Inorganic oxide particle
Inorganic oxide particles with tailored particle size and fluidity characteristics address uneven material distribution in binder jet methods, achieving uniform layers and low shrinkage in additive manufacturing.
Patent Information
- Application Number
- JP2024123491
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-12-26
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-29
AI Technical Summary
The binder jet method in additive manufacturing often results in uneven distribution of constituent materials, leading to voids and uneven structures in the three-dimensional layered product, necessitating powders with good spreading properties, uniformity, and low shrinkage during sintering.
Inorganic oxide particles with specific particle size distributions, fluidity, and bulk density characteristics, such as D50 of 5.5-9.0 μm, pressure loss of 1.75-2.81 kPa, and circularity of 0.90 or more, allowing for uniform layer formation and shape stability from binder application to sintering.
These particles enable the formation of uniform powder layers with maintained shape stability and low shrinkage rates during sintering, enhancing the quality of three-dimensional additive manufacturing products.
Smart Images

Figure 2024153813000001 
Figure 2024153813000002 
Figure 2024153813000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to inorganic oxide particles, a sintered body thereof, and a method for producing a binder jet additive manufacturing product. [Background technology]
[0002] In recent years, processing methods called additive manufacturing (AM) technology, 3D printing technology, etc., have been attracting attention. This is a technology in which a cross-sectional shape of a target object is created based on data of the three-dimensional shape and then laminated. As additive manufacturing technologies, processing methods such as a binder jet type (Patent Document 1) in which a binder is sprayed onto a powder material on a modeling stage to selectively model an object, a material jet type in which a photocurable resin or the like is sprayed from an inkjet nozzle to selectively model an object, a powder bed melting type in which a laser or electron beam is irradiated onto a powder bed covered with metal powder or the like to selectively melt and model an object, and a photolithography method (Patent Document 2) in which light is irradiated onto a slurry in which a liquid photocurable resin and an inorganic powder are mixed to form an object. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-117069 A [Patent Document 2] Patent Publication No. 2021-11050 Summary of the Invention [Problem to be solved by the invention]
[0004] The binder jet method is also known by the term "3D inkjet powder printing." This method includes, for example, a step of supplying powder material to a modeling stage using a roller to form a uniform powder layer, and a step of applying a liquid binder to the powder layer using an inkjet print head to selectively bond a part of the powder layer. By repeating these steps, the desired three-dimensional additive manufacturing object can be obtained. The three-dimensional additive manufacturing object is then subjected to a sintering process as necessary. In the binder jet method, a structure in which the distribution of constituent materials, such as voids, is uneven in the obtained three-dimensional additive manufacturing object may occur. In order to suppress this, it is desirable for the additive manufacturing powder to have good laying properties that allow it to be smoothly supplied to the modeling stage and to be laid out uniformly. In addition, it is believed that a highly uniform three-dimensional additive manufacturing object can be obtained by filling the additive manufacturing powder at a high density. In order to achieve good laying properties and high density filling, it is useful to increase the fluidity of the powder material. On the other hand, when applying the binder, it is also required that the powder layer is not disturbed and that the binder can penetrate between the powder materials. In addition, it is also desirable that the shrinkage rate during sintering is low.
[0005] The present disclosure provides inorganic oxide particles that, when used as a powder for additive manufacturing, have appropriate fluidity to achieve both good spreadability to form a uniform powder layer and shape stability to maintain the shape from the application of the binder to the sintering process, and an appropriate bulk density that allows the binder to penetrate between the powder materials and achieves a low shrinkage rate during sintering. [Means for solving the problem]
[0006] The present disclosure relates to the following: [1] D50 is 5.5 to 9.0 μm, Inorganic oxide particles having a pressure loss of 1.75 to 2.81 kPa with respect to air permeation under a pressure of 12 kPa. [2] The inorganic oxide particles according to [1], wherein (D10+D90) / D50 is 2.7 or more. [3] BET specific surface area is 0.10 to 10.00 m 2 / g of the inorganic oxide particles according to [1] or [2]. [4] The inorganic oxide particles according to any one of [1] to [3], wherein the volume ratio of particles having a particle diameter of 16.8 to 60.0 μm is 4.3 to 33.5 vol %. [5] The inorganic oxide particles according to any one of [1] to [4], wherein the volume ratio of particles having a particle diameter of 2.0 μm or more is 90.0 volume % or more. [6] The inorganic oxide particles according to any one of [1] to [5], which are alumina. [7] The inorganic oxide particles according to any one of [1] to [6], which have a circularity of 0.90 or more. [8] The inorganic oxide particles according to any one of [1] to [7], which are used in powder additive manufacturing. [9] Press molding under a pressure of 98 MPa. Bulk density is 2.45 to 2.54 g / cm 3 [6] Inorganic oxide particles according to the present invention.
