Method for manufacturing plating film

By forming a metal oxide layer and sequentially applying heat treatments and copper plating on glass substrates, the method addresses adhesion and coverage issues, resulting in a cost-effective and efficient plating process for high-frequency circuitry.

JP2024155434AActive Publication Date: 2024-10-31C UYEMURA & CO LTD

Patent Information

Application Number
JP2023070142
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-31
Estimated Expiration
2043-04-21

AI Technical Summary

Technical Problem

Conventional electroless copper plating processes struggle to achieve sufficient adhesion and coverage on glass substrates, leading to poor performance in forming circuits, and copper sputtering is costly and unsuitable for mass production.

Method used

A method involving forming a metal oxide layer on a glass substrate, followed by heat treatment, electroless copper plating, and additional heat treatment, culminating in electrolytic copper plating, to enhance adhesion and deposition properties.

Benefits of technology

The method produces a plating film with excellent adhesion to glass substrates, suitable for high-frequency applications, and avoids the limitations of copper sputtering by ensuring uniform coverage and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155434000001_ABST
    Figure 2024155434000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a plating film capable of manufacturing a plating film that exerts preferable adhesion to a glass substrate.SOLUTION: A method for manufacturing a plating film includes: a step (1) of forming a metal oxide layer at a surface of a glass substrate; a step (2) of performing first heat treatment after the step (1); a step (3) of forming an electroless copper plating film on the metal oxide layer after the step (2); a step (4) of performing second heat treatment after the step (3); and a step (5) of forming an electrolytic copper plating film on the electroless copper plating film after the step (4).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a plating film. [Background technology]

[0002] The core materials of conventional printed circuit boards and package boards are mainly made of a mixture of resin and glass cloth. For conventional materials, the undercoat film for forming circuits by electrolytic copper plating has been made using an electroless copper plating process. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-256122 A Summary of the Invention [Problem to be solved by the invention]

[0004] As electronic devices become faster in communication speed, the fields of printed circuit boards and package boards are becoming increasingly dense, and various specification requirements, such as warpage, thermal expansion coefficient, smoothness, dielectric constant, and cost, are becoming more stringent. Since high frequencies are used to increase communication speeds, the smoothness of the board is important. For this reason, glass, which has excellent smoothness, is being used as the core material for boards, instead of the conventional mixed material of resin and glass cloth (for example, Patent Document 1).

[0005] In order to perform electrolytic copper underplating on a glass substrate, it is difficult to obtain sufficient deposition and adhesion with the conventional electroless copper plating process. Thus, even if the conventional process is applied to a glass substrate having excellent smoothness, it is difficult to obtain a plating film exhibiting good adhesion. Therefore, when forming a circuit on a glass substrate, a copper sputtering process is used for the undercoat film, rather than an electroless copper plating process. However, the copper sputtering process has poor coverage in through holes present in printed circuit boards and package boards, and the inventors' investigation has revealed that the copper plating may not be deposited in the subsequent electrolytic copper plating process or may not have sufficient adhesion to the glass substrate. Furthermore, the sputtering device is expensive and not suitable for mass production.

[0006] As described above, as a result of the investigations conducted by the present inventors, it has become clear that there is room for improvement in the conventional techniques in terms of producing a plating film that exhibits good adhesion to a glass substrate.

[0007] An object of the present invention is to solve the above-mentioned problems newly discovered by the present inventors, and to provide a method for producing a plating film that can produce a plating film that exhibits good adhesion to a glass substrate. [Means for solving the problem]

[0008] The present invention (1) comprises a step of forming a metal oxide layer on a surface of a glass substrate; A step (2) of performing a first heat treatment after the step (1); After the step (2), a step (3) of forming an electroless copper plating film on the metal oxide layer; A step (4) of performing a second heat treatment after the step (3); and After the step (4), a step (5) of forming an electrolytic copper plating film on the electroless copper plating film. Includes The present invention relates to a method for producing a plating film.

[0009] The present invention (2) relates to the method for producing a plating film according to the present invention (1), wherein the step (1) includes the following steps (1-2) and (1-3), which are carried out in this order: Step (1-2): A catalyst is applied to the surface of a glass substrate. Step (1-3): A metal oxide layer is formed on the surface of a glass substrate.

[0010] The present invention (3) relates to the method for producing a plating film according to the present invention (1) or (2), in which the metal oxide is an oxide containing zinc.

[0011] The present invention (4) relates to the method for producing a plating film according to any one of the present inventions (1) to (3), wherein the step (1) is a step of forming a metal oxide layer using an aqueous solution containing zinc ions, nitrate ions, and an amine borane compound.

[0012] The present invention (5) relates to the method for producing a plating film according to any one of the present inventions (1) to (4), wherein the step (3) includes the following steps (3-1) and (3-2), which are performed in this order: Step (3-1): A catalyst is applied to the surface of a metal oxide layer. Step (3-2): An electroless copper plating film is formed on the heat-treated metal oxide layer.

[0013] The present invention (6) relates to the method for producing a plating film according to any one of the present inventions (1) to (5), wherein the atmosphere in which the step (4) is carried out is an inert gas atmosphere.

