Liquid discharge head and manufacturing method for the same

A liquid ejection head with an epoxy resin composition and coumaron resin addresses bleeding and ink resistance issues, ensuring accurate ejection and manufacturing stability by controlling adhesive fluidity.

JP2024151971APending Publication Date: 2024-10-25CANON KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023065827
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing adhesives for liquid ejection heads, particularly those using thermosetting one-component epoxy resin compositions, suffer from bleeding issues due to the liquid epoxy resin bleeding out and uncured components coming into contact with liquids, affecting ejection accuracy and ink resistance.

Method used

A liquid ejection head using an epoxy resin composition with a specific weight average molecular weight range (300 to 600) and containing a coumaron resin soluble in the epoxy resin, along with a powder curing agent, to control bleeding and enhance ink resistance.

Benefits of technology

The solution effectively suppresses bleeding and maintains ink resistance, ensuring accurate liquid ejection and improved manufacturing stability by controlling the fluidity of the adhesive during curing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151971000005
    Figure 2024151971000005
  • Figure 2024151971000006
    Figure 2024151971000006
  • Figure 2024151971000001
    Figure 2024151971000001
Patent Text Reader

Abstract

To provide a liquid discharge head including an adhesive that balances ink resistance and breed suppression, and a manufacturing method for the same.SOLUTION: In a manufacturing method for a liquid discharge head, an epoxy resin composition is used as an adhesive in the liquid discharge head. The epoxy resin composition includes an epoxy resin mixture and a powder curing agent. The epoxy resin mixture includes an epoxy resin that is liquid at ordinary temperature and a coumarone resin that can be dissolved into the epoxy resin. The weight average molecular weight of the epoxy resin mixture is 300 or more and 600 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid ejection head for ejecting liquid such as ink from ejection ports, and to a method for manufacturing the same. [Background technology]

[0002] The manufacture of a liquid ejection head, typified by an inkjet recording head, begins with providing energy generating elements and wiring conductors for supplying power to the energy generating elements on a silicon substrate. Then, after providing a protective film on the wiring conductors, liquid flow paths and liquid ejection ports are patterned with resist. Next, through holes (liquid supply ports) for supplying liquid to the energy generating element section from the back side of the silicon substrate are opened in the silicon substrate. Then, this recording element substrate is attached to a support member such as alumina or resin with an adhesive, and the recording element substrate and the electrical wiring member are electrically joined.

[0003] In the manufacture of liquid ejection heads, from the viewpoint of manufacturing costs, the adhesive and sealing material used in the final process for bonding and sealing other components are fully cured together. In other words, in the process of attaching the support plate and the recording element substrate, the adhesive has not yet been cured. Therefore, the recording element substrate, which is positioned when attached, may deviate from the attachment position due to movement to the next process, etc. For the reasons mentioned above, in order to prevent the recording element substrate from shifting in position, it is desirable to temporarily fix and cure the adhesive within the device that attaches the recording element substrate. The adhesive used to attach the recording element substrate and the support member is required to have high adhesiveness and ink resistance, and is preferably easy to use in the manufacturing process. For the above reasons, a thermosetting one-component epoxy resin composition is often used as an adhesive for bonding the recording element substrate and the support member. As an example of a thermosetting one-component epoxy resin composition, an adhesive containing the epoxy resin composition described in Patent Document 1 has been disclosed. On the other hand, Patent Documents 2 and 3 disclose adhesives that contain epoxy resin compositions that contain coumarone resins. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-21011 A [Patent Document 2] JP 2019-172911 A [Patent Document 3] Patent Publication No. 2021-138809 Summary of the Invention [Problem to be solved by the invention]

[0005] A thermosetting one-part epoxy resin composition cures by the reaction between the epoxy resin and the curing agent caused by heat. Since it is a solvent-free system, an epoxy resin that is liquid at room temperature is used. On the other hand, from the viewpoint of storage stability, it is preferable that the curing agent is in powder form (solid). However, in the case of adhesives that use epoxy resin that is liquid at room temperature and a powder curing agent, bleeding can be an issue. This is a phenomenon in which the adhesive applied to a support member is thinly pressed against the recording element substrate and then cured, causing the epoxy resin to bleed out and leaving uncured components behind. If the remaining uncured components come into contact with liquids such as ink, they may adhere to the liquid ejection surface or cause a decrease in liquid ejection accuracy, so there is a need to suppress bleeding in adhesives used in the flow paths of liquid ejection heads.

[0006] As mentioned above, bleeding is a phenomenon in which only liquid epoxy resin bleeds out as the thermosetting reaction of an epoxy resin composition progresses. In the thermosetting reaction, the powder curing agent first softens and liquefies, and the reaction progresses, but at the same time, the fluidity of the liquid epoxy resin increases due to heat. Therefore, in order to suppress bleeding, it is necessary to control the fluidity of the epoxy resin. The thermosetting one-component epoxy resin composition described in Patent Document 1 is an invention that aims to suppress the above-mentioned bleeding.

