Maintenance method for glass-coated floor material, and release agent
A maintenance method using a stripping agent with alkali metal hydroxide and surfactant effectively removes the glass coat from glass-coated flooring while preserving the base coat, addressing inefficiencies and damage issues in existing methods, and allowing for efficient regeneration of the flooring.
Patent Information
- Application Number
- JP2023070938
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
AI Technical Summary
Existing methods for maintaining glass-coated flooring are inefficient and often damage the flooring surface due to difficulties in removing the glass coat and base coat without damaging the underlying material, leading to increased work time and costs, and potential damage from organic solvents in stripping agents.
A maintenance method involving a remover that decomposes the glass coat while leaving the base coat intact, using a stripping agent composed of alkali metal hydroxide, surfactant, and water, without organic solvents, and a process to regenerate the flooring by forming a new glass coat.
Enables easy maintenance of glass-coated flooring without adverse effects on the flooring surface, reducing work time and costs, and preventing damage to the base coat and underlying material.
Smart Images

Figure 2024156459000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a maintenance method for glass-coated flooring materials and a remover. [Background technology]
[0002] For floor materials in commercial facilities, surface coating treatments are widely performed for the purpose of maintaining the beauty and protecting the surface of the floor material. As a surface coating treatment, a method of forming a coating film by applying a coating agent to the floor material is known. Various studies have been conducted on coating agents for obtaining a coating film. For example, Patent Document 1 proposes a floor coating agent containing a silane coupling agent or an alkoxysilane as a floor coating agent that can improve the beauty and durability of the floor material. The coating film obtained by applying the coating agent proposed in Patent Document 1 contains a component having a siloxane bond. Such a coating film containing a component having a siloxane bond is called a glass coat, a glass coating, a top coat, etc. (hereinafter referred to as a glass coat). Usually, when forming a glass coat, it is widely performed to apply a base agent containing a resin to the floor material to form a base coat, and then form a glass coat on the base coat. The base coat plays a role in improving the adhesion between the flooring material and the glass coat, and in improving the smoothness of the flooring surface by filling in any irregularities present on the flooring surface. A flooring material, a base coat, and a glass coat laminated in this order is called a glass-coated flooring material (hereinafter referred to as a glass-coated flooring material).
[0003] In order to improve the deterioration of the glass coat, the deterioration of the appearance of the glass-coated flooring material due to scratches on the glass coat, and the like, and the deterioration of the durability of the glass-coated flooring material, periodic maintenance work is performed on the glass-coated flooring material. In the maintenance work, a removal work is performed to remove both the base coat and the glass coat from the flooring material, and a regeneration work is performed to form a new base coat and a new glass coat in that order on the flooring material after the removal work. Conventionally, in such a removal work, the glass coat and the base coat are scraped off using a polisher or the like. However, it is very difficult to completely scrape off only the glass coat and the base coat without damaging the surface of the flooring material, and if the surface of the flooring material is damaged, a repair work for the surface of the flooring material is required, which causes problems such as an increase in work time and an increase in work cost. In addition, the surface of the flooring material has various large and small unevenness, and when the base coat or the glass coat is formed, a part of it exists so as to fill the internal space of the recess of the flooring material. In this case, it is difficult to scrape off the base coat or the glass coat existing in the internal space of the recess of the flooring material without damaging the flooring material.
[0004] Under such circumstances, Patent Document 2 proposes a top coat composition containing an alkyloxysilane, an alkyl polysilicate, an organic polymer, an organic solvent, and an alkali-soluble resin as a coating composition for forming a glass coat. According to the top coat composition proposed in Patent Document 2, it is said that the top coat (glass coat) formed using this top coat composition can be easily removed together with the base coat made of resin wax by a stripping agent. However, in the method of removing both the base coat and the top coat as proposed in Patent Document 2, it is necessary to form the base coat again in the regeneration work, which leads to an increase in the work time and high costs in the regeneration work. In particular, the base coat is protected by the glass coat formed thereon, and in many cases, the base coat itself does not deteriorate or get scratched, and can be used as it is without any problems. In addition, the stripping agent usually contains an organic solvent, and when the base coat is removed, the floor material itself may be damaged by the organic solvent contained in the stripping agent. Furthermore, in commercial facility flooring, stickers such as store guides are often affixed to the flooring, and a base coat and glass coat are then applied on top of the stickers. If the base coat is removed with a stripping agent, the stickers may be damaged by the stripping agent, which can cause problems. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-48991 A [Patent Document 2] JP 2011-236706 A Summary of the Invention [Problem to be solved by the invention]
[0006] The main object of the present invention is to provide a maintenance method for easily maintaining a glass-coated floor material without adversely affecting the floor material, and a stripping agent that can be suitably used for this maintenance method. [Means for solving the problem]
[0007] A maintenance method for a glass-coated floor material according to an embodiment of the present disclosure is a maintenance method for a glass-coated floor material in which a first base coat containing a resin and a first glass coat containing a component having a siloxane bond are laminated in that order on a floor material, and includes a glass coat removal step of using a stripping agent capable of decomposing the first glass coat to dissolve and remove the first glass coat while leaving behind the first base coat. In the above-mentioned maintenance method, the resin contained in the first base coat may be a resin having a urethane bond, or a crosslinked acrylic resin obtained by crosslinking an acrylic resin with a crosslinking agent. In the above-mentioned maintenance method, the glass coat removing step may be followed by a glass coat forming step of forming a second glass coat containing a component having a siloxane bond on the first base coat. In the above-mentioned maintenance method, a base coat forming step of forming a second base coat containing a resin on the first base coat may be carried out before the glass coat forming step. In the above-mentioned maintenance method, the second base coat may be one that can be dissolved and removed by the stripping agent.