[0014] The present invention (7) relates to the method for producing a plating film according to any one of the present inventions (1) to (6), wherein the step (5) is a step of forming an electrolytic copper plating film using an electrolytic copper plating bath having a pH of 2.0 or less. Effect of the Invention

[0015] According to the present invention, the method for producing a plating film includes the steps of: (1) forming a metal oxide layer on the surface of a glass substrate; (2) performing a first heat treatment after the step (1); (3) forming an electroless copper plating film on the metal oxide layer after the step (2); (4) performing a second heat treatment after the step (3); and (5) forming an electrolytic copper plating film on the electroless copper plating film after the step (4). Therefore, a plating film that exhibits good adhesion to a glass substrate can be produced. [Brief description of the drawings]

[0016] [Figure 1] 1 is a photograph showing an example of a plating film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The method for producing a plating film of the present invention comprises the steps of: (1) forming a metal oxide layer on a surface of a glass substrate; A step (2) of performing a first heat treatment after the step (1); After the step (2), a step (3) of forming an electroless copper plating film on the metal oxide layer; A step (4) of performing a second heat treatment after the step (3); and After the step (4), a step (5) of forming an electrolytic copper plating film on the electroless copper plating film. This makes it possible to produce a plating film that exhibits good adhesion to the glass substrate. The method for producing a plating film of the present invention is a method for carrying out the steps (1) to (5) in this order, but other steps may be included between each step as long as the steps (1) to (5) are carried out in this order (step (1), step (2), step (3), step (4), step (5)). After each step described below, ordinary post-treatment operations such as washing with water and drying can be carried out.

[0018] The reason why the above-mentioned effects are obtained by the above-mentioned method for producing a plating film is presumed to be as follows. The adhesion between the glass substrate and the metal oxide can be further strengthened by carrying out step (1) of forming a metal oxide layer on the surface of the glass substrate, and step (2) of performing a first heat treatment after step (1). Furthermore, the adhesion between the metal oxide layer and the electroless copper plating film can be further strengthened by carrying out step (3) of forming an electroless copper plating film on the metal oxide layer after step (2), and step (4) of performing a second heat treatment after step (3). The plating film formed on the surface of the glass substrate by the above steps (1) to (4) has strong adhesion between the glass substrate and the metal oxide, and between the metal oxide layer and the electroless copper plating film, and has good adhesion to the glass substrate, making it highly suitable as a base for an electrolytic copper plating film. By forming an electrolytic copper plating film on the plating film formed on the surface of the glass substrate by the above steps (1) to (4), a plating film that exhibits good adhesion to the glass substrate can be produced. Furthermore, in the method for producing a plating film in which the steps (1) to (5) are carried out in this order, a metal oxide layer and an electroless copper plating film can be uniformly formed regardless of the shape of the workpiece, and therefore the method has excellent deposition and adhesion to the surface of a glass substrate and into through-holes present in the substrate.

[0019] In this specification, the surface of a glass substrate means on the glass substrate, and other similar expressions, such as the surface of a metal oxide layer, also mean on the metal oxide layer in the same sense.

[0020] <Glass substrate> The glass substrate is not particularly limited, and a known glass substrate used as a circuit substrate for various electronic devices can be used. The glass substrate is preferably a base material for forming wiring, for example, a glass substrate used in the manufacture of electronic devices that are becoming faster in communication speed.

[0021] The glass substrate is an amorphous substrate made of a silica network, and may contain a network former (network-forming oxide) such as aluminum, boron, or phosphorus, or a network modifier (network-modifying oxide) such as an alkali metal, alkaline earth metal, or magnesium.

[0022] Specific examples of the glass constituting the glass substrate include soda glass, soda lime glass, non-alkali glass, quartz glass, etc. The glass substrate may preferably be made of aluminosilicate glass or the like, which is used as reinforced glass.

[0023] The glass content in 100% by mass of the glass substrate is preferably 90% by mass or more, more preferably 95% by mass or more, further preferably 98% by mass or more, and may be 100% by mass, which tends to more suitably obtain the effect. In this specification, the glass content in the glass substrate is measured in terms of oxide using an inductively coupled plasma (ICP) emission spectrometer.

[0024] The thickness of the glass substrate is not particularly limited and can be appropriately set depending on the purpose, but is usually about 200 to 1000 μm.

[0025] <Process (1)> In step (1), a metal oxide layer is formed on the surface of a glass substrate. Step (1) is not particularly limited as long as it is a step of forming a metal oxide layer on the surface of a glass substrate, but may be, for example, a step including the following steps (1-1) to (1-3), for example, a step including the following steps (1-1) to (1-3) and performed in the following order of steps (1-1), (1-2), and (1-3). Among these, it is preferable to include the following steps (1-2) and (1-3), and it is more preferable to include the following steps (1-2) and (1-3) and perform the following steps (1-2) and (1-3) in the following order.

[0026] <<Process (1-1)>> In step (1-1), contamination (foreign matter) is removed from the surface of the glass substrate, which removes organic residues adsorbed on the surface of the glass substrate, increases the number of OH groups on the surface of the glass substrate, and improves hydrophilicity.

[0027] In step (1-1), for example, the surface of the glass substrate is washed with at least one selected from the group consisting of an organic solvent, an alkaline solution, and an acidic solution. These may be used alone or in combination of two or more. By washing the surface of the glass substrate with an organic solvent, organic residues adsorbed on the surface of the glass substrate are removed. In addition, by washing the surface of the glass substrate with an alkaline solution or an acidic solution, organic residues adsorbed on the surface of the glass substrate are removed, and the number of OH groups on the surface of the glass substrate is increased, improving hydrophilicity.

[0028] As the organic solvent, for example, methanol, ethanol, acetone, ethyl acetate, hexane, etc. can be used. These may be used alone or in combination of two or more kinds.

[0029] The conditions for the glass cleaning treatment with an organic solvent are not particularly limited.

