 MPa, a time of about 3 to 15 seconds, and a number of times of about 1 to 3. In addition, when the metal terminal with the adhesive film for metal terminal is interposed between the exterior material for the electricity storage device and heat-sealed, the heating temperature is usually in the range of about 180 to 210°C, the pressure is usually about 1.0 to 5.0 MPa, the time of about 1 to 5 seconds, and the number of times is about 1.
[0021] The adhesive film 1 for metal terminals (hereinafter, sometimes simply referred to as "adhesive film") of the present disclosure is provided to enhance the adhesion between the metal terminal 2 and the exterior material 3 for an electricity storage device. By enhancing the adhesion between the metal terminal 2 and the exterior material 3 for an electricity storage device, the sealing property of the electricity storage device element 4 is improved. As described above, when the electricity storage device element 4 is heat-sealed, the electricity storage device element is sealed such that the metal terminal 2 electrically connected to the electrode of the electricity storage device element 4 protrudes to the outside of the exterior material 3 for an electricity storage device. At this time, the metal terminal 2 formed of metal and the heat-sealable resin layer 35 (a layer formed of a heat-sealable resin such as polyolefin) located in the innermost layer of the exterior material 3 for an electricity storage device are formed of different materials, so that if such an adhesive film is not used, the sealing property of the electricity storage device element is likely to be reduced at the interface between the metal terminal 2 and the heat-sealable resin layer 35.
[0022] [Polypropylene layer 11] The adhesive film 1 for metal terminals of the present disclosure includes a polypropylene layer having an island ratio of 20% or less in a sea-island structure described below. In the present disclosure, the polypropylene layer having an island ratio of 20% or less in a sea-island structure described below is referred to as a "polypropylene layer 11." As described below, when the adhesive film 1 for metal terminals of the present disclosure is a multilayer film, the adhesive film 1 for metal terminals of the present disclosure may further include a polypropylene layer having an island ratio of more than 20% in a sea-island structure, in addition to the polypropylene layer 11. For example, the first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, the substrate, and the like described below may be polypropylene layers having an island ratio of more than 20% in a sea-island structure.
[0023] In the polypropylene layer 11, the island portions of the sea-island structure are regions in which ethylene is the main component (e.g., ethylene content is 80 mass% or more, 90 mass% or more, 95 mass% or more, 99 mass% or more), and the sea portions of the sea-island structure are regions in which polypropylene is the main component (e.g., propylene content is 80 mass% or more, 90 mass% or more, 95 mass% or more, 99 mass% or more).
[0024] The adhesive film 1 for metal terminals of the present disclosure includes at least one polypropylene layer 11. The adhesive film 1 for metal terminals may be a single layer or multiple layers. The adhesive film 1 for metal terminals is preferably composed of, for example, a single layer of polypropylene layer 11. FIG. 4 shows a diagram in which the adhesive film 1 for metal terminals is composed of a single layer of polypropylene layer 11.
[0025] In addition, when the adhesive film 1 for metal terminals is composed of multiple layers, the polypropylene layer 11 is preferably a layer that does not constitute the surface of the adhesive film 1 for metal terminals. In the case where the adhesive film 1 for metal terminals is composed of multiple layers, the adhesive film 1 for metal terminals is preferably a laminated structure of 3 to 6 layers, and the polypropylene layer 11 is preferably a layer that does not constitute the surface of the adhesive film 1 for metal terminals. FIG. 5 shows a laminated structure of a three-layer adhesive film 1 for metal terminals in which the first layer 12a located on the exterior material 3 side for power storage devices, the polypropylene layer 11, and the second layer 12b located on the metal terminal 2 side are laminated in this order. In addition, FIG. 6 shows a laminated structure of a four-layer adhesive film 1 for metal terminals in which the first layer 12a located on the exterior material 3 side for power storage devices, the polypropylene layer 11, the third layer 12c, and the second layer 12b located on the metal terminal 2 side are laminated in this order. In addition, FIG. 7 shows a laminated structure in which an adhesion promoter layer 13 is provided between the polypropylene layer 11 and the first layer 12a, and between the polypropylene layer 11 and the second layer 12b, for the purpose of firmly adhering these layers, as described below.
[0026] From the viewpoint of more suitably exerting the effects of the present disclosure, the ratio of the thickness of the polypropylene layer 11 to the thickness of the adhesive film 1 for metal terminals is preferably about 0.20 or more, more preferably about 0.25 or more, even more preferably about 0.30 or more, and is preferably about 0.90 or less, more preferably about 0.85 or less, even more preferably about 0.80 or less. Preferred ranges include about 0.20 to 0.90, about 0.20 to 0.85, about 0.20 to 0.80, about 0.25 to 0.90, about 0.25 to 0.85, about 0.25 to 0.80, about 0.30 to 0.90, about 0.30 to 0.85, and about 0.30 to 0.80.
[0027] The polypropylene layer 11 is a layer formed of polypropylene. Examples of polypropylene include crystalline or amorphous polypropylene such as homopolypropylene, block copolymer of polypropylene (e.g., block copolymer of propylene and ethylene), random copolymer of polypropylene (e.g., random copolymer of propylene and ethylene), and terpolymer of ethylene-butene-propylene. Among these polypropylenes, homopolypropylene and block copolymer of polypropylene are preferable. Note that, even in the case of homopolypropylene, those composed only of propylene are rare, and ethylene is usually copolymerized. In the present disclosure, it is preferable to use homopolypropylene with a particularly low ratio of ethylene (i.e., those with an island ratio of 20% or less in the above-mentioned sea-island structure).
[0028] The polypropylene of the polypropylene layer 11 may contain modified polypropylene or may be modified polypropylene. An example of modified polypropylene is acid-modified polypropylene. The acid-modified propylene is not particularly limited as long as it is an acid-modified polypropylene, but preferably includes polypropylene graft-modified with an unsaturated carboxylic acid or anhydride thereof. Specific examples of acid-modified polypropylene include crystalline or amorphous polypropylene such as homopolypropylene, polypropylene block copolymer (e.g., propylene and ethylene block copolymer), and polypropylene random copolymer (e.g., propylene and ethylene random copolymer); ethylene-butene-propylene terpolymer, etc. Among these polypropylenes, homopolypropylene and polypropylene block copolymer are preferred.
[0029] Examples of the carboxylic acid or anhydride thereof used for the acid modification include maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, itaconic anhydride, etc. When a resin layer containing maleic anhydride is analyzed by infrared spectroscopy, it is preferable that a peak derived from maleic anhydride is detected. For example, when maleic anhydride-modified polyolefin is measured by infrared spectroscopy, a peak derived from maleic anhydride is detected at a wave number of 1760 cm. -1 Nearby and wave number 1780cm -1 A peak derived from maleic anhydride is detected near the peak. When the polypropylene layer 11 is a layer composed of maleic anhydride-modified polypropylene, a peak derived from maleic anhydride is detected by infrared spectroscopy. However, if the degree of acid modification is low, the peak becomes small and may not be detected. In that case, analysis can be performed by nuclear magnetic resonance spectroscopy.
[0030] The polypropylene layer 11 may be formed of one type of resin component alone, or may be formed of a blend polymer of two or more types of resin components.
[0031] In the present disclosure, the island ratio of the sea-island structure of the polypropylene layer 11 may be 20% or less. From the viewpoint of more suitably exerting the effects of the present disclosure, the island ratio is preferably about 18% or less, more preferably about 15% or less, even more preferably about 10% or less, even more preferably about 5% or less, even more preferably less than about 5%, even more preferably about 3% or less, even more preferably about 1% or less, and also preferably about 0% or more, about 0.02% or more, about 0.04% or more, and the preferred range is about 0 to 20%, 0 to 18%. %, about 0 to 15%, about 0 to 10%, about 0 to 5%, 0% or more and less than about 5%, about 0 to 3%, about 0 to 1%, about 0.02 to 20%, about 0.02 to 18%, about 0.02 to 15%, about 0.02 to 10%, about 0.02 to 5%, 0.02% or more and less than about 5%, about 0.02 to 3%, about 0.02 to 1%, about 0.04 to 20%, about 0.04 to 18%, about 0.04 to 15%, about 0.04 to 10%, about 0.04 to 5%, 0.04% or more and less than about 5%, about 0.04 to 3%, and about 0.04 to 1%. The island ratio of the sea-island structure of the polypropylene layer 11 can be adjusted by controlling, for example, the polyethylene content in the polypropylene film, the polymerization type (homo, block, or random), and the film formation conditions (temperature and speed during film formation, cooling temperature and speed, etc.) The island ratio of the sea-island structure of the polypropylene layer is a value measured by the following method.
[0032] <Measurement of island ratio in sea-island structure of polypropylene layer> The adhesive film is embedded in a thermosetting epoxy resin and cured. A cross section in the desired direction (parallel to TD and in the thickness direction) is prepared using a commercially available rotary microtome and a diamond knife, and the cross section is prepared at -70°C using a cryomicrotome using liquid nitrogen. After staining with ruthenium tetroxide for 12 hours together with the embedded resin, the expanded part is trimmed with a microtome and cut in 100-300 nm increments in the MD direction until a total of 1-2 μm is cut. The cross section where the polypropylene layer is exposed is observed as follows. The stained cross section is observed with a field emission scanning electron microscope (measurement conditions: 3 kV 20 mA High WD 6 mm detector (Upper)) to obtain an image (magnification 10,000 times). Next, using image processing software capable of binarizing images, the island and sea parts of the sea-island structure are binarized for the image, and the ratio of the total area of the island parts (total area of the island parts / area of the measurement range of the image) is calculated.
[0033] [Image processing conditions] Image processing is performed using the image analysis software ImageJ. Specifically, the SEM image is acquired as a digital file of a grayscale image (JPEG) and processed according to the binarization procedure and parameters below, outputting pixels with a gradation above the threshold (bright) as 1 and pixels with a gradation below the threshold (dark) as 0, defining them as island and sea areas, respectively. <Binarization processing> 1. Spike noise removal (Despeckle) 2.Remove Island Contours (Remove Outliers radius=4 threshold=1 which=Bright) 3. Remove Outliers radius=4 threshold=1 which=Dark 4. Spike noise removal (Despeckle) 5. Gaussian blur along the X axis (sampling width) (threshold = 3 pixels) 6. Contrast Enhancement (saturated = 0.2) 7.Remove Outliers radius=4 threshold=1 which=Bright 8. Remove Outliers radius=4 threshold=1 which=Dark 9. Otsu's Binarization
[0034] From the viewpoint of more suitably exerting the effects of the present disclosure, the adhesive film 1 for metal terminals is heated under conditions of a temperature of 200°C, a surface pressure of 0.25 MPa, and a period of 16 seconds, and then the ratio of soft segment components measured by a Solid Echo method using pulse NMR in an environment at a temperature of 40°C is preferably about 20% or less, more preferably about 18% or less, and even more preferably about 16% or less, and is also preferably about 3% or more, more preferably about 8% or more, and even more preferably about 10% or more. Preferred ranges include about 3 to 20%, about 3 to 18%, about 3 to 16%, about 8 to 20%, about 8 to 18%, about 8 to 16%, about 10 to 20%, about 10 to 18%, and about 10 to 16%. The ratio of the soft segment component of the adhesive film 1 after heating can be adjusted, for example, by controlling the content of polyethylene in the polypropylene film, the polymerization type (homo, block, or random), and the film formation conditions (temperature and speed during film formation, cooling temperature and speed, etc.) The method for measuring the ratio of the soft segment component of the adhesive film for metal terminals after heating is as follows.
[0035] <Measurement of the ratio of soft segment components after heating of adhesive film> The adhesive film is heated at a temperature of 200°C, a surface pressure of 0.25MPa, and for 16 seconds to obtain a sample. This heating treatment is based on the assumption that the adhesive film will have properties after it is placed between an exterior material for a power storage device and a metal terminal and heat-sealed. The sample is introduced into a glass sample tube with a diameter of 10 mm, and the sample tube is placed in a pulse NMR device and held at 440°C for 5 minutes, after which a free induction decay curve of 1H spin-spin relaxation is obtained at 40°C using the Solid Echo method. The number of scans in the Solid Echo method was set to 64. The obtained decay curve is waveform-separated into three curves derived from the three components of the hard segment component, the intermediate segment component, and the soft segment component. The waveform separation is obtained by fitting the hard segment component to a Gaussian type function and the intermediate segment component and the soft segment component to an exponential type function using the analysis software "TD-NMRA (Version 4.3 Rev 0.8)" manufactured by BRUKER. Measurement points up to 0.6 msec on the relaxation curve are used for the analysis. The following equation is used for fitting: Y = A1 × exp(-(t / τ1) w1 )+A2×exp(-(t / τ2) w2 )+A3×exp(-(t / τ3) w3 ) Here, w1 to w3 are Weibull coefficients, with w1 being 2, and w2 and w3 being 1. A1 is the component ratio of the hard segment component, A2 is the intermediate segment component, and A3 is the component ratio of the soft segment component, and τ1 is the relaxation time of the hard segment component, τ2 is the intermediate segment component, and τ3 is the relaxation time of the soft segment component. t is time. The component ratios A1, A2, and A3 were calculated by averaging the values obtained by performing three measurements at the same level.