[10] A sintered body of inorganic oxide particles according to any one of [1] to [9].
[11] A method for producing a binder jet type additive manufacturing object, comprising applying a liquid containing a binder to inorganic oxide particles according to any one of [1] to [9] to form a three-dimensional additive manufacturing object.
[12] Applying a liquid containing a binder to the inorganic oxide particles according to any one of [1] to [9] to form a three-dimensional additive manufacturing object; and The three-dimensional laminated body is subjected to a sintering process. A method for producing a sintered body, comprising: Effect of the Invention
[0007] According to the present disclosure, when used as a powder for additive manufacturing, it is possible to provide inorganic oxide particles that have suitable fluidity to achieve both good spreadability to form a uniform powder layer and shape stability to maintain the shape between the application of the binder and the sintering process, and suitable bulk density to allow the binder to penetrate between the powder materials and achieve a low shrinkage rate during sintering. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the present invention will be described. Note that the embodiments described below are representative examples of the present invention, and the present invention is not limited thereto.
[0009] In this specification, when "~" is used for a numerical range, the numerical values at both ends are the upper limit and the lower limit, respectively, and are included in the numerical range. When multiple upper or lower limits are listed, numerical ranges can be created from all combinations of the upper and lower limits. Similarly, when multiple numerical ranges are listed, separate numerical ranges can be created by individually selecting and combining the upper and lower limits from those numerical ranges.
[0010] In this specification, D10, D50, and D90 are the 10% particle size, 50% particle size, and 90% particle size, respectively, in the volume-based cumulative particle size distribution measured using an electrical resistance method particle size distribution measurement device (Beckman Coulter, Multisizer 4) with an aperture size of 100 μm.
[0011] In this specification, the press-molded bulk density means the density of a molded body obtained by filling a sample into a circular mold with an inner diameter of 30 mm and pressing it under a predetermined pressure using a commercially available press. The press-molded bulk density is a value that serves as an index of the bulk density of a powder layer when a thin layer of powder is formed using a roller or the like.
[0012] In this specification, the angle of repose is a value measured and calculated according to JIS R 9301-2-2:1999 (alumina powder--Part 2: Measurement of physical properties--2: Angle of repose).
[0013] In this specification, the BET specific surface area is a value measured and calculated in accordance with "6.2 Fluidized method (3.5) Single point method" of JIS R 1626:1996 (Method of measuring specific surface area of fine ceramic powder by gas adsorption BET method). The measurement is performed by heating the sample to 180°C as a pretreatment, flowing nitrogen gas for 20 minutes, and then using nitrogen gas as the adsorbate.
[0014] In this specification, the circularity is the average value of values calculated from the following formula (1) for 2,000 or more particles, where S is the area of a projection image of a particle obtained by an image particle size distribution analyzer and L is the circumferential length. 4πS / L 2 (1)
[0015] In this specification, the pressure loss for air permeation under a certain pressure is the pressure loss measured using a powder rheometer FT4 (Freeman Technology) when air at room temperature (23°C) is passed through a powder bed at a linear velocity of 2 mm / sec. Specifically, a sample is placed in a column with a column diameter of 25 mm and a column length of 20 mm, and the powder bed is pressurized at a certain pressure using a mesh piston to perform the measurement. Note that, before the measurement, the powder placed in the column is subjected to a downward conditioning operation three times. The sample volume is 10 mL based on the volume after conditioning.
[0016] <Inorganic oxide particles> The inorganic oxide particles have a D50 of 5.5 to 9.0 μm and a pressure loss of 1.75 to 2.81 kPa with respect to air permeation under a pressure of 12 kPa. By satisfying the above ranges, a good balance between the fluidity and bulk density of the powder material can be achieved.
[0017] The circularity of the inorganic oxide particles is preferably 0.90 or more. If the circularity is 0.90 or more, the friction between particles is small, so that good flowability can be obtained. If the circularity is 0.90 or more, the packing property of the particles is high, so that the press molding bulk density can be increased. From the same viewpoint, the circularity of the inorganic oxide particles is preferably 0.93 or more, more preferably 0.95 or more. The upper limit of the circularity of the inorganic oxide particles is not particularly limited, but may be, for example, 1.00 or 0.99.
[0018] The pressure loss of the inorganic oxide particles with respect to air permeation under a pressure of 12 kPa is 1.75 kPa or more, preferably 2.00 kPa or more, and more preferably 2.20 kPa or more. The pressure loss of the inorganic oxide particles with respect to air permeation under a pressure of 12 kPa is 2.81 kPa or less, preferably 2.79 kPa or less, and more preferably 2.77 kPa or less. It is considered that a low shrinkage rate during sintering can be achieved when the pressure loss is 1.75 kPa or more. Inorganic oxide particles with a D50 that is not too large and a pressure loss with respect to air permeation under a pressure of 12 kPa of 2.81 kPa or less have a moderate bulk density, and the binder easily penetrates between the powder materials.
