Core spun yarn comprising short cellulosic staple fibers and process for producing the same

A core spun yarn with a polyester core and a mixed cellulose sheath addresses the limitations of recycled cotton fibers in ring spinning, enhancing mechanical properties and durability while maintaining appearance and dyeability.

JP2024155859APending Publication Date: 2024-10-31SANKO TEKSTIL ISLETMELERI SANAYI VE TICARET AS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024068030
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-19
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Recycled cotton fibers are too short for effective use in ring spinning, leading to poor yarn quality and mechanical properties, and blending with virgin cotton or polyester results in appearance and dyeability issues.

Method used

A core spun yarn structure comprising a polyester filament core and a sheath made of a mixture of natural cellulose and regenerated cellulose fibers, with specific length and content ratios, to enhance mechanical properties and processability.

Benefits of technology

The yarn achieves good mechanical properties, appearance, and dyeability, allowing for high recycled cotton content without core slippage, and produces fabrics with improved durability and abrasion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155859000001_ABST
    Figure 2024155859000001_ABST
Patent Text Reader

Abstract

To provide a yarn using short cellulosic, e.g. cotton staple fibers obtained from recycling of yarns and fabrics, and a process for producing the yarn.SOLUTION: A method for producing a yarn comprises the steps of: a. selecting a filament core comprising a plurality of polyester filaments, in which the elongation at break of the polyester filaments is in a range of 5% to 15%, preferably between 10% and 12%, when tested with DIN ISO 2062; b. selecting a staple fiber sheath, in whish at least 95% of the sheath is made of first staple fibers and second staple fibers, the first staple fibers being recycled cotton fibers, the second staple fibers being regenerated cellulosic fibers; and c. combining the filament core and the staple fiber sheath via ring spinning.SELECTED DRAWING: Figure 2a
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of yarn manufacturing, more particularly to yarns using short cellulose, such as short cotton fibers, typically obtained from yarn and fabric recycling, and to a method for producing said yarns. [Background technology]

[0002] Due to the cost and environmental impact of producing natural fibers, methods have been developed to recycle and reuse natural fibers from textile waste. A prominent example is the recycling of cotton from waste textiles, especially fabric and yarn waste, to obtain recycled cotton fibers.

[0003] Known fabric and yarn recycling processes generally involve mechanically breaking down the fabric into loose fibers that can be used to spin new yarn. This process uses machines that break down the fabric, such as by rotating drums with metal pins. When the yarn fibers are subjected to a mechanical load, the original fibers are cut into shorter fibers. Summary of the Invention [Problem to be solved by the invention]

[0004] The problem with recycled cotton fibres is that they contain short fibres, making them unsuitable or poorly suited for yarn production, especially on ring spinning machines for denim production. Virgin cotton staple fibres contain more long fibres than recycled cotton fibres. For example, the average length L(n) of virgin cotton fibres (considering the total fibres in a yarn) is usually over 20 mm, while the average length L(n) of recycled cotton staple fibres is usually less than 15 mm, usually between 6 and 15 mm, more commonly between 9 and 12 mm.

[0005] Therefore, it is difficult to properly use recycled (short) cotton fibres in ring-spun yarn production.

[0006] If the length of the cotton fibre is short, the yarn strength will be too low resulting in poor fabric quality, and the composite fibres may break on the yarn making machine and cannot be processed into yarn. Therefore, by mixing recycled cotton fibres with virgin cotton fibres, the final yarn is endowed with acceptable mechanical properties and physical properties such as bulk and appearance of yarns containing 100% virgin natural fibres such as virgin cotton. The weight ratio of virgin cotton fibres (CO) to recycled cotton fibres (RCO) in the yarn varies depending on the yarn production technology. Typically, open-end yarns consist of up to 100% recycled cotton, while in ring-spun yarns the RCO content does not exceed 40% (by weight), and the weight ratio of CO / RCO generally ranges from 70 / 30 to 90 / 10.

[0007] It has also been proposed to use polyester filaments and fibers to improve the mechanical properties of yarns containing recycled cotton fibers. In one form, polyester staple fibers are mixed with cotton fibers and then spun into yarn, but these yarns have the disadvantage that they cannot be easily dyed and have a poor, non-cotton-like appearance due to the presence of polyester. The embodiment in which polyester filaments are provided as the core filament in the recycled cotton sheath suffers from the above-mentioned drawback of necessarily having a low recycled cotton fiber content, and furthermore, the recycled cotton fiber sheath is particularly unable to solve this problem since it easily breaks when stretched or under tension.

[0008] Therefore, there is a need to solve these problems of the prior art and provide a yarn which is made of all recycled cotton fibers, is a ring spun yarn, has good appearance, and has good to excellent mechanical properties.

[0009] One object of the present invention is to provide a yarn in which all cotton fibers are recycled, and which has short cotton fibers, good or excellent mechanical properties, and the appearance and texture of yarn containing virgin cotton fibers.

[0010] Another object of the present invention is to provide a corespun yarn containing short cotton fibers that have elastic and stretchable properties. [Means for solving the problem]

[0011] This object is achieved by the present invention with respect to a yarn and a method according to the independent claims.

