Photosensitive resin composition, cured product, substrate with partition and method for producing the same, and image display device

A photosensitive resin composition with a fluorine-containing liquid repellent addresses the issue of quantum dot ink overflow in micro LED displays by forming partition walls with sufficient ink repellency, enhancing manufacturing precision and display quality.

JP2024157185AInactive Publication Date: 2024-11-07RESONAC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023071364
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The challenge in manufacturing micro LED displays is the overflow of quantum dot ink along partition walls due to high affinity, despite the use of fluorine-based liquid repellents, which do not effectively impart sufficient ink repellency in the partition walls formed by photolithography methods.

Method used

A photosensitive resin composition comprising an alkali-soluble binder polymer, photopolymerizable monomer, photopolymerization initiator, and a fluorine-containing liquid repellent with a weight average molecular weight of 2000 or more, which forms partition walls with sufficient ink repellency by incorporating the fluorine compound into the cured product, enhancing its repellency and segregation on the surface.

Benefits of technology

The solution effectively prevents quantum dot ink overflow by forming partition walls with high ink repellency, ensuring precise application and retention of quantum dot ink in micro LED displays, thereby improving manufacturing efficiency and display quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157185000012
    Figure 2024157185000012
  • Figure 2024157185000013
    Figure 2024157185000013
  • Figure 2024157185000014
    Figure 2024157185000014
Patent Text Reader

Abstract

To provide a photosensitive resin composition or the like capable of forming a partition with sufficient ink-repelling capability.SOLUTION: A photosensitive resin composition disclosed herein includes: an alkali-soluble binder polymer; a photopolymerizable monomer with an ethylenically unsaturated group; a photopolymerization initiator; and a liquid repellent agent, where the liquid repellent agent includes a fluorine-containing compound with a photocurable group, featuring a weight average molecular weight of 2000 or more, and the content of the fluorine-containing compound is 1 mass% or more relative to the total amount of the photosensitive resin composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a photosensitive resin composition, a cured product, a substrate with partition walls and a method for producing the same, and an image display device. [Background technology]

[0002] Display devices such as liquid crystal displays and LED displays usually emit red, green, or blue light in each area partitioned by patterned partitions (see, for example, Patent Document 1 below). In the case of LED displays, there are also known configurations that use only blue LED elements as light emitters and have a color conversion device that converts blue light into red or green light in a predetermined partitioned area.

[0003] In recent years, quantum dots have been attracting attention as light-emitting materials. Quantum dots are semiconductor nanocrystals with diameters ranging from several nm to several tens of nm, and exhibit unique optical and electrical properties. Their use in displays has also been proposed. For example, Patent Document 2 below proposes the production of quantum dot light-emitting elements by applying quantum dot ink by an inkjet method.

[0004] Meanwhile, advances in LED manufacturing technology have led to the development of micro LED elements, which are expected to be applied to next-generation displays (see, for example, Patent Document 3 below). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2012 / 147626 [Patent Document 2] US Patent Application Publication No. 2017 / 0174921 [Patent Document 3] JP 2012-142489 A Summary of the Invention [Problem to be solved by the invention]

[0006] Therefore, the inventors have investigated the configuration and productivity of a micro LED display in which micro LED elements are arranged.

[0007] When a color conversion device that converts the color of the light of a micro LED element in a predetermined partitioned region is mounted on a micro LED display, the color conversion section surrounded by the partition wall is also miniaturized. As a method for forming such a color conversion section with good productivity, a process is considered in which a partition wall is formed on a substrate by a photolithography method in which a photosensitive resin composition is used for exposure and development, and a quantum dot ink is applied to a recess in which the color conversion section is to be formed by an inkjet method. However, in such a process, if the affinity between the partition wall and the quantum dot ink is high, there is a problem that the quantum dot ink easily flows down the partition wall and overflows from the recess.

[0008] A fluorine-based liquid repellent agent is known as a technique for imparting liquid repellency to the surface of a substrate. However, the present inventors have found through their investigations that even if a liquid repellent agent is blended into a photosensitive resin composition, the partition walls formed by the above-mentioned method may not exhibit the desired ink repellency.

[0009] The present disclosure has been made in consideration of the above circumstances, and aims to provide a photosensitive resin composition capable of forming a partition wall having sufficient ink repellency, a cured product, a substrate with partition wall, and an image display device, as well as a method for manufacturing a substrate with partition wall and a method for manufacturing a color conversion device. [Means for solving the problem]

[0010] One aspect of the present disclosure relates to the following [1] to

[14] . [1] A photosensitive resin composition comprising an alkali-soluble binder polymer, a photopolymerizable monomer having an ethylenically unsaturated group, a photopolymerization initiator, and a liquid repellent agent, wherein the liquid repellent agent contains a fluorine-containing compound having a photocurable group and having a weight-average molecular weight of 2000 or more, and the content of the fluorine-containing compound is 1 mass% or more based on the total amount of the photosensitive resin composition. [2] The photosensitive resin composition according to [1], wherein the fluorine-containing compound has an alicyclic skeleton. [3] The photosensitive resin composition according to [1] or [2], wherein the alkali-soluble binder polymer has an acid value of 25 to 125 mgKOH / g. [4] The photosensitive resin composition according to any one of [1] to [3], wherein the photopolymerizable monomer has three or more functional groups in one molecule, and the three or more functional groups include an ethylenically unsaturated group and a hydroxyl group. [5] The photosensitive resin composition according to any one of [1] to [4], wherein the photopolymerization initiator includes an acylphosphine oxide-based photopolymerization initiator. [6] A cured product obtained by curing the photosensitive resin composition according to any one of [1] to [5]. [7] A substrate with partition walls, comprising a substrate and partition walls provided on the substrate, the partition walls being made of the cured product according to [6]. [8] An image display device comprising the substrate with partition walls according to [7]. [9] A method for producing a substrate with partition walls, comprising: a photosensitive resin layer forming step of forming a photosensitive resin layer on a substrate using the photosensitive resin composition according to any one of [1] to [5]; an exposure step of exposing the photosensitive resin layer provided on the substrate to light in a predetermined pattern; and a development step of forming partition walls by alkaline development of the exposed photosensitive resin layer.

[10] A method for manufacturing a color conversion device having a color conversion section surrounded by a partition, the method comprising: preparing a substrate with partitions as described in [7], in which the partitions define a recess that serves as a formation area for the color conversion section; and applying a quantum dot ink to the recess by an inkjet method. Effect of the Invention

[0011] According to the present disclosure, there are provided a photosensitive resin composition capable of forming partition walls having sufficient ink repellency, a cured product, a substrate with partition walls, and an image display device, as well as a method for manufacturing a substrate with partition walls and a method for manufacturing a color conversion device. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a partial cross-sectional view showing a photosensitive resin layer forming step in an embodiment of a method for producing a substrate with partition walls according to the present disclosure. [Diagram 2] FIG. 2 is a partial cross-sectional view showing an exposure step in an embodiment of a method for producing a substrate with partition walls according to the present disclosure. [Diagram 3] 3 is a partial cross-sectional view showing a second laminate obtained in the exposure step of FIG. 2. [Figure 4] FIG. 2 is a partial cross-sectional view showing a development step in an embodiment of a method for producing a substrate with partition walls according to the present disclosure. [Diagram 5] FIG. 1 is a plan view showing a substrate with partition walls according to the present disclosure. [Figure 6] 4A to 4C are partial cross-sectional views showing a coating step in an embodiment of a method for manufacturing a color conversion device according to the present disclosure. [Figure 7] 1 is a partial cross-sectional view of a color conversion device according to the present disclosure. [Figure 8] FIG. 1 is a plan view illustrating a color conversion device according to the present disclosure. [Figure 9] 1 is a partial cross-sectional view showing an image display device according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the embodiments for carrying out the present disclosure will be described in detail with reference to the drawings as needed. However, the present disclosure is not limited to the following embodiments. In this specification, "(meth)acrylic acid" means acrylic acid or methacrylic acid, and "(meth)acrylate" means acrylate or the corresponding methacrylate.

[0014] <Photosensitive resin composition and its cured product> The photosensitive resin composition of the present disclosure contains (A) an alkali-soluble binder polymer (hereinafter, sometimes referred to as component (A)), (B) a photopolymerizable monomer having an ethylenically unsaturated group (hereinafter, sometimes referred to as component (B)), (C) a photopolymerization initiator (hereinafter, sometimes referred to as component (C)), and (D) a liquid repellent (hereinafter, sometimes referred to as component (D)). Here, the liquid repellent contains a fluorine-containing compound (hereinafter, sometimes referred to as component (D-1)) having a photocurable group and a weight average molecular weight of 2000 or more, and the content of the fluorine-containing compound is 1 mass% or more based on the total amount of the photosensitive resin composition. The cured product of the present disclosure is obtained by curing the above-mentioned photosensitive resin composition.

