Ceramic wafer and manufacturing method for them
The ceramic wafer's enhanced orientation flat surface roughness addresses the issue of displacement and chipping, ensuring secure placement and efficient cleaning without contamination.
Patent Information
- Application Number
- JP2023068531
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-04-19
AI Technical Summary
Ceramic wafers and dummy wafers are prone to displacement from jigs during cleaning due to their higher density and repeated use, leading to reduced cleaning efficiency and potential contamination.
The ceramic wafer design features an orientation flat part with increased surface roughness compared to the circumferential part, ensuring secure placement on jigs during cleaning and repeated use.
The design enhances the anti-slip properties of the ceramic wafer, preventing displacement during cleaning and reducing the risk of chipping, thereby maintaining cleaning efficiency and minimizing contamination.
Smart Images

Figure 2024154610000001_ABST
Abstract
Description
[Technical field]
[0001] The embodiments relate to a ceramic wafer and a manufacturing method thereof. [Background technology]
[0002] A silicon nitride substrate is disclosed as a ceramic wafer for arranging a single crystal body (Patent Document 1). According to Patent Document 1, a reference example of a silicon nitride substrate having a high strength of 755 MPa in three-point bending strength is described, and an orientation flat is provided on the circumference to adjust the orientation of the wafer. In addition, a ceramic dummy wafer is a product form similar to a ceramic wafer. Dummy wafers are used to set manufacturing conditions in the film formation process and etching process of semiconductor manufacturing processes. Among dummy wafers, a ceramic dummy wafer that causes less contamination of thin films is disclosed (Patent Document 2). According to Patent Document 1, it has been found that a dummy wafer made of aluminum oxide ceramics does not cause detection omissions by an optical sensor. In addition, a dummy wafer made of the same ceramic with an orientation flat formed thereon is disclosed (Patent Document 3). In the figure of Patent Document 3, an orientation flat is formed, and a dummy wafer with a diameter of 100 mm and a thickness of 0.635 mm is produced by pressing granulated powder made of aluminum powder or the like and then sintering and processing. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 6992364 [Patent Document 2] Patent No. 3943197 [Patent Document 3] JP 2003-8647 A Summary of the Invention [Problem to be solved by the invention]
[0004] Ceramic wafers are heavier than silicon wafer products because their density is greater. This causes a problem that when a heavy ceramic wafer is set on a jig and cleaned with a chemical solution, the wafer may shift out of position from the jig. In addition, ceramic dummy wafers have excellent corrosion resistance and can be cleaned with chemicals and used repeatedly, but similarly cause a problem that the wafer may shift out of position from the jig when cleaned. The ceramic wafer according to the embodiment is intended to address such a problem, and provides a ceramic wafer and a ceramic dummy wafer (hereinafter, ceramic and ceramic dummy wafers will be simply referred to as "ceramic wafers") that can be set well on a jig even during cleaning during repeated use. [Means for solving the problem]
[0005] The ceramic wafer according to the embodiment is a ceramic wafer whose outer periphery is composed of an orientation flat portion and a circumferential portion, and is characterized in that the surface roughness of the end face of the orientation flat portion is greater than the surface roughness of the end face of the circumferential portion. [Brief description of the drawings]
[0006] [Figure 1] FIG. 2 is a diagram showing an example of a ceramic wafer according to an embodiment. [Diagram 2] FIG. 2 is a diagram showing an example in which a ceramic wafer according to an embodiment is set on a jig. [Diagram 3] FIG. 2 is a diagram showing an example in which a ceramic wafer according to an embodiment is set on a jig. [Figure 4] FIG. 13 is a diagram showing an example of a ceramic wafer set on a jig. [Diagram 5] FIG. 2 is a diagram showing an example of a process flow using a ceramic wafer according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The ceramic wafer according to the embodiment is a ceramic wafer whose outer periphery is composed of an orientation flat portion and a circumferential portion, and is characterized in that the surface roughness of the end face of the orientation flat portion is greater than the surface roughness of the end face of the circumferential portion.
[0008] An example of a ceramic wafer according to an embodiment is shown in Fig. 1. In Fig. 1, 1 is a ceramic wafer, 2 is an orientation flat portion, and 3 is a circumferential portion. The size (length) of the orientation flat (hereinafter simply abbreviated as "orientation flat") of the ceramic wafer according to the embodiment varies.
