Short-wavelength light shielding ink, short-wavelength light shielding film using the ink, laminated body, and packaging material
A short-wavelength light-shielding ink with zinc oxide, orange, and yellow pigments effectively blocks UV and visible light in the 200 to 500 nm range, enabling visible recognition in packaging materials without complex multilayer structures.
Patent Information
- Application Number
- JP2023067716
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-30
AI Technical Summary
Existing packaging materials fail to effectively block both ultraviolet rays and short-wavelength visible light while allowing contents to be visually recognized, particularly for items like syringes and drug solution bags, and require complex multilayer structures that are difficult to manufacture.
A short-wavelength light-shielding ink containing zinc oxide, orange pigment, and yellow pigment is applied to a transparent film, achieving high blocking properties against ultraviolet rays and short-wavelength visible light with a transmittance of 1.0% or less in the 200 to 500 nm range, allowing contents to be visibly recognized.
The ink provides a single-layer solution that effectively shields short-wavelength light and maintains visibility, addressing the need for simple and efficient light protection in packaging materials.
Smart Images

Figure 2024154093000001 
Figure 2024154093000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a short wavelength light-shielding film for use in soft packaging film materials for various foods, cosmetics, infusion preparations, ampoules, medicines, syringes, and other pharmaceutical products, and a laminated product using said film. More specifically, the present invention relates to a short wavelength light-shielding film for use in film packaging materials that allow the contents to be seen through and block short wavelength light, and a laminated product using said film. [Background technology]
[0002] Aluminum-deposited film is often used as packaging material for food, medicine, etc. to protect the contents from deterioration due to ultraviolet rays, but from the perspective of safety and security, there is an emerging demand for film packaging materials that allow the contents to be seen and block ultraviolet rays.
[0003] On the other hand, for syringes and drug solution bags filled with liquid medicines that are particularly susceptible to deterioration due to light, photodegradation cannot be sufficiently prevented even if they are secondary-packaged with a film that blocks ultraviolet light. Therefore, there has been a demand for a film that blocks not only ultraviolet light but also short-wavelength visible light, and that allows the contents to be viewed.
[0004] Patent Document 1 discloses an exterior bag for such an infusion bag. However, the invention disclosed in the document requires laminating multiple functional layers to form a multilayer structure, which is difficult to manufacture and does not meet the social demand for reducing the volume of plastic packaging materials. Therefore, there has been a demand for an ink that can block short wavelength light and allows the contents to be visually recognized by simply applying one type of ink. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2013-75453 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention provides a short wavelength light shielding ink that has high blocking properties against ultraviolet light and short wavelength visible light, i.e., short wavelength light, while allowing the contents to be visually recognized. [Means for solving the problem]
[0007] As a result of extensive research to solve the above-mentioned problems, the inventors have discovered that an ink containing zinc oxide, a yellow pigment, and an orange pigment can achieve both high short-wavelength light blocking properties and high visibility of contents.
[0008] That is, the present invention relates to a short wavelength light shielding ink comprising zinc oxide, an orange pigment and a yellow pigment.
[0009] The present invention also relates to a method for producing a transparent film using the ink. 2 The present invention relates to a short wavelength light shielding ink that has a transmittance of 1.0% or less at wavelengths of 200 to 500 nm when coated with a
[0010] The present invention also relates to a short wavelength light shielding ink, wherein the orange pigment is CI Pigment Orange 13.
[0011] In addition, the present invention is a method for producing a transparent film having a coating amount of 3.0 g / m 2 The present invention relates to a short wavelength light shielding film having the above-described coated ink layer, a laminate using the short wavelength light shielding film, a packaging material using the laminate, and a medicine secondarily packaged with the laminate. Effect of the Invention
[0012] The present invention provides a short wavelength light shielding film that, by applying only one type of ink, has high blocking properties against ultraviolet light and short wavelength light of 500 nm or less while allowing the contents to be visually recognized, and a laminate using said film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail. In the following description, all "ink compositions" refer to "short wavelength light shielding ink compositions." Furthermore, all "parts" refer to "parts by mass."
[0014] (Definition of words) In the present invention, "short wavelength light" refers to light with a wavelength of 200 to 500 nm. That is, the short wavelength light blocking ink refers to an ink that has the effect of blocking light with a wavelength of 200 to 500 nm. In the present invention, "shielding" refers to a transmittance of 5% or less over the entire wavelength range, for example, "short wavelength light shielding" refers to a transmittance of 5% or less over the entire wavelength range of 200 to 500 nm (i.e., the transmittance does not exceed 5% over the entire wavelength range of 200 to 500 nm). Furthermore, "transmittance of a certain wavelength range is equal to or greater than a certain level" refers to a transmittance of a certain level or less over the entire wavelength range, for example, "transmittance of 80% or more over the wavelength range of 500 to 800 nm" refers to a transmittance of 80% or more over the entire wavelength range of 500 to 800 nm.
[0015] (Short wavelength light blocking ink) The short wavelength light shielding ink of the present invention contains zinc oxide, an orange pigment and a yellow pigment.
[0016] (Zinc Oxide) The zinc oxide used in the present invention has an average particle size of 5 to 200 nm, preferably 10 to 150 nm, and more preferably 15 to 100 nm. In order to increase the transparency of the ink layer, a smaller particle size is preferable.
[0017] The zinc oxide used in the present invention is preferably 5 to 30 mass% based on the total mass of the ink composition, more preferably 5 to 20 mass%, and even more preferably 8 to 18 mass%. Furthermore, the zinc oxide is preferably 20 to 52 mass%, and more preferably 30 to 52 mass%, based on the total mass of the ink solid content. In the present invention, the ink solid content refers to the sum of the pigment solid content and the resin solid content. In order to enhance the effect of blocking ultraviolet light, it is preferable to increase the content of zinc oxide.
[0018] (Orange pigment) Examples of orange pigments used in the present invention include CI Pigment Orange 5, CI Pigment Orange 13, CI Pigment Orange 16, CI Pigment Orange 34, CI Pigment Orange 36, CI Pigment Orange 37, CI Pigment Orange 38, CI Pigment Orange 43, CI Pigment Orange 51, CI Pigment Range 55, CI Pigment Orange 59, CI Pigment Orange 61, CI Pigment Orange 64, CI Pigment Orange 71, and CI Pigment Orange 74. One type of pigment may be used, or two or more types may be used in combination. Among these, it is preferable to use CI Pigment Orange 13 as the orange pigment.
[0019] In addition, it is preferable to use an orange pigment having a transmittance of less than 5% at wavelengths of 450 nm and 500 nm, which is determined by the pigment selection method described below.
[0020] (Pigment selection method) Ink with a pigment concentration of 39% or more by mass relative to the total solids concentration of the ink was applied to a polyethylene terephthalate (PET) film (thickness 12 μm) at a coating weight of 3.6 g / m 2 After applying the above, the product was dried with a hair dryer for at least 5 seconds. The transmittance of this ink-coated film in the range of 300 to 600 nm was measured using an ultraviolet-visible-near infrared spectrophotometer (Shimadzu Corporation UV3600). In this case, examples of pigments having transmittances of less than 5% at wavelengths of 450 nm and 500 nm include CI Pigment Orange 13. By combining such an orange pigment with a yellow pigment and zinc oxide, it becomes possible to control the transmittance low over a wide range of 200 to 500 nm.
[0021] The content of the orange pigment used in the present invention is preferably 2 to 13 mass % based on the total mass of the ink composition, more preferably 4 to 12 mass %, and even more preferably 5 to 11 mass %. Also, the content of the orange pigment is preferably 10 to 35 mass %, and more preferably 13 to 35 mass %, based on the total mass of the ink solid content.
[0022] (Yellow pigment) Examples of the yellow pigments used in the present invention include CI Pigment Yellow 1, CI Pigment Yellow 3, CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Yellow 14, Pigment Yellow 17, CI Pigment Yellow 24, CI Pigment Yellow 42, CI Pigment Yellow 55, CI Pigment Yellow 62, CI Pigment Yellow 65, CI Pigment Yellow 74, CI Pigment Yellow 83, CI Pigment Yellow 86, CI Pigment Yellow 93, CI Pigment Yellow 94, CI Pigment Yellow 95, CI Pigment Yellow 109, CI Pigment Yellow 110, CI Pigment Yellow 117, CI Pigment Yellow 120, Pigment Yellow 131, Pigment Yellow 132, Pigment Yellow 133, Pigment Yellow 134, Pigment Yellow 135, Pigment Yellow 136, Pigment Yellow 137, Pigment Yellow 138, Pigment Yellow 139, Pigment Yellow 140, Pigment Yellow 141, Pigment Yellow 142, Pigment Yellow 143, Pigment Yellow 144, Pigment Yellow 145, Pigment Yellow 146, Pigment Yellow 147, Pigment Yellow 148, Pigment Yellow 149, Pigment Yellow 150, Pigment Yellow 151, Pigment Yellow 152, Pigment Yellow 153, Pigment Yellow 154, Pigment Yellow 155, Pigment Yellow 156, Pigment Yellow 157, Pigment Yellow 158, Pigment Yellow 159, Pigment Yellow 160, Pigment Yellow 161, Pigment Yellow 162, P Examples of the pigments include CI Pigment Yellow 125, CI Pigment Yellow 128, CI Pigment Yellow 129, CI Pigment Yellow 137, CI Pigment Yellow 138, CI Pigment Yellow 139, CI Pigment Yellow 147, CI Pigment Yellow 148, CI Pigment Yellow 150, CI Pigment Yellow 151, CI Pigment Yellow 153, CI Pigment Yellow 154, CI Pigment Yellow 155, CI Pigment Yellow 166, CI Pigment Yellow 168, CI Pigment Yellow 174, CI Pigment Yellow 180, CI Pigment Yellow 185, and CI Pigment Yellow 213. These pigments may be used alone or in combination of two or more. Among these, it is preferable to use CI Pigment Yellow 180 as the yellow pigment.
