Method for manufacturing base material including vapor-deposited film, method for manufacturing base material including multilayer vapor-deposited film, and vapor deposition apparatus
By employing multiple electron guns to irradiate vapor deposition materials from different locations with controlled deposition rates, the method addresses the issue of foreign matter inclusion in large-sized vapor-deposited films, ensuring high productivity and quality in optical components.
Patent Information
- Application Number
- JP2023065865
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional methods for producing large-sized vapor-deposited films in optical components, such as near-infrared cut filters, increase the likelihood of foreign matter inclusion, leading to reduced yield and productivity in optical members.
A method involving the use of multiple electron guns to irradiate vapor deposition materials from different locations simultaneously, with specific content ratios and deposition rates to form vapor-deposited films, and a vapor deposition apparatus with multiple electron guns and controlled electron beam irradiation to minimize foreign substances.
The method enables the production of large-area vapor-deposited films with few foreign substances, maintaining high productivity and yield, suitable for optical components like near-infrared cut filters.
Smart Images

Figure 2024151992000009 
Figure 2024151992000010 
Figure 2024151992000011
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a substrate having a vapor-deposited film, a method for producing a substrate having a multilayer vapor-deposited film, and a vapor deposition apparatus. [Background technology]
[0002] Conventionally, optical members such as lenses for cameras and near-infrared cut filters have optical films formed on their surfaces in order to suppress light reflection or to transmit or reflect light of a specific wavelength. Vacuum deposition and sputtering are mainly used as methods for forming such optical films, and among them, vacuum deposition is mainly used for mass production applications because it is possible to form optical films of a large area at once.
[0003] In vacuum deposition, in order to prevent foreign matter from being mixed into the deposition film formed on the deposition target such as a substrate, deposition is performed in a vacuum chamber that has been evacuated to a vacuum. Inside the vacuum chamber, a hearth liner containing the deposition material and a deposition source including a heating source for heating and evaporating the deposition material are placed, and the substrate, which is the deposition target, is usually placed in a position facing the hearth liner (above the hearth liner).
[0004] As a method for heating the deposition material, electron beam deposition and resistance heating deposition are often used in the field of optical film formation. Among these, electron beam deposition is mainly used because it can irradiate electrons accelerated to very high energy, it can form a deposition film even when a deposition material with a high melting point is used, and it is easy to control the melting state of the deposition material by scanning the electron beam with a magnetic field, etc.
[0005] In recent years, for example, cameras have been required to capture images with higher resolution. This demand for higher pixel counts has led to demands for higher quality in the optical components used in cameras, and further in the optical films (evaporated films) formed on their surfaces. In particular, there is a demand for evaporated films to have fewer foreign bodies (defects). As a technique for satisfying such a demand, for example, the technique described in Patent Document 1 has been proposed. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2018-135593 A Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, with the trend toward higher image quality, particularly in smartphone cameras, the sensors used in the cameras have become larger. This has led to a demand for larger optical components, such as near-infrared cut filters, and therefore larger optical films (vapor-deposited films) used in the sensors. However, when attempting to form a large vapor-deposited film using conventional vapor-deposited film manufacturing methods, the area of the vapor-deposited film to be formed becomes large, which inevitably increases the possibility of the film containing foreign matter, thereby reducing the yield of the optical components obtained and decreasing productivity.
[0008] The present invention has been made in view of the above, and an object of the present invention is to provide a method for producing a substrate having a (multi-layer) vapor-deposited film with little foreign matter. [Means for solving the problem]
[0009] As a result of intensive research into solving the above problems, the present inventors have found that the above problems can be solved by the following configuration examples, and have thus completed the present invention. In the present invention, the expression "A to B" expressing a numerical range is synonymous with "A or more, B or less," and A and B are included in the numerical range.
[0010] [1] A method for producing a substrate having a vapor-deposited film, comprising the following steps (1) or (2): Step (1): A step of irradiating one deposition material A with electron beams from multiple electron guns to evaporate the deposition material A and form a deposition film of the deposition material A on a substrate (however, there is a time (band) during which one deposition material A is simultaneously irradiated with electron beams from multiple electron guns). Step (2): A step of irradiating each of a plurality of deposition materials A (wherein the plurality of deposition materials A have the same main component) with an electron beam from an electron gun corresponding to each deposition material A to evaporate the deposition material A and form a deposition film of the deposition material A on the substrate (wherein there is a time (band) during which the electron beams from the electron guns corresponding to each of the plurality of deposition materials A are irradiated simultaneously on each deposition material A).
[0011] [2] The method for producing a substrate having a vapor-deposited film according to [1], wherein the vapor deposition material A includes a vapor deposition material A1 selected from Si, SiO2, Ti2O3, Ti3O5, TiO2, Nb2O5, HfO2, La2O3, Al2O3, Y2O3, Yb2O3, Ta2O5, MgF2, Ag and ZrO2.
[0012] [3] The method for producing a substrate having a vapor-deposition film according to [2], wherein the content of the one selected from the vapor deposition materials A1 in one vapor deposition material A in the step (1), and the content of the one selected from the vapor deposition materials A1 in each vapor deposition material A in the step (2) are each 90 mass% or more.
[0013] [4] A method for producing a substrate having a vapor-deposited film according to any one of [1] to [3], which satisfies the following requirement (i): Requirement (i): The irradiation area of the electron beam from the electron gun irradiating the deposition material A is S [cm 2 ], and the deposition speed at which the deposition film of the deposition material A is formed is V [Å / sec], V / S is 1.5 [Å / (sec cm 2 )] is less than
[0014] [5] The irradiation area S is 5 cm 2 The method for producing a substrate having a vapor-deposited film according to [4] above.
[0015] [6] A step I of forming a vapor-deposited film a of a vapor-deposition material A on a substrate by the method for producing a substrate having a vapor-deposited film according to any one of [1] to [5]; [1] to [5], the method for producing a substrate having a vapor-deposited film according to any one of the above-mentioned items, comprising: a step II of forming a vapor-deposited film b of the vapor-deposited material B on the substrate having the vapor-deposited film a by using a vapor-deposited material B having a refractive index different from that of the vapor-deposited material A instead of the vapor-deposited material A; A method for producing a substrate having a multilayer vapor-deposited film, comprising:
[0016] [7] The method for producing a substrate having a multilayer vapor-deposited film according to [6], wherein the multilayer vapor-deposited film has a light transmittance of 10% or less in a wavelength range of 400 to 1600 nm.
[0017] [8] A deposition apparatus for forming a deposition film of a deposition material on a substrate by evaporating the deposition material, comprising the following configuration (I) or (II): Configuration (I): The deposition device includes a deposition material placement section for placing a deposition material, and a plurality of electron guns for irradiating an electron beam to each deposition material placement section. Configuration (II): The deposition device includes a plurality of deposition material placement sections for placing deposition materials therein, and an electron gun for irradiating an electron beam to at least two of the deposition material placement sections is provided.
[0018] [9] The deposition apparatus according to [8], further comprising a control device for controlling irradiation of the electron beam by the electron gun.
[0019]
[10] The deposition apparatus according to [8] or [9], which is an ion-assisted deposition apparatus having at least one selected from a neutralization gun and an ion gun.
[0020]
[11] A correction plate for adjusting a thickness of a deposition film to be formed is provided above the deposition material placement unit, The deposition apparatus according to any one of [8] to
[10] , wherein the number of the correction plates is equal to or greater than the number of the electron guns.
[0021]
[12] The deposition apparatus according to any one of [8] to
[11] , wherein the number of electron guns in the deposition apparatus is three or more. Effect of the Invention
[0022] According to the present invention, a substrate having a (multi-layer) vapor-deposited film with little foreign matter can be produced with high productivity (high yield). In particular, according to the present invention, even when a large-area (multi-layer) vapor-deposited film is formed, it is possible to form a (multi-layer) vapor-deposited film with little foreign matter. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is a schematic diagram (plan view) showing an example of the positional relationship between a deposition material placement section for placing a deposition material and an electron gun for irradiating an electron beam onto the deposition material placed in the deposition material placement section. [Diagram 2] FIG. 2 is a schematic diagram (side view) showing an example of a vapor deposition apparatus. [Diagram 3] FIG. 3 is a schematic diagram (plan view) showing an example in which two types of deposition materials are placed in the hearth liner 9-2. [Figure 4] FIG. 4 is an explanatory diagram (side view) showing a method for measuring the number of foreign matter particles in the following example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] <Method for producing a substrate having a vapor-deposited film> The method for producing a substrate having a vapor-deposited film (hereinafter also referred to as the present laminate) according to the present invention (hereinafter also referred to as the present production method) includes the following steps (1) or (2). In short, this production method is a method in which, when forming a vapor-deposited film of vapor deposition material A, vapor deposition material A evaporates from at least two different locations, and a vapor-deposited film of vapor deposition material A is formed on a substrate. Step (1): A step of irradiating one deposition material A with electron beams from multiple electron guns to evaporate the deposition material A and form a deposition film of the deposition material A on a substrate (however, there is a time (band) during which one deposition material A is simultaneously irradiated with electron beams from multiple electron guns). Step (2): A step of irradiating each of a plurality of deposition materials A (wherein the plurality of deposition materials A have the same main component) with an electron beam from an electron gun corresponding to each deposition material A to evaporate the deposition material A and form a deposition film of the deposition material A on the substrate (wherein there is a time (band) during which the electron beams from the electron guns corresponding to each of the plurality of deposition materials A are irradiated simultaneously on each deposition material A).
