Antistatic hard coat film

The antistatic hard coat film addresses interference unevenness and adhesion issues by using a specific composition with controlled film thickness and permeability, enhancing display clarity and durability.

JP2024154480AActive Publication Date: 2024-10-31TOYO INK MFG CO LTD +1

Patent Information

Application Number
JP2023068292
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-31
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

Existing hard coat films for displays suffer from interference unevenness and poor adhesion due to refractive index differences and moisture permeability, leading to reduced visibility and durability issues, especially in thinner displays.

Method used

An antistatic hard coat film with a triacetyl cellulose base, a mixed layer, and a hard coat layer composed of specific copolymers, compounds with ethylenically unsaturated groups, and solvents, which form a composition that enhances adhesion and suppresses interference unevenness by controlling the film thickness ratio and permeability.

Benefits of technology

The film effectively reduces interference unevenness and improves adhesion, maintaining display clarity and durability even in high humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154480000001_ABST
    Figure 2024154480000001_ABST
Patent Text Reader

Abstract

To provide an antistatic hard coat film which is suppressed in interference unevenness and has excellent adhesion.SOLUTION: An antistatic hard coat film is provided, including a triacetyl cellulose film, a mixed layer and a hard coat layer. The hard coat layer is formed of composition for forming an antistatic hard coat layer, including a specific antistatic copolymer (A), a compound (B) having three or more ethylenically unsaturated groups, a compound (C) having one ethylenically unsaturated group, a photoinitiator (D) and a solvent (E). The mixed layer is a layer formed by dissolving or swelling the triacetyl cellulose film with the composition for forming the antistatic hard coat layer. When a cross section in the thickness direction of the antistatic hard coat film is observed with a scanning electron microscope, a film thickness ratio of the mixed layer to the total film thickness of the hard coat layer and the mixed layer is 65% or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an antistatic hard-coated film. [Background technology]

[0002] Hard coat films are used to protect the surfaces of various displays, such as liquid crystal displays, plasma displays, EL displays, rear projection displays, and CRT displays, which are used as image display devices in televisions, computers, car navigation systems, in-vehicle instrument panels, mobile phones, etc.

[0003] Hard coat films have excellent properties such as mechanical properties, dimensional stability, and electrical insulation, and therefore transparent plastics are widely used as substrates for many applications, including optical display materials, packaging materials, electrical insulation materials, various photographic materials, and graphic arts materials. Among transparent plastics, triacetyl cellulose (TAC) film is often used for optical display materials such as monitors because of its transparency, refractive index, impact resistance, heat resistance, and durability.

[0004] Typically, a hard coat film is produced by forming a hard coat layer on a triacetyl cellulose film substrate by coating or printing a resin composition. A cured coating film (hard coat layer) formed from a compound having a (meth)acryloyl group in the molecule that is cured by active energy rays such as ultraviolet rays has a high specific surface resistance and is prone to generating static electricity, which causes problems such as dust adsorption and static electricity, resulting in significant loss of productivity. In order to solve these problems, attempts have been made to develop antistatic hard-coated films that are provided with antistatic properties.

[0005] Patent Document 1 discloses an antistatic coating composition containing an antistatic copolymer having a quaternary ammonium salt group, a compound having three or more ethylenically unsaturated groups, a photopolymerization initiator, and a solvent selected from alcohols, carbonates, and cyclic ethers. It also describes an antistatic hard coat film in which an antistatic layer having excellent durability is formed by applying this antistatic coating composition to a substrate.

[0006] On the other hand, in hard coat films, due to the difference in refractive index between the hard coat layer and the triacetyl cellulose that forms the base film, or due to discontinuous changes in refractive index across the interface, light reflected from the surface of the hard coat layer and light reflected from the interface between the hard coat layer and the base film interfere with each other, causing interference unevenness (iridescent unevenness), which degrades the visibility of the display and mars the aesthetic appearance of the display. In recent years, as displays have become thinner and lighter, the film substrate has become thinner, and the level of demand for suppressing interference irregularities has been increasing.

[0007] Furthermore, hard coat films using triacetyl cellulose film as a substrate have high moisture permeability, and therefore, in high temperature and high humidity environments, the film absorbs moisture, causing dimensional changes and distortion, as well as reduced adhesion.

[0008] An antistatic hard coat film using a triacetyl cellulose film as a substrate, which suppresses interference unevenness and also has excellent adhesion, has not yet been developed. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2012-102166 A Summary of the Invention [Problem to be solved by the invention]

[0010] In view of the above problems, an object of the present invention is to provide an antistatic hard coat film which suppresses interference unevenness and further has excellent adhesion. [Means for solving the problem]

[0011] The present inventors have conducted extensive research to solve the above problems and have arrived at the present invention.

[0012] That is, the present invention provides an antistatic hard-coated film having a triacetyl cellulose film, a mixed layer, and a hard-coat layer, the hard coat layer is formed from a composition for forming an antistatic hard coat layer, the composition comprising an antistatic copolymer (A), a compound (B) having three or more ethylenically unsaturated groups, a compound (C) having one ethylenically unsaturated group, a photopolymerization initiator (D), and a solvent (E); the mixed layer is a layer formed by dissolving or swelling the triacetyl cellulose film with the composition for forming an antistatic hard coat layer; when a cross section of the antistatic hard coat film is observed in the thickness direction with a scanning electron microscope, the thickness ratio of the mixed layer to the total thickness of the hard coat layer and the mixed layer is 65% or more; The present invention relates to an antistatic hard coat film, wherein the antistatic copolymer (A) is a copolymer having, as essential components, a compound (a-1) having a quaternary ammonium salt group represented by the following general formula (1) and a compound (a-2) having an alkylene oxide chain represented by the following general formula (2). General formula (1) CH2=C(R1)COZ(CH2)kN + (R2)(R3)R4·X - (In the formula, R1 is H or CH3, R2 to R4 are hydrocarbon groups having 1 to 9 carbon atoms, Z is an oxygen atom or an NH group, k is an integer of 1 to 10, and X - represents a monovalent anion.) General formula (2) CH2=C(R5)COO(AO)nR6 (In the formula, R5 represents H or CH3, R6 represents hydrogen or a hydrocarbon group having 1 to 22 carbon atoms, n represents an integer of 2 to 200, and A represents an alkylene group having 2 to 4 carbon atoms.)

[0013] The present invention also relates to the above antistatic hard coat film, wherein the mass ratio of compound (C) / solvent (E) is from 0.03 to 0.30.

[0014] The present invention also relates to the antistatic hard coat film, wherein the solvent (E) is selected from the group consisting of dimethyl carbonate, ethyl acetate, acetone, methyl ethyl ketone and 1,3-dioxolane.

