New magnesium secondary battery
The new magnesium secondary battery design addresses energy density and safety issues by using a nickel oxide electrode, magnesium alloy, and a chelate ligand in an alkaline electrolyte, achieving higher capacity and safety for diverse applications.
Patent Information
- Application Number
- JP2023077492
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing secondary batteries, such as nickel-metal hydride and lithium-ion batteries, face issues with volumetric energy density, safety concerns, and high costs, while magnesium-air batteries struggle with nonconductivity and magnesium hydroxide formation.
A new magnesium secondary battery design featuring a nickel oxide positive electrode, magnesium alloy negative electrode, alkaline electrolyte with a magnesium ion chelate ligand, and nano-carbon components to enhance safety and capacity.
The new battery achieves higher volumetric energy density, safety through hydrogen management, and cost-effectiveness, suitable for various applications including electric vehicles and space probes.
Smart Images

Figure 2024155639000001 
Figure 2024155639000002
Abstract
Description
Detailed Description of the Invention [Technical field]
[0001] The present invention relates to a "new type of magnesium secondary battery," and more specifically, to a "new type of magnesium battery" that is characterized in that it comprises a positive electrode made of nickel oxide, a negative electrode made of a magnesium alloy, a separator provided between the positive electrode and the negative electrode, and an alkaline electrolyte, the electrolyte containing a ligand that forms a chelate with magnesium ions. [Background technology]
[0002] In recent years, electronic and electrical machinery has steadily become smaller, lighter, thinner, and more functional in order to increase convenience. As a result, there has been a demand for the batteries used as power sources for these devices to be small, light, thin, and high-capacity, and in particular rechargeable secondary batteries. The small secondary battery that responded to these demands was the nickel-metal hydride battery, which had 2.5 times the electric capacity of the nickel-cadmium storage battery (weight energy density 60-120Wh / kg, volume energy density 140-200Wh / L). This was called the Ni-MH type, which used nickel for the positive electrode material and misch metal, a hydrogen storage alloy, for the negative electrode material. Since then, lithium-ion secondary batteries with even larger electric capacity have been developed, which has taken over the market share in the field of portable devices, but in the field of dry batteries, it has replaced the Ni-Cad battery as the mainstream. In the field of electric vehicles and hybrid cars, even larger nickel-metal hydride batteries have been developed, and Ni-H types, which store hydrogen in high-pressure tanks and share hydrogen as the cathode, are being considered. Nickel-metal hydride batteries for vehicles have a small volume energy density, so there is a problem that their size becomes large when trying to obtain a large amount of electricity. Nickel-metal hydride batteries are used as the driving power source for automobile motors because they are less likely to explode than lithium-ion batteries, which will be described later. However, the biggest drawback of nickel-metal hydride batteries is that when they are topped up and charged into a nickel-metal hydride storage battery, a memory phenomenon occurs in which the voltage drops temporarily during discharging, and therefore the battery must be rapidly discharged to its final voltage before being recharged again each time it is charged.
[0003] Lithium-ion secondary batteries followed the nickel-hydrogen rechargeable battery. Lithium-ion secondary batteries use a lithium transition metal composite oxide for the positive electrode, a carbon material for the negative electrode, and a non-aqueous electrolyte such as an organic solvent for the electrolyte. Lithium ions move between the positive and negative electrodes to charge the battery. With a weight energy density of 100-243Wh / kg and three times the volumetric energy density (250-456Wh / L), they quickly took over the nickel-hydrogen battery in the electronic and electrical appliance field. However, because of their high energy density, they have been known to generate abnormal heat during charging and even cause fires, so measures are being called for.