[0012] In particular, the invention relates to a yarn and an associated manufacturing method as claimed in the accompanying independent claims, with preferred embodiments being set out in the dependent claims.

[0013] According to the invention, the yarn comprises a filament core and a staple fiber sheath, said staple fiber sheath being made exclusively of a mixture of first and second staple fibers or comprising at least 95% by weight of a mixture of first and second staple fibers, said first staple fibers being natural cellulose fibers and said second staple fibers being regenerated cellulose fibers. The average length of the sheath fibers is in the range of 10 to 34 mm, preferably 12 to 29 mm, the 5%(n) index of the sheath fibers is in the range of 25 to 40 mm, more preferably 28 to 36 mm, and even more preferably 30 to 34 mm, the short fiber content SFC(n) of the sheath is in the range of 2% to 70%, preferably 10% to 60%, and the filament core comprises a plurality of polyester filaments. The elongation at break of the polyester filaments of said filament core, measured according to DIN ISO 2062, is in the range of 5% to 15%, more preferably between 10% and 12%.

[0014] The weight ratio of the first short fibers to the second short fibers is in the range of 20 / 80 to 80 / 20, preferably in the range of 20 / 80 to (less than) 70 / 30. The average length is the L(n) value measured according to DIN 53805:1980-06.

[0015] Test machines capable of measuring the above indices, i.e. L(n), 5%(n), SFC(n), such as USTER AFIS PRO 2 and Textechno FCS-Fibrotest, are known in the art. The average fiber length (Ln) can be calculated by the following formula:

[0016]

number

[0017] where Ln is the average fiber length, ni is the number of fibers of length li, and li is the length of fiber i.

[0018] In the sheath, the fibre 5%(n) index (measured as mentioned above to DIN 53805:1980-06) is at least 25 mm, preferably between 25 mm and 40 mm, more preferably between 28 and 38 mm, and the short fibre content SFC(n) of the sheath (measured to DIN 53805:1980-06) is between 30% and 70%, with preferred values ​​being 35% or more, more preferably 40% or more, i.e. between 40 and 70%.

[0019] The elongation at break claimed is the elongation of all filaments of the core tested together. In particular, it has been found that a low core elongation (i.e., less than 15% as mentioned above) facilitates the yarn manufacturing and weaving process. In particular, in these embodiments, the core elongation is typically similar to that of cotton fibers. In fact, when the final yarn is subjected to tension, high elongation of the polyester core (i.e., greater than 15% or 20%) can cause the sheath to slip off the core or the staple fiber sheath to break.

[0020] The use of low elongation polyester filaments in the core helps to avoid the above problems. Low elongation polyester filaments are known in the art and are commercially available. They can be obtained in various ways. A possible solution is to provide a draft during the texturing process of the POY polyester filaments. Such a draft is preferably between 1.7 and 2.5, more preferably between 1.8 and 2.1.

[0021] The polyester filaments are preferably textured in nature, and as previously mentioned, stretching during the texturing process can usually also be achieved by heating the filaments during the stretching step of the texturing process.

[0022] According to one embodiment of the invention, the amount of polyester filaments in the core is between 10% and 35% of the yarn weight, more preferably between 15% and 25%, even more preferably about 20%. The above percentages relate to the total count of the polyester filaments, i.e. the sum of the total counts of the filaments.

[0023] According to one aspect of the invention, the polyester filaments have an overall count of 50-150 denier, more preferably 60-120 denier, and even more preferably 75-100 denier. The use of low elongation polyester is beneficial in improving the mechanical properties of the final yarn and preventing problems such as core slippage during yarn manufacture. This is particularly true for embodiments with a high percentage of cotton. However, it has been found that low elongation polyester also helps prevent core slippage in embodiments with a low percentage of cotton.

[0024] The invention, according to one aspect thereof, also relates to a yarn comprising a filament core and a staple fiber sheath, the staple fiber sheath being a mixture or comprising at least 95% by weight of a mixture of first and second staple fibers, the first staple fibers being natural cellulose fibers and the second staple fibers being regenerated cellulose fibers. The weight ratio of the first staple fiber to the second staple fiber is in the range of 20 / 80 (or more) to 80 / 20 (or more), preferably 20 / 80 (or more) to 70 / 30 (less); the average length of the sheath fibers is in the range of 13 to 34 mm, preferably 15 to 29 mm; the 5%(n) index of the sheath fibers is in the range of 25 to 40 mm, more preferably 28 to 36 mm, and even more preferably 30 to 34 mm; the sheath staple fiber content SFC(n) is 2% to 61%, preferably 10% to 51%; and the filament core contains a plurality of polyester filaments. The elongation at break of the polyester filaments of the filament core, measured according to DIN ISO 2062, is in the range of less than 5% to 15%, more preferably between 10% and 12%.

[0025] Tests on multiple yarns showed that the L(n) index increased with increasing proportion of the first fiber in the blended yarn, whereas the SFC(n) index decreased with increasing proportion of the first fiber in the blended yarn. As will be explained in more detail later, the relationship between the percentage of cotton in the blended yarn and the L(n) and SFC(n) indices is approximately linear, or more closely approximated as a parabola, with a very low quadratic coefficient.

