Method for reducing cellulose content in recovered fabric containing cellulose

By using ethylene glycol treatment and subsequent purification steps, the method effectively reduces cellulose content in recycled polyester fabrics to enhance chemical recycling efficiency and quality.

JP2024157609APending Publication Date: 2024-11-08TORAY INDUSTRIES INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023072048
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing chemical recycling methods for polyester fibers mixed with cotton fail to effectively remove cellulose and cotton-derived contaminants, leading to reduced quality and additional processing steps, and existing separation techniques have low accuracy and residual cellulose content.

Method used

Contacting recovered fabrics with ethylene glycol at specific temperatures and times to reduce cellulose content to 0.4% or less, followed by depolymerization and purification steps to obtain high-quality bis-2-hydroxyethyl terephthalate.

Benefits of technology

Achieves a cellulose content reduction to 0.4% or less, enabling high-quality chemical recycling of polyester fibers without additional processing steps and maintaining resin quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157609000001
    Figure 2024157609000001
  • Figure 2024157609000002
    Figure 2024157609000002
Patent Text Reader

Abstract

To provide a technique that sufficiently reduces the content of cotton fibers and cellulose powder in the recovered fabric, and enables the recycling into plastic materials with the same quality as before they were discarded, without the need for a special process to remove thermal decomposition impurities from cellulose in subsequent chemical recycling processes.SOLUTION: The present invention provides a method that brings a recovered fabric with a cellulose content of 0.5% or more and less than 5.0% into contact with an ethylene glycol at 150°C or more and 205°C or less for 5 minutes or more and 120 minutes or less, thereby reducing the cellulose content to the range of 0% or more and 0.4% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for reducing the cellulose content of cellulose-containing recycled fabrics. [Background technology]

[0002] Modern economic society has been maintained by a social system of mass production, mass consumption, and mass waste, but various adverse effects on the environment have been confirmed, such as the depletion of natural resources, destruction of nature due to resource extraction, global warming caused by greenhouse gas emissions, and rising sea levels. Therefore, in order to continue sustainable growth by efficiently using limited resources, it has become essential to build a recycling-oriented social system that minimizes waste generation and reuses and recycles generated waste in a way that does not burden the environment.

[0003] To realize a recycling-oriented society system, it is necessary to establish recycling systems such as thermal recycling, material recycling, and chemical recycling. In particular, attention is being paid to chemical recycling technology, which breaks down and refines waste plastics down to their raw monomer units, and then uses the resulting monomers to regenerate plastic materials of the same quality as before disposal.

[0004] Polyester fibers, which are inexpensive and have suitable physical properties for clothing, are also expected to be regenerated by chemical recycling, and the application of technologies to regenerate them down to the raw material monomer unit through hydrolysis or glycol decomposition has been considered. However, many of the waste clothing items collected as polyester clothing contain polyester and cotton blends, and when attempting to obtain raw material monomers from polyester fibers that contain cotton through hydrolysis or glycol decomposition, there is a major problem in that cellulose-derived pyrolysis foreign matter gets mixed in, making it impossible to regenerate them into polyester resin of the same quality as before disposal.

[0005] Therefore, Patent Document 1 proposes a technology in which, when polyester fibers containing cotton are glycol-decomposed, the cotton residue in the glycol decomposition product is subjected to solid-liquid separation to recover crude bis(2-hydroxyethyl) terephthalate (BHET), which is then reacted with methanol to convert it to dimethyl terephthalate, and distilled and purified to obtain a high-purity raw material monomer from which cellulose-derived thermal decomposition foreign matter has been removed.

[0006] Furthermore, Patent Documents 2 and 3 propose a technique in which recovered fabric containing cotton is treated with an organic acid aqueous solution or in an ozone environment to oxidize the cotton and turn it into cellulose powder, and then the cellulose powder is removed from the fabric by solid-solid separation that takes advantage of the difference in shape between the cellulose powder and synthetic fibers. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2002-060542 A [Patent Document 2] JP 2019-035022 A [Patent Document 3] Special Publication No. 2022-515368 Summary of the Invention [Problem to be solved by the invention]

[0008] In the method of Patent Document 1, a step of reacting BHET with methanol to convert it to dimethyl terephthalate is adopted in order to facilitate the removal of cellulose-derived pyrolysis foreign matter, and therefore the final raw material monomer is not BHET but dimethyl terephthalate. When producing polyethylene terephthalate (PET) from BHET, it is sufficient to carry out only the step of distilling off ethylene glycol (EG) by heating under reduced pressure, but when producing polyethylene terephthalate (PET) from dimethyl terephthalate, an additional reaction is required in which EG is added to dimethyl terephthalate, methanol is distilled off under heating at normal pressure, and the product is converted into BHET, which is significantly disadvantageous in terms of cost and energy consumption.