[0004] On the other hand, there is an air magnesium battery that uses metallic magnesium for the negative electrode and oxygen from the air for the positive electrode. This is a type of air battery and fuel cell, and if the magnesium hydroxide produced by the discharge of the battery is regenerated into magnesium using solar heat, a concept has been proposed that would create a "magnesium recycling society," which has attracted attention, but it has not yet reached completion. There are attempts to avoid this by adding an auxiliary agent that makes it easier for the magnesium hydroxide produced to dissolve in the electrolyte (see Patent Documents 1 and 2), or to use an alloy of magnesium and calcium for the electrode, where calcium takes hydroxide ions from magnesium and suppresses the formation of a non-conductive state, but none of these attempts have been sufficiently effective. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Application No. 2008-191821 [Patent Document 2] JP2009-064730A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made to solve these problems, and its object is to provide a "new magnesium secondary battery" that has a larger electric capacity than conventional lithium ion secondary batteries, can be made smaller, and is safer and less expensive than lithium secondary batteries. [Means for solving the problem]
[0007] The [new type of magnesium secondary battery] of the present invention, made to achieve the above-mentioned object, comprises a positive electrode made of nickel oxide, a negative electrode made of a magnesium alloy, a separator provided between the positive electrode and the negative electrode, and an alkaline electrolyte filled between the positive electrode and the negative electrode, and is characterized in that the electrolyte contains a ligand that forms a chelate complex with magnesium ions.
[0008] Preferably, the ligand is ethylenediaminetetraacetic acid. It is preferable to have a catalyst layer around the negative electrode, in which nano-carbon particles carrying a precious metal catalyst are attached. The negative electrode can be a flame-retardant magnesium alloy containing calcium, iron, zinc, or the like.
[0009] The positive electrode is preferably a porous molded body made by sintering nickel hydroxide, nano-carbon, manganese dioxide, or the like. It is preferable that a layer of activated carbon is formed between the positive electrode and the separator. Effect of the Invention
[0010] According to the present invention, the [new magnesium secondary battery] of the present invention prevents the formation of a non-conductive state, which is the biggest problem with magnesium-air batteries, by blending a ligand that forms a chelate complex with magnesium into the alkaline electrolyte, and can provide a secondary battery with a larger electric capacity than conventional lithium-ion secondary batteries. Increasing the volumetric energy density makes it possible to miniaturize batteries, making it possible to provide batteries that are suitable not only for electric vehicles and hybrid cars, but also for renewable energy storage batteries, artificial satellites, and space probes. The new magnesium secondary battery of the present invention has a catalytic layer of nano-carbon particles carrying a precious metal catalyst around the negative electrode, which converts hydrogen (H2) generated by the reaction between magnesium at the negative electrode and water in the electrolyte into hydrogen ions (H + ) and electrons (e - ) and prevents hydrogen gas from accumulating inside the battery cell, thereby preventing the expansion of the cell and preventing accidents such as leakage. The new magnesium secondary battery of the present invention has nano-sized activated carbon between the positive electrode and the separator, which buffers the violent oxidation-reduction reactions at the positive and negative electrodes during charging, ensuring safety. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view of a square-shaped [new magnesium secondary battery] according to one embodiment of the present invention. [Diagram 2] FIG. 1 shows the structure of a chelate complex of magnesium ion with ethylenediaminetetraacetic acid (EDTA). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] This invention relates to a new type of magnesium secondary battery that can be used as a secondary battery for various electronic and electrical devices such as smartphones, digital cameras and videos, portable music players, and dedicated batteries for laptops; as a secondary battery to drive the motors and interior equipment of electric and hybrid cars; as a storage battery for renewable energy; and even for artificial satellites and space probes. The new magnesium secondary battery of the present invention can be provided in a variety of shapes to meet the many needs listed above, such as D, AA, AAA, button, square, box, and other special industrial shapes. The "new type of magnesium secondary battery" of the present invention is characterized by comprising a positive electrode made of nickel oxide, nano-carbon, and manganese dioxide, a negative electrode made of magnesium alloy (magnesium, iron, zinc), a separator provided between the positive electrode and the negative electrode, and an alkaline electrolyte filled between the positive electrode and the negative electrode, the electrolyte containing a ligand that forms a chelate with magnesium ions. FIG. 1 is a cross-sectional view of a prismatic "new magnesium secondary battery" according to one embodiment of the present invention. In FIG. 1, reference numeral 1 denotes a new type of magnesium secondary battery, 10 denotes a positive electrode, 20 denotes a negative electrode, 30 denotes a separator, 40 denotes an electrolyte, 50 denotes a catalyst layer, and 60 denotes an activated carbon layer.
