Composite spun yarn for fiber-reinforced thermoplastic plastic and molded body manufacturing method using the same
The composite spun yarn with a core-sheath structure addresses the issues of yarn slippage and poor moldability in fiber-reinforced thermoplastics by ensuring uniform resin penetration and improved binding, resulting in high-strength, uniformly integrated molded products.
Patent Information
- Application Number
- JP2023064679
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-25
AI Technical Summary
Existing fiber-reinforced thermoplastics using long reinforcing fibers face issues with yarn slippage, fuzzing, and poor moldability due to insufficient binding and uneven penetration of thermoplastic resin, leading to reduced strength and uniformity in molded products.
A composite spun yarn with a core-sheath structure is developed, where thermoplastic long fibers are wound around a substantially untwisted fiber bundle composed of continuous reinforcing fibers and short thermoplastic fibers, ensuring uniform penetration of the resin and improved binding, thereby enhancing moldability and strength.
The composite spun yarn achieves uniform integration of reinforcing fibers and thermoplastic resin, resulting in molded products with high strength, good moldability, and consistent physical properties by preventing yarn slippage and fluffing, and reducing stress concentration.
Smart Images

Figure 2024151410000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a conjugate spun yarn for fiber-reinforced thermoplastics, which is composed of continuous reinforcing fibers and thermoplastic fibers, and a method for producing a molded article using the same. [Background technology]
[0002] Traditionally, metals have been used as materials for constructing articles that require light weight and strength, such as automobiles, airplanes, and prosthetic limbs, but recently metals have been replaced by fiber-reinforced plastics (FRPs) that use a mixture of carbon fiber and glass fiber, which are particularly excellent in terms of light weight, high rigidity, high strength, and durability. The reinforcing fibers used in FRP come in the form of long fiber, short fiber, whiskers, etc., and thermosetting resins such as epoxy resins are the mainstream for matrix resins, although thermoplastic resins such as nylon and polyphenylene ether are also used in some cases.
[0003] When a thermoplastic resin is used as the matrix, short fibers are mainly used as the reinforcing fibers and the product is manufactured by the injection molding method. However, since the length of the reinforcing fibers is short, the rigidity and strength are low, and in order to compensate for this, the wall thickness is increased, which increases the weight.
[0004] In recent years, some fiber-reinforced thermoplastics (FRTPs) have been seen, which use long fibers as reinforcing fibers. Reflecting the properties of the long fibers, FRTPs are expected to exhibit properties such as impact resistance and vibration damping that could not be achieved by conventional FRPs using short fibers. For example, Patent Document 1 proposes an FRTP in which reinforcing long fibers and thermoplastic long fibers that serve as matrix resins are aligned. However, this FRTP is simply a yarn made by doubling the reinforcing long fibers and thermoplastic fibers with each other, and the reinforcing long fibers are exposed to the surface, which causes the reinforcing long fibers to break during spinning, making it difficult to handle.
[0005] In order to prevent the reinforcing long fibers from appearing on the surface of the composite spun yarn, for example, Patent Documents 2 and 3 propose a composite spun yarn in which the reinforcing long fibers are covered with slit yarns of a thermoplastic resin film. However, the method of covering with slit yarns has the disadvantage that when the reinforcing long fibers are carbon fibers or glass fibers, the slit yarns are easily slippery with respect to the reinforcing long fibers, the fiber bundles are insufficiently bound, and when the fiber bundles are curved, the yarns are displaced and rub against each other, which makes the fiber bundles prone to fluffing. In addition, excessive force is easily applied to the fiber bundles during covering, which may cause the fiber bundles to break. Furthermore, the composite spun yarns covered with slit yarns are very hard, which makes them difficult to handle. Furthermore, in a composite spun yarn in which a reinforcing long fiber is coated with a slit yarn of a thermoplastic resin film as in Patent Documents 2 and 3, when the composite spun yarn is heated to melt the slit yarn to produce a molded body, the thermoplastic resin of the molten slit yarn does not easily penetrate between the monofilaments of the reinforcing long fiber that constitutes the core, resulting in problems such as poor moldability and poor strength of the obtained molded body. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 60-56545 [Patent Document 2] Japanese Patent Application Publication No. 60-28543 [Patent Document 3] WO2009 / 131149 publication Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been devised to solve the problems of the prior art described above, and its object is to provide a composite spun yarn for fiber-reinforced thermoplastics, which has sufficient fiber bundle binding, is less prone to yarn slippage and fuzzing, and further, which allows molten thermoplastic resin to easily penetrate between the single fibers of the reinforcing long fibers (continuous reinforcing fibers) that make up the core when producing a molded article, has good moldability, and produces molded articles with high strength, and a method for producing molded articles using the same. [Means for solving the problem]
[0008] As a result of intensive research into achieving the above-mentioned object, the present inventors have found that by forming a conjugate spun yarn in which a thermoplastic long fiber is wound around a fiber bundle having a core-sheath structure formed from a core made of continuous reinforcing fiber and a sheath made of thermoplastic short fiber, the thermoplastic resin of the wound long fiber tightly binds the fiber bundle, making it possible to reduce yarn slippage and fluffing, and that when such conjugate spun yarn is filled in a mold and the thermoplastic short fiber and thermoplastic long fiber are heated and melted, the thermoplastic resin of the short fiber in the sheath portion sufficiently permeates between the monofilaments of the continuous reinforcing fiber in the core of the fiber bundle, thereby obtaining a molded product with uniform physical properties that are excellent in moldability and strength, and further that this permeation of the thermoplastic resin can be carried out even more rapidly and uniformly by making the fiber bundle substantially untwisted, which has led to the completion of the present invention.
[0009] That is, the present invention has the following configurations (1) to (6). (1) A composite spun yarn for fiber-reinforced thermoplastics, characterized in that a thermoplastic long fiber is wound around a substantially untwisted fiber bundle formed from a core made of continuous reinforcing fiber and a sheath made of thermoplastic short fiber. (2) A composite spun yarn for fiber-reinforced thermoplastics according to (1), characterized in that each of the thermoplastic short fiber and the thermoplastic long fiber is a fiber made of at least one thermoplastic resin selected from the group consisting of polyamide, polypropylene, polyphenylene sulfide, polyetherimide, and phenoxy. (3) A composite spun yarn for fiber-reinforced thermoplastics according to (1), characterized in that the continuous reinforcing fiber is at least one type of fiber selected from the group consisting of carbon fiber, glass fiber, basalt fiber, PBO fiber, and aramid fiber, and the mixing ratio of the continuous reinforcing fiber is 20 to 80 mass%. (4) A conjugate spun yarn for fiber reinforced thermoplastics according to (1), characterized in that the conjugate spun yarn has a total fineness of 200 to 500,000 dtex. (5) A conjugate spun yarn for fiber reinforced thermoplastics according to (1), characterized in that the thermoplastic long fiber is wound around a substantially untwisted fiber bundle with a twist number of 1 to 1000 T / m. (6) A method for producing a molded product, comprising filling a mold with the conjugate spun yarn for fiber-reinforced thermoplastics according to any one of (1) to (5) at a filling rate of 100 to 350%, and heating the mold at a temperature higher than the higher of the melting points of the thermoplastic short fibers and the thermoplastic long fibers to melt the thermoplastic short fibers and the thermoplastic long fibers. Effect of the Invention
[0010] The composite spun yarn for fiber-reinforced thermoplastics of the present invention has a continuous reinforcing fiber as a core, and the thermoplastic short fiber that becomes the matrix resin when made into FRTP is wrapped around the core to form a fiber bundle with a core-sheath structure in which the thermoplastic short fiber is directly wrapped around the continuous reinforcing fiber, and further, the thermoplastic long fiber is wrapped around the fiber bundle to bind it, so that the contact area between the continuous reinforcing fiber and the thermoplastic resin around it can be increased. Therefore, when it is heated to a temperature higher than the melting point of the thermoplastic resin that forms the two types of long and short thermoplastic fibers and melted, the molten thermoplastic resin sufficiently penetrates between the single fibers of the continuous reinforcing fiber, and the continuous reinforcing fiber and the thermoplastic resin can be uniformly integrated. As a result, a fiber-reinforced plastic molded body with good moldability, high strength, and uniform physical properties can be easily obtained.