[0007] However, according to the investigations of the present inventors, it has been confirmed that the adhesive disclosed in Patent Document 1 has a problem in terms of ink resistance when used in a liquid ejection head. Furthermore, according to the present inventors' investigations, it has been confirmed that the adhesives disclosed in Patent Documents 2 and 3 have a problem in achieving both ink resistance and bleeding suppression. SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a liquid ejection head having an adhesive that is both ink-resistant and bleed-suppressive, and a method for manufacturing the same. [Means for solving the problem]

[0008] The present invention, which achieves the above object, is a liquid ejection head in which an epoxy resin composition is used as an adhesive, the epoxy resin composition comprising an epoxy resin mixture and a powder curing agent, The epoxy resin mixture includes an epoxy resin that is liquid at room temperature and a coumarone resin that is soluble in the epoxy resin, The liquid ejection head further comprises a liquid ejection head having a weight average molecular weight of the epoxy resin mixture of 300 or more and 600 or less. The present invention also provides a liquid ejection head including a recording element substrate that ejects liquid, a support member that supports the recording element substrate and has a supply flow path that supplies ink to the recording element substrate, and a flow path member that supplies liquid to the supply flow path, At least one bonding surface between any two of the recording element substrate, the support member, and the flow path member is An epoxy resin composition comprising an epoxy resin mixture and a powder curing agent, The epoxy resin mixture includes an epoxy resin that is liquid at room temperature and a coumarone resin that is soluble in the epoxy resin, A liquid ejection head comprising a cured product of an adhesive containing an epoxy resin composition in which the weight average molecular weight of the epoxy resin mixture is 300 or more and 600 or less. Further, the present invention relates to A method for manufacturing a liquid ejection head having a recording element substrate that ejects liquid, a support member that supports the recording element substrate and has a supply flow path that supplies liquid to the recording element substrate, and a flow path member that supplies liquid to the supply flow path, comprising the steps of: applying the adhesive to at least one joining surface between at least two of the recording element substrate, the support member, and the flow path member; A step of bonding the two members together; and a main curing process of thermally curing the adhesive to bond the two members together, The adhesive may include An epoxy resin composition comprising an epoxy resin mixture and a powder curing agent, The epoxy resin mixture includes an epoxy resin that is liquid at room temperature and a coumarone resin that is soluble in the epoxy resin, A method for manufacturing a liquid ejection head using an adhesive containing an epoxy resin composition in which the weight average molecular weight of the epoxy resin mixture is 300 or more and 600 or less. Effect of the Invention

[0009] According to the present invention, it is possible to provide a liquid ejection head having an adhesive that is both ink-resistant and bleed-resistant, and a method for manufacturing the same. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic perspective view illustrating one embodiment of a liquid ejection head of the present invention. [Diagram 2] 1 is a schematic cross-sectional view of a liquid ejection head according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] As a result of intensive research, the inventors of the present invention have succeeded in producing an adhesive that combines ink resistance and bleeding suppression by using a coumarone-indene resin (hereinafter referred to as coumarone resin) that can be dissolved in epoxy resin. Coumarone resin is a copolymer resin whose main components are coumarone, indene, and styrene. By dissolving the coumarone resin in epoxy resin, the weight average molecular weight of the epoxy resin mixture increases, making it possible to reduce the fluidity at high temperatures. Furthermore, since the coumarone resin has a skeleton that does not swell with ink, it is also possible to achieve ink resistance. That is, the liquid ejection head of the present invention is a liquid ejection head in which an epoxy resin composition is used as an adhesive, the epoxy resin composition being an epoxy resin composition containing an epoxy resin mixture and a powder curing agent, The epoxy resin mixture includes an epoxy resin that is liquid at room temperature and a coumarone resin that is soluble in the epoxy resin, The epoxy resin mixture has a weight average molecular weight of 300 or more and 600 or less. A preferred embodiment of the liquid ejection head of the present invention will be described below. First, the epoxy resin composition used as the adhesive will be described.

[0012] <Adhesive> The adhesive used in the liquid ejection head of the present invention will be described. The adhesive used in the liquid ejection head of the present invention is an epoxy resin composition containing an epoxy resin mixture and a powdered hardener. The epoxy resin mixture contains an epoxy resin that is liquid at room temperature and a coumarone resin that is soluble in the epoxy resin. When heated, the powdered hardener is first liquefied, and the liquefied hardener reacts with the epoxy resin to gel, and finally becomes a hardened product.

[0013] As the epoxy resin that is liquid at room temperature, an alicyclic epoxy resin, an aromatic epoxy resin, an aliphatic epoxy resin, etc. can be used.