[0013] The positive electrode 10 is a porous body made of nickel oxide. The positive electrode 10 absorbs electrons (e - ) moves through the cell and electrons (e - ) reacts with oxygen (O2) in the air. In this case, the uptake of oxygen (O2) is the rate-limiting step, so it is preferable that the positive electrode is porous so that it can easily absorb oxygen. The nickel oxide used in the positive electrode 10 may be nickel hydroxide (Ni(OH)2), nickel oxide hydroxide (NiOOH) or nickel oxide (NiO), nano carbon (C), or manganese dioxide (MnO2). There is no particular restriction on the casting method for the electrodes, but ceramic molding and sintering methods can be applied. For example, nickel oxide powder can be placed in a mold, pressure molded, and then baked in a sintering furnace. Another method that can be used is to mix a mixture of molten synthetic resin and nickel oxide powder, then injection mold the mixture, heat sinter the molded product, and remove the resin.
[0014] The negative electrode 20 is made of metallic magnesium (Mg), iron (Fe), and zinc (Zn). During discharge, the negative electrode reacts with the alkaline electrolyte 40 on its surface to produce magnesium ions (Mg 2+ ) and electrons (e - ) becomes. Electron (e - ) move inside the cell toward the positive electrode 10. The negative electrode 20 can be made of metallic magnesium (Mg) with a purity of 99% or more, but since this is likely to be weak and lack hardness, an alloy of 2 to 10% aluminum (Al) and about 1% iron (Fe) and zinc (Zn) is usually used. The magnesium ions (Mg 2+ ) is the surrounding hydroxide ions (OH - ) to form poorly soluble magnesium hydroxide (Mg(OH)2), which then becomes passive. In order to prevent the formation of the passivation state, the negative electrode 20 is preferably a flame-retardant magnesium alloy containing calcium. The amount of calcium mixed is usually about 1 to 5% based on the weight of the negative electrode 20. If the amount of calcium mixed is less than 1% by weight, there is a risk that the effect of preventing the formation of the passivation state will not be sufficiently obtained, and if it exceeds 5%, there is a risk that the electrode will become brittle and crack. Calcium (Ca) has a smaller ionization tendency than magnesium (Mg), so it is easier to ionize than magnesium (Mg). Therefore, it forms hydroxides (OH - ) from magnesium (Mg), so hydroxide ions (OH - The moment the magnesium (Mg 2+ ) dissolves, delaying the formation of the passive state.
[0015] A separator 30 is provided between the negative electrode 20 and the positive electrode 10. The separator 30 is provided to separate the negative electrode side from the positive electrode side, and is used to separate electrons (e - ) moves from the negative electrode to the positive electrode, and during charging, electrons (e - For this reason, the separator 30 is preferably a non-polar porous membrane. Examples of materials used for separator 30 include nonwoven fabrics made from inorganic fibers such as glass wool, rock wool, and sludge wool; woven or nonwoven fabrics made from synthetic fibers such as polyvinyl alcohol, polyamide, polyacrylonitrile, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyethylene terephthalate, and polyurethane; membrane filters made from fluorinated resins such as polytetrafluoroethylene, polyvinylidene fluoride, and polyvinyl fluoride, or cellulose acetate; and cotton cloth or Japanese paper made from natural materials such as cellulose. Among these, Japanese paper made of pure cellulose is preferably used as the separator 30 of the [new magnesium secondary battery] 1.