[0036] The polypropylene layer 11 may contain known additives as necessary.
[0037] For example, the polypropylene layer 11 may contain a filler as necessary. When the polypropylene layer 11 contains a filler, the filler functions as a spacer, making it possible to effectively suppress a short circuit between the metal terminal 2 and the barrier layer 33 of the exterior material 3 for an electrical storage device. The particle size of the filler is in the range of about 0.1 to 35 μm, preferably about 5.0 to 30 μm, and more preferably about 10 to 25 μm. The content of the filler is about 5 to 30 parts by mass, and more preferably about 10 to 20 parts by mass, relative to 100 parts by mass of the resin component forming the polypropylene layer 11.
[0038] As the filler, either inorganic or organic can be used. Examples of inorganic fillers include carbon (carbon, graphite), silica, aluminum oxide, barium titanate, iron oxide, silicon carbide, zirconium oxide, zirconium silicate, magnesium oxide, titanium oxide, calcium aluminate, calcium hydroxide, aluminum hydroxide, magnesium hydroxide, calcium carbonate, etc. Examples of organic fillers include fluororesin, phenolic resin, urea resin, epoxy resin, acrylic resin, benzoguanamine-formaldehyde condensate, melamine-formaldehyde condensate, polymethyl methacrylate crosslinked product, polyethylene crosslinked product, etc. From the viewpoints of shape stability, rigidity, and content resistance, aluminum oxide, silica, fluororesin, acrylic resin, and benzoguanamine-formaldehyde condensate are preferred, and among these, spherical aluminum oxide and silica are more preferred. As a method for mixing the filler into the resin component forming the polypropylene layer 11, a method in which the two are melt-blended in advance using a Banbury mixer or the like to prepare a master batch and then mixed in a predetermined ratio, or a method in which the filler is directly mixed with the resin component can be used.
[0039] The polypropylene layer 11 may contain a colorant such as a pigment as necessary. The colorant is not particularly limited, and a colorant capable of coloring the resin layer can be suitably used. Specific examples of the colorant include pigments. Various inorganic or organic pigments can be used as the pigment. Specific examples of the pigment include carbon (carbon, graphite), silica, titanium oxide, iron oxide, zinc oxide, magnesium oxide, and calcium oxide, which are exemplified as the above-mentioned filler, as well as inorganic oxides such as titanium nitride, zirconia black, copper oxide, cobalt oxide, and barium sulfate, and organic pigments such as quinacridone pigments, polyazo pigments, and isoindolinone pigments. Carbon (carbon, graphite) is a material that is generally used inside an electricity storage device, and there is no risk of it dissolving in the electrolyte. In addition, it has a large coloring effect, and a sufficient coloring effect can be obtained with an amount added that does not inhibit adhesion, and it does not melt with heat, and the apparent melt viscosity of the added resin can be increased. Furthermore, it is possible to prevent the pressed portion from becoming thin during thermal adhesion (heat sealing), thereby imparting excellent sealing properties between the exterior material for an electricity storage device and the metal terminal.
[0040] The color of the polypropylene layer 11 is not particularly limited and can be selected according to the purpose. The polypropylene layer 11 is preferably, for example, black, gray, or white.
[0041] When a pigment is added to the polypropylene layer 11, the amount of the pigment added is, for example, about 0.05 to 0.3 parts by mass, preferably about 0.1 to 0.2 parts by mass, per 100 parts by mass of the resin component forming the polypropylene layer 11, when carbon black with a particle size of about 0.03 μm is used. By adding a pigment to the polypropylene layer 11, the presence or absence of the adhesive film 1 for metal terminals can be detected by a sensor or visually inspected. When the above-mentioned filler and pigment are added to the polypropylene layer 11, the filler and pigment may be added to the same polypropylene layer 11, but from the viewpoint of not impairing the thermal fusion property of the adhesive film 1 for metal terminals, it is preferable to add the filler and pigment separately to a plurality of layers.
[0042] When a pigment is added to the polypropylene layer 11, the amount of the pigment added is, for example, about 0.05 to 0.3 parts by mass, preferably about 0.1 to 0.2 parts by mass, per 100 parts by mass of the resin component forming the polypropylene layer 11, when carbon black with a particle size of about 0.03 μm is used. By adding a pigment to the polypropylene layer 11, the presence or absence of the adhesive film 1 for metal terminals can be detected by a sensor or visually inspected. When a filler and a pigment are added to the polypropylene layer 11, the filler and the pigment may be added to the same polypropylene layer 11, but from the viewpoint of not impairing the thermal fusion property of the adhesive film 1 for metal terminals, it is preferable to add the filler and the pigment separately to different layers (for example, the first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, the polypropylene layer 11, etc., which will be described later).
[0043] From the viewpoint of more suitably achieving the effects of the present disclosure, the melting peak temperature of the polypropylene layer 11 is preferably about 140° C. or higher, more preferably about 145° C. or higher, and even more preferably about 150° C. or higher. From the same viewpoint, the melting peak temperature is, for example, 180° C. or lower, preferably 175° C. or lower, more preferably 170° C. or lower, and even more preferably about 165° C. or lower. Preferred ranges of the melting peak temperature include about 140 to 180° C., about 140 to 175° C., about 140 to 170° C., about 140 to 165° C., about 145 to 180° C., about 145 to 175° C., about 145 to 170° C., about 145 to 165° C., about 150 to 180° C., about 150 to 175° C., about 150 to 170° C., and about 150 to 165° C. In the present disclosure, the method for measuring the melting peak temperature is as follows.
[0044] <Measurement of melting peak temperature> The melting peak temperature of the adhesive film is measured in accordance with the provisions of JIS K7121:2012 (Method of measuring transition temperature of plastics (JIS K7121:1987 Supplement 1)). The measurement is performed using a differential scanning calorimeter. The measurement sample is held at -50°C for 15 minutes, then heated from -50°C to 210°C at a heating rate of 10°C / min, the first melting peak temperature P (°C) is measured, and then held at 210°C for 10 minutes. Next, the temperature is lowered from 210°C to -50°C at a heating rate of 10°C / min and held for 15 minutes. Furthermore, the temperature is raised from -50°C to 210°C at a heating rate of 10°C / min, and the second melting peak temperature Q (°C) is measured. The flow rate of nitrogen gas is 50 ml / min. The melting peak temperature P (°C) measured the first time and the melting peak temperature Q (°C) measured the second time are obtained by the above procedure. The melting peak temperature P (°C) measured the first time according to the above procedure is adopted.
[0045] When the adhesive film for metal terminal 1 of the present disclosure is composed of a single layer of the polypropylene layer 11 , the total thickness of the adhesive film for metal terminal 1 described below corresponds to the thickness of the polypropylene layer 11 .
[0046] In addition, when the adhesive film for metal terminal 1 of the present disclosure is composed of multiple layers, from the viewpoint of more suitably achieving the effects of the present disclosure, the thickness of the polypropylene layer 11 is preferably about 10 μm or more, more preferably about 15 μm or more, even more preferably about 20 μm or more, and is preferably about 120 μm or less, more preferably about 100 μm or less, even more preferably 80 μm or less. Preferred ranges of the thickness of the polypropylene layer 11 include about 10 to 120 μm, about 10 to 100 μm, about 10 to 80 μm, about 15 to 120 μm, about 15 to 100 μm, about 15 to 80 μm, about 20 to 120 μm, about 20 to 100 μm, and about 20 to 80 μm. From the viewpoint of improving the insulating properties of the adhesive film for metal terminal, the thickness of the polypropylene layer 11 is preferably about 55 μm or more, more preferably about 60 μm or more, and is also preferably about 100 μm or less, more preferably about 90 μm or less, and preferred ranges include about 55 to 100 μm, about 55 to 90 μm, about 60 to 100 μm, and about 60 to 90 μm. When the adhesive film for metal terminal 1 of the present disclosure contains a plurality of polypropylene layers 11, it is preferable that each of the polypropylene layers 11 has the above-mentioned thickness.
[0047] As described above, the adhesive film 1 for metal terminals of the present disclosure can be configured to have at least the first layer 12a, the polypropylene layer 11, and the second layer 12b laminated in this order, as shown in, for example, FIG. 5 to FIG. 7. In this configuration, the first layer 12a is disposed on the side of the exterior material 3 for an electric storage device, and the second layer 12b is disposed on the side of the metal terminal 2. The polypropylene layer 11 can be disposed between the first layer 12a and the second layer 12b to constitute an intermediate layer. In the laminate configurations of FIG. 5 to FIG. 7, the first layer 12a and the second layer 12b are located on the surfaces of both sides, respectively. In addition, in the laminate configuration of FIG. 6, the third layer 12c is provided between the polypropylene layer 11 and the second layer 12b. Although not shown, the fourth layer 12d may be provided between the first layer 12a and the polypropylene layer 11. When the adhesive film 1 for metal terminals of the present disclosure is composed of multiple layers, it is preferable that the adhesive film 1 for metal terminals is composed of 3 to 6 layers, and preferably has at least a first layer 12a that forms the surface facing the exterior material 3 for an electricity storage device, a second layer 12b that forms the surface facing the metal terminal 2, and a polypropylene layer 11 located between the first layer 12a and the second layer 12b.
[0048] When the adhesive film 1 for metal terminal of the present disclosure is disposed between the metal terminal 2 of the electricity storage device 10 and the exterior material 3 for the electricity storage device, the surface of the metal terminal 2 made of metal and the heat-sealable resin layer 35 (a layer formed of a heat-sealable resin such as polyolefin) of the exterior material 3 for the electricity storage device are bonded via the adhesive film 1 for metal terminal. The first layer 12a of the adhesive film 1 for metal terminal is disposed on the exterior material 3 for the electricity storage device, and the second layer 12b is disposed on the metal terminal 2 side, with the first layer 12a in close contact with the heat-sealable resin layer 35 of the exterior material 3 for the electricity storage device, and the second layer 12b in close contact with the metal terminal 2. The first layer 12a may be a single layer or a multilayer. The second layer 12b may be a single layer or a multilayer.
[0049] The first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, etc., which may be included in the adhesive film for metal terminal 1, can each be formed of, for example, a resin film. When the first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, etc. are each formed of a resin film, when the first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, etc. are laminated with the polypropylene layer 11, etc. to produce the adhesive film for metal terminal 1 of the present disclosure, a preformed resin film may be used as the first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, etc. Furthermore, the resins forming the first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, etc. may be formed into a film on the surface of the polypropylene layer 11, etc. by extrusion molding, coating, etc., to form the first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, etc., made of a resin film.
[0050] The first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, etc., which may be included in the adhesive film for metal terminal 1, may each be composed of a resin. Examples of resins that compose the first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, etc. include polyolefin resins, polyamide resins, polyester resins, epoxy resins, acrylic resins, fluororesins, silicone resins, phenol resins, polyetherimides, polyimides, polycarbonates, and mixtures and copolymers thereof, etc., and among these, polyolefin resins are particularly preferred. Examples of polyolefin resins include polyolefins and acid-modified polyolefins. Specific examples of polyolefins include polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; crystalline or amorphous polypropylenes such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); and ethylene-butene-propylene terpolymers. Among these polyolefins, polyethylene and polypropylene are preferred, and polypropylene is more preferred. The resin forming the surface layer of the adhesive film for metal terminal 1 is preferably random polypropylene from the viewpoint of reducing the amount of heat required during heat fusion and shortening the heat fusion time (from the viewpoint of seal adhesion).
[0051] The first layer 12a arranged on the side of the exterior material 3 for an electric storage device more preferably contains polyolefin as a main component, and even more preferably contains polypropylene as a main component. Here, the main component means that the content of the resin component contained in the first layer 12a is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more. For example, the first layer 12a containing polypropylene as a main component means that the content of polypropylene of the resin component contained in the first layer 12a is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more.
[0052] Moreover, the second layer 12b arranged on the metal terminal 2 side preferably contains an acid-modified polyolefin as a main component, and more preferably contains an acid-modified polypropylene as a main component. Here, the main component means that the content of the resin component contained in the second layer 12b is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more. For example, the second layer 12b containing an acid-modified polypropylene as a main component means that the content of the acid-modified polypropylene among the resin components contained in the second layer 12b is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more.
[0053] The melting peak temperatures of the first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, etc. are preferably 125° C. or higher, more preferably about 130° C. or higher, and even more preferably about 135° C. or higher. The melting peak temperatures are, for example, 180° C. or lower, preferably 175° C. or lower, more preferably 170° C. or lower, even more preferably about 165° C. or lower, and even more preferably about 160° C. or lower. Preferred ranges of the melting peak temperature include about 125 to 180°C, about 125 to 175°C, about 125 to 170°C, about 125 to 165°C, about 125 to 160°C, about 130 to 180°C, about 130 to 175°C, about 130 to 170°C, about 130 to 165°C, about 130 to 160°C, about 135 to 180°C, about 135 to 175°C, about 135 to 170°C, about 135 to 165°C, and about 135 to 160°C.