[0015] According to the photosensitive resin composition of the present disclosure, a partition wall having sufficient ink repellency can be formed. The reason for obtaining such an effect is presumed to be as follows. When forming a partition wall using a photosensitive resin composition, the photosensitive resin composition is applied onto a substrate to form a photosensitive resin layer, which is exposed to light in a predetermined pattern, and then developed with an alkaline developer. It is considered that the above-mentioned fluorine compound has a photocurable group and the above-mentioned specific weight-average molecular weight, and therefore (i) the fluorine-containing compound is firmly incorporated into the cured product in the exposed portion of the photosensitive resin layer, thereby suppressing elution during development, and (ii) the amount of fluorine contained in one molecule can be increased and easily segregated on the surface, and the like, thereby imparting sufficient ink repellency to the partition wall.

[0016] (Alkali-soluble binder polymer) Examples of the alkali-soluble binder polymer include acrylic resins, styrene resins, epoxy resins, amide resins, amide epoxy resins, alkyd resins, phenol resins, ester resins, urethane resins, epoxy acrylate resins obtained by reacting epoxy resins with (meth)acrylic acid, acid-modified epoxy acrylate resins obtained by reacting epoxy acrylate resins with acid anhydrides, etc. These resins may have an ethylenically unsaturated group.

[0017] The alkali-soluble binder polymer may have a carboxy group from the viewpoint of improving the alkali developability.

[0018] From the viewpoint that the ink repellency due to the (D-1) component is easily expressed in the cured product of the present disclosure, the alkali-soluble binder polymer may contain a polymer (hereinafter sometimes referred to as the (A-1) component) containing the structural unit (a) represented by the following formula (1), the structural unit (b) represented by the following formula (2), the structural unit (c) represented by the following formula (3), and the structural unit (d) represented by the following formula (4). From the same viewpoint, the alkali-soluble binder polymer may contain a polymer (hereinafter sometimes referred to as the (A-2) component) containing the structural unit (a) represented by the following formula (1), the structural unit (b) represented by the following formula (2), the structural unit (d) represented by the following formula (4), and the structural unit (e) represented by the following formula (5). [ka] (In the above formula (1), R 1 represents a hydrogen atom or a methyl group, and X represents an alicyclic hydrocarbon group which may have a substituent. [ka] (In the above formula (2), R 2 represents a hydrogen atom or a methyl group, and Y represents an aromatic group which may have a substituent. [ka] (In the above formula (3), R 3 represents a hydrogen atom or a methyl group. [ka] (In the above formula (4), R 4 and R 5 each independently represents a hydrogen atom or a methyl group. [ka] (In the above formula (5), R 6 and R 7 each independently represents a hydrogen atom or a methyl group.

[0019] X in the formula (1) representing the structural unit (a) represents an alicyclic hydrocarbon group which may have a substituent. The number of carbon atoms in the alicyclic hydrocarbon group may be 7 to 20. Examples of the substituent include halogen atoms such as fluoro, chloro, and bromo, and hydroxyl groups. Examples of the alicyclic hydrocarbon group include an adamantyl group, a tricyclodecyl group, an isobornyl group, and a cyclohexyl group.

[0020] The structural unit (a) can be introduced by using an alicyclic hydrocarbon group-containing polymerizable monomer as the polymerizable monomer used when producing an alkali-soluble binder polymer by copolymerization. The alicyclic hydrocarbon group-containing polymerizable monomer is represented, for example, by the following general formula (1A). CH2=C(R 1 )-COOX…(1A)

[0021] Examples of the alicyclic hydrocarbon group-containing polymerizable monomer represented by the above general formula (1A) include adamantyl (meth)acrylate, tricyclodecanyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, etc. These alicyclic hydrocarbon group-containing polymerizable monomers may be used alone or in combination of two or more.

[0022] In formula (2) representing the structural unit (b), Y represents an aromatic group which may have a substituent. The aromatic group may have an aromatic ring, and is represented, for example, by -PQ. Here, P represents a single bond or -COO-, and Q represents an aromatic hydrocarbon group which may have a substituent. Examples of the aromatic hydrocarbon group include aryl groups such as a phenyl group and a naphthyl group, aralkyl groups such as a benzyl group, and a styryl group.

[0023] The structural unit (b) can be introduced by using an aromatic hydrocarbon group-containing polymerizable monomer as the polymerizable monomer used when producing an alkali-soluble binder polymer by copolymerization. The aromatic hydrocarbon group-containing polymerizable monomer is represented by the following general formula (2A). CH2=C(R 2 )-Y …(2A)

[0024] Examples of the aromatic hydrocarbon group-containing polymerizable monomer represented by the general formula (2A) include aromatic hydrocarbon group-containing (meth)acrylates such as benzyl (meth)acrylate, phenyl (meth)acrylate, naphthyl (meth)acrylate, etc., and aromatic vinyl compounds such as styrene, etc. These aromatic hydrocarbon group-containing polymerizable monomers may be used alone or in combination of two or more.

[0025] The structural unit (c) can be introduced by using (meth)acrylic acid as a polymerizable monomer when producing an alkali-soluble binder polymer by copolymerization. (Meth)acrylic acid is highly reactive and easily available.

[0026] The structural unit (d) can be introduced, for example, by using a polymerizable monomer represented by the following formula (4A) as the polymerizable monomer used when producing an alkali-soluble binder polymer. [ka] The structural unit (d) can also be introduced by adding glycidyl (meth)acrylate to some of the carboxy groups of the structural unit (c).

[0027] The structural unit (e) may be introduced, for example, by introducing the structural unit (c) using (meth)acrylic acid as a polymerizable monomer used in producing an alkali-soluble binder polymer, followed by adding glycidyl (meth)acrylate to a portion of the carboxy groups in the structural unit (c), and then reacting with succinic anhydride; alternatively, the structural unit (d) may be introduced using a polymerizable monomer represented by the above formula (4A) as a polymerizable monomer used in producing an alkali-soluble binder polymer, followed by reacting with succinic anhydride.

[0028] In the component (A-1), when the total of the above structural units (a), (b), (c), and (d) is taken as the standard (100 mol%), the proportion of the structural unit (a) is not particularly limited as long as it is greater than 0 mol%, but it may be 0.1 mol% or more, 0.5 mol% or more, or 1 mol% or more, the proportion of the structural unit (a) may be 30 mol% or less, 29 mol% or less, or 28 mol% or less, and the proportion of the structural unit (a) may be 10 to 25 mol%, or 15 to 20 mol%.

[0029] In the component (A-1), when the total of the above structural units (a), (b), (c), and (d) is taken as the standard (100 mol%), the proportion of the structural unit (b) is not particularly limited as long as it is greater than 0 mol%, but may be 0.1 mol% or more, 0.5 mol% or more, or 1.0 mol% or more, the proportion of the structural unit (b) may be less than 20 mol%, 19 mol% or less, or 18 mol% or less, and the proportion of the structural unit (b) may be 0.5 to 10 mol%, or may be 1 to 5 mol%.

[0030] In the component (A-1), when the total of the above structural units (a), (b), (c), and (d) is taken as the standard (100 mol%), the proportion of structural unit (c) is not particularly limited as long as it is greater than 0 mol%, but may be 1 mol% or more, 2 mol% or more, or 3 mol% or more, the proportion of structural unit (c) may be 35 mol% or less, 34 mol% or less, or 33 mol% or less, and the proportion of structural unit (c) may be 10 to 25 mol%, or 15 to 20 mol%.

[0031] In the component (A-1), when the total of the structural units (a), (b), (c), and (d) is taken as 100 mol%, the proportion of structural units (d) may be 45 mol% or more, 47 mol% or more, or 49 mol% or more, the proportion of structural units (d) may be 85 mol% or less, 83 mol% or less, or 81 mol% or less, and the proportion of structural units (d) may be 50 to 70 mol%, or may be 60 to 65 mol%.

[0032] In the component (A-2), Y in the structural unit (b) may be a phenyl group, and R in the structural unit (d) may be 5 may be a hydrogen atom.

[0033] In the component (A-2), when the total of the structural units (a), (b), (d), and (e) is taken as the standard (100 mol%), the proportion of the structural unit (a) is not particularly limited as long as it is greater than 0 mol%, but it may be 1 mol% or more, 2 mol% or more, or 3 mol% or more, the proportion of the structural unit (a) may be 50 mol% or less, 45 mol% or less, or 40 mol% or less, and the proportion of the structural unit (a) may be 20 to 40 mol%, or may be 25 to 35 mol%.

[0034] In the component (A-2), when the total of the above structural units (a), (b), (d), and (e) is taken as the standard (100 mol%), the proportion of structural unit (b) is not particularly limited as long as it is greater than 0 mol%, but may be 1 mol% or more, 3 mol% or more, or 5 mol% or more, the proportion of structural unit (b) may be 35 mol% or less, 30 mol% or less, or 25 mol% or less, and the proportion of structural unit (b) may be 5 to 20 mol%, or may be 5 to 15 mol%.

[0035] In the component (A-2), when the total of the structural units (a), (b), (d), and (e) is taken as the standard (100 mol%), the proportion of the structural unit (d) is not particularly limited as long as it is greater than 0 mol%, but may be 1 mol% or more, 5 mol% or more, or 10 mol% or more, the proportion of the structural unit (d) may be 55 mol% or less, 50 mol% or less, or 45 mol% or less, and the proportion of the structural unit (d) may be 20 to 40 mol%, or may be 25 to 35 mol%.