[0009] An orientation flat is a flat portion formed on a semiconductor wafer (hereinafter simply referred to as "wafer") to indicate the crystal orientation of the wafer. For this reason, similar orientation flats are also formed on ceramic wafers used in the same wafer manufacturing process. The edge face of a ceramic wafer with an orientation flat is curved at the circumferential portion and flat at the orientation flat portion. The ceramic wafer according to the embodiment is a ceramic wafer whose outer periphery consists of an orientation flat portion and a circumferential portion, and is characterized in that the surface roughness of the edge face of the orientation flat portion is greater than the surface roughness of the edge face of the circumferential portion.
[0010] Surface roughness is a measure of surface quality, and is measured by the amount of vertical deviation when comparing the surface shape of an object with an ideal surface. If the deviation is large overall, the surface is rough, and if it is small, the surface is smooth. Surface roughness is It is defined in JIS-B-0601 (2013). There are various methods for evaluating surface roughness depending on the characteristics, but any evaluation method can be used as long as it is easy to measure. Representative surface roughness indices are arithmetic mean height (Ra), maximum height (Rz), maximum peak height (Rp), maximum valley depth (Rv), and maximum profile height (Rt), but other surface roughness indices can also be used.
[0011] The measurement method for Ra, Rz, Rp, Rv, and Rt shall be in accordance with JIS-B-0601 (2013). The measurement conditions are: measurement length: 4.0 mm, measurement speed: 0.6 mm / s, shape removal: least squares straight line, λs filter: yes, λs cutoff ratio: 300, cutoff type: Gaussian, cutoff wavelength (λc): 0.8 mm. Each roughness is calculated by rounding off the measured value to two decimal places. If a measurement length of 4.0 mm cannot be ensured in one measurement, it may be measured multiple times. The measurement points may be any points within the range where the measurement part forms the orientation flat and the circumference.
[0012] A number of ceramic wafers are set on a jig made of plastic or the like and oscillated in chemicals or cleaning water. To clean efficiently, it is necessary to set many ceramic wafers on the jig and oscillate them widely. However, ceramics are denser than wafers and therefore heavier. For this reason, if a heavy ceramic dummy wafer is set on the jig for cleaning, it will come off the jig if it is oscillated widely and quickly. Conversely, if it is oscillated slowly and narrowly so that it does not come off the jig, the cleaning efficiency decreases. Furthermore, ceramic dummy wafers (hereinafter simply referred to as "dummy wafers") are used repeatedly, and therefore will be cleaned with chemicals and the like more repeatedly than ceramic wafers.
[0013] Figure 2 shows an example of a ceramic wafer according to the embodiment set on a jig. The jig is inclined to make it easier to insert and remove the dummy wafer. In addition, grooves are formed so that multiple ceramic wafers can be placed on it. In Figure 2, the edge of the orientation flat is placed in contact with the jig plane. By making the surface roughness of this edge of the orientation flat greater than that of the circumferential portion, it is possible to prevent the wafer from slipping on the jig, as opposed to rocking when only the circumferential portion is in contact with the jig plane.
[0014] The ceramic wafer according to the embodiment is a ceramic wafer whose outer periphery is composed of an orientation flat portion and a circumferential portion, and the surface roughness of the end face of the orientation flat portion is greater than the surface roughness of the end face of the circumferential portion. The ratio of the surface roughness of the end face of the circumferential portion to the surface roughness of the end face of the orientation flat portion is in the range of 1.1 to 3.0. If the surface roughness ratio is less than 1.1 times, the effect of roughening the orientation flat portion is reduced, and it may come off the jig during swinging. If the surface roughness ratio is more than 3.0 times, the effect of coming off the jig is obtained, but the processing to increase the roughness of the end face of the orientation flat portion is costly. Furthermore, ceramics have the characteristic of being hard but brittle, and if the surface roughness of the end face of a thin shape is increased, the unevenness of the edges of the flat portion and the end face portion may become large and the wafer may easily chip. If the edges of the ceramic wafer are easily chipped, the edges may chip during semiconductor manufacturing processes such as film formation, cleaning, transportation, etc., resulting in contamination. Furthermore, repeated regeneration processes on dummy wafers can chip the edges, increasing the possibility of contamination. For this reason, it is preferable that the ratio of the surface roughness of the end face of the circumferential portion to the surface roughness of the end face of the orientation flat portion is within a range of 1.1 to 3.0, and more preferably 1.5 to 2.5.