[0025] According to the present production method, a substrate having a (multi-layer) vapor-deposited film with few foreign matters can be produced with high productivity (high yield) even if the substrate is large. In addition, the foreign matter in the vapor deposition film is mainly due to bumping (so-called splash) that occurs during vapor deposition. Although it is possible to reduce the film formation speed in order to suppress the generation and adhesion of foreign matter in the vapor deposition film, such a reduction in the film formation speed leads to an increase in takt time, which reduces productivity. Furthermore, the increase in takt time also increases the possibility that foreign matter will adhere to the vapor deposition film. For this reason, it is desirable to keep the film formation speed as low as possible, but with conventional methods, it has not been easy to suppress the generation and adhesion of foreign matter without reducing the film formation speed. On the other hand, according to the present production method, it is possible to suppress the generation and adhesion of foreign matter in the evaporated film without reducing the film formation rate.
[0026] In addition, when warping occurs in the laminate formed by the present manufacturing method, in order to eliminate the warping, the surface of the base material on which the vapor-deposited film is formed may be irradiated with electromagnetic waves such as ultraviolet rays. In addition, when irradiating with electromagnetic waves, irradiation may be performed during the formation of the vapor-deposited film, or irradiation may be performed separately after the formation of the vapor-deposited film.
[0027] <Vapor deposition equipment> Specifically, this production method is preferably carried out using a deposition apparatus. The deposition apparatus is not particularly limited as long as it is a deposition apparatus that can satisfy the above-mentioned step (1) or (2), and any deposition apparatus known in the art can be used as long as it is configured so that the relationship between the deposition material and the electron beam from the electron gun satisfies the above-mentioned step (1) or (2).
[0028] The following configuration (I) or (II) can be given as an example of a configuration in which the relationship between the deposition material and the electron beam from the electron gun satisfies the step (1) or (2). The deposition apparatus may be a deposition apparatus including the following configuration (I), a deposition apparatus including the following configuration (II), or a deposition apparatus including the following configurations (I) and (II). Configuration (I): The deposition device includes a deposition material placement section for placing a deposition material, and a plurality of electron guns for irradiating an electron beam to each deposition material placement section. Configuration (II): The deposition device includes a plurality of deposition material placement sections for placing deposition materials therein, and an electron gun for irradiating an electron beam to at least two of the deposition material placement sections is provided.
[0029] FIG. 1 is a schematic diagram (plan view, viewed from above) showing an example of the positional relationship between a deposition material placement section for placing a deposition material and an electron gun for irradiating an electron beam onto the deposition material placed in the deposition material placement section. FIG. 1(A) shows an example of the configuration (I), and FIG. 1(B) shows an example of the configuration (II).
[0030] FIG. 1A shows an example in which two different electron guns 5-1 and 5-2 for irradiating electron beams are provided for one deposition material placement unit 9-1. The step (1) can be performed by placing deposition material A in one of the deposition material placement sections 9-1, irradiating electron beams from electron guns 5-1 and 5-2, and evaporating the deposition material A to form a deposition film of the deposition material A on the substrate.
[0031] In the case of the above-mentioned configuration (I), it is preferable that the multiple electron guns that irradiate electron beams to one deposition material placement section 9-1 are arranged so that the electron beams from each electron gun are irradiated to different locations on the deposition material placement section 9-1. 1A shows an embodiment in which two electron guns for irradiating an electron beam are provided for one deposition material placement section 9-1, but the number of electron guns for irradiating an electron beam for one deposition material placement section 9-1 may be three or more. The number of electron guns for irradiating an electron beam for one deposition material placement section is preferably 2 to 6, and more preferably 2 to 4. In the configuration (I), for example, one deposition material placement section may have a plurality of electron guns for irradiating an electron beam, and the electron guns may be fixed in position and the deposition material placement section may be moved (rotated) while irradiating the electron beam, or the deposition material placement section may be fixed and the electron guns may be moved while irradiating the electron beam. Of these, the former is preferred from the viewpoint of ease of configuration of the deposition apparatus, etc. For example, when two electron guns are used to irradiate electron beams onto one circular deposition material placement section, the positions of the electron guns are fixed, and the deposition material placement section is moved (rotated) while irradiating the electron beams from the electron guns, it is preferable that the two electron guns are positioned 90 to 180° apart (positions 90° apart in Figure 1(A)).
[0032] 1B has a plurality of deposition material placement parts 9-2, and at least two of the deposition material placement parts 9-2 are provided with electron guns for irradiating an electron beam. In FIG. 1B, two deposition material placement parts 9-2 at the 6 o'clock and 9 o'clock directions in FIG. 1B out of the 12 deposition material placement parts 9-2 are provided with electron guns 5-3 and 5-4 for irradiating an electron beam. The step (2) can be performed by placing deposition material A (wherein the deposition materials A have the same main component) in at least two of the deposition material placement sections 9-2 (e.g., deposition material placement sections 9-2 at the 6 o'clock and 9 o'clock positions out of the 12 deposition material placement sections 9-2), irradiating the deposition material A with an electron beam from an electron gun (e.g., electron guns 5-3 and 5-4) corresponding to each deposition material A, and evaporating the deposition material A to form a deposition film of the deposition material A on the substrate. 1(B), the electron gun corresponding to the deposition material arranged in the deposition material arrangement portion 9-2 at the 6 o'clock direction among the 12 deposition material arrangement portions 9-2 is the electron gun 5-3, and the electron gun corresponding to the deposition material arranged in the deposition material arrangement portion 9-2 at the 9 o'clock direction is the electron gun 5-4. In addition, when irradiating the electron beam by the electron gun while rotating the deposition material arrangement portion as described below, for example, when rotating the deposition material arrangement portion by 90° clockwise, the electron gun corresponding to the deposition material arranged in the deposition material arrangement portion 9-2 at the 6 o'clock direction before rotation in FIG. 1(B) may be the electron gun 5-4.
[0033] In addition, while FIG. 1(B) shows an embodiment having 12 deposition material placement sections 9-2, in the configuration (II) described above, the number of the deposition material placement sections provided in the deposition device is not particularly limited, and is preferably 2 to 36, and more preferably 2 to 30, from the viewpoint of reducing interference between electron beams from adjacent electron guns, etc. In addition, while FIG. 1(B) shows an embodiment having two electron guns 5-3 and 5-4, the deposition apparatus may be provided with the same number of electron guns as the deposition material placement sections 9-2 provided in the deposition apparatus, and it is preferable to provide 2 to 4 electron guns (however, the number should be equal to or less than the number of the deposition material placement sections provided in the deposition apparatus) in the deposition apparatus. In the configuration (II), for example, the position of the electron gun may be fixed and the deposition material placement part may be rotated (moved) by the rotation mechanism 11 while irradiating the electron beam from the electron gun, or the deposition material placement part may be fixed and the electron gun may be moved while irradiating the electron beam from the electron gun. Of these, the former is preferred from the viewpoint of ease of configuration of the deposition apparatus, etc. For example, when multiple deposition material placement sections are arranged to form a circle as a whole (e.g., FIG. 1(B)), the number of electron guns that irradiate the electron beam is two, the positions of the electron guns are fixed, and the electron beam is irradiated by the electron guns while rotating (moving) the entire multiple deposition material placement sections, it is preferable to arrange the two electron guns at positions 90 to 180° apart (at positions 90° apart in FIG. 1(B)).
[0034] The deposition apparatus may be, for example, a deposition container for performing a step of evaporating a deposition material to form a deposition film of the deposition material on a substrate; a substrate placement unit provided in an upper portion of the deposition container and configured to place and hold the substrate; a deposition material placement part that is provided in a lower part of the deposition container opposite to the base material placement part and that places a deposition material that is a raw material of a deposition film; an electron gun that irradiates an electron beam onto the evaporation material placed in the evaporation material placement section to evaporate the evaporation material; An example of the deposition apparatus is a deposition apparatus having the following structure.
