Method for manufacturing welding member
By employing sub-welds and strategically positioning main weld start and end points, along with adjustment welds, the method addresses thermal distortion issues in welded components, ensuring controlled bending and reduced deformation.
Patent Information
- Application Number
- JP2023067188
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-17
AI Technical Summary
Existing welding methods struggle to control the bending direction of welded members due to unmanaged thermal distortion, particularly in components like brake devices where thermal deformation is a concern.
A method involving the formation of sub-welds to temporarily fix parts before creating a main weld, with the main weld's start and end points strategically positioned to control thermal strain direction, and optionally incorporating adjustment welds to offset thermal distortion.
This approach effectively controls the bending direction of welded members by managing thermal strain, enhancing positional accuracy and reducing thermal distortion through strategic weld placement and additional adjustment welds.
Smart Images

Figure 2024153353000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing a welded component. [Background technology]
[0002] Patent Document 1 discloses a welding method for laser welding a ring provided in a brake device, which has a side surface perpendicular to the axial direction, and a plate having an abutment surface against which the side surface of the ring abuts. In this welding method, with the side surface and the abutment surface abutting, four or more spot-like welds are formed that are spaced equally apart in the circumferential direction around the axis of the ring as the center, and then the plate and ring are welded to form a circular weld along the circumferential direction, thereby reducing thermal distortion of the brake device. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2021-165560 Summary of the Invention [Problem to be solved by the invention]
[0004] In the above-described welding method, the deformation occurring in the circular weld of the welded member formed by welding two parts is suppressed, thereby reducing the thermal distortion of the welded member. However, it is difficult to control the direction in which the welded member bends due to the thermal distortion of the welded member.
[0005] An object of one aspect of the present disclosure is to provide a welding method capable of controlling the bending direction of a welded member. [Means for solving the problem]
[0006] One aspect of the present disclosure is a manufacturing method for a welded member in which a first part and a second part are welded, the method including welding the first part and the second part to form a main weld extending in a circumferential direction centered on an axis of the welded member extending in a direction in which the first part and the second part are arranged. The main weld extends from a welding start point to a welding end point. A deformation point is a position located in a range from the welding start point of the main weld to approximately the center of the main weld in the circumferential direction and having a high degree of contribution to deformation occurring in the main weld. The deformation point is located at a position that contributes to a direction that thermally distorts the welded member.
[0007] According to this configuration, the bending direction of the welded member can be controlled by adjusting the position of the deformation point of the main weld.
[0008] One aspect of the present disclosure may further include welding the first component and the second component to form one or more sub-welds for temporarily fixing the second component to the first component. The main weld may be formed after the sub-welds are formed. With this configuration, temporary fixing of the first component and the second component by the sub-welds can prevent the first component and the second component from shifting in position when the main weld is formed. As a result, it is possible to prevent the position at which the deformation point is located from shifting when the main weld is formed.
[0009] In one embodiment of the present disclosure, two or three sub-welds may be formed. With this configuration, it is possible to more effectively prevent the first component and the second component from becoming misaligned when the main weld is formed, compared to when one sub-weld is formed.
[0010] In one embodiment of the present disclosure, two sub-welds may be formed. The two sub-welds may be arranged at a distance of approximately 180° from each other in the circumferential direction. In this configuration, the temporary fixing of the first part and the second part by the two sub-welds tends to restrict the direction of thermal distortion occurring in the main weld in the first direction perpendicular to the straight line connecting the two sub-welds and the second direction opposite to the first direction. This makes it possible to arrange the deformation point of the main weld on the first direction side of the straight line to cause thermal distortion in the first direction, or to arrange the deformation point of the main weld on the second direction side of the straight line to cause thermal distortion in the second direction. As a result, it becomes easier to control the bending direction of the welded member.
[0011] In one aspect of the present disclosure, the main weld may be formed by circumferential welding. A welding start point of the main weld may be disposed at a position that does not overlap with the sub-weld. With this configuration, it is possible to control the bending direction of the welded member having the main weld formed by circumferential welding.
[0012] In one aspect of the present disclosure, the deformation points may be welding end points, which are a welding start point and a welding end point of the main weld. With this configuration, the bending direction of the welded member can be controlled by adjusting the positions of the welding end points of the main weld.
[0013] In one embodiment of the present disclosure, the first part and the second part may be cylindrical parts. An end of the second part may be inserted into the first part. The main weld and the sub weld may be formed in a portion where the first part and the second part overlap. With this configuration, it is possible to control the bending direction of the welded member formed by welding the cylindrical first part and the second part.
