Film-like adhesive for semiconductor, method for manufacturing the same, adhesive tape, semiconductor device, and method for manufacturing the same

The film adhesive for semiconductors, with separate adhesive regions, addresses the issue of oxidation and impurities in flip-chip bonding by reducing fillets and maintaining sealing performance, thereby improving connection reliability in semiconductor devices.

JP2024156394AActive Publication Date: 2024-11-06RESONAC CORP

Patent Information

Application Number
JP2023070817
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-11-06
Estimated Expiration
2043-04-24

AI Technical Summary

Technical Problem

Existing methods for connecting semiconductor chips and substrates, such as flip-chip bonding, face challenges due to oxidation of metal surfaces forming oxide films and impurities, which degrade connection reliability and sealing performance.

Method used

A film adhesive for semiconductors is developed with distinct adhesive regions: one region without a flux compound and another with a flux compound, composed of specific epoxy resins, imidazole curing agents, and (meth)acrylic compounds, designed to suppress fillet formation while ensuring sufficient sealing performance.

Benefits of technology

The adhesive effectively reduces fillet formation and maintains sealing performance, enhancing connection reliability by controlling adhesive flow and curing rates, thus improving the integrity of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156394000006
    Figure 2024156394000006
  • Figure 2024156394000007
    Figure 2024156394000007
  • Figure 2024156394000008
    Figure 2024156394000008
Patent Text Reader

Abstract

To provide a film-like adhesive for a semiconductor capable of suppressing an amount of generation of a fillet while securing sufficient sealing property.SOLUTION: A film-like adhesive for a semiconductor includes a first adhesive region including no flux compound and a second adhesive region including a flux compound along a thickness direction. The first adhesive region includes a first epoxy resin, a first imidazole-based curing agent, and a (meth) acrylic compound. The second adhesive region includes a second epoxy resin, a second imidazole-based curing agent, and a flux compound.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a film-like adhesive for semiconductors, a method for producing a film-like adhesive for semiconductors, an adhesive tape, a method for producing a semiconductor device, and a semiconductor device. [Background technology]

[0002] Conventionally, wire bonding using thin metal wires such as gold wires has been widely used to connect semiconductor chips and substrates. On the other hand, in order to meet the demands for higher performance, higher integration, higher speed, etc. for semiconductor devices, flip chip connection (FC connection) in which conductive protrusions called bumps are formed on the semiconductor chip or substrate to directly connect the semiconductor chip and substrate is becoming more widespread.

[0003] For example, the COB (Chip On Board) type connection method, which is widely used for BGA (Ball Grid Array), CSP (Chip Size Package), etc., in connection between semiconductor chips and substrates, also corresponds to the FC connection method. The FC connection method is also widely used in the COC (Chip On Chip) type connection method, which forms connection parts (e.g., bumps and wiring) on ​​semiconductor chips to connect between semiconductor chips.

[0004] In addition, for packages that are strongly required to be smaller, thinner, and more functional, chip-stack packages, POP (Package On Package), TSV (Through-Silicon Via), etc., which stack and multi-layer chips using the above-mentioned connection method, are beginning to become widespread. These stacking and multi-layering technologies arrange semiconductor chips and other components three-dimensionally, making it possible to make packages smaller than methods that arrange them two-dimensionally. In addition, they are also effective in improving semiconductor performance, reducing noise, reducing mounting area, and saving power, and are therefore attracting attention as the next-generation semiconductor wiring technology.

[0005] Generally, metal bonding is used to connect the connecting parts from the viewpoint of ensuring sufficient connection reliability (e.g., insulation reliability). The main metals used for the above-mentioned connecting parts (e.g., bumps and wiring) include solder, tin, gold, silver, copper, nickel, etc., and conductive materials containing a plurality of these metals are also used. The metals used for the connecting parts may have impurities on the connecting surfaces of the connecting parts due to the surface being oxidized to form an oxide film, and impurities such as oxides adhering to the surface. If such impurities remain, the connection reliability (e.g., insulation reliability) between the semiconductor chip and the substrate, or between two semiconductor chips, may decrease, and there is a concern that the advantage of adopting the above-mentioned connecting method may be lost.

[0006] In addition, one method of suppressing the generation of these impurities is to coat the connection parts with an oxidation-preventing film, known as OSP (Organic Solderbility Preservatives) treatment, but this oxidation-preventing film can sometimes cause a decrease in solder wettability and connectivity during the connection process.

[0007] As a method for removing the above-mentioned oxide film and impurities, there have been proposed a method using a single-layer film containing a flux agent in a semiconductor material (see, for example, Patent Document 1), a method using a two-layer film consisting of a thermosetting resin layer and a thermoplastic resin layer containing an acid component (see, for example, Patent Document 2), and the like. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2013 / 125086 [Patent Document 2] International Publication No. 2016 / 117350 Summary of the Invention [Problem to be solved by the invention]

[0009] An object of one aspect of the present disclosure is to provide a film-like adhesive for semiconductors that can reduce the amount of fillet formation while ensuring sufficient sealing properties. [Means for solving the problem]

[0010] This disclosure provides the following [1] to

[15] .

[0011] [1] A first adhesive region along a thickness direction is free of a flux compound and a second adhesive region is inclusive of a flux compound; the first adhesive region comprises a first epoxy resin, a first imidazole-based curing agent, and a (meth)acrylic compound; The second adhesive region includes a second epoxy resin, a second imidazole-based curing agent, and the flux compound.

[0012] [2] The film-like adhesive for semiconductors described in [1], wherein the first adhesive region does not contain a radical polymerization initiator.

[0013] [3] The film-like adhesive for semiconductors according to [1] or [2], wherein at least one of the first epoxy resin and the second epoxy resin contains an epoxy resin that is liquid at 25°C.

[0014] [4] The film-like adhesive for a semiconductor according to any one of [1] to [3], wherein at least one of the first epoxy resin and the second epoxy resin contains a triphenolmethane type epoxy resin.

[0015] [5] The film-like adhesive for a semiconductor according to any one of [1] to [4], wherein at least one of the first imidazole-based curing agent and the second imidazole-based curing agent has a triazine ring.

[0016] [6] A film-like adhesive for semiconductors described in any of [1] to [5], wherein the ratio of the content of the first epoxy resin to the content of the (meth)acrylic compound in the first adhesive region is 3 to 11, in terms of mass ratio.

[0017] [7] The film-like adhesive for semiconductors according to any one of [1] to [6], wherein the (meth)acrylic compound comprises a polyfunctional (meth)acrylic compound having 2 to 8 (meth)acryloyl groups.

[0018] [8] The film-like adhesive for a semiconductor according to any one of [1] to [7], wherein the flux compound contains a polycarboxylic acid.

[0019] [9] The thickness of the first adhesive region is 1 to 50 μm; The film-like adhesive for a semiconductor according to any one of [1] to [8], wherein the thickness of the second adhesive region is 0.5 to 2 times the thickness of the first adhesive region.

[0020]

[10] The film-like adhesive for a semiconductor according to any one of [1] to [9], which is non-conductive.

[0021]

[11] The film-like adhesive for semiconductors according to any one of [1] to

[10] , which is used to bond a semiconductor chip and a base and to seal a gap between the semiconductor chip and the base.

[0022]

[12] A method for producing a film-like adhesive for semiconductors according to any one of [1] to

[11] , providing one of a first adhesive layer and a second adhesive layer on the other; the first adhesive layer does not contain a flux compound, and is a layer containing the first epoxy resin, the first imidazole-based curing agent, and the (meth)acrylic compound; A method for producing a film-like adhesive for semiconductors, wherein the second adhesive layer is a layer containing the second epoxy resin, the second imidazole-based curing agent, and the flux compound.

[0023]

[13] [1] to

[11] , and An adhesive tape comprising: a backgrind tape provided on the film-like adhesive for semiconductors, the backgrind tape being provided on the opposite side of the first adhesive region from the second adhesive region.

[0024]

[14] A step of preparing a semiconductor chip with a film-like adhesive, the semiconductor chip including a semiconductor chip and the film-like adhesive for semiconductor according to any one of [1] to

[11] , the film-like adhesive for semiconductor being provided on the semiconductor chip such that the surface of the first adhesive region opposite to the second adhesive region faces the semiconductor chip; a step of placing the semiconductor chip with the film-like adhesive on a base from the film-like adhesive side, and heating the semiconductor chip to electrically connect the connection portion of the semiconductor chip to the connection portion of the base and seal the gap between the semiconductor chip and the base.

[0025]

[15] a semiconductor chip having a first connection portion, a base having a second connection portion electrically connected to the first connection portion, and a sealing portion that bonds the semiconductor chip and the base and fills a gap between the semiconductor chip and the base, A semiconductor device, wherein the sealing portion is a cured product of the film-like adhesive for a semiconductor according to any one of [1] to

[11] . Effect of the Invention

[0026] According to the present disclosure, it is possible to provide a film-like adhesive for semiconductors that can reduce the amount of fillet generation while ensuring sufficient sealing properties. [Brief description of the drawings]

[0027] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of the film-like adhesive for semiconductors of the present disclosure. [Diagram 2] FIG. 2(a) is a schematic cross-sectional view showing one embodiment of a semiconductor device according to the present disclosure, and FIG. 2(b) is a schematic cross-sectional view showing another embodiment of a semiconductor device according to the present disclosure. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing another embodiment of the semiconductor device according to the present disclosure. [Figure 4] 4A to 4C are cross-sectional views illustrating steps in one embodiment of a method for manufacturing a semiconductor device according to the present disclosure. [Diagram 5] FIG. 5 is a cross-sectional view illustrating a process following the process in FIG. [Figure 6] FIG. 6 is a cross-sectional view illustrating a process following the process in FIG. [Figure 7] FIG. 7 is a cross-sectional view illustrating a process following the process in FIG. [Figure 8] FIG. 8 is a cross-sectional view illustrating a process following the process in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] In this specification, "(meth)acrylic" means at least one of acrylic and the corresponding methacrylic. The same applies to other similar expressions such as "(meth)acryloyl" and "(meth)acrylate". In addition, a numerical range indicated using "~" indicates a range including the numerical values ​​described before and after "~" as the minimum and maximum values, respectively. In addition, in the numerical range described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples. In addition, the upper limit and lower limit values ​​described individually can be arbitrarily combined. In addition, the materials exemplified below may be used alone or in combination of two or more types, unless otherwise specified. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified.