[0054] The thickness of the first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, etc. is preferably about 10 μm or more, more preferably about 15 μm or more, and even more preferably about 20 μm or more, and is preferably about 120 μm or less, more preferably about 100 μm or less, and even more preferably 80 μm or less. Preferred ranges of the thickness of the first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, etc. include about 10 to 120 μm, about 10 to 100 μm, about 10 to 80 μm, about 15 to 120 μm, about 15 to 100 μm, about 15 to 80 μm, about 20 to 120 μm, about 20 to 100 μm, and about 20 to 80 μm.
[0055] The first layer 12a, the second layer 12b, the third layer 12c, the fourth layer 12d, etc. may contain known additives (such as the above-mentioned fillers and pigments) in the same manner as the polypropylene layer 11. The types and amounts of the fillers and pigments are the same as those of the polypropylene layer 11.
[0056] From the viewpoint of more suitably achieving the effects of the present disclosure, the total thickness of the adhesive film 1 for a metal terminal is, for example, about 50 μm or more, preferably about 80 μm or more, more preferably about 90 μm or more, and even more preferably about 100 μm or more. The total thickness of the adhesive film 1 for a metal terminal of the present disclosure is about 500 μm or less, preferably about 300 μm or less, more preferably about 250 μm or less, and even more preferably 200 μm or less. Preferred ranges for the total thickness of the adhesive film 1 for metal terminals of the present disclosure include about 50 to 500 μm, about 50 to 300 μm, about 50 to 250 μm, about 50 to 200 μm, about 80 to 500 μm, about 80 to 300 μm, about 80 to 250 μm, about 80 to 200 μm, about 90 to 500 μm, about 90 to 300 μm, about 90 to 250 μm, about 90 to 200 μm, about 100 to 500 μm, about 100 to 300 μm, about 100 to 250 μm, and about 100 to 200 μm. As a more specific example, when the adhesive film 1 for metal terminals of the present disclosure is used in a relatively small power storage device for a mobile phone, smartphone, or tablet, the total thickness is preferably about 60 to 100 μm, and when it is used in a relatively large power storage device for a power storage system or vehicle-mounted power storage device, the total thickness is preferably about 100 to 250 μm.
[0057] In addition, from the viewpoint of more suitably exerting the effects of the present disclosure, the heat of fusion of the adhesive film for metal terminal 1 of the present disclosure measured after heating under conditions of a temperature of 200° C., a surface pressure of 0.25 MPa, and a period of 16 seconds is preferably about 50 J / g or more, more preferably about 55 J / g or more, even more preferably about 60 J / g or more, and even more preferably 65 J / g or more, and is preferably about 100 J / g or less, more preferably about 90 J / g or less, more preferably about 80 J / g or less, and preferred ranges include about 50 to 100 J / g, about 50 to 90 J / g, about 50 to 80 J / g, about 55 to 100 J / g, about 55 to 90 J / g, about 55 to 80 J / g, about 60 to 100 J / g, about 60 to 90 J / g, about 60 to 80 J / g, about 65 to 100 J / g, about 65 to 90 J / g, and about 65 to 80 J / g. The heat of fusion of the adhesive film after heating can be adjusted by controlling the content of polyethylene in the polypropylene film constituting the polypropylene layer 11, the polymerization type (homo, block, or random), and the film formation conditions (temperature and speed during film formation, cooling temperature and speed, etc.). The method for measuring the heat of fusion of the adhesive film after heating is as follows.
[0058] <Measurement of heat of fusion of adhesive film after heating> The adhesive film 1 for metal terminals of the present disclosure is heated under conditions of a temperature of 200°C, a surface pressure of 0.25MPa, and 16 seconds. This heat treatment is heating assuming the physical properties after the adhesive film is arranged between the exterior material for a power storage device and the metal terminal and heat-sealed. Next, the heat of fusion is measured in accordance with the provisions of JIS K 7122:2012. The measurement is performed using a differential scanning calorimeter. The adhesive film 1 for metal terminals after the heat treatment is held at -50°C for 15 minutes, then heated from -50°C to 210°C at a heating rate of 10°C / min, the first heat of fusion ΔH (J / g) is measured, and then held at 210°C for 10 minutes. Next, the temperature is lowered from 210°C to -50°C at a heating rate of 10°C / min, and held for 15 minutes. Furthermore, the temperature is raised from -50°C to 210°C at a heating rate of 10°C / min, and the second heat of fusion ΔH (J / g) is measured. The flow rate of nitrogen gas is 50 ml / min. The value of the heat of fusion ΔH (J / g) measured the first time using the above procedure is adopted as the heat of fusion. The heat of fusion is the area enclosed by the baseline (the line formed by connecting the start and end points of the ridge from base to base) and the peak in the DSC curve.
[0059] In order to more suitably exert the effects of the present disclosure, the water vapor permeability of the adhesive film 1 for metal terminal of the present disclosure is preferably about 5.10 g mm / (m 2 ·day) or less, more preferably about 4.20g·mm / (m 2 ·day) or less, and more preferably about 4.10g·mm / (m 2 ·day) or less, and more preferably about 4.00 g·mm / (m 2 ·day) or less, and for example, about 3.00 g·mm / (m 2 ·day) or more, approximately 0g·mm / (m 2 ·day) or more, and the preferred range is 0 to 5.10g·mm / (m 2 ·day), 0~4.20g·mm / (m 2 ·day), 0~4.10g·mm / (m 2 ·day), 0~4.00g·mm / (m 2 ·day), 3.0~5.10g·mm / (m 2·day), 3.00~4.20g·mm / (m 2 ·day), 3.00~4.10g·mm / (m 2 ·day) about 3.00~4.00g·mm / (m 2 The water vapor permeability of the adhesive film is measured as follows.
[0060] <Measurement of water vapor permeability of adhesive film> First, an exterior material for a power storage device (hereinafter, sometimes simply referred to as "exterior material") is prepared by the following procedure. For example, a biaxially oriented polyethylene terephthalate (PET) film (thickness 12 μm) and an oriented nylon (ONy) film (thickness 15 μm) were prepared as a base material layer. The PET film and the ONy film were bonded using a two-liquid urethane adhesive (polyol compound and aromatic isocyanate compound) and aging treatment was performed to obtain a base material layer (thickness 30 μm) in which the PET film (thickness 12 μm) / adhesive layer (thickness after curing is 3 μm) / ONy film (thickness 15 μm) were laminated from the outside in this order. In addition, an aluminum foil (JIS H4160:1994 A8021H-O (thickness 40 μm)) was prepared as a barrier layer. Next, the surface of the ONy film side of the base material layer and the barrier layer are bonded using a two-component urethane adhesive (a polyol compound and an aromatic isocyanate compound), and an aging treatment is performed to obtain a pseudo exterior material for an electricity storage device (total thickness 73 μm) that is missing the inner side of the barrier layer, and is composed of a laminate of the base material layer (thickness 30 μm) / adhesive layer (thickness 3 μm after curing) / barrier layer (thickness 40 μm) laminated in that order.
[0061] Next, as shown in the schematic diagram of Figure 9, the obtained exterior material 3 is cut into a square with a length (MD) of 120 mm and a width (TD) of 120 mm (Figure 9a). In addition, two pieces of adhesive film 1 are cut into rectangles with a length (MD) of 120 mm and a width (TD) of 10 mm, and two pieces are cut into rectangles with a length (MD) of 100 mm and a width (TD) of 10 mm. On top of the barrier layer side of the exterior material 3, an adhesive film with the same length is placed facing along the periphery of the exterior material 3 (Figure 9b). At this time, the second layer side of the adhesive film is placed on the barrier layer side of the exterior material 3. Next, a polytetrafluoroethylene film (PTFE film, 100 μm thick) is placed on the adhesive film of the laminate (the surface of the adhesive film is covered with the PTFE film), and the silicone sheet / PTFE / laminate / PTFE / silicone sponge sheet is placed on a press machine heated to 200°C and left for 16 seconds under a pressure of 0.25 MPa to heat-seal the adhesive film to the exterior material 3. The laminate after heat-sealing is naturally cooled to 25°C, and the PTFE film is peeled off from the laminate. This heating process is heating that assumes the physical properties after the adhesive film is placed between the exterior material for the power storage device and the metal terminal and heat-sealed. Next, the exterior material 3 is folded in half vertically so that the adhesive film is on the inside (FIG. 9c). Two adhesive films for metal terminals with a length (MD) of 120 mm are placed between the exterior materials 3 along the long side to be heat-sealed as described below, and the adhesive film for metal terminals with a length (MD) of 100 mm is folded in half and placed between the exterior materials 3 along the short side to be heat-sealed as described below. The periphery of the exterior material 3 is a laminate in which exterior material / adhesive film / adhesive film / exterior material are layered in this order (Figure 9c).
[0062] Next, a heat seal bar (stainless steel plate) is used to heat seal the layers of the laminate at the long and short sides of the laminate, leaving one short side unheat-sealed (Figure 9c). The conditions for heat sealing are as follows: for the long side, a 7 mm wide heat seal bar is used, and heat sealing is performed once at a temperature of 190°C, a surface pressure of 0.5 MPa, and for 1.5 seconds (s1 in Figure 9c). For the short side, a 7 mm wide heat seal bar is used, and heat sealing is performed once at a temperature of 190°C, a surface pressure of 0.5 MPa, and for 1.5 seconds (s2 in Figure 9c). The laminate is then dried for one day in a dry room. Next, about 3.0 g of a liquid (moisture content 0%) of ethylene carbonate:diethyl carbonate:dimethyl carbonate = 1:1:1 (volume ratio) is injected from the position of the short side that is not heat-sealed (Figure 9d), and the short side that is not heat-sealed is also heat-sealed in the same manner as the short side described above (s3 in Figure 9e) to form a sealed bag (Figure 9e). This sealed bag is left to stand for 30 days in an environment with a temperature of 65°C and a relative humidity of 90%, and then the moisture content of the liquid removed from the sealed bag is measured in a dry room using the Karl Fischer method to obtain the moisture content (ppm). The amount of electrolyte injected (g), the permeation distance (mm), and the permeation cross-sectional area (m 2 ), and the number of days of storage (days), the water vapor permeability (g mm / (m 2 Find the day. Water vapor permeability (g mm / (m 2 ·day) = [obtained moisture content (ppm) × added electrolyte (g) × permeation distance (mm)] / [permeation cross-sectional area (m 2 ) × number of storage days (days)] Obtained water content (ppm): Obtained by Karl Fischer method. Electrolyte added (g): 3.0g -Transmission distance (mm): Seal width 7mm ·Transmission cross section (m 2 ): remaining thickness (μm) x inner circumference of seal (mm) Storage period: 30 days
[0063] [Base material] In the adhesive film for metal terminal 1, the substrate is a layer that functions as a support for the adhesive film for metal terminal 1, and is provided as necessary. For example, a polypropylene layer 11 can be used as the substrate. For example, in the case of an adhesive film for metal terminal 1 having a substrate as an intermediate layer, a roll of the substrate is prepared in advance, and an extruder and a T-die casting device are used to extrude polypropylene or the like to a predetermined thickness onto the surface of the substrate unwound from the roll, thereby producing an adhesive film for metal terminal 1 having a multilayer structure.
[0064] The substrate may be formed of the aforementioned polypropylene layer 11, or may be formed of the aforementioned first layer 12a, second layer 12b, third layer 12c, fourth layer 12d, and the like.
[0065] The substrate can be formed, for example, from a resin film. When the substrate is formed from a resin film, a preformed resin film may be used as the substrate when the substrate is laminated with the first layer 12a or the like to produce the adhesive film for metal terminal 1 of the present disclosure. The resin forming the substrate may be formed into a film on the surface of the first layer 12a or the like by extrusion molding, coating, or the like to form a substrate formed from a resin film.
[0066] The material forming the substrate is not particularly limited. Examples of the material forming the substrate include polyolefin resins, polyamide resins, polyester resins, epoxy resins, acrylic resins, fluororesins, silicon resins, phenol resins, polyetherimides, polyimides, polycarbonates, and mixtures and copolymers thereof, among which polyolefin resins are particularly preferred. That is, the material forming the substrate is preferably a resin containing a polyolefin skeleton such as polyolefin or acid-modified polyolefin. The resin constituting the substrate can be analyzed to contain a polyolefin skeleton, for example, by infrared spectroscopy, gas chromatography mass spectrometry, or the like.
[0067] The substrate preferably contains a polyolefin resin, more preferably contains a polyolefin, and more preferably is a layer formed of a polyolefin. The layer formed of a polyolefin may be a stretched polyolefin film or an unstretched polyolefin film, but is preferably an unstretched polyolefin film. Specific examples of polyolefin include polyethylene such as low density polyethylene, medium density polyethylene, high density polyethylene, and linear low density polyethylene; crystalline or amorphous polypropylene such as homopolypropylene, block copolymer of polypropylene (e.g., block copolymer of propylene and ethylene), and random copolymer of polypropylene (e.g., random copolymer of propylene and ethylene); and terpolymer of ethylene-butene-propylene. Among these polyolefins, polyethylene and polypropylene are preferred, and polypropylene is more preferred. In addition, since the substrate has excellent electrolyte resistance, it is preferred that the substrate contains homopolypropylene, more preferably is formed of homopolypropylene, and even more preferably is an unstretched homopolypropylene film.