[0014] One aspect of the present disclosure may further include welding the first component and the second component such that, after the main weld is formed, an adjustment weld is formed that thermally distorts the welded member in a direction opposite to the direction of thermal distortion of the welded member. According to this configuration, by forming the adjustment weld after the main weld is formed, the bending direction of the welded member can be controlled and deformation occurring in the main weld can be offset by deformation occurring in the adjustment weld. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1A is a cross-sectional view taken along the central axis, which diagrammatically shows a state in which a sub-weld has been formed, and FIG. 1B is a cross-sectional view taken along the central axis, which diagrammatically shows a welded member of the first embodiment. [Diagram 2] FIG. 2A is a cross-sectional view taken along line IIA-IIA of FIG. 1B, and FIGS. 2B to 2E are cross-sectional views perpendicular to the central axis showing the direction of thermal distortion when the welding end point is positioned at a different circumferential position from the example shown in FIG. 2A. [Diagram 3] FIG. 3A is a cross-sectional view perpendicular to the central axis showing the direction of thermal distortion caused by forming only the main weld in a modified example of the first embodiment, and FIG. 3B is a cross-sectional view along the central axis showing typically how the welded member is bent due to thermal distortion in a predetermined direction. [Figure 4] 10 is a cross-sectional view perpendicular to the central axis, illustrating the direction of thermal distortion caused by the formation of one sub-weld and a main weld in a modified example of the first embodiment. FIG. [Diagram 5] Fig. 5A is a cross-sectional view perpendicular to the central axis showing the direction of thermal distortion caused by the formation of three sub-welds and a main weld in a modified example of the first embodiment, and Fig. 5B is a cross-sectional view perpendicular to the central axis showing the direction of thermal distortion when the welding end point is disposed at a different circumferential position from the example shown in Fig. 5A. [Figure 6]Fig. 6A is a cross-sectional view perpendicular to the central axis showing the direction of thermal distortion caused by the formation of four sub-welds and a main weld in a modified example of the first embodiment, and Fig. 6B is a cross-sectional view perpendicular to the central axis showing the direction of thermal distortion when the welding end point is disposed at a different circumferential position from the example shown in Fig. 6A. [Figure 7] FIG. 11 is a cross-sectional view perpendicular to the central axis, illustrating the direction of thermal distortion caused by the formation of only the main weld, which is an arc, in a modified example of the first embodiment. [Figure 8] 10 is a cross-sectional view perpendicular to the central axis, illustrating the direction of thermal distortion caused by the formation of two sub-welds and a main weld that is an arc in a modified example of the first embodiment. FIG. [Figure 9] FIG. 9A is a cross-sectional view along the central axis that shows a schematic representation of the state in which a sub-welded portion has been formed, FIG. 9B is a cross-sectional view along the central axis that shows a schematic representation of the state in which a main welded portion has been formed, and FIG. 9C is a cross-sectional view along the central axis that shows a schematic representation of a welded member of the second embodiment. [Figure 10] FIG. 10A is a cross-sectional view taken along the XA-XA line in FIG. 9C, and FIGS. 10B to 10E are cross-sectional views perpendicular to the central axis, showing the direction of thermal distortion when the welding end point is positioned at a different circumferential position from the example shown in FIG. 10A, and the arrangement of adjustment welds that offset the thermal distortion. [Figure 11] 13 is a cross-sectional view perpendicular to the central axis, showing the arrangement of adjustment welds that offset thermal distortion caused by forming only main welds in a modified example of the second embodiment. FIG. [Figure 12] 13 is a cross-sectional view perpendicular to the central axis, showing the arrangement of adjustment welds that offset thermal distortion caused by the formation of one sub-weld and a main weld in a modified example of the second embodiment. FIG. [Figure 13] Fig. 13A is a cross-sectional view perpendicular to the central axis showing the arrangement of adjustment welds that offset thermal distortion caused by the formation of three sub-welds and a main weld in a modified example of the second embodiment. Fig. 13B is a cross-sectional view perpendicular to the central axis showing the direction of thermal distortion and the arrangement of adjustment welds that offset the thermal distortion when the welding end point is arranged at a different circumferential position from the example shown in Fig. 13A. [Figure 14] Fig. 14A is a cross-sectional view perpendicular to the central axis showing the arrangement of adjustment welds that offset thermal distortion caused by the formation of four sub-welds and a main weld in a modified example of the second embodiment. Fig. 14B is a cross-sectional view perpendicular to the central axis showing the direction of thermal distortion and the arrangement of adjustment welds that offset the thermal distortion when the welding end point is arranged at a different circumferential position from the example shown in Fig. 14A. [Figure 15] 13 is a cross-sectional view perpendicular to the central axis, showing the arrangement of adjustment welds that offset thermal distortion caused by the formation of only main welds that are circular arcs in a modified example of the second embodiment. FIG. [Figure 16] 13 is a cross-sectional view perpendicular to the central axis showing a modified example of a linear sub-weld portion. FIG. [Figure 17] 11A to 11C are cross-sectional views perpendicular to the central axis showing modified examples of sub-welds having different line lengths. [Figure 18] 10A and 10B are cross-sectional views perpendicular to the central axis, showing a modified example of a method for forming a main weld. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, exemplary embodiments of the present disclosure will be described with reference to the drawings. [1. First embodiment] [1-1. Configuration] 1B is an on-vehicle part that is mounted on a vehicle. An example of the on-vehicle part is an exhaust system part that constitutes at least a part of a flow path for passing exhaust gas from an internal combustion engine mounted on the vehicle.
[0017] 1A and 1B, the welded member 100 includes a first part 1, a second part 2, a sub-weld part SW, and a main weld part MW. In this embodiment, the welded member 100 has a central axis A that extends linearly. The welded member 100 is manufactured by welding the first part 1 and the second part 2, which are arranged side by side along the central axis A, by, for example, arc welding.
[0018] The first part 1 and the second part 2 are tubes formed into a cylindrical shape with a constant diameter. The inner diameter of the first part 1 is larger than the outer diameter of the second part 2. The inner diameter of the first part may be substantially the same as the outer diameter of the second part. It is preferable that there is no gap in the radial direction between the end of the first part 1 and the end of the second part, but there may be a gap. The central axes of the first part 1 and the second part 2 coincide with the central axis A of the welded member 100. In this embodiment, the first part 1 and the second part 2 are connected in a state where the end of the second part 2 is inserted into an opening on one end side of the first part 1.