[0009] Patent Documents 2 and 3 disclose techniques for separating and removing cotton from recovered fabrics in advance to prevent contamination with cellulose-derived pyrolysis foreign matter during the chemical recycling process. However, these techniques involve oxidizing cotton to produce cellulose powder, and then performing solid-solid separation by utilizing the difference in shape between the cellulose powder and synthetic fibers, resulting in a problem that the separation accuracy is low and about 1% of cotton fibers and cellulose powder remain even after the separation process. If about 1% of cotton fibers and cellulose powder remain, this is undesirable because it becomes necessary to carry out some additional foreign matter removal process during the chemical recycling of synthetic fibers.

[0010] The object of the present invention is to provide a technology that solves the problems of the conventional technology described above, sufficiently reduces the content of cotton fiber and cellulose powder in recovered fabric, and enables the fabric to be recycled into plastic materials of the same quality as before disposal without the need for an additional process for removing cellulose-derived pyrolyzed foreign matter in the subsequent chemical recycling. [Means for solving the problem]

[0011] The above problem is solved by the method of the present invention, in which recovered fabric having a cellulose content in the range of 0.5% or more and less than 5.0% is contacted with ethylene glycol at 150°C or more and 205°C or less for 5 minutes or more and 120 minutes or less, thereby reducing the cellulose content to the range of 0% or more and 0.4% or less.

[0012] The weight average molecular weight of cellulose in the recovered fabric is preferably in the range of 7000 to 150000. When the recovered fabric contains cellulose in the range of 5% to 90%, it is preferable to carry out the above-mentioned method after subjecting the recovered fabric to a hydrolysis treatment to obtain a recovered fabric with a cellulose content of 0.5% to less than 5.0% and a cellulose weight average molecular weight in the range of 7000 to 150000.

[0013] It is also preferable that the recovered fabric contains 10.0% or more and 99.5% or less of polyester fibers.

[0014] Furthermore, the present invention provides a method for obtaining bis-2-hydroxyethyl terephthalate having a color tone b* value in the range of −5 or more and 5 or less, by subjecting the fabric obtained by the above method to the following steps (1) to (5). (1) A process of adding ethylene glycol to a fabric to depolymerize it, thereby obtaining an ethylene glycol solution containing bis-2-hydroxyethyl terephthalate. (2) A step of removing ethylene glycol from the ethylene glycol solution containing bis-2-hydroxyethyl terephthalate after depolymerization until the ethylene glycol is in the range of 0 mass % or more and 5 mass % or less to recover bis-2-hydroxyethyl terephthalate. (3) A process of dissolving the recovered bis-2-hydroxyethyl terephthalate in hot water at 85°C or higher and 100°C or lower, and filtering the water while hot. (4) After carrying out the step (3), the filtered solution at 85°C or higher and 100°C or lower is cooled to 30°C or lower to crystallize and recover bis-2-hydroxyethyl terephthalate. (5) A step in which, in either the step (3) and / or the step (4), bis-2-hydroxyethyl terephthalate is dissolved in hot water and subjected to an activated carbon treatment or an ion exchange treatment. Effect of the Invention

[0015] According to the present invention, the cellulose content can be sufficiently reduced by simply contacting the recovered fabric with ethylene glycol. For example, when the recovered fabric is a blend of polyester and cellulose, the content of cotton or cotton-derived cellulose can be reduced to 0.4% or less, and a polyester resin of the same quality as that before recycling can be produced without an additional step of removing cellulose-derived pyrolysis foreign matter in the subsequent chemical recycling. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will be described in detail below.

[0017] The present invention relates to a method for reducing the cellulose content to a range of 0% to 0.4% by contacting recovered fabric having a cellulose content of 0.5% or more and less than 5.0% with ethylene glycol at 150°C or more and 205°C or less for 5 minutes to 120 minutes.

[0018] In addition, the recovered fabric in the present invention is not limited to fabric-shaped fabric, but also includes cut pieces of recovered fabric.

[0019] The cellulose contained in the recovered fabric according to the present invention is assumed to be cotton, rayon, polynosic, and hydrolysates thereof, but is not limited to these so long as it is cellulose.

[0020] The recovered fabric may contain any other fibers as long as it contains 0.5% or more and less than 5.0% cellulose. Specifically, it may be composed of polyester fibers such as polyethylene terephthalate fibers, polypropylene terephthalate fibers, and polybutylene terephthalate fibers, polyolefin fibers such as polyethylene fibers and polypropylene fibers, acrylic fibers such as polyacrylonitrile fibers, and nylon fibers such as polyamide 6 fibers and polyamide 66 fibers. However, if it is assumed that the synthetic fibers will ultimately be chemically recycled, it is preferable that the fabric is composed of only one of these fibers in addition to cellulose. In addition, since there is no need to provide a cleaning process for the attached ethylene glycol after the contact treatment with ethylene glycol, it is more preferable to apply the method to polyester fibers such as polyethylene terephthalate fibers, polypropylene terephthalate fibers, and polybutylene terephthalate fibers, and most preferably to polyethylene terephthalate fibers. In addition, the reason why there is no need to provide a cleaning process for ethylene glycol in the case of polyester fibers is that ethylene glycol functions as a depolymerization solvent for polyester fibers and does not become a foreign substance in the subsequent chemical recycling process.