[0026] In contrast, it has been found that the 5%(n) index remains substantially constant when the ratio of the first to second fibers is in the range of 20 / 80 to 70 / 30.As a result, preferred values ​​of the L(n) and SFC(n) indices for the blends are discussed below.

[0027] According to one embodiment of the present invention, the weight ratio of the first short fiber to the second short fiber is in the range of 20 / 80 (or more) to 30 / 70 (less), the average length of the sheath fibers is in the range of 19 to 34 mm, preferably 21 to 29 mm, and the sheath short fiber content SFC(n) is 2% to 41%, preferably 10% to 31%.

[0028] According to one embodiment of the present invention, the weight ratio of the first short fiber to the second short fiber is in the range of 30 / 70 (or more) to 40 / 60 (less), the average length of the sheath fibers is in the range of 18 to 33 mm, preferably 20 to 28 mm, and the sheath short fiber content SFC(n) is 3% to 43%, preferably 13% to 33%.

[0029] According to one embodiment of the present invention, the weight ratio of the first short fiber to the second short fiber is in the range of 40 / 60 (or more) to 50 / 50 (less), the average length of the sheath fibers is in the range of 16 to 31 mm, preferably 18 to 26 mm, and the sheath short fiber content SFC(n) is 8% to 48%, preferably 18% to 38%.

[0030] According to one embodiment of the present invention, the weight ratio of the first short fiber to the second short fiber is in the range of 50 / 50 (or more) to 60 / 40 (less), the average length of the sheath fibers is in the range of 15 to 30 mm, preferably 17 mm to 25 mm, and the sheath short fiber content SFC(n) is 14% to 54%, preferably 24% to 44%.

[0031] According to one embodiment of the present invention, the weight ratio of the first short fiber to the second short fiber is in the range of 60 / 40 (or more) to 70 / 30 (less), the average length of the sheath fibers is in the range of 13 to 28 mm, preferably 15 to 23 mm, and the sheath short fiber content SFC(n) is 21% to 61%, preferably 31% to 51%.

[0032] According to one embodiment of the present invention, the weight ratio of the first short fiber to the second short fiber is in the range of 70 / 30 (or more) to 80 / 20 (or less), preferably about 75 / 25, the average length of the sheath fibers is in the range of 10 to 25 mm, preferably 12 mm to 20 mm, and the sheath short fiber content SFC(n) is 30% to 70%, preferably 40% to 60%.

[0033] The phrase "blend of fibers" is used herein to refer to a mixture of different fibers suitable for use in a ring spinning process to form the sheath of a corespun yarn. Individual fibers within the sheath of the yarn of the invention are identifiable and can be physically removed from the sheath-forming mixture, if desired. In the present invention, the term "regenerated cellulose fibers" or "man-made fibers" refers to any kind of industrially produced cellulosic staple fiber, including any kind of regenerated cellulose fiber, such as lyocell, viscose, modal, bamboo (commercially available bamboo fiber is usually a regenerated cellulose fiber produced from bamboo, i.e. a synthetic rayon made from cellulose extracted from bamboo), polynosic fiber, cupro, acetate, etc. Since such artificial short fibers have a substantially constant length, the length of these fibers falls within a very narrow range, i.e. the CV (coefficient of variation) value is low. In the present invention, the average length of these fibers, measured according to DIN 53805:1980-06, is in the range of 25 mm to 38 mm, preferably 29 mm to 35 mm. The preferred count of regenerated fibers suitable for the present invention is in the range of 1 dtx to 3 dtx, preferably about 1.2 dtx. Preferred regenerated cellulose fibers for the present invention are sustainable cellulose fibers, such as FSC certified regenerated cellulose fibers.

[0034] For the purposes of this invention, the term "virgin fiber" refers to staple cotton fibers obtained from cotton that has not been processed into yarn or fabric and therefore has a long average fiber length.

[0035] In the present invention, the term "natural cellulose fibers" refers to fibers obtained from plants or animal bodies. Preferred natural cellulose fibers are fibers obtained or obtained from recycling processes of fabrics and fibers of plant origin such as cotton, hemp, linen, etc. Typically, the natural cellulose fibers used in the present invention are recycled fibers having a count that is close to one another, typically within the count range of regenerated cellulose fibers.

[0036] The term "recycled cotton fibres" in the following description refers to short cotton fibres obtained from mechanical treatments of yarns and fabrics, such as opening and sorting; a possible way to identify these fibres is to measure their average fibre length. In an embodiment, the average fibre length L(n) measured according to DIN 53805:1980-06 is in the range of 6-16 mm. Noil falls within the definition of recycled cotton fibres. As is well known, noil are short fibres generated as waste during yarn manufacture and are usually removed from the yarn during the combing process.

[0037] In the final sheath mixture, the high 5%(n) index is mainly due to the presence of long regenerated cellulose fibres, whereas the high SFC(n) value is mainly due to the presence of short primary staple fibres, e.g. recycled cotton fibres with a high proportion of short fibres.