[0019] One or more sub-welds SW are formed at a predetermined position in the circumferential direction centered on the central axis A in the overlapping portion between the first component 1 and the second component 2, and temporarily fix the second component 2 to the first component 1. The sub-welds SW are formed by partially welding a welding path that goes around the outer circumferential surfaces of the first component 1 and the second component 2. As shown in FIGS. 2A to 2E, in this embodiment, the shape of the sub-welds SW is dot-like, and two sub-welds SW are formed by, for example, arc welding. When viewed along the central axis A, the two sub-welds SW are disposed approximately 180° apart from each other in the circumferential direction with the center point of each sub-weld SW as a reference. That is, the two sub-welds SW face each other with the central axis A as a center.
[0020] As a result, the welding path is divided into two paths by a straight line L connecting the two sub-welded portions SW: a first welding path located above the straight line L in the drawings, and a second welding path located below the straight line L. In the following description, among the directions perpendicular to the straight line L in the drawings, the direction toward the top (i.e., toward the first welding path) is referred to as a first direction D1, and the direction opposite to the first direction D1, toward the bottom (i.e., toward the second welding path) is referred to as a second direction D2.
[0021] As shown in FIG. 1B, the main weld MW is formed to extend in the circumferential direction in the portion where the first component 1 and the second component 2 overlap, and joins the first component 1 and the second component 2. That is, the main weld MW permanently fixes the temporarily fixed first component 1 and the second component 2 by a stronger joint than the joint of the temporary fixation. The main weld MW is formed at the same position as the position where the sub-weld SW is formed in the direction along the central axis A. In the example shown in FIG. 2A to FIG. 2E, the welding direction of the main weld MW is clockwise. The welding direction may be counterclockwise. In this embodiment, the main weld MW is formed by full circumference welding along the welding path. In full circumference welding, the welding start point and the welding end point overlap. Hereinafter, the welding start point and the welding end point in the main weld MW are referred to as the welding end point S. That is, as shown in FIG. 2A to FIG. 2E, in a cross section perpendicular to the central axis A, the shape of the main weld MW is a circle that closes the welding path. Note that the state where "the welding start point and the welding end point overlap" includes a state where the welding start point and the welding end point overlap in whole or in part.
[0022] It is preferable that the welding end point S of the main weld MW is disposed at a position that does not overlap with the sub-weld SW in the circumferential direction. However, the welding end point S may be disposed at a position that overlaps with the sub-weld SW in the circumferential direction. The state in which the welding end point S overlaps with the sub-weld SW in the circumferential direction includes a state in which the welding end point S and the sub-weld SW overlap in whole or in part.
[0023] [1-2. Manufacturing methods for welding components] 1A, 1B, and 2A, a method for manufacturing welded member 100 will be described. Specifically, a method for welding first component 1 and second component 2, which is included in the method for manufacturing welded member 100, will be described.
[0024] First, an end of the second component 2 is inserted into an opening on one end side of the first component 1 to connect the first component 1 and the second component 2. Then, as shown in Fig. 1A and Fig. 2A, the first component 1 and the second component 2 are partially welded in the circumferential direction so as to form two sub-welds SW facing each other about the central axis A.
[0025] 1B and 2A, after the formation of the sub-weld SW, the first component 1 and the second component 2 are welded all around along the circumferential direction so that the main weld MW is formed overlapping the sub-weld SW. At this time, the position where the welding end point S of the main weld MW is located is adjusted so that the welded member 100 is bent in the desired direction at the joining position of the first component 1 and the second component 2, and welding of the main weld MW is started. In other words, the welding start position is adjusted so that the main weld end point S is located in the direction in which thermal distortion is desired to be generated in the welded member 100, among the joining positions of the first component 1 and the second component 2, and welding of the main weld MW is started.
[0026] In the arc welding as the welding of the main weld MW, the formation of the weld easily causes deformation in the weld. In the full circumference welding, the welds overlap at the points located in the range from the welding start point of the weld to the approximate center of the circumference of the weld, particularly at the welding end point, and the time for the heat of the welding to be transmitted to the welded object is long, so that the heat capacity is likely to increase. For this reason, in the main weld MW formed by full circumference welding by arc welding in a state where the sub-weld SW is not formed, the position that is the center of the deformation generated in the main weld MW is the welding end point S. The position that is the center of the deformation is, for example, the part of the weld that is most deformed by thermal distortion. Therefore, as shown in FIG. 3A, when there is no temporary fixation by the sub-weld SW, the formation of the main weld MW causes thermal distortion in the direction from the central axis A toward the welding end point S. Hereinafter, thermal distortion in a predetermined direction means that the welded member 100 bends so that the sections on both sides of the joining position in the welded member 100 are inclined in the predetermined direction (see FIG. 3B).
[0027] On the other hand, in this embodiment, before the main weld MW is formed, two sub-welds SW arranged at approximately 180° intervals in the circumferential direction are formed, and the first component 1 and the second component 2 are temporarily fixed. This makes it easier to restrict the direction of thermal strain occurring in the main weld MW to the first direction D1 and the second direction D2. For this reason, in this embodiment, the direction of thermal strain occurring in the main weld MW is either the first direction D1 or the second direction D2, rather than the direction from the central axis A toward the welding end point S. In other words, in this embodiment, the welding end point S functions as a position that contributes greatly to the deformation occurring in the main weld MW, rather than being the center of the deformation occurring in the main weld MW.