[0023] In addition, it is preferable to use a yellow pigment having a transmittance of less than 5% at wavelengths of 380 nm and 450 nm, respectively, determined by the pigment selection method described above. Examples of yellow pigments having transmittances of less than 5% at wavelengths of 380 nm and 450 nm, respectively, determined by the pigment selection method include CI Pigment Yellow 180 and CI Pigment Yellow 14. By combining such a yellow pigment with an orange pigment and zinc oxide, it becomes possible to control the transmittance to a low level over a wide range of 200 to 500 nm.
[0024] The yellow pigment used in the present invention is preferably 2 to 6 mass % and more preferably 2 to 4 mass % based on the total mass of the ink composition, and more preferably 5 to 15 mass % and more preferably 7 to 13 mass % and even more preferably 10 to 13 mass % based on the total mass of the ink solid content.
[0025] The ratio of each pigment to the total amount of pigments is preferably 40% by mass to 65% by mass for zinc oxide, 15% by mass to 45% by mass for orange pigment, and 10% by mass to 25% by mass for yellow pigment. When the pigment ratio is within this range, the effect of blocking light in a wide range of wavelengths from 200 to 500 nm is high, and the visibility of the contents can be maintained. In addition, the ratio of the orange pigment to the yellow pigment to the total amount of the orange pigment and the yellow pigment is preferably 45:55 to 80:20, more preferably 50:50 to 80:20, and even more preferably 55:45 to 75:25. By setting the ratio of the orange pigment to the yellow pigment in the above range, it is possible to achieve both blocking of the short wavelength region of visible light and visibility of the contents.
[0026] (binder resin) The short wavelength light shielding ink of the present invention preferably contains a binder resin. The binder resin is not particularly limited, but a binder resin that is usually used in liquid inks applied to printing methods using printing plates, such as gravure ink or flexographic ink, can be used. Examples of the resin include polyurethane resin, vinyl chloride-vinyl acetate copolymer resin (sometimes called vinyl chloride-vinyl acetate resin), chlorinated polypropylene resin, ethylene-vinyl acetate copolymer resin, vinyl acetate resin, polyamide resin, acrylic resin, polyester resin, alkyd resin, polyvinyl chloride resin, rosin resin, rosin-modified maleic acid resin, ketone resin, cyclized rubber, chlorinated rubber, polyvinyl butyral resin, and petroleum resin. These resins can be used alone or in a mixture of two or more. Of these, it is preferable to use a polyurethane resin as the main binder resin because it has excellent adhesion to film substrates, blocking resistance, lamination suitability, etc., and when a polyurethane resin is used as the main binder, the proportion of polyurethane resin to the total amount of resin in the ink is preferably 50 mass% or more, preferably 60 mass% or more, preferably 70 mass% or more, preferably 80 mass% or more, and preferably 90 mass% or more.
[0027] (Polyurethane resin) The polyurethane resin is not particularly limited as long as it is a polyurethane resin obtained by reacting a polyol with a polyisocyanate. The polyol is preferably a polyurethane resin made of a polyether polyol, and the content ratio of the polyether polyol is preferably in the range of 1 to 30 parts by mass of a polyether polyol having a number average molecular weight of 100 to 3500 relative to 100 parts by mass of the polyurethane resin. As will be described in detail later, examples of the polyether polyol resin include polyether polyols of polymers or copolymers of ethylene oxide, propylene oxide, tetrahydrofuran, etc. Specifically, known general-purpose resins such as polyethylene glycol resin, polypropylene glycol resin, and polytetramethylene glycol resin may be used. By containing the polyether resin in the above range, the adhesion to the film is significantly improved, and as a result, the blocking resistance and lamination strength are excellent.
[0028] If the number average molecular weight of the polyether polyol resin, which is a component of the polyurethane resin, is less than 100, the polyurethane resin film tends to become hard, and in particular the adhesion to polyester film becomes poor. If the number average molecular weight is more than 3500, the polyurethane resin film tends to become fragile, and the blocking resistance of the ink film becomes poor. If the ratio of polyether polyol to 100 parts by mass of polyurethane resin is less than 1 part by mass, the solubility of the polyurethane resin in ketone, ester, and alcohol-based solvents becomes poor. In addition, the resolubility of the ink film in the solvent becomes poor, and the tone reproducibility of the printed matter becomes poor. In addition, if it exceeds 30 parts by mass, the blocking resistance tends to be poor.
[0029] As the polyol used in combination with the polyurethane resin as required, various known polyols generally used in the production of polyurethane resins can be used, and one or more of them may be used in combination. For example, polyether polyols (1) of polymers or copolymers of methylene oxide, ethylene oxide, tetrahydrofuran, etc.; ethylene glycol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, pentanediol, 3-methyl-1,5-pentanediol, hexanediol, octanediol, 1,4-butynediol, 1,4 - Butylene diol, diethylene glycol, triethylene glycol, dipropylene glycol, glycerin, trimethylolpropane, trimethylolethane, 1,2,6-hexanetriol, 1,2,4-butanetriol, sorbitol, pentaerythritol, and other saturated or unsaturated low molecular weight polyols (2); these low molecular weight polyols (2) and adipic acid, phthalic acid, isophthalic acid, terephthalic acid, maleic acid, fumaric acid, succinic acid, oxalic acid, malonic acid, glutaric acid, pimelic acid, sulfuric acid, and the like. Polyester polyols (3) obtained by dehydration condensation or polymerization of polycarboxylic acids such as peric acid, azelaic acid, sebacic acid, trimellitic acid, pyromellitic acid, etc., or their anhydrides; polyester polyols (4) obtained by ring-opening polymerization of cyclic ester compounds, such as lactones such as polycaprolactone, polyvalerolactone, poly(β-methyl-γ-valerolactone); polycarbonate polyols (5) obtained by reacting the low molecular weight polyols (2) or the like with, for example, dimethyl carbonate, diphenyl carbonate, ethylene carbonate, phosgene, etc.; polybutadiene glycols (6); glycols (7) obtained by adding ethylene oxide or propylene oxide to bisphenol A; acrylic polyols (8) obtained by copolymerizing one or more hydroxyethyl groups, hydroxypropyl acrylate, hydroxybutyl acrylate, etc., or the corresponding methacrylic acid derivatives, etc., in one molecule with, for example, acrylic acid, methacrylic acid, or an ester thereof, and the like.
[0030] In addition, among the polyester polyols (3), the high molecular weight diol obtained from a diol (glycol) and a dibasic acid can be substituted with up to 5 mol % of the diol by the low molecular weight polyols (2) having three or more hydroxyl groups.
[0031] Examples of the diisocyanate compound used in the polyurethane resin include various known aromatic diisocyanates, aliphatic diisocyanates, alicyclic diisocyanates, etc. that are generally used in the production of polyurethane resins. For example, 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, tolylene diisocyanate, butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, cyclohexane-1,4-diisocyanate, cyclohexane-2,4-di ... ,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, dimeryl diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, methylcyclohexane diisocyanate, norbornane diisocyanate, m-tetramethylxylylene diisocyanate, 4,4-diphenylmethane diisocyanate, tolylene diisocyanate, bis-chloromethyl-diphenylmethane-diisocyanate, 2,6-diisocyanate-benzyl chloride, and dimer diisocyanate in which the carboxyl group of dimer acid is converted to an isocyanate group, etc. These diisocyanate compounds can be used alone or in combination of two or more kinds.
[0032] Examples of the chain extender used in the polyurethane resin include ethylenediamine, propylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, isophoronediamine, dicyclohexylmethane-4,4'-diamine, etc., as well as amines having a hydroxyl group in the molecule such as 2-hydroxyethylethylenediamine, 2-hydroxyethylpropyldiamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, di-2-hydroxypropylethylenediamine, di-2-hydroxypropylethylenediamine, etc. These chain extenders can be used alone or in combination of two or more.
[0033] In addition, a monovalent active hydrogen compound can be used as a terminal blocking agent for the purpose of stopping the reaction. Examples of such compounds include dialkylamines such as di-n-butylamine, and alcohols such as ethanol and isopropyl alcohol. Furthermore, when it is particularly desired to introduce a carboxyl group into the polyurethane resin, amino acids such as glycine and L-alanine can be used as a reaction stopping agent. These terminal blocking agents can be used alone or in combination of two or more.
