Treatment agent for producing carbon fiber-containing spun yarn, carbon fiber-containing spun yarn, and method for producing carbon fiber-containing spun yarn

A treatment agent containing an epoxy compound with a diphenylmethane skeleton, optionally with a nonionic surfactant and ester compound, addresses the low strength issue in carbon fiber-containing spun yarns, resulting in improved strength and reduced fluff.

JP2024155065AActive Publication Date: 2024-10-31TAKEMOTO OIL & FAT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023069462
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-31
Estimated Expiration
2043-04-20

AI Technical Summary

Technical Problem

The strength of spun yarn obtained from carbon fibers treated with conventional treatment agents is low, necessitating an improvement in the strength of carbon fiber-containing spun yarns.

Method used

A treatment agent comprising an epoxy compound with a diphenylmethane skeleton, optionally combined with a nonionic surfactant and an ester compound, is applied to carbon fibers to enhance the strength and reduce fluff in the spun yarn.

Benefits of technology

The treatment agent significantly improves the strength of the spun yarn while reducing fluff, achieving enhanced performance characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155065000001
    Figure 2024155065000001
  • Figure 2024155065000002
    Figure 2024155065000002
  • Figure 2024155065000003
    Figure 2024155065000003
Patent Text Reader

Abstract

To provide a treatment agent for producing carbon fiber-containing spun yarn that improves the strength of spun yarn obtained from carbon fibers; carbon fiber-containing spun yarn; and a method for producing carbon fiber-containing spun yarn.SOLUTION: This treatment agent for producing carbon fiber-containing spun yarn contains an epoxy compound (A).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a treatment agent for producing carbon fiber-containing spun yarn, a carbon fiber-containing spun yarn having such a treatment agent adhered thereto, and a method for producing carbon fiber-containing spun yarn using such a treatment agent. [Background technology]

[0002] Generally, carbon fiber fabrics or spun yarns made of carbon fibers are known. Carbon fibers are widely used in various fields such as building materials and transportation equipment as carbon fiber composite materials or flame-retardant materials combined with matrix resins such as epoxy resins. For example, carbon fibers are produced through a process of spinning acrylic fibers as a carbon fiber precursor, a process of drawing the fibers, a process of flame-retarding, and a carbonization process.

[0003] Conventionally, a treatment agent is known as disclosed in Patent Document 1. The treatment agent disclosed contains a (poly)oxyalkylene derivative having a number average molecular weight of 30,000 or less, and an ester compound, and is used for producing a carbon fiber-containing spun yarn. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 7140438 Summary of the Invention [Problem to be solved by the invention]

[0005] However, there is a problem in that the strength of the spun yarn obtained from the carbon fiber to which the treatment agent has been applied is low. There has been a demand for a treatment agent for producing a carbon fiber-containing spun yarn that can further improve the strength of the spun yarn obtained from the carbon fiber. [Means for solving the problem]

[0006] As a result of research aimed at solving the above problems, the present inventors have found that a treatment agent for producing carbon fiber-containing spun yarn containing an epoxy compound (A) is preferably used. Various aspects for solving the above problems will be described below.

[0007] The treatment agent for producing a carbon fiber-containing spun yarn according to the first aspect is Contains diphenylmethane as the main structure It is characterized by containing an epoxy compound (A). A second aspect is the treatment agent for producing a carbon fiber-containing spun yarn according to the first aspect, wherein the epoxy compound (A) has at least one selected from a bisphenol A skeleton and a bisphenol F skeleton.

[0008] Aspect 3 is the treatment agent for producing a carbon fiber-containing spun yarn according to Aspect 1 or 2, in which the content of the epoxy compound (A) in the non-volatile matter of the treatment agent is 5 to 90 mass %. A fourth aspect is the treatment agent for producing a carbon fiber-containing spun yarn according to any one of the first to third aspects, further comprising a nonionic surfactant (B), and the content of the nonionic surfactant (B) in the non-volatile matter of the treatment agent is 5 to 60 mass %.

[0009] A fifth aspect relates to the treating agent for producing a carbon fiber-containing spun yarn according to any one of the first to fourth aspects, further comprising the following ester compound (C), and the content of the ester compound (C) in the non-volatile matter of the treating agent is 5 to 50 mass %.