[0035] FIG. 2 shows a schematic diagram (side view) of an example of a more specific configuration of the deposition apparatus. FIG. 2 shows a deposition container 10 for performing a process of evaporating a deposition material to form a deposition film of the deposition material on a substrate, a substrate placement unit 1 that is provided in an upper portion of the deposition container 10 and that places and holds the substrate; deposition material placement units 4-1 and 4-2, which are provided in a lower portion of the deposition container 10 opposite the substrate placement unit 1 and in which deposition materials serving as raw materials for a deposition film are placed; The deposition apparatus further includes electron guns 5-1 to 5-3 which irradiate the deposition materials placed in the deposition material placement units 4-1 and 4-2 with an electron beam to evaporate the deposition materials.
[0036] <Deposition container> The deposition vessel is not particularly limited, and examples thereof include known deposition vessels (eg, vacuum chamber, vacuum bell jar, vacuum tank) that are generally used in deposition devices. The deposition vessel may be, for example, a vessel made of iron, stainless steel, an aluminum alloy, or the like, which has high airtightness.
[0037] In the deposition container, it is preferable to form a deposition film by reducing the pressure (particularly vacuum) inside the container. In this case, a vacuum exhaust part that reduces the pressure (particularly vacuum) inside the deposition container is usually connected via a pipe. The deposition vessel may also be provided with a gas introduction means for introducing a gas such as argon gas for adjusting the degree of vacuum, or for introducing a trace amount of oxygen gas or the like as a process gas for forming a stable oxide film.
[0038] The pressure in the deposition vessel when the deposition material is evaporated to form a deposition film of the deposition material on the substrate is preferably 1×10 -2 Pa or less, preferably 2×10 -3 Pa or less.
[0039] <Base material placement section> The substrate placement section is a location where the substrate is placed and held. The substrate placement section is not particularly limited as long as it can hold the substrate within the deposition vessel, but it preferably has a dome shape as shown in FIG. 2 from the standpoint of uniformity of the deposited film thickness, etc. The substrate holding section is preferably a member capable of rotating the substrate while holding it, for example, by one or more rotation mechanisms. The substrate holding unit may be a member equipped with a transport means for transporting the substrate in a roll-to-roll manner within the deposition apparatus.
[0040] <Deposition material placement section> The deposition material placement section is a section where the deposition material is placed in the deposition device, and typically, a deposition material placement container containing the deposition material is placed in the deposition material placement section. The number of deposition material placement parts provided in the deposition device may be one or two or more. When the deposition apparatus includes one deposition material placement section, at least two electron guns are used so that the one deposition material placement section is irradiated with an electron beam from at least two electron guns. In this case, it is preferable to provide an electron gun or a deposition material placement section so that at least two different positions on the deposition material placement section are irradiated with an electron beam from each of the electron guns. When the deposition apparatus includes two or more deposition material placement sections, the deposition apparatus includes at least two electron guns. When the deposition apparatus includes two or more deposition material placement sections, the number of electron guns irradiating an electron beam to one of the deposition material placement sections may be two (e.g., FIG. 2) or three or more. The deposition material placement section may be provided with a rotation mechanism as shown at 11 in FIG. 1(B).
[0041] One type of deposition material may be placed in one deposition material placing section or deposition material placing container, or two or more types of deposition materials may be placed in one deposition material placing section or deposition material placing container. When two or more types of deposition materials are placed in one deposition material placing section or deposition material placing container, it is preferable to place each of the two or more deposition materials so that each of the two or more deposition materials can be evaporated by irradiation with an electron beam to form a deposition film. Specifically, for example, when two or more types of deposition materials are placed in one deposition material placing container, it is preferable to place each of the deposition materials in the deposition material placing container so that each of the deposition materials is exposed (so that each of the deposition materials can be seen when viewed from above the opening of the deposition material placing container) (e.g., FIG. 3).
[0042] The deposition material container is not particularly limited as long as it does not react with the deposition material and has sufficient heat resistance, and any conventional container that has been used for deposition (e.g., hearth liner, crucible) can be used. Examples of the deposition material container include containers made of metal, metal alloy, and ceramics, and may be appropriately selected depending on the type of deposition material. The shape of the deposition material placement container is not particularly limited, but it is usually a hollow container with an open top, and it is preferable that the shape does not vary in cross section in a direction perpendicular to the vertical direction of the tube, such as a cylindrical shape or a rectangular tube shape.
[0043] Electron Gun The type of electron gun is not particularly limited, and any conventionally known electron gun can be used, including, for example, a linear electron gun and a deflection electron gun. The electron gun is usually connected to a power supply device for emitting the electron beam. When a linear electron gun is used, it is preferable to set a certain angle and position in advance and install the electron gun in the deposition apparatus so that the electron beam hits the deposition material linearly. When a deflection type electron gun is used, it is preferable to deflect electrons emitted from the electron gun by a magnetic field so that the electron beam strikes the deposition material.
[0044] The number of electron guns provided in the deposition apparatus is not limited to the number of deposition material placement sections and is at least two. From the viewpoint of easily obtaining a deposition apparatus capable of easily forming a multilayer deposition film, it is preferable that the number of electron guns provided in the deposition apparatus is three or more.
[0045] <Other configurations> As the other components of the deposition apparatus other than the deposition vessel, the substrate placement unit, the deposition material placement unit, and the electron gun, any components that have been used in conventionally known deposition apparatuses can be adopted without any restrictions.
[0046] It is preferable that the deposition apparatus is provided with a control device that controls the irradiation of the electron beam by the electron gun, specifically, adjusts the irradiation area of the electron beam, adjusts the electron beam output (adjusts the deposition speed of the evaporated film formed by the irradiation of the electron beam), and further controls the timing of the irradiation of the electron beam by the electron gun.
[0047] The deposition apparatus is preferably provided with a correction plate (e.g., 2-1 and 2-2 in FIG. 2) located above the deposition material placement section (between the substrate placement section and the deposition material placement section) for adjusting the thickness of the deposition film to be formed; specifically, for adjusting the thickness so that a deposition film of approximately the same thickness is obtained regardless of which part of the substrate placement section the substrate is placed on.
[0048] In the deposition apparatus, in a stage where bumping of the deposition material is likely to occur, such as at the start of deposition, in order to suppress deposition of the deposition material onto the substrate due to the bumping and to suppress adhesion of deposition materials other than the desired deposition material to the substrate, it is preferable to provide a shutter (e.g., 3-1 and 3-2 in FIG. 2 ) between the deposition material placement part and the substrate placement part (e.g., above the deposition material placement part). In particular, when two or more deposition material placement sections are provided in the deposition container and the deposition material is to be evaporated from only some of the deposition material placement sections and deposited on the substrate, it is preferable to provide shutters from the remaining deposition material placement sections so that the deposition material placed therein does not evaporate and is deposited on the substrate.
[0049] The deposition apparatus is preferably an ion-assisted deposition apparatus having at least one selected from a neutralization gun (eg, 6 in FIG. 2) and an ion gun (eg, 7 in FIG. 2). By using a neutralization gun and / or an ion gun, a dense vapor deposition film can be easily formed.
[0050] The deposition apparatus may have a thickness control unit including a quartz crystal oscillator (e.g., 8 in FIG. 2) or an optical reflectance measuring device for monitoring the thickness of the deposited film formed, and may also be provided with a thermometer, a vacuum gauge, a heating device, a cooling device, a substrate rotation mechanism, and the like so as to observe the environment inside the deposition apparatus during film formation and form a desired deposited film.
[0051] <Base material> The substrate is not particularly limited, and any substrate on which a vapor-deposited film is to be formed may be used. Examples of the material of the substrate include glass, reinforced glass, special glass, and resin. The substrate may have two or more glass layers (including glass, reinforced glass, and special glass), may have two or more resin layers, or may have one or more glass layers and one or more resin layers. The substrate may have a layer having functions such as light absorption, electrical conductivity, antistatic effect, foreign matter adhesion prevention effect, scratch prevention effect, antifogging property, heat resistance improvement effect, gas barrier property, high elasticity, scratch removal effect, flatness, rough surface property, moisture absorption, and anti-aging effect. The substrate preferably includes a layer having a glass transition temperature of 140° C. or higher, and more preferably includes a layer made of resin (resin layer) because it is less likely to break.