[0011] Furthermore, in the composite spun yarn for fiber-reinforced thermoplastics of the present invention, since the continuous reinforcing fibers and the thermoplastic short fibers are not substantially twisted, the thermoplastic resin can penetrate between the monofilaments of the continuous reinforcing fibers more quickly and uniformly. In addition, the load on the continuous reinforcing fibers due to the twisting is reduced, and uneven stress concentration can be prevented when tension is applied, resulting in a uniform increase in the strength of the resulting fiber-reinforced plastic molding. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic perspective view of an example of the conjugate spun yarn for fiber-reinforced thermoplastics of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of an example of an apparatus for producing a composite spun yarn for fiber-reinforced thermoplastics according to the present invention. [Diagram 3] FIG. 3 is a photograph of a woven prepreg showing an application example of the present invention. [Figure 4] FIG. 4 is a cross-sectional photograph showing the state of impregnation of the thermoplastic resin in the conjugate spun yarn of Example 2. [Diagram 5] FIG. 5 is a cross-sectional photograph showing the state of impregnation of the thermoplastic resin in the conjugate spun yarn of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The composite spun yarn for fiber-reinforced thermoplastics of the present invention is characterized in that a thermoplastic long fiber is wound around a substantially untwisted fiber bundle formed from a core made of continuous reinforcing fibers and a sheath made of thermoplastic short fibers. In the composite spun yarn of the present invention, the thermoplastic short fibers are directly coated around the core made of continuous reinforcing fibers, so that when heated and melted, the resin derived from the molten thermoplastic short fibers easily penetrates between the single fibers of the continuous reinforcing fibers that constitute the core. Furthermore, since the fiber bundle, i.e., the continuous reinforcing fibers and the thermoplastic short fibers, are not substantially twisted, the thermoplastic short fibers can be melted by heating in a state in which the fibers are aligned in the yarn axis direction, and as a result, the thermoplastic resin that constitutes the thermoplastic fibers quickly and uniformly penetrates the continuous reinforcing fiber bundle, and the composite integration can be efficiently performed. In addition, the obtained molded body has few voids and small variation in strength.
[0014] The continuous reinforcing fiber used in the composite spun yarn of the present invention is a reinforcing fiber that extends continuously in the length direction, and is synonymous with "long reinforcing fiber". As the continuous reinforcing fiber used in the composite spun yarn of the present invention, it is preferable to use a high-strength fiber having a tensile strength of 1000 MPa or more and a tensile modulus of elasticity of 30 GPa or more. Since such high-strength fibers are very difficult to bend, it is difficult to stably produce a uniform spun yarn by the conventional spinning methods such as those described in Patent Documents 1 to 3, but it is possible to produce the composite spun yarn of the present invention without any problems. Examples of continuous reinforcing fibers include carbon fiber, glass fiber, aramid fiber, polyparaphenylene benzobisoxazole fiber (PBO fiber), phenol fiber, metal fiber, aramid fiber, and ceramic fiber. In the present invention, it is preferable to use at least one type of fiber selected from the group consisting of carbon fiber, glass fiber, basalt fiber, PBO fiber, and aramid fiber. More preferably, it is carbon fiber or glass fiber, and even more preferably, it is carbon fiber. Carbon fiber is preferable because it has excellent specific strength and specific modulus and excellent water absorption resistance.
[0015] The blending ratio of the continuous reinforcing fibers in the composite spun yarn of the present invention is preferably 15 to 80% by mass, more preferably 20 to 75% by mass, and even more preferably 30 to 70% by mass. If the blending ratio is less than the above range, the strength improving effect of the reinforcing fibers is likely to decrease. If the blending ratio exceeds the above range, the coverage of the thermoplastic fibers becomes too low, and voids are likely to occur.
[0016] The single yarn fineness (single fiber fineness) of the continuous reinforcing fibers is preferably 0.3 to 10 dtex, more preferably 0.5 to 5 dtex. The total fineness of the continuous reinforcing fibers is preferably 500 to 50,000 dtex, more preferably 650 to 40,000 dtex. The number of filaments is preferably 700 to 70,000, more preferably 900 to 60,000. A fineness within this range is easy to handle as a reinforcing fiber for FRTP. The continuous reinforcing fibers are preferably substantially untwisted, and even if there is a small amount of twist, the number of twists is preferably 10 times / inch or less, more preferably 5 times / inch or less. If the number of twists exceeds the above range, the permeability of the thermoplastic resin that becomes the matrix is likely to decrease.
[0017] The strength of the continuous reinforcing fibers is preferably 1000 to 8000 MPa. More preferably, it is 2000 MPa or more. If the strength is below the above range, it becomes difficult for the molded FRTP to maintain sufficient strength. If it exceeds the above range, it becomes difficult to stably produce the composite spun yarn.
[0018] The thermoplastic short fibers used in the composite spun yarn of the present invention are preferably made of a thermoplastic resin that is usually used as a matrix resin for FRTP and has a melting point lower than the decomposition temperature of the continuous reinforcing fibers. For example, when carbon fibers are used as the continuous reinforcing fibers, the thermoplastic short fibers are preferably short fibers made of a resin having a melting point or glass transition temperature of 300°C or lower. The thermoplastic short fibers are preferably short fibers made of at least one thermoplastic resin selected from polyamide, polypropylene, polyphenylene sulfide, polyetherimide, polyethersulfone, polyketone, polyetheretherketone, phenol, polysulfone, polyphenylene ether, polyimide, polyamideimide, and phenoxy. In particular, the thermoplastic short fibers are preferably short fibers made of at least one thermoplastic resin selected from the group consisting of polyamide, polypropylene, polyphenylene sulfide, polyetherimide, and phenoxy.