[0029] Hereinafter, an embodiment of the present disclosure will be described in detail with reference to the drawings as needed. In the drawings, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted. In addition, unless otherwise specified, the positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to the illustrated ratios.

[0030] <Film adhesive for semiconductors> One embodiment of a film-type adhesive for semiconductors (hereinafter simply referred to as "film-type adhesive") is an adhesive used for connecting (joining) and sealing connection members such as semiconductor chips, and is preferably used for joining a semiconductor chip to a base and sealing gaps between the semiconductor chip and the base.

[0031] FIG. 1 is a schematic cross-sectional view showing a film-like adhesive of one embodiment. The film-like adhesive 1 shown in the figure has a first adhesive region 2 that does not contain a flux compound and a second adhesive region 3 that contains a flux compound along the thickness direction (the vertical direction in FIG. 1). The first adhesive region 2 contains an epoxy resin, an imidazole-based curing agent, and a (meth)acrylic compound, and the second adhesive region contains an epoxy resin, an imidazole-based curing agent, and the above-mentioned flux compound. Hereinafter, the adhesive constituting the first adhesive region 2 is referred to as the first adhesive, and the adhesive constituting the second adhesive region 3 is referred to as the second adhesive. In addition, the epoxy resin and the imidazole-based curing agent contained in the first adhesive are referred to as the first epoxy resin and the first imidazole-based curing agent, respectively, and the epoxy resin and the imidazole-based curing agent contained in the second adhesive are referred to as the second epoxy resin and the second imidazole-based curing agent, respectively.

[0032] The first adhesive region 2 and the second adhesive region 3 have a predetermined thickness and extend along the main surface direction of the film-like adhesive 1 (left and right direction in FIG. 1), for example, as shown in FIG. 1. The first adhesive region 2 and the second adhesive region 3 may be layered. That is, the first adhesive region 2 and the second adhesive region 3 may be a first adhesive layer and a second adhesive layer, respectively. The boundary between the first adhesive region 2 and the second adhesive region 3 is not necessarily clear and may not be visible. In FIG. 1, the first adhesive region 2 and the second adhesive region 3 are adjacent to each other, but a region different from the first adhesive region 2 and the second adhesive region 3 (for example, a region containing a mixture of the first adhesive and the second adhesive) may be present between the first adhesive region 2 and the second adhesive region 3.

[0033] However, in recent years, as the functionality and integration of packages have become more sophisticated, the gap between layers and the pitch between wirings have become narrower, so that the adhesive that flows during connection is more likely to overflow from the edge of the connection member (e.g., a semiconductor chip), and overflowing parts called fillets are more likely to be formed. Since such fillets can cause damage to the connection member, there is a need to develop a method for reducing the amount of fillets that occur while ensuring sufficient sealing. If an adhesive with low fluidity is simply used to suppress fillets, the gap between the connection parts of the connection members may not be sufficiently filled with adhesive, which may cause defects such as voids, so it is difficult to solve the above problem by simply reducing the fluidity of the adhesive.

[0034] On the one hand, as a result of the inventors' studies, it has been clarified that according to the above film-like adhesive, it is possible to suppress the generation of voids and the generation of fillets due to excessive flow of the adhesive when connecting connection members while ensuring sufficient sealing properties. Although the reason for such an effect is not clear, since the first adhesive region 2 and the second adhesive region 3 have the above specific compositions, the first adhesive region 2 has an appropriate fluidity that hardly causes an unfilled portion that causes void generation during pasting, and at the same time, it is inferred that the first adhesive region 2 cures earlier than the second adhesive region 3 during connection and hardly causes excessive flow that causes fillet generation, and the second adhesive region 3 is more likely to flow than the first adhesive region 2 and hardly causes an unsealed portion, etc. are the reasons.

[0035] The thickness of the first adhesive region 2 (the length in the thickness direction of the film-like adhesive 1) may be appropriately set in relation to the height of the connection portion in the connection member to which the film-like adhesive 1 is pasted. Assuming that the height of the connection portion is y1 and the thickness of the first adhesive region 2 is x1, from the viewpoint that the cured product of the first adhesive is difficult to intervene between the connection portions and the connection reliability can be further improved, it is preferable that x1 < y1, and it is more preferable that 1.0x1 < y1 ≤ 1.5x1. Specifically, the thickness of the first adhesive region 2 may be 1 to 50 μm, and may also be 3 to 50 μm, 4 to 30 μm, or 5 to 20 μm.

[0036] The thickness of the second adhesive region 3 may be 0.5 to 2 times the thickness of the first adhesive region 2, and may also be 0.5 to 2.5 times or 0.5 to 3 times. Specifically, the thickness of the second adhesive region 3 (the length in the thickness direction of the film-like adhesive 1) may be 1 to 50 μm, and may also be 3 to 50 μm, 4 to 30 μm, or 5 to 20 μm.

[0037] The thickness of the film-like adhesive 1 (for example, the sum of the thickness of the first adhesive region 2 and the thickness of the second adhesive region 3) may be appropriately set in relation to the connection parts of the connection member. When the sum of the heights of the connection parts is x and the total thickness of the film-like adhesive is y, the relationship between x and y preferably satisfies 0.70x≦y≦1.3x, and more preferably satisfies 0.80x≦y≦1.2x, from the viewpoint of the connectivity during pressure bonding and the filling property of the adhesive. From the viewpoint of making it difficult for the cured product of the first adhesive to intervene between the connection parts and further improving the connection reliability, it is preferable to satisfy y>x. Specifically, the thickness of the film-like adhesive 1 may be 2 to 100 μm, or may be 6 to 100 μm, 8 to 60 μm, or 10 to 40 μm.

[0038] The first adhesive constituting the first adhesive region 2 and the second adhesive constituting the second adhesive region 3 will be described below.

[0039] (First adhesive) The first adhesive contains a first epoxy resin, a first imidazole-based curing agent, and a (meth)acrylic compound, but does not contain a flux compound. Here, the fact that the first adhesive does not contain a flux compound means that the content of the flux compound in the first adhesive is equal to or lower than the current detection limit (for example, equal to or lower than 0.01 mass% based on the total amount of the first adhesive).

[0040] [First epoxy resin] The first epoxy resin is a compound having two or more epoxy groups in the molecule. For example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, naphthalene type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, phenol aralkyl type epoxy resin, biphenyl type epoxy resin, triphenylmethane type epoxy resin, triphenolmethane type epoxy resin, dicyclopentadiene type epoxy resin and various multifunctional epoxy resins can be used as the first epoxy resin. These can be used alone or as a mixture of two or more kinds. Among these, when a triphenolmethane type epoxy resin (an epoxy resin containing a triphenolmethane skeleton) is used, the amount of fillet generation tends to be further reduced.

[0041] From the viewpoint of preventing the first epoxy resin from decomposing and generating volatile components during connection at high temperatures, it is preferable to use an epoxy resin whose thermal weight loss rate at 250°C is 5% or less when the temperature during connection is 250°C, and it is preferable to use an epoxy resin whose thermal weight loss rate at 300°C is 5% or less when the temperature during connection is 300°C.

[0042] As the first epoxy resin, an epoxy resin that is liquid at 25°C (hereinafter simply referred to as "liquid epoxy resin") may be used from the viewpoint of easily suppressing the occurrence of cracks and fissures on the film surface. Here, "liquid at 25°C" means that the viscosity at 25°C measured with an E-type viscometer is 400 Pa·s or less. Examples of liquid epoxy resins include glycidyl ethers of bisphenol A type, glycidyl ethers of bisphenol AD ​​type, glycidyl ethers of bisphenol S type, glycidyl ethers of bisphenol F type, glycidyl ethers of water-added bisphenol A type, glycidyl ethers of ethylene oxide adducts of bisphenol A type, glycidyl ethers of propylene oxide adducts of bisphenol A type, glycidyl ethers of naphthalene resins, trifunctional or tetrafunctional glycidyl amines, and the like.

[0043] The content of the liquid epoxy resin in the first adhesive is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, based on the total amount of the first epoxy resin contained in the first adhesive, from the viewpoint of easily suppressing the occurrence of cracks and fissures on the film surface. The content of the liquid epoxy resin is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on the total amount of the first epoxy resin, from the viewpoint of easily suppressing an excessive increase in tackiness of the film and from the viewpoint of easily suppressing edge fusion.

[0044] The epoxy equivalent of the first epoxy resin may be 100 to 3000 g / eq, or 100 to 2000 g / eq, or 100 to 1500 g / eq. When the epoxy equivalent of the first epoxy resin is within the above range, the balance between reactivity and fluidity during heating tends to be good.

[0045] The content of the first epoxy resin in the first adhesive is preferably 25% by mass or more, more preferably 30% by mass or more, and even more preferably 35% by mass or more, based on the total amount of the first adhesive, from the viewpoint of easily suppressing the occurrence of fillets. The content of the first epoxy resin is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less, based on the total amount of the first adhesive, from the viewpoint of easily obtaining good sealing properties and easily suppressing the occurrence of voids.