[0052] Examples of the glass include silicate glass, borosilicate glass, phosphate glass, copper phosphate glass, fluorophosphate glass, and copper fluorophosphate glass. Examples of the tempered glass include physically tempered glass, tempered laminated glass, and chemically tempered glass. Among these, chemically tempered glass is preferred because it has a thin compression layer and can be processed to reduce the thickness of the substrate. Examples of the special glass include alumina glass, yttrium aluminate, and yttrium oxide.
[0053] Examples of the resin include polyester resins, polyether resins, acrylic resins, polyolefin resins, polycycloolefin resins, norbornene resins, polycarbonate resins, enethiol resins, epoxy resins, polyamide resins, polyimide resins, polyurethane resins, and polystyrene resins. Among these, norbornene resins, polyimide resins, and polyether resins are preferred. The resins may be used alone or in combination of two or more.
[0054] The base material may further contain additives such as a (near) infrared absorbing agent, a (near) ultraviolet absorbing agent, an antioxidant, an ultraviolet absorbing agent, a dispersing agent, a flame retardant, a plasticizer, a heat stabilizer, a light stabilizer, and a metal complex compound, within a range that does not impair the effects of the present invention. Each of these additives may be used alone or in combination of two kinds. The content of these additives is appropriately selected depending on the desired properties, but is, for example, usually 0.01 to 5.0 parts by mass, and preferably 0.05 to 2.0 parts by mass, per 100 parts by mass of glass or resin.
[0055] The base material preferably has 1 to 5 layers. When the base material has six or more layers, there are concerns about the adhesion between the layers and an increase in manufacturing costs.
[0056] The total thickness of the base material is preferably 30 to 300 μm, and within this range, the present laminate obtained can be suitably used for thin solid-state imaging devices and the like. The total thickness of the substrate is more preferably 30 to 220 μm, and further preferably 40 to 150 μm. If the total thickness is within this range, the present laminate obtained can be suitably used for a thin solid-state imaging device having a total thickness of 6.5 mm or less. If the total thickness of the substrate is less than 30 μm, there is a concern that the substrate may be prone to warping or cracking.
[0057] <Deposition material A> The deposition material A is not particularly limited as long as it is a material that can be evaporated by an electron beam from an electron gun, and may be appropriately selected depending on the physical properties of the deposition film to be formed. Specific examples of the deposition material A include metal (semi)metals, metal (semi)oxides, fluorides, and sulfides. The deposition material A preferably includes a deposition material A1 selected from Si, SiO2, Ti2O3, Ti3O5, TiO2, Nb2O5, HfO2, La2O3, Al2O3, Y2O3, Yb2O3, Ta2O5, MgF2, Ag, and ZrO2.
[0058] <Process (1)> In step (1), one deposition material A is irradiated with electron beams from multiple electron guns to evaporate the deposition material A and form a deposition film of the deposition material A on a substrate. However, there is a time (band) during which one deposition material A is irradiated with electron beams from multiple electron guns at the same time. The "one vapor deposition material A" refers to one vapor deposition material placement portion, particularly the entire vapor deposition material placed in a vapor deposition material placement container (eg, hearth liner). The step (1) is preferably a step of irradiating electron beams from a plurality of electron guns to different locations of an evaporation material A placed in one evaporation material container to evaporate the evaporation material A. In this step (1), there is required to be a period (zone) during which one deposition material A is simultaneously irradiated with electron beams from multiple electron guns, and it is not necessary for the electron beams from multiple electron guns to be irradiated with one deposition material A at exactly the same time.
[0059] In the step (1), a vapor-deposited film of the vapor deposition material A may be formed on the entire surface of the substrate, or may be formed only on a part of the substrate. In the step (1), it is preferable to form a vapor-deposited film of the vapor deposition material A on one or both of the main surfaces of the substrate. Here, the main surface of the substrate refers to the surface of the substrate that has the largest area.
[0060] The content of one of the deposition materials A1 in one deposition material A in step (1) is preferably 90 mass% or more, more preferably 95 to 100 mass%, from the viewpoints that bumping of the deposition material can be suppressed, and a deposition film having a substantially uniform refractive index can be easily formed regardless of the position of the substrate in the substrate placement part, etc. In other words, one embodiment of one deposition material A in step (1) is preferably composed of only one of the deposition materials A1.
[0061] The number of the plurality of electron guns used when irradiating one deposition material A with an electron beam in the step (1) is preferably 2 to 4, more preferably 2 to 3, and particularly preferably 2.
[0062] In step (1), the total irradiation area S of the electron beams from the multiple electron guns irradiating the deposition material A is preferably 5 cm 2 More than 8cm, preferably 2 The upper limit of the irradiation area S is preferably 12 cm 2 It is. When the irradiation area S is within the above range, it is possible to achieve both a foreign matter reduction effect and a high film formation rate. 2 If the temperature rise of the deposition material caused by the irradiation of the electron beam is kept constant, the deposition rate can be stabilized.
[0063] In step (1), it is desirable to irradiate the electron beam by adjusting the electron beam output (EB output) so that the total deposition rate V of the evaporated film formed by each electron gun is preferably 1 Å / sec or more, more preferably 2 Å / sec or more. The upper limit of the deposition rate V is preferably 14 Å / sec. When the deposition rate V is within the above range, the tact time is not extended, and the desired present laminate can be easily formed by a method with excellent productivity.
[0064] In step (1), the total irradiation area of each of the electron beams from the multiple electron guns is defined as S [cm 2 ], and the total deposition rate of the vapor-deposited film formed in step (1) is V [Å / sec], V / S is preferably 1.5 Å / (sec cm 2 ), more preferably 0.1 to 1.0 Å / (sec cm 2 ) or less, and more preferably 0.2 to 0.8 Å / (sec cm 2 ). When the V / S is within the above range, a vapor-deposited film containing few foreign matters can be easily formed without decreasing the film formation rate.
[0065] <Process (2)> In step (2), a plurality of deposition materials A (each of which has the same main component) are irradiated with an electron beam from an electron gun corresponding to each deposition material A to evaporate the deposition material A and form a deposition film of the deposition material A on the substrate. However, there is a time (band) during which the electron beams from the electron guns corresponding to each of the deposition materials A are irradiated simultaneously on each deposition material A. The phrase "the multiple vapor deposition materials A have the same vapor deposition material as a main component" means that the multiple vapor deposition materials A are all vapor deposition materials whose main component is vapor deposition material A, specifically, the content of vapor deposition material A in each of the multiple vapor deposition materials used is 80 mass % or more, and the content is preferably 90 mass % or more.
[0066] The "plurality of deposition materials A" corresponds to using (placing in a vacuum deposition apparatus) a plurality of deposition material placement sections, particularly deposition material placement containers (e.g., hearth liners), containing deposition material A, or to using (placing in a vacuum deposition apparatus) one deposition material placement section, particularly one deposition material placement container containing deposition material A in two or more different locations (e.g., positions B and C of hearth liner 9-2 used in deposition condition 3-1 below) of a single deposition material placement section, particularly a deposition material placement container (e.g., hearth liner). When the deposition material A is placed in one deposition material placement section, particularly in two or more different locations in a deposition material placement container, it is preferable to place each deposition material in such a way that each of the deposition materials in the two or more different locations can be evaporated by irradiation with an electron beam to form a deposition film (e.g., FIG. 3).
[0067] In the step (2), there is only required a time (band) during which each of the multiple deposition materials A is simultaneously irradiated with an electron beam from a corresponding electron gun, and it is not necessary for each deposition material A to be irradiated with an electron beam from a corresponding electron gun at exactly the same time. The number of electron guns corresponding to one deposition material A may be one or more, but it is preferable that the number of electron guns is one.
[0068] In the step (2), a vapor-deposited film of the vapor deposition material A may be formed on the entire surface of the substrate, or may be formed only on a part of the substrate. In the step (2), it is preferable to form a vapor-deposited film of the vapor deposition material A on one or both of the main surfaces of the substrate.
[0069] The content of one of the deposition materials A1 in each deposition material A in step (2) is preferably 90% by mass or more, more preferably 95 to 100% by mass, from the viewpoints that bumping of the deposition material can be suppressed, and a deposition film having a substantially uniform refractive index can be easily formed regardless of the position of the substrate in the substrate placement section, etc. In other words, it is also preferable that one embodiment of each of the multiple deposition materials A in step (2) is composed of only one of the deposition materials A1.
[0070] The number of the multiple deposition materials A used in step (2) is preferably 2 to 4, more preferably 2 to 3, and particularly preferably 2.