[0034] The polyurethane resin is produced, for example, by reacting polypropylene glycol and a polyol to be used in combination with a diisocyanate compound in a ratio in which the isocyanate group is in excess to obtain a prepolymer having an isocyanate group at the end, and then reacting the prepolymer with a chain extender and / or a terminal blocking agent in a suitable solvent, i.e., an ester solvent such as ethyl acetate, propyl acetate, or butyl acetate, which is usually used as a solvent for non-toluene gravure ink; a ketone solvent such as acetone, methyl ethyl ketone, or methyl isobutyl ketone; an alcohol solvent such as methanol, ethanol, isopropyl alcohol, or n-butanol; a hydrocarbon solvent such as methylcyclohexane or ethylcyclohexane; or a mixture of these solvents, in a two-stage method, or by reacting polypropylene glycol and a polyol to be used in combination with the diisocyanate compound, a chain extender, and / or a terminal blocking agent at once in a suitable solvent among the above. Among these methods, the two-stage method is preferable in order to obtain a uniform polyurethane resin. In addition, when the polyurethane resin is produced by the two-stage method, it is preferable to react the chain extender and / or the terminal blocking agent so that the total amino group (equivalent ratio) of the chain extender and / or the terminal blocking agent is 1 / 0.9 to 1.3. If the equivalent ratio of the isocyanate group to the amino group is less than 1 / 1.3, the chain extender and / or the terminal blocking agent may remain unreacted, causing the polyurethane resin to yellow or emitting an odor after printing.
[0035] The weight average molecular weight of the polyurethane resin thus obtained is preferably within the range of 15,000 to 100,000, and from the viewpoint of obtaining adhesion of the laminate ink composition to the film substrate and scratch resistance, the glass transition point (Tg) is preferably −45 to −10° C., and more preferably within the range of 20,000 to 60,000. If the weight average molecular weight of the polyurethane resin is less than 15,000, the blocking resistance of the resulting ink composition and the strength and oil resistance of the printed film tend to be reduced, whereas if it exceeds 100,000, the viscosity of the resulting ink composition tends to be high, the smoothness of the printed film surface tends to be reduced, and the gloss tends to be low.
[0036] The content of the above polyurethane resin in the ink is preferably 3% by mass or more based on the total mass of the laminate ink finally prepared with solvents from the viewpoint of sufficient adhesion of the ink to the printed substrate, and 25% by mass or less from the viewpoint of appropriate ink viscosity and work efficiency during ink production and printing, and more preferably in the range of 3 to 15% by mass.
[0037] The polyurethane resin can be used without any particular limitation as long as it has the above-mentioned composition, but among these, those containing active hydrogen-containing functional groups, such as hydroxyl groups, primary or secondary amino groups, etc. in the polyurethane resin are preferred because crosslinking between the polyurethane resin and the blocked isocyanate proceeds smoothly and the resulting printed ink layer becomes strong. Even if the polyurethane resin does not contain active hydrogen-containing functional groups, the ink layer can be heated at a high temperature to obtain the same results as when a polyurethane resin containing active hydrogen is used.
[0038] As the binder resin, various resins such as vinyl chloride-vinyl acetate copolymer resin can be used in combination with the polyurethane resin, and it is preferable to use a polyurethane resin in combination with a vinyl chloride-vinyl acetate copolymer resin.
[0039] (Vinyl chloride-vinyl acetate copolymer resin) The vinyl chloride-vinyl acetate copolymer resin (sometimes referred to as vinyl chloride-vinyl acetate resin) is not particularly limited and any known resin can be used, but among them, a vinyl chloride-vinyl acetate copolymer resin having a hydroxyl group is preferred, and a vinyl chloride-vinyl acetate copolymer resin having a hydroxyl group with a hydroxyl value of 50 to 200 mgKOH / g and a content ratio of vinyl chloride components in the copolymer resin of 80 to 95 mass % is even more preferred.
[0040] Vinyl chloride-vinyl acetate copolymer resins having hydroxyl groups can be obtained by two methods. One is obtained by copolymerizing vinyl chloride monomer, vinyl acetate monomer, and vinyl alcohol in an appropriate ratio. The other is obtained by copolymerizing vinyl chloride and vinyl acetate, and then partially saponifying the vinyl acetate. The properties of the resin coating and the resin dissolution behavior of the vinyl chloride-vinyl acetate copolymer resins having hydroxyl groups are determined by the monomer ratio of vinyl chloride, vinyl acetate, and vinyl alcohol. That is, vinyl chloride gives the resin coating strength and hardness, vinyl acetate gives adhesion and flexibility, and vinyl alcohol gives good solubility in polar solvents.
[0041] In addition, as the monomer ratio of the vinyl chloride-vinyl acetate copolymer resin having a hydroxyl group, for example, 80 to 95 parts by mass of vinyl chloride per 100 parts by mass of the vinyl chloride-vinyl acetate copolymer resin having a hydroxyl group is more preferable since it balances blocking resistance and adhesiveness. If it is 80 parts by mass or more, the toughness of the resin coating can be maintained and blocking resistance can be ensured. If it is 95 parts by mass or less, the resin coating does not become too hard and adhesiveness is unlikely to decrease. In addition, the hydroxyl value obtained from vinyl alcohol is preferably 50 to 200 mgKOH / g. If it is 50 mgKOH / g or more, the solubility in polar solvents is good and the printability is easily stabilized. If it is 200 mgKOH / g or less, the lamination suitability can be maintained well.
[0042] When a hydroxyl group-containing vinyl chloride-vinyl acetate copolymer resin is used in combination with a polyurethane resin, the amount is preferably in the range of 1 to 30 mass % relative to the total resin solids content of the liquid printing ink, and more preferably in the range of 1 to 20 mass %.
[0043] In addition, in consideration of the construction of a recycling-based society (sustainability) that should be developed in a sustainable manner, it is preferable to use a binder resin using a plant-derived raw material. Examples of plant-derived raw materials include cellulose resins such as cellulose acetate propionate resin and nitrocellulose, polyamide resins using dimer acid or polymerized fatty acid derived from natural oils such as soybean oil, palm oil, and rice bran oil, polycarboxylic acids such as succinic acid, succinic anhydride, adipic acid, azelaic acid, sebacic acid, dimer acid, glutaric acid, malic acid, polyols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, pentylene glycol, 1,10-dodecanediol, dimer diol, isosorbide, polyisocyanates such as 1,5-pentamethylene diisocyanate, dimer diisocyanate, and biomass polyurethanes synthesized from plant-derived raw materials, and rosin resins.
[0044] The short wavelength light shielding ink may contain various additives such as a pigment dispersant, a leveling agent, a defoaming agent, a wax, a plasticizer, a fragrance, and a flame retardant.
[0045] (Organic solvent) The short wavelength light shielding ink preferably contains an organic solvent. Although various organic solvents can be used as the organic solvent, it is preferable to use an organic solvent other than aromatic organic solvents. For example, ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ester-based solvents such as methyl acetate, ethyl acetate, isopropyl acetate, n-propyl acetate, butyl acetate, amyl acetate, ethyl formate, butyl propionate, and propylene glycol monomethyl ether acetate; alcohol-based solvents such as methanol, ethanol, isopropyl alcohol, n-propanol, isopropanol, n-butanol, and propylene glycol monomethyl ether; ethylene glycol (mono, di)methyl ether, ethylene glycol (mono, di)ethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monomethyl ether; Examples of the glycol ethers include glycol ethers such as ethylene glycol monoisopropyl ether, monobutyl ether, diethylene glycol (mono, di) methyl ether, diethylene glycol (mono, di) ethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monobutyl ether, triethylene glycol (mono, di) methyl ether, propylene glycol (mono, di) methyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, and dipropylene glycol (mono, di) methyl ether, and these can be used alone or in a mixture of two or more. In recent years, from the viewpoint of the working environment, it is desirable not to use aromatic solvents or ketone solvents such as toluene, xylene, Solvesso #100, and Solvesso #150. Among them, from the viewpoint of solubility in polyurethane resin, a mixed solution containing ethyl acetate, isopropyl alcohol, and normal propyl acetate is more preferable.
[0046] The short wavelength light shielding ink can be produced by dissolving and / or dispersing zinc oxide, orange pigment, yellow pigment, and other constituent materials in an organic solvent. Specifically, for example, a dispersion is produced by dispersing zinc oxide, orange pigment, and yellow pigment in an organic solvent using a polyurethane resin and a vinyl chloride-vinyl acetate copolymer resin (vinyl chloride-vinyl acetate resin) having a hydroxyl group, and the ink can be produced by blending other compounds, etc., with the obtained dispersion as necessary. As a dispersing machine, a commonly used machine, such as a roller mill, ball mill, pebble mill, attritor, sand mill, etc., can be used.