[0038] According to the invention, the yarn is a core-spun yarn having a core comprising or consisting of polyester filaments. The linear density of the polyester filaments ranges from 20 to 300 denier. The number of filaments ranges from 6 to 288, and the total number in the final yarn ranges from 5 / 1 to 60 / 1Ne. In a preferred embodiment, the weight ratio of the polyester filaments ranges from 10 to 35% with respect to the total weight of the yarn.

[0039] According to one aspect of the invention, the yarn comprises a filament core and a staple fiber sheath. The fiber sheath is made of a first staple fiber and a second staple fiber. The first staple fiber is a natural cellulosic fiber, preferably a recycled cotton staple fiber having an average length of 6-16 mm, more preferably about 10 mm.

[0040] The second staple fibers are synthetic fibers, e.g., regenerated staple fibers, preferably viscose, and have an average length greater than that of the first staple fibers, preferably 25 mm to 40 mm, more preferably 28 mm to 36 mm. In particular, high quality yarns have been obtained with second staple fibers of about 32 mm, such as 30 mm to 34 mm.

[0041] At least 95% of the fibres of the sheath are the aforementioned first and second staple fibres, the weight ratio of the first staple fibres to the second staple fibres being (less than) 20 / 80 to 70 / 30. In other words, a preferred embodiment is such that the sheath comprises (at least 95% of its weight) a mixture consisting of 20% to 70% of the first staple fibres, i.e. recycled cotton fibres, and the remaining 80% to 30% by weight of the mixture consists of the second staple fibres, i.e. viscose.

[0042] As previously mentioned, the blend of fiber sheath and the presence of one or more polyester filaments in the core allows the claimed fibers and filaments to be processed into yarns and, as a result, fabrics with superior market properties. In particular, the resulting yarns can be ring spun, a process that was previously not possible with yarns containing a high percentage of staple fibers, such as recycled cotton fibers. The breaking elongation of the polyester filaments of the filament core, when tested according to DIN ISO2062, is less than 15%, preferably 5% to 15%, more preferably 8% to 12%, and further preferably 10% to 12%.

[0043] As mentioned above, the average length of the second staple fibers in the sheath is greater than the average length of the first staple fibers. The fiber length can be measured by suitable machines such as the Uster Afis Pro 2 or the TexTechno FCS-Fibro test, according to DIN 53805:1980-06 (Advanced Fiber Information System) or by methods known in the art such as ASTM D1447.

[0044] To measure the fiber properties and fiber length of the sheath of a finished yarn (i.e., L(n), SFC(n), and 5%(n) values), it is first necessary to separate the sheath from the core. This can be done by untwisting the yarn (i.e., applying an opposite twist to one of the yarns, e.g., applying an S twist to a Z-twisted yarn). This can be done manually or on a yarn twisting machine. The resulting fibers can be tested to determine their nature, i.e., the presence of natural and regenerated cellulose fibers. Known methods include AATCC 20 and 20A, or ISO 1833. The fiber length can then be tested, for example, via DIN 53805 or ASTM D1447, Uster Afis Pro 2 or TexTechno FCS-Fibro test.

[0045] Preferably, the length of the second short fibers is not much greater than that of the first short fibers, in order to improve the interaction between the first and second short fibers of the sheath. The preferred ratio between the average length L(n) of the second short fibers and the average length L(n) of the first short fibers is between 1.5 and 3.8, more preferably between 2 and 3.5. It has been found that the best results are obtained when said ratio is between 2.5 and 3.3.

[0046] The yarn according to one or more of the above-mentioned embodiments can be used to manufacture fabrics, in particular fabrics (preferably denim) and garments comprising such fabrics. In particular, it is possible to manufacture fabrics using the yarn according to the invention in both the warp and weft direction.

[0047] It has been found that such fabrics, and in particular garments made from such fabrics, can be made without virgin (i.e., regular) cotton and have similar wear characteristics (hand, softness, etc.) and optical characteristics (brightness, dyeability, etc.) as fabrics made from regular cotton yarns. Also, compared to fabrics made from regular cotton yarns, the fabrics of the present invention exhibit similar mechanical properties, such as similar tensile strength, as well as better wear characteristics.

[0048] As an example, the abrasion of a fabric can be tested to BS ENISO 12947-2 method e test, where 25,000 to 30,000 cycles are run. If the test is continued after these number of cycles until the fabric breaks, the fabric of the present invention will have a greater resistance (i.e., break after a greater number of cycles) than a standard cotton yarn fabric or a fabric made with recycled cotton yarn.

[0049] When three identical garments are tested, the only difference between the garments is that a first garment is made with virgin cotton yarn, a second garment is made with yarn containing recycled cotton, and a third garment is made according to the present invention with recycled cotton fibres as the first staple fibre, and when the tested garments are subjected to abrasion testing until they break, the third garment is tested to be two to three times as durable as the first garment and three to four times as durable as the second garment.

[0050] The core may be composed of a plurality of polyester filaments and may also include elastomeric filaments such as elastane, typically in this case the core is composed of polyester filaments and elastomeric filaments. The elastomeric filaments, which typically range from 40 to 140 denier, are typically drafted (stretched) at least 2.0 times, and more preferably about 3 times, before being applied to the sheath, to reduce their yarn count in the yarn (a 3.0 draft would result in about 13 to 47 denier).