[0021] In addition, when the fiber other than cellulose contained in the recovered fabric is polyester fiber, its content is preferably 10.0% or more and 99.5% or less. If the content of polyester fiber is within this range, raw material ester monomer can be efficiently obtained when carrying out chemical recycling after carrying out the treatment described in the present invention. If the content of polyester fiber is less than 10.0%, it is difficult to obtain raw material polyester enough to carry out chemical recycling. If it is contained more than 99.5%, chemical recycling of polyester is possible without the need to carry out the method described in the present invention.

[0022] In order to reduce the cellulose content to 0% or more and 0.4% or less by contacting the recovered fabric with ethylene glycol, it is essential that the cellulose content in the recovered fabric is 0.5% or more and less than 5.0%. When the cellulose content in the recovered fabric is less than 0.5%, even if the recovered fabric is chemically recycled without performing a cellulose content reduction treatment, there is almost no need to perform an additional cellulose-derived pyrolysis foreign matter removal step, and there is no point in applying the present invention. On the other hand, when the cellulose content in the recovered fabric is more than 5.0%, it is difficult to remove cellulose to 0.4% or less by contact treatment with ethylene glycol alone. In terms of enabling more efficient removal of cellulose, the cellulose content in the recovered fabric to be contacted with ethylene glycol is preferably 3.0% or less, and more preferably 1.0% or less.

[0023] When the cellulose content in the recovered fabric is more than 5.0%, the cellulose content in the recovered fabric is adjusted to a range of 0.5% or more and less than 5.0% by some method before the contact treatment with ethylene glycol is performed. The method of adjusting the cellulose content to a range of 0.5% or more and less than 5.0% is not particularly limited, and known techniques such as dissolving and extracting cellulose using a dimethylacetamide solution or ionic liquid to which lithium chloride has been added, or removing cellulose by oxidative or enzymatic decomposition by heat treatment of cotton in an ozone treatment, an acidic aqueous solution, or an enzyme aqueous solution can be adopted. Among them, the method of heat treatment of cotton in an acidic aqueous solution to oxidatively decompose cellulose and process it into a powder form to be released from the recovered fabric can be preferably adopted because it can be carried out at low cost and low energy consumption. As the acidic aqueous solution, an inorganic acid aqueous solution such as an aqueous hydrochloric acid solution, an aqueous nitric acid solution, an aqueous phosphoric acid solution, or an aqueous sulfuric acid solution adjusted to a concentration of 0.2% to 5.0% may be used, or an organic acid aqueous solution such as an aqueous citric acid solution or an aqueous succinic acid solution may be used. The recovered fabric is immersed in these acidic aqueous solutions and heated to 90°C to 150°C to hydrolyze the cellulose, and then the powdery cellulose is removed from the recovered fabric by washing with water or the like, thereby quickly adjusting the cellulose content of the recovered fabric to a range of 0.5% or more and less than 5.0%.

[0024] The cellulose in the recovered fabric usually has a weight-average molecular weight in the range of 160,000 to 1,500,000, but it is preferable to adjust the weight-average molecular weight to a range of 7,000 to 150,000 by some method before contacting with ethylene glycol. By adjusting the weight-average molecular weight of cellulose to 150,000 or less, more preferably 60,000 or less, the cellulose content can be quickly reduced to a range of 0% to 0.4% during contacting with ethylene glycol. On the other hand, if the weight-average molecular weight of cellulose is decomposed to less than 7,000, regardless of the method, the molecules constituting the synthetic fibers in the recovered fabric will also be deteriorated, which is undesirable because it has a negative effect on chemical recycling. There is no particular limit to the method for adjusting the weight-average molecular weight of cellulose to a range of 7,000 to 150,000, but a method of oxidatively decomposing cotton in an acidic aqueous solution can be preferably adopted because it can be carried out at low cost and with low energy consumption. The acidic aqueous solution may be an inorganic acid aqueous solution such as an aqueous hydrochloric acid solution, an aqueous nitric acid solution, an aqueous phosphoric acid solution, or an aqueous sulfuric acid solution adjusted to a concentration of 0.2% to 5.0%, or an organic acid aqueous solution such as an aqueous citric acid solution or an aqueous succinic acid solution. The recovered fabric is immersed in such an acidic aqueous solution and heated to 90° C. to 150° C. to hydrolyze the cellulose, thereby quickly adjusting the weight-average molecular weight of the cellulose in the recovered fabric to a range of 7,000 to 150,000.