[0047] (film) The film substrate is not particularly limited as long as it is transparent, and examples thereof include films and laminates made of thermoplastic resins such as polyethylene terephthalate (hereinafter sometimes referred to as PET), polyethylene naphthalate, polytrimethylene terephthalate, polytrimethylene naphthalate, polybutylene terephthalate, and polybutylene naphthalate, polyamides such as nylon 6, nylon 66, and nylon 46, polyhydroxycarboxylic acids such as polylactic acid, aliphatic polyester resins such as poly(ethylene succinate) and poly(butylene succinate), polyolefins such as polypropylene (CPP: non-oriented polypropylene film, OPP: biaxially oriented polypropylene film), polyethylene (LLDPE: low-density polyethylene film, HDPE: high-density polyethylene film), polyimide, polyarylate, polystyrene, polyacrylonitrile, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, and mixtures thereof. Among these, films made of polyethylene terephthalate, polyethylene, and polypropylene can be preferably used.
[0048] It is also preferable to use a film formed from a material containing a biomass-derived component as the film substrate. Biomass films are sold by various companies, and for example, sheets such as those listed in the list of biomass certified products listed in the Japan Organics Resources Association can be used.
[0049] Specifically, a well-known film is made from biomass-derived ethylene glycol. Biomass-derived ethylene glycol is made from ethanol (biomass ethanol) produced from biomass. For example, biomass-derived ethylene glycol can be obtained by a method of producing ethylene glycol from biomass ethanol via ethylene oxide using a conventionally known method. Commercially available biomass ethylene glycol may also be used, and for example, biomass ethylene glycol commercially available from India Glycoal Limited can be suitably used.
[0050] Alternatively, products using biomass raw materials classified by the degree of biomass plastic as specified by ISO16620 or ASTM D6866 are also on the market. Radioactive carbon-14C exists in the atmosphere at a ratio of 1 in 1012 particles, and this ratio does not change even in atmospheric carbon dioxide, so this ratio does not change even in plants that fix this carbon dioxide through photosynthesis. For this reason, the carbon in plant-derived resins contains radioactive carbon-14C. In contrast, the carbon in fossil fuel-derived resins contains almost no radioactive carbon-14C. Therefore, by measuring the concentration of radioactive carbon-14C in the resin with an accelerator mass spectrometer, the proportion of plant-derived resin in the resin, i.e., the degree of biomass plastic, can be determined. Examples of plant-derived low-density polyethylene, which is a biomass plastic having a biomass plastic content of 80% or more, preferably 90% or more as specified by ISO16620 or ASTM D6866, include products manufactured by Braskem under the trade names "SBC818", "SPB608", "SBF0323HC", "STN7006", "SEB853", and "SPB681", and films using these as raw materials can be suitably used.
[0051] For example, as an alternative to conventional polyethylene terephthalate films using petroleum-based raw materials, biomass polyesters containing ethylene glycol derived from biomass as diol units and dicarboxylic acids derived from fossil fuels as dicarboxylic acid units, biomass polyethylene terephthalate, etc., are known. The dicarboxylic acid units of the biomass polyesters use dicarboxylic acids derived from fossil fuels. As the dicarboxylic acid, aromatic dicarboxylic acids, aliphatic dicarboxylic acids, and derivatives thereof can be used without any restrictions.
[0052] In addition to the above diol component and dicarboxylic acid component, the copolymer polyester may be a copolymer polyester containing a copolymer component as a third component, such as a bifunctional oxycarboxylic acid or at least one polyfunctional compound selected from the group consisting of a trifunctional or higher functional polyhydric alcohol, a trifunctional or higher functional polycarboxylic acid and / or its anhydride, and a trifunctional or higher functional oxycarboxylic acid, in order to form a crosslinked structure.
[0053] In addition, for example, as an alternative to conventional polyolefin films using petroleum-based raw materials, biomass polyolefin films such as biomass polyethylene films and biomass polyethylene-polypropylene films, which contain polyethylene resins made from biomass-derived ethylene glycol, are also known.
[0054] The polyethylene resin is not particularly limited except that ethylene glycol derived from biomass is used as part of the raw material, and examples thereof include ethylene homopolymers, copolymers of ethylene and α-olefins containing ethylene as the main component (ethylene-α-olefin copolymers containing 90% by mass or more of ethylene units), and the like, which may be used alone or in combination of two or more.
[0055] The biomass film may be a laminate of a plurality of biomass films, or may be a laminate of a conventional petroleum-based film and a biomass film.
[0056] It is also preferable to use a film containing recycled resin as the film substrate. The recycled resin may be a film that has been once used for packaging and then collected and recycled, or a film obtained as a packaging waste material may be recycled. When recycling a film that has been printed or laminated, it is preferable to use a recycled resin that has been deinked or delaminated to reduce impurities.
[0057] These films may be unstretched or stretched, and the manufacturing method is not limited. As a stretching method, a resin is melt-extruded into a sheet by an extrusion film forming method or the like, and then simultaneous biaxial stretching or sequential biaxial stretching is generally performed. In the case of sequential biaxial stretching, a longitudinal stretching process is generally performed first, and then a transverse stretching process is generally performed. Specifically, a method of combining longitudinal stretching utilizing the speed difference between rolls and transverse stretching using a tenter is often used.
[0058] The thickness of the base film is not particularly limited, but may usually be in the range of 1 to 500 μm. The film surface may be subjected to various surface treatments such as flame treatment and corona discharge treatment as necessary so that an adhesive layer without defects such as film breaks and repellency is formed.
[0059] (Short wavelength light shielding film) The short wavelength light shielding film of the present invention is a film having a short wavelength light shielding layer formed thereon by applying a short wavelength light shielding ink to the above-mentioned film. 2 The above is a coating layer of short wavelength light blocking ink. The coating amount is 3.6g / m 2 By setting the coating amount at 3.7 g / m or more, a sufficient short wavelength light shielding effect can be obtained. 2 It is preferable that the content is 3.8 g / m or more. 2 More preferably, it is equal to or greater than this. On the other hand, there is no particular upper limit to the coating amount, but from the viewpoint of adhesion of the shielding layer, it is set to 10.0 g / m 2 Preferably, it is 8 g / m or less.2 It is preferable that:
[0060] In addition, it is preferable that the short wavelength light shielding film of the present invention contains one short wavelength light shielding layer, which makes it possible to achieve both short wavelength light shielding effect and visibility of contents, but this does not prevent the short wavelength light shielding film from containing two or more short wavelength light shielding layers.
[0061] In the short wavelength light shielding film of the present invention, the component consisting of the transparent film and the short wavelength light shielding layer preferably has a transmittance of 5% or less at wavelengths of 200 to 500 nm and 80% or more at wavelengths of 500 to 800 nm.
[0062] Specifically, the transmittance of the component consisting of the film and the short wavelength light-shielding layer in the short wavelength light-shielding film using a polyolefin film is preferably 5% or less at a wavelength of 200 to 500 nm and 80% or more at a wavelength of 500 to 800 nm, more preferably 1.5% or less at a wavelength of 200 to 500 nm, and even more preferably 1.0% or less at a wavelength of 200 to 500 nm.
[0063] In a laminate-type laminate having at least a laminated component in which a CPP film is laminated via an adhesive to the short-wavelength light-shielding film using the above-mentioned polyolefin film, the transmittance of the laminated component in the laminate is preferably 5% or less at a wavelength of 200 to 50 nm, while it is preferably 83% or more at a wavelength of 500 to 800 nm, more preferably 84% or more, and particularly preferably 85% or more.
[0064] Furthermore, when a polyethylene terephthalate (PET) film is used as the film, it is preferable that the transmittance of the component consisting of the film and the short wavelength light-shielding layer in the short wavelength light-shielding film using the film is 5% or less at a wavelength of 200 to 500 nm and 80% or more at a wavelength of 500 to 800 nm.
[0065] In the laminate-type laminate having at least a laminated structure in which a CPP film is laminated via an adhesive on the short-wavelength light shielding film using the above-mentioned PET film, the transmittance of the laminated structure in the laminated structure is preferably 5% or less, more preferably 1.5% or less, and even more preferably 1.2% or less at a wavelength of 200 to 500 nm. Meanwhile, the transmittance of the laminated structure in the laminated structure in this case in a wavelength of 500 to 800 nm is preferably 81% or more, more preferably 82% or more, and even more preferably 83% or more.
[0066] The short wavelength light shielding film of the present invention can be produced by applying a short wavelength light shielding ink onto a film. Specifically, it can be obtained by printing the short wavelength light shielding ink onto at least one side of the film. The printing method can be a known printing method such as gravure printing or flexographic printing, but it is particularly preferable to print by gravure printing. It may also be formed by a known coating method such as a spray method, a spin coating method, a dip method, a roll coating method, a blade coating method, a doctor roll method, a doctor blade method, a curtain coating method, a slit coating method, a screen printing method, an ink jet method, a dispense method, a die coating method, a direct gravure method, a reverse gravure method, a flexographic method, a knife coating method, or a dot coating method. After applying the short wavelength light shielding ink onto the film by these methods, the ink is dried or cured in an oven as necessary to fix the ink, thereby obtaining a short wavelength light shielding film.
[0067] The short wavelength light shielding film of the present invention may have, in addition to the short wavelength light shielding layer on the film, other coating layers and / or deposition layers such as a colored ink layer, a resin layer having barrier properties, a heat-resistant coating layer, a layer made of a heat sealant or cold sealant, a metal deposition layer, etc.