[0051] The present invention also relates to a method for producing a yarn, comprising the steps of: a) selecting a filament core comprising a plurality of polyester filaments; b) selecting a first staple fiber, the first staple fiber being a natural cellulose fiber; c) selecting second staple fibers that are regenerated cellulose fibers; and d) providing a staple fiber sheath, the weight ratio of the mixture of said first staple fibers and said second staple fibers being in the range of 20 / 80 to 70 / 30. wherein the average length of the sheath fibers is between 10 and 34 mm, preferably between 12 and 29 mm, the 5%(n) index of the sheath fibers is between 25 and 40 mm, preferably between 28 and 38 mm, and the short fiber content SFC(n) of the sheath is between 2% and 70%, more preferably between 10% and 60%, and said filament core and said short fiber sheath are combined by ring spinning.

[0052] The present invention also relates to a method for producing a yarn, comprising the steps of: a) selecting a filament core comprising a plurality of polyester filaments; b) selecting a staple fiber sheath, at least 95% of the sheath being made of first staple fibers and second staple fibers; and c) combining said filament core and said staple fiber sheath, preferably by ring spinning. wherein the first short fibers are natural cellulose fibers and preferably have an average length of 6 to 16 mm; the second short fibers are regenerated cellulose fibers and preferably have an average length longer than the first fibers, preferably exceeding 25 mm, more preferably exceeding 30 mm; The first staple fibers are recycled cotton fibers, and the second staple fibers are regenerated cellulose fibers, and the weight ratio of the first staple fibers to the second staple fibers is in the range of 20 / 80 to 70 / 30 (or less). As mentioned above, preferably recycled materials are used, so that the first staple fibers of the sheath are recycled cotton fibers and / or the polyester filaments are made from recycled polyester. [Brief description of the drawings]

[0053] [Figure 1] 1 is a histogram of recycled cotton fibers. [Figure 2a] 1 is a histogram of the fiber blend of the yarn sheath according to the present invention, the blend (weight percentage) being 20% ​​recycled cotton and 80% viscose. [Figure 2b] 1 is a histogram of the fiber blend of the yarn sheath according to the present invention, the blend (weight percent) being 50% recycled cotton and 50% viscose. [Figure 3a] 1 is a comparison of tests performed on fibers of the same yarn made according to the present invention, shown removed from the fabric. [Figure 3b] 1 is a comparison of tests performed on fibers of the same yarn made in accordance with the present invention, shown before being woven. [Figure 4] FIG. 1 shows the preferred range of L(n) as a function of the percentage of natural cellulose fibers. [Diagram 5]FIG. 1 shows the preferred range of SFC(n) as a function of the percentage of natural cellulose fibers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0054] Exemplary and non-limiting embodiments are described below with reference to the accompanying non-limiting figures. For ease of discussion, the general discussion below refers to the following: Recycled cotton fibers as the primary fiber of the sheath: However, unless otherwise specified, the following description applies to other natural cellulosic fibers as the primary fiber of the sheath. Viscose fibres as the second fibre of the sheath:However, unless otherwise specified, the following description applies to other regenerated cellulose fibres as the second fibre of the sheath. The elastane filaments may be present as one or more elastomeric filaments within the core; however, unless otherwise specified, the following description applies to a single elastane filament as well as to a core containing one or more different elastomeric filaments.

[0055] In a preferred embodiment, the yarn comprises a core with polyester filaments and possibly also elastane filaments, and the sheath is made of staple fibers including recycled cotton and viscose fibers. The polyester filaments usually comprise within 10%-35% of the total weight of the yarn, usually about 20% of the yarn. The overall count of the polyester filaments is typically 20-300 denier, although in the most preferred embodiment, a polyester count of 75-100 denier is used. The elongation at break of the polyester filaments (i.e. the polyester component of the core) is less than 15%, more preferably between 8% and 12%, even more preferably between 10% and 12%. The test for measuring the elongation at break is DINISO 2062.

[0056] In comparison, conventional polyester yarns initially produced in the same manner, but produced without the claimed draft, will be heavier (i.e., have a higher count) and, when tested in the same test, will have an elongation at break in excess of 15%, typically in the range of about 17%-25%. Elastane, when present, is usually highly elongated (draft greater than 2.0, usually about 3.0) and is present in the yarn in small amounts, thus usually about 5-15% of the total yarn weight.

[0057] According to one aspect of the invention, the polyester filaments and the elastane filaments are joined at least at a plurality of connection points by known methods, preferably by interweaving, twisting, or mechanical co-extrusion. As mentioned above, the elastane filaments are preferably stretched before being joined with the polyester filaments. According to one aspect of the invention, the continuous core fiber and the elastomeric filaments are continuously or substantially continuously combined, preferably under tension, by "mechanical co-extrusion" of the filaments. During such co-extrusion (also called co-feeding), two (or more) fiber bundles (under tension) are passed (fed together) through a restriction, causing the fibers to adhere to the extent that they remain attached after exiting the restriction.