[0008] The stripping agent according to an embodiment of the present disclosure is a stripping agent for use on a glass-coated flooring material having a flooring material on which a base coat containing a resin and a glass coat containing a component having a siloxane bond are laminated in that order, the stripping agent containing an alkali metal hydroxide, a surfactant and water, the mass of the alkali metal hydroxide relative to the total mass of the stripping agent is 4 mass% or more and the mass of the surfactant relative to the total mass of the stripping agent is 0.01 mass% or more, and (i) the stripping agent does not contain an organic solvent, or (ii) the mass of the organic solvent relative to the total mass of the stripping agent is 6 mass% or less.
[0009] The above summary of the invention does not list all of the necessary features of the present invention, and any subcombination of these features may also constitute an invention. Effect of the Invention
[0010] According to the method for maintaining a glass-coated floor material of the present invention, the glass-coated floor material can be easily maintained without adversely affecting the floor material. Also, according to the stripping agent of the present invention, the glass-coated floor material can be easily maintained without adversely affecting the floor material. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a process diagram showing an example of a maintenance method for a glass-coated floor material according to the present embodiment. [Diagram 2] FIG. 2 is a process diagram showing an example of a maintenance method for a glass-coated floor material according to the present embodiment. [Diagram 3] FIG. 2 is a process diagram showing an example of a maintenance method for a glass-coated floor material according to the present embodiment. [Figure 4] FIG. 2 is a process diagram showing an example of a maintenance method for a glass-coated floor material according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Preferred embodiments for carrying out the present invention will be described below with reference to the drawings. Note that the following embodiments do not limit the inventions according to the claims, and all of the combinations of features described in the embodiments are not necessarily essential to the solution of the invention.
[0013] <<Maintenance method for glass coating flooring>> Hereinafter, a method for maintaining a glass-coated floor material according to an embodiment of the present disclosure (hereinafter, referred to as a maintenance method of one embodiment) will be described. Figs. 1 to 4 are process diagrams showing an example of a maintenance method for a glass-coated floor material according to this embodiment. The maintenance method of one embodiment is a method for maintaining a glass-coated floor material 10 in which a first base coat 2A containing a resin and a first glass coat 3A containing a component having a siloxane bond are laminated in this order on a floor material 1, and includes a removal step. According to the maintenance method of one embodiment, the glass-coated floor material 10 can be easily maintained without adversely affecting the floor material 1.
[0014] <Removal process> The removal step is a step of dissolving and removing the first glass coat 3A while leaving the first base coat, using a stripping agent 5 capable of decomposing the first glass coat 3A.
[0015] (Glass coating flooring) The glass-coated floor material 10 applied to the maintenance method of one embodiment may be any material that satisfies the following conditions (i) to (iii): (i) a laminate in which a floor material 1, a first base coat 2A, and a first glass coat 3A are laminated in this order, (ii) the first base coat contains a resin, and (iii) the first glass coat 3A contains a component having a siloxane bond. First, an example of a glass-coated floor material 10 that satisfies these conditions will be described.