[0019] The single fiber fineness of the thermoplastic short fiber is preferably 0.3 to 5 dtex, more preferably 0.5 to 3.0 dtex, and even more preferably 0.8 to 2.0 dtex. If the single fiber fineness is smaller than the above range, spinnability is likely to decrease. If it is thicker than the above range, the fiber bundle becomes too stiff, making it difficult to stably produce a composite spun yarn. The fiber length of the thermoplastic short fiber is preferably 25 to 70 mm, more preferably 30 to 60 mm, and even more preferably 32 to 55 mm. If the fiber length is outside the above range, uniform spinning becomes difficult.
[0020] The composite spun yarn of the present invention is in the form of a fiber bundle in which continuous reinforcing fibers and thermoplastic short fibers are mixed substantially without twisting, and has a core-sheath structure in which the continuous reinforcing fibers are present on the inside of the fiber bundle cross section as the core, and the thermoplastic short fibers are present on the outer periphery of the fiber bundle cross section as the sheath. In this core-sheath structure, the thermoplastic short fibers are present on the outer periphery of the fiber bundle cross section, but it is sufficient that the thermoplastic short fibers cover most of the continuous reinforcing fibers, and they do not have to cover them completely. In addition, the core-sheath structure of the present invention also includes cases in which further thermoplastic fibers are present on the inside of the continuous reinforcing fibers that are the core, or in which the continuous reinforcing fibers are mixed with the thermoplastic fibers in the core.
[0021] In this way, by forming a core-sheath structure of a fiber bundle with substantially no twist, the thermoplastic short fibers are sufficiently covered with the continuous reinforcing fibers, and when the thermoplastic short fibers are melted by heating to form a matrix resin, the matrix resin can be sufficiently and uniformly infiltrated into the continuous reinforcing fibers, the occurrence of voids can be suppressed, and the variation in strength can be reduced. In the present invention, "substantially no twist" means that the twist is so loose that the convergence of the fiber bundle cannot be maintained when the thermoplastic long fibers are removed from the composite spun yarn. Specifically, when the composite fiber is attached to a twist detector and both ends of the composite spun yarn are held, the thermoplastic long fibers are removed to leave only the fiber bundle, and the center of the fiber bundle is pinched with tweezers and squeezed in the fiber axial direction, the short fibers in the sheath part of the fiber bundle are pulled out of the long fibers in the core part of the fiber bundle, and the fiber bundle cannot be maintained.
[0022] The mixing ratio of the continuous reinforcing fibers in the fiber bundle is preferably 20 to 90% by mass, and more preferably 20 to 70% by mass. If the mixing ratio of the continuous reinforcing fibers is less than the above range, the strength improving effect of the reinforcing fibers is likely to decrease. If the mixing ratio exceeds the above range, the coverage of the thermoplastic fibers becomes too low, and voids are likely to occur.
[0023] In the composite spun yarn of the present invention, the core-sheath structure is made of fiber bundles that are substantially untwisted, and thus the yarn can be spun stably. If the fiber bundles of the core-sheath structure are twisted, the continuous reinforcing fiber bundles are exposed to the surface of the composite spun yarn, reducing the covering property, and the rigidity of the continuous reinforcing fibers causes the composite spun yarn to untwist, making it difficult to stably spin the yarn and to produce a composite spun yarn with stable quality. In contrast, the composite spun yarn of the present invention has a core-sheath structure with fiber bundles that are substantially untwisted, and thus the above problems do not occur, making it easy to stably spin the yarn.
[0024] The fiber bundle of the composite spun yarn of the present invention is substantially untwisted and therefore easily falls apart. Therefore, in the present invention, the thermoplastic long fiber is wound around the fiber bundle as a pressing thread (a thread for binding the fiber bundle) to prevent the fiber bundle from falling apart. The thermoplastic long fiber is preferably made of a thermoplastic resin that is usually used as a matrix resin for FRTP and has a melting point lower than the decomposition temperature of the continuous reinforcing fiber. For example, when carbon fiber is used as the continuous reinforcing fiber, the thermoplastic long fiber is preferably made of a resin having a melting point or glass transition temperature of 300°C or lower. The thermoplastic long fiber is preferably made of at least one thermoplastic resin selected from polyamide, polypropylene, polyphenylene sulfide, polyetherimide, polyethersulfone, polyketone, polyetheretherketone, phenol, polysulfone, polyphenylene ether, polyimide, polyamideimide, and phenoxy. In particular, the thermoplastic long fiber is preferably made of at least one thermoplastic resin selected from the group consisting of polyamide, polypropylene, polyphenylene sulfide, polyetherimide, and phenoxy. The thermoplastic short fibers and thermoplastic long fibers described above may be made of different types of thermoplastic resins, but when recycling FRTP, they are preferably made of the same type of thermoplastic resin.
[0025] The total fineness of the thermoplastic long fibers is preferably 10 to 1000 dtex. More preferably, it is 30 to 800 dtex. If the total fineness is smaller than the above range, the binding of the composite spun yarn may be weak and easily fluffed, or the long fibers may break due to friction and the yarn may come off. If the total fineness is larger than the above range, the fiber bundles consisting of the continuous reinforcing fibers and the thermoplastic short fibers may be twisted when bundling them with the thermoplastic long fibers, making stable production difficult. The single fiber fineness of the thermoplastic long fibers is preferably 0.1 to 10 dtex. More preferably, it is 0.5 to 5.0 dtex, and even more preferably, it is 0.8 to 3.0 dtex. If the single fiber fineness is smaller than the above range, the single fibers may be broken and easily fluffed during the process until the molded body is produced, and the process passability may be reduced. If the total fineness is larger than the above range, the long fibers may be too hard, and when bundling the fiber bundles with the long fibers, the fiber bundles may be twisted, making stable production difficult.
[0026] The bundling twist number of the thermoplastic long fiber is preferably 1 to 1000 T / m, more preferably 30 to 800 T / m, and even more preferably 50 to 500 T / m. If the bundling twist number is less than the above range, the bundling force is weak and the fiber bundle is likely to come loose. If it exceeds the above range, the fiber bundle is too tightly fastened, making it difficult to stably produce the composite yarn. The twist direction when winding the fiber bundle may be either the S direction or the Z direction.
[0027] The total fineness of the composite spun yarn of the present invention is preferably 200 to 500,000 dtex, more preferably 500 to 150,000 dtex, and even more preferably 700 to 100,000 dtex. If the total fineness is less than the above range, it is likely to be difficult to produce a uniform spun yarn. If it exceeds the above range, a special device will be required to produce the composite yarn of the present invention, and there is a concern that the production cost will increase.
[0028] Next, the conjugate spun yarn of the present invention will be described with reference to the drawings. FIG. 1 is a perspective view of an example of the conjugate spun yarn of the present invention. As can be seen from FIG. 1, the conjugate spun yarn 1 is in the form of a conjugate spun yarn in which a thermoplastic long fiber 5 is wound around a fiber bundle 4 having a core-sheath structure composed of a continuous reinforcing fiber 2 that forms the core and a thermoplastic short fiber 3 that covers the continuous reinforcing fiber 2 and forms the sheath. FIG. 1 shows an example in which the thermoplastic long fiber 5 is wound around the fiber bundle 4 in an S twist. The thermoplastic short fiber 3 and the thermoplastic long fiber 5 are melted by heating when forming the FRTP to become a matrix resin.