[0068] Specific examples of polyamides include aliphatic polyamides such as nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, and copolymers of nylon 6 and nylon 66; hexamethylenediamine-isophthalic acid-terephthalic acid copolymer polyamides such as nylon 6I, nylon 6T, nylon 6IT, and nylon 6I6T (I represents isophthalic acid, and T represents terephthalic acid) containing structural units derived from terephthalic acid and / or isophthalic acid, and aromatic polyamides such as polymetaxylylene adipamide (MXD6); alicyclic polyamides such as polyaminomethylcyclohexyl adipamide (PACM6); polyamides copolymerized with lactam components and isocyanate components such as 4,4'-diphenylmethane-diisocyanate, polyesteramide copolymers and polyetheresteramide copolymers which are copolymers of copolymerized polyamides with polyesters or polyalkylene ether glycols; and copolymers thereof. These polyamides may be used alone or in combination of two or more.
[0069] Specific examples of polyesters include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, copolymerized polyesters mainly composed of ethylene terephthalate as repeating units, copolymerized polyesters mainly composed of butylene terephthalate as repeating units, etc. Specific examples of copolymerized polyesters mainly composed of ethylene terephthalate as repeating units include copolymer polyesters in which ethylene terephthalate as a main repeating unit is polymerized with ethylene isophthalate (hereinafter abbreviated as polyethylene (terephthalate / isophthalate)), polyethylene (terephthalate / isophthalate), polyethylene (terephthalate / adipate), polyethylene (terephthalate / sodium sulfoisophthalate), polyethylene (terephthalate / sodium isophthalate), polyethylene (terephthalate / phenyl-dicarboxylate), polyethylene (terephthalate / decane dicarboxylate), etc. Specific examples of copolymer polyesters containing butylene terephthalate as the main repeating unit include copolymer polyesters in which butylene terephthalate is the main repeating unit and is polymerized with butylene isophthalate (hereinafter abbreviated as polybutylene (terephthalate / isophthalate)), polybutylene (terephthalate / adipate), polybutylene (terephthalate / sebacate), polybutylene (terephthalate / decanedicarboxylate), polybutylene naphthalate, etc. These polyesters may be used alone or in combination of two or more.
[0070] The substrate may be made of a nonwoven fabric formed from the above resin. When the substrate is a nonwoven fabric, the substrate is preferably made of the above polyolefin resin, polyamide resin, or the like.
[0071] The melting peak temperature of the base material is preferably 120° C. or higher, more preferably about 130° C. or higher, and even more preferably about 140° C. or higher. From the same viewpoint, the melting peak temperature is, for example, 210° C. or lower, preferably 200° C. or lower, more preferably 190° C. or lower, even more preferably about 180° C. or lower, and even more preferably about 170° C. or lower. Preferred ranges of the melting peak temperature include about 120 to 210°C, about 120 to 200°C, about 120 to 190°C, about 120 to 180°C, about 120 to 170°C, about 130 to 210°C, about 130 to 200°C, about 130 to 190°C, about 130 to 180°C, about 130 to 170°C, about 140 to 210°C, about 140 to 200°C, about 140 to 190°C, about 140 to 180°C, and about 140 to 170°C.
[0072] The substrate may be a single layer or multiple layers.
[0073] In addition, by blending a colorant in the substrate, the substrate can be made into a layer containing the colorant. In addition, the light transmittance can be adjusted by selecting a resin with low transparency. When the substrate is a film, a colored film or a film with low transparency can be used. When the substrate is a nonwoven fabric, a nonwoven fabric using a fiber or binder containing a colorant or a nonwoven fabric with low transparency can be used.
[0074] When the substrate is made of a resin film, the surface of the substrate may be subjected to a known adhesion enhancing treatment such as corona discharge treatment, ozone treatment, plasma treatment or the like, if necessary.
[0075] From the viewpoint of more suitably achieving the effects of the present disclosure, the thickness of the substrate is preferably about 20 μm or more, more preferably about 30 μm or more, and even more preferably about 40 μm or more, and is preferably about 120 μm or less, more preferably about 110 μm or less, and even more preferably 100 μm or less. Preferred ranges of the thickness of the substrate include about 20 to 120 μm, about 20 to 110 μm, about 20 to 100 μm, about 30 to 120 μm, about 30 to 110 μm, about 30 to 100 μm, about 40 to 120 μm, about 40 to 110 μm, and about 40 to 100 μm.
[0076] [Adhesion promoter layer 13] The adhesion promoter layer 13 is a layer that is provided as necessary for the purpose of, for example, firmly adhering the polypropylene layer 11 to the first layer 12a and the polypropylene layer 11 to the second layer 12b (see FIG. 7). The adhesion promoter layer 13 may be provided on only one side between the polypropylene layer 11 and the first layer 12a and between the polypropylene layer 11 and the second layer 12b, or on both sides.
[0077] The adhesion promoter layer 13 can be formed using known adhesion promoters such as isocyanate-based, polyethyleneimine-based, polyester-based, polyurethane-based, polybutadiene-based, etc. From the viewpoint of obtaining strong adhesion strength, it is preferable to form the adhesion promoter using an isocyanate-based adhesion promoter among these. As the isocyanate-based adhesion promoter, one made of an isocyanate component selected from triisocyanate monomer and polymeric MDI has excellent laminate strength and is less likely to decrease in laminate strength at high temperatures. It is particularly preferable to form the adhesive using an adhesion promoter made of triphenylmethane-4,4',4"-triisocyanate, which is a triisocyanate monomer, or polymethylene polyphenyl polyisocyanate, which is a polymeric MDI (NCO content of approximately 30%, viscosity of 200 to 700 mPa s). It is also preferable to form the adhesive using a two-component curing adhesion promoter that uses tris(p-isocyanatephenyl)thiophosphate, which is a triisocyanate monomer, or a polyethyleneimine-based agent as the main agent and polycarbodiimide as the crosslinking agent.
[0078] The adhesion promoter layer 13 can be formed by coating and drying using a known coating method such as bar coating, roll coating, gravure coating, etc. The coating amount of the adhesion promoter is 20 to 100 mg / m in the case of an adhesion promoter made of triisocyanate. 2 Approximately, preferably 40 to 60 mg / m 2 In the case of adhesion promoters made of polymeric MDI, the concentration is 40 to 150 mg / m 2 Approximately, preferably 60 to 100 mg / m 2 In the case of a two-component curing adhesion promoter that uses polyethyleneimine as the base agent and polycarbodiimide as the crosslinking agent, the adhesive strength is about 5 to 50 mg / m 2 Approximately, preferably 10 to 30 mg / m 2 Triisocyanate monomer is a monomer with three isocyanate groups in one molecule, and polymeric MDI is a mixture of MDI and MDI oligomers formed by polymerization of MDI, and is represented by the following formula:
[0079] [ka]
[0080] In order to more suitably exert the effects of the present invention, it is preferable that the first layer 12a and the polypropylene layer 11 are in contact with each other, and that the second layer 12b and the polypropylene layer 11 are in contact with each other.
[0081] Specific examples of preferred laminated structures of the adhesive film 1 for metal terminals of the present disclosure include a three-layer structure in which a first layer 12a formed from polypropylene / a polypropylene layer 11 formed from polypropylene / a second layer 12b formed from acid-modified polypropylene are laminated in this order; a three-layer structure in which a first layer 12a formed from acid-modified polypropylene / a polypropylene layer 11 formed from polypropylene / a second layer 12b formed from acid-modified polypropylene are laminated in this order; a four-layer structure in which a first layer 12a formed from polypropylene / a polypropylene layer 11 formed from polypropylene / a third layer 12c formed from polypropylene / a second layer 12b formed from acid-modified polypropylene are laminated in this order; and a four-layer structure in which a first layer 12a formed from acid-modified polypropylene / a polypropylene layer 11 formed from polypropylene / a third layer 12c formed from polypropylene / a second layer 12b formed from acid-modified polypropylene are laminated in this order.
[0082] The adhesive film 1 for metal terminals of the present disclosure is preferably formed of a polyolefin-based resin. For example, the resin component contained in the adhesive film 1 for metal terminals of the present disclosure is preferably only a polyolefin-based resin, more preferably only an acid-modified polyolefin and a polyolefin, and even more preferably only an acid-modified polypropylene and a polypropylene. The preferred acid-modified polyolefin and polyolefin are as described above.
[0083] The method for interposing the adhesive film 1 for a metal terminal between the metal terminal 2 and the exterior material 3 for an electricity storage device is not particularly limited, and for example, as shown in Figures 1 to 3, the adhesive film 1 for a metal terminal may be wrapped around the metal terminal 2 in a portion where the metal terminal 2 is sandwiched by the exterior material 3 for an electricity storage device. Furthermore, although not shown, in a portion where the metal terminal 2 is sandwiched by the exterior material 3 for an electricity storage device, the adhesive film 1 for a metal terminal may be disposed on both sides of the metal terminal 2 so as to cross the two metal terminals 2.
[0084] [Metal terminal 2] The adhesive film 1 for metal terminals of the present disclosure is used by being interposed between a metal terminal 2 and an exterior material 3 for an electricity storage device. The metal terminal 2 (tab) is a conductive member electrically connected to an electrode (positive electrode or negative electrode) of an electricity storage device element 4, and is made of a metal material. The metal material constituting the metal terminal 2 is not particularly limited, and examples thereof include aluminum, nickel, and copper. For example, the metal terminal 2 connected to the positive electrode of a lithium ion electricity storage device is usually made of aluminum or the like. Moreover, the metal terminal 2 connected to the negative electrode of a lithium ion electricity storage device is usually made of copper, nickel, or the like.
[0085] From the viewpoint of enhancing electrolyte resistance, it is preferable that the surface of the metal terminal 2 is subjected to a chemical conversion treatment. For example, when the metal terminal 2 is made of aluminum, specific examples of the chemical conversion treatment include known methods for forming a corrosion-resistant film such as a phosphate, a chromate, a fluoride, or a triazine thiol compound. Among the methods for forming a corrosion-resistant film, a phosphate chromate treatment using a material composed of three components: a phenolic resin, a chromium (III) fluoride compound, and phosphoric acid is preferable.
[0086] The size of the metal terminal 2 may be appropriately set depending on the size of the electricity storage device to be used. The thickness of the metal terminal 2 is preferably about 50 to 1000 μm, more preferably about 70 to 800 μm. The length of the metal terminal 2 is preferably about 1 to 200 mm, more preferably about 3 to 150 mm. The width of the metal terminal 2 is preferably about 1 to 200 mm, more preferably about 3 to 150 mm.
[0087] [Exterior materials for energy storage devices 3] The exterior material 3 for an electricity storage device may have a laminated structure including at least a base material layer 31, a barrier layer 33, and a heat-sealable resin layer 35 in this order. FIG. 8 shows an example of a cross-sectional structure of the exterior material 3 for an electricity storage device, in which the base material layer 31, an adhesive layer 32 provided as needed, a barrier layer 33, an adhesive layer 34 provided as needed, and a heat-sealable resin layer 35 are laminated in this order. In the exterior material 3 for an electricity storage device, the base material layer 31 is the outer layer, and the heat-sealable resin layer 35 is the innermost layer. When assembling the electricity storage device, the heat-sealable resin layers 35 located on the periphery of the electricity storage device element 4 are brought into contact with each other and heat-sealed to seal the electricity storage device element 4, thereby sealing the electricity storage device element 4. Note that FIGS. 1 to 3 show an electricity storage device 10 using an embossed type exterior material 3 for an electricity storage device formed by embossing or the like, but the exterior material 3 for an electricity storage device may be an unformed pouch type. The pouch type includes three-sided seal, four-sided seal, pillow type, etc., and any type may be used.
[0088] The thickness of the laminate constituting the electricity storage device exterior material 3 is not particularly limited, but the upper limit, from the viewpoints of cost reduction, energy density improvement, and the like, is, for example, about 190 μm or less, preferably about 180 μm or less, about 160 μm or less, about 155 μm or less, about 140 μm or less, about 130 μm or less, and about 120 μm or less. The lower limit, from the viewpoint of maintaining the function of the electricity storage device exterior material 3 to protect the electricity storage device element 4, is preferably about 35 μm or more, about 45 μm or more, about 60 μm or more, and about 80 μm or more. Preferred ranges are, for example, about 35 to 190 μm, about 35 to 180 μm, and about 35 to 160 μm. degree, about 35-155μm, about 35-140μm, about 35-130μm, about 35-120μm, about 45-190μm, about 45-180μm, 45 ~160μm, 45~155μm, 45~140μm, 45~130μm, 45~120μm, 60~190μm, 60~180μm Examples of the thickness include about 60 to 160 μm, about 60 to 155 μm, about 60 to 140 μm, about 60 to 130 μm, about 60 to 120 μm, about 80 to 190 μm, about 80 to 180 μm, about 80 to 160 μm, about 80 to 155 μm, about 80 to 140 μm, about 80 to 130 μm, and about 80 to 120 μm.