[0030] As the alkaline solution, for example, a NaOH solution, a KOH solution, etc. can be used. These may be used alone or in combination of two or more kinds.

[0031] The conditions for the glass cleaning treatment with the alkaline solution are not particularly limited.

[0032] Examples of the acidic solution that can be used include sulfuric acid, hydrochloric acid, nitric acid, hydrogen peroxide / sulfuric acid, hydrogen peroxide / nitric acid, etc. These may be used alone or in combination of two or more kinds.

[0033] The conditions for the glass cleaning treatment with the acidic solution are not particularly limited.

[0034] <<Process (1-2)>> In step (1-2), a catalyst (catalytic metal) is applied to the surface of the glass substrate. This activates the surface of the glass substrate, making it possible to more suitably form a metal oxide layer on the surface of the glass substrate. In addition, by carrying out step (1-2), it becomes possible to form a metal oxide layer without roughening the surface of the glass substrate. This makes it possible to form a wiring pattern with a fine pitch in circuit formation, and also reduces the effect on transmission loss in the high frequency band. In addition, fluorides are usually used to roughen the surface of the glass substrate, but the use of fluorides is inappropriate from the standpoint of human safety and environmental protection. By carrying out step (1-2), it becomes possible to form a metal oxide layer on the surface of the glass substrate without using fluorides.

[0035] The catalytic metal is not particularly limited as long as it is a metal having catalytic activity for the formation of a metal oxide layer in a subsequent step, and examples thereof include Ag, Pd, Pt, and Au. These may be used alone or in combination of two or more. Among them, Pd and Ag are preferred, and Pd is more preferred.

[0036] Since it is important to apply a catalyst (catalytic metal) to the surface of the glass substrate, the method of applying the catalyst to the surface of the glass substrate is not particularly limited, and examples thereof include a method of adsorbing metal ions onto the glass substrate and reducing them to metal, and a method of adsorbing metal colloid onto the glass substrate. These methods may be used alone or in combination of two or more. For the same reason, the catalyst application treatment conditions are not particularly limited.

[0037] A specific method for step (1-2) may include, for example, performing cleaner conditioning (promoting catalyst adsorption and allowing the catalyst to be uniformly adsorbed), pre-dip, catalyst application (activator), and activation treatment (accelerator) in this order.

[0038] <<Process (1-3)>> In the step (1-3), a metal oxide layer is formed on the surface of the glass substrate, and the metal oxide layer serves as an intermediate layer between the glass and the electroless copper plating, thereby easily improving the adhesion between the glass and the electroless copper plating. In the step (1-3), it is preferable to form a metal oxide layer on the surface of the glass substrate to which the catalyst (catalytic metal) has been applied, as this tends to produce a more suitable effect.

[0039] The metal oxide is preferably an oxide containing zinc, and examples thereof include zinc oxide, or an oxide of an alloy containing zinc and at least one metal selected from the group consisting of titanium, aluminum, silicon, tin, zirconium, nickel, indium, vanadium, chromium, iron, manganese, cobalt, and copper. These may be used alone or in combination of two or more. Among them, an oxide of an alloy containing zinc and at least one metal selected from the group consisting of indium, titanium, silicon, tin, manganese, and cobalt, or zinc oxide is preferred, and zinc oxide is more preferred.

[0040] The thickness of the metal oxide layer is preferably 0.05 to 0.5 μm, and more preferably 0.1 to 0.3 μm, which tends to improve production efficiency and provide good adhesion.

[0041] The metal oxide layer is formed, for example, by immersing a glass substrate to which a catalyst has been applied in a treatment liquid for forming a metal oxide layer. The treatment liquid for forming a metal oxide layer is preferably an aqueous solution containing zinc ions, nitrate ions, and an amine borane compound.

[0042] As the zinc ion source, a water-soluble zinc salt may be used, such as zinc nitrate, zinc sulfate, zinc chloride, zinc acetate, zinc phosphate, zinc pyrophosphate, zinc carbonate, etc. Among these, zinc nitrate is preferred. These may be used alone or in combination of two or more.

[0043] As the nitrate ion source, nitric acid, water-soluble nitrates, etc. may be used, for example, nitric acid, zinc nitrate, ammonium nitrate, sodium nitrate, potassium nitrate, lithium nitrate, urea nitrate, etc. are listed. Among them, zinc nitrate is preferable. These may be used alone or in combination of two or more kinds. It is preferable to use zinc nitrate alone as an ion source for both zinc ions and nitrate ions.

[0044] The concentrations of zinc ions and nitrate ions in the metal oxide layer forming treatment liquid can be adjusted over a wide range, but if either one of the ion concentrations is too low, a metal oxide film cannot be formed, and if either one of the ion concentrations is too high, a metal hydroxide film is likely to be formed and the purity of the metal oxide film is likely to decrease. Therefore, the respective concentrations of zinc ions and nitrate ions are preferably within the range of about 0.001 mol / l to 0.5 mol / l (0.065 to 32.7 g / l in terms of zinc content), and more preferably within the range of about 0.01 mol / l to 0.2 mol / l (0.65 to 13 g / l in terms of zinc content).

[0045] The amine borane compound may be any water-soluble compound, such as dimethylamine borane, trimethylamine borane, etc. These may be used alone or in combination of two or more. Among these, dimethylamine borane is preferred.

[0046] The concentration of the amine borane compound in the metal oxide layer forming treatment liquid is preferably 0.3 to 20 g / L, more preferably 0.5 to 5 g / L, which tends to improve production efficiency and provide good metal oxide precipitation properties.