[0071] In step (2), the total irradiation area S of the electron beams from the corresponding electron guns irradiating each of the multiple deposition materials A is preferably 5 cm 2 More than 8cm, preferably 2 More than 10cm, more preferably 2 The upper limit of the irradiation area S is preferably 12 cm 2 It is. When the irradiation area S is within the above range, it is possible to achieve both a foreign matter reduction effect and a high film formation rate.
[0072] In step (2), it is desirable to irradiate the electron beam by adjusting the electron beam output (EB output) so that the total deposition rate V of the evaporated film formed by each electron gun is preferably 2 Å / sec or more, more preferably 3 Å / sec or more. The upper limit of the deposition rate V is preferably 20 Å / sec. When the deposition rate V is within the above range, the tact time is not extended, and the desired present laminate can be easily formed by a method with excellent productivity.
[0073] In step (2), the total irradiation area S [cm 2 ] of the electron beams from the corresponding electron guns irradiating each of the multiple deposition materials A 2 ] and the total deposition rate of the vapor-deposited film formed in step (2) is V [Å / sec], V / S is preferably 1.5 Å / (sec cm 2), more preferably 0.1 to 1.0 Å / (sec cm 2 ) or less, and more preferably 0.2 to 0.8 Å / (sec cm 2 ). When the V / S is within the above range, a vapor-deposited film containing few foreign matters can be easily formed without decreasing the film formation rate.
[0074] <Method of manufacturing a substrate having a multilayer deposition film> The present production method may be a method for producing a substrate having a multilayer vapor-deposited film. Since the substrate having the multilayer vapor-deposited film is also one embodiment of the substrate having a vapor-deposited film, the substrate will hereinafter be referred to as the present laminate. The method for producing a substrate having a multilayer vapor deposition film is preferably a method including the following steps I and II. Step I: A step of forming a vapor deposition film a of a vapor deposition material A on a substrate by the present manufacturing method. Step II: In the present manufacturing method, a step of forming a vapor-deposited film b of the vapor-deposited material B on the substrate having the vapor-deposited film a by using a vapor-deposited material B having a refractive index different from that of the vapor-deposited material A instead of the vapor-deposited material A.
[0075] In addition, when warping occurs in the substrate having the multilayer deposition film formed by the manufacturing method of the substrate having the multilayer deposition film, in order to eliminate the warping, the surface of the substrate on which the multilayer deposition film is formed may be irradiated with electromagnetic waves such as ultraviolet rays. In addition, when irradiating with electromagnetic waves, irradiation may be performed during the formation of the multilayer deposition film, or irradiation may be performed separately after the formation of the multilayer deposition film.
[0076] In the method for producing a substrate having a multilayer vapor-deposited film, the multilayer vapor-deposited film may be formed on the entire surface of the substrate, or may be formed on only a part of the substrate. In the method for producing a substrate having a multilayer vapor-deposited film, it is preferable to form a multilayer vapor-deposited film on one or both of the main surfaces of the substrate, and it is more preferable to form a multilayer vapor-deposited film on both of the main surfaces of the substrate.
[0077] In the method including the steps I and II, the deposition material A and the deposition material B are simply defined as different deposition materials. For example, when three kinds of deposition materials A to C are used, the method including the steps I and II may include a step of forming a deposition film a of the deposition material A (=step I), a step of forming a deposition film b of the deposition material B (=step II), a step of forming a deposition film c of the deposition material C (=step I), a step of forming a deposition film a of the deposition material A (=step II), and a step of forming a deposition film b of the deposition material B (=step I), in this order.
[0078] In the method including the steps I and II, the steps I and II may be performed alternately. For example, the step I may be performed two or more times, followed by the step II and then the step I. The order in which the steps I and II are performed is not particularly limited, but it is preferable to perform the steps I and II alternately.
[0079] When the method for producing a substrate having a multilayer vapor deposition film includes step I multiple times, the present production method may be the same or different in each step I. For example, when step I is performed twice, the first step I may be step (1), and the second step I may be step (2). When step I is performed multiple times, it is preferable that the present production method is the same in each step I. The same applies to the case where step II is carried out multiple times.
[0080] Specific examples of the method including the steps I and II include: A method in which a deposition material disposing container containing a deposition material A and a deposition material disposing container containing a deposition material B are placed in one deposition container, and the step I is first performed on the deposition material A, and then the step II is performed on the deposition material B (repeated); or A method of placing a deposition material container in which a deposition material A and a deposition material B are placed in a different location from the deposition material A in a deposition container, and first performing the step I on the deposition material A and then performing the step II on the deposition material B (repeated); One example of a method is to use two connected deposition vessels a and b, place a deposition material placement vessel containing deposition material A in the deposition vessel a, and place a deposition material placement vessel containing deposition material B in the deposition vessel b, and then perform (repeated) step I on the deposition material A in the deposition vessel a in which a substrate is placed, and then move the substrate to the deposition vessel b and perform step II on the deposition material B in the deposition vessel b.
[0081] The deposition material B is a material that is evaporated by an electron beam from an electron gun, and is not particularly limited as long as it has a refractive index different from that of the deposition material A, and may be appropriately selected depending on the physical properties of the deposition film to be formed. Specifically, the same materials as those listed in the column for the deposition material A can be used.
[0082] The multilayer vapor deposition film may be, for example, a multilayer vapor deposition film in which high refractive index material layers and low refractive index material layers are alternately laminated. To form such a multilayer deposition film, for example, a method may be used in which a high refractive index material is used as deposition material A and a low refractive index material is used as deposition material B, and the above-mentioned steps I and II are carried out alternately.
[0083] As the high refractive index material, a material having a refractive index of 1.7 or more can be used, and a material having a refractive index in the range of 1.7 to 2.5 is usually selected. Examples of such materials include TiO2, Ti2O3, Ti3O5, CeO2, ZrO2, Ta2O5, Nb2O5, La2O3, Y2O3, Yb2O3, ZnO, ZnS, In2O3, ZnO, ZnS, In2O3, WO3, Si, and HfO2 as main components, and titanium oxide, tin oxide, and / or cerium oxide are contained in small amounts (for example, 0 to 5 mass% of the main component). Among these, TiO2, Ti2O3, Ti3O5, ZrO2, Ta2O5, Nb2O5, La2O3, Y2O3, Yb2O3, and Si, which are materials that are evaporated in a non-sublimation manner, are preferred in terms of foreign matter reduction effect, etc. In particular, TiO2, Ti2O3, Ti3O5, ZrO2, Nb2O5, La2O3, Y2O3, Yb2O3, and Si, which have melting points of 2500°C or less, are more preferable.
[0084] As the low refractive index material, a material with a refractive index of less than 1.7 can be used, and a material with a refractive index ranging from 1.2 to less than 1.7 is usually selected. Examples of such materials include SiO2, Al2O3, MgF2, LaF3, YF3, and Na3AlF6. Among these, SiO2, Al2O3, and MgF2, which are materials that are not evaporated by sublimation, are preferred. Ag may also be used as a material with a refractive index of less than 1.7.
[0085] The multilayer vapor deposition film desirably has a light transmittance of 10% or less, preferably 5% or less, and more preferably 1% or less in the wavelength range of 400 to 1600 nm. By including a multilayer vapor deposition film having such a wavelength transmittance, an optical filter having few foreign matters and exhibiting the desired optical characteristics can be easily obtained, even if the thickness of each layer of the multilayer vapor deposition film, the thickness of the multilayer vapor deposition film as a whole of this laminate, or the total number of layers is large.
[0086] As described below, the present laminate is suitably used as an optical member, in particular as an optical filter.
[0087] When the laminate is used as an optical filter that reflects near-infrared rays, the thickness of each of the deposition films constituting the multilayer deposition film is usually preferably 0.1λ to 0.5λ, where λ (nm) is the wavelength of near-infrared rays to be reflected. Note that, as each deposition film constituting the multilayer deposition film, a layer having a thickness outside the range of 0.1λ to 0.5λ may be used depending on the purpose of reducing reflection in the visible light region or improving the shielding performance in a specific wavelength region. When the laminate is used as a near-infrared cut filter (NIR-CF), the value of λ (nm) is, for example, 700 to 1400 nm, preferably 750 to 1300 nm. When the thickness of each deposition film constituting the multilayer deposition film is within this range, the optical film thickness, which is the product (n×d) of the refractive index (n) and the film thickness (d), is approximately the same value as λ / 4, and the relationship between the optical properties of reflection and refraction tends to make it easy to control the blocking and transmission of a specific wavelength.
[0088] When the present laminate is used as an NIR-CF, the total number of layers in the multilayer vapor-deposited film is preferably 16 to 70 layers, and more preferably 20 to 60 layers, as a whole of the multilayer vapor-deposited film included in the present laminate, for example.