[0089] (Base material layer 31) In the packaging material 3 for an electricity storage device, the base material layer 31 is a layer that functions as the base material of the packaging material for an electricity storage device, and is a layer that forms the outermost layer side.
[0090] The material for forming the base layer 31 is not particularly limited, as long as it has insulating properties. Examples of materials for forming the base layer 31 include polyester, polyamide, epoxy, acrylic resin, fluororesin, polyurethane, silicone resin, phenol, polyetherimide, polyimide, and mixtures and copolymers thereof. Polyesters such as polyethylene terephthalate and polybutylene terephthalate have the advantage of being excellent in electrolyte resistance and being unlikely to cause whitening due to adhesion of electrolyte, and are preferably used as materials for forming the base layer 31. In addition, polyamide films have excellent stretchability and can prevent whitening due to resin cracking of the base layer 31 during molding, and are preferably used as materials for forming the base layer 31.
[0091] The base layer 31 may be formed of a uniaxially or biaxially stretched resin film, or may be formed of an unstretched resin film. Among them, a uniaxially or biaxially stretched resin film, especially a biaxially stretched resin film, is preferably used as the base layer 31 because its heat resistance is improved by oriented crystallization.
[0092] Among these, the resin film forming the base layer 31 is preferably nylon or polyester, and more preferably biaxially oriented nylon or biaxially oriented polyester.
[0093] The base layer 31 may be laminated with resin films of different materials in order to improve pinhole resistance and insulation when used as a package for a power storage device. Specifically, it may be a multi-layer structure in which a polyester film and a nylon film are laminated, or a multi-layer structure in which a biaxially oriented polyester and a biaxially oriented nylon are laminated. When the base layer 31 has a multi-layer structure, each resin film may be bonded via an adhesive, or may be directly laminated without an adhesive. When bonding without an adhesive, for example, a method of bonding in a hot melt state such as a co-extrusion method, a sand lamination method, or a thermal lamination method may be used.
[0094] The base layer 31 may be made to have low friction in order to improve formability. When making the base layer 31 low-friction, the coefficient of friction of the surface is not particularly limited, but may be, for example, 1.0 or less. To make the base layer 31 low-friction, for example, matte treatment, formation of a thin film layer of a slip agent, a combination of these, etc. may be used.
[0095] The thickness of the base layer 31 is, for example, about 10 to 50 μm, and preferably about 15 to 30 μm.
[0096] (Adhesive layer 32) In the exterior material 3 for an electricity storage device, the adhesive layer 32 is a layer that is disposed on the base material layer 31 as necessary in order to impart adhesion to the base material layer 31. That is, the adhesive layer 32 is provided between the base material layer 31 and the barrier layer 33.
[0097] The adhesive layer 32 is formed of an adhesive capable of bonding the base material layer 31 and the barrier layer 33. The adhesive used to form the adhesive layer 32 may be a two-component curing adhesive or a one-component curing adhesive. The adhesion mechanism of the adhesive used to form the adhesive layer 32 is not particularly limited, and may be any of a chemical reaction type, a solvent volatilization type, a thermal melting type, a thermal pressure type, and the like.
[0098] The resin component of the adhesive that can be used to form the adhesive layer 32 is preferably a polyurethane-based two-component curing adhesive; or a blend resin of polyamide, polyester, or these with modified polyolefin, from the viewpoint of having excellent ductility, durability under high humidity conditions, yellowing prevention, and thermal degradation prevention during heat sealing, and of effectively suppressing a decrease in the laminate strength between the base layer 31 and the barrier layer 33 and preventing the occurrence of delamination.
[0099] The adhesive layer 32 may be multi-layered with different adhesive components. When the adhesive layer 32 is multi-layered with different adhesive components, it is preferable to select a resin having excellent adhesion to the base material layer 31 as the adhesive component arranged on the base material layer 31 side, and an adhesive component having excellent adhesion to the barrier layer 33 as the adhesive component arranged on the barrier layer 33 side, from the viewpoint of improving the laminate strength between the base material layer 31 and the barrier layer 33. When the adhesive layer 32 is multi-layered with different adhesive components, specifically, the adhesive component arranged on the barrier layer 33 side is preferably an acid-modified polyolefin, a metal-modified polyolefin, a mixed resin of polyester and acid-modified polyolefin, a resin containing a copolymerized polyester, or the like.
[0100] The thickness of the adhesive layer 32 is, for example, about 2 to 50 μm, and preferably about 3 to 25 μm.
[0101] (Barrier layer 33) In the electrical storage device exterior material 3, the barrier layer 33 is a layer that has the function of preventing water vapor, oxygen, light, and the like from penetrating into the electrical storage device in addition to improving the strength of the electrical storage device exterior material. The barrier layer 33 is preferably a metal layer, that is, a layer formed of a metal. Specific examples of metals constituting the barrier layer 33 include aluminum, stainless steel, and titanium, and preferably aluminum. The barrier layer 33 can be formed, for example, of a metal foil, a metal vapor deposition film, an inorganic oxide vapor deposition film, a carbon-containing inorganic oxide vapor deposition film, or a film provided with these vapor deposition films, and is preferably formed of a metal foil, and more preferably formed of an aluminum foil. From the viewpoint of preventing the occurrence of wrinkles or pinholes in the barrier layer 33 during the manufacture of the exterior material for an electricity storage device, it is more preferable that the barrier layer be formed from a soft aluminum foil such as annealed aluminum (JIS H4160:1994 A8021H-O, JIS H4160:1994 A8079H-O, JIS H4000:2014 A8021P-O, JIS H4000:2014 A8079P-O).
[0102] The thickness of the barrier layer 33 is preferably about 10 to 200 μm, more preferably about 20 to 100 μm, about 20 to 45 μm, about 45 to 65 μm, or about 65 to 85 μm, from the viewpoint of making the exterior material for an electricity storage device thin while making it difficult for pinholes to occur during molding.
[0103] Moreover, it is preferable that at least one surface, and preferably both surfaces, of the barrier layer 33 are subjected to a chemical conversion treatment in order to stabilize adhesion, prevent dissolution or corrosion, etc. Here, the chemical conversion treatment refers to a treatment for forming a corrosion-resistant film on the surface of the barrier layer.
[0104] (adhesive layer 34) In the packaging material 3 for an electricity storage device, the adhesive layer 34 is a layer that is provided, if necessary, between the barrier layer 33 and the heat-sealable resin layer 35 in order to firmly bond the heat-sealable resin layer 35.
[0105] The adhesive layer 34 is formed of an adhesive capable of bonding the barrier layer 33 and the heat-fusible resin layer 35. The composition of the adhesive used to form the adhesive layer is not particularly limited, and examples thereof include a resin composition containing an acid-modified polyolefin. Examples of the acid-modified polyolefin include the same ones as those exemplified for the first layer 12a and the second layer 12b.
[0106] The thickness of the adhesive layer 34 is, for example, about 1 to 40 μm, and preferably about 2 to 30 μm.
[0107] (Thermal adhesive resin layer 35) In the electricity storage device packaging material 3, the heat-sealable resin layer 35 corresponds to the innermost layer, and is a layer that seals the electricity storage device elements by being heat-sealed to each other when the electricity storage device is assembled.
[0108] The resin component used in the heat-fusible resin layer 35 is not particularly limited as long as it is heat-fusible, and examples thereof include polyolefin and cyclic polyolefin.
[0109] Specific examples of the polyolefin include polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; crystalline or amorphous polypropylenes such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); and ethylene-butene-propylene terpolymers. Among these polyolefins, polyethylene and polypropylene are preferable.
[0110] The cyclic polyolefin is a copolymer of an olefin and a cyclic monomer, and examples of the olefins constituting the cyclic polyolefin include ethylene, propylene, 4-methyl-1-pentene, butadiene, and isoprene. Examples of the cyclic monomers constituting the cyclic polyolefin include cyclic alkenes such as norbornene; specifically, cyclic dienes such as cyclopentadiene, dicyclopentadiene, cyclohexadiene, and norbornadiene. Among these polyolefins, preferred are cyclic alkenes, and more preferred are norbornene. Another example of the constituting monomer is styrene.
[0111] Among these resin components, preferred are crystalline or amorphous polyolefins, cyclic polyolefins, and blend polymers thereof; more preferred are polyethylene, polypropylene, copolymers of ethylene and norbornene, and blend polymers of two or more of these.
[0112] The heat-sealable resin layer 35 may be formed of one type of resin component alone, or may be formed of a blend polymer of two or more types of resin components. The heat-sealable resin layer 35 may be formed of only one layer, or may be formed of two or more layers of the same or different resin components. It is particularly preferable that the second layer 12b and the heat-sealable resin layer 35 use the same resin, since this improves the adhesion between these layers.
[0113] The thickness of the heat-sealable resin layer 35 is not particularly limited, but may be about 2 to 2000 μm, preferably about 5 to 1000 μm, and more preferably about 10 to 500 μm. The thickness of the heat-sealable resin layer 35 may be, for example, about 100 μm or less, preferably about 85 μm or less, and more preferably about 15 to 85 μm. For example, when the thickness of the adhesive layer 34 described below is 10 μm or more, the thickness of the heat-sealable resin layer 35 is preferably about 85 μm or less, and more preferably about 15 to 45 μm. For example, when the thickness of the adhesive layer 34 described below is less than 10 μm or when the adhesive layer 34 is not provided, the thickness of the heat-sealable resin layer 35 is preferably about 20 μm or more, and more preferably about 35 to 85 μm.
[0114] The exterior material for an electricity storage device of the present disclosure can also be in the form of a kit including the exterior material for an electricity storage device for use in an electricity storage device and the adhesive film for a metal terminal of the present disclosure. In this case, the electricity storage device to which the kit is applied includes at least an electricity storage device element having a positive electrode, a negative electrode, and an electrolyte, an exterior material for an electricity storage device that seals the electricity storage device element, and metal terminals that are electrically connected to the positive electrode and the negative electrode and protrude outside the exterior material for an electricity storage device. The kit of the present disclosure is used such that the adhesive film for a metal terminal of the present disclosure is interposed between the metal terminal and the exterior material for an electricity storage device when used.
[0115] 2. Energy storage devices The electricity storage device 10 of the present disclosure comprises at least an electricity storage device element 4 having a positive electrode, a negative electrode, and an electrolyte, an exterior material for an electricity storage device 3 that seals the electricity storage device element 4, and a metal terminal 2 that is electrically connected to each of the positive electrode and the negative electrode and protrudes to the outside of the exterior material for an electricity storage device 3. The electricity storage device 10 of the present disclosure is characterized in that an adhesive film for a metal terminal 1 of the present disclosure is interposed between the metal terminal 2 and the exterior material for an electricity storage device 3. That is, the electricity storage device 10 of the present disclosure can be manufactured by a method including a step of interposing an adhesive film for a metal terminal 1 of the present disclosure between the metal terminal 2 and the exterior material for an electricity storage device 3.
[0116] Specifically, an electric storage device element 4 having at least a positive electrode, a negative electrode, and an electrolyte is covered with an electric storage device exterior material 3 in a state in which metal terminals 2 connected to the positive and negative electrodes are protruding outward, and an adhesive film 1 for metal terminals of the present disclosure is interposed between the metal terminals 2 and a heat-sealable resin layer 35, and the electric storage device element 4 is covered so that a flange portion (a region where the heat-sealable resin layers 35 contact each other, the peripheral portion 3a of the electric storage device exterior material 3) of the electric storage device exterior material 3 can be formed, and the heat-sealable resin layers 35 of the flange portion are heat-sealed to each other to provide an electric storage device 10 using the electric storage device exterior material 3. When the electric storage device element 4 is housed using the electric storage device exterior material 3, the heat-sealable resin layer 35 of the electric storage device exterior material 3 is used so that it faces inside (the surface in contact with the electric storage device element 4).
[0117] The exterior material for an electric storage device of the present disclosure can be suitably used for an electric storage device such as a battery (including a condenser, a capacitor, etc.). The exterior material for an electric storage device of the present disclosure may be used for either a primary battery or a secondary battery, but is preferably a secondary battery. The type of secondary battery to which the exterior material for an electric storage device of the present disclosure is applied is not particularly limited, and examples thereof include lithium ion batteries, lithium ion polymer batteries, all-solid batteries, semi-solid batteries, quasi-solid batteries, polymer batteries, all-resin batteries, lead-acid batteries, nickel-hydrogen batteries, nickel-cadmium batteries, nickel-iron batteries, nickel-zinc batteries, silver oxide-zinc batteries, metal-air batteries, polyvalent cation batteries, condensers, capacitors, etc. Among these secondary batteries, examples of suitable applications of the exterior material for an electric storage device of the present disclosure include lithium ion batteries and lithium ion polymer batteries. EXAMPLES
[0118] The present disclosure will be described in detail below with reference to examples and comparative examples. However, the present disclosure is not limited to the examples.