[0068] For example, by providing a colored ink layer, it is possible to display the product name and improve the design, and the short wavelength light blocking effect can be improved due to the short wavelength light absorbing effect of the colorant.
[0069] In addition, various functions can be enhanced by applying other functional coating agents. A specific example of the structure is a layer of a heat seal agent or cold seal agent / a resin layer having a barrier property / a film / a colored printed layer / a short wavelength light shielding layer / a heat resistant coating layer, but the stacking order and the type of coating layer are not limited to these.
[0070] (Colored printing layer) The colored printing layer is formed by a colored printing ink. Printing inks are used as gravure printing inks or flexographic printing inks, and are roughly divided into organic solvent-based liquid printing inks that use organic solvents as the main solvent, and water-based liquid printing inks that use water as the main solvent, but either may be used in the present invention. In addition, there are so-called front-side printing inks and back-side printing inks that are intended for lamination, but either may be used in the present invention.
[0071] The mainstream organic solvent-based liquid printing ink contains a binder resin, a colorant, an organic solvent, and other additives as required.
[0072] The binder resin and organic solvent may be the same as those used in the above-mentioned short wavelength light shielding ink.
[0073] Examples of the colorant include inorganic pigments, organic pigments, and dyes used in general inks, paints, and recording agents, etc., and pigments are preferred. Examples of organic pigments include soluble azo-based, insoluble azo-based, azo-based, phthalocyanine-based, halogenated phthalocyanine-based, anthraquinone-based, anthanthrone-based, dianthraquinonyl-based, anthrapyrimidine-based, perylene-based, perinone-based, quinacridone-based, thioindigo-based, dioxazine-based, isoindolinone-based, quinophthalone-based, azomethine azo-based, flavanthrone-based, diketopyrrolopyrrole-based, isoindoline-based, indanthrone-based, carbon black-based, and other pigments. Other examples include carmine 6B, lake red C, permanent red 2B, disazo yellow, pyrazolone orange, carmine FB, chromophthalic yellow, chromophthalic red, phthalocyanine blue, phthalocyanine green, dioxazine violet, quinacridone magenta, quinacridone red, indanthrone blue, pyrimidine yellow, thioindigo bordeaux, thioindigo magenta, perylene red, perinone orange, isoindolinone yellow, aniline black, diketopyrrolopyrrole red, daylight fluorescent pigments, etc. In addition, both non-acid-treated pigments and acid-treated pigments can be used.
[0074] Examples of inorganic pigments include white inorganic pigments such as titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, chromium oxide, silica, litbones, antimony white, and gypsum. Among inorganic pigments, titanium oxide is particularly preferred. Titanium oxide is white and is preferred in terms of coloring power, hiding power, chemical resistance, and weather resistance, and from the viewpoint of printing performance, the titanium oxide is preferably treated with silica and / or alumina. Examples of inorganic pigments other than white include aluminum particles, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine, Prussian blue, red iron oxide, yellow iron oxide, and zircon. Aluminum is in powder or paste form, but it is preferable to use it in paste form from the standpoint of handleability and safety. Whether leafing or non-leafing aluminum is used is appropriately selected from the standpoint of brightness and concentration.
[0075] The pigments are preferably contained in an amount sufficient to ensure the concentration and coloring strength of the liquid printing ink, i.e., 1 to 60% by mass relative to the total mass of the liquid printing ink, and 10 to 90% by mass in terms of the solid content ratio in the liquid printing ink. These pigments may be used alone or in combination of two or more kinds.
[0076] Organic solvent-based liquid printing inks may further contain waxes, chelating crosslinking agents, extender pigments, leveling agents, defoamers, plasticizers, infrared absorbing agents, ultraviolet absorbing agents, fragrances, flame retardants, etc., as required.
[0077] In the liquid printing ink used for the colored printing layer, it is preferable to use a liquid printing ink made from plant-derived raw materials, taking into consideration the creation of a recycling-based society that should develop sustainably (sustainability). Commercially available products can also be used as biomass liquid printing ink. Examples of commercially available products that can be used include inks listed in the Japan Organics Resources Association.
[0078] (Resin layer having barrier properties) To form a resin layer having barrier properties, a method of laminating a film having barrier properties and a method of forming a coating layer by applying a barrier coating agent can be mentioned. The method of forming a coating layer by applying a barrier coating agent is preferable because it is simple. Examples of the barrier coating agent include coating agents containing polymers such as polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), polysaccharides, acrylic acid or methacrylic acid-based polymers, starch or starch derivatives, cellulose nanofibers (CNF), nanocrystalline cellulose (NCC), chitosan, or other cellulose derivatives, hemicellulose, polyvinylidene chloride (PVDC), or coating agents containing these polymers and inorganic fine particles such as silica, alumina, aluminum flakes, glass flakes, hydrous silicates (phyllosilicate minerals, etc.), kaolinite-serpentine clay minerals (halloysite, kaolinite, endelite, dickite, etc.), etc. Known coating agents include inorganic compounds such as platy inorganic compounds, such as pyrophyllite-talc group (pyrophyllite, talc, kerolithium, etc.), smectite group clay minerals (montmorillonite, beidellite, nontronite, saponite, hectorite, sauconite, stevensite, etc.), vermiculite group clay minerals (vermiculite, etc.), mica or mica group clay minerals (muscovite, phlogopite, etc. mica, margarite, tetrasilylic mica, taeniolite, etc.), chlorite group (cookite, sudoite, clinochlore, chamosite, nimite, etc.), hydrotalcite, plate-like barium sulfate, boehmite, and aluminum polyphosphate.
[0079] In the present invention, known barrier coating agents can be used without any particular limitation. Known barrier coating agents include the "Sunbar" series manufactured by Sun Chemical Co., Ltd. and polyester-based barrier coating agents described in Patent No. 5617831.
[0080] (heat-resistant coating layer) The heat-resistant coating layer is a coating layer of a coating agent having heat resistance. As a coating agent having heat resistance, a material having a cellulose skeleton, a benzene ring, an isocyanuric skeleton, or an alicyclic skeleton is effective. Specifically, cellulose derivatives such as nitrocellulose, cellulose acetate, cellulose propionate, and cellulose butyrate, benzene rings such as phthalic acid, naphthalene dicarboxylic acid, and EO adducts of bisphenol A, and / or polyester resins having an alicyclic skeleton such as cyclopentanediol and dimethylol tricyclodecane, or aromatic isocyanates such as diphenylmethane diisocyanate, toluene diisocyanate, xylene diisocyanate, and naphthalene diisocyanate, alicyclic isocyanates such as isophorone diisocyanate and norbornene diisocyanate, and / or polyurethane resins in which isocyanuric triisocyanate is bonded to a polyol and / or tris(2-hydroxyethyl)isocyanurate can be mentioned. Also, polyisocyanates using the above-mentioned isocyanates may be used as the curing agent.Other examples include compounds having a benzene ring and an unsaturated double bond, such as styrene and phenoxydiethylene glycol acrylate, and / or compounds having an alicyclic structure and an unsaturated double bond, such as isobornyl acrylate and dicyclopentanyl acrylate, and radical copolymers such as (meth)acrylate. The heat-resistant coating agent may be colored. The colorant is not particularly limited, and for example, the liquid printing ink used in the present invention contains a colorant and can be used as a liquid printing ink containing a colorant for design printing or the like for the purpose of imparting cosmetic properties. Examples of the colorant include inorganic pigments, organic pigments, and dyes used in general inks, paints, and recording agents, and pigments are preferred. Examples of organic pigments include soluble azo-based, insoluble azo-based, azo-based, phthalocyanine-based, halogenated phthalocyanine-based, anthraquinone-based, anthanthrone-based, dianthraquinonyl-based, anthrapyrimidine-based, perylene-based, perinone-based, quinacridone-based, thioindigo-based, dioxazine-based, isoindolinone-based, quinophthalone-based, azomethine azo-based, flavanthrone-based, diketopyrrolopyrrole-based, isoindoline-based, indanthrone-based, and carbon black-based pigments. Other examples include carmine 6B, lake red C, permanent red 2B, disazo yellow, pyrazolone orange, carmine FB, chromophthalic yellow, chromophthalic red, phthalocyanine blue, phthalocyanine green, dioxazine violet, quinacridone magenta, quinacridone red, indanthrone blue, pyrimidine yellow, thioindigo bordeaux, thioindigo magenta, perylene red, perinone orange, isoindolinone yellow, aniline black, diketopyrrolopyrrole red, daylight fluorescent pigments, etc. In addition, both non-acid-treated pigments and acid-treated pigments can be used.
[0081] Examples of inorganic pigments include white inorganic pigments such as titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, chromium oxide, silica, litbones, antimony white, and gypsum. Among inorganic pigments, titanium oxide is particularly preferred. Titanium oxide is white and is preferred in terms of coloring power, hiding power, chemical resistance, and weather resistance, and from the viewpoint of printing performance, the titanium oxide is preferably treated with silica and / or alumina. Examples of inorganic pigments other than white include aluminum particles, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine, Prussian blue, red iron oxide, yellow iron oxide, and zircon. Aluminum is in powder or paste form, but it is preferable to use it in paste form from the standpoint of handleability and safety. Whether leafing or non-leafing aluminum is used is appropriately selected from the standpoint of brightness and concentration.