[0015] The present invention also relates to the antistatic hard coat film, which contains a compound (c1) having one ethylenically unsaturated group, and in which the mass change value [(X2) / (X1)] between the initial mass (X1) of a triacetyl cellulose film having short sides of 2 cm, long sides of 4 cm, and a thickness of 80 μm, and the mass (X2) of the triacetyl cellulose film after the triacetyl cellulose film is immersed in 35 g of a compound having one ethylenically unsaturated group in an environment of 25° C. for 2 hours, is 1.2 or more. Effect of the Invention

[0016] By using the composition for forming an antistatic hard coat layer of the present invention, it is possible to provide an antistatic hard coat film which suppresses interference unevenness and has excellent adhesion. [Brief description of the drawings]

[0017] [Figure 1] 1 is a schematic cross-sectional view showing an example of a configuration of an antistatic hard coat film of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] A preferred embodiment of the present invention will be described below. In this specification, a numerical range specified using "to" includes the numerical values ​​before and after "to" as the lower and upper limit ranges. In this specification, "film" and "sheet" are not distinguished by thickness. In other words, in this specification, "sheet" includes thin film-like objects, and "film" includes thick sheet-like objects.

[0019] In this specification, the term "(meth)acrylic" means "acrylic or methacrylic" unless otherwise specified. In addition, an "antistatic hard coat film" may be referred to as a "hard coat film", an "antistatic hard coat layer" as a "hard coat layer", an "antistatic copolymer (A)" as a "copolymer (A)", a "compound (B) having three or more ethylenically unsaturated groups" as a "compound (B)", a "compound (C) having one ethylenically unsaturated group" as a "compound (C)", and a "compound (c1) having one ethylenically unsaturated group" as a "compound (c1)". Unless otherwise noted, the various components appearing in this specification may be used independently as a single type, or as a mixture of two or more types.

[0020] <Antistatic hard coat film> The antistatic hard-coated film of the present invention is a hard-coated film having a triacetyl cellulose film, a mixed layer, and a hard-coat layer.

[0021] <Triacetyl cellulose film> The triacetyl cellulose film used in the present invention may be of an optically transparent grade that can be used as a substrate for a polarizing plate, etc., and the thickness of the triacetyl cellulose film is not particularly limited, but is generally about 10 to 500 μm in terms of strength, workability such as handling, thin layer property, etc. In particular, 20 to 250 μm is preferable.

[0022] <Mixed layer> The mixed layer is a layer formed by dissolving or swelling a triacetyl cellulose film with a composition for forming an antistatic hard coat layer. When a cross section of the hard coat film in the thickness direction is observed with a scanning electron microscope, the thickness ratio of the mixed layer to the total thickness of the hard coat layer and the mixed layer is 65% or more. The film thickness ratio is more preferably 67% or more, and even more preferably 70% or more. From the viewpoint of improving adhesion, it is preferably 90% or less. By making the film thickness ratio of the mixed layer 65% or more, it is possible to reduce interference unevenness. From the viewpoint of excellent reduction of interference unevenness, the higher the film thickness ratio, the more preferable it is.

[0023] <Hard coat layer> The hard coat layer of the present invention is formed by coating an antistatic hard coat layer forming composition containing an antistatic copolymer (A), a compound (B) having three or more ethylenically unsaturated groups, a compound (C) having one ethylenically unsaturated group, a photopolymerization initiator (D), and a solvent (E), drying the solvent, and then curing the coating by irradiating with ultraviolet light.

[0024] In order to make the thickness ratio of the mixed layer 65% or more, it is important to include a compound (C) having one ethylenically unsaturated group and a solvent (E). When the composition for forming an antistatic hard coat layer is applied to a triacetyl cellulose film, the compound (C) having one ethylenically unsaturated group and the solvent (E) corrode the triacetyl cellulose film to form a mixed layer. The thickness ratio of the mixed layer can be controlled by the type of compound (C) and solvent (E) and the content thereof. When the compound (C) is the compound (c1) described later, or / and the solvent (E) is the solvent (e1) described later, it is particularly preferable because the thickness ratio of the mixed layer is easily made 65% or more. That is, it is particularly preferable that the compound (C) is the compound (c1) and the solvent (E) is the solvent (e1). In addition, the film thickness ratio of the mixed layer can be made 65 mass % or more by improving the substrate permeability (substrate erosion) by a manufacturing method such as adjusting the nonvolatile concentration of the antistatic hard coat layer forming composition or by applying the hard coat layer forming composition to a triacetyl cellulose film and then leaving it to stand.

[0025] (Antistatic hard coat layer forming composition) The composition for forming an antistatic hard coat layer contains an antistatic copolymer (A), a compound (B) having three or more ethylenically unsaturated groups, a compound (C) having one ethylenically unsaturated group, a photopolymerization initiator (D), and a solvent (E). Moreover, the compound (C) is preferably a compound having one ethylenically unsaturated group, in which the mass change value [(X2) / (X1)] described below is 1.2 or more. Moreover, the solvent (E) is preferably a solvent having a haze change value [(Y2)-(Y1)], which will be described later, of 0.10 or more. It is particularly preferred that the compound (C) is a compound (c1) having one ethylenically unsaturated group and having a mass change value [(X2) / (X1)] of 1.2 or more, and the solvent (E) is a solvent (e1) having a haze change value [(Y2)-(Y1)] of 0.10 or more. This improves the substrate permeability and is effective in reducing interference unevenness.

[0026] The non-volatile content of the composition for forming an antistatic hard coat layer is preferably 70% by mass or less, more preferably 60% by mass or less, from the viewpoint of improving the substrate permeability. From the viewpoint of suppressing the decrease in the coating haze, the non-volatile content is preferably 25% by mass or more, more preferably 35% by mass or more. By adjusting the non-volatile content of the composition for forming an antistatic hard coat layer, it becomes easy to control the film thickness ratio of the mixed layer to 65% by mass or more.

[0027] [Antistatic copolymer (A)] The antistatic copolymer (A) contains, as essential components, a compound (a-1) having a quaternary ammonium salt group represented by the following general formula (1) and a compound (a-2) having an alkylene oxide chain represented by the following general formula (2), and, if necessary, is obtained by radical copolymerization of a compound (a-3) copolymerizable with the above-mentioned (a-1) and (a-2) in an alcohol solvent.

[0028] General formula (1) CH2=C(R1)COZ(CH2)kN + (R2)(R3)R4·X - (In the formula, R1 is H or CH3, R2 to R4 are hydrocarbon groups having 1 to 9 carbon atoms, Z is an oxygen atom or an NH group, k is an integer of 1 to 10, and X - represents a monovalent anion.) General formula (2) CH2=C(R5)COO(AO)nR6 (In the formula, R5 represents H or CH3, R6 represents hydrogen or a hydrocarbon group having 1 to 22 carbon atoms, n represents an integer of 2 to 200, and A represents an alkylene group having 2 to 4 carbon atoms.)