[0010] Ester compound (C): An ester compound consisting of a monohydric aliphatic alcohol and a monobasic carboxylic acid. A sixth aspect is the treatment agent for producing a carbon fiber-containing spun yarn according to any one of the first to third aspects, further comprising a nonionic surfactant (B), and The followingThe composition contains an ester compound (C), and when the total content of the epoxy compound (A), the nonionic surfactant (B), and the ester compound (C) is taken as 100 mass%, the composition contains the epoxy compound (A) in an amount of 5 to 90 mass%, the nonionic surfactant (B) in an amount of 5 to 60 mass%, and the ester compound (C) in an amount of 5 to 50 mass%. Ester compound (C): An ester compound consisting of a monohydric aliphatic alcohol and a monobasic carboxylic acid.

[0011] The carbon fiber-containing spun yarn of the seventh aspect is characterized in that the treating agent according to any one of the first to sixth aspects is adhered to the carbon fiber-containing spun yarn. A method for producing a carbon fiber-containing spun yarn according to an eighth aspect is characterized by including a step of adhering the treating agent according to any one of the first to sixth aspects to short carbon fibers. Effect of the Invention

[0012] According to the present invention, it is possible to improve the strength of a spun yarn obtained from carbon fibers to which a treatment agent for producing a carbon fiber-containing spun yarn has been applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] First Embodiment A first embodiment of the treatment agent for producing carbon fiber-containing spun yarn of the present invention (hereinafter, referred to as the treatment agent) will be described below. The treatment agent of this embodiment contains the following epoxy compound (A), and may further contain a nonionic surfactant (B) and an ester compound (C).

[0014] (Epoxy compound (A)) The epoxy compound (A) is a compound having an epoxy group in the molecule. The epoxy compound (A) may be either a monoepoxy compound having one epoxy group in the molecule or a multifunctional epoxy compound having two or more epoxy groups in the molecule.

[0015] The main chain may be, for example, diphenylmethane, more specifically, bisphenol. Specific examples of bisphenol include bisphenol A, AP, AF, B, BP, C, E, F, G, M, S, P, PH, TMC, and Z. Among these, from the viewpoint of further improving the strength of the spun yarn, the epoxy compound (A) is preferably one having a bisphenol A skeleton and a bisphenol F skeleton. In the present invention, the epoxy compound (A) is a compound containing a diphenylmethane skeleton as the main skeleton. Examples of the compound containing a diphenylmethane skeleton as the main skeleton include compounds containing at least one skeleton selected from bisphenol A skeleton, bisphenol F skeleton, diaminodiphenylmethane skeleton, and cresol novolac skeleton. Hereinafter, compounds other than the epoxy compound (A) of the present invention are given as reference examples.

[0016] Specific examples of the epoxy compound (A) include amine-type epoxy compounds such as polymers of polyoxyalkylene-added p-tert-butylphenol monoglycidyl ether, bisphenol A diglycidyl ether, resorcinol diglycidyl ether, polypropylene glycol diglycidyl ether, trimethylolpropane polyglycidyl ether, pentaerythritol polyglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, polyethylene glycol diglycidyl ether, polyglycerol polyglycidyl ether, alkyl glycidyl ether, polyoxyalkylene-added alkyl glycidyl ether, phenyl glycidyl ether, polyoxyalkylene-added phenyl glycidyl ether, triglycidylamine, and tetraglycidylamine.

[0017] In addition, as the epoxy compound (A), a commercially available product may be used. Specific examples of commercially available products include jER828 (manufactured by Mitsubishi Chemical Corporation), jER834 (manufactured by Mitsubishi Chemical Corporation), jER1001 (manufactured by Mitsubishi Chemical Corporation), jER1002 (manufactured by Mitsubishi Chemical Corporation), Epotohto YD-128 (manufactured by Nippon Steel Chemical & Material Co., Ltd.), Epotohto YD-011 (manufactured by Nippon Steel Chemical & Material Co., Ltd.), Epotohto YD-012 (manufactured by Nippon Steel Chemical & Material Co., Ltd.), Sumiepoxy ELM-434 (manufactured by Sumitomo Chemical Co., Ltd.), EPICRON N-660 (manufactured by DIC Corporation), etc.

[0018] These epoxy compounds (A) may be used alone or in appropriate combination of two or more. The content of the epoxy compound (A) in the non-volatile content of the treatment agent is preferably 3 to 100% by mass, more preferably 5 to 90% by mass. By specifying the content within this range, the effect of the present invention can be further improved. Any combination of the upper and lower limits above is also conceivable. The non-volatile content refers to the treatment agent that has been heat-treated at 105°C for 2 hours to thoroughly remove volatile components. Hereinafter, the definition of the non-volatile content will adopt the same conditions.