[0089] When the thickness of each layer, the thickness of the multilayer deposition film as the entire laminate, and the total number of layers are within the above ranges, sufficient manufacturing margins can be ensured, and warping of the optical filter and cracks in the multilayer deposition film can be reduced. If the total number of layers in the multilayer deposition film exceeds the above ranges, foreign matter may increase during the formation of the dielectric multilayer film.
[0090] With this laminate, by appropriately selecting the type of deposition material, the thickness of each layer of the multilayer deposition film, the order of stacking, and the number of layers in accordance with the absorption characteristics of the base material, etc., it is possible to easily obtain this laminate having the desired optical characteristics (e.g., having sufficient transmittance in the wavelength range to be transmitted [e.g., visible light range], while having sufficient light blocking characteristics in the near-infrared wavelength range to be blocked).
[0091] When the laminate is used as an optical filter, the thickness and number of layers constituting the multilayer deposition film can be optimized using optical thin film design software (Essential Macleod, manufactured by Thin Film Center) in accordance with the wavelength-dependent characteristics of the refractive index of the substrate and the light absorption characteristics so as to achieve the desired optical characteristics, for example, anti-reflection effect in the visible range and selective transmission / reflection performance in the near infrared range. For example, when forming a multilayer deposition film of NIR-CF, the input parameters (target values) to the software during optimization can be set to a target transmittance of 100% for wavelengths of 400 to 700 nm and a target tolerance value of 1, and then a target transmittance of 0% for wavelengths of 705 to 950 nm and a target tolerance value of 0.5. These parameters can also be used to further divide the wavelength range into smaller sections to change the Target Tolerance value in accordance with the characteristics of the substrate, etc.
[0092] The thickness of the present laminate is preferably 32 to 300 μm, and within this range, the present laminate can be suitably used for thin solid-state imaging devices and the like. Moreover, the thickness of the present laminate is more preferably 32 to 220 μm, and further preferably 42 to 150 μm. If it is within this range, it can be suitably used in a thin solid-state imaging device having a total thickness of 6.5 mm or less.
[0093] <Application> The present laminate is useful as an optical member (optical element), and is particularly suitable for use as an optical filter. Specific examples of the optical filters include near-infrared cut filters (NIR-CF), color purity enhancing filters, visible light-near-infrared selective transmission filters (DBPF), near-infrared transmission filters (IRPF), and filters for alternative light sources (ALS) used in scientific investigations and the like.
[0094] The present laminate is particularly useful for digital still cameras, smartphone cameras, mobile phone cameras, digital video cameras, wearable device cameras, PC cameras, surveillance cameras, automotive cameras, infrared cameras, televisions, car navigation systems, personal digital assistants, video game consoles, portable game consoles, fingerprint authentication systems, digital music players, various sensing systems, infrared communications, etc. Furthermore, the present laminate is also useful as a heat-cutting filter to be attached to glass panels of automobiles, buildings, etc.
[0095] When the present laminate is used as a filter that cuts off part or all of near-infrared radiation, it is desirable that the present laminate has a region in which the average transmittance in a specific wavelength region is 0.5% or less, preferably 0.1% or less.
[0096] In the present invention, the average value (average transmittance) of the transmittance in a certain wavelength region (wavelengths A to B nm) is a value calculated by measuring the transmittance at each wavelength in 1 nm increments from Anm to B nm, and dividing the sum of the transmittances by the number of measured transmittances (wavelength range, B-A+1).
[0097] When the present laminate is used as a filter that transmits visible light, it is desirable that the present laminate has a region in which the average transmittance in the wavelength region of 400 to 630 nm is preferably 85% or more, and more preferably 90% or more. EXAMPLES
[0098] The present invention will be described below with reference to examples, but the present invention is not limited to these examples in any way.
[0099] [Example 1] As hearth liners attached to the deposition apparatus Sapio 1300i (manufactured by Showa Vacuum Co., Ltd.), the following hearth liner 9-1 and hearth liner 9-2 were used. The deposition apparatus was equipped with the following electron guns EB1 to EB4: Note that the electron guns with different reference symbols (eg, EB1 and EB2) are different electron guns.
[0100] The deposition material, SiO2 (Canon Optron, Inc.), was placed in hearth liner 9-1. The deposition material Ti3O5 (manufactured by Soltec Co., Ltd.) was placed at an arbitrary position (position A) of the hearth liner 9-2. The deposition material, Y2O3 (manufactured by Soltec Co., Ltd.), was placed in a position (position B) different from position A of the hearth liner 9-2. The deposition material, Y2O3 (manufactured by Soltec Co., Ltd.), was placed in a position (position C) different from positions A and B on the hearth liner 9-2. It should be noted that positions A to C are positions where each material divides a circular plan view seen from above the opening of the hearth liner 9-2 into approximately three equal parts.
[0101] The following resin substrate was placed on the substrate placement section of a deposition apparatus (Sapio 1300i [manufactured by Showa Vacuum Co., Ltd.]), hearth liners 9-1 and 9-2 containing the deposition material were placed on the deposition material placement section, and electron guns (EB1 and 2) corresponding to hearth liner 9-1 and electron guns (EB3 and 4) corresponding to hearth liner 9-2 were placed, respectively. After closing the shutters on the top of each hearth liner, the pressure in the deposition apparatus was reduced to 8×10 -4 I made it Pa.
[0102] Thereafter, the shutter on the upper part of the hearth liner 9-2 is opened, and the electron beam is adjusted by a control device for controlling the irradiation of the electron beam at position A of the hearth liner 9-2 so that the irradiation area of the electron beam from the electron gun (hereinafter also referred to as "EB4") is 4 cm 2 The electron beam output (EB output) was adjusted so that the deposition rate of the deposition film by EB4 was 3 Å / sec, and the electron beam was irradiated (hereinafter, the condition for irradiating the position A of the hearth liner 9-2 with the electron beam is also referred to as "deposition condition 2-1"). The deposition rate was calculated using a quartz crystal oscillator provided in the center of the deposition apparatus. According to the deposition condition 2-1, a Ti3O5 deposited film having a physical thickness of 14 nm was formed on the substrate. After the deposition film was formed, the shutter on the top of the hearth liner 9-2 was closed.
[0103] Thereafter, the shutter on the upper part of the hearth liner 9-1 is opened, and the electron beam is adjusted by a control device for controlling the irradiation of the electron beam on the hearth liner 9-1 so that the irradiation area of the electron beam from the electron gun (hereinafter also referred to as "EB1") is 4 cm 2 The electron beam was irradiated by adjusting the electron beam output (EB output) so that the deposition rate of the evaporated film by EB1 was 3 Å / sec. At the same time as the electron beam from EB1 is irradiated onto the hearth liner 9-1, the electron beam is adjusted by a control device that controls the irradiation of the electron beam onto a part of the same hearth liner 9-1 different from the part onto which the electron beam from EB1 is irradiated, so that the irradiation area of the electron beam from the electron gun (hereinafter also referred to as "EB2") is 4 cm 2The electron beam output (EB output) was adjusted so that the deposition rate of the evaporated film by EB2 was 3 Å / sec, and the electron beam was irradiated (hereinafter, the conditions for irradiating the hearth liner 9-1 with the electron beam by EB1 and 2 are also referred to as "evaporation condition 1-1"). The film formation rate was calculated from a quartz crystal oscillator provided in the center of the deposition device. According to the deposition conditions 1-1, a deposited SiO2 film with a physical thickness of 33 nm was formed on the deposited film (physical thickness: 14 nm) formed under the deposition conditions 2-1. After the deposition film was formed, the shutter on the top of the hearth liner 9-1 was closed.
[0104] Next, the shutter on the top of the hearth liner 9-2 was opened, and according to the deposition condition 2-1, a deposition film with a physical thickness of 101 nm was formed on the deposition film (physical thickness 33 nm) formed under the deposition condition 1-1, and then the shutter on the top of the hearth liner 9-2 was closed.