[0047] The pH of the metal oxide layer forming treatment liquid is preferably 3.0 to 7.0, and more preferably 4.0 to 7.0, which tends to improve production efficiency and provide good metal oxide precipitation properties.

[0048] The temperature of the metal oxide forming treatment is preferably 50 to 90° C., more preferably 60 to 85° C. This allows the decomposition reaction rate of the amine borane compound to be within an appropriate range, and tends to result in good deposition properties of the metal oxide.

[0049] The time for the metal oxide formation treatment is preferably 2 to 180 minutes, more preferably 5 to 60 minutes, and even more preferably 10 to 30 minutes. If it is 2 minutes or more, the metal oxide layer will have a sufficient thickness, and there is a tendency that sufficient adhesion between the glass substrate and the metal oxide can be obtained. On the other hand, while it usually takes more than 180 minutes to form a metal oxide layer, in the present invention, by using an aqueous solution containing zinc ions, nitrate ions, and an amine borane compound as the treatment liquid for forming a metal oxide layer, the treatment time can be shortened, and the metal oxide layer can be formed with high production efficiency and cost advantage.

[0050] The above steps (1-2) and (1-3) make it possible to form a metal oxide layer on the surface of a glass substrate without using fluoride. The fluorine content in the metal oxide layer is preferably 0.1% by mass or less, more preferably 0.01% by mass or less, and even more preferably none (0% by mass), based on 100% by mass of the metal oxide layer. This tends to produce a more favorable effect. In this specification, the fluorine content is measured using a fluoride ion electrode.

[0051] The plating film manufacturing method of the present invention does not require the use of fluoride, and therefore does not require a step of removing fluorine from the metal oxide layer. In other words, since the plating film manufacturing method of the present invention does not include a step of removing fluorine from the metal oxide layer, a plating film that exhibits good adhesion to a glass substrate can be manufactured with high production efficiency.

[0052] <Process (2)> In step (2), a first heat treatment is performed after step (1). Specifically, in step (2), a first heat treatment is performed on the glass substrate obtained in step (1) and having a metal oxide layer formed on its surface. As a result, some of the metal hydroxides that remained in the metal oxide layer formation in step (1) become metal oxides through a dehydration reaction, and chemical bonds are formed between the glass substrate and the metal oxide through condensation of OH groups, thereby making it possible to further strengthen the adhesion between the glass substrate and the metal oxide.

[0053] The atmosphere in which step (2) is carried out is not particularly limited, but it is preferable that oxygen is present in order to promote the dehydration reaction, and therefore, for example, step (2) may be carried out in the air.

[0054] The temperature of the heat treatment is preferably 100 to 800° C., more preferably 200 to 600° C., even more preferably 250 to 500° C., particularly preferably 300 to 450° C., and most preferably 300 to 350° C. If the temperature is 100° C. or higher, the dehydration reaction proceeds sufficiently, and the adhesion between the glass substrate and the metal oxide tends to be improved. If the temperature is 800° C. or lower, dimensional changes such as warping and distortion of the glass substrate tend to be more suppressed.

[0055] The heat treatment time is preferably 5 to 180 minutes, more preferably 15 to 90 minutes, and further preferably 25 to 90 minutes, which allows the dehydration reaction to proceed sufficiently without reducing production efficiency, and tends to improve the adhesion between the glass substrate and the metal oxide.

[0056] <Process (3)> In step (3), an electroless copper plating film is formed on the metal oxide layer after step (2). Specifically, in step (3), an electroless copper plating film is formed on the metal oxide layer that has been subjected to the heat treatment after step (2).

[0057] Step (3) is not particularly limited as long as it is a step of forming an electroless copper plating film on a metal oxide layer, and examples thereof include a step including the following steps (3-1) and (3-2), for example, a step including the following steps (3-1) and (3-2), which are performed in the order of the following steps (3-1) and (3-2).

[0058] <<Process (3-1)>> In step (3-1), a catalyst (catalytic metal) is applied to the surface of the metal oxide layer. This activates the surface of the metal oxide layer, making it possible to more suitably form an electroless copper plating film on the surface of the metal oxide layer. In addition, by carrying out step (3-1), it becomes possible to form an electroless copper plating film without roughening the surface of the metal oxide layer. This also reduces the effect on transmission loss in the high frequency band.

[0059] The catalytic metal is not particularly limited as long as it has catalytic activity for the formation of the electroless copper plating film in the subsequent process, and examples thereof include Cu, Ni, Ag, Pd, Pt, and Au. These may be used alone or in combination of two or more. Among them, Pd, Ag, Pd, and Pt are preferred, and Pd is more preferred.

[0060] Since it is important to apply a catalyst (catalytic metal) to the surface of the metal oxide layer, the method of applying the catalyst is not particularly limited, and for example, there is a method of substituting metal ions on the metal oxide, and after (1) substituting the metal ions, (2) the catalytic metal may be activated by immersing in a solution of a reducing agent. The composition of the catalyst application bath is also not particularly limited.

[0061] The pH of the catalyst imparting bath is preferably 3.0 to 13, and more preferably 4.0 to 7.0, which can further suppress dissolution of the metal oxide layer and further suppress deterioration of adhesion. In this specification, pH is a value measured at 25°C.

[0062] In this specification, the metal concentration and metal content are measured by an inductively coupled plasma (ICP) emission spectrometer. In addition, in this specification, the concentration of each compound in the liquid is measured by liquid chromatography (manufactured by Shimadzu Corporation).