[0058] The sheath is made of staple fibers, at least 95% of which is a blend of recycled cotton fibers and regenerated cellulose fibers, preferably viscose fibers. In a preferred embodiment, the blend contains 20% to 80% (more preferably 20% to 70%) recycled cotton fibers by weight, with the remainder of the blend being viscose fibers. The average length of the recycled cotton fibers is between 6 and 16 mm. Typically, 90% or more (by number) of the recycled cotton fibers are less than 30 mm. Embodiments are contemplated in which 50% of the fibers are less than 15 mm.

[0059] The viscose fibers are longer than the recycled cotton fibers to provide strength to the sheath, but as previously mentioned, it is preferred that the viscose fibers are not much longer than the recycled cotton fibers to promote bonding and intermixing of the sheath fibers. The average length of the viscose fibres is more than 25 mm, preferably more than 30 mm, and usually between 28 mm and 36 mm. In particular, it has been pointed out that if the viscose fibers are too long, the quality of the final yarn may be reduced. In consideration of this, in the most preferred embodiment, viscose fibers of about 32 mm, for example 30 mm to 34 mm, are used. Generally, regenerated cellulose staple fibers such as viscose staple fibers are produced by cutting viscose filaments, and therefore have a uniform length.

[0060] The viscose filaments are selected so that their average length is 1.5 to 3.8 times, preferably 2 to 3.5 times, and more preferably 2.5 to 3.3 times, the average length of the recycled cotton fibers. As mentioned above, the viscose fiber and the recycled cotton fiber are mixed so that they account for at least 95% by weight of the sheath fiber. The ratio (by weight) of the viscose fiber to the recycled cotton fiber is 20 / 80 to 80 / 20, preferably 20 / 80 to 70 / 30.

[0061] The average length L(n) of the sheath fibers is 10-34 mm, preferably 12-29 mm, the 5%(n) index of the sheath fibers is at least 25 mm, preferably 25 mm-40 mm, more preferably 28-38 mm. The short fiber content SFC(n) of the sheath is 2%-70%. As mentioned above, the L(n) and 5%(n) indices are functions of the percentage of cotton in the blend (i.e., the weight ratio of cotton to viscose).

[0062] It has been found that as the percentage of cotton increases, the L(n) index decreases. This relationship can be roughly approximated as an inverse proportional relationship. A better approximation is a negative parabolic relationship with a very small quadratic component. Similarly, it has been found that as the percentage of cotton increases, the 5%(n) index increases. This relationship can be roughly approximated as a proportional relationship. A better approximation is a parabolic relationship with a very small quadratic component. L(n) as a function of percentage of cotton in an exemplary embodiment is shown in FIG. 4, and the possible trend of the SFC(n) index is shown in FIG. 5.

[0063] In view of the above, preferred embodiments provide narrow ranges for the L(n) and SFC(n) indices as a function of the percentage of cotton in the cotton / viscose blend. In particular, in embodiments where the ratio of the first short fibers to the second short fibers is in the range of 20 / 80 (or more) to 30 / 70 (less), the average length of the sheath fibers is in the range of 19-34 mm, preferably 21-29 mm, and the sheath short fiber content SFC(n) is in the range of 2%-41%, preferably 10%-31%.

[0064] In an embodiment in which the weight ratio of the first short fibers to the second short fibers is in the range of 30 / 70 (or more) to 40 / 60 (less), the average length of the sheath fibers is in the range of 18 to 33 mm, preferably 20 to 28 mm, and the sheath short fiber content SFC(n) is in the range of 3% to 43%, preferably 13% to 33%. In an embodiment in which the weight ratio of the first short fibers to the second short fibers is in the range of 40 / 60 (or more) to 50 / 50 (or less), the average length of the sheath fibers is in the range of 16 to 31 mm, preferably 18 to 26 mm, and the sheath short fiber content SFC(n) is in the range of 8% to 48%, preferably 18% to 38%.

[0065] In an embodiment in which the weight ratio of the first short fibers to the second short fibers is in the range of 50 / 50 (or more) to 60 / 40 (less), the average length of the sheath fibers is in the range of 15 to 30 mm, preferably 17 mm to 25 mm, and the sheath short fiber content SFC(n) is 14% to 54%, preferably 24% to 44%. In an embodiment in which the weight ratio of the first short fibers to the second short fibers is in the range of 60 / 40 (or more) to 70 / 30 (less), the average length of the sheath fibers is in the range of 13 to 28 mm, preferably 15 mm to 23 mm, and the sheath short fiber content SFC(n) is 21% to 61%, preferably 31% to 51%.

[0066] In embodiments where the weight ratio of the first short fibers to the second short fibers is in the range of 70 / 30 (or more) to 80 / 20 (or more), preferably about 75 / 25, the average length of the sheath fibers is in the range of 10-25 mm, preferably 12-20 mm, while the sheath short fiber content SFC(n) is in the range of 30%-70%, preferably 40%-60.

[0067] In all the above embodiments, the 5%(n) index of the sheath fibers is from 25 mm to 40 mm, more preferably from 28 to 36 mm, and even more preferably from 30 to 34 mm. Manufacturing equipment is known in the art and will not be described in detail here.