[0029] <Compound (a-1) having a quaternary ammonium base> The compound (a-1) having a quaternary ammonium salt group is represented by the above general formula (1), and when R2 to R4 in the general formula (1) are hydrocarbon groups having 1 to 9 carbon atoms, the hydrocarbon groups can be selected to be substituted or unsubstituted, preferably unsubstituted, and more preferably unsubstituted alkyl groups. The unsubstituted alkyl groups include those with or without branches, You can use either one. If the carbon numbers of R2 to R4 are greater than 10, the hydrophobicity of the produced antistatic copolymer (A) increases, and as a result, the moisture absorption of the antistatic layer containing the antistatic copolymer (A) decreases, and good antistatic performance may not be obtained. Among R2 to R4 in the general formula (1), the unsubstituted alkyl group is preferably an alkyl group having 1 to 3 carbon atoms, and those having an unsubstituted alkyl group such as a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, etc. are preferred in terms of ease of availability.

[0030] The compound (a-1) having a quaternary ammonium base can be obtained, for example, by quaternizing (meth)acrylates or (meth)acrylamides having an amino group with a quaternizing agent. Commercially available (meth)acrylates or (meth)acrylamides having a quaternary ammonium base can also be used.

[0031] Examples of (meth)acrylates having an amino group for forming a compound (a-1) in which Z in general formula (1) has a quaternary ammonium salt group of an oxygen atom include dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, dimethylaminobutyl (meth)acrylate, diethylaminoethyl (meth)acrylate, diethylaminopropyl (meth)acrylate, dipropylaminoethyl (meth)acrylate, dibutylaminoethyl (meth)acrylate, and dihydroxyethylaminoethyl (meth)acrylate.

[0032] Examples of (meth)acrylamides having an amino group for forming compound (a-1) in which Z in general formula (1) has a quaternary ammonium salt group of an NH group include dimethylaminoethyl(meth)acrylamide, dimethylaminopropyl(meth)acrylamide, dimethylaminobutyl(meth)acrylamide, diethylaminoethyl(meth)acrylamide, diethylaminopropyl(meth)acrylamide, dipropylaminoethyl(meth)acrylamide, dibutylaminoethyl(meth)acrylamide, and dihydroxyethylaminoethyl(meth)acrylamide.

[0033] As a quaternizing agent for converting the (meth)acrylates having an amino group or the (meth)acrylamides having an amino group into quaternary salts, various halides such as alkylbenzyl chloride, benzyl chloride, alkyl chloride, alkyl bromide, etc.; alkyl sulfates such as dimethyl sulfate, diethyl sulfate, dipropyl sulfate, etc.; sulfonate esters such as methyl p-toluenesulfonate, methyl benzenesulfonate, etc.; and alkyl phosphates such as trimethyl phosphite, etc. can be used.

[0034] <Compound (a-2) Having an Alkylene Oxide Chain> Next, the compound (a-2) having an alkylene oxide chain, which is another essential component used in forming the antistatic copolymer (A) used in the present invention, will be described. The compound (a-2) having an alkylene oxide chain is represented by the above general formula (2) and can be obtained, for example, by ring-opening polymerization of ethylene oxide with an alkyl alcohol, followed by ester exchange reaction with methyl (meth)acrylate, or reaction with (meth)acrylic acid chloride.

[0035] In the general formula (2), the alkylene oxide group (AO) is an alkylene oxide group having 2 to 4 carbon atoms, such as an ethylene oxide group, a propylene oxide group, or a butylene oxide group. In addition, alkylene oxide groups having different numbers of carbon atoms may exist in the same monomer. The number of alkylene oxide groups (n) is an integer of 2 to 200, and preferably an integer of 10 to 100. If it is 2 or less or 101 or more, sufficient compatibility with the compound (B) having three or more ethylenically unsaturated groups in the molecule, which will be described later, may not be obtained. R6 is hydrogen or a hydrocarbon group having a carbon number of 1 to 22. If the carbon number is 23 or more, it is not practical because the raw material is expensive. The hydrocarbon group having 1 to 22 carbon atoms may be substituted or unsubstituted, preferably unsubstituted, and more preferably an unsubstituted alkyl group. As the unsubstituted alkyl group, either branched or unbranched groups may be used.

[0036] Specific examples of the compound (a-2) having an alkylene oxide chain include polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polybutylene glycol mono(meth)acrylate, poly(ethylene glycol-propylene glycol) mono(meth)acrylate, poly(ethylene glycol-tetramethylene glycol) mono(meth)acrylate, poly(propylene glycol-tetramethylene glycol) mono(meth)acrylate, polyethylene glycol mono(meth)acrylate monomethyl ether, polyethylene glycol mono(meth)acrylate monobutyl ether, polyethylene glycol mono(meth)acrylate monooctyl ether, polyethylene glycol mono(meth)acrylate monobenzyl ether ...methyl ether, polyethylene glycol mono(meth)acrylate monomethyl ether, polyethylene glycol mono(meth)acrylate monoethyl ether, polyethylene glycol mono(meth)acrylate monoethyl ether, polyethylene glycol mono(meth)acrylate monoethyl ether, polyethylene glycol mono(meth)acrylate monoethyl ether, polyethylene glycol mono(meth)acrylate monoethyl ether, polyethylene glycol mono(meth)acrylate monoethyl ether, polyethylene glycol mono(meth)acrylate monoethyl ether, polyethylene glycol mono(meth)acrylate monoethyl ether, polyethylene glycol Examples of the monophenyl ether include acrylate monophenyl ether, polyethylene glycol mono(meth)acrylate monodecyl ether, polyethylene glycol mono(meth)acrylate monododecyl ether, polyethylene glycol mono(meth)acrylate monotetradecyl ether, polyethylene glycol mono(meth)acrylate monohexadecyl ether, polyethylene glycol mono(meth)acrylate monooctadecyl ether, poly(ethylene glycol-propylene glycol) mono(meth)acrylate octyl ether, poly(ethylene glycol-propylene glycol) mono(meth)acrylate octadecyl ether, and poly(ethylene glycol-propylene glycol) mono(meth)acrylate nonylphenyl ether.

[0037] <Compound (a-3) copolymerizable with (a-1) and (a-2)> The antistatic copolymer (A) used in the present invention contains, as essential components, a compound (a-1) having a quaternary ammonium salt group and a compound (a-2) having an alkylene oxide chain, and is obtained by further radical copolymerizing, as necessary, a compound (a-3) copolymerizable with the above-mentioned (a-1) and (a-2) in an alcohol solvent. The compound (a-3) copolymerizable with (a-1) and (a-2) in the present invention is not particularly limited as long as it is a compound having one ethylenically unsaturated group, and examples thereof include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, and octadecyl (meth)acrylate; hydroxyethyl (meth)acrylate. hydroxyalkyl (meth)acrylates such as hydroxypropyl (meth)acrylate and hydroxybutyl (meth)acrylate; various (meth)acrylates such as benzyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, butoxyethyl (meth)acrylate, cyanoethyl (meth)acrylate and glycidyl (meth)acrylate; styrene, methylstyrene, and the like.