[0119] <Production of adhesive film for metal terminals> Example 1 Using an extruder and a T-die casting device, a polypropylene film (CPP layer (unstretched homopolypropylene layer), melting peak temperature 160°C, thickness 80μm) was extruded on one side as a polypropylene layer, a maleic anhydride modified polypropylene (r-PPa layer (maleic anhydride modified random polypropylene layer), melting peak temperature 140°C) was extruded on the other side as a first layer on the exterior material side, each with a thickness of 60μm, to obtain an adhesive film (total thickness 200μm) in which the first layer (r-PP layer, thickness 60μm) / polypropylene layer (CPP layer, thickness 80μm) / second layer (r-PPa layer, thickness 60μm) were laminated in that order.
[0120] In the adhesive films of each of the Examples and Comparative Examples, the island ratio of the sea-island structure of the polypropylene layer described below, the soft segment component ratio of the adhesive film, and the heat of fusion of the adhesive film after heating were adjusted by controlling the polyethylene content in the polypropylene film, the polymerization type (homo, block, or random), and the film formation conditions (temperature and speed during film formation, cooling temperature and speed, etc.).
[0121] Example 2 Using an extruder and a T-die casting device, a maleic anhydride-modified polypropylene (r-PPa layer (maleic anhydride-modified random polypropylene layer), melting peak temperature 140°C) was extruded to a thickness of 100 μm as the second layer on the metal terminal side onto one side of a polypropylene film (CPP layer (unstretched homopolypropylene layer), melting peak temperature 160°C, thickness 50 μm) as a polypropylene layer, and a polypropylene (r-PP layer (random polypropylene layer), melting peak temperature 140°C) was extruded to a thickness of 50 μm as the first layer on the exterior material side onto the other side, to obtain an adhesive film (total thickness 200 μm) in which the first layer (r-PP layer (random polypropylene layer), thickness 50 μm) / polypropylene layer (CPP layer, thickness 50 μm) / second layer (r-PPa layer, thickness 100 μm) were laminated in that order.
[0122] Example 3 Using an extruder and a T-die casting device, a maleic anhydride-modified polypropylene (r-PPa layer (maleic anhydride-modified random polypropylene layer), peak melting temperature 140°C) was extruded onto one side of a polypropylene film (CPP layer (unstretched homopolypropylene layer), peak melting temperature 160°C, thickness 80 μm) as a polypropylene layer, as a second layer on the metal terminal side, and a maleic anhydride-modified polypropylene (h-PPa layer (maleic anhydride-modified homopolypropylene layer), peak melting temperature 160°C) was extruded onto one side of a polypropylene film (CPP layer (unstretched homopolypropylene layer), peak melting temperature 160°C) as a third layer located between the polypropylene layer and the second layer, to thicknesses of 40 μm and 20 μm, respectively. In addition, polypropylene (r-PP layer (random polypropylene layer), melting peak temperature 140°C) was extruded to a thickness of 60 μm as the first layer on the exterior material side onto the other side of the polypropylene film as the polypropylene layer, to obtain an adhesive film (total thickness 200 μm) in which the first layer (r-PP layer, thickness 60 μm) / polypropylene layer (CPP layer, thickness 80 μm) / third layer (h-PPa layer, thickness 20 μm) / second layer (r-PPa layer, thickness 40 μm) were laminated in that order.
[0123] Example 4 Using an extruder and a T-die casting device, a maleic anhydride-modified polypropylene (r-PPa layer (maleic anhydride-modified random polypropylene layer), peak melting temperature 140°C) was extruded onto one side of a polypropylene film (CPP layer (unstretched homopolypropylene layer), peak melting temperature 160°C, thickness 80 μm) as a polypropylene layer, and a maleic anhydride-modified polypropylene (h-PPa layer (maleic anhydride-modified homopolypropylene layer), peak melting temperature 160°C) was extruded onto one side of the polypropylene film, peak melting temperature 160°C, thickness 80 μm as a second layer on the metal terminal side, and a maleic anhydride-modified polypropylene (h-PPa layer (maleic anhydride-modified homopolypropylene layer), peak melting temperature 160°C) was extruded into a thickness of 30 μm as a third layer located between the polypropylene layer and the second layer. In addition, polypropylene (r-PP layer (random polypropylene layer), melting peak temperature 140°C) was extruded to a thickness of 60 μm as the first layer on the exterior material side onto the other side of the polypropylene film as the polypropylene layer, to obtain an adhesive film (total thickness 200 μm) in which the first layer (r-PP layer, thickness 60 μm) / polypropylene layer (CPP layer, thickness 80 μm) / third layer (h-PPa layer, thickness 30 μm) / second layer (r-PPa layer, thickness 30 μm) were laminated in that order.
[0124] Example 5 Using an extruder and a T-die casting device, a polypropylene film (CPP layer (unstretched homopolypropylene layer), melting peak temperature 160°C, thickness 40μm) was extruded on one side as a polypropylene layer, a maleic anhydride modified polypropylene (r-PPa layer (maleic anhydride modified random polypropylene layer), melting peak temperature 140°C) was extruded on the other side as a first layer on the exterior material side, each with a thickness of 20μm, to obtain an adhesive film (total thickness 80μm) in which the first layer (r-PP layer, thickness 20μm) / polypropylene layer (CPP layer, thickness 40μm) / second layer (r-PPa layer, thickness 20μm) were laminated in that order.
[0125] Example 6 Using an extruder and a T-die casting device, a polypropylene film (CPP layer (unstretched homopolypropylene layer), melting peak temperature 160°C, thickness 30μm) was extruded on one side as a polypropylene layer, a maleic anhydride modified polypropylene (r-PPa layer (maleic anhydride modified random polypropylene layer), melting peak temperature 140°C) was extruded on the other side as a first layer on the exterior material side, each with a thickness of 25μm, to obtain an adhesive film (total thickness 80μm) in which the first layer (r-PP layer, thickness 25μm) / polypropylene layer (CPP layer, thickness 30μm) / second layer (r-PPa layer, thickness 25μm) were laminated in that order.
[0126] Example 7 Using an extruder and a T-die casting device, a polypropylene film (CPP layer (unstretched homopolypropylene layer), melting peak temperature 160°C, thickness 30μm) was extruded on one side of the polypropylene film as the polypropylene layer (CPP layer (unstretched homopolypropylene layer), melting peak temperature 160°C, thickness 30μm) with a maleic anhydride modified polypropylene (r-PPa layer (maleic anhydride modified random polypropylene layer), melting peak temperature 140°C) as the second layer on the metal terminal side, and on the other side with a polypropylene (r-PP layer (random polypropylene layer), melting peak temperature 140°C) as the first layer on the exterior material side, with thicknesses of 20μm and 30μm, respectively, to obtain an adhesive film (total thickness 80μm) in which the first layer (r-PP layer, thickness 30μm) / polypropylene layer (CPP layer, thickness 30μm) / second layer (r-PPa layer, thickness 20μm) were laminated in that order.
[0127] Example 8 Using multi-layer air-cooled inflation molding, a polypropylene film (PP layer) as the polypropylene layer, melting peak temperature 160°C, thickness 80μm), a maleic anhydride modified polypropylene (r-PPa layer (maleic anhydride modified random polypropylene layer), melting peak temperature 140°C, thickness 37.5μm) as the second layer on the metal terminal side, and a maleic anhydride modified polypropylene (r-PPa layer (maleic anhydride modified random polypropylene layer), melting peak temperature 140°C, thickness 37.5μm) as the first layer on the exterior material side were molded, and an adhesive film for metal terminals (total thickness 150μm) was obtained in which the first polyolefin layer (PPa layer thickness 37.5μm) / base material (PP layer thickness 80μm) / second polyolefin layer (PPa layer thickness 37.5μm) were laminated in this order.
[0128] Example 9 A polypropylene film (CPP layer (unstretched homopolypropylene layer), melting peak temperature 160°C, thickness 80 μm) was used as the polypropylene layer to prepare an adhesive film (total thickness 80 μm). The island ratio of the sea-island structure was adjusted by the amount of polyethylene added to the polypropylene layer.
[0129] Example 10 Using an extruder and a T-die casting device, a polypropylene film (CPP layer (unstretched homopolypropylene layer), melting peak temperature 160°C, thickness 80μm) was extruded on one side as a polypropylene layer, a maleic anhydride modified polypropylene (r-PPa layer (maleic anhydride modified random polypropylene layer), melting peak temperature 140°C) was extruded on the other side as a first layer on the exterior material side, each with a thickness of 60μm, to obtain an adhesive film (total thickness 200μm) in which the first layer (h-PP layer, thickness 60μm) / polypropylene layer (CPP layer, thickness 80μm) / second layer (r-PPa layer, thickness 60μm) were laminated in that order.
[0130] Example 11 Using an extruder and a T-die casting device, a polypropylene film (CPP layer (unstretched homopolypropylene layer), melting peak temperature 160°C, thickness 80μm) was extruded on one side as a polypropylene layer, maleic anhydride modified polypropylene (h-PPa layer (maleic anhydride modified homopolypropylene layer), melting peak temperature 160°C) as a second layer on the metal terminal side, and polypropylene (r-PP layer (random polypropylene layer), melting peak temperature 140°C) as a first layer on the exterior material side, each with a thickness of 60μm, to obtain an adhesive film (total thickness 200μm) in which the first layer (r-PP layer, thickness 60μm) / polypropylene layer (CPP layer, thickness 80μm) / second layer (h-PPa layer, thickness 60μm) were laminated in that order.
[0131] Example 12 Using an extruder and a T-die casting device, a polypropylene film (CPP layer (unstretched random polypropylene layer), melting peak temperature 140°C, thickness 80μm) was extruded on one side as a polypropylene layer, a maleic anhydride modified polypropylene (r-PPa layer (maleic anhydride modified random polypropylene layer), melting peak temperature 140°C) was extruded on the other side as a first layer on the exterior material side, each with a thickness of 60μm, to obtain an adhesive film (total thickness 200μm) in which the first layer (h-PP layer, thickness 60μm) / polypropylene layer (CPP layer, thickness 80μm) / second layer (r-PPa layer, thickness 60μm) were laminated in that order.
[0132] Example 13 Using an extruder and a T-die casting device, a polypropylene film (CPP layer (unstretched random polypropylene layer), melting peak temperature 140°C, thickness 80μm) was extruded on one side as a polypropylene layer, a maleic anhydride modified polypropylene (h-PPa layer (maleic anhydride modified homopolypropylene layer), melting peak temperature 160°C) was extruded on the other side as a first layer on the exterior material side, each with a thickness of 60μm, to obtain an adhesive film (total thickness 200μm) in which the first layer (r-PP layer, thickness 60μm) / polypropylene layer (CPP layer, thickness 80μm) / second layer (h-PPa layer, thickness 60μm) were laminated in that order.
[0133] Example 14 Using multi-layer air-cooled inflation molding, a polypropylene film (h-PP layer) as the polypropylene layer, melting peak temperature 160°C, thickness 30μm), a maleic anhydride modified polypropylene (r-PPa layer (maleic anhydride modified random polypropylene layer), melting peak temperature 140°C, thickness 50μm) as the second layer on the metal terminal side, and a polypropylene (r-PP layer (random polypropylene layer, melting peak temperature 140°C, thickness 20μm)) as the first layer on the exterior material side were molded, and an adhesive film for metal terminals (total thickness 100μm) was obtained in which the first polyolefin layer (PP layer, thickness 20μm) / base material (PP layer, thickness 30μm) / second polyolefin layer (PPa layer, thickness 50μm) were laminated in this order.
[0134] Comparative Example 1 Using multi-layer air-cooled inflation molding, a polypropylene film (PP layer) as a polypropylene layer, melting peak temperature 160°C, thickness 20μm), a maleic anhydride modified polypropylene (r-PPa layer (maleic anhydride modified random polypropylene layer), melting peak temperature 140°C, thickness 40μm) as a second layer on the metal terminal side, a polypropylene (r-PP layer (random polypropylene layer, melting peak temperature 140°C, thickness 35μm)), a polypropylene (r-PP layer (random polypropylene layer, melting peak temperature 140°C, thickness 20μm)) as a first layer on the exterior material side, a polypropylene (r-PP layer (random polypropylene layer, melting peak temperature 140°C, thickness 35μm))) was molded, and an adhesive film (total thickness 150μm) in which the PP layer (thickness 20μm) / PP layer (thickness 35μm) / PP layer (thickness 20μm) / PP layer (thickness 35μm) / PPa layer (thickness 40μm) was obtained.
[0135] Comparative Example 2 A polypropylene film (CPP layer (unstretched homopolypropylene layer), homopolypropylene, melting peak temperature 160°C, thickness 80 μm) was used as the polypropylene layer to form an adhesive film (total thickness 80 μm). The island ratio of the sea-island structure was adjusted by the amount of polyethylene added to the polypropylene layer.