[0016] (Flooring) In one embodiment of the maintenance method, the first glass coat 3A is dissolved and removed while leaving the first base coat 2A, and the surface of the floor material 1 is protected by the first base coat 2A during and after the removal of the first glass coat 3A. In other words, in one embodiment of the maintenance method, the contact between the stripping agent 5 and the floor material 1 can be suppressed. In one embodiment of the maintenance method, the first glass coat 3A can be removed from a glass-coated floor material 10 having any floor material 1 without adversely affecting the floor material 1. For example, even for a glass-coated floor material 10 having a floor material 1 that is damaged by the stripping agent 5, the first glass coat 3A can be removed from the floor material 1 without adversely affecting the floor material 1. Examples of the floor material 1 include plastic-based floor materials, stone-based floor materials, and wood-based floor materials. Examples of the plastic-based floor materials include vinyl-based floor materials, rubber-based floor materials, olefin-based floor materials, and coated floors. Examples of stone-based flooring materials include marble, granite, terrazzo, ceramic flooring materials, ceramics, etc. Examples of wood-based flooring materials include hardwood flooring, cork tiles, etc.
[0017] (First base coat) The glass-coated flooring material 10 is provided with a first base coat 2A located on the flooring material 1. The first base coat 2A contains a resin. Examples of the resin include acrylic resin, urethane resin, and acrylic urethane. The resin may be a crosslinked resin crosslinked with a crosslinking agent. Among the first base coats 2A containing these resins, the first base coat 2A containing a resin having a urethane bond and the first base coat 2A containing a crosslinked acrylic resin crosslinked with an acrylic resin crosslinked with a crosslinking agent have extremely good durability against the release agent 5 described below compared to base coats containing other resins. The maintenance method of one embodiment is particularly suitable for a glass-coated flooring material 10 provided with a first base coat 2A containing either or both of a resin having a urethane bond and a crosslinked acrylic resin. As an example, the first base coat 2A contains either or both of a resin having a urethane bond and a crosslinked acrylic resin in an amount of 60% by mass or more relative to the total mass of the first base coat 2A. The first base coat 2A may contain, in addition to the resin, components other than the resin and various functional components, such as surfactants, preservatives, defoamers, disinfectants, dyes, and fragrances.
[0018] (First glass coat) The glass-coated flooring material 10 has a first glass coat 3A located on a first base coat 2A. The first glass coat 3A contains a component having a siloxane bond. As an example, the first glass coat 3A is formed using a coating agent containing alkoxysilane, silica, a surfactant, a catalyst, and water. As an example, the first glass coat 3A is formed using a conventionally known siloxane-based coating agent.
[0019] (Removal agent) The release agent 5 used should be one that can decompose and dissolve the first glass coat 3A containing a component having a siloxane bond, but cannot dissolve the first base coat 2A containing a resin. An example of the release agent 5 that can be used in the maintenance method of the embodiment will be specifically described below.
[0020] In this specification, "capable of dissolving and removing the first glass coating" means that when 15 g of glass-coated pieces are placed in a beaker containing 500 ml of stripping agent, the presence of the glass-coated pieces cannot be visually confirmed after 60 minutes. Additionally, in this specification, "while leaving the first base coat behind" means that when a 15 g piece of base coat is placed in a beaker containing 500 ml of stripper, the mass loss rate of the base coat piece after 60 minutes is 10% or less.
[0021] A preferred form of the stripping agent 5 that can be used in the maintenance method of one embodiment contains an alkali metal hydroxide, a surfactant, and water. According to this form of the stripping agent 5, the alkali metal hydroxide can cut the siloxane bond of the first glass coat 3A, thereby decomposing the glass coat. In addition, the surfactant can improve the wettability of the stripping agent 5 to the surface (first glass coat 3A) of the glass-coated floor material 10. The stripping agent 5 containing an alkali metal hydroxide, a surfactant, and water will be described below.
[0022] Examples of alkali metal hydroxides include sodium hydroxide, potassium hydroxide, and lithium hydroxide. The mass of the alkali metal hydroxide relative to the total mass of the stripping agent 5 is preferably 4 mass% or more. The stripping agent 5 of this form can improve the solubility of the first glass coat 3A. The mass of the alkali metal hydroxide is preferably an amount that complies with the provisions of the Poisonous and Deleterious Substances Control Law (hereinafter referred to as the Poisonous and Deleterious Substances Control Law). Specifically, when sodium hydroxide or potassium hydroxide is used as the alkali metal hydroxide, the amount of each is preferably 5 mass% or less relative to the total mass of the stripping agent 5. In addition, when the mass of the alkali metal hydroxide relative to the total mass of the stripping agent 5 is made to be more than 5 mass%, it is preferable to combine multiple alkali metal hydroxides and adjust each mass to be 5 mass% or less relative to the total mass of the stripping agent 5. In addition, from the viewpoint of handling, the total mass of the alkali metal hydroxide is preferably 30 mass% or less relative to the total mass of the stripping agent 5.