[0082] (Layer with heat seal or cold seal) The layer of heat or cold sealant is provided by coating a sealant with a solution of thermoplastic elastomer polyester, vinyl chloride-vinyl acetate resin, EVOH, acrylic resin, polyolefin resin, or rubber resin. The coating can be applied to the entire surface or a portion of the surface, and the thickness of the solid portion is 1 to 5 μm.
[0083] (deposited layer) The vapor-deposited layer is provided by subjecting the film to vapor deposition of a metal such as aluminum.
[0084] (Laminated body using short-wavelength light shielding film) The laminate of the present invention is obtained by laminating a plurality of substrates, and has the short wavelength light shielding film of the present invention on at least one of the substrates. The substrates can be laminated by bonding with an adhesive or by extrusion lamination.
[0085] More specifically, the laminate has the following structure: (1) Base film 1 / short wavelength light shielding layer / adhesive layer 1 / sealant film (2) Base film 1 / short wavelength light shielding layer / adhesive layer 1 / metal-deposited unstretched film (3) Base film 1 / short wavelength light shielding layer / adhesive layer 1 / metal vapor deposition stretched film (4) Transparent vapor-deposited stretched film / printed layer / adhesive layer 1 / sealant film (5) Base film 1 / short wavelength light shielding layer / adhesive layer 1 / base film 2 / adhesive layer 2 / sealant film (6) Base film 1 / short wavelength light shielding layer / adhesive layer 1 / metal vapor deposition stretched film / adhesive layer 2 / sealant film (7) Base film 1 / short wavelength light shielding layer / adhesive layer 1 / transparent vapor deposition stretched film / adhesive layer 2 / sealant film (8) Base film 1 / short wavelength light shielding layer / adhesive layer 1 / metal layer / adhesive layer 2 / sealant film (9) Base film 1 / short wavelength light shielding layer / adhesive layer 1 / base film 2 / adhesive layer 2 / metal layer / adhesive layer 3 / sealant film (10) Base film 1 / short wavelength light shielding layer / adhesive layer 1 / metal layer / adhesive layer 2 / base film 2 / adhesive layer 3 / sealant film Examples include, but are not limited to, the above. The above "base film 1 / short wavelength light-shielding layer" corresponds to the above "short wavelength light-shielding film". In the above configurations (1) to (10), a configuration in which a short wavelength light-shielding layer is provided on the surface of the base film 1 on the adhesive layer 1 side has been described, but a short wavelength light-shielding layer may be provided on the surface (front surface) of the base film 1 opposite to the adhesive layer 1, or a short wavelength light-shielding layer may be provided on the base film 2, and the "base film 1 / short wavelength light-shielding layer" may be the "short wavelength light-shielding film".
[0086] Furthermore, the laminate may further have other coating layers and / or deposition layers, such as a colored ink layer, a resin layer having barrier properties, a heat-resistant coating layer, a layer made of a heat-sealing agent or a cold-sealing agent, or a metal deposition layer.
[0087] Examples of the base film 1 used in the structure (1) include an OPP film, a PET film, and a nylon film (hereinafter also referred to as an Ny film). The base film 1 may be coated with a coating for the purpose of improving the gas barrier properties and the ink receptivity when a printing layer is provided, which will be described later. Examples of commercially available base films 1 with coatings include K-OPP films and K-PET films. Examples of sealant films include CPP films and LLDPE films.
[0088] The base film 1 used in the structures (2) and (3) can be an OPP film, a PET film, etc. As the metal-vapor-deposited unstretched film, a VM-CPP film obtained by depositing a metal such as aluminum on a CPP film can be used, and as the metal-vapor-deposited stretched film, a VM-OPP film obtained by depositing a metal such as aluminum on an OPP film can be used.
[0089] Examples of the transparent evaporated stretched film used in the structure (4) include films obtained by evaporating silica or alumina onto OPP film, PET film, nylon film, etc. For the purpose of protecting the inorganic evaporated layer of silica or alumina, a film having a coating applied onto the evaporated layer may be used. Examples of the sealant film include the same as those in the structure (1).
[0090] The base film 1 used in the structure (5) may be a PET film, etc. The base film 2 may be a nylon film, etc. The sealant film may be the same as that in the structure (1).
[0091] The base film 1 of the structure (6) may be the same as that of the structures (2) and (3). The metal-vapor-deposited stretched film may be a VM-OPP film or a VM-PET film in which a metal such as aluminum is vapor-deposited on an OPP film or a PET film. The sealant film may be the same as that of the structure (1).
[0092] The base film 1 in the structure (7) may be a PET film, etc. The transparent deposition stretched film may be the same as that in the structure (4). The sealant film may be the same as that in the structure (1).
[0093] The base film 1 in the structure (8) may be a PET film, etc. The metal layer may be an aluminum foil, etc. The sealant film may be the same as that in the structure (1).
[0094] In the structures (9) and (10), the base film 1 may be a PET film or the like. The base film 2 may be a nylon film or the like. The metal layer may be an aluminum foil or the like. The sealant film may be the same as that in the structure (1). (Adhesive layer) The adhesive layer may be formed by a known adhesive for film lamination. When laminating by extrusion lamination, a known anchor coating agent for extrusion lamination may be used as an adhesive auxiliary. When a material having gas barrier properties is used as the adhesive or anchor coating agent, a laminate having particularly excellent barrier properties can be obtained.
[0095] As an adhesive with excellent gas barrier properties, 3 g / m 2 The oxygen barrier property of the cured coating of the adhesive applied at (solid content) is 300cc / m 2 / day / atm or less, or water vapor barrier property of 120g / m 2 / day. Commercially available products include the "PASLIM" series, such as PASLIM VM001 and PASLIM J350X, manufactured by DIC Corporation, and "Maxive" manufactured by Mitsubishi Gas Chemical Company.
[0096] The adhesive layer may be made of any known material without particular limitation, but preferably contains a cured product of a polyol and an isocyanate compound. When the polyol and / or isocyanate compound contains a biomass-derived component, a laminate with a high biomass content can be obtained, thereby reducing the environmental load.
[0097] In addition, the adhesive may contain an adhesion promoter, an acid anhydride, a compound having an oxygen scavenging function, a tackifier, a gas barrier adhesive stabilizer (antioxidant, heat stabilizer, ultraviolet absorber, etc.), a plasticizer, an antistatic agent, a lubricant, an antiblocking agent, a colorant, a crystal nucleating agent, etc. These various additives may be added in advance to either one or both of the polyol composition (A) and the polyisocyanate composition (B), or may be added when the polyol composition (A) and the polyisocyanate composition (B) are mixed.
[0098] The gas barrier adhesive used may be either a solvent-based or solventless type. When the gas barrier adhesive used is a solvent-based adhesive, the adhesive of the present invention is applied onto the surface of the printed layer printed on the first substrate using a roll such as a gravure roll, and the organic solvent is evaporated by heating in an oven or the like, and then the other substrate is laminated to obtain the laminate of the present invention. After lamination, it is preferable to perform an aging treatment. The aging temperature is preferably room temperature to 80°C, and the aging time is preferably 12 to 240 hours.
[0099] When the gas barrier adhesive used is a solventless type, the adhesive of the present invention, which has been preheated to about 40°C to 100°C, is applied to the printed layer surface of the first substrate using a roll such as a gravure roll, and the other substrate is immediately laminated to obtain the laminate of the present invention. After lamination, it is preferable to carry out an aging treatment. The aging temperature is preferably room temperature to 70°C, and the aging time is preferably 6 to 240 hours.
[0100] When the gas barrier adhesive is used as an adhesion promoter, the adhesion promoter of the present invention is applied to the printed layer surface printed on the first substrate using a roll such as a gravure roll, and the organic solvent is evaporated by heating in an oven or the like, and then the polymer material melted by an extruder is laminated to obtain the laminate of the present invention. As the polymer material to be melted, polyolefin resins such as low-density polyethylene resin, linear low-density polyethylene resin, and ethylene-vinyl acetate copolymer resin are preferred. The aging temperature is preferably room temperature to 70°C, and the aging time is preferably 6 to 240 hours.
[0101] The amount of gas barrier adhesive to be applied is adjusted as appropriate. For example, in the case of a solvent-based adhesive, the solid content is 1 g / m 2 More than 10g / m 2 Less than 2 g / m 2 More than 5g / m 2 Adjust the amount of adhesive applied so that it is as follows: For a solvent-free adhesive, the amount of adhesive applied is, for example, 1 g / m 2 More than 5g / m 2 Less than 1 g / m 2 More than 3g / m 2 The following is the result.
[0102] When using an adhesive as an adhesive auxiliary, the amount of application is adjusted appropriately. For example, 2 More than 2g / m 2 The solid content is as follows:
[0103] In the laminate configurations including the above configurations, it is preferable that each film constituting the laminate is made of a single main raw material as much as possible in order to improve the quality of the recycled plastic when the laminate is recycled. For example, it is preferable to use a laminate film (sometimes called a mono-material film) made of only polyolefin films such as polyethylene films and polypropylene films and laminated in multiple layers as a packaging material.