[0015] In addition, by increasing the surface roughness of the orientation flat end face, it is possible to prevent the orientation flat from slipping on the jig in contact with it. For this reason, the arithmetic surface roughness Ra of the orientation flat end face is 1.5 μm or more. Even when set in a normal cleaning jig, if the arithmetic surface roughness Ra is less than 1.5 μm, the anti-slip effect is reduced even if the orientation flat is rougher than the circumferential part, and there is a possibility that it will come off the jig when oscillating. In addition, although there is no limit to the maximum value of the arithmetic mean surface roughness, if it is more than 10.0 μm, it will be effective in preventing it from coming off the jig, but it will be costly to process it to increase the roughness of the orientation flat end face. Furthermore, ceramics are hard but brittle, and if the surface roughness of a thin end face is increased, the unevenness of the edges between the flat part and the end face will increase, making them more likely to chip. In addition, if the edges of a ceramic wafer are easily chipped, there is a possibility that the edges will chip during semiconductor manufacturing processes such as film formation, cleaning, transportation, and the regeneration process of dummy wafers, resulting in contamination. For this reason, the arithmetic surface roughness Ra of the end face of the orientation flat portion is preferably within a range of 1.5 μm to 10.0 μm, and more preferably 2.0 μm to 8.0 μm.
[0016] The ceramic wafer is preferably one of silicon nitride, aluminum nitride, aluminum oxide (alumina), and silicon carbide. Silicon nitride has a three-point bending strength of 600 MPa or more, and can be increased to 700 MPa or more. Its thermal conductivity can be increased to 50 W / (m·k) or more, and can be increased to 80 W / (m·k) or more, making it a thin ceramic wafer with excellent heat dissipation. Aluminum nitride has a three-point bending strength of about 300 to 450 MPa, but its thermal conductivity can be increased to 170 W / (m·k) or more, and can be increased to 200 W / (m·k) or more, making it a ceramic wafer with high heat dissipation. Aluminum oxide has a three-point bending strength of about 300 to 450 MPa and a thermal conductivity of about 20 W / (m·k), but is inexpensive and therefore a versatile ceramic wafer. Silicon carbide has a three-point bending strength of about 300 to 450 MPa, but has excellent chemical resistance and can be used as a chemical-resistant ceramic wafer. In particular, when using a ceramic wafer with a surface function such as a semiconductor or piezoelectric, it is preferable to use a dummy wafer of the same type with similar characteristics. It is also possible to use a dummy wafer of a different type from the ceramic wafer by utilizing the characteristics of the respective dummy wafer materials.
[0017] In addition, it is desirable that the size of the ceramic wafer conforms to the diameter and orientation flat determined by the SEMI standard (Semiconductor Equipment and Materials International), which is the standard for silicon (semiconductor) wafers. If the size is the same as that of a silicon wafer, the equipment and jigs can be shared. For example, a 2-inch wafer has a diameter of 50.8 mm, a thickness of 279 μm, and an orientation flat of 15.88 mm, while an 8-inch wafer has a diameter of 200 mm, a thickness of 725 μm, and an orientation flat of 57.5 mm. Silicon wafers are becoming larger, such as 12 inches (300 mm), and the size of ceramic wafers is also becoming larger. In response to this, the thickness of the ceramic wafer is adjusted according to the application. In other words, if heat dissipation is desired rather than insulation, the ceramic wafer will be thinner than the standard value, and if insulation is desired rather than heat dissipation, the ceramic wafer will be thicker than the standard value. For this reason, the thickness of the ceramic wafer is preferably within the range of 0.2 mm to 3 mm.
[0018] Representative resins used for jigs include polypropylene (PP), fluororesin (PFA), polycarbonate (PC), polyether ether ketone (PEEK), polybutylene terephthalate (PBT), and polytetrafluoroethylene (PTFT). The top of the roughly rectangular parallelepiped jig has a rectangular opening to allow easy insertion and removal of wafers. The jig also has a slope from the bottom to the sides to support and store wafers. Grooves are formed on the bottom and sides to store multiple wafers. Multiple wafers are inserted through the opening and aligned in a parallel state. One or both sides of the jig that correspond to the outermost surface of the aligned multiple wafers may be open to improve cleaning and draining effects. The side of the jig where the multiple outer wafers are placed may have slits to improve cleaning and draining effects. The jig with the wafers placed in it is clamped by the handle to move and clean it. The handle is U-shaped and the bars at the ends of both legs are fitted into the grooves of the jig to attach it.