[0036] In the component (A-2), when the total of the structural units (a), (b), (d), and (e) is taken as the standard (100 mol%), the proportion of the structural unit (e) is not particularly limited as long as it is greater than 0 mol%, but it may be 1 mol% or more, 10 mol% or more, or 15 mol% or more, the proportion of the structural unit (e) may be 75 mol% or less, 70 mol% or less, or 65 mol% or less, and the proportion of the structural unit (e) may be 25 to 45 mol%, or 30 to 40 mol%.

[0037] When the alkali-soluble binder polymer has a double bond such as an ethylenically unsaturated group, the double bond equivalent may be 250 g / mol or more, 260 g / mol or more, 270 g / mol or more, or 280 g / mol or more from the viewpoint of photocurability, and may be 440 g / mol or less, 400 g / mol or less, or 380 g / mol or less from the viewpoint of photocurability. The double bond equivalent of the alkali-soluble binder polymer is the mass of the polymer per mole of the polymerizable unsaturated bond, and is calculated based on the amount of monomer used.

[0038] The solid acid value of the alkali-soluble binder polymer is not particularly limited, but may be 25 mgKOH / g or more, or 30 mgKOH / g or more. When the solid acid value of the alkali-soluble binder polymer is 25 mgKOH / g or more, the solubility in the developer during development can be improved. The solid acid value of the alkali-soluble binder polymer may be 125 mgKOH / g or less, or 120 mgKOH / g or less. When the solid acid value of the alkali-soluble binder polymer is 125 mgKOH / g or less, the binder polymer is unlikely to show excessive solubility in the developer during development. The solid acid value means the number of mg of potassium hydroxide required to neutralize the acid present in 1 g of the alkali-soluble binder polymer.

[0039] The weight average molecular weight of the alkali-soluble binder polymer may be 3,000 to 30,000, 3,500 to 25,000, or 4,000 to 20,000 from the viewpoint of balancing mechanical strength and alkali developability. In order to obtain excellent developer resistance after exposure, the weight average molecular weight may be 4,000 or more. In addition, in terms of development time, the weight average molecular weight may be 20,000 or less. The weight average molecular weight is a value measured by gel permeation chromatography (GPC) and converted using a calibration curve prepared using standard polystyrene.

[0040] The alkali-soluble binder polymers can be used alone or in combination of two or more.

[0041] (Photopolymerizable monomer) The photopolymerizable monomer may be one having an ethylenically unsaturated group.

[0042] Examples of photopolymerizable monomers having an ethylenically unsaturated group include compounds obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid, bisphenol A-based (meth)acrylate compounds such as 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane, 2,2-bis(4-((meth)acryloxypolypropoxy)phenyl)propane, and 2,2-bis(4-((meth)acryloxypolyethoxypolypropoxy)phenyl)propane, compounds obtained by reacting a glycidyl group-containing compound with an α,β-unsaturated carboxylic acid, urethane monomers such as (meth)acrylate compounds having a urethane bond, γ-chloro-β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate, β-hydroxyethyl-β'-(meth)acryloyloxyethyl-o-phthalate, β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate, and (meth)acrylic acid alkyl esters.

[0043] Examples of compounds obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid include polyethylene glycol di(meth)acrylate having 2 to 14 ethylene groups, polypropylene glycol di(meth)acrylate having 2 to 14 propylene groups, polyethylene polypropylene glycol di(meth)acrylate having 2 to 14 ethylene groups and 2 to 14 propylene groups, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane ethoxy tri(meth)acrylate, trimethylolpropane diethoxy tri(meth)acrylate, and trimethylolpropane diethoxy tri(meth)acrylate. acrylate, trimethylolpropane triethoxy tri(meth)acrylate, trimethylolpropane tetraethoxy tri(meth)acrylate, trimethylolpropane pentaethoxy tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, polypropylene glycol di(meth)acrylate having 2 to 14 propylene groups, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0044] Examples of the urethane monomer include an addition reaction product of a (meth)acrylic monomer having a hydroxyl group at the β-position with a diisocyanate compound such as isophorone diisocyanate, 2,6-toluene diisocyanate, 2,4-toluene diisocyanate, or 1,6-hexamethylene diisocyanate, tris[(meth)acryloxytetraethylene glycol isocyanate]hexamethylene isocyanurate, EO-modified urethane di(meth)acrylate, and EO,PO-modified urethane di(meth)acrylate. Note that "EO" stands for ethylene oxide, and an EO-modified compound has a block structure of ethylene oxide groups. Also, "PO" stands for propylene oxide, and a PO-modified compound has a block structure of propylene oxide groups.

[0045] The number of functional groups in one molecule of the photopolymerizable monomer may be 2 or more, or 3 or more. Two or more types of photopolymerizable monomers, a photopolymerizable monomer having 2 or more functional groups and a photopolymerizable monomer having 3 or more functional groups, may be used in combination.

[0046] In the case where the number of functional groups in one molecule of the photopolymerizable monomer is 3 or more, all of the 3 or more functional groups may be ethylenically unsaturated groups, but the 3 or more functional groups may further include a hydroxyl group in addition to the ethylenically unsaturated group. In this case, the developability of the partially cured layer obtained after the exposure of the photosensitive resin layer is further improved. In addition, the swelling of the cured part due to the exposure of the partially cured layer during development by the developer can be suppressed, and the resolution of the photosensitive resin composition can be further improved.

[0047] The number of functional groups in one molecule may be 26 or less, or 5 or less.

[0048] As the photopolymerizable monomer, the above-mentioned compounds can be used alone or in combination of two or more kinds.

[0049] The content of the photopolymerizable monomer in the photosensitive resin composition may be 5 to 50 parts by mass or 5 to 30 parts by mass relative to 100 parts by mass of the total amount of the alkali-soluble binder polymer and the photopolymerizable monomer. When the content of the photopolymerizable monomer is 5 parts by mass or more, the photocurability of the photosensitive resin layer tends to be good, and when it is 50 parts by mass or less, when a photosensitive resin layer is formed on a substrate using the photosensitive resin composition, the photosensitive resin layer tends to have excellent shape retention before exposure.

[0050] (Photopolymerization initiator) The photopolymerization initiator is a compound that initiates the reaction between the alkali-soluble binder polymer and the photopolymerizable monomer, and the reaction between the photopolymerizable monomers themselves, and the photopolymerization initiator can be appropriately selected depending on the light wavelength of the exposure machine used, and known initiators such as photoradical polymerization initiators and photocationic polymerization initiators can be used. The photopolymerization initiator can be used alone or in combination of two or more types.

[0051] Examples of the photoradical polymerization initiator include aromatic ketones such as benzophenone, N,N'-tetraalkyl-4,4'-diaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propanone-1, 4,4'-bis(dimethylamino)benzophenone (Michler's ketone), 4,4'-bis(diethylamino)benzophenone, and 4-methoxy-4'-dimethylaminobenzophenone; quinones such as alkylanthraquinone and phenanthrenequinone; benzoin compounds such as benzoin and alkylbenzoin; benzoin ether compounds such as benzoin alkyl ether and benzoin phenyl ether; benzoin ether compounds such as benzoin alkyl ether and benzoin phenyl ether; benzyl derivatives such as aryl dimethyl ketal; 2,4,5-triarylimidazole dimers such as 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(m-methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, 2,4-di(p-methoxyphenyl)-5-phenylimidazole dimer, and 2-(2,4-dimethoxyphenyl)-4,5-diphenylimidazole dimer; N-phenylglycine, N-phenylglycine derivatives, and acridine derivatives such as 9-phenylacridine; 1-[4-(phenylthio)phenyl]-1,2-octanedione. Examples of such compounds include oxime esters such as 2-(O-benzoyloxime), coumarin compounds such as 7-diethylamino-4-methylcoumarin, thioxanthone compounds such as 2,4-diethylthioxanthone, and acylphosphine oxide compounds such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide.

[0052] Among them, the acylphosphine oxide-based photopolymerization initiator has a photobleaching function, and therefore becomes less likely to absorb light after being decomposed by exposure. Therefore, during exposure, light can reach a sufficiently deep position from the surface of the photosensitive resin layer over time, and therefore insufficient curing of the exposed portion can be suppressed. Therefore, dissolution or swelling of the cured portion due to exposure during development can be suppressed, and the resolution of the partition wall (particularly the partition wall having light-shielding properties) can be further improved.

[0053] The acylphosphine oxide photopolymerization initiator has an acylphosphine oxide group (>P(=O)-C(=O)- group), and examples thereof include (2,6-dimethoxybenzoyl)-2,4,6-pentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide (product name: IRGACURE-TPO, manufactured by BASF), ethyl-2,4,6-trimethylbenzoylphenylphosphinenate, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (product name: IRGACURE-819, manufactured by BASF), (2,5-dihydroxyphenyl)diphenylphosphine oxide, (p-hydroxyphenyl)diphenylphosphine oxide, bis(p-hydroxyphenyl)phenylphosphine oxide, and tris(p-hydroxyphenyl)phosphine oxide.