[0025] In order to reduce the cellulose content to a range of 0% to 0.4% by contacting the recovered fabric with ethylene glycol, it is essential that the temperature of the ethylene glycol to be contacted is 150°C to 205°C. When the temperature of ethylene glycol is 150°C or higher, more preferably 185°C or higher, the cellulose in the recovered fabric is solvolyzed to a lower molecular weight and quickly extracted from the fabric, and the cellulose content can be reduced to a range of 0% to 0.4%. On the other hand, when the temperature is 205°C or lower, the solvolysis of cellulose can be promoted while suppressing the decomposition of the synthetic fibers constituting the recovered fabric. When the recovered fabric is contacted with ethylene glycol vapor or a pressurized ethylene glycol solution at a temperature higher than 205°C, the decomposition of the synthetic fibers constituting the recovered fabric also proceeds quickly, and the yield of the fabric is reduced.

[0026] Furthermore, when the recovered fabric is contacted with ethylene glycol, in order to most efficiently remove cellulose and obtain a high yield of fabric, a method of simultaneously contacting the recovered fabric with ethylene glycol vapor at 195°C to 205°C and ethylene glycol liquid at 150°C to 195°C may be adopted, that is, a method of exposing the recovered fabric to an ethylene glycol reflux environment. By adopting this method, the cellulose content can be reduced to 0% to 0.4% even in a short treatment time of 5 minutes. In addition, as a secondary advantage of adopting this method, when the fibers other than cellulose constituting the recovered fabric are polyester fibers containing dyes, it is expected that the dyes in the polyester can be extracted, making chemical recycling easier.

[0027] In the present invention, it is essential that the time for contacting the recovered fabric with ethylene glycol is 5 minutes or more and 120 minutes or less. By contacting with ethylene glycol for 5 minutes or more, preferably 15 minutes or more, more preferably 30 minutes or more, the cellulose in the recovered fabric is decomposed into lower molecular weights by solvolysis and is quickly extracted from the fabric, and the cellulose content can be reduced to a range of 0% to 0.4%. On the other hand, when the contact time is 120 minutes or less, more preferably 60 minutes or less, the solvolysis of cellulose is completed before the decomposition of the synthetic fibers constituting the recovered fabric progresses, and the cellulose content can be reduced to a range of 0% to 0.4% with good yield. If the contact time is longer than 120 minutes, the decomposition of the synthetic fibers constituting the recovered fabric also progresses, and the yield of the fabric deteriorates.

[0028] In order to increase the purity of the regenerated resin and suppress coloration when chemically recycling the fabric obtained by the method of the present invention, the cellulose content in the fabric obtained must be 0.4% or less, preferably 0.3% or less, more preferably 0.2% or less, even more preferably 0.1% or less, and most preferably 0.05% or less. The lower limit of the cellulose content is 0%.

[0029] The method of the present invention can reduce the cellulose content to a range of 0% or more and 0.4% or less. However, when the fibers other than cellulose constituting the fabric obtained by the method of the present invention are mainly polyester fibers, the following chemical recycling steps (1) to (5) can be further carried out to obtain bis-2-hydroxyethyl terephthalate (BHET) having a color tone b* value in the range of -5 to 5. (1) A process of adding ethylene glycol to a fabric to depolymerize it, thereby obtaining an ethylene glycol solution containing bis-2-hydroxyethyl terephthalate. (2) A step of removing ethylene glycol from the ethylene glycol solution containing bis-2-hydroxyethyl terephthalate after depolymerization until the ethylene glycol is in the range of 0 mass % or more and 5 mass % or less to recover bis-2-hydroxyethyl terephthalate. (3) A process of dissolving the recovered bis-2-hydroxyethyl terephthalate in hot water at 85°C or higher and 100°C or lower, and filtering the water while hot. (4) After carrying out the step described in (3), the filtered solution having a temperature of 85°C or higher and 100°C or lower is cooled to 30°C or lower to crystallize and recover bis-2-hydroxyethyl terephthalate. (5) A step of subjecting bis-2-hydroxyethyl terephthalate dissolved in hot water to an activated carbon treatment or an ion exchange treatment in either step (3) and / or (4).

[0030] The ion exchange treatment means exposing the target solution to an ion exchange membrane or ion exchange resin. When the cellulose content in the fabric is more than 0.4%, even if the above-mentioned chemical recycling steps (1) to (5) are performed, it is not possible to obtain a BHET having a color tone b* value in the range of -5 to 5, and an additional purification step is required.

