Modified recycled carbon black and rubber composition
By modifying recycled carbon black through oxidation and hydrocarbon treatment, the bonding with rubber components is strengthened, enhancing the reinforcing properties of rubber products.
Patent Information
- Application Number
- JP2023067333
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-17
AI Technical Summary
Recycled carbon black obtained from waste tires has weak reinforcing properties for rubber products due to rubber residues adhering to its surface, which inhibit bonding with rubber components.
The surface of recycled carbon black is modified by contacting it with an oxidizing gas under heating to remove rubber residues, followed by contacting with hydrocarbons to adjust the specific surface area and enhance bonding with rubber components.
The modified recycled carbon black exhibits a strong bond with rubber components, improving the reinforcing properties of rubber products and achieving performance equivalent to virgin carbon black.
Smart Images

Figure 2024153435000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to recycled carbon black having a modified surface state, a method for producing the same, and a rubber composition in which the same is used. [Background technology]
[0002] In recent years, efforts to reduce the burden on the global environment, such as carbon neutral and sustainable initiatives, have been actively undertaken. As part of these sustainability activities, the carbon black industry is also considering the use of recycled carbon black obtained by pyrolyzing rubber products such as waste tires.
[0003] As a method for producing recycled carbon black by pyrolysis of waste tires, for example, Patent Document 1 discloses a method for pyrolyzing waste tires at about 500° C. while circulating nitrogen gas. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5813985 [Patent Document 2] WO2013 / 095145A1 Summary of the Invention [Problem to be solved by the invention]
[0005] However, recycled carbon black, which is obtained by pyrolyzing rubber products such as waste tires, has rubber residues, mainly composed of rubber charcoal, adhering to its surface. When the recycled carbon black is mixed with a rubber composition, the rubber residues inhibit the adsorption of the recycled carbon black to the rubber component.
[0006] Therefore, recycled carbon black has a problem in that it has a low reinforcing effect on rubber products due to its weak bond with the rubber component.
[0007] Therefore, an object of the present invention is to provide recycled carbon black which has strong bonding with rubber components and has high reinforcing properties for rubber products. [Means for solving the problem]
[0008] As a result of extensive investigation, the present inventors have found that It has been discovered that by contacting recycled carbon black with an oxidizing gas under heating, the rubber residue, mainly composed of rubber charcoal, adhering to the surface of the recycled carbon black can be oxidized and removed, exposing the surface of the recycled carbon black, which in turn strengthens the bond with the rubber component and thereby enhances the reinforcing properties of rubber products. The present inventors have also found the following: When the rubber residue adhering to the surface of recycled carbon black is removed by oxidative decomposition, if the oxidation of the recycled carbon black itself proceeds too far, the bond with the rubber component will be strong, but the specific surface area will be too high and the cohesive force of the recycled carbon black will be too strong, resulting in poor dispersion in the rubber and poor rubber reinforcement. However, the inventors have found that by contacting the recycled carbon black, which has a large specific surface area due to contact with an oxidizing gas, with a hydrocarbon under heating to generate a char, and filling the pores generated on the surface of the recycled carbon black with the char, it is possible to adjust the specific surface area, reduce the cohesive force, and increase the reinforcement of rubber products, which has led to the completion of the present invention.
[0009] That is, the present invention provides (1)N 2 SA is 50m 2 / g or more 250m 2 / g or less, In the Raman spectrum obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm, the peak intensity was 1350 ± 20 cm -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1The peak intensity of a peak having a peak top in the range of 84 to 111. Modified recycled carbon black. (2) The modified recycled carbon black according to (1), characterized in that the ash content is 3.0% or more and 50.0% or less. (3) The recycled carbon black having rubber carbonized particles attached thereto is contacted with an oxidizing gas in a reactor heated to 600°C or higher and 1400°C or lower. N 2 SA is 50m 2 / g or more 250m 2 / g or less, In the Raman spectrum obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm, the peak intensity was 1350 ± 20 cm -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1 The peak intensity of a peak having a peak top in the range of 84 to 111. Modified recycled carbon black. (4) The carbon black having rubber carbonized material adhering thereto is obtained by carrying out a step of contacting an oxidizing gas with the recycled carbon black and a step of contacting a hydrocarbon gas with the recycled carbon black in a reactor heated to 600°C or higher and 1400°C or lower, N 2 SA is 50m 2 / g or more 250m 2 / g or less, In the Raman spectrum obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm, the peak intensity was 1350 ± 20 cm -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1 The peak intensity of a peak having a peak top in the range of 84 to 111. Modified recycled carbon black. (5) The recycled carbon black to which the rubber carbonized material is attached has a Raman spectrum of 1350±20 cm when measured by laser Raman spectroscopy at an excitation wavelength of 532 nm. -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1 The modified recycled carbon black according to (3) or (4), characterized in that the peak intensity of a peak having a peak top in the range is 112 or more and 200 or less. (6) A method for producing modified recycled carbon black, comprising the step of contacting recycled carbon black having rubber carbonized material adhered thereto with an oxidizing gas in a reactor heated to a temperature of 600°C or higher and 1400°C or lower. (7) A method for producing modified recycled carbon black, comprising the steps of: contacting recycled carbon black having rubber carbonized material adhered thereto with an oxidizing gas and contacting the recycled carbon black with a hydrocarbon gas in a reactor heated to a temperature of 600°C or higher and 1400°C or lower. (8) The method for producing modified recycled carbon black according to (7), further comprising the step of contacting a hydrocarbon gas after the step of contacting an oxidizing gas. (9) The recycled carbon black to which the rubber carbonized material is attached has a Raman spectrum of 1350±20 cm when measured by laser Raman spectroscopy at an excitation wavelength of 532 nm. -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1 The method for producing modified recycled carbon black according to (6) or (7), characterized in that the carbon black has a peak having a peak top in the range of 112 or more and 200 or less in peak intensity. (10) a rubber component; (1) modified recycled carbon black in an amount of 1 part by mass or more and 100 parts by mass or less per 100 parts by mass of the rubber component; A rubber composition comprising: This provides: Effect of the Invention
[0010] According to the present invention, it is possible to provide recycled carbon black which has strong bonds with rubber components and has high reinforcing properties for rubber products. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is an explanatory diagram showing a method for calculating the G band intensity when the D band intensity is taken as 100 in the modified recycled carbon black of the present invention. [Diagram 2] FIG. 2 is a diagram for explaining a method for measuring the Raman spectrum of the modified recycled carbon black of the present invention. [Diagram 3] 1 is a Raman spectrum of an example morphology of recycled carbon black before modification. [Figure 4] FIG. 1 is a schematic diagram of an example of a fluidized bed reactor. [Diagram 5] FIG. 1 is a graph showing the relationship between dynamic storage modulus (E′) and tensile stress (M300) for Examples, Comparative Examples, Reference Examples, and rCB1. [Figure 6A] This is an electron microscope photograph of virgin carbon black (SEAST6). The white areas indicate scale. [Figure 6B] Electron microscope photographs of recycled carbon black before modification (rCB before modification and rCB1). The white areas indicate the scale. [Figure 6C] 1 is an electron microscope photograph of modified recycled carbon black (modified rCB Example 7), where the white areas indicate scale. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings as appropriate. The detailed description of the present invention below is an example of an embodiment, and the present invention is not to be construed as being limited to this embodiment.
[0013] The modified recycled carbon black of the present invention is N2 SA is 50m 2 / g or more 250m 2 / g or less, In the Raman spectrum obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm, the peak intensity was 1350 ± 20 cm -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1 The peak intensity of a peak having a peak top in the range of 84 to 111. It is characterized by:
[0014] The modified recycled carbon black of the present invention is a surface-modified recycled carbon black obtained by pyrolyzing rubber products such as waste tires, etc. More specifically, the modified recycled carbon black of the present invention is a surface-modified recycled carbon black obtained by pyrolyzing rubber products such as waste tires, etc., from which all or a part of the rubber residues mainly composed of rubber charcoal that were attached to the surface of the recycled carbon black have been removed.
[0015] Recycled carbon black with rubber carbonized material on its surface has a Raman spectrum of 1350±20cm when measured with a laser Raman spectroscopy at an excitation wavelength of 532 nm. -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1 The peak intensity of the peak having a peak top in the range is 112 or more.