[0016] An electrolyte 40 is filled between the positive electrode 10 and the negative electrode 20. An alkaline aqueous solution is used for the electrolyte 40. An acidic electrolyte reacts with the magnesium (Mg) of the electrode to generate hydrogen (H2), resulting in self-discharge. The alkaline electrolyte 40 may be prepared by dissolving a basic compound in water. There are no particular limitations on the basic substance used as long as the water solubility is alkaline, but potassium hydroxide (KOH) or sodium hydroxide (NaOH) is usually used due to its cost and availability, and its concentration is 0.3 to 32%. When alkaline electrolyte 40 is used, magnesium (Mg) and hydroxide ions (OH - ) reacts to produce magnesium hydroxide (Mg(OH)2) and electrons (e - ) is produced. - ) moves toward the positive electrode 10, but magnesium hydroxide (Mg(OH)2) has low water solubility, with only 1.2 mg dissolving in 100 mL of water, so magnesium hydroxide (Mg(OH)2) precipitates on the surface of the negative electrode, making it passive and stopping the reaction. To solve this problem, research is being conducted on auxiliary agents that dissolve magnesium hydroxide (Mg(OH)2) in water, but nothing practical has yet been developed. The present invention does not dissolve magnesium hydroxide (Mg(OH)2), but rather magnesium ions (Mg 2+ ) is isolated outside the electrolyte system as a chelate complex to prevent the formation of a non-conductor.
[0017] The electrolyte 40 of the [new magnesium secondary battery] 1 of the present invention contains magnesium ions (Mg 2+ ) and a ligand that forms a chelate. A chelate is a bond to a metal ion by a ligand with multiple coordination sites. A compound formed by a chelate bond is called a chelate complex. Magnesium ions (Mg 2+ The chelate complex of Mg 2+ ) at the center of the magnesium ion (Mg 2+ ) is located at the center of the metal ion, which is surrounded by ligands with shared electrons to form a complex compound. In a chelate complex, the ligands have multiple coordination sites and surround the metal, making it difficult to separate the metal from the substance to which it is coordinated. This is called the chelate effect, and it is known that magnesium ions (Mg 2+ ) outside the electrolyte solution system. Metal chelates have a number of ligands, either 2, 4 or 6, depending on the nature of the metal. Magnesium (Mg) has 6 ligands. 2+ The structure of the chelate complex of ethylenediaminetetraacetic acid (EDTA: (HOCOCH2)2NCH2CH2N(CH2COOH)2) is a regular octahedral hexadentate ligand.
[0018] Figure 2 shows the effect of ethylenediaminetetraacetic acid (EDTA) on magnesium ions (Mg 2+ The structure of the chelate complex of magnesium ion (Mg 2+ ) is coordinated by two nitrogens (N) and four oxygens (O) of ethylenediaminetetraacetic acid (EDTA). Ethylenediaminetetraacetic acid (EDTA) is freely soluble in alkaline water. The concentration of ethylenediaminetetraacetic acid (EDTA) in the electrolyte of the present invention is 0.5 to 50% by weight, preferably 3 to 30% by weight, and more preferably 6 to 24% by weight. When the concentration of ethylenediaminetetraacetic acid (EDTA) is less than 0.5% by weight, the magnesium ions (Mg 2+ ) is small, and there is a risk that the generation of passivation cannot be sufficiently suppressed. On the other hand, if the concentration of ethylenediaminetetraacetic acid (EDTA) is 50% by weight or more, sodium hydroxide (NaOH) or potassium hydroxide (KOH) dissolved in the electrolyte 40 will start to precipitate, and the function of the electrolyte may deteriorate.
[0019] Magnesium (Mg) powder reacts with water to generate hydrogen (H2). Because magnesium (Mg) forming the negative electrode 20 is a metal lump, it does not react violently with the alkaline electrolyte 40, but reacts gently to generate hydrogen (H2). The generated hydrogen (H2) may deteriorate the performance of the battery because it remains in the cell, and furthermore, if hydrogen gas accumulates in the cell, the cell may expand and cause leakage. In order to prevent deterioration of battery performance and leakage accidents, it is preferable to form a catalyst layer 50 made of fine particles of carbon carrying a catalyst around the negative electrode 20. The catalyst layer 50 formed around the negative electrode 20 converts hydrogen (H2) generated by the reaction between magnesium (Mg) of the negative electrode 20 and water of the electrolyte 40 into hydrogen ions (H + ) and electrons (e - ) and hydrogen ions (H + ) is the hydroxide ion (OH - ) to produce water (HO) and electrons (e - ) is transferred to the positive electrode 10. The catalyst supported on the catalyst layer 50 formed around the negative electrode 20 is preferably one or more selected from catalysts containing precious metals such as platinum (Pt), palladium (Pd), rhodium (Rh), and ruthenium (Ru). The precious metal catalyst may be fine particles of metal, or may be a chelate catalyst in which a precious metal catalyst is coordinated. Among them, a platinum black catalyst obtained by reducing fine particles (Adams catalyst) of platinum oxide (PtO2) is preferably used. The catalyst may be supported on carbon, for example, by immersing nano-sized carbon in a state in which chloroplatinic acid (H2PtCl6) or ammonium chloroplatinate ((NH4)2PtCl6) is dissolved in sodium nitrate (NaNO3) to support platinum, washing with water to remove nitrates to form platinum oxide (PtO), and reducing the platinum black (Pt) with hydrogen (H2) or formaldehyde (HCHO). The carbon carrying the catalyst is applied to the surface of the negative electrode 20 via water or a liquid having a boiling point of 500°C or less, and the catalyst layer can be fixed to the surface of the negative electrode 20 by baking the mixture in an argon (Ar) or nitrogen (N2) atmosphere at a temperature near the melting point of the magnesium alloy (500 to 1000°C). The amount of catalyst contained in the catalyst layer 50 is about 0.001% of the weight of the negative electrode 20 .