[0031] When the fabric obtained by the method of the present invention is mainly composed of polyester fibers as a component other than cellulose and is subjected to chemical recycling to obtain its raw material monomer, BHET, the color tone b* value is preferably in the range of -5 to 5, more preferably in the range of -2 to 2. When the color tone b* value is in this range, the color tone of the recycled polyester resin obtained by polycondensation of BHET will be equivalent to that of virgin polyester resin.

[0032] Steps (1) to (5) will be described in detail. First, in step (1), ethylene glycol is added to the polyester fabric obtained by the method of the present invention to depolymerize it, and an ethylene glycol solution containing bis-2-hydroxyethyl terephthalate is obtained. If the amount of EG added during depolymerization is less than 2.0 parts by weight per part by weight of PET fabric, the molecular weight of the resulting BHET increases, resulting in a poor yield in the subsequent purification step, and thus a decrease in efficiency. The amount of EG added is preferably 2.0 parts by weight or more per part by weight of PET fabric. In addition, adding more than 10.0 parts by weight of EG produces the same effect, and is therefore undesirable from the standpoint of cost.

[0033] In step (1), the temperature in the depolymerization is preferably 190° C. or higher and 210° C. or lower. From the viewpoint of efficient depolymerization, it is preferable to add sodium hydroxide or sodium carbonate in an amount of 0.5% by weight or higher and 2.0% by weight or lower based on BHET per 100 parts by weight of EG.

[0034] When chemically recycling the polyester fiber obtained by the method of the present invention, it is preferable to carry out a step of removing EG from the BHET after depolymerization until the EG content falls within the range of 0% by weight or more and 5% by weight or less. If the EG content in the BHET is more than 5% by weight, this is not preferable because it will result in a decrease in yield in the subsequent hot filtration step and crystallization step.

[0035] Next, in step (2), ethylene glycol is removed from the ethylene glycol solution containing the bis-2-hydroxyethyl terephthalate after depolymerization until the ethylene glycol concentration is in the range of 0% by mass or more and 5% by mass or less to recover the bis-2-hydroxyethyl terephthalate. Any of the following methods may be used as a step for removing EG from the BHET after depolymerization. The first is a reprecipitation step in which the EG solution of BHET obtained by depolymerization is dropped into water adjusted to 20°C or less to obtain a cloudy solution, and then the BHET containing impurities is recovered using a filter. The water temperature is preferably 15°C or less in terms of increasing the yield, and more preferably 10°C or less. The second is a distillation step in which the EG contained in the EG solution obtained by depolymerization is distilled off and concentrated. Specifically, EG can be quickly removed by reducing the pressure to a range of 200 to 1000 Pa while heating to 80 to 150°C.

[0036] Next, in step (3), the recovered bis-2-hydroxyethyl terephthalate is dissolved in hot water at 85°C to 100°C and filtered while hot. In order to remove impurities (metal compounds such as titanium oxide and inorganic compounds such as silica gel) contained in the polyester fiber, it is preferable to adopt a hot water dissolution step and a hot filtration step. Water is dropped onto the recovered BHET obtained in the EG removal step, heated to 85°C or higher, and passed through a filter to obtain a transparent high-temperature aqueous solution in which BHET is dissolved.

[0037] Next, in step (4), the filtered solution at 85°C to 100°C is cooled to 30°C or less to crystallize and recover bis-2-hydroxyethyl terephthalate. From the viewpoint of obtaining BHET in high yield, the cooling temperature is preferably 30°C or less, more preferably 15°C or less, even more preferably 10°C or less, and most preferably in the range of 2 to 5°C. In addition, it is preferable to carry out the adsorption treatment described in the lower part before crystallization from the viewpoint of obtaining BHET with excellent color tone. After crystallization, BHET is subjected to solid-liquid separation by a method such as filtration or centrifugation, and then dried by blowing or hot air at 40 to 90°C to reduce the moisture content, which is preferable because the subsequent repolymerization can be carried out quickly.

[0038] Finally, as step (5), it is preferable to have an adsorption step in which an adsorbent such as activated carbon or an ion exchange membrane / ion exchange resin is added to the high-temperature aqueous solution of BHET after the hot filtration in step (3) or before the cooling in step (4) to remove impurities from the aqueous solution. An activated carbon treatment step is more preferable since it is possible to adsorb the coloring components regardless of their structures, and an ion exchange resin can also be suitably used when it is clear that most of the coloring components are derived from cationic dyes.

[0039] When exposing to activated carbon, etc., it is preferable to pass the solution through a column packed with activated carbon, etc., or to add activated carbon, etc. directly to the solution. When using a column, for example, when passing a 2.5% BHET aqueous solution, the passing time is preferably 10 minutes or more in order to improve the removal rate of impurities. On the other hand, in order not to deteriorate the BHET yield, the passing time is preferably 180 minutes or less.