[0104] For example, when a laminate is made of only polyolefin films, it is preferable to provide a heat-resistant coating layer to improve heat resistance during heat sealing, etc. Also, it is preferable to use an adhesive or coating agent with barrier properties to improve barrier properties. An example of a specific embodiment of such a configuration is shown below. Note that " / " indicates that layers are in contact with each other. Heat-resistant coating layer (A) / Short-wavelength light shielding layer / Olefin resin layer (B1) Heat-resistant coating layer (A) / Short-wavelength light shielding layer / Olefin resin layer (B1) / Adhesive layer (C) / Olefin resin layer (B2) Heat-resistant coating layer (A) / Short-wavelength light shielding layer / Olefin resin layer (B1) / Adhesive layer (C) / Resin layer with barrier properties (D) / Olefin resin layer (B2) Heat-resistant coating layer (A) / Short wavelength light shielding layer / Olefin resin layer (B1) / Heat-resistant coating layer (A) Heat-resistant coating layer (A) / Short-wavelength light shielding layer / Olefin resin layer (B1) / Heat-resistant coating layer (A) / Adhesive layer (C) / Olefin resin layer (B2) Heat-resistant coating layer (A) / Short-wavelength light shielding layer / Olefin resin layer (B1) / Heat-resistant coating layer (A) / Adhesive layer (C) / Resin layer with barrier properties (D) / Olefin resin layer (B2) Heat-resistant coating layer (A) / olefin resin layer (B1) / resin layer with barrier properties (D) Heat-resistant coating layer (A) / Short-wavelength light shielding layer / Olefin resin layer (B1) / Resin layer with barrier properties (D) Heat-resistant coating layer (A) / Short-wavelength light shielding layer / Olefin resin layer (B1) / Resin layer with barrier properties (D) / Olefin resin layer (B2) Heat-resistant coating layer (A) / Short-wavelength light shielding layer / Olefin resin layer (B1) / Resin layer with barrier properties (D) / Adhesive layer (C) / Olefin resin layer (B2) Heat-resistant coating layer (A) / Short-wavelength light shielding layer / Olefin resin layer (B1) / Resin layer with barrier properties (D) / Adhesive layer (C) / Resin layer with barrier properties (D) / Olefin resin layer (B2) Heat-resistant coating layer (A) / olefin resin layer (B1) / short-wavelength light shielding layer / olefin resin layer (B2) Heat-resistant coating layer (A) / olefin resin layer (B1) / short-wavelength light shielding layer / adhesive layer (C) / olefin resin layer (B2) Heat-resistant coating layer (A) / olefin resin layer (B1) / short-wavelength light shielding layer / resin layer with barrier properties (D) / adhesive layer (C) / olefin resin layer (B2) Heat-resistant coating layer (A) / olefin resin layer (B1) / short-wavelength light shielding layer / adhesive layer (C) / resin layer with barrier properties (D) / olefin resin layer (B2) Heat-resistant coating layer (A) / olefin resin layer (B1) / resin layer with barrier properties (D) / short-wavelength light shielding layer / adhesive layer (C) / olefin resin layer (B2) The above-mentioned "short wavelength light-shielding layer / olefin resin layer (B1)" or "olefin resin layer (B1) / short wavelength light-shielding layer" corresponds to the above-mentioned "short wavelength light-shielding film".
[0105] (Olefin resin layer (B1)) As the olefin resin used in the olefin resin layer (B1), a polyethylene resin, a polypropylene resin, or a copolymer thereof can be used. Examples of the polyethylene resin include polyethylene resins such as very low density polyethylene (VLDPE), linear low density polyethylene (LLDPE), linear medium density polyethylene (LMDPE), low density polyethylene (LDPE), medium density polyethylene (MDPE), and high density polyethylene (HDPE); ethylene copolymers such as ethylene-vinyl acetate copolymer (EVA), ethylene-methyl methacrylate copolymer (EMMA), ethylene-ethyl acrylate copolymer (EEA), ethylene-methyl acrylate (EMA) copolymer, ethylene-ethyl acrylate-maleic anhydride copolymer (E-EA-MAH), ethylene-acrylic acid copolymer (EAA), and ethylene-methacrylic acid copolymer (EMAA); and further ionomers of ethylene-acrylic acid copolymer and ionomers of ethylene-methacrylic acid copolymer. These may be used alone or in combination of two or more. Among these, LLDPE can be preferably used since it is easy to suppress the volatilization of transdermal absorption ingredients and the decrease in the patch performance (hereinafter sometimes referred to as volatilization of contents, etc.), and to realize favorable heat sealability such as a wide suitable temperature range for heat seal and favorable adhesion.
[0106] The LDPE may be any branched low-density polyethylene obtained by high-pressure radical polymerization, and is preferably a branched low-density polyethylene obtained by homopolymerizing ethylene by high-pressure radical polymerization.
[0107] LLDPE and LMDPE are produced by copolymerizing ethylene monomer as the main component with α-olefins such as butene-1, hexene-1, octene-1, and 4-methylpentene as comonomers by low-pressure radical polymerization using a single-site catalyst. The comonomer content is preferably in the range of 0.5 to 20 mol%, and more preferably in the range of 1 to 18 mol%.
[0108] Examples of the single-site catalyst include various single-site catalysts such as metallocene catalyst systems, such as combinations of metallocene compounds of transition metals of Group IV or V of the periodic table with organoaluminum compounds and / or ionic compounds. In addition, single-site catalysts have uniform active sites, and therefore, compared with multi-site catalysts, which have non-uniform active sites, the molecular weight distribution of the resulting resin is sharper, and thus low-molecular-weight components are less likely to precipitate when the catalyst is formed into a film, and a resin having excellent physical properties, such as excellent stability of the adhesive strength between resin layers, is obtained, which is preferable.
[0109] The MFR (190°C, 21.18N) of the polyethylene resin is preferably 2 to 20 g / 10 min, more preferably 3 to 10 g / 10 min. If the MFR is within this range, the extrusion moldability of the film is improved. The density of LLDPE is 0.905 g / cm3 in view of packaging suitability, foreign matter sealability, and pinhole resistance. 3 ~0.925g / cm 3 is preferable, and 0.915 g / cm is particularly preferable because it is easy to suppress the evaporation of the contents. 3 ~0.925g / cm 3 It is particularly preferred that:
[0110] Examples of the polypropylene-based resin include propylene homopolymers, propylene-α-olefin random copolymers, such as propylene-ethylene copolymers, propylene-butene-1 copolymers, propylene-ethylene-butene-1 copolymers, and metallocene-catalyzed polypropylenes. These may be used alone or in combination. Propylene-α-olefin random copolymers are preferable, and propylene-α-olefin random polymers polymerized using a metallocene catalyst are particularly preferable. When these polypropylene-based resins are used as the intermediate layer (B), the heat resistance of the film is improved and the softening temperature can be increased, so that the film can be suitably used as a lamination film for packaging materials that has excellent steam and high-pressure heat sterilization properties, such as boiling at 100°C or less, hot filling, or retort sterilization at 100°C or more.
[0111] Moreover, these polypropylene-based resins preferably have an MFR (230° C.) of 0.5 to 30.0 g / 10 min and a melting point of 110 to 165° C., and more preferably have an MFR (230° C.) of 2.0 to 15.0 g / 10 min and a melting point of 115 to 162° C. If the MFR and melting point are within these ranges, the film formability is improved.
[0112] The olefin resin layer (B1) is preferably composed mainly of an olefin resin, since it is easy to realize suitable adhesion, and preferably 80% by mass or more of the resin components constituting the olefin resin layer (B1) is an olefin resin other than the cyclic polyolefin resins exemplified above, more preferably 90% by mass or more, and particularly preferably 100% by mass. In addition, 80% by mass of the olefin resin contained in the olefin resin layer (B1) is an olefin resin having a density of 0.9 g / cm 3 The olefin resin layer (B1) preferably contains linear low-density polyethylene resin in an amount of 80% by mass or more, more preferably 90% by mass or more, because it is particularly easy to obtain adhesion.
[0113] In order to suppress evaporation of the contents, it is also preferable that the olefin resin layer (B1) contains a cyclic polyolefin resin. However, in order to easily ensure suitable adhesion, the content of the cyclic polyolefin resin in the olefin resin layer (B1) is preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably substantially none.
[0114] The thickness of the olefin resin layer (B1) may be appropriately adjusted depending on the mode of use, but is preferably 2 to 8 μm, more preferably 3 to 6 μm, in order to ensure favorable heat sealability while favorably suppressing the volatilization of the contents, etc.
[0115] (Adhesive layer (C)) The adhesive layer (C) may be the same as the adhesive layer described above. It is preferable to use an adhesive having functionality. For example, as an adhesive having barrier properties, the oxygen barrier adhesive PASLIM series manufactured by DIC Corporation, which is a two-liquid reactive adhesive of polyester polyol and isocyanate compound, may be used.
[0116] (Olefin resin layer (B2)) The olefin resin layer (B2) may be a resin layer similar to the olefin resin layer (B1), and is preferably a polyethylene-based resin or a polypropylene-based resin.