[0019] The D50 of the inorganic oxide particles is 5.5 μm or more, preferably 6.0 μm or more, and more preferably 6.5 μm or more. The D50 of the inorganic oxide particles is 9.0 μm or less, preferably 8.5 μm or less, and more preferably 8.0 μm or less. If the D50 of the inorganic oxide particles is 5.5 μm or more, the packing property of the particles is high, so that the press molding bulk density can be increased. If the D50 of the inorganic oxide particles is 5.5 μm or more, when the inorganic oxide particles are used as powder for additive manufacturing, the shape stability of the formed powder layer is good and the shrinkage rate during sintering can be reduced. If the D50 of the inorganic oxide particles is 9.0 μm or less, the packing property and fluidity of the particles can be set to a range appropriate for powder additive manufacturing and coating applications.
[0020] The D10 of the inorganic oxide particles is preferably 1.0 to 4.0 μm, more preferably 2.0 to 3.8 μm, and even more preferably 3.0 to 3.6 μm. If the D10 of the inorganic oxide particles is 1.0 μm or more, the packing property of the particles is high, so that the press molding bulk density can be increased. If the D10 of the inorganic oxide particles is 1.0 μm or more, when the inorganic oxide particles are used as powder for additive manufacturing, the shrinkage rate during sintering can be reduced. If the D10 of the inorganic oxide particles is 4.0 μm or less, the packing property and fluidity of the particles can be within a range suitable for powder additive manufacturing and coating applications.
[0021] The D90 of the inorganic oxide particles is preferably 13.0 to 40.0 μm, more preferably 15.0 to 30.0 μm, and even more preferably 21.0 to 25.0 μm. If the D90 of the inorganic oxide particles is 13.0 μm or more, the packing property of the particles is high, so that the press molding bulk density can be increased. If the D90 of the inorganic oxide particles is 13.0 μm or more, when the inorganic oxide particles are used as a powder for additive manufacturing, the shape stability of the formed powder layer is good. If the D90 of the inorganic oxide particles is 40.0 μm or less, the packing property and fluidity of the particles can be set to a range appropriate for powder additive manufacturing and coating applications. If the D90 of the inorganic oxide particles is 40.0 μm or less, when the inorganic oxide particles are used as a powder for additive manufacturing, the uniformity of the formed powder layer is better.
[0022] The volume ratio of particles having a particle diameter of 16.8 to 60.0 μm in the inorganic oxide particles is preferably 4.3 vol% or more, more preferably 10.0 vol% or more, and even more preferably 15.0 vol% or more. The volume ratio of particles having a particle diameter of 16.8 to 60.0 μm in the inorganic oxide particles is preferably 33.5 vol% or less, more preferably 21.0 vol% or less, and even more preferably 20.0 vol% or less. If the volume ratio of particles having a particle diameter of 16.8 to 60.0 μm is within the above range, appropriate fluidity can be expected when the inorganic oxide particles are used as powder for additive manufacturing. The volume ratio of particles having a particle diameter of 16.8 to 60.0 μm in the inorganic oxide particles is a value determined by measuring with an aperture size of 100 μm using an electrical resistance method particle size distribution measuring device (Beckman Coulter, Multisizer 4).
[0023] The volume ratio of particles having a particle diameter of 2.0 μm or more in the inorganic oxide particles is preferably 90.0 to 100 volume%, more preferably 93.0 to 100 volume%, and even more preferably 95.0 to 100 volume%. If the volume ratio of particles having a particle diameter of 2.0 μm or more is 90.0 volume% or more, when the inorganic oxide particles are used as a powder for additive manufacturing, the shrinkage rate during sintering can be reduced. The volume ratio of particles having a particle diameter of 2.0 μm or more in the inorganic oxide particles is a value determined by a laser diffraction / scattering type particle size distribution measuring device (Microtrack Bell Co., Ltd., MT3300EXII).
[0024] The ratio of D50 to D10 (D50 / D10) of the inorganic oxide particles is preferably 2.0 to 2.3. If D50 / D10 is within the above range, when the inorganic oxide particles are used in a binder jet method, it is expected that the inorganic oxide particles have a suitable fluidity that satisfies both good laying property that allows a uniform powder layer to be formed and shape stability that allows the shape to be maintained from the application of the binder to the sintering process.