[0136] Comparative Example 3 Using an extruder and a T-die casting device, a polypropylene film (PP layer (polypropylene layer), polypropylene, melting peak temperature 160°C, thickness 70 μm) was extruded as the polypropylene layer, and a maleic anhydride-modified polypropylene (r-PPa layer (maleic anhydride-modified random polypropylene layer), melting peak temperature 140°C) was extruded to a thickness of 70 μm as the second layer on the metal terminal side. On the other side, a polypropylene (r-PP layer (random polypropylene layer), melting peak temperature 140°C) was co-extruded to a thickness of 60 μm as the first layer on the exterior material side, to obtain an adhesive film (total thickness 200 μm) in which the first layer (r-PP layer (random polypropylene layer), thickness 60 μm) / polypropylene layer (PP layer, thickness 70 μm) / second layer (r-PPa layer, thickness 70 μm) were laminated in that order.
[0137] Comparative Example 4 Using an extruder and a T-die casting device, a polypropylene film (PP layer (homopolypropylene layer), polypropylene, melting peak temperature 160°C, thickness 60μm) was extruded as the polypropylene layer, and a maleic anhydride-modified polypropylene (r-PPa layer (maleic anhydride-modified random polypropylene layer), melting peak temperature 140°C) was extruded to a thickness of 50μm as the second layer on the metal terminal side. On the other side, a polypropylene (r-PP layer (random polypropylene layer), melting peak temperature 140°C) was extruded to a thickness of 40μm as the first layer on the exterior material side, to obtain an adhesive film (total thickness 150μm) in which the first layer (r-PP layer (random polypropylene layer), thickness 40μm) / polypropylene layer (PP layer, thickness 60μm) / second layer (r-PPa layer, thickness 50μm) were laminated in that order.
[0138] <Measurement of island ratio in sea-island structure of polypropylene layer> The island ratio of the sea-island structure of the polypropylene layer of the adhesive film was measured by the following method. When the adhesive film was composed of a single polypropylene layer, the single polypropylene layer was the object of measurement. When the adhesive film was composed of multiple layers, the polypropylene layer that did not constitute the surface of the adhesive film was the object of measurement, and the island ratio in the polypropylene layer with the smallest island ratio (specifically, the h-CPP layer or r-CPP layer in Examples 1 to 14 and Comparative Examples 2 to 4, and the h-PP layer in Comparative Example 1) is shown in Table 1.
[0139] The adhesive film was embedded in a thermosetting epoxy resin and cured. A cross section in the desired direction (parallel to TD and in the thickness direction) was prepared using a commercially available rotary microtome (LEICA UC6) and a diamond knife, and the cross section was prepared at -70°C using a cryomicrotome using liquid nitrogen. The embedded resin was stained with ruthenium tetroxide for 12 hours. Since the polypropylene expands when stained, the expanded part was trimmed with a microtome and cut in 100nm to 300nm increments in the MD direction, and when a total of 1μm to 2μm was cut, the cross section where the polypropylene layer was exposed was observed as follows. The stained cross section was observed with a field emission scanning electron microscope (Hitachi High-Technologies S-4800 TYPE1, measurement conditions: 3kV 20mA High WD6mm detector (Upper)) and images (magnification 10,000 times) were obtained. Next, image processing software capable of binarizing images (Mitani Shoji's image analysis software WinROOF (Ver7.4)) was used to binarize the island and sea parts of the sea-island structure for the image, and the ratio of the total area of the island parts (total area of island parts / area of measurement range of image) was calculated. The results are shown in Table 1. Note that in this measurement, the island parts were stained more than the sea parts, and therefore the island parts were observed to be brighter than the sea parts.
[0140] [Image processing conditions] Image processing was performed using the image analysis software ImageJ. Specifically, SEM images were acquired as digital files of grayscale images (JPEG) and processed according to the binarization procedure and parameters below, with pixels with a gradation above the threshold (bright) being output as 1 and pixels with a gradation below the threshold (dark) being output as 0, and these were defined as island and sea areas, respectively. <Binarization processing> 1. Spike noise removal (Despeckle) 2.Remove Island Contours (Remove Outliers radius=4 threshold=1 which=Bright) 3. Remove Outliers radius=4 threshold=1 which=Dark 4. Spike noise removal (Despeckle) 5. Gaussian blur along the X axis (sampling width) (threshold = 3 pixels) 6. Contrast Enhancement (saturated = 0.2) 7.Remove Outliers radius=4 threshold=1 which=Bright 8. Remove Outliers radius=4 threshold=1 which=Dark 9. Otsu's Binarization
[0141] <Measurement of the ratio of soft segment components after heating of adhesive film> The adhesive film was heated at 200°C, with a surface pressure of 0.25 MPa for 16 seconds to obtain a sample. Next, the ratio of the soft segment component of the adhesive film after heating (the ratio of the soft segment component by the Solid Echo method using pulse NMR) was measured by the following method.
[0142] The sample was introduced into a glass sample tube with a diameter of 10 mm, and the sample tube was placed in a pulse NMR device (the minispec mq20 manufactured by BRUKER) and held at 440 °C for 5 minutes, after which a free induction decay curve of 1H spin-spin relaxation was obtained by the Solid Echo method at 40 °C. The number of scans in the Solid Echo method was set to 64. The obtained decay curve was waveform-separated into three curves derived from the three components of the hard segment component, the middle segment component, and the soft segment component. The waveform separation was obtained by fitting the hard segment component to a Gaussian type function and the middle segment component and the soft segment component to an exponential type function using the analysis software "TD-NMRA (Version 4.3 Rev 0.8)" manufactured by BRUKER. The measurement points up to 0.6 msec of the relaxation curve were used for the analysis. The following equation was used for fitting. Y = A1 × exp(-(t / τ1) w1 )+A2×exp(-(t / τ2)w2 )+A3×exp(-(t / τ3) w3 ) Here, w1 to w3 are Weibull coefficients, w1 is 2, and w2 and w3 are 1. A1 is the component ratio of the hard segment component, A2 is the intermediate segment component, and A3 is the component ratio of the soft segment component, τ1 is the relaxation time of the hard segment component, τ2 is the intermediate segment component, and τ3 is the relaxation time of the soft segment component, and t is time.
[0143] <Measurement of heat of fusion of adhesive film after heating> The adhesive film was heated at a temperature of 200°C, a surface pressure of 0.25MPa, and for 16 seconds. The heat of fusion was then measured in accordance with the provisions of JIS K 7122:2012. The measurement was performed using a differential scanning calorimeter (DSC, Hitachi High-Tech differential scanning calorimeter TA7000). The measurement sample was held at -50°C for 15 minutes, then heated from -50°C to 210°C at a heating rate of 10°C / min, the first heat of fusion ΔH (J / g) was measured, and then held at 210°C for 10 minutes. Next, the temperature was lowered from 210°C to -50°C at a heating rate of 10°C / min, and held for 15 minutes. Furthermore, the temperature was raised from -50°C to 210°C at a heating rate of 10°C / min, and the second heat of fusion ΔH (J / g) was measured. The flow rate of nitrogen gas was 50ml / min. The heat of fusion ΔH (J / g) measured in the first measurement was used as the heat of fusion. The heat of fusion was defined as the area enclosed by the baseline (the line formed by connecting the start and end points of the ridge from base to base) and the peak in the DSC curve.
[0144] <Measurement of water vapor permeability of adhesive film> First, an exterior material for a power storage device (hereinafter, sometimes simply referred to as "exterior material") was prepared by the following procedure. As a base layer, a biaxially oriented polyethylene terephthalate (PET) film (thickness 12 μm) and an oriented nylon (ONy) film (thickness 15 μm) were prepared. The PET film and the ONy film were bonded using a two-liquid urethane adhesive (polyol compound and aromatic isocyanate compound), and aging treatment was performed to obtain a base layer (thickness 30 μm) in which the PET film (thickness 12 μm) / adhesive layer (thickness after curing is 3 μm) / ONy film (thickness 15 μm) were laminated from the outside in this order. In addition, an aluminum foil (JIS H4160:1994 A8021H-O (thickness 40 μm)) was prepared as a barrier layer. Next, the surface of the ONy film side of the base material layer and the barrier layer were bonded using a two-component urethane adhesive (polyol compound and aromatic isocyanate compound), and an aging treatment was performed to obtain an exterior material for an electricity storage device (total thickness 73 μm) in which a laminate of base material layer (thickness 30 μm) / adhesive layer (thickness 3 μm after curing) / barrier layer (thickness 40 μm) was laminated in that order.
[0145] Next, as shown in the schematic diagram of Figure 9, the obtained exterior material 3 was cut into a square with a length (MD) of 120 mm and a width (TD) of 120 mm (Figure 9a). In addition, two pieces of adhesive film 1 were cut into rectangles with a length (MD) of 120 mm and a width (TD) of 10 mm, and two pieces were cut into rectangles with a length (MD) of 100 mm and a width (TD) of 10 mm. On the barrier layer side of the exterior material 3, an adhesive film with the same length was placed facing along the periphery of the exterior material 3 (Figure 9b). At this time, the second layer side of the adhesive film was placed on the barrier layer side of the exterior material 3. Next, a polytetrafluoroethylene film (PTFE film, 100 μm thick) was placed on the adhesive film of the laminate (the surface of the adhesive film was covered with the PTFE film), and the silicone sheet / PTFE / laminate / PTFE / silicone sponge sheet state was placed on a press machine heated to 200°C and left for 16 seconds under a pressure of 0.25 MPa to heat-seal the adhesive film to the exterior material 3. The laminate after heat-sealing was naturally cooled to 25°C, and the PTFE film was peeled off from the laminate. This heating treatment was performed assuming the physical properties after the adhesive film was placed between the exterior material for the power storage device and the metal terminal and heat-sealed. Next, the exterior material 3 was folded in half vertically so that the adhesive film was on the inside (FIG. 9c). Two adhesive films for metal terminals with a length (MD) of 120 mm were placed between the exterior materials 3 along the long side to be heat-sealed as described below, and the adhesive film for metal terminals with a length (MD) of 100 mm was folded in half and placed between the exterior materials 3 along the short side to be heat-sealed as described below. The periphery of the exterior material 3 is a laminate in which exterior material / adhesive film / adhesive film / exterior material are layered in this order (Figure 9c).
[0146] Next, a heat seal bar (stainless steel plate) was used to heat seal the layers of the laminate at the long and short sides of the laminate, leaving one short side unheat-sealed (Fig. 9c). The conditions for heat sealing were as follows: for the long side, a 7 mm-wide heat seal bar was used, and heat sealing was performed once at a temperature of 190°C, a surface pressure of 0.5 MPa, and for 1.5 seconds (s1 in Fig. 9c). For the short side, a 7 mm-wide heat seal bar was used, and heat sealing was performed once at a temperature of 190°C, a surface pressure of 0.5 MPa, and for 1.5 seconds (s2 in Fig. 9c). The laminate was dried for one day in a dry room. Next, about 3.0 g of a liquid (moisture content 0%) of ethylene carbonate:diethyl carbonate:dimethyl carbonate = 1:1:1 (volume ratio) was injected from the position of the short side that was not heat-sealed (Figure 9d), and the short side that was not heat-sealed was also heat-sealed in the same manner as the short side described above (s3 in Figure 9e) to form a sealed bag (Figure 9e). This sealed bag was left to stand for 30 days in an environment at a temperature of 65°C and a relative humidity of 90%, and then the moisture content of the liquid removed from the sealed bag was measured by the Karl Fischer method in a dry room to obtain the moisture content (ppm). From the obtained moisture content, the amount of electrolyte injected (g), the permeation distance (mm), and the permeation cross-sectional area (m 2 ), and the number of days of storage (days), the water vapor permeability (g mm / (m 2 We asked for the number of days. Water vapor permeability (g mm / (m 2 ·day) = [obtained moisture content (ppm) × added electrolyte (g) × permeation distance (mm)] / [permeation cross-sectional area (m 2 ) × number of storage days (days)] Obtained water content (ppm): Obtained by Karl Fischer method. Electrolyte added (g): 3.0g -Transmission distance (mm): Seal width 7mm ·Transmission cross section (m 2 ): remaining thickness (μm) x seal inner circumference 200 (mm) Storage period: 30 days
[0147] <Measurement of adhesive strength between adhesive film and metal terminal> The adhesive strength between the adhesive film and the metal terminal was measured by the following procedure. The results are shown in Table 1. The adhesive strength of the adhesive film to the metal terminal was measured by the following method. The results are shown in Table 1. As the metal terminal, aluminum (JIS H4160:1994 A8079H-O) with a length of 50 mm, a width of 22.5 mm, and a thickness of 400 μm was prepared. In addition, each adhesive film for metal terminal obtained in the examples and comparative examples was cut to a length of 45 mm and a width of 10 mm. Next, the adhesive film for metal terminal was placed on the metal terminal to obtain a laminate of metal terminal / adhesive film. At this time, the vertical and horizontal directions of the metal terminal were aligned with the length and width directions of the adhesive film for metal terminal, respectively, and the metal terminal and the adhesive film for metal terminal were laminated so that the centers were aligned. In addition, the second layer of the adhesive film for metal terminal was disposed on the metal terminal side. Next, a polytetrafluoroethylene film (PTFE film, thickness 100 μm) was placed on the adhesive film for metal terminal of the laminate (the surface of the adhesive film for metal terminal was covered with the PTFE film), and the laminate was placed on a press machine heated to 200 ° C (metal terminal was on the hot plate side), and a silicone sponge sheet was placed on it, and the laminate was left standing for 16 seconds at a pressure of 0.25 MPa to heat-seal the adhesive film to the metal terminal. The laminate (pre-seal tab) after heat-sealing was naturally cooled to 25 ° C. Next, in an environment of 25 ° C, the adhesive film for metal terminal was peeled off from the metal terminal using a Tensilon universal material testing machine (RTG-1210 manufactured by A & D Co., Ltd.). Specifically, a cut was made in the center of the obtained pre-seal tab along the horizontal direction to the metal terminal, and the cut part was folded several times to cut only the metal terminal due to metal fatigue. Next, as shown in the schematic diagram of Fig. 12, the metal terminal protruding from the adhesive film was cut off on one side of the metal terminal in the longitudinal direction (x direction, MD) with the cut portion of the metal terminal (the center portion of the pre-seal tab 20) as the boundary. The part of the metal terminal that was cut is indicated by the two-dot chain line in Fig. 12. Next, as shown in Fig. 13, tape 21 was attached to the side of the pre-seal tab where the metal terminal 2 was cut. A jig 22 for fixing the pre-seal tab was attached to the other side of the pre-seal tab.The tape 21 and the jig 22 were attached to the chucks 23 of a Tensilon universal material testing machine, and the adhesive film for metal terminals was peeled off from the metal terminal by pulling the chucks in a 180° direction. The maximum strength at the time of peeling was taken as the adhesion strength to the metal terminal (N / 15 mm). The peeling speed was 50 mm / min, the peeling angle was 180°, and the distance between the chucks was 30 mm, and the average value was taken from three measurements. The results are shown in Table 1. The process of leaving the sample for 16 seconds in a heated and pressurized environment at a temperature of 200°C and a surface pressure of 0.25 MPa is a process that simulates the heat and pressure applied in the temporary adhesion process and the main adhesion process.