[0046] The content of the first epoxy resin in the first adhesive may be set in relation to the content of the (meth)acrylic compound. When the ratio of the content of the first epoxy resin to the content of the (meth)acrylic compound in the first adhesive is 3 to 11 in mass ratio, high connection reliability is easily obtained, and the occurrence of fillets tends to be further reduced. The above ratio may be 5 or more, 7 or more, or 9 or more from the viewpoint of further reducing the occurrence of fillets, and may be 10 or less from the viewpoint of easily obtaining good sealing properties and easily suppressing the occurrence of voids in addition to the above effect.

[0047] [First imidazole curing agent] Examples of the imidazole-based curing agent include 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, and 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine. -[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and adducts of epoxy resin and imidazoles. In addition, latent curing agents in which these are microencapsulated can also be used. These can be used alone or in combination of two or more. Among these, compounds having a triazine ring are preferably used from the viewpoint of obtaining better sealing properties and suppressing the occurrence of voids.

[0048] The content of the first imidazole curing agent in the first adhesive is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more, relative to 100 parts by mass of the first epoxy resin contained in the first adhesive, from the viewpoint of improving the curing property when heated. The content of the first imidazole curing agent is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of the first epoxy resin, from the viewpoint of making it more difficult for the first adhesive to be interposed between the connecting parts.

[0049] [(Meth)acrylic compounds] The (meth)acrylic compound is a compound having one or more (meth)acryloyl groups in the molecule. As the (meth)acrylic compound, for example, (meth)acrylic compounds containing a skeleton of bisphenol A type, bisphenol F type, naphthalene type, phenol novolac type, cresol novolac type, phenol aralkyl type, biphenyl type, triphenylmethane type, dicyclopentadiene type, fluorene type, adamantane type or isocyanuric acid type; various polyfunctional (meth)acrylic compounds (excluding (meth)acrylic compounds containing the above skeleton) can be used. As the polyfunctional (meth)acrylic compound, pentaerythritol tri(meth)acrylate, dipentaerythritol poly(meth)acrylate (dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, etc.), trimethylolpropane di(meth)acrylate, etc. can be mentioned. Among these, polyfunctional (meth)acrylic compounds are preferred, and dipentaerythritol poly(meth)acrylate is more preferred. The number of functional groups (the number of (meth)acryloyl groups) of the polyfunctional (meth)acrylic compound is preferably 2 to 8, more preferably 3 to 7, and even more preferably 4 to 6.

[0050] The molecular weight of the (meth)acrylic compound is, for example, 400 to 2000. The molecular weight of the (meth)acrylic compound is preferably smaller than 2000, and more preferably equal to or less than 1000. The smaller the molecular weight of the (meth)acrylic compound, the easier the reaction proceeds and the higher the curing reaction rate.

[0051] The (meth)acrylic compounds can be used alone or in combination of two or more.

[0052] The content of the (meth)acrylic compound in the first adhesive is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, based on the total amount of the first adhesive, from the viewpoint of further reducing the occurrence of fillets. The content of the (meth)acrylic compound is preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 5% by mass or less, based on the total amount of the first adhesive, from the viewpoint of improving sealing properties and suppressing the occurrence of voids. From these viewpoints, the content of the (meth)acrylic compound is preferably 1 to 10% by mass, more preferably 3 to 7% by mass, and even more preferably 3 to 5% by mass, based on the total amount of the first adhesive.

[0053] [Other ingredients] The first adhesive may further contain components other than those mentioned above (other components).

[0054] For example, the first adhesive may contain a thermosetting resin other than epoxy resin (a compound that hardens by reaction with a thermosetting agent by heat). Examples of thermosetting resins other than epoxy resin include phenol resin and acrylic resin. When the first adhesive contains a thermosetting resin other than epoxy resin, the content of the first epoxy resin in the first adhesive is preferably 80 mass % or more, more preferably 90 mass % or more, based on the total amount of the thermosetting resin contained in the first adhesive. The content of the first epoxy resin may be 100 mass % based on the total amount of the thermosetting resin.

[0055] For example, the first adhesive may contain a heat curing agent other than the imidazole-based curing agent. Examples of heat curing agents other than the imidazole-based curing agent include phenol resin-based curing agents, acid anhydride-based curing agents, amine-based curing agents, and phosphine-based curing agents. When the first adhesive contains a heat curing agent other than the imidazole-based curing agent, the content of the first imidazole-based curing agent in the first adhesive is preferably 80% by mass or more, more preferably 90% by mass or more, based on the total amount of the heat curing agent contained in the first adhesive, from the viewpoints that the curing can be rapidly progressed when heating is performed at a low temperature, and the connection reliability can be improved by the flux activity that suppresses the generation of an oxide film at the connection portion. The content of the first imidazole-based curing agent may be 100% by mass, based on the total amount of the heat curing agent.

[0056] Also, for example, the first adhesive may contain a radical polymerizable compound other than a (meth)acrylic compound (a compound capable of undergoing a radical polymerization reaction with the generation of radicals by heat, light, radiation, electrochemical action, etc.). Examples of radical polymerizable compounds other than a (meth)acrylic compound include vinyl compounds. When the first adhesive contains a radical polymerizable compound other than a (meth)acrylic compound, the content of the (meth)acrylic compound in the first adhesive is preferably 80% by mass or more, more preferably 90% by mass or more, based on the total amount of the radical polymerizable compound contained in the first adhesive. The content of the (meth)acrylic compound may be 100% by mass, based on the total amount of the radical polymerizable compound.

[0057] Also, for example, the first adhesive may contain a thermoplastic resin. The thermoplastic resin contributes to improving heat resistance and film formability. Examples of the thermoplastic resin include phenoxy resin, polyimide resin, polyamide resin, polycarbodiimide resin, cyanate ester resin, acrylic resin, polyester resin, polyethylene resin, polyethersulfone resin, polyetherimide resin, polyvinyl acetal resin, urethane resin, and acrylic rubber. Among these, from the viewpoint of easily obtaining excellent heat resistance and film formability, phenoxy resin, polyimide resin, acrylic rubber, cyanate ester resin, and polycarbodiimide resin are preferred, and phenoxy resin, polyimide resin, and acrylic rubber are more preferred. These thermoplastic resins can be used alone or as a mixture or copolymer of two or more kinds.

[0058] The weight average molecular weight of the thermoplastic resin is, for example, 10,000 or more, and may be 20,000 or more, or 30,000 or more. Such a thermoplastic resin can further improve the heat resistance and film formability of the first adhesive. The weight average molecular weight of the thermoplastic resin may be 1,000,000 or less, or may be 500,000 or less, from the viewpoint of easily obtaining an improved effect in heat resistance. In this specification, the weight average molecular weight means the weight average molecular weight measured in terms of polystyrene using high performance liquid chromatography (manufactured by Shimadzu Corporation, product name: C-R4A). For the measurement, for example, the following conditions can be used. Detector: LV4000 UV Detector (product name, manufactured by Hitachi, Ltd.) Pump: L6000 Pump (product name, manufactured by Hitachi, Ltd.) Column: Gelpack GL-S300MDT-5 (total of 2) (Hitachi Chemical Co., Ltd., product name) Eluent: THF / DMF=1 / 1 (volume ratio) + LiBr (0.03mol / L) + H3PO4 (0.06mol / L) Flow rate: 1mL / min

[0059] From the viewpoint of excellent adhesion of the film-like adhesive 1 to a connecting member (e.g., a semiconductor chip), the glass transition temperature (Tg) of the thermoplastic resin is preferably 120° C. or less, more preferably 100° C. or less, and even more preferably 85° C. or less. The above Tg is the Tg measured using a DSC (manufactured by PerkinElmer, product name: DSC-7) under the conditions of a sample amount of 10 mg, a heating rate of 10° C. / min, and a measurement atmosphere of air.

[0060] The content of the thermoplastic resin in the first adhesive is preferably 5% by mass or more, more preferably 7% by mass or more, and even more preferably 10% by mass or more, based on the total amount of the first adhesive, from the viewpoint of easily improving the heat resistance and film formability of the first adhesive. The content of the thermoplastic resin is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less, based on the total amount of the first adhesive, from the viewpoint of easily suppressing the occurrence of fillets.

[0061] For example, the first adhesive may contain a filler. The filler is effective in controlling the viscosity of the first adhesive and the physical properties of the cured product of the first adhesive. Specifically, by using the filler, it is possible to suppress the generation of voids during connection and reduce the moisture absorption rate of the cured product of the first adhesive. The filler may be an inorganic filler (inorganic particles) or an organic filler (organic particles). Examples of the inorganic filler include insulating inorganic fillers such as glass, silica, alumina, titanium oxide, mica, and boron nitride. Among these, it is preferable to use at least one selected from the group consisting of silica, alumina, titanium oxide, and boron nitride, and it is more preferable to use at least one selected from the group consisting of silica, alumina, and boron nitride. Examples of the organic filler include resin fillers (resin particles). Examples of the resin filler include polyurethane and polyimide. The resin filler can impart flexibility at high temperatures such as 260°C. It should be noted that an organic filler made of a thermoplastic resin does not fall under the category of the above-mentioned thermoplastic resin.

[0062] From the viewpoint of achieving even better insulation reliability, the filler is preferably insulating.The first adhesive preferably does not contain a filler containing a conductive material such as silver, solder, or carbon black (conductive filler).

[0063] The physical properties of the filler may be appropriately adjusted by surface treatment. The filler may be a filler that has been surface-treated from the viewpoint of improving dispersibility or adhesive strength. Examples of the surface treatment agent include glycidyl-based (epoxy-based), amine-based, phenyl-based, phenylamino-based, (meth)acrylic-based, and vinyl-based compounds.

[0064] The average particle size of the filler is, for example, 0.5 to 1.5 μm. From the viewpoint of preventing jamming during flip chip connection, the average particle size of the filler is preferably 1.5 μm or less, and from the viewpoint of excellent visibility (transparency), it is more preferably 1.0 μm or less. The average particle size of the filler is the particle size at the point corresponding to 50% volume when a cumulative frequency distribution curve of particle sizes is calculated assuming the total volume of the particles to be 100%, and can be measured by a particle size distribution measuring device using a laser diffraction scattering method, or the like.