[0016] In contrast to such recycled carbon black having rubber charcoal attached to the surface, the modified recycled carbon black of the present invention has the rubber residue, the main component of which is rubber charcoal attached to the surface, removed. Therefore, in the Raman spectrum obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm, the peak intensity is 1350±20 cm -1 When the peak intensity of the peak (D band) having a peak top in the range of 1580 ± 20 cm is taken as 100, -1The peak intensity of a peak (G band) having a peak top in the range (hereinafter also referred to as the G band intensity when the D band intensity is 100) is 84 or more and 111 or less. When the G band intensity when the D band intensity of the recycled carbon black is 100, is in the above range, there is no or very little rubber residue adhering to the surface of the recycled carbon black, and the bond between the recycled carbon black and the rubber component is strong, so that the reinforcing properties of rubber products are high. When the D band intensity is 100, the G band intensity is preferably 85 or more and 110 or less from the viewpoint of ensuring an appropriate bond strength between the recycled carbon black surface and the rubber, and more preferably 86 or more and 109 or less from the viewpoint of ensuring a stronger bond strength. On the other hand, when the D band intensity of the recycled carbon black is taken as 100, if the G band intensity exceeds the above range, a large amount of rubber residue adheres to the surface of the recycled carbon black, and the bond between the recycled carbon black and the rubber component will be weak. On the other hand, if the G band intensity is below the above range, there will be many defects in the graphite structure on the carbon black surface, and the surface activity will be too high, promoting the aggregation of carbon black particles in the rubber and reducing the reinforcing properties of the rubber.
[0017] FIG. 1 is a diagram showing a method for calculating the G band intensity when the D band intensity is taken as 100 in the modified recycled carbon black of the present invention. As shown in FIG. 1, the modified recycled carbon black of the present invention has a Raman spectrum of 1350±20 cm 2 obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm. -1 A peak with a peak top in the range of 1580 ± 20 cm (D band) -1 A peak (G band) having a peak top in the range of
[0018] Then, from the values of the peak intensity of the D band and the peak intensity of the G band, the peak intensity of the G band is calculated when the peak intensity of the D band is set to 100. According to the studies of the present inventors, the greater the amount of rubber charcoal attached to the recycled carbon black, the greater the intensity of the G band, and therefore it was found that the state of removal of the rubber charcoal from the recycled carbon black can be grasped based on the magnitude of the peak intensity of the G band compared with the peak intensity of the D band.
[0019] In the present invention, the G band intensity, when the D band intensity is taken as 100, means a value calculated from a Raman spectrum obtained by performing measurement under the measurement conditions of (1) below and then performing data processing of (2). (1) Using a laser Raman spectrometer, HR-800 manufactured by Horiba, Ltd., several grains of the carbon black sample to be measured are placed on a slide glass and rubbed several times with a spatula to make the surface flat. Measurement is performed under the following measurement conditions. YAG laser (excitation wavelength): 532 nm Number of grooves: 600gr / mm Filter: D0.6 Objective lens magnification: 100x Exposure time: 150 seconds Number of times: 2 An example of the spectrum obtained in this way is shown in FIG. (2) Measurement wavelength of the obtained spectrum (Raman Shift) 2100cm -1 The signal intensity at the measurement wavelength of 1350±20 cm was set to 0, and the average value was calculated for each of the 39 adjacent data points constituting the spectrum. Then, a spectral curve connecting the average values was obtained by smoothing. -1 The peak top intensity observed in this range is set to 100. An example of the Raman spectrum obtained in this way is shown in FIG.
[0020] Fig. 1 is a Raman spectrum of an example of the modified recycled carbon black of the present invention, in which the peak intensity of the G band is 95 when the peak intensity of the D band is 100, which is in the range of 84 to 111. On the other hand, Fig. 3 is a Raman spectrum of an example of the recycled carbon black before modification, in which the peak intensity of the G band is 113 when the peak intensity of the D band is 100, which is outside the range of 84 to 111. It can be seen from these that the recycled carbon black before modification shown in Fig. 3 has rubber charcoal attached to its surface, and the modified recycled carbon black shown in Fig. 1 has the rubber charcoal attached to its surface removed by modification.
[0021] The nitrogen adsorption specific surface area N of the modified recycled carbon black of the present invention 2 SA is 50m 2 / g or more 250m 2 The nitrogen adsorption specific surface area N 2 By setting the SA within the above range, the cohesive force of the recycled carbon black is kept low, and the reinforcing properties of rubber products are enhanced. The nitrogen adsorption specific surface area N 2 From the viewpoint of dispersibility in the rubber composition, SA is preferably 55m 2 / g or more 245m 2 / g or less, and from the viewpoint of the reinforcement of the rubber composition, it is more preferably 60m 2 / g or more 240m 2 On the other hand, the nitrogen adsorption specific surface area N 2 If the SA is less than the above range, the number of bonding points between the rubber and the recycled carbon black will be small, resulting in weak reinforcing properties. If the SA exceeds the above range, the cohesive force of the recycled carbon black will be too high, resulting in a low reinforcing property of the rubber product.
[0022] In the present invention, the nitrogen adsorption specific surface area N 2SA means a value measured by the amount of nitrogen adsorption in accordance with the method specified in JIS K6217-2 2017 "Carbon black for rubber - Basic properties - Part 2, Determination of specific surface area."
[0023] The DBP (dibutylphthalate) absorption amount of the modified recycled carbon black of the present invention is 60 cm in terms of dispersibility in rubber compositions. 3 / 100g or more 200cm 3 / 100g or less is preferable, and 70cm 3 / 100g or more 195cm 3 / 100g or less is preferable, and 80cm 3 / 100g or more 190cm 3 On the other hand, if the DBP absorption is less than the above range, the dispersibility of the carbon black deteriorates when the carbon black is compounded in a rubber composition, and the reinforcing properties of the resulting rubber tend to decrease, while if the DBP absorption exceeds the above range, the processability of the resulting rubber may decrease when the carbon black is compounded in a rubber composition.
[0024] In the present invention, the DBP absorption amount means a value measured by the method specified in JIS K6217-4 2017 "Carbon black for rubber - Basic properties - Part 4, Determination of DBP absorption amount".
[0025] The modified recycled carbon black of the present invention is obtained by modifying recycled carbon black obtained by pyrolysis of rubber products such as waste tires, and therefore the ash content of the modified recycled carbon black of the present invention is 3.0% or more and 50.0% or less. The ash content of the modified recycled carbon black of the present invention is preferably 4.0% or more and 45.0% or less, more preferably 5.0% or more and 40.0% or less.
[0026] In the present invention, the ash content means a value measured by the method specified in JIS K6218-2 2005 "Carbon black for rubber - Additional characteristics - Part 2, Determination of ash content".
[0027] The first embodiment of the present invention is a method for producing modified recycled carbon black, which is characterized by having a step of contacting recycled carbon black having rubber carbonized material adhered thereto with an oxidizing gas in a reactor heated to 600°C or higher and 1400°C or lower (hereinafter also referred to as step A1).
[0028] Step A1 is a process in which the recycled carbon black having rubber charcoal adhering thereto is brought into contact with an oxidizing gas in a reactor heated to a prescribed temperature, thereby oxidizing, decomposing and removing the rubber residue, which is mainly composed of rubber charcoal adhering to the surface of the recycled carbon black.
[0029] In the step A1, the recycled carbon black to be contacted with the oxidizing gas is carbon black obtained by pyrolyzing rubber products such as waste tires, and is carbon black having a rubber residue composed mainly of rubber charcoal attached to its surface. Examples of the recycled carbon black to be contacted with the oxidizing gas include PB365 (trade name) manufactured by Enrestec, BolderBlack (trade name) manufactured by Bolder Industries, DE-Black (trade name) manufactured by Delta Energy, and MondoBlack (trade name) manufactured by ECOLOMONDO. Such recycled carbon black may be produced by any production method, and is not particularly limited, but an example thereof includes the method described in Patent Document 2.