[0038] The antistatic copolymer (A) used in the present invention can be obtained by radical copolymerization of the compounds (a-1), (a-2) and, optionally, (a-3) in an alcohol solvent. The amounts of the compounds (a-1), (a-2) and (a-3) used are preferably 30-60% by mass for the compound (a-1) from the viewpoint of antistatic performance, and 10-50% by mass for the compound (a-2) from the viewpoint of compatibility with the compound (B) having three or more ethylenically unsaturated groups, based on 100% by mass of the total radical polymerizable compounds. The compound (a-3) is used in the range of 0-50% by mass as necessary for the purpose of adjusting the antistatic property, solubility and rigidity of the antistatic copolymer (A) to be produced.

[0039] The antistatic copolymer (A) can be obtained by subjecting the compounds (a-1), (a-2) and, optionally, (a-3) mixed in the above-mentioned ratio to a solution polymerization method using a polymerization initiator such as a peroxide-based or azobis-based initiator. The solvent used in the polymerization is not particularly limited as long as it is an alcohol solvent, but an alcohol solvent selected from the group consisting of methyl alcohol, ethyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, cyclohexyl alcohol, 2-methoxyethanol, 2-ethoxyethanol, 2-propoxyethanol, 2-butoxyethanol, 1-methoxy-2-propanol, 3-methoxy-1-propanol, 1-ethoxy-2-propanol, 2-ethoxy-1-propanol, and 3-ethoxy-1-propanol is preferably used.

[0040] The amount of the antistatic copolymer (A) used is preferably 1 to 20 parts by mass, more preferably 5 to 15 parts by mass, based on 100 parts by mass of the compound (B) having three or more ethylenically unsaturated groups and the compound (C) having one ethylenically unsaturated group, which will be described later. When the amount is 1 part by mass or more, sufficient antistatic performance can be obtained, and when the amount is 20 parts by mass or less, the adhesion of the formed hard coat layer is improved.

[0041] [Compound (B) having three or more ethylenically unsaturated groups] Next, the compound (B) having three or more ethylenically unsaturated groups used in the composition for forming an antistatic hard coat layer of the present invention will be described. The compound (B) having three or more ethylenically unsaturated groups is preferably a crosslinkable reactive compound having at least three or more (meth)acryloyl groups in the molecule, and may contain an ether bond, a thioether bond, an ester bond, an amide bond, a urethane bond, etc. in the molecule.

[0042] Compound (B) is a compound having three or more ethylenically unsaturated groups. For example, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, PO-modified trimethylolpropane tri(meth)acrylate, tris(acryloxyethyl)isocyanurate, caprolactone-modified tris(acryloxyethyl)isocyanurate, trimethylolethane tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate ester compounds of polyhydric alcohols and (meth)acrylic acid, such as dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, alkyl-modified dipentaerythritol tri(meth)acrylate, alkyl-modified dipentaerythritol tetra(meth)acrylate, alkyl-modified dipentaerythritol penta(meth)acrylate, caprolactone-modified dipentaerythritol hexa(meth)acrylate, and 1,2,3-cyclohexane tetra(meth)acrylate; Polyfunctional poly(meth)acrylate compounds such as polyurethane poly(meth)acrylate, polyester poly(meth)acrylate, polyether poly(meth)acrylate, polyacryl poly(meth)acrylate, polyalkyd poly(meth)acrylate, polyepoxy poly(meth)acrylate, polyspiroacetal poly(meth)acrylate, polybutadiene poly(meth)acrylate, polythiol polyene poly(meth)acrylate, and polysilicon poly(meth)acrylate; Examples of the ester compound include an ester compound synthesized from a polyhydric alcohol, a polybasic acid, and (meth)acrylic acid, such as an ester compound synthesized from trimethylolethane / succinic acid / acrylic acid=2 / 1 / 4 (molar ratio).

[0043] From the viewpoint of adhesion, the compound (B) is preferably pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, polyurethane poly(meth)acrylate, polyester poly(meth)acrylate, polyether poly(meth)acrylate, and polyacryl poly(meth)acrylate, and more preferably pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, polyurethane poly(meth)acrylate, and polyester poly(meth)acrylate. These can be combined arbitrarily. In particular, it is preferable to combine polyurethane poly(meth)acrylate having urethane with pentaerythritol poly(meth)acrylate or / and dipentaerythritol poly(meth)acrylate.

[0044] The content of the compound (B) is preferably 70 to 97% by mass, more preferably 80 to 95% by mass, based on 100% by mass of the total of the compound (B) and the compound (C) having one ethylenically unsaturated group described below. This range is preferable because it improves the coating film strength and adhesion.

[0045] [Compound (C)] Compound (C) is a compound having one ethylenically unsaturated group, and like organic solvent (E) described below, it plays a role in increasing the substrate permeability of the composition for forming an antistatic hard coat layer into the triacetyl cellulose film. When the composition for forming an antistatic hard coat layer is applied onto the triacetyl cellulose film, compound (C) corrodes the triacetyl cellulose film, allowing the composition for forming an antistatic hard coat layer to penetrate, increasing the film thickness ratio of the mixed layer and reducing interference unevenness. The effect of organic solvent (E) described below is observed from the time of film application to drying, whereas compound (C) is considered to be effective from the time of film application to UV irradiation.

[0046] Examples of the compound (C) include ester compounds such as methyl (meth)acrylate, ethyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, lauryl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and 2-(meth)acryloyloxyethyl acid phosphate; Styrenic compounds such as styrene and alpha-methylene; silane compounds such as γ-(meth)acryloxypropyltrimethoxysilane and γ-(meth)acryloxypropyltriethoxysilane; Nitrogen-containing compounds such as 2-(N,N-dimethylamino)ethyl (meth)acrylate, N-methylol (meth)acrylamide, diethyl (meth)acrylamide, N-vinyl-ε-caprolactam, and acryloylmorpholine; Fluorine-containing compounds such as trifluoroethyl (meth)acrylate and 2,2,3,3,3-pentafluoropropyl (meth)acrylate; Examples of the polymerizable silicone compound include a polymer main chain that is a silicone component and one end of which is modified with a (meth)acrylate group.

[0047] It is preferable that the compound (C) is a compound (c1) in which the mass change value [(X2) / (X1)] between the initial mass (X1) of a triacetyl cellulose film having a short side of 2 cm, a long side of 4 cm, and a thickness of 80 μm and the mass (X2) of the triacetyl cellulose film after the triacetyl cellulose film is immersed in 35 g of a compound (C) having one ethylenically unsaturated group in an environment of 25° C. for 2 hours is 1.2 or more, since this makes it easy to control the film thickness ratio of the mixed layer to 65% or more and provides an excellent reduction in interference unevenness. The mass change value [(X2) / (X1)] is more preferably 2.0 to 10.0, and even more preferably 3.0 to 6.0. By using the compound (C) that satisfies this range, the adhesion can be improved and the reduction of interference unevenness can be more excellent. A more preferable range of [(X2) / (X1)] is 3.5 to 4.5.