[0054] As the photocationic polymerization initiator, an onium salt that releases a Lewis acid when irradiated with active energy rays may be used. Examples of such onium salts include aromatic sulfonium salts of Group VIIa elements, aromatic onium salts of Group VIa elements, and aromatic onium salts of Group Va elements. Specific examples include triarylsulfonium hexafluoroantimonate, triphenylphenacylphosphonium tetrafluoroborate, triphenylsulfonium hexafluoroantimonate, bis-[4-(diphenylsulfonio)phenyl]sulfide bisdihexafluoroantimonate, bis-[4-(di-4'-hydroxyethoxyphenylsulfonio)phenyl]sulfide bisdihexafluoroantimonate, bis-[4-(diphenylsulfonio)phenyl]sulfide bisdihexafluorophosphate, and diphenyliodonium tetrafluoroborate.

[0055] From the viewpoint of achieving both photosensitivity and internal photocurability, the content of the photopolymerization initiator in the photosensitive resin composition may be 2.0 to 15.0 parts by mass, 3.0 to 12.0 parts by mass, or 4.0 to 10.0 parts by mass relative to 100 parts by mass of the total amount of the alkali-soluble binder polymer and the photopolymerizable monomer.

[0056] (Liquid repellent) The photosensitive resin composition of the present disclosure contains, as a liquid repellent, (D-1) a fluorine-containing compound having a photocurable group and a weight average molecular weight of 2000 or more. The (D-1) component may be an oligomer. The weight average molecular weight of the (D-1) component means a converted value based on a calibration curve of standard polystyrene measured by gel permeation chromatography (GPC). Specifically, the measurement is performed under the following measurement conditions, and the weight average molecular weight can be calculated from the following calibration curve. [Measurement conditions] Measuring device: "HLC-8320GPC" manufactured by Tosoh Corporation Column: "Gelpack GL-A150-S / GL-A160-S" manufactured by Resonac Co., Ltd. Eluent: Tetrahydrofuran Flow rate: 1mL / min Column temperature: 40℃ [Calibration curve] A set of five standard polystyrene samples (PStQuick MP-H and PStQuick B, manufactured by Tosoh Corporation) is used to approximate the universal calibration curve with a cubic equation in accordance with JIS K 7252-2 (2016).

[0057] The weight-average molecular weight of the (D-1) component is 2000 or more, but may be 3000 or more. In particular, when the (D-1) component is an oligomer, if the weight-average molecular weight is within the above range, the fluorine content in one molecule is large, and high liquid repellency can be exhibited. In addition, the weight-average molecular weight of the (D-1) component may be 6000 or less, or 5000 or less, from the viewpoint of viscosity at the time of addition.

[0058] Examples of the photocurable group contained in the (D-1) component include ultraviolet-curable groups such as acryloyl, methacryloyl, and vinyl groups. The (D-1) component may contain two or more, three or more, or four or more photocurable groups in one molecule. The number of photocurable groups in one molecule may be five or six or less. In this case, it is easy to control the residual film property and pattern width of the partition wall.

[0059] The component (D-1) may have a perfluoroalkyl group, a perfluoroether group, etc. When the component (D-1) is an oligomer, the repeating unit may have the above group.

[0060] The component (D-1) may have an alicyclic skeleton. From the viewpoint of photocurability, the number of ring members of the alicyclic skeleton may be 5 to 20, 5 to 18, 6 to 18, 6 to 14, or 6 to 12. From the same viewpoint, the number of rings of the alicyclic skeleton contained in the liquid repellent agent may be 2 or more, or may be 3 or more. In this case, the liquid repellency of the partition wall obtained by curing the photosensitive resin composition against ink can be further improved. The number of rings of the alicyclic skeleton contained in the liquid repellent agent may be 4 or less. Examples of the alicyclic skeleton having one ring include a cyclohexane skeleton and a cyclohexene skeleton, and examples of the alicyclic skeleton having two or more rings include a norbornane skeleton, a decalin skeleton, a bicycloundecane skeleton, and a saturated dicyclopentadiene skeleton.

[0061] The component (D-1) may be a commercially available product, such as "Megafac RS-72-A", "Megafac RS-78", and "Megafac RS-90" (all of which are product names manufactured by DIC Corporation), "DAC-100", and "DAC-HP" (all of which are product names manufactured by Daikin Industries, Ltd.).

[0062] The content of the (D-1) component is 1% by mass or more based on the total amount of the photosensitive resin composition, and from the viewpoint of further expressing liquid repellency, it may be 1.2% by mass or more or 1.5% by mass or more. Also, from the viewpoint of compatibility with other components, the content of the (D-1) component may be 10% by mass or less or 8% by mass or less based on the total amount of the photosensitive resin composition.

[0063] The content of the liquid repellent agent relative to the total amount of 100 parts by mass of the alkali-soluble binder polymer and the photopolymerizable monomer may be 0.05 to 10.0 parts by mass, 0.1 to 8.0 parts by mass, or 0.2 to 6.0 parts by mass. When the content of the liquid repellent agent is 0.05 to 10.0 parts by mass, it becomes easier to achieve both photosensitivity and internal photocurability.

[0064] The content ratio of the liquid repellent agent relative to 100 parts by mass of the total amount of the photopolymerizable monomer and the liquid repellent agent may be 1.0 parts by mass or more, 3.0 parts by mass or more, or 5.0 parts by mass or more. In this case, even if the exposure dose during exposure is low, the resolution of the partition wall can be effectively improved. The content ratio of the liquid repellent agent relative to 100 parts by mass of the total amount of the photopolymerizable monomer and the liquid repellent agent may be 60.0 parts by mass or less, 50.0 parts by mass or less, or 30.0 parts by mass or less. In this case, the resolution of the partition wall can be further improved and the spread of the pattern width can also be suppressed.

[0065] (Multifunctional thiol compounds) The photosensitive resin composition may further contain a polyfunctional thiol compound.

[0066] When the photosensitive resin layer obtained by exposing the photosensitive resin composition to light is heated, the polyfunctional thiol compound causes a radical chain reaction, and the reaction between the photopolymerizable monomers and between the photopolymerizable monomers and the mercapto group of the polyfunctional thiol compound proceeds moderately even after exposure, making it easier to harden the photosensitive resin layer. The polyfunctional thiol compound may contain two or more mercapto groups in one molecule, may contain three or more mercapto groups, or may contain four or more mercapto groups. When the polyfunctional thiol compound contains three or more mercapto groups in one molecule, the resolution of the partition wall can be further improved even if the exposure dose during exposure is low. The number of mercapto groups in one molecule may be six or less.

[0067] Examples of the polyfunctional thiol compound include primary polyfunctional thiols and secondary polyfunctional thiols. Among them, secondary polyfunctional thiols have high storage stability and can suppress odors.

[0068] Examples of secondary polyfunctional thiols include pentaerythritol tetrakis(3-mercaptobutyrate), trimethylolpropane tris(3-mercaptobutyrate), and 1,3,5-tris[2-(3-mercaptobutanoyloxy)ethyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione.

[0069] Examples of primary polyfunctional thiols include trimethylolpropane tris(3-mercaptopropionate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, pentaerythritol tetrakis(3-mercaptopropionate), and dipentaerythritol hexakis(3-mercaptopropionate).

[0070] The polyfunctional thiol compounds can be used alone or in combination of two or more.

[0071] The content of the polyfunctional thiol compound may be 0.05 to 10.0 parts by mass, 0.1 to 8.0 parts by mass, or 0.2 to 6.0 parts by mass, relative to 100 parts by mass of the total amount of the alkali-soluble binder polymer and the photopolymerizable monomer. When the content of the polyfunctional thiol compound is 0.05 to 10.0 parts by mass, it becomes easier to achieve both photosensitivity and internal photocurability.

[0072] The content of the polyfunctional thiol compound may be 1.0 parts by mass or more, 3.0 parts by mass or more, or 5.0 parts by mass or more, based on 100 parts by mass of the total amount of the photopolymerizable monomer and the polyfunctional thiol compound. In this case, even if the exposure dose during exposure is low, the resolution of the partition wall can be effectively improved. The content of the polyfunctional thiol compound may be 60.0 parts by mass or less, 50.0 parts by mass or less, or 30.0 parts by mass or less, based on 100 parts by mass of the total amount of the photopolymerizable monomer and the polyfunctional thiol compound. In this case, the resolution of the partition wall can be further improved, and the spread of the pattern width can also be suppressed.

[0073] (Coloring agent) The photosensitive resin composition may further contain a colorant, in which case the formed partition wall can function as a light-shielding pattern.

[0074] Examples of the colorant include pigments and dyes. The pigment may be either an organic pigment or an inorganic pigment, but may be an organic pigment. When the pigment is an organic pigment, the organic pigment can transmit ultraviolet light, so that light can reach a sufficiently deep position from the surface of the photosensitive resin layer during exposure, compared to when an inorganic pigment is used, and insufficient curing of the exposed part can be further suppressed. Therefore, dissolution or swelling of the cured part due to exposure during development can be further suppressed, and the resolution of the partition wall can be further improved. The colorant may contain two or more types.