[0148] <Measurement of adhesive strength between adhesive film and exterior material> The adhesive strength between the adhesive film exterior material and the metal terminal was measured by the following procedure. The results are shown in Table 1. (Fabrication of exterior materials) First, an exterior material for a power storage device (hereinafter, sometimes simply referred to as "exterior material") was produced by the following procedure. A base layer (thickness 30 μm) consisting of a polyethylene terephthalate film (thickness 12 μm) / adhesive layer (thickness 3 μm) / nylon film (thickness 15 μm) was laminated on an aluminum alloy foil (thickness 40 μm) by a dry lamination method, and a heat-sealing resin layer was laminated on the other surface by co-extrusion. Specifically, a two-liquid urethane adhesive (polyol compound and aromatic isocyanate compound) was applied on the nylon film, and an adhesive layer (thickness 3 μm) was formed on the nylon film. Next, the adhesive layer and a polyethylene terephthalate film were laminated on the nylon film to produce a base layer. Next, a two-liquid urethane adhesive (polyol compound and aromatic isocyanate compound) was applied on one surface of a barrier layer consisting of an aluminum alloy foil, and an adhesive layer (thickness 3 μm) was formed on the aluminum alloy foil. Next, the adhesive layer and the substrate layer with the nylon film side as the adhesive surface were laminated on the aluminum alloy foil, and then aging treatment was performed to produce a substrate layer / adhesive layer / barrier layer laminate. Next, an adhesive layer (40 μm thick, arranged on the metal layer side) made of maleic anhydride-modified polypropylene resin and a heat-sealable resin layer (40 μm thick, innermost layer) made of random polypropylene resin were co-extruded on the barrier layer of the laminate to laminate the adhesive layer / heat-sealable resin layer on the barrier layer, thereby obtaining an exterior material for a power storage device in which the substrate layer, adhesive layer, barrier layer, adhesive layer, and heat-sealable resin layer were laminated in this order.
[0149] Next, an aluminum foil (JIS H4160:1994 A8079H-O) with MD 25 mm, TD 22.5 mm, and thickness 400 μm was prepared as the metal terminal 2. Also, each adhesive film 1 obtained in the examples and comparative examples was cut to MD 25 mm and TD 20 mm. Next, as shown in the schematic diagram of FIG. 10, a metal terminal was sandwiched between two adhesive films to obtain an adhesive film / metal terminal / adhesive film laminate. At this time, the MD and TD of the metal terminal were aligned with the length direction and width direction of the adhesive film, respectively, and the metal terminal and the adhesive film were laminated so that the centers of the metal terminal and the adhesive film were aligned (see FIG. 10(a)). Also, the second layer of the adhesive film for metal terminal is disposed on the metal terminal side. Next, the laminate was sandwiched between two polytetrafluoroethylene films (PTFE films, thickness 100 μm), and heated at a temperature of 200° C., surface pressure of 0.25 MPa, and time of 16 seconds to heat-seal the adhesive film to the metal terminal, thereby producing a metal terminal with an adhesive film (see FIG. 10(b)). At this time, as shown in the schematic diagram of FIG. 10, the metal terminal was sandwiched between the adhesive films, so that the periphery of the metal terminal was covered with the adhesive film, and a portion in which the two adhesive films were heat-sealed to each other was formed. Next, the exterior material was cut to a size of TD 60 mm and MD 200 mm, and as shown in the schematic diagram of FIG. 11, the exterior material was placed facing each other with the heat-sealable resin layer of the exterior material facing inside, and the obtained laminate was sandwiched between the opposing heat-sealable resin layers (see FIG. 11(a)). At this time, the exterior material was laminated so that the MD and TD were aligned with the width direction and length direction of the laminate, respectively. In this state, a heat seal tester was used to perform heat sealing (see the shaded area S in FIG. 11(b)) at a width of 7 mm (7 mm in the y-axis direction in FIG. 11(b)), at 200°C, with a surface pressure of 3.0 MPa, for 1.5 seconds, and the laminate was naturally cooled to 25°C, and a laminate in which the exterior material and the adhesive film were heat-sealed was obtained (see FIG. 11(b)). Next, the center of the short side direction of the obtained laminate was cut to a width of 15 mm (see the two-dot dashed line in FIG. 11(b) for the cutting position). Next, in an environment of 25°C, the adhesive film was peeled off from the heat-sealable resin layer of the exterior material using a Tensilon universal material testing machine (RTG-1210 manufactured by A&D Co., Ltd.). The maximum strength at the time of peeling was taken as the peel strength (N / 15 mm) against the exterior material.The peel speed was 20 mm / min, the peel angle was 180°, and the chuck distance was 30 mm. The average value was calculated from three measurements.
[0150] [Table 1]
[0151] In Table 1, the numerical values in the laminated structure of the adhesive film indicate the thickness (μm) of each layer.
[0152] As described above, the present disclosure provides the inventions of the following aspects. Item 1. An adhesive film for a metal terminal, which is interposed between a metal terminal electrically connected to an electrode of an electricity storage device element and an exterior material for an electricity storage device that encapsulates the electricity storage device element, The adhesive film for metal terminals includes at least a polypropylene layer, A sea-island structure is observed in a cross-sectional image of the polypropylene layer taken in a direction parallel to the TD and in a thickness direction thereof using a scanning electron microscope; An adhesive film for metal terminal, wherein the island ratio of the sea-island structure of the polypropylene layer is 20% or less. Item 2. The adhesive film for a metal terminal according to item 1, wherein the adhesive film for a metal terminal is composed of a single layer of the polypropylene layer. Item 3. The adhesive film for metal terminals is composed of multiple layers, Item 2. The adhesive film for metal terminal according to item 1, wherein the polypropylene layer is a layer that does not constitute a surface of the adhesive film for metal terminal. Item 4. The adhesive film for a metal terminal according to item 3, wherein the ratio of the thickness of the polypropylene layer to the thickness of the adhesive film for a metal terminal is 0.20 or more. Item 5. The adhesive film for a metal terminal according to any one of Items 1 to 4, wherein the polypropylene layer contains modified polypropylene. Item 6. The adhesive film for metal terminal according to any one of Items 1 to 5, wherein the adhesive film for metal terminal has a ratio of soft segment components of 20% or less, as measured by a Solid Echo method using pulse NMR in a 40°C environment after heating the adhesive film for metal terminal under conditions of a temperature of 200°C, a surface pressure of 0.25 Pa, and a time of 16 seconds. Item 7. The adhesive film for metal terminal according to any one of Items 1 to 6, wherein the heat of fusion measured after heating the adhesive film for metal terminal under conditions of a temperature of 200° C., a surface pressure of 0.25 Pa, and a time of 16 seconds is 50 J / g or more. Item 8. The adhesive film for metal terminals has a water vapor permeability of 5.10 g mm / (m 2 8. The adhesive film for metal terminal according to any one of items 1 to 7, wherein the adhesive film for metal terminal has a shelf life of 1.0 days or less. Item 9. A method for producing an adhesive film for a metal terminal, which is interposed between a metal terminal electrically connected to an electrode of an electricity storage device element and an exterior material for an electricity storage device that encapsulates the electricity storage device element, comprising: The adhesive film for metal terminals includes at least a polypropylene layer, A direction parallel to the TD and thickness direction of the polypropylene layer A sea-island structure was observed in the cross-sectional image obtained using a scanning electron microscope. A method for producing an adhesive film for a metal terminal, wherein the island ratio of the sea-island structure of the polypropylene layer is 20% or less. Item 10. A metal terminal with an adhesive film for a metal terminal, comprising the adhesive film for a metal terminal according to any one of items 1 to 8 attached to a metal terminal. Item 11. An electricity storage device including at least an electricity storage device element having a positive electrode, a negative electrode, and an electrolyte, an exterior material for an electricity storage device that seals the electricity storage device element, and metal terminals that are electrically connected to the positive electrode and the negative electrode, respectively, and protrude to the outside of the exterior material for an electricity storage device, Item 9. An electricity storage device, comprising the adhesive film for a metal terminal according to any one of items 1 to 8 interposed between the metal terminal and the exterior material for an electricity storage device. Item 12. A method for manufacturing an electricity storage device including at least an electricity storage device element including a positive electrode, a negative electrode, and an electrolyte, an exterior material for an electricity storage device that seals the electricity storage device element, and metal terminals that are electrically connected to the positive electrode and the negative electrode, respectively, and protrude to the outside of the exterior material for an electricity storage device, A method for producing an electricity storage device, comprising a step of interposing the adhesive film for metal terminal according to any one of items 1 to 8 between the metal terminal and the exterior material for an electricity storage device, and sealing the electricity storage device element with the exterior material for an electricity storage device. Item 13. An exterior material for an electricity storage device for use in an electricity storage device, The electricity storage device includes at least an electricity storage device element having a positive electrode, a negative electrode, and an electrolyte, the electricity storage device exterior material sealing the electricity storage device element, and the metal terminals electrically connected to the positive electrode and the negative electrode, respectively, and protruding to the outside of the electricity storage device exterior material, and an adhesive film for metal terminals is interposed between the metal terminals and the electricity storage device exterior material, The adhesive film for a metal terminal is an adhesive film for a metal terminal according to any one of items 1 to 8, The electrical storage device packaging material is composed of a laminate including at least a base layer, a barrier layer, and a heat-sealable resin layer. Item 14. A kit comprising an exterior material for an electricity storage device for use in an electricity storage device and the adhesive film for a metal terminal according to any one of items 1 to 8, The electricity storage device includes at least an electricity storage device element having a positive electrode, a negative electrode, and an electrolyte, the electricity storage device exterior material sealing the electricity storage device element, and the metal terminals electrically connected to the positive electrode and the negative electrode, respectively, and protruding to the outside of the electricity storage device exterior material, The kit is used such that, when used, the adhesive film for a metal terminal is interposed between the metal terminal and the exterior material for an electricity storage device. [Explanation of symbols]
[0153] 1. Adhesive film for metal terminals 2 metal terminals 3. Exterior materials for energy storage devices 3a Periphery of exterior material for power storage device 4. Energy storage device elements 10. Energy storage devices 11 Polypropylene layer 12a 1st layer 12b 2nd layer 12c 3rd layer 31 Base material layer 32 Adhesive layer 33 Barrier Layer 34 Adhesive layer 35 Heat-fusible resin layer
Claims
[Claim 1] An adhesive film for a metal terminal, which is interposed between a metal terminal electrically connected to an electrode of an electricity storage device element and an exterior material for an electricity storage device that encapsulates the electricity storage device element, The adhesive film for metal terminals includes at least a polypropylene layer, A sea-island structure is observed in a cross-section image of the polypropylene layer taken in a direction parallel to the TD and in the thickness direction, the cross-section image being obtained using a scanning electron microscope; An adhesive film for metal terminals, wherein the island ratio of the sea-island structure of the polypropylene layer is 20% or less.
Citation Information
Patent Citations
Terminal with adhesive tape, method of manufacturing terminal with adhesive tape, and thin battery