[0040] Furthermore, when activated carbon or the like is added directly to the solution and the adsorption treatment is carried out for 60 to 90 minutes, the amount added is preferably in the range of 1% by weight to 65% by weight based on the BHET. After the adsorption treatment, a transparent high-temperature aqueous solution from which impurities and adsorbents such as activated carbon have been removed can be obtained by passing the solution through a filter, but this may not be necessary depending on the type of adsorbent.

[0041] When the polyester fiber obtained by the method according to the present invention is chemically recycled, the above-mentioned purification step can be carried out to obtain high-quality BHET having excellent color tone. The obtained high-quality BHET can be polymerized in the presence of a polymerization catalyst according to a known PET polymerization method to produce high-quality PET equivalent to virgin PET.

[0042] The absorbance intensity in the BHET obtained by chemically recycling the polyester fabric obtained by the method of the present invention can be evaluated using a spectrophotometer, and the absorbance intensity area (peak area) observed in the wavelength region of 450 nm to 800 nm can be 20 or less. In terms of obtaining a low amount of absorbance and high-quality BHET and PET resin, it is more preferably 15 or less, more preferably 10 or less, particularly preferably 5 or less, and most preferably 0.5 or less. The lower detection limit is 0.1.

[0043] In the method for producing the recycled polyester resin according to the present invention, the absorbance intensity is evaluated using a spectrophotometer as follows: A mixed solvent (1:4) of water and hexafluoroisopropanol is prepared, and then a solution containing 10% by weight of BHET is prepared using this mixed solvent. A spectrophotometer, for example a U3010 spectrophotometer manufactured by Hitachi High-Tech Science Corporation, is used to calculate the integrated value of the absorbance intensity from 450 to 800 nm in wavelength scan mode.

[0044] By chemically recycling the polyester fabric obtained by the method of the present invention, the BHET obtained can be polycondensed to obtain a polyethylene terephthalate resin having the same quality as that before recycling. EXAMPLES

[0045] A. Identification of the polymer types and their contents that make up the fabric The polymer species constituting the fabric and their content were identified by the following procedure. First, the recovered fabric was immersed in hexafluoro-2-propanol to dissolve the polyester fiber, acrylic fiber, and polyamide fiber, and then filtrate A and filter cake B were collected by filtration. Filtrate A was distilled to dryness to obtain solidified product C, and the weight was measured. 50 mg of solidified product C was dissolved in 1 mL of a heavy solvent (hexafluoro-2-propanol-D2), and composition analysis was performed using a nuclear magnetic resonance device (NMR, JEOL Ltd. "AL-400") with an accumulation number of 128 times to identify the polymer species (polyester fiber, acrylic fiber, or polyamide fiber), and the content of each was calculated.

[0046] Next, the filter cake B was immersed in an 8% LiCl (lithium chloride) / DMAc (dimethylacetamide) solution to dissolve the cellulose over 1 to 2 weeks, and then filtrate D and filter cake E were collected by filtration. The filtrate D was distilled to dryness to obtain solidified material F, which was washed with water and the dry weight was measured. It was confirmed that the solidified material F was cellulose using a Fourier transform infrared spectrometer (FT-IR, "NicoletiS10" manufactured by Thermo Fisher Scientific), and the cellulose content was calculated. Note that filter cake E may not be obtained depending on the composition of the fabric.

[0047] Furthermore, if fibrous matter remains in the filter cake E, it is immersed in o-dichlorobenzene heated to 150°C to dissolve the polyolefin fibers, and then filtered to collect the filtrate G. The filtrate G is distilled to dryness to obtain solidified matter I, whose weight is measured, and it is confirmed that the solidified matter I is polyethylene or polypropylene using a Fourier transform infrared spectrometer (FT-IR, Thermo Fisher Scientific's "NicoletiS10"), after which the polyethylene or polypropylene content is calculated.

[0048] B. Color analysis of fabric and BHET A Minolta CM-3700d spectrophotometer was used to analyze the color tone of the fabric and BHET. The samples were placed against a black calibration plate, and the L*, a*, and b* values ​​of the color tone were measured.

[0049] C. Molecular weight measurement of cellulose The molecular weight of cellulose was measured using gel permeation chromatography (Shimadzu Corporation's "Nexcera GPC system," detector: differential refractive index detector RI (RID-20A), column: PLgel 20 μm MIXED-A: 1 column, solvent: 8% LiCl / DMAc, flow rate: 0.5 mL / min, temperature: 23° C., standard substance: monodisperse pullulan) using the filtrate D described in Example A (adjusted to a cellulose concentration of 0.6%).

[0050] D. Fabric yield measurement in EG contact process The fabric yield in the EG contact step was calculated by subtracting the weight reduction rate, which was calculated by measuring the weight of the fabric before and after the EG contact step, from 100%.