[0014] Examples of alicyclic epoxy resins include the following: Polyglycidyl ethers of polyhydric alcohols having at least one cyclic aliphatic group (alicyclic group), a compound containing a cyclohexene oxide structure or a compound containing a cyclopentene oxide structure obtained by epoxidizing a compound containing a cyclohexene or cyclopentene ring with an oxidizing agent; Examples of the compound include compounds containing a vinylcyclohexane oxide structure obtained by epoxidizing a compound having a vinylcyclohexane structure with an oxidizing agent.

[0015] Examples of alicyclic epoxy resins include the following: Hydrogenated bisphenol A diglycidyl ether, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexyl carboxylate, 3,4-epoxy-1-methylcyclohexyl-3,4-epoxy-1-methylcyclohexane carboxylate, 6-methyl-3,4-epoxycyclohexylmethyl-6-methyl-3,4-epoxycyclohexane carboxylate, 3,4-epoxy-3-methylcyclohexylmethyl-3,4-epoxy-3-methylcyclohexane carboxylate, 3,4-epoxy-5-methylcyclohexylmethyl-3,4-epoxy-5-methylcyclohexane carboxylate, 2-(3,4-epoxycyclohexyl-5,5-spiroyl) b-3,4-epoxy)cyclohexane-metadioxane, bis(3,4-epoxycyclohexylmethyl)adipate, vinylcyclohexene dioxide, 4-vinylepoxycyclohexane, bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, 3,4-epoxy-6-methylcyclohexylcarboxylate, methylene bis(3,4-epoxycyclohexane), dicyclopentadiene diepoxide, ethylene glycol di(3,4-epoxycyclohexylmethyl)ether, ethylene bis(3,4-epoxycyclohexanecarboxylate), dioctyl epoxyhexahydrophthalate, di-2-ethylhexyl epoxyhexahydrophthalate, and the like.

[0016] Specific examples of aromatic epoxy resins include the following: Polyglycidyl ethers of polyhydric phenols having at least one aromatic ring or their alkylene oxide adducts, or those containing a naphthalene ring, such as glycidyl ethers of bisphenol A, bisphenol F, and compounds obtained by further adding alkylene oxide to these, epoxy novolac resins, bisphenol A novolac diglycidyl ether, bisphenol F novolac diglycidyl ether, etc.

[0017] Aliphatic epoxy resins include the following: Examples of the polyglycidyl ethers include polyglycidyl ethers of aliphatic polyhydric alcohols or their alkylene oxide adducts, polyglycidyl esters of aliphatic long-chain polybasic acids, epoxy-containing compounds obtained by oxidizing aliphatic long-chain unsaturated hydrocarbons with an oxidizing agent, homopolymers of glycidyl acrylate or glycidyl methacrylate, and copolymers of glycidyl acrylate or glycidyl methacrylate.

[0018] Representative examples of aliphatic epoxy resins include the following compounds: Glycidyl ethers of polyhydric alcohols such as 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, triglycidyl ether of glycerin, triglycidyl ether of trimethylolpropane, tetraglycidyl ether of sorbitol, hexaglycidyl ether of dipentaerythritol, diglycidyl ether of polyethylene glycol, and diglycidyl ether of polypropylene glycol; polyglycidyl ethers of polyether polyols obtained by adding one or more alkylene oxides to aliphatic polyhydric alcohols such as propylene glycol and glycerin; and diglycidyl esters of aliphatic long-chain dibasic acids. Monoglycidyl ethers of higher aliphatic alcohols, phenol, cresol, butylphenol, and monoglycidyl ethers of polyether alcohols obtained by adding alkylene oxides to these, glycidyl esters of higher fatty acids, epoxidized soybean oil, epoxy octyl stearate, epoxy butyl stearate, epoxidized linseed oil, etc.

[0019] Examples of the coumarone resin that can be dissolved in the epoxy resin include trade names: Nitto Resin (registered trademark) Coumarone R-100, Nitto Resin Coumarone V-120, and Nitto Resin Coumarone H-100 (all manufactured by Nippon Paint Chemical Co., Ltd.). When dissolving the coumarone resin in the epoxy resin, heat may be applied.

[0020] The weight average molecular weight of the epoxy resin mixture in which the coumarone resin is dissolved in the epoxy resin must be 300 or more and 600 or less. This is because if the weight average molecular weight is less than 300, it is difficult to suppress bleeding. Also, if the weight average molecular weight is more than 600, it is difficult to disperse uniformly when mixed with the powder curing agent, and there is a possibility that the ink resistance will decrease. The weight average molecular weight is calculated in terms of polystyrene using gel permeation chromatography (e.g., manufactured by Shimadzu Corporation) as described in the examples.