[0025] The ratio of D90 to D10 (D90 / D10) of the inorganic oxide particles is preferably 4.0 to 8.0, more preferably 5.0 to 7.5, and even more preferably 5.5 to 7.0. If D90 / D10 is 8.0 or less, the particle size distribution of the inorganic oxide particles falls within a certain range, so that when used as a powder for additive manufacturing, fine particles are appropriately arranged between coarse particles, and flowability can be made appropriate. If D90 / D10 is 4.0 or more, when used as a powder for additive manufacturing, fine particles are appropriately arranged between coarse particles, and bulk density can be made appropriate.
[0026] The ratio of D90 to D50 (D90 / D50) of the inorganic oxide particles is preferably 2.3 to 3.6, more preferably 2.5 to 3.5, and even more preferably 2.8 to 3.4. If D90 / D50 is 3.6 or less, the particle size distribution of the inorganic oxide particles falls within a certain range, so that when used as a powder for additive manufacturing, fine particles are appropriately arranged between coarse particles, and flowability can be made appropriate. If D90 / D50 is 2.3 or more, if used as a powder for additive manufacturing, fine particles are appropriately arranged between coarse particles, and bulk density can be made appropriate.
[0027] It is preferable that the inorganic oxide particles have D10, D50 and D90 that satisfy the relationship of the following formula (I). (D10+D90) / D50≧2.7 (I)
[0028] (D10+D90) / D50 is an index of the particle size distribution of inorganic oxide particles, and the larger the value, the wider the particle size distribution width. When the value of (D10+D90) / D50 is 2.7 or more, that is, when the inorganic oxide particles satisfy the relationship of formula (I), the particle size distribution width is appropriately wide. In this case, the particles are likely to be in an appropriate packed state in which the binder can penetrate between the powder materials. The value of (D10+D90) / D50 is more preferably 2.9 or more, and even more preferably 3.0 or more. The value of (D10+D90) / D50 is preferably 6.0 or less, and more preferably 4.0 or less.
[0029] The angle of repose of the inorganic oxide particles is preferably 55 to 59°, and more preferably 56 to 58°. The angle of repose is one of the indicators of powder fluidity. If the angle of repose of the inorganic oxide particles is 55° or more, the shape stability of the powder layer formed using the inorganic oxide particles as powder for additive manufacturing is good. If the angle of repose of the inorganic oxide particles is 59° or less, when the inorganic oxide particles are used in powder additive manufacturing, the inorganic oxide particles can be smoothly supplied to the modeling stage and evenly spread.
[0030] The BET specific surface area of the inorganic oxide particles is preferably 0.10 m 2 / g or more, more preferably 0.20m 2 / g or more, more preferably 0.30m 2 The BET specific surface area of the inorganic oxide particles is preferably 10.00 m 2 / g or less, more preferably 5.00m 2 / g or less, and more preferably 2.00m 2 / g or less, and particularly preferably 0.50m 2 The BET specific surface area of the inorganic oxide particles is preferably 0.10 to 10.00 m 2 / g, more preferably 0.10 to 5.00 m 2 / g, and more preferably 0.20 to 2.00 m 2 / g, and particularly preferably 0.30 to 0.50 m 2 / g. The BET specific surface area is 0.10 m 2 When the BET specific surface area is 10.00 m / g or more, the powder layer formed by using the inorganic oxide particles as a powder for additive manufacturing has good shape stability. 2 If the inorganic oxide particles have a molecular weight of 1000 or less, when used in powder additive manufacturing, the inorganic oxide particles can be smoothly supplied to a modeling stage and spread evenly.
[0031] The shape of the inorganic oxide particles is not particularly limited. For example, it may be spherical, ellipsoidal, scaly, irregular, etc. Among them, the spherical shape is preferred because it is easy to obtain an appropriate bulk density.
[0032] The inorganic oxide particles are preferably at least one selected from silica, alumina, zirconia, and titania, more preferably alumina, and more preferably spherical alumina. Alumina is preferred because it has high thermal conductivity, melting point, and hardness, is inexpensive, and is resistant to acids and alkalis. The volume ratio of alumina in the inorganic oxide particles is preferably 50% by volume or more, more preferably 60% by volume or more, and even more preferably 80% by volume or more. The upper limit of the volume ratio of alumina in the inorganic oxide particles is not particularly limited. For example, it may be 100% by volume, 98% by volume, or 95% by volume.
[0033] When the inorganic oxide particles are alumina, the press-molded bulk density of the inorganic oxide particles under a pressure of 98 MPa is preferably 2.45 to 2.54 g / cm. 3 The bulk density of inorganic oxide particles pressed under a pressure of 98 MPa is 2.45 g / cm 3 If the inorganic oxide particles have a bulk density of 2.54 g / cm3 or more when used as a powder for additive manufacturing, the dimensional stability during sintering is good. 3 If the inorganic oxide particles are used in a binder jet method, the binder can easily penetrate between the powder materials when applied, and the strength of the shaped body and sintered body can be sufficient if the binder is within the range of 0.1 to 1.0.