[0048] Examples of the mass change value [(X2) / (X1)] of the compound (C) are acryloylmorpholine (3.9), 4-hydroxybutyl acrylate (2.9), tetrahydrofurfuryl acrylate (1.5), N-vinyl-ε-caprolactam (4.3), diethylacrylamide (5.2), lauryl acrylate (1.0), isobornyl acrylate (1.0), and phenoxyethyl acrylate (1.1). It is preferable to use acryloylmorpholine, N-vinyl-ε-caprolactam, diethylacrylamide, etc. as the compound (c1). From the viewpoint of improving the substrate permeability and effectively reducing interference unevenness, acryloylmorpholine and N-vinyl-ε-caprolactam are more preferable, and acryloylmorpholine is further preferable.

[0049] The content of compound (C) is preferably 3 to 30 mass%, more preferably 4 to 25 mass%, and even more preferably 5 to 20 mass%, relative to 100 mass% of the total of compound (B) and compound (C). When the content of compound (C) is 3 mass% or more, the effect of reducing interference unevenness due to penetration into the substrate becomes large, and when the content is 30 mass% or less, the coating film strength is improved and the adhesion is more excellent, which are preferable.

[0050] [Photopolymerization initiator (D)] The photopolymerization initiator (D) is not particularly limited as long as it has a function of initiating radical polymerization by photoexcitation, and examples thereof include acetophenone compounds, benzoin compounds, benzophenone compounds, phosphine oxide compounds, ketal compounds, anthraquinone compounds, and thioxanthone compounds. Specific examples thereof include benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, diethoxyacetophenone, benzyl dimethyl ketal, 1-hydroxycyclohexyl phenyl ketone, benzophenone, 2,4,6-trimethylbenzoin diphenylphosphine oxide, N,N-dimethylaminobenzoic acid isoamyl, 2-chlorothioxanthone, and 2,4-diethylthioxanthone. In addition, a known organic amine can be added as a sensitizer.

[0051] The amount of the photopolymerization initiator (D) used is preferably 0.1 to 20 parts by mass, more preferably 1 to 15 parts by mass, based on 100 parts by mass of the total of the compounds (B) and (C). Within this range, a sufficient polymerization initiation effect is obtained, which is effective in improving adhesion.

[0052] In the composition for forming an antistatic hard coat layer in the present invention, a sensitizer can be used in combination with the photopolymerization initiator (D). Examples of the sensitizer include amine-based sensitizers, anthracene-based sensitizers, thioxanthone-based sensitizers, etc. The sensitizers can be used alone or in combination of two or more kinds. Examples of the amine sensitizer include trimethylamine, methyldimethanolamine, triethanolamine, p-diethylaminoacetophenone, ethyl p-dimethylaminobenzoate, isoamyl p-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, N,N-dimethylbenzylamine, and 4'-bis(diethylamino)benzophenone. Examples of the anthracene sensitizer include 9,10-dibutoxyanthracene, 9,10-diethoxyanthracene, 9,10-dipropoxyanthracene, and 9,10-bis(2-ethylhexyloxy)anthracene. Examples of thioxanthone sensitizers include 2,4-diethylthioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, etc. Representative examples of commercially available products include EPA (manufactured by Nippon Kayaku Co., Ltd.) as an amine sensitizer, DBA and DEA (manufactured by Kawasaki Kasei Chemical Industries, Ltd.) as an anthracene sensitizer, and DETX and ITX (manufactured by Lambson Co., Ltd.) as a thioxanthone sensitizer. The sensitizer is preferably a thioxanthone-based sensitizer.

[0053] When a sensitizer is used, the content thereof is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the total of the compound (B) and the compound (C).

[0054] Solvent The solvent (E) plays a role in increasing the substrate permeability of the composition for forming an antistatic hard coat layer into the triacetyl cellulose film. When the composition for forming an antistatic hard coat layer is applied onto the triacetyl cellulose film, the solvent (E) corrodes the triacetyl cellulose film, and the composition for forming an antistatic hard coat layer penetrates, increasing the film thickness ratio of the mixed layer, thereby reducing interference unevenness. That is, the solvent (E) exerts its effect at a stage before the solvent is evaporated and dried by heating. Note that if the solvent (E) remains in the hard coat layer, the coating hardness decreases, adversely affecting the basic performance of the hard coat, such as scratch resistance, so the solvent (E) needs to be dried before ultraviolet irradiation.

[0055] Examples of the solvent (E) include ethers such as dibutyl ether, dimethoxyethane, diethoxyethane, propylene oxide, 1,4-dioxane, 1,3-dioxolane, 1,3,5-trioxane, tetrahydrofuran, anisole, phenetole, and propylene glycol monomethyl ether; Ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, diethyl ketone, dipropyl ketone, diisobutyl ketone, cyclopentanone, cyclohexanone, and methylcyclohexanone; Esters such as ethyl formate, propyl formate, pentyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, dimethyl carbonate, and γ-butyrolactone; Other examples include methyl 2-methoxyacetate, methyl 2-ethoxyacetate, ethyl 2-ethoxyacetate, ethyl 2-ethoxypropionate, 2-methoxyethanol, 2-propoxyethanol, 2-butoxyethanol, 1,2-diacetoxyacetone, acetylacetone, diacetone alcohol, methyl acetoacetate, and ethyl acetoacetate.

[0056] The solvent (E) is preferably a solvent (e1) in which the initial haze value (Y1) of a triacetyl cellulose film having a short side of 10 cm, a long side of 10 cm, and a thickness of 80 μm and the haze value (Y2) of the triacetyl cellulose film after 0.1 g of solvent (E) is dropped onto the triacetyl cellulose film in an environment of 25° C. and left for 2 minutes, and then heated for 1 minute at 60° C. have a haze change value [(Y2)-(Y1)] of 0.10 or more. Solvent (e1) is preferable in that it is easy to control the film thickness ratio of the mixed layer to 65% or more and is excellent in reducing interference unevenness. The haze change value [(Y2)-(Y1)] is more preferably 0.10 to 0.80, and even more preferably 0.11 to 0.40. A solvent (E) that satisfies this range improves the substrate permeability without decreasing the haze of the coating film, and is effective in reducing interference unevenness.