[0021] In addition, it is preferable that the functional group equivalent of the epoxy resin in the epoxy resin mixture is 100 or more and 200 or less. When the functional group equivalent is 100 or more, excellent ink resistance is obtained, and when it is 200 or less, excellent temporary fixing property is obtained. In addition, the epoxy resin functional group equivalent of the epoxy resin mixture is calculated by adding acetic acid and tetraethylammonium bromide acetate solution to the epoxy mixture, and then potentiometric titration with a 0.1 mol / L perchloric acid acetic acid standard solution, as described in the examples.

[0022] Furthermore, the content of the coumarone resin relative to the epoxy resin is preferably 10 parts by mass or more and 50 parts by mass or less, more preferably 20 parts by mass or more and 45 parts by mass or less, and even more preferably 21 parts by mass or more and 40 parts by mass or less, relative to 100 parts by mass of the epoxy resin. It is preferably more than 20 parts by mass and 40 parts by mass or less. When the content is 10 parts by mass or more, bleeding is suppressed, and when it is 50 parts by mass or less, excellent temporary fixing properties are obtained.

[0023] The hydroxyl value (mg KOH / g) of the coumarone resin relative to the epoxy resin mixture is preferably not more than 50, and particularly preferably not more than 40. When the hydroxyl value is not more than 50, excellent ink resistance can be obtained.

[0024] Examples of the powder curing agent include amine-based curing agents, phenol-based curing agents, and acid anhydride-based curing agents. The softening point of the powder curing agent is preferably 80° C. or higher and 100° C. or lower. When the softening point is 80° C. or higher, excellent ink resistance is obtained, and when the softening point is 100° C. or lower, excellent temporary fixing properties are obtained.

[0025] The content of the powder curing agent relative to the epoxy resin is preferably 40 parts by mass or more and 65 parts by mass or less relative to 100 parts by mass of the epoxy resin. When the content is 40 parts by mass or more, bleeding is suppressed and excellent temporary fixing properties are obtained, and when the content is 65 parts by mass or less, excellent ink resistance is obtained.

[0026] The powdered hardener is preferably an amine-based hardener having an average particle size of 70 nm or less. As the amine-based hardener, primary amines, secondary amines, tertiary amines, etc. are used.

[0027] Diluents and other additives may be added to these resin compositions by a commonly used method. For example, a silane coupling agent may be added. As the silane coupling agent, a silane coupling agent having an epoxy group, a mercapto group, an isocyanate group, or a fluorene skeleton may be used.

[0028] In the method for producing the adhesive of the present invention, the coumarone resin is preferably dissolved in the epoxy resin before mixing the epoxy resin with the powdered hardener, and may be heated and stirred at this time.

[0029] <Liquid ejection head> The configuration of the liquid ejection head of the present invention will be described with reference to the drawings. Fig. 1 is a schematic perspective view for explaining one embodiment of the liquid ejection head of the present invention, and Fig. 2 is a schematic cross-sectional view of the liquid ejection head. The liquid ejection head 1 comprises a recording element substrate 2 that ejects liquid such as ink, a support member 4 that supports the recording element substrate and has a supply flow path 3 that supplies liquid to the recording element substrate, and a flow path member 5 that supplies liquid to the liquid supply flow path. At least one joint surface between any two of the recording element substrate 2, the support member 4, and the flow path member 5 comprises a cured product of the adhesive described above. The flow path member 5 may be composed of a plurality of parts. For example, the flow path member 5 may be composed of a first flow path member 6, a second flow path member 7, and a third flow path member 8 as shown in FIG. The support member 4 and the flow path member 5 can be made of ceramics such as alumina, or resins (engineering plastics) with excellent dimensional accuracy such as modified polyphenylene ether resin (Zylon (registered trademark), manufactured by Asahi Kasei Corporation, etc.).

[0030] <Method of Manufacturing Liquid Ejection Head> The method for producing a liquid ejection head of the present invention includes the steps of: The method includes at least a coating step, a bonding step, and a main curing step. The application step is a step of applying the above-mentioned adhesive to at least one bonding surface between any two of the recording element substrate 2, the support member 4, and the flow path member 5. The lamination step is a step in which the adhesive applied onto the recording element substrate 2, the support member 4, and the flow path member 5 is pressed and squashed by any two of the recording element substrate 2, the support member 4, and the flow path member 5. When the flow path member 5 is a flow path member 5 consisting of three members as shown in FIG. 2, the third flow path member 8 and the second flow path member 7 are bonded together in advance, and then the first flow path member 6 is bonded to the second flow path member 7 to produce the flow path member 5. In the bonding process, it is desirable to compress the adhesive to a thickness of 10 μm or less. The main curing process is a process of curing the adhesive by heat. A temporary fixing curing process may be included before the main curing process. The temporary fixing curing process is a process of applying heat to the adhesive to harden it in order to prevent misalignment of parts during the manufacturing process. The temporary fixing curing process is characterized by having a shorter curing time than the main curing process, and may be performed simultaneously with the above-mentioned bonding process or after the bonding process. Bleeding is a phenomenon that occurs in the main curing process, in which the fluidity of the epoxy resin increases due to heat, causing it to bleed out, resulting in unreacted components of the epoxy resin remaining after curing. In the present invention, by dissolving a coumarone resin as an adhesive component in the epoxy resin, the weight average molecular weight of the epoxy resin mixture is increased, making it possible to reduce the fluidity at high temperatures, and thus suppressing the bleeding out of the epoxy resin in the main curing process. EXAMPLES

[0031] The present invention will be described below based on examples and comparative examples, but is not limited thereto. The unit of the amount of each component added in Tables 1 to 4 is "parts by mass" unless otherwise specified.