[0019] (Nonionic surfactant (B)) The treatment agent may further contain a nonionic surfactant (B). By containing the nonionic surfactant (B) in the treatment agent, it is possible to reduce fuzz in the spun yarn obtained from the carbon fiber to which the treatment agent has been applied.

[0020] Examples of the nonionic surfactant (B) include compounds having a (poly)oxyalkylene structure in which alkylene oxides are added to alcohols or carboxylic acids, ether / ester compounds having a (poly)oxyalkylene structure in which alkylene oxides are added to ester compounds of carboxylic acids and polyhydric alcohols, compounds in which alkylene oxides are added to natural fats and oils or compounds in which such compounds are esterified with carboxylic acids, amine compounds such as compounds having a (poly)oxyalkylene structure in which alkylene oxides are added to primary organic amines, compounds having a (poly)oxyalkylene structure in which alkylene oxides are added to fatty acid amides, amide compounds in which an amine compound is condensed with a carboxylic acid, partial ester compounds of carboxylic acids and polyhydric alcohols, etc.

[0021] Specific examples of alcohols used as raw materials for the nonionic surfactant (B) include, for example, (1) linear alkyl alcohols such as methanol, ethanol, propanol, butanol, pentanol, hexanol, octanol, nonanol, decanol, undecanol, dodecanol, tridecanol, tetradecanol, pentadecanol, hexadecanol, heptadecanol, octadecanol, nonadecanol, eicosanol, heneicosanol, docosanol, tricosanol, tetracosanol, pentacosanol, hexacosanol, heptacosanol, octacosanol, nonacosanol, and triacontanol; (2) isopropanol, isobutanol, isohexanol, 2-ethylhexanol, isononanol, isodecanol, isododecanol, isotridecanol, isotetradecanol, isotriacontanol, and isoheptadecanol; (3) linear alkenyl alcohols such as tetradecenol, hexadecenol, heptadecenol, octadecenol, and nonadecenol; (4) branched alkenyl alcohols such as isohexadecenol and isooctadecenol; (5) cyclic alkyl alcohols such as cyclopentanol and cyclohexanol; and (6) aromatic alcohols such as phenol, nonylphenol, benzyl alcohol, monostyrenated phenol, distyrenated phenol, and tristyrenated phenol.

[0022] Specific examples of carboxylic acids used as raw materials for the nonionic surfactant (B) include: (1) linear alkyl carboxylic acids such as octylic acid, nonanoic acid, decanoic acid, undecanoic acid, dodecanoic acid, tridecanoic acid, tetradecanoic acid, pentadecanoic acid, hexadecanoic acid, heptadecanoic acid, octadecanoic acid, nonadecanoic acid, eicosanoic acid, heneicosanoic acid, and docosanoic acid; (2) branched alkyl carboxylic acids such as 2-ethylhexanoic acid, isododecanoic acid, isotridecanoic acid, isotetradecanoic acid, isohexadecanoic acid, and isooctadecanoic acid; (3) linear alkenyl carboxylic acids such as octadecenoic acid, octadecadienoic acid, and octadecatrienoic acid; (4) aromatic carboxylic acids such as benzoic acid; and (5) hydroxycarboxylic acids such as ricinoleic acid.

[0023] The alkylene oxide used as a raw material for forming the (poly)oxyalkylene structure of the nonionic surfactant (B) is preferably an alkylene oxide having 2 to 4 carbon atoms. Specific examples of alkylene oxide include, for example, ethylene oxide, propylene oxide, and butylene oxide. The number of moles of alkylene oxide added is appropriately set, but is preferably 0.1 to 150 moles, more preferably 1 to 100 moles, and even more preferably 2 to 50 moles. Any combination of the above upper and lower limits is also possible. The number of moles of alkylene oxide added indicates the number of moles of alkylene oxide per mole of the compound to be added in the raw material. The alkylene oxide may be one type of alkylene oxide used alone, or two or more types of alkylene oxides may be used in appropriate combination. When two or more types of alkylene oxides are used, the addition form may be any of block addition, random addition, and a combination of block addition and random addition, and is not particularly limited.

[0024] Specific examples of polyhydric alcohols used as a raw material for the nonionic surfactant (B) include ethylene glycol, propylene glycol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2-methyl-1,2-propanediol, 1,5-pentanediol, 1,6-hexanediol, 2,5-hexanediol, 2-methyl-2,4-pentanediol, 2,3-dimethyl-2,3-butanediol, glycerin, diglycerin, 2-methyl-2-hydroxymethyl-1,3-propanediol, trimethylolpropane, sorbitan, pentaerythritol, and sorbitol.