[0075] Examples of organic pigments include lactam black, perylene black, and aniline black.

[0076] Examples of inorganic pigments include carbon black and titanium black.

[0077] The dyes include leuco dyes.

[0078] The content of the colorant in the total solid content may be 4% by mass or more, or 6% by mass or more, from the viewpoint of improving the light-shielding property of the partition wall to be formed. However, the content of the colorant in the total solid content may be 15% by mass or less, 12% by mass or less, or 4% by mass or less. When the content of the colorant in the total solid content is 15% by mass or less, the depth of light reaching from the surface can be increased during exposure of the photosensitive resin layer formed using the photosensitive resin composition, and insufficient curing of the exposed portion can be suppressed. Therefore, dissolution or swelling of the cured portion due to exposure during development with a developer is sufficiently suppressed.

[0079] (Other Ingredients) The photosensitive resin composition may further contain a solvent such as methanol, ethanol, acetone, methyl ethyl ketone, methyl cellosolve, ethyl cellosolve, toluene, N,N-dimethylformamide, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, etc., as necessary. These may be used alone or in combination of two or more. The amount of the solvent may be appropriately determined so that the total solid content concentration in the photosensitive resin composition is, for example, about 10 to 60 mass%.

[0080] The photosensitive resin composition may further contain additives such as plasticizers, fillers, defoamers, flame retardants, stabilizers, adhesion promoters, leveling agents, peeling promoters, antioxidants, fragrances, and thermal crosslinking agents, as necessary. Each of these may be used alone or in combination of two or more. The amount of each of these additives may be 0.01 to 20 parts by mass per 100 parts by mass of the total of the alkali-soluble binder polymer and the photopolymerizable monomer.

[0081] <Substrate with partition walls and its manufacturing method> The method for producing a substrate with partition walls of the present disclosure includes a photosensitive resin layer forming step of forming a photosensitive resin layer on a substrate using the photosensitive resin composition of the present disclosure, an exposure step of exposing the photosensitive resin layer provided on the substrate to light in a predetermined pattern, and a development step of forming partition walls by alkaline development of the exposed photosensitive resin layer. The substrate with partition walls of the present disclosure includes a substrate and partition walls provided on the substrate, and the partition walls are made of a cured product of the photosensitive resin composition of the present disclosure.

[0082] Hereinafter, an embodiment of a method for producing a substrate with partition walls according to one aspect of the present disclosure will be described with reference to Fig. 1 to Fig. 5. Fig. 1, Fig. 2, and Fig. 4 are schematic cross-sectional views showing a series of steps in the method for producing a substrate with partition walls, Fig. 3 is a partial cross-sectional view showing a second laminate obtained in the exposure step of Fig. 2, and Fig. 5 is a plan view showing the substrate with partition walls in Fig. 4.

[0083] The method for manufacturing a substrate with partition walls in this embodiment includes a photosensitive resin layer formation step (see FIG. 1) of forming a photosensitive resin layer 20 on a substrate 10 using the above-mentioned photosensitive resin composition to obtain a first laminate 100, an exposure step (see FIGS. 2 and 3) of exposing the photosensitive resin layer 20 provided on the substrate 10 in a predetermined pattern (partially irradiating the photosensitive resin layer 2 with light L) to form a partially cured layer 30 and obtain a second laminate 110, and a development step (see FIG. 4) of alkaline-developing the partially cured layer 30 of the second laminate 110 (removing the uncured portions 22) and, if necessary, performing a post-curing step to form partition walls 21 to obtain a substrate with partition walls 120.

[0084] (Photosensitive resin layer formation process) Examples of the substrate 10 in the photosensitive resin layer forming step include glass substrates, sapphire substrates, plastic substrates such as polycarbonate and cycloolefin polymer, and circuit substrates such as TFT or CMOS.

[0085] The height of the photosensitive resin layer 20 from the substrate 10 varies depending on the application, but from the viewpoint of achieving both coatability and photocurability, the thickness after drying may be 1 to 200 μm, or 10 to 100 μm.

[0086] The photosensitive resin layer 20 can be formed by applying a solution of the above-mentioned photosensitive resin composition (coating liquid for forming a photosensitive resin layer) onto the substrate 10 and drying it. In this case, however, the amount of the organic solvent remaining in the photosensitive resin layer 20 may be 2 mass % or less in order to prevent the organic solvent from diffusing in a later step.

[0087] Coating can be performed by a known method such as roll coating, comma coating, gravure coating, air knife coating, die coating, bar coating, spray coating, spin coating, etc. After coating, drying to remove the organic solvent and the like can be performed at 70 to 150° C. for about 1 to 30 minutes using a hot air convection dryer or the like.

[0088] (Exposure process) The exposure method in the exposure step includes a method (mask exposure method) in which light (active light rays) are irradiated imagewise through a mask M having a plurality of openings in order to irradiate a predetermined portion of the photosensitive resin layer 20 with light (active light rays) (see FIG. 2). As a light source of the active light rays, known light sources, for example, carbon arc lamps, mercury vapor arc lamps, ultra-high pressure mercury lamps, high pressure mercury lamps, xenon lamps, and other light sources that effectively radiate ultraviolet light, visible light, and the like, can be used. In addition, Ar ion lasers, semiconductor lasers, and other light sources that effectively radiate ultraviolet light, visible light, and the like can also be used. Furthermore, photographic flood lamps, sun lamps, and other light sources that effectively radiate visible light can also be used. A method of irradiating active light rays imagewise by a direct drawing method using a laser exposure method or the like may also be adopted. In this case, the mask M is not necessary.

[0089] The amount of exposure in the exposure step varies depending on the apparatus used and the composition of the photosensitive resin layer 20, but from the viewpoint of excellent photocuring properties, a value of 30 mJ / cm 2 or more than 50 mJ / cm 2 The exposure amount in the exposure step is preferably 500 mJ / cm or more in terms of resolution. 2 or less than 400mJ / cm 2 It may be the following:

[0090] The exposure can be carried out in air, in vacuum, or the like, and the atmosphere for the exposure is not particularly limited.

[0091] After exposure, the photosensitive resin layer 20 becomes a partially cured layer 30. Specifically, the exposed parts of the photosensitive resin layer 20 become cured parts serving as partition walls 21, and the unexposed parts of the photosensitive resin layer 20 become non-cured parts 22 (see FIG. 3).

[0092] (Development process) The alkaline development in the development step is carried out by a known method such as spraying, shaking immersion, brushing, scrubbing, etc., using a developer such as an alkaline aqueous solution.

[0093] The developer may be any solution capable of dissolving an alkali-soluble binder polymer, and may be, for example, an alkaline aqueous solution that is safe, stable, and easy to handle. Examples of the base in the alkaline aqueous solution include alkali hydroxides such as hydroxides of lithium, sodium, potassium, or ammonium, alkali carbonates such as carbonates or bicarbonates of lithium, sodium, potassium, or ammonium, alkali metal phosphates such as potassium phosphate and sodium phosphate, and alkali metal pyrophosphates such as sodium pyrophosphate and potassium pyrophosphate.

[0094] The alkaline aqueous solution used for development may be a 0.1 to 5 mass% aqueous solution of tetraammonium hydroxide, a 0.1 to 5 mass% aqueous solution of sodium carbonate, a 0.1 to 5 mass% aqueous solution of potassium carbonate, a 0.1 to 5 mass% aqueous solution of sodium hydroxide, a 0.1 to 5 mass% aqueous solution of sodium tetraborate, or the like. The pH of the alkaline aqueous solution used for development may be in the range of 9 to 11, and the temperature is adjusted according to the developability of the photosensitive resin layer 20. The alkaline aqueous solution may contain a surfactant, an antifoaming agent, a small amount of an organic solvent for promoting development, or the like.

[0095] Also, an aqueous developer consisting of an alkaline aqueous solution and one or more organic solvents can be used. Here, examples of the base contained in the alkaline aqueous solution include, in addition to the above-mentioned bases, borax, sodium metasilicate, ethanolamine, ethylenediamine, diethylenetriamine, 2-amino-2-hydroxymethyl-1,3-propanediol, 1,3-diaminopropanol-2, and morpholine. Examples of the organic solvent include diacetone alcohol, acetone, ethyl acetate, alkoxyethanol having an alkoxy group with 1 to 4 carbon atoms, ethyl alcohol, isopropyl alcohol, butyl alcohol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether. These can be used alone or in combination of two or more.

[0096] The above-mentioned developers may be used in combination of two or more kinds, if necessary.

[0097] Examples of the developing method include a dipping method, a paddle method, a spray method, brushing, scrubbing, etc. Among these, when the high pressure spray method is used, the resolution of the partition walls is improved.

[0098] The development time is not particularly limited, and may be, for example, 3 seconds or more, or 5 seconds or more. When the development time is 5 seconds or more, overdevelopment is unlikely to occur, and manufacturing variations in the line width and thickness of the partition wall are reduced. The development time may be 300 seconds or less, or 200 seconds or less.