[0034] Inorganic oxide particles are suitable for use in powder additive manufacturing. By using inorganic oxide particles, a molded body with fewer voids can be produced, and the effect of reducing heat shrinkage during sintering of the molded body can be expected. In particular, inorganic oxide particles have good laying properties, shape stability of the powder layer, and appropriate bulk density, so they are suitable for use in the binder jet method in which a liquid binder is sprayed onto a spread powder material to solidify it. Inorganic oxide particles can also be applied to the powder bed melting method in which a powder bed spread with powder material is irradiated with a laser or electron beam to selectively melt and mold the material, and other powder additive manufacturing methods.
[0035] Since inorganic oxide particles have a suitable fluidity and a suitable bulk density that allows liquid to easily penetrate, they can be used as a filler material that imparts fluidity and thermal conductivity. Specifically, they can be used as a filler in a heat dissipating material, for example, a filler in a paint such as a heat dissipating paint, a heat insulating paint, and an abrasion resistant paint that require good coating properties, a filler in a heat conductive resin composition having adhesive properties, and a filler in a heat conductive coating material that has a function of curing in the atmosphere.
[0036] <Method of manufacturing inorganic oxide particles> The inorganic oxide particles can be produced, for example, by mixing a plurality of inorganic oxide particles having different particle size distributions so that the particle size distribution of the inorganic oxide particles falls within a predetermined range. The particle size distribution of the inorganic oxide particles may be adjusted by sieving or the like. The particle size distribution of the inorganic oxide particles can be adjusted to an appropriate range by selecting the type and amount of inorganic oxide particles to be blended. The method of mixing the materials is not particularly limited, and examples of the method include a method of dry mixing or wet mixing the materials. The mixing may be performed manually or using a blender.
[0037] A more specific example of a method for producing inorganic oxide particles is a method of mixing coarse inorganic oxide particles (A) and fine inorganic oxide particles (B) having a D50 smaller than that of the coarse inorganic oxide particles (A) shown below. The coarse inorganic oxide particles (A) and the fine inorganic oxide particles (B) may be different types of inorganic oxide particles or the same type of inorganic oxide. The same type of inorganic oxide particles is preferable because the particles are easily mixed and dispersed uniformly.
[0038] [Coarse inorganic oxide particles (A)] The D50 of the coarse inorganic oxide particles (A) preferably used is 9.0 to 25.0 μm, more preferably 12.0 to 20.0 μm, and even more preferably 14.0 to 18.0 μm. The D10 of the coarse inorganic oxide particles (A) is preferably 1.0 to 8.0 μm, more preferably 2.0 to 7.5 μm, and even more preferably 3.0 to 7.0 μm. The D90 of the coarse inorganic oxide particles (A) is preferably 28.0 to 40.0 μm, more preferably 28.5 to 38.0 μm, and even more preferably 29.0 to 36.0 μm.
[0039] The ratio of D50 to D10 (D50 / D10) of the coarse inorganic oxide particles (A) is preferably 1.5 to 3.5, more preferably 1.7 to 3.2, and even more preferably 2.0 to 3.0. The ratio of D90 to D10 (D90 / D10) of the coarse inorganic oxide particles (A) is preferably 3.5 to 9.0, more preferably 4.0 to 7.0, and even more preferably 4.5 to 6.0. The ratio of D90 to D50 (D90 / D50) of the coarse inorganic oxide particles (A) is preferably 1.7 to 2.3, more preferably 1.8 to 2.2, and even more preferably 1.9 to 2.0.
[0040] The shape of the coarse inorganic oxide particles (A) is not particularly limited. For example, it may be spherical, ellipsoidal, scaly, irregular, etc. Among them, the spherical shape is preferred because it is easy to obtain an appropriate bulk density.
[0041] The coarse inorganic oxide particles (A) are preferably at least one selected from silica, alumina, zirconia, and titania, more preferably alumina, and even more preferably spherical alumina. The volume ratio of alumina in the coarse inorganic oxide particles (A) is preferably 50 volume% or more, more preferably 60 volume% or more, and even more preferably 80 volume% or more. The upper limit of the volume ratio of alumina in the coarse inorganic oxide particles (A) is not particularly limited. For example, it may be 100 volume%, 98 volume%, or 95 volume%.