[0019] Figure 5 shows an example of the manufacturing process flow for semiconductor products that use ceramic wafers. Depending on the process, the steps from film formation to cleaning after resist removal may be repeated. Of these, cleaning is the process of removing dirt and stains from the wafer. The dirt and stains that are targeted in cleaning include a variety of types, such as dust and dirt present in the air, metals generated from equipment and chemicals, organic matter generated from paint and resin parts, and oils and grease generated by workers. This dirt and stains become foreign matter when the circuit patterns are created, causing defects. For this reason, the cleaning process is important for ensuring the quality of semiconductor products.
[0020] Ceramic wafers can be made into semiconductor products by placing single crystals on the surface and dicing them. Examples of single crystals include silicon and compound semiconductors. Compound semiconductors include GaN, I nN-based, AlN-based, SiC-based, etc. GaN-based materials include GaN, GaInN, GaAlN, GaInAlN, etc. Examples of the process of disposing the single crystal include a process of stacking the single crystal on a ceramic wafer, and a process of crystal growing the single crystal. Examples of the process of stacking the single crystal on a ceramic wafer include a method of directly disposing the single crystal on a ceramic wafer. Also, the single crystal may be disposed after forming a thin film on the ceramic wafer. Also, examples of the process of crystal growing the single crystal include a gas phase method and a liquid phase method. A thin film may be formed on the ceramic wafer before performing the crystal growth process.
[0021] Dummy wafers are used for testing and adjusting manufacturing equipment in some or all of the semiconductor manufacturing processes. Since dummy wafers are used repeatedly, for example, when they are used for film formation as shown in Figure 5, the formed film is removed and the wafer is reused. In this case, there is a process of immersing the wafer in the chemical solution to be removed and a process of washing the wafer with the chemical solution.
[0022] These solvent immersions and cleaning are carried out in multi-tank or single-tank batch tanks. In the multi-tank type, the wafers are immersed in a processing tank containing chemicals, and cleaning is performed by rinsing off any chemicals adhering to the wafers and jigs with pure water or the like. In the single-tank type, immersion and cleaning are performed by replacing the chemicals in one processing tank. Both the multi-tank and single-tank types can process a large number of wafers at once by setting the wafers in a jig. In order to process a large number of wafers quickly and uniformly, it is necessary to rock them in each tank.
[0023] Next, a method for manufacturing a ceramic wafer according to an embodiment will be described with a silicon nitride wafer as an example. As long as the silicon nitride wafer according to the embodiment has the above configuration, the manufacturing method is not limited, but the following method can be used to obtain the wafer with a good yield. First, silicon nitride powder and sintering aid powder are prepared. The amount of sintering aid added is within the range of 1 mass% to 20 mass%. The sintering aid can be one or more oxides selected from rare earth elements, magnesium, hafnium, and titanium. In particular, it is preferable to use an oxide of a rare earth element as an essential component and add one or more oxides selected from magnesium, hafnium, and titanium. A mixed raw material powder of silicon nitride powder and sintering aid powder is prepared.
[0024] The mixed raw material powder is mixed with a binder and the like to prepare a raw material powder slurry. Next, a molding process is carried out using the raw material powder slurry. The molding process can be carried out by a known method such as a sheet molding method or an extrusion molding method. It is also preferable to process the obtained molded body into a desired shape. For example, a disk-shaped green sheet can be obtained by punching out a green sheet molded by the sheet molding method with a circular die, and a disk-shaped green sheet with an orientation flat can be obtained by punching out a disk-shaped green sheet with an orientation flat with a circular die. It is also possible to stack the molded bodies in order to adjust the thickness.
[0025] When press molding is performed without using sheet molding, the raw material powder slurry is granulated by a method such as spray drying and molded by die pressing. It is preferable to process the obtained molded body into the desired shape. For example, a disk-shaped molded body can be obtained by press molding using a circular mold, and a disk-shaped molded body with an orientation flat can be obtained by using a mold with an orientation flat.
[0026] Next, a step of degreasing the compact is carried out. The degreasing step is preferably carried out at a temperature in the range of 300° C. to 700° C. In addition, a step of sintering the obtained degreasing body is carried out. The sintering step is preferably carried out at a temperature in the range of 1600° C. to 1900° C.