[0023] Examples of the surfactant include nonionic surfactants and anionic surfactants. Among them, nonionic surfactants are preferable because they can realize good wettability in the release agent 5 containing an alkali metal hydroxide. Examples of the nonionic surfactant include polyoxyalkylene decyl ether, polyoxyethylene alkylphenyl ether, polyoxyethylene polyoxypropylene oxyblock copolymer, polyoxyethylene alkyl ether, polyoxyethylene sorbitan fatty acid ester, and sorbitan fatty acid ester. Examples of the anionic surfactant include sodium alkyl diphenyl ether sulfonate, sodium alkyl sulfate, and sodium alkyl benzene sulfonate.
[0024] The mass of the surfactant relative to the total mass of the stripping agent 5 is preferably 0.01 mass % or more and 10 mass % or less. Furthermore, when the protective material 7 is used in the maintenance method of one embodiment, the mass of the surfactant relative to the total mass of the stripping agent 5 is preferably 0.01 mass % or more and 2 mass % or less. By using such a stripping agent 5, it is possible to sufficiently prevent the stripping agent 5 from leaking out of the protective material 7 during the removal process. Specifically, it is possible to sufficiently prevent the stripping agent 5 from leaking out of the surface of the protective material 7 and the stripping agent 5 from penetrating between the glass-coated floor material 10 and the protective material 7.
[0025] The contact angle between the first glass coat 3A and the stripping agent 5 is preferably 59° or less. In other words, it is preferable to use a stripping agent 5 that can set the contact angle with the first glass coat 3A to 59° or less. By using such a stripping agent 5, the wettability of the stripping agent 5 with respect to the first glass coat 3A can be made sufficient. Furthermore, when a protective material 7 is used in the maintenance method of one embodiment, it is preferable to use a stripping agent 5 that can set the contact angle with the first glass coat 3A to 35° or more and 59° or less. By using such a stripping agent 5, it is possible to sufficiently prevent the stripping agent 5 from leaking out of the protective material 7 during the removal process.
[0026] The contact angle referred to in this specification means the contact angle measured by dropping 2 μL of the release agent 5 to be used on the surface of the glass-coated floor material 10 (the surface of the first glass coat 3A) to be maintained, and then measuring the contact angle 30 seconds after the drop landed using an automatic contact angle meter (CA-V type, Kyowa Interface Science Co., Ltd.).
[0027] The pH of the release agent 5 is preferably greater than 13, more preferably 13.5 or greater, even more preferably 13.9 or greater, and particularly preferably 14. Such a release agent 5 can improve the solubility of the first glass coat 3A that contains a component having a siloxane bond.
[0028] The first base coat 2A of the glass-coated flooring material 10 contains a resin. Conventionally known resins used in the first base coat 2A have low durability against organic solvents, so in order to suppress damage to the first base coat 2A, it is necessary to suppress contact between the first base coat 2A and the organic solvent. Therefore, a preferred form of the stripping agent 5 is (i) one that does not contain an organic solvent, or (ii) one that contains an organic solvent, and the content of the organic solvent is 6% by mass or less, more preferably 3% by mass or less, based on the total mass of the stripping agent 5. By using a stripping agent 5 that does not contain an organic solvent or has a reduced amount of organic solvent, damage to the first base coat 2A containing a resin can be suppressed, and as a result, the first glass coat 3A can be dissolved and removed using the stripping agent 5 while leaving the first base coat 2A. Examples of organic solvents include ethanol, benzyl alcohol, isopropyl alcohol, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, and diethylene glycol monomethyl ether.
[0029] The release agent 5 may contain functional components for imparting various functions. As an example, the release agent 5 contains a colorant. Examples of the colorant include various dyes and various pigments. Examples of the dye include ERIONYL RED A-3BN-01 (Huntsman Japan Co., Ltd.). Examples of the pigment include azo pigments (Seika First Disazo Orange PO-13 (Dainichiseika Chemicals Co., Ltd.)). As an example, the release agent 5 contains 0.001% by mass or more and 3% by mass or less of the colorant relative to the total mass of the release agent 5. By using the release agent 5 containing the colorant, it is easy to visually check whether the release agent 5 is present on the glass-coated floor material 10, that is, whether maintenance is being performed or not.
[0030] In one embodiment of the maintenance method, in the removal step, a stripping agent 5 is brought into contact with the glass-coated floor material 10 to dissolve and remove the first glass coat 3A (see Figures 1(A) and 2(B)). There is no limitation on the method of bringing the stripping agent 5 into contact with the glass-coated floor material 10, and examples thereof include a method of applying the stripping agent 5 to the surface of the glass-coated floor material 10. Examples of application methods include spray application, application using a mop, and application using a roller. There is no limitation on the amount of application of the stripping agent 5, and it may be determined appropriately depending on the thickness of the first glass coat 3A, etc. An example application amount is 1 m 2 More than 250mL per dose.