[0068] The process for producing the yarn according to the invention comprises drawing polyester filaments to provide a core, optionally combined with elastane filaments. The core is then combined with a sheath, which is usually provided in the form of one or more rovings of staple fibers. The resulting product is then spun into yarn, preferably by ring spinning. The resulting yarns can be used in the manufacture of fabrics, in particular the yarns according to the invention can be used in fabrics, in particular they can be used as warp and / or weft yarns in the fabric.

[0069] In particular, the subject of the invention is a fabric, preferably a denim fabric, in which all warp and weft threads are yarns according to the invention. The warp threads can be dyed, for example with indigo dye, while the weft threads can be left undyed (although dyeing is possible). As mentioned above, the fabrics obtained with the yarns of the present invention have improved abrasion resistance performance compared to fabrics made with standard cotton yarns and recycled cotton yarns.

[0070] Below is an exemplary comparison: Fabric 1 is a fabric made with standard cotton yarns and Fabric 2 is a fabric made with warp and weft yarns according to the invention. Fabric 1 is made according to the following parameters: -Warp composition: 100% cotton -Warp count: 10 / 1 Ne -Weft composition: 94% cotton / 6% elastane - Weft count: 16 / 1 Ne -Fabric weave: denim fabric 3 / 1 -Fabric composition: 98% cotton / 2% elastane.

[0071] Fabric 2 is made according to the following parameters: -Warp composition: 61% recycled cotton / 20% viscose / 19% recycled polyester -Warp count: 10 / 1 Ne (same as Fabric 1) -Weft composition: 60% recycled cotton / 20% viscose / 14% recycled polyester / 6% elastane - Weft count: 16 / 1 Ne (same as Fabric 1) -Fabric weave: 3 / 1 denim fabric (same as fabric 1) -Fabric composition: 60% cotton / 20% viscose / 18% recycled polyester / 2% elastane. The two sets of fabrics were tested as shown in Table 1.

[0072] [Table 1]

[0073] Tear tests were performed according to ISO 13937-1 and were routinely subjected to 5 and 10 home washes at 40°C and then tumble dried. For each cell, the top line shows the crosswise value and the bottom line shows the longitudinal value.

[0074] [Table 2]

[0075] Tensile strength tests were performed according to ISO 1393-1 and were routinely subjected to 5 and 10 home washes at 40°C and then tumble dried. For each cell, the top line indicates the crosswise value and the bottom line indicates the longitudinal value.

[0076] [Table 3]

[0077] The abrasion test was carried out according to IS012947-2 and continued until the fabric under test broke.

[0078] As can be seen from the above tests, the fabric of the present invention has comparable tensile strength and slightly improved tear strength compared to standard virgin cotton fabric, resulting in the fabric of the present invention having similar abrasion resistance while maintaining similar optical properties compared to standard virgin cotton fabric.

[0079] The fabric of the present invention also exhibits better abrasion resistance, improving the lifespan of the fabric.Fiber composition and length can be tested according to the methods described above.

[0080] The fibers could be removed from the fabric before and after they were woven and tested with similar results. In this regard, Figures 1 and 2 are tests performed on fibers that have not been woven into a fabric. Figures 3a and 3b show a comparison of fibers from the same yarn set according to the invention, where the fibers in the test in Figure 3a are from yarns that have been removed from the fabric, and the fibers in the test in Figure 3b are from yarns after yarn manufacture before they are woven into a fabric. As can be seen, the fiber length distribution is substantially the same.

Claims

1. A method for producing a yarn, comprising the steps of: a. selecting a filament core comprising a plurality of polyester filaments; b. selecting a staple fiber sheath; c. combining the filament core and the staple fiber sheath by ring spinning; In step a), the elongation at break of the polyester filaments of the filament core is between 5% and 15% when tested according to DINISO 2062; A method for producing a yarn, characterized in that in step b, at least 95% by weight of the sheath is composed of first staple fibers and second staple fibers, the first staple fibers being recycled cotton fibers and the second staple fibers being regenerated cellulose fibers.

2. 2. The method of claim 1, wherein the weight ratio of the first staple fiber to the second staple fiber is in the range of 20 / 80 to 70 / 30 (or less).

3. 3. A method for producing a yarn according to claim 1 or 2, characterized in that the recycled cotton fibres have an average length L(n) of 6 to 16 mm and / or the regenerated cellulose fibres have an average length L(n) of 25 to 40 mm.

4. A method for producing a yarn, comprising the steps of: a. selecting a filament core comprising a plurality of polyester filaments, the filament core having a polyester filament elongation at break in the range of 5% to 15%, more preferably between 10% to 12%, when tested to DINISO 2062; b. selecting a first staple fiber, the first staple fiber being a natural cellulose fiber; c. selecting second staple fibers that are regenerated cellulose fibers; d. providing a staple fiber sheath comprising at least 95% by weight of the mixture of the first staple fibers and the second staple fibers; e. combining said filament core and said staple fiber sheath by ring spinning; a weight ratio of the first staple fibers to the second staple fibers is in the range of 20 / 80 to 70 / 30 (or less); the average length of the fibers in the sheath is between 10 and 34 mm; The 5%(n) index of the fibers of the sheath is between 25 mm and 40 mm; 2. A method for producing a yarn, comprising the steps of: producing a yarn having a sheath short fiber content SFC(n) of 2% to 70%.