[0030] In the step A1, the recycled carbon black to be brought into contact with the oxidizing gas has a Raman spectrum of 1350±20 cm2 obtained by measuring with an excitation wavelength of 532 nm by laser Raman spectroscopy. -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1 The peak intensity of the peak having a peak top in this range is 112 or more and 200 or less, preferably 112 or more and 190 or less.
[0031] In the step A1, the ash content of the recycled carbon black to be contacted with the oxidizing gas is preferably 4.0% or more and 45.0% or less, more preferably 5.0% or more and 40.0% or less.
[0032] In step A1, N of recycled carbon black contacted with oxidizing gas 2 SA is 10m 2 / g or more 200m 2 / g or less, preferably 20m 2 / g or more 190m 2 / g or less, more preferably 25m 2 / g or more 185m 2 / g or less.
[0033] In step A1, the oxidizing gas to be brought into contact with the recycled carbon black is oxygen gas, a gas containing oxygen, air, etc. The amount of the oxidizing gas to be contacted is appropriately selected depending on the recycled carbon black to be treated, the amount of rubber residue adhered, the type of oxidizing gas to be used, the specific surface area of the target modified recycled carbon black, etc.
[0034] In step A1, the temperature in the reactor when the oxidizing gas is brought into contact with the recycled carbon black is from 600° C. to 1400° C., preferably from 700° C. to 1300° C., and more preferably from 800° C. to 1200° C. When the temperature in the reactor is within the above range, oxidation proceeds appropriately, making it easy to remove the rubber residue.
[0035] In the A1 step, the conditions such as the temperature in the reactor when the oxidizing gas is brought into contact with the recycled carbon black, the amount of the oxidizing gas in contact, and the time are determined by the G band intensity and N band intensity when the D band intensity is taken as 100. 2 The SA is appropriately selected so that it falls within the range specified for the modified recycled carbon black of the present invention.
[0036] In process A1, the recycled carbon black having rubber charcoal attached thereto is placed in a reactor, which is then heated to a prescribed temperature. An oxidizing gas is supplied into the reactor while discharging the decomposition gas outside the reactor. In this way, the oxidizing gas is brought into contact with the recycled carbon black having rubber charcoal attached thereto at the prescribed temperature in the reactor, and the rubber residues mainly composed of rubber charcoal attached to the surface of the recycled carbon black are oxidized, decomposed and removed.
[0037] For example, step A1 can be performed by placing recycled carbon black having rubber carbonized material attached thereto in a fluidized bed reactor such as fluidized bed reactor 1 shown in FIG. 4, heating the inside of the fluidized bed reactor to a predetermined temperature, and discharging gas resulting from oxidative decomposition from the top of the fluidized bed reactor while supplying an oxidizing gas from the bottom of the fluidized bed reactor.
[0038] The fluidized bed reactor 1 shown in FIG. 4 has a generally cylindrical shape, and the reactor axis extends vertically. The fluidized bed reactor 1 has a gas inlet 21 for supplying gas to be brought into contact with carbon black from the bottom to the top of the reactor body 2, and an exhaust port 22 at the top of the reactor body 2. As shown in FIG. 4, the fluidized bed reactor 1 has a heater coil 3 in which an electric heating wire is wound in a spiral shape around the entire outer periphery of the furnace wall of the reactor body 2, and has a structure capable of heating the stirring region 4 provided inside the reactor body 2. In addition, a filter 5 is provided at the inlet of the gas inlet 21 at the bottom of the reactor body 2 to prevent the carbon black in the reactor body 2 from leaking from the reactor body 2 to the gas inlet 21.
[0039] An oxidizing gas is then supplied to the fluidized bed reactor 1 to generate a gas flow. The oxidizing gas is preferably supplied in a preheated state to the fluidized bed reactor 1, and in this case, the preheating temperature is preferably 400° C. to 600° C., more preferably 450° C. to 600° C., even more preferably 450° C. to 550° C., even more preferably 480° C. to 550° C., and even more preferably 480° C. to 520° C. The oxidizing gas is supplied to the fluidized bed reactor 1 at a flow rate of 0.40 Nm3 per 100 g of recycled carbon black to which rubber carbonized material is attached. 3 / hour more than 3.50Nm 3 It is preferable to supply the amount of water so that the amount is less than 0.450 Nm 3 / hour more than 3.45Nm 3 More preferably, the supply is at 0.50 Nm 3 / hour over 3.40Nm 3 More preferably, the supply is at least 0.55 Nm 3 / hour more than 3.35Nm 3 More preferably, the supply is at 0.60 Nm / hour or less. 3 / hour more than 3.30Nm 3 It is even more preferable to supply the mixture at a rate of 1 / hour or less.
[0040] In addition, the oxidizing gas introduced into the fluidized bed reactor 1 is preferably supplied so that the pressure at the gas inlet is 1.0 MPa or more and 2.0 MPa or less, more preferably 1.1 MPa or more and 2.0 MPa or less, even more preferably 1.1 MPa or more and 1.8 MPa or less, even more preferably 1.2 MPa or more and 1.8 MPa or less, and even more preferably 1.2 MPa or more and 1.5 MPa or less.
[0041] When the fluidized bed reactor 1 is used, an oxidizing gas is supplied from a gas inlet 21. The oxidizing gas may be supplied in a state where the recycled carbon black having the rubber carbonized material adhered thereto has been previously introduced into the fluidized bed reactor, or the oxidizing gas may be supplied into the fluidized bed reactor, and then the recycled carbon black having the rubber carbonized material adhered thereto may be introduced from a supply port separately provided in the fluidized bed reactor.
[0042] The recycled carbon black having the rubber carbonized material attached thereto is introduced into the fluidized bed reactor 1 and stirred and fluidized under heating by the gas flow of the oxidizing gas. The heating temperature is 600° C. to 1400° C., preferably 700° C. to 1300° C., and more preferably 800° C. to 1200° C. The stirring and fluidization time is preferably 100 seconds to 300 seconds, more preferably 110 seconds to 300 seconds, even more preferably 110 seconds to 280 seconds, even more preferably 120 seconds to 280 seconds, and even more preferably 120 seconds to 250 seconds.
[0043] When using a fluidized bed reactor 1, an oxidizing gas is supplied from a gas inlet 21, and then the recycled carbon black to which the rubber carbonized material is attached is stirred and mixed in a stirring zone 4 heated by a heater coil 3. An oxidizing gas is supplied into the furnace under heating, and the recycled carbon black to which the rubber carbonized material is attached is stirred and fluidized by the gas flow of the oxidizing gas, thereby bringing the two into contact with each other.
[0044] After stirring with the oxidizing gas, the supply of the oxidizing gas is stopped, and preferably nitrogen gas is introduced to naturally cool the produced carbon black, thereby stopping the reaction. The nitrogen gas is introduced into the fluidized bed reactor 1 at a flow rate of 6.50 Nm 3 / hour more than 8.50Nm 3 It is preferable to supply the amount of water so that the amount is not more than 7.00 Nm 3 / hour more than 8.50Nm 3 More preferably, the supply is at 7.00 Nm 3 / hour more than 8.00Nm 3More preferably, the supply is at 7.50 Nm / hour or less. 3 / hour more than 8.00Nm 3 More preferably, the supply is at 7.50 Nm / hour or less. 3 / hour more than 7.80Nm 3 It is even more preferable to supply the mixture at a rate of 1 / hour or less.
[0045] The cooled carbon black particles can be separated and collected by a separation and collection device such as a cyclone or a bag filter, thereby recovering the desired modified recycled carbon black.
[0046] In the first embodiment of the present invention, the modified recycled carbon black is produced by carrying out the step A1. 2 SA is 50m 2 / g or more 250m 2 / g or less, preferably 55m 2 / g or more 245m 2 / g or less, more preferably 60m 2 / g or more 240m 2 / g or less, and the Raman spectrum obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm is 1350 ± 20 cm -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1 In this manner, a modified recycled carbon black having a peak intensity of 84 or more and 111 or less, preferably 85 or more and 110 or less, and more preferably 86 or more and 109 or less, is obtained.
[0047] The second embodiment of the method for producing modified recycled carbon black of the present invention is characterized by comprising a step of contacting recycled carbon black having rubber carbonized material adhered thereto with an oxidizing gas and a step of contacting the recycled carbon black with a hydrocarbon gas in a reactor heated to 600°C or higher and 1400°C or lower.