[0025] Specific examples of the aliphatic amine or primary organic amine used as a raw material for the nonionic surfactant (B) include methylamine, ethylamine, butylamine, octylamine, laurylamine, octadecylamine (stearylamine), octadecenylamine, and coconut amine.

[0026] Specific examples of fatty acid amides used as raw materials for the nonionic surfactant (B) include, for example, octylic acid amide, lauric acid amide, palmitic acid amide, stearic acid amide, oleic acid amide, behenic acid amide, lignoceric acid amide, amides of fatty acids and diethanolamine, and amides of fatty acids and ethyleneamine.

[0027] These nonionic surfactants (B) may be used alone or in appropriate combination of two or more kinds. The content of the nonionic surfactant (B) in the nonvolatile content of the treatment agent is preferably 3 to 70 mass%, more preferably 5 to 60 mass%. By specifying the content within this range, it is possible to further reduce the fluff of the spun yarn obtained from the carbon fiber to which the treatment agent is applied. Note that any combination of the above upper and lower limits is also possible.

[0028] (Ester Compound (C)) The ester compound (C) used in the treatment agent of this embodiment is an ester compound composed of a monohydric aliphatic alcohol and a monobasic carboxylic acid. By using this ester compound (C), it is possible to reduce the fluff of the spun yarn obtained from the carbon fiber to which the treatment agent has been applied.

[0029] The monovalent carboxylic acid constituting the ester compound (C) may be a saturated aliphatic carboxylic acid or an unsaturated aliphatic carboxylic acid, and may be either a straight-chain or branched-chain structure.

[0030] Specific examples of saturated aliphatic carboxylic acids include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, hexanoic acid (caproic acid), octylic acid (2-ethylhexanoic acid), octanoic acid (caprylic acid), nonanoic acid, decanoic acid (capric acid), dodecanoic acid (lauric acid), tetradecanoic acid (myristic acid), hexadecanoic acid (palmitic acid), octadecanoic acid (stearic acid), isooctadecanoic acid (isostearic acid), eicosanoic acid (arachidic acid), docosanoic acid (behenic acid), and tetracosanoic acid.

[0031] Specific examples of unsaturated aliphatic carboxylic acids include crotonic acid, myristoleic acid, palmitoleic acid, oleic acid, vaccenic acid, eicosenoic acid, linoleic acid, α-linolenic acid, γ-linolenic acid, and arachidonic acid.

[0032] Specific examples of the monohydric aliphatic alcohol include the specific examples of the monohydric aliphatic alcohols among the alcohols used as raw materials for the nonionic surfactant (B) described above. These ester compounds (C) may be used alone or in combination of two or more.

[0033] In the non-volatile content of the treatment agent, the content of the ester compound (C) is preferably 3 to 60 mass%, more preferably 5 to 50 mass%. By specifying the content within this range, it is possible to further reduce the fluff of the spun yarn obtained from the carbon fiber to which the treatment agent is applied. Note that a range that combines the above upper and lower limits is also envisioned.

[0034] In the treatment agent, when the total content of the epoxy compound (A), the nonionic surfactant (B), and the ester compound (C) is 100 mass%, it is preferable that the epoxy compound (A) is contained in an amount of 5 to 90 mass%, the nonionic surfactant (B) is contained in an amount of 5 to 60 mass%, and the ester compound (C) is contained in an amount of 5 to 50 mass%. By specifying the content ratio within such a range, the effect of the present invention can be further improved. Note that a range in which the above upper and lower limits are arbitrarily combined is also assumed.

[0035] <Second embodiment> A second embodiment of the carbon fiber-containing spun yarn according to the present invention will be described. The carbon fiber-containing spun yarn of this embodiment is a carbon fiber-containing spun yarn to which the treatment agent of the first embodiment is attached. There is no particular restriction on the amount of the treatment agent of the first embodiment (not including the solvent) attached to the carbon fiber-containing spun yarn, but from the viewpoint of further improving the effects of the present invention, it is preferable that the amount of the treatment agent of the first embodiment (not including the solvent) attached to the carbon fiber-containing spun yarn is 0.1 mass % or more and 10 mass % or less.