[0065] The content of the filler in the first adhesive is preferably 25% by mass or more, more preferably 30% by mass or more, and even more preferably 35% by mass or more, based on the total amount of the first adhesive, from the viewpoint of suppressing a decrease in heat dissipation and of easily suppressing the occurrence of voids, an increase in moisture absorption rate, etc. The content of the filler is preferably 60% by mass or less, more preferably 55% by mass or less, and even more preferably 50% by mass or less, based on the total amount of the first adhesive, from the viewpoint of suppressing the occurrence of biting (trapping) of the filler in the connection portion.

[0066] When the filler contains an inorganic filler and an organic filler, the content of the inorganic filler in the first adhesive may be 60 mass% or more, 70 mass% or more, or 80 mass% or more, and may be 98 mass% or less, 95 mass% or less, or 90 mass% or less, or may be 60 to 98 mass%, 70 to 95 mass%, or 80 to 90 mass%, based on the total amount of filler contained in the first adhesive.

[0067] For example, the first adhesive may contain a radical polymerization initiator. The radical polymerization initiator may be a photoradical polymerization initiator or a thermal radical polymerization initiator.

[0068] The photoradical polymerization initiator is, for example, a compound that decomposes when irradiated with light having a wavelength in the range of 150 to 750 nm (for example, ultraviolet light) to generate free radicals, and examples of such a compound include known photopolymerization initiators having an oxime ester structure, a bisimidazole structure, an acridine structure, an α-aminoalkylphenone structure, an aminobenzophenone structure, an N-phenylglycine structure, an acylphosphine oxide structure, a benzyl dimethyl ketal structure, an α-hydroxyalkylphenone structure, an α-hydroxyacetophenone structure, or the like.

[0069] Thermal radical polymerization initiators include 1,1,3,3-tetramethylbutyl peroxyneodecanoate, di(4-t-butylcyclohexyl) peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, cumyl peroxyneodecanoate, dilauroyl peroxide, 1-cyclohexyl-1-methylethyl peroxyneodecanoate, t-hexyl peroxyneodecanoate, t-butyl peroxyneodecanoate, and t-butyl peroxy. Pivalate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyneoheptanoate, t-amylperoxy-2-ethylhexanoate, di-t-butylperoxyhexahydroterephthalate, t-amylperoxy-3,5, 5-trimethylhexanoate, 3-hydroxy-1,1-dimethylbutyl peroxyneodecanoate, t-amyl peroxyneodecanoate, di(3-methylbenzoyl) peroxide, dibenzoyl peroxide, di(4-methylbenzoyl) peroxide, t-hexylperoxyisopropyl monocarbonate, t-butylperoxymaleic acid, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate, 2, organic peroxides such as 5-dimethyl-2,5-di(3-methylbenzoylperoxy)hexane, t-butylperoxy-2-ethylhexyl monocarbonate, t-hexyl peroxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butyl peroxybenzoate, dibutyl peroxytrimethyladipate, t-amyl peroxy normal octoate, t-amyl peroxy isononanoate, and t-amyl peroxybenzoate;Examples of azo compounds include 2,2'-azobis-2,4-dimethylvaleronitrile, 1,1'-azobis(1-acetoxy-1-phenylethane), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 4,4'-azobis(4-cyanovaleric acid), and 1,1'-azobis(1-cyclohexanecarbonitrile).

[0070] From the viewpoint of further enhancing the effects of suppressing fillets, reducing voids, and improving sealing properties, the content of the radical polymerization initiator in the first adhesive is preferably less than 0.1 parts by mass, and more preferably 0.01 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic compound contained in the first adhesive. From the same viewpoint, it is more preferable that the first adhesive does not contain a radical polymerization initiator. Here, the fact that the first adhesive does not contain a radical polymerization initiator means that the content of the radical polymerization initiator in the first adhesive is below the current detection limit (for example, 0.01% by mass or less based on the total amount of the first adhesive).

[0071] The first adhesive may further contain additives such as an antioxidant, a silane coupling agent, a titanium coupling agent, a leveling agent, an ion trapping agent, etc. These may be used alone or in combination of two or more. The content of these may be appropriately adjusted so that the effect of each additive is exerted.

[0072] (Second adhesive) The second adhesive includes a second epoxy resin, a second imidazole-based hardener, and a flux compound.

[0073] [Second epoxy resin and second imidazole-based curing agent] The second epoxy resin and the second imidazole-based heat curing agent can be the same as those exemplified as the first epoxy resin and the first imidazole-based curing agent, and the preferred embodiments thereof are also the same. The first epoxy resin and the second epoxy resin may be the same or different, and the first imidazole-based curing agent and the second imidazole-based curing agent may be the same or different.

[0074] From the viewpoint of easily suppressing the occurrence of fillets, the content of the second epoxy resin in the second adhesive is preferably 25% by mass or more, more preferably 30% by mass or more, and even more preferably 35% by mass or more, based on the total amount of the second adhesive. From the viewpoint of easily obtaining good sealing properties and adhesive properties, the content of the second epoxy resin is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less, based on the total amount of the second adhesive.

[0075] The content of the second imidazole curing agent in the second adhesive is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more, relative to 100 parts by mass of the second epoxy resin contained in the second adhesive, from the viewpoint of improving the curing property when heated. The content of the second imidazole curing agent is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of the second epoxy resin contained in the second adhesive, from the viewpoint of making it more difficult for the second adhesive to be interposed between the connecting parts.

[0076] [Flux compounds] The flux compound is a compound having flux activity. As the flux compound, any known compound can be used without particular limitation as long as it can reduce and remove the oxide film on the surface of the solder or the like to facilitate metal bonding. The flux compound may be used alone or in combination of two or more kinds.

[0077] From the viewpoint of obtaining sufficient flux activity and obtaining better connection reliability, the flux compound is preferably a compound having a carboxy group (carboxylic acid), and more preferably a polycarboxylic acid having two or more carboxy groups. The number of carboxy groups in the polycarboxylic acid is preferably two. Compared with a compound having one carboxy group (monocarboxylic acid), polycarboxylic acid is less likely to volatilize due to high temperatures during connection. Therefore, the compound can further suppress the generation of voids. Furthermore, among polycarboxylic acids, a compound having two carboxy groups is more effective at suppressing the increase in viscosity of the film-like adhesive 1 during storage, connection work, etc., compared with a compound having three or more carboxy groups.

[0078] As the flux compound having a carboxy group, a compound having a group represented by the following formula (1) is preferably used.

[0079] [ka]

[0080] In formula (1), R 1 represents a hydrogen atom or an electron-donating group.

[0081] From the viewpoint of excellent reflow resistance and even better connection reliability, R 1 In this embodiment, the second adhesive contains an epoxy resin, and further contains a compound having a group represented by formula (1), R 1 is an electron donating group. In this case, even in the flip chip connection method, it becomes easy to manufacture a semiconductor device having excellent reflow resistance and connection reliability.

[0082] Examples of the electron-donating group include an alkyl group, a hydroxyl group, an amino group, an alkoxy group, an alkylamino group, etc. As the electron-donating group, a group that is less reactive with other components (e.g., an epoxy resin) is preferable, and specifically, an alkyl group, a hydroxyl group, or an alkoxy group is preferable, and an alkyl group is more preferable.

[0083] The alkyl group may be linear or branched, but is preferably linear. The alkyl group is preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 5 carbon atoms. The greater the carbon number of the alkyl group, the greater the electron donating property and steric hindrance tend to be. An alkyl group having a carbon number within the above range has an excellent balance between electron donating property and steric hindrance.

[0084] As a flux compound having two carboxy groups, a compound represented by the following formula (2) can be suitably used. The compound represented by the following formula (2) can further improve the reflow resistance and connection reliability of a semiconductor device.

[0085] [ka]

[0086] In formula (2), R 1 is the same as formula (1). 2 represents a hydrogen atom or an electron-donating group, and n represents an integer of 0 or 1 or more.

[0087] R 2 The electron donating property indicated by R 1 The examples of the electron donating group are the same as those described above. 2 is R 1 may be the same as or different from each other. 2 may be the same or different from each other.

[0088] In formula (2), n is preferably 1 or more. When n is 1 or more, the flux compound is less likely to volatilize even at high temperatures during connection, and the generation of voids can be further suppressed, compared with the case where n is 0. Furthermore, in formula (2), n is preferably 15 or less, more preferably 11 or less, and may be 6 or less or 4 or less. When n is 15 or less, even better connection reliability can be obtained.

[0089] Specific examples of the above-mentioned flux compounds include dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, and dodecanedioic acid, as well as compounds in which an electron donating group is substituted at the 2-position of these dicarboxylic acids (e.g., 2-methylglutaric acid), etc. Among these, 2-methylglutaric acid is preferably used from the viewpoint of further improving the effects of suppressing fillets, reducing voids, and improving sealing properties by combining with an epoxy resin and an imidazole-based curing agent.

[0090] The melting point of the flux compound is preferably 150°C or less, more preferably 140°C or less, and even more preferably 130°C or less. Such a flux compound is likely to fully exhibit flux activity before the curing reaction between the epoxy resin and the imidazole-based curing agent occurs. Therefore, by using such a flux compound, a semiconductor device with even better connection reliability can be obtained. The flux compound is preferably solid at room temperature (25°C). The melting point of the flux compound is preferably 25°C or more, more preferably 50°C or more. In this specification, a melting point of 150°C or less means that the upper limit of the melting point is 150°C or less, and a melting point of 25°C or more means that the lower limit of the melting point is 25°C or more.