[0028] 2A to 2D, thermal distortion in the first direction D1 can be generated by forming the main weld MW so that the welding end point S is located on the first welding path on the first direction D1 side of the straight line L. Note that even if the circumferential position of the welding end point S differs, as long as it is on the first welding path, it is possible to generate thermal distortion in the first direction D1.
[0029] 2E, by forming the main weld MW so that the welding end point S is located on the second welding path on the second direction D2 side of the straight line L, it is possible to generate thermal distortion in the second direction D2. Note that although only one example of the position of the welding end point S on the second welding path is shown, as with the first welding path, it is possible to generate thermal distortion in the second direction D2 even if the circumferential position of the welding end point S is different on the second welding path.
[0030] That is, among the welding paths, a position on the first welding path is a position that contributes to thermally distorting the welded member 100 in the first direction D1, and a position on the second welding path is a position that contributes to thermally distorting the welded member 100 in the second direction D2. By locating the welding end point S on the first welding path or the second welding path as described above, it is possible to intentionally cause thermal distortion in the first direction D1 or the second direction D2 at the main weld MW, and control the direction in which the welded member 100 bends.
[0031] [1-3. Effects] According to the first embodiment described above in detail, the following effects can be obtained. (1a) In the first embodiment, two sub-welds SW are formed so as to be spaced apart from each other by approximately 180° in the circumferential direction. Then, after the two sub-welds SW are formed, the main weld MW is formed by full-circumference welding. Therefore, the direction of thermal distortion occurring in the main weld MW is likely to be restricted to the first direction D1 and the second direction D2 by the temporary fixing of the first component 1 and the second component 2 by the two sub-welds SW. Therefore, it is possible to arrange the welding end point S of the main weld MW on the first welding path to cause thermal distortion in the first direction D1, or to arrange the welding end point S of the main weld MW on the second welding path to cause thermal distortion in the second direction D2.
[0032] In this manner, by locating the welding end point S on either the first welding path or the second welding path, the direction in which the welded member 100 bends can be easily controlled.
[0033] (1b) In the first embodiment, before the main weld MW is formed, the sub-weld SW is formed and the first component 1 and the second component 2 are temporarily fixed. Therefore, the sub-weld SW can prevent the first component 1 and the second component 2 from being misaligned when the main weld MW is formed. As a result, the positional accuracy of the weld end point S is improved, and therefore the accuracy of controlling the bending direction of the welded member 100 can be improved. In the first embodiment, the welding end point S corresponds to an example of a deformation point.
[0034] [1-4. Other embodiments] Although the first embodiment of the present disclosure has been described above, it goes without saying that the present disclosure is not limited to the above-described first embodiment and can take on various forms.
[0035] (2a) In the first embodiment described above, two sub-welds SW are formed, but the number of sub-welds is not limited to this. For example, as shown in Fig. 3A, no sub-weld SW may be formed. Specifically, the sub-weld SW may not be formed before the main weld MW is formed. That is, only the main weld MW may be formed. In this case, the formation of the main weld MW generates thermal distortion in the direction from the central axis A toward the welding end point S. For this reason, the bending direction of the welded member 100 can be easily controlled by adjusting the position where the welding end point S of the main weld MW is located.
[0036] Also, for example, as shown in Fig. 4, one sub-weld SW may be formed. Specifically, after one sub-weld SW is formed, a main weld MW may be formed. In this case, too, the formation of the main weld MW generates thermal distortion in the direction from the central axis A toward the welding end point S. Note that even if the relative positions of the welding end point S and one sub-weld SW on the welding path change, thermal distortion in the direction from the central axis A toward the welding end point S occurs. For this reason, the bending direction of the welded member 100 can be easily controlled by adjusting the position where the welding end point S of the main weld MW is located.
[0037] 5A and 5B, three sub-welds SW may be formed at equal intervals along the circumferential direction. Specifically, the main weld MW may be formed after the three sub-welds SW are formed. In this case, too, the formation of the main weld MW generates thermal distortion in the direction from the central axis A toward the welding end point S. Note that even if the position of the welding end point S on the welding path changes, thermal distortion also generates in the direction from the central axis A toward the welding end point S. For this reason, the bending direction of the welded member 100 can be easily controlled by adjusting the position at which the welding end point S of the main weld MW is located.
[0038] 6A and 6B, four sub-welds SW may be formed at equal intervals along the circumferential direction. Specifically, the main weld MW may be formed after the four sub-welds SW are formed. In this case, too, the formation of the main weld MW generates thermal distortion in the direction from the central axis A toward the welding end point S. Note that even if the position of the welding end point S on the welding path changes, thermal distortion also generates in the direction from the central axis A toward the welding end point S. For this reason, the bending direction of the welded member 100 can be easily controlled by adjusting the position at which the welding end point S of the main weld MW is located.
[0039] (2b) In the first embodiment, the main weld MW is formed by circumferential welding, but the method of forming the main weld is not limited to this. For example, the main weld may be formed by welding a section of a predetermined length of a welding path that goes around the outer circumferential surface of the member. Specifically, as shown in Fig. 7, in a cross section perpendicular to the central axis A, the shape of the main weld MWa may be a circular arc in which the welding path is not closed.