[0036] The carbon fibers constituting the carbon fiber-containing spun yarn are not particularly limited, but examples thereof include PAN-based carbon fibers obtained from acrylic fibers as a raw material, pitch-based carbon fibers obtained from pitch as a raw material, recycled carbon fibers extracted from carbon fiber composite materials by chemical decomposition or pyrolysis, and carbon fibers obtained from polyester fibers, polyethylene resins, phenolic resins, cellulose resins, lignin resins, etc.

[0037] The length of the carbon fiber is not particularly limited, and may be a short fiber having a length of 1 cm or less, also called a short cut, or a short fiber having a length of 3 cm to 7 cm, also called a staple. It may also be a long fiber having a length of 10 cm or more, also called a filament. When carbon fiber is recycled from a carbon fiber fabric used in a composite material, a large amount of short fiber is contained. In addition, carbon fiber obtained by mixing and spinning two or more different types of staple may be used. Examples of synthetic fibers to be spun include polyamide fibers such as nylon 6, nylon 66, polyamide 9T, and polyamide 10, polypropylene, and polyethylene. The ratio of synthetic fiber to carbon fiber when spinning is not particularly limited, but is preferably 10:90 to 90:10, and more preferably 20:80 to 80:20. When spinning, the treatment agent may be applied either before or after the carbon fiber and synthetic fiber are spun.

[0038] The method for producing a carbon fiber-containing spun yarn includes an application step of applying the treatment agent of the first embodiment to carbon fibers, and a carding step of aligning the fiber direction of the carbon fibers that have been subjected to the application step to form a string-like sliver. The method also includes a drawing step of drawing several slivers together. The drawing step is performed by drawing several slivers together into one while conveying them with the rollers of a drawing frame. The method also includes a roving step of drawing the sliver that has been subjected to the drawing step and winding it into a roving, a ring spinning step of drawing the roving and winding it into a spun yarn, and a winding step of winding the spun yarn into a package while adjusting the quality of the spun yarn. By performing each of these steps in order, a carbon fiber-containing spun yarn can be produced.

[0039] In the application step, the treatment agent of the first embodiment is applied to the carbon fiber by oiling. As the oiling method, for example, a known oiling method can be applied using an aqueous liquid containing the treatment agent of the first embodiment and water, an aqueous solution obtained by further diluting the aqueous liquid, or an organic solvent solution. Examples of known oiling methods include a dipping method, a spray method, a roller method, and a guide oiling method using a metering pump.

[0040] The aqueous liquid can be prepared by a known mechanical emulsification method using a homomixer, homogenizer, or the like. The timing of the imparting step is not particularly limited as long as it is performed before the drawing step.

[0041] The effects of the treatment agent and carbon fiber-containing spun yarn of this embodiment will be described. (1) The treatment agent of this embodiment is constituted by blending an epoxy compound (A). Therefore, the strength of the carbon fiber-containing spun yarn to which the treatment agent is applied can be improved. In addition, the fluff of the carbon fiber-containing spun yarn to which the treatment agent is applied can be reduced.

[0042] (2) When the treatment agent contains a predetermined amount of the nonionic surfactant (B) or the ester compound (C), the fuzz of the carbon fiber-containing spun yarn to which the treatment agent is applied can be further reduced. The above embodiment may be modified as follows: The above embodiment and the following modifications may be combined with each other to the extent that no technical contradiction occurs.

[0043] The treatment agent of the above embodiment may further contain components that are typically used in treatment agents, such as a stabilizer for maintaining the quality of the treatment agent, an antistatic agent, a binder, an antioxidant, and an ultraviolet absorber, within the scope of not impairing the effects of the present invention. EXAMPLES

[0044] In the following, examples will be given to more specifically describe the configuration and effects of the present invention, but the present invention is not limited to these examples. In the following examples and comparative examples, parts means parts by mass, and % means % by mass.

[0045] Test category 1 (preparation of treatment agent) As shown in Table 1, the treatment agent of each example was prepared by gradually adding water or an organic solvent to an epoxy compound (A), a nonionic surfactant (B), an ester compound (C), and other components (D) while stirring so that the solids concentration was 30%.

[0046] [Table 1]

[0047] [Table 2]

[0048] [Table 3] Test Category 2 (Manufacturing of Carbon Fiber-Containing Spun Yarn) Using the treatment agent prepared in Test Section 1, a carbon fiber-containing spun yarn was produced.

[0049] The aqueous solution or organic solvent solution of each treatment agent thus prepared was further diluted with water to obtain a 1 to 4% aqueous solution of each treatment agent. This aqueous solution was applied to short carbon fibers having a fiber length of 45 mm by a spray oiling method. The fibers were then dried in a hot air dryer at 105°C for 60 minutes to obtain treated short carbon fibers to which the treatment agent was applied. The treated short carbon fibers thus obtained were conditioned overnight in an atmosphere at 25°C and 65% RH and then subjected to evaluation. In addition, in Example 48 and the like, the synthetic fibers shown in the table were blended in a predetermined ratio.