[0091] The content of the flux compound in the second adhesive is preferably 0.1 mass% or more, more preferably 0.3 mass% or more, and even more preferably 0.5 mass% or more, based on the total amount of the second adhesive, from the viewpoint of obtaining a better flux effect. The content of the flux compound is preferably 5 mass% or less, more preferably 3 mass% or less, and even more preferably 2 mass% or less, based on the total amount of the second adhesive, from the viewpoint of reducing the amount of warping of a wafer during the manufacture of a semiconductor device.

[0092] [Other ingredients] The second adhesive may contain the components exemplified as other components that may be contained in the first adhesive. The thermoplastic resin in the first adhesive and the thermoplastic resin in the second adhesive may be the same or different. The same applies to other components such as fillers.

[0093] The content of the thermoplastic resin in the second adhesive is preferably 5% by mass or more, more preferably 7% by mass or more, and even more preferably 10% by mass or more, based on the total amount of the second adhesive, from the viewpoint of easily improving the heat resistance and film formability of the second adhesive. From the viewpoint of easily suppressing the occurrence of fillets, the content of the thermoplastic resin is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less, based on the total amount of the second adhesive.

[0094] The content of the filler in the second adhesive is preferably 25% by mass or more, more preferably 30% by mass or more, and even more preferably 35% by mass or more, based on the total amount of the second adhesive, from the viewpoint of suppressing a decrease in heat dissipation and of easily suppressing the occurrence of voids, an increase in moisture absorption rate, etc. The content of the filler is preferably 60% by mass or less, more preferably 55% by mass or less, and even more preferably 50% by mass or less, based on the total amount of the second adhesive, from the viewpoint of suppressing the occurrence of biting (trapping) of the filler in the connection portion.

[0095] The content of the radical polymerization initiator in the second adhesive may be 0.01 parts by mass or less based on the total amount of the second adhesive, that is, the second adhesive does not need to contain a radical polymerization initiator.

[0096] Since some flux compounds react with radicals, and the presence of a radical polymerizable compound causes a curing reaction to proceed rapidly when heated, making it easier for a cured product to intervene between the connecting parts, it is preferable that the second adhesive does not contain a radical polymerizable compound. The content of the radical polymerizable compound is preferably 0.5 mass% or less, more preferably 0.05 mass% or less, and even more preferably 0 mass% based on the total amount of the second adhesive.

[0097] The film-like adhesive 1 is preferably non-conductive, that is, the film-like adhesive 1 is preferably a so-called NCF (Non Conductive Film).

[0098] The film-like adhesive 1 described above may be provided with a substrate such as a support film or a protective film provided on the surface of the first adhesive region 2 (the side opposite to the second adhesive region 3) and / or on the surface of the second adhesive region 3 (the side opposite to the first adhesive region 2). In the present disclosure, a laminate comprising a substrate and a film-like adhesive provided on the substrate is referred to as an adhesive tape.

[0099] The substrate may be any of the substrates exemplified as substrates used in the manufacturing method for a film-like adhesive described below, but the substrate provided on the second adhesive region 3 side of the film-like adhesive 1 is preferably a backgrind tape. That is, another preferred embodiment of the present disclosure is an adhesive tape (adhesive tape with backgrind tape) comprising the above-mentioned film-like adhesive 1 and a backgrind tape provided on the film-like adhesive 1 on the side opposite the first adhesive region 2 side as viewed from the second adhesive region 3.

[0100] The backgrind tape is usually configured so that one main surface side is an adhesive layer, but in this case, the backgrind tape is provided on the film-like adhesive 1 so that the surface on the adhesive layer side faces the film-like adhesive 1 (for example, so that the adhesive layer and the film-like adhesive are in contact). The thickness of the substrate (for example, the thickness of the backgrind tape) may be 20 to 300 μm.

[0101] The adhesive tape may be a laminate of a substrate and a film-like adhesive obtained by a method for producing a film-like adhesive described later, i.e., a method for applying a coating liquid onto a substrate, forming a coating film, and drying the coating film, or may be a laminate obtained by attaching a substrate to the film-like adhesive 1 (for example, laminating the film-like adhesive 1 and a substrate). When the substrate is a backgrind tape, applying and drying the coating liquid on the adhesive layer of the backgrind tape may cause problems such as destruction of the adhesive layer and component transfer between the adhesive and the adhesive, so it is preferable to obtain the adhesive tape by attaching the backgrind tape to the film-like adhesive 1.

[0102] <Method of manufacturing film adhesive for semiconductors> One embodiment of the manufacturing method of the film-like adhesive 1 includes a step of providing one of a first adhesive layer and a second adhesive layer on the other. Here, the first adhesive layer is a layer composed of the above-mentioned first adhesive (i.e., a layer not containing a flux compound and containing a first epoxy resin, a first imidazole-based curing agent, and a (meth)acrylic compound), and forms a first adhesive region 2 in the film-like adhesive 1. The second adhesive layer is a layer composed of the above-mentioned second adhesive (i.e., a layer containing a second epoxy resin, a second imidazole-based curing agent, and a flux compound), and forms a second adhesive region 3 in the film-like adhesive 1.

[0103] In one embodiment, the step may be, for example, a step of bonding a first adhesive film having the first adhesive layer and a second adhesive film having the second adhesive layer. In this embodiment, the method for producing the film-like adhesive 1 may further include a step of preparing the first adhesive film and the second adhesive film.

[0104] The step of preparing the first adhesive film may include forming a first adhesive layer on a substrate (e.g., a film-like substrate). When forming a first adhesive layer on a substrate, for example, first, a first epoxy resin, a first imidazole-based curing agent, a (meth)acrylic compound, and other components (filler, thermoplastic resin, additives, etc.) added as necessary are added to an organic solvent, and dissolved or dispersed by stirring, mixing, kneading, etc. to prepare a coating liquid containing the first adhesive. Thereafter, the coating liquid is applied to a substrate that has been subjected to a release treatment using a knife coater, roll coater, applicator, etc. to form a coating film, and then the organic solvent is reduced from the coating film by heating. This allows the first adhesive layer to be formed on the substrate.

[0105] The organic solvent used in preparing the coating liquid is preferably one that has the property of uniformly dissolving or dispersing each component, and examples thereof include dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone, dimethylsulfoxide, diethylene glycol dimethyl ether, toluene, benzene, xylene, methyl ethyl ketone, tetrahydrofuran, ethyl cellosolve, ethyl cellosolve acetate, butyl cellosolve, dioxane, cyclohexanone, and ethyl acetate. These organic solvents can be used alone or in combination of two or more. The stirring, mixing, and kneading in preparing the coating liquid can be performed using, for example, a stirrer, a grinding machine, a three-roll mill, a ball mill, a bead mill, or a homodisper.

[0106] The substrate is not particularly limited as long as it has heat resistance that can withstand the heating conditions when volatilizing the organic solvent, and examples thereof include polyolefin films such as polypropylene film and polymethylpentene film, polyester films such as polyethylene terephthalate film and polyethylene naphthalate film, polyimide film, and polyetherimide film. The substrate is not limited to a single layer of these films, and may be a multilayer film made of two or more materials. The substrate may be a film whose surface has been subjected to a release treatment.

[0107] The drying conditions for volatilizing the organic solvent from the coating film on the substrate are preferably conditions that allow the organic solvent to volatilize sufficiently, specifically, heating is preferably performed at 50 to 200° C. for 0.1 to 90 minutes. If there is no effect on voids or viscosity adjustment after mounting, the organic solvent is preferably removed to 1.5 mass % or less with respect to the total amount of the first adhesive.

[0108] The step of preparing the second adhesive film may include forming a second adhesive layer on the substrate. The second adhesive layer can be formed on the substrate by the same method as the method of forming the first adhesive layer, except that the second epoxy resin, the second imidazole curing agent, the flux compound, and other components (filler, thermoplastic resin, additives, etc.) that are added as necessary are used.

[0109] Examples of the method for bonding the first adhesive film and the second adhesive film include hot pressing, roll lamination, vacuum lamination, etc. Lamination may be performed under heating conditions of, for example, 30 to 120°C.

[0110] The film-like adhesive 1 may be obtained, for example, by forming one of a first adhesive layer and a second adhesive layer on a substrate, and then forming the other of the first adhesive layer and the second adhesive layer on the obtained first adhesive layer or second adhesive layer. The first adhesive layer and the second adhesive layer can be formed by the method described above.

[0111] For example, the film-like adhesive 1 may be obtained by forming a first adhesive and a second adhesive substantially simultaneously on a substrate. Examples of methods for simultaneously coating and preparing the first adhesive and the second adhesive include coating methods such as a sequential coating method and a multi-layer coating method.

[0112] <Semiconductor device> Next, a semiconductor device manufactured using the film-like adhesive for semiconductors of the above embodiment will be described.

[0113] FIG. 2 is a schematic cross-sectional view showing one embodiment of a semiconductor device. The semiconductor device 100 shown in FIG. 2(a) has a semiconductor chip 20 and a base 25 facing each other, wiring (first connection part and second connection part) 15 arranged on the surfaces facing each other of the semiconductor chip 20 and the base 25, connection bumps 30 connecting the wiring 15 of the semiconductor chip 20 and the base 25 to each other, and a sealing part 40 made of a hardened product of adhesive (first adhesive and second adhesive) filling the gap between the semiconductor chip 20 and the base 25. The semiconductor chip 20 and the base 25 are flip-chip connected by the wiring 15 and the connection bumps 30. The wiring 15 and the connection bumps 30 are sealed by the hardened product of the adhesive and are isolated from the external environment. The sealing part 40 has an upper part 40a including the hardened product of the first adhesive and a lower part 40b including the hardened product of the second adhesive.