[0042] [Fine inorganic oxide particles (B)] The D50 of the fine inorganic oxide particles (B) is smaller than the D50 of the coarse inorganic oxide particles (A). The D50 of the fine inorganic oxide particles (B) preferably used is 5.0 to 8.0 μm, more preferably 5.5 to 7.8 μm, and even more preferably 6.0 to 7.5 μm. The D10 of the fine inorganic oxide particles (B) is preferably 1.0 to 4.0 μm, more preferably 2.0 to 3.8 μm, and even more preferably 2.5 to 3.5 μm. The D90 of the fine inorganic oxide particles (B) is preferably 9.0 to 25.0 μm, more preferably 12.0 to 24.0 μm, and even more preferably 14.0 to 23.0 μm.
[0043] The ratio of D50 to D10 (D50 / D10) of the fine inorganic oxide particles (B) is preferably 1.5 to 5.0, more preferably 1.7 to 4.0, and even more preferably 1.8 to 3.0. The ratio of D90 to D10 (D90 / D10) of the fine inorganic oxide particles (B) is preferably 3.5 to 9.0, more preferably 4.5 to 8.0, and even more preferably 5.5 to 7.0. The ratio of D90 to D50 (D90 / D50) of the fine inorganic oxide particles (B) is preferably 2.5 to 3.5, more preferably 2.7 to 3.2, and even more preferably 2.9 to 3.1.
[0044] The shape of the fine inorganic oxide particles (B) is not particularly limited. For example, it may be spherical, ellipsoidal, scaly, irregular, etc. Among them, the spherical shape is preferred because it is easy to obtain an appropriate bulk density.
[0045] The fine inorganic oxide particles (B) are preferably at least one selected from silica, alumina, zirconia, and titania, more preferably alumina, and even more preferably spherical alumina. The volume ratio of alumina in the fine inorganic oxide particles (B) is preferably 50 volume% or more, more preferably 60 volume% or more, and even more preferably 80 volume% or more. The upper limit of the volume ratio of alumina in the fine inorganic oxide particles (B) is not particularly limited. For example, it may be 100 volume%, 98 volume%, or 95 volume%.
[0046] The volume ratio of the coarse inorganic oxide particles (A) to the total volume of the coarse inorganic oxide particles (A) and the fine inorganic oxide particles (B) before mixing is selected so that the particle size distribution of the inorganic oxide particles is in an appropriate range, and may be, for example, 9.5 to 29.0 volume %.
[0047] <Manufacturing method for 3D additive manufacturing> The three-dimensional additive manufacturing object can be manufactured by processing inorganic oxide particles by a known powder additive manufacturing method. Examples of the powder additive manufacturing method include the binder jet method and the powder bed fusion method. The powder additive manufacturing method using inorganic oxide particles as the additive manufacturing powder generally includes the following steps. (1) A step of supplying inorganic oxide particles to the modeling stage of a powder additive manufacturing device (2) A process in which the supplied inorganic oxide particles are spread evenly and thinly using a roller or the like to form a thin layer of inorganic oxide particles. (3) A step of irradiating the formed thin layer of inorganic oxide particles with a laser or an electron beam, or applying a liquid containing a binder to bind the inorganic oxide particles. (4) A step of supplying new inorganic oxide particles onto the solidified inorganic oxide particles. Thereafter, steps (2) to (4) are repeated to produce the desired three-dimensional layered object.
[0048] As a method for applying the binder-containing liquid, a method for ejecting the binder-containing liquid is preferred. The method for ejecting the binder-containing liquid is not particularly limited, and examples thereof include a dispenser method, a spray method, and an inkjet method. Among these, the inkjet method is preferred because it has good quantitation of droplets and can be applied over a large area.
[0049] When using the inkjet method, the liquid containing the binder can be applied by an inkjet head having a nozzle for ejecting the liquid. As the inkjet head, an inkjet head in a known inkjet printer can be suitably used, for example, an industrial inkjet RICOH MH / GH series (RICOH Co., Ltd.).
[0050] The binder is not particularly limited, and known binders such as polyvinylpyrrolidone, polyvinyl alcohol, polyethylene glycol, polyvinyl butyral, acrylic resins, polyamides, etc. The binder can be used by adjusting the viscosity with an appropriate solvent.
[0051] <Method of manufacturing sintered body> A sintered body can be produced by sintering the three-dimensional laminated body by a known sintering method. It is preferable to perform a degreasing treatment before the sintering treatment. A specific method for producing a sintered body is exemplified below.