[0050] Next, drawing and roving were carried out under the following drawing conditions. The short carbon fibers obtained as described above were combed by a carding machine to obtain a fiber bundle of 10 g / m. Next, one fiber bundle was elongated 5.1 times by a first drawing frame to obtain a fiber bundle of 1.96 g / m. Furthermore, two of these fiber bundles were combined and drawn 3.2 times by a second drawing frame to obtain one fiber bundle, and further, two of these fiber bundles were combined and drawn 2.0 times by a third drawing frame to obtain one fiber bundle. This fiber bundle was spun by a roving frame at a drawing rate of 12 times and a twist rate of 180 times / m to obtain a spun yarn (roving yarn) of 100 tex.

[0051] Test category 3 (strength of roving yarn) The strength of the roving yarn produced in Test Section 2 was evaluated by measuring the strength at the time of breakage using a tensile strength and elongation tester. First, the roving yarn produced in Test Section 2 was stretched in the tensile strength and elongation tester with a grip length of 10 cm and a pulling speed of 1 cm / min, and the test force at the time of breakage of the roving yarn was measured. Evaluation was made according to the following criteria.

[0052] Evaluation criteria for strength of roving yarn ◎(Good): 3.0kg or more ○(OK): 2.0kg or more, less than 3.0kg × (Not acceptable): Less than 2.0 kg Test category 4 (lint) The appearance of the roving yarn produced in Test Section 2 was visually inspected and evaluated for fuzz. The amount of fuzz on 10 m of the roving yarn was measured and evaluated according to the following criteria.

[0053] -Fuzziness evaluation criteria ◎◎(Excellent): No fluff at all ◎ (Good): Fuzz is occasionally observed, but there is no problem in practical use. ○(Acceptable): Some fluff is observed, but there is no problem with practical use. × (Not acceptable): If a lot of fluff is generated and the product cannot be used. As is clear from the evaluation results of each Example and each Comparative Example in the above table, the treatment agent of the present invention can improve the strength of the carbon fiber-containing spun yarn to which the treatment agent is applied, and can also reduce the fuzz of the carbon fiber-containing spun yarn to which the treatment agent is applied.

Claims

1. A treatment agent for producing carbon fiber-containing spun yarn, comprising an epoxy compound (A).

2. 2. The treatment agent for producing a carbon fiber-containing spun yarn according to claim 1, wherein the epoxy compound (A) has at least one skeleton selected from a bisphenol A skeleton and a bisphenol F skeleton.

3. 2. The treatment agent for producing carbon fiber-containing spun yarn according to claim 1, wherein the content of the epoxy compound (A) in the non-volatile matter of the treatment agent is 5 to 90 mass %.

4. Further, it contains a nonionic surfactant (B), The treatment agent for producing carbon fiber-containing spun yarn according to claim 1, wherein the content of the nonionic surfactant (B) in the nonvolatile matter of the treatment agent is 5 to 60 mass %.

5. Further, the composition contains the following ester compound (C):

2. The treatment agent for producing carbon fiber-containing spun yarn according to claim 1, wherein the content of the ester compound (C) in the non-volatile matter of the treatment agent is 5 to 50 mass %. Ester compound (C): An ester compound consisting of a monohydric aliphatic alcohol and a monobasic carboxylic acid.

6. Further, the composition contains a nonionic surfactant (B) and an ester compound (C), 2. The treatment agent for producing a carbon fiber-containing spun yarn according to claim 1, wherein the treatment agent contains the epoxy compound (A) in an amount of 5 to 90 mass%, the nonionic surfactant (B) in an amount of 5 to 60 mass%, and the ester compound (C) in an amount of 5 to 50 mass%, assuming that the total content of the epoxy compound (A), the nonionic surfactant (B), and the ester compound (C) is 100 mass%.

7. A carbon fiber-containing spun yarn having the treating agent according to any one of claims 1 to 6 adhered thereto.

8. A method for producing a carbon fiber-containing spun yarn, comprising a step of adhering the treating agent according to any one of claims 1 to 6 to short carbon fibers.

Citation Information

Patent Citations

  • Treatment agent for producing carbon fiber spun yarn, and carbon fiber spun yarn

    JP7140438B1