[0048] One example of the method for producing the modified recycled carbon black according to the second embodiment of the present invention includes a step of contacting recycled carbon black having rubber carbonized material adhered thereto with an oxidizing gas in a reactor heated to 600° C. to 1400° C. (hereinafter, referred to as step A2), and a step of contacting a hydrocarbon gas with the recycled carbon black that has been subjected to the step of contacting with the oxidizing gas (step B2). In other words, the step of contacting with the oxidizing gas is performed before the step of contacting with the hydrocarbon gas.
[0049] Step A2 is a process in which the recycled carbon black to which rubber charcoal is attached is brought into contact with an oxidizing gas in a reactor heated to a specified temperature, thereby oxidizing, decomposing, and removing the rubber residue, which is mainly composed of rubber charcoal attached to the surface of the recycled carbon black.
[0050] In step A2, the recycled carbon black to be contacted with the oxidizing gas is carbon black obtained by pyrolyzing rubber products such as waste tires, and is carbon black having a rubber residue composed mainly of rubber charcoal attached to its surface. Examples of the recycled carbon black to be contacted with the oxidizing gas include PB365 (trade name) manufactured by Enrestec, BolderBlack (trade name) manufactured by Bolder Industries, DE-Black (trade name) manufactured by Delta Energy, and MondoBlack (trade name) manufactured by ECOLOMONDO. Such recycled carbon black may be produced by any production method, and is not particularly limited, but examples thereof include the method described in Patent Document 2.
[0051] In step A2, the recycled carbon black that is brought into contact with the oxidizing gas has a Raman spectrum of 1350±20 cm2 obtained by measuring with an excitation wavelength of 532 nm by laser Raman spectroscopy. -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1The peak intensity of the peak having a peak top in this range is 112 or more and 200 or less, preferably 112 or more and 190 or less.
[0052] In step A2, the ash content of the recycled carbon black to be contacted with the oxidizing gas is preferably 3.0% or more and 50.0% or less, and more preferably 4.0% or more and 45.0% or less.
[0053] In step A2, the oxidizing gas to be brought into contact with the recycled carbon black is oxygen gas, a gas containing oxygen, air, etc. The amount of the oxidizing gas to be contacted is appropriately selected depending on the recycled carbon black to be treated, the amount of rubber residue adhered, the type of oxidizing gas to be used, the specific surface area of the target modified recycled carbon black, etc.
[0054] In step A2, the temperature in the reactor when the oxidizing gas is brought into contact with the recycled carbon black is from 600° C. to 1400° C., preferably from 700° C. to 1300° C., and more preferably from 800° C. to 1200° C. When the temperature in the reactor is within the above range, oxidation proceeds appropriately, making it easy to remove the rubber residue.
[0055] In step A2, the conditions such as the temperature in the reactor, the amount of oxidizing gas in contact, and the time when the oxidizing gas is brought into contact with the recycled carbon black are appropriately selected so that the removal of rubber residues can be confirmed when observed with a transmission electron microscope or the like.
[0056] In process A2, the recycled carbon black with rubber carbonized matter adhering thereto is placed in a reactor, which is then heated to a prescribed temperature. An oxidizing gas is supplied into the reactor while discharging the decomposition gas outside the reactor. In this way, the oxidizing gas is brought into contact with the recycled carbon black with rubber carbonized matter adhering thereto at the prescribed temperature in the reactor, and the rubber residues mainly composed of rubber carbonized matter adhering to the surface of the recycled carbon black are oxidized, decomposed, and removed.
[0057] For example, step A2 is performed by placing recycled carbon black having rubber carbonized material attached thereto in a fluidized bed reactor such as fluidized bed reactor 1 shown in FIG. 4, heating the inside of the fluidized bed reactor to a predetermined temperature, and discharging gas produced by oxidative decomposition from the upper part of the fluidized bed reactor while supplying an oxidizing gas from the lower part of the fluidized bed reactor.
[0058] An oxidizing gas is supplied to the fluidized bed reactor 1 to generate a gas flow. The oxidizing gas is preferably supplied in a preheated state to the fluidized bed reactor 1. In this case, the preheating temperature is preferably 400° C. to 600° C., more preferably 450° C. to 600° C., even more preferably 450° C. to 550° C., even more preferably 480° C. to 550° C., and even more preferably 480° C. to 520° C. In addition, the oxidizing gas is supplied to the fluidized bed reactor 1 at a flow rate of 2.50 Nm3 per 100 g of recycled carbon black to which rubber carbonized material is attached. 3 / hour more than 8.50Nm 3 / hour or less, and 2.55 Nm 3 / hour over 8.45Nm 3 More preferably, the supply is 2.60 Nm 3 / hour over 8.40Nm 3 More preferably, the supply is at 2.65 Nm / hour or less. 3 / hour more than 8.35Nm 3 More preferably, the supply is at 2.70 Nm / hour or less. 3 / hour more than 8.30Nm 3 It is even more preferable to supply the mixture at a rate of 1 / hour or less.
[0059] In addition, the oxidizing gas introduced into the fluidized bed reactor 1 is preferably supplied so that the pressure at the gas inlet is 1.0 MPa or more and 2.0 MPa or less, more preferably 1.1 MPa or more and 2.0 MPa or less, even more preferably 1.1 MPa or more and 1.8 MPa or less, even more preferably 1.2 MPa or more and 1.8 MPa or less, and even more preferably 1.2 MPa or more and 1.5 MPa or less.
[0060] When the fluidized bed reactor 1 is used, an oxidizing gas is supplied from a gas inlet 21. The oxidizing gas may be supplied in a state where the recycled carbon black having the rubber carbonized material adhered thereto has been previously introduced into the reactor, or the oxidizing gas may be supplied into the reactor, and then the recycled carbon black having the rubber carbonized material adhered thereto may be introduced from a supply port separately provided in the reactor.
[0061] The recycled carbon black having the rubber carbonized material attached thereto is introduced into the fluidized bed reactor 1 and stirred and fluidized under heating by the gas flow of the oxidizing gas. The heating temperature is 600° C. to 1400° C., preferably 700° C. to 1300° C., and more preferably 800° C. to 1200° C. The stirring and fluidization time is preferably 100 seconds to 300 seconds, more preferably 110 seconds to 300 seconds, even more preferably 110 seconds to 280 seconds, even more preferably 120 seconds to 280 seconds, and even more preferably 120 seconds to 250 seconds.
[0062] When using a fluidized bed reactor 1, an oxidizing gas is supplied from a gas inlet 21, and then the recycled carbon black to which the rubber carbonized material is attached is stirred and mixed in a stirring zone 4 heated by a heater coil 3. An oxidizing gas is supplied into the furnace under heating, and the recycled carbon black to which the rubber carbonized material is attached is stirred and fluidized by the gas flow of the oxidizing gas, thereby bringing the two into contact with each other.
[0063] Step B2 is a process in which the recycled carbon black after step A2 is brought into contact with a hydrocarbon gas in a reactor heated to a specified temperature, thereby filling the pores formed on the surface of the recycled carbon black with charcoal produced by thermal decomposition of the hydrocarbon gas, thereby reducing the specific surface area of the recycled carbon black.
[0064] In step B2, the hydrocarbon gas to be contacted with the recycled carbon black after step A2 is not particularly limited as long as it is heated at a predetermined temperature in the reactor and pyrolyzed to produce a char, and examples of the hydrocarbon gas include methane gas, ethane gas, propane gas, butane gas, etc. The amount of the hydrocarbon gas to be contacted is appropriately selected depending on the specific surface area of the recycled carbon black to be treated, the type of hydrocarbon gas used, the specific surface area of the target modified recycled carbon black, etc.
[0065] In step B2, the temperature in the reactor when the recycled carbon black is brought into contact with the hydrocarbon gas is 600° C. or higher and 1400° C. or lower, preferably 700° C. or higher and 1300° C. or lower, and more preferably 800° C. or higher and 1200° C. or lower. When the temperature in the reactor is within the above range, the hydrocarbon gas is adsorbed into pores having a diameter of several nm or less that exist on the surface of the recycled carbon black, and carbonized, thereby appropriately increasing the specific surface area N 2 SA decreases.