[0052] The three-dimensional laminated model is placed in a sintering furnace, and the temperature inside the furnace is raised to a degreasing temperature. The degreasing temperature can be set appropriately within the range of, for example, 500 to 700°C. Then, the temperature inside the furnace is maintained at the degreasing temperature for 0.5 to 4 hours to perform a degreasing process in which organic components are burned. The degreasing process is performed in an air atmosphere. The degreasing time can be set according to the type of binder and the organic component ratio in the three-dimensional laminated model. Next, the temperature inside the furnace is raised to a sintering temperature. The sintering temperature can be set appropriately within the range of, for example, 900 to 1300°C. Then, the temperature inside the furnace is maintained at the sintering temperature for 1 to 7 hours to perform a sintering process in which the three-dimensional laminated model is sintered, thereby obtaining a sintered body. The sintering temperature and sintering time can be set according to the type of inorganic oxide particles. The sintering process may be performed in an inert gas atmosphere or an air atmosphere. EXAMPLES
[0053] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0054] <Materials used> Coarse inorganic oxide particles (A): spherical alumina (Alnabeads (trademark) / CB, Resonac Co., Ltd.): true density 3.95 g / m 3 Coarse inorganic oxide particles (B): spherical alumina (Alnabeads (trademark) / CB, Resonac Co., Ltd.): true density 3.95 g / m 3
[0055] <Evaluation method> (bulk density) The bulk density was evaluated from the press-molded bulk density under a pressure of 98 MPa. Specifically, a sample was packed in a circular mold with an inner diameter of 30 mm, and a molded body was produced under a pressure of 98 MPa using a commercially available press. The density of the obtained molded body was determined as the press-molded bulk density under a pressure of 98 MPa. When the press-molded bulk density was 2.45 g / cm 3 When the press molding bulk density is 2.54 g / cm or more, the density of the three-dimensional layered product manufactured using the inorganic oxide particles is high, and the shrinkage rate during sintering is low, which is excellent. 3 When the binder is applied in the binder jet method, the binder can penetrate between the powder materials, which is excellent. That is, the press molding bulk density is 2.45 to 2.54 g / cm 3 In this case, the bulk density was evaluated as good.
[0056] (Circularity) The area S and perimeter L were measured using FPIA-3000 (Malvern Panalytical). As a pretreatment, due to the measurement range of the device, about 10 g of the sample was placed in a gold sieve with a diameter of 200 mm and an opening of 25 μm, and particles larger than 25 μm were removed with shower water. The sample under the sieve was transferred to a plastic container and used as the measurement sample. The measurement conditions were LPF / HPF standard (20x lens) and bright field, and Particle Sheath (Malvern Panalytical) was used as the measurement solvent. 2 g of the sample was weighed in a 50 mL beaker, 50 mL of pure water was added, and the sample was dispersed for 3 minutes with a 200 W ultrasonic disperser, and then placed in the device and measured. As data processing after the measurement, objects with multiple particles on one screen were deleted, and the circularity was calculated.
[0057] (Liquidity) The fluidity was evaluated from the angle of repose. If the angle of repose is 55° or more, when the inorganic oxide particles are used in the binder jet method, the shape stability is excellent in that the shape can be maintained from the application of the binder to the sintering process. If the angle of repose is 59° or less, when the inorganic oxide particles are used in the binder jet method, the inorganic oxide particles can be smoothly supplied to the modeling stage and can be uniformly spread, and therefore the laying property is excellent. In other words, when the angle of repose is 55 to 59°, the fluidity was evaluated as being good in terms of the balance between shape stability and laying property.
[0058] (Pressure loss for air permeation) The pressure loss for air permeation was measured at a pressure of 12 kPa.
[0059] [Example 1] Coarse inorganic oxide particles (A) and fine inorganic oxide particles (B) having the particle size and particle size ratio shown in Table 1 were mixed using a rocking mixer (Aichi Electric Co., Ltd. RMC-600(S) / LH) in such a ratio that the volume ratio of the coarse inorganic oxide particles (A) to the total volume of the coarse inorganic oxide particles (A) and the fine inorganic oxide particles (B) before mixing was 11.1 volume %, to obtain inorganic oxide particles. Table 1 also shows the particle size volume ratio calculated by the following formula (2). (Volume ratio of coarse inorganic oxide particles (A) × D50 of coarse inorganic oxide particles (A)) / (Volume ratio of fine inorganic oxide particles (B) × D50 of fine inorganic oxide particles (B)) (2) The particle size distribution, BET specific surface area, circularity, fluidity, pressure loss for air permeation, and press molding bulk density of the obtained inorganic oxide particles were evaluated. The results are shown in Table 2.
[0060] [Examples 2 to 4, Comparative Examples 1 to 3] Inorganic oxide particles were obtained in the same manner as in Example 1, except that the volume ratio of the coarse inorganic oxide particles (A) to the total volume of the coarse inorganic oxide particles (A) and the fine inorganic oxide particles (B), and the volume ratio of the coarse inorganic oxide particles (A) to the total volume of the coarse inorganic oxide particles (A) and the fine inorganic oxide particles (B) before mixing were set as shown in Table 1. Table 1 also shows the particle size volume ratio calculated by the above formula (2). The particle size distribution, BET specific surface area, circularity, fluidity, pressure loss for air permeation, and press molding bulk density of the obtained inorganic oxide particles were evaluated. The results are shown in Table 2. Items that were not evaluated are marked with "-".