[0031] In one embodiment of the maintenance method, the release agent 5 is brought into contact with the glass-coated floor material 10 by coating or the like, and then the release agent 5 is kept in contact with the glass-coated floor material 10 until the decomposition of the first glass coat 3A is completed. The contact time may be appropriately determined depending on the thickness of the glass coating, etc. An example of the contact time is 40 minutes or more.
[0032] In one embodiment of the maintenance method, when removing a part of an area (called the first area) of the glass-coated floor material 10, the first area may be separated from another part of an area (called the second area) by a protective material 7 (see FIG. 2(A)), and then the stripping agent 5 may be brought into contact with the first area (see FIG. 2(B)). By using the protective material 7, the first glass coat 3A in the target area (first area) can be dissolved and removed. As the protective material 7, a material that is not damaged by the stripping agent 5 may be used. As the protective material 7, an adhesive type protective material 7 can be exemplified. As the adhesive type protective material 7, masking tape, vinyl tape, masking tape with cloth tape, and gum tape can be exemplified.
[0033] In the removal step, the stripping agent 5 is removed after a predetermined contact time has elapsed (see Fig. 1(B), Fig. 2(C), Fig. 3(B), Fig. 4(B)). The removal step is completed by removing the stripping agent 5. Examples of methods for removing the stripping agent 5 include a method of sucking and removing the stripping liquid using an automatic floor washer or a vacuum cleaner (wet type), and a method of scraping and removing it with a floor squeegee. After removing the stripping agent 5, the surface of the first base coat 2A may be washed with water or wiped with water.
[0034] <<Glass coating process>> The maintenance method of one embodiment may include a glass coat forming step. The glass coat forming step is a step of forming a second glass coat 3B containing a component having a siloxane bond on the first base coat 2A after the removal step. Figures 3 and 4 are process diagrams showing an example of a maintenance method for a glass-coated floor material 10 of one embodiment, and include a removal step and a glass coat forming step. In the illustrated embodiment, in the glass coat forming step performed after the removal step (see Figures 3(A), (B), 4(A), (B)), a second glass coat 3B containing a component having a siloxane bond is formed on the first base coat 2A (see Figures 3(C) and 4(D)).
[0035] In one embodiment of the maintenance method including the glass coat forming step, the glass-coated floor material 10 can be regenerated by forming a second glass coat 3B in place of the first glass coat 3A removed in the removing step. Figures 3(C) and 4(D) show the regenerated glass-coated floor material 10.
[0036] The second glass coat 3B can be formed by applying a coating agent for the second glass coat directly onto the first base coat 2A, or indirectly via a second base coat 2B, which will be described later. As the coating agent for the second glass coat, a siloxane-based glass coating agent that has been conventionally known can be appropriately selected and used. One example of the coating agent contains alkoxysilane, silica, a surfactant, a catalyst, and water.
[0037] There is no limitation on the thickness of the second glass coat, but it is preferably 2 μm or more and 50 μm or less. By setting the thickness of the second glass coat 3B to a preferred thickness, the durability of the glass-coated floor material 10 can be made sufficient, and cracks in the second glass coat 3B can be suppressed.
[0038] <<Base coat formation process>> The maintenance method of one embodiment may include a base coat forming step (see FIG. 4(C)). The base coat forming step is a step of forming a second base coat 2B on the first base coat 2A before the glass coat forming step. The second base coat 2B can be formed by applying a coating agent for the second base coat 2B onto the first base coat 2A.
[0039] The maintenance method of one embodiment includes a removing step and a base coat forming step. The maintenance method of one embodiment includes a removing step, a base coat forming step, and a glass coat forming step.
[0040] The second base coat 2B may be the same as or different from the first base coat 2A. An example of the base coat contains the components described in the base coat of the glass-coated flooring material 10. An example of the second base coat 2B contains either or both of a resin having a urethane bond and a cross-linked acrylic resin.
[0041] Another example of the second base coat 2B contains a component that can be dissolved by the above-mentioned stripping agent 5. Another example of the second base coat 2B contains an alkali-soluble component. Examples of the alkali-soluble component include acrylic acid copolymer, acrylic acid-styrene copolymer, and styrene-maleic acid copolymer. The second base coat 2B of this form can remove the second base coat 2B together with the second glass coat 3B using the above-mentioned stripping agent 5 when maintaining the glass-coated floor material 10 after the maintenance method of one embodiment including the glass coat formation process is completed, specifically, the glass-coated floor material 10 in which the floor material 1, the first base coat 2A, the second base coat 2B, and the second glass coat 3B are laminated in this order, and the base coat can be prevented from being laminated each time the glass coat removal and regeneration work are repeated.