[0099] Fig. 5 is a plan view showing the partition-attached substrate 120 obtained by the development process. As shown in Fig. 5, the partition 21 has a plurality of openings (through holes). S in Fig. 5 represents the width of the opening, i.e., the space width, and L represents the line width of the partition 21.

[0100] (Post-curing process) The post-curing step is a step of curing the cured portion after development. The exposure method in the post-curing step includes a method of irradiating the cured portion with light (actinic rays). The light source of the actinic rays can be the same as the light source used in the exposure step.

[0101] The exposure dose in the post-curing step varies depending on the equipment used and the composition of the curing part, but in terms of excellent photocuring properties, 100 mJ / cm 2 or more than 300mJ / cm 2 The exposure dose in the post-curing step may be 10,000 mJ / cm or more. 2 or less than 5000mJ / cm 2 It may be the following:

[0102] The post-curing step can be carried out in air, in vacuum, or the like, and the atmosphere for the post-curing step is not particularly limited.

[0103] When the post-curing step is carried out, the hardened portion which is further hardened by the post-curing step finally becomes the partition wall 21.

[0104] In the manufacturing method of the partition-formed substrate of this embodiment, when the photosensitive resin composition contains a polyfunctional thiol compound, a heating step of heating the partially cured layer 30 of the second laminate 110 may be further provided between the exposure step and the development step.

[0105] In the heating step, the partially cured layer 30 is heated, so that the curing reaction between the photopolymerizable monomers or between the photopolymerizable monomer and the mercapto group of the polyfunctional thiol compound can be appropriately promoted in the portion of the partition wall 21 on the substrate 10 side. By heating the partially cured layer 30, the polyfunctional thiol compound undergoes a radical chain reaction, so that the reaction between the photopolymerizable monomers and between the photopolymerizable monomer and the mercapto group of the polyfunctional thiol compound can be appropriately promoted and cured even after exposure.

[0106] When the partially cured layer 30 is heated in the heating step, a hot plate, a box-type dryer, a reflow furnace, a clean oven, or the like can be used as a heating means.

[0107] In the heating step, the temperature may be from 70 to 150° C., or from 85 to 130° C. The heating time may be from 1 to 30 minutes, or from 2 to 20 minutes.

[0108] The substrate with partition walls according to the present disclosure can be used as a substrate for forming a color conversion device. The substrate for forming a color conversion device may be for a micro LED element. According to the manufacturing method of the substrate with partition walls described above, the partition walls that divide the light of the micro LED element can be formed with high precision, and a substrate with partition walls having excellent ink repellency can be obtained. As a result, when the quantum dot ink is applied to the recessed portion that is the formation region of the color conversion part by the inkjet method, the contact angle between the ink and the partition walls can be increased, and the ink can be prevented from overflowing along the partition walls.

[0109] <Manufacturing method of color conversion device> The method for manufacturing a color conversion device disclosed herein is a method for manufacturing a color conversion device having a color conversion section surrounded by a partition, and includes a coating process of preparing a substrate with a partition as disclosed herein, in which a recess is formed by the partition to serve as a formation area for the color conversion section, and coating a quantum dot ink into the recess by an inkjet method.

[0110] The partition wall may be provided so that a plurality of recesses serving as formation regions of the color conversion portion are arranged, or may be provided so that the recesses are arranged in a matrix.

[0111] The height of the partition wall may be 1 to 100 μm, 10 to 50 μm, or 15 to 25 μm from the viewpoints of ease of entry of droplets and good pattern shape, and the width of the partition wall may be 10 to 500 μm, 50 to 250 μm, or 75 to 150 μm from the viewpoints of ease of entry of droplets and good pattern shape.

[0112] The opening area of ​​the recess is set to 100 to 100,000 μm from the viewpoints of ease of entry of droplets and good pattern shape. 2 , 800~10,000μm 2 , or 1000~3000μm 2 may be also possible.

[0113] Opening area A of the recess (μm 2 The relationship (A / H) between the diameter of the particle and the height H (μm) of the partition wall may be 1 to 100,000, 10 to 10,000, or 100 to 1,000.

[0114] When the color conversion device forming substrate is used for producing a color conversion device for a micro LED element, the height of the partition may be 0.1 to 100 μm, and the opening area of ​​the recess may be 0.5 to 50 μm. 2 may be also possible.

[0115] The partition wall may have light transmitting property or light blocking property. The partition wall having light blocking property may contain, for example, the above-mentioned coloring agent and may function as a black matrix.

[0116] The light-transmitting barrier rib can transmit light from the light emitter as it is to be used as display light. The light-transmitting barrier rib may have a total light transmittance (Tt) of 85% or more, 90% or more, or 91% or more as measured in accordance with ASTM D1003-21. The haze value of the light-transmitting barrier rib may be 1% or less, 0.5% or less, or 0.3% or less as measured in accordance with ASTM D1003-21.

[0117] The light-transmitting partition walls may have a yellowness index (YI) of 3 or less, 0.2 to 2, or 0.5 to 1.5, as measured in accordance with ASTM E313-05 (D65).

[0118] Fig. 6 is a partial cross-sectional view showing a coating step of an embodiment of a manufacturing method for a color conversion device according to the present disclosure. Fig. 6 shows a coating step in which quantum dot inks 31a and 32a are applied by an inkjet method to a recess formed by a partition wall 21. This embodiment may also include a curing step in which the coating film of the quantum dot ink in the recess is cured to form a quantum dot-containing layer. The quantum dot-containing layer can function as a color conversion layer by wavelength conversion.

[0119] The quantum dot ink may contain quantum dots, a binder resin, and a solvent.

[0120] Examples of quantum dots include semiconductor crystals containing II-VI group semiconductor compounds such as MgS, MgSe, MgTe, CaS, CaSe, CaTe, SrS, SrSe, SrTe, BaS, BaSe, BaTe, ZnS, ZnSe, ZnTe, CdS, CdSe, CdTe, HgS, HgSe and HgTe, IIIV group semiconductor compounds such as AlN, AlP, AlAs, AlSb, GaAs, GaP, GaN, GaSb, InN, InAs, InP, InSb, TiN, TiP, TiAs and TiSb, IV group semiconductors such as Si, Ge and Pb, and semiconductor compounds containing three or more elements such as InGaP. Quantum dots can also be obtained by adding Eu to the above semiconductor compounds.3+ , Tb 3+ , Ag + , Cu + The semiconductor crystal may be doped with a cation of a rare earth metal or a cation of a transition metal such as ZnO.

[0121] The quantum dots may be made of one type of semiconductor compound, or may be made of two or more types of semiconductor compounds.

[0122] The size of the quantum dot can be appropriately adjusted depending on the material that constitutes the quantum dot so that light of a desired wavelength can be obtained. For example, known quantum dots such as quantum dots having a central emission wavelength in a wavelength band of 600 nm to 680 nm for emitting red light, quantum dots having a central emission wavelength in a wavelength band of 500 nm to 600 nm for emitting green light, and quantum dots having a central emission wavelength in a wavelength band of 400 nm to 500 nm for emitting blue light can be used.

[0123] The binder resin may be any resin capable of forming a quantum dot-containing layer in which quantum dots are dispersed, and may be a known heat- and / or light-curable resin. The binder resin may be a combination of a polymerizable compound and a polymerization initiator. The polymerizable compound may be a (meth)acrylic monomer, a vinyl monomer, a maleimide, or the like. The (meth)acrylic monomer may have two or more (meth)acryloyl groups, or may have a (meth)acryloyl group and a functional group such as a glycidyl group, a benzyl group, a phenyl group, a hydroxyl group, or a carboxyl group.

[0124] As the solvent, known organic solvents can be used. Examples of the organic solvent include cyclohexane and toluene. These may be used alone or in combination of two or more, taking into consideration the dispersibility of the quantum dots and the ejection stability in the inkjet method.

[0125] The quantum dot ink may contain various additives, such as an antioxidant, a polymerization terminator, a chain transfer agent, a leveling agent, a plasticizer, a surfactant, an antifoaming agent, a silane coupling agent, an ultraviolet absorber, and an adhesion promoter, as necessary.

[0126] The quantum dot ink may be the ink disclosed in U.S. Patent Application Publication No. 2017 / 0174921, U.S. Patent Application Publication No. 2015 / 0021531, and U.S. Patent Application Publication No. 2015 / 0075397.

[0127] In the application step, the quantum dot ink can be applied to the recesses of the color conversion device formation substrate by ejecting the quantum dot ink using an inkjet printer.

[0128] In FIG. 6, two types of quantum dot inks 31a, 32a are ejected from two inkjet nozzles 41, 42, but the number of nozzles, the type of quantum dot ink, etc. can be changed as appropriate depending on the type and arrangement pattern of the color conversion section to be formed.

[0129] In the curing step, the coating film of the quantum dot ink in the recesses can be cured by heating, light irradiation, drying, or a combination of these depending on the composition of the quantum dot ink, to form a quantum dot-containing layer.