[0066] In the B2 step, the conditions such as the temperature in the reactor when contacting the recycled carbon black with the hydrocarbon gas, the amount of the hydrocarbon gas contacted, and the time are as follows: 2 The SA is appropriately selected so that it falls within the range specified for the modified recycled carbon black of the present invention.
[0067] In step B2, the recycled carbon black after step A2 is placed in a reactor, the reactor is heated to a predetermined temperature, and a hydrocarbon gas is supplied into the reactor while the reactive gas is discharged outside the reactor. In this way, the recycled carbon black after step A2 is brought into contact with the hydrocarbon gas at the predetermined temperature in the reactor to generate a carbonized material, and the pores formed on the surface of the recycled carbon black are filled with the carbonized material.
[0068] For example, in a fluidized bed reactor such as the fluidized bed reactor 1 shown in FIG. 4, the recycled carbon black after the A2 step is placed in the fluidized bed reactor, the inside of the fluidized bed reactor is heated to a predetermined temperature, and while a hydrocarbon gas is supplied from the bottom of the fluidized bed reactor, the reaction gas is discharged from the top of the fluidized bed reactor, thereby carrying out the B2 step.
[0069] A hydrocarbon gas is supplied to the fluidized bed reactor 1 to generate a gas flow. The hydrocarbon gas is preferably supplied in a preheated state to the fluidized bed reactor 1. In this case, the preheating temperature is preferably 400° C. to 600° C., more preferably 450° C. to 600° C., even more preferably 450° C. to 550° C., still more preferably 480° C. to 550° C., and even more preferably 480° C. to 520° C. In addition, the hydrocarbon gas is supplied to the fluidized bed reactor 1 at a flow rate of 0.30 Nm per 100 g of recycled carbon black after the A2 step. 3 / hour more than 3.00Nm 3 / hour or less, and 0.35 Nm 3 / hour over 2.95Nm 3 More preferably, the supply is at 0.40 Nm 3 / hour over 2.90Nm 3 More preferably, the supply is at 0.45 Nm / hour or less. 3 / hour over 2.85Nm 3 More preferably, the supply is at 0.50 Nm / hour or less. 3 / hour over 2.80Nm 3 It is even more preferable to supply the mixture at a rate of 1 / hour or less.
[0070] In addition, the hydrocarbon gas introduced into the fluidized bed reactor 1 is preferably supplied so that the pressure at the gas inlet is 1.0 MPa or more and 2.0 MPa or less, more preferably 1.1 MPa or more and 2.0 MPa or less, even more preferably 1.1 MPa or more and 1.8 MPa or less, even more preferably 1.2 MPa or more and 1.8 MPa or less, and even more preferably 1.2 MPa or more and 1.5 MPa or less.
[0071] When the fluidized bed reactor 1 is used, a hydrocarbon gas is supplied from a gas inlet 21. The hydrocarbon gas may be supplied in a state in which the recycled carbon black after the A2 step has been carried out has been previously introduced into the fluidized bed reactor, or the hydrocarbon gas may be supplied into the fluidized bed reactor, and then the recycled carbon black after the A2 step may be introduced from a supply port separately provided in the fluidized bed reactor.
[0072] The recycled carbon black after the A2 step introduced into the fluidized bed reactor 1 is stirred and fluidized under heating by the gas flow of the hydrocarbon gas. The heating temperature is 600° C. to 1400° C., preferably 700° C. to 1300° C., and more preferably 800° C. to 1200° C. The stirring and fluidization time is preferably 100 seconds to 300 seconds, more preferably 110 seconds to 300 seconds, even more preferably 110 seconds to 280 seconds, even more preferably 120 seconds to 280 seconds, and even more preferably 120 seconds to 250 seconds.
[0073] When using a fluidized bed reactor 1, a hydrocarbon gas is supplied from a gas inlet 21, and then the recycled carbon black after the A2 step is stirred and mixed in the stirring area 4 heated by a heater coil 3. Hydrocarbon gas is supplied into the furnace under heating, and the recycled carbon black after the A2 step is stirred and fluidized by the gas flow of the hydrocarbon gas, thereby bringing the two into contact with each other.
[0074] After stirring with the hydrocarbon gas, the supply of the hydrocarbon gas is stopped, and preferably nitrogen gas is introduced to naturally cool the produced carbon black, thereby stopping the reaction. The nitrogen gas is introduced into the fluidized bed reactor 1 at a flow rate of 6.50 Nm 3 / hour more than 8.50Nm 3 It is preferable to supply the amount of water so that the amount is not more than 7.00 Nm 3 / hour more than 8.50Nm 3 More preferably, the supply is at 7.00 Nm 3 / hour more than 8.00Nm3 More preferably, the supply is at 7.50 Nm / hour or less. 3 / hour more than 8.00Nm 3 More preferably, the supply is at 7.50 Nm / hour or less. 3 / hour more than 7.80Nm 3 It is even more preferable to supply the mixture at a rate of 1 / hour or less.
[0075] The cooled carbon black particles can be separated and collected by a separation and collection device such as a cyclone or a bag filter, thereby recovering the desired modified recycled carbon black.
[0076] One example of a method for producing the modified recycled carbon black of the second embodiment of the present invention is a method for producing modified recycled carbon black, which includes a step of contacting recycled carbon black having rubber carbonized material adhered thereto with an oxidizing gas and a hydrocarbon gas in a reactor heated to 600°C or higher and 1400°C or lower (hereinafter, step C2).
[0077] Step C2 is a process in which an oxidizing gas and a hydrocarbon gas are brought into contact with the recycled carbon black having rubber charcoal attached thereto in a reactor heated to a prescribed temperature, thereby oxidizing, decomposing and removing the rubber residue mainly composed of rubber charcoal attached to the surface of the recycled carbon black, and also, by bringing a hydrocarbon gas into contact with the recycled carbon black from which the rubber residue mainly composed of rubber charcoal has been removed, pores formed on the surface of the recycled carbon black are filled with charcoal produced by the thermal decomposition of the hydrocarbon gas, thereby reducing the specific surface area of the recycled carbon black.
[0078] In the C2 step, the recycled carbon black to be contacted with the oxidizing gas and the hydrocarbon gas is carbon black obtained by pyrolyzing rubber products such as waste tires, and is carbon black having a rubber residue, mainly composed of rubber charcoal, attached to its surface. Examples of the recycled carbon black to be contacted with the oxidizing gas and the hydrocarbon gas include PB365 (trade name) manufactured by Enrestec, BolderBlack (trade name) manufactured by Bolder Industries, DE-Black (trade name) manufactured by Delta Energy, and MondoBlack (trade name) manufactured by ECOLOMONDO. Such recycled carbon black may be produced by any production method, and is not particularly limited, but an example thereof includes the method described in Patent Document 2.
[0079] In the C2 step, the recycled carbon black that is brought into contact with the oxidizing gas and the hydrocarbon gas has a Raman spectrum of 1350±20 cm2 obtained by measuring with an excitation wavelength of 532 nm by laser Raman spectroscopy. -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1 The peak intensity of the peak having a peak top in this range is 112 or more and 200 or less, preferably 112 or more and 190 or less.
[0080] In step C2, the ash content of the recycled carbon black to be contacted with the oxidizing gas is preferably 3.0% or more and 50.0% or less, and more preferably 5.0% or more and 45.0% or less.
[0081] In the C2 step, the oxidizing gas contacted with the recycled carbon black is oxygen gas, a gas containing oxygen, air, etc. In addition, in the C2 step, the hydrocarbon gas contacted with the recycled carbon black is not particularly limited as long as it is heated at a predetermined temperature in the reactor and pyrolyzed to produce a char, and examples thereof include methane gas, ethane gas, propane gas, and butane gas. The contact amount of the oxidizing gas is appropriately selected depending on the recycled carbon black to be treated, the amount of rubber residue attached, the type of oxidizing gas used, the specific surface area of the target modified recycled carbon black, etc. In addition, the contact amount of the hydrocarbon gas is appropriately selected depending on the specific surface area of the recycled carbon black to be treated, the type of hydrocarbon gas used, the specific surface area of the target modified recycled carbon black, etc.