[0063] A catalyst (catalytic metal) can be applied to the surface of the metal oxide layer by contacting the surface of the metal oxide layer with a catalyst application bath. The specific method is not particularly limited, but usually, the workpiece is immersed in the catalyst application bath. In addition, the catalyst application treatment can also be performed by spraying or applying the catalyst application bath to the surface of the material to be electroless plated.

[0064] The temperature of the catalyst application treatment is preferably 10 to 60° C., more preferably 20 to 40° C. If the temperature is 10° C. or higher, the amount of catalyst applied is sufficient, and good deposition properties of electroless copper plating tend to be obtained. If the temperature is 60° C. or lower, dissolution of the metal oxide layer can be further suppressed, and deterioration of adhesion can be further suppressed.

[0065] The time for the catalyst application treatment is preferably 10 seconds to 10 minutes, more preferably 30 seconds to 5 minutes. When it is 10 seconds or more, the amount of catalyst applied becomes sufficient, and good deposition properties of electroless copper plating tend to be obtained. When it is 10 minutes or less, dissolution of the metal oxide layer can be further suppressed, and the decrease in adhesion can be further suppressed.

[0066] (1) When activating the catalytic metal after metal ion substitution, (2) as the reducing agent, for example, dimethylamine borane, trimethylamine borane, sodium hypophosphite, sodium phosphite, formaldehyde, glyoxylic acid, hydrazine, sodium formate, etc. can be used. These may be used alone or in combination of two or more.

[0067] The treatment conditions (temperature, etc.) for activating the catalytic metal are not particularly limited as long as the bath type has a pH of 3.0 or more. When the pH is 3.0 or more, dissolution of the metal oxide layer can be further suppressed, and the decrease in adhesion can be further suppressed.

[0068] Another feature of the present invention is that after the first heat treatment, a step (3-1) is carried out in which a catalyst (catalytic metal) is applied to the surface of the metal oxide layer, which allows for efficient production of a plating film that exhibits good adhesion to a glass substrate. On the other hand, if the first heat treatment is performed after applying a catalyst (catalytic metal) to the surface of the metal oxide layer, the catalyst will be oxidized and the electroless copper plating film will not be able to be formed satisfactorily, making it necessary to perform a reduction treatment after the heat treatment, which reduces production efficiency.

[0069] <<Process (3-2)>> In step (3-2), an electroless copper plating film is formed on the heat-treated metal oxide layer, which makes the metal oxide layer conductive and enables electrolytic copper plating. In the step (3-2), it is preferable to form an electroless copper plating film on the surface of the metal oxide layer to which the catalyst (catalytic metal) has been applied, which tends to produce a more suitable effect.

[0070] The thickness of the electroless copper plating film is preferably 0.1 to 2 μm, more preferably 0.5 to 1 μm. If it is 0.1 μm or more, dissolution of the metal oxide layer can be more effectively prevented even when using strongly acidic electrolytic copper plating, and a decrease in adhesion can be more effectively prevented. If it is 2 μm or less, insufficient adhesion between the glass substrate and the metal oxide due to the stress of the electroless copper plating film can be more effectively prevented.

[0071] The electroless copper plating film is formed, for example, by bringing an electroless copper plating bath into contact with the surface of a metal oxide layer to which a catalyst (catalytic metal) has been applied.

[0072] The electroless copper plating bath is not particularly limited, and the treatment conditions (temperature, pH, etc.) of the electroless copper plating are also not particularly limited.

[0073] <Process (4)> In step (4), a second heat treatment is performed after step (3). Specifically, in step (4), a second heat treatment is performed on the glass substrate obtained in step (3) and having an electroless copper plating film formed on its surface. This allows a diffusion layer to be formed between the metal oxide layer and the electroless copper plating film, thereby further strengthening the adhesion between the metal oxide and the electroless copper plating.

[0074] The atmosphere in which step (4) is carried out is preferably an inert gas atmosphere such as nitrogen, argon, helium, etc. By carrying out step (4) in an inert gas atmosphere, excessive oxidation of the electroless copper plating film can be suppressed, and a plating film exhibiting better adhesion to the glass substrate tends to be produced.

[0075] The temperature of the heat treatment is preferably 100 to 600° C., more preferably 200 to 500° C., and further preferably 300 to 450° C. If the temperature is 100° C. or higher, the diffusion layer is sufficiently formed, and the adhesion between the metal oxide and the electroless copper plating tends to be improved. Also, if the temperature is 600° C. or lower, dimensional changes such as warping and distortion of the glass substrate tend to be more suppressed.

[0076] The heat treatment time is preferably 5 to 180 minutes, more preferably 15 to 90 minutes, and further preferably 25 to 90 minutes, which tends to form a sufficient diffusion layer without reducing production efficiency and improve adhesion between the metal oxide and the electroless copper plating.

[0077] <Process (5)> In step (5), an electrolytic copper plating film is formed on the electroless copper plating film after step (4). Specifically, in step (5), an electrolytic copper plating film is formed on the electroless copper plating film that has been subjected to the heat treatment after step (4).

[0078] The thickness of the electrolytic copper plating film is not particularly limited, but is, for example, 10 to 20 μm.

[0079] The electrolytic copper plating film is formed, for example, by contacting the electroless copper plating film with an electrolytic copper plating bath.

[0080] The electrolytic copper plating bath is not particularly limited, but preferably contains a water-soluble copper salt, sulfuric acid, and chloride ions.