[0029] Next, an example of a method for producing a composite spun yarn of the present invention will be described with reference to FIG. 2. FIG. 2 is a schematic diagram of an example of a manufacturing apparatus for a composite spun yarn of the present invention. As can be seen from FIG. 2, first, a continuous reinforcing fiber 2 is supplied as a core yarn. A thermoplastic short fiber 3 to be a sheath portion is drafted by a draft device 6 and then supplied. Next, the continuous reinforcing fiber 2 of the core yarn and the drafted thermoplastic short fiber 3 are combined through a guide 7 to form a fiber bundle 4 having a core-sheath structure. This fiber bundle 4 is substantially untwisted. After that, the fiber bundle 4 is wound with a thermoplastic long fiber 5 drawn out from a hollow bobbin 8 to bind the fiber bundle, and a composite spun yarn 1 is produced. The composite spun yarn 1 passes through a feed roller 9 and is wound on a winding package to produce a cheese 10 of a composite spun yarn.
[0030] The coverage of the core of the fiber bundle of the composite spun yarn of the present invention by the sheath is preferably 89 to 100%, more preferably 93% or more, and even more preferably 95% or more. If the coverage is low, voids are likely to occur when the fiber bundle is molded into a molded article such as a prepreg, and the strength of the prepreg is likely to vary greatly.
[0031] The strength of the core of the fiber bundle in the composite spun yarn of the present invention is preferably 500 to 8000 MPa, and more preferably 1300 to 7000 MPa. The strength of the core depends on the physical properties of the continuous reinforcing fibers, but in the present invention, the continuous reinforcing fibers are substantially not twisted and are converged, resulting in a yarn form that allows the continuous reinforcing fibers to easily exert their inherent strength.
[0032] The composite spun yarn of the present invention can be formed into an FRTP by arranging the yarn itself by a roving method or the like, or can be formed into a woven fabric, knitted fabric, multiaxial insertion warp knitted fabric, or braided fabric to be used as an intermediate for fiber reinforced resin. These intermediates can also be made into prepregs for use in final molded products. The composite spun yarns arranged, woven fabrics, knitted fabrics, and multiaxial insertion warp knitted fabrics can be formed into sheets or tapes for use, and braided fabrics can be formed into pipes for use. Any known structure can be used for the woven fabric and knitted fabric.
[0033] Such a molded product can be produced by filling the composite spun yarn of the present invention into a mold, heating the mold at a temperature higher than the higher melting point of the thermoplastic short fiber and the thermoplastic long fiber (glass transition temperature in the case of a resin without a melting point) to melt the thermoplastic short fiber and the thermoplastic long fiber. The heating temperature is preferably lower than the decomposition temperature of the continuous reinforcing fiber. Considering the permeability of the thermoplastic resin into the continuous reinforcing fiber, it is preferable to heat and melt the thermoplastic short fiber and the thermoplastic long fiber at a temperature 15°C to 300°C higher than the higher melting point of the thermoplastic short fiber and the thermoplastic long fiber for molding. For example, when the same nylon 6 fiber is used as the thermoplastic long fiber and the thermoplastic short fiber, the mold temperature is preferably about 220 to 300°C. The filling rate into the mold is preferably 100 to 350%, and more preferably 105 to 200%.
[0034] The above-mentioned molded body can be produced by a conventionally known molding method, such as a hot stamping method, a prepreg molding method, an SMC molding method, etc. Also, it may be molded by a film stacking method in which a thermoplastic resin film is melted and compressed.
[0035] The composite spun yarn of the present invention can be used as a fiber-reinforced intermediate for woven fabric, which can then be layered and hot-pressed to form a prepreg. Figure 3 shows a photograph of a prepreg produced by weaving the composite spun yarn of the present invention into fabric, layering multiple sheets of the fabric, and pressing them together.
[0036] The prepreg made with the composite spun yarn of the present invention can have a uniform and excellent appearance. As shown in Figure 3, there is no disturbance of the continuous reinforcing fibers due to the flow of the resin during molding. The surface of a conventionally molded prepreg tends to be of poor quality due to the occurrence of many irregularities caused by voids in areas where the matrix resin has not penetrated sufficiently, but when the composite spun yarn of the present invention is used, the matrix resin penetrates sufficiently and uniformly with few voids, making it possible to make the surface of the prepreg smooth.
[0037] The prepreg produced as described above from the composite spun yarn of the present invention can achieve a tensile strength of 150 to 1000 MPa, a tensile modulus of 20 to 100 GPa, a bending strength of 150 to 1000 MPa, and a bending modulus of 15 to 80 GPa.
[0038] The prepreg made from the composite spun yarn of the present invention as described above has a small void ratio, which is an index of the amount of voids, even if the fiber volume content (Vf) is high. Specifically, the Vf is 20 to 80%, and the void ratio of the woven fabric cross section is 1.0% or less, or even 0.8% or less, and furthermore, no voids are observed at all. EXAMPLES
[0039] The effects of the present invention will be specifically described below based on examples, but the present invention is not limited to these. The methods for measuring the respective characteristic values in the present invention are as follows.
[0040] (1) Total fineness of long fibers and single yarn fineness The total fineness was measured by the fineness (total fineness) A method according to JIS-L1013-8.3 and converted into decitex (dtex). The number of filaments was measured according to JIS-L1013-8.4, and the single yarn fineness (dpf) was calculated by dividing the total fineness by the number of filaments.
[0041] (2) Single fiber fineness of staple fibers The single yarn fineness (single fiber fineness) was determined based on JIS-L1015-8.5.1 Correct Fineness Method A.
[0042] (3) Confirmation that the fiber bundle is substantially untwisted The composite spun yarn was attached to a twist detector and both ends of the composite spun yarn were gripped, then a needle was inserted between the fiber bundle and the thermoplastic long fiber, and the thermoplastic long fiber was carefully removed using tweezers and scissors while untwisting it to the extent that the thermoplastic long fiber was loosened. The fiber bundle was then twisted by the amount that was untwisted. When the center of the fiber bundle was pinched with tweezers and squeezed in the fiber axial direction, if the thermoplastic short fiber moved from the fiber bundle in accordance with the movement of the tweezers, it was judged to be substantially untwisted. This is a state in which the fiber bundle cannot be maintained.
[0043] (4) The number of twists of the thermoplastic long fiber wrapped around the fiber bundle The number of twists was determined according to JIS-L1095-9.15.1 Method A. Specifically, the composite spun yarn was attached to a twist detector, and a needle was inserted between the fiber bundle and the thermoplastic long fiber to untwist it. The number of twists at which the fiber bundle and the thermoplastic long fiber were separated was defined as the bundling twist.