[0114] The semiconductor device 200 shown in FIG. 2(b) has a semiconductor chip 20 and a base 25 facing each other, bumps (first and second connection parts) 32 arranged on the facing surfaces of the semiconductor chip 20 and the base 25, respectively, and a sealing part 40 made of a hardened adhesive (first and second adhesive) that fills the gap between the semiconductor chip 20 and the base 25. The semiconductor chip 20 and the base 25 are flip-chip connected by connecting the facing bumps 32 to each other. The bumps 32 are sealed with the hardened adhesive and are isolated from the external environment. The sealing part 40 has an upper part 40a including the hardened first adhesive and a lower part 40b including the hardened second adhesive.

[0115] The semiconductor chip 20 is not particularly limited, and may be a semiconductor chip made of an elemental semiconductor made of the same type of element, such as silicon or germanium, or a semiconductor chip made of a compound semiconductor, such as gallium arsenide or indium phosphide.

[0116] There are no particular limitations on the base 25 as long as it can be used to mount the semiconductor chip 20, and examples thereof include a semiconductor chip, a semiconductor wafer, and a wiring circuit board.

[0117] Examples of the semiconductor chip that can be used as the base 25 are the same as the examples of the semiconductor chip 20 described above, and the same semiconductor chip as the semiconductor chip 20 may be used as the base 25.

[0118] The semiconductor wafer that can be used as the base 25 is not particularly limited, and may be one having a configuration in which a plurality of semiconductor chips such as the semiconductor chip 20 described above are connected together.

[0119] The wired circuit board that can be used as the base 25 is not particularly limited, and examples that can be used include a circuit board having wiring (wiring pattern) 15 formed by etching away unnecessary parts of a metal film on the surface of an insulating substrate whose main component is glass epoxy, polyimide, polyester, ceramic, epoxy, bismaleimide triazine, etc., a circuit board in which wiring 15 is formed on the surface of the insulating substrate by metal plating or the like, and a circuit board in which wiring 15 is formed by printing a conductive material on the surface of the insulating substrate.

[0120] The connection parts such as wiring 15 and bumps 32 contain as their main components gold, silver, copper, solder (the main components being, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, tin-silver-copper, etc.), nickel, tin, lead, etc., and may contain multiple metals.

[0121] Among the above metals, from the viewpoint of obtaining a package having excellent electrical and thermal conductivity at the connection portion, gold, silver and copper are preferred, and silver and copper are more preferred. From the viewpoint of obtaining a package at reduced cost, inexpensive materials such as silver, copper and solder are preferred, copper and solder are more preferred, and solder is even more preferred. Since the formation of an oxide film on the surface of a metal at room temperature can reduce productivity and increase costs, from the viewpoint of suppressing the formation of an oxide film, gold, silver, copper and solder are preferred, gold, silver and solder are more preferred, and gold and silver are even more preferred.

[0122] A metal layer mainly composed of gold, silver, copper, solder (main components are, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, etc.), tin, nickel, etc. may be formed, for example, by plating, on the surfaces of the wiring 15 and bumps 32. This metal layer may be composed of only a single component, or may be composed of multiple components. The metal layer may have a structure in which a single layer or multiple metal layers are laminated.

[0123] The semiconductor device may be a stack of a plurality of structures (packages) such as those shown in the semiconductor devices 100 and 200. In this case, the semiconductor devices 100 and 200 may be electrically connected to each other by bumps, wiring, or the like containing gold, silver, copper, solder (whose main component is, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, tin-silver-copper, etc.), tin, nickel, or the like.

[0124] As a method for stacking a plurality of semiconductor devices, for example, TSV (Through-Silicon Via) technology can be mentioned as shown in FIG. 3. In the semiconductor device 500 shown in FIG. 3, the wiring 15 formed on the interposer 50 is connected to the wiring 15 of the semiconductor chip 20 via the connection bump 30, so that the semiconductor chip 20 and the interposer 50 are flip-chip connected. The gap between the semiconductor chip 20 and the interposer 50 is filled with a hardened product of the adhesive (first adhesive and second adhesive), forming a sealing part 40. On the surface of the semiconductor chip 20 opposite to the interposer 50, the semiconductor chips 20 are repeatedly stacked via the wiring 15, the connection bump 30 and the sealing part 40. The wiring 15 on the pattern surfaces on the front and back of the semiconductor chip 20 are connected to each other by the through electrodes 34 filled in the holes penetrating the inside of the semiconductor chip 20. The material of the through electrodes 34 can be copper, aluminum, or the like.

[0125] Such TSV technology makes it possible to obtain signals from the back surface of the semiconductor chip, which is not normally used. Furthermore, since the through electrodes 34 are vertically passed through the semiconductor chip 20, the distance between the opposing semiconductor chips 20 and between the semiconductor chip 20 and the interposer 50 can be shortened, enabling flexible connection. The film-like adhesive for semiconductors of this embodiment can be applied as a film-like adhesive for semiconductors between the opposing semiconductor chips 20 and between the semiconductor chip 20 and the interposer 50 in such TSV technology.

[0126] Furthermore, in a highly flexible bump formation method such as area bump chip technology, a semiconductor chip can be directly mounted on a motherboard without an interposer. The film-like adhesive for semiconductors of this embodiment can also be applied to such cases where a semiconductor chip is directly mounted on a motherboard. The film-like adhesive for semiconductors of this embodiment can also be applied to sealing the gap (void) between two wiring circuit boards when stacking the boards.

[0127] <Method of Manufacturing Semiconductor Device> Next, a method for manufacturing a semiconductor device using the film-like adhesive for semiconductors of the above embodiment will be described.

[0128] A method for manufacturing a semiconductor device according to an embodiment includes, for example, a step of preparing a semiconductor chip with a film-like adhesive, the semiconductor chip including the film-like adhesive of the above embodiment, the film-like adhesive being provided on the semiconductor chip such that the surface of the first adhesive region opposite to the second adhesive region faces the semiconductor chip, and a step of placing the semiconductor chip with the film-like adhesive on a base from the film-like adhesive side and heating the semiconductor chip to electrically connect the connection portion of the semiconductor chip to the connection portion of the base and seal the gap between the semiconductor chip and the base. The method for manufacturing a semiconductor device may further include a step of attaching the film-like adhesive of the above embodiment to the connection surface of the semiconductor chip or its precursor from the first adhesive region side. Here, the precursor of the semiconductor chip means a member that will become a semiconductor chip by processing. A specific example of the precursor of the semiconductor chip is a semiconductor wafer. When a semiconductor wafer is used as the precursor of the semiconductor chip, the method for manufacturing a semiconductor device may further include a step of dicing the semiconductor wafer or the semiconductor wafer with the film-like adhesive.

[0129] The method for manufacturing a semiconductor device may use the adhesive tape with backgrind tape described above. In this case, the method for manufacturing a semiconductor device may further include a lamination step of attaching the adhesive tape with backgrind tape from the film-like adhesive for semiconductors to a connection surface of a semiconductor wafer, which is a precursor of a semiconductor chip, and a backgrinding step of grinding the semiconductor wafer with the adhesive tape attached from the side opposite to the adhesive tape.

[0130] Hereinafter, the method for manufacturing a semiconductor device will be described in more detail, taking as an example an embodiment in which a precursor of a semiconductor chip (semiconductor wafer) is used.

[0131] 4 to 8 are cross-sectional views illustrating steps of a method for manufacturing a semiconductor device according to an embodiment of the present invention. The method for manufacturing a semiconductor device according to an embodiment of the present invention includes the following steps (a) to (e). Step (a): A step of preparing a laminate 6 including a semiconductor wafer A having a connection portion (first connection portion) 5 on one main surface (connection surface) and a film-like adhesive 1 provided on the main surface of the semiconductor wafer A such that the surface on the side of the first adhesive region 2 faces the semiconductor wafer A (see FIG. 4). Step (b): A back-grinding step of grinding the side of the laminate 6 opposite to the side on which the film-like adhesive 1 is provided (the side opposite to the side on which the connection portion 5 of the semiconductor wafer A is provided) (see FIG. 5). Step (c): A step of dividing the laminate 6 into individual pieces to obtain semiconductor chips 8 with a film-like adhesive having connection portions 5 (see FIG. 6). Step (d): A step of picking up the semiconductor chip 8 with the film-like adhesive from the singulated film-like adhesive 1a side (see FIG. 7). Step (e): A step of placing the semiconductor chip 8 with the film-like adhesive on one of the main surfaces (connection surface) of a base 9 having a connection portion (second connection portion) 10 from the film-like adhesive 1a side, and heating the semiconductor chip 8 with the film-like adhesive and the connection portion 10 of the base 9 electrically connecting them, and sealing the gap between the semiconductor chip 8 and the base 9 (see FIG. 8). When a semiconductor wafer whose thickness has been adjusted in advance is used, step (b) does not need to be performed.

[0132] (Step (a)) Step (a) may be a step of preparing a laminate 6 that has been produced in advance, or a step of producing the laminate 6. The laminate 6 may be produced, for example, by the following method.

[0133] First, an adhesive tape having a substrate 4 provided on the second adhesive region 3 side of the film-like adhesive 1 is prepared, and this is placed in a specified device (see FIG. 4(a)). The substrate 4 is, for example, a backgrind tape. Next, a semiconductor wafer A having a connection portion 5 (wiring, bumps, etc.) on one main surface is prepared, and the film-like adhesive 1 is attached to the main surface (the surface on which the connection portion 5 is provided, the connection surface) of the semiconductor wafer A. This results in a laminate 6 in which the semiconductor wafer A, the first adhesive region 2, and the second adhesive region 3 are laminated in this order (see FIG. 4(b)).

[0134] The film-like adhesive 1 can be applied by hot pressing, roll lamination, vacuum lamination, etc. The supply area and thickness of the film-like adhesive 1 are appropriately set depending on the size of the semiconductor wafer and the base, the height of the connection part, etc. In FIG. 4, the thickness of the film-like adhesive 1 is greater than the height of the connection part 5 of the semiconductor wafer A, and the connection part 5 is covered by the film-like adhesive 1, but the thickness of the film-like adhesive 1 may be less than the height of the connection part 5.