[0081] The water-soluble copper salt is included as a copper ion supply source, and examples of the copper compound salt include copper sulfate, copper chloride, copper oxide, copper carbonate, copper pyrophosphate, copper fluoroborate, copper methanesulfonate, copper propanesulfonate, copper isethionate, and copper propanolsulfonate. These copper compounds can be used alone or in combination of two or more. In the case of copper sulfate, for example, the concentration of the water-soluble copper salt in the copper plating bath is preferably 30 to 300 g / L, more preferably 70 to 90 g / L, in terms of copper sulfate pentahydrate.

[0082] The sulfuric acid concentration in the electrolytic copper plating bath is preferably 30 to 300 g / L, more preferably 180 to 220 g / L. When the sulfuric acid concentration is 30 g / L or more, the copper film thickness on the surface to be plated tends to be uniform, and when the sulfuric acid concentration is 300 g / L or less, the water-soluble copper salt tends to be sufficiently dissolved.

[0083] The chloride ion concentration in the electrolytic copper plating bath is preferably 5 to 150 mg / L, more preferably 20 to 100 mg / L, and even more preferably 30 to 60 mg / L. When the chloride ion concentration is 150 mg / L or less, there is a tendency that the generation of copper chloride on the anode surface and the occurrence of passivation of the anode can be suppressed. On the other hand, when the chloride ion concentration is 5 mg / L or more, there is a tendency that the suppression effect can be suppressed from acting partially, and the risk of step plating can be further reduced.

[0084] In addition to the above components, the electrolytic copper plating bath preferably contains a leveler (leveling agent). Here, the leveler is an additive consisting of a nitrogen-containing compound, which acts as a cation in an acidic plating bath and electrically concentrates on areas with high current density, such as the surface side of vias and through-holes of the plated object, increasing the activation overvoltage and suppressing copper deposition. On the other hand, the leveler exhibits leveling properties by being adsorbed in small amounts at the bottoms of fine grooves and holes, etc., and giving priority to copper deposition and creating a bottom-up deposition state.

[0085] The leveler is not particularly limited as long as it is a nitrogen-containing organic compound, and examples thereof include polyethyleneimine and its derivatives, polyvinylimidazole and its derivatives, polyvinylalkylimidazole and its derivatives, copolymers of vinylpyrrolidone and vinylalkylimidazole and its derivatives, dyes such as Janus Green B, diallyldimethylammonium chloride polymers, diallyldimethylammonium chloride-sulfur dioxide copolymers, partially 3-chloro-2-hydroxypropylated diallylamine hydrochloride-diallyldimethylammonium chloride copolymers, diallyldimethylammonium chloride-acrylamide copolymers, diallylamine hydrochloride-sulfur dioxide copolymers, allylamine hydrochloride polymers, allylamine (free) polymers, allylamine hydrochloride-diallylamine hydrochloride copolymers, diamine and epoxy polymers, morpholine and epichlorohydrin polymers, epichlorohydrin-modified polycondensates of diethylenetriamine, adipic acid, and ε-caprolactam, and the like.

[0086] The leveler concentration in the electrolytic copper plating bath is preferably 0.01 to 3000 mg / L.

[0087] In addition to the above components, the electrolytic copper plating bath preferably contains a brightener. A brightener is an additive that inhibits crystal growth during plating precipitation and promotes the formation of growth nuclei, thereby making the plating film finely crystalline and dense, thereby enabling the formation of a glossy film.

[0088] The brightener is not particularly limited as long as it is a sulfur-containing organic compound, and examples thereof include the sulfur-containing compounds shown in the following formula. [ka] (In the formula, R1 is a hydrogen atom or a group represented by -(S)m-(CH2)n-(O)p-SO3M, each R2 is independently an alkyl group having 1 to 5 carbon atoms, M is a hydrogen atom or an alkali metal, m is 0 or 1, n is an integer of 1 to 8, and p is 0 or 1.)

[0089] The brightener concentration in the electrolytic copper plating bath is preferably 0.01 to 1000 mg / L.

[0090] In addition to the above components, the electrolytic copper plating bath preferably contains a carrier, which is an additive that is adsorbed on the copper surface through interaction with chloride ions to form a monomolecular film that uniformly suppresses crystal growth and improves throwing power.

[0091] The carrier is not particularly limited as long as it is a polyether compound. For example, the polyether compound may be a compound containing a polyalkylene glycol having four or more -O- groups. More specifically, the polyether compound may include polyethylene glycol, polypropylene glycol, and copolymers thereof, polyethylene glycol fatty acid esters, polyethylene glycol alkyl ethers, etc.

[0092] The carrier concentration in the electrolytic copper plating bath is preferably 5 to 5000 mg / L.

[0093] The treatment conditions for electrolytic copper plating are not particularly limited. However, the pH of the electrolytic copper plating bath is preferably 6.0 or less, more preferably 4.0 or less, even more preferably 2.0 or less, and particularly preferably 1.5 or less, with no particular lower limit. This tends to provide more favorable effects. The treatment temperature for electrolytic copper plating is preferably 37 to 43°C, and the current density is preferably 3 to 5 A / dm 2 It is.

[0094] <<Other processes>> The method for producing a plating film of the present invention is a method for producing the plating film by carrying out the above steps (1) to (5) in this order, but may include other steps as long as the above steps (1) to (5) are carried out in this order.

[0095] Other steps include steps of electroless nickel plating, electroless silver plating, electroless cobalt plating, electroless palladium plating, etc., between steps (2) and (3). The chemicals used in each step can be appropriately selected from known ones.