[0027] Next, the end faces of the obtained silicon nitride sintered body are processed. If the sintered body is not in a circular shape such as a square plate, the circumferential part and the orientation flat part are formed by stacking them and performing wire cutting or polishing, or by performing laser processing one by one. In the case of wire cutting, the surface roughness of the processed surface decreases as the number of processing times increases, so the number of times of processing is increased for the orientation flat part compared to the circumferential part. For example, the surface roughness of the orientation flat part can be increased by processing the circumferential part twice and the orientation flat part once. In the case of polishing, the surface roughness of the processed surface decreases by using a larger grindstone, so the surface roughness of the orientation flat part can be increased by processing the orientation flat part with a smaller grindstone than the circumferential part. In laser processing, the surface roughness of the processed surface decreases when the laser dot width is large, so the surface roughness of the orientation flat part can be increased by making the laser dot width wider than that of the circumferential part.
[0028] If the sintered body is in a disk shape, an orientation flat is formed. The orientation flat can be formed by wire cutting, polishing, or laser processing. In each case, the processing conditions are adjusted so that the surface roughness of the orientation flat is greater than that of the circumferential part. Furthermore, if the orientation flat is already formed in the shape of a disk, or if the surface roughness of the end face of the orientation flat is not large due to the above-mentioned processing, the surface roughness can be increased by blasting treatment or the like.
[0029] Next, the surface (both the front and back sides) of the obtained silicon nitride sintered body is polished. Although it is possible to perform the surface processing before the end face processing, it is preferable to perform it after, since the surface roughness of the front face is often processed to be smaller than that of the end face.
[0030] (Examples 1 to 7, Comparative Examples 1 to 6) The following ceramic wafers were prepared. The silicon nitride sintered body is one to which an oxide of a rare earth element and one or more oxides of magnesium, hafnium, and titanium are added as sintering aids. The aluminum nitride sintered body is one to which an oxide of a rare earth element is added as a sintering aid. The aluminum oxide sintered body is one to which one or more sintering aids selected from an alkaline earth metal compound and a silicon compound are added. The silicon carbide is one to which one or more sintering aids selected from boron, carbon, and their compounds are added.
[0031] Silicon nitride, aluminum nitride, and aluminum oxide were made into a slurry by mixing the raw material powder with added additives with resin and organic solvent, and then molded into sheets using a sheet molding machine to obtain green sheets. The green sheets were punched into squares using a die to obtain square green sheets. The green sheets were degreased and then sintered to obtain sintered bodies. The sintered bodies were processed into a circumference and orientation flat using laser, wire processing, and polishing to obtain sintered bodies. In addition, the green sheets were punched into a circle using a die and the orientation flat was cut to obtain disk-shaped green sheets with orientation flats. The green sheets were degreased and then sintered to obtain sintered bodies with orientation flats. Sintered bodies that were not processed or that were blasted were obtained.
[0032] Next, the surfaces (front and back) of the disk-shaped ceramic wafer were polished to an arithmetic mean roughness Ra of 0.1 μm (confirmation required). The obtained ceramic wafer is shown in Table 1. Note that the circumference diameter of 150.0 mm corresponds to 6 inches, and the circumference diameter of 76.2 mm corresponds to 3 inches.
[0033] [Table 1]
[0034] Next, the surface roughness of the circumference edge and orientation flat edge of the ceramic wafer was measured. The measurement conditions for the arithmetic mean surface roughness Ra were as described above. Table 2 shows the arithmetic mean roughness A of the orientation flat edge, the arithmetic mean roughness B of the circumference edge, and the ratio of A to B (A / B). The arithmetic mean roughness was rounded off to one decimal place.
[0035] The arithmetic mean roughness Ra of the ceramic wafers according to the examples was 1.5 μm or more. On the other hand, the comparative examples had a small arithmetic mean roughness of the orientation flat end face. The ceramic wafers according to the examples had a value of A / B, which is the ratio of the surface roughness of the circumferential end face to the surface roughness of the orientation flat end face, in the range of 1.1 to 3.0. The comparative examples had a small value of less than 1.1.
[0036] Next, 25 ceramic wafers of Example 1 were placed in a PFA jig that can store 25 wafers as shown in FIG. 3, so that the orientation flat part was in contact with the inclined surface of the jig. A test was conducted in which the jig containing the ceramic wafer was placed in a tank in which pure water was flowing upward in the center, and the jig was oscillated up and down 30 cm 10 times, and then removed. The number of ceramic wafers that were displaced from the location where they were placed was examined. The positional displacement was determined when the markings, which were placed so as to overlap, were separated by 5 mm or more for a 150 mm diameter ceramic wafer and 3 mm or more for a 76.2 mm diameter ceramic wafer after the test. The jig and ceramic wafer were then dried, the ceramic wafer was removed from the jig, and the test was conducted by placing the ceramic wafer in the jig again, and the number of displaced wafers was examined. The above test was conducted four times in total for a total of 100 ceramic wafers, and the pure water in the tank was replaced, and similar tests were repeated using the same jig for other examples and comparative examples. Table 2 shows the cleaning test results, excluding the percentage of samples that were confirmed to be misaligned from the jig.