[0040] In arc-shaped welding, the time required for the heat of welding to be transferred to the welded object is long in the range from the welding start point of the weld to the approximate center of the circumferential direction of the weld, and the heat capacity is likely to increase. In the arc-shaped main weld MWa, the deformation point T located in the range from the welding start point S1a of the main weld MWa to the approximate center of the circumferential direction of the main weld MWa is the center of deformation occurring in the main weld MWa. For example, the range from the welding start point of the main weld to the approximate center of the circumferential direction of the main weld is a range of approximately 180 degrees from the welding start point when the circumferential angle of the main weld is 360 degrees, and is a range of approximately 90 degrees from the welding start point when the circumferential angle of the main weld is 180 degrees. For this reason, as shown in FIG. 7, in the case where only the main weld MWa is formed without the sub-weld SW, the formation of the main weld MWa causes thermal distortion in the direction from the central axis A toward the deformation point T.
[0041] For convenience, in Fig. 7 and Fig. 8, the deformation point T is illustrated at a position that is the center of the main welded portion MWa. However, the deformation point T is not limited to this central position as long as it is a position that is the center of deformation in the range from the welding start point S1a of the main welded portion MWa to approximately the center in the circumferential direction of the main welded portion MWa. In addition, the position of the welding start point S1a is not limited to the position illustrated in Fig. 7 and Fig. 8, and may be located at the other end of the arc.
[0042] On the other hand, as shown in Fig. 8, when two sub-welds SW arranged at approximately 180° intervals in the circumferential direction are formed before the main weld MWA is formed, and the first component 1 and the second component 2 are temporarily fixed, the direction of thermal strain generated in the main weld MWA is likely to be restricted to the first direction D1 and the second direction D2, as in the first embodiment described above. Therefore, the direction of thermal strain generated in the main weld MWA is either the first direction D1 or the second direction D2, rather than the direction from the central axis A toward the deformation point T. In other words, the deformation point T functions as a position that contributes greatly to the deformation generated in the main weld MWA, rather than as a position that is the center of the deformation generated in the main weld MWA.
[0043] 8, by forming the main weld MWe such that the deformation point T is located on the first welding path on the first direction D1 side of the straight line L, it is possible to generate thermal distortion in the first direction D1. Furthermore, although not shown, by forming the main weld MWe such that the deformation point T is located on the second welding path on the second direction D2 side of the straight line L, it is possible to generate thermal distortion in the second direction D2. Therefore, similarly to the first embodiment described above, by locating the deformation point T on the first welding path or the second welding path, it is possible to control the direction in which the welded member 100 bends.
[0044] [2. Second embodiment] The welding method disclosed in the above-mentioned Patent Publication No. 2021-165560 may not be able to sufficiently reduce thermal distortion in a welded member formed by welding two parts, so a new method for suppressing thermal distortion in a welded member is desired.
[0045] A new method for suppressing thermal distortion of a welded member will be described below. As will be described in detail later, after forming a main weld MW, an adjustment weld CW shown in Fig. 9C is formed to control the bending direction of the welded member 100a, thereby suppressing thermal distortion of the welded member 100a.
[0046] 9A to 9C and 10A, the second embodiment differs from the welded member 100 of the first embodiment in that the welded member 100a includes an adjusted weld CW. Otherwise, the basic configuration of the welded member 100a is similar to that of the first embodiment, so the same reference numerals are used for configurations common to the first embodiment, and descriptions are omitted, and the configurations different from the first embodiment will be mainly described.
[0047] [2-1. Configuration] As shown in FIG. 9C, the adjustment weld CW is formed at a portion where the first part 1 and the second part 2 overlap, specifically, in the direction along the central axis A, at the same position as the position where the sub-weld SW and the main weld MW are formed. The adjustment weld CW is formed by partially welding a welding path that goes around the outer circumferential surfaces of the first part 1 and the second part 2. As shown in FIG. 10A, in this embodiment, the shape of the adjustment weld CW is a line extending a predetermined length along the circumferential direction, and one adjustment weld CW is formed, for example, by arc welding. The adjustment weld CW is disposed at a position on the welding path that can generate thermal strain in a direction opposite to the thermal strain caused by the formation of the main weld MW after the formation of the two sub-welds SW.
[0048] [2-2. Manufacturing methods for welding components] Next, a method for manufacturing the welded member 100a will be described with reference to Figures 9A to 9C and 10A. Specifically, a method for welding the first component 1 and the second component 2, which is included in the method for manufacturing the welded member 100a, will be described.
[0049] First, an end of the second component 2 is inserted into an opening on one end side of the first component 1 to connect the first component 1 and the second component 2. Then, as shown in Fig. 9A and Fig. 10A, the first component 1 and the second component 2 are partially welded in the circumferential direction so as to form two sub-welds SW facing each other about the central axis A.
[0050] Next, as shown in Figures 9B and 10A, after the sub-weld SW is formed, the first part 1 and the second part 2 are welded all around in the circumferential direction so that the main weld MW is formed overlapping the sub-weld SW.
[0051] 9C and 10A, after the main weld MW is formed, the first component 1 and the second component 2 are further partially welded in the circumferential direction so that an adjustment weld CW is formed overlapping the main weld MW. At this time, the adjustment weld CW is formed at a position on the welding path where thermal distortion in the opposite direction to the thermal distortion in the first direction D1 or the second direction D2 caused by the formation of the main weld MW after the formation of the two sub-welds SW can be generated.