[0082] In step C2, the temperature in the reactor when the oxidizing gas and the hydrocarbon gas are brought into contact with the recycled carbon black is 600° C. to 1400° C., preferably 700° C. to 1300° C., and more preferably 800° C. to 1200° C. When the temperature in the reactor is within the above range, the hydrocarbon gas is adsorbed into pores having a diameter of several nm or less present on the surface of the recycled carbon black and carbonized, thereby appropriately increasing the specific surface area N 2 SA decreases.
[0083] In the C2 step, the conditions such as the temperature in the reactor when the oxidizing gas and the hydrocarbon gas are brought into contact with the recycled carbon black, the amount and time of contact of the oxidizing gas and the hydrocarbon gas, etc. are determined by the G band intensity and N 2 The SA is appropriately selected so that it falls within the range specified for the modified recycled carbon black of the present invention.
[0084] In process C2, the recycled carbon black to which rubber charcoal is attached is placed in a reactor, which is heated to a prescribed temperature. An oxidizing gas and a hydrocarbon gas are supplied into the reactor while the decomposition gas and reaction gas are discharged outside the reactor. In the reactor, the oxidizing gas is brought into contact with the recycled carbon black to which rubber charcoal is attached at the prescribed temperature to oxidize, decompose and remove the rubber residue composed mainly of rubber charcoal attached to the surface of the recycled carbon black. At the same time, the hydrocarbon gas is brought into contact with the recycled carbon black from which the rubber residue composed mainly of rubber charcoal has been removed, filling the pores formed on the surface of the recycled carbon black with charcoal produced by thermal decomposition of the hydrocarbon gas, thereby reducing the specific surface area of the recycled carbon black.
[0085] For example, the recycled carbon black having rubber carbonized material attached thereto is placed in a fluidized bed reactor such as the fluidized bed reactor 1 shown in FIG. 4, and then the inside of the fluidized bed reactor is heated to a predetermined temperature. An oxidizing gas and a hydrocarbon gas are supplied from the lower part of the fluidized bed reactor, while a decomposition gas oxidized by the oxidizing gas and a reaction gas generated by thermal decomposition of the hydrocarbon gas are discharged from the upper part of the fluidized bed reactor, thereby carrying out the C2 process.
[0086] An oxidizing gas and a hydrocarbon gas are simultaneously supplied to the fluidized bed reactor 1 to generate a gas flow. The oxidizing gas and the hydrocarbon gas are preferably supplied in a preheated state to the fluidized bed reactor 1, and in this case, the preheating temperature is preferably 400° C. to 600° C., more preferably 450° C. to 600° C., even more preferably 450° C. to 550° C., still more preferably 480° C. to 550° C., and even more preferably 480° C. to 520° C. In addition, the oxidizing gas and the hydrocarbon gas are supplied to the fluidized bed reactor 1 at a flow rate of 2.50 Nm3 per 100 g of recycled carbon black to which the rubber carbonized material is attached. 3 / hour more than 8.50Nm 3 / hour or less, and 2.55 Nm 3 / hour over 8.45Nm 3 More preferably, the supply is 2.60 Nm3 / hour over 8.40Nm 3 More preferably, the supply is at 2.65 Nm / hour or less. 3 / hour more than 8.35Nm 3 More preferably, the supply is at 2.70 Nm / hour or less. 3 / hour more than 8.30Nm 3 It is more preferable to supply the hydrocarbon gas to the fluidized bed reactor 1 at a rate of 0.30 Nm3 / hr or less. 3 / hour more than 3.00Nm 3 / hour or less, and 0.35 Nm 3 / hour over 2.95Nm 3 More preferably, the supply is at 0.40 Nm 3 / hour over 2.90Nm 3 More preferably, the supply is at 0.45 Nm / hour or less. 3 / hour over 2.85Nm 3 More preferably, the supply is at 0.50 Nm / hour or less. 3 / hour over 2.80Nm 3 It is even more preferable to supply the mixture at a rate of 1 / hour or less.
[0087] In addition, the oxidizing gas and the hydrocarbon gas to be introduced into the fluidized bed reactor 1 are preferably supplied so that the pressure at the gas inlet is 1.0 MPa or more and 2.0 MPa or less, more preferably 1.1 MPa or more and 2.0 MPa or less, even more preferably 1.1 MPa or more and 1.8 MPa or less, even more preferably 1.2 MPa or more and 1.8 MPa or less, and even more preferably 1.2 MPa or more and 1.5 MPa or less.
[0088] When the fluidized bed reactor 1 is used, an oxidizing gas and a hydrocarbon gas are supplied from a gas inlet 21. The oxidizing gas may be supplied in a state where the recycled carbon black having the rubber carbonized material adhered thereto has been previously introduced into the reactor, or the oxidizing gas and the hydrocarbon gas may be supplied into the fluidized bed reactor, and then the recycled carbon black having the rubber carbonized material adhered thereto may be introduced from a supply port separately provided in the fluidized bed reactor.
[0089] The recycled carbon black having the rubber carbonized material attached thereto is introduced into the fluidized bed reactor 1 and stirred and fluidized under heating by the gas flows of the oxidizing gas and the hydrocarbon gas. The heating temperature is 600° C. to 1400° C., preferably 700° C. to 1300° C., and more preferably 800° C. to 1200° C. The stirring and fluidization time is preferably 100 seconds to 300 seconds, more preferably 110 seconds to 300 seconds, even more preferably 110 seconds to 280 seconds, even more preferably 120 seconds to 280 seconds, and even more preferably 120 seconds to 250 seconds.
[0090] When using the fluidized bed reactor 1, an oxidizing gas and a hydrocarbon gas are supplied from the gas inlet 21, and then the recycled carbon black to which the rubber carbonized material is attached is stirred and mixed in the stirring zone 4 heated by the heater coil 3. The oxidizing gas and the hydrocarbon gas are supplied into the furnace under heating, and the recycled carbon black to which the rubber carbonized material is attached is stirred and fluidized by the gas flows of the oxidizing gas and the hydrocarbon gas, thereby bringing the two into contact with each other.
[0091] After stirring with the oxidizing gas and the hydrocarbon gas, the supply of the oxidizing gas and the hydrocarbon gas is stopped, and preferably nitrogen gas is introduced to naturally cool the produced carbon black, thereby stopping the reaction. The nitrogen gas is introduced into the fluidized bed reactor 1 at a flow rate of 6.50 Nm 3 / hour more than 8.50Nm 3 It is preferable to supply the amount of water so that the amount is not more than 7.00 Nm 3 / hour or more~8.50Nm 3 More preferably, the supply is at 7.00 Nm3 / hour more than 8.00Nm 3 More preferably, the supply is at 7.50 Nm / hour or less. 3 / hour more than 8.00Nm 3 More preferably, the supply is at 7.50 Nm / hour or less. 3 / hour more than 7.80Nm 3 It is even more preferable to supply the mixture at a rate of 1 / hour or less.
[0092] The cooled carbon black particles can be separated and collected by a separation and collection device such as a cyclone or a bag filter, thereby recovering the desired modified recycled carbon black.
[0093] In the second embodiment of the method for producing the modified recycled carbon black of the present invention, N is obtained by carrying out the steps A2 and B2 or by carrying out the step C2. 2 SA is 50m 2 / g or more 250m 2 / g or less, preferably 55m 2 / g or more 245m 2 / g or less, more preferably 60m 2 / g or more 240m 2 / g or less, and the Raman spectrum obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm is 1350 ± 20 cm -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1 In this manner, a modified recycled carbon black having a peak intensity of 84 or more and 111 or less, preferably 85 or more and 110 or less, and more preferably 86 or more and 109 or less, is obtained.
[0094] In the first embodiment of the present invention, the method for producing the modified recycled carbon black comprises the steps of: (a) oxidatively decomposing a rubber residue, the main component of which is rubber charcoal, attached to the recycled carbon black to which rubber charcoal is attached; and (b) determining whether the G band intensity and N band intensity of the recycled carbon black are 100; 2This is a method for setting both the SA and the modified recycled carbon black of the present invention to their specified values.