[0105] Then, as shown in the film design 1 in Table 2 below, lamination under the deposition conditions 2-1 and 1-1 was repeated a total of 12 times, and then the shutter at the top of the hearth liner 9-2 was opened, and the electron beam was adjusted by a control device that controls the irradiation of the electron beam at the position B of the hearth liner 9-2 so that the irradiation area of the electron beam from the electron gun (hereinafter also referred to as "EB3") was 4 cm. 2 The electron beam output (EB output) was adjusted so that the deposition rate of the deposited film by EB3 was 2 Å / sec, and the electron beam was irradiated. The deposition rate was calculated from a quartz crystal oscillator installed in the center of the deposition device. In addition, the hearth liner 9-2 is rotated, and the electron beam EB3 is irradiated to the position B of the hearth liner 9-2. At the same time, the electron beam is adjusted by a control device for controlling the irradiation of the electron beam so that the irradiation area of the electron beam from the EB4 is 4 cm2 at the position C of the hearth liner 9-2. 2The electron beam output (EB output) was adjusted so that the deposition rate of the deposition film by EB4 was 2 Å / sec, and the electron beam was irradiated (hereinafter, the condition of irradiating the electron beam to two different positions on the hearth liner 9-2 by EB3 and EB4 is also referred to as "deposition condition 3-1"). The deposition rate was calculated from a quartz crystal oscillator installed in the center of the deposition device. According to the deposition conditions 3-1, a deposition film of Y2O3 having a physical thickness of 112 nm was formed on the deposition film (physical thickness: 142 nm) formed under the deposition conditions 1-1. After the deposition film was formed, the shutter on the top of the hearth liner 9-2 was closed.
[0106] In the same manner as described above, a deposition film having the physical film thickness shown in Table 2 was formed under each deposition condition to conform to film design 1 shown in Table 2, and a multilayer deposition film of 40 layers was formed on one of the main surfaces (first surface) of the substrate (single surface film design).
[0107] Using film design 1, a multilayer vapor deposition film of 40 layers was formed on one of the main surfaces (side 1) of the substrate, and then a vapor deposition film of the physical film thickness shown in Table 2 was formed on the other main surface (side 2) of the substrate under each vapor deposition condition according to film design 2 shown in Table 2, thereby forming a multilayer vapor deposition film of 22 layers, thereby producing a substrate (hereinafter also referred to as a "laminate") having multilayer vapor deposition films on both main surfaces of the substrate. The total time required to form the multilayer vapor-deposited film on both main surfaces of this substrate is shown in Table 1 as film formation time.
[0108] [Examples 2 to 12 and Comparative Examples 1 to 3] A substrate shown in Table 1 was used, and a multilayer vapor deposition film was formed on one of its main surfaces (side 1) with the single-side film design shown in Table 1, and a multilayer vapor deposition film was formed on the other main surface (side 2) of the substrate with the double-side film design shown in Table 1, thereby producing a substrate (laminate) having multilayer vapor deposition films on both main surfaces of the substrate. In Example 3, the deposition material TNO (manufactured by Canon Optron Inc.) was placed at one of the positions (position A) that divide the circular plan view of the opening of the hearth liner 9-2 into approximately two equal parts when viewed from above, and the deposition material Al2O3 (manufactured by Canon Optron Inc.) was placed at the other position (position B) (an example of this case is shown in FIG. 3). Similarly, in Example 10 and Comparative Example 2, the deposition material Ti3O5 (manufactured by Soltec Corporation) was placed at one of the positions (position A) that divide the circular plan view of the opening of the hearth liner 9-2 into approximately two equal parts when viewed from above, and the deposition material Al2O3 (manufactured by Canon Optron Inc.) was placed at the other position (position B).
[0109] In addition, "resin" in the column for substrate in Table 1 refers to a resin substrate prepared as follows. In addition, in the column for substrate in Table 1, "D263" refers to a colorless borosilicate glass substrate manufactured by SCHOTT, and "BS-13" refers to blue glass (near-infrared absorbing glass) manufactured by Matsunami Glass Industry Co., Ltd.
[0110] <Resin substrate> 8-Methyl-8-methoxycarbonyltetracyclo[4.4.0.1] represented by the following formula (X1): 2,5 .1 7,10 100 parts by mass of dodeca-3-ene (hereinafter also referred to as "DNM"), 18 parts by mass of 1-hexene (molecular weight regulator), and 300 parts by mass of toluene (solvent for ring-opening polymerization reaction) were charged into a nitrogen-substituted reaction vessel, and the solution was heated to 80°C. Next, 0.2 parts by mass of a toluene solution of triethylaluminum (0.6 mol / L) and 0.9 parts by mass of a toluene solution of methanol-modified tungsten hexachloride (concentration 0.025 mol / L) were added as polymerization catalysts to the solution in the reaction vessel, and the solution was heated and stirred at 80°C for 3 hours to carry out a ring-opening polymerization reaction, thereby obtaining a ring-opening polymer solution. The polymerization conversion rate in this polymerization reaction was 97%.
[0111] [ka]
[0112] 1,000 parts by mass of the ring-opened polymer solution thus obtained was charged into an autoclave, and 0.12 parts by mass of RuHCl(CO)[P(C6H5)3]3 was added to the ring-opened polymer solution, and hydrogen gas pressure was 100 kg / cm 2 The hydrogenation reaction was carried out for 3 hours with heating and stirring at a reaction temperature of 165°C. The resulting reaction solution (hydrogenated polymer solution) was cooled, and then the hydrogen gas pressure was released. The reaction solution after the hydrogen gas pressure was released was poured into a large amount of methanol to separate and recover a coagulated product, which was then dried to obtain a hydrogenated polymer (hereinafter also referred to as "resin A").
[0113] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the obtained resin A, calculated in terms of standard polystyrene, were measured using a GPC apparatus manufactured by Tosoh Corporation (HLC-8220 type, column: TSKgel α-M, developing solvent: THF). The Mn was 32,000 and the Mw was 137,000.
[0114] The glass transition temperature (Tg) of the obtained resin A was measured under a nitrogen gas flow at a temperature rise rate of 20°C per minute using a differential scanning calorimeter (DSC6200) manufactured by Hitachi High-Tech Science Corp. Tg was 165°C.
[0115] Dichloromethane was added to Resin A to prepare a solution with a resin concentration of 20% by mass. The resulting solution was cast onto a smooth glass plate, dried at 20°C for 8 hours, and then peeled off from the glass plate. The peeled coating film was further dried at 100°C for 8 hours under reduced pressure to produce a resin substrate with a thickness of 0.1 mm, length of 210 mm, and width of 210 mm.
[0116] <Number of foreign objects> The number of foreign particles in Table 1 was measured as follows. As shown in FIG. 4, a surface inspection lamp FY-100R manufactured by Funatec Co., Ltd. was used as the light source 20, and a 100 cm2 lamp was placed 15 cm above the light source 20. 2 The laminate 21 thus manufactured was placed in the room. The laminate 21 was observed with the naked eye 22 from a position 1 m above the light source 20, and the number of foreign bodies (white dots) detected was counted.
[0117] [Table 1]
[0118] <Membrane design> Details of each membrane design in Table 1 are shown in Tables 2 and 3. Each film was designed by simulating the spectral transmittance of the resulting multilayer vapor deposition film using optical thin film design software (Essential Macleod, manufactured by Thin Film Center).
[0119] [Table 2]
[0120] [Table 3]
[0121] <Transmittance of multi-layer deposition film> In addition, in order to measure the transmittance of the multilayer deposition film formed in each of the film designs 1 to 9, a substrate having a multilayer deposition film on both main surfaces of the substrate was manufactured in the same manner as described above, except that the above-mentioned D263 was used as the substrate. The transmittance of light incident from a vertical direction of the substrate having the multilayer deposition film was measured in 1 nm increments using a UV-visible spectrophotometer V-630 manufactured by JASCO Corporation. The minimum transmittance value in the wavelength range of 400 to 1600 nm and the wavelength at that time (wavelength at the minimum transmittance) are shown in Table 4 below.
[0122] [Table 4]
[0123] <Deposition conditions> The deposition conditions for each film design described in Tables 2 and 3 are shown in Tables 5 to 7. The details of each deposition condition are as follows.
[0124] <Deposition conditions 1-2 to 1-6 and 1-8 to 1-10> In the deposition condition 1-1, the type of deposition material, the irradiation area of the electron beam, and the EB output were changed as shown in Table 5, and the electron beam was irradiated from EB1 and EB2 in the same manner as in the deposition condition 1-1.
[0125] <Deposition conditions 1-7> In FIG. 3, except that hearth liner 9-1 was used instead of hearth liner 9-2, the deposition material SiO2 (manufactured by Canon Optron Inc.) was placed in one of the positions (position A) that divides the circular plan view of the opening of hearth liner 9-1 into approximately two equal parts, and the deposition material L5 (manufactured by Merck & Co.) was placed in the other position (position B). At position A of the hearth liner 9-1, the electron beam is adjusted by a control device that controls the irradiation of the electron beam so that the irradiation area of the electron beam from EB1 is 3 cm 2 The electron beam was irradiated by adjusting the electron beam output (EB output) so that the deposition rate of the evaporated film by EB1 was 1.5 Å / sec. At the same time as the electron beam EB1 is irradiated to the position A of the hearth liner 9-1, the electron beam is adjusted by a control device for controlling the irradiation of the electron beam to a position B of the hearth liner 9-1 so that the irradiation area of the electron beam from EB2 is 3 cm 2 The electron beam was irradiated by adjusting the electron beam output (EB output) so that the deposition rate of the evaporated film by EB2 was 1.5 Å / sec. The film formation rate was calculated from a quartz crystal oscillator provided in the center of the deposition device.