[0061] [Table 1]
[0062] [Table 2-1] [Table 2-2]
[0063] As shown by Examples 1 to 4 and Comparative Examples 1 to 3, inorganic oxide particles having a D50 of 5.5 to 9.0 μm and a pressure loss of 1.75 to 2.81 kPa for air permeation under a pressure of 12 kPa have good bulk density and fluidity. Examples 1 to 4 have an angle of repose in the range of 55 to 59° and have appropriate fluidity for the binder jet method. Therefore, it is considered that when Examples 1 to 4 are used in the binder jet method, a uniform powder layer can be formed when a thin layer is formed, and the shape can be maintained from the application of the binder to the sintering process. In addition, Examples 1 to 4 have a press molding bulk density of 2.45 to 2.54 g / cm 3 This ranges from 0.01 to 0.15, and the press molding bulk density is appropriate for the binder jet method. Therefore, when Examples 1 to 4 are used in the binder jet method, it is considered that the binder can penetrate between the powder materials and a low shrinkage rate can be achieved during sintering.
[0064] Comparative Example 1 has a low press molding bulk density, which is presumed to be due to the fact that the adhesion between particles is high due to the small D50, and air is easily taken in during pressing. As a result, it is expected that Comparative Example 1 will have a large shrinkage rate during sintering when used in the binder jet method. Comparative Example 2 has a larger D50 than Comparative Example 1, so it is expected that the adhesion between particles is lower than that of Comparative Example 1, and that the air is less taken in during pressing. In addition to the small air intake, Comparative Example 2 has a high pressure loss for air penetration under a pressure of 12 kPa, so it is a material that is easily packed at a high density. Such a material has a high press molding bulk density and the binder is less likely to penetrate between the particles, so it is expected that it is difficult to obtain a desired shape when used in the binder jet method. Comparative Example 3 has a large D50 and is a material with low adhesion between particles. The low pressure loss for air penetration under a pressure of 12 kPa also suggests that Comparative Example 3 has low adhesion between particles. Such materials have a small angle of repose, which is an index of fluidity, and it is expected that it will be difficult to form a uniform powder layer when forming a thin layer of powder for additive manufacturing. Materials with a large D50 and low pressure loss for air permeation under a pressure of 12 kPa are presumed to be materials whose gaps in the powder are easily clogged by pressing. Such materials have a high press molding bulk density, and the binder does not easily penetrate between the particles, so it is expected that it will be difficult to obtain the desired shape when used in the binder jet method.
Claims
1. D50 is 5.5 to 9.0 μm, Inorganic oxide particles having a pressure loss of 1.75 to 2.81 kPa with respect to air permeation under a pressure of 12 kPa.
2. 2. The inorganic oxide particles according to claim 1, wherein (D10+D90) / D50 is 2.7 or more.
3. BET specific surface area: 0.10 to 10.00 m 2 The inorganic oxide particles according to claim 1, wherein the molecular weight of the inorganic oxide particles is 1 / g.
4. 4. The inorganic oxide particles according to claim 1, wherein the volume ratio of particles having a particle diameter of 16.8 to 60.0 μm is 4.3 to 33.5% by volume.
5. 4. The inorganic oxide particles according to claim 1, wherein the volume ratio of particles having a particle diameter of 2.0 μm or more is 90.0 volume % or more.
6. 4. The inorganic oxide particles according to claim 1, which are made of alumina.
7. 4. The inorganic oxide particles according to claim 1, having a circularity of 0.90 or more.
8. The inorganic oxide particles according to any one of claims 1 to 3, which are used in a powder layered manufacturing method.
9. Press molding bulk density under a pressure of 98 MPa is 2.45 to 2.54 g / cm 3 The inorganic oxide particles according to claim 6,
10. A sintered body of inorganic oxide particles according to any one of claims 1 to 3.
11. A method for producing a binder jet type layered object, comprising applying a liquid containing a binder to the inorganic oxide particles according to any one of claims 1 to 3 to form a three-dimensional layered object.
12. Applying a liquid containing a binder to the inorganic oxide particles according to any one of claims 1 to 3 to form a three-dimensional layered object; and The three-dimensional laminated body is subjected to a sintering process. A method for producing a sintered body, comprising:
Citation Information
Patent Citations
Material for laminate molding, method of manufacturing cast by powder fixing lamination method and casting mold
JP2016117069A
Powder for lamination molding, slurry for lamination molding, three-dimensional lamination molded body, sintered compact, method for producing slurry for lamination molding, lamination molding method and sintering method
JP2021011050A