[0095] In one example of the method for producing the modified recycled carbon black of the second embodiment of the present invention, the rubber residue mainly composed of rubber charcoal attached to the recycled carbon black having rubber charcoal attached thereto is oxidatively decomposed in step A2. When the D band intensity of the recycled carbon black is taken as 100, the G band intensity can be adjusted to the specified value of the modified recycled carbon black of the present invention. However, due to the progress of oxidation, many pores are formed in the recycled carbon black, and the N band intensity is reduced. 2 When the SA of the modified recycled carbon black of the present invention becomes larger than the specified value, the B2 step is carried out to fill the pores with carbon. 2 Alternatively, one example of a method for producing the modified recycled carbon black of the second embodiment of the present invention is a method for adjusting the SA to the specified value of the modified recycled carbon black of the present invention by oxidative decomposition of rubber residues mainly composed of rubber charcoal adhering to the recycled carbon black to which rubber charcoal is adhering in the step A2, whereby the G band intensity and N 2 Although the SA could be set to the specified value of the modified recycled carbon black of the present invention, further, N 2 If you want to adjust the SA, you can fill the pores with carbide in step B2 to reduce the amount of N 2 This is a method for adjusting the SA within the specified range of the modified recycled carbon black of the present invention.
[0096] In one example of the method for producing the modified recycled carbon black of the second embodiment of the present invention, the rubber residue mainly composed of rubber charcoal attached to the recycled carbon black having rubber charcoal attached thereto is oxidatively decomposed in step C2. When the D band intensity of the recycled carbon black is taken as 100, the G band intensity can be adjusted to the specified value of the modified recycled carbon black of the present invention. However, due to the progress of oxidation, many pores are formed in the recycled carbon black, and therefore the N band intensity is reduced. 2If the SA is greater than the specified value of the modified recycled carbon black of the present invention, or if N 2 If you want to adjust the SA, you can fill the pores with carbide at the same time in the C2 process to reduce the amount of N 2 This is a method for adjusting the SA to the specified value of the modified recycled carbon black of the present invention or within the range of the specified value.
[0097] The modified recycled carbon black of the first embodiment of the present invention is obtained by a step of contacting recycled carbon black having rubber carbonized material adhered thereto with an oxidizing gas in a reactor heated to 600° C. or more and 1,400° C. or less, N 2 SA is 50m 2 / g or more 250m 2 / g or less, preferably 55m 2 / g or more 245m 2 / g or less, more preferably 60m 2 / g or more 240m 2 / g or less, In the Raman spectrum obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm, the peak intensity was 1350 ± 20 cm -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1 the peak intensity of a peak having a peak top in the range of 84 to 111, preferably 85 to 110, more preferably 86 to 109; It is characterized by:
[0098] The step of contacting the recycled carbon black having rubber carbonized material adhered thereto with an oxidizing gas in a reactor heated to 600°C or higher and 1400°C or lower in the modified recycled carbon black of the first embodiment of the present invention is the same as step A1 in the method for producing the modified recycled carbon black of the first embodiment of the present invention.
[0099] The modified recycled carbon black of the second embodiment of the present invention is obtained by carrying out a step of contacting an oxidizing gas with recycled carbon black having rubber carbonized material adhered thereto in a reactor heated to 600° C. or more and 1400° C. or less, and a step of contacting a hydrocarbon gas with the same. N 2 SA is 50m 2 / g or more 250m 2 / g or less, preferably 55m 2 / g or more 245m 2 / g or less, more preferably 60m 2 / g or more 240m 2 / g or less, In the Raman spectrum obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm, the peak intensity was 1350 ± 20 cm -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is taken as 100, -1 the peak intensity of a peak having a peak top in the range of 84 to 111, preferably 85 to 110, more preferably 86 to 109; It is characterized by:
[0100] An example of the modified recycled carbon black of the second embodiment of the present invention is a modified recycled carbon black obtained by carrying out a step of contacting recycled carbon black having rubber carbonized material adhered thereto with an oxidizing gas in a reactor heated to 600°C or higher and 1400°C or lower (hereinafter, step A2), and a step of contacting the recycled carbon black that has been subjected to the step of contacting with the oxidizing gas with a hydrocarbon gas (step B2).
[0101] An example of the modified recycled carbon black of the second embodiment of the present invention is a modified recycled carbon black obtained by a process (hereinafter, referred to as process C2) in which recycled carbon black having rubber carbonized material attached thereto is contacted with an oxidizing gas and a hydrocarbon gas in a reactor heated to 600°C or higher and 1400°C or lower.
[0102] Steps A2, B2, and C2 relating to the modified recycled carbon black of the second embodiment of the present invention are the same as steps A2, B2, and C2 relating to the method for producing the modified recycled carbon black of the second embodiment of the present invention.
[0103] The modified recycled carbon black of the present invention, the modified recycled carbon black obtained by carrying out the method for producing modified recycled carbon black of the first embodiment of the present invention, and the modified recycled carbon black obtained by carrying out the method for producing modified recycled carbon black of the second embodiment of the present invention have no adhesion of rubber residues mainly composed of rubber carbonized material, or even if adhesion is present, it is very small, and the cohesiveness is suppressed to a low level, so that the bond with the rubber component can be made as strong as that of carbon black that has never been used as a tire filler, and the reinforcing properties of rubber products can be increased.
[0104] The rubber composition of the present invention comprises a rubber component and 1 part by mass or more and 100 parts by mass or less of the modified recycled carbon black of the present invention relative to 100 parts by mass of the rubber component; The present invention is characterized in that it contains:
[0105] In the rubber composition of the present invention, the rubber component may be at least one selected from diene rubbers such as natural rubber, styrene-butadiene rubber, polybutadiene rubber, isoprene rubber, butyl rubber, chloroprene rubber, and acrylonitrile-butadiene copolymer rubber.
[0106] The rubber composition of the present invention contains the modified recycled carbon black of the present invention, and the details of the modified recycled carbon black of the present invention contained in the rubber composition are as described above. Furthermore, the modified recycled carbon black of the present invention has had the rubber residue, mainly composed of rubber charcoal, adhered to the surface of the recycled carbon black removed and has low cohesiveness. Therefore, the bond with the rubber component is strong, and the rubber composition has a high reinforcing property, so that the rubber composition of the present invention has high strength.
[0107] In the rubber composition of the present invention, the content of the modified recycled carbon black of the present invention is 1 part by mass or more and 100 parts by mass or less per 100 parts by mass of the rubber component, preferably 10 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the rubber component, and more preferably 15 parts by mass or more and 70 parts by mass or less per 100 parts by mass of the rubber component. When the content of the modified recycled carbon black of the present invention is within the above range in the rubber composition of the present invention, a rubber composition with high strength can be obtained.
[0108] The rubber composition of the present invention may also contain necessary components that are commonly used, such as inorganic reinforcing materials, silane coupling agents, vulcanizing agents, vulcanization accelerators, antioxidants, vulcanization aids, softeners, plasticizers, etc. The rubber composition of the present invention preferably contains these components in a total amount of 1% by mass or more and 40% by mass or less, more preferably 2% by mass or more and 30% by mass or less, and even more preferably 3% by mass or more and 25% by mass or less.
[0109] The rubber composition of the present invention can be obtained by kneading a predetermined amount of the modified recycled carbon black of the present invention and, if necessary, desired amounts of an inorganic reinforcing material, a silane coupling agent, a vulcanizing agent, a vulcanization accelerator, an antiaging agent, a vulcanization aid, a softener, a plasticizer, etc., with a rubber component. The kneading can be performed using a kneading machine such as a known mixer or mill.
[0110] The rubber composition of the present invention can be molded into a predetermined shape and then appropriately heated at 130 to 180° C. to cure, thereby obtaining a desired rubber molded article. EXAMPLES
[0111] The invention will now be illustrated by the following examples.
[0112] (Examples 1 to 9, Comparative Examples 1 to 6) 100 g of recycled carbon black (before modification) to be treated as shown in Table 1 was placed in a fluidized bed reactor shown in Fig. 4, and a contact step with an oxidizing gas (step 1) and / or a contact step with a hydrocarbon gas (step 2) was carried out under the conditions shown in Table 1 to obtain modified recycled carbon black. When both steps 1 and 2 were carried out, step 2 was carried out after step 1 in Examples 1 to 8 and Comparative Examples 1 to 6. In Example 9, the oxidizing gas and the hydrocarbon gas were supplied simultaneously to carry out steps 1 and 2 simultaneously.