[0130] Through the application and curing steps, a color conversion device 130 can be obtained, which includes the substrate 10, the partition wall 21, and the color conversion portions 31b and 32b including the quantum dot-containing layer formed in the recess, as shown in Fig. 7. Fig. 8 is a plan view showing the color conversion device of Fig. 7.

[0131] In addition, color conversion device 130 is provided with color conversion section 31b that converts blue LED light to red, color conversion section 32b that converts blue LED light to green, and an area that transmits blue LED light, but the configuration of the color conversion section may be changed as appropriate depending on the application.

[0132] 7 shows an embodiment in which only the quantum dot-containing layer is formed as the color conversion part, but the color conversion part may be composed of multiple layers. The color conversion part may be composed of two layers, for example, a quantum dot-containing layer and a color filter layer. In this case, the quantum dot-containing layer and the color filter layer can be formed in this order or in the reverse order in the recess.

[0133] <Image display device> The image display device of the present disclosure includes the partition-formed substrate of the present disclosure.

[0134] The image display device may include a light emitting device having a micro LED element, and a color conversion device according to the present disclosure disposed opposite the light emitting device.

[0135] Fig. 9 is a partial cross-sectional view showing an image display device according to the present disclosure. The image display device 200 shown in Fig. 9 includes a light-emitting device 60 having a substrate 50 for mounting LEDs and a plurality of micro LED elements 51 provided on the substrate 50 for mounting LEDs, and a color conversion device 130 in which the color conversion units 31b and 32b are arranged to correspond to the arrangement of the micro LED elements 51 of the light-emitting device 60. In the image display device 200, the substrate 10 side of the color conversion device 130 is opposed to the micro LED elements 51 side of the light-emitting device 60, and a second substrate 40 is provided on the side opposite the substrate 10 of the color conversion device 130, but the side opposite the substrate 10 of the color conversion device 130 may be opposed to the micro LED elements 51 side of the light-emitting device 60.

[0136] A micro LED element refers to a tiny LED (semiconductor light-emitting diode) element, and examples of such elements include LED elements that use gallium nitride, indium gallium nitride, silicon, etc.

[0137] The shape of the micro LED element is not particularly limited, and examples thereof include shapes in which the shape of the main surface is a square, a rectangle, a rhombus, a trapezoid, a polygon, and a shape having a curved surface such as a circle, an ellipse, and an arc. The micro LED element may also have a shape with projections and recesses in the thickness direction. The size of the micro LED element may be, for example, when the shape of the main surface is a square, the length of one side is 0.1 to 2000 μm, and when the shape of the main surface is a rectangle, the length of the long side is 0.2 μm to 2000 μm and the length of the short side is 0.1 to 1500 μm. The thickness of the micro LED element is, for example, 0.1 to 20 μm.

[0138] In the image display device 200, a micro LED element that emits blue light may be used as the micro LED element 51, the color conversion unit 31b and the color conversion unit 32b may be a color conversion unit that converts blue light into red light and a color conversion unit that converts blue light into green light, and the light emitting region may be partitioned by the partition wall 21. As shown in Fig. 9, such an image display device 200 can emit red light L1, green light L2, and blue light L3 as display light in respective predetermined regions.

[0139] The color conversion device and display device of the present embodiment are not limited to those described above, and various modifications are possible. EXAMPLES

[0140] The present disclosure will be described more specifically below with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.

[0141] <Preparation of Alkali-Soluble Binder Polymer Solution> Alkali-soluble binder polymer solutions (hereinafter sometimes simply referred to as "polymer solutions") 1 and 2 were prepared as follows. The constituent units 1 to 7 of the alkali-soluble binder polymer (hereinafter sometimes simply referred to as "polymer") are as follows. Here, the constituent unit 1 is included in the constituent unit (a), the constituent units 2 and 5 are included in the constituent unit (b), the constituent unit 3 is included in the constituent unit (c), the constituent units 4 and 6 are included in the constituent unit (d), and the constituent unit 7 is included in the constituent unit (e). [ka] [ka]

[0142] (Binder polymer solution 1 To a flask equipped with a stirrer, a dropping funnel, a condenser, a thermometer, and a gas inlet tube, 180.1 g of propylene glycol monomethyl ether (PGME) was added as a solvent, and the mixture was stirred while replacing the gas in the flask with nitrogen gas and heated to 120°C. Next, a monomer mixture consisting of 39.6 g (0.18 mol) of tricyclodecanyl methacrylate, 3.52 g (0.02 mol) of benzyl methacrylate, and 68.8 g (0.80 mol) of methacrylic acid was prepared by adding 5.93 g of t-butylperoxy-2-ethylhexanoate (polymerization initiator, manufactured by NOF Corporation, Perbutyl (registered trademark) O). This mixture of monomers and polymerization initiator was dropped into the flask from the dropping funnel over 1 hour. After the dropping was completed, the liquid in the flask was stirred for another 2 hours at 120 ° C to carry out a copolymerization reaction, and a precursor solution of polymer 1 was synthesized. Thereafter, the gas in the flask was replaced with air, and 88.1 g (0.62 mol) of glycidyl methacrylate, 0.6 g of triphenylphosphine (catalyst), and 0.6 g of methylhydroquinone (polymerization inhibitor) were added to the precursor solution of polymer 1. Then, the reaction was continued at 110 ° C for 10 hours to obtain a resin solution. The weight average molecular weight of polymer 1 contained in this resin solution was 13,100, the double bond equivalent was 340 g / mol, and the glass transition temperature (Tg) was 59° C. The proportions of the structural units 1 to 7 in polymer 1 were as shown in Table 1, with the total of all structural units 1 to 7 being taken as the standard (100 mol%). PGME was further added to this resin solution to prepare polymer solution 1 (solid concentration: 49.1% by mass). At this time, polymer solution 1 was prepared so that polymer 1 and PGME were mixed in a mass ratio of 78.4:81.3. The solid content means the heating residue when the polymer solution is heated at 130° C. for 2 hours, and the main component of the solid content is polymer 1. The resin acid value of this polymer solution 1 was 28.9 KOHmg / g, and the solid content acid value of the solid content contained in polymer solution 1 was 58.9 KOHmg / g.

[0143] (Binder polymer solution 2) To a flask equipped with a stirrer, a dropping funnel, a condenser, a thermometer, and a gas inlet tube, 167.1 g of PGMEA was added as a solvent, and the mixture was heated to 120°C with stirring while replacing the gas in the flask with nitrogen gas. Next, a monomer mixture consisting of 66.0g (0.30 mol) of tricyclodecanyl methacrylate, 10.4g (0.10 mol) of styrene, and 85.2g (0.60 mol) of glycidyl methacrylate was prepared by adding 10.3g of t-butylperoxy-2-ethylhexanoate (polymerization initiator, manufactured by NOF Corporation, Perbutyl (registered trademark) O). This mixture of monomers and polymerization initiator was dropped into the flask from the dropping funnel over 1 hour. After the dropping was completed, the liquid in the flask was stirred at 120°C for another 2 hours to carry out a copolymerization reaction, and a binder polymer precursor was generated. Thereafter, the gas in the flask was replaced with air, and 43.2g (0.60 mol) of acrylic acid, 0.61g of triphenylphosphine (catalyst), and 0.31g of methylhydroquinone (polymerization inhibitor) were added to the above binder polymer precursor solution. Then, the reaction was continued at 110°C for 10 hours. Next, 33.0 g (0.33 mol) of succinic anhydride was added to the flask, and the reaction was continued for 3 hours at 110° C. to obtain a resin solution. The binder polymer contained in this resin solution had a weight average molecular weight of 8700, a double bond equivalent of 440 g / mol, and a glass transition temperature (Tg) of 48° C. The proportions of each of the structural units 1 to 7 in polymer 2 were as shown in Table 1, assuming the total of all structural units 1 to 7 as the standard (100 mol%). PGMEA was further added to this resin solution to prepare polymer solution 2 (solid concentration 57.6 mass%). At this time, polymer solution 2 was prepared so that polymer 2 and PGMEA were mixed in a mass ratio of 78.4:57.7. The resin acid value of this polymer solution 2 was 44.4 KOHmg / g, and the solid acid value of the solid content contained in polymer solution 2 was 77.1 KOHmg / g.