[0135] (Step (b)) In step (b), the semiconductor wafer A of the laminate 6 is ground using, for example, a grinder G (see Figs. 5(a) and 5(b)). This thins the semiconductor wafer A. The thickness of the semiconductor wafer after grinding may be, for example, 10 µm to 300 µm. From the viewpoint of miniaturizing and thinning the semiconductor device, it is preferable that the thickness of the semiconductor wafer is 20 µm to 100 µm.

[0136] (Process (c)) In step (c), for example, first, a dicing tape 7 is attached to the semiconductor wafer A side of the laminate 6, and the laminate is placed in a predetermined device (see FIG. 6(a)). The substrate 4 may be peeled off before or after the laminate 6 is attached to the dicing tape 7. Next, the laminate 6 is diced with a dicing saw D. In this way, the laminate 6 is divided into individual pieces, and a semiconductor chip 8 with a film-like adhesive having a film-like adhesive 1a on the semiconductor chip A' is obtained (see FIG. 6(b)). A connection portion 5 is provided on the surface of the semiconductor chip A' facing the film-like adhesive 1a. The film-like adhesive 1a has a first adhesive region (region made of the first adhesive) 2a and a second adhesive region (region made of the second adhesive) 3a.

[0137] (Step (d)) In step (d), for example, the dicing tape 7 is expanded to separate the semiconductor chips 8 with the film-like adhesive obtained by the above dicing, and the semiconductor chips 8 with the film-like adhesive pushed up by the needle N from the dicing tape 7 side are picked up by a pickup tool P from the film-like adhesive 1a side (see FIG. 7). The picked-up semiconductor chips 8 with the film-like adhesive are transferred to a bonding tool and used for bonding in step (e).

[0138] (Step (e)) In step (e), for example, first, a base 9 for mounting a semiconductor chip having a connection portion 10 (second connection portion) on one side is prepared, and the semiconductor chip 8 with a film-like adhesive and the base 9 are aligned. Next, the semiconductor chip 8 with a film-like adhesive is placed on the main surface of the base 9 on which the connection portion 10 (wiring, bumps, etc.) is provided from the film-like adhesive 1a side using a bonding tool, and heated to bond the semiconductor chip 8 with a film-like adhesive and the base 9 (see Fig. 8(a) and Fig. 8(b)). As a result, the connection portion 5 of the semiconductor chip 8 with a film-like adhesive and the connection portion 10 of the base 9 are electrically connected, and a sealing portion 1a' made of a cured product of the film-like adhesive 1a is formed between the semiconductor chip A' and the base 9, and the gap between the semiconductor chip 8 and the base 9 is sealed, thereby obtaining a semiconductor device 11 which is a bonded body of the semiconductor chip 8 with a film-like adhesive and the base 9. The sealing portion 1a' has an upper portion 2a' containing a cured product of the first adhesive, and a lower portion 3a' containing a cured product of the second adhesive.

[0139] When a solder bump is used for one of the connection parts 5 and 10 (for example, when the connection part 5 or the connection part 10 is a wiring provided with a solder bump), the connection part 5 and the connection part 10 are electrically and mechanically connected by being soldered.

[0140] The heating in step (e) may be performed while arranging the semiconductor chip, or after arranging the semiconductor chip. The heating and arranging in step (e) may be thermocompression bonding. Step (e) may include a step of temporarily fixing after alignment (temporary fixing step), and a step of melting bumps (e.g. solder bumps) provided on the connection part by heat treatment to bond the semiconductor chip A' and the base body 9 and seal the connection part (sealing step). Since it is not necessarily required to form a metal bond at the stage of temporary fixing, the temporary fixing step can be performed with a low load, in a short time, and at a low temperature. Therefore, when the temporary fixing step and the sealing step are performed in step (e), productivity is improved and deterioration of the connection part can be suppressed.

[0141] The load applied for temporary fixation is appropriately set in consideration of the number of connection parts (bumps), absorbing the variation in height of the connection parts (bumps), controlling the deformation amount of the connection parts (bumps), etc. From the viewpoint of eliminating voids and making it easier to contact the connection parts, the larger the load, the more preferable it is. For example, the load is preferably 0.009 N to 0.2 N per connection part (e.g., bump).

[0142] Heating in the sealing step may be performed using an apparatus capable of heating to a temperature equal to or higher than the melting point of the metal of the connection portion. The heating temperature is preferably a temperature at which the film-like adhesive begins to harden, and more preferably a temperature at which the film-like adhesive is completely hardened. The heating temperature and heating time are appropriately set.

[0143] The heating time in the sealing step varies depending on the type of metal constituting the connection, but from the viewpoint of improving productivity, the shorter the heating time, the better. When solder bumps are used for the connection, the heating time is preferably 20 seconds or less, more preferably 10 seconds or less, and even more preferably 5 seconds or less. In the case of copper-copper or copper-gold metal connection, the connection time is preferably 60 seconds or less.

[0144] In the sealing step, heating and pressure may be applied using a device capable of heating and pressure application. That is, the heating in the sealing step may be heating by thermocompression. In this case, the load (connection load) is set in consideration of the size of the connection member, the number of connection parts, the variation in height, the deformation amount of the connection parts due to pressure, and the like. The connection load may be, for example, 1 MPa or less exceeding atmospheric pressure. From the viewpoint of suppressing voids and improving connectivity, the higher the load, the more preferable, and from the viewpoint of suppressing fillets, the lower the load, the more preferable. From these viewpoints, the load is preferably 0.05 to 0.5 MPa. The pressure bonding time (connection time) varies depending on the type of metal constituting the connection parts, but from the viewpoint of improving productivity, the shorter the time, the more preferable. When the connection parts are solder bumps, the pressure bonding time is preferably 20 seconds or less, more preferably 10 seconds or less, and even more preferably 5 seconds or less. In addition, since direct pressure application using a pressure bonding machine makes it difficult for the heat of the pressure bonding machine to be transmitted to the fillets, pressure application by air pressure is preferable from the viewpoint of easily achieving a sufficient effect on the fillets. From the viewpoint of en bloc sealing and suppression of fillets, it is preferable that the pressure during heating be applied by atmospheric pressure (pressure using a pressurized reflow furnace, a pressurized oven, or the like).

[0145] After the semiconductor chip A' and the base 9 are connected, a heat treatment may be carried out in an oven or the like to further improve the connection reliability. EXAMPLES

[0146] The present disclosure will be described more specifically below with reference to examples, but the present disclosure is not limited to these examples.

[0147] Details of the materials used in the examples and comparative examples are as follows. (liquid epoxy resin) YX7110B80: Flexible epoxy, manufactured by Mitsubishi Chemical Corporation. Product name "jERYX7110B80" and "jER" are registered trademarks (hereinafter the same). YL983U: Bisphenol F type liquid epoxy, manufactured by Mitsubishi Chemical Corporation, product name "jERYL983U" (Solid epoxy resin) EP1032: Triphenolmethane skeleton-containing multifunctional solid epoxy, manufactured by Mitsubishi Chemical Corporation, product name "jER1032H60" (Imidazole-based hardener) 2PHZ-PW: 2-phenyl-4,5-dihydroxymethylimidazole, product name, manufactured by Shikoku Chemical Industry Co., Ltd. 2MAOK-PW: 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, manufactured by Shikoku Chemical Industry Co., Ltd., trade name (Phenoxy resin) ZX-1356-2: Phenoxy resin, Tohto Kasei Co., Ltd., product name, Tg = approx. 71°C, weight average molecular weight Mw = approx. 63,000 (Acrylic Compounds) A-DPH: Dipentaerythritol polyacrylate, product name, manufactured by Shin-Nakamura Chemical Co., Ltd. (Organic filler) EXL-2655: Core-shell type organic particles, manufactured by Rohm and Haas Japan Co., Ltd., product name (Silica filler) ·KE180G-HLA: Silica filler, manufactured by Admatechs Co., Ltd., product name (Flux Compounds) 2-Methylglutaric acid: Aldrich, melting point: approx. 78°C

[0148] <Examples 1 to 7 and Comparative Example 1> (Preparation of the first adhesive film) The components shown in Table 1 were added to an organic solvent (methyl ethyl ketone) so that the NV value ([mass of paint after drying] / [mass of paint before drying]×100) was 60%, to obtain a mixed solution. At this time, the amount of each component added was the amount shown in Table 1 (unit: parts by mass). Then, beads of Φ1.0 mm and beads of Φ2.0 mm were added to the above mixed solution, and the mixture was stirred for 30 minutes with a beads mill (Fritsch Japan Co., Ltd., planetary fine grinding machine P-7). The amount of beads added was the same mass as the non-volatile content of the mixed solution (total amount of components other than the organic solvent). After stirring, the beads were removed by filtration. In this way, coating solutions 1A to 8A for forming a first adhesive layer were obtained.

[0149] Using the obtained coating liquids 1A to 8A, first adhesive films (first adhesive films 1A to 8A) having first adhesive layers 1A to 8A, respectively, were obtained. Specifically, the coating liquid was first applied to a base film (manufactured by Teijin DuPont Films Co., Ltd., product name "Purex A54") using a small precision coating device (Kanei Seiki) so that the film thickness after drying would be 4.5 μm. Next, the coating film was dried (80°C / 10 min) in a clean oven (manufactured by ESPEC) to obtain a first adhesive film having a first adhesive layer.