[0042] There is no limitation on the thickness of the second base coat 2 B. As an example, the thickness of the second base coat 2 B is smaller than the thickness of the first base coat 2 A.
[0043] The above describes the maintenance method of one embodiment, focusing on the case where the glass-coated floor material 10 to be maintained is a glass-coated floor material consisting only of the floor material 1, the first base coat 2A, and the first glass coat 3A, but is not limited to this structure. For example, the glass-coated floor material 10 may have multiple base coats. In this case, at least one of the multiple base coats may be the first base coat 2A. Similarly, the glass-coated floor material 10 may have multiple glass coats including the first glass coat 3A. The floor material 1 and the first base coat 2A may not be in contact. The first base coat 2A and the first glass coat 3A may not be in contact.
[0044] <<Removal agent>> A stripper 5 according to an embodiment of the present disclosure (hereinafter referred to as a stripper 5 of one embodiment) is a stripper 5 used for a glass-coated floor material 10 having a floor material 1 on which a first base coat 2A containing a resin and a first glass coat 3A containing a component having a siloxane bond are laminated in that order, the stripper 5 containing an alkali metal hydroxide, a surfactant and water, the mass of the alkali metal hydroxide relative to the total mass of the stripper 5 is 4 mass% or more, the mass of the surfactant relative to the total mass of the stripper 5 is 0.01 mass% or more, and (i) the stripper 5 does not contain an organic solvent, or (ii) the mass of the organic solvent relative to the total mass of the stripper 5 is 6 mass% or less.
[0045] According to the stripping agent 5 of one embodiment, the glass-coated floor material 10, which is composed of the floor material 1, the first base coat 2A containing a resin, and the first glass coat 3A having a siloxane bond laminated in this order, can be easily maintained without adversely affecting the floor material 1. The stripping agent 5 of one embodiment can be appropriately selected from those described in the maintenance method of one embodiment. The same applies to the glass-coated floor material 10 for which the stripping agent 5 is used. EXAMPLES
[0046] The present invention will be described in more detail below with reference to examples and comparative examples. In the following, "parts" means parts by mass.
[0047] (Preparation of glass-coated flooring material (1)) A 7μm thick base coat was formed on a 3mm thick vinyl chloride flooring material, then a 16μm thick glass coat was formed on the base coat, and a glass-coated flooring material was produced in which the flooring material, the resin-containing base coat, and the glass coat containing a component with a siloxane bond were laminated in that order. The resin component of the base coat was a urethane resin. The glass coat was formed using a coating agent containing alkoxysilane, silica, a surfactant, a catalyst, and water.
[0048] (Preparation of glass coating floor materials (2) to (7)) Glass-coated floor materials (2) to (7) were produced in the same manner as glass-coated floor material (1), except that the base coat in glass-coated floor material (1) was changed to a base coat containing the following resin components and a base coat with a thickness of 7 μm was formed. In the base coats of glass-coated floor materials (1) to (7), the total mass (total mass) of the resin components relative to the total mass of the base coat is 60 mass% or more in all cases.
[0049] Glass coating flooring (2) ··· Urethane resin: Acrylic resin = 50:50 Glass coating flooring (3) ··· Urethane resin: Acrylic resin = 25:75 Glass coating flooring material (4) ··· Urethane resin: Acrylic resin = 21:79 Glass coating flooring material (5) ··· Urethane resin: Acrylic resin = 17:83 Glass coating flooring material (6) ··· Cross-linked acrylic resin (acrylic resin: cross-linking agent = 98:2) Glass coating flooring material (7) ··· Cross-linked acrylic resin (acrylic resin: cross-linking agent = 97:3)
[0050] (Preparation of glass coating flooring precursors (1) to (7)) In the preparation of the glass-coated flooring materials (1) to (7) prepared above, those not forming a glass coating were designated as glass-coated flooring material precursors (1) to (7).
[0051] (Preparation of release agent) Release agents (Release Agents No. 1 to No. 12) were prepared with the compositions shown in Table 1 below. The units of values in the table are parts by mass.