[0117] Sealant films may be used to seal contents such as food and medicine. Sealant films are generally made of polyethylene resins such as unoriented very low density polyethylene (VLDPE), linear low density polyethylene (LLDPE), linear medium density polyethylene (LMDPE), low density polyethylene (LDPE), medium density polyethylene (MDPE), polypropylene resin, or co-extruded resins that have these resins on the surface layer.
[0118] In addition, the olefin resin layer (B2) may be a single film, and a sealant may be provided by coating a solution of thermoplastic elastomer polyester, vinyl chloride-vinyl acetate resin, EVOH, acrylic resin, polyolefin resin, or rubber resin. When used as a coating, it can be coated all over or partially, and the film thickness of the solid content is 1 μm to 5 μm.
[0119] The heat-resistant coating layer (A), the printed layer (E), and the resin layer having barrier properties (D) can be the same as the heat-resistant coating layer, the colored printed layer, and the resin layer having barrier properties described above.
[0120] (Laminate other layers) The laminate of the present invention may be used alone or may further include other films or substrates. As the other substrates, in addition to the above-mentioned stretched film, unstretched film, and transparent deposition film, porous substrates such as paper, wood, and leather can also be used. The adhesive used when bonding the other substrates may or may not be a gas barrier adhesive as described above. In addition, in order to fully exert the effect of the short-wavelength light shielding film of the present invention, it is preferable to use a transparent substrate for the laminate.
[0121] <Packaging material> The short wavelength light shielding film of the present invention and a laminate including the short wavelength light shielding film can be used as a packaging material for protecting foods, medicines, etc. When used as a packaging material, the layer structure can be changed depending on the contents, the usage environment, and the usage form.
[0122] The packaging material of the present invention can be obtained, for example, by using the laminate of the present invention, overlapping the surfaces of the sealant film of the laminate so that they face each other, and then heat-sealing the peripheral edge. Examples of the bag-making method include folding or overlapping the laminate of the present invention so that the surfaces of the inner layers (the surfaces of the sealant film) face each other, and heat-sealing the peripheral edge, for example, by a side seal type, a two-sided seal type, a three-sided seal type, a four-sided seal type, an envelope seal type, a grooving seal type, a pleated seal type, a flat bottom seal type, a square bottom seal type, a gusset type, or other heat seal type. The packaging material of the present invention can take various forms depending on the contents, the environment of use, and the form of use. Self-supporting packaging materials (standing pouches) and the like are also possible. Heat sealing can be performed by known methods such as bar seal, rotary roll seal, belt seal, impulse seal, high frequency seal, and ultrasonic seal.
[0123] The packaging material of the present invention is filled with contents through its opening, and the opening is then heat-sealed to produce a product using the packaging material of the present invention. As the contents, particularly preferred are drug solution bags, infusion bags, syringes filled with drug solutions, and the like. The use of the packaging material is not particularly limited, but packaging materials using the printed matter or laminate of the present invention can be suitably used for film packaging applications such as food, medicine, cosmetics, electronic components, infusion packs, and vacuum insulation materials.
[0124] (Secondary packaging) The laminated laminate of the present invention can effectively block short wavelength light and maintain the visibility of the contents, and is therefore particularly useful as a packaging material for secondary packaging for packaging drug solution bags, infusion bags, syringes containing drug solutions, ampoules, etc., which contain drugs that are susceptible to photodegradation. It can also be used as a cover for covering an infusion bag to prevent the drug solution from degrading during infusion. The laminated laminate of the present invention is suitable for such secondary packaging of drugs. EXAMPLES
[0125] The present invention will be described more specifically with reference to examples. In the following, all "parts" and "%" are based on mass.
[0126] (Preparation of polyurethane resin solution P) In a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser and a nitrogen gas inlet tube, 84.5 parts of neopentyl glycol adipate diol (hydroxyl value: 56.6 mg KOH / g), 15.5 parts of polyethylene glycol (hydroxyl value: 278 mg KOH / g) and 27.55 parts of isophorone diisocyanate were charged, and reacted at 90 ° C for 10 hours under a nitrogen stream to produce a urethane prepolymer with an isocyanate group content of 2.84 wt%, and then 68.7 parts of ethyl acetate were added to the mixture to obtain a uniform solution of the urethane prepolymer. Next, the urethane prepolymer solution was added to a mixture consisting of 7.83 parts of isophorone diamine, 0.11 parts of di-n-butylamine, 136.8 parts of ethyl acetate and 110.7 parts of isopropyl alcohol, and the mixture was stirred and reacted at 45 ° C for 5 hours to obtain a polyurethane resin solution P.
[0127] The obtained polyurethane resin solution P had a resin solid concentration of 30.4% by weight, and the weight average molecular weight Mw of the resin solid was 54,000. In addition, the polyurethane resin (total 137.76 parts) contained 11.3% by mass of polyethylene glycol (15.5 parts) as a polyether polyol.
[0128] (Method of preparing vinyl chloride / vinyl acetate solution) A vinyl chloride-vinyl acetate resin having a hydroxyl group (Solvine A) manufactured by Nissin Chemical Industry Co., Ltd. was dissolved in methyl ethyl ketone to a solid content of 15 mass % to prepare a vinyl chloride-vinyl acetate resin solution.
[0129] Example 1 The short wavelength light-shielding ink of Example 1 was prepared by kneading a mixture of 16.8 parts of the prepared polyurethane resin P (solid content 30 parts), 11.9 parts of the prepared vinyl chloride-vinyl acetate resin solution (solid content 15 parts), 9.9 parts of zinc oxide with an average particle size of 20 nm, 3.5 parts of a yellow pigment (Pigment yellow 180), 10.0 parts of an orange pigment (Pigment Orange 13), and the remainder being a solvent (a mixed solvent with a mass ratio of normal propyl acetate:methyl ethyl ketone:ethyl acetate:isopropyl alcohol = 7:3:2:1) for a total of 100 parts.
[0130] (Examples 2 to 7 and Comparative Examples 1 to 3) Inks of Examples 2 to 7 and Comparative Examples 1 to 3 were prepared in the same manner as in Example 1, except that the ink blending ratios shown in Tables 1 and 2 were used.
[0131] Each ink of Examples 1 to 7 and Comparative Examples 1 to 3 was diluted with a mixed solution of methyl ethyl ketone, ethyl acetate and isopropyl alcohol (weight ratio 40:40:20) and adjusted to a viscosity of 16 seconds (25°C) using a Zahn cup #3 (manufactured by Rigo Co., Ltd.). Using a gravure proofing machine equipped with a 30μ solid laser plate, the ink was printed solid twice on a PET film (Toyobo Co., Ltd. E5100, thickness 12μm) and dried for 5 to 6 seconds with a dryer to obtain the printed matter of Examples 1 to 8 and Comparative Examples 1 to 3. The coating amount of the short wavelength light shielding layer was about 3.6 g / m 2 It was.
[0132] The printed matter of the examples and comparative examples was evaluated as follows. 1) Light transmittance (%) The light transmittance of the printed area of the printed matter was measured using a Shimadzu UV-3600 ultraviolet-visible-near infrared spectrophotometer (integrating sphere type) at a measurement wavelength of 200 nm to 800 nm. 2) Character point size: Print data having a sentence composed of characters with DTP points of 6, 8, 10, 12, 16, 24, and 36 points was printed on copy paper using a Xerox laser printer to create a point index, which was then placed on the desk. The printed matter of Example 1 was placed at a height of 3 cm above the desk, and the point index was observed through the printed matter of Example 1 at a height of 30 cm perpendicular to the desk. The smallest point among the characters that could be read was used as an evaluation of the character point number. The printed matter of Examples 2 to 7 and Comparative Examples 1 to 3 was also evaluated for the character point number in the same manner. If the point index was not visible, the evaluation was made as x.
[0133] The results of Examples 1 to 7 are shown in Table 1, and the results of Comparative Examples 1 to 3 are shown in Table 2.
[0134] [Table 1]
[0135] [Table 2]
[0136] From the examples and comparative examples, it was found that the short wavelength light shielding ink containing zinc oxide, orange pigment, and yellow pigment has a high shielding effect in the wavelength region of 200 to 500 nm and also has high visibility.
Claims
1. A short wavelength light blocking ink comprising zinc oxide, an orange pigment and a yellow pigment.
2. The ink is applied to a transparent film at a coating weight of about 3.6 g / m 2 The short wavelength light shielding ink according to claim 1, which has a transmittance of 1.0% or less at wavelengths of 200 to 500 nm when coated with said ink.
3. 2. The short wavelength light shielding ink according to claim 1, wherein the orange pigment is C.I. Pigment Orange 13.
4. The ink is applied to the transparent film in an amount of 3.0 g / m 2 4. The short wavelength light shielding film according to claim 1, having an ink layer coated as described above.
5. A laminate comprising the short wavelength light shielding film according to claim 4.
6. A packaging material using the laminate according to claim 5.
7. A medicine that is secondarily packaged with the laminate of claim 6.
Citation Information
Patent Citations
Light-shielding laminated packaging material
JP2013075453A