[0044] (5) Volume fraction of continuous reinforcing fibers in composite spun yarn (Vf') The volume content Vf' (%) of the continuous reinforcing fibers in the composite spun yarn was calculated using the following formula. Vf'=(Tf / ρf) / (Tf / ρf+Tr / ρr)×100 Tf: Continuous reinforcing fiber fineness (dtex) Tr: Thermoplastic fiber (short fiber + long fiber) fineness (dtex) ρf: Specific gravity of continuous reinforcing fiber (g / cm 3 ) ρr: Specific gravity of thermoplastic fiber (short fiber + long fiber) (g / cm 3 )
[0045] (6) Coverage of the core Photographs of the side of the yarn were taken 10 times in a continuous manner so that a 1.5 cm long composite spun yarn was included, and a continuous photograph of a length of 15 cm was taken. From the photographs enlarged 10 times, the area of the entire side of the composite spun yarn (total area) and the area of the part not covered with thermoplastic fiber (uncovered area) were measured over a 15 cm yarn length range, and the coverage rate was calculated using the following formula. Photographs were taken at five random locations, and the arithmetic average of the coverage rates of the core at the five locations was used as the coverage rate of the core. Core coverage rate (%) = ((total area - uncovered area) / total area) x 100
[0046] (7) Tensile strength of composite spun yarn (i) Preparation of test specimens A 250 mm long composite spun yarn was used as a test specimen, and 50 mm of the coated fiber bundle was removed from both ends. Tabs 50 mm long and 20 mm wide were attached to both ends with epoxy adhesive, with a tab distance of 150 mm. (ii) Tensile strength measurement Using the obtained test pieces, a tensile test was performed at 23°C and 50% humidity with a gripping distance of 135 mm and a speed of 2 mm / min to measure the tensile strength. The test machine used was Shimadzu Corporation's "Autograph AGS-X 1kN." The average value of the measured values obtained (n=3) was used as the tensile strength.
[0047] (8) Spinning stability The spinnability was judged according to the following criteria. ○: Spinning is stable, and the continuous reinforcing fibers are not exposed on the surface of the composite spun yarn. ×: Spinning is unstable, and the continuous reinforcing fibers are exposed on the surface of the composite spun yarn.
[0048] (9) Filling rate The filling rate was calculated using the following formula. Filling rate (%)=W / (V×(d1×Vf' / 100+d2×(1-Vf' / 100)) W: Weight of composite material actually filled during molding (g) V: Volume of prepreg to be obtained (cm 3 ) Vf': Mixing ratio by volume of continuous reinforcing fibers and thermoplastic fibers (short fibers + long fibers) (vol%) d1: Specific gravity of continuous reinforcing fiber (g / cm 3 ) d2: Specific gravity of thermoplastic fiber (short fiber + long fiber) (g / cm 3 )
[0049] (10) Prepreg appearance (i) Appearance 1: Disorder of continuous reinforcing fibers ○: No or almost no disturbance of the continuous reinforcing fibers is observed ×: Disorder of continuous reinforcing fibers is noticeable (ii) Appearance 2: Surface irregularities ○: No or almost no irregularities are observed on the prepreg surface ×: The prepreg surface is uneven.
[0050] (11) Fiber volume fraction of prepreg (Vf) Measurement was performed according to the sulfuric acid decomposition method specified in JIS-K7075. After measuring the mass W0 of the prepreg test piece, the test piece was heated in 30 ml of concentrated sulfuric acid until it started to smoke (approximately 220°C), and the resin was dissolved. The fibers were separated and filtered using a glass filter (mass W1) and washed. The glass filter was then placed in a hot air dryer and dried at 105°C for 90 minutes. After drying, the test piece was allowed to cool. The mass W2 of the test piece together with the glass filter was then measured, and the fiber volume content Vf was calculated using the following formula. Fiber volume fraction Vf(%)=((W2-W1) / W0)ρr / ρf W0: Mass of test piece before sulfuric acid decomposition (g) W1: Mass of the glass filter (g) W2: Mass of carbon fiber and glass filter in the test piece after sulfuric acid decomposition (g) ρf: Density of continuous reinforcing fibers (g / cm 3 ) ρr: Density of thermoplastic resin (short fiber + long fiber) (g / cm 3 )
[0051] (12) Void ratio (Vv) The thickness direction cross section of the prepreg test piece was observed as follows. A sample was prepared by punching out the prepreg to 15 mm x 15 mm so that the cut sides were aligned with the warp and weft yarns, and embedded in epoxy resin. The sample was polished until the thickness direction cross section of the prepreg could be observed well. The polished sample was photographed at a magnification of 50 times using a high-grade inverted metallurgical microscope GX71 / DP73 microscope digital camera (manufactured by Olympus). The photographed range was 1.5 mm in the thickness direction of the prepreg x 2.0 mm in the weft direction (direction in which the warp cross section is observed). In the photographed image, the area of the entire observation surface and the area of the portion that was a void were obtained, and the void ratio was calculated using the following formula, and the average of five points was adopted as the void ratio. Cavity rate (%) = 100 × (total area of cavity) / (total area of observation surface)
[0052] (13) Bending strength and bending modulus of prepreg Measurements were performed according to the test piece dimensions and test methods specified in JIS-K7074. (i) Preparation of test specimens A test piece having a length of 100 mm and a width of 15 mm was cut out from the obtained prepreg in the direction parallel to the fiber direction (0°). (ii) Measurement of bending strength and bending modulus The cut specimens were used to measure strength and elastic modulus by performing compression tests at a speed of 5mm / min with a support distance of 80mm in an environment of 23℃ and 50% humidity. The test machine used was Shimadzu Corporation's "Autograph AG-X plus 100kN." The average values of the measured values obtained (n=3 each) were used as the bending strength and bending elastic modulus.
[0053] (14) Tensile strength and tensile modulus of prepreg Measurements were performed according to the test piece dimensions and test methods specified in JIS-K7164. (i) Preparation of test specimens A test piece measuring 200 mm in length and 25 mm in width was cut out from the obtained prepreg in the direction parallel to the fiber direction (0°). (ii) Measurement of tensile strength and tensile modulus Using the cut test pieces, a tensile test was performed at 23°C and 50% humidity with a gripping distance of 115 mm and a speed of 2 mm / min to measure the tensile strength and tensile modulus. The test machine used was Shimadzu Corporation's Autograph AG-X plus 100kN. Kyowa Electric Industry Co., Ltd.'s KFRPB-5-120-C1-3 L3M2R was attached as a strain gauge. The average values of the measured values obtained (n=3 each) were used as the tensile strength and tensile modulus.
[0054] Example 1 The raw fibers for producing the composite spun yarn were prepared as follows. (Continuous reinforcing fiber) The continuous reinforcing fiber was PAN-based carbon fiber manufactured by Toray Industries, Inc. ("TORAYCA T300B-1000" total fineness 660 dtex, 1000 filaments, single yarn fineness 0.66 dtex, tensile strength 3530 MPa, density 1.76 g / cm). 3 The decomposition temperature of this continuous reinforcing fiber is 500℃ or higher in an oxygen atmosphere.
[0055] (Thermoplastic Staple Fiber) Nylon 6 polymer (Ny6) was spun as a thermoplastic staple fiber to produce a 770 dtex / 770 filament long fiber (single yarn fineness 1.0 dtex, density 1.13 g / cm 3 ) was obtained. A large number of these long fibers were collected and cut to a length of 38 mm using a guillotine cutter to obtain short fibers. 100% of the nylon 6 short fibers were mixed and beaten using a cotton blending machine manufactured by Ohara Iron Works. After that, a carded sliver was made using a carding machine manufactured by Toyowa, and the carded sliver was passed through a drawing frame manufactured by Hara Loom Works three times to obtain a sliver of 371.2 grains / 6 yds. Next, a draft of 7.90 times was applied using a roving frame manufactured by Toyoda Automatic Loom Works, and a roving yarn of 124 grains / 15 yds of thermoplastic short fibers was spun. The melting point of this thermoplastic short fiber was 225°C.