[0126] <Deposition Conditions 1-11> The electron beam was adjusted by the control device that controlled the irradiation of the electron beam on the hearth liner 9-1, which contained the deposition material SiO2 (manufactured by Canon Optron Co., Ltd.) so that the irradiation area of the electron beam from EB1 was 6 cm 2The electron beam output (EB output) was adjusted so that the deposition rate of the deposited film by EB1 was 15 Å / sec. The deposition rate was calculated from a quartz crystal oscillator installed in the center of the deposition device.
[0127] <Deposition conditions 1-12~1-13> In the deposition conditions 1-11, except that the irradiation area of the electron beam and the EB output were changed to those shown in Table 5, the deposition conditions were the same as those in the deposition conditions 1-11, and the electron beam was irradiated from EB1.
[0128] <Deposition Condition 2-2> The deposition conditions were the same as those of the deposition conditions 2-1, except that the type of deposition material was changed to those shown in Table 6, and an electron beam was irradiated from EB4.
[0129] <Deposition conditions 2-3> The deposition material Ti3O5 (manufactured by Soltec Corporation) was placed in the hearth liner 9-2. The electron beam was adjusted by a control device for controlling the irradiation of the electron beam on the hearth liner 9-2, so that the irradiation area of the electron beam from EB3 was 4 cm 2 The electron beam output (EB output) was adjusted so that the deposition rate of the evaporated film by EB3 was 1.5 Å / sec. The deposition rate was calculated from a quartz crystal oscillator installed in the center of the deposition device. At the same time as the electron beam is irradiated onto the hearth liner 9-2, the electron beam is adjusted by a control device for controlling the irradiation of the electron beam onto a part of the same hearth liner 9-2 different from the part onto which the electron beam from EB3 is irradiated, so that the irradiation area of the electron beam from EB4 is 4 cm 2 The electron beam output (EB output) was adjusted so that the deposition rate of the deposited film by EB4 was 1.5 Å / sec, and the electron beam was irradiated. The deposition rate was calculated from a quartz crystal oscillator installed in the center of the deposition device.
[0130] <Deposition conditions 2-4 and 2-5> In the deposition conditions 2-3, except that the type of deposition material was changed as shown in Table 6, electron beams were irradiated from EB3 and EB4 in the same manner as in the deposition conditions 2-3.
[0131] <Deposition Condition 3-2> The electron beam was adjusted by the control device that controlled the irradiation of the electron beam on the hearth liner 9-2, which contained the deposition material Al2O3 (manufactured by Canon Optron Co., Ltd.), so that the irradiation area of the electron beam from EB3 was 5 cm 2 The electron beam output (EB output) was adjusted so that the deposition rate of the deposited film by EB3 was 3 Å / sec, and the deposition rate was calculated from a quartz crystal oscillator installed in the center of the deposition device.
[0132] Details of the deposition materials in Tables 5 to 7 are as follows. "SiO2": Manufactured by Canon Optron Co., Ltd. "L5": Substance L5 granules about 1-2mm Patinal (a mixture containing 90% or more by mass of SiO2 and less than 10% by mass of Al2O3, manufactured by Merck) "Al2O3": Canon Optron Co., Ltd. "Ti3O5": Soltec Co., Ltd. "TNO": LUMILEAD TNO (manufactured by Canon Optron, Inc.) "Ta2O5": OA-100 (Canon Optron Co., Ltd.) "Nb2O5": Manufactured by Rare Metals Co., Ltd. "Y2O3": Manufactured by Soltec Co., Ltd.
[0133] [Table 5]
[0134] [Table 6]
[0135] [Table 7] [Explanation of symbols]
[0136] 1: Base material placement part 2-1 and 2-2: Correction plates 3-1 and 3-2: Shutter 4-1 and 4-2: Deposition material placement section 5-1~5-4: Electron gun 6: Neutralizing gun 7: Ion gun 8: Crystal oscillator 9-1 and 9-2: Deposition material placement section (hearth liner) 10: Deposition container 11: Rotation mechanism 20:Light source 21: Laminate (substrate having a multilayer deposition film) 22: Visual observation (observation position)
Claims
1. A method for producing a substrate having a vapor-deposited film, comprising the steps of: Step (1): A step of irradiating one deposition material A with electron beams from a plurality of electron guns to evaporate the deposition material A to form a deposition film of the deposition material A on a substrate (however, there is a time (band) during which the electron beams from the plurality of electron guns are simultaneously irradiated onto one deposition material A). Step (2): A step of irradiating a plurality of deposition materials A (wherein the plurality of deposition materials A have the same main component) with an electron beam from an electron gun corresponding to each deposition material A to evaporate the deposition material A to form a deposition film of the deposition material A on the substrate (wherein there is a time (band) during which the electron beams from the electron guns corresponding to each of the plurality of deposition materials A are irradiated simultaneously on each deposition material A).
2. The deposition material A is Si, SiO 2 , Ti 2 O 3 , Ti 3 O 5 , TiO 2 , Nb 2 O 5 , HfO 2 , La 2 O 3 , Al 2 O 3 , Y 2 O 3 , Yb 2 O 3 , Ta 2 O 5 , MgF 2 , Ag and ZrO 2 The method for producing a substrate having a vapor-deposited film according to claim 1 , comprising the vapor deposition material A1 selected from the group consisting of:
3. 3. The method for producing a substrate having a vapor-deposition film according to claim 2, wherein a content of the one selected from the vapor deposition materials A1 in one vapor deposition material A in the step (1), and a content of the one selected from the vapor deposition materials A1 in each vapor deposition material A in the step (2) are each 90 mass% or more.
4. The method for producing a substrate having a vapor-deposited film according to claim 1 , which satisfies the following requirement (i): Requirement (i): The irradiation area of the electron beam from the electron gun irradiating the deposition material A is S [cm 2 ], and the deposition speed at which the deposition film of the deposition material A is formed is V [Å / sec], V / S is 1.5 [Å / (sec cm 2 ) is less than
5. The irradiation area S is 5 cm 2 The method for producing a substrate having a vapor-deposited film according to claim 4 .
6. A step I of forming a vapor-deposited film a of a vapor-deposition material A on a substrate by the method for producing a substrate having a vapor-deposited film according to any one of claims 1 to 5; The method for producing a substrate having a vapor-deposited film according to any one of claims 1 to 5, further comprising: a step II of forming a vapor-deposited film b of the vapor-deposited material B on the substrate having the vapor-deposited film a by using a vapor-deposited material B having a refractive index different from that of the vapor-deposited material A instead of the vapor-deposited material A; A method for producing a substrate having a multilayer vapor-deposited film, comprising:
7. 7. The method for producing a substrate having a multilayer vapor-deposited film according to claim 6, wherein the multilayer vapor-deposited film has a light transmittance of 10% or less in a wavelength range of 400 to 1600 nm.
8. 1. A vapor deposition apparatus for forming a vapor deposition film of a vapor deposition material on a substrate by vaporizing the vapor deposition material, the vapor deposition apparatus comprising: Configuration (I): A deposition material placement section for placing a deposition material is provided in the deposition device, and a plurality of electron guns for irradiating an electron beam are provided for each deposition material placement section. Configuration (II): A deposition device includes a plurality of deposition material placement units for placing a deposition material, and an electron gun for irradiating an electron beam is provided for at least two deposition material placement units among the plurality of deposition material placement units.
9. The deposition apparatus according to claim 8 , further comprising a control device for controlling irradiation of the electron beam by the electron gun.
10. 10. The deposition apparatus according to claim 8, wherein the deposition apparatus is an ion-assisted deposition apparatus having at least one selected from a neutralization gun and an ion gun.
11. a correction plate for adjusting a thickness of a deposition film to be formed on an upper portion of the deposition material placement unit; 10. The deposition apparatus according to claim 8, wherein the number of the correction plates is equal to or greater than the number of the electron guns.
12. The deposition apparatus according to claim 8 or 9, wherein the number of electron guns in the deposition apparatus is three or more.
Citation Information
Patent Citations
Vapor deposition apparatus
JP2018135593A