[0052] 10A to 10D, when the welding end point S of the main weld MW is positioned on the first welding path on the first direction D1 side of the straight line L, the adjustment weld CW is positioned approximately in the center of the second welding path on the second direction D2 side of the straight line L. This makes it easier for thermal distortion in the first direction D1 caused by the formation of the main weld MW to be offset by thermal distortion in the second direction D2 caused by the formation of the adjustment weld CW.
[0053] 10E, when the welding end point S of the main weld MW is positioned on the second welding path on the second direction D2 side of the line L, the adjustment weld CW is positioned approximately in the center of the first welding path on the first direction D1 side of the line L. This makes it easier for the thermal strain in the second direction D2 caused by the formation of the main weld MW to be offset by the thermal strain in the first direction D1 caused by the formation of the adjustment weld CW.
[0054] As described above, by forming adjustment weld CW after forming main weld MW and controlling the bending direction of welded member 100a, thermal distortion of welded member 100a is suppressed.
[0055] [2-3. Effects] According to the second embodiment described above in detail, the following effects can be obtained. (3a) In the second embodiment, after the two sub-welds SW and the main weld MW are formed, an adjustment weld CW is formed to thermally distort the welded member 100a in the direction opposite to the first direction D1 or the second direction D2 in which the welded member 100a is thermally distorted. This allows the bending direction of the welded member 100a to be controlled so that the deformation occurring in the main weld MW is offset by the deformation occurring in the adjustment weld CW. This makes it possible to suppress the thermal distortion of the welded member 100a.
[0056] [2-4. Other embodiments] Although the second embodiment of the present disclosure has been described above, it goes without saying that the present disclosure is not limited to the second embodiment and can take various forms.
[0057] (4a) In the second embodiment described above, two sub-welds SW are formed, but the number of sub-welds is not limited to this. For example, as shown in FIG. 11, no sub-weld SW may be formed. Specifically, the sub-weld SW may not be formed before the main weld MW is formed. That is, the main weld MW and the adjustment weld CW may be formed. In this case, the formation of the main weld MW generates thermal distortion in the direction from the central axis A toward the welding end point S. For this reason, the adjustment weld CW is disposed such that the center point of the adjustment weld CW in the circumferential direction is spaced approximately 180° from the welding end point S when viewed along the central axis A. Specifically, the center point of the adjustment weld CW in the circumferential direction is disposed on an extension of a straight line connecting the welding end point S and the central axis A. That is, the adjustment weld CW and the welding end point S face each other with the central axis A as the center. This allows the bending direction of the welded member 100a to be controlled, and the thermal distortion occurring in the main welded part MW in the direction from the central axis A toward the welding finish point S to be offset by the thermal distortion occurring in the adjustment welded part CW in the opposite direction to the central axis A. This makes it possible to suppress the thermal distortion of the welded member 100a.
[0058] Also, for example, as shown in FIG. 12, one sub-weld SW may be formed. Specifically, after one sub-weld SW is formed, a main weld MW may be formed, and then an adjustment weld CW may be formed. In this case, too, the formation of the main weld MW generates thermal distortion in the direction from the central axis A toward the welding end point S. Even if the relative positions of the welding end point S and one sub-weld SW on the welding path change, thermal distortion occurs in the direction from the central axis A toward the welding end point S. For this reason, the adjustment weld CW and the welding end point S are disposed so as to face each other with the central axis A as the center. This allows the bending direction of the welded member 100a to be controlled, and the thermal distortion in the direction from the central axis A toward the welding end point S generated in the main weld MW to be offset by the thermal distortion in the opposite direction generated in the adjustment weld CW. Therefore, the thermal distortion of the welded member 100a can be suppressed.
[0059] Also, for example, as shown in FIG. 13A and FIG. 13B, three sub-welds SW may be formed so as to be arranged at equal intervals along the circumferential direction. Specifically, after the formation of three sub-welds SW, a main weld MW may be formed, and then an adjustment weld CW may be formed. In this case, too, the formation of the main weld MW generates thermal distortion in the direction from the central axis A toward the welding end point S. Note that even if the position of the welding end point S on the welding path is changed, thermal distortion occurs in the direction from the central axis A toward the welding end point S. For this reason, the adjustment weld CW and the welding end point S are disposed so as to face each other with the central axis A as the center. This allows the bending direction of the welded member 100a to be controlled, and the thermal distortion in the direction from the central axis A toward the welding end point S generated in the main weld MW to be offset by the thermal distortion in the opposite direction generated in the adjustment weld CW. Therefore, the thermal distortion of the welded member 100a can be suppressed.
[0060] Also, for example, as shown in FIG. 14A and FIG. 14B, four sub-welds SW may be formed so as to be arranged at equal intervals along the circumferential direction. Specifically, after the four sub-welds SW are formed, the main weld MW may be formed, and then the adjustment weld CW may be formed. In this case, too, the formation of the main weld MW generates thermal distortion in the direction from the central axis A toward the welding end point S. Note that even if the position of the welding end point S on the welding path is changed, thermal distortion occurs in the direction from the central axis A toward the welding end point S. For this reason, the adjustment weld CW and the welding end point S are disposed so as to face each other with the central axis A as the center. This allows the bending direction of the welded member 100a to be controlled, and the thermal distortion in the direction from the central axis A toward the welding end point S generated in the main weld MW to be offset by the thermal distortion in the opposite direction generated in the adjustment weld CW. Therefore, the thermal distortion of the welded member 100a can be suppressed.