[0056] (Thermoplastic Long Fiber) Thermoplastic long fiber, 78dtex, 24 filament (single yarn fineness 3.25dtex, density 1.13g / cm 3The melting point of this thermoplastic long fiber was 225°C.
[0057] (Making composite yarn) A composite spun yarn was produced using a try spinning machine (ON-2000H) manufactured by Koseki Noboru Shoten Co., Ltd. Specifically, the above-mentioned continuous reinforcing fiber was supplied as the core yarn 2 in FIG. 2, the above-mentioned thermoplastic short fiber roving was supplied as the sheath yarn 3, and the above-mentioned thermoplastic short fiber roving 3 was subjected to a 6.2-fold draft in a draft device 6, and one roving was overlapped with the continuous reinforcing fiber 2 to form a substantially untwisted core-sheath fiber bundle 4. Thereafter, the above-mentioned thermoplastic long fiber was wound as a bundling yarn 5 around the core-sheath fiber bundle 4 with an S-twist at a spindle rotation speed of 1420 rpm of a bobbin 8 to bundling the fiber bundles, producing a composite spun yarn 1, which was then wound around a cheese 10. The blend ratio of the continuous reinforcing fiber in the fiber bundle was 28%. Details of the obtained composite spun yarn and the evaluation results are shown in Table 1.
[0058] (Preparation of woven prepregs) The above composite spun yarn (183 strands) was warped using a warping machine manufactured by Toyoshima Business Co., Ltd. and wound on a loom beam. This was woven using a sample type rapier loom manufactured by Toyoshima Business Co., Ltd. to produce a plain weave fabric with 15 strands / inch, 15 weft strands / inch, and a width of 31 cm. This fabric was cut into a size of 15.0 cm x 20.0 cm, 12 of which were stacked, and heated and compressed for 5 minutes using a press molding machine manufactured by Sankogosei Co., Ltd. at a mold temperature of 240°C and a pressure of 1 MPa to produce one prepreg. The details of this prepreg and the evaluation results are shown in Table 1.
[0059] Example 2 The same continuous reinforcing fibers, thermoplastic short fibers, and thermoplastic long fibers were used as in Example 1, and a composite spun yarn was produced in the same manner as in Example 1 using the same device as in Example 1. However, in Example 1, when the roving of the thermoplastic short fibers was overlapped with the continuous reinforcing fibers, a draft of 6.2 times was applied to the roving, but in Example 2, a single roving was overlapped with the continuous reinforcing fiber bundle and then a draft of 8.1 times was applied, thereby changing the fineness of the fiber bundle to 911 dtex. The blend ratio of the continuous reinforcing fibers in the fiber bundle was 40%. Details of the obtained composite spun yarn and the evaluation results are shown in Table 1.
[0060] This composite spun yarn was used to produce a woven fabric using the same equipment and weaving density as in Example 1. This woven fabric was cut into 20.0 cm x 20.0 cm pieces, 17 of which were stacked, and then heat-compressed and molded for 5 minutes at a mold temperature of 240°C and a pressure of 1 MPa using a Sankogosei press molding machine to produce one prepreg. Details of this prepreg and the evaluation results are shown in Table 1.
[0061] Example 3 The same continuous reinforcing fibers, thermoplastic short fibers, and thermoplastic long fibers were used as in Example 1, and a composite spun yarn was produced in the same manner as in Example 1 using the same device as in Example 1. However, in Example 1, when the roving of the thermoplastic short fibers was overlapped with the continuous reinforcing fibers, a draft of 6.2 times was applied to the roving, but in Example 3, a single roving was overlapped with the continuous reinforcing fiber bundle and then a draft of 10.1 times was applied, thereby changing the fineness of the fiber bundle to 558 dtex. The blend ratio of the continuous reinforcing fibers in the fiber bundle was 51%. Details of the obtained composite spun yarn and the evaluation results are shown in Table 1.
[0062] This composite spun yarn was used to produce a woven fabric using the same equipment and weaving density as in Example 1. This woven fabric was cut into 20.0 cm x 20.0 cm pieces, 23 of which were stacked together, and then heat-compressed and molded for 5 minutes at a mold temperature of 240°C and a pressure of 1 MPa using a Sankogosei press molding machine to produce one prepreg. Details of this prepreg and the evaluation results are shown in Table 1.
[0063] Example 4 The continuous reinforcing fiber is TORAYCA T300B-3000, a PAN-based carbon fiber manufactured by Toray Industries, Inc., with a total fiber size of 1980 dtex, 3000 filaments, a single fiber size of 0.66 dtex, a tensile strength of 3530 MPa, and a density of 1.76 g / cm. 3 ) was used. The decomposition temperature of this continuous reinforcing fiber is 500°C or higher in an oxygen atmosphere. The same thermoplastic short fibers and thermoplastic long fibers were used as in Example 1, and a composite spun yarn was produced in the same manner as in Example 1 using the same device as in Example 1. However, in Example 1, when one thermoplastic short fiber roving was overlapped with the continuous reinforcing fiber, a draft of 6.2 times was applied to the roving, but in Example 4, this was changed to 10.1 times, and the number of rovings overlapped with the continuous reinforcing fiber was changed from 1 to 3, thereby changing the fineness of the fiber bundle to 1829 dtex. The mixing ratio of continuous reinforcing fiber in the fiber bundle was 51%. Details of the obtained composite spun yarn and the evaluation results are shown in Table 1.
[0064] This composite spun yarn was used to produce a woven fabric using the same equipment and weaving density as in Example 1. This woven fabric was cut into 20.0 cm x 20.0 cm pieces, eight of which were stacked, and then heat-compressed and molded for five minutes at a mold temperature of 240°C and a pressure of 1 MPa using a Sankogosei press molding machine to produce one prepreg. Details of this prepreg and the evaluation results are shown in Table 1.
[0065] Example 5 The continuous reinforcing fiber was PAN-based carbon fiber manufactured by Mitsubishi Chemical Corporation ("Pyrofil TR50S6L" total fineness 4000dtex, 6000 filaments, single yarn fineness 0.667dtex, tensile strength 4900MPa, density 1.82g / cm). 3) was used. The decomposition temperature of this continuous reinforcing fiber is 500°C or higher in an oxygen atmosphere. The same thermoplastic short fibers and thermoplastic long fibers were used as in Example 1, and a composite spun yarn was produced in the same manner as in Example 1 using the same device as in Example 1. However, in Example 1, when one thermoplastic short fiber roving was overlapped with the continuous reinforcing fiber, a draft of 6.2 times was applied to the roving, but in Example 5, this was changed to 10.1 times, and the number of rovings overlapped with the continuous reinforcing fiber was changed from 1 to 6, thereby changing the fineness of the fiber bundle to 3647 dtex. The mixing ratio of the continuous reinforcing fiber in the fiber bundle was 52%. Details of the obtained composite spun yarn and the evaluation results are shown in Table 1.