[0057] Examples of the haze change value [(Y2)-(Y1)] of the solvent (E) are dimethyl carbonate (0.15), ethyl acetate (0.47), acetone (0.81), methyl ethyl ketone (0.42), 1,3-dioxolane (0.48), methyl isobutyl ketone (0.01), isopropyl alcohol (0.04), and propylene glycol monomethyl ether (0.00). It is preferable that the solvent (e1) is selected from the group consisting of dimethyl carbonate, ethyl acetate, acetone, methyl ethyl ketone, and 1,3-dioxolane. Dimethyl carbonate, methyl ethyl ketone, 1,3-dioxolane, or ethyl acetate is more preferred, and dimethyl carbonate is even more preferred, as these improve the substrate permeability and are effective in reducing interference unevenness without reducing the haze of the coating film.

[0058] The total content of the compound (C) and the solvent (E) is preferably 30 to 80 mass %, more preferably 40 to 70 mass %, in 100 mass % of the composition for forming a hard coat layer. If it is 30 mass % or more, the substrate permeability is high, and the adhesion is further improved, and if it is 80 mass % or less, the substrate permeability is not too high, and the deterioration of the coating haze can be further suppressed.

[0059] The mass ratio of compound (C) / solvent (E) is preferably 0.03 to 0.30, more preferably 0.05 to 0.20. When it is 0.03 or more, the adhesion is improved, and when it is 0.30 or less, sufficient permeability into the substrate can be ensured, so that the effect of reducing interference unevenness is further improved.

[0060] The antistatic hard coat layer forming composition of the present invention may contain other additives as necessary. Examples of the other additives include a plasticizer, a surface conditioner, a light stabilizer, an antioxidant, and a polymerization inhibitor.

[0061] <Production of antistatic hard coat film> The method for producing the antistatic hard coat film is not particularly limited, and the film can be produced by a conventionally known method, such as coating a composition for forming an antistatic hard coat layer on a triacetyl cellulose film. For example, the composition for forming an antistatic hard coat layer of the present invention is applied to a triacetyl cellulose film, and then the solvent is dried as necessary. The applied composition for forming an antistatic hard coat layer is crosslinked and cured by irradiating it with active energy rays, to obtain an antistatic hard coat film having a triacetyl cellulose film, a mixed layer, and a hard coat layer. This provides an antistatic hard-coated film in which, when a cross section of the antistatic hard-coated film is observed with a scanning electron microscope, the thickness ratio of the mixed layer to the total thickness of the hard-coat layer and the mixed layer is 65% or more. In addition, it is preferable to coat a triacetyl cellulose film with the composition for forming an antistatic hard coat layer and leave it to stand, since this improves the permeability into the substrate and makes it easier to achieve a film thickness ratio of the mixed layer of 65% by mass or more.

[0062] Examples of the coating method include bar coating, blade coating, spin coating, reverse coating, die coating, spray coating, roll coating, gravure coating, microgravure coating, lip coating, air knife coating, and dipping.

[0063] Examples of active energy rays that can be used include electron beams and ultraviolet rays emitted from light sources such as xenon lamps, low-pressure mercury lamps, high-pressure mercury lamps, extra-high-pressure mercury lamps, metal halide lamps, carbon arc lamps, and tungsten lamps.

[0064] The thickness of the hard coat layer is not particularly limited as long as it has hard coat properties, and is usually 1 to 20 μm, preferably 2 to 15 μm. The combined thickness of the hard coat layer and the mixed layer is also not particularly limited, but is preferably 0.5 to 100 μm, more preferably 1.1 to 30 μm, and even more preferably 1.2 to 25 μm in order to reduce interference unevenness. The thickness of the hard coat film is not particularly limited, but is preferably from 50 to 300 μm, more preferably from 81 to 100 μm, and further preferably from 82 to 95 μm. EXAMPLES

[0065] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In addition, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass". The blend amounts in the table are in parts by mass, and amounts other than the solvent are calculated as non-volatile contents. Note that blanks in the table indicate that no blend was made.

[0066] <Mass change value of compound (C) [(X2) / (X1)]> The mass change value of compound (C) [(X2) / (X1)] was determined by the following method. First, the initial mass (X1) of a triacetyl cellulose film with a short side of 2 cm, a long side of 4 cm, and a thickness of 80 μm was measured. Next, this triacetyl cellulose film was immersed in 35 g of a compound (C) having one ethylenically unsaturated group for 2 hours in an environment of 25° C. After that, the triacetyl cellulose film was taken out and lightly wiped with a Kimtowel, and then the mass (X2) of the triacetyl cellulose film was measured. As the triacetyl cellulose film, a triacetyl cellulose film with a thickness of 80 μm (manufactured by Fuji Film Co., Ltd.) was used (this film was also used for the haze described later).

[0067] <Haze change value of solvent (E) [(Y2)-(Y1)]> The haze change value [(Y2)-(Y1)] of the solvent (E) was determined by the following method. First, the initial haze value (Y1) of a triacetyl cellulose film with a short side of 10 cm, a long side of 10 cm, and a thickness of 80 μm was measured. Next, 0.1 g of solvent (D) was dropped onto the triacetyl cellulose film in an environment of 25° C., and the film was left for 2 minutes. After that, the film was heated to 60° C. for 1 minute, and the film was returned to room temperature, and then the haze value (Y2) of the triacetyl cellulose film was measured.

[0068] (Synthesis example) (Production of Compound (a-2) Having an Alkylene Oxide Chain) An autoclave equipped with a stirrer, a thermometer, an alkylene oxide inlet tube, and a nitrogen gas inlet tube was charged with 511.7 parts of stearyl alcohol, 752.9 parts of toluene, and 2 parts of potassium hydroxide, and the system was replaced with nitrogen gas. After that, 30 moles of ethylene oxide relative to the stearyl alcohol were injected over a period of 4 hours at a pressure of 8 kgf / cm2 or less and a temperature of 90°C or less in the reaction vessel, and the reaction was allowed to proceed for a further 5 hours at 90°C. Next, unreacted ethylene oxide was removed by passing air through the mixture, and then 42.0 parts of Kyoward 600 [adsorbent for alkaline (earth) metal hydroxides] manufactured by Kyowa Chemical Industry Co., Ltd. was added. The mixture was treated for 2 hours under conditions of dry air at 5 kPa and 30°C, and then filtered. The toluene was removed from the obtained filtrate by heating and reducing the pressure, and a polyethylene oxide-added alcohol was obtained. 317.7 parts of the obtained polyethylene oxide-added alcohol were transferred to a flask equipped with a stirrer, a thermometer, an air inlet tube, a liquid addition line, and a distillation column, and 200 parts of methyl methacrylate (10 times the molar amount relative to the polyethylene oxide-added alcohol) and 0.04 parts of hydroquinone monomethyl ether were charged. After heating to 80°C while blowing in dry air, 0.2 parts of tetraisopropyl orthotitanate were added every hour to carry out an ester exchange reaction. During the reaction, the by-products methanol and methyl methacrylate were distilled out of the reaction system as an azeotropic mixture as necessary. After 4 hours, the reaction was terminated when the alcohol conversion rate reached 95%. The resulting solution was cooled, washed with water, dehydrated, concentrated, and filtered to obtain a compound (a-2) having 30 ethylene oxide groups and an octadecyl group. The number of alkylene oxide groups is represented by the molar ratio (theoretical value) of the alkylene oxide and the alcohol used in the alkylene oxide addition step.