[0096] The total thickness of the plating film (plating film laminate) produced by the plating film production method of the present invention is not particularly limited, but is, for example, 10 to 20 μm.

[0097] In this specification, the thickness and total thickness of a plating film or the like are the average values ​​of measurements taken at five locations using an X-ray fluorescence spectrometer.

[0098] The processing conditions and various concentration settings in the above-described processing are not limited to the above conditions, and it goes without saying that they can be appropriately changed depending on the thickness of the film to be formed, etc.

[0099] The plating film produced by the plating film production method of the present invention has good adhesion to glass substrates. Therefore, the plating film of the present invention is preferably used for printed circuit boards and package substrates of electronic devices, more preferably for high-density printed wiring boards. Since the plating film of the present invention can form a plating film (wiring) that exhibits good adhesion to glass substrates, it is ideal for the production of electronic devices that are becoming faster in communication speed.

[0100] Examples of electronic devices include home appliances, in-vehicle devices, power transmission systems, transportation equipment, and communication equipment. Specific examples of electronic devices include air conditioners, elevators, electric vehicles, hybrid vehicles, trains, power modules such as power control units for power generation devices, general home appliances, and personal computers. EXAMPLES

[0101] The present invention will be specifically described based on examples, but the present invention is not limited to these examples.

[0102] Non-alkali glass (ABC-1, manufactured by Nippon Electric Glass Co., Ltd.) cut to a size of 50 mm x 50 mm was used as the glass substrate. A plating film was formed on the glass substrate according to the conditions shown in Tables 1 and 2. Here, in Table 1, the steps are performed in order from top to bottom. In addition, if there is a discrepancy between the description in the text and the conditions shown in the table, the conditions shown in the table take precedence.

[0103] (Example) (Process (1-1)) The surface of the glass substrate was subjected to alcohol cleaning using ethanol at 25° C. for 5 minutes, and then washed with water at a temperature of 25° C. for 1 minute. Next, the surface of the glass substrate was subjected to alkali cleaning using an aqueous sodium hydroxide solution at 50° C. for 5 minutes, and then washed with water at a temperature of 25° C. for 1 minute.

[0104] (Process (1-2)) The surface of the glass substrate was subjected to cleaner conditioning at 50°C for 5 minutes using a through cup MTE-1A manufactured by Uemura Kogyo Co., Ltd., then washed with water at a temperature of 40°C for 1 minute, and further washed with water at a temperature of 25°C for 1 minute. Next, the surface of the glass substrate was subjected to pre-dip at 25°C for 2 minutes using a through cup PED-104 manufactured by Uemura Kogyo Co., Ltd., then activated at 30°C for 8 minutes using a through cup AT-105 manufactured by Uemura Kogyo Co., Ltd., then washed with water at a temperature of 25°C for 1 minute. Next, the surface of the glass substrate was subjected to accelerator treatment at 25°C for 3 minutes using a through cup accelerator ALF-406-A manufactured by Uemura Kogyo Co., Ltd., then washed with water at a temperature of 25°C for 1 minute. Palladium (Pd) was applied to the surface of the glass substrate by the process (1-2).

[0105] (Process (1-3)) The glass substrate to which the catalyst was applied was immersed at 80° C. for 20 minutes in a treatment liquid for forming a metal oxide layer (containing zinc nitrate hexahydrate and dimethylamine borane, pH 6.0) shown in Table 1. It was then washed with water at 25° C. for 1 minute, and further dried in a dryer at 60° C. for 10 minutes. As a result, a metal oxide layer (zinc oxide layer, film thickness 0.3 μm) was formed on the surface of the glass substrate.

[0106] (Process (2)) The glass substrate on which the metal oxide layer was formed was subjected to a first heat treatment under the conditions shown in Table 2.

[0107] (Process (3-1)) The glass substrate that had been heat-treated in step (2) was immersed in a catalyst imparting bath (Uemura Kogyo Co., Ltd., ALCUP Activator MAT-2-A, pH 5.0) at 25°C for 1 minute. It was then washed with water at 25°C for 1 minute. This provided palladium (Pd) to the surface of the metal oxide layer.

[0108] (Process (3-2)) The glass substrate obtained in step (3-1) was immersed in Slucup PEA ver.2 manufactured by Uemura Kogyo Co., Ltd. at 36°C for 20 minutes. It was then washed with water at 25°C for 1 minute, and further dried in a dryer at 60°C for 10 minutes. As a result, an electroless copper plating film (film thickness 0.7 μm) was formed on the surface of the metal oxide layer.

[0109] (Step (4)) The glass substrate on which the electroless copper plating film was formed was subjected to a second heat treatment under the conditions shown in Table 2.

[0110] (Step (5)) The glass substrate obtained in step (4) was washed with sulfuric acid at 25°C for 10 seconds, and then immersed in a through-cup ECD-H (pH 1.0 or less) manufactured by Uemura Kogyo Co., Ltd. at 40°C for 23 minutes at a current density of 3 A / dm 2The plate was then immersed under the conditions of 1.0 μm to 3.5 μm. The plate was then washed with water at 25° C. for 1 minute, dried in a dryer at 60° C. for 10 minutes, and heat-treated in air at 200° C. for 60 minutes. As a result, an electrolytic copper plating film (film thickness 15 μm) was formed on the surface of the electroless copper plating film. In Table 1, Through-Cup ECD-1A, Through-Cup ECD-4B, and Through-Cup ECD-H manufactured by Uemura Kogyo Co., Ltd. correspond to the above-mentioned leveler, brightener, and carrier, respectively.