[0052] [Table 1]
[0053] The components in Table 1 used were as follows: Sodium hydroxide (caustic soda (granular) AGC Co., Ltd.) Potassium hydroxide (flake caustic potash, Toagosei Co., Ltd.) Lithium hydroxide (Lithium hydroxide monohydrate (Wako special grade) Fujifilm Wako Pure Chemical Industries, Ltd.) Sodium orthosilicate (Granular Orthosilicate, Nippon Chemical Industry Co., Ltd.) Ethanol (SS-K-75 Shinwa Alcohol Industry Co., Ltd.) Sodium alkyl diphenyl ether sulfonate (Pelex SS-L, Kao Corporation)
[0054] Release agents (Release Agents No. 21 to No. 31) were prepared with the compositions shown in Table 2 below. The units of values in the table are parts by mass.
[0055] [Table 2]
[0056] The components shown in Table 2 were as follows: Sodium hydroxide (caustic soda (granular) AGC Co., Ltd.) Potassium hydroxide (flake caustic potash, Toagosei Co., Ltd.) Sodium orthosilicate (Granular Orthosilicate, Nippon Chemical Industry Co., Ltd.) Sodium metasilicate nonahydrate (Sodium metasilicate nonahydrate, Nippon Chemical Industry Co., Ltd.) Sodium carbonate (soda ash (light) Tokuyama Corporation) Monoisopropanolamine (Monoisopropanolamine Dow Chemical Japan Co., Ltd.) Limonene (D-Limonene, Yasuhara Chemical Co., Ltd.) Diethylene glycol monoethyl ether (Hisorb DE, Toho Chemical Industry Co., Ltd.) ·Diethylene glycol monobutyl ether (Butyl Carbitol (registered trademark) Solvent Dow Chemical Japan Co., Ltd.) Propylene glycol monoethyl ether (PE-P KH Neochem Co., Ltd.) Dipropylene glycol monomethyl ether (DOWANOL® DPM glycol ether, Dow Chemical Japan Co., Ltd.) Benzyl alcohol (Benzyl alcohol Kusumoto Chemicals Co., Ltd.) Ethanol (SS-K-75 Shinwa Alcohol Industry Co., Ltd.) 3-Methoxy-3-methyl-1-butanol (Solfit Kuraray Co., Ltd.) Sodium alkyl diphenyl ether sulfonate (Pelex SS-L, Kao Corporation) Polyoxyalkylene decyl ether (Noigen XL-80, Daiichi Kogyo Seiyaku Co., Ltd.) Tetradecyldimethylbenzylammonium chloride (Japanese Pharmacopoeia benzalkonium chloride, NOF Corp.) Tetrasodium ethylenediaminetetraacetate (Trilon® BX Powder BASF Ltd.) · Trisodium nitrilotriacetate (Sodium nitrilotriacetate monohydrate, Fujifilm Wako Pure Chemical Industries, Ltd.) Citric acid (Citric acid (crystal) S Iwata Chemical Industry Co., Ltd.)
[0057] (Glass coating removability evaluation) The glass-coated flooring material and the release agent prepared above were combined as shown in Table 3 below, and the release agent was applied to the glass-coated flooring material in a thickness of 1 m. 2 The coating amount was 500 mL per 1000 mm, and after 60 minutes, the release agent was wiped off with a paper rag, and then washed with running water. The condition of the glass-coated flooring material after washing was confirmed by visual inspection and infrared absorption spectrum measurement, and the removability of the glass coat was evaluated according to the following evaluation criteria. The evaluation results are also shown in Table 3. Note that only in Example 21, the release agent was wiped off with a paper rag after 40 minutes.
[0058] "Evaluation Criteria" A: The infrared absorption spectrum showed no absorption band of the glass coating, and more than 90% of the glass coating was visually peeled off. NG(1): The infrared absorption spectrum showed an absorption band of the glass coating, but visual inspection revealed that 10% to less than 90% of the glass coating was peeled off. NG(2): Although there is an absorption band of the glass coating in the infrared absorption spectrum, less than 10% of the glass coating was peeled off visually, or none of the glass coating was peeled off.
[0059] (Evaluation of impact on base coat) The glass-coated flooring precursor and release agent prepared above were combined as shown in Table 3 below, and a 3 cm diameter filter paper was placed on the glass-coated flooring precursor, soaked in 0.5 mL of release agent, and left to stand for 1 hour. After 1 hour, the release agent was wiped off with a paper rag, and then washed with running tap water. After washing with water, the condition of the glass-coated flooring precursor in the area that had come into contact with the release agent was confirmed visually and by infrared absorption spectrum measurement, and the impact on the base coat was evaluated according to the following evaluation criteria. The evaluation results are also shown in Table 3.