5. 5. A method for producing a yarn according to claim 1 or 4, wherein the polyester filaments of the core are made from recycled polyester.

6. A method for producing the yarn according to any one of claims 1 and 4, comprising the steps of: a. the weight ratio of the first short fibers to the second short fibers is in the range of 20 / 80 (or more) to 30 / 70 (or less); i. the average length of the fibers in the sheath is in the range of 19 to 34 mm; ii. the short fiber content SFC(n) of the sheath is between 2% and 41%; or b. The weight ratio of the first short fibers to the second short fibers is in the range of 30 / 70 (or more) to 40 / 60 (or less); i. the average length of the fibers in the sheath is in the range of 18 to 33 mm; ii. the short fiber content SFC(n) of the sheath is between 3% and 43%; or c. The weight ratio of the first staple fiber to the second staple fiber is in the range of 40 / 60 (or more) to 50 / 50 (or less); i. the average length of the fibers in the sheath is in the range of 16 to 31 mm; ii. the short fiber content SFC(n) of the sheath is between 8% and 48%; or d. the weight ratio of the first staple fiber to the second staple fiber is in the range of 50 / 50 (or more) to 60 / 40 (or less); i. the average length of the fibers in the sheath is in the range of 15 to 30 mm; ii. the short fiber content SFC(n) of the sheath is between 14% and 54%; or e. the weight ratio of the first staple fiber to the second staple fiber is in the range of 60 / 40 (or more) to 70 / 30 (or less); i. the average length of the fibers in the sheath ranges from 13 to 28 mm; ii. A method for producing a yarn, characterized in that the short fiber content SFC(n) of the sheath is 21% to 61%.

7. A yarn comprising a filament core and a staple fiber sheath, the staple fiber sheath is made from or comprises at least 95% by weight of a mixture of first staple fibers and second staple fibers, the first staple fibers being natural cellulose fibers and the second staple fibers being regenerated cellulose fibers; a weight ratio of the first short fiber to the second short fiber is in the range of 20 / 80 to 70 / 30 (or less); the average length of the fibers in the sheath is in the range of 10 to 34 mm; The 5% (n) index of the fibers of the sheath is between 25 and 40 mm; the short fiber content SFC(n) of the sheath is between 2% and 70%; the filament core comprises a plurality of polyester filaments; A yarn characterized in that the elongation at break of the polyester filaments of the filament core, measured according to DINISO 2062, is in the range of 5% to 15%.

8. The yarn of claim 7, a. the weight ratio of the first short fibers to the second short fibers is in the range of 20 / 80 (or more) to 30 / 70 (or less); i. the average length of the fibers in the sheath is in the range of 19 to 34 mm; ii. the short fiber content SFC(n) of the sheath is in the range of 2% to 41%; or b. the weight ratio of the first staple fiber to the second staple fiber is in the range of 30 / 70 (or more) to 40 / 60 (or less); i. the average length of the fibers in the sheath is in the range of 18 to 33 mm; ii the short fiber content SFC(n) of the sheath is between 3% and 43%; or c. the weight ratio of the first staple fiber to the second staple fiber is in the range of 40 / 60 (or more) to 50 / 50 (or less); i. the average length of the fibers in the sheath is in the range of 16 to 31 mm; ii. the short fiber content SFC(n) of the sheath is between 8% and 48%; or d. the weight ratio of the first staple fiber to the second staple fiber is in the range of 50 / 50 (or more) to 60 / 40 (or less); i. the average length of the fibers in the sheath is in the range of 15 to 30 mm; ii. the short fiber content SFC(n) of the sheath is between 14% and 54%; or e. the weight ratio of the first staple fiber to the second staple fiber is in the range of 60 / 40 (or more) to 70 / 30 (or less); i. the average length of the fibers in the sheath ranges from 13 to 28 mm; ii. The short fiber content SFC(n) of the sheath is between 21% and 61%.

9. A yarn according to any one of claims 7 or 8, characterized in that the ratio of the average length of the regenerated cellulose fibers to the average length of the first short fibers is in the range of 1.5 to 3.

8.

10. 9. The yarn according to claim 7 or 8, characterized in that the core comprises one or more elastomeric filaments and has a draft of 2.0 to 4.

0.

11. 9. The yarn according to claim 7 or 8, characterized in that the draft of the polyester filaments is between 1.5 and 2.

5.

12. A yarn according to any one of claims 7 or 8, The yarn, wherein the polyester filaments are textured filaments.

13. A yarn according to any one of claims 7 or 8, A yarn, characterized in that the amount of said polyester filaments in said core ranges from 10% to 30% by weight of said yarn.

14. A yarn according to any one of claims 7 or 8, The yarn is characterized in that the total number of polyester filaments is from 50 to 150 denier.

15. 9. A fabric or garment comprising the yarn according to any one of claims 7 or 8.