[0111] (Comparative Examples 1 and 2) According to the conditions shown in Table 2, a plating film was formed in the same manner as in the example.

[0112] Comparative Example 3 Non-alkali glass (ABC-1, Nippon Electric Glass Co., Ltd.) cut to a size of 50 mm x 50 mm was used as the glass substrate. At Geomatec Co., Ltd., 100 nm of Ti was sputtered onto the glass substrate, and 200 nm of Cu was sputtered on top of that. The glass substrate on which Ti and Cu were sputtered was washed at 25°C for 10 seconds using sulfuric acid, and then placed in a through cup ECD-H (pH 1 or less) manufactured by Uemura Kogyo Co., Ltd. at 40°C for 23 minutes with a current density of 3 A / dm. 2 The specimen was then washed with water at 25°C for 1 minute, dried in a dryer at 60°C for 10 minutes, and heat-treated in air at 200°C for 60 minutes. As a result, an electrolytic copper plating film (film thickness 15 μm) was formed on the Cu sputtered surface.

[0113] <Measurement of film thickness> The thickness of the coating was calculated as the average value of measurements taken at five locations using an X-ray fluorescence spectrometer (manufactured by Hitachi High-Tech Science Corporation, product name: SFT-9550).

[0114] <Adhesion evaluation> The adhesion of the plating film was evaluated by making a 10 mm wide cut with a cutter knife on the glass substrate on which the plating film was formed, peeling off the electrolytic copper plating film with a tensile tester (AGS-X, Shimadzu Corporation), and measuring the peel strength. The adhesion was evaluated according to the following evaluation criteria. The higher the peel strength value, the better the adhesion. The results are shown in Table 2. ◎: Peel strength is 300gf / cm or more ◯: Peel strength is 200 gf / cm or more and less than 300 gf / cm. △: Peel strength is 100 gf / cm or more and less than 200 gf / cm. ×: Peel strength is less than 100 gf / cm.

[0115] [Table 1]

[0116] [Table 2]

[0117] From Table 2, it can be seen that the plating film manufacturing method of the embodiment, which includes step (1) of forming a metal oxide layer on the surface of the glass substrate, step (2) of performing a first heat treatment after step (1), step (3) of forming an electroless copper plating film on the metal oxide layer after step (2), step (4) of performing a second heat treatment after step (3), and step (5) of forming an electrolytic copper plating film on the electroless copper plating film after step (4), can produce a plating film that exhibits good adhesion to the glass substrate.

[0118] Fig. 1(a) shows a photograph of the plating film of Example 1 observed by an electron microscope, and Fig. 1(b) shows a photograph of the plating film of Comparative Example 3 formed by a copper sputtering process observed by an electron microscope. Comparative Example 3 showed poor coverage in the through-holes present in the substrate, while Fig. 1(a) shows that the manufacturing method of the present invention showed excellent deposition and adhesion in the through-holes present in the substrate.

Claims

1. (1) forming a metal oxide layer on a surface of a glass substrate; A step (2) of performing a first heat treatment after the step (1); After the step (2), a step (3) of forming an electroless copper plating film on the metal oxide layer; A step (4) of performing a second heat treatment after the step (3); and After the step (4), a step (5) of forming an electrolytic copper plating film on the electroless copper plating film. Includes A method for manufacturing plating films.

2. 2. The method for producing a plating film according to claim 1, wherein the step (1) includes the following steps (1-2) and (1-3), which are carried out in this order: Step (1-2): A catalyst is applied to the surface of the glass substrate. Step (1-3): A metal oxide layer is formed on the surface of a glass substrate.

3. 3. The method for producing a plating film according to claim 1, wherein the metal oxide is an oxide containing zinc.

4. 3. The method for producing a plating film according to claim 1, wherein the step (1) is a step of forming a metal oxide layer using an aqueous solution containing zinc ions, nitrate ions, and an amine borane compound.

5. The method for producing a plating film according to claim 1 or 2, wherein the step (3) includes the following steps (3-1) and (3-2), which are carried out in this order: Step (3-1): Applying a catalyst to the surface of a metal oxide layer. Step (3-2): An electroless copper plating film is formed on the heat-treated metal oxide layer.

6. 3. The method for producing a plating film according to claim 1, wherein the atmosphere in which the step (4) is carried out is an inert gas atmosphere.

7. 3. The method for producing a plating film according to claim 1, wherein the step (5) is a step of forming an electrolytic copper plating film using an electrolytic copper plating bath having a pH of 2.0 or less.

Citation Information

Patent Citations

  • Formation of wiring and wiring board

    JP1998245682A

  • Method for depositing electroless zinc oxide film

    JP2002241951A

  • Developing sleeve and method of manufacturing the same

    JP2003107897A

  • Electrolytic copper plating

    JP2009024203A

  • A Novel Adhesion Promotion Method for Metallizing Substrate Surfaces

    JP2016533429A

Cited By

  • Electroless copper plating film, electroless copper plating bath, and method for producing electroless copper plating film

    CN122502110A

  • Electroless copper plating deposit, electroless copper plating bath, and method of producing electroless copper plating deposit

    EP4786638A2

  • Electroless copper plating film, electroless copper plating bath, and method for manufacturing electroless copper plating film

    JP2026132096A

  • Electroless copper plating film, electroless copper plating bath, and method for manufacturing electroless copper plating film

    JP2026132397A

  • Electroless copper plating film, electroless copper plating bath, and method for manufacturing electroless copper plating film

    JP7942355B2