[0051] E. Absorption intensity area The absorbance area using a spectrophotometer was measured as follows. For the sample used in the evaluation, a mixed solvent (1:4) of water and hexafluoroisopropanol was prepared, and then a solution of 10% by weight of BHET was prepared in this mixed solvent. Using a spectrophotometer (Hitachi High-Tech Science U3010 spectrophotometer) in wavelength scan mode, the integrated value of the absorbance from 450 to 800 nm (absorbance area) was calculated.

[0052] [Example 1] White waste clothing composed of 65% polyester and 35% cellulose was cut into 5 mm squares to prepare cellulose-containing recovered fabric. The polyester was polyethylene terephthalate fiber, and the cellulose was cotton fiber with a weight-average molecular weight of 1,300,000. 20.0 g of this recovered fabric was hydrolyzed in 500 mL of 0.3% hydrochloric acid solution at 130°C for 1 hour, washed with water for 30 minutes, and air-dried at 50°C to obtain 13.1 g of recovered fabric with a cellulose content of 0.5% or more and less than 5.0%. The cellulose content and weight-average molecular weight of the recovered fabric after hydrolysis are shown in Table 1.

[0053] A 2L four-neck flask was charged with 1000g of EG and 0.1g of sodium hydroxide, and then placed in a mantle heater. 13.1g of recovered fabric with a cellulose content of 0.5% or more and less than 5.0% was filled into a glass tube with a diameter of 25mm and a length of 300mm, and connected to the 2L four-neck flask. A Dimroth condenser was then connected to the top of the connected glass tube. The mantle heater was set to a temperature of 210°C and heating was started. The cellulose was extracted by exposing the fabric to EG reflux for 15 minutes to bring the fabric into contact with EG steam and high-temperature EG liquid. The temperature of the steam passing through the bottom of the glass tube was 195-205°C, and the temperature of the liquid EG refluxed through the Dimroth condenser was 185-195°C. The cellulose content in the recovered fabric after the EG contact treatment is shown in Table 1.

[0054] The extracted fabric was washed with water and dried, and 10.0 g was placed in a 1 L four-neck flask, 55 g of EG was added, and the mixture was stirred and depolymerized for 5.5 hours at an EG temperature of 200° C. When the depolymerized solution was cooled to 100° C. or lower, it was added dropwise to 500 mL of water adjusted to 10° C. or lower to obtain a cloudy solution. The resulting cloudy solution was filtered through a 4 μm filter to obtain low-purity BHET.

[0055] The obtained low-purity BHET was dissolved in hot water at 95°C and filtered using a 1.6μ filter. Activated carbon from Osaka Gas Chemicals was added to the obtained clear filtrate at 10% by weight based on the crude BHET, and the mixture was stirred while heating. After 1 hour, the activated carbon was removed using a 1.0μ filter. The obtained clear filtrate was cooled to below 20°C, and BHET was crystallized to perform solid-liquid separation. The solids were air-dried at 50°C to obtain purified BHET.

[0056] [Example 2] The cellulose-containing recovered fabric was black waste clothing dyed with a disperse dye (TERASIL BLACK WW-KSN) at a concentration of 5% owf, and the procedure was carried out in the same manner as in Example 1, except that the duration of the EG contact step was changed from 15 minutes to 30 minutes.

[0057] [Examples 3 to 5] The same procedure as in Example 1 was carried out except that the ratio of the constituent fibers of the cellulose-containing recovered fabric was as shown in Table 1.

[0058] [Examples 6 and 7] The same procedure as in Example 1 was repeated except that the acidic aqueous solution used in the hydrolysis treatment was changed as shown in Table 1.

[0059] [Examples 8 to 10] The same procedure as in Example 1 was carried out except that the duration of the EG contact step was changed as shown in Table 1.

[0060] [Examples 11 and 12] The EG contact step was carried out in the same manner as in Example 1, except that the recovered fabric was not packed in a glass tube but was directly placed in a 2 L four-neck flask and immersed in EG, a Dimroth condenser was connected directly to the 2 L four-neck flask instead of a glass tube, and the set temperature of the mantle heater was changed to 150°C or 190°C.

[0061] [Table 1]

[0062] [Comparative Examples 1 and 2] The ratio of the constituent fibers of the cellulose-containing recovered fabric is as shown in Table 2. The same procedure as in Example 1 was repeated, except that no prior hydrolysis treatment was performed and the EG contact step was carried out on recovered fabrics with a cellulose content of 35% or 5.0%.

[0063] In Comparative Examples 1 and 2, since recycled fabrics with a cellulose content of 5.0% or more were used, it was not possible to obtain a fabric with a cellulose content of 0% to 0.4% by the EG contact step alone. As a result, the purified BHET obtained by chemically recycling polyester fiber, the main component of the fabric, contained residual cellulose-derived pyrolysis foreign matter and had an inferior color tone b* value.