[0066] A woven fabric was produced using the same equipment and weaving density as in Example 1. This woven fabric was cut into 20.0 cm x 20.0 cm pieces, four of which were stacked together, and then heat-compressed and molded for 5 minutes at a mold temperature of 240°C and a pressure of 1 MPa using a Sankogosei press molding machine to produce one prepreg. Details of this prepreg and the evaluation results are shown in Table 1.
[0067] Example 6 The continuous reinforcing fiber was PAN-based carbon fiber manufactured by Mitsubishi Chemical Corporation ("Pyrofil TR50S12L" total fineness 8000 dtex, 12000 filaments, single yarn fineness 0.667 dtex, tensile strength 4900 MPa, density 1.82 g / cm). 3 ) was used. The decomposition temperature of this continuous reinforcing fiber is 500°C or higher in an oxygen atmosphere. The same thermoplastic short fibers and thermoplastic long fibers were used as in Example 1, and a composite spun yarn was produced in the same manner as in Example 1 using the same device as in Example 1. However, in Example 1, when one thermoplastic short fiber roving was overlapped with the continuous reinforcing fiber, a draft of 6.2 times was applied to the roving, but in Example 6, this was changed to 10.1 times, and the number of rovings overlapped with the continuous reinforcing fiber was changed from 1 to 12, thereby changing the fineness of the fiber bundle to 7373 dtex. The mixing ratio of continuous reinforcing fiber in the fiber bundle was 52%. Details of the obtained composite spun yarn and the evaluation results are shown in Table 1.
[0068] A woven fabric was produced using the same equipment and weaving density as in Example 1. This woven fabric was cut into 20.0 cm x 20.0 cm pieces, two of which were stacked together, and then heat-compressed and molded for 5 minutes at a mold temperature of 240°C and a pressure of 1 MPa using a Sankogosei press molding machine to produce one prepreg. Details of this prepreg and the evaluation results are shown in Table 1.
[0069] Example 7 As a thermoplastic short fiber, polypropylene polymer (PP) was spun to produce a long fiber of 770 dtex / 770 filament (single yarn fineness 1.0 dtex, density 0.9 g / cm 3 ) was obtained. A large number of these long fibers were collected and cut to a length of 38 mm using a guillotine cutter to obtain short fibers. 100% of the polypropylene short fibers were mixed and beaten using a cotton blending machine manufactured by Ohara Iron Works. After that, a carded sliver was made using a carding machine manufactured by Toyowa, and the carded sliver was passed through a drawing frame manufactured by Hara Loom Works three times to obtain a sliver of 371.9 grains / 6 yds. Next, a draft of 7.90 times was applied using a roving frame manufactured by Toyoda Automatic Loom Works, and a roving yarn of thermoplastic short fibers of 122 grains / 15 yds was spun. The melting point of this thermoplastic short fiber was 168°C.
[0070] Thermoplastic long fiber, 78dtex, 24 filament (single yarn fineness 3.25dtex, density 0.9g / cm 3 ) Commercially available semi-dull polypropylene (PP) long fibers (raw silk) were used. The melting point of this thermoplastic long fiber was 168°C. The same continuous reinforcing fibers as in Example 1 were used, and a composite spun yarn was produced in the same manner as in Example 1 using the same device as in Example 1. However, in Example 1, when a single thermoplastic short fiber roving was overlapped with the continuous reinforcing fiber, a draft of 6.2 times was applied to the roving, but in Example 7, a single roving was overlapped with the continuous reinforcing fiber bundle and then a draft of 11.4 times was applied, thereby changing the fineness of the fiber bundle to 428 dtex. The blending ratio of the continuous reinforcing fiber in the fiber bundle was 57%. Details of the obtained composite spun yarn and the evaluation results are shown in Table 1.
[0071] A woven fabric was produced using the same equipment and weaving density as in Example 1. This woven fabric was cut into 20.0 cm x 20.0 cm pieces, 24 of which were stacked together, and then heat-compressed and molded for 5 minutes at a mold temperature of 180°C and a pressure of 1 MPa using a Sankogosei press molding machine to produce one prepreg. Details of this prepreg and the evaluation results are shown in Table 1.
[0072] Example 8 The continuous reinforcing fiber was E-glass fiber manufactured by Nippon Electric Glass Co., Ltd. ("ECG 751 / 01ZY-95S" total fiber size 660 dtex, 1000 filaments, single fiber diameter 9.0 μm, tensile strength 6.09 cN / dtex, density 2.6 g / cm 3 ) was used. The softening temperature of this continuous reinforcing fiber was about 845°C. The same thermoplastic short fibers and thermoplastic long fibers were used as in Example 1, and a composite spun yarn was produced in the same manner as in Example 1 using the same device as in Example 1. However, in Example 1, when a single thermoplastic short fiber roving was overlapped with the continuous reinforcing fiber, a draft of 6.2 times was applied to the roving, but in Example 8, a single roving was overlapped with the continuous reinforcing fiber bundle and then a draft of 13.5 times was applied, thereby changing the fineness of the fiber bundle to 352 dtex. The blend ratio of continuous reinforcing fiber in the fiber bundle was 61%. Details of the obtained composite spun yarn and the evaluation results are shown in Table 1.
[0073] A woven fabric was produced using the same equipment and weaving density as in Example 1. This woven fabric was cut into 20.0 cm x 20.0 cm pieces, 35 of which were stacked together, and then heat-compressed and molded for 5 minutes at a mold temperature of 240°C and a pressure of 1 MPa using a Sankogosei press molding machine to produce one prepreg. Details of this prepreg and the evaluation results are shown in Table 1.
[0074] Example 9 Polyphenylene sulfide polymer (PPS) was spun as a thermoplastic staple fiber to produce a 770 dtex / 770 filament long fiber (single yarn fineness 1.0 dtex, density 1.35 g / cm 3) was obtained. A large number of these long fibers were collected and cut to a length of 38 mm using a guillotine cutter to obtain short fibers. 100% of the polyphenylene sulfide short fibers were mixed and beaten using a cotton blending machine manufactured by Ohara Iron Works. After that, a carded sliver was made using a carding machine manufactured by Toyowa, and the carded sliver was passed through a drawing frame manufactured by Hara Loom Works three times to obtain a sliver of 369.7 grains / 6 yds. Next, a roving frame manufactured by Toyoda Automatic Loom Works was used to apply a 7.9 times draft to spin a roving yarn of thermoplastic short fibers of 122 grains / 15 yds. The melting point of this thermoplastic short fiber was 275°C.