[0032] Tables 1 to 3 show the composition ratios of the epoxy resin compositions used in the examples, and Table 4 shows the composition ratios of the epoxy resin compositions used in the comparative examples. The materials used in Tables 1 to 4 are as follows: (Bis A type epoxy resin / liquid at room temperature) Product name: jER825 Manufactured by Mitsubishi Chemical Corporation Product name: jER828, manufactured by Mitsubishi Chemical Corporation Product name: jER806 Manufactured by Mitsubishi Chemical Corporation (Multifunctional epoxy resin / liquid at room temperature) Product name: jER630 Manufactured by Mitsubishi Chemical Corporation (Epoxy resin that is solid at room temperature) Product name: jER1001 Manufactured by Mitsubishi Chemical Corporation (Cumarone Resin) Product name: R100 (hydroxyl value: 10mg KOH / g) manufactured by Nippon Paint Chemical Co., Ltd. Product name: V120 (hydroxyl value: 30 mg KOH / g) manufactured by Nippon Paint Chemical Co., Ltd. Product name: H100 (hydroxyl value: 50mg KOH / g) manufactured by Nippon Paint Chemical Co., Ltd. (Amine-based powder hardener) Product name: EH-5030S (Manufactured by ADEKA Corporation) Product name: EH-5015S (Manufactured by ADEKA Corporation) Product name: EH-5046S (Manufactured by ADEKA Corporation) Product name: PN23J manufactured by Ajinomoto Fine-Techno Co., Ltd. (Phenol-based powder hardener) Product name: jER 171N, manufactured by Mitsubishi Chemical Corporation (Acid anhydride powder hardener) Product name: TMTA-C manufactured by Shin-Nippon Rika Co., Ltd. (Silane coupling agent) Product name: A-187 Momentive Performance Materials Japan

[0033] Next, a method for preparing an epoxy resin composition based on the composition ratios shown in Tables 1 to 4 will be described, but the method is not limited thereto. First, a specific coumarone resin was added to the epoxy resin shown in Tables 1 to 4, and the mixture was kneaded until the coumarone resin changed from a bead-like state to a powder. The mixture was then stirred for 5 minutes under vacuum at a rotation speed of 1200 rpm using a stirrer (manufactured by Primix Corporation, product name: HIVIS MIX model 3) until the coumarone resin was completely dissolved in the epoxy resin. Thereafter, a powder curing agent shown in the table was added to the epoxy resin mixture, and the mixture was stirred for 5 minutes under vacuum at a rotation speed of 600 rpm using the stirrer to prepare an epoxy resin composition. The prepared epoxy resin compositions were evaluated for bleeding properties, swelling ratio, adhesive properties, and temporary fixing properties.

[0034] The bleeding properties were evaluated by applying an epoxy resin composition to an adherend to a thickness of 100 μm, then pressing it with another adherend to thicknesses of 10 μm, 20 μm, and 50 μm, curing it at 100° C. for 1 hour, and then peeling the adherend off. The presence or absence of uncured components was visually observed and evaluated according to the following criteria. No uncured components are observed even at a thickness of 10 μm. At a thickness of 10 μm, uncured components are observed, but at a thickness of 20 μm, no uncured components are observed. △: Uncured components are observed at a thickness of 20 μm, but not at a thickness of 50 μm. × Uncured components are observed even at a thickness of 50 μm.

[0035] The swelling rate was evaluated by immersing the sample in 20 times the amount of ink (service head ink, manufactured by Canon) by weight and conducting an accelerated test at 121°C for 10 hours. The swelling rate was measured from the weight before and after immersion in the ink and evaluated based on the following criteria. ◎ The swelling rate is less than 10%. ○ The swelling rate is between 10% and 15%. △: Swelling rate is 15% or more and less than 20%. ×: Swelling rate is 20% or more.

[0036] The adhesion was evaluated by applying the epoxy composition to a non-adherent body to a thickness of 100 μm, then pressing it with another adherend to a thickness of 10 μm, curing it at 100°C for 1 hour, and then peeling the adherend off. The peeling mode was observed and evaluated according to the following criteria. The adherend is damaged. The adhesive has undergone total cohesive failure. △: A mixture of cohesive failure of the adhesive and interfacial peeling between the adhesive and adherend. ×: The entire interface between the adherend and the adhesive has peeled off.