[0020] A layer of activated carbon 60 is formed between the positive electrode 10 and the separator 30. This layer of activated carbon 60 serves as a support to maintain the structure of the cell, and at the same time, absorbs electrons (e - ) pool. The rate-limiting step of the [new magnesium secondary battery] 1 of the present invention is the uptake of oxygen (O2) at the positive electrode 10. Therefore, the electrons (e - ) will wait their turn to be oxidized. Activated carbon is a conductive SP 2 Bonded carbon and non-conductive SP 3 It is a mixture of bonded carbon and is non-conductive overall. SP 3 At the ends of the bonded carbon, there are many covalent bond branches that have no bond partners, and these terminal bonds carry waiting electrons (e - ) is thought to remain. The layer of activated carbon 60 between the positive electrode 10 and the separator 30 prevents electrons (e - ) to buffer the violent oxidation-reduction reactions that occur in the positive electrode 10 and the negative electrode 20 during charging, thereby ensuring safety.
[0021] The chemical reactions occurring during charging and discharging of the [new type magnesium secondary battery] 1 of the present invention are shown by the following chemical formulas. [Discharge] ·Negative electrode Mg+20H - -> Mg(OH)2+2e - ·Electrolyte Mg(OH)2+EDTA -> EDTA-Mg 2+ +2OH - ·Positive electrode O2+2H2O+4e - -> 4OH - 〔charging〕 ·Positive electrode NiOOH+H2O+e - -> Ni(OH)2+OH - ·Electrolyte EDTA-Mg 2+ +2e - -> Mg+EDTA ·Negative electrode Mg(OH)2+2e - -> Mg+2OH - During discharge, magnesium (Mg) and hydroxide ions (OH - ) reacts to produce magnesium hydroxide (Mg(OH)2) and electrons (e - ) electron (e - ) migrates through the electrolyte 40 toward the positive electrode 10. Magnesium hydroxide (Mg(OH)2) is converted to magnesium ions (Mg 2+ ) chelate complex (EDTA-Mg 2+ ), and the interaction with the ions present in the electrolyte 40 becomes extremely small. During discharge, oxygen (O2) from the atmosphere, water (H2O) from the electrolyte, and electrons (e- ) combine to form hydroxide ions (OH - ) reaction occurs. On the other hand, during charging, the electrons (e - ) is used to convert nickel oxide hydroxide (NiOOH) to nickel hydroxide (Ni(OH)2), which is then converted into a chelate complex (EDTA-Mg 2+ ) that existed as magnesium ions (Mg 2+ ) is supplied to the - ) to form metallic magnesium (Mg), which then forms a chelate complex (EDTA-Mg 2+ ) releases magnesium ions (Mg) and becomes free. During charging, magnesium hydroxide (Mg(OH)2) in the negative electrode 20 uses the supplied electrons to convert metallic magnesium (Mg) and hydroxide ions (OH - ) EXAMPLES
[0022] Examples of the "new type magnesium secondary battery" of the present invention will be described below. positive electrode Nickel hydroxide (nickel powder manufactured by Sumitomo Metal Mining Co., Ltd.), carbon, manganese dioxide were crushed and dried to prepare an oxide. Fine nickel hydroxide powder was pressed to create a porous nickel plate, which was then pressed to create a box-shaped container (cell) 100 mm wide, 1000 mm long, and 1500 mm wide. This was sintered at 210° C. in a nitrogen atmosphere to form a positive electrode. negative electrode A plate (1.25 mm thick) of flame-retardant magnesium alloy (manufactured by Kurimoto Iron Works Ltd.) containing 4% calcium, 7% aluminum, 1% iron and 1% zinc was cut into a rectangle 950 mm long and 1,450 mm wide to serve as the negative electrode. catalyst layer Chloroplatinic acid (H2PtCl6·6H2O: Yoneyama Pharmaceutical