[0064] [Comparative Examples 3 to 5] As shown in Table 2, the same procedure as in Example 1 was repeated except that the EG contact step was not performed or the EG contact time was changed to 2 minutes or 150 minutes.

[0065] In Comparative Examples 3 and 4, the cellulose content of the fabric could not be reduced to the range of 0% to 0.4% because the cellulose extraction in the EG contact step was insufficient. As a result, the purified BHET obtained by chemically recycling the polyester fiber, the main component of the fabric, contained residual cellulose-derived pyrolysis foreign matter and had an inferior color tone b* value.

[0066] In Comparative Example 5, the EG contact step was excessive, so that the decomposition of polyester fiber, which is the main component of the fabric to be chemically recycled, also progressed, resulting in a significantly poor yield.

[0067] [Comparative Example 6] The EG contact step was carried out in the same manner as in Example 1, except that the recovered fabric was not packed in a glass tube but was directly placed in a 2 L four-neck flask and immersed in EG, a Dimroth condenser was connected directly to the 2 L four-neck flask instead of a glass tube, and the set temperature of the mantle heater was changed to 135°C.

[0068] In Comparative Example 6, the temperature of the EG in the EG contact step was insufficient, so that the extraction of cellulose did not proceed. As a result, the purified BHET obtained by chemically recycling polyester fiber, the main component of the fabric, contained residual cellulose-derived pyrolysis foreign matter and had an inferior color tone b* value.

[0069] [Table 2] [Industrial Applicability]

[0070] According to the present invention, the cellulose content can be sufficiently reduced simply by contacting recovered fabric with ethylene glycol, making the present invention useful in the chemical recycling of textiles and textile products.

Claims

1. A method for reducing the cellulose content to a range of 0% to 0.4% by contacting recovered fabric having a cellulose content of 0.5% or more and less than 5.0% with ethylene glycol at 150°C or more and 205°C or less for 5 minutes to 120 minutes.

2. 2. The method according to claim 1, wherein the weight average molecular weight of the cellulose in the recovered fabric is adjusted to 7,000 or more and 150,000 or less before contacting with ethylene glycol.

3. A method for reducing the cellulose content to a range of 0% or more and 0.4% or less, comprising hydrolyzing a recovered fabric containing cellulose in the range of 5% or more and 90% or less, thereby reducing the cellulose content to a range of 0.5% or more and less than 5.0%, and the cellulose weight average molecular weight to a range of 7,000 or more and 150,000 or less, and carrying out the treatment described in claim 1 on the recovered fabric.

4. The method according to any one of claims 1 to 3, wherein the recovered fabric contains 10.0% or more and 99.5% or less polyester fibers.

5. The method according to any one of claims 1 to 3, characterized in that in contacting the recovered fabric with ethylene glycol, the recovered fabric is simultaneously contacted with ethylene glycol vapor at 195°C or more and 205°C or less and ethylene glycol liquid at 150°C or more and 195°C or less for 5 minutes or more and 120 minutes or less.

6. A method for obtaining bis-2-hydroxyethyl terephthalate from a fabric containing a polyester obtained by the method according to any one of claims 1 to 3, the method comprising the steps (1) to (5) of obtaining bis-2-hydroxyethyl terephthalate having a color tone b* value in the range of -5 to 5: (1) A step of adding ethylene glycol to a fabric to depolymerize it, thereby obtaining an ethylene glycol solution containing bis-2-hydroxyethyl terephthalate. (2) A step of removing ethylene glycol from the ethylene glycol solution containing the depolymerized bis-2-hydroxyethyl terephthalate until the ethylene glycol content is in the range of 0 mass % or more and 5 mass % or less to recover bis-2-hydroxyethyl terephthalate. (3) A step of dissolving the recovered bis-2-hydroxyethyl terephthalate in hot water at 85° C. or higher and 100° C. or lower, and filtering the resultant while hot. (4) A step of cooling the filtered solution at 85° C. or higher and 100° C. or lower to 30° C. or lower to crystallize and recover bis-2-hydroxyethyl terephthalate. (5) A step of carrying out an activated carbon treatment or an ion exchange treatment on bis-2-hydroxyethyl terephthalate dissolved in hot water in the steps (3) and / or (4).

7. 6. Bis-2-hydroxyethyl terephthalate obtained by the method for obtaining bis-2-hydroxyethyl terephthalate according to claim 5, wherein the absorption intensity area observed in the range of 450 nm to 800 nm using a spectrophotometer is 20 or less.

8. A polyethylene terephthalate resin obtained by polycondensation of the bis-2-hydroxyethyl terephthalate according to claim 5.

Citation Information

Patent Citations

  • Method for recovering useful component from polyester waste

    JP2002060542A

  • Separation method of mixed fiber, production method of first fiber, production method of decomposed material of second fiber, and production method of decomposed material of third fiber

    JP2019035022A

  • Fiber separation

    JP2022515368A