[0061] (4b) In the second embodiment, the main weld MW is formed by full circumference welding, but the method of forming the main weld is not limited to this. For example, the main weld may be formed by welding a section of a predetermined length of a welding path that goes around the outer circumferential surface of the member. Specifically, as shown in FIG. 15, in a cross section perpendicular to the central axis A, the shape of the main weld MWa may be a circular arc in which the welding path is not closed. The circumferential length of the adjustment weld CW is shorter than the circumferential length of the arc-shaped main weld MW.
[0062] In arc-shaped welding, the time required for the heat of welding to be transferred to the welded object is long at points located in the range from the welding start point of the weld to the approximate center of the circumferential direction of the weld, so the heat capacity is likely to increase. In the arc-shaped main weld MWa, the deformation point T located in the range from the welding start point S1a of the main weld MWa to the approximate center of the circumferential direction of the main weld MWa is the center of deformation occurring in the main weld MWa. For example, the range from the welding start point of the main weld to the approximate center of the circumferential direction of the main weld is a range of approximately 180 degrees from the welding start point when the circumferential angle of the main weld is 360 degrees, and is a range of approximately 90 degrees from the welding start point when the circumferential angle of the main weld is 180 degrees. For this reason, as shown in FIG. 15, in the case where there is no sub-weld SW and the adjustment weld CW is formed after the main weld MWa is formed, the main weld MWa generates thermal distortion in the direction from the central axis A toward the deformation point T. Therefore, the adjustment weld CW and the deformation point T are disposed to face each other with respect to the central axis A. This makes it possible to control the bending direction of the welded member 100a, and offset the thermal distortion occurring in the main weld MW in the direction from the central axis A toward the deformation point T by the thermal distortion occurring in the adjustment weld CW in the opposite direction to the thermal distortion. This makes it possible to suppress the thermal distortion of the welded member 100a.
[0063] For convenience, in Fig. 15, the deformation point T is illustrated at a position that is the center of the main welded portion MWa. However, the deformation point T is not limited to this central position as long as it is a position that is the center of deformation within the range from the welding start point S1a of the main welded portion MWa to approximately the center in the circumferential direction of the main welded portion MWa. In addition, the position of the welding start point S1a is not limited to the position illustrated in Fig. 15, and may be located at the other end of the arc.
[0064] (4c) In the second embodiment, the shape of the adjustment weld CW is linear, but the shape of the adjustment weld is not limited to this. For example, the adjustment weld may be formed in a dot shape.
[0065] (4d) In the second embodiment described above, there is one adjustment weld CW. However, for example, there may be a plurality of adjustment welds.
[0066] [3. Other embodiments common to the first and second embodiments] (5a) In each of the above embodiments, the shape of the sub-weld SW is a dot, but the shape of the sub-weld is not limited to this. For example, the sub-weld may be formed in a line extending along the circumferential direction. For example, as shown in FIG. 16, when a plurality of linearly formed sub-welds SWa are provided, the sub-welds SWa may be arranged at equal intervals so as not to overlap. The three sub-welds SWa shown in FIG. 16 may have the same circumferential length. Also, for example, as shown in FIG. 17, the three sub-welds SWb1 to SWb3 arranged at intervals so as not to overlap may have different circumferential lengths.
[0067] Furthermore, when multiple sub-welds are provided, the multiple sub-welds do not have to be disposed at equal intervals. Furthermore, for example, both point-shaped sub-welds and line-shaped sub-welds may be provided.
[0068] (5b) In each of the above embodiments, the main weld is welded all around by one operation in the circumferential direction. However, for example, the main weld MWb may be welded in a plurality of separate steps. For example, as shown in FIG. 18, after the formation of two sub-welds SW, the main weld MWb may be formed by two separate steps of welding so that the welding start points S1 and S2 overlap. In this case, too, the main weld MWb may be formed so that the welding start points S1 and S2 are located on the first welding path on the first direction D1 side of the straight line L, thereby generating thermal distortion in the first direction D1. Although not shown in the drawings, after the formation of the main weld MWb, an adjustment weld CW may be formed in the approximate center of the second welding path on the second direction D2 side of the straight line L. This allows the thermal distortion in the first direction D1 generated by the formation of the main weld MW to be offset by the thermal distortion in the second direction D2 generated by the formation of the adjustment weld CW.
[0069] (5c) In each of the above embodiments, the first part 1 and the second part 2 are connected with an end of the second part 2 inserted into an opening on one end side of the first part 1. However, for example, the first part and the second part may be connected with one end of the first part and an end of the second part butted together. In this case, the sub-weld, main weld, and adjustment weld are formed in the portion where the first part and the second part are connected.
[0070] Furthermore, the first part 1 and the second part 2 may be configured such that an end of the first part 1 is inserted into an opening on one end side of the second part 2.
[0071] (5d) In each of the above embodiments, the first part 1 and the second part 2 are cylindrical parts, but the shape of the first part and the second part is not limited to this. For example, the first part and the second part may be cylindrical parts having a shape other than a circle, or may be solid parts. The solid part may be plate-shaped, block-shaped, column-shaped, etc.