[0075] Thermoplastic long fiber, 78dtex, 24 filament (single yarn fineness 3.25dtex, density 1.35g / cm 3 ) Semi-dull commercial polyphenylene sulfide (PPS) long fibers (raw silk) were used. The melting point of this thermoplastic long fiber was 275°C. The same continuous reinforcing fibers as in Example 1 were used, and a composite spun yarn was produced in the same manner as in Example 1 using the same device as in Example 1. However, in Example 1, when a single thermoplastic short fiber roving was overlapped with the continuous reinforcing fiber, a draft of 6.2 times was applied to the roving, but in Example 9, this was changed to 9.4 times, and the fineness of the fiber bundle was changed to 681 dtex. The blend ratio of continuous reinforcing fibers in the fiber bundle was 47%. Details of the obtained composite spun yarn and the evaluation results are shown in Table 1.
[0076] A woven fabric was produced using the same equipment and weaving density as in Example 1. This woven fabric was cut into 20.0 cm x 20.0 cm pieces, 24 of which were stacked together, and then heat-compressed and molded for 5 minutes at a mold temperature of 290°C and a pressure of 1 MPa using a Sankogosei press molding machine to produce one prepreg. Details of this prepreg and the evaluation results are shown in Table 1.
[0077] Comparative Example 1 Comparative Example 1 is an example in which thermoplastic short fibers were not used and a long fiber bundle covering yarn having no sheath portion was used. The continuous reinforcing fibers used were the same as those used in Example 1. No thermoplastic short fibers were used. As the thermoplastic long fibers, 154 dtex, 48 filaments (single filament fineness 3.2 dtex, density 1.13 g / cm 3) Semi-dull commercial nylon 6 (Ny6) filament (raw silk) x 6 and 110 dtex, 24 filament (single yarn fineness 4.58 dtex, density 1.13 g / cm 3 ) A 1034 dtex long fiber bundle was used, which was prepared by twisting together a semi-dull, commercially available nylon 6 (Ny6) long fiber (raw silk). The melting point of this thermoplastic long fiber was 225°C. A composite filament yarn of continuous reinforcing fiber and thermoplastic long fiber was produced by twisting the continuous reinforcing fiber and thermoplastic long fiber with an S-twist at 110 T / m using a doubling and twisting machine. Details of the obtained composite filament yarn and the evaluation results are shown in Table 1.
[0078] A woven fabric was produced using the same equipment and weaving density as in Example 1. This woven fabric was cut into 20.0 cm x 20.0 cm pieces, 17 of which were stacked together, and then heat-compressed and molded for 5 minutes at a mold temperature of 240°C and a pressure of 1 MPa using a Sankogosei press molding machine to produce one prepreg. Details of this prepreg and the evaluation results are shown in Table 1.
[0079] Comparative Example 2 Comparative Example 2 is an example in which thermoplastic long fibers were used in place of the continuous reinforcing fibers in the core portion. The thermoplastic long fiber core is 110 dtex, 24 filaments (single fiber fineness 4.583 dtex, density 1.13 g / cm 3 ) A continuous fiber bundle was used in which six semi-dull commercially available nylon 6 continuous fibers (raw silk) were aligned. The melting point of this thermoplastic continuous fiber was 225°C. A composite spun yarn was produced in the same manner as in Example 1, except for this change in the core. Details of the obtained composite spun yarn and the evaluation results are shown in Table 1.
[0080] A woven fabric was produced using the same equipment and weaving density as in Example 1. This woven fabric was cut into 20.0 cm x 20.0 cm pieces, 11 of which were stacked together, and then heat-compressed and molded for 5 minutes at a mold temperature of 240°C and a pressure of 1 MPa using a Sankogosei press molding machine to produce one prepreg. Details of this prepreg and the evaluation results are shown in Table 1.
[0081] [Table 1]
[0082] As can be seen from Table 1, the composite spun yarns of Examples 1 to 9, which satisfy the conditions of the present invention, were excellent in tensile strength and spinning stability. In addition, the prepregs made from the composite spun yarns of Examples 1 to 9 obtained satisfactory results in all items of appearance, void ratio, strength, and elastic modulus. In contrast, Comparative Example 1, which does not have a core-sheath structure, had poor spinning stability. In addition, as can be seen from the large void ratio of the prepreg (the black area in the white frame in Figure 5 is a void), the thermoplastic resin of the matrix did not sufficiently and uniformly penetrate the continuous reinforcing fibers of the core, and therefore the prepreg strength varied greatly (data not shown). The composite spun yarn of Comparative Example 2, which does not use continuous reinforcing fibers, was significantly inferior in tensile strength, and the prepreg was also significantly inferior in bending strength, bending elastic modulus, tensile strength, and tensile elastic modulus. [Industrial Applicability]
[0083] The conjugate spun yarn of the present invention has excellent strength and spinnability, and therefore when it is heated and melted to form a fiber-reinforced plastic product, it can provide a product with excellent moldability, strength, and uniformity of physical properties. [Explanation of symbols]
[0084] 1. Composite spun yarn 2 Continuous reinforcing fibers 3 Thermoplastic short fibers 4 Fiber bundles 5 Thermoplastic long fibers 6 Draft device 7 Guide 8 Hollow Bobbin 9 Feed Roller 10. Cheese
Claims
1. A composite spun yarn for fiber-reinforced thermoplastics, characterized in that a thermoplastic long fiber is wound around a substantially untwisted fiber bundle formed from a core portion made of continuous reinforcing fiber and a sheath portion made of thermoplastic short fiber.
2. 2. The composite spun yarn for fiber-reinforced thermoplastics according to claim 1, characterized in that each of the thermoplastic short fibers and the thermoplastic long fibers is a fiber made of at least one thermoplastic resin selected from the group consisting of polyamide, polypropylene, polyphenylene sulfide, polyetherimide, and phenoxy.
3. The composite spun yarn for fiber-reinforced thermoplastics according to claim 1, characterized in that the continuous reinforcing fiber is at least one type of fiber selected from the group consisting of carbon fiber, glass fiber, basalt fiber, PBO fiber, and aramid fiber, and the mixing ratio of the continuous reinforcing fiber is 20 to 80 mass%.
4. The composite spun yarn for fiber reinforced thermoplastics according to claim 1, characterized in that the total fineness of the composite spun yarn is 200 to 500,000 dtex.
5. The composite spun yarn for fiber reinforced thermoplastics according to claim 1, characterized in that the thermoplastic long fiber is wound around a substantially untwisted fiber bundle with a twist number of 1 to 1000 T / m.
6. A method for producing a molded product, comprising filling a mold with the composite spun yarn for fiber-reinforced thermoplastics according to any one of claims 1 to 5 at a filling rate of 100 to 350%, and heating the mold at a temperature higher than the higher of the melting points of the thermoplastic short fibers and the thermoplastic long fibers to melt the thermoplastic short fibers and the thermoplastic long fibers.
Citation Information
Patent Citations
Composite material and dimensional recoverable article
JP1989238923A
Composite spun yarn and method for producing the same
JP1995243140A
Fiber reinforced thermoplastic resin molding material
JP1985028543A
Manufacture of laminate
JP1985056545A
Composite yarn and intermediate for fiber-reinforced resin and molded fiber-reinforced resin obtained therefrom
WO2009131149A1
Cited By
Composite spun yarn for fiber-reinforced thermoplastics
JP7745819B1
Composite spun yarn for fiber-reinforced thermoplastic
WO2026088457A1