[0069] <Production of antistatic copolymer (A) (copolymerization process)> In a flask equipped with a stirring blade, a reflux condenser, and a gas inlet, 30 parts of the (a-2) synthesized above, 50 parts of methacryloyloxyethyl trimethylammonium chloride, 20 parts of cyclohexyl methacrylate, 1.5 parts of azobisisobutyronitrile, and 233 parts of ethanol were charged and reacted under a nitrogen stream at 70° C. for 8 hours. After completion of the reaction, the mixture was cooled to obtain an ethanol solution of antistatic copolymer (A) (solid content 30% by weight).

[0070] The components used in Table 1 are shown below. <Quaternary ammonium salt> DQ-100: Dimethylaminoethyl methacrylate quaternary salt (Kyoeisha Chemical Co., Ltd.: Light Ester DQ-100) <Compound (B) Having Three or More Ethylenically Unsaturated Groups> · UA-306H: (Kyoeisha Chemical Co., Ltd.: 6-functional urethane acrylate) M405: Dipentaerythritol hexaacrylate (Toagosei Co., Ltd.: Aronix M405, hexafunctional monomer) PET30: Pentaerythritol triacrylate (KAYARAD PET30, trifunctional monomer, manufactured by Nippon Kayaku Co., Ltd.)

[0071] <Compound (C) Having One Ethylenically Unsaturated Group> The numbers in parentheses are the mass change values ​​[(X2) / (X1)]. [Compound (c1)] ACMO: Acryloylmorpholine (KJ Chemicals Co., Ltd.: ACMO, monofunctional monomer, 3.9) 4-HBA: 4-hydroxybutyl acrylate (Mitsubishi Chemical Corporation: 4HBA, monofunctional monomer, 2.9), THF-A: Tetrahydrofurfuryl acrylate (Kyoeisha Chemical Co., Ltd.: Light Acrylate THF-A, monofunctional monomer, 1.5) NVP: N-vinylcaprolactam (ASHLAND: V-Cap / RC, monofunctional monomer, 4.3) DEAA: Diethylacrylamide (KJ Chemicals Co., Ltd.: DEAA, monofunctional monomer, 5.2) [Others (compounds having one other ethylenically unsaturated group)] LA: Lauryl acrylate (Kyoeisha Chemical Co., Ltd.: Light Acrylate LA, monofunctional monomer, 1.0) IBXA: Isobornyl acrylate (Osaka Organic Chemical Industry Co., Ltd.: IBXA, monofunctional monomer, 1.0) PEA: Phenoxyethyl acrylate (Kyoeisha Chemical Co., Ltd.: Light Acrylate PO-A, monofunctional monomer, 1.1)

[0072] <Photopolymerization initiator (D)> APO: Diphenyl-2,4,6-trimethylbenzoylphosphine oxide (manufactured by Daido Chemical Industry Co., Ltd.: DAIDO UV-CURE APO)

[0073] <Solvent (E)> The value in parentheses is the haze change value [(Y2)-(Y1)]. [Solvent (e1)] DMC: Dimethyl carbonate (Ube Industries, Ltd., 0.15) Ethyl acetate (manufactured by Daicel Corporation, 0.47) Acetone (Mitsubishi Chemical Corporation, 0.81) MEK: Methyl ethyl ketone (Maruzen Petrochemical Co., Ltd., 0.42) 1,3-Dioxolane (Toho Chemical Industry Co., Ltd., 0.48) [Other (other solvents)] MIBK: Methyl isobutyl ketone (Mitsubishi Chemical Corporation, 0.01) IPA: Isopropyl alcohol (Kishida Chemical Co., Ltd., 0.04) PGM: Propylene glycol monomethyl ether (manufactured by Taishin Chemical Co., Ltd., 0.00) EtOH: Ethanol (from antistatic copolymer (A), 0.01)

[0074] <Example 1> An ethanol solution of the antistatic copolymer (A) produced in the synthesis example was added so that the antistatic copolymer was 10 parts by mass in terms of solid content, and 50 parts of a urethane prepolymer mainly composed of a 2:1 adduct of pentaerythritol triacrylate and hexamethylene diisocyanate (manufactured by Kyoeisha Chemical Co., Ltd.: UA-306H, a hexafunctional urethane acrylate), 30 parts of dipentaerythritol hexaacrylate (manufactured by Toagosei Co., Ltd.: ARONIX M405, a hexafunctional monomer), 30 parts of pentaerythritol triacrylate (manufactured by Nippon Kayaku Co., Ltd.: KAYARAD An antistatic hard coat layer forming composition was obtained by mixing 10 parts of PET30 (trifunctional monomer), 10 parts of acryloylmorpholine (ACMO, monofunctional monomer, manufactured by KJ Chemicals Co., Ltd.) as compound (C), 3 parts of diphenyl-2,4,6-trimethylbenzoylphosphine oxide (DAIDO UV-CURE APO, manufactured by Daido Chemical Industry Co., Ltd.) as photopolymerization initiator (D), and 428.7 parts of dimethyl carbonate (DMC, manufactured by Ube Industries, Ltd.) as solvent (E).

[0075] Next, the obtained composition for forming an antistatic hard coat layer was applied onto a triacetyl cellulose film (manufactured by Fuji Film Co., Ltd.) having a thickness of 80 μm under an atmosphere of 25° C. and 50% relative humidity using a bar coater No. 10, and dried in a hot air oven for 1 minute. Then, the coating layer was cured by irradiating ultraviolet rays from a high pressure mercury lamp with an output of 80 w / cm to obtain an antistatic hard coat film having a triacetyl cellulose film, a mixed layer, and a hard coat layer. The total thickness of the hard coat layer and the mixed layer was 9.3 μm, and the thickness of the hard coat film was 87.0 μm. The thickness ratio of the mixed layer to the total thickness of the hard coat layer and the mixed layer was 71.4%.

[0076] <Examples 2 to 36 and Comparative Examples 1 to 3> As shown in Tables 1 to 4, except that the compositions and blending amounts (parts by mass) were changed, antistatic hard coat layer-forming compositions of Examples 2 to 36 and Comparative Examples 1 to 3 were produced in the same manner as in Example 1, and antistatic hard coat films were obtained. The total thickness of the hard coat layer and the mixed layer of the obtained antistatic hard coat films, the thickness of the hard coat film, and the thickness ratio of the mixed layer to the total thickness of the hard coat layer and the mixed layer are shown in Tables 1 to 4.