[0037] The temporary bonding property was evaluated by measuring the gel time at 100° C. using a sample having a thickness of 100 μm, and the evaluation criteria were as follows. ◎ Gel time is less than 8 seconds. Gel time is between 8 and 12 seconds. △ The gel time is between 12 and 15 seconds.

[0038] The weight average molecular weight of the epoxy resin mixture was calculated in terms of polystyrene using gel permeation chromatography (e.g., manufactured by Shimadzu Corporation). The epoxy resin functional group equivalent of the epoxy resin mixture was calculated by adding acetic acid and tetraethylammonium bromide acetate solution to the mixture, followed by potentiometric titration with 0.1 mol / L perchloric acid acetate standard solution. The hydroxyl value of the coumarone resin can be calculated by acetylating the hydroxyl groups in the coumarone resin with acetic anhydride for 1 g of sample, and titrating the remaining acetic acid with potassium hydroxide solution. In the case of commercially available products, the hydroxyl value of the coumarone resin can be calculated using data (catalog value) disclosed by the manufacturer.

[0039] [Table 1]

[0040] Table 1 shows Examples 1 to 4 of the present invention. In Examples 1 to 4, the weight-average molecular weight of the epoxy resin mixture was changed by changing the type of epoxy resin. When the weight-average molecular weight was between 300 and 600, the bleeding property, ink resistance, and temporary fixing property were all achieved. Furthermore, in Examples 1 to 4, the epoxy resin functional group equivalent of the epoxy resin mixture was changed by changing the type and amount of coumarone resin added. In comparison with Examples 1 and 2, when the equivalent exceeded 200, the ink resistance decreased. This is considered to be because the amount of coumarone resin that does not swell with ink was less than the amount required to maintain ink resistance, and the ink resistance of the epoxy resin composition decreased. Similarly, when the equivalent exceeded 200, the bleeding property also decreased. This is considered to be because the amount of coumarone resin with low fluidity was reduced, and the fluidity of the epoxy resin mixture increased. On the other hand, in comparison with Examples 3 and 4, when the amount of coumarone resin added exceeded 45 parts by mass, the ink resistance and temporary fixing property decreased. This is believed to be because the excess coumarone resin inhibited the reaction between the epoxy resin and the curing agent, resulting in a decrease in the reaction rate.

[0041] [Table 2]

[0042] Example 5 of the present invention is shown in Table 2. A coumarone resin with a high hydroxyl value (mg KOH / g) was used in Example 5. It is believed that when the hydroxyl value of the coumarone resin becomes high, the ink components are adsorbed to the hydroxyl groups in the coumarone resin, resulting in a decrease in the swelling rate, but if the hydroxyl value is 50 or less, bleeding properties, ink resistance, and temporary fixing properties are all achieved.

[0043] [Table 3]

[0044] Examples 6 to 11 of the present invention are shown in Table 3. In Examples 6 to 9, the amount of powder hardener added was changed, and the type of powder hardener was changed to increase or decrease the softening point of the hardener. In particular, in Examples 7 and 8, the amount of curing agent added is 40 parts by mass or more and 65 parts by mass or less, and the softening point of the curing agent is 80°C or more and 100°C or less, so that bleeding properties, ink resistance, and temporary fixing properties are all achieved simultaneously. When the amount of the curing agent added is 40 parts by mass or more and 65 parts by mass or less, the epoxy resin and the curing agent react just right, the curing reaction rate does not decrease, and the bleeding out of the unreacted epoxy resin or the curing agent is suppressed, and sufficient temporary fixing properties are obtained. In addition, even if the cured product is immersed in ink after curing, the unreacted curing agent is prevented from dissolving into the ink. When the softening point of the curing agent is 80°C or higher and 100°C or lower, the time it takes for the curing agent to soften and liquefy and the time it takes for the curing reaction to start and gel are shortened, and a sufficient reaction speed is obtained. Therefore, bleeding out of unreacted epoxy resin and curing agent is suppressed, and sufficient temporary bonding is obtained. Furthermore, since a sufficient crosslink density can be obtained after curing, even if the cured product is immersed in ink after curing, ink absorption is suppressed.

[0045] Comparing Example 9 with Example 8, Example 9 is inferior to Example 8 in all of the bleeding properties, ink resistance, and temporary fixing properties. The decrease in bleeding properties is believed to be due to the following reasons. When the amount of the curing agent is more than 65 parts by mass, unreacted curing agent remains after curing. Furthermore, when the softening point of the curing agent is higher than 100°C, it takes a long time for the curing agent to soften and liquefy. For these reasons, the epoxy resin is more likely to bleed out. The decrease in ink resistance is believed to be due to the following reasons. If the amount of hardener added is more than 65 parts by mass, unreacted hardener remains after hardening, and the remaining hardener dissolves into the ink when immersed in ink. Furthermore, if the softening point of the hardener is higher than 100°C, it takes a long time for the hardening reaction to start and for the ink to gel.