[0113] (Reference examples 1~2) As the unused carbon black, unused products of the commercially available products SEAST 3 (Reference Example 1) and SEAST 6 (Reference Example 2) were used.
[0114] Next, the nitrogen adsorption specific surface area N of the recycled carbon black before modification, the modified recycled carbon black, and the unused carbon black was measured. 2 The G band intensity was measured when the SA and D band intensities were set at 100. The results are shown in Table 2. Electron micrographs obtained by observing unused carbon black (SEAST6), recycled carbon black before modification (rCB before modification, rCB1), and modified recycled carbon black (rCB after modification, Example 7) with an electron microscope are shown in Figures 6A, 6B, and 6C, respectively.
[0115] Next, as shown in Table 3, 100 parts by mass of natural rubber (RSS#1) as a rubber component, any of the modified recycled carbon blacks obtained in the above Examples and Comparative Examples, 45 parts by mass of recycled carbon black or unused carbon black before modification, 3 parts by mass of stearic acid, 1 part by mass of an antioxidant (Antage 6C, manufactured by Kawaguchi Chemical Industry Co., Ltd.), and 4 parts by mass of zinc oxide were kneaded in a closed mixer (MIXTRON BB-2, manufactured by Kobe Steel, Ltd.), and then 0.5 parts by mass of a vulcanization accelerator (Accel NS, manufactured by Kawaguchi Chemical Industry Co., Ltd.) and 1.5 parts by mass of sulfur were kneaded with the kneaded mixture in an open roll to obtain a rubber composition. Next, each of the obtained rubber compositions was vulcanized at a temperature of 145° C. for 35 minutes to form a vulcanized rubber. The dynamic storage modulus (E') and tensile stress (M300) of the obtained vulcanized rubber were measured by the methods described below. The results are shown in Table 2. The relationship between the dynamic storage modulus (E') and tensile stress (M300) of the examples, comparative examples, and unused carbon black is shown in Figure 5.
[0116] Recycled Carbon Black 1 (rCB1) Recycled carbon black obtained by pyrolysis of waste tires Enrestec, PB365, Ash content: 18.6%, G band intensity when D band intensity is 100: 113 N 2 SA:78m 2 / g Oxidizing gas: Air gas Hydrocarbon gas: methane gas
[0117] <Measurement of (Dynamic Storage Modulus) (E')> Test pieces measuring 2 mm in thickness, 35 mm in length and 5 mm in width were cut from each of the vulcanized rubbers obtained, and the dynamic storage modulus (E') was measured using a fully automatic viscoelasticity analyzer (VR-7130 manufactured by Ueshima Seisakusho Co., Ltd.) in accordance with JIS K6394 2007 "Vulcanized rubber and thermoplastic rubber - Determination of dynamic properties - General guidelines" under the measurement conditions of a frequency of 50 Hz, a dynamic strain rate of 1.26%, and a measurement temperature of 60°C.
[0118] <Measurement of (tensile stress) (M300)> JIS dumbbell-shaped No. 3 test pieces were cut out from each of the obtained vulcanized rubbers, and the stress at 300% elongation was measured using a Strograph AE-CT manufactured by Toyo Seiki Co., Ltd. in accordance with JIS K6251 2017 "Vulcanized rubber and thermoplastic rubber - Determination of tensile properties".
[0119] [Table 1]
[0120] [Table 2]
[0121] [Table 3]
[0122] In Examples 1 to 9, E' was high, at 4.7 MPa or more. On the other hand, E' was low, at 4.0 MPa or less, in rCB1 and Comparative Examples 1 to 6. It was therefore found that the modified recycled carbon blacks of Examples 1 to 9 have strong bonds with the rubber component and can enhance the reinforcing properties of the rubber composition. In addition, in Examples 1 to 9, M300 is 100 kgf / cm 2 From the above, we can see that the M300 can also be made taller. [Industrial Applicability]
[0123] According to the present invention, it is possible to provide a novel recycled carbon black which has strong bonds with rubber components and has a high reinforcing property for rubber products. Therefore, it is possible to produce rubber products having the same performance as virgin carbon black by using recycled carbon black obtained by pyrolysis of rubber products such as waste tires. [Explanation of symbols]
[0124] 1 Fluidized Bed Reactor 2. Reactor body 3 Heater coil 4 Stirring area 5. Filters 21 Gas inlet 22 Exhaust port
Claims
1. N 2 SA is 50m 2 / g or more 250m 2 / g or less, In the Raman spectrum obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm, -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is set to 100, -1 The peak intensity of a peak having a peak top in the range of 84 to 111. Modified recycled carbon black.
2. 2. The modified recycled carbon black according to claim 1, characterized in that the ash content is 3.0% or more and 50.0% or less.
3. The carbon black is obtained by a process of contacting recycled carbon black having rubber carbonized material adhered thereto with an oxidizing gas in a reactor heated to 600° C. or more and 1,400° C. or less. N 2 SA is 50m 2 / g or more 250m 2 / g or less, In the Raman spectrum obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm, -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is set to 100, -1 The peak intensity of a peak having a peak top in the range of 84 to 111. Modified recycled carbon black.
4. The carbon black is obtained by carrying out a step of contacting an oxidizing gas with recycled carbon black having rubber carbonized material adhered thereto and a step of contacting a hydrocarbon gas with the recycled carbon black in a reactor heated to 600° C. or more and 1,400° C. or less, N 2 SA is 50m 2 / g or more 250m 2 / g or less, In the Raman spectrum obtained by measuring with a laser Raman spectroscopy at an excitation wavelength of 532 nm, -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is set to 100, -1 The peak intensity of a peak having a peak top in the range of 84 to 111. Modified recycled carbon black.
5. The recycled carbon black to which the rubber carbonized material is attached has a Raman spectrum of 1350±20 cm in a Raman spectrum obtained by measuring the recycled carbon black at an excitation wavelength of 532 nm by laser Raman spectroscopy. -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is set to 100, -1 5. The modified recycled carbon black according to claim 3, wherein the peak intensity of a peak having a peak top in the range of from 112 to 200.
6. A method for producing modified recycled carbon black, comprising the step of contacting recycled carbon black having rubber carbonized material adhered thereto with an oxidizing gas in a reactor heated to 600°C or higher and 1400°C or lower.
7. A method for producing modified recycled carbon black, comprising the steps of contacting recycled carbon black having rubber carbonized material adhered thereto with an oxidizing gas and contacting the recycled carbon black with a hydrocarbon gas in a reactor heated to 600°C or higher and 1400°C or lower.
8. 8. The method for producing modified recycled carbon black according to claim 7, wherein the step of contacting the hydrocarbon gas is carried out after the step of contacting the oxidizing gas.
9. The recycled carbon black to which the rubber carbonized material is attached has a Raman spectrum of 1350±20 cm in a Raman spectrum obtained by measuring the recycled carbon black at an excitation wavelength of 532 nm by laser Raman spectroscopy. -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is set to 100, -1 8. The method for producing modified recycled carbon black according to claim 6, wherein the carbon black has a peak intensity of 112 or more and 200 or less, the peak intensity having a peak top in the range of 112 or more and 200 or less.
10. A rubber component, The modified recycled carbon black according to claim 1 in an amount of 1 part by mass or more and 100 parts by mass or less per 100 parts by mass of the rubber component; A rubber composition comprising:
Citation Information
Patent Citations
Regenerated carbon black, preparation method and application thereof
CN113667328A
Method for preparing superfine waste tire thermal cracking carbon black for rubber by wet method
CN114381290A
Method for recycling carbonaceous materials from waste tires and products derived from waste tires
JP2012521443A
Fin tube for heat exchange used for tunnel kiln
JP1983013985A
JPS3717807B1
Cited By
Method of recovering carbon black of waste tire
JP2024157149A
Carbon black, method for producing the same, and its use
JP2025117569A
Method for Recovering Carbon Black from Waste Tires
JP7717113B2