Co., Ltd.) was dissolved in sodium nitrate (NaNo3: Wako Pure Chemical Industries, Ltd.), and the mixture was immersed in carbon black (Mitsubishi Chemical Co., Ltd., brand: No. 44) to support platinum, then washed with water to remove the nitrates to form platinum oxide (PtO), which was then immersed in formaldehyde (HCHO: Wako Pure Chemical Industries, Ltd.). The mixture was stirred at 60°C for 1 hour to reduce and prepare platinum black (Pt). This suspension was applied to both sides of the negative electrode, and the mixture was heated at 500°C in a nitrogen atmosphere to fix the catalyst layer.
[0023] Separator The negative electrode with a catalyst layer attached to its surface was wrapped in handmade Japanese paper (Mino paper) and placed in the center of a cell made of nickel oxide, the positive electrode. electrolyte Potassium hydroxide (manufactured by Wako Pure Chemical Industries, Ltd.) and ethylenediaminetetraacetic acid (EDTA: manufactured by Tokyo Chemical Industry Co., Ltd.) were dissolved in deionized water to prepare an alkaline electrolyte containing 24% by weight of potassium hydroxide and 16% by weight of ethylenediaminetetraacetic acid (EDTA). Activated carbon (manufactured by Kuraray Chemical Co., Ltd., product name: Kuraray Coal (registered trademark), brand: PW, standard particle size: 100 μm or less) was suspended in this alkaline electrolyte and poured into the space between the positive and negative electrodes to form an activated carbon layer impregnated with the electrolyte.
[0024] Terminal leads were provided to the positive and negative electrodes, and an ammeter, a voltmeter, and a resistor were connected to measure the amount of power generated. As a result, it was found that the [new magnesium secondary battery] of the present invention had a weight energy density of 515 Wh / kg and a volumetric energy density of 650 Wh / L, and thus had a power capacity more than twice that of conventional lithium-ion secondary batteries. [Explanation of symbols]
[0025] 1: New magnesium secondary battery 10: Positive electrode 20: Negative electrode 30: Separator 40: Electrolyte 50: Catalyst layer 60: Activated carbon layer
Claims
1. a positive electrode made of nickel oxide; a negative electrode made of a magnesium alloy; a separator provided between the positive electrode and the negative electrode; and an alkaline electrolyte filled between the positive electrode and the negative electrode, The electrolyte contains a ligand that forms a chelate with magnesium ions. [New type of magnesium secondary battery].
2. The new magnesium secondary battery according to claim 1, characterized in that the ligand is ethylenediaminetetraacetic acid.
3. The new magnesium secondary battery according to claim 1, characterized in that the negative electrode is surrounded by a catalyst layer in which nano-carbon particles carrying a precious metal catalyst are attached.
4. 2. The new magnesium secondary battery according to claim 1, wherein the negative electrode is a flame-retardant magnesium alloy containing calcium.
5. The new magnesium secondary battery according to claim 1, characterized in that the positive electrode is a porous body made of sintered nickel hydroxide.
6. 2. The magnesium battery according to claim 1, further comprising a layer of activated carbon formed between the positive electrode and the separator.
Citation Information
Patent Citations
Input test device
JP2008191821A
Magnesium ion containing nonaqueous electrolyte, manufacturing method thereof, and electrochemical device