[0060] "Evaluation Criteria" A: The absorption band of the base coat can be confirmed in the infrared absorption spectrum, and there is no change in the base coat to the naked eye. B: The absorption band of the base coat can be confirmed in the infrared absorption spectrum, and changes can be seen with the naked eye, but the base coat remains. NG: The absorption band of the base coat cannot be confirmed in the infrared absorption spectrum, or part or all of the base coat has been removed.
[0061] (Wettability evaluation) The glass-coated flooring material prepared above and the release agent were combined as shown in Table 3 below, and the release agent was dropped onto the surface of the glass-coated flooring material cut to 45 cm x 45 cm (the surface of the glass coat). 2 The mixture was spread evenly with a spreading rag so that the amount of coating was 500 mL per sample. Five minutes after spreading, the condition was visually checked, and wettability was evaluated based on the following evaluation criteria. The evaluation results are also shown in Table 3. Note that a state in which the entire surface of a 45 cm x 45 cm area is wet is considered to be 100%.
[0062] "Evaluation Criteria" A: More than 90% of the area is evenly coated. B: Coating is successful over 50% to less than 90% of the area. NG: The release agent is repelled and coating is not possible, or less than 50% of the area is coated.
[0063] (Durability evaluation of protective materials) The glass-coated flooring material prepared above was combined with a release agent as shown in Table 3 below, and the durability of the protective material was evaluated. For the durability evaluation, a 5 cm length of vinyl tape No. 21 (Nittoms Corporation) was attached to the surface (glass-coated surface) of a glass-coated flooring material cut to 10 cm x 5 cm, and a roller was used to remove air from the adhesive surface to prepare a glass-coated flooring material with protective material. 500 mL of release agent was poured into a 500 mL beaker, and the glass-coated flooring material with protective material was immersed in this beaker. After 60 minutes, the condition of the vinyl tape was visually confirmed and evaluated according to the following evaluation criteria. The evaluation results are also shown in Table 3.
[0064] "Evaluation Criteria" A: Vinyl tape is attached to the entire surface of the glass-coated flooring. NG: Part of the vinyl tape is floating away from the glass-coated flooring material, or the vinyl tape has peeled off from the glass-coated flooring material.
[0065] (Contact angle measurement) The glass-coated flooring materials prepared above were combined with release agents as shown in Table 3 below, and 2 μL of the release agent was dropped onto the surface of the glass-coated flooring materials (glass-coated surface). 30 seconds after the drops had landed, the contact angles were measured three times using an automatic contact angle meter (CA-V type, Kyowa Interface Science Co., Ltd.). The measurement results are also shown in Table 3. The contact angles in the table are the average values of three measurements.
[0066] [Table 3] [Explanation of symbols]
[0067] 1. Flooring 2A: First base coat 2B: Second base coat 3A: First glass coating 3B: Second glass coat 5. Stripping agent 7...Curing material 10. Glass coating flooring
Claims
1. A maintenance method for a glass-coated floor material in which a first base coat containing a resin and a first glass coat containing a component having a siloxane bond are laminated in this order on a floor material, comprising: A glass coat removing step of dissolving and removing the first glass coat while leaving the first base coat by using a stripping agent capable of decomposing the first glass coat. How to maintain glass coating flooring.
2. The resin contained in the first base coat is a resin having a urethane bond or a crosslinked acrylic resin obtained by crosslinking an acrylic resin with a crosslinking agent. A maintenance method for the glass-coated floor material according to claim 1.
3. A glass coat forming step of forming a second glass coat containing a component having a siloxane bond on the first base coat after the glass coat removing step is included. A maintenance method for the glass-coated floor material according to claim 1 or 2.
4. A base coat forming step of forming a second base coat containing a resin on the first base coat before the glass coat forming step is included. A maintenance method for the glass-coated floor material according to claim 3.
5. The second base coat can be dissolved and removed by the stripping agent. A maintenance method for the glass-coated floor material according to claim 4.
6. A release agent for use on a glass-coated flooring material in which a base coat containing a resin and a glass coat containing a component having a siloxane bond are laminated in this order on a flooring material, The stripping agent contains an alkali metal hydroxide, a surfactant, and water, the mass of the alkali metal hydroxide is 4 mass% or more relative to the total mass of the stripping agent; the mass of the surfactant relative to the total mass of the release agent is 0.01 mass% or more; (i) the stripping agent does not contain an organic solvent, or (ii) the mass of the organic solvent relative to the total mass of the stripping agent is 6 mass% or less; Stripping agent.
Citation Information
Patent Citations
Topcoat composition and floor structure
JP2011236706A
Coating agent for floor, coating method for floor, and method for manufacturing floor structure