[0144] <Method of measuring physical properties> The above resin acid value, solid content acid value, double bond equivalent, weight average molecular weight and glass transition temperature are values ​​obtained by the methods described below. (1) Resin acid value The resin acid value is the acid value of the polymer solution measured using a mixed indicator of bromothymol blue and phenol red according to JIS K6901 5.3.2. The resin acid value means the number of milligrams of potassium hydroxide required to neutralize the acidic components contained in 1 g of the polymer solution. (2) Acid value of solid content The solid content acid value is a value calculated by the following formula. Solid acid value = 100 × resin acid value / (solid concentration of polymer solution (mass%)) (3) Double bond equivalent The double bond equivalent is the mass of a polymer per mole of a polymerizable unsaturated bond, and is a calculated value calculated based on the amount of monomer used. (4) Weight average molecular weight (Mw) The weight average molecular weight means a weight average molecular weight measured by gel permeation chromatography (GPC) under the following conditions and converted into standard polystyrene. Column: Showdex (registered trademark) LF-804 + LF-804 (manufactured by Showa Denko K.K.) Column temperature: 40℃ Sample: 0.2% solution of copolymer in tetrahydrofuran Developing solvent: Tetrahydrofuran Detector: Differential refractometer (Shodex (registered trademark) RI-71S) (manufactured by Showa Denko K.K.) Flow rate: 1mL / min (5) Glass transition temperature (Tg) The Tg of the polymer was measured using a differential scanning calorimeter (DSC7000X, manufactured by Hitachi High-Tech Science Corporation). Specifically, 1 g of each polymer solution was collected, dried at 130°C for 120 minutes to volatilize the solvent, and 10 mg of each sample was collected from each solid obtained. Then, differential scanning calorimetry was performed by changing the temperature of the sample from -0°C to 200°C at a heating rate of 10°C / min using a differential scanning calorimeter (DSC), and the endothermic start temperature due to the observed glass transition was taken as the glass transition temperature (Tg). When two Tgs were observed, the average value of the two Tgs was taken as the Tg of the polymer.

[0145] [Table 1]

[0146] <Preparing the liquid repellent> The following liquid repellents were prepared: Water repellent 1: Megafac RS-72-A (manufactured by DIC Corporation, trade name), weight average molecular weight: 5,405 Water repellent 2: DAC-100 (trade name, manufactured by Daikin Industries, Ltd.), weight average molecular weight: 3,812 Water repellent 3: Viscoat 13F (trade name, manufactured by Osaka Organic Industry Co., Ltd.), molecular weight: 418 Water repellent 4: Pentafluorobenzyl methacrylate (Tokyo Chemical Industry Co., Ltd.) Molecular weight: 266 Water repellent 5: Octafluorohexanediol diacrylate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Molecular weight: 370 Water repellent 6: Pentafluorotoluene (Tokyo Chemical Industry Co., Ltd.) Molecular weight: 182 Water repellent 7: Heptafluorocyclopentene (Tokyo Chemical Industry Co., Ltd.) Molecular weight: 264

[0147] <Method of measuring physical properties> The weight average molecular weight is a value obtained by the method described below. (6) Weight average molecular weight The weight average molecular weight of the liquid repellent agent means a converted value based on a calibration curve of standard polystyrene, measured by gel permeation chromatography (GPC) under the following conditions. [Measurement conditions] Measuring device: "HLC-8320GPC" manufactured by Tosoh Corporation Column: "Gelpack GL-A150-S / GL-A160-S" manufactured by Resonac Co., Ltd. Eluent: Tetrahydrofuran Flow rate: 1mL / min Column temperature: 40℃ [Calibration curve] A set of five standard polystyrene samples (PStQuick MP-H and PStQuick B, manufactured by Tosoh Corporation) was used to approximate the universal calibration curve with a cubic equation in accordance with JIS K 7252-2 (2016).

[0148] <Examples 1 to 4 and Comparative Examples 1 to 10> [Preparation of photosensitive resin composition] The components (A), (B), (C), (D) and other components shown in Table 2 or Table 3 were blended to obtain the contents (unit: mass%) shown in the same table, and mixed for 15 minutes using a stirrer to prepare a coating liquid for forming a photosensitive resin layer as a photosensitive resin composition.

[0149] [Table 2]

[0150] [Table 3]

[0151] In Table 2 or Table 3, details of the component (A), the component (B), the component (C), the component (D), and other components are as follows: Component (A) Solutions 1-2: Polymer solutions 1-2 prepared by the above-mentioned method

[0152] (B) Component Photopolymerizable monomer: Pentaerythritol tri- and tetraacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., product name "A-TMM-3")

[0153] (C) Component Photopolymerization initiator: 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (product name: "Lunacure TPO", manufactured by DKSH Japan Co., Ltd.)

[0154] (D) Component Liquid repellent agents 1 to 7: Liquid repellent agents 1 to 7 prepared above

[0155] Other Ingredients Multifunctional thiol compound: pentaerythritol tetrakis(3-mercaptobutyrate) (KarenzMT (registered trademark) PE1 (number of SH groups = 4), manufactured by Resonac Co., Ltd.) Colorant: A mixture of lactam black (solid content) represented by the following structural formula as a pigment, a non-amine-based dispersant (solid content) as a dispersant, and PGMEA in a ratio of 15.0:4.5:80.5 (mass ratio) (lactam black organic pigment dispersion (product name "SF BLACK BJ4379", Sanyo Pigment Co., Ltd., solid content: 19.5 mass%, lactam black organic pigment: 15 mass%)) Adhesion aid: Si coupling agent (product name "KBM-803", manufactured by Shin-Etsu Chemical Co., Ltd.)

[0156] [Preparation of evaluation samples] The photosensitive resin layer forming coating solution obtained as described above was dropped onto a glass plate having a thickness of 3.0 mm, and a coating film was formed by spin coating to obtain a laminate having a coating film on the glass plate. Then, this laminate was placed on a hot plate and heated at 120°C for 2 minutes to remove the solvent, and a first laminate having a photosensitive resin layer was produced. When obtaining the first laminate, the thickness of the coating film was adjusted by adjusting the rotation speed in the spin coating method so that the thickness of the photosensitive resin layer was 20±1 μm. Next, the first laminate was exposed to ultraviolet light over the entire surface using an ultraviolet exposure machine (product name "MA-20", manufactured by Mikasa Co., Ltd.) to obtain a second laminate having a cured layer. At this time, the exposure dose was 355 mJ / cm 2 Next, the second laminate was placed on a hot plate and heated (post-baked) at 100°C for 1 minute. Next, the second laminate was exposed to ultraviolet light over its entire surface using an ultraviolet exposure machine (product name "MA-20", manufactured by Mikasa Co., Ltd.). At this time, the exposure dose was 1000 mJ / cm2. 2 It was decided. In this manner, an evaluation sample was prepared.

[0157] <Performance evaluation> The contact angle of the evaluation sample with respect to the liquids listed below was measured as described below, and the ink repellency was evaluated. Liquid 1: Quantum dot ink ((meth)acrylic monomer-based) Liquid 2: Propylene glycol monomethyl ether acetate (PGMEA)

[0158] <Contact angle measurement> The static contact angle was measured in accordance with ASTM D7334-08 (2013). The measurement was performed using "SA-301" (product name, manufactured by Kyowa Interface Science Co., Ltd.) at a measurement temperature of 25°C. The measurement was performed after placing a 2 μl droplet on the cured layer of the evaluation sample and waiting 5 seconds. [Explanation of symbols]

[0159] Reference Signs List 10: substrate, 20: photosensitive resin layer, 21: partition wall, 30: partially cured layer, 51: micro LED element, 60: light emitting device, 120: substrate with partition wall, 130: color conversion device, 200: image display device.

Claims

1. A photosensitive resin composition comprising an alkali-soluble binder polymer, a photopolymerizable monomer having an ethylenically unsaturated group, a photopolymerization initiator, and a liquid repellent agent, the liquid repellent agent contains a fluorine-containing compound having a photocurable group and a weight average molecular weight of 2000 or more, The content of the fluorine-containing compound is 1 mass % or more based on the total amount of the photosensitive resin composition.

2. The photosensitive resin composition according to claim 1 , wherein the fluorine-containing compound has an alicyclic skeleton.

3. 2. The photosensitive resin composition according to claim 1, wherein the alkali-soluble binder polymer has an acid value of 25 to 125 mg KOH / g.

4. 2. The photosensitive resin composition according to claim 1, wherein the photopolymerizable monomer has three or more functional groups in one molecule, and the three or more functional groups include an ethylenically unsaturated group and a hydroxyl group.

5. The photosensitive resin composition according to claim 1 , wherein the photopolymerization initiator comprises an acylphosphine oxide-based photopolymerization initiator.

6. A cured product obtained by curing the photosensitive resin composition according to any one of claims 1 to 5.

7. A substrate and a partition wall provided on the substrate, A substrate with partition walls, wherein the partition walls comprise the cured product according to claim 6.

8. An image display device comprising the partition-formed substrate according to claim 7 .

9. a photosensitive resin layer forming step of forming a photosensitive resin layer on a substrate using the photosensitive resin composition according to any one of claims 1 to 5; an exposure step of exposing the photosensitive resin layer provided on the base material to light in a predetermined pattern; a developing step of forming partition walls by alkali developing the photosensitive resin layer after exposure; A method for manufacturing a substrate with partition walls, comprising:

10. A method for manufacturing a color conversion device having a color conversion portion surrounded by a partition wall, comprising the steps of: A method for manufacturing a color conversion device, comprising: preparing a substrate with partition walls according to claim 7, in which a recess is provided by the partition walls to form an area for forming the color conversion section; and applying a quantum dot ink to the recess by an inkjet method.

Citation Information

Patent Citations

  • Light emitting device, lighting device, and display device

    JP2012142489A

  • Quantum dot ink

    US20170174921A1

  • Negative photosensitive resin composition, cured film, partition wall, black matrix, method for producing partition wall, method for producing black matrix, color filter, and organic el element

    WO2012147626A1