[0150] [Table 1]

[0151] (Preparation of the Second Adhesive Film) The components shown in Table 2 were added to an organic solvent (methyl ethyl ketone) so that the NV value was 60%, to obtain a mixed solution. At this time, the amount of each component added was the amount shown in Table 2 (unit: mass parts). Then, Φ1.0 mm beads and Φ2.0 mm beads were added to the above mixed solution, and the mixture was stirred for 30 minutes with a bead mill (Fritsch Japan Co., Ltd., planetary type fine grinder P-7). The amount of beads added was the same mass as the non-volatile content of the mixed solution (total amount of components other than the organic solvent). After stirring, the beads were removed by filtration, and coating solution 1B and coating solution 2B for forming the second adhesive layer were obtained.

[0152] The obtained coating liquid 1B was applied to a substrate film (manufactured by Teijin DuPont Films Co., Ltd., product name "Purex A54") using a small precision coating device (Kanei Seiki) so that the film thickness after drying would be 4.5 μm. The coating film was then dried (80° C. / 10 min) in a clean oven (manufactured by ESPEC) to obtain a second adhesive film 1B having a second adhesive layer 1B. A second adhesive film 2B having a second adhesive layer 2B was obtained in the same manner, except that coating liquid 2B was used instead of coating liquid 1B.

[0153] [Table 2]

[0154] (Preparation of film-like adhesive) Any one of the first adhesive films 1A to 8A prepared above was laminated with the second adhesive film 1B or 2B in the combinations shown in Table 3 to laminate the first adhesive layer and the second adhesive layer, thereby preparing the film-like adhesives (total thickness 9.0 μm) of Examples 1 to 7 and Comparative Example 1. The lamination temperature was 50° C.

[0155] <Comparative Example 2> A second adhesive film 1B having a second adhesive layer 1B was obtained in the same manner as in "Preparation of a second adhesive film" above, and then two of the obtained second adhesive layers 1B were laminated to obtain a film-like adhesive of Comparative Example 2 (total thickness 9.0 μm).

[0156] <Evaluation> A connection structure (semiconductor device) was produced in the following manner using the film-like adhesives obtained in Examples 1 to 7 and Comparative Examples 1 and 2. The obtained connection structures were also evaluated for fillet length, voids, and sealing performance by the methods described below. The results are shown in Table 3.

[0157] (Preparation of connection structure) The film-like adhesive obtained in Examples 1 to 7 and Comparative Examples 1 to 2 was cut into a predetermined size (8 mm long x 8 mm wide x 9.0 μm thick) to prepare an evaluation sample. Next, the evaluation sample was attached to the surface (connection surface) of a semiconductor chip with solder bumps (chip size: 7.3 mm long x 7.3 mm wide x 0.15 mm thick, bump height: copper pillar + solder total about 40 μm, number of bumps 328) on which the solder bumps were provided, to obtain a laminate of the evaluation sample and the semiconductor chip with solder bumps. At this time, in Examples 1 to 7 and Comparative Example 1, the first adhesive layer side (opposite side to the second adhesive layer) was attached to the semiconductor chip with solder bumps. Next, the above laminate was mounted on a glass epoxy substrate (glass epoxy substrate: 420 μm thick, copper wiring: 9 μm thick) from the evaluation sample side using a flip mounting device "FCB3" (manufactured by Panasonic, product name). The mounting was performed under the conditions of a pressure head temperature of 350°C, a pressure time of 3 seconds, and a pressure pressure of 0.5 MPa. As a result, a connection structure (semiconductor device) was obtained in which a glass epoxy substrate and a semiconductor chip with solder bumps were daisy-chain connected.

[0158] (Fillet amount) The connection structure obtained above was observed from the semiconductor chip side using a digital microscope VHX-6000 (manufactured by Keyence), and the length of the adhesive (fillet) protruding from the four peripheral sides of the semiconductor chip was measured. The length of the fillet on each side was the maximum value of the shortest distance from the end of the protruding adhesive to the semiconductor chip. The amount of fillet was evaluated based on the average value of the lengths of the fillets measured on each of the four sides. If the average value was less than 100 μm, it was determined that the amount of fillet generation was sufficiently reduced, and if the average value was 100 μm or more, it was determined that the fillet suppression effect was insufficient.

[0159] (Void) The external image of the connection structure obtained above was taken with an ultrasonic imaging diagnostic device (trade name "Insight-300", manufactured by Insight), and an image of the adhesive layer (layer consisting of a cured product of a film-like adhesive for semiconductors) on the chip was captured with a scanner GT-9300UF (trade name, manufactured by EPSON), and the void portion was identified by color correction and two-tone gradation using image processing software Adobe Photoshop (registered trademark), and the proportion of the void portion was calculated using a histogram. The area of ​​the adhesive portion on the chip was taken as 100%, and the void occurrence rate was evaluated as "A" when it was 5% or less, "B" when it was more than 5% and less than 10%, and "C" when it was more than 10%.

[0160] (Sealability) The connection structure obtained above was observed from the semiconductor chip side using a semiconductor / FPD inspection microscope MX63 (manufactured by OLYMPUS), and the length of the unfilled part of the chip corner was measured. The length of the unfilled part was taken as the maximum shortest distance from the chip corner to the filled part. The sealing ability was evaluated as "A" if the length of the unfilled part was less than 500 μm, and "B" if it was 500 μm or more.

[0161] [Table 3] [Explanation of symbols]

[0162] 1,1a...film-like adhesive for semiconductors, 2,2a...first adhesive region, 3,3a...second adhesive region, 4...base material, 5...connection portion (first connection portion), 9...base, 10...connection portion (first connection portion), 11...semiconductor device, 15...wiring (first connection portion and second connection portion), 20...semiconductor chip, 25...base, 30...connection bump, 32...bump (first connection portion and second connection portion), 40...sealing portion, 100,200,500...semiconductor device, A...semiconductor wafer, A'...semiconductor chip.

Claims

1. A first adhesive region along a thickness direction is free of a flux compound and a second adhesive region is free of a flux compound, the first adhesive region comprises a first epoxy resin, a first imidazole-based curing agent, and a (meth)acrylic compound; The second adhesive region comprises a second epoxy resin, a second imidazole-based curing agent, and the flux compound.

2. The film-like adhesive for semiconductors according to claim 1 , wherein the first adhesive region does not contain a radical polymerization initiator.

3. 2. The film-like adhesive for semiconductors according to claim 1, wherein at least one of the first epoxy resin and the second epoxy resin comprises an epoxy resin that is liquid at 25°C.

4. 2. The film-like adhesive for semiconductors according to claim 1, wherein at least one of the first epoxy resin and the second epoxy resin contains a triphenolmethane type epoxy resin.

5. 2. The film-like adhesive for semiconductors according to claim 1, wherein at least one of the first imidazole-based curing agent and the second imidazole-based curing agent has a triazine ring.

6. The film-like adhesive for semiconductors according to claim 1, wherein the ratio of the content of the first epoxy resin to the content of the (meth)acrylic compound in the first adhesive region is 3 to 11, in mass ratio.

7. 2. The film-like adhesive for semiconductors according to claim 1, wherein the (meth)acrylic compound comprises a polyfunctional (meth)acrylic compound having 2 to 8 (meth)acryloyl groups.

8. The film-like adhesive for semiconductors according to claim 1 , wherein the flux compound comprises a polycarboxylic acid.

9. the thickness of the first adhesive region is 1 to 50 μm; 2. The film-like adhesive for semiconductors according to claim 1, wherein the thickness of the second adhesive region is 0.5 to 2 times the thickness of the first adhesive region.

10. The film-like adhesive for semiconductors according to claim 1 , which is non-conductive.

11. 2. The film-like adhesive for semiconductors according to claim 1, which is used to bond a semiconductor chip to a base and to seal a gap between the semiconductor chip and the base.

12. A method for producing a film-like adhesive for semiconductors according to any one of claims 1 to 11, providing one of a first adhesive layer and a second adhesive layer over the other; the first adhesive layer does not contain a flux compound, and is a layer containing the first epoxy resin, the first imidazole-based curing agent, and the (meth)acrylic compound; A method for producing a film-like adhesive for semiconductors, wherein the second adhesive layer is a layer containing the second epoxy resin, the second imidazole-based curing agent, and the flux compound.

13. A film-like adhesive for semiconductors according to any one of claims 1 to 11, An adhesive tape comprising: a backgrind tape provided on the film-like adhesive for semiconductors, the backgrind tape being provided on the opposite side of the first adhesive region from the second adhesive region.

14. A step of preparing a semiconductor chip with a film-like adhesive, the semiconductor chip comprising: a semiconductor chip; and the film-like adhesive for semiconductors according to any one of claims 1 to 11, the film-like adhesive being provided on the semiconductor chip such that a surface of the first adhesive region opposite to the second adhesive region faces the semiconductor chip; a step of placing the semiconductor chip with the film-like adhesive on a base from the film-like adhesive side, and heating the semiconductor chip to electrically connect the connection portion of the semiconductor chip to the connection portion of the base and seal the gap between the semiconductor chip and the base.

15. a semiconductor chip having a first connection portion, a base having a second connection portion electrically connected to the first connection portion, and a sealing portion that bonds the semiconductor chip and the base and fills a gap between the semiconductor chip and the base, A semiconductor device, wherein the sealing portion is a cured product of the film-like adhesive for semiconductors according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Film for semiconductor, method for manufacturing semiconductor device, and semiconductor device

    JP2009239138A

  • Semiconductor device, and method for manufacturing the same

    JP2010123911A

  • Composite functional tape for semiconductor packaging and method for manufacturing semiconductor devices using the same

    JP2011515839A

  • Adhesive composition for connecting semiconductor circuits and adhesive film containing the same

    JP2021531374A

  • Film-like adhesive for semiconductors, semiconductor device manufacturing method and semiconductor device

    JP2022186809A

Cited By

  • Semiconductor adhesive, adhesive tape, semiconductor device manufacturing method, and semiconductor device

    WO2026134100A1