[0046] Furthermore, in Example 10, a phenol-based curing agent was used instead of an amine-based curing agent, and the average particle size of the curing agent was increased. As a result, the bleeding property and ink resistance were reduced. The decrease in bleeding property is believed to be due to the fact that the average particle size of the curing agent is large, which increases the time from gelation to complete liquefaction. The decrease in ink resistance is believed to be due to the fact that the phenol-based curing agent used in Example 10 is more susceptible to the influence of ink swelling than the amine-based curing agents used in Examples 6 to 9. Furthermore, since a silane coupling agent was not added to Example 10, it is believed that the adhesion was further reduced.

[0047] An acid anhydride-based curing agent was used in Example 11. As a result, bleeding properties and ink resistance were reduced, similar to the case where a phenol-based curing agent was used in Example 11. The decrease in bleeding is believed to be due to the slower reaction rate and larger average particle size of the acid anhydride-based hardener compared to the amine-based hardener, while the decrease in ink resistance is believed to be due to the susceptibility to ink swelling compared to the amine-based hardener, just like the phenol-based hardener.

[0048] [Table 4]

[0049] Table 4 shows Comparative Examples 1 to 3. In Comparative Example 1, the weight average molecular weight of the epoxy resin mixture was less than 300, and the bleeding property was not achieved. This is believed to be because the epoxy resin bleeds out due to the high fluidity of the epoxy resin mixture during curing. On the other hand, in Comparative Example 2, the weight average molecular weight of the epoxy resin mixture was large, and the ink resistance was not achieved. This is believed to be because the reaction rate with the curing agent decreased due to the low fluidity of the epoxy resin. Furthermore, in Comparative Example 3, an epoxy resin that is solid at room temperature was dissolved instead of the coumarone resin, but the ink resistance was not achieved. This is believed to be because the coumarone resin does not absorb ink, while the epoxy resin absorbs ink between molecules.

[0050] The present invention includes the following configurations. [Configuration 1] A liquid ejection head in which an epoxy resin composition is used as an adhesive, the epoxy resin composition including an epoxy resin mixture and a powder curing agent, The epoxy resin mixture includes an epoxy resin that is liquid at room temperature and a coumarone resin that is soluble in the epoxy resin, The weight average molecular weight of the epoxy resin mixture is 300 or more and 600 or less. [Configuration 2] The liquid ejection head according to [Configuration 1], wherein the functional group equivalent of the epoxy resin in the epoxy resin mixture is 100 or more and 200 or less. [Configuration 3] A liquid ejection head according to [Configuration 1] or [Configuration 2], wherein the content of the coumarone resin in the epoxy resin mixture is 10 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass of the epoxy resin. [Configuration 4] The liquid ejection head according to any one of [Configuration 1] to [Configuration 3], wherein the hydroxyl value (mg KOH / g) of the coumarone resin is 50 or less. [Configuration 5] The liquid ejection head according to any one of [Configuration 1] to [Configuration 4], wherein the powder curing agent contained in the epoxy resin composition has a softening point of 80°C or higher and 100°C or lower. [Configuration 6] The liquid ejection head according to any one of [Configuration 1] to [Configuration 5], wherein the content of the powder curing agent contained in the epoxy resin composition is 40 parts by mass or more and 65 parts by mass or less with respect to 100 parts by mass of the epoxy resin. [Configuration 7] The liquid ejection head according to any one of [Configuration 1] to [Configuration 6], wherein the powder curing agent is an amine-based curing agent. [Configuration 8] The liquid ejection head according to any one of [Configuration 1] to [Configuration 7], wherein the powder curing agent has an average particle size of 70 nm or less. [Configuration 9] The liquid ejection head according to any one of [Configuration 1] to [Configuration 8], wherein the epoxy resin composition contains a silane coupling agent. [Configuration 10] A liquid ejection head including a recording element substrate that ejects liquid, a support member that supports the recording element substrate and has a supply flow path that supplies ink to the recording element substrate, and a flow path member that supplies liquid to the supply flow path, At least one bonding surface between any two of the recording element substrate, the support member, and the flow path member is An epoxy resin composition comprising an epoxy resin mixture and a powder curing agent, The epoxy resin mixture includes an epoxy resin that is liquid at room temperature and a coumarone resin that is soluble in the epoxy resin, A liquid ejection head comprising a cured product of an adhesive made of an epoxy resin composition in which the weight average molecular weight of the epoxy resin mixture is 300 or more and 600 or less.