[0077] [evaluation] The antistatic hard coat films obtained in the respective Examples and Comparative Examples were measured and evaluated by the following methods. The results are shown in Tables 1 to 4.

[0078] [Thickness ratio of mixed layer] The cross section of the obtained antistatic hard coat film in the thickness direction was smoothed by cutting it several times with a diamond knife using an ultramicrotome (Leica Microsystems, model: EM UC7), and then the cross section was observed with a scanning electron microscope (JEOL, model: JSM-7800F) at a voltage of 5 kV. The film thickness ratio of the mixed layer was calculated from the following formula. Mixed layer thickness ratio (%) = mixed layer thickness (μm) / (hard coat layer thickness (μm) + mixed layer thickness (μm)) × 100

[0079] [Antistatic hard coat film thickness] The film thickness (μm) of the obtained antistatic hard coat film was measured using a Digimicro (Nikon Corporation, model: MH-15M).

[0080] [Adhesion] The antistatic hard-coated film thus obtained was subjected to a tape adhesion test in accordance with JIS K5600. The antistatic hard-coated film was cut with a cutter knife to a depth that reached but did not cut the substrate, leaving a total of 100 squares (10 x 10 squares) spaced 1 mm apart. Cellophane tape (25 mm wide, made by Nichiban Co., Ltd.) was then attached to the surface of the coating, and the cellophane tape was then quickly peeled off by hand to evaluate the condition of the remaining squares. Evaluation criteria +++: No peeling (very good). ++: The edges of the mass are slightly chipped (good). +: Peeling of 1 to 5 squares was observed (no problem in practical use). NG: Peeling of 6 or more squares is observed (not practical).

[0081] [Interference Unevenness] The obtained antistatic hard-coated film was cut to 5 cm x 5 cm, and the surface of the TAC substrate opposite to the coated surface was rubbed back and forth about 10 times with sandpaper to smooth the surface, after which a black matte paint was dropped onto it and dried for 2 minutes at 70°C. The 5° absolute reflectance of this was measured using a spectrophotometer (Hitachi High-Technologies Corporation, model: U-4100) and the presence or absence of ripples in the reflection curve was observed. Evaluation criteria +++: No ripples observed (very good). ++: Below the above standard. Almost no ripples observed (good). +: Below the above standard. Some ripples are observed (no problem in practical use). NG: Below the above standard. Ripples are observed (not practical).

[0082] [Antistatic properties] The obtained antistatic hard-coated film was left to stand for 24 hours in an atmosphere of 25°C and relative humidity of 50%, and then the surface resistivity (Ω / □) was measured after 1 minute using a HIOKI surface resistivity meter (SM-8000 series SME-8310) under conditions of a temperature of 25°C and a relative humidity of 50% with an applied voltage of 100 V. Evaluation criteria +++: Less than 1.0E+09Ω / □ (very good). ++: 1.0E+09Ω / □ or more and less than 1.0E+10Ω / □ (good). +: 1.0E+10Ω / □ or more, less than 1.0E+11Ω / □ (no problem in practical use). NG: 1.0E+11Ω / □ or higher (not practical).

[0083] [Table 1]

[0084] [Table 2]

[0085] [Table 3]

[0086] [Table 4]

[0087] From the results in Tables 1 to 4, it was confirmed that the present antistatic hard coat film, in which the film thickness ratio of the mixed layer to the total film thickness of the hard coat layer and the mixed layer formed from the composition for forming an antistatic hard coat layer containing the antistatic copolymer (A), the compound (B) having three or more ethylenically unsaturated groups, the compound (C) having one ethylenically unsaturated group, the photopolymerization initiator (D), and the solvent (E) is 65% or more, can provide an antistatic hard coat film in which interference unevenness is suppressed and which also has excellent adhesion. [Explanation of symbols]

[0088] 1 Triacetyl cellulose film 2 mixed layer 3 Hard coat layer

Claims

1. An antistatic hard-coat film having a triacetyl cellulose film, a mixed layer, and a hard-coat layer, The hard coat layer is formed from a composition for forming an antistatic hard coat layer, the composition comprising: an antistatic copolymer (A), a compound having three or more ethylenically unsaturated groups (B), a compound having one ethylenically unsaturated group (C), a photopolymerization initiator (D), and a solvent (E); the mixed layer is a layer formed by dissolving or swelling the triacetyl cellulose film with the composition for forming an antistatic hard coat layer, when a cross section of the antistatic hard coat film in the thickness direction is observed with a scanning electron microscope, the ratio of the thickness of the mixed layer to the total thickness of the hard coat layer and the mixed layer is 65% or more; The antistatic hard coat film, wherein the antistatic copolymer (A) is a copolymer containing, as essential components, a compound (a-1) having a quaternary ammonium salt group represented by the following general formula (1) and a compound (a-2) having an alkylene oxide chain represented by the following general formula (2): General formula (1) CH 2 =C(R1)COZ(CH 2 ) kN + (R2) (R3) R4・X - (Wherein, R1 is H or CH 3 R2 to R4 are each a hydrocarbon group having 1 to 9 carbon atoms; Z is an oxygen atom or an NH group; k is an integer from 1 to 10; X - represents a monovalent anion.) General formula (2) CH 2 =C(R5)COO(AO)nR6 (Wherein, R5 is H or CH 3 R6 represents hydrogen or a hydrocarbon group having 1 to 22 carbon atoms, n represents an integer of 2 to 200, and A represents an alkylene group having 2 to 4 carbon atoms.

2. 2. The antistatic hard coat film according to claim 1, wherein the mass ratio of the compound (C) to the solvent (E) is from 0.03 to 0.

30.

3. 3. The antistatic hard coat film according to claim 1, wherein the solvent (E) is selected from the group consisting of dimethyl carbonate, ethyl acetate, acetone, methyl ethyl ketone and 1,3-dioxolane.

4. The antistatic hard coat film according to claim 3, characterized in that it contains a compound (c1) having one ethylenically unsaturated group, in which the mass change value [(X2) / (X1)] between the initial mass (X1) of a triacetyl cellulose film having a short side of 2 cm, a long side of 4 cm, and a thickness of 80 μm and the mass (X2) of the triacetyl cellulose film after the triacetyl cellulose film is immersed in 35 g of a compound having one ethylenically unsaturated group in an environment of 25° C. for 2 hours is 1.2 or more.

Citation Information

Patent Citations

  • Ultraviolet-curing elastic resin for 3D printing

    CN111138602A

  • Antistatic coating composition

    JP2011225796A

  • Hard coat layer-forming composition, optical film, production method for optical film, polarizing plate and image display device

    JP2012072275A

  • Antistatic coating composition

    JP2012102166A

  • Radiation curable coating composition

    JP2013185017A

Cited By

  • Laminates and hard coating agents

    JP7941880B1