[0037] [Table 2]
[0038] As can be seen from the table, the ceramic wafers according to the examples had little misalignment during the cleaning test, and the ceramic wafers placed on the jig were fixed without moving due to rocking. This shows that controlling the arithmetic mean roughness of the orientation flat is effective. In contrast, the comparative examples, in which the ratio of the arithmetic mean roughness of the orientation flat to the arithmetic mean roughness of the circumference was outside the range, showed increased misalignment in the cleaning test. Furthermore, the comparative examples 1 and 6, in which the arithmetic mean value of the orientation flat was outside the range, showed increased misalignment in the cleaning test. In other words, the ceramic wafers placed on the jig moved due to rocking, increasing the possibility of them falling.
[0039] To compare with evaluations using surface roughness indices other than arithmetic mean roughness, the maximum height and other surface roughness values were measured for the sample of Comparative Example 1. The measurement results are shown in Table 3. As can be seen from the table, when the surface roughness of the orientation flat is high using the arithmetic mean roughness, it is possible to use the surface roughness as an index even when other indices are used, because the orientation flat is rough.
[0040] [Table 3]
[0041] Although some embodiments of the present invention have been illustrated above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. In addition, the above-mentioned embodiments can be implemented in combination with each other. [Explanation of symbols]
[0042] 1...Ceramic wafer 2. Orientation flat 3...Circumference 4…Jig
Claims
1. A ceramic wafer having an outer periphery composed of an orientation flat portion and a circumferential portion, characterized in that the surface roughness of the end face of the orientation flat portion is greater than the surface roughness of the end face of the circumferential portion.
2. 2. The ceramic wafer according to claim 1, wherein a ratio of a surface roughness of an end face of the circumferential portion to a surface roughness of an end face of the orientation flat portion is within a range of 1.1 to 3.
0.
3. 3. The ceramic wafer according to claim 1, wherein an arithmetic surface roughness Ra of an end face of the orientation flat portion is 1.5 μm or more.
4. 3. The ceramic wafer according to claim 1, wherein the ceramic wafer is made of any one of aluminum oxide, aluminum nitride, silicon nitride, and silicon carbide.
5. 3. The ceramic wafer according to claim 1, wherein the ceramic wafer has a single crystal disposed thereon.
6. 4. The ceramic wafer according to claim 3, wherein the ceramic wafer has a single crystal disposed thereon.
7. 3. The ceramic wafer according to claim 1, wherein the ceramic wafer is a ceramic dummy wafer.
8. 4. The ceramic wafer according to claim 3, which is a ceramic dummy wafer.
9. A method for manufacturing a ceramic wafer, characterized in that in a ceramic wafer whose outer periphery is composed of an orientation flat portion and a circumferential portion, the surface roughness of the end face of the orientation flat portion is processed to be greater than the surface roughness of the end face of the circumferential portion, and the processing method is processing comprising laser, wire cutting, polishing, and blasting.
10. 10. The method for producing a ceramic wafer according to claim 9, wherein the ratio of the surface roughness of the end face of the circumferential portion to the surface roughness of the end face of the orientation flat portion is processed to be within a range of 1.1 to 3.
0.
11. 11. The method for producing a ceramic wafer according to claim 9, wherein the arithmetic surface roughness Ra of the end face of the orientation flat portion is 1.5 μm or more.
12. 11. The method for producing a ceramic wafer according to claim 9, wherein the ceramic wafer is made of any one of aluminum oxide, aluminum nitride, silicon nitride, and silicon carbide.
Citation Information
Patent Citations
Mask alignment for compound semiconductor wafer
JP1988307727A
Wet treatment method for semiconductor wafer and wet treating apparatus
JP2000012508A
Dummy wafer, manufacturing method therefor and detection method using the same
JP2003086475A
EDGE POLISHED NITRIDE SEMICONDUCTOR SUBSTRATE, EDGE POLISHED GaN FREE-STANDING SUBSTRATE, AND EDGE PROCESSING METHOD OF NITRIDE SEMICONDUCTOR SUBSTRATE
JP2004319951A
Semiconductor substrate, display panel, and method of manufacturing display
JP2009135451A