[0051] The present invention also includes the following method. [Method 1] A method for manufacturing a liquid ejection head having a recording element substrate that ejects liquid, a support member that supports the recording element substrate and has a supply flow path that supplies liquid to the recording element substrate, and a flow path member that supplies liquid to the supply flow path, comprising the steps of: applying the adhesive to at least one joining surface between at least two of the recording element substrate, the support member, and the flow path member; A step of bonding the two members together; and a main curing process of thermally curing the adhesive to bond the two members together, The adhesive may include An epoxy resin composition comprising an epoxy resin mixture and a powder curing agent, The epoxy resin mixture includes an epoxy resin that is liquid at room temperature and a coumarone resin that is soluble in the epoxy resin, A method for manufacturing a liquid ejection head using an adhesive containing an epoxy resin composition in which the weight average molecular weight of the epoxy resin mixture is 300 or more and 600 or less. [Method 2] The method for producing a liquid ejection head according to [Method 1], wherein in the laminating step, the thickness of the epoxy resin composition after lamination is 10 μm or less. [Method 3] The method for manufacturing a liquid ejection head according to [Method 1] or [Method 2], further comprising a temporary fixing and curing step of temporarily fixing the two members with the adhesive prior to the main curing step. [Explanation of symbols]

[0052] 1 Liquid ejection head 2. Recording element board 3 Supply route 4 Support member 5 Flow path components 6 First flow path member 7 Second flow path member 8 Third flow path member

Claims

1. A liquid ejection head in which an epoxy resin composition is used as an adhesive, the epoxy resin composition including an epoxy resin mixture and a powder curing agent, The epoxy resin mixture includes an epoxy resin that is liquid at room temperature and a coumarone resin that is soluble in the epoxy resin, The weight average molecular weight of the epoxy resin mixture is 300 or more and 600 or less.

2. 2. A liquid ejection head according to claim 1, wherein the functional group equivalent of the epoxy resin in the epoxy resin mixture is 100 or more and 200 or less.

3. 3. The liquid ejection head according to claim 2, wherein the content of the coumarone resin contained in the epoxy resin mixture is 10 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass of the epoxy resin.

4. 4. The liquid ejection head according to claim 3, wherein the hydroxyl value (mg KOH / g) of the coumarone resin is 50 or less.

5. 3. The liquid ejection head according to claim 1, wherein the powder curing agent contained in the epoxy resin composition has a softening point of 80° C. or higher and 100° C. or lower.

6. 6. The liquid ejection head according to claim 5, wherein the content of the powder curing agent in the epoxy resin composition is 40 parts by mass or more and 65 parts by mass or less with respect to 100 parts by mass of the epoxy resin.

7. 7. A liquid ejection head according to claim 6, wherein the powdered hardener is an amine-based hardener.

8. 8. The liquid ejection head according to claim 7, wherein the powdered hardener has an average particle size of 70 nm or less.

9. 3. The liquid ejection head according to claim 1, wherein the epoxy resin composition contains a silane coupling agent.

10. A liquid ejection head including a recording element substrate that ejects liquid, a support member that supports the recording element substrate and has a supply flow path that supplies ink to the recording element substrate, and a flow path member that supplies liquid to the supply flow path, At least one bonding surface between any two of the recording element substrate, the support member, and the flow path member is An epoxy resin composition comprising an epoxy resin mixture and a powder curing agent, The epoxy resin mixture includes an epoxy resin that is liquid at room temperature and a coumarone resin that is soluble in the epoxy resin, A liquid ejection head comprising a cured product of an adhesive made of an epoxy resin composition in which the weight average molecular weight of the epoxy resin mixture is 300 or more and 600 or less.

11. A method for manufacturing a liquid ejection head having a recording element substrate that ejects liquid, a support member that supports the recording element substrate and has a supply flow path that supplies liquid to the recording element substrate, and a flow path member that supplies liquid to the supply flow path, comprising the steps of: applying the adhesive to at least one bonding surface between at least two of the recording element substrate, the support member, and the flow path member; a step of bonding the two members together; a main curing process of thermally curing the adhesive to bond the two members together, The adhesive may include An epoxy resin composition comprising an epoxy resin mixture and a powder curing agent, The epoxy resin mixture includes an epoxy resin that is liquid at room temperature and a coumarone resin that is soluble in the epoxy resin, The epoxy resin composition has a weight average molecular weight of 300 or more and 600 or less.

12. The method for producing a liquid ejection head according to claim 10, wherein in the laminating step, the thickness of the epoxy resin composition after lamination is 10 μm or less.

13. 12. The method for manufacturing a liquid ejection head according to claim 10, further comprising a temporary fixing and curing step of temporarily fixing the two members with the adhesive prior to the main curing step.

Citation Information

Patent Citations

  • Cap adhesive

    JP2015021011A

  • Resin composition and semiconductor device

    JP2019172911A

  • Sealing resin composition, and semiconductor device

    JP2021138809A