[0072] (5e) In each of the above embodiments, the central axis A of the welded member 100 extends linearly. However, for example, the central axis of the welded member may be curved.
[0073] (5f) The function of one component in each of the above embodiments may be distributed among multiple components, or the functions of multiple components may be integrated into one component. Also, part of the configuration of the above embodiments may be omitted. Also, at least part of the configuration of the above embodiments may be added to or substituted for the configuration of another of the above embodiments.
[0074] [Technical idea disclosed in this specification] [Item 1] A method for manufacturing a welded component in which a first part and a second part are welded together, comprising the steps of: welding the first part and the second part together so as to form a main weld part extending in a circumferential direction about an axis of the weld member extending in a direction in which the first part and the second part are arranged; The main weld extends from a weld start point to a weld end point, A deformation point is a position located in a range from the welding start point of the main weld portion to approximately the center of the main weld portion in the circumferential direction and having a high contribution to deformation occurring in the main weld portion, A method for manufacturing a welded component, wherein the deformation point is positioned at a position that contributes to a direction in which the welded component is thermally distorted.
[0075] [Item 2] A method for producing a welded component according to item 1, The method further includes welding the first part and the second part to form one or more sub-welds for temporarily fixing the second part to the first part, The method for manufacturing a welded component, wherein the main weld is formed after the sub-weld is formed.
[0076] [Item 3] A method for producing a welded component according to item 2, A method for manufacturing a welded component, wherein two or three sub-welds are formed.
[0077] [Item 4] A method for producing a welded component according to item 3, The sub-weld is formed in two parts, A method for manufacturing a welded component, wherein the two sub-welds are positioned approximately 180° apart from each other in the circumferential direction.
[0078] [Item 5] A method for producing a welded member according to any one of items 2 to 4, The main weld is formed by full circumference welding, A method for manufacturing a welded component, wherein the welding start point of the main weld is positioned at a position that does not overlap with the sub-weld.
[0079] [Item 6] A method for producing a welded component according to item 5, A method for manufacturing a welded component, wherein the deformation points are the welding start point and the welding end point of the main weld.
[0080] [Item 7] A method for producing a welded member according to any one of items 2 to 5, the first part and the second part are cylindrical parts, An end of the second part is inserted into the first part, A method for manufacturing a welded member, wherein the main weld and the sub-weld are formed in an overlapping portion of the first component and the second component.
[0081] [Item 8] A method for producing a welded member according to any one of items 1 to 7, The method for manufacturing a welded member further includes welding the first part and the second part together so that, after forming the main weld, an adjustment weld is formed, which thermally distorts the welded member in a direction opposite to a direction in which the welded member is thermally distorted. [Explanation of symbols]
[0082] 1...first part, 2...second part, 100, 100a...welding member, A...center axis, CW...adjusted weld, L...straight line, MW, MWa, MWb...main weld, S...welding end point, S1, S1a, S2...welding start point, SW, SWa, SWb1 to SWb3...sub-weld, T...deformation point.
Claims
1. A method for manufacturing a welded component in which a first part and a second part are welded together, comprising the steps of: welding the first component and the second component to form a main weld portion extending in a circumferential direction about an axis of the weld member extending in a direction in which the first component and the second component are arranged; The main weld extends from a weld start point to a weld end point, A deformation point is a position located in a range from the welding start point of the main weld portion to approximately the center of the main weld portion in the circumferential direction and having a high contribution to deformation occurring in the main weld portion, A method for manufacturing a welded component, wherein the deformation point is positioned at a position that contributes to a direction in which the welded component is thermally distorted.
2. A method for manufacturing a welded member according to claim 1, The method further includes welding the first part and the second part to form one or more sub-welds for temporarily fixing the second part to the first part, The method for manufacturing a welded component, wherein the main weld is formed after the sub-weld is formed.
3. A method for manufacturing a welded member according to claim 2, A method for manufacturing a welded component, wherein two or three sub-welds are formed.
4. A method for manufacturing a welded member according to claim 3, Two sub-welds are formed, A method for manufacturing a welded component, wherein the two sub-welds are positioned approximately 180° apart from each other in the circumferential direction.
5. A method for manufacturing a welded member according to any one of claims 2 to 4, The main weld is formed by full circumference welding, A method for manufacturing a welded component, wherein the welding start point of the main weld is positioned at a position that does not overlap with the sub-weld.
6. A method for manufacturing a welded member according to claim 5, A method for manufacturing a welded component, wherein the deformation points are the welding start point and the welding end point of the main weld.
7. A method for manufacturing a welded member according to any one of claims 2 to 4, the first part and the second part are cylindrical parts, An end of the second part is inserted into the first part, The main weld and the sub-weld are formed in an overlapping portion of the first component and the second component.
8. A method for manufacturing a welded member according to any one of claims 1 to 4, a welding portion for welding the first part and the second part together such that, after the main weld portion is formed, an adjustment weld portion is formed that thermally distorts the weld portion in a direction opposite to a direction in which the weld portion is thermally distorted.
Citation Information
Patent Citations
Vehicle exhaust system flange joint
JP1991041113U
Method and jig for tack welding of stainless steel steel pipe
JP1995024595A
Method for executing butt welding
JP2004001011A
Welding method and manufacturing method for combination members and manufacturing method for valve structure
JP3528746B2